Gradient silicone thin film and preparation method therefor
Through the polymerization of two-component silicone rubber thin layer, the problem of low damping performance of silicone rubber is solved, and efficient and uniform gradient material production is achieved, and the damping performance and production efficiency are improved.
Patent Information
- Application Number
- PCT/CN2024/094874
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Silicone rubber has low damping performance in speakers and is difficult to meet performance requirements. Traditional gradient material formation methods are time-consuming and the materials are uneven.
Using two-component silicone rubber, a material with gradient changes in thickness direction is formed by thin layer polymerization. Components A and component B contain silicone matrix components, fillers, catalysts and crosslinking agents, respectively, and are formed by laminating each other or spraying each other. Gradient silicone films achieve gradient changes in mechanical properties.
The damping performance of the material is improved, production time and investment are reduced, and the polymer formed has a macro gradient and the center changes to both sides, avoiding the phase separation problem caused by the introduction of heterogeneous elements, and is suitable for high transmittance places.
Smart Images

Figure CN2024094874_05122024_PF_FP_ABST
Abstract
Description
A gradient organic silicon film and preparation method thereof Technical Field
[0001] The invention belongs to the field of membrane technology, and in particular relates to a gradient organic silicon film and a preparation method thereof. Background Art
[0002] Loudspeaker films usually require good damping properties. Generally speaking, such films are divided into two categories: single-layer films and composite films. For single-layer films, it is often necessary to improve various performances at the same time to match the requirements, and the performance of each part of the film material is uniform; for composite films, excellent performance is usually achieved by superimposing advantageous performances. It consists of two parts: a support layer and a functional layer. The two parts can be stacked once or multiple times to form a multi-layer composite structure to meet the performance requirements of the loudspeaker. Silicone rubber is used in diaphragms, usually in the form of a single-layer film, which places high demands on the various properties of silicone rubber. However, the damping of silicone rubber is very low, which is a fatal flaw when it is used.
[0003] Gradient materials can be formed in a variety of ways, such as stacking, diffusion, and lamination. Diffusion is a common method for two-dimensional gradient materials. Typically, one or more substances are infiltrated into the bulk material through methods such as immersion-swelling, coating, and steam permeation, forming a concentration gradient. Subsequent methods (such as cross-linking polymerization) then form the gradient material. This method typically requires determining the concentration gradient based on the infiltration time, which is often time-consuming. The resulting material often has a high surface concentration and a low middle concentration, or a high concentration on one side and a low concentration on the other.
[0004] In addition, gradient materials can be formed using electric or magnetic fields. Driven by the electric or magnetic field, certain substances in the material are enriched on one side, resulting in a gradient material with high concentration on one side and low concentration on the other. In some cases, it is also possible to form a gradient material with high concentration on two sides (but different substances on each side) and low concentration in the middle (where there is little concentration of both substances in the middle).
[0005] Another approach is to form gradient materials during the polymerization stage through chemical polymerization, such as graft polymerization and block polymerization. Alternatively, gradient polymers can be formed by interfacial polymerization at the interface between droplets and solvents, similar to emulsion and suspension polymerization. These gradient polymers are often used in two broad directions: a) Direct use. When used directly, these materials are uniform macroscopically and exhibit gradient variations microscopically. Their properties are similar to those of uniform materials, but they offer the advantage of broadening the performance range. b) Self-assembly is often used in scenarios involving multi-block polymers. In such applications, it is difficult to form materials with a certain thickness (tens to hundreds of microns). These polymers are typically used as templates and surface modifiers to enhance the compatibility of different materials.
[0006] In addition, chemical polymerization, such as grafting and block polymerization, often uses different monomers as raw materials to polymerize into polymers composed of different materials, such as PMMA-g-PS (grafting) and PMMA-b-PS (block). The same material will not form such polymers.
[0007] Summary of the Invention
[0008] In order to solve the above problems, the purpose of the present invention is to provide a gradient organic silicon film and a preparation method thereof. The gradient organic silicon film prepared by this preparation method forms a characteristic of gradient change of mechanical properties in the thickness direction, which is of great value in improving the damping of the material.
[0009] In order to achieve the above object, the present invention provides a method for preparing a gradient organic silicon film, which comprises the following steps:
[0010] (1) preparing component A and component B, wherein component A comprises an organosilicon matrix component, a filler, and a catalyst; and component B comprises an organosilicon matrix component, a filler, a crosslinking agent, and an inhibitor;
[0011] (2) preparing the components A and B into thin layers A and B respectively, so that the thin layers A and B are spaced apart and laminated to each other, and the number of the thin layers A and B is ≥1, and curing to obtain the gradient organic silicone film. The specific lamination forms of the "spaced apart and laminated to each other" can be AB, ABAB..., BABAB..., etc.; or,
[0012] Component A and component B are sprayed alternately in a spraying manner, and after curing, the gradient organic silicon film is formed.
[0013] According to a specific embodiment of the present invention, preferably, the viscosity of component A and component B is 100-2000 Pa·s, more preferably 300-1500 Pa·s, and further preferably 600-1200 Pa·s respectively; too low a viscosity will make it difficult to form a good gradient structure after bonding and curing; too high a viscosity requires more precise film thickness control to achieve a gradient structure, which is relatively high in investment and slightly low in efficiency.
[0014] According to a specific embodiment of the present invention, preferably, based on the mass of component A being 100%, the mass fraction of the organosilicon matrix component in component A is 50-95wt%; based on the mass of component B being 100%, the mass fraction of the organosilicon matrix component in component B is 50-95wt%.
[0015] According to a specific embodiment of the present invention, preferably, the mass fraction of the organosilicon matrix component in component A is the same as the mass fraction of the organosilicon matrix component in component B.
[0016] According to a specific embodiment of the present invention, preferably, the organosilicon matrix component in component A is the same as the organosilicon matrix component in component B.
[0017] According to a specific embodiment of the present invention, preferably, the organic silicon matrix component comprises an organic siloxane polymer having terminal double bonds.
[0018] According to a specific embodiment of the present invention, preferably, the organosiloxane polymer with terminal double bonds is selected from:
[0019] One or a combination of two or more, wherein X, Y, and Z are 1-1000 respectively.
[0020] According to a specific embodiment of the present invention, preferably, the molecular weight of the organosiloxane polymer with terminal double bonds is 5,000-200,000 g / mol, more preferably 10,000-150,000 g / mol, and further preferably 15,000-100,000 g / mol.
[0021] According to a specific embodiment of the present invention, preferably, based on the mass of component A being 100%, the mass fraction of the filler in component A is 0-50 wt%; based on the mass of component B being 100%, the mass fraction of the filler in component B is 0-50 wt%.
[0022] According to a specific embodiment of the present invention, preferably, the mass fraction of the filler in component A is the same as the mass fraction of the filler in component B.
[0023] According to a specific embodiment of the present invention, preferably, the filler in component A is the same as the filler in component B.
[0024] According to a specific embodiment of the present invention, preferably, the filler includes one or a combination of two or more of precipitated silica, fumed silica, carbon black, activated calcium carbonate, quartz powder, diatomaceous earth, titanium dioxide, and MQ silicone resin.
[0025] According to a specific embodiment of the present invention, preferably, in component A, the content of the catalyst calculated as Pt equivalent is 10-1000 ppm.
[0026] According to a specific embodiment of the present invention, preferably, the catalyst comprises a Pt complex.
[0027] According to a specific embodiment of the present invention, preferably, the catalyst includes one or a combination of two or more of a platinum-vinylsiloxane complex and an improved product thereof, an alcohol-modified chloroplatinic acid catalyst, a platinum-alkyne complex, trimethyl(methyl-cyclopentadienyl)platinum ((Me-Cp)PtMe3(Ⅳ)), acetylacetonate platinum (Pt(caca)2(Ⅱ)), cis-dichlorobis(triphenylphosphine)platinum (cis-Cl2(Ph3P)2Pt(Ⅱ)), dichlorodicyclopentadieneplatinum (Cl2Cp2Pt(Ⅱ)), and 1,5-cyclooctadiene dichloroplatinum (Cl2(1,5-COD)Pt(Ⅱ)).
[0028] According to a specific embodiment of the present invention, preferably, the platinum-vinylsiloxane complex and its improved product include a complex of platinum and 1,3-divinyltetramethyldisiloxane (i.e., platinum-tetramethyldivinyldisiloxane complex) and / or a complex of platinum and 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane.
[0029] According to a specific embodiment of the present invention, preferably, the alcohol-modified chloroplatinic acid catalyst includes an octanol-modified chloroplatinic acid catalyst and / or an ethanol-modified chloroplatinic acid catalyst.
[0030] According to a specific embodiment of the present invention, preferably, the platinum-alkyne-based complex comprises a bis(alkynyl)bis(triphenylphosphine)platinum complex and / or a bis(alkynyl)(cyclodiene)platinum complex.
[0031] According to a specific embodiment of the present invention, preferably, in component B, the mass fraction of the crosslinking agent is 0.5-10 wt%.
[0032] According to a specific embodiment of the present invention, preferably, the cross-linking agent includes hydrogen-containing silicone oil.
[0033] According to a specific embodiment of the present invention, preferably, the cross-linking agent is selected from
[0034] wherein m, n, and p are respectively 0-100, and the value of m+n+p is 1-300, preferably 3-200, and more preferably 5-150; and R is -CH3 or H.
[0035] According to a specific embodiment of the present invention, preferably, in component B, the mass fraction of the inhibitor is 0.01-1 wt %.
[0036] According to a specific embodiment of the present invention, preferably, the inhibitor comprises one or a combination of two or more of acetylenic alcohol compounds, polyvinyl polysiloxane, amide compounds, and maleate compounds.
[0037] When configuring component A and component B, other ingredients can be added according to actual needs. According to a specific embodiment of the present invention, preferably, a dye is added according to color requirements, a photosensitizer is added according to catalyst requirements, a silane coupling agent and a thickener are added according to bonding requirements, and tetramethyltetravinylcyclotetrasiloxane (V4), a linear organosiloxane, a carbon-nitrogen unsaturated bond six-membered ring compound, etc. are added according to performance requirements, wherein the end group of the linear organosiloxane includes a hydroxyl group, the degree of polymerization is small, and the repeating unit is ≤50.
[0038] According to a specific embodiment of the present invention, preferably, based on the weight of component A or component B being 100%, the added amount of the other ingredients is ≤1 wt%.
[0039] According to a specific embodiment of the present invention, preferably, in step (2), the curing method is thermal curing, photocuring or photothermal mixed curing, depending on the type of catalyst.
[0040] According to a specific embodiment of the present invention, preferably, the temperature of the thermal curing is 120-150°C.
[0041] According to a specific embodiment of the present invention, preferably, the curing time is 30-600s.
[0042] According to a specific embodiment of the present invention, the lamination of thin layer A and thin layer B (or component A and component B) can be single or multiple times, and there is no particular restriction on whether the outermost layer is thin layer A or thin layer B; as shown in Figure 1, wherein the depth after curing represents the degree of curing.
[0043] The present invention also provides a gradient organic silicon film prepared by the above preparation method.
[0044] According to a specific embodiment of the present invention, preferably, the thickness of a single thin layer A or a single thin layer B in the gradient organic silicon film is 1-1000 μm, more preferably 5-500 μm, and further preferably 10-100 μm.
[0045] According to a specific embodiment of the present invention, preferably, the thicknesses of the single thin layer A and the single thin layer B are similar, and more preferably, the thickness difference is ≤5 μm.
[0046] The present invention also provides application of the gradient organic silicon film in a loudspeaker.
[0047] The present invention adopts two-component organic silicone rubber to form a material with thickness gradient change by thin layer polymerization: component A and component B are made into thin layers with a thickness of 1-1000 μm, and compounded and cured as needed. Since the catalyst and curing agent of the two-component silicone rubber are respectively in component A and component B, they can be well cured after contact. Therefore, the degree of curing is relatively high at the interface contact and the mechanical properties are relatively strong; the degree of curing is relatively low away from the contact position and the mechanical properties are relatively weak, thereby forming a characteristic of mechanical property gradient change in the thickness direction, which has great value in improving material damping. The preparation method of the present invention forms an internal fine structure adjustment through its own chemical reaction without changing the material composition, and the thickness gradient change characteristic formed is close to the performance of homogeneous silicone in tensile deformation, but in deformation involving thickness slip such as shear or bending, it shows obvious damping excellence, which has great advantages for low damping materials such as silicone.
[0048] The present invention has the following beneficial effects:
[0049] (1) In the present invention, components A and B are laminated with film materials, and are directly cured after the rollers are exhausted (or other laminating methods are used). There is no need for waiting time or additional means to control input, and continuous production is possible. Compared with traditional diffusion methods and electromagnetic field methods, the method is more efficient and requires less input.
[0050] (2) In the present invention, the polymer formed is the same polymer, which is essentially different from the use of grafting, blocking, modification and other methods to introduce different groups to achieve performance improvement. There will be no problems such as phase separation and poor uniformity caused by the introduction of heterogeneous elements. It is also applicable to places where uniform material is required, such as high transmittance.
[0051] (3) The gradient material formed in the present invention is a macroscopic gradient, and the gradient changes from the center to the two sides. This is significantly different from the gradient material formed by the conventional diffusion method. The gradient material obtained by the conventional concentration gradient method as shown in Figure 2 has a high concentration on the surface and a low concentration in the middle, or a high concentration on one side and a low concentration on the other side.
[0052] (4) In the present invention, the improvement of damping performance is not the expansion of the damping range (including frequency range and / or temperature range), but the improvement of the damping value, which is significantly different from the macroscopic uniform and microscopic gradient structure of microphase separation. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] FIG1 is a schematic diagram of the lamination and curing of the gradient organosilicon film of the present invention;
[0054] FIG2 is a schematic diagram of a gradient material prepared by a conventional concentration gradient method;
[0055] FIG3 is a schematic diagram showing the gradient change of the cross-linking degree of the cured organic silicone film in the thickness direction;
[0056] Figure 4 is a schematic diagram of film bending mode, stretching mode and shear mode;
[0057] Figure 5 is a diagram of shear test results;
[0058] Figure 6 shows the tensile test results. DETAILED DESCRIPTION
[0059] In order to have a clearer understanding of the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be understood as limiting the scope of implementation of the present invention.
[0060] Example 1
[0061] This embodiment provides a gradient organic silicon film, which is prepared by the following steps:
[0062] Components A and B were each made into 75 μm thick adhesive layers. After bonding, the two were cured at 120°C for 10 minutes and then removed to produce a gradient silicone monolayer film with a thickness of 150 μm. The test results are shown in Figures 5 and 6.
[0063] Component A comprises: 75 wt% of a mixture of organosilicon matrix components (a) and (b) in a mass ratio of 9:1 (wherein the organosilicon matrix component (a) has a molecular weight of approximately 30,000 g / mol and a vinyl content of 0.07 mol / kg; the organosilicon matrix component (b) has a molecular weight of approximately 10,000 g / mol and a vinyl content of 0.89 mol / kg), 25 wt% of fumed silica filler, and 100 ppm of platinum-tetramethyldivinyldisiloxane complex;
[0064] Component B is composed of: 73.9 wt% of a mixture of silicone matrix components (a) and (b) (same as component A), 25 wt% of fumed silica filler, 1 wt% of a crosslinker (C) (wherein R = H, m = 1, n ≈ 31), and 0.1 wt% of an acetylene alcohol inhibitor. Its structure is:
[0065] Example 2
[0066] This embodiment provides a gradient organic silicon film, which is prepared by the following steps:
[0067] Component A was made into three adhesive layers A1, A2, and A3 with thicknesses of 20 μm, 25 μm, and 30 μm, and component B was made into three adhesive layers B1, B2, and B3 with thicknesses of 20 μm, 25 μm, and 30 μm, respectively. They were bonded in the order of A1, B1, A2, B2, A3, and B3, with a final thickness of 150 μm. After curing at 150°C for 1 min, a gradient silicone film was obtained.
[0068] Component A comprises: 80 wt% of a mixture of silicone matrix components (a), (b), and (e) in a mass ratio of 9:0.5:0.5 (silicone matrix components (a) and (b) are the same as in Example 1; silicone matrix component (e) has a molecular weight of approximately 3000 g / mol, a vinyl content of approximately 0.18 mol / kg, and a phenyl content of approximately 13 wt%), 20 wt% of fumed silica filler, and 100 ppm of a platinum-tetramethyldivinyldisiloxane complex. An additional 1 wt% of tetramethyltetravinylcyclotetrasiloxane additive is added.
[0069] The composition of component B is: 78.9wt% of a mixture of silicone matrix components (a), (b), and (e) (same as component A), 20wt% of fumed silica filler, 1wt% of a crosslinker (D) (wherein R=1, m≈1, n≈31, p≈1), and 0.1wt% of an acetylene alcohol inhibitor (same as Example 1).
[0070] In this silicone diaphragm, the introduction of tetramethyltetravinylcyclotetrasiloxane improves its modulus and hardness. The addition of the silicone matrix component (e) ensures that the damping will not decrease significantly due to the increase in modulus and hardness. The damping factor at 1% strain reaches 0.101, and the damping factor at 10% strain reaches 0.130.
[0071] Example 3
[0072] This embodiment provides a gradient organic silicon film, which is prepared by the following steps:
[0073] Component A and component B are coated on the surface of the TPEE film respectively to form two thin layers with a thickness of about 10 μm. After the two layers are bonded together, they are compression molded at 150°C to produce a speaker diaphragm (gradient silicone film), forming a three-layer structure of TPEE-silicone-TPEE.
[0074] Component A is composed of: 75 wt% of a mixture of the silicone matrix components (a), (b), and (e) (the composition is the same as in Example 2), 20 wt% of fumed silica filler, 5 wt% of MQ resin, 100 ppm of a platinum-tetramethyldivinyldisiloxane complex, and an additional silane coupling agent of 1 wt% of γ-methacryloxypropyltrimethoxysilane for a total weight after mixing.
[0075] The composition of component B is: 74.9wt% of a mixture of silicone matrix components (a), (b), and (e) (same as component A), 20wt% of fumed silica filler, 4wt% of MQ resin, 1wt% of a crosslinker (D) (wherein R=1, m≈1, n≈31, p≈1), and 0.1wt% of an acetylene alcohol inhibitor (same as Example 1).
[0076] In this embodiment, a silane coupling agent is introduced to improve the bonding strength between the silicone diaphragm and TPEE. The introduction of the silicone matrix component (e) further improves the damping: the damping factor at 1% strain reaches 0.119, and the damping factor at 10% strain reaches 0.332.
[0077] Example 4
[0078] This embodiment provides a gradient organic silicon film, which is prepared by the following steps:
[0079] Component A and component B were sprayed on the surface of the PEEK film to form two thin layers of about 10 μm thick. The two layers were bonded together and compression molded at 150° C. to produce a speaker diaphragm (gradient silicone film) to form a PEEK-silicone-PEEK three-layer structure.
[0080] Component A comprises: 80 wt% of a mixture of silicone matrix components (a), (b), and (f) in a mass ratio of 9:0.5:0.5 (silicone matrix components (a) and (b) are the same as in Example 1; silicone matrix component (f) has a molecular weight of approximately 2000 g / mol, a vinyl content of approximately 0.2 mol / kg, and a phenyl content of approximately 18 wt%), 20 wt% of fumed silica filler, and 100 ppm of a platinum-tetramethyldivinyldisiloxane complex. A silane coupling agent is additionally added, comprising 1 wt% of γ-methacryloxypropyltrimethoxysilane for a total weight of the mixture.
[0081] The composition of component B is: 78.9wt% of a mixture of silicone matrix components (a), (b), and (f) (same as component A), 20wt% of fumed silica filler, 1wt% of a crosslinker (D) (wherein R=1, m≈1, n≈31, p≈1), and 0.1wt% of an acetylene alcohol inhibitor (same as Example 1).
[0082] In this embodiment, the introduction of a silane coupling agent improves the bonding strength between the silicone diaphragm and PEEK. The introduction of the silicone matrix component (f) further improves the damping: the damping factor at 1% strain reaches 0.102, and the damping factor at 10% strain reaches 0.232.
[0083] Example 5
[0084] This embodiment provides a spray-coated gradient organic silicon film, which is prepared by the following steps:
[0085] On the speaker diaphragm mold (or other mold surface that needs to be prepared), a spray molding scheme is adopted to alternately spray component A and component B. The thickness of a single spray is 5-20μm, and the final thickness is 100μm. After UV curing, a silicone diaphragm (or other diaphragm) is formed.
[0086] Component A comprises: 80 wt% of a mixture of the organosilicon matrix components (a), (b), and (f) (same as in Example 4), 20 wt% of fumed silica filler, and 400 ppm of trimethyl(methyl-cyclopentadienyl)platinum. An additional 1 wt% of a linear organic siloxane (hydroxyl-terminated, with a double bond in the side chain) additive is added, based on the total weight of the mixture. The structure is as follows:
[0087] where k≈15;
[0088] The composition of component B is: 78.9wt% of a mixture of silicone matrix components (a), (b), and (f) (same as component A), 20wt% of fumed silica filler, 1wt% of a crosslinker (D) (wherein R=1, m≈1, n≈31, p≈1), and 0.1wt% of N,N,N',N'-tetraallyl terephthalamide as an inhibitor.
[0089] In this embodiment, linear organic siloxane is introduced as an additive to improve the fatigue resistance of the organosilicon membrane, and the introduction of the organosilicon matrix component (f) further improves the damping; photocatalytic organic platinum is used to directly form the organosilicon membrane under light curing.
[0090] The damping factor of the diaphragm reaches 0.102 at 1% strain and 0.135 at 10% strain.
[0091] Comparative Example 1
[0092] This comparative example provides an organosilicon film, which is prepared by the following steps:
[0093] After fully mixing component A and component B, the mixture was pressed into a 150 μm thick adhesive layer, cured at 120° C. for 10 min, and then taken out to prepare a uniform organosilicon single-layer film.
[0094] Component A and component B are the same as in Example 1. The test results are shown in Figures 5 and 6.
[0095] Comparative Example 2
[0096] This comparative example attempts to prepare a gradient silicone film using a low viscosity composition:
[0097] Component A comprises: 90 wt% of an organosilicon matrix component (a) (wherein the organosilicon matrix component (a) has a molecular weight of approximately 10,000 g / mol and a vinyl content of 0.54 mol / kg), 10 wt% of fumed silica filler, and 100 ppm of a platinum-tetramethyldivinyldisiloxane complex;
[0098] The composition of component B is: 88.9wt% silicone matrix component (a) (same as component A), 10wt% fumed silica filler, 1wt% crosslinker (C) (wherein R=H, m=1, n≈31), and 0.1wt% acetylene alcohol inhibitor (same as Example 1).
[0099] The viscosity of components A and B was approximately 90 Pa·s. When the two components were formed into a film, significant flow occurred, making it difficult to control the adhesion and establish effective curing conditions, resulting in failure to form a film.
[0100] Comparative Example 3
[0101] This comparative example attempts to prepare a gradient silicone film using a high viscosity composition:
[0102] Component A is composed of: 65 wt% of an organosilicon matrix component (a) (wherein the organosilicon matrix component (a) is a mixture of low and high molecular weight materials in a mass ratio of 9:1: the low molecular weight organosilicon matrix component (a) has a molecular weight of approximately 30,000 g / mol and a vinyl content of 0.07 mol / kg; the high molecular weight organosilicon matrix component (a) has a molecular weight of approximately 600,000 g / mol and a vinyl content of 0.009 mol / kg), 35 wt% of fumed silica filler, and 100 ppm of a platinum-tetramethyldivinyldisiloxane complex;
[0103] The composition of component B is: 63.9wt% silicone matrix component (a) (same as component A), 35wt% fumed silica filler, 1wt% crosslinker (C) (wherein R=H, m=1, n≈31), and 0.1wt% acetylene alcohol inhibitor (same as Example 1).
[0104] Components A and B have a viscosity of approximately 2300 Pa·s. When the two components were bonded together and cured at 120°C for 10 minutes, the surfaces of the two adhesives were not fully cured, exhibiting cohesive failure, and no silicone film was obtained.
[0105] Performance Testing
[0106] The double-layer composite of component A and component B shows a gradient change in the degree of crosslinking in the thickness direction of the cured silicone film, as shown in Figure 3 (the depth represents the degree of curing). This makes its performance similar to that of a uniformly cross-linked material when subjected to a tensile force perpendicular to the thickness direction; and it exhibits a significant damping effect under bending and shearing.
[0107] Since the bending mode of the film is difficult to measure, and the bending mode can be qualitatively regarded as a complex superposition of tension and shear, as shown in FIG4 , the performance of the tension and shear modes was tested. The test results of Example 1 and Comparative Example 1 are shown in FIG5 and FIG6 . The test method is as follows:
[0108] Test instrument: DMA Q850
[0109] Test method: strain sweep test, 20 points per order of magnitude;
[0110] Strain range: 0.1%-10%;
[0111] Test frequency: 1Hz;
[0112] Test temperature: 25℃;
[0113] Test mode: tensile mode, sandwich shear mode.
[0114] As can be seen from the test results of Figures 5 and 6, in the tensile test, the performance of Example 1 (gradient change) and Comparative Example 1 (uniform) are basically the same; in the shear test, the modulus changes of Example 1 and the comparative example are basically the same, but the damping performance of Example 1 is significantly better than that of the comparative example.
Claims
1. A method for preparing a gradient organic silicon film, wherein The following steps are involved: (1) preparing component A and component B, wherein component A comprises an organic silicon matrix component, a filler, and a catalyst; and component B comprises an organic silicon matrix component, a filler, a crosslinking agent, and an inhibitor; (2) preparing the component A and the component B into thin layers A and B respectively, so that the thin layers A and B are spaced and attached to each other, and the number of the thin layers A and B is ≥ 1 respectively, and curing to obtain the gradient organic silicon film; or, The component A and the component B are sprayed alternately in a spraying manner, and after curing, the gradient organic silicon film is formed.
2. The preparation method according to claim 1, in, The viscosity of the component A and the component B is 100-2000 Pa·s respectively.
3. The preparation method according to claim 2, in, The viscosities of component A and component B are 300-1500 Pa·s respectively.
4. The preparation method according to claim 3, in, The viscosities of component A and component B are 600-1200 Pa·s respectively.
5. The preparation method according to claim 1, in, Taking the mass of component A as 100%, the mass fraction of the organic silicon matrix component in component A is 50-95wt%; taking the mass of component B as 100%, the mass fraction of the organic silicon matrix component in component B is 50-95wt%.
6. The preparation method according to claim 5, in, The mass fraction of the organosilicon matrix component in the component A is the same as the mass fraction of the organosilicon matrix component in the component B.
7. The preparation method according to claim 5, in, The organic silicon matrix component in the component A is the same as the organic silicon matrix component in the component B.
8. The preparation method according to claim 5, in, The organic silicon matrix component comprises an organic siloxane polymer having terminal double bonds.
9. The preparation method according to claim 8, in, The organosiloxane polymer with terminal double bonds is selected from: One or a combination of two or more of , wherein X, Y, and Z are 1-1000 respectively.
10. The preparation method according to claim 8, in, The molecular weight of the organosiloxane polymer with terminal double bonds is 5000-200000 g / mol.
11. The preparation method according to claim 10, in, The molecular weight of the organosiloxane polymer with terminal double bonds is 10000-150000 g / mol.
12. The preparation method according to claim 11, in, The molecular weight of the organosiloxane polymer with terminal double bonds is 15000 to 100000 g / mol.
13. The preparation method according to claim 1, in, Taking the mass of component A as 100%, the mass fraction of the filler in component A is 0-50wt%; taking the mass of component B as 100%, the mass fraction of the filler in component B is 0-50wt%.
14. The preparation method according to claim 13, in, The mass fraction of the filler in component A is the same as the mass fraction of the filler in component B.
15. The preparation method according to claim 13, in, The filler in component A is the same as the filler in component B.
16. The preparation method according to claim 13, in, The filler includes one or a combination of two or more of precipitated silica, fumed silica, carbon black, activated calcium carbonate, quartz powder, diatomaceous earth, titanium dioxide, and MQ silicone resin.
17. The preparation method according to claim 1, in, In component A, the content of the catalyst calculated as Pt equivalent is 10-1000 ppm.
18. The preparation method according to claim 1, in, The catalyst includes a Pt complex.
19. The preparation method according to claim 18, in, The catalyst includes one or a combination of two or more of a platinum-vinylsiloxane complex and an improved product thereof, an alcohol-modified chloroplatinic acid catalyst, a platinum-alkyne-based complex, trimethyl(methyl-cyclopentadienyl)platinum, platinum acetylacetonate, cis-dichlorobis(triphenylphosphine)platinum, dichlorodicyclopentadieneplatinum, and 1,5-cyclooctadiene dichloroplatinum.
20. The preparation method according to claim 19, in, The platinum-vinylsiloxane complex and its improved product include a complex of platinum and 1,3-divinyltetramethyldisiloxane and / or a complex of platinum and 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane.
21. The preparation method according to claim 19, in, The alcohol-modified chloroplatinic acid catalyst includes an octanol-modified chloroplatinic acid catalyst and / or an ethanol-modified chloroplatinic acid catalyst.
22. The preparation method according to claim 19, in, The platinum-alkyne-based complex includes a bis(alkynyl)bis(triphenylphosphine)platinum complex and / or a bis(alkynyl)(cyclodiene)platinum complex.
23. The preparation method according to claim 1, in, In component B, the mass fraction of the crosslinking agent is 0.5-10wt%.
24. The preparation method according to claim 1, in, The crosslinking agent includes hydrogen-containing silicone oil.
25. The preparation method according to claim 1, in, The cross-linking agent is selected from Wherein, m, n, and p are 0-100 respectively, and the value of m+n+p is 1-300; R is -CH 3 or H.
26. The preparation method according to claim 25, in, The value of m+n+p is 3-200.
27. The preparation method according to claim 25, in, The value of m+n+p is 5-150.
28. The preparation method according to claim 1, in, In component B, the mass fraction of the inhibitor is 0.01-1 wt %.
29. The preparation method according to claim 1, in, The inhibitor comprises one or a combination of two or more of acetylenic alcohol compounds, polyvinyl polysiloxane, amide compounds and maleate compounds.
30. The preparation method according to claim 1, in, The component A and / or component B further include other ingredients, which include one or a combination of two or more of a dye, a photosensitizer, a silane coupling agent, a thickener, tetramethyltetravinylcyclotetrasiloxane, a linear organosiloxane, and a carbon-nitrogen unsaturated bond six-membered ring compound, wherein the end group of the linear organosiloxane includes a hydroxyl group, and the repeating unit is ≤50.
31. The preparation method according to claim 30, in, Based on the weight of component A or component B being 100%, the added amount of the other components is ≤1wt%.
32. The preparation method according to claim 1, in, In step (2), the curing method is thermal curing, light curing or light-heat mixed curing.
33. The preparation method according to claim 32, in, The temperature of the thermal curing is 120-150°C.
34. The preparation method according to claim 32, in, The curing time is 30-600s.
35. The gradient organosilicon film obtained by the preparation method of claim 1.
36. The gradient organosilicon film according to claim 35, in, The thickness of a single thin layer A or a single thin layer B in the gradient organic silicon film is 1-1000 μm.
37. The gradient organosilicon film according to claim 35, in, The thickness of a single thin layer A or a single thin layer B in the gradient organic silicon film is 5-500 μm.
38. The gradient organosilicon film according to claim 35, in, The thickness of a single thin layer A or a single thin layer B in the gradient organic silicon film is 10-100 μm.
39. The gradient organosilicon film according to claim 35, in, The difference in thickness between the single thin layer A and the single thin layer B is ≤5 μm.
40. Use of the gradient organic silicon film according to claim 35 in a loudspeaker.
Citation Information
Patent Citations
Reflective organic silicon synthetic leather and preparation method thereof
CN109940930A
Low-viscosity high-strength addition type room-temperature-curable liquid silicone rubber and preparation method thereof
CN110577746A
Organosilicon liquid optical adhesive and preparation method thereof
CN112646543A
Gradient organic silicon film and preparation method thereof
CN116675882A
Definite-form adhesive
JP2005060549A
Cited By
Diaphragm and preparation method therefor, and micro speaker
WO2026178903A1