High-crystallinity and high-transparency rare-earth-doped fluorine-oxygen microcrystalline glass and preparation method therefor

By adjusting the components of oxyfluoroglass and optimizing the heat treatment process, KYF4 nanocrystalline precipitation is achieved, reducing the refractive index difference and phonon radiation-free relaxation rate, solving the optical loss problem of traditional oxyfluoroglass and improving high crystallinity and transparency The performance of rare earth doped oxygen fluoride glass is suitable for high-performance fiber lasers.

WO2024244429A1PCT designated stage expired Publication Date: 2024-12-05SOUTH CHINA UNIV OF TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/141130
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-30
Filing Date
2023-12-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

During the light penetration process of traditional oxyfluoroglass glass, due to the light scattering phenomenon caused by the interface conditions and refractive index differences between nanocrystals and substrate glass, limits its application in high-performance fiber lasers, resulting in serious optical loss and is difficult to achieve. High crystallinity and transparency.

Method used

By adjusting the components of oxyfluorofluoro glass and optimizing the heat treatment process, KYF4 nanocrystals are precipitated in the glass, reducing the refractive index difference between the glass matrix and the KYF4 crystal, improving the crystallinity and optical transmittance of the microcrystalline glass, and passing through Er3+ Ions enter the KYF4 nanolattice, reducing the phonon radiation-free relaxation rate and improving luminous efficiency.

Benefits of technology

The contradiction between crystallinity and transmittance in microcrystalline glass was overcome, the chemical stability and luminous performance of microcrystalline glass were improved, and the optical transmittance and luminous intensity were significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023141130_05122024_PF_FP_ABST
    Figure CN2023141130_05122024_PF_FP_ABST
Patent Text Reader

Abstract

High-crystallinity and high-transparency rare-earth-doped fluorine-oxygen microcrystalline glass and a preparation method therefor. The molar percentage composition of the microcrystalline glass comprises: B2O3: 29-54 mol%, SiO2: 10-20 mol%, ZnO: 5-15 mol%, K2O: 15-20 mol%, YF3: 5-25 mol%, and RF3: 1-5 mol% (R is a rare earth element). The preparation method therefor comprises: preparing precursor glass, and then subjecting the precursor glass to crystallization treatment by means of a heat treatment process to obtain the rare-earth-doped fluorine-oxygen microcrystalline glass. The prepared microcrystalline glass has good light transmission in the range from near-infrared light to visible light, thereby significantly enhancing the light-emitting of rare earth ions. The prepared rare-earth-doped fluorine-oxygen microcrystalline glass containing KYF4 nanocrystalline alleviates the contradiction between transmittance and crystallinity, and achieves high crystallinity and high transmittance at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency and preparation method thereof Technical Field

[0001] The present invention belongs to the technical field of luminescent materials, and in particular relates to rare earth-doped fluorine-oxygen microcrystalline glass with high crystallinity and transparency and a preparation method thereof. Background Art

[0002] High-performance lasers have attracted widespread attention for their wide applications in biomedicine, spectroscopy, nanomaterial science, remote sensing and other fields. In order to achieve high-efficiency and compact laser output, researchers have made great efforts in creating new gain media (such as rare earth ion-doped glass and single crystal materials) in recent decades. However, due to the weak crystal field of glass and the complex crystal preparation process, neither is the optimal gain medium for fiber lasers. Therefore, the development of a new generation of gain materials for advanced lasers is urgent. Fortunately, microcrystalline glass combines the excellent glass fiber forming properties of the glass matrix and the superior optical properties of nanocrystals, which can overcome these limitations and has attracted considerable attention in high-performance and compact fiber laser applications.

[0003] Traditional oxyfluoride glass-ceramics are multiphase optical gain materials composed of a homogeneous glass phase and a well-dispersed fluoride crystal phase. They combine the advantages of crystals (high field strength and size controllability) and glass (ease of fabrication, high optical transparency, and chemical durability). However, when light penetrates the glass-ceramics, the interface between the nanocrystals and the matrix glass, as well as differences in refractive index, causes light scattering. Rayleigh scattering, a primary type of scattering, arises from random microinhomogeneities that are small compared to the wavelength of the radiation. These inhomogeneities manifest as fluctuations in refractive index and composition, imposing strict limits on the size of the crystalline phase. This optical loss severely limits the development of oxyfluoride glass-ceramics as high-performance gain materials. Therefore, resolving the conflict between crystallinity and transmittance in glass-ceramics would be highly beneficial for the application of high-crystallinity, high-transmittance glass-ceramics in high-performance fiber lasers.

[0004] Summary of the Invention

[0005] The present invention provides a rare earth doped oxyfluoride glass-ceramics with high crystallinity and transparency and a preparation method thereof to solve the above technical problems. The glass-ceramics prepared by the present invention not only has high crystallinity, luminescence and chemical stability, but also has high optical transmittance.

[0006] The object of the present invention is to provide the rare earth-doped fluorine-oxygen glass-ceramics with improved crystallinity and transparency and a preparation method thereof.

[0007] In order to achieve the above object, the technical solution of the present invention is:

[0008] Rare earth-doped fluoride oxyglass-ceramics with high crystallinity and transparency, whose components are expressed in the form of molar percentage: B2O3: 29-54 mol%, SiO2: 10-20 mol%, ZnO: 5-15 mol%, K2O: 15-20 mol%, YF3: 5-25 mol%, RF3: 1-5 mol%, where R is a rare earth element.

[0009] Preferably, the rare earth element is one or more of Ce, Pr, Nd, Pr, Sm, Er, Tb, Dy, Ho, Tm, and Yb.

[0010] The method for preparing the rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency comprises the following steps:

[0011] (1) Heating the glass raw materials to 900-1100°C and keeping the temperature for 0.5-2 hours to obtain molten glass;

[0012] (2) pouring the molten glass obtained in step (1) into a preheated mold, keeping it at 300-400°C for 2-8 hours, and then cooling it to below 50°C to obtain a precursor glass;

[0013] (3) The precursor glass obtained in step (3) is heated to 450-600° C. and kept at this temperature for 1-5 hours to obtain rare earth-doped fluorine-oxygen microcrystalline glass with high crystallinity and transparency.

[0014] Preferably, in step (1), the glass raw material needs to be ground before heating, and the grinding time is 20-40 minutes.

[0015] Preferably, in step (1), the glass raw materials are selected from B2O3, SiO2, ZnO, K2CO3, YF3 and RF3, wherein R is a rare earth element, and the rare earth element includes one or more of Ce, Pr, Nd, Pr, Sm, Er, Tb, Dy, Ho, Tm, and Yb.

[0016] Preferably, in step (1), the heating to 900-1100°C is specifically: heating to 900-1100°C at a rate of 2-10°C / min.

[0017] Preferably, in step (2), the mold needs to be preheated to 25-300°C.

[0018] Preferably, in step (2), the cooling to below 50°C is specifically: cooling to below 50°C at a rate of 5-20°C / h.

[0019] Preferably, in step (3), the heating to 450-600°C is specifically: heating from room temperature to 450-600°C at a rate of 2-10°C / min.

[0020] Preferably, the heat preservation in step (2) and the heat preservation in step (3) are both carried out in a muffle furnace.

[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0022] The present invention realizes the precipitation of KYF4 nanocrystals in oxyfluoride glass by adjusting the components of oxyfluoride glass and optimizing the heat treatment process. 3+ The entry of light from the glass matrix into the KYF4 crystal causes the refractive index of the glass matrix to decrease, thereby reducing the refractive index difference between the glass matrix and the KYF4 crystal. Ultimately, as the heat treatment temperature increases, the optical transmittance is increased while the crystallinity of the microcrystalline glass is increased, overcoming the contradiction between crystallinity and transmittance in the microcrystalline glass.

[0023] Rare earth ion Er 3+ With Y 3+ The ionic radius is similar and the valence state is the same, Er 3+ Partial replacement of Y 3+ Compared with borosilicate glass (phonon energy 1400 cm -1 ), KYF4 has a lower phonon energy (down to 360 cm -1 ), which reduces the multi-phonon non-radiative relaxation rate of rare earth ions, thereby significantly improving the luminescence efficiency of rare earth ions in microcrystalline glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] FIG1 is an XRD (X-ray diffraction) diagram of rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 1 and the precursor glass in the preparation process of Example 1.

[0025] FIG2 is a graph showing the UV-visible-near-infrared transmission spectra of the rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 1 and the precursor glass in the preparation process of Example 1.

[0026] FIG3 is a fluorescence spectrum diagram of rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 1 and the precursor glass in the preparation process of Example 1.

[0027] FIG4 is an XRD (X-ray diffraction) diagram of rare earth-doped fluorine oxy-glass-ceramics prepared at different heat treatment temperatures in Example 2 and the precursor glass in the preparation process of Example 2.

[0028] FIG5 is a graph showing the UV-visible-near-infrared transmission spectra of the rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 2 and the precursor glass in the preparation process of Example 2.

[0029] FIG6 is a fluorescence spectrum of rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 2 and the precursor glass in the preparation process of Example 2.

[0030] FIG7 is an XRD graph of rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 3 and the precursor glass in the preparation process of Example 3.

[0031] FIG8 is a graph showing the UV-visible-near-infrared transmission spectra of the rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 3 and the precursor glass in the preparation process of Example 3.

[0032] FIG9 is a fluorescence spectrum of rare earth-doped fluorine-oxygen glass-ceramics prepared at different heat treatment temperatures in Example 3 and the precursor glass in the preparation process of Example 3.

[0033] DETAILED DESCRIPTION

[0034] In order to better understand the present invention, the present invention is further described below with reference to the embodiments, but the scope of protection claimed in the present invention is not limited thereto.

[0035] Example 1

[0036] The glass composition (S1) of this embodiment is: B2O3: 44 mol%, SiO2: 20 mol%, ZnO: 5 mol%, K2O: 20 mol%, YF3: 10 mol%, ErF3: 1 mol%. The raw materials are analytically pure B2O3, SiO2, ZnO, K2CO3 and spectrally pure YF3 and ErF3. 20 g of the raw material was weighed according to the above molar percentage and ground in a mortar for 20 minutes. It was then transferred to a dense corundum crucible and heated to 900 °C at a rate of 5 °C / min and melted for 0.5 hours. The resulting glass melt was then poured onto an iron mold that was not preheated (e.g., room temperature 25 °C) and quickly formed. The mold was annealed at 400 °C for 2 hours and cooled to 50 °C at a rate of 5 °C / h to obtain a transparent precursor glass. The precursor glass was then placed in a muffle furnace and heat-treated at 470, 510, and 550 °C from room temperature at a rate of 5 °C / min for 5 hours to obtain rare earth-doped fluorine-oxygen glass-ceramics with different degrees of transparency.

[0037] Figure 1 shows the X-ray diffraction patterns of rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency obtained in Example 1 and the precursor glass in the preparation process of Example 1. The crystal phase of the control PDF card is KYF4, and it can be seen that the X-ray diffraction peak is enhanced with the increase of heat treatment temperature, indicating an increase in the crystallinity of the microcrystalline glass.

[0038] Figure 2 shows the UV-visible-near-infrared transmittance spectra of the rare earth-doped fluorine oxyglass microcrystalline with different degrees of transparency obtained in Example 1 and the precursor glass in the preparation process of Example 1. It can be seen that as the heat treatment temperature increases, the transmittance of the microcrystalline glass first decreases and then increases. The microcrystalline glass heat-treated at 550 °C for 5 h has a higher transmittance than the microcrystalline glass sample heat-treated at 510 °C for 5 h.

[0039] Figure 3 shows the emission spectra of the rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency obtained in Example 1 and the precursor glass prepared in the process of Example 1. It can be seen from the emission spectrum that with the increase of heat treatment temperature, the luminescence intensity of the microcrystalline glass increases significantly, and its luminescence intensity is enhanced by orders of magnitude compared with the precursor glass.

[0040] Example 2

[0041] The glass composition (S1) of this embodiment is: B2O3: 39 mol%, SiO2: 20 mol%, ZnO: 5 mol%, K2O: 20 mol%, YF3: 15 mol%, ErF3: 1 mol%. The raw materials are analytically pure B2O3, SiO2, ZnO, K2CO3 and spectrally pure YF3 and ErF3. 20 g of the raw material was weighed according to the above molar percentage and ground in a mortar for 20 minutes. It was then transferred to a dense corundum crucible and melted at 900 °C at a heating rate of 5 °C / min for 0.5 hour. The resulting glass melt was then poured onto an iron mold that was not preheated (e.g., room temperature 25 °C) to quickly form it. It was annealed at 400 °C for 2 hours and cooled to 50 °C at a rate of 5 °C / h to obtain a transparent precursor glass. The precursor glass was then placed in a muffle furnace and heat-treated at 470, 510, and 550 °C from room temperature at a rate of 5 °C / min for 5 hours to obtain rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency.

[0042] Figure 4 shows the X-ray diffraction patterns of the rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency obtained in Example 2 and the precursor glass in the preparation process of Example 2. The crystal phase of the control PDF card is KYF4, and it can be seen that the X-ray diffraction peak is enhanced with the increase of heat treatment temperature, indicating an increase in the degree of crystallization of the microcrystalline glass.

[0043] Figure 5 is the ultraviolet-visible-near-infrared transmittance spectra of the rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency obtained in Example 2 and the precursor glass in the preparation process of Example 2. It can be seen that as the heat treatment temperature increases, the transmittance of the microcrystalline glass first decreases and then increases. The transmittance of the microcrystalline glass obtained by treating at 510°C for 5h is greater than that of the microcrystalline glass obtained by treating at 470°C for 5h.

[0044] Figure 6 shows the emission spectra of the rare earth-doped fluorine-oxygen glass-ceramics with different degrees of transparency obtained in Example 2 and the precursor glass prepared in the process of Example 2. It can be seen from the emission spectra that with the increase of the heat treatment temperature, the luminescence intensity of the glass-ceramics increases significantly, and its luminescence intensity is enhanced by orders of magnitude compared with the precursor glass.

[0045] Example 3

[0046] The glass composition (S1) of this embodiment is: B2O3: 34 mol%, SiO2: 20 mol%, ZnO: 5 mol%, K2O: 20 mol%, YF3: 20 mol%, ErF3: 1 mol%. The raw materials are analytically pure B2O3, SiO2, ZnO, K2CO3 and spectrally pure YF3 and ErF3. 20 g of the raw material was weighed according to the above molar percentage and ground in a mortar for 30 minutes. It was then transferred to a dense corundum crucible and melted at 1000 °C at a heating rate of 5 °C / min for 1 hour. The resulting glass melt was then poured onto an iron mold that was not preheated (such as room temperature 25 °C) and quickly pressed into shape. It was annealed at 400 °C for 4 hours and cooled to 50 °C at a rate of 10 °C / h to obtain a transparent precursor glass. The precursor glass was then placed in a muffle furnace and heat-treated at 470, 510 and 550 °C from room temperature at a rate of 5 °C / min for 5 hours to obtain rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency.

[0047] Figure 7 shows the X-ray diffraction patterns of the rare earth-doped fluorine oxyglass-ceramics with different degrees of transparency obtained in Example 3 and the precursor glass in the preparation process of Example 3. The crystal phase of the control PDF card is KYF4. It can be observed that the glass has undergone crystallization without any treatment, and the KYF4 crystal phase is detected by XRD, indicating that the component has self-crystallization phenomenon, and it can be seen that the X-ray diffraction peak is enhanced with the increase of heat treatment temperature, indicating that the degree of crystallization of the glass-ceramics increases.

[0048] Figure 8 shows the ultraviolet-visible-near-infrared transmittance spectra of the rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency obtained in Example 3 and the precursor glass in the preparation process of Example 3. It can be seen that as the heat treatment temperature increases, the transmittance of the microcrystalline glass sample increases.

[0049] Figure 9 shows the emission spectra of the rare earth-doped fluorine-oxygen glass-ceramics with different degrees of transparency obtained in Example 3 and the precursor glass prepared in the process of Example 3. From the emission spectra, we can see that with the increase of heat treatment temperature, the luminescence intensity of the glass-ceramics increases significantly, and its luminescence intensity is enhanced by orders of magnitude compared with the precursor glass.

[0050] Example 4

[0051] The glass composition (S1) of this embodiment is: B2O3: 29 mol%, SiO2: 20 mol%, ZnO: 5 mol%, K2O: 18 mol%, YF3: 25 mol%, ErF3: 3 mol%. The raw materials are analytically pure B2O3, SiO2, ZnO, K2CO3 and spectrally pure YF3 and ErF3. 20 g of the raw material was weighed according to the above molar percentage and ground in a mortar for 30 minutes. It was then transferred to a dense corundum crucible and melted at 1000 °C at a heating rate of 2 °C / min for 1 hour. The resulting glass melt was then poured onto an iron mold preheated to 150 °C and quickly pressed into shape. It was annealed at 350 °C for 4 hours and cooled to 50 °C at a rate of 10 °C / h to obtain a completely devitrified precursor glass. The precursor glass was then placed in a muffle furnace and heat-treated at 2 °C / min from room temperature to 450 °C, 500 °C, 550 °C and 600 °C for 1 hour to obtain rare earth-doped fluorine-oxygen micro-ceramics with different degrees of transparency.

[0052] Example 5

[0053] The glass composition (S1) of this embodiment is: B2O3: 54 mol%, SiO2: 15 mol%, ZnO: 8 mol%, K2O: 14 mol%, YF3: 5 mol%, ErF3: 4 mol%. The raw materials are analytically pure B2O3, SiO2, ZnO, K2CO3 and spectrally pure YF3 and ErF3. 20 g of the raw material was weighed according to the above molar percentage and ground in a mortar for 40 minutes. It was then transferred to a dense corundum crucible and melted at 1100 °C at a heating rate of 2 °C / min for 2 hours. The resulting glass melt was then poured onto an iron mold preheated to 150 °C and quickly pressed into shape. It was annealed at 300 °C for 8 hours and cooled to 50 °C at a rate of 20 °C / h to obtain a transparent precursor glass. The precursor glass was then placed in a muffle furnace and heated from room temperature to 450 °C, 500 °C, 550 °C and 600 °C at a rate of 2 °C / min for 3 hours to obtain rare earth-doped fluorine-oxygen microcrystalline glass with different degrees of transparency.

[0054] Example 6

[0055] The glass composition (S1) of this embodiment is: B2O3: 50 mol%, SiO2: 10 mol%, ZnO: 15 mol%, K2O: 15 mol%, YF3: 5 mol%, ErF3: 5 mol%. The raw materials are analytically pure B2O3, SiO2, ZnO, K2CO3 and spectrally pure YF3 and ErF3. 20 g of the raw material was weighed according to the above molar percentage and ground in a mortar for 40 minutes. It was then transferred to a dense corundum crucible and melted at 1100 °C at a heating rate of 10 °C / min for 2 hours. The resulting glass melt was then poured onto an iron mold preheated to 300 °C and quickly pressed into shape. It was annealed at 300 °C for 8 hours and cooled to 50 °C at a rate of 20 °C / h to obtain a transparent precursor glass. The precursor glass was then placed in a muffle furnace and heat-treated at 450 °C, 500 °C, 550 °C and 600 °C at a rate of 10 °C / min for 5 hours each to obtain rare earth-doped fluorine-oxygen glass-ceramics with different degrees of transparency.

[0056] Example 7

[0057] The glass composition (S1) of this embodiment is: B2O3: 44 mol%, SiO2: 20 mol%, ZnO: 5 mol%, K2O: 20 mol%, YF3: 10 mol%, PrF3: 1 mol%. The raw materials are analytically pure B2O3, SiO2, ZnO, K2CO3 and spectrally pure YF3 and PrF3. 20 g of the raw material was weighed according to the above molar percentage and ground in a mortar for 20 minutes. It was then transferred to a dense corundum crucible and melted at 900 °C at a heating rate of 10 °C / min for 0.5 hour. The resulting glass melt was then poured onto an iron mold preheated to 300 °C for rapid molding, annealed at 400 °C for 2 hours, and cooled to 50 °C at a rate of 5 °C / h to obtain a transparent precursor glass. The precursor glass was then placed in a muffle furnace and heat-treated at 470, 510, and 550 °C from room temperature at a rate of 10 °C / min for 5 hours to obtain rare earth-doped fluorine-oxygen glass-ceramics with different degrees of transparency.

[0058] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. Rare earth doped oxyfluoride glass-ceramics with high crystallinity and transparency, characterized in that: The rare earth doped fluorine oxygen microcrystalline glass components are expressed in the form of molar percentage: B2O3: 29-54 mol%, SiO2: 10-20 mol%, ZnO: 5-15 mol%, K2O: 15-20 mol%, YF3: 5-25 mol%, RF3: 1-5 mol%, wherein R is a rare earth element.

2. The rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency according to claim 1, characterized in that: The rare earth elements include one or more of Ce, Pr, Nd, Pr, Sm, Er, Tb, Dy, Ho, Tm, and Yb.

3. The method for preparing rare earth-doped fluorine-oxygen glass-ceramics with high crystallinity and transparency according to claim 1 or 2, characterized in that: The following steps are involved: (1) Heating the glass raw material to 900-1100°C and keeping the temperature for 0.5-2 hours to obtain a glass melt; (2) pouring the molten glass obtained in step (1) into a preheated mold, keeping it at 300-400° C. for 2-8 hours, and then cooling it to below 50° C. to obtain a precursor glass; (3) The precursor glass obtained in step (3) is heated to 450-600° C. and then kept at this temperature for 1-5 hours to obtain rare earth-doped fluorine-oxygen microcrystalline glass with high crystallinity and transparency.

4. The method for preparing rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency according to claim 3, characterized in that: In step (1), the glass raw material needs to be ground before heating, and the grinding time is 20-40 minutes.

5. The method for preparing rare earth-doped fluorine-oxygen glass-ceramics with high crystallinity and transparency according to claim 3, characterized in that: In step (1), the glass raw materials are selected from B2O3, SiO2, ZnO, K2CO3, YF3 and RF3, wherein R is a rare earth element, and the rare earth element includes one or more of Ce, Pr, Nd, Pr, Sm, Er, Tb, Dy, Ho, Tm, and Yb.

6. The method for preparing rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency according to claim 3, characterized in that: In step (1), the heating to 900-1100° C. is specifically: heating to 900-1100° C. at a rate of 2-10° C. / min.

7. The method for preparing rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency according to claim 3, characterized in that: In step (2), the mold needs to be preheated to 25-300°C.

8. The method for preparing rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency according to claim 3, characterized in that: In step (2), the cooling to below 50°C is specifically: cooling to below 50°C at a rate of 5-20°C / h.

9. The method for preparing rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency according to claim 3, characterized in that: In step (3), the temperature is raised to 450-600°C, specifically, from room temperature to 450-600°C at a rate of 2-10°C / min.

10. The method for preparing rare earth-doped oxyfluoride glass-ceramics with high crystallinity and transparency according to claim 3, characterized in that: The heat preservation in step (2) and the heat preservation in step (3) are both carried out in a muffle furnace.

Citation Information

Patent Citations

  • Rear earth doping oxygen-fluorine borosilicate microcrystalline glass and preparation method thereof

    CN101265029A

  • Fluorine-oxygen microcrystalline glass based on rare earth ion in-situ crystallization as well as preparation method and application of fluorine-oxygen microcrystalline glass

    CN112010564A

  • High-crystallinity intermediate infrared light-emitting nano glass ceramic material and preparation method thereof

    CN115010371A

  • Rare earth doped oxyfluoride glass ceramic with high crystallinity and transparency and preparation method of rare earth doped oxyfluoride glass ceramic

    CN116730621A

  • glass

    JP2008019103A