Method for synthesizing olefin functional polymer in continuous feeding mode and use based on olefin functional polymer

The pressurized reaction between low-carbon gaseous olefins and liquid functional monomers is carried out through continuous feeding, which solves the problems of low efficiency and high cost of synthesis of existing olefin functional polymers, and achieves efficient and environmentally friendly olefin functional polymer production.

WO2024245300A1PCT designated stage expired Publication Date: 2024-12-05JIANGSU YANGNONG CHEMICAL GROUP CO LTD
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/096139
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-19
Filing Date
2024-05-29
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

In the existing olefin functional polymer synthesis methods, especially low-carbon olefins below C4 and functional monomer polymers are low in polymerization efficiency, and traditional methods require a large number of stabilizers, which affects performance, and the polymerized monomer concentration is low, resulting in production efficiency. Not high and costly.

Method used

The pressurized reaction between low-carbon gaseous olefins and liquid functional monomers is carried out by continuous feeding. Through heterogeneous polymerization, the monomer concentration and reaction efficiency are improved, the same-chain alternating copolymerization is achieved, the separation process is simplified, and energy consumption and cost are reduced.

Benefits of technology

The reaction efficiency and product yield of olefin functional polymers are improved, the process flow is simplified, the production cost is reduced, and the recycling and environmental protection effect of raw materials is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024096139_05122024_PF_FP_ABST
    Figure CN2024096139_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Provided in the present application are a method for synthesizing an olefin functional polymer in a continuous feeding mode and the use based on an olefin functional polymer. The method comprises: introducing a light olefin into a reactor, heating and pressurizing same, adding a raw material solution prepared from a functional monomer, an initiator and a solvent to the reactor after the reaction temperature and pressure are reached, and allowing same to undergo a polymerization reaction; and subjecting the reacted system to gas-solid-liquid separation, recovering a light olefin, and subjecting the residual material to solid-liquid separation, so as to obtain an olefin functional polymer and a liquid-phase material. In the present application, the same-chain alternating copolymerization of the gaseous light olefin and the functional monomer is realized by means of a pressurized reaction of the two, the concentration of the monomer and the utilization rate of the raw materials are improved by means of a heterogeneous polymerization mode, olefin functional polymers with different molecular weights are synthesized by adjusting the process parameters, and the reaction efficiency is high; moreover, the post-treatment process is simple, separation and purification are easy, and the solvent and unreacted raw materials can be recycled, such that the conversion rate of the raw materials and the product yield are improved.
Need to check novelty before this filing date? Find Prior Art

Description

A method for synthesizing olefin functional polymers in a continuous feeding manner and uses of olefin functional polymers

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 29, 2023, with application number "202310617195.3" and application name "A method for synthesizing olefin functional polymers by continuous feeding", and the Chinese patent application filed with the Patent Office of China on June 19, 2023, with application number "202310727190.6" and application name "A use based on olefin functional polymers". All contents are incorporated by reference into this application. Technical Field

[0003] The present application relates to the technical field of organic polymerization, and in particular to a method for synthesizing olefin functional polymers in a continuous feeding manner and uses of olefin functional polymers. Background Art

[0004] As functional polymer materials, olefin-functionalized polymers have attracted significant attention for their wide applications in engineering plastic chain extension, high-performance composites, nylon impregnation, ink dispersion, microencapsulation, and filtration membrane formation. Olefin-functionalized polymers contain numerous reactive groups on their molecular chains, which can react with various functional groups, such as the terminal hydroxyl or amino groups of nylon products, to increase molecular weight, enhance mechanical properties, and adjust viscosity. Furthermore, olefin-functionalized polymers can be used in the preparation of microcapsules and hold great promise for applications in pesticides, fragrances, and pharmaceuticals.

[0005] The raw materials for the synthesis of olefin functional polymers are mainly olefins and functional monomers. The currently available polymerization methods include emulsion polymerization, suspension polymerization and precipitation polymerization. The former two require the use of a large amount of stabilizers, which remain on the polymer particles through physical adsorption or chemical adsorption, affecting their performance. Although precipitation polymerization does not require the addition of stabilizers, the concentration of polymerized monomers in the traditional precipitation polymerization system is low, resulting in low polymerization efficiency, and therefore the polymerization method needs to be improved.

[0006] According to the different types of olefins or functional monomers in the olefin functional polymer synthesis raw materials, it is necessary to adopt a corresponding synthesis process. CN101235117A discloses a method for styrene / maleic anhydride copolymerization, which involves dissolving monomers maleic anhydride and styrene, and initiator organic peroxides or azo compounds in a medium under nitrogen protection, and reacting them at 60-90°C for 0.25-12 hours to obtain a dispersion of polymer microspheres. CN102212166A discloses a novel method for the copolymerization of dicyclopentadiene and maleic anhydride, which involves adding monomers and initiators to an organic medium and dissolving them under nitrogen protection, and reacting them at 60-90°C for 2-12 hours to obtain a self-stabilizing dispersion of alternating copolymer monodisperse microspheres, and then centrifuging and drying to obtain a white solid of dicyclopentadiene / maleic anhydride alternating copolymer.

[0007] All of the above patents use maleic anhydride as a functional monomer for polymerization with olefins. However, the olefins used are typically C4+ olefins, typically liquid olefins such as diolefins, cycloolefins, and isoolefins. The polymerization of gaseous olefins below C4 is not discussed. CN113388123A discloses a method for preparing high-viscosity nylon, which comprises mixing a nylon salt prepolymer and an olefin-maleic anhydride copolymer and conducting a polycondensation reaction to produce the high-viscosity nylon. While the olefin-maleic anhydride copolymer used in this method can be an ethylene-maleic anhydride alternating copolymer, the process for synthesizing the copolymer from lower carbon olefins is not clearly defined.

[0008] In summary, for the synthesis of olefin functional polymers, especially the polymerization of low-carbon olefins below C4 and functional monomers, it is also necessary to select a suitable synthesis process based on the characteristics of the raw materials to improve production efficiency, simplify the separation process, and reduce raw material and process costs.

[0009] Summary of the Invention

[0010] In response to the problems existing in the prior art, one of the purposes of the present application is to provide a method for synthesizing olefin functional polymers in a continuous feeding manner. The method realizes the alternating copolymerization of the same chain of low-carbon gaseous olefins and functional monomers through a pressurized reaction, and adopts a heterogeneous polymerization method to improve the monomer concentration and raw material utilization rate. By adjusting the process parameters, olefin functional polymers of different molecular weights are synthesized, and the reaction efficiency is high. The post-reaction treatment process is simple, easy to separate and purify, energy consumption is saved, and cost is reduced.

[0011] To achieve this purpose, in the first aspect of this application, the present application adopts the following technical solutions:

[0012] The present application provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0013] (1) After introducing a low-carbon olefin into a reactor and raising the temperature and pressure to reach the reaction temperature and pressure, a raw material liquid prepared by a functional monomer, an initiator, and a solvent is continuously fed into the reactor to cause a polymerization reaction;

[0014] (2) The system after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins, and the discharged light olefins are returned to step (1) for reuse. The remaining material is discharged and then subjected to solid-liquid separation to obtain a solid-phase olefin functional polymer and a liquid-phase material.

[0015] In the present application, for the synthesis of olefin functional polymers, the selection of olefins and functional monomers has an important influence on the performance of the polymers. The difference in phase between the two makes it relatively difficult to react with the olefins and functional monomers when both are liquid, and low-carbon gaseous olefins usually do not contain side chains, which makes the reaction more difficult than liquid olefins. The present application selects low-carbon gaseous olefins to react with liquid functional monomers, and increases the monomer concentration and reaction rate through pressurized reaction and heterogeneous polymerization, thereby increasing the raw material conversion rate and product yield, achieving same-chain alternating copolymerization of gaseous olefin monomers and functional monomers, and synthesizing olefin functional polymers of different molecular weights by adjusting process parameters; after the polymerization is completed, a relatively stable emulsion dispersion system can be directly obtained, the post-processing process is simple, and separation and purification are easy; the method is simple to operate, the reaction conditions are mild, the raw materials can be recycled, energy consumption is saved, the cost is low, and it is green and environmentally friendly.

[0016] The continuous feeding method adopted in the present application can control the monomer and initiator concentrations in the reaction in real time, improve the monomer concentration and raw material utilization rate, control the molecular weight of the olefin functional polymer, increase the initiator concentration, reduce the polymerization pressure, shorten the polymerization time, and at the same time, the solvent can be recycled and reused, which has obvious advantages; in the present application, the reaction raw materials are continuously added to the reactor, so the reaction in the reactor occurs continuously, but the materials after the reaction are intermittently post-processed, so the olefin functional polymer is not continuously synthesized.

[0017] The following are preferred technical solutions of this application, but are not intended to limit the technical solutions provided in this application. Through the following technical solutions, the technical objectives and beneficial effects of this application can be better achieved and realized.

[0018] As a preferred technical solution of the present application, the light olefins in step (1) include any one of ethylene, propylene, butene or butadiene, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of ethylene and propylene, a combination of propylene and butene, a combination of ethylene, propylene and butene, etc., wherein the butene includes isomers such as 1-butene, 2-butene or isobutylene.

[0019] Preferably, before the light olefin is introduced in step (1), the reactor is first evacuated and then replaced with a protective gas, wherein the protective gas can be nitrogen or an inert gas.

[0020] As a preferred technical solution of the present application, the reactor in step (1) includes any one of a reactor, a tubular reactor, a microchannel reactor, a fluidized bed reactor or an ebullient bed reactor.

[0021] Preferably, the tubular reactor includes any one of a horizontal tubular reactor, a vertical tubular reactor, a coiled tubular reactor or a U-shaped tubular reactor.

[0022] Preferably, the microchannel reactor comprises a gas-liquid-solid three-phase catalytic microreactor.

[0023] In the present application, the selection of the above reactor types is based on whether the reactor can enhance the mixing, mass transfer and heat transfer processes of the polymerization process. For example, when a microchannel reactor is used, the heat and mass transfer efficiency is high and the reaction conditions are precisely controlled.

[0024] As a preferred technical solution of the present application, the functional monomer in step (1) includes any one of maleic anhydride, maleimide or maleic acid, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of maleic anhydride and maleimide, a combination of maleimide and maleic acid, a combination of maleic anhydride, maleimide and maleic acid, etc.

[0025] Preferably, the initiator in step (1) comprises an azo compound and / or a peroxide compound.

[0026] Preferably, the azo compound includes any one of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, azobiscyclohexylcarbonitrile or dimethyl azobisisobutyrate, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of azobisisobutyronitrile and azobisisovaleronitrile, a combination of azobisisobutyronitrile and azobisisoheptanenitrile, a combination of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate, a combination of azobisisovaleronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate, and the like.

[0027] Preferably, the peroxide compound includes dibenzoyl peroxide, diisopropyl peroxide, diisobutyryl peroxide, di(2,4-dichlorobenzoyl) peroxide, dodecyl peroxide, tert-butyl peroxyneoheptanoate, tert-butyl peroxyneodecanoate, di-sec-butyl peroxydicarbonate, dihexadecyl peroxide, tert-amyl peroxyneodecanoate, tert-butyl peroxypivalate, di-(4-tert-butylcyclohexyl peroxydicarbonate), dicyclohexyl peroxydicarbonate, diisopropyl peroxydicarbonate, dibutyl peroxydicarbonate, di(2-ethylhexyl peroxydicarbonate), 2-ethylhexyl peroxydicarbonate, Any one or a combination of at least two of tert-butyl peroxide, ditetradecyl peroxydicarbonate, tert-butyl peroxyacetate, cumyl peroxyneodecanoate, di-tert-butyl peroxide, cyclohexylsulfonylacetyl peroxide, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di-3-methoxybutyl peroxydicarbonate or 1,1,3,3-tetramethylbutyl peroxypivalate, typical but non-limiting examples of the combination include: a combination of dibenzoyl peroxide and dodecanoyl peroxide, a combination of dibenzoyl peroxide and diisopropyl peroxide, a combination of dodecanoyl peroxide, diisopropyl peroxide and diisopropyl peroxydicarbonate, etc.

[0028] Preferably, the solvent in step (1) comprises any one or a combination of at least two of an organic alkanoate compound, an alkane compound or an aromatic compound. Typical but non-limiting examples of the combination include: a combination of an organic alkanoate compound and an alkane compound, a combination of an alkane compound and an aromatic compound, a combination of an organic alkanoate compound, an alkane compound and an aromatic compound, etc.

[0029] Preferably, the general formula of the organic alkanoate compound is Wherein, R1 is any one of H, C1-C20 alkane group or C6-C10 aromatic hydrocarbon group, and R2 is any one of C1-C20 alkane group or C6-C10 aromatic hydrocarbon group.

[0030] Preferably, the organic alkanoate compound comprises any one or a combination of at least two of ethyl formate, propyl formate, isobutyl formate, pentyl formate, ethyl acetate, butyl acetate, isobutyl acetate, pentyl acetate, isoamyl acetate, benzyl acetate, phenyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, isobutyl butyrate, isoamyl butyrate, ethyl isobutyrate, ethyl isovalerate, isoamyl isovalerate, methyl benzoate, ethyl benzoate, propyl benzoate, butyl benzoate, isoamyl benzoate, methyl phenylacetate, ethyl phenylacetate, propyl phenylacetate, butyl phenylacetate or isoamyl phenylacetate. Typical but non-limiting examples of the combination include: a combination of ethyl acetate and butyl acetate, a combination of propyl formate and ethyl acetate, a combination of ethyl acetate, ethyl propionate and ethyl butyrate, etc.

[0031] Preferably, the alkane compound includes any one of cyclohexane, n-hexane, n-heptane, n-pentane, n-octane or n-decane, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of cyclohexane and n-hexane, a combination of n-hexane and n-heptane, a combination of n-hexane and n-heptane, a combination of cyclohexane, n-hexane and n-heptane, and the like.

[0032] Preferably, the aromatic hydrocarbon compound includes any one of benzene, toluene, ethylbenzene or xylene, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of benzene and ethylbenzene, a combination of benzene and toluene, a combination of toluene and ethylbenzene, a combination of ethylbenzene and xylene, a combination of benzene, ethylbenzene and xylene, etc.

[0033] As a preferred technical solution of the present application, the molar ratio of the initiator to the functional monomer in step (1) is (0.001-0.2):1, for example, 0.001:1, 0.005:1, 0.01:1, 0.05:1, 0.1:1, 0.15:1 or 0.2:1, etc., but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably (0.001-0.03):1.

[0034] Preferably, the mass ratio of the solvent to the functional monomer in step (1) is (2-50):1, for example, 2:1, 5:1, 10:1, 20:1, 25:1, 30:1, 35:1, 40:1 or 50:1, but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, preferably (2-10):1.

[0035] Preferably, the raw material liquid in step (1) is first subjected to impurity removal and preheating before being added to the reactor.

[0036] In this application, the raw material liquid must be preheated before feeding to ensure that the monomers in the system are fully dissolved and do not precipitate. At the same time, the preheating temperature should not be too high, which may cause premature decomposition and consumption of the initiator. To form the raw material liquid, the components must be mixed. If any undissolved impurities are present after mixing, they must be removed by filtration or other operations.

[0037] Preferably, the raw material liquid in step (1) is pressurized by a delivery pump and then pumped into the reactor at a uniform speed.

[0038] In the present application, the raw material liquid is continuously introduced and discharged after the residence time is reached to ensure the continuous progress of the reaction, and the reaction discharge is then subjected to subsequent separation and distillation processes.

[0039] As a preferred technical solution of the present application, the temperature of the polymerization reaction in step (1) is 50 to 150°C, for example, 50°C, 60°C, 70°C, 75°C, 80°C, 90°C, 100°C, 110°C, 120°C or 150°C, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 70 to 120°C.

[0040] Preferably, the pressure of the polymerization reaction in step (1) is 0.1 to 10 MPa, for example, 0.1 MPa, 0.5 MPa, 1 MPa, 3 MPa, 5 MPa, 6 MPa, 8 MPa or 10 MPa, but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, preferably 2 to 8 MPa.

[0041] Preferably, the feeding time of the raw material liquid in step (1) is 0.1 to 10 h, for example, 0.1 h, 0.5 h, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h, 8 h or 10 h, etc., but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0042] Preferably, the residence time of the raw material liquid in step (1) is 0.1 to 15 h, for example, 0.1 h, 0.5 h, 1 h, 3 h, 5 h, 6 h, 8 h, 10 h, 12 h or 15 h, etc., but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0043] Preferably, during the polymerization reaction in step (1), light olefins are continuously introduced to maintain the pressure.

[0044] As a preferred technical solution of the present application, during the gas-solid-liquid separation process in step (2), the low-carbon olefins are discharged for recovery and replaced with a protective gas, and the protective gas can be nitrogen or an inert gas.

[0045] Preferably, the remaining material after recovering the light olefins in step (2) is discharged in a solid-liquid manner.

[0046] Preferably, the discharged light olefins are pressurized and then returned to step (1) for reuse, and the pressure after pressurization is selected within the above-mentioned reaction pressure range.

[0047] As a preferred technical solution of the present application, the method of solid-liquid separation in step (2) includes any one of decantation, filtration or centrifugation, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of decantation and filtration, a combination of filtration and centrifugation, a combination of decantation, filtration and centrifugation, etc.

[0048] Preferably, the filtration comprises any one of gravity filtration, vacuum filtration or pressure filtration.

[0049] Preferably, the filter used for the filtration includes a normal pressure filter, a vacuum filter or a pressurized filter.

[0050] Preferably, the remaining material is filter-filtered using protective gas, and the obtained filter cake is washed, dried and then crushed.

[0051] Preferably, the washing is carried out using the solvent in step (1). In addition, an ether compound may also be used, wherein the ether compound comprises any one or a combination of at least two of C1-C10 saturated ether compounds, preferably diethyl ether and / or propyl ether.

[0052] Preferably, the drying temperature is 30 to 150°C, for example, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, preferably 80 to 120°C.

[0053] Preferably, the drying time is 1 to 72 hours, for example, 1 hour, 6 hours, 12 hours, 18 hours, 24 hours, 30 hours, 36 hours, 42 hours, 48 ​​hours, 54 hours, 60 hours, 66 hours or 72 hours, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable, preferably 24 to 72 hours.

[0054] Preferably, the drying pressure is 0.1 to 101 kPa, such as 0.1 kPa, 1 kPa, 10 kPa, 20 Pa, 40 kPa, 60 kPa, 80 kPa or 101 kPa, etc., but is not limited to the listed values. Other unlisted values ​​within this numerical range are also applicable, preferably 1 to 10 kPa.

[0055] Preferably, the olefin functional polymer in step (2) is in the form of microspherical particles having a particle size of 10 to 50 μm, for example, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm or 50 μm, etc., but is not limited to the listed values, and other values ​​not listed within this numerical range are also applicable.

[0056] As a preferred technical solution of the present application, the liquid phase material in step (2) is separated, and the recovered solvent is returned to step (1) for reuse.

[0057] In the present application, the liquid phase material can also be directly reused without separation, and used for the preparation of raw material liquid or as a washing solvent.

[0058] Preferably, the method for separating the liquid phase material in step (3) comprises any one or a combination of at least two of distillation, membrane separation, washing or extraction. Typical but non-limiting examples of the combination include: a combination of distillation and membrane separation, a combination of distillation and extraction, a combination of distillation, membrane separation and washing, etc., preferably distillation.

[0059] Preferably, the recovered solvent is returned to step (1) and / or step (2) and reused for preparing the raw material solution and / or washing the filter cake.

[0060] As a preferred technical solution of this application, the method includes the following steps:

[0061] (1) After introducing a low-carbon olefin into a reactor and raising the temperature and pressure, the low-carbon olefin includes any one of ethylene, propylene, butene or butadiene or a combination of at least two thereof; the reactor includes any one of a reactor, a tubular reactor, a microchannel reactor, a fluidized bed reactor or an ebullient bed reactor; after reaching the reaction temperature and reaction pressure, a raw material liquid prepared from a functional monomer, an initiator and a solvent is continuously fed into the reactor; the functional monomer includes any one of maleic anhydride, maleimide or maleic acid or a combination of at least two thereof; the initiator includes an azo compound and / or a peroxide compound; The solvent comprises any one or a combination of at least two of an organic alkanoate compound, an alkane compound, or an aromatic compound; the molar ratio of the initiator to the functional monomer is (0.001-0.2):1; the mass ratio of the solvent to the functional monomer is (2-50):1; the raw material liquid is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction; the polymerization reaction temperature is 50-150° C., the pressure is 0.1-10 MPa, the feeding time is 0.1-10 h, the residence time is 0.1-15 h, and light olefins are continuously introduced during the polymerization reaction to maintain the pressure;

[0062] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, discharging the remaining low-carbon olefins during the gas-solid-liquid separation process and replacing them with protective gas, returning the discharged low-carbon olefins to step (1) for reuse after pressurization, discharging the remaining materials in a solid-liquid manner and subjecting them to solid-liquid separation, subjecting the remaining materials to pressure filtration using protective gas, washing the obtained filter cake, drying it, and then crushing it to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is in the form of microspherical particles with a particle size of 10 to 50 μm;

[0063] (3) separating the liquid phase material obtained in step (2), wherein the separation method comprises any one of distillation, membrane separation, washing or extraction, or a combination of at least two thereof; and the recovered solvent is returned to step (1) and / or step (2) and reused for preparing the raw material liquid and / or washing the filter cake.

[0064] Compared with the prior art, this application has the following beneficial effects:

[0065] (1) The method described in this application adopts a heterogeneous polymerization method, and realizes the alternating copolymerization of the same chain of low-carbon gaseous olefins and liquid functional monomers through the pressurized reaction of the two, thereby producing olefin functional polymers with high functional group content, high reactivity, and wide application;

[0066] (2) After the polymerization is completed, a relatively stable emulsion dispersion system can be directly obtained. The post-processing process is simple and easy to separate and purify. The raw materials can be recycled, thereby improving the conversion rate of the raw materials and the product yield.

[0067] (3) The method described in the present application adopts a method of continuous feeding of raw material liquid, which can regulate the concentration of monomers and initiators in the reaction in real time, improve the monomer concentration and raw material utilization rate, regulate the molecular weight of olefin functional polymers, increase the initiator concentration, reduce the polymerization pressure, and shorten the total process time;

[0068] (4) The method described in this application can achieve full sealing of the reaction system equipment, and can prevent impurities in the air from entering the reaction system during the circulation of light olefins;

[0069] (5) The method described in this application is simple to operate, has mild reaction conditions, saves energy, is low in cost, and is environmentally friendly.

[0070] In the second aspect of the present application, the present application further provides the use of the olefin functional polymer obtained based on the first aspect above, and the use includes the use of the olefin functional polymer in the preparation of modified reinforcing resin, adhesive, scale inhibitor or glass fiber sizing. Among them, the use of the olefin functional polymer in the preparation of reinforced resin includes the following steps: mixing the olefin functional polymer with a base resin and a filler to obtain a modified reinforcing resin; the use of the olefin functional polymer in the preparation of a modified adhesive includes the following steps: esterifying the olefin functional polymer with an alcohol to obtain an adhesive; the use of the olefin functional polymer in the preparation of a scale inhibitor includes the following steps: subjecting the olefin functional polymer to an anionic and cationic reaction to obtain a scale inhibitor; the use of the olefin functional polymer in the preparation of a glass fiber sizing includes the following steps: mixing the olefin functional polymer with a coupling agent, a pH regulator and water to obtain a glass fiber sizing.

[0071] In the present application, for the synthesis of olefin functional polymers, the selection of olefins and functional monomers has an important influence on the performance of the polymers. The present application selects low-carbon gaseous olefins to react with liquid functional monomers. The difference in phase between the two makes it relatively difficult to react with both the olefins and the functional monomers when they are liquid. In addition, low-carbon gaseous olefins usually do not contain side chains, and are more difficult to react with than liquid olefins. The present application increases the monomer concentration and reaction rate, improves the raw material conversion rate and product yield through pressurized reaction and heterogeneous polymerization, and realizes the same-chain alternating copolymerization of gaseous olefin monomers and functional monomers. The present application has a simple operating process, mild reaction conditions, easy separation and purification, and the raw materials can be recycled, which saves energy, is low in cost, and is green and environmentally friendly.

[0072] At the same time, this application utilizes the characteristics of high functional group content and high reaction activity in olefin functional polymers, uses olefin functional polymers as a reaction platform, and utilizes its derivatization pathway to prepare a variety of modified materials suitable for different fields through chemical reactions such as esterification, hydrolysis, and modification, and develops a variety of downstream products, such as compatible modifiers, adhesives, and scale inhibitors, thereby broadening the application scope of olefin functional polymers.

[0073] (A) Use of olefin functional polymers in the preparation of reinforced resins

[0074] As a preferred technical solution of the present application, the olefin functional polymer obtained in the first aspect is used as a compatibilizer and mixed with the base resin and filler.

[0075] Preferably, the matrix resin comprises thermoplastics and / or thermosetting plastics.

[0076] Preferably, the thermoplastic plastic includes any one of PC, PA, POM, PBT, PET, PVC, PS, PE or ABS, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of PC and PA, a combination of PA and PET, a combination of PET, PVC and PS, a combination of PC, PBT, PVC and ABS, etc.

[0077] Preferably, the thermosetting plastic comprises any one of EP, UPR, PU or UF or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of EP and UPR, a combination of UPR and PU, a combination of EP, PU and UF, etc.

[0078] Preferably, the filler comprises an inorganic filler and / or an organic filler.

[0079] Preferably, the amount of the base resin added is 30-90wt% of the total mixture, for example, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%, 80wt% or 90wt%, etc., but is not limited to the listed values, and other values ​​not listed within this numerical range are equally applicable; the amount of the filler added is 5-65wt% of the total mixture, for example, 5wt%, 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, 60wt% or 65wt%, etc., but is not limited to the listed values, and other values ​​not listed within this numerical range are equally applicable; the amount of the olefin functional polymer added is 3-15wt% of the total mixture, for example, 3wt%, 5wt%, 8wt%, 10wt%, 12wt% or 15wt%, etc., but is not limited to the listed values, and other values ​​not listed within this numerical range are equally applicable.

[0080] As a preferred technical solution of the present application, the mixing method includes any one of mechanical blending, solution blending or latex blending.

[0081] Preferably, the mechanical blending comprises: preliminarily mixing the olefin functional polymer with the matrix resin and the filler, performing banburying mixing, and then extruding and granulating to prepare the modified reinforced resin.

[0082] Preferably, the internal mixing is carried out in an internal mixer, and the temperature of the internal mixing is 120-400°C, for example, 120°C, 150°C, 180°C, 200°C, 250°C, 300°C, 350°C or 400°C, but is not limited to the listed values, and other unlisted values ​​within this numerical range are also applicable.

[0083] Preferably, the extrusion granulation is carried out using a twin-screw extruder or a single-screw extruder.

[0084] Preferably, the solution blending comprises: dissolving the olefin functional polymer, the matrix resin and the filler in a solvent, mixing them uniformly and then removing the solvent to obtain the modified reinforced resin.

[0085] Preferably, the solvent comprises any one or a combination of at least two of organic alkanoates, alkanes or aromatic compounds. Typical but non-limiting examples of the combination include: a combination of organic alkanoates and alkanes, a combination of alkanes and aromatics, a combination of organic alkanoates, alkanes and aromatics, etc.

[0086] Preferably, the method of removing the solvent is filter pressing.

[0087] Preferably, the latex blending comprises: dissolving the olefin functional polymer, the matrix resin and the filler in a solvent respectively, and then distilling to prepare latex, and then uniformly mixing, coagulating, drying and plasticizing to obtain the modified reinforced resin.

[0088] (B) Use of olefin functional polymers in the preparation of adhesives

[0089] As a preferred technical solution of the present application, the alcohol includes any one of methanol, ethanol, propanol or butanol, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of methanol and ethanol, a combination of ethanol and butanol, a combination of methanol, ethanol and butanol, etc.

[0090] Preferably, the molar ratio of anhydride to alcohol in the olefin functional polymer is 1:(2-5), for example, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0091] Preferably, the temperature of the esterification reaction is 60-80°C, such as 60°C, 65°C, 70°C, 75°C or 80°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0092] Preferably, the esterification reaction time is 3 to 5 hours, such as 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0093] Preferably, after the esterification reaction, the product is concentrated and dried to obtain an esterification product.

[0094] As a preferred technical solution of the present application, before the anionization and cationization reaction, an esterification reaction of the olefin functional polymer and alcohols is also included to generate a monoesterified olefin functional polymer.

[0095] Preferably, the alcohol comprises any one of methanol, ethanol, butanol, ethylene glycol or propylene glycol, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of methanol and ethanol, a combination of ethanol and ethylene glycol, a combination of methanol, ethanol and butanol, a combination of ethanol, ethylene glycol and propylene glycol, etc.

[0096] Preferably, the molar ratio of anhydride to alcohol in the olefin functional polymer is 1:(1-10), for example, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:8 or 1:10, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0097] Preferably, the temperature of the esterification reaction is 50-80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0098] Preferably, the pressure of the esterification reaction is 0 to 0.5 MPa, such as 0 MPa, 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa or 0.5 MPa, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0099] Preferably, the esterification reaction time is 0.5 to 24 h, for example, 0.5 h, 1 h, 2 h, 4 h, 6 h, 8 h, 12 h, 16 h, 20 h or 24 h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0100] (C) Use of olefin functional polymers in the preparation of scale inhibitors

[0101] Preferably, the anionization and cationization reaction comprises the reaction of an olefin functional polymer or a monoesterified olefin functional polymer with a quaternary ammonium salt, a base or an acid.

[0102] Preferably, the quaternary ammonium salt includes any one of glycidyltrimethylammonium chloride, octadecyldimethylammonium chloride, octadecylamine polyoxyethylene ether diquaternary ammonium salt or didodecylamine polyoxyethylene ether monoquaternary ammonium salt, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of glycidyltrimethylammonium chloride and octadecyldimethylammonium chloride, a combination of octadecyldimethylammonium chloride and octadecylamine polyoxyethylene ether diquaternary ammonium salt, a combination of glycidyltrimethylammonium chloride, octadecyldimethylammonium chloride and didodecylamine polyoxyethylene ether monoquaternary ammonium salt, etc.

[0103] Preferably, the base comprises caustic, added in the form of an alkaline solution.

[0104] Preferably, when the quaternary ammonium salt is used, an alkaline solution is added simultaneously.

[0105] Preferably, the acid comprises any one of sulfuric acid, persulfuric acid or phosphorus pentoxide, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of sulfuric acid and persulfuric acid, a combination of persulfuric acid and phosphorus pentoxide, a combination of sulfuric acid, persulfuric acid and phosphorus pentoxide, and the like.

[0106] Preferably, the anionization and cationization reaction includes any one or a combination of at least two of the following: reacting a monoesterified olefin functional polymer with a quaternary ammonium salt in an alkaline solution to prepare a cationic polymer scale inhibitor; reacting an olefin functional polymer with a quaternary ammonium salt in an alkaline solution to prepare a cationic polymer scale inhibitor; saponifying an olefin functional polymer with an alkaline solution to prepare a carboxylate-type anionic polymer scale inhibitor; reacting a glycol-type monoesterified olefin functional polymer with sulfuric acid to prepare a sulfate-type anionic polymer scale inhibitor; or reacting a glycol-type monoesterified olefin functional polymer with phosphorus pentoxide to prepare a phosphate-type anionic polymer scale inhibitor.

[0107] (D) Use of olefin functional polymers in the preparation of glass fiber sizings

[0108] As a preferred technical solution of the present application, the coupling agent includes any one of a silane coupling agent, an aluminate coupling agent or a titanate coupling agent, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of a silane coupling agent and an aluminate coupling agent, a combination of a silane coupling agent and a titanate coupling agent, a combination of a silane coupling agent, an aluminate coupling agent and a titanate coupling agent, and the like.

[0109] In this application, the most widely used coupling agent among the above coupling agents is silane coupling agent, and the available types include A-151 (vinyl triethoxysilane), KH550 (γ-aminopropyl triethoxysilane), KH570 (γ-methacryloxypropyl trimethoxysilane), etc. At present, new silane coupling agents are also used, such as silicone peroxide coupling agents.

[0110] Preferably, the pH regulator includes an acid regulator or an alkaline regulator.

[0111] Preferably, the acid regulator comprises any one of acetic acid, citric acid, formic acid or oxalic acid, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of formic acid and acetic acid, a combination of citric acid and oxalic acid, a combination of acetic acid, citric acid and formic acid, etc.

[0112] Preferably, the alkaline regulator includes any one or a combination of at least two of ammonia water, sodium hydroxide, sodium bicarbonate, basic amino acids or organic amines. Typical but non-limiting examples of the combination include: a combination of ammonia water and sodium hydroxide, a combination of sodium hydroxide and sodium bicarbonate, a combination of ammonia water and organic amines, a combination of sodium bicarbonate, basic amino acids and organic amines, etc.

[0113] Preferably, the preparation step of the glass fiber sizing includes: first adding a coupling agent into water and stirring, then adding a solid-phase olefin functional polymer, stirring evenly, and then adding a pH regulator to obtain the glass fiber sizing.

[0114] Preferably, the stirring time after the coupling agent is added is 20 to 30 minutes, for example, 20 minutes, 22 minutes, 25 minutes, 27 minutes or 30 minutes, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0115] Preferably, the stirring time after the addition of the olefin functional polymer is 60 to 240 min, for example, 60 min, 90 min, 120 min, 150 min, 180 min, 210 min or 240 min, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the stirring rate is 100 to 800 rpm, for example, 100 rpm, 200 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm or 800 rpm, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0116] Preferably, after adding the pH adjuster, the pH value is adjusted to 6-10, such as 6, 7, 8, 9 or 10, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0117] Preferably, the mass proportion of water in the glass fiber sizing is 20 to 95 wt%, for example, 20 wt%, 30 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%, 80 wt%, 90 wt% or 95 wt%, etc., but is not limited to the listed values. Other values ​​not listed within this numerical range are also applicable, and the rest are solid phase components.

[0118] As a preferred technical solution of the present application, the glass fiber sizing in step (3) further includes any one of a lubricant, a defoaming agent or an antioxidant, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of a lubricant and a defoaming agent, a combination of a defoaming agent and an antioxidant, a combination of a lubricant, a defoaming agent and an antioxidant, etc.

[0119] Preferably, the lubricant comprises any one of stearic acid amide, oleic acid amide, palmitic acid amide, stearic acid, methyl stearate, butyl stearate, polyethylene wax or polypropylene wax, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of stearic acid amide and oleic acid amide, a combination of stearic acid and methyl stearate, a combination of polyethylene wax and polypropylene wax, a combination of oleic acid amide, palmitic acid amide and stearic acid, and the like.

[0120] Preferably, the defoaming agent comprises any one of a higher alcohol fatty acid ester complex, polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropyl alcohol amine ether, polyoxypropylene glycerol ether or a combination of at least two of polyoxypropylenes. Typical but non-limiting examples of the combination include: a combination of a higher alcohol fatty acid ester complex and polyoxyethylene polyoxypropylene pentaerythritol ether, a combination of polyoxyethylene polyoxypropyl alcohol amine ether and polyoxypropylene glycerol ether, a combination of polyoxyethylene polyoxypropylene pentaerythritol ether, polyoxyethylene polyoxypropyl alcohol amine ether and polyoxypropylene glycerol ether, and the like.

[0121] Preferably, the antioxidant comprises a hindered phenol antioxidant and / or a phosphite antioxidant.

[0122] Preferably, the antioxidant includes any one or a combination of at least two of antioxidant 1010 (tetrakis[β-(3.5-di-tert-butyl, 4-hydroxyphenyl) propionate] pentaerythritol), antioxidant 1076 (β-(3.5-di-tert-butyl, 4-hydroxyphenyl) propionate octadecyl), antioxidant 3114 (1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl) isocyanuric acid), antioxidant 168 (tris(2,4-di-tert-butylphenyl) phosphite) or antioxidant 626 (bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite). Typical but non-limiting examples of the combination include: a combination of antioxidant 1010 and antioxidant 1076, a combination of antioxidant 168 and antioxidant 626, antioxidant 3114 and antioxidant 168, etc.

[0123] Preferably, the lubricant, defoamer and antioxidant are added together with the olefin functional polymer during the preparation of the glass fiber sizing.

[0124] In the present application, when an olefin functional polymer is used to prepare a glass fiber sizing, a comonomer may be added to the olefin functional polymer during synthesis. In this case, a multi-olefin functional polymer is obtained, which can effectively adjust the acid anhydride value of the olefin functional polymer. The types of the comonomers include any one or a combination of at least two of methyl acrylate, methyl methacrylate, vinyl acetate, N,N-dimethylacrylamide, acrylamide or acrylonitrile. Typical but non-limiting examples of the combinations include: a combination of methyl acrylate and methyl methacrylate, a combination of methyl acrylate and vinyl acetate, a combination of N,N-dimethylacrylamide, acrylamide and acrylonitrile, a combination of methyl methacrylate, vinyl acetate and acrylamide, etc.

[0125] As a preferred technical solution of this application, the use includes the following steps:

[0126] (1) After introducing a low-carbon olefin into a reactor and raising the temperature and pressure, the low-carbon olefin includes any one of ethylene, propylene, butene or butadiene or a combination of at least two thereof, and the reactor includes any one of a tank reactor, a tubular reactor, a microchannel reactor, a tower reactor, a fluidized bed reactor or an ebullient bed reactor. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared from a functional monomer, an initiator and a solvent is added into the reactor, the functional monomer includes any one of maleic anhydride, maleimide or maleic acid or a combination of at least two thereof, and the initiator includes an azo compound and / or a peroxide. The solvent comprises any one or a combination of at least two of an organic alkanoate compound, an alkane compound, or an aromatic compound; the molar ratio of the initiator to the functional monomer is (0.001-0.2):1; the mass ratio of the solvent to the functional monomer is (2-50):1; the raw material liquid is pressurized by a delivery pump and then pumped into the reactor at a uniform speed to cause a polymerization reaction; the polymerization reaction temperature is 50-150° C., the pressure is 0.1-10 MPa, the residence time is 10 s-10 h, and light olefins are continuously introduced during the polymerization reaction to maintain the pressure;

[0127] (2) subjecting the material after the polymerization reaction in step (1) to gas-solid-liquid separation, recovering the low-carbon olefins, returning the discharged low-carbon olefins to step (1) after pressurization for reuse, discharging the remaining material in a solid-liquid manner and subjecting it to solid-liquid separation, performing filter pressing with protective gas, and drying the obtained filter cake to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle with a particle size of 10 to 50 μm; separating the liquid-phase material, and separating the material by a method comprising any one or a combination of at least two of distillation, membrane separation, washing or extraction, and returning the recovered solvent after separation to step (1) and / or step (2) for reuse to prepare a raw material liquid and / or wash the filter cake;

[0128] (3) the olefin functional polymer obtained in step (2) is mixed as a compatibilizer with a base resin and a filler, wherein the base resin comprises a thermoplastic plastic and / or a thermosetting plastic, and the filler comprises an inorganic filler and / or an organic filler, the base resin is added in an amount of 30 to 90 wt % of the total amount of the mixture, the filler is added in an amount of 5 to 65 wt % of the total amount of the mixture, and the olefin functional polymer is added in an amount of 3 to 15 wt % of the total amount of the mixture, and the mixing method comprises any one of mechanical blending, solution blending or latex blending to obtain a modified reinforced resin;

[0129] Esterifying the olefin functional polymer obtained in step (2) with alcohols, wherein the alcohols include any one of methanol, ethanol, propanol or butanol or a combination of at least two thereof, and the molar ratio of the acid anhydride to the alcohol in the olefin functional polymer is 1:(2-5), and the esterification reaction is carried out at a temperature of 60-80° C. for 3-5 hours, followed by concentration and drying to obtain an adhesive;

[0130] The olefin functional polymer obtained in step (2) is subjected to anionization and cationization reaction to obtain a scale inhibitor; before the anionization and cationization reaction, an esterification reaction of the olefin functional polymer with alcohols is also included to generate a monoesterified olefin functional polymer, wherein the alcohols include any one of methanol, ethanol, butanol, ethylene glycol or propylene glycol or a combination of at least two thereof; the anionization and cationization reaction includes a reaction of the olefin functional polymer or the monoesterified olefin functional polymer with a quaternary ammonium salt, an alkali or an acid, wherein the quaternary ammonium salt includes epoxypropyltrimethylammonium chloride, octadecyldimethylammonium chloride, octadecylamine polyoxyethylene ether diquaternary ammonium salt or didodecylamine polyoxyethylene ether monoquaternary Any one or a combination of at least two of ammonium salts; the anionization and cationization reaction includes any one or a combination of at least two of the following: reacting a monoesterified olefin functional polymer with a quaternary ammonium salt in an alkaline solution to prepare a cationic polymer scale inhibitor, reacting an olefin functional polymer with a quaternary ammonium salt in an alkaline solution to prepare a cationic polymer scale inhibitor, saponifying an olefin functional polymer with an alkaline solution to prepare a carboxylate type anionic polymer scale inhibitor, reacting a glycol monoesterified olefin functional polymer with sulfuric acid to prepare a sulfate type anionic polymer scale inhibitor, or reacting a glycol monoesterified olefin functional polymer with phosphorus pentoxide to prepare a phosphate type anionic polymer scale inhibitor;

[0131] Alternatively, the olefin functional polymer obtained in step (2) is mixed with a coupling agent, a pH regulator, and water, specifically comprising: first adding the coupling agent into water and stirring for 20 to 30 minutes, then adding a lubricant, an olefin functional polymer, a defoaming agent, and an antioxidant, stirring for 60 to 240 minutes at a stirring rate of 100 to 800 rpm, and then adding a pH regulator to adjust the pH value to 6 to 10 to obtain a glass fiber sizing.

[0132] Compared with the prior art, this application has the following beneficial effects:

[0133] (1) The present application uses a heterogeneous polymerization method to prepare a process for continuous feeding of raw liquid by pressurized reaction of low-carbon gaseous olefins and liquid functional monomers to obtain a low-carbon gaseous olefin and functional monomer homochain alternating copolymer, which has a controllable molecular weight, a high content of functional groups, high reactivity, and a wide range of applications.

[0134] (2) The present invention has a simple operation process, mild reaction conditions, easy separation and purification, and the raw materials can be recycled, thus saving energy consumption, having low cost and high economic benefits;

[0135] (3) This application utilizes the high content of functional groups and high reactivity of olefin functional polymers, uses olefin functional polymers as a reaction platform, and prepares a variety of modified materials suitable for different fields through chemical reactions such as esterification, hydrolysis, and modification, develops a variety of downstream products, and broadens the application range of olefin functional polymers. BRIEF DESCRIPTION OF THE DRAWINGS

[0136] FIG1 is a process flow chart of the method for synthesizing olefin functional polymers in a continuous feeding manner provided in Example 1 of the present application. DETAILED DESCRIPTION

[0137] To better illustrate the present application and facilitate understanding of the technical solution of the present application, the present application is further described below. However, the following embodiments are merely simplified examples of the present application and do not represent or limit the scope of protection of the present application. The scope of protection of the present application shall be subject to the claims.

[0138] (1) A method for synthesizing olefin functional polymers by continuous feeding

[0139] The specific embodiment of the present application provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0140] (1) After introducing a low-carbon olefin into a reactor and raising the temperature and pressure to reach the reaction temperature and pressure, a raw material liquid prepared from a functional monomer, an initiator, and a solvent is added into the reactor to cause a polymerization reaction;

[0141] (2) The system after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins, and the discharged light olefins are returned to step (1) for reuse. The remaining material is discharged and then subjected to solid-liquid separation to obtain a solid-phase olefin functional polymer and a liquid-phase material.

[0142] The following are typical but non-limiting examples of this application:

[0143] Example I-1:

[0144] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner. The process flow chart of the method is shown in FIG1 , and comprises the following steps:

[0145] (1) After a low-carbon olefin is introduced into a microchannel reactor, the temperature and pressure are increased, wherein the low-carbon olefin is ethylene, and nitrogen is first introduced before the low-carbon olefin is introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the reactor. The functional monomer is maleic anhydride, the initiator is dibenzoyl peroxide, and the solvent is isoamyl acetate. The molar ratio of the initiator to the functional monomer is 0.01:1, and the mass ratio of the solvent to the functional monomer is 5:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 100°C, the pressure is 6 MPa, the feeding time is 0.1 h, and the total residence time is 0.1 h. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0146] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering the remaining materials with nitrogen through a three-in-one filter, washing the obtained filter cake, drying it, and then crushing it, and the washing solvent is n-hexane, and the drying temperature is 30° C., the time is 10 h, and the pressure is 101 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0147] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse in preparing raw material liquid and washing filter cake.

[0148] Example I-2:

[0149] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, wherein the method comprises the following steps:

[0150] (1) After introducing a low-carbon olefin into a reactor, the temperature and pressure are increased. The low-carbon olefin is ethylene. Before the low-carbon olefin is introduced, nitrogen is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the reactor in a continuous feeding manner. The functional monomer is maleic anhydride, the initiator is azobisisobutyronitrile, and the solvent is ethyl acetate and butyl acetate in a volume ratio of 1:1. The molar ratio of the initiator to the functional monomer is 0.1:1, and the mass ratio of the solvent to the functional monomer is 20:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor through a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 70°C, the pressure is 4 MPa, the feeding time is 8 hours, and the total residence time is 10 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0151] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering the remaining materials with nitrogen through a three-in-one filter, washing the obtained filter cake, drying it, and then crushing it, the washing solvent being butyl acetate, the drying temperature being 120° C., the drying time being 48 h, and the pressure being 50 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is in the form of microspherical particles;

[0152] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse in preparing raw material liquid and washing filter cake.

[0153] Example 1-3:

[0154] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0155] (1) After introducing a low-carbon olefin into a reactor, the temperature and pressure are increased. The low-carbon olefin is isobutylene. Before the low-carbon olefin is introduced, nitrogen is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the reactor. The functional monomer is maleic anhydride, the initiator is azobisisoheptanonitrile, and the solvent is ethyl acetate. The molar ratio of the initiator to the functional monomer is 0.06:1, and the mass ratio of the solvent to the functional monomer is 8:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor through a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 90°C, the pressure is 3.5 MPa, the feeding time is 5 hours, and the total residence time is 7 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0156] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering the remaining materials with nitrogen through a three-in-one filter, washing the obtained filter cake, drying it, and then crushing it, and the washing solvent is ethyl acetate, and the drying temperature is 60° C., the time is 24 h, and the pressure is 20 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0157] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is used as a recovery solvent, which is returned to step (1) and reused for preparing the raw material liquid.

[0158] Example 1-4:

[0159] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0160] (1) After a low-carbon olefin is introduced into a fluidized bed reactor, the temperature and pressure are increased. The low-carbon olefin is propylene. Before the low-carbon olefin is introduced, argon is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the fluidized bed reactor. The functional monomer is maleimide, the initiator is diisopropylbenzene peroxide, and the solvent is benzene and xylene in a volume ratio of 1:1. The molar ratio of the initiator to the functional monomer is 0.006:1, and the mass ratio of the solvent to the functional monomer is 10:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 120°C, the pressure is 10 MPa, the feeding time is 4 hours, and the total residence time is 6 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0161] (2) The system after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation, and light olefins are recovered at the same time. The discharged light olefins are pressurized and returned to step (1) for reuse. The remaining material is filtered through argon pressure using a three-in-one filter. The obtained filter cake is washed, dried and then crushed. The solvent used for washing is cyclohexane. The drying temperature is 110° C., the time is 24 hours, and the pressure is 1 kPa to obtain a solid-phase olefin functional polymer and a liquid-phase material. The olefin functional polymer is in the form of microspherical particles;

[0162] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse in preparing raw material liquid and washing filter cake.

[0163] Example 1-5:

[0164] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0165] (1) After a low-carbon olefin is introduced into a tubular reactor, the temperature and pressure are increased. The low-carbon olefin is ethylene. Before the low-carbon olefin is introduced, argon is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the tubular reactor. The functional monomer is maleic acid, the initiator is azobisisobutyronitrile and dodecyl peroxide in a molar ratio of 1:1, the solvent is xylene, the molar ratio of the initiator to the functional monomer is 0.2:1, and the mass ratio of the solvent to the functional monomer is 40:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 50°C, the pressure is 3 MPa, the feeding time is 10 hours, and the total residence time is 15 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0166] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering and separating the remaining materials using a normal pressure filter, washing the obtained filter cake, drying it, and then crushing it, the washing solvent used is xylene, the drying temperature is 120° C., the time is 12 h, and the pressure is 10 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0167] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is used as a recovery solvent, which is returned to step (1) and step (2) and reused for preparing the raw material liquid and washing the filter cake.

[0168] Example I-6:

[0169] The present embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps: (1) introducing a low-carbon olefin into a reactor and then heating and pressurizing the reactor, wherein the low-carbon olefin is ethylene, and nitrogen is introduced before the low-carbon olefin is introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by functional monomer, initiator and solvent is pumped into the reactor, wherein the functional monomer is maleic anhydride, the initiator is dimethyl azobisisobutyrate, and the solvent is butyl acetate and ethyl acetate in a volume ratio of 5:1. The molar ratio of the initiator to the functional monomer is 0.008:1, and the mass ratio of the solvent to the functional monomer is 10:1. After preheating, the raw material liquid is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 110° C., the pressure is 6 MPa, the feeding time is 3 h, and the total residence time is 5 h. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0170] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering and separating the remaining materials using a normal pressure filter, washing the obtained filter cake, drying it, and then crushing it, the washing solvent used is propyl ether, the drying temperature is 50° C., the time is 36 hours, and the pressure is 70 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0171] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse in preparing raw material liquid and washing filter cake.

[0172] Example I-7:

[0173] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0174] (1) After introducing a low-carbon olefin into a reactor, the temperature and pressure are increased. The low-carbon olefin is propylene. Before the low-carbon olefin is introduced, nitrogen is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the reactor. The functional monomer is maleic anhydride, the initiator is azobiscyclohexylcarbonitrile, and the solvent is n-octane. The molar ratio of the initiator to the functional monomer is 0.15:1, and the mass ratio of the solvent to the functional monomer is 30:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor through a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 60°C, the pressure is 3.5 MPa, the feeding time is 7 hours, and the total residence time is 10 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0175] The operations of step (2) and step (3) refer to Example 4.

[0176] Based on the tests of the raw monomers and olefin functional polymers in Examples I-1 to I-7 above, the conversion rate of the functional monomers, the yield of the olefin functional polymer, and the anhydride value were calculated. The particle size and weight-average molecular weight of the polymers were also tested and calculated. The results are shown in Table 1.

[0177] Table 1 Results of the polymerization reactions in Examples I-1 to I-7

[0178] As shown in Table 1, by using the method described in this application to synthesize olefin functional polymers, by adjusting the polymerization process parameters such as temperature, pressure, feed ratio, time, solvent mass ratio, etc., the conversion rate of functional monomers can reach more than 98%, and the polymer yield can also reach more than 93%. The anhydride value of the polymer is above 63.5%, the average particle size is in the range of 12 to 22 μm, the particle size range is about 10 to 50 μm, and the weight-average molecular weight can be controlled at about 60,000. During the polymerization process, the higher the temperature, the faster the initiator decomposes, the lower the monomer free radicals and initiator free radicals in the system, the lower the degree of polymerization, and the lower the product molecular weight; the higher the pressure during the polymerization process, the higher the monomer free radical ratio, and the higher the product molecular weight. At the same time, parameters such as the initiator feed ratio, solvent feed amount, and feed time have a great influence on the polymerization effect.

[0179] The method described in this application can also be used to synthesize olefin functional polymers of different molecular weights by regulating process parameters such as temperature, pressure, raw material liquid ratio, and feed rate. The following are typical but non-limiting supplementary examples of the synthesis of olefin functional polymers of different molecular weights in this application:

[0180] Example I-8

[0181] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0182] (1) After a low-carbon olefin is introduced into a tubular reactor, the temperature and pressure are increased. The low-carbon olefin is ethylene. Before the low-carbon olefin is introduced, nitrogen is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the tubular reactor. The functional monomer is maleic anhydride, the initiator is azobisisobutyronitrile, and the solvent is isoamyl acetate. The molar ratio of the initiator to the functional monomer is 0.02:1, and the mass ratio of the solvent to the functional monomer is 20:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 150°C, the pressure is 1 MPa, the feeding time is 4 hours, and the total residence time is 6 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0183] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering and separating the remaining materials using a normal pressure filter, washing the obtained filter cake, drying it, and then crushing it, the washing solvent used is n-hexane, the drying temperature is 30° C., the time is 16 h, and the pressure is 30 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0184] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse in preparing raw material liquid and washing filter cake.

[0185] Example I-9:

[0186] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0187] (1) After a low-carbon olefin is introduced into a tubular reactor, the temperature and pressure are increased. The low-carbon olefin is ethylene. Before the low-carbon olefin is introduced, nitrogen is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the tubular reactor. The functional monomer is maleic anhydride, the initiator is azobisisobutyronitrile, and the solvent is isoamyl acetate. The molar ratio of the initiator to the functional monomer is 0.01:1, and the mass ratio of the solvent to the functional monomer is 10:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 120°C, the pressure is 3 MPa, the feeding time is 5 hours, and the total residence time is 8 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0188] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering and separating the remaining materials using a normal pressure filter, washing the obtained filter cake, drying it, and then crushing it, the washing solvent used isoamyl acetate, the drying temperature is 140° C., the time is 36 hours, and the pressure is 60 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0189] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is used as a recovery solvent, which is returned to step (1) and step (2) and reused for preparing the raw material liquid and washing the filter cake.

[0190] Example I-10

[0191] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0192] (1) After a low-carbon olefin is introduced into a tubular reactor, the temperature and pressure are increased. The low-carbon olefin is ethylene. Before the low-carbon olefin is introduced, nitrogen is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the tubular reactor. The functional monomer is maleic anhydride, the initiator is azobisisobutyronitrile, and the solvent is isoamyl acetate. The molar ratio of the initiator to the functional monomer is 0.008:1, and the mass ratio of the solvent to the functional monomer is 3:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 80°C, the pressure is 6 MPa, the feeding time is 6 hours, and the total residence time is 8 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0193] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering and separating the remaining materials using a normal pressure filter, washing the obtained filter cake, drying it, and then crushing it, the washing solvent used is xylene, the drying temperature is 100° C., the time is 60 h, and the pressure is 101 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0194] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse in preparing raw material liquid and washing filter cake.

[0195] Example I-11:

[0196] This embodiment provides a method for synthesizing olefin functional polymers in a continuous feeding manner, the method comprising the following steps:

[0197] (1) After a low-carbon olefin is introduced into a tubular reactor, the temperature and pressure are increased. The low-carbon olefin is ethylene. Before the low-carbon olefin is introduced, nitrogen is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously pumped into the tubular reactor. The functional monomer is maleic anhydride, the initiator is azobisisobutyronitrile, and the solvent is isoamyl acetate. The molar ratio of the initiator to the functional monomer is 0.01:1, and the mass ratio of the solvent to the functional monomer is 5:1. After the raw material liquid is preheated, it is pressurized and pumped into the reactor by a delivery pump to cause a polymerization reaction. The polymerization reaction temperature is 70°C, the pressure is 4.5 MPa, the feeding time is 8 hours, and the total residence time is 10 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0198] (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, and recovering light olefins at the same time, and returning the discharged light olefins to step (1) for reuse after pressurization, and filtering and separating the remaining materials using a normal pressure filter, washing the obtained filter cake, drying it, and then crushing it, the washing solvent used is ether, the drying temperature is 30° C., the time is 8 hours, and the pressure is 80 kPa, to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle;

[0199] (3) The liquid phase material obtained in step (2) is subjected to distillation separation, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse in preparing raw material liquid and washing filter cake.

[0200] Based on the tests of the raw monomers and olefin functional polymers in Examples I-8 to I-11 above, the conversion rate of the functional monomers, the yield of the olefin functional polymer and the anhydride value were calculated, and the particle size and weight-average molecular weight of the polymer were tested and calculated. The results are shown in Table 2.

[0201] Table 2 Results of the polymerization reactions in Examples I-8 to I-11

[0202] As shown in Table 2, by adopting the method described in the present application to synthesize olefin functional polymers, under the premise that the conversion rate of functional monomers and polymer yield are not significantly reduced, by adjusting appropriate process parameters, olefin functional polymers with a weight-average molecular weight of 10,000 to 150,000 can be prepared.

[0203] From the above examples, it can be seen that the method described in the present application realizes the alternating copolymerization of the same chain of low-carbon gaseous olefins and functional monomers through the pressurized reaction of the two, and adopts a heterogeneous polymerization method to improve the monomer concentration and raw material utilization rate, and synthesizes olefin functional polymers of different molecular weights by adjusting the process parameters, with high reaction efficiency; after the polymerization of the present application is completed, a relatively stable emulsion dispersion system can be directly obtained, the post-processing process is simple, easy to separate and purify, the raw materials can be recycled, and the conversion rate of the raw materials and the product yield are improved; the method is simple to operate, the reaction conditions are mild, energy consumption is saved, the cost is low, and it is green and environmentally friendly.

[0204] (II) Applications of olefin-based functional polymers

[0205] The specific embodiment of the present application provides a use of an olefin-based functional polymer, which includes the following steps:

[0206] (1) After introducing a low-carbon olefin into a reactor and raising the temperature and pressure to reach the reaction temperature and pressure, a raw material liquid prepared from a functional monomer, an initiator, and a solvent is added into the reactor to cause a polymerization reaction;

[0207] (2) subjecting the material after the polymerization reaction in step (1) to gas-solid-liquid separation to recover the light olefins, and subjecting the remaining material to solid-liquid separation after discharge to obtain a solid-phase olefin functional polymer and a liquid-phase material;

[0208] (3) mixing the olefin functional polymer obtained in step (2) with a matrix resin and a filler to obtain a modified reinforced resin;

[0209] Esterifying the olefin functional polymer obtained in step (2) with alcohols to obtain an adhesive;

[0210] The olefin functional polymer obtained in step (2) is subjected to anionization and cationization reaction to obtain a scale inhibitor;

[0211] Alternatively, the olefin functional polymer obtained in step (2) is mixed with a coupling agent, a pH regulator, and water to obtain a glass fiber sizing.

[0212] The following are typical but non-limiting examples of this application:

[0213] Example II-1:

[0214] This embodiment provides a method for synthesizing an olefin functional polymer, the method comprising the following steps:

[0215] (1) After introducing a low-carbon olefin into a tubular reactor, the temperature and pressure are increased, wherein the low-carbon olefin is ethylene, and nitrogen is introduced before the low-carbon olefin is introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the tubular reactor, wherein the functional monomer is maleic anhydride, the initiator is azobisisoheptanonitrile, the solvent is n-heptane, the molar ratio of the initiator to the functional monomer is 0.2:1, and the mass ratio of the solvent to the functional monomer is 50:1, and a polymerization reaction occurs. The polymerization reaction temperature is 60°C, the pressure is 5 MPa, and the residence time is 10 h. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0216] (2) The material after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins, the discharged light olefins are pressurized and returned to step (1) for reuse, the remaining material is discharged in a solid-liquid manner and then filtered with nitrogen, the obtained filter cake is washed and dried, the washing solvent is n-hexane, and a solid-phase olefin functional polymer and a liquid-phase material are obtained, wherein the olefin functional polymer is a microspherical particle; the liquid-phase material is distilled, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse, respectively, to prepare the raw material liquid and wash the filter cake.

[0217] Example II-2:

[0218] This embodiment provides a method for synthesizing an olefin functional polymer, the method comprising the following steps:

[0219] (1) After a low-carbon olefin is introduced into a microchannel reactor, the temperature and pressure are increased, wherein the low-carbon olefin is ethylene, and nitrogen is first introduced before the low-carbon olefin is introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the reactor, wherein the functional monomer is maleic anhydride, the initiator is azobisisovaleronitrile, and the solvent is ethyl benzoate. The molar ratio of the initiator to the functional monomer is 0.1:1, and the mass ratio of the solvent to the functional monomer is 25:1. A polymerization reaction occurs, wherein the polymerization reaction temperature is 90°C, the pressure is 10 MPa, and the residence time is 0.01 h. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0220] (2) The material after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins, the discharged light olefins are pressurized and returned to step (1) for reuse, the remaining material is discharged in a solid-liquid manner and then filtered with nitrogen, the obtained filter cake is washed and dried, the washing solvent is n-hexane, and a solid-phase olefin functional polymer and a liquid-phase material are obtained, wherein the olefin functional polymer is a microspherical particle; the liquid-phase material is distilled, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse and used to prepare the raw material liquid and wash the filter cake.

[0221] Example II-3:

[0222] This embodiment provides a method for synthesizing an olefin functional polymer, the method comprising the following steps:

[0223] (1) After introducing a low-carbon olefin into a reactor, the temperature and pressure are increased, wherein the low-carbon olefin is ethylene, and nitrogen is first introduced before the low-carbon olefin is introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the reactor, wherein the functional monomer is maleic anhydride, the initiator is azobisisoheptanenitrile, and the solvent is isoamyl acetate. The molar ratio of the initiator to the functional monomer is 0.015:1, and the mass ratio of the solvent to the functional monomer is 10:1. A polymerization reaction occurs, and the polymerization reaction temperature is 110°C, the pressure is 3 MPa, and the residence time is 5 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0224] (2) The material after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins, the discharged light olefins are pressurized and returned to step (1) for reuse, the remaining material is discharged in a solid-liquid manner and then filtered using nitrogen, the obtained filter cake is dried to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle; the liquid-phase material is distilled, and the top fraction after distillation is a recovered solvent, which is returned to step (1) for reuse in preparing the raw material liquid.

[0225] Example II-4:

[0226] This embodiment provides a method for synthesizing an olefin functional polymer, the method comprising the following steps:

[0227] (1) After introducing a low-carbon olefin into a tubular reactor, the temperature and pressure are increased. The low-carbon olefin is propylene. Before the low-carbon olefin is introduced, argon is replaced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the tubular reactor. The functional monomer is maleimide, the initiator is diisopropylbenzene peroxide, and the solvent is butyl acetate and xylene in a volume ratio of 1:1. The molar ratio of the initiator to the functional monomer is 0.005:1, and the mass ratio of the solvent to the functional monomer is 6:1. A polymerization reaction occurs. The polymerization reaction temperature is 120°C, the pressure is 2 MPa, and the residence time is 4 hours. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0228] (2) The material after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins, the discharged light olefins are pressurized and returned to step (1) for reuse, the remaining material is discharged in a solid-liquid manner and then filtered with argon, the obtained filter cake is washed and dried, the washing solvent is n-hexane, and a solid-phase olefin functional polymer and a liquid-phase material are obtained, wherein the olefin functional polymer is a microspherical particle; the liquid-phase material is distilled, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse, respectively, to prepare the raw material liquid and wash the filter cake.

[0229] Example II-5:

[0230] This embodiment provides a method for synthesizing an olefin functional polymer, the method comprising the following steps:

[0231] (1) After introducing a low-carbon olefin into a tubular reactor, the temperature and pressure are increased, wherein the low-carbon olefin is 1-butene, and argon is introduced before the low-carbon olefin is introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the tubular reactor, wherein the functional monomer is maleic acid, the initiator is dodecyl peroxide, and the solvent is ethyl phenylacetate. The molar ratio of the initiator to the functional monomer is 0.08:1, and the mass ratio of the solvent to the functional monomer is 20:1. A polymerization reaction occurs, wherein the polymerization reaction temperature is 100°C, the pressure is 7 MPa, and the residence time is 3 h. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0232] (2) The material after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins. The discharged light olefins are pressurized and returned to step (1) for reuse. The remaining material is discharged in a solid-liquid manner and then filtered using argon. The obtained filter cake is washed and dried. The washing solvent is n-hexane to obtain a solid-phase olefin functional polymer and a liquid-phase material. The olefin functional polymer is in the form of microspherical particles. The liquid-phase material is distilled. The top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse to prepare the raw material liquid and wash the filter cake.

[0233] Example II-6:

[0234] This embodiment provides a method for synthesizing a multi-olefin functional polymer, the method comprising the following steps:

[0235] (1) After introducing low-carbon olefins into a reactor, the temperature and pressure are increased. The low-carbon olefins are ethylene and propylene in a molar ratio of 1:1. Nitrogen is first introduced before the low-carbon olefins are introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by functional monomer, initiator, comonomer and solvent is pumped into the reactor. The functional monomer is maleic anhydride, the initiator is dibenzoyl peroxide, the solvent is cyclohexane and ethyl acetate in a volume ratio of 5:1, the comonomer is vinyl acetate, the molar ratio of the initiator to the functional monomer is 0.15:1, the mass ratio of the solvent to the functional monomer is 35:1, and the molar ratio of the comonomer to the functional monomer is 5:1. A polymerization reaction occurs. The polymerization reaction temperature is 80°C, the pressure is 6 MPa, and the residence time is 8 hours. During the polymerization reaction, low-carbon olefins are continuously introduced to maintain the pressure;

[0236] (2) The material after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the light olefins, the discharged light olefins are pressurized and returned to step (1) for reuse, the remaining material is discharged in a solid-liquid manner and then filtered with nitrogen, the obtained filter cake is washed and dried, the washing solvent is propyl ether, and a terolefin functional polymer and a liquid phase material are obtained, wherein the terolefin functional polymer is a microspherical particle; the liquid phase material is distilled, and the top fraction after distillation is the recovered solvent of each component, which is returned to step (1) and step (2) for reuse, and is used to prepare the raw material liquid and wash the filter cake.

[0237] Example II-7:

[0238] This embodiment provides a method for synthesizing an olefin functional polymer, the method comprising the following steps:

[0239] (1) After introducing a low-carbon olefin into a fluidized bed reactor, the temperature and pressure are increased, wherein the low-carbon olefin is 1-butene, and argon is introduced before the low-carbon olefin is introduced. After reaching the reaction temperature and reaction pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is pumped into the fluidized bed reactor, wherein the functional monomer is maleic anhydride, the initiator is dimethyl azobisisobutyrate and dodecyl peroxide in a molar ratio of 1:1, the solvent is ethyl acetate, the molar ratio of the initiator to the functional monomer is 0.002:1, and the mass ratio of the solvent to the functional monomer is 3:1, and a polymerization reaction occurs. The polymerization reaction temperature is 150°C, the pressure is 0.5 MPa, and the residence time is 1.5 h. During the polymerization reaction, the low-carbon olefin is continuously introduced to maintain the pressure;

[0240] The operation of step (2) is similar to that of Example 1.

[0241] Based on the content detection of the raw material monomers and the olefin functional polymer before and after the reaction in the above examples, the conversion rate of the functional monomers, the yield of the olefin functional polymer and the anhydride value were calculated, and the molecular weight and particle size of the polymer were tested and calculated. The results are shown in Table 3.

[0242] Table 3 Results of the polymerization reactions in Examples II-1 to II-7

[0243] As can be seen from Table 1, in the above Examples II-1 to II-5 and II-7, low-carbon olefins and functional monomers are used as raw materials, and the method is adopted to synthesize olefin functional polymers. The conversion rate of the functional monomers can reach more than 88%, and the polymer yield can also reach more than 95%. The acid anhydride value of the polymer is more than 60%, the molecular weight is in the range of 25,000 to 65,000, and the particle size range is 10 to 50 μm. When the comonomer is added as a raw material in Example 6, the acid anhydride value of the synthesized multi-olefin copolymer can be effectively adjusted.

[0244] Application Example 1:

[0245] This application example uses the olefin functional polymer synthesized in Example II-1 as a compatibilizer to prepare a modified reinforced resin, comprising the following steps:

[0246] An olefin functional polymer is used as a compatibilizer and mixed with a base resin PA6 and a filler glass fiber. The added amount of the base resin accounts for 67.0wt% of the total mixture, the added amount of the filler accounts for 28.7wt% of the total mixture, and the added amount of the olefin functional polymer accounts for 4.3wt% of the total mixture. The mixing method is mechanical blending, specifically comprising: preliminarily mixing the olefin functional polymer with the base resin and the filler, performing banbury mixing in a banbury mixer at a temperature of 230°C, and then extruding and granulating the mixture through a twin-screw extruder to prepare a glass fiber modified and reinforced PA6 resin.

[0247] Application Example 2:

[0248] This application example uses the olefin functional polymer synthesized in Example II-2 as a compatibilizer to prepare a modified reinforced resin, comprising the following steps:

[0249] An olefin functional polymer is used as a compatibilizer and mixed with a matrix resin PET and a filler glass fiber. The added amount of the matrix resin accounts for 73.6wt% of the total mixture, the added amount of the filler accounts for 18.4wt% of the total mixture, and the added amount of the olefin functional polymer accounts for 8wt% of the total mixture. The mixing method is solution blending, specifically comprising: dissolving the olefin functional polymer, the matrix resin and the filler in N-methylpyrrolidone solvent, mixing them uniformly and then removing the solvent. The solvent removal method is distillation to obtain a glass fiber modified and reinforced PET resin.

[0250] Application Example 3:

[0251] This application example uses the olefin functional polymer synthesized in Example II-1 to prepare an adhesive, comprising the following steps:

[0252] The olefin functional polymer is subjected to an esterification reaction with methanol, wherein the molar ratio of the acid anhydride to the methanol in the olefin functional polymer is 1:3. The esterification reaction temperature is 65° C. and the reaction time is 4 hours. The esterification product is then concentrated and dried to obtain an esterification product which can be used as an adhesive.

[0253] Application Example 4:

[0254] This application example uses the olefin functional polymer synthesized in Example II-3 to prepare an adhesive, comprising the following steps:

[0255] An olefin functional polymer is subjected to an esterification reaction with ethanol, wherein the molar ratio of the acid anhydride to the ethanol in the olefin functional polymer is 1:5, the temperature of the esterification reaction is 80°C, the time is 3 hours, and then the reaction is concentrated and dried to obtain an esterification product. The esterification product is then stirred and mixed with a tackifier, a filler, and water, wherein the tackifier includes diphenylmethane diisocyanate, and the filler includes calcium carbonate. The mass ratio of the esterification product, diphenylmethane diisocyanate, calcium carbonate, and water is 10:2:5:40, the stirring rate is 200 r / min, and the stirring time is 10 minutes to obtain an adhesive.

[0256] Application Example 5:

[0257] This application example uses the olefin functional polymer synthesized in Example II-1 to prepare a scale inhibitor, comprising the following steps:

[0258] The olefin functional polymer is subjected to an esterification reaction with methanol, wherein the molar ratio of the acid anhydride in the olefin functional polymer to the methanol is 1:5, the temperature of the esterification reaction is 65° C., the pressure is 0.13 MPa, and the time is 4 hours, followed by condensation and phase separation, and the ester-containing fraction is filtered and dried to obtain monoesterified polyethylene maleic anhydride;

[0259] The monoesterified polyethylene maleic anhydride is then mixed with epoxypropyltrimethylammonium chloride and solvent dichloromethane to react, and a sodium hydroxide alkaline solution is added at the same time. The molar ratio of the carboxyl group in the monoesterified polyethylene maleic anhydride to the epoxypropyltrimethylammonium chloride is 1:1.5. The reaction temperature is 80° C. and the reaction time is 4 hours. After the reaction, the solvent is removed by distillation under reduced pressure. The residue is recrystallized using an acetone / ethanol mixed solvent and then vacuum dried to obtain an amine salt type cationic polymer scale inhibitor.

[0260] Application Example 6:

[0261] This application example uses the olefin functional polymer synthesized in Example II-4 to prepare a scale inhibitor, comprising the following steps:

[0262] An olefin functional polymer is mixed with a sodium hydroxide solution and then subjected to a saponification reaction. The molar ratio of the acid anhydride to the sodium hydroxide in the olefin functional polymer is 1:4. The reaction temperature is 120° C. and the reaction time is 6 hours. After the reaction, water is removed by distillation under reduced pressure. The residue is washed with cyclohexane and then vacuum dried to obtain a carboxylate type anionic polymer scale inhibitor.

[0263] Application Example 7:

[0264] This application example uses the olefin functional polymer synthesized in Example II-5 to prepare a scale inhibitor, comprising the following steps:

[0265] Esterification reaction is carried out with olefin functional polymer and ethylene glycol, wherein the molar ratio of anhydride to ethylene glycol in the olefin functional polymer is 1:2, the temperature of the esterification reaction is 75° C., the pressure is 0.4 MPa, and the time is 4.5 hours, followed by condensation and phase separation, and the ester-containing fraction is filtered and dried to obtain monoesterified polyethylene maleic anhydride;

[0266] The monoesterified polyethylene maleic anhydride is dissolved in dichloromethane, and then concentrated sulfuric acid is added to react. The molar ratio of hydroxyl groups in the monoesterified polypropylene maleic anhydride to sulfuric acid is 1:2. The reaction temperature is 80° C. and the reaction time is 2 hours. After the reaction, sodium hydroxide solution is added to adjust the pH to 7. The dichloromethane is removed by distillation under reduced pressure. The residue is dried and crushed to obtain a sulfate-type anionic polymer scale inhibitor.

[0267] Application Example 8:

[0268] This application example uses the olefin functional polymer synthesized in Example II-5 to prepare a glass fiber sizing, comprising the following steps:

[0269] The olefin functional polymer is mixed with a coupling agent A-151, a lubricant stearamide, a defoaming agent polyoxypropylene glycerol ether and water, wherein the mass fraction of water is 95%, and the remaining components are calculated by mass as follows: 80% of the terolefin functional polymer, 10% of the coupling agent, 5% of the lubricant, and 5% of the defoaming agent. Specifically, the coupling agent is first added into the water and stirred for 25 minutes, and then the lubricant, the terolefin functional polymer and the defoaming agent are added and stirred for 60 minutes at a stirring rate of 800 rpm to finally obtain a glass fiber sizing.

[0270] Application Example 9:

[0271] This application example uses the terolefin functional polymer synthesized in Example II-6 to prepare a glass fiber sizing, comprising the following steps:

[0272] The method comprises the following steps: mixing a terolefin functional polymer with a coupling agent KH570, a pH regulator ammonia water, a lubricant oleic acid amide, a defoaming agent polyoxyethylene polyoxypropylene pentaerythritol ether, an antioxidant 1076 and water, wherein the mass fraction of water is 80%, and the remaining components are calculated by mass as follows: 70% of the terolefin functional polymer, 20% of the coupling agent, 5% of the defoaming agent, 1% of the antioxidant and 4% of the pH regulator. The method comprises the following steps: firstly adding the coupling agent into water and stirring for 30 minutes, then adding the lubricant, the terolefin functional polymer, the defoaming agent and the antioxidant, stirring for 80 minutes at a stirring rate of 600 rpm, and then adding the pH regulator to adjust the pH value to 9 to obtain a glass fiber sizing.

[0273] According to the above application examples, it can be seen that the olefin functional polymers synthesized by the examples can be further reacted and can be used to prepare modified reinforced resins, adhesives, scale inhibitors and glass fiber impregnation agents, and can be applied in multiple fields. The performance of the products meets the standards of corresponding types of products.

[0274] From the above embodiments, it can be seen that the present application realizes alternating copolymerization of the same chain of low-carbon gaseous olefins and liquid functional monomers by a heterogeneous polymerization method through a pressurized reaction, thereby obtaining olefin functional polymers with high functional group content, high reactivity, and wide application; by continuously feeding the raw material liquid, the concentrations of monomers and initiators in the reaction can be controlled in real time, the monomer concentration and raw material utilization rate can be increased, and the molecular weight of the olefin functional polymer can be controlled; and by using the olefin functional polymer as a reaction platform, through chemical reactions such as esterification, hydrolysis, and modification, a variety of modified materials suitable for different fields are prepared, a variety of downstream products are developed, and the application range of the olefin functional polymer is broadened; the present application has a simple operation process, mild reaction conditions, easy separation and purification, and the raw materials can be recycled, which saves energy, has low cost, and high economic benefits.

[0275] The present application uses the above-mentioned embodiments to illustrate the detailed methods of the present application. However, the present application is not limited to the above-mentioned detailed methods, that is, it does not mean that the present application must rely on the above-mentioned detailed methods to be implemented. Those skilled in the art should understand that any improvements to the present application, equivalent replacements for the methods of the present application, additions of auxiliary steps, selection of specific methods, etc., all fall within the scope of protection and disclosure of the present application.

Claims

1. A method for synthesizing olefin functional polymers in a continuous feeding manner, characterized in that: The method comprises the following steps: (1) After introducing a low-carbon olefin into a reactor, the temperature and pressure are increased. After reaching the reaction temperature and pressure, a raw material liquid prepared by a functional monomer, an initiator and a solvent is continuously fed into the reactor to cause a polymerization reaction; (2) The system after the polymerization reaction in step (1) is first subjected to gas-solid-liquid separation to recover the low-carbon olefins, and the discharged low-carbon olefins are returned to step (1) for reuse. The remaining material is discharged and then subjected to solid-liquid separation to obtain a solid-phase olefin functional polymer and a liquid-phase material.

2. The method according to claim 1, characterized in that The light olefin in step (1) includes any one of ethylene, propylene, butene or butadiene, or a combination of at least two thereof; Preferably, before the light olefin is introduced in step (1), the reactor is first evacuated and then replaced with a protective gas.

3. The method according to claim 1 or 2, characterized in that: The reactor in step (1) comprises any one of a reactor, a tubular reactor, a microchannel reactor, a fluidized bed reactor or an ebullient bed reactor; Preferably, the tubular reactor comprises any one of a horizontal tubular reactor, a vertical tubular reactor, a coil reactor or a U-shaped tubular reactor; Preferably, the microchannel reactor comprises a gas-liquid-solid three-phase catalytic microreactor.

4. The method according to any one of claims 1 to 3, characterized in that: The functional monomer in step (1) comprises any one of maleic anhydride, maleimide or maleic acid, or a combination of at least two thereof; Preferably, the initiator in step (1) comprises an azo compound and / or a peroxide compound; Preferably, the azo compound includes any one of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, azobiscyclohexylcarbonitrile or dimethyl azobisisobutyrate, or a combination of at least two thereof; Preferably, the peroxide compound includes any one of dibenzoyl peroxide, diisopropyl peroxide, diisopropyl peroxydicarbonate, diisobutyryl peroxide, di(2,4-dichlorobenzoyl) peroxide, dodecyl peroxide or tert-butyl peroxyneoheptanoate, or a combination of at least two thereof; Preferably, the solvent in step (1) comprises any one or a combination of at least two of an organic alkanoate compound, an alkane compound or an aromatic compound; Preferably, the general structural formula of the organic alkanoate compound is Wherein R1 is any one of H, C1-C20 alkane group or C6-C10 aromatic group, and R2 is any one of C1-C20 alkane group or C6-C10 aromatic group; Preferably, the alkane compound includes any one or a combination of at least two of n-hexane, cyclohexane, n-pentane, n-heptane, n-octane or n-decane; Preferably, the aromatic hydrocarbon compound includes any one of benzene, toluene, ethylbenzene or xylene, or a combination of at least two of them.

5. The method according to any one of claims 1 to 4, characterized in that: The molar ratio of the initiator to the functional monomer in step (1) is (0.001-0.2):1, preferably (0.001-0.03):1; Preferably, the mass ratio of the solvent to the functional monomer in step (1) is (2-50):1, preferably (2-10):1; Preferably, the raw material liquid in step (1) is firstly removed from impurities and preheated before being added to the reactor; Preferably, the raw material liquid in step (1) is pressurized by a delivery pump and then pumped into the reactor at a uniform speed.

6. The method according to any one of claims 1 to 5, characterized in that: The polymerization reaction temperature in step (1) is 50 to 150° C., preferably 70 to 120° C.; Preferably, the polymerization reaction pressure in step (1) is 0.1 to 10 MPa, preferably 2 to 8 MPa; Preferably, the feeding time of the raw material liquid in step (1) is 0.1 to 10 hours; Preferably, the residence time of the raw material solution in step (1) is 0.1 to 15 h; Preferably, during the polymerization reaction in step (1), light olefins are continuously introduced to maintain the pressure.

7. The method according to any one of claims 1 to 6, characterized in that: In step (2), the low-carbon olefins discharged during the gas-solid-liquid separation are recovered and replaced with protective gas; Preferably, the remaining material after recovering the light olefins in step (2) is discharged in a solid-liquid form; Preferably, the discharged low-carbon olefins are pressurized and returned to step (1) for reuse.

8. The method according to any one of claims 1 to 7, characterized in that: The solid-liquid separation method in step (2) includes any one of decantation, filtration or centrifugation or a combination of at least two thereof; Preferably, the filtration comprises any one of gravity filtration, vacuum filtration or pressure filtration; Preferably, the remaining material is filtered by protective gas, and the obtained filter cake is washed, dried and crushed; Preferably, the washing is carried out using the solvent in step (1); Preferably, the solvent used for washing further comprises an ether compound, and the ether compound comprises any one or a combination of at least two of C1-C10 saturated ether compounds, preferably diethyl ether and / or propyl ether; Preferably, the drying temperature is 30-150°C, the time is 1-72h, and the pressure is 0.1-101kPa; Preferably, the olefin functional polymer in step (2) is in the form of microspherical particles with a particle size of 10 to 50 μm.

9. The method according to any one of claims 1 to 8, characterized in that: The liquid phase material in step (2) is separated, and the recovered solvent is returned to step (1) for reuse; Preferably, the method for separating the liquid phase material comprises any one or a combination of at least two of distillation, membrane separation, washing or extraction, preferably distillation; Preferably, the recovered solvent is returned to step (1) and / or step (2) and reused for preparing the raw material solution and / or washing the filter cake.

10. The method according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: (1) After introducing a low-carbon olefin into a reactor and raising the temperature and pressure, the low-carbon olefin includes any one of ethylene, propylene, butene or butadiene or a combination of at least two thereof; the reactor includes any one of a reactor, a tubular reactor, a microchannel reactor, a fluidized bed reactor or an ebullient bed reactor; after reaching the reaction temperature and reaction pressure, a raw material liquid prepared from a functional monomer, an initiator and a solvent is added into the reactor in a continuous feeding manner; the functional monomer includes any one of maleic anhydride, maleimide or maleic acid or a combination of at least two thereof; the initiator includes an azo compound and / or a peroxide compound , the solvent includes any one or a combination of at least two of an organic alkanoate compound, an alkane compound or an aromatic compound, the molar ratio of the initiator to the functional monomer is (0.001-0.2):1, the mass ratio of the solvent to the functional monomer is (2-50):1, the raw material liquid is pressurized by a delivery pump and pumped into the reactor at a uniform speed to cause a polymerization reaction, the polymerization reaction temperature is 50-150° C., the pressure is 0.1-10 MPa, the feeding time is 0.1-10 h, the residence time is 0.1-15 h, and the low-carbon olefin is continuously introduced during the polymerization reaction to maintain the pressure; (2) subjecting the system after the polymerization reaction in step (1) to gas-solid-liquid separation, discharging the remaining low-carbon olefins during the gas-solid-liquid separation and replacing them with protective gas, returning the discharged low-carbon olefins to step (1) for reuse after being pressurized, discharging the remaining materials in a solid-liquid manner and subjecting them to solid-liquid separation, subjecting the remaining materials to filter pressure using protective gas, washing the obtained filter cake, drying it, and crushing it to obtain a solid-phase olefin functional polymer and a liquid-phase material, and drying and crushing it to obtain a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle with a particle size of 10 to 50 μm; (3) separating the liquid phase material obtained in step (2), wherein the separation method comprises any one of distillation, membrane separation, washing or extraction, or a combination of at least two thereof; and the recovered solvent obtained is returned to step (1) and / or step (2) and reused for preparing the raw material liquid and / or washing the filter cake.

11. A use of olefin functional polymers, characterized in that: The olefin functional polymer is an olefin functional polymer obtained by the method according to any one of claims 1 to 10, and the olefin functional polymer is mixed with a base resin and a filler to obtain a modified reinforced resin; preferably, the olefin functional polymer is mixed with a base resin and a filler as a compatibilizer; Preferably, the matrix resin comprises thermoplastics and / or thermosetting plastics; Preferably, the thermoplastic plastic includes any one or a combination of at least two of PC, PA, POM, PBT, PET, PVC, PS, PE or ABS; Preferably, the thermosetting plastic comprises any one of EP, UPR, PU or UF or a combination of at least two thereof; Preferably, the filler comprises an inorganic filler and / or an organic filler; Preferably, the addition amount of the matrix resin accounts for 30-90wt% of the total amount of the mixture, and the addition amount of the filler accounts for The amount of the olefin functional polymer added is 5 to 65 wt% of the total amount of the mixture, and the amount of the olefin functional polymer added is 3 to 15 wt% of the total amount of the mixture; Preferably, the mixing method includes any one of mechanical blending, solution blending or latex blending.

12. A use of olefin functional polymers, characterized in that: The olefin functional polymer is an olefin functional polymer obtained by the method according to any one of claims 1 to 10, and the olefin functional polymer is subjected to an esterification reaction with an alcohol to obtain an adhesive; Preferably, the alcohol includes any one of methanol, ethanol, propanol or butanol, or a combination of at least two thereof; Preferably, the molar ratio of anhydride to alcohol in the olefin functional polymer is 1:(2-5); Preferably, the temperature of the esterification reaction is 60-80°C; Preferably, the esterification reaction time is 3 to 5 hours; Preferably, after the esterification reaction, the product is concentrated and dried to obtain an esterification product.

13. A use of olefin functional polymers, characterized in that: The olefin functional polymer is an olefin functional polymer obtained by the method according to any one of claims 1 to 10, and the olefin functional polymer is subjected to anionization and cationization reaction to obtain a scale inhibitor; Preferably, before the anionization and cationization reaction, an esterification reaction of the olefin functional polymer and alcohols is also included to generate a monoesterified olefin functional polymer; Preferably, the alcohol includes any one of methanol, ethanol, butanol, ethylene glycol or propylene glycol, or a combination of at least two thereof; Preferably, the anionization and cationization reaction comprises the reaction of an olefin functional polymer or a monoesterified olefin functional polymer with a quaternary ammonium salt, a base or an acid; Preferably, the quaternary ammonium salt includes any one of glycidyltrimethylammonium chloride, octadecyldimethylammonium chloride, octadecylamine polyoxyethylene ether diquaternary ammonium salt or didodecylamine polyoxyethylene ether monoquaternary ammonium salt, or a combination of at least two thereof; Preferably, the base comprises caustic soda, which is added in the form of an alkaline solution; Preferably, the acid comprises any one of sulfuric acid, persulfuric acid or phosphorus pentoxide or a combination of at least two thereof; Preferably, the anionization and cationization reaction includes any one of the following or a combination of at least two of the following: a monoesterified olefin functional polymer reacts with a quaternary ammonium salt in an alkaline solution to prepare a cationic polymer scale inhibitor; a monoesterified olefin functional polymer reacts with a quaternary ammonium salt in an alkaline solution to prepare a cationic polymer scale inhibitor; a saponification reaction of an olefin functional polymer with an alkaline solution to prepare a carboxylate-type anionic polymer scale inhibitor; a diol monoesterified olefin functional polymer reacts with sulfuric acid to prepare a sulfate-type anionic polymer scale inhibitor; or a diol monoesterified olefin functional polymer reacts with phosphorus pentoxide to prepare a phosphate-type anionic polymer scale inhibitor.

14. A use of olefin functional polymers, characterized in that: The olefin functional polymer is an olefin functional polymer obtained by the method according to any one of claims 1 to 10, and the olefin functional polymer is mixed with a coupling agent, a pH regulator, and water to obtain a glass fiber sizing; Preferably, the coupling agent includes any one of a silane coupling agent, an aluminate coupling agent or a titanate coupling agent, or a combination of at least two thereof; The pH regulator includes an acid regulator or an alkali regulator; Preferably, the acid regulator comprises any one of acetic acid, citric acid, formic acid or oxalic acid, or a combination of at least two thereof; Preferably, the alkaline regulator includes any one or a combination of at least two of ammonia water, sodium hydroxide, sodium bicarbonate, basic amino acids or organic amines; Preferably, the preparation step of the glass fiber sizing comprises: firstly adding a coupling agent into water and stirring, then adding an olefin functional polymer, stirring evenly, and then adding a pH regulator to obtain the glass fiber sizing; Preferably, the stirring time after the coupling agent is added is 20 to 30 minutes; Preferably, the stirring time after the addition of the olefin functional polymer is 60 to 240 minutes, and the stirring rate is 100 to 800 rpm; Preferably, after adding the pH adjuster, the pH value is adjusted to 6 to 10; Preferably, the mass proportion of water in the glass fiber sizing agent is 20-95wt%, and the rest is solid phase components; Preferably, the glass fiber sizing agent further comprises any one of a lubricant, a defoaming agent or an antioxidant, or a combination of at least two thereof; Preferably, the lubricant, defoamer and antioxidant are added during the preparation of the glass fiber sizing at the same time as the multi-olefin functional polymer.

15. A use of olefin functional polymers, characterized in that: The olefin functional polymer is an olefin functional polymer obtained by the method according to any one of claims 1 to 10, and the use comprises the following steps: (1) After introducing a low-carbon olefin into a reactor and raising the temperature and pressure, the low-carbon olefin includes any one of ethylene, propylene, butene or butadiene or a combination of at least two thereof; the reactor includes any one of a kettle reactor, a tubular reactor, a microchannel reactor, a tower reactor, a fluidized bed reactor or an ebullient bed reactor; after reaching the reaction temperature and reaction pressure, a raw material liquid prepared from a functional monomer, an initiator and a solvent is added into the reactor; the functional monomer includes any one of maleic anhydride, maleimide or maleic acid or a combination of at least two thereof; the initiator includes an azo compound and / or a peroxide The solvent comprises any one or a combination of at least two of an organic alkanoate compound, an alkane compound or an aromatic compound, the molar ratio of the initiator to the functional monomer is (0.001-0.2):1, the mass ratio of the solvent to the functional monomer is (2-50):1, the raw material liquid is pressurized by a delivery pump and then pumped into the reactor at a uniform speed to cause a polymerization reaction, the polymerization reaction temperature is 50-150° C., the pressure is 0.1-10 MPa, the residence time is 10 s-10 h, and light olefins are continuously introduced during the polymerization reaction to maintain the pressure; (2) subjecting the material after the polymerization reaction in step (1) to gas-solid-liquid separation, recovering the low-carbon olefins, returning the discharged low-carbon olefins to step (1) after pressurization for reuse, discharging the remaining material in a solid-liquid manner for solid-liquid separation, filtering with protective gas, washing and drying the obtained filter cake, and obtaining a solid-phase olefin functional polymer and a liquid-phase material, wherein the olefin functional polymer is a microspherical particle with a particle size of 10 to 50 μm; separating the liquid-phase material, wherein the separation method comprises any one of distillation, membrane separation, washing or extraction or a combination of at least two thereof, and returning the recovered solvent after separation to step (1) and / or step (2) for reuse to prepare a raw material liquid and / or wash the filter cake; (3) the olefin functional polymer obtained in step (2) is used as a compatibilizer to mix with a base resin and a filler, wherein the base resin comprises a thermoplastic and / or a thermosetting plastic, and the filler comprises an inorganic filler and / or an organic filler, the base resin is added in an amount of 30 to 90 wt % of the total amount of the mixture, the filler is added in an amount of 5 to 65 wt % of the total amount of the mixture, and the olefin functional polymer is added in an amount of 3 to 15 wt % of the total amount of the mixture, and the mixing method comprises any one of mechanical blending, solution blending or latex blending to obtain a modified reinforced resin; The olefin functional polymer obtained in step (2) is subjected to an esterification reaction with an alcohol, wherein the alcohol comprises any one of methanol, ethanol, propanol or butanol or a combination of at least two thereof, and the molar ratio of the anhydride to the alcohol in the olefin functional polymer is 1:(2-5), the temperature of the esterification reaction is 60-80° C., the time is 3-5 hours, and then the reaction is concentrated and dried to obtain an adhesive; The olefin functional polymer obtained in step (2) is subjected to anionization and cationization reaction to obtain a scale inhibitor; before the anionization and cationization reaction, an esterification reaction of the olefin functional polymer with an alcohol is also included to generate a monoesterified olefin functional polymer, wherein the alcohol includes any one of methanol, ethanol, butanol, ethylene glycol or propylene glycol or a combination of at least two thereof; the anionization and cationization reaction includes a reaction of the olefin functional polymer or the monoesterified olefin functional polymer with a quaternary ammonium salt, an alkali or an acid, wherein the quaternary ammonium salt includes glycidyl trimethyl ammonium chloride, octadecyl dimethyl ammonium chloride, octadecyl amine polyoxyethylene ether diquaternary ammonium salt or didodecyl amine polyoxyethylene ether monoquaternary Any one or a combination of at least two of ammonium salts; the anionization reaction includes the reaction of monoesterified olefin functional polymer with quaternary ammonium salt in alkaline solution to prepare cationic polymer scale inhibitor, the reaction of olefin functional polymer with quaternary ammonium salt in alkaline solution to prepare cationic polymer scale inhibitor, the saponification reaction of olefin functional polymer with alkaline solution to prepare carboxylate type anionic polymer scale inhibitor, the reaction of glycol monoesterified olefin functional polymer with sulfuric acid to prepare sulfate type anionic polymer scale inhibitor or the reaction of glycol monoesterified olefin functional polymer with phosphorus pentoxide to prepare phosphate type anionic polymer scale inhibitor. Alternatively, the olefin functional polymer obtained in step (2) is mixed with a coupling agent, a pH adjusting agent and water, specifically comprising: first adding the coupling agent into water and stirring for 20 to 30 minutes, then adding a lubricant, an olefin functional polymer, a defoaming agent and an antioxidant, stirring for 60 to 240 minutes at a stirring rate of 100 to 800 rpm, and then adding a pH adjusting agent to adjust the pH value to 6 to 10 to obtain a glass fiber sizing; wherein the coupling agent comprises any one of a silane coupling agent, an aluminate coupling agent or a titanate coupling agent or a combination of at least two thereof, the pH adjusting agent comprises an acid adjusting agent or an alkali adjusting agent, and the mass proportion of water in the glass fiber sizing is 20 to 95 wt %, and the rest is a solid phase component.

Citation Information

Patent Citations

  • Preparation method of water soluble dispersant

    CN103304736A

  • Method and device for using 2-butene-containing carbon tetra-light hydrocarbon

    CN107722175A

  • Mixed C4 utilizing method and device

    CN107722177A

  • High-dipping-property alkali-free glass fiber impregnating agent for LFT reinforced polypropylene as well as application thereof

    CN108996923A

  • Reaction device and method for preparing light hydrocarbon alternating copolymerization microsphere

    CN111087539A