Freeze-stretched thin film and preparation process therefor

By using multi-layer structure and electron beam cross-linking treatment composed of olefin A polymer and olefin A-ethylene copolymer, the problems of non-recyclable use and high cost of existing frozen film materials are solved, and environmentally friendly and low-cost frozen pulling are achieved Extension film has excellent cold resistance and drop resistance.

WO2024244847A1PCT designated stage expired Publication Date: 2024-12-05ANHUI SHUANGJIN CO LTD

Patent Information

Application Number
PCT/CN2024/089958
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-29
Filing Date
2024-04-26
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Due to the inrecyclable use of PA and PE and the high cost of existing frozen membrane materials, environmental pollution and market competitiveness have declined, and their structure is not environmentally friendly.

Method used

The corona layer, subsurface layer, intermediate layer and heat sealing layer are used to make the polymer of olefin A. The compatibility of olefin A-ethylene copolymer is improved to form an environmentally friendly and low-cost frozen stretch film. Electron beam cross-linking is also performed to enhance puncture and drop resistance.

Benefits of technology

It realizes an environmentally friendly and low-cost frozen stretch film, with excellent cold resistance, body bonding, puncture resistance and drop resistance, avoids the phenomenon of sticking the knife and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024089958_05122024_PF_FP_ABST
    Figure CN2024089958_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a freeze-stretched thin film and a preparation process therefor. The freeze-stretched thin film sequentially comprises a corona layer, a secondary surface layer, a middle layer, a secondary inner layer and a heat seal layer, wherein the raw materials of the corona layer comprise a polymer of olefin A, and the melting point of the polymer of olefin A is greater than that of polyethylene; the raw materials of the secondary surface layer comprise a polymer of olefin A and an olefin A-ethylene copolymer; the raw materials of the middle layer comprise polyethylene and an olefin A-ethylene copolymer, and the content of the olefin A-ethylene copolymer in the middle layer is lower than that of the olefin A-ethylene copolymer in the secondary surface layer; the raw materials of the secondary inner layer comprise polyethylene; and the raw materials of the heat seal layer comprise metallocene polyethylene. The freeze-stretched thin film not only has good cold resistance, body-fitting effect, tensile strength, impact strength and puncture resistance, but also is inexpensive, recyclable and has good environmental protection performance.
Need to check novelty before this filing date? Find Prior Art

Description

A frozen stretch film and its preparation process Technical Field

[0001] The invention belongs to the technical field of frozen films, and in particular relates to a frozen stretched film and a preparation process thereof. Background Art

[0002] Freezer film is a packaging material used for frozen foods such as glutinous rice balls, dumplings, and seafood. This application places high demands on the film's cold resistance, form-fitting properties, and strength. The resulting packaging bag must resist cracking in freezing conditions and adhere tightly to the packaged item. Due to its excellent puncture resistance and form-fitting properties, this film is also suitable for packaging electronic products and medical devices.

[0003] At present, most commercially available freezing films are five-layer co-extruded materials of PA (polyamide) / adhesive layer / PE / PE / PE (polyethylene). Among them, PA material is in the outermost layer of the film because of its good gas barrier and moisture resistance, and PE is in the inner layer of the film because of its good heat sealing performance.

[0004] However, because PA and PE are two completely different substances, after their first use, they cannot enter the next recycling system (such as granulation) and can only be discarded or incinerated, causing environmental pollution. Therefore, this structure is not environmentally friendly and its materials cannot be recycled, which does not comply with relevant national policies. In addition, PA is more expensive than polyolefins, which does not meet market competition requirements. Summary of the Invention

[0005] The purpose of the present invention is to provide a freeze-stretched film and a preparation process thereof, wherein the freeze-stretched film not only has good cold resistance, body-fitting effect, tensile strength, impact strength and puncture resistance, but also is low in price, can be recycled and has good environmental performance.

[0006] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is:

[0007] A frozen stretch film comprises a corona layer, a sub-surface layer, an intermediate layer, a sub-inner layer and a heat-sealing layer in sequence, wherein:

[0008] The raw material of the corona layer includes a polymer of olefin A, and the melting point of the polymer of olefin A is greater than the melting point of polyethylene;

[0009] The raw materials of the subsurface layer include polymers of olefin A and olefin A-ethylene copolymers;

[0010] The raw materials of the intermediate layer include polyethylene and olefin A-ethylene copolymer, and the content of olefin A-ethylene copolymer in the intermediate layer is lower than that in the subsurface layer;

[0011] The material of the secondary inner layer includes polyethylene;

[0012] The raw material of the heat sealing layer includes metallocene polyethylene.

[0013] In the present invention, the raw materials of each layer are olefin polymers, which have the same properties, are easy to recycle in the later stage, and have good environmental performance. In addition, the price of olefin is lower than that of PA, which greatly reduces the preparation cost of the film.

[0014] In the present invention, olefin A can be any olefin except ethylene, as long as the melting point of the polymer of olefin A is greater than the melting point of polyethylene and a temperature difference exists between the corona layer and the heat-sealing layer to facilitate bag making.

[0015] In the present invention, the sub-surface layer contains not only the same olefin A polymer as the corona layer, but also olefin A-ethylene copolymer, and the middle layer contains not only the same polyethylene as the sub-inner layer, but also olefin A-ethylene copolymer, which forms a transition between the corona layer and the sub-inner layer. The olefin A-ethylene copolymer has excellent compatibility with the olefin A polymer and the polyethylene. This excellent compatibility allows entanglement between the molecules of the blended materials, effectively improving the interlayer bonding strength. Therefore, the corona layer and the sub-inner layer can be tightly bonded without the use of an adhesive, so that the film has excellent cold resistance (can be quickly frozen at -40°C and stored in an environment of -18°C), puncture resistance and drop resistance (high impact strength).

[0016] Preferably, in the above-mentioned freeze-stretched film, the olefin A is propylene. There is a 50°C temperature difference between the melting points of polypropylene and polyethylene, so during heat sealing, the heat sealing layer melts and adheres at the heat sealing temperature, while the corona layer does not melt.

[0017] Preferably, in the freeze-stretched film, the polymer of olefin A is homopolypropylene. Compared with other types of polypropylene, homopolypropylene has higher strength.

[0018] Preferably, in the above-mentioned freeze-stretched film, the content of olefin A in the olefin A-ethylene copolymer is higher than the content of ethylene; for example, Vistamaxx, a product of Mobil Corporation of the United States, has an ethylene content of about 15% and a propylene content of about 85%.

[0019] Because the olefin A-ethylene copolymer content in the subsurface layer is higher than that in the middle layer, the subsurface layer has a higher olefin A content and greater compatibility with the corona layer, while the middle layer has a higher ethylene content and greater compatibility with the subinner layer. In this case, the olefin A content decreases from the corona layer toward the heat-seal layer, while the ethylene content increases, resulting in a stronger bond between the layers.

[0020] Preferably, in the above-mentioned freeze-stretched film, the content of olefin A-ethylene copolymer in the sub-surface layer is 40-80% by mass;

[0021] In the described middle layer, the content of olefin A-ethylene copolymer is 30-70%.As preferably, in the above-mentioned freeze-stretched film, in the described middle layer and the secondary inner layer, the polyethylene is at least one of low-density polyethylene and metallocene high-density polyethylene.

[0022] Preferably, in the above-mentioned freeze-stretched film, the thicknesses of the corona layer, sub-surface layer, middle layer, sub-inner layer and heat-sealing layer are 5%-50%, 10%-50%, 10%-50%, 10%-50% and 5%-50% of the film thickness respectively.

[0023] Preferably, the thickness of the freeze-stretched film is 80-160 microns.

[0024] As a further preference, the thickness of the above-mentioned freeze-stretched film is 100-120 microns.

[0025] The present invention also provides a process for preparing the above-mentioned freeze-stretched film, which comprises the following steps:

[0026] (1) Using the preset raw materials, a five-layer composite film is obtained in a five-layer co-extrusion film blowing machine;

[0027] Among them, the extrusion temperature of the A extruder used for extruding the corona layer is: 160°C in zone 1, 180°C in zone 2, 200°C in zone 3, and 220°C in zone 4;

[0028] The extrusion temperatures of the B extruder used for extruding the secondary outer layer are: 120°C in zone 1, 160°C in zone 2, 180°C in zone 3, and 190°C in zone 4;

[0029] The extrusion temperatures of the C extruder used to extrude the middle layer are: 100°C in zone 1, 150°C in zone 2, 180°C in zone 3, and 190°C in zone 4;

[0030] The extrusion temperatures of the D extruder used for extruding the secondary inner layer are: 110°C in zone 1, 160°C in zone 2, 180°C in zone 3, and 190°C in zone 4;

[0031] The extrusion temperatures of the E extruder used for extruding the heat seal layer are: 110°C in zone 1, 150°C in zone 2, 170°C in zone 3, and 180°C in zone 4;

[0032] (2) The five-layer composite film is subjected to thickness measurement, corona treatment, winding, plasticization, cross-linking, and slitting to obtain the freeze-stretched film.

[0033] In the present invention, the five-layer composite film is also subjected to electron beam cross-linking treatment. The electron beam cross-linking treatment can change the way the molecules between the film layers are entangled, and the branched structure is converted into a network cross-linked structure, thereby not only further improving the puncture resistance and drop resistance of the film, but also making the film softer (high tensile strength), better in body adhesion, and without knife sticking.

[0034] The crosslinking step is carried out in a scanning box, where the electron beam bombards the film to achieve the crosslinking purpose. The electron beam voltage is 0.5 MeV, the beam current is 50 mA, and the vacuum degree of the scanning box is less than 2×10 -4 .

[0035] Compared with the prior art, the beneficial effects of the present invention are embodied in:

[0036] (1) In the present invention, the raw materials of each layer are polymers of olefins, which have the same properties, are easy to recycle in the later stage, and have good environmental performance. In addition, the price of olefins is lower than that of PA, which greatly reduces the preparation cost of the film.

[0037] (2) In the present invention, the sub-surface layer contains not only the same olefin A polymer as the corona layer, but also olefin A-ethylene copolymer, and the middle layer contains not only the same polyethylene as the sub-inner layer, but also olefin A-ethylene copolymer, which forms a transition between the corona layer and the sub-inner layer. The olefin A-ethylene copolymer has excellent compatibility with the olefin A polymer and polyethylene. This excellent compatibility allows entanglement between the molecules of the blended materials, effectively improving the interlayer bonding force. Therefore, the corona layer and the sub-inner layer can be tightly bonded without the use of an adhesive, so that the film has excellent cold resistance, puncture resistance and drop resistance (high impact strength).

[0038] (3) The preparation method of the present invention includes the step of subjecting the five-layer composite film to electron beam cross-linking treatment. The electron beam cross-linking treatment can change the way the molecules between the film layers are entangled, and convert the branched structure into a network cross-linked structure, thereby not only further improving the puncture resistance and drop resistance of the film, but also making the film softer (high tensile strength), better in body adhesion, and without knife sticking. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] FIG1 is a schematic structural diagram of a freeze-stretched film according to the present invention;

[0040] FIG2 is a flow chart of the preparation process of the freeze-stretched film of the present invention. DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0042] Example 1

[0043] As shown in FIG1 , a frozen stretched film according to this embodiment includes a corona layer, a subsurface layer, an intermediate layer, a subinner layer, and a heat-sealing layer in sequence; the raw material compositions of each layer are as follows, calculated by mass percentage:

[0044] Corona layer: isotactic homopolymer polypropylene (Singapore, TPC, FS3028; without anti-sticking agent and slip agent; TM (melt point) = 163 ° C, MI = 3.5) 100%;

[0045] Second outer layer: isotactic homopolymer polypropylene 20% + propylene-ethylene copolymer (USA, Mobil, Vistamaxx; TM (melt point) = 59 ° C, MI = 5.0) 80%;

[0046] Middle layer: Metallocene high-density polyethylene (UK, INEOS, F4330; does not contain anti-sticking agent and slip agent. Density 0.938, MI=4.0) 70% + propylene-ethylene copolymer 30%;

[0047] Second inner layer: low-density polyethylene (USA, Dow, ELITE AT6201; TM (melt point) = 106 ° C, MI = 0.85) 100%;

[0048] Heat seal layer: Metallocene polyethylene (Japan, SP0510, MLLDPE; TM (melt point) = 98 ° C, MI = 1.2) 97% + synthetic silica (An color, CHAB-10, active ingredient accounts for 10%) 3%.

[0049] The preparation process of the freeze-stretched film is shown in FIG2 and includes the following steps:

[0050] (1) Using the preset raw materials, a five-layer composite film is obtained in a five-layer co-extrusion film blowing machine;

[0051] Among them, the extrusion temperature of the A extruder used for extruding the corona layer is: 160°C in zone 1, 180°C in zone 2, 200°C in zone 3, and 220°C in zone 4;

[0052] The extrusion temperatures of the B extruder used for extruding the secondary outer layer are: 120°C in zone 1, 160°C in zone 2, 180°C in zone 3, and 190°C in zone 4;

[0053] The extrusion temperatures of the C extruder used to extrude the middle layer are: 100°C in zone 1, 150°C in zone 2, 180°C in zone 3, and 190°C in zone 4;

[0054] The extrusion temperatures of the D extruder used for extruding the secondary inner layer are: 110°C in zone 1, 160°C in zone 2, 180°C in zone 3, and 190°C in zone 4;

[0055] The extrusion temperatures of the E extruder used for extruding the heat seal layer are: 110°C in zone 1, 150°C in zone 2, 170°C in zone 3, and 180°C in zone 4;

[0056] (2) The five-layer composite film is subjected to thickness measurement, corona treatment, winding, plasticization, cross-linking, and slitting to obtain the freeze-stretched film;

[0057] The cross-linking step is carried out in a scanning box, where the electron beam bombards the film to achieve the cross-linking purpose. The electron beam voltage is 0.5 MeV, the beam current is 50 mA, and the vacuum degree of the scanning box is less than 2×10 -4 .

[0058] The other steps are performed according to methods known in the art.

[0059] The thickness of the frozen stretched film prepared in this embodiment is 110 microns, wherein the thickness of the corona layer is 10 microns, the thickness of the subsurface layer is 25 microns, the thickness of the middle layer is 25 microns, the thickness of the subinner layer is 25 microns, and the thickness of the heat sealing layer is 15 microns. Example

[0060] This embodiment is a freeze-stretched film, and its structure and preparation process are the same as those of Example 1, except that the raw material composition of each layer of the film is as follows:

[0061] Corona layer: isotactic homopolymer polypropylene (Korea, Samsung, HF429; TM (melt point) = 162 ° C, MI = 8.0) 100%;

[0062] Second outer layer: isotactic homopolymer polypropylene 20% + propylene-ethylene copolymer (USA, Mobil, Vistamaxx; TM (melt point) = 59 ° C, MI = 5.0) 80%;

[0063] Middle layer: low-density polyethylene (USA, Dow, ELITE AT6201; TM (melt point) = 106 ° C, MI = 0.85) 70% + propylene-ethylene copolymer 30%;

[0064] Second inner layer: low-density polyethylene (Mobil, 151BW, USA; without anti-sticking agent and slip agent, density 0.933, MI = 3.0) 50% + metallocene high-density polyethylene (Dow Chemical, USA, 2047G; without anti-sticking agent and slip agent, density 0.917, MI = 2.3) 50%;

[0065] Heat seal layer: Metallocene polyethylene (Japan, SP0510, MLLDPE; TM (melt point) = 98 ° C, MI = 1.2) 95% + synthetic silica (An color, CHAB-10, active ingredient accounts for 10%) 5%. Example

[0066] This embodiment is a freeze-stretched film, and its structure and preparation process are the same as those of Example 1, except that the content of propylene-ethylene copolymer in the sub-outer layer is 40%, and the content of propylene-ethylene copolymer in the middle layer is 70%.

[0067] The structure and preparation process of the freeze-stretched film of this comparative example are basically the same as those of Example 1, except that the content of the propylene-ethylene copolymer in the sub-outer layer is 10%, and the content of the propylene-ethylene copolymer in the middle layer is 90%.

[0068] The structure and preparation process of the freeze-stretched film of this comparative example are basically the same as those of Example 1, except that the preparation process does not include a cross-linking step.

[0069] The freeze-stretched films prepared in Examples 1-3 and Comparative Examples 1-2 were tested for various physical properties. The test results are shown in Table 1.

[0070]

[0071] As shown in Table 1, compared to Comparative Examples 1-2, the films of Examples 1-3 have higher temperature resistance (increased by 5-7°C), making them less susceptible to knife sticking during slitting operations. Furthermore, the films of Examples 1-3 exhibit superior cold resistance, tensile strength, impact strength, puncture resistance, and body-fitting properties. In Comparative Example 1, the propylene-ethylene polymer content in the subsurface layer is lower than that in the intermediate layer, resulting in a lack of transition between the corona layer and the subinner layer, leading to a decrease in various physical properties. In Comparative Example 2, the lack of cross-linking during the preparation process results in insufficient interlayer bonding, which also leads to a decrease in various physical properties.

Claims

1. A frozen stretched film, comprising a corona layer, a sub-surface layer, an intermediate layer, a sub-inner layer and a heat sealing layer in sequence, characterized in that: The raw material of the corona layer includes a polymer of olefin A, and the melting point of the polymer of olefin A is greater than the melting point of polyethylene; The raw materials of the sub-surface layer include polymers of olefin A and olefin A-ethylene copolymers; The raw materials of the intermediate layer include polyethylene and olefin A-ethylene copolymer, and the content of olefin A-ethylene copolymer in the intermediate layer is lower than that in the sub-surface layer; The material of the secondary inner layer includes polyethylene; The raw material of the heat sealing layer includes metallocene polyethylene.

2. The freeze-stretched film according to claim 1, wherein The olefin A is propylene.

3. The freeze-stretched film according to claim 2, wherein The polymer of olefin A is homopolypropylene.

4. The freeze-stretched film according to claim 1, characterized in that The content of olefin A in the olefin A-ethylene copolymer is higher than that of ethylene.

5. The freeze-stretched film according to claim 1, characterized in that In terms of mass percentage, the content of olefin A-ethylene copolymer in the sub-surface layer is 40-80%; In the intermediate layer, the content of olefin A-ethylene copolymer is 30-70%.

6. The freeze-stretched film according to claim 1, characterized in that In the middle layer and the sub-inner layer, the polyethylene is at least one of low-density polyethylene and metallocene high-density polyethylene.

7. The freeze-stretched film according to any one of claims 1 to 6, characterized in that The thicknesses of the corona layer, sub-surface layer, middle layer, sub-inner layer and heat-sealing layer are 5%-50%, 10%-50%, 10%-50%, 10%-50% and 5%-50% of the film thickness respectively.

8. The freeze-stretched film according to claim 7, characterized in that The film thickness is 80-160 microns.

9. The freeze-stretched film according to claim 8, characterized in that The film thickness is 100-120 microns.

10. The process for preparing a freeze-stretched film according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Using the preset raw materials, a five-layer composite film is obtained in a five-layer co-extrusion film blowing machine; Among them, the extrusion temperature of the A extruder used for extruding the corona layer is: 160°C in zone 1, 180°C in zone 2, 200°C in zone 3, and 220°C in zone 4; The extrusion temperatures of the B extruder used for extruding the secondary outer layer are: 120°C in zone 1, 160°C in zone 2, 180°C in zone 3, and 190°C in zone 4; The extrusion temperatures of the C extruder used to extrude the middle layer are: 100°C in zone 1, 150°C in zone 2, 180°C in zone 3, and 190°C in zone 4; The extrusion temperatures of the D extruder used for extruding the secondary inner layer are: 110°C in zone 1, 160°C in zone 2, 180°C in zone 3, and 190°C in zone 4; The extrusion temperatures of the E extruder used for extruding the heat seal layer are: 110°C in zone 1, 150°C in zone 2, 170°C in zone 3, and 180°C in zone 4; (2) The five-layer composite film is subjected to thickness measurement, corona treatment, winding, plasticization, cross-linking, and slitting to obtain the freeze-stretched film.

Citation Information

Patent Citations

  • Perforated laminate and its manufacturing method

    CN101267934A

  • Multilayer composite polyolefin lithium ion battery diaphragm and production method thereof

    CN104993085A

  • Polyethylene film, packaging composite film, and making method of packaging composite film

    CN105172290A

  • Polyethylene film and application thereof

    CN109291591A

  • Multi-layer co-extrusion medical plastic suction composite packaging film

    CN110901192A

Cited By

  • Coating type light-conversion high-heat-preservation pinhole mulching film used in greenhouse and preparation method

    CN120439641A