Expansion-joint filling material and preparation method therefor
By using a combination of caulking materials and waterproof protection materials in road expansion joints, the problems of high construction difficulty and poor waterproof performance in the prior art are solved, the temperature adaptability and waterproof performance of the material are improved, and traffic safety and Filling quality.
Patent Information
- Application Number
- PCT/CN2024/092172
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-10
- Publication Date
- 2024-12-05
AI Technical Summary
The existing road expansion joint filling materials are difficult in construction and lack good temperature adaptability and waterproofing performance, resulting in traffic safety hazards and low filling quality.
Using a combination of caulking materials and waterproof protection materials, the caulking materials consist of cement and short steel fibers coated with polyurethane rubber. The waterproof protection materials include modified emulsified asphalt and flocculant. The continuous waterproof layer is formed by spraying to improve the material's Bonding and permeability.
The temperature adaptability and waterproof performance of the expansion joint filling materials are improved, the construction process is simplified, the compressive strength, tensile strain resistance and impact resistance are enhanced, and the traffic safety hazards are reduced.
Smart Images

Figure PCTCN2024092172-FTAPPB-I100001 
Figure PCTCN2024092172-FTAPPB-I100002
Abstract
Description
Expansion joint filling material and preparation method thereof Technical Field
[0001] The present invention relates to the technical field of building construction, and more particularly to an expansion joint filling material and a preparation method thereof. Background Art
[0002] Currently, due to vehicle overload, increased traffic volume, tight road construction deadlines, and insufficient construction quality, the concrete surfaces of road expansion joints have suffered varying degrees of damage. Bridgehead jumping (a phenomenon in which vehicles jump when passing due to differential settlement between the bridgehead and the expansion joint or damage to the expansion joint, resulting in steps in the longitudinal slope of the road surface) is a serious problem, posing a significant safety hazard to traffic safety and congestion. Furthermore, the stress mechanism of road expansion joints is complex, subject to both vertical pressure from vehicles and horizontal impact loads and warping forces caused by temperature differences. Therefore, the filling materials for road expansion joints are required to have high compressive strength, good tensile strain capacity, and good impact and wear resistance. CN101418126A discloses a bridge deck joint filling material and its preparation method. The filling material comprises 70% to 90% propylene deasphalted asphalt, 6% to 15% extracted oil, and 4% to 15% styrene-butadiene-styrene block copolymer, which are uniformly mixed at 170-190°C and a stirring speed of 4000-5000 r / min. The high amount of styrene-butadiene-styrene block copolymer (SBS) in the filler results in a high viscosity, making joint filling difficult.
[0003] Summary of the Invention
[0004] An object of the present invention is to provide an expansion joint filling material and a preparation method thereof. The expansion joint filling material prepared by the preparation method has good temperature adaptability and waterproofness and is easy to construct.
[0005] To achieve these objects and other advantages according to the present invention, according to one aspect of the present invention, the present invention provides an expansion joint filling material, comprising a caulking material and a waterproof protective material, wherein the waterproof protective material is sprayed on top of the caulking material;
[0006] The caulking material contains, by mass: 100 parts of cement, 4 to 8 parts of short steel fibers coated with polyurethane rubber;
[0007] The waterproof protective material contains component A and component B. Component A comprises, by mass, 40 to 60 parts of modified emulsified asphalt and 30 to 50 parts of rubber latex. The modified emulsified asphalt is prepared by emulsifying low-density polyethylene modified asphalt. Component B is a flocculant with a mass concentration of 5 to 25%.
[0008] Preferably, the average length of the short steel fibers is 1 to 3 mm, and the average diameter is 50 to 200 μm.
[0009] Preferably, the weight ratio of component A to component B is 5:1 to 20:1.
[0010] Preferably, the flocculant is an inorganic salt flocculant.
[0011] Preferably, the rubber latex is one or more of carboxylated styrene-butadiene rubber latex, carboxylated nitrile-butadiene rubber latex, and carboxylated chloroprene rubber latex.
[0012] The present invention also provides a method for preparing an expansion joint filling material, comprising the following steps:
[0013] Step 1: Mix polyethylene glycol and diphenylmethane diisocyanate in a mass ratio of 2:1 to 1:1, and stir under heating conditions of 100°C to obtain a mixed solution, stop heating, immerse the short steel fiber in the viscous mixed solution, and vacuum stir for 2 to 4 hours. Take out the short steel fiber coated with the mixed solution, and cure it at 80°C for 2 hours to obtain the short steel fiber coated with polyurethane rubber;
[0014] Step 2: 100 parts of the cement in the caulking material and 4 to 8 parts of the short steel fibers coated with polyurethane rubber obtained above are mixed and stirred uniformly to prepare the caulking material;
[0015] Step 3: blending asphalt with low-density polyethylene at 140-180° C., wherein the amount of low-density polyethylene added is 1%-5% by weight of the asphalt, mixing well, and then subjecting to high-speed shearing to obtain modified asphalt;
[0016] Step 4: Heat water to 55-65°C, add an emulsifier and a stabilizer to prepare a soap solution, heat the modified asphalt to 135-145°C, mix with the soap solution, and emulsify in a high-speed emulsifier for 2-5 minutes to obtain the modified emulsified asphalt, wherein the amount of the emulsifier added is 0.5%-2%, the amount of the stabilizer added is 0.06%-0.2%, and the asphalt content in the modified emulsified asphalt is 38-45%;
[0017] Step 5: 40 to 60 parts of the modified emulsified asphalt and 30 to 50 parts of rubber latex are stirred and mixed uniformly to obtain component A, and a flocculant with a mass concentration of 5 to 25% is prepared to obtain component B.
[0018] Preferably, the emulsifier in step 4 is an anionic emulsifier and the stabilizer is sodium hydroxide.
[0019] The present invention includes at least the following beneficial effects: the expansion joint filling material of the present invention includes a caulking material and a waterproof protective material, the caulking material includes cement and short steel fibers, the short steel fibers are coated with elastic rubber on the periphery, thereby improving the bonding strength between the short steel fibers and the cement, and at the same time improving the deformability of the caulking material; the waterproof protective material includes component A and component B, and during construction and use, component A and component B are sprayed out and mixed at the same time, and then sprayed on the surface of the caulking material to form a continuous waterproof layer, the modified emulsified asphalt used in component A has good permeability and good bonding with the caulking material, thereby effectively improving the waterproof performance.
[0020] Other advantages, objectives and features of the present invention will be reflected in part from the following description and will be understood by those skilled in the art through study and practice of the present invention. DETAILED DESCRIPTION
[0021] The present invention will be further described in detail below in conjunction with specific embodiments so that those skilled in the art can implement the invention with reference to the description.
[0022] It should be understood that terms such as “having”, “including” and “comprising” used herein do not preclude the existence or addition of one or more other elements or combinations thereof.
[0023] It should be noted that the experimental methods described in the following embodiments are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial channels unless otherwise specified.
[0024] Example 1
[0025] An expansion joint filling material, comprising a caulking material and a waterproof protective material, wherein the waterproof protective material is sprayed on top of the caulking material;
[0026] The caulking material contains, by mass: 100 parts of cement, 5 parts of short steel fibers coated with polyurethane rubber;
[0027] The waterproof protective material contains component A and component B. Component A comprises, by mass, 45 parts of modified emulsified asphalt and 38 parts of rubber latex. The modified emulsified asphalt is prepared by emulsifying low-density polyethylene modified asphalt. Component B is a flocculant with a mass concentration of 15%.
[0028] The method for preparing the expansion joint filling material comprises the following steps:
[0029] Step 1: Mix polyethylene glycol and diphenylmethane diisocyanate in a mass ratio of 1.2:1, and stir under heating conditions of 100°C to obtain a mixed solution. Stop heating, immerse the short steel fiber in the viscous mixed solution, and vacuum stir for 3 hours. Take out the short steel fiber coated with the mixed solution, and cure it at 80°C for 2 hours to obtain the short steel fiber coated with polyurethane rubber;
[0030] Step 2: 100 parts of the cement in the caulking material and 5 parts of the short steel fibers coated with polyurethane rubber obtained above are mixed and stirred uniformly to prepare the caulking material;
[0031] Step 3: Asphalt is blended with low-density polyethylene at 150° C., wherein the amount of low-density polyethylene added is 3% of the weight of the asphalt, and the mixture is uniformly mixed and then subjected to high-speed shearing to obtain modified asphalt;
[0032] Step 4: Heat water to 60°C, add an emulsifier and a stabilizer to prepare a soap solution, heat the modified asphalt to 140°C, mix with the soap solution, and emulsify in a high-speed emulsifier for 3 minutes to obtain the modified emulsified asphalt, wherein the amount of the emulsifier added is 1%, the amount of the stabilizer added is 0.1%, and the asphalt content in the modified emulsified asphalt is 40%;
[0033] Step 5: 45 parts of the modified emulsified asphalt and 38 parts of rubber latex are stirred and mixed uniformly to obtain component A, and a flocculant with a mass concentration of 15% is prepared to obtain component B.
[0034] During construction, the prepared caulking material is filled into the expansion joint. After it solidifies and hardens, the components A and B are sprayed out simultaneously using construction equipment. The components A and B are cross-mixed outside the construction equipment and then sprayed on the surface of the caulking material to form a continuous waterproof protective layer, completing the expansion joint filling process.
[0035] Example 2
[0036] An expansion joint filling material, comprising a caulking material and a waterproof protective material, wherein the waterproof protective material is sprayed on top of the caulking material;
[0037] The caulking material contains, by mass: 100 parts of cement, 4 parts of short steel fibers coated with polyurethane rubber;
[0038] The waterproof protective material contains component A and component B. Component A comprises, by mass, 40 parts of modified emulsified asphalt and 30 parts of rubber latex. The modified emulsified asphalt is prepared by emulsifying low-density polyethylene modified asphalt. Component B is a flocculant with a mass concentration of 5%.
[0039] The method for preparing the expansion joint filling material comprises the following steps:
[0040] Step 1: Mix polyethylene glycol and diphenylmethane diisocyanate in a mass ratio of 1:1, and stir under heating conditions of 100°C to obtain a mixed solution, stop heating, immerse the short steel fiber in the viscous mixed solution, and vacuum stir for 2 hours. Take out the short steel fiber coated with the mixed solution, and cure it at 80°C for 2 hours to obtain the short steel fiber coated with polyurethane rubber;
[0041] Step 2: 100 parts of the cement in the caulking material and 4 parts of the short steel fibers coated with polyurethane rubber obtained above are mixed and stirred uniformly to prepare the caulking material;
[0042] Step 3: Asphalt is blended with low-density polyethylene at 140° C., wherein the amount of low-density polyethylene added is 1% of the weight of the asphalt, and the mixture is uniformly mixed and then subjected to high-speed shearing to obtain modified asphalt;
[0043] Step 4: Heat water to 55°C, add an emulsifier and a stabilizer to prepare a soap solution, heat the modified asphalt to 135°C, mix with the soap solution, and emulsify in a high-speed emulsifier for 2 minutes to obtain the modified emulsified asphalt, wherein the amount of the emulsifier added is 0.5%, the amount of the stabilizer added is 0.06%, and the asphalt content in the modified emulsified asphalt is 38%;
[0044] Step 5: 40 parts of the modified emulsified asphalt and 30 parts of rubber latex are stirred and mixed uniformly to obtain component A, and a flocculant with a mass concentration of 5% is prepared to obtain component B.
[0045] Example 3
[0046] An expansion joint filling material, comprising a caulking material and a waterproof protective material, wherein the waterproof protective material is sprayed on top of the caulking material;
[0047] The caulking material contains, by mass: 100 parts of cement, 8 parts of short steel fibers coated with polyurethane rubber;
[0048] The waterproof protective material contains component A and component B. Component A comprises, by mass, 60 parts of modified emulsified asphalt and 50 parts of rubber latex. The modified emulsified asphalt is prepared by emulsifying low-density polyethylene modified asphalt. Component B is a flocculant with a mass concentration of 25%.
[0049] The method for preparing the expansion joint filling material comprises the following steps:
[0050] Step 1: Mix polyethylene glycol and diphenylmethane diisocyanate in a mass ratio of 2:1, and stir under heating conditions of 100°C to obtain a mixed solution, stop heating, immerse the short steel fiber in the viscous mixed solution, and vacuum stir for 4 hours. Take out the short steel fiber coated with the mixed solution, and cure it at 80°C for 2 hours to obtain the short steel fiber coated with polyurethane rubber;
[0051] Step 2: 100 parts of the cement in the caulking material and 8 parts of the short steel fibers coated with polyurethane rubber obtained above are mixed and stirred uniformly to prepare the caulking material;
[0052] Step 3: Asphalt is blended with low-density polyethylene at 180° C., wherein the amount of low-density polyethylene added is 5% of the weight of the asphalt, and the mixture is uniformly mixed and then subjected to high-speed shearing to obtain modified asphalt;
[0053] Step 4: Heat water to 65°C, add an emulsifier and a stabilizer to prepare a soap solution, heat the modified asphalt to 145°C, mix with the soap solution, and emulsify in a high-speed emulsifier for 5 minutes to obtain the modified emulsified asphalt, wherein the amount of the emulsifier added is 2%, the amount of the stabilizer added is 0.2%, and the asphalt content in the modified emulsified asphalt is 45%;
[0054] Step 5: 60 parts of the modified emulsified asphalt and 50 parts of rubber latex are stirred and mixed uniformly to obtain component A, and a flocculant with a mass concentration of 25% is prepared to obtain component B.
[0055] Comparative Example 1
[0056] An expansion joint filling material and a preparation method thereof, which differs from Example 1 in that the modified emulsified asphalt in component A of the waterproof protective material is replaced with ordinary commercially available emulsified asphalt.
[0057] Comparative Example 2
[0058] An expansion joint filling material and a preparation method thereof, which differs from Example 1 in that, in steps 3 and 4 of the preparation method, the asphalt is first emulsified and then modified, specifically:
[0059] Step 3: Heat water to 60°C, add an emulsifier and a stabilizer to prepare a soap solution, heat the asphalt to 140°C, mix with the soap solution, and emulsify in a high-speed emulsifier for 3 minutes to prepare emulsified asphalt, wherein the addition amount of the emulsifier is 1% and the addition amount of the stabilizer is 0.1%;
[0060] Step 4: Take the above-mentioned emulsified asphalt and blend it with low-density polyethylene at 150°C, wherein the addition amount of low-density polyethylene is 3% of the weight of the asphalt. After mixing evenly, high-speed shearing is performed to obtain emulsified modified asphalt, and the asphalt content in the emulsified modified asphalt is 40%.
[0061] Comparative Example 3
[0062] A expansion joint filling material and a preparation method thereof, which differs from Example 1 in that the short steel fibers in the caulking material are commercially available short steel fibers, and their outer surfaces are not coated with polyurethane rubber.
[0063] Comparative Example 4
[0064] An expansion joint filling material and a preparation method thereof, which differ from Example 1 in that no waterproof protective material is included.
[0065] Comparison of the penetration performance of waterproof protection materials to caulking materials
[0066] Take the caulking materials and waterproof protective materials prepared in Examples 1 to 3 and Comparative Examples 1 to 2. After the caulking materials solidify and harden, use construction equipment to spray out component A and component B at the same time. After cross-mixing, component A and component B are sprayed on the surface of the caulking materials outside the construction equipment to form a continuous waterproof protective layer. After all solidification and hardening, the penetration depth is calculated by using the method of taking multiple measurements at multiple points using core sampling and taking the average value. The results are shown in Table 1.
[0067] Table 1
[0068] As shown in Table 1, the penetration depth of the waterproof protective material into the caulking material in Examples 1-3 was greater than that in Comparative Examples 1 and 2. This is because Comparative Example 1 used standard commercially available emulsified asphalt, while Comparative Example 2 used asphalt that was first emulsified and then modified, while Examples 1-3 used asphalt that was first modified and then emulsified. The penetration depth of asphalt is primarily related to the viscosity of the emulsion and the fineness of the particles. The addition of low-density polyethylene in the present invention reduces the viscosity of the asphalt, and the asphalt that is first modified and then emulsified results in more uniform emulsification and smaller emulsion particles, which improves the penetration of the emulsion particles into the gaps of the semi-rigid base layer.
[0069] Comparison of caulking material properties
[0070] Take the caulking materials and waterproof protective materials prepared in Examples 1 to 3 and Comparative Examples 1 to 4. After the caulking materials solidify and harden, use construction equipment to spray out component A and component B at the same time. After the components A and B are cross-mixed outside the construction equipment, they are sprayed on the surface of the caulking materials to form a continuous waterproof protective layer. After all of them solidify and harden, their compressive strength, tensile strength, elongation at break and low-temperature shrinkage are tested respectively. The results are shown in Table 2. Among them, the test methods for tensile strength and elongation at break are carried out in accordance with the standard JT / T327-2004; the tensile strength is carried out in accordance with the cube compressive strength test implementation standard GBJ81-85; the test method for low-temperature shrinkage is to prepare a sample with a size of 10cm×10cm×10cm, immerse the sample in room temperature water for 15 minutes, then take it out and use a wet towel to absorb the water attached to the surface, put it in a refrigerator at -20℃ for 16 hours, and immediately test the three-dimensional geometric dimensions of the sample after taking it out, calculate the volume and compare it with the original volume, and the ratio of the shrunken volume to the original volume is the low-temperature shrinkage rate.
[0071] Table 2
[0072] As can be seen from Table 2, the caulking material in the expansion joint filling material of the present invention has better compressive strength, tensile strength and elongation at break than Comparative Examples 1 to 4 after solidification and hardening. This is because the ordinary commercially available emulsified asphalt and the asphalt that is first emulsified and then modified used in Comparative Examples 1 and 2 have poor permeability, which makes the bonding between the waterproof protective material and the caulking material poor, and thus leads to poor overall performance; the short steel fiber directly added to the cement in Comparative Example 3 has poor bonding with the cement base and lacks the effect of polyurethane rubber, resulting in poor tensile strength and elongation at break of the material; there is no waterproof protective material in Comparative Example 4, resulting in poor waterproof performance of the expansion joint filling material, and the simple caulking material has poor tensile strength, elongation at break, and poor temperature adaptability.
[0073] In Examples 1 to 3 of the present invention, the waterproof protective material used has good thixotropy and can be covered on the surface of the caulking material to achieve a waterproof effect. Even if it is slightly broken, it will expand by itself to block the broken parts to avoid serious damage. When a larger range of defects occurs, it can also be re-sprayed at any time to achieve the purpose of timely repairing the expansion joint.
[0074] Although the embodiments of the present invention have been disclosed above, they are not limited to the applications listed in the description and implementation methods. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and embodiments shown and described herein.
Claims
1. Expansion joint filling material, characterized in that: It includes caulking material and waterproof protection material, wherein the waterproof protection material is sprayed on the top of the caulking material; The caulking material contains, by mass: 100 parts of cement, 4 to 8 parts of short steel fibers coated with polyurethane rubber; The waterproof protective material contains component A and component B. Component A includes, by mass, 40 to 60 parts of modified emulsified asphalt and 30 to 50 parts of rubber latex. The modified emulsified asphalt is prepared by emulsifying low-density polyethylene modified asphalt. Component B is a flocculant with a mass concentration of 5 to 25%.
2. The expansion joint filling material according to claim 1, characterized in that: The average length of the short steel fibers is 1 to 3 mm, and the average diameter is 50 to 200 μm.
3. The expansion joint filling material according to claim 1, characterized in that: The weight ratio of the component A to the component B is 5:1 to 20:
1.
4. The expansion joint filling material according to claim 1, characterized in that: The flocculant is an inorganic salt flocculant.
5. The expansion joint filling material according to claim 1, characterized in that: The rubber latex is one or more of carboxylated styrene-butadiene rubber latex, carboxylated nitrile-butadiene rubber latex, and carboxylated chloroprene rubber latex.
6. The method for preparing the expansion joint filling material according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1, polyethylene glycol and diphenylmethane diisocyanate are mixed in a mass ratio of 2:1 to 1:1, and stirred under heating conditions of 100°C to obtain a mixed solution, the heating is stopped, the short steel fiber is immersed in the viscous mixed solution, and vacuum stirred for 2 to 4 hours, the short steel fiber coated with the mixed solution is taken out, and cured at 80°C for 2 hours to obtain the short steel fiber coated with polyurethane rubber; Step 2: 100 parts of cement in the caulking material and 4 to 8 parts of the short steel fibers coated with polyurethane rubber obtained above are mixed and stirred evenly to obtain the caulking material; Step 3: blending asphalt with low-density polyethylene at 140-180° C., wherein the amount of low-density polyethylene added is 1%-5% of the weight of the asphalt, and mixing well and subjecting to high-speed shearing to obtain modified asphalt; Step 4: Heat water to 55-65°C, add emulsifier and stabilizer to prepare soap solution, heat the modified asphalt to 135-145°C, mix with the soap solution, and emulsify in a high-speed emulsifier for 2-5 minutes. The modified emulsified asphalt is obtained, wherein the addition amount of the emulsifier is 0.5% to 2%, the addition amount of the stabilizer is 0.06% to 0.2%, and the asphalt content in the modified emulsified asphalt is 38% to 45%; Step 5: 40 to 60 parts of the modified emulsified asphalt and 30 to 50 parts of rubber latex are stirred and mixed uniformly to obtain component A, and a flocculant with a mass concentration of 5 to 25% is prepared to obtain component B.
7. The method for preparing the expansion joint filling material according to claim 4, characterized in that: The emulsifier in step 4 is an anionic emulsifier, and the stabilizer is sodium hydroxide.
Citation Information
Patent Citations
Polyolefin hybrid asphalt with stable thermal storage and preparation method thereof
CN102604397A
Rubber modified asphalt waterproof coating as well as preparation method and use method thereof
CN107118695A
Concrete for casting of modified steel fiber enhanced bridge
CN107721327A
Steel fiber capable of being used for restoring building concrete micro cracks and preparation method thereof
CN108395131A
High-load adjustable anti-sedimentation intelligent well lid and construction method thereof
CN114351768A
Cited By
Bridge expansion joint filling material and preparation method thereof
CN117682810A