Modified polypropylene film, preparation method therefor and use thereof

By introducing terpene alcohol modifier into the polypropylene film, the surface tension and dielectric constant are improved, and the problems of poor adhesion and hole defects in the composite fluid collection are solved, and modified polypropylene films with excellent performance are prepared. The acrylic film realizes the stability and high performance of the composite fluid collection.

WO2024244050A1PCT designated stage expired Publication Date: 2024-12-05JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/099589
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2023-06-12
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

When preparing the composite liquid collector, traditional polypropylene film has low surface tension and low dielectric constant, resulting in poor adhesion between the base film and the metal layer and is prone to electrostatic breakdown, resulting in hole defects.

Method used

By introducing terpene alcohol as a modifier, the surface tension and dielectric constant of the polypropylene film are enhanced, and a conjugated structure is formed to enhance the force between the metal and the film, and by controlling the grafting rate and preparation process, the film is improved. Mechanical properties.

Benefits of technology

Modified polypropylene film with strong surface adhesion performance, high dielectric constant and good mechanical properties was prepared, which solved the problems of weak adhesion between the base film and metal layer and hole defects, and prepared a composite set with stable structure and low defects. fluid.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023099589_05122024_PF_FP_ABST
    Figure CN2023099589_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A modified polypropylene film, a preparation method therefor and a use thereof. A preparation raw material of the modified polypropylene film comprises modified polypropylene, and a modifier for the modified polypropylene comprises terpenol. The preparation method comprises the following steps: (1) melting, filtering and extruding the preparation raw material of the modified polypropylene film to obtain a molten material; and (2) casting the molten material obtained in step (1) onto a casting roller, performing cooling for formation, and carrying out two-way stretching to obtain the modified polypropylene film. Modified polypropylene is prepared using a specific modifier, and a modified polypropylene film having excellent performance is prepared by using the modified polypropylene as a preparation raw material, so that the modified polypropylene film is suitable for being used as a composite current collector base film.
Need to check novelty before this filing date? Find Prior Art

Description

A modified polypropylene film and its preparation method and application

[0001] This application claims priority to the Chinese patent application number 202310614748.X filed with the China Patent Office on May 29, 2023. The entire contents of the above application are incorporated by reference into this application. Technical Field

[0002] The present application belongs to the technical field of polymer membranes, for example, a modified polypropylene membrane and its preparation method and application. Background Art

[0003] At present, composite current collectors based on polymer membranes have received widespread attention and application in the new energy industry. The preparation process of the composite current collector is usually: a layer of metal (aluminum, copper, etc.) material is deposited on a polymer film (such as polypropylene, polyethylene, polyester, etc.) by physical vapor deposition (PVD) method. The prepared surface metallized film with a certain conductivity is the composite current collector. Compared with traditional current collectors, composite current collectors based on polymer membranes have the characteristics of low cost, light weight, and good internal insulation. These characteristics enable the composite current collector to reduce the cost of the battery and improve the energy density and safety of the battery when used in the battery.

[0004] Among the many composite current collectors based on polymer films, composite current collectors based on polypropylene films are relatively common. However, in the process of preparing composite current collectors using traditional polypropylene films as base films, the following problems exist: ① Due to the weak polarity of the polypropylene film itself, its surface tension is low, and the affinity between the low surface tension polypropylene film and the high surface tension metal layer is poor, resulting in low adhesion between the interface between the two and a weak bond, that is, the problem of poor surface adhesion of the polypropylene film. ② The dielectric constant of the polypropylene film is 2.1, which is relatively low. As a result, in the process of preparing composite current collectors using the physical vapor deposition method using the polypropylene film as the base film, the polypropylene film is easily broken down by a locally high electrostatic voltage, thereby generating hole defects.

[0005] Therefore, in order to solve the above problems of traditional polypropylene membranes and prepare high-performance composite current collectors, it is necessary to develop a modified polypropylene membrane.

[0006] Summary of the Invention

[0007] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0008] The purpose of this application is to provide a modified polypropylene film and its preparation method and application. In this application, modified polypropylene is prepared by selecting a specific modifier, and this modified polypropylene is used as a preparation raw material to prepare a modified polypropylene film with excellent performance, making it suitable for use as a composite current collector base film.

[0009] To achieve this goal, this application adopts the following technical solutions:

[0010] In a first aspect, an embodiment of the present application provides a modified polypropylene film, wherein the raw material for preparing the modified polypropylene film includes modified polypropylene;

[0011] The modifier for modifying polypropylene includes terpene alcohol.

[0012] In the examples of the present application, modified polypropylene is obtained by selecting a specific modifier, and the modified polypropylene is used as a raw material to prepare a modified polypropylene film with excellent performance, making it suitable for use as a composite current collector base film.

[0013] In the embodiments of the present application, on the one hand, the hydroxyl groups in the terpene alcohol molecules are used to increase the surface tension of the prepared modified polypropylene film, and the terpene alcohol molecules have a conjugated structure and can form an electronic conjugated system with metal atoms. The increase in surface tension and the formation of the conjugated structure jointly promote the interaction between the metal atoms and the modified polypropylene film, thereby increasing the adhesion between the base film and the metal layer in the prepared composite current collector; on the other hand, the dielectric constant of the terpene alcohol-modified polypropylene is higher than that of polypropylene. Introducing terpene alcohol-modified polypropylene into the raw materials for preparing the modified polypropylene film can increase the dielectric constant of the modified polypropylene film, thereby solving the problem of holes caused by the breakdown of the polypropylene film during the physical vapor deposition process.

[0014] In the embodiments of the present application, the dielectric constant of the modified polypropylene film is improved by introducing polar functional groups and conjugated structures into the modified polypropylene film.

[0015] The following are optional technical solutions for this application, but are not intended to limit the technical solutions provided in this application. Through the following preferred technical solutions, the objectives and beneficial effects of this application can be better achieved and realized.

[0016] As an optional technical solution of the present application, the grafting rate of terpene alcohol in the modified polypropylene is ≥0.05% (for example, it can be 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9% or 10%, etc.), preferably 0.05%-10%.

[0017] In the embodiments of the present application, the grafting rate is the ratio of the mass of the terpene alcohol monomer grafted onto the polypropylene to the mass of the grafted polypropylene.

[0018] In the examples of the present application, by controlling the grafting ratio of terpene alcohols in the modified polypropylene within a specific range, the performance of the modified polypropylene film is improved, resulting in a higher dielectric constant and higher mechanical properties. If the grafting ratio of terpene alcohols in the modified polypropylene is too low, the performance improvement of the prepared polypropylene film is limited. If the grafting ratio of terpene alcohols in the modified polypropylene is too high, the modified polypropylene with such a high grafting ratio may affect the orientation and crystallization of the polypropylene polymer during stretching, thereby reducing the tensile strength of the prepared modified polypropylene film.

[0019] In one embodiment, the terpene alcohol includes any one of 4-terpene alcohol, α-terpineol, carveol, lavandulol, nerol, and geraniol, or a combination of at least two thereof.

[0020] In the embodiment of the present application, the preparation method of the modified polypropylene comprises the following steps:

[0021] The reactor is fully replaced with nitrogen and dried, and then the terpene alcohol, polypropylene, organic solvent and catalyst are added to the reactor, and then the temperature is raised to 60-100°C under a nitrogen atmosphere, and the reaction is carried out for 2-24 hours, and then the temperature is lowered to room temperature. The mixed liquid is discharged from the reactor with nitrogen, filtered, washed and dried to obtain modified polypropylene;

[0022] In one embodiment, the organic solvent is selected from C6-C20 alkane solvents (for example, C6, C7, C8, C9, C10, C11, C12, C13, C14, C15, C16, C17, C18, C19 or C20, etc.), and is further selected from n-hexane.

[0023] In one embodiment, the catalyst is selected from any one of a Ziegler-Natta catalyst, a DQC catalyst or a HR catalyst.

[0024] It should be noted that there is no special restriction on the manufacturer of the catalyst in the examples of the present application, and an exemplary example includes: HR catalyst is purchased from Sinopec Catalyst Co., Ltd.

[0025] The mass of the added terpene alcohol is 0.50-150 g, the mass of the polypropylene is 890.0-999.5 g, the volume of the organic solvent is 800-2000 mL, and the mass of the catalyst is 10-50 g.

[0026] In the embodiments of the present application, the mass of the added terpene alcohol can be 0.50g, 1.00g, 2.00g, 5.00g, 10.0g, 20.0g, 40.0g, 60.0g, 80.0g, 100g, 120g, 135g or 150g, etc.

[0027] The mass of the polypropylene can be 890.0g, 900.0g, 910.0g, 920.0g, 930.0g, 940.0g, 950.0g, 960.0g, 970.0g, 980.0g, 990.0g or 999.5g, etc.

[0028] The volume of the organic solvent can be 800 mL, 900 mL, 1000 mL, 1100 mL, 1200 mL, 1300 mL, 1400 mL, 1500 mL, 1600 mL, 1700 mL, 1800 mL, 1900 mL or 2000 mL, etc.

[0029] The mass of the catalyst can be 10g, 15g, 20g, 25g, 30g, 35g, 40g, 45g or 50g, etc.

[0030] The reaction temperature for preparing the modified polypropylene can be 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C, and the reaction time can be 2h, 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h or 24h, etc.

[0031] As an optional technical solution of the present application, the melt index of the polypropylene in the modified polypropylene is 3.0-4.0 g / 10min, for example, it can be 3.0 g / 10min, 3.1 g / 10min, 3.2 g / 10min, 3.3 g / 10min, 3.4 g / 10min, 3.5 g / 10min, 3.6 g / 10min, 3.7 g / 10min, 3.8 g / 10min, 3.9.g / 10min or 4.0 g / 10min, etc.

[0032] In the examples of the present application, by selecting polypropylene with a melt index within a specific range, film formation is facilitated during the stretching step of preparing the modified polypropylene film, and the resulting modified polypropylene film has good performance. If the melt index of the polypropylene is too low and the molecular weight is too high, the film-forming properties of the modified polypropylene film during the stretching process will be poor; if the melt index of the polypropylene is too high and the molecular weight is too low, the film-forming properties will be poor and the mechanical properties of the resulting modified polypropylene film will be poor.

[0033] In the examples of the present application, the test conditions for the melt index are 230°C / 2.16kg.

[0034] In one embodiment, the molecular weight distribution of the polypropylene in the modified polypropylene is 4.5-5.5, for example, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4 or 5.5.

[0035] In the examples of the present application, by controlling the molecular weight distribution of polypropylene within a specific range, the resulting modified polypropylene film exhibits excellent mechanical properties and a high yield rate. If the molecular weight distribution index of polypropylene is too high, the content of low-molecular-weight polypropylene increases, resulting in poor mechanical properties and film-forming properties of the prepared film. If the molecular weight distribution index of polypropylene is too low, the film-forming properties of the modified polypropylene deteriorate during the film drawing process, resulting in a low product yield rate.

[0036] In one embodiment, the isotacticity of the polypropylene in the modified polypropylene is ≥95%, for example, it can be 95%, 95.5%, 96%, 96.5%, 97%, 97.5% or 98%.

[0037] In the embodiments of the present application, the mechanical properties of the modified polypropylene film can be further improved by controlling the isotacticity of the polypropylene to ≥95%. A higher isotacticity of the polypropylene increases the regularity of the polypropylene molecules. This increased regularity of the polypropylene can improve the orientation and crystallinity of the prepared film, thereby improving the mechanical properties of the modified polypropylene film.

[0038] As an optional technical solution of the present application, taking the mass percentage of the raw materials for preparing the modified polypropylene film as 100%, the mass percentage of the modified polypropylene is ≥0.5%, for example, it can be 0.5%, 1%, 2%, 5%, 7%, 10%, 13%, 15%, 18%, 20% or 24%, etc.

[0039] In the embodiment of the present application, the performance of the modified polypropylene film can be significantly improved by controlling the weight percentage of modified polypropylene in the raw materials for preparing the modified polypropylene film to ≥ 0.5%. If the weight percentage of modified polypropylene is too low, the improvement in the performance of the modified polypropylene film is limited.

[0040] In one embodiment, the raw materials for preparing the modified polypropylene film further include polypropylene.

[0041] As an optional technical solution of the present application, the thickness of the modified polypropylene film is ≥1μm (for example, it can be 1μm, 2μm, 5μm, 7μm, 10μm, 12μm, 15μm, 18μm, 20μm, 24μm, 27μm or 30μm, etc.), preferably 2-20μm.

[0042] The thinner the modified polypropylene film is, the more it can promote the improvement of the energy density of the composite current collector, but the production difficulty needs to be taken into account at the same time. Since the thinner the modified polypropylene film is, the greater the production difficulty and the lower the yield rate, therefore, in the embodiment of the present application, the thickness of the modified polypropylene film is controlled to be ≥1μm, which can not only prepare a modified polypropylene film with excellent performance, but also take into account the production process of the modified polypropylene film, so that it has a higher yield rate.

[0043] In a second aspect, an embodiment of the present application provides a method for preparing the modified polypropylene film as described in the first aspect, the preparation method comprising the following steps:

[0044] (1) melting, filtering, and extruding the raw materials for preparing the modified polypropylene film to obtain a molten material;

[0045] (2) Casting the molten material obtained in step (1) onto a casting roll, cooling and forming the molten material, and then biaxially stretching the molten material to obtain the modified polypropylene film.

[0046] In the embodiments of the present application, by selecting modified polypropylene as the raw material for preparing the modified polypropylene film and selecting the melt extrusion-biaxial stretching preparation process, a modified polypropylene film with a higher dielectric constant and better mechanical properties is prepared, making it suitable for use as a composite current collector base film.

[0047] As an optional technical solution of the present application, the melting temperature is 200-260°C, for example, it can be 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C or 260°C, etc.

[0048] In one embodiment, the filtering method includes filtering through a filter with a filter mesh of 10 μm.

[0049] In one embodiment, the cooling molding method is molding through water cooling treatment.

[0050] In one embodiment, the cooling molding temperature is 15-60°C, for example, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C or 60°C.

[0051] It should be noted that, in the examples of the present application, melting and extrusion are carried out in a twin-screw extruder.

[0052] As an optional technical solution of the present application, the biaxial stretching includes synchronous stretching and asynchronous stretching.

[0053] In one embodiment, the simultaneous stretching process includes preheating, stretching and heat setting.

[0054] In one embodiment, the preheating area includes a first preheating zone and a second preheating zone.

[0055] In one embodiment, the temperature of the first preheating zone is 130-145°C, for example, 130°C, 132°C, 135°C, 137°C, 140°C, 142°C or 145°C.

[0056] In one embodiment, the temperature of the second preheating zone is 145-155°C, for example, 145°C, 146°C, 147°C, 148°C, 149°C, 150°C, 151°C, 152°C, 153°C, 154°C or 155°C.

[0057] In one embodiment, the stretching temperature includes a first stretching temperature and a second stretching temperature.

[0058] In one embodiment, the first stretching temperature is 155-160°C, for example, 155°C, 156°C, 157°C, 158°C, 159°C or 160°C.

[0059] In one embodiment, the second stretching temperature is 160-165°C, for example, 160°C, 161°C, 162°C, 163°C, 164°C or 165°C.

[0060] In one embodiment, the longitudinal stretching ratio of the stretching is 6-8, for example, it can be 6, 6.3, 6.5, 6.8, 7, 7.2, 7.5, 7.7 or 8.

[0061] In one embodiment, the transverse stretching zone of the stretching is 5-7, for example, it can be 5, 5.2, 5.5, 5.8, 6, 6.3, 6.5, 6.8 or 7, etc.

[0062] In one embodiment, the heat setting temperature is 165-169°C, for example, 165°C, 166°C, 167°C, 168°C or 169°C.

[0063] In one embodiment, the asynchronous stretching process includes longitudinal stretching, transverse stretching and heat treatment.

[0064] In one embodiment, the preheating temperature for longitudinal stretching is 115-140°C, for example, 115°C, 118°C, 120°C, 124°C, 127°C, 130°C, 132°C, 135°C, 138°C or 140°C.

[0065] In one embodiment, the stretching temperature of the longitudinal stretching is 140-150°C, for example, 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C or 150°C.

[0066] In one embodiment, the longitudinal stretching ratio is 6-8, for example, 6, 6.3, 6.5, 6.8, 7, 7.2, 7.5, 7.7 or 8.

[0067] In one embodiment, the longitudinal stretching further includes a post-processing step.

[0068] In one embodiment, the post-treatment method includes cooling to room temperature.

[0069] In one embodiment, the preheating temperature for transverse stretching is 120-140°C, for example, 120°C, 122°C, 124°C, 126°C, 128°C, 130°C, 132°C, 134°C, 136°C, 138°C or 140°C.

[0070] In one embodiment, the stretching temperature of the transverse stretching is 140-160°C, for example, 140°C, 142°C, 144°C, 146°C, 148°C, 150°C, 152°C, 154°C, 156°C, 158°C or 160°C.

[0071] In one embodiment, the heat setting temperature for transverse stretching is 165-169°C, for example, 165°C, 166°C, 167°C, 168°C or 169°C.

[0072] In one embodiment, the stretching ratio of the transverse stretching is 5-7, for example, it can be 5, 5.2, 5.5, 5.8, 6, 6.3, 6.5, 6.8 or 7.

[0073] In one embodiment, the heat treatment temperature is 110-140°C, for example, 110°C, 112°C, 115°C, 118°C, 120°C, 124°C, 127°C, 130°C, 132°C, 135°C, 138°C or 140°C.

[0074] In one embodiment, the biaxial stretching further includes a post-processing step.

[0075] In one embodiment, the post-processing method includes: after air cooling in the platform area, the film enters the winding system through the traction system to be wound up.

[0076] In one embodiment, the winding tension is 20-30 N / m, for example, it can be 20 N / m, 21 N / m, 22 N / m, 23 N / m, 24 N / m, 25 N / m, 26 N / m, 27 N / m, 28 N / m, 29 N / m or 30 N / m, etc.

[0077] In the present application, the preparation method of the modified polypropylene film comprises the following steps:

[0078] (1) placing the raw materials for preparing the modified polypropylene film in a twin-screw extruder, melting them at 200-260° C., filtering them through a filter with a 10 μm filter screen, and extruding them through a die to obtain a molten material;

[0079] (2) casting the molten material obtained in step (1) onto a casting roller, cooling the molten material with water at 15-60° C. to form the film, biaxially stretching the film, and then air-cooling the film in a platform area. The film enters a winding system through a traction system, and is wound under a winding tension of 20-30 N / m to obtain the modified polypropylene film.

[0080] The biaxial stretching is synchronous stretching or asynchronous stretching.

[0081] The biaxial stretching is synchronous stretching, and the synchronous stretching includes the following process:

[0082] ① Preheating: divided into two stages, the temperature increases successively, i.e. 130-145℃ and 145-155℃;

[0083] ② Stretching: divided into two stages, with the temperature increasing successively, i.e. 155-160℃ and 160-165℃; stretching ratio: longitudinal stretching ratio is 6-8, transverse stretching ratio is 5-7;

[0084] ③ Heat setting: temperature is 165-169℃;

[0085] Alternatively, the biaxial stretching is asynchronous stretching, and the asynchronous stretching includes the following process:

[0086] ① Longitudinal stretching: preheating temperature: 115-140℃; stretching temperature: 140-150℃; longitudinal stretching ratio: 6-8, then cool to room temperature;

[0087] ② Transverse stretching: preheating temperature: 120-140℃; stretching temperature: 140-160℃; heat setting temperature: 165-169℃; transverse stretching ratio: 5-7;

[0088] ③ Heat treatment: The heat treatment temperature is 110-140℃, the purpose is to eliminate the internal stress of the membrane and improve the thermal stability of the membrane.

[0089] In a third aspect, an embodiment of the present application further provides a composite current collector, the composite current collector comprising a metal layer and a polymer film layer;

[0090] The polymer film layer is the modified polypropylene film as described in the first aspect.

[0091] The modified polypropylene film provided in the first aspect of the present application serves as a carrier and a supporting layer of the composite current collector.

[0092] In one embodiment, the material of the metal layer is selected from metal or metal alloy, and the metal is selected from any one of copper, aluminum, silver, gold, nickel, or a combination of at least two thereof.

[0093] In one embodiment, the composite current collector includes a first protective layer, a first metal layer, a polymer film layer, a second metal layer, and a second protective layer stacked in sequence;

[0094] The polymer film layer is the modified polypropylene film as described in the first aspect.

[0095] As an optional technical solution of the present application, the materials of the first metal layer and the second metal layer are each independently selected from metals or metal alloys.

[0096] In one embodiment, the metal is selected from any one of copper, aluminum, silver, gold, nickel, or a combination of at least two thereof.

[0097] In one embodiment, the thickness of the first metal layer and the second metal layer are independently selected from 500-2000 nm (for example, 500 nm, 700 nm, 1000 nm, 1200 nm, 1500 nm, 1800 nm or 2000 nm, etc.), and more preferably 700-1500 nm.

[0098] In the present application, the first metal layer and the second metal layer are each independently prepared by physical vapor deposition (such as resistance heating vacuum evaporation, electron beam heating vacuum evaporation, laser heating vacuum evaporation, magnetron sputtering, etc.), electroplating or chemical plating, or a combination of at least two of them.

[0099] In one embodiment, the materials of the first protective layer and the second protective layer are independently selected from any one or a combination of at least two of aluminum oxide, nickel oxide, chromium oxide, cobalt oxide, copper oxide, copper chromium oxide, formate-copper complex, nickel-chromium alloy, graphite, carbon nano-quantum dots, carbon nanotubes, carbon nanofibers and graphene.

[0100] In one embodiment, the thickness of the first protective layer and the second protective layer are each independently selected from 10-150nm (for example, it can be 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm or 150nm, etc.), and more preferably 20-100nm.

[0101] In one embodiment, the sum of the thicknesses of the first protective layer and the second protective layer is less than or equal to one tenth of the sum of the thicknesses of the first metal layer and the second metal layer.

[0102] In the embodiments of the present application, the preparation methods of the first protective layer and the second protective layer each independently include any one of physical vapor deposition, chemical vapor deposition, in-situ forming, and coating, or a combination of at least two thereof. Among these, the physical vapor deposition method is preferably vacuum evaporation and magnetron sputtering; the chemical vapor deposition method is preferably atmospheric pressure chemical vapor deposition and plasma-enhanced chemical vapor deposition; the in-situ forming method is preferably a method of forming a metal oxide passivation layer in situ on the surface of the metal layer; and the coating method is preferably die coating, blade coating, or extrusion coating.

[0103] In a fourth aspect, an embodiment of the present application provides a battery, comprising the composite current collector as described in the third aspect.

[0104] This application has the following beneficial effects:

[0105] (1) The present application obtains modified polypropylene by selecting a specific modifier, and uses the modified polypropylene as a raw material. The prepared modified polypropylene film has the characteristics of strong surface adhesion, high dielectric constant, and good mechanical properties. Its surface tension is 38 to 59 mN / m, the dielectric constant is 2.6 to 4.0 mN / m, and the tensile strength is 185 to 225 MPa.

[0106] (2) The composite current collector is prepared using the modified polypropylene film provided in the present application as the base film, which can solve the problems of weak adhesion between the base film and the metal layer in the composite current collector and many pore defects in the prepared composite current collector, thereby preparing a composite current collector with stable structure and low defects. The adhesion between the polymer film (modified polypropylene film) and the metal layer in the composite current collector is relatively large, which is 0.9 to 2.7 N / cm, and there are no holes on the prepared composite current collector. The square resistance of the composite current collector is relatively small, which is 17 to 18 mΩ, which promotes the promotion and application of the composite current collector in batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0107] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0108] FIG1 is a schematic structural diagram of a composite current collector provided in Application Example 1;

[0109] Among them, 1 is the first protective layer, 2 is the first metal layer, 3 is the polymer film layer, 4 is the second metal layer, and 5 is the second protective layer. DETAILED DESCRIPTION

[0110] The technical solution of the present application will be further described below with reference to the accompanying drawings and through specific implementation methods. Those skilled in the art should understand that the embodiments are only for the purpose of helping to understand the present application and should not be regarded as specific limitations of the present application.

[0111] The sources of some components in the following examples and comparative examples are as follows:

[0112] Polypropylene: melt index 3.0 g / 10 min (230°C / 2.16 kg), molecular weight distribution index 4.5, isotacticity 96%, purchased from TPC Company, Singapore, model FS3028;

[0113] Polypropylene: melt index 3.0 g / 10 min (230°C / 2.16 kg), molecular weight distribution index 4.5, isotacticity 93%, purchased from TPC Company, Singapore, model FS3025;

[0114] Catalyst: HR catalyst, purchased from Sinopec Catalyst Co., Ltd.

[0115] The polypropylene used in the following preparation examples is all polypropylene with model number FS3028.

[0116] Preparation Examples 1-9 and Comparative Example 1

[0117] Preparation Examples 1-5 provide a 4-terpene alcohol modified polypropylene, Preparation Examples 6-9 and Comparative Preparation Example 1 provide an α-terpineol modified polypropylene, lavandulol modified polypropylene, geraniol modified polypropylene, and propylene alcohol modified polypropylene, respectively;

[0118] The preparation method of the above-mentioned modified polypropylene is as follows:

[0119] The reactor was fully replaced with nitrogen and dried, and then the uniformly mixed modifier, polypropylene, n-hexane (1500 mL) and HR catalyst were added to the reactor. Then, under a nitrogen atmosphere, the temperature was raised to carry out the modification reaction, and then the temperature was lowered. The mixed liquid was discharged from the reactor with nitrogen, filtered, washed, and dried to obtain modified polypropylene;

[0120] The amounts of the modifier, polypropylene and HR catalyst are shown in Table 1 below, as are the reaction temperature and time.

[0121] Table 1

[0122] Example 1

[0123] This embodiment provides a modified polypropylene film and a preparation method thereof. The raw materials for preparing the modified polypropylene film include the following components in percentage by mass: 0.5% of the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1 and 99.5% of polypropylene;

[0124] Among them, the melt index of polypropylene is 3.0g / 10min (230℃ / 2.16kg), the molecular weight distribution index is 4.5, and the isotacticity is 96%;

[0125] The grafting rate of 4-terpene alcohol in the 4-terpene alcohol-modified polypropylene is 0.05%.

[0126] The preparation method of the above-mentioned modified polypropylene film is as follows:

[0127] (1) The raw materials for preparing the modified polypropylene film were placed in a twin-screw extruder, melted at 240°C, filtered through a filter with a 10 μm filter screen, and extruded through a die to obtain a molten material. The temperature of the die was 250°C.

[0128] (2) casting the molten material obtained in step (1) onto a casting roll, water-cooling the molten material at 20° C. to form the molten material, biaxially stretching the molten material, air-cooling the molten material in the platform area, and then passing through a traction system to a winding system. The molten material is wound under a winding tension of 30 N / m to obtain a modified polypropylene film having a thickness of 4.5 μm;

[0129] The biaxial stretching is asynchronous stretching, and the asynchronous stretching includes the following process:

[0130] ① Longitudinal stretching: preheating temperature: 138℃; stretching temperature: 145℃; longitudinal stretching ratio: 7. After longitudinal stretching, cool to room temperature;

[0131] ② Transverse stretching: preheating temperature: 130℃; stretching temperature: 152℃; heat setting temperature: 165℃; transverse stretching ratio: 6;

[0132] ③Heat treatment: heat treatment temperature 130℃.

[0133] Example 2

[0134] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that, calculated by weight percentage, the raw materials for preparing the modified polypropylene film include the following components in weight percentage: 50% of the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1 and 50% of polypropylene. Other conditions are the same as in Example 1.

[0135] Example 3

[0136] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the raw material for preparing the modified polypropylene film is only the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1, and other conditions are the same as those in Example 1.

[0137] Example 4

[0138] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that, calculated by weight percentage, the raw materials for preparing the modified polypropylene film include the following components in weight percentage: 0.4% of 4-terpene alcohol-modified polypropylene and 99.6% of polypropylene provided in Preparation Example 1. Other conditions are the same as those in Example 1.

[0139] Example 5

[0140] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1 is replaced by the 4-terpene alcohol-modified polypropylene with a grafting rate of 1.0% provided in Preparation Example 2. Other conditions are the same as those in Example 1.

[0141] Example 6

[0142] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1 is replaced by the 4-terpene alcohol-modified polypropylene with a grafting rate of 5.0% provided in Preparation Example 3. Other conditions are the same as in Example 1.

[0143] Example 7

[0144] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1 is replaced by the 4-terpene alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 4. Other conditions are the same as in Example 1.

[0145] Example 8

[0146] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1 is replaced with the 4-terpene alcohol-modified polypropylene with a grafting rate of 11.0% provided in Preparation Example 5. Other conditions are the same as in Example 1.

[0147] Example 9

[0148] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the 4-terpene alcohol-modified polypropylene provided in Preparation Example 1 is replaced by the 4-terpene alcohol-modified polypropylene with a grafting rate of 0.04% provided in Preparation Example 6. Other conditions are the same as in Example 1.

[0149] Example 10

[0150] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the raw material for preparing the modified polypropylene film is only the 4-terpene alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 4, and other conditions are the same as those in Example 1.

[0151] Example 11

[0152] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 10 is that the 4-terpene alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 4 is replaced with the α-terpineol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 7. Other conditions are the same as those in Example 10.

[0153] Example 12

[0154] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 10 is that the 4-terpene alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 4 is replaced by the lavender alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 8. Other conditions are the same as those in Example 10.

[0155] Example 13

[0156] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 10 is that the 4-terpene alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 4 is replaced by the geraniol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 9. Other conditions are the same as those in Example 10.

[0157] Example 14

[0158] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 1 is that the polypropylene (FS3028) with a melt index of 3.0 g / 10 min (230°C / 2.16 kg), a molecular weight distribution index of 4.5, and an isotacticity of 96% is replaced by a polypropylene (FS3025) with a melt index of 3.0 g / 10 min (230°C / 2.16 kg), a molecular weight distribution index of 4.5, and an isotacticity of 93%. Other conditions are the same as in Example 1.

[0159] Comparative Example 1

[0160] This comparative example provides a polypropylene film and a preparation method thereof. The only difference from Example 1 is that the raw material for preparing the polypropylene film is only polypropylene (FS3028), and other conditions are the same as those in Example 1.

[0161] Comparative Example 2

[0162] This embodiment provides a modified polypropylene film and a preparation method thereof. The only difference from Example 10 is that the 4-terpene alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Example 4 is replaced by the propylene alcohol-modified polypropylene with a grafting rate of 10.0% provided in Preparation Comparative Example 1. Other conditions are the same as those in Example 10.

[0163] Application Example 1

[0164] This application example provides a composite current collector and a preparation method thereof. The structural schematic diagram of the composite current collector is shown in FIG1 , comprising a first protective layer 1, a first metal layer 2, a polymer film layer 3, a second metal layer 4, and a second protective layer 5 stacked in sequence;

[0165] The polymer film layer 3 is the modified polypropylene film provided in Example 1.

[0166] The preparation method of the composite current collector is as follows:

[0167] The modified polypropylene film provided in Example 1 was placed in a magnetron sputtering chamber. Copper metal with a purity of 99.99% was used as a target material and argon gas was used as a gas source. A copper metal layer with a thickness of 100 nm was deposited on both sides of the modified polypropylene film by magnetron sputtering in the magnetron sputtering chamber to obtain a composite film. The composite film prepared was used as a substrate for electroplating to thicken the conductive copper layer and obtain a first protective layer 1 and a second protective layer 5. The electroplating process was divided into the following three steps: ① Electroplating to thicken the metal layer: the electroplating solution contained 120 g / L copper sulfate, 100 g / L sulfuric acid, 50 mg / L chloride ion, 1.2 mg / L sodium 3-mercapto-1-propanesulfonate, and 0.5 mg / L 2- Mercaptopyridine, 180 mg / L polyethylene glycol 10000, the plating solution temperature is 25°C, the average cathode current density is 2A / dm2, and the electroplating treatment is 5 minutes; ② Preparation of the first protective layer 1 and the second protective layer 5: After the electroplating is completed, the plated film is washed in a clean water tank, and then the surface protective layer is prepared in a protective layer preparation tank filled with 5 g / L potassium dichromate aqueous solution. The treatment temperature is 25°C, the treatment is 25s, and finally it is washed with a clean water tank; ③ Drying: The cleaned film is dried in an oven at a temperature of 65°C to finally obtain a composite current collector with a total thickness of 1.2 μm (wherein the thickness of the metal layer is 1170 nm and the thickness of the protective layer is 30 nm).

[0168] Application Example 2-14

[0169] Application Examples 2-14 respectively provide a composite current collector and a preparation method thereof. The difference from Application Example 1 is that the modified polypropylene film provided in Example 1 is replaced by the modified polypropylene film provided in Examples 2-14 in sequence, and other conditions are the same as those in Application Example 1.

[0170] Comparative Application Examples 1-2

[0171] Comparative Application Examples 1-2 respectively provide a composite current collector and a preparation method thereof. The difference from Application Example 1 is that the modified polypropylene film provided in Example 1 is replaced by the polypropylene film provided in Comparative Example 1 and the modified polypropylene film provided in Comparative Example 2, respectively. Other conditions are the same as those in Application Example 1.

[0172] The purpose of preparing a modified polypropylene film in this application is to improve the surface adhesion performance and dielectric constant of the polymer film, and thereby improve the performance of the composite current collector prepared with this modified polypropylene film as the substrate. The surface adhesion performance of the polypropylene film mainly depends on its surface tension, which is ultimately reflected in the adhesion between the base film and the metal layer in the composite current collector; and the change in the dielectric constant of the polypropylene film directly affects the number of holes in the composite current collector prepared therefrom. Therefore, this application tests the surface tension and dielectric constant of the prepared modified polypropylene film, the adhesion between the base film and the metal layer in the prepared composite current collector, and the number of hole defects. In addition, the tensile strength of the prepared modified polypropylene film and the square resistance of the prepared composite current collector were also tested. The specific method is as follows:

[0173] ① Surface tension: The surface tension of the modified polypropylene film prepared above was tested according to the standard GB / T 14216-2008;

[0174] ② Dielectric constant: The dielectric constant of the modified polypropylene film prepared above was tested according to standard SJ / T1147-1993;

[0175] ③ Tensile strength: The tensile strength of the modified polypropylene film prepared above was tested according to standard GB / T 1040.3-2006.

[0176] ④ The adhesion between the polypropylene film and the metal layer in the composite current collector: a layer of Permacel P-94 double-sided tape was adhered to a 1 mm thick aluminum foil, the composite current collector was adhered on top of the double-sided tape, and a layer of ethylene acrylic acid copolymer film (DuPont Nurcel0903, thickness of 50 μm) was covered on the composite current collector, and then the adhesion between the polypropylene film and the metal layer was tested at 1.3 × 105 N / m 2 , hot pressing at 120°C for 10 seconds, cooling to room temperature, and cutting into 150mm x 15mm strips. Finally, the ethylene acrylic acid copolymer film of the sample strip is fixed to the upper fixture of the tensile testing machine, and the rest of the film is fixed to the lower fixture. After fixing, the two are peeled at an angle of 180° and a speed of 100mm / min to test the peel force, that is, the adhesion between the polypropylene film and the metal layer;

[0177] ⑤ Number of hole defects per unit area of ​​composite current collector: The prepared composite current collector sample is placed in a surface quality detection system (micro-visual charge-coupled device CCD), its surface is scanned, and then the optical signal is converted into an electrical signal and transmitted to a computer. The number of hole defects per unit area of ​​the composite current collector with a pore size of less than 100 μm is counted (it is generally required that the finished product cannot have holes larger than 100 μm);

[0178] ⑥ Square resistance: Place the prepared composite current collector sample on the sample table and use a four-probe square resistance meter to test the square resistance of the sample.

[0179] The performance test results of the modified polypropylene films or polypropylene films provided in the above examples and comparative examples are shown in Table 2 below:

[0180] Table 2

[0181] As can be seen from the data in the above table, in this application, by selecting polypropylene with a specific melt index, a specific molecular weight distribution index, and a specific regularity, and selecting a specific modifier, while controlling the grafting rate of the modifier within a specific range, a modified polypropylene with excellent performance is prepared. This modified polypropylene is used as a raw material for preparing a modified polypropylene film, and the content of the modified polypropylene in the modified polypropylene film is controlled within a specific range. The prepared modified polypropylene film has a high surface tension, a high dielectric constant, and a high tensile strength. Its surface tension is 38 to 59 mN / m, the dielectric constant is 2.6 to 4.0 mN / m, and the tensile strength is 185 to 225 MPa.

[0182] Compared with Example 1, if the content of modified polypropylene in the raw materials for preparing the modified polypropylene film is too low (Example 4), the performance improvement of the prepared modified polypropylene film is limited compared with the polypropylene film (Comparative Example 1), and its surface tension, dielectric constant and tensile strength are all lower.

[0183] Compared with Example 1, if the grafting rate of the modifier in the modified polypropylene is low (Example 9), the surface tension, dielectric constant and tensile strength of the prepared modified polypropylene film are also poor; if the grafting rate of the modifier in the modified polypropylene is high (Example 8), the mechanical properties of the prepared modified polypropylene film are poor.

[0184] Compared with Example 1, the surface tension, dielectric constant and tensile strength of the polypropylene film prepared using polypropylene (Comparative Example 1) are all lower; if polypropylene modified with other modifiers is used to prepare the polypropylene film (Comparative Example 2), the surface tension, dielectric constant and tensile strength of the modified polypropylene film prepared are also poor.

[0185] In summary, in the present application, by selecting polypropylene with a specific melt index, a specific molecular weight distribution index and a specific regularity, and selecting a specific modifier, while controlling the grafting rate of the modifier within a specific range, a modified polypropylene with excellent performance is prepared. This modified polypropylene is used as a raw material for preparing a modified polypropylene film, and the content of the modified polypropylene in the modified polypropylene film is controlled within a specific range. The prepared modified polypropylene film has a higher surface tension, a higher dielectric constant and a higher tensile strength.

[0186] The performance test results of the composite current collectors provided by the above application examples and comparative application examples are shown in Table 3 below:

[0187] Table 3

[0188] It can be seen from the contents of the above table that in this application, a modified polypropylene film with excellent performance was prepared by designing the raw materials for preparing the modified polypropylene film. The bonding force between the polymer film (modified polypropylene film) and the metal layer is relatively large, which is 0.9 to 2.7 N / cm. There are no holes on the prepared composite current collector, and the square resistance of the composite current collector is relatively small, which is 17 to 18 mΩ.

[0189] Compared with Application Example 1, if the content of modified polypropylene in the raw materials for preparing the modified polypropylene film is too low (Application Example 4), the performance improvement of the prepared composite current collector is limited compared with the composite current collector (Comparative Application Example 1), and its adhesion is smaller, the number of pores is larger, and the square resistance is larger.

[0190] Compared with Application Example 1, if the grafting rate of the modifier in the modified polypropylene is lower (Application Example 9), the prepared composite current collector has a smaller bonding force, a larger number of pores, and a larger square resistance.

[0191] Compared with Application Example 1, the composite current collector prepared with polypropylene film (Comparative Example 1) has weaker adhesion, more pores, and larger square resistance; if polypropylene modified with other modifiers is used to prepare polypropylene film, the performance of the composite current collector (Comparative Example 2) obtained is also poor.

[0192] In summary, in this application, by designing the raw materials for preparing modified polypropylene film, a modified polypropylene film with excellent performance was prepared, and then a composite current collector with strong adhesion between the modified polypropylene film and the metal layer, no holes and small square resistance was prepared.

[0193] The applicant declares that while the above-mentioned embodiments are used to illustrate the detailed process flow of the present application, the present application is not limited to the above-mentioned detailed process flow, which does not mean that the present application must rely on the above-mentioned detailed process flow in order to be implemented. Those skilled in the art should understand that any improvements to the present application, equivalent replacements for the raw materials of the present application's products, addition of auxiliary ingredients, and selection of specific methods, etc., fall within the scope of protection and disclosure of the present application.

Claims

1. A modified polypropylene film, wherein the raw material for preparing the modified polypropylene film comprises modified polypropylene; The modifier for modifying the polypropylene includes terpene alcohol.

2. The modified polypropylene film according to claim 1, wherein The grafting rate of terpene alcohol in the modified polypropylene is ≥0.05%.

3. The modified polypropylene film according to claim 1 or 2, wherein The terpene alcohol includes any one of 4-terpene alcohol, α-terpineol, carveol, lavandulol, nerol, and geraniol, or a combination of at least two of them.

4. The modified polypropylene film according to any one of claims 1 to 3, wherein The melt index of the polypropylene in the modified polypropylene is 3.0-4.0 g / 10 min.

5. The modified polypropylene film according to any one of claims 1 to 4, wherein: The molecular weight distribution of the polypropylene in the modified polypropylene is 4.5-5.

5.

6. The modified polypropylene film according to any one of claims 1 to 5, wherein: The isotacticity of the polypropylene in the modified polypropylene is ≥95%.

7. The modified polypropylene film according to any one of claims 1 to 6, wherein: Taking the mass percentage of the raw materials for preparing the modified polypropylene film as 100%, the mass percentage of the modified polypropylene is ≥0.5%.

8. A method for preparing the modified polypropylene film according to any one of claims 1 to 7, the method comprising the following steps: (1) melting, filtering and extruding the raw materials for preparing the modified polypropylene film to obtain a molten material; (2) Casting the molten material obtained in step (1) onto a casting roll, cooling and forming the molten material, and then biaxially stretching the molten material to obtain the modified polypropylene film.

9. A composite current collector, comprising a metal layer and a polymer layer; The polymer film layer is a modified polypropylene film as described in any one of claims 1 to 7. 10 . A battery comprising the composite current collector according to claim 9 .

Citation Information

Patent Citations

  • Highly filled plastic packaging bag

    CN107814999A

  • Modified polypropylene material with cockroach preventing feature, as well as preparation method and application thereof

    CN108659353A

  • Preparation method of modified polymer film, modified polymer film and application thereof

    CN115312786A

  • Polypropylene film, preparation method thereof, composite current collector and application

    CN115850863A

  • Modified composite current collector and preparation method and application thereof

    CN115911404A