Aluminum oxide film structure for heat dissipation and cooling of high-voltage bare conductor and preparation method
By generating a porous alumina film structure on high-voltage wires, the problem of increasing conductor temperature is solved, and better heat dissipation and cooling effect and low resistance characteristics are achieved, which is suitable for industrial production.
Patent Information
- Application Number
- PCT/CN2023/139469
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2023-12-18
- Publication Date
- 2024-12-05
AI Technical Summary
When high-voltage wires operate at high power, heat accumulation inside the conductor leads to an increase in temperature, affecting the performance and safety of the wire. Existing heat dissipation technologies such as passive heat dissipation and active heat dissipation coatings are not effective, and the cost and process are complex.
The porous alumina film with a single or double-layer composite pore structure is generated on the outermost layer of aluminum conductors or aluminum stranded wires. It is prepared by anodizing technology. The film thickness is 15-30μm and the pore range is 100-300nm. It is used to improve the conductors. heat dissipation and cooling performance.
It realizes low current temperature rise and faster heat dissipation and cooling characteristics under high voltage bare wires, and does not increase the resistance of the wires. It has a simple process and is suitable for large-scale industrial production, and is cost-controllable.
Smart Images

Figure CN2023139469_05122024_PF_FP_ABST
Abstract
Description
Aluminum oxide film structure and preparation method for heat dissipation and cooling of high-voltage bare wires Technical Field
[0001] The present invention belongs to the technical field of electric wires and cables, and in particular relates to an aluminum oxide film structure for heat dissipation and temperature reduction of high-voltage bare wires and a preparation method thereof. Background Art
[0002] High-voltage power lines generally refer to transmission lines carrying voltages of 10kV and above. Currently, aluminum-clad steel stranded wire is commonly used as the conductor, with the steel core primarily providing strength and the aluminum stranded wire primarily transmitting power. High-voltage power lines are typically transmitted underground using insulated cables in urban areas, while overhead lines supported by towers are typically used in outdoor areas. Generally speaking, 10kV high-voltage distribution lines within urban areas mostly use insulated conductors, while high-voltage transmission lines of 35kV and above use bare conductors.
[0003] With the rapid development of the economy and society, the demand for electricity is further increasing, posing new challenges to the power grid's transmission capacity. Currently, conductor capacity expansion technology is considered a potential and effective solution to addressing insufficient transmission capacity. There are two main approaches to conductor capacity expansion: static expansion and dynamic expansion. Static expansion measures primarily include ultra-high voltage transmission technology, dynamic reactive power compensation, flexible AC transmission technology, compact transmission technology, large-section heat-resistant conductors, and increasing the conductor's permissible operating temperature. Raising the conductor's permissible operating temperature to 80°C or even 90°C can increase the conductor's transmission capacity by 20% or 35%, respectively, and is simple to implement. However, this measure requires consideration of the associated issues of accessory capacity, line lifespan, and other impacts of the increased temperature on conductor accessories and other equipment. Compared to increasing the conductor's permissible operating temperature, the other measures require new lines, resulting in significant capital investment, strict environmental requirements, and increased maintenance complexity.
[0004] However, when high-voltage power lines operate at high power levels for extended periods, heat buildup within the conductors can cause the ambient temperature to rise. Especially during extremely hot summers, when demand for industrial and residential electricity surges, the primary approach used to increase the capacity of transmission lines is to raise the permissible operating temperature of the conductors. However, this approach inevitably increases the internal temperature of the conductors. Furthermore, summer temperatures are already high, and the rise in internal transmission line temperature and the rising ambient temperature mutually reinforce each other, significantly impacting the performance and safety of the lines. Furthermore, when the temperature of a transmission line reaches a certain level, it will sag. The degree of sag is directly proportional to the temperature, and placing sagged conductors too close to buildings can cause secondary safety incidents. Furthermore, higher conductor temperature increases the resistance and, consequently, the losses in the line.
[0005] To address the heat dissipation problem of wires, passive and active heat dissipation are currently the most common methods. Passive heat dissipation relies on external conditions such as air and wind to dissipate heat through convection. This method primarily relies on the external environment, is greatly affected by the environment, and has unstable results, resulting in poor heat dissipation. Active heat dissipation, currently a common method, involves coating the surface of the conductor with a heat-dissipating coating. This coating layer relies on the combined effects of thermal conductivity and auxiliary heat to rapidly dissipate heat, achieving the purpose of heat dissipation and cooling. However, heat-dissipating coatings primarily reflect heat from solar radiation and cannot, by themselves, reduce the heat generated within the conductor. Furthermore, coatings can have problems such as low thermal conductivity and increased electrical resistance. Some heat-resistant conductors can improve the heat resistance of steel-core aluminum stranded wire by adding elements such as zirconium to the aluminum. However, adding alloying elements to aluminum is a complex process and expensive.
[0006] In summary, there is an urgent need to propose an economical, simple and technologically simple technical solution for heat dissipation and cooling of high-voltage bare wires.
[0007] Summary of the Invention
[0008] In view of this, the purpose of the present invention is to provide an aluminum oxide film structure and preparation method for heat dissipation and cooling of high-voltage bare wires. The specific technical solution is as follows.
[0009] An aluminum oxide membrane structure for heat dissipation and cooling of high-voltage bare wires. The aluminum oxide membrane structure is an aluminum oxide membrane layer with a single pore or a double-layer composite pore structure generated on the outermost surface of an aluminum conductor or aluminum stranded wire. The thickness of the porous aluminum oxide membrane layer is 15-30 μm, and the pore range of the single pore or double-layer composite pore is 100-300 nm, and the pore size range is 30-300 nm (this can achieve the effect of convective heat transfer).
[0010] Preferably, the pore size of the single pore or double-layer composite pore is in the range of 100 to 200 nm.
[0011] The double-layer composite pore structure described in the present invention is a pore structure with upper and lower layers, the pores in the upper layer have a larger pore diameter and the pores in the lower layer have a smaller pore diameter, and the number of pores arranged in the upper layer is less than that in the lower layer.
[0012] Furthermore, the high-voltage bare wire is a pure aluminum conductor or an aluminum stranded wire twisted with an aluminum-clad steel core, and the outermost layer is an aluminum monofilament; the radius of the high-voltage bare wire includes 3mm, 7mm, 10mm, 15mm or 20mm.
[0013] The present invention also provides an aluminum stranded wire having low temperature rise characteristics and active heat dissipation and temperature reduction characteristics, which is made of pure aluminum conductors or aluminum-clad steel cores with the above-mentioned porous aluminum oxide film structure on the outermost layer.
[0014] The method for preparing the porous alumina membrane structure is to immerse a pure aluminum wire or an aluminum strand in an electrolyte for anodization to generate a porous alumina membrane structure with a thickness of 15-30 μm, and specifically comprises the following steps:
[0015] Step 1: Connect the pure aluminum wire or aluminum stranded wire to be treated to the anode output line of the device. Before oxidation, turn on the circulating cooling of the device to circulate the electrolyte in the cooler and electrolytic cell to ensure that the electrolyte temperature is maintained at about 25°C during the anodizing process.
[0016] Step 2: Adding an acid solution to tap water to prepare an electrolyte and adding the electrolyte to the electrolytic cell. The electrolyte includes sulfuric acid, phosphoric acid, oxalic acid, a sulfuric acid / chromic acid mixture, a sulfuric acid / oxalic acid / chromic acid mixture, or a nitric acid / chromic acid mixture;
[0017] Step 3: Turn on the power and apply 0.04A / cm 2 ~0.3A / cm 2 The current density is 200 nm and the oxidation time is 8 min to 25 min.
[0018] The electrolyte used in the present invention can be a single strong acid such as sulfuric acid or nitric acid, or a mixed acid such as a sulfuric acid / chromic acid mixture, a sulfuric acid / oxalic acid / chromic acid mixture, or a nitric acid / chromic acid mixture. When a strong acid is used as the electrolyte for anodic oxidation, the hydrogen ions in the strong acid can be completely ionized to participate in the oxidation reaction, but this can lead to an overly rapid reaction and poor process control. However, the hydrogen ions in chromic acid and oxalic acid are not completely dissociated, so after mixing and neutralizing with a strong acid, a stable reaction effect can be achieved.
[0019] Furthermore, during the entire anodic oxidation process, the current density is controlled by adjusting the voltage, and the voltage range is 50V to 100V.
[0020] Further, the current density includes 0.04A / cm 2 , 0.13A / cm 2 , 0.27A / cm 2 or 0.3A / cm 2 .
[0021] Furthermore, the oxidation time includes 8 min, 10 min, 20 min or 25 min.
[0022] Furthermore, the concentration range of chloride ions in the tap water is controlled to be 0-15 mg / L.
[0023] Furthermore, the voltage range is 70V-90V.
[0024] A porous alumina membrane structure is used in heat dissipation and cooling of high-voltage bare wires. The porous alumina membrane structure has a thickness of 15-30 μm, and the porous structure is a single pore or a double-layer composite pore structure. The pore range of the single pore or double-layer composite pore is 100-300 nm, and the pore diameter range is 30-300 nm. The porous alumina membrane structure can be used for heat dissipation and cooling after the conductor is expanded.
[0025] Beneficial technical effects
[0026] 1) This invention provides a porous alumina membrane structure for heat dissipation and cooling of high-voltage bare wires. This porous alumina membrane is formed on the outermost surface of an aluminum conductor or stranded aluminum wire. Compared to bare wire, this porous alumina membrane structure enables the aluminum conductor or stranded aluminum wire to exhibit lower current temperature rise and better and faster heat dissipation and cooling at the same current.
[0027] 2) The porous aluminum oxide film structure with a specific thickness provided by the present invention, which is generated on the outermost surface of the aluminum conductor or aluminum stranded wire, will not affect the conductive ability of the conductor and will not increase the resistance, breaking the conventional cognition of those skilled in the art. At present, those skilled in the art generally believe that there is a skin effect in the conductor. That is, when there is alternating current or an alternating electromagnetic field in the conductor, the current distribution inside the conductor is uneven, and the current is concentrated in the "skin" part of the conductor, that is, the current is concentrated in the thin layer on the surface of the conductor. The closer to the surface of the conductor, the greater the current density, and the current inside the conductor is actually smaller. The result is that the resistance of the conductor increases and the power loss also increases. This phenomenon is called the skin effect. Alumina is an insulator with a resistance of 10 14 -10 16 ohm·cm, which is generally believed to increase resistance. However, the present invention has experimentally demonstrated that the formation of a porous alumina film structure with the specific thickness and structural characteristics provided by the present invention on the surface of an aluminum conductor does not increase resistance. However, an increase in resistance was indeed observed on aluminum conductors with thicknesses outside the specified range of the present invention.
[0028] 3) The resistance of the wire having the porous alumina membrane structure of the present invention is slightly lower than that of the bare wire.
[0029] 4) The preparation process of the porous alumina membrane structure of the present invention is simple and suitable for industrial large-scale production. In particular, tap water is used to prepare the electrolyte, and the cost is controllable. This is because the cost of preparing the electrolyte with tap water is much lower than that with distilled water, and the source of tap water is wider, so the preparation method of the present invention is suitable for industrial large-scale preparation and application. However, substances in tap water will form corrosion pits on the surface of aluminum wires / aluminum strands. Therefore, the present invention further confirms that it is the chloride ions in tap water that form corrosion pits on the surface of aluminum wires / aluminum strands, so by controlling the chloride ion concentration, the corrosion of the wires is reduced to an acceptable range, breaking through the technical barriers. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be derived from these drawings without inventive effort.
[0031] FIG1 is a schematic diagram of an aluminum wire anodizing device;
[0032] Figure 2 is a schematic diagram of the aluminum conductor current temperature rise test platform;
[0033] Figure 3 is a graph showing the heating effect of porous alumina membrane structures with different thicknesses;
[0034] FIG4 is a diagram showing the cooling effect of aluminum conductors with porous alumina film structures of different thicknesses;
[0035] FIG5 is a diagram showing the heat dissipation effect of porous alumina membrane structures with different pores under conventional current;
[0036] Figure 6 is a microscopic SEM image of each pore;
[0037] FIG7 is a diagram showing the heat dissipation effect of the conductor under high current;
[0038] FIG8 is a diagram showing the heating effect of wires with different hole structures;
[0039] Figure 9 shows the temperature rise effect of wires with different radii under current (a: control and experimental groups with radii of 3 mm and 7 mm, b: experimental groups with different radii);
[0040] Figure 10 shows the SEM microscopic images of pores at different current densities;
[0041] Figure 11 shows the corrosion effects of different chloride ion concentrations on the surface of aluminum wire (a: macroscopic image of chloride ion concentration of 5 mg / L, b: macroscopic image of chloride ion concentration of 15 mg / L, c: macroscopic image of chloride ion concentration of 20 mg / L, d: microscopic image of chloride ion concentration of 20 mg / L; e: macroscopic image of distilled water without chloride ions; f: macroscopic and microscopic images of distilled water without chloride ions);
[0042] FIG12 is a diagram showing the heat dissipation effect of anodized aluminum wires using electrolytes prepared with distilled water and electrolytes prepared with tap water;
[0043] FIG13 is a SEM image of the aluminum oxide film thickness at different oxidation times. DETAILED DESCRIPTION
[0044] To make the purpose, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making any creative efforts shall fall within the scope of protection of the present invention.
[0045] It should be noted that, in this document, the terms "comprises," "includes," or any other variations thereof are intended to encompass non-exclusive inclusion, such that a process, method, article, or apparatus comprising a series of elements includes not only those elements but also other elements not explicitly listed, or elements inherent to such process, method, article, or apparatus. In the absence of further limitations, an element defined by the phrase "comprising a ..." does not exclude the presence of other identical elements in the process, method, article, or apparatus comprising the element.
[0046] As used in this specification, the term "about" typically means + / - 5% of the stated value, more typically + / - 4% of the stated value, more typically + / - 3% of the stated value, more typically + / - 2% of the stated value, even more typically + / - 1% of the stated value, and even more typically + / - 0.5% of the stated value.
[0047] In this specification, some embodiments may be disclosed in a format of being within a certain range. It should be understood that such description of "being within a certain range" is only for convenience and brevity and should not be interpreted as a rigid limitation on the disclosed range. Therefore, the description of a range should be considered to have specifically disclosed all possible sub-ranges and independent numerical values within this range. For example, the range The description of should be considered to have specifically disclosed subranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numbers within this range, for example, 1, 2, 3, 4, 5, and 6. The above rules apply regardless of the breadth of the range.
[0048] Glossary
[0049] The "pores" mentioned in the present invention refer to the distance between pores.
[0050] The "pore size" described in the present invention refers to the size of the pore.
[0051] The "single pore" described in the present invention is a single-layer arrangement of nanoscale micropores, which can also be referred to as a single pore for short.
[0052] The "double-layer composite pores" described in the present invention are nanoscale micropores arranged in two layers, upper and lower, and can also be referred to as composite pores for short.
[0053] It can be understood that the alumina membrane structure in the following specific embodiments is an abbreviation of the porous alumina membrane structure described in the present invention.
[0054] Example 1
[0055] This embodiment provides a preparation process and process for anodizing aluminum wire
[0056] Samples: The test aluminum conductors are pure aluminum wire (1060, GB / T3190-1996); and JL / LB 120 / 20 aluminum-clad steel-core aluminum stranded wire.
[0057] Preparation apparatus: The apparatus consists of a DC power supply (100A / 200V), circulating cooling equipment, an electrolytic cell, and a cathode. The cell is 50cm wide and has holes at both ends. The aluminum wire to be treated is placed inside the cell and sealed with sealing rings at both ends. A schematic diagram of the aluminum wire anodizing apparatus is shown in Figure 1.
[0058] Classification of electrodes: Two 304 stainless steel cathode plates with a size of 50cm×20cm; and a ring cathode composed of 6 stainless steel plates, each with a size of 50cm×7cm, and an overall diameter of 20cm.
[0059] Specific steps: Connect the aluminum wire to be treated to the anode output line of the power supply. Before oxidation, enable circulating cooling to circulate the electrolyte through the cooler and electrolytic cell to ensure that the electrolyte temperature remains around 25°C during the anodizing process. Each oxidation treatment is performed on a 50cm length of wire. Samples of corresponding lengths can be prepared based on actual needs.
[0060] Different electrolytes: including sulfuric acid, phosphoric acid, oxalic acid, sulfuric acid / chromic acid mixture, sulfuric acid / oxalic acid / chromic acid mixture or nitric acid / chromic acid mixture.
[0061] Aluminum single wires of different diameters: 3mm, 7mm, 10mm, 15mm, 20mm.
[0062] Different current density: 0.01A / cm 2 ~0.3A / cm 2 .
[0063] Different oxidation times: 5min~30min.
[0064] Different oxidation voltages: 70V~90V.
[0065] Ambient wind speed: 0-5m / s.
[0066] Example 2
[0067] Provide a method for adjusting current density by adjusting voltage
[0068] In the preliminary experimental stage of the present invention, the experimental material used was an aluminum plate. By adjusting the voltage, different current densities per unit area of the aluminum plate can be obtained. When the anodized material is an aluminum wire, the required voltage is calculated based on a constant current density and the effective area of the aluminum wire. In this way, the desired current density can be adjusted by adjusting the voltage during the preparation method.
[0069] Example 3
[0070] This embodiment provides the electrical performance test of the aluminum wire prepared in Example 1.
[0071] 1) Conductivity
[0072] Referring to the method in the literature, the standard four-point lead method was used to test the DC resistance of the aluminum conductor, and the test environment temperature was 20°C. Since the anodizing treatment mainly generates an insulating aluminum oxide film on the surface of the outermost aluminum monofilament or the surface of the aluminum wire, the outermost aluminum monofilament of the aluminum conductor was selected as the test sample. The two lead wires of the current source and the voltmeter are clamped at both ends of the wire to be tested with a special clamp, with two voltage leads on the inside and two current leads on the outside. Before the test, the diameter d (unit: mm) of the aluminum monofilament and the length L (unit: m) between the two voltage leads are measured, and the resistivity is calculated by the following formula: p = UπD 2 / 4LI.
[0073] I is the current (A) passing through the conductor, provided by a Keithley 2400 current source with a maximum current of 1A. U is the voltage, acquired by a Keithley 2010 Multimeter. During the test, the current was increased by 100mA each time, and the voltage corresponding to each current was recorded. The test was stopped when it reached 1A. The slope of the IU line is the resistance of the test section sample. Each sample was tested three times and the average value was used as the final result. The conductivity of the conductor is calculated using the following formula: %IACS=(0.172 / p)×100%
[0074] 2) Current temperature rise test
[0075] Figure 2 shows a schematic diagram of the aluminum conductor current temperature rise test platform. It primarily consists of a test control cabinet, a current booster, a temperature recorder, a temperature sensor, and test conductors. The test aluminum conductors are either pure aluminum or steel-coated aluminum stranded wire, and the test conductor length is 3 meters. A temperature sensor is fixed to the center of the conductor, and a thermocouple is connected to the temperature sensor to monitor changes in the conductor surface temperature as the current changes. The conductor ends are connected to the current booster outlet, and the current flowing through the conductor is regulated using the control cabinet. After each current increase, the conductor temperature is recorded after stabilization, and the next temperature increase is repeated to obtain curves showing how the conductor temperature changes with current at different locations.
[0076] Example 4
[0077] Discussion of various factors and experimental verification
[0078] 1. Influence of aluminum oxide film thickness on heat dissipation and cooling
[0079] The aluminum oxide film structure provided by the present invention has a thickness of 15 to 30 μm. If the thickness is less than 15 μm, the heat dissipation effect is poor; if the thickness is greater than 30 μm, the heat dissipation effect is poor and the resistance increases, as shown in Figures 3 and 4.
[0080] The aluminum oxide film structures provided in this example have thicknesses of 5μm, 15μm, 23μm, 30μm, and 48μm, with bare wire used as a control. Heat dissipation experiments and the resistance test results in Table 1 show that both too thin and too thick aluminum oxide films have poor heat dissipation. Calculations show that both too thin and too thick films result in higher AC resistance, increasing load losses. Therefore, a film thickness between 15 and 30μm is recommended for optimal heat dissipation and loss reduction.
[0081] Table 1 Resistance data of aluminum oxide films with different thicknesses
[0082] 2. Heat dissipation experiment of different pores under conventional current
[0083] FIG5 shows the heat dissipation results of composite double-layer porous alumina membranes with different pores under conventional current (A).
[0084] Using a bare wire as a control, when the pore size is 30nm, the wire temperature gradually rises with increasing current, reaching a temperature higher than the bare wire. When the pore size is 100nm, the wire temperature rises slightly higher than the bare wire. However, when the pore size is 200nm or 300nm, the wire temperature rises lower than the bare wire. Microscopic images of each pore are shown in Figure 6.
[0085] Under normal current conditions, the aluminum oxide film structure provided by the present invention does not provide a significant heat dissipation and cooling effect. This is because the heat generated within the conductor itself is not very high under normal current conditions, so the cooling effect is not very effective. However, under high current conditions, the aluminum oxide film structure provided by the present invention can achieve a significant heat dissipation and cooling effect.
[0086] 3. Heat dissipation experiment of wires under high current
[0087] Table 2 shows the currents of various aluminum conductors at 70°C. 70°C is the temperature limit for pure aluminum conductors for power transmission as stipulated by national standards. Exceeding this temperature can cause the conductors to sag, leading to safety accidents.
[0088] Table 2
[0089] Figure 7 shows the results of a high-current heat dissipation experiment. In this example, the aluminum oxide film on the aluminum wire has a thickness of 30 μm and a pore size of approximately 200 nm (there is a slight error in the measurement of single pores and composite double-layer pores). These results demonstrate that the aluminum oxide film structure provided by the present invention is suitable for increasing the capacitance of conductors.
[0090] 4. Wire temperature rise results with different hole structures
[0091] Figure 8 shows the temperature rise results for wires with different pore structures. Using a bare wire as a blank control, the aluminum oxide film on the aluminum wire in the experimental group had a thickness of 30 μm and a pore size of approximately 200 nm (there was a slight error in the measurement of single pores and composite double-layer pores). This shows that both the single-pore and composite pore structures of the aluminum oxide film provided by the present invention can reduce the temperature rise of the wire as the current increases.
[0092] 5. Temperature rise results of aluminum wires with different radii under current
[0093] Figure 9a shows the temperature rise results for 3mm, 3mm*, 3mm, and 7mm* conductors under current. * represents aluminum conductors with the aluminum oxide film structure of the present invention, while the conductors without * represent pure aluminum conductors, serving as a control. It can be seen that the aluminum conductors with the aluminum oxide film structure of the present invention have significantly lower temperature rise characteristics. Figure 9b shows the results for conductors with different radii having the aluminum oxide film structure. It can be seen that as the current increases, the conductors with radii of 15mm and 20mm have lower temperature rise characteristics.
[0094] 6. Pore data generated at different oxidation current densities
[0095] Table 3
[0096] Figure 10 shows SEM micrographs of pores at different current densities. Therefore, it can be understood that pores of different sizes can be generated by adjusting and controlling different oxidation densities.
[0097] 7. Effect of chloride ion concentration on the surface of aluminum wire
[0098] The preparation method of the present invention is based on the perspective of industrial large-scale production and application. Tap water is used to prepare the electrolyte for anodization. In early experimental exploration, the team of the present invention found that the Cl ions in tap water can cause some corrosion to the surface of aluminum wire.
[0099] Experiments in this example revealed that: 1) when the Cl ion concentration was low (5 mg / L), no obvious corrosion defects were observed (see Figure 11a). 2) when the Cl ion concentration was moderate (15 mg / L), smaller corrosion pits appeared (see Figure 11b). 3) when the Cl ion concentration was too high (20 mg / L), larger corrosion pits were observed (see Figures 11c and 11d). 4) In comparison, no defects were observed in an electrolyte prepared with distilled water (without Cl ions) (see Figures 11e and 11f).
[0100] Figure 12 shows the heat dissipation experiments of aluminum wire anodized with electrolytes prepared with distilled water and tap water. The results show that the heat dissipation effects of the two are almost the same.
[0101] 8. Effect of different oxidation times on the thickness of aluminum oxide film
[0102] Sulfuric acid was used as the electrolyte and the current density was 0.13A / cm 2 The preparation results are shown in Table 4. It is understood that the electrolyte of the present invention can also be phosphoric acid, oxalic acid, sulfuric acid / chromic acid mixture, sulfuric acid / oxalic acid / chromic acid mixture or nitric acid / chromic acid mixture.
[0103] Table 4
[0104] Figure 13 shows SEM images of aluminum oxide film thickness at different oxidation times. Therefore, it can be understood that adjusting the oxidation time can produce aluminum oxide films of different thicknesses.
[0105] This example found that when the oxidation time was 8 minutes, the thickness of the aluminum oxide film was close to 15 μm, while when the oxidation time exceeded 25 minutes, the thickness of the aluminum oxide film exceeded 30 μm. In Part 1 of this example, the effects of aluminum oxide films of different thicknesses were verified, and the optimal heat dissipation thickness was 15 to 30 μm. Therefore, the anodization time should be controlled within 8 to 25 minutes.
[0106] 9. Comparison of resistivity between the aluminum oxide film structure of the present invention and pure aluminum bare wire
[0107] The experiment, based on GB / T 1179-2017, "Round Wire Concentric Stranded Overhead Conductors," tested the DC resistivity of bare and anodized JL / LB20A-240 / 30 aluminum conductors, as shown in Table 5. Treated conductors 1 and 2 have different cross-sectional areas. In this example, the aluminum oxide film on the aluminum wire had a thickness of 30 μm and a pore size of 200 nm.
[0108] Table 5
[0109] The experiment in this embodiment shows that forming the aluminum oxide film structure of the present invention on the surface of the aluminum wire not only does not increase the resistance, but instead slightly reduces the resistance compared to the bare wire, breaking the conventional cognition of researchers.
[0110] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are protected by the present invention.
Claims
1. An aluminum oxide film structure for heat dissipation and cooling of high-voltage bare wires, characterized in that: The alumina membrane structure is an alumina membrane layer with a single hole or a double-layer composite hole structure generated on the outermost surface of an aluminum conductor or an aluminum stranded wire. The thickness of the porous alumina membrane layer is 15-30 μm; the pore range of the single hole or the double-layer composite hole is 100 to 300 nm, and the pore size range is 30 to 300 nm.
2. The aluminum oxide film structure according to claim 1, characterized in that: The high-voltage bare wire is a pure aluminum conductor or an aluminum stranded wire twisted with an aluminum-clad steel core, and the outermost layer is an aluminum monofilament; the radius of the high-voltage bare wire includes 3mm, 7mm, 10mm, 15mm or 20mm.
3. The method for preparing the aluminum oxide film structure according to claim 1 or 2, characterized in that: The method comprises immersing a pure aluminum conductor or an aluminum stranded wire in an electrolyte for anodization to generate a porous aluminum oxide membrane structure with a thickness of 15-30 μm, and specifically comprising the following steps: Step 1: Connect the pure aluminum wire or aluminum stranded wire to be treated to the anode output line of the device. Before oxidation, turn on the circulating cooling of the device to circulate the electrolyte in the cooler and the electrolytic cell to ensure that the electrolyte is maintained at a temperature of 25°C during the anodizing process; Step 2: Adding tap water and an acid solution to prepare an electrolyte and adding the electrolyte into the electrolytic cell, wherein the electrolyte includes sulfuric acid, phosphoric acid, oxalic acid, a sulfuric acid / chromic acid mixture, a sulfuric acid / oxalic acid / chromic acid mixture or a nitric acid / chromic acid mixture; Step 3: Turn on the power and apply 0.04A / cm 2 ~0.3A / cm 2 The current density is 200 nm and the oxidation time is 8 min to 25 min.
4. The preparation method according to claim 3, characterized in that: During the entire anodizing process, the current density is controlled by adjusting the voltage, and the voltage range is 50V to 100V.
5. The preparation method according to claim 3, characterized in that: The current density includes 0.04A / cm 2 , 0.13A / cm 2 , 0.27A / cm 2 or 0.3A / cm 2 .
6. The preparation method according to claim 3, characterized in that: The oxidation time includes 8 min, 10 min, 20 min or 25 min.
7. The method according to claim 3, characterized in that The concentration range of chloride ions in the tap water is controlled to be 0-15 mg / L.
8. The preparation method according to claim 4, characterized in that: The voltage range is 70V-90V.
9. Application of a porous aluminum oxide film structure in heat dissipation and cooling of high-voltage bare wires, characterized in that: The thickness of the porous alumina membrane structure is 15-30 μm, the porous structure is a single hole or a double-layer composite hole structure, the pore range of the single hole or the double-layer composite hole is 100-300 nm, and the pore size range is 30-300 nm; the porous alumina membrane structure can be used for heat dissipation and cooling after the capacity of the wire is increased.
Citation Information
Patent Citations
Method and device for preparing ordered porous alumina template
CN101624717A
Method for improving cooling effect of pure aluminum cooling fin
CN103981557A
High-reliability aluminum-based copper-clad plate and preparation method thereof
CN112277406A
Alumina film structure for heat dissipation and cooling of high-voltage bare wire and preparation method thereof
CN116646118A
Fast stable growth process of alumina film with nanometer pore array in relatively great pore distance
CN1974873A