Silicon carbide wafer with uniformly distributed stress, and method for non-destructively and accurately measuring anisotropic stress of wafer

By combining XRD diffraction testing with in-plane and inter-plane rotation, the problem of non-destructive testing of anisotropic stress in silicon carbide wafers was solved, enabling accurate stress distribution analysis and making it suitable for industrial testing.

WO2024244459A1PCT designated stage expired Publication Date: 2024-12-05SICC SHANGHAI CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/143173
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2023-12-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve non-destructive and accurate detection of anisotropic stress in silicon carbide wafers, particularly in distinguishing and measuring anisotropic stress distributions without damaging the wafer.

Method used

By employing XRD diffraction testing combined with in-plane and inter-plane rotation, and calculating the diffraction peaks of different diffraction crystal planes, and combining this with elastic constants to calculate anisotropic stress, a non-destructive and accurate measurement method is provided.

Benefits of technology

It enables non-destructive and accurate detection of anisotropic stress in silicon carbide wafers, simplifies the detection process, improves detection accuracy and applicability, and is suitable for large-scale industrial testing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023143173_05122024_PF_FP_ABST
    Figure CN2023143173_05122024_PF_FP_ABST
Patent Text Reader

Abstract

A silicon carbide wafer with uniformly distributed stress, and a method for non-destructively and accurately measuring the anisotropic stress of a wafer, which wafer and method belong to the technical fields of silicon carbide wafers and stress measurements therefor. The measurement method comprises the following steps: (1) performing an XRD test on a wafer, performing intra-plane and inter-plane rotation on the wafer during the test, so as to obtain test results under at least six diffraction crystal planes, and comparing diffraction peaks of different diffraction crystal planes with standard peaks of corresponding diffraction crystal planes in a stress-free wafer, so as to obtain an anisotropic strain value of the wafer; and (2) calculating the anisotropic stress of the wafer according to the anisotropic strain value and an elastic constant. The method can realize non-destructive and accurate measurement of the anisotropic stress of the wafer, provides a new way to analyze the anisotropic stress of the wafer, and can be generalized to be used for standardized measurement of the anisotropic stress of the wafer.
Need to check novelty before this filing date? Find Prior Art

Description

A silicon carbide wafer with uniformly distributed stress and a method for non-destructively and accurately measuring the isotropic stress of the wafer Technical Field

[0001] The present application relates to a silicon carbide wafer with uniformly distributed stress and a method for non-destructively and accurately measuring the isotropic stress of the wafer, belonging to the technical field of silicon carbide wafers and stress detection thereof. Background Art

[0002] Several methods exist for measuring residual stress in silicon carbide, including neutron scattering, micro-Raman spectroscopy, optical interferometry, and XRD diffraction. Neutron scattering analysis of wafer stress requires the use of a small-angle neutron diffractometer. Currently, such diffractometers are relatively rare in the industry, primarily due to the high cost of the equipment, making industrial testing impractical. Raman spectroscopy can measure stress at different depths depending on the wavelength, but it is currently not possible to directly measure in-plane anisotropic stress using Raman spectroscopy. Optical interferometry has relatively poor accuracy and cannot resolve in-plane anisotropic stress.

[0003] XRD diffraction can obtain absolute stress parameters and is a relatively convenient testing method. However, characterizing the stress tensor of a single crystal using traditional XRD diffraction methods is difficult and inaccurate. Currently, anisotropic stress analysis can only be performed by cutting the wafer into small pieces. However, this method is destructive and cannot achieve non-destructive testing of the wafer. Summary of the Invention

[0004] To address the above-mentioned issues, a silicon carbide wafer with isotropic stress distribution and a method for non-destructively and accurately measuring the isotropic stress of the wafer are provided. The isotropic stress values ​​of the silicon carbide wafer can be calculated through XRD diffraction testing. The first normal stress, second normal stress, and third normal stress of the silicon carbide wafer are low and approximately the same, thereby obtaining a silicon carbide wafer with isotropic stress distribution, which can improve the quality and subsequent use value of the wafer.

[0005] This method for measuring the isotropic stress of a wafer rotates the wafer in-plane and between-planes during the test, calculates the isotropic strain value of the wafer based on the diffraction peaks of different diffraction crystal planes, and calculates the isotropic stress of the wafer based on the isotropic strain value and elastic constant. This method can achieve non-destructive and accurate detection of the isotropic stress of the wafer, provides a new idea for the analysis of the isotropic stress of the wafer, and can be promoted for standardized detection of the isotropic stress of the wafer.

[0006] According to one aspect of the present application, a silicon carbide wafer with isotropically distributed stress is provided, wherein the isotropic stress of the silicon carbide wafer is obtained by XRD diffraction testing, and the first normal stress, second normal stress and third normal stress of the silicon carbide wafer are all no greater than 60 MPa.

[0007] Optionally, the first shear stress, the second shear stress and the third shear stress of the silicon carbide wafer are all no greater than 30 MPa.

[0008] The first normal stress, the second normal stress and the third normal stress of the silicon carbide wafer are all no greater than 60 MPa, and the first shear stress, the second shear stress and the third shear stress are all no greater than 30 MPa.

[0009] The first normal stress is the stress along the X-axis direction, the second normal stress is the stress along the Y-axis direction, and the third normal stress is the stress along the Z-axis direction. The above-mentioned first normal stress, second normal stress and third normal stress represent the mechanical properties of the silicon carbide wafer. If the value is too large, it will cause damage to the wafer, microcracks or cracks. Therefore, the first normal stress, second normal stress and third normal stress can determine whether the wafer can be used. In the silicon carbide wafer of the present application, the difference between the first normal stress, the second normal stress and the third normal stress is not greater than 30MPa, that is, the stress of the wafer in the above three directions is evenly distributed, and the mechanical properties of the wafer are more evenly distributed.

[0010] Preferably, the difference between the first normal stress, the second normal stress and the third normal stress is no more than 20 MPa.

[0011] The first shear stress is a stress acting on the X-axis normal and along the Y-axis direction, the second shear stress is a stress acting on the Y-axis normal and along the Z-axis direction, and the third shear stress is a stress acting on the Z-axis normal and along the X-axis direction. The above-mentioned first shear stress, second shear stress and third shear stress represent the ability of dislocation slip in the wafer product. The greater the shear stress, the more dislocations in the wafer will increase sharply during the processing of the wafer, thereby causing the device produced by the wafer to fail. Therefore, the first shear stress, second shear stress and third shear stress can affect the performance of the wafer device. In the silicon carbide wafer of the present application, the difference between the first shear stress, the second shear stress and the third shear stress is not more than 20MPa, that is, the stress of the wafer in the above three directions is also uniformly distributed, and dislocation slip can be weakened in any direction, so the device performance obtained using the wafer is also more uniform and stable.

[0012] Preferably, the difference between the first shear stress, the second shear stress and the third shear stress is no more than 15 MPa.

[0013] Preferably, the first normal stress, the second normal stress, the third normal stress, the first shear stress, the second shear stress and the third shear stress are uniformly distributed in the horizontal and vertical directions of the wafer, that is, the difference of each stress in the horizontal and vertical directions is relatively low.

[0014] According to another aspect of the present application, a method for non-destructively and accurately measuring isotropic stress of a wafer is provided, comprising the following steps:

[0015] (1) Perform XRD diffraction test on the wafer. During the test, the wafer is rotated in-plane and between-planes to obtain test results under at least 6 diffraction crystal planes. The diffraction peaks of different diffraction crystal planes are compared with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer to obtain the isotropic strain value of the wafer.

[0016] (2) Calculate the isotropic stress of the chip based on the isotropic strain value and elastic constant.

[0017] This test method is simple and uses a self-designed optimization algorithm to obtain accurate isotropic stress data of the wafer and the distribution of isotropic stress on the wafer surface.

[0018] Optionally, in step (1), the calculation formula of the isotropic strain value is:

[0019] ε xy =cos 2 αsin 2 β×ε 11 +sin2αsin 2 β×ε 12 +cosαsin2β×ε 13 +sin 2 αsin 2 β×ε 22 +sinαsin2β×ε 23 +cos2β×ε 33 Formula (1);

[0020] Among them, ε 11 is the first normal strain of the test point, ε 22 is the second normal strain of the test point, ε 33 is the third normal strain of the test point, ε 12 is the first shear strain at the test point, ε 23 is the second shear strain at the test point, ε 13 is the third shear strain of the test point, α is the in-plane rotation angle, β is the inter-plane rotation angle, ε xy is the total strain value, and its calculation formula is:

[0021] Formula (2),

[0022] where d hkl is the actual interplanar spacing of any test crystal plane, d 0 hkl is the theoretical interplanar spacing of any tested crystal plane.

[0023] To obtain the isotropic stress of the chip, it is necessary to first obtain the isotropic strain value of the chip. The isotropic strain value of the chip is a second-order tensor expressed as a 3×3 matrix. The matrix is ​​written as follows:

[0024] ,

[0025] ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 21 , ε 23 , ε 31 , ε 32 is the isotropic strain value at the test point, where ε 12 = ε 21 , ε 13 = ε 31 , ε 23 =ε 32 , so we only need to find ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 21 The value of can be used together with the elastic constant to calculate the isotropic stress of the chip.

[0026] In actual testing, different ε can be obtained for each diffraction crystal plane. xy value, so the above ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 is an unknown variable, so according to formula (1), the following equation can be constructed for the six diffraction crystal planes:

[0027] .

[0028] In this formula:

[0029] .

[0030] For each diffraction crystal plane, its α and β are known, so a 11 、a 12 、a 13 、a 14 、a 15 、a 16 is a known quantity, ε xy It is a quantity that can be calculated based on the interplanar spacing. Based on the above known quantities, ε can be obtained. 11 , ε 22 , ε33 , ε 12 , ε 13 , ε 23 value.

[0031] In the above calculation method, the elastic constant is an important parameter for studying the mechanical properties of materials. The elastic constant is a fourth-order tensor, and its writing is relatively complicated. The specific parameters of the elastic constants of different wafers can be queried in the database. For hexagonal silicon carbide crystals, the elastic constant can be written in matrix form:

[0032] ,

[0033] Therefore, the calculation formula for the stress in each direction is:

[0034] ,

[0035] where σ 11 is the first normal stress at the test point, σ 22 is the second normal stress at the test point, σ 33 is the third normal stress of the test point, σ 12 is the first shear stress at the test point, σ 23 is the second shear stress at the test point, σ 13 is the third shear stress at the test point, C 66 =(C 11 -C 12 ) / 2, C 11 、C 12 、C 13 、C 33 and C 44 There are five independent parameters in the hexagonal crystal system.

[0036] The above formula can be used to calculate the isotropic stress of the wafer. The matrix expression of the isotropic stress is as follows:

[0037] .

[0038] Optionally, there are at least 7 diffraction crystal planes.

[0039] The above stress values ​​refer to the absolute stress of the wafer at the test point, that is, the residual stress compared to the stress-free wafer. The first normal stress is the stress along the X-axis, the second normal stress is the stress along the Y-axis, the third normal stress is the stress along the Z-axis, and the first shear stress σ 12 is the stress acting on the normal line of the X axis and along the Y axis, and the stress acting on the normal line of the Y axis and along the X axis σ 21 Equal, the second shear stress σ 23is the stress acting on the Y-axis normal and along the Z-axis direction, and the stress acting on the Z-axis normal and along the Y-axis direction σ 32 Equal, the third shear stress σ 13 is the stress acting on the normal line of the X axis and along the Z axis, and is the stress acting on the normal line of the Z axis and along the X axis σ 31 equal.

[0040] The above-mentioned diffraction crystals constructed with 6 diffraction crystal planes contain ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 Detecting at least seven diffraction crystal planes here can further improve the accuracy of the above-mentioned solutions to the isotropic strain values, thereby accurately determining the isotropic stress distribution of the chip.

[0041] Optionally, the diffraction crystal planes include (002) plane, (004) plane, (006) plane, (008) plane, (102) plane, (103) plane, (104) plane, (105) plane, (024) plane, (026) plane, (044) plane, (113) plane, (114) plane, and (115) plane.

[0042] Optionally, the peak intensity of the diffraction crystal plane is not less than 20,000 cps, and the half-width is not greater than 100 arcsec.

[0043] The diffraction plane has a strong diffraction intensity and a moderate half-width, which can scan accurate information about the chip, thereby calculating a more accurate total strain value. If the height and width of the diffraction plane are greater than 100 arcsec, the detection accuracy of the chip will be reduced, and the total strain value obtained from the test will be unusable.

[0044] Optionally, the value range of α is 0-180°, and the value range of β is 0-90°. The chip can be rotated within the above range and between planes to facilitate finding the required diffraction surface during the test process.

[0045] Optionally, in the XRD diffraction test, the penetration depth of XRD is 3-60 μm.

[0046] Optionally, the wafer is a silicon carbide wafer, and the silicon carbide wafer includes a semi-insulating type and a conductive type.

[0047] Optionally, the diameter of the wafer is greater than 6 inches, preferably 8 inches.

[0048] According to another aspect of the present application, a standard method for detecting isotropic stress of a wafer is provided, comprising the following steps:

[0049] Step 1: Place the wafer on the XRD test sample table, select the initial diffraction crystal plane, obtain the diffraction peak of the initial diffraction crystal plane, then rotate the wafer in-plane and between-planes to obtain diffraction peaks under at least 6 diffraction crystal planes, compare the diffraction peaks of the above diffraction crystal planes with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer, and obtain the total strain value ε under each diffraction crystal plane xy ;

[0050] Step 2: Calculate the isotropic strain value of the wafer according to the calculation formula of the total strain value and the isotropic strain value;

[0051] Step 3: Calculate the isotropic stress of the chip based on the isotropic strain values ​​calculated in the second step and the elastic constants of the chip.

[0052] In this standard method for detecting isotropic stress in a wafer, the calculation formulas for the isotropic strain value in the second step and the isotropic stress in the third step are the same as those for the method for non-destructively and accurately measuring isotropic stress in a wafer. Operators can calculate the isotropic stress in the wafer according to the steps and procedures of the above standard method for detecting isotropic stress in a wafer.

[0053] The beneficial effects of this application include but are not limited to:

[0054] 1. Currently available detection methods are unable to distinguish and detect normal stress and shear stress in a wafer. The present invention's non-destructive and precise method for measuring wafer isotropic stresses allows calculation of the isotropic stress at a specific test point on the wafer while testing different diffraction planes, thereby obtaining the isotropic stress distribution of the entire wafer.

[0055] 2. According to the present invention's method for nondestructively and accurately measuring wafer isotropic stress, the values ​​of the first normal strain, second normal strain, third normal strain, first shear strain, second shear strain, and third shear strain can be simplified and calculated based on the isotropic strain calculation formula. This allows the calculation of the wafer's isotropic stress values, providing a theoretical basis for the study of wafer isotropic stress.

[0056] 3. The nondestructive and precise method for measuring isotropic stress in a wafer according to this application utilizes in-plane and inter-plane rotation of the wafer to obtain measurements at different diffraction planes. This method allows for the determination of isotropic stress values ​​at the test point without destroying the wafer, making it suitable for industrial, large-scale testing.

[0057] 4. According to the method for non-destructively and accurately measuring isotropic stress of a wafer of the present application, the diffraction crystal plane provided can obtain a strong diffraction peak in XRD diffraction, further improving the test accuracy of the method.

[0058] 5. According to the method for non-destructively and accurately measuring the isotropic stress of a wafer in this application, the isotropic stress is calculated using elastic constants, which mathematically simplifies the elastic constants of the fourth-order tensor, making the calculation process simpler and the calculation results more accurate.

[0059] 6. The silicon carbide wafer according to the present application has substantially the same first normal stress, second normal stress, and third normal stress, and substantially the same first shear stress, second shear stress, and third shear stress. The stresses are uniformly distributed, which prevents slippage of the wafer in all directions, thereby reducing the number of dislocations in the wafer and improving the uniformity of dislocation distribution, reducing lattice distortion, and improving the stability and reliability of devices fabricated from the wafer. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0061] FIG1 is a top view of a fixture for wafer stress detection according to Example 1 of the present application;

[0062] FIG2 is a side view of a fixture for wafer stress detection according to Example 1 of the present application;

[0063] FIG3 is a top view of the permanent magnetic base involved in Example 1 of the present application;

[0064] FIG4 is a top view of the wafer to be tested according to Example 1 of the present application;

[0065] FIG5 is a schematic diagram of XRD diffraction of a silicon carbide wafer according to Example 2 of the present application;

[0066] FIG6 is a diffraction result diagram of the silicon carbide wafer involved in Example 2 of the present application on the (004) plane;

[0067] FIG7 is a diagram showing the diffraction results of the silicon carbide wafer involved in Example 2 of the present application at the (024), (114), (105), (102), (026), and (104) diffraction crystal planes;

[0068] FIG8 is a schematic diagram showing the directions of the anisotropic stresses in the silicon carbide wafer according to Example 2 of the present application;

[0069] List of parts and reference numerals:

[0070] 1. Wafer to be tested; 2. Sample holder; 3. Sample placement plate; 4. Permanent magnetic base; 5. Sample stage; 6. Scale line; 7. Marking line. Implementation Method

[0071] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0072] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels. Example

[0073] 1-4 , this embodiment discloses a fixture for wafer stress detection, comprising: a permanent magnetic base 4, a connecting component being provided at the bottom of the permanent magnetic base 4, the connecting component being used to connect to a sample stage 5 of a detection instrument; a sample placement tray 3, the sample placement tray 3 being provided above the permanent magnetic base 4, the sample placement tray 3 containing metal particles therein, the sample placement tray 3 being used to place a wafer to be tested 1; a sample clamp 2, the sample clamp 2 being provided above the sample placement tray 3, the sample clamp 2 being in circumferential contact with the wafer to be tested 1, and being used to clamp the wafer to be tested 1.

[0074] The permanent magnetic base 4 in the fixture is fixed to the sample stage 5 via a connecting component, achieving a fixed connection between the entire fixture and the sample stage 5, thereby improving the stability of the entire fixture during testing. The metal particles set inside the sample placement plate 3 and the permanent magnetic base 4 are attracted by magnetic force, achieving a fixed connection between the sample placement plate 3 and the permanent magnetic base 4. The chip 1 to be tested is placed on the sample placement plate 3 and fixed by the sample clamp 2. Therefore, with the cooperation of the sample placement plate 3 and the sample clamp 2, the fixture can replace the existing vacuum adsorption method to achieve the fixation of the chip 1 to be tested during the stress testing process. No additional stress is caused during the overall testing process, ensuring the accuracy of the stress testing of the chip 1 to be tested. When the sample stage 5 is tilted to perform stress testing on the chip 1 to be tested, the fixture can also clamp the chip 1 to be tested, so that when the chip 1 to be tested is subjected to in-plane and inter-plane rotation testing, the coordinates of the test point can still be guaranteed to remain unchanged.

[0075] Moreover, the sample placement plate 3 and the permanent magnetic base 4 are magnetically adsorbed, which facilitates adjustment of the position of the sample placement plate 3 on the permanent magnetic base 4. Under this setting, the position of the wafer to be tested 1 can be adjusted without the sample stage 5 moving, thereby realizing stress detection of different positions of the wafer to be tested 1, thereby improving the ease of use of the fixture.

[0076] In one embodiment, there are at least two sample holders 2. The sides of the sample holders 2 that abut the wafer 1 to be tested are curved and are evenly arranged along the circumference of the wafer 1 to be tested. This arrangement allows the wafer 1 to be clamped and secured uniformly along its circumference, improving the stability of the fixture during use. Furthermore, when testing wafers 1 of different sizes, the wafer 1 can be re-secured by replacing or moving a portion of the sample holders 2, thereby increasing the fixture's adjustment flexibility.

[0077] In one embodiment, the sample holder 2 contains metal particles and is movable along the upper surface of the sample tray 3. This arrangement allows the sample tray 3 and the sample holder 2 to be separately connected, allowing the position of the sample holder 2 on the tray 3 to be adjusted to clamp wafers 1 of varying sizes without the need to replace any components, further enhancing the ease of use and universality of the fixture.

[0078] In one embodiment, the permanent magnetic base 4 is made of neodymium iron boron (NdFeB). Both the permanent magnetic base 4 and the sample tray 3 are less than 3 mm thick. Because the fixture is fixed to the sample stage 5, the overall height of the fixture is relatively low. NdFeB is used to make the permanent magnetic base 4 because it is relatively easy to process into thin sheets, which reduces the overall height of the fixture and facilitates its installation on the sample stage 5 of the testing instrument.

[0079] In one embodiment, the permanent magnetic base 4 is provided with scale lines 6, and the sample tray 3 is made of a transparent material. Providing scale lines 6 on the permanent magnetic base 4 and using the transparent material for the sample tray 3 facilitates positioning of the wafer 1 under test, improves the adjustment efficiency of the wafer 1 under test, and enables stress detection at different positions of the wafer 1 under test.

[0080] In actual use, as shown in Figure 3, which is a top view of the permanent magnetic base 4, the scale line 6 is a cross line, and the intersection of the cross lines is the positioning point. Before the stress test is performed on the wafer 1 to be tested, a number of vertical marking lines 7 are drawn on its surface using a marker. The points where the marking lines 7 intersect are the test points. As shown in Figure 4, during the test, the position of the sample placement plate 3 on the permanent magnetic base 4 is adjusted, and a certain test point of the wafer 1 to be tested is aligned with the positioning point of the permanent magnetic base 4 to achieve the positioning of a certain test point, so that subsequent stress testing can be performed.

[0081] As a preferred embodiment, the sample placement plate 3 is made of polycarbonate or polymethyl methacrylate, the sample holder 2 is made of polytetrafluoroethylene, and the connecting member is adhesive. This arrangement can prevent scratches on the wafer 1 to be tested and achieve stable clamping of the wafer 1 to be tested while ensuring safety.

[0082] Example 2

[0083] This embodiment relates to a method for processing a 6-inch silicon carbide wafer and a method for measuring isotropic stress:

[0084] 1. The processing method of silicon carbide wafer comprises the following steps:

[0085] (1) The cut silicon carbide wafers were annealed by raising the temperature to 1800°C. The silicon carbide wafers were then naturally cooled to room temperature in a heating furnace and then ground using alumina with an average particle size of 1 μm for 5 hours. The TTV of the silicon carbide wafers after grinding was less than 4 μm.

[0086] (2) Then, polishing is performed using silica and ceria abrasives with a hardness lower than that of silicon carbide. The particle size of the two abrasives is 100 nm, and the weight ratio of silica to ceria is 1:1. The mixing method is ball milling, and the polishing time is 3 to 5 hours to obtain a wafer with relatively uniform surface stress and completely remove the damaged layer on the wafer surface to eliminate the influence of inelastic deformation. After polishing, the roughness of the silicon carbide wafer is less than 1 nm, or the TTV is less than 2 μm.

[0087] 2. The method for measuring the stress in each direction includes the following steps:

[0088] (1) The ground or polished wafer is placed on the fixture in Example 1, and an XRD diffraction test is performed on the silicon carbide wafer, as shown in Figure 5 (a). The (004) plane with higher diffraction intensity is selected as the initial diffraction crystal plane. The diffraction result is shown in Figure 6. Then, as shown in Figure 5 (b), the wafer is rotated in-plane and between-planes to obtain diffraction peaks under the (024), (114), (105), (102), (026), and (104) diffraction crystal planes. The result is shown in Figure 7. The in-plane rotation angle α and the inter-plane rotation angle β of each diffraction crystal plane from the initial diffraction crystal plane are recorded. The diffraction peaks of the above six diffraction crystal planes are compared with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer. The total strain value ε of each of the six diffraction crystal planes is calculated according to the following formula: xy :

[0089] ,

[0090] where d hkl is the actual interplanar spacing of any test crystal plane, d 0 hkl is the theoretical interplanar spacing of any test crystal plane;

[0091] Substitute the obtained 6 total strain values ​​into the following formula:

[0092] ε xy =cos 2 αsin 2 β×ε 11 +sin2αsin 2 β×ε 12 +cosαsin2β×ε 13 +sin 2 αsin 2 β×ε 22+sinαsin2β×ε 23 +cos2β×ε 33 ;

[0093] In the above formula, ε of each diffraction crystal plane is xy If , α and β are known, they can be listed as seven equations, and ε can be calculated based on these seven equations. 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 The value of ε 11 , ε 22 , ε 33 , ε 12 , ε 13 , ε 23 That is the isotropic strain value of the chip.

[0094] (2) Calculate the isotropic stress of the wafer based on the isotropic strain value and the elastic constant. The calculation formula is as follows, where the elastic constant is the parameter in the query database:

[0095] .

[0096] In the above stress matrix, the directions of the stresses expressed by the parameters are shown in Figure 8, σ 11 , σ 22 , σ 33 is the normal stress, and the remaining components are shear stresses. The obtained stress results in various directions are shown in Table 1 below. The center point of the chip in Table 1 is the coordinate (0,0).

[0097] Table 1

[0098]

[0099] Example 3

[0100] This embodiment relates to a method for processing an 8-inch silicon carbide wafer and a method for measuring isotropic stress. The steps in the processing method and the measuring method are the same as those in Example 2. The isotropic stress data of the 8-inch silicon carbide wafer are obtained. The results are shown in Table 2 below. In Table 2, the center point of the wafer is the coordinate (0, 0).

[0101] Table 2

[0102]

[0103] Reliability Verification

[0104] The reliability of the silicon carbide wafer tested by the isotropic stress determination method of the above-mentioned embodiment 2 and embodiment 3 was verified, specifically: using an X-ray diffractometer with different wavelengths to verify the reliability of the strain test, and then obtain a feasibility analysis of the stress test. The strain value tested with the Cu target is recorded as , the strain value measured by Mo target is recorded as ,pass The reliability is judged by comparing the difference between the two. In the measurement method of the present application, Δ is less than 1%, which proves that the measurement method of the present application for isotropic stress has high reliability and accuracy.

[0105] The foregoing is merely an embodiment of the present application, and the scope of protection of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application may have various modifications and variations. Any modifications, equivalent substitutions, improvements, etc. made within the technical ideas and principles of the present application should be included in the scope of protection of the present application.

Claims

1. A method for non-destructive and accurate determination of the stress in all directions of a wafer, It is characterized in that The steps include: (1) Performing an XRD diffraction test on the wafer. During the test, the wafer is rotated within and between planes to obtain test results on at least 6 diffraction crystal planes. The diffraction peaks of different diffraction crystal planes are compared with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer to obtain the isotropic strain value of the wafer. (2) Calculate the isotropic stress of the chip based on the isotropic strain value and elastic constant.

2. The method according to claim 1, It is characterized in that In step (1), the calculation formula of the strain value in each direction is: e xy =cos 2 asin 2 b×e 11 +sin2αsin 2 b×e 12 +cosαsin2β×ε 13 +sin 2 asin 2 b×e 22 +sinαsin2β×ε 23 +cos2β×ε 33 formula (1); Among them, ε 11 is the first normal strain of the test point, ε 22 is the second normal strain of the test point, ε 33 is the third normal strain of the test point, ε 12 is the first shear strain at the test point, ε 23 is the second shear strain at the test point, ε 13 is the third shear strain of the test point, α is the in-plane rotation angle, β is the inter-plane rotation angle, and ε xy is the total strain value, and its calculation formula is: Formula (2), where d hkl is the actual interplanar spacing of any tested crystal plane, d 0 hkl is the theoretical interplanar spacing of any tested crystal plane.

3. The method according to claim 2, It is characterized in that The calculation formula for the stress in each direction is: , where σ 11 is the first normal stress at the test point, σ 22 is the second normal stress at the test point, σ 33 is the third normal stress at the test point, σ 12 is the first shear stress at the test point, σ 23 is the second shear stress at the test point, σ 13 is the third shear stress at the test point, C 66 =(C 11 -C 12 ) / 2, C 11 , C 12 , C 13 , C 33 and C 44 There are five independent parameters in the hexagonal crystal system.

4. The method according to any one of claims 1 to 3, It is characterized in that The diffraction crystal planes include (002) plane, (004) plane, (006) plane, (008) plane, (102) plane, (103) plane, (104) plane, (105) plane, (024) plane, (026) plane, (044) plane, (113) plane, (114) plane, and (115) plane.

5. The method according to claim 4, It is characterized in that The peak intensity of the diffraction crystal plane is not less than 20,000 cps, and the half-height width is not greater than 100 arcsec.

6. The method according to claim 2 or 3, It is characterized in that The value range of α is 0-180°, and the value range of β is 0-90°.

7. The method according to any one of claims 1 to 3, It is characterized in that In the XRD diffraction test, the penetration depth of XRD is 3-60 μm.

8. A silicon carbide wafer having uniformly distributed stress, It is characterized in that The first normal stress, the second normal stress and the third normal stress of the silicon carbide wafer tested by the method according to claim 1 are all no greater than 60 MPa.

9. The silicon carbide wafer according to claim 8, It is characterized in that The first shear stress, the second shear stress and the third shear stress of the silicon carbide wafer are all no greater than 30 MPa.

10. A standard method for detecting isotropic stress in wafers. It is characterized in that The steps include: Step 1: Place the wafer on the XRD test sample table, select the initial diffraction crystal plane, obtain the diffraction peak of the initial diffraction crystal plane, then rotate the wafer in-plane and between-planes to obtain diffraction peaks under at least 6 diffraction crystal planes, compare the diffraction peaks of the above diffraction crystal planes with the standard peaks of the corresponding diffraction crystal planes in the stress-free wafer, and obtain the total strain value ε under each diffraction crystal plane xy ; Step 2: According to the total strain value ε xy and the calculation formula of the isotropic strain value, calculate the isotropic strain value of the wafer; Step 3: Calculate the isotropic stress of the chip based on the isotropic strain values ​​calculated in the second step and the elastic constants of the chip.

Citation Information

Patent Citations

  • Method for evaluating internal stress of silicon carbide monocrystalline wafer and method for predicting warpage in silicon carbide monocrystalline wafer

    CN105556649A

  • Silicon carbide single crystal wafer and method for producing silicon carbide single crystal ingot

    CN112626618A

  • Method for detecting internal stress of bulk silicon carbide single crystal

    CN114509457A

  • Method and system for detecting residual stress of silicon carbide crystal

    CN114858324A

  • Silicon carbide wafer with uniformly distributed stress and method for lossless and accurate determination of stress in each direction of wafer

    CN116657249A