Efficient preparation method for high-temperature-resistant wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material

Quartz fiber reinforcement is solved by coating the low-dielectric nanoparticles/micrometer high-temperature resistant polymer sizing layer on the surface of quartz fibers and dispersing nanoparticles in the thermoplastic resin to form a micro-nano multi-scale interface layer, and synergistically modifying fibers and resins. The problem of poor heat resistance and interface bonding performance of thermoplastic composite materials has significantly improved the mechanical and wave transmittance properties of the materials.

WO2024244128A1PCT designated stage expired Publication Date: 2024-12-05ZHONGBEI UNIV

Patent Information

Application Number
PCT/CN2023/107164
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-07-13
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The existing quartz fiber-reinforced thermoplastic composite materials have low heat resistance, poor interfacial bonding performance between fiber and resin, resulting in a decrease in mechanical properties. The traditional sizing agent is easy to decompose at high temperatures, destroying the interface of the composite material.

Method used

The sizing coating is formed on the surface of the quartz fiber using low dielectric nanoparticles/micrometer high temperature resistant polymer, and the low dielectric high temperature resistant nanoparticles are dispersed into the thermoplastic resin matrix, and a micro-nano multi-scale interface layer is formed by mechanical blending. Coordinate the modification of fibers and resins to improve the comprehensive performance of composite materials.

Benefits of technology

It significantly improves the mechanical, wave-transmissive and high-temperature resistance of quartz fiber-reinforced thermoplastic composites, solves the problem of decomposition of traditional sizing agents at high temperatures, and realizes the interface modification and performance improvement of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2023107164-FTAPPB-I100001
    Figure PCTCN2023107164-FTAPPB-I100001
  • Figure PCTCN2023107164-FTAPPB-I100002
    Figure PCTCN2023107164-FTAPPB-I100002
Patent Text Reader

Abstract

An efficient preparation method for a high-temperature-resistant wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material, comprising the following specific steps: first, uniformly dispersing low-dielectric nanoparticles and a micron high-temperature-resistant sizing polymer to obtain a sizing agent, and then carrying out ultrasonic immersion on quartz fiber cloth in the sizing agent, so that the surface of quartz fibers is coated with a composite sizing layer formed by the low-dielectric nanoparticles and the micron high-temperature-resistant polymer; dispersing the low-dielectric high-temperature-resistant nanoparticles into a high-temperature-resistant thermoplastic resin matrix by using a mechanical blending method; and finally compounding the modified quartz fibers and a thermoplastic resin to prepare the composite material. By synergistically modifying the quartz fiber cloth and the resin, a micro-nano multi-scale interface layer is formed on the interface of the composite material, thereby remarkably improving the comprehensive properties of the composite material such as mechanical properties, dielectric properties, and thermal properties; moreover, the preparation method is simple and efficient, involves low costs, and is free of environmental pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Efficient preparation method of high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composites Technical Field

[0001] The present invention relates to the technical field of composite materials, and in particular to a method for efficiently preparing a high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material. Background Art

[0002] Wave-transmitting materials are multifunctional dielectric materials that combine structural, heat-resistant, and wave-transmitting properties. They are widely used in the manufacture of antenna systems such as radomes for spacecraft, rockets, satellites, and missiles. Aircraft often operate in extremely harsh environments such as high temperatures and high fields. Radomes must ensure that other systems, such as communications, detonation, guidance, and telemetry, can function properly without interference from external factors. Therefore, considering the operating environment of radomes, wave-transmitting materials must possess not only low dielectric constant and low dielectric loss properties, but also excellent high-temperature resistance, mechanical properties, and processing properties.

[0003] Wave-transmitting materials are typically made by combining low-dielectric fibers with high-performance resins, and are a typical type of fiber-reinforced resin-based composite material. Currently, quartz fiber-reinforced resin-based composites (QFRP) offer corrosion resistance, fatigue resistance, high strength, high modulus, excellent dielectric properties, and a simple molding process. They can be made into ideal broadband wave-transmitting materials and are widely used in the aerospace field. Quartz fiber-reinforced resin-based composites are categorized by the polymer matrix resin into: quartz fiber-reinforced thermosetting resin-based composites (QFRTS) and quartz fiber-reinforced thermoplastic resin-based composites (QFRTP).

[0004] Traditional thermosetting resin matrices offer advantages such as high heat resistance, corrosion resistance, and resistance to deformation under pressure. However, they still suffer from disadvantages such as low mechanical properties, poor toughness, inability to reshape, and non-recyclability, which significantly limit their widespread application. Compared to thermosetting resins, thermoplastic resins offer advantages such as high mechanical properties, good toughness, fatigue resistance, strong plasticity, easy processing and molding, reusability, and environmental friendliness. They have attracted widespread attention in aerospace, defense, automotive, and construction industries.

[0005] Therefore, the use of high-performance thermoplastic resin as a matrix to prepare quartz fiber reinforced thermoplastic resin-based composite materials can not only maintain its original excellent performance, but also have excellent dielectric properties, and can remain stable over a wide temperature and frequency range, which is an important way to develop new thermoplastic wave-transparent composite materials. However, with the continuous application of quartz fiber reinforced thermoplastic resin-based composite materials, the products produced have also exposed some shortcomings. For example, the heat resistance of the material is relatively low, the poor interface bonding performance between the fiber and the resin causes a serious decline in its mechanical properties, etc., so it is necessary to modify the composite material, and synergistic modification is one of the simple and efficient methods to obtain high-performance composite materials, that is, through the synergistic effect between the fiber surface modification and the resin matrix modification, the comprehensive performance of the composite material is further improved.

[0006] Among existing fiber modification methods, fiber sizing is the most efficient and lowest-cost modification method and is widely used in composite material systems. Fiber sizing involves applying a layer of resin coating to the fiber surface. This coating protects the fiber surface from contamination by impurities such as dust in the air; it also improves the bundling of the carbon fibers and prevents the generation of lint and broken fibers during use from affecting the performance of the fiber itself. The sizing layer is generally made of a polymer with a similar structure to the resin matrix, which can improve the interfacial compatibility between the fiber and the resin. Traditional commercial fiber sizing layers (epoxy resin, phenolic resin, etc.) are mainly suitable for composite material systems with thermosetting resins as the matrix. Furthermore, this type of sizing agent has poor heat resistance and cannot withstand the higher thermoforming temperatures of high-performance thermoplastic resin matrix composite material systems (such as polyetheretherketone, polyimide, polyphenylene sulfide, and polyethersulfone, which have thermoforming temperatures above 300°C). It is also prone to decomposition during processing, causing serious damage to the composite material interface. Therefore, it is of great significance to develop a new high-temperature resistant sizing agent that uses thermoplastic resin as the main agent and meets high processing and molding temperatures.

[0007] Furthermore, introducing nanoparticles into the sizing agent can increase the roughness of the fiber surface and enhance the mechanical engagement between the fiber and the resin matrix. Patent CN201710565223.6 discloses a high-temperature-resistant carbon fiber sizing agent containing graphene oxide and its preparation method. This improves the heat resistance and single-filament breaking strength of the carbon fiber, as well as the overall performance of the composite material. However, the conductive filler graphene oxide introduced into this sizing agent makes it unsuitable for use in wave-transmitting composite materials.

[0008] Resin matrix modification is usually carried out by adding nanoparticles to the resin matrix. Nanoparticles have a small size effect, volume effect, surface effect, quantum size effect and macroscopic quantum tunneling effect, which enable them to form a very large interface in the matrix resin at a low content. They can form a special network structure in the matrix resin, which can effectively transmit stress when deformed by force, and prevent cracks from expanding internally through bridging and crack deflection mechanisms, thereby further improving the comprehensive performance of the composite material. Patent CN201811335147.0 discloses a method for preparing a carbon nanotube-modified resin carbon fiber composite shell. The bending properties of the modified resin composite shell are improved by 15% compared to the unmodified resin, the tensile properties are improved by 23% compared to the unmodified resin, and the impact absorption energy is also improved by 150% compared to the unmodified resin. However, the above-mentioned modified method uses strong acids such as concentrated sulfuric acid and concentrated nitric acid, which will cause environmental pollution and equipment damage.

[0009] Summary of the Invention

[0010] The present invention overcomes the shortcomings of the existing technology and provides an efficient preparation method for high-temperature resistant and wave-transparent micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material. It fully gives full play to the synergistic reinforcement effect of fiber surface modification and resin modification on quartz fiber reinforced thermoplastic composite material, and can improve the comprehensive performance of quartz fiber reinforced thermoplastic composite material such as mechanics, wave transmission, and high temperature resistance. It is of great significance for expanding the application of wave-transparent composite materials in antenna cover related fields.

[0011] The present invention uses a sizing method to successfully coat the surface of quartz fiber with a sizing coating formed by low-dielectric nanoparticles / micron high-temperature resistant polymers. At the same time, a mechanical blending method is used to disperse the low-dielectric high-temperature resistant nanoparticles into a high-temperature resistant thermoplastic resin matrix. By jointly modifying both the fiber and the resin, a micro-nano multi-scale interface layer is formed at the interface of the composite material, thereby achieving a significant improvement in the comprehensive performance of the composite material.

[0012] To solve the above technical problems, the technical solution adopted by the present invention is: an efficient preparation method of a high-temperature resistant and wave-transparent micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material, comprising the following steps:

[0013] (1) mixing low dielectric nanoparticles, a high temperature resistant sizing polymer, and a solvent, mechanically stirring, and then ultrasonically treating for 0.5 to 4 hours to obtain a uniformly dispersed sizing agent;

[0014] (2) soaking the unsized quartz fiber cloth in a sizing tank containing the sizing agent of step (1), and performing low-power ultrasound with an ultrasonic power of 30 to 80 W for a soaking time of 0.5 to 2 hours, and finally taking out the fiber and placing it in a blast drying oven to dry it, thereby obtaining a sizing-modified quartz fiber cloth;

[0015] (3) using a high-speed mixer to uniformly mix the low-dielectric high-temperature resistant nano powder and the high-temperature resistant thermoplastic resin powder to obtain a mixed powder;

[0016] (4) Using the mixed powder obtained in step (3) as a resin matrix and the sizing-modified quartz fiber cloth obtained in step (2) as a reinforcement, hot pressing is performed to prepare a high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material.

[0017] Preferably, the mass ratio of the low dielectric nanoparticles, the high temperature resistant sizing polymer and the solvent in step (1) is 0.1-3:0.1-3:94-99.8; the mechanical stirring time in step (1) is 1-3h, and the stirring speed is 300-1000r / min.

[0018] Furthermore, the low dielectric nanoparticles described in step (1) are one of SiO2, BN and POSS.

[0019] Furthermore, the high temperature resistant sizing polymer described in step (1) is at least one of polyimide, polyamic acid and polyetherimide.

[0020] Furthermore, the solvent in step (1) is at least one of water, dimethylmethanolamine, dimethylethanolamine, diethanolamine, triethanolamine, N-methylpyrrolidone and tetrahydrofuran.

[0021] Preferably, the drying temperature of the blast drying oven in step (2) is 80-300° C., and the drying time is 6-12 hours.

[0022] Preferably, the rotation speed of the high-speed mixer in step (3) is 100-2000 r / min, and the mass ratio of the low-dielectric high-temperature resistant nano powder to the high-temperature resistant thermoplastic resin powder is 1-10:90-99.

[0023] Preferably, it is characterized in that the low dielectric high temperature resistant nano powder described in step (3) is at least one of Si3N4, AlN, SiC and ZrO2.

[0024] Preferably, the high temperature resistant thermoplastic resin in step (3) is one of polyetheretherketone, polyimide, polyphenylene sulfide and polyethersulfone.

[0025] Preferably, in step (4), the mass ratio of the matrix to the reinforcement is 1:1-2.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The sizing agent provided by the present invention has the advantages of a wide range of raw material sources, a simple preparation process, and less fiber damage, and has great development prospects.

[0028] (2) The sizing agent provided by the present invention has excellent heat resistance and can meet the higher processing temperature requirements of high-performance thermoplastic composite materials, effectively solving the problem of traditional sizing agents decomposing during the thermoforming process and causing damage to the composite material interface.

[0029] (3) The present invention adopts a mechanical blending method to disperse low-dielectric and high-temperature resistant nanoparticles into a high-temperature resistant thermoplastic resin matrix, which has the characteristics of being simple, efficient, low-cost, and environmentally friendly.

[0030] (4) The present invention adopts a sizing method to coat a low-dielectric nanoparticle / micron high-temperature resistant polymer sizing layer on the surface of the quartz fiber, and simultaneously adopts a mechanical blending method to disperse the low-dielectric high-temperature resistant nanoparticles into the high-temperature resistant thermoplastic resin matrix. By synergistically modifying both the fiber and the resin, the interface modification of the composite material and the micro-nano multi-scale enhancement effect of the composite material are achieved. DETAILED DESCRIPTION

[0031] The present invention will be further described below with reference to specific embodiments.

[0032] Example 1

[0033] A high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced polyetheretherketone composite material comprises the following steps:

[0034] (1) Weigh 1 g of nano-SiO2 and 1 g of polyamic acid (PAA) particles and add them to a beaker containing 8 g of dimethylethanolamine and 90 g of deionized water, stirring them mechanically at a speed of 600 r / min for 2 h; then ultrasonically treat them for 0.5 h at an ultrasonic power of 100 W to obtain a uniformly dispersed PAA-SiO2 composite sizing agent;

[0035] (2) Immerse the unsized quartz fiber cloth in a sizing tank containing a PAA-SiO2 composite sizing agent and perform low-power ultrasound at 50W for 0.5h. Finally, take out the fiber and dry it in a 120°C forced air drying oven for 12h to obtain a sizing-modified quartz fiber cloth.

[0036] (3) Weigh 5 g of nano-SiC powder and 95 g of polyetheretherketone (PEEK) resin powder, stir them at a speed of 1000 r / min for 1 h using a high-speed mixer to obtain a uniformly mixed SiC-PEEK powder;

[0037] (4) First, 40 g of the SiC-PEEK powder obtained in step (3) was weighed as a resin matrix, and 60 g of the sizing-modified quartz fiber cloth obtained in step (2) was weighed as a reinforcement. The SiC-PEEK powder was evenly spread on each layer of sizing-modified fiber to obtain a prepreg. The prepreg was placed in a mold and hot-pressed at 390°C, 10 MPa, and 1.5 h to prepare a high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced polyetheretherketone composite material.

[0038] Comparative Example 1

[0039] First, 40g of PEEK powder was weighed as the resin matrix, and 60g of quartz fiber cloth was weighed as the reinforcement. The PEEK powder was evenly spread on each layer of fiber to form a prepreg. The prepreg was placed in a mold and hot-pressed at 390°C, 10MPa, for 1.5 hours to obtain a quartz fiber cloth-reinforced polyetheretherketone composite.

[0040] Example 2

[0041] (1) Weigh 1 g of nano-BN and 1 g of (PAA) particles and add them to a beaker containing 98 g of N-methylpyrrolidone, stir them mechanically at a speed of 800 r / min for 2 h, and then ultrasonicate them for 1 h at an ultrasonic power of 120 W to obtain a uniformly dispersed PAA-BN composite sizing agent.

[0042] (2) Immerse the unsized quartz fiber cloth in a sizing tank containing a PAA-BN composite sizing agent and perform low-power ultrasound at 30W for 0.5 h. Finally, take out the fiber and dry it in a 180°C forced air drying oven for 8 h to obtain a sizing-modified quartz fiber cloth.

[0043] (3) Weigh 7 g of nano-Si3N4 powder and 93 g of thermoplastic polyimide (TPI) resin powder, stir them at a speed of 900 r / min for 0.5 h using a high-speed mixer to obtain a uniformly mixed Si3N4-TPI powder;

[0044] (4) First, 35 g of the Si3N4-TPI powder obtained in step (3) was weighed as a resin matrix, and 65 g of the sizing-modified quartz fiber cloth obtained in step (2) was weighed as a reinforcement. The Si3N4-TPI powder was evenly spread on each layer of sizing-modified fiber to obtain a prepreg. The prepreg was placed in a mold and hot-pressed at 290°C for 0.5 h, micro-pressure; and 340°C for 2 h, 15 MPa to prepare a high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced polyimide composite material.

[0045] Comparative Example 2

[0046] First, 35g of TPI powder was weighed as the resin matrix, and 65g of quartz fiber cloth was weighed as the reinforcement. The TPI powder was evenly applied to each layer of fiber to form a prepreg. The prepreg was placed in a mold and hot-pressed at 290°C for 0.5h under light pressure, and then at 340°C for 2h under 15MPa to produce a quartz fiber cloth-reinforced polyimide composite.

[0047] Example 3

[0048] (1) Weigh 1 g of nano-POSS and 1 g of polyetherimide (PEI) particles and add them to a beaker containing 98 g of tetrahydrofuran and mechanically stir them at a stirring speed of 700 r / min for 1.5 h; then ultrasonicate them for 1 h at an ultrasonic power of 90 W to obtain a uniformly dispersed PEI-POSS composite sizing agent;

[0049] (2) Immersing the unsized quartz fiber cloth in a sizing tank containing a PEI-POSS composite sizing agent and subjecting it to low-power ultrasound at 40 W for 1 h, finally taking the fiber out and drying it in a 60° C. forced air drying oven for 10 h to obtain a sizing-modified quartz fiber cloth;

[0050] (3) Weigh 9 g of nano-AlN powder and 91 g of polyethersulfone (PES) resin powder, stir them at 600 r / min using a high-speed mixer for 1 h to obtain a uniformly mixed AlN-PES powder;

[0051] (4) First, 30 g of the AlN-PES powder obtained in step (3) was weighed as a resin matrix, and 70 g of the sizing-modified quartz fiber cloth obtained in step (2) was weighed as a reinforcement. The AlN-PES powder was evenly spread on each layer of sizing-modified fiber to obtain a prepreg. The prepreg was placed in a mold and hot-pressed at 280°C, 1 MPa, for 0.5 h; and 310°C, 5 MPa, for 1.5 h to prepare a high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced polyethersulfone composite material.

[0052] Comparative Example 3

[0053] First, 30g of PES powder was weighed as the resin matrix, and 70g of quartz fiber cloth was weighed as the reinforcement. The PES powder was evenly spread on each layer of fiber to form a prepreg. The prepreg was placed in a mold and hot-pressed at 280°C, 1MPa for 0.5h, and 310°C, 5MPa for 1.5h to obtain a quartz fiber cloth-reinforced polyethersulfone composite.

[0054] Example 4

[0055] (1) Weigh 1.5 g of nano-SiO2 and 1.5 g of polyimide (PI) particles and add them to a beaker containing 97 g of dimethylcarbinolamine. Stir mechanically at a speed of 800 r / min for 3 h. Ultrasonic treatment is then performed for 1 h at an ultrasonic power of 150 W to obtain a uniformly dispersed PI-SiO2 composite sizing agent.

[0056] (2) Immerse the unsized quartz fiber cloth in a sizing tank containing a PI-SiO2 composite sizing agent and perform low-power ultrasound at 30W for 0.5h. Finally, take out the fiber and dry it in a 120°C forced air drying oven for 9h to obtain a sizing-modified quartz fiber cloth.

[0057] (3) Weigh 6 g of nano-Si3N4 powder and 94 g of polyphenylene sulfide (PPS) resin powder, stir them at a speed of 1000 r / min for 0.5 h using a high-speed mixer to obtain a uniformly mixed Si3N4-PPS powder;

[0058] (4) First, 45 g of the Si3N4-PPS powder obtained in step (3) was weighed as a resin matrix, and 55 g of the sizing-modified quartz fiber cloth obtained in step (2) was weighed as a reinforcement. The Si3N4-PPS powder was evenly spread on each layer of sizing-modified fiber to obtain a prepreg. The prepreg was placed in a mold and hot-pressed at 330°C, 15 MPa, and 1 h to prepare a high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced polyphenylene sulfide composite material.

[0059] Comparative Example 4

[0060] First, 45g of PPS powder was weighed as the resin matrix, and 55g of quartz fiber cloth was weighed as the reinforcement. The PPS powder was evenly spread on each layer of fiber to form a prepreg. The prepreg was placed in a mold and hot-pressed at 330°C, 15MPa, for 1 hour to obtain a quartz fiber cloth-reinforced polyphenylene sulfide composite.

[0061] Table 1 Comparison of properties of composite materials obtained in Examples and Comparative Examples

[0062] The above are merely embodiments of the present invention and do not limit the scope of protection of the present invention. Without departing from the technical concept of the present invention, it is apparent to those skilled in the art that various modifications and variations may be made to the embodiments of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.

Claims

1. An efficient preparation method of a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material, characterized in that: The following steps are involved: (1) mixing low dielectric nanoparticles, a high temperature resistant sizing polymer and a solvent, mechanically stirring, and then ultrasonically treating for 0.5 to 4 hours to obtain a uniformly dispersed sizing agent; (2) soaking the unsized quartz fiber cloth in a sizing tank containing the sizing agent of step (1), and performing low-power ultrasound, the ultrasound power is 30 to 80 W, the soaking time is 0.5 to 2 hours, and finally taking out the fiber and placing it in a blast drying oven to dry it, so as to obtain a sizing-modified quartz fiber cloth; (3) using a high-speed mixer to uniformly mix the low-dielectric high-temperature-resistant nano powder and the high-temperature-resistant thermoplastic resin powder to obtain a mixed powder; (4) Using the mixed powder obtained in step (3) as a resin matrix and the sizing-modified quartz fiber cloth obtained in step (2) as a reinforcement, hot pressing is performed to prepare a high-temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material.

2. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: The mass ratio of the low dielectric nanoparticles, the high temperature resistant sizing polymer and the solvent in step (1) is 0.1-3:0.1-3:94-99.8; the mechanical stirring time in step (1) is 1-3h, and the stirring speed is 300-1000r / min.

3. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: The low dielectric nanoparticles described in step (1) are one of SiO2, BN and POSS.

4. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: The high temperature resistant sizing polymer described in step (1) is at least one of polyimide, polyamic acid and polyetherimide.

5. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: The solvent described in step (1) is at least one of water, dimethylmethanolamine, dimethylethanolamine, diethanolamine, triethanolamine, N-methylpyrrolidone and tetrahydrofuran.

6. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: In step (2), the drying temperature of the blast drying oven is 80 to 300° C., and the drying time is 6 to 12 hours.

7. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: In step (3), the rotation speed of the high-speed mixer is 100-2000 r / min, and the mass ratio of the low-dielectric high-temperature resistant nano powder to the high-temperature resistant thermoplastic resin powder is 1-10:90-99.

8. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: The low dielectric and high temperature resistant nano powder described in step (3) is at least one of Si3N4, AlN, SiC and ZrO2.

9. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: The high temperature resistant thermoplastic resin described in step (3) is one of polyetheretherketone, polyimide, polyphenylene sulfide and polyethersulfone.

10. The method for efficiently preparing a high temperature resistant and wave-transmitting micro-nano multi-scale quartz fiber cloth reinforced thermoplastic composite material according to claim 1, characterized in that: In step (4), the mass ratio of the matrix to the reinforcement is 1:1-2.

Citation Information

Patent Citations

  • Antioxidant polyimide prepreg and preparation method thereof

    CN111154260A

  • Preparation method and system of high-toughness thermosetting resin-based prepreg

    CN114133606A

  • Low-dielectric high-toughness polyimide composite material and preparation method thereof

    CN115466509A

  • High interface bonding sizing agent, preparation thereof, modified carbon fiber reinforced polyether-ether-ketone composite material based on high interface bonding sizing agent and preparation method of modified carbon fiber reinforced polyether-ether-ketone composite material

    CN115748244A

  • prepreg

    US20120148753A1

Cited By

  • Composite ceramic stealth material based on super-structure surface sub-wavelength structure and preparation method of composite ceramic stealth material