Method for producing modified (METH)acrylic resin
The described method for producing (meth)acrylic resins through UV-irradiated RAFT polymerization addresses the challenge of achieving narrow molecular weight distribution at high molecular weights, enhancing material properties and adhesion in photocrosslinkable cured products.
Patent Information
- Application Number
- PCT/JP2024/013451
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-04-01
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional methods for producing (meth)acrylic resins struggle to achieve a desired molecular weight with a narrow molecular weight distribution, especially at high molecular weights, due to difficulties in controlling production conditions and suppressing free radical polymerization.
A method involving UV-irradiated reversible addition-fragmentation chain transfer (RAFT) polymerization using a hydroxy group-containing (meth)acrylate and alkyl (meth)acrylate with a RAFT agent and isocyanato group-containing ethylenically unsaturated compounds to produce a modified (meth)acrylic resin with controlled weight average molecular weight and distribution.
This method enables the production of (meth)acrylic resins with a narrow molecular weight distribution even at high molecular weights, improving material properties and stability, and results in photocrosslinkable cured products with excellent adhesion and peeling properties.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Method for producing modified (meth)acrylic resin
[0001] The present disclosure relates to a method for producing a modified (meth)acrylic resin, a method for producing a curable resin composition using the modified (meth)acrylic resin obtained by the production method, and a method for producing a photocrosslinkable cured product, a dicing tape, and a dicing and die bonding integrated film using the curable resin composition.
[0002] Conventionally, (meth)acrylic resins have been used in various fields, such as various coatings, printing, paints, adhesives, color filters, and the manufacture of electronic components such as semiconductors. In particular, there is a high demand for (meth)acrylic resins as materials that enable more precise processing, for example, during the manufacture of electronic components, and various methods for producing (meth)acrylic resins have been investigated.
[0003] In order to improve various properties of materials, such as performance, precision, and quality stability, there are cases where materials with an optimal molecular weight and a narrow molecular weight distribution are required. Living radical polymerization is often used as a manufacturing method for (meth)acrylic resins to meet such needs.
[0004] For example, Patent Document 1 describes a coloring composition having a block copolymer having a weight average molecular weight (Mw) of 3,000 to 40,000 and a molecular weight distribution (Mw / Mn) of 2.5 or less. Patent Document 2 describes a method for producing a polymer using a microreactor as a method for obtaining a polymer having a narrow molecular weight distribution.
[0005] JP 2023-35200 A JP 2022-111355 A
[0006] However, in conventional production methods, it has been difficult to freely design polymers with a desired molecular weight and a narrow molecular weight distribution due to the difficulty in controlling various production conditions and uniform reaction control. In particular, it has been difficult to suppress the progress of free radical polymerization to a high level and allow living radical polymerization to proceed predominantly. Therefore, the higher the molecular weight of the designed polymer, the greater the influence of free radical polymerization, resulting in a broader molecular weight distribution.
[0007] The present disclosure provides a production method that can obtain a modified (meth)acrylic resin having a narrow molecular weight distribution even in a high molecular weight region. The present disclosure also relates to a method for producing a curable resin composition using the modified (meth)acrylic resin obtained by the production method, and a method for producing a photocrosslinkable cured product, a dicing tape, and a dicing and die bonding integrated film using the curable resin composition.
[0008] The present disclosure includes the following aspects: [1] A method for producing a modified (meth)acrylic resin, comprising: a step (i) of performing reversible addition-fragmentation chain transfer (RAFT) polymerization, while irradiating a reaction raw material liquid containing raw material monomers (M) containing a hydroxy group-containing (meth)acrylate (m-1) and an alkyl (meth)acrylate (m-2), as well as a radical polymerization initiator and a RAFT agent, to obtain a copolymer (A-0); and a step (ii) of adding an isocyanato group-containing ethylenically unsaturated compound (a) to some of the side chain hydroxy groups of the copolymer (A-0) to obtain a modified (meth)acrylic resin (A) having an ethylenically unsaturated group. [2] A method for producing a modified (meth)acrylic resin according to [1], wherein the step (i) is performed by solution polymerization, and the total concentration of components excluding the solvent in the reaction raw material liquid is 30 to 90 mass%. [3] The method for producing a modified (meth)acrylic resin according to [1] or [2], wherein in the step (i), 0.0002 to 1.7 parts by mass of the radical polymerization initiator and 0.0005 to 10 parts by mass of the RAFT agent are used relative to 100 parts by mass of the raw material monomer group (M). [4] The method for producing a modified (meth)acrylic resin according to any of [1] to [3], wherein the RAFT agent is a trithiocarbonate. [5] The method for producing a modified (meth)acrylic resin according to any of [1] to [4], wherein in the step (i), 5 to 50 mol % of the hydroxy group-containing (meth)acrylate (m-1) and 50 to 95 mol % of the alkyl (meth)acrylate (m-2) are used relative to 100 mol % of the raw material monomer group (M). [6] The method for producing a modified (meth)acrylic resin according to any one of [1] to [5], wherein the weight average molecular weight (Mw) of the modified (meth)acrylic resin (A) is 7,000 to 1,500,000 and the molecular weight distribution (Mw / Mn) is 1.1 to 3.0.[7] The method for producing a modified (meth)acrylic resin according to any one of [1] to [6], wherein 0.5 to 49 moles of the isocyanato group-containing ethylenically unsaturated compound (a) are used in the step (ii) relative to 100 moles of the raw material monomer group (M) in the step (i), and the ratio of the number of moles of the isocyanato group-containing ethylenically unsaturated compound (a) in the step (ii) to the number of moles of the hydroxy group-containing (meth)acrylate (m-1) in the step (i) is 30 to 99%. [8] In the step (i), the UV irradiance is 1 to 50 mW / cm. 2and polymerization is carried out under conditions of 10 to 40°C. [9] A method for producing a modified (meth)acrylic resin according to any one of [1] to [8], wherein in step (i), UV irradiation time is 1 to 50 hours.
[10] A method for producing a curable resin composition, comprising step (iii) of mixing the modified (meth)acrylic resin (A) obtained by the production method according to any one of [1] to [9], a photopolymerization initiator (B), and a crosslinking agent (C).
[11] A method for producing a curable resin composition according to
[10] , wherein the crosslinking agent (C) in step (iii) is at least one selected from the group consisting of polyisocyanates and polyepoxy compounds.
[12] A method for producing a photocrosslinkable cured product, comprising step (iv) of applying the curable resin composition obtained by the production method according to
[10] or
[11] onto a substrate or a release sheet, and thermally curing the composition.
[13] A method for producing a cured product, comprising the step (vi) of irradiating a photocrosslinkable cured product obtained by the production method according to
[12] with UV light to form a crosslinked structure.
[14] A method for producing a dicing tape, comprising the steps of: applying the curable resin composition obtained by the production method according to
[10] or
[11] onto a release sheet to obtain a curable resin composition layer; (iv-2) thermally curing the curable resin composition layer to obtain a photocrosslinkable cured product layer; and (iv-3) laminating a substrate on the curable resin composition layer or the photocrosslinkable cured product layer.
[15] A method for producing a dicing and die bonding integrated film, comprising the step (v) of laminating a dicing tape obtained by the production method according to
[14] and a die bonding tape.
[0009] According to the present disclosure, there is provided a production method that can obtain a modified (meth)acrylic resin with a narrow molecular weight distribution even in the high molecular weight region. Furthermore, according to the present disclosure, there is provided a method for producing a curable resin composition using the modified (meth)acrylic resin obtained by the production method, as well as a method for producing a photocrosslinkable cured product, a dicing tape, and a dicing / die bonding integrated film using the curable resin composition. According to the present disclosure, there is provided a photocrosslinkable cured product that has sufficient adhesive strength to the adhesive layer, exhibits excellent peelability, dicing properties, and pick-up properties after UV irradiation, and is less likely to cause DAF skipping.
[0010] A schematic diagram of a test piece for a tensile test is shown.
[0011] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to the embodiments described below.
[0012] In this specification, when "to" is used to describe a numerical range, the numerical values at both ends are the upper and lower limits, respectively, and are included in the numerical range. When multiple upper or lower limits are listed, numerical ranges can be created using all combinations of the upper and lower limits. Similarly, when multiple numerical ranges are listed, separate numerical ranges can be created by individually selecting and combining the upper and lower limits from those numerical ranges.
[0013] In this specification, "(meth)acrylic" means methacrylic or acrylic, "(meth)acrylate" means acrylate or methacrylate, and "(meth)acryloyloxy" means acryloyloxy or methacryloyloxy.
[0014] In this specification, the term "photocrosslinkable cured product" refers to a thermoset product of a thermosetting resin composition that has photocrosslinkability in the thermoset state. The photocrosslinkable cured product can be crosslinked by ultraviolet irradiation.
[0015] In this specification, the "weight average molecular weight" and "number average molecular weight" refer to values measured using gel permeation chromatography (GPC) at room temperature (23°C) under the following conditions and determined using a standard polystyrene calibration curve. Apparatus: Shodex™ GPC-101 (Resonac Inc.) Column: Shodex™ LF-804 (Resonac Inc.) Column temperature: 40°C Sample: 0.2% by mass solution of sample in tetrahydrofuran Flow rate: 1 mL / min Eluent: Tetrahydrofuran Detector: Shodex™ RI-71S (Resonac Inc.)
[0016] In this specification, the term "glass transition temperature (Tg)" refers to the endothermic onset temperature due to glass transition observed when a 10 mg sample is collected and subjected to differential scanning calorimetry using a differential scanning calorimeter (DSC) while changing the temperature of the sample from -100°C to 200°C at a heating rate of 10°C / min. When two or more endothermic onset temperatures are observed, Tg is the simple average of the two or more endothermic onset temperatures.
[0017] [Method for producing modified (meth)acrylic resin (A) having an ethylenically unsaturated group] The method for producing the modified (meth)acrylic resin (A) having an ethylenically unsaturated group (also simply referred to as "modified (meth)acrylic resin (A)") includes the steps of: (i) performing reversible addition-fragmentation chain transfer (RAFT) polymerization on a reaction raw material liquid containing raw material monomers (M) containing a hydroxy group-containing (meth)acrylate (m-1) and an alkyl (meth)acrylate (m-2), as well as a radical polymerization initiator and a RAFT agent, while irradiating the reaction raw material liquid with UV light, to obtain a copolymer (A-0); and (ii) adding an isocyanato group-containing ethylenically unsaturated compound (a) to some of the side chain hydroxy groups of the copolymer (A-0), to obtain the modified (meth)acrylic resin (A) having an ethylenically unsaturated group. The raw material monomer group (M) may contain other monomers (m-3).
[0018] <Step (i)> The copolymer (A-0) can be obtained by RAFT polymerization of raw material monomers (M) containing a hydroxy group-containing (meth)acrylate (m-1), an alkyl (meth)acrylate (m-2), and optionally other monomers (m-3) in the presence of a radical polymerization initiator and a reversible addition-fragmentation chain transfer agent (RAFT agent) while irradiating them with UV light. In this specification, RAFT polymerization refers to radical polymerization carried out in the presence of a RAFT agent. RAFT polymerization is a type of living radical polymerization. Living radical polymerization is generally known as a polymerization method capable of producing polymers with narrow molecular weight distributions; specific examples include atom transfer radical polymerization, organotellurium-mediated radical polymerization, and RAFT polymerization. Of these, RAFT polymerization is suitable for electronic material applications because it does not use halogens or heavy metals.
[0019] The RAFT polymerization in step (i) is carried out under UV irradiation. UV irradiation allows for control of the initiation and termination of RAFT polymerization, thereby enabling strict control of the weight-average molecular weight and molecular weight distribution of the copolymer (A-0). The weight-average molecular weight of the copolymer (A-0) can be controlled, for example, by adjusting the amounts of the radical polymerization initiator and the RAFT agent used. Furthermore, by using such a copolymer (A-0), the modified (meth)acrylic resin (A) obtained in the subsequent step (ii) can also have a strictly controlled weight-average molecular weight and molecular weight distribution. This allows for the design of a resin that has excellent quality stability as a cured product and maximizes optimal performance for various applications. Furthermore, UV irradiation allows for control of the initiation and termination of RAFT polymerization, thereby minimizing the generation of radicals during heating in the subsequent reaction step (ii). This prevents gelation and the by-production of low-molecular-weight polymers due to unintended reactions in step (ii).
[0020] The UV irradiance is preferably 1 to 50 mW / cm from the viewpoint of the radical generation rate (decomposition rate of the radical polymerization initiator). 2 and more preferably 1 to 30 mW / cm 2 and more preferably 1 to 10 mW / cm 2The UV irradiance is 1 mW / cm 2 If the UV irradiance is 50 mW / cm or more, sufficient radicals are generated and RAFT polymerization proceeds well. 2 When the temperature is equal to or lower than this, the generated radicals react sufficiently with the RAFT agent, allowing living radical polymerization to proceed preferentially over free radical polymerization. In addition, by suppressing the progress of free radical polymerization, runaway reaction due to reaction heat accompanying polymerization can be suppressed.
[0021] The irradiation time depends on the target weight-average molecular weight of copolymer (A-0), but is preferably 1 to 50 hours, more preferably 1 to 40 hours, and even more preferably 1 to 25 hours. By setting the irradiation time within the above range, the weight-average molecular weight of copolymer (A-0) can be controlled to approach the target value and the progress of free radical polymerization can be suppressed. Irradiation may be performed intermittently or continuously, but continuous irradiation is preferred. For example, irradiation may be performed intermittently in the early stages of polymerization (e.g., within 1 hour from the start of irradiation), but continuous irradiation is preferred from the perspective of efficiency after 1 hour has elapsed from the start of irradiation, and continuous irradiation from the start of irradiation is preferred from the perspective of controlling the molecular weight distribution more narrowly. If UV irradiation is performed intermittently after polymerization has progressed to a certain extent after the start of irradiation, the molecular weight distribution tends to broaden due to the generation of radicals from the radical polymerization initiator multiple times at different times.
[0022] The reaction temperature can be set appropriately depending on the type of radical polymerization initiator used, etc. The reaction temperature is preferably 10°C or higher, more preferably 15°C or higher. The reaction temperature is preferably 40°C or lower, more preferably 30°C or lower. Any combination of these lower and upper limits may be used. Since the RAFT polymerization in step (i) proceeds by UV irradiation, there is no need to heat the reaction mixture and it can be carried out at room temperature. Therefore, the progress of free radical polymerization can be suppressed to a high level, and a copolymer (A-0) having a narrow molecular weight distribution can be obtained.
[0023] The weight-average molecular weight (Mw) of copolymer (A-0) is preferably 2,000 or more, more preferably 150,000 or more, even more preferably 250,000 or more, and even more preferably 550,000 or more. The weight-average molecular weight (Mw) of copolymer (A-0) is preferably 1,450,000 or less, more preferably 1,150,000 or less, even more preferably 950,000 or less, and even more preferably 850,000 or less. Any combination of these lower and upper limits may be used. When the weight-average molecular weight is 2,000 or more, the curability when used as a curable resin composition and the strength of the photocrosslinkable cured product obtained by thermally curing the same are sufficient. For example, when the curable resin composition is used for resist applications, good curability and developability are obtained. When the curable resin composition is used in pressure-sensitive adhesive applications, it can maintain good cohesive strength when attached to an adherend, achieving the desired adhesive strength, and can reduce contamination of the adherend, such as adhesive residue, when peeled from the adherend. A weight-average molecular weight of 1,450,000 or less can appropriately suppress the viscosity when used as a curable resin composition, improving workability, such as coatability on substrates and film thickness control. For example, when the curable resin composition is used in a pressure-sensitive adhesive layer, the weight-average molecular weight is preferably 250,000 to 950,000 from the viewpoints of achieving the desired adhesive properties, suppressing adhesive residue when peeled from an adherend, and workability, and more preferably 550,000 to 850,000 from the viewpoint of maximizing the effects of the manufacturing method of the present disclosure.
[0024] The molecular weight distribution (Mw / Mn) of the copolymer (A-0) is preferably 1.1 to 3.0, more preferably 1.1 to 2.5, and even more preferably 1.1 to 2.0. By achieving a narrow molecular weight distribution, on the one hand, the copolymer (A-0) in the high molecular weight region falls within an appropriate range, making it easy to control the viscosity of the composition. On the other hand, the copolymer (A-0) in the low molecular weight region falls within an appropriate range, making it possible to suppress the effects caused by low molecular weight components. For example, when the curable resin composition is used in a pressure-sensitive adhesive layer, adhesive residue is suppressed when the pressure-sensitive adhesive sheet is peeled from the adherend.
[0025] As the polymerization method, a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method, an alternating copolymerization method, etc. Among these polymerization methods, in consideration of the addition reaction in step (ii), it is preferable to use a solution polymerization method from the viewpoint of ease of reaction.
[0026] In solution polymerization, the total concentration of components excluding the solvent in the reaction raw material liquid is preferably 30% by mass or more, more preferably 50% by mass or more, from the viewpoint of the polymerization rate of the raw material monomer group (M). On the other hand, the total concentration of components excluding the solvent in the reaction raw material liquid is preferably 90% by mass or less, more preferably 80% by mass or less. Any combination of these lower and upper limits may be used. Since step (i) is RAFT polymerization, polymerization proceeds by an equilibrium reaction. Therefore, polymerization proceeds very gently, and polymerization can be performed at a high concentration.
[0027] (Hydroxy Group-Containing (Meth)acrylate (m-1)) The hydroxy group-containing (meth)acrylate (m-1) is not particularly limited as long as it has a hydroxy group and one (meth)acryloyloxy group. Specific examples include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and (meth)acrylates having an aromatic ring and a hydroxy group, such as hydroxyphenyl (meth)acrylate and 2-hydroxy-3-phenoxypropyl (meth)acrylate. Among these, from the viewpoint of curability when combined with a crosslinking agent (C) as a curable resin composition described later, and from the viewpoint of reactivity with an isocyanato group-containing ethylenically unsaturated compound (a) described later, hydroxyalkyl(meth)acrylates are preferred, hydroxyalkyl(meth)acrylates in which the hydroxyalkyl group has 1 to 6 carbon atoms are more preferred, hydroxyalkyl(meth)acrylates in which a linear alkyl group has a hydroxy group at the terminal are even more preferred, and 2-hydroxyethyl(meth)acrylate, 3-hydroxypropyl(meth)acrylate, and 4-hydroxybutyl(meth)acrylate are particularly preferred.
[0028] The content of the hydroxy group-containing (meth)acrylate (m-1) is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 15 mol% or more, based on 100 mol% of the raw material monomer group (M). The content of the hydroxy group-containing (meth)acrylate (m-1) is preferably 50 mol% or less, more preferably 40 mol% or less, and even more preferably 35 mol% or less, based on 100 mol% of the raw material monomer group (M). Any combination of these lower and upper limits is acceptable. When the content of the hydroxy group-containing (meth)acrylate (m-1) is 5 mol% or more, the modified (meth)acrylic resin (A) has sufficient hydroxy groups, and sufficient curability can be obtained when used in combination with the crosslinking agent (C). For example, when this cured product, i.e., a photocrosslinkable cured product, is used in a pressure-sensitive adhesive layer, a pressure-sensitive adhesive layer with sufficient cohesive strength can be obtained. In addition, reaction sites for introducing ethylenically unsaturated groups can be secured. Therefore, a high crosslink density can be obtained when irradiated with UV light. As a result, when the photocrosslinkable cured product is used in the pressure-sensitive adhesive layer, better releasability can be obtained when peeling the pressure-sensitive adhesive sheet from an adherend. On the other hand, when the content of the hydroxy group-containing (meth)acrylate (m-1) is 50 mol % or less, the progress of unintended reactions in the curable resin composition can be suppressed, and the storage stability is good.
[0029] (Alkyl (meth)acrylate (m-2)) The alkyl (meth)acrylate (m-2) is not particularly limited as long as it does not have a hydroxy group and has an alkyl group and one (meth)acryloyloxy group. Specific examples include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isoamyl (meth)acrylate, and dodecyl (meth)acrylate; and alicyclic alkyl (meth)acrylates such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, ethylcyclohexyl (meth)acrylate, norbornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, isobornyl (meth)acrylate, and adamantyl (meth)acrylate. Among these, alkyl(meth)acrylates and alicyclic alkyl(meth)acrylates in which the alkyl group has 1 to 20 carbon atoms are preferred, since they can provide a viscosity suitable for coating properties even when the molecular weight is increased; and from the viewpoint of adjusting the glass transition temperature (Tg) of the modified (meth)acrylic resin (A) within a desired range when the curable resin composition is used as a pressure-sensitive adhesive, thereby improving the tackiness of the pressure-sensitive adhesive sheet and improving the releasability from an adherend after UV irradiation, one or more selected from methyl(meth)acrylate, ethyl(meth)acrylate, propyl(meth)acrylate, butyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, dodecyl(meth)acrylate, cyclohexyl(meth)acrylate, isobornyl(meth)acrylate, and dicyclopentanyl(meth)acrylate are more preferred.
[0030] The content of alkyl (meth)acrylate (m-2) is preferably 50 mol% or more, more preferably 60 mol% or more, and even more preferably 65 mol% or more, based on 100 mol% of the raw material monomer group (M). The content of alkyl (meth)acrylate (m-2) is preferably 95 mol% or less, more preferably 90 mol% or less, and even more preferably 85 mol% or less, based on 100 mol% of the raw material monomer group (M). Any combination of these lower and upper limits may be used. When the content of alkyl (meth)acrylate (m-2) is 50 mol% or more, good coatability can be obtained when used as a curable resin composition. When the curable resin composition is used as an adhesive, desired adhesive properties can be obtained depending on the application. When the content of alkyl (meth)acrylate (m-2) is 95 mol% or less, the content of hydroxy groups and ethylenically unsaturated groups in the modified (meth)acrylic resin (A) can be sufficiently ensured, and therefore a curable resin composition having balanced physical properties from the viewpoints of curability and improved crosslink density after UV irradiation can be obtained. When the curable resin composition is used in a pressure-sensitive adhesive layer, a pressure-sensitive adhesive layer having balanced physical properties from the viewpoints of cohesive strength of the pressure-sensitive adhesive layer and releasability of the pressure-sensitive adhesive sheet after UV irradiation can be obtained.
[0031] (Other Monomers (m-3)) The raw material monomer group (M) may contain another RAFT polymerizable monomer (m-3) other than (m-1) and (m-2). Specific examples include carboxy group-containing monomers; dienes such as butadiene and dicyclopentadiene; styrenes; unsaturated dicarboxylic acid diesters; and other vinyl compounds.
[0032] Examples of the carboxy group-containing monomer include unsaturated monobasic acids such as (meth)acrylic acid, crotonic acid, vinylbenzoic acid, and acrylic acid substituted with a haloalkyl, alkoxyl, halogen, nitro, or cyano at the α-position, and unsaturated dibasic acids such as itaconic acid. Among these, (meth)acrylic acid is preferred because of the ease of producing a photocrosslinkable cured product.
[0033] Specific examples of styrenes include styrene and α-, o-, m-, or p-alkyl derivatives of styrene.
[0034] Specific examples of the unsaturated dicarboxylic acid diester include diethyl citraconate, diethyl maleate, diethyl fumarate, and diethyl itaconate.
[0035] Specific examples of other vinyl compounds include norbornene (bicyclo[2.2.1]hept-2-ene), 5-methylbicyclo[2.2.1]hept-2-ene, 5-ethylbicyclo[2.2.1]hept-2-ene, tetracyclo[4.4.0.1]hept-2-ene, 2,5 .1 7,10 ] dodec-3-ene, 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-ethyltetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, tricyclo[5.2.1.0 2,6 ]dec-8-ene, tricyclo[5.2.1.0 2,6 ]dec-3-ene, tricyclo[4.4.0.1 2,5 ]undec-3-ene, tricyclo[6.2.1.0 1,8 ]undec-9-ene, tricyclo[6.2.1.0 1,8 ]undec-4-ene, tetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ] dodec-3-ene, 8-methyltetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ] dodec-3-ene, 8-ethylidenetetracyclo[4.4.0.1 2,5 .1 7,12 ] dodec-3-ene, 8-ethylidenetetracyclo[4.4.0.1 2,5 .1 7,10 .0 1,6 ] dodec-3-ene, pentacyclo[6.5.1.1 3,6 .0 2,7 .0 9,13 ]pentadec-4-ene, pentacyclo[7.4.0.1 2,5 .19,12 .0 8,13 ] Pentadec-3-ene, (meth)acrylic acid anilide, vinylpyridine, vinyl acetate, and the like.
[0036] (Reversible Addition-Fragmentation Chain Transfer Agent (RAFT Agent)) As the RAFT agent, known agents can be used without any particular limitation. Examples of RAFT agents include trithiocarbonates, dithioesters, dithiocarbonates, and dithiocarbamates. When polymerization is carried out in the presence of these RAFT agents, the polymerization proceeds while radical species undergo a chain reaction between a sulfur atom in the RAFT agent and a carbon atom adjacent to the sulfur atom. Among these, trithiocarbonates are preferred because they increase the reaction rate and reaction rate of polymerization due to the large transfer constant, and tend to narrow the molecular weight distribution.
[0037] Specific examples of the RAFT agent include sulfur-based compounds (trithiocarbonates, dithioesters, dithiocarbonates, and dithiocarbamates) represented by the following formula (1), formula (2), formula (3), or formula (4).
[0038] <Trithiocarbonate> (In formula (1), R 1a and R 1b each independently represents a hydrogen atom, a hydrocarbon group, a carboxy group, or a cyano group; R 1c represents a cyano group, a saturated or unsaturated aliphatic hydrocarbon group which may be substituted with a cyano group or a carboxy group, or a phenyl group which may be substituted; R 2 represents a saturated or unsaturated aliphatic hydrocarbon group in which some of the hydrogen atoms may be substituted with carboxy groups, or a benzyl group in which some of the hydrogen atoms may be substituted with substituted carbamoyl groups, alkoxycarbonyl groups having 2 to 5 carbon atoms which may be substituted with hydroxy groups, or alkenyloxycarbonyl groups having 3 to 5 carbon atoms.
[0039] <Dithioester> (In formula (2), R 3a and R 3b each independently represents a hydrogen atom, a hydrocarbon group, or a cyano group; R 3crepresents a carboxy group, an acetoxymethyl group, or a hydrocarbon group which may be substituted with a cyano group or a carboxy group; R 4 represents a hydrocarbon group.)
[0040] <Dithiocarbonate> (In formula (3), R 5a and R 5b each independently represents a hydrogen atom, a hydrocarbon group, a carboxy group which may be substituted with a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms, or a cyano group; R 5c represents a hydrocarbon group which may be substituted with an alkoxy group, and R 6 represents a hydrocarbon group.)
[0041] <Dithiocarbamate> (In formula (4), R 7a and R 7b each independently represents a hydrogen atom or a hydrocarbon group, R 7c represents a cyano group, and R 8 and R 9 each independently represents a hydrocarbon group, or R 8 and R 9 may be bonded to form a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms or a pyrazole ring which may be substituted with a chlorine atom.
[0042] In formula (1), R 1a and R 1b Examples of the hydrocarbon group represented by the formula (1) include linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 20 carbon atoms, and among these, linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 12 carbon atoms are preferred. Examples of the hydrocarbon group include linear, branched, or cyclic saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, and octadecyl; aryl groups having 6 to 12 carbon atoms, such as phenyl; and arylalkyl groups having 7 to 10 carbon atoms, such as benzyl and phenethyl. In formula (1), R 1cExamples of the saturated or unsaturated aliphatic hydrocarbon group represented by the formula (1) include linear, branched, or cyclic, saturated or unsaturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, and among these, linear, branched, or cyclic, saturated or unsaturated aliphatic hydrocarbon groups having 1 to 12 carbon atoms are preferred. Examples of the aliphatic hydrocarbon group include linear, branched, or cyclic, saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, and octadecyl groups. In formula (1), R 1c For example, 1 to 3 hydrogen atoms of the saturated or unsaturated aliphatic hydrocarbon group represented by the formula (1) may be substituted with a carboxy group or a cyano group, and the carboxy group may be further substituted with a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms. 1c Examples of the substituent of the optionally substituted phenyl group represented by the formula (1) include a substituted carbamoyl group, an alkoxycarbonyl group having 2 to 5 carbon atoms which may be substituted with a hydroxy group, and an alkenyloxycarbonyl group having 3 to 5 carbon atoms. Examples of the substituent of the substituted carbamoyl group include a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms which may be substituted with a hydroxy group or an acetyloxy group. In formula (1), R 2 Examples of the saturated or unsaturated aliphatic hydrocarbon group represented by the formula (1) include linear, branched, or cyclic saturated or unsaturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, and among these, aliphatic hydrocarbon groups having 1 to 12 carbon atoms are preferred. Examples of the aliphatic hydrocarbon group include linear, branched, or cyclic saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a cyclohexyl group, a dodecyl group, and an octadecyl group. In formula (1), R 2 In formula (1), for example, 1 to 3 hydrogen atoms of the saturated or unsaturated aliphatic hydrocarbon group represented by the formula (1) may be substituted with a carboxy group. 2Examples of the substituent of the substituted carbamoyl group of the optionally substituted benzyl group represented by the formula (I) include saturated aliphatic hydrocarbon groups having 1 to 3 carbon atoms which may be substituted with a hydroxy group or an acetyloxy group. 1a and R 1b are each independently a hydrogen atom, a hydrocarbon group having 1 to 4 carbon atoms, a carboxy group, or a cyano group, and R 1c is a hydrocarbon group having 1 to 4 carbon atoms which may be substituted with a carboxy group, or a phenyl group which may be substituted, and R 2 is a linear, branched or cyclic, saturated or unsaturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, or an optionally substituted benzyl group, and 1a and R 1b is a hydrogen atom, a combination of a methyl group or an ethyl group with a carboxy group, or a hydrogen atom, and R 1c is a methyl group, an ethyl group, or an optionally substituted phenyl group, and R 2 is a linear saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms, or a benzyl group in which some of the hydrogen atoms may be substituted with a substituted carbamoyl group, an alkoxycarbonyl group having 2 to 5 carbon atoms which may be substituted with a hydroxy group, or an alkenyloxycarbonyl group having 3 to 5 carbon atoms, is more preferred.
[0043] In formula (2), R 3a , R 3b , R 3c and R 4Examples of the hydrocarbon group represented by the formula (2) include linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 20 carbon atoms, and among these, linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 12 carbon atoms are preferred. Examples of the hydrocarbon group include linear, branched, or cyclic saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, and octadecyl; aryl groups having 6 to 12 carbon atoms, such as phenyl; and arylalkyl groups having 7 to 10 carbon atoms, such as benzyl and phenethyl. In formula (2), R 3c Examples of the hydrocarbon group represented by the formula (I) which may be substituted with a cyano group or a carboxy group include the above-mentioned hydrocarbon group in which 1 to 3 hydrogen atoms have been substituted with a cyano group or a carboxy group. 3a and R 3b are each independently a linear saturated hydrocarbon group having 1 to 4 carbon atoms, and R 3c is an aryl group, and R 4 is an aryl group or a benzyl group, and 3a and R 3b are each independently a methyl group or an ethyl group, and R 3c is a phenyl group, and R 4 More preferred are compounds of formula (2) in which is a phenyl group or a benzyl group.
[0044] In formula (3), R 5a , R 5b , R 5c and R 6Examples of the hydrocarbon group represented by the formula (3) include linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 20 carbon atoms, and among these, linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 12 carbon atoms are preferred. Examples of the hydrocarbon group include linear, branched, or cyclic saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, and octadecyl; aryl groups having 6 to 12 carbon atoms, such as phenyl; and arylalkyl groups having 7 to 10 carbon atoms, such as benzyl and phenethyl. In formula (3), R 5c Examples of the hydrocarbon group which may be substituted with an alkoxy group include the above hydrocarbon group in which 1 to 3 hydrogen atoms have been substituted with an alkoxy group.
[0045] In formula (4), R 7a , R 7b , R 8 and R 9 Examples of the hydrocarbon group represented by the formula (I) include linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 20 carbon atoms, and among these, linear, branched, or cyclic, saturated or unsaturated hydrocarbon groups having 1 to 12 carbon atoms are preferred. Examples of the hydrocarbon group include linear, branched, or cyclic saturated aliphatic hydrocarbon groups having 1 to 20 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclohexyl, dodecyl, and octadecyl; aryl groups having 6 to 12 carbon atoms, such as phenyl; and arylalkyl groups having 7 to 10 carbon atoms, such as benzyl and phenethyl. R 8 and R 9 may form a pyrazole ring together with the nitrogen atom of formula (4). The pyrazole ring may be substituted with a saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms or a chlorine atom.
[0046] Many RAFT agents are commercially available, and those that are not commercially available can be easily synthesized by known or conventional methods.
[0047] Specific examples of RAFT agents include S-cyanomethyl-S-dodecyltrithiocarbonate, 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid, bis{4-[ethyl-(2-hydroxyethyl)carbamoyl]benzyl}trithiocarbonate, 4-[(2-carboxyethylsulfanylthiocarbonyl)sulfanyl]-4-cyanopentanoic acid, and 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid. S,S-dibenzyltrithiocarbonate, methyl 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoate, 2-cyano-2-propyldodecyltrithiocarbonate, bis[4-(allyloxycarbonyl)benzyl]trithiocarbonate, bis[4-(2,3-dihydroxypropoxycarbonyl)benzyl]trithiocarbonate, bis{4-[ethyl-(2-acetyloxyethyl)carbamoyl]benzyl}trithiocarbonate, bis[4-(2-hydroxyethoxycarbonyl)benzyl]trithiocarbonate trithiocarbonates such as cyanoethyl dithiopropionate, benzyl dithiopropionate, benzyl dithiobenzoate, acetoxyethyl dithiobenzoate, 2-phenyl-2-propyldithiobenzoic acid, 2-cyano-2-propyldithiobenzoic acid, 4-cyano-4-(phenylcarbonothioylthio)pentanoic acid, and S-(thiobenzoyl)thioglycolic acid; dithioesters such as ethyl 2-[(ethoxycarbonothioyl)thio]propionate, O-ethyl-S-(2-propoxyethyl)dithiocarbonate, dithiocarbonates such as dithiocarbonate and O-ethyl-S-(1-cyano-1-methylethyl)dithiocarbonate; and dithiocarbamates such as 2-cyano-2-propyldiethyldithiocarbamate, 2'-cyanobutan-2'-yl 4-chloro-3,5-dimethylpyrazole-1-dithiocarbamate, 2'-cyanobutan-2'-yl 3,5-dimethylpyrazole-1-dithiocarbamate, cyanomethyl 3,5-dimethylpyrazole-1-dithiocarbamate, and cyanomethyl N-methyl-N-phenyldithiocarbamate.Of these, from the viewpoint of ease of polymerization of the modified (meth)acrylic resin (A), trithiocarbonates and dithioesters are preferred, and 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid, 2-{[(2-carboxyethyl)sulfanylthiocarbonyl]sulfanyl}propanoic acid, 2-phenyl-2-propyldithiobenzoic acid, S,S-dibenzyltrithiocarbonate, and bis{4-[ethyl-(2-acetyloxyethyl)carbamoyl]benzyl}trithiocarbonate are more preferred.
[0048] The RAFT agents may be used alone or in combination of two or more.
[0049] The weight-average molecular weight of the polymer to be synthesized can be adjusted by adjusting the amount of the RAFT agent used. The amount of the RAFT agent used relative to 100 parts by mass of the total amount of the raw material monomer group (M) is preferably 0.0005 to 10 parts by mass when the target weight-average molecular weight of the polymer (copolymer (A-0)) is 2,000 to 1,450,000, preferably 0.0008 to 0.4 parts by mass when the target weight-average molecular weight of the polymer is 150,000 to 1,150,000, preferably 0.001 to 0.2 parts by mass when the target weight-average molecular weight of the polymer is 250,000 to 950,000, and preferably 0.002 to 0.1 parts by mass when the target weight-average molecular weight of the polymer is 550,000 to 850,000. When the amount is 0.0005 parts by mass or more, polymerization can be performed with an efficient reaction time. When the amount is 10 parts by mass or less, a copolymer (A-0) with a sufficiently high molecular weight can be obtained. For example, when used in pressure-sensitive adhesive applications, it is preferable to use a modified (meth)acrylic resin (A) having a weight-average molecular weight of 300,000 or more, and in this case, the amount of the RAFT agent used is preferably 0.0005 to 0.2 parts by mass.
[0050] (Radical Polymerization Initiator) RAFT polymerization is carried out in the presence of a radical polymerization initiator. Since the RAFT polymerization in step (i) is carried out under UV irradiation, a photopolymerization initiator is used as the radical polymerization initiator. Examples of the radical polymerization initiator include carbonyl-based photopolymerization initiators, sulfide-based photopolymerization initiators, quinone-based photopolymerization initiators, sulfochloride-based photopolymerization initiators, and thioxanthone-based photopolymerization initiators.
[0051] Specific examples include benzophenone, benzil, benzoin, ω-bromoacetophenone, chloroacetone, acetophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bisdiethylaminobenzophenone, Michler's ketone, benzoin methyl ether, benzoin isobutyl ether, benzoin-n-butyl ether, benzyl methyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methyl carbonyl-based photopolymerization initiators such as dibenzoyl formate, 4'-dimethylaminoacetophenone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one; sulfide-based photopolymerization initiators such as diphenyl disulfide, dibenzyl disulfide, tetraethylthiuram disulfide, and tetramethylammonium monosulfide; acyl phosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide; quinone-based photopolymerization initiators such as benzoquinone and anthraquinone; sulfochloride-based photopolymerization initiators; and thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, and 2-methylthioxanthone.
[0052] Among these radical polymerization initiators, from the viewpoint of solubility in a solvent, carbonyl-based photopolymerization initiators and acylphosphine oxides are preferred, and it is more preferred to use at least one selected from 1-hydroxycyclohexyl phenyl ketone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0053] The radical polymerization initiators may be used alone or in combination of two or more.
[0054] The weight-average molecular weight of the polymer to be synthesized can be adjusted by adjusting the amount of radical polymerization initiator used. The amount of radical polymerization initiator used per 100 parts by mass of the total amount of raw material monomer group (M) is preferably 0.0002 to 1.7 parts by mass when the target weight-average molecular weight of the polymer (copolymer (A-0)) is 2,000 to 1,450,000, 0.0005 to 0.1 parts by mass when the target weight-average molecular weight of the polymer is 150,000 to 1,150,000, 0.0008 to 0.08 parts by mass when the target weight-average molecular weight of the polymer is 250,000 to 950,000, and 0.001 to 0.02 parts by mass when the target weight-average molecular weight of the polymer is 550,000 to 850,000. When the amount is 0.0002 parts by mass or more, polymerization can be performed with an efficient reaction time. When the amount is 1.7 parts by mass or less, a copolymer (A-0) with a sufficiently high molecular weight can be obtained. For example, when used in pressure-sensitive adhesive applications, it is preferable to use a modified (meth)acrylic resin (A) having a weight-average molecular weight of 300,000 or more, and in this case, the amount of radical polymerization initiator used is preferably 0.0002 to 0.07 parts by mass.
[0055] The molar ratio of the radicals generated from the radical polymerization initiator to the RAFT agent is preferably 1.0:1.0 to 1.0:1.3, from the viewpoint of preferentially proceeding living radical polymerization over free radical polymerization.
[0056] (Solvent) The solvent that may be used in step (i) may be a common solvent. Examples of the solvent include esters such as ethyl acetate, propyl acetate, and butyl acetate; aromatic hydrocarbons such as toluene, xylene, and benzene; aliphatic hydrocarbons such as hexane and heptane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; ketones such as methyl ethyl ketone and methyl isobutyl ketone; glycols such as ethylene glycol, propylene glycol, and dipropylene glycol; glycol ethers such as methyl cellosolve, propylene glycol monomethyl ether, and dipropylene glycol monomethyl ether; glycol esters such as ethylene glycol diacetate and propylene glycol monomethyl ether acetate. The solvent may be used alone or in combination of two or more.
[0057] <Step (ii)> The modified (meth)acrylic resin (A) is obtained by adding an isocyanato group-containing ethylenically unsaturated compound (a) to some of the side chain hydroxy groups derived from the hydroxy group-containing (meth)acrylate (m-1) of the copolymer (A-0). Adding the isocyanato group-containing ethylenically unsaturated compound (a) to all of the side chain hydroxy groups of the copolymer (A-0) would eliminate sites for reaction with the crosslinking agent (C) described below, so addition is limited to some of the side chain hydroxy groups. Specifically, when the side chain hydroxy groups are taken as 100 mol %, it is preferable that 30 to 99 mol % be subjected to the addition reaction. The method for adding the isocyanato group-containing ethylenically unsaturated compound (a) is not particularly limited, and methods known in the technical field of this specification can be used. Because the modified (meth)acrylic resin (A) has an ethylenically unsaturated group in its side chain, the length of the molecular chain between crosslinking points is relatively short compared to a (meth)acrylic copolymer having an ethylenically unsaturated group introduced at the terminal, and the crosslinking density can be efficiently improved by UV irradiation. Therefore, when the modified (meth)acrylic resin (A) is used as a pressure-sensitive adhesive material, the adhesive strength can be significantly reduced after UV irradiation. Therefore, a pressure-sensitive adhesive sheet using the modified (meth)acrylic resin (A) has excellent peelability from an adherend. In addition, because the modified (meth)acrylic resin (A) has an appropriate molecular weight distribution, a pressure-sensitive adhesive composition produced using the modified (meth)acrylic resin (A) has excellent adhesion to an adhesive layer. Therefore, a pressure-sensitive adhesive composition produced using the modified (meth)acrylic resin (A) is suitable for use in a pressure-sensitive adhesive layer of a dicing / die-bonding integrated film.
[0058] The molecular weight distribution (Mw / Mn) of the modified (meth)acrylic resin (A) is preferably 1.1 to 3.0, more preferably 1.1 to 2.5, and even more preferably 1.1 to 2.0. By achieving a narrow molecular weight distribution, on the one hand, the modified (meth)acrylic resin (A) in the high molecular weight region falls within an appropriate range, making it easy to control the viscosity of the composition. On the other hand, the modified (meth)acrylic resin (A) in the low molecular weight region falls within an appropriate range, making it possible to suppress the effects caused by low molecular weight components. For example, when the curable resin composition is used in a pressure-sensitive adhesive layer, adhesive residue is suppressed when the pressure-sensitive adhesive sheet is peeled from the adherend.
[0059] The weight average molecular weight (Mw) of the modified (meth)acrylic resin (A) is preferably 7,000 or more, more preferably 200,000 or more, even more preferably 300,000 or more, and even more preferably 600,000 or more. The weight average molecular weight (Mw) of the modified (meth)acrylic resin (A) is preferably 1,500,000 or less, more preferably 1,200,000 or less, even more preferably 1,000,000 or less, and even more preferably 900,000 or less. Any combination of these lower and upper limits may be used. When the weight average molecular weight is 7,000 or more, the curability when used as a curable resin composition and the strength of the photocrosslinkable cured product obtained by thermally curing the same are sufficient. For example, when the curable resin composition is used for resist applications, good curability and developability are obtained. When the curable resin composition is used in pressure-sensitive adhesive applications, it can maintain good cohesive strength when attached to an adherend, thereby achieving the desired adhesive strength, and can reduce contamination of the adherend, such as adhesive residue, when peeled from the adherend. A weight-average molecular weight of 1,500,000 or less can appropriately suppress the viscosity when used as a curable resin composition, improving workability, such as coatability to a substrate and film thickness control. For example, when the curable resin composition is used in a pressure-sensitive adhesive layer, the weight-average molecular weight is preferably 300,000 to 1,000,000 from the viewpoints of achieving the desired adhesive properties, suppressing adhesive residue when peeled from an adherend, and workability, and more preferably 600,000 to 900,000 from the viewpoint of maximizing the effects of the manufacturing method of the present invention.
[0060] The ethylenically unsaturated group equivalent of the modified (meth)acrylic resin (A) is preferably 100 g / mol or more, more preferably 250 g / mol or more, and even more preferably 500 g / mol or more. The ethylenically unsaturated group equivalent of the modified (meth)acrylic resin (A) is preferably 5,000 g / mol or less, more preferably 3,500 g / mol or less, and even more preferably 2,500 g / mol or less. Any combination of these lower and upper limits may be used. Within the above upper and lower limit ranges, the amount of crosslinking of the photocrosslinkable cured product produced using the modified (meth)acrylic resin (A) upon UV irradiation is sufficient, and when the photocrosslinkable cured product is used in a pressure-sensitive adhesive sheet, excellent releasability when peeled from an adherend and excellent pick-up ability of fragmented elements are obtained. In this specification, the ethylenically unsaturated group equivalent of the modified (meth)acrylic resin (A) refers to the mass of the modified (meth)acrylic resin (A) per mole of ethylenically unsaturated bond. In one embodiment, the ethylenically unsaturated group equivalent of the modified (meth)acrylic resin (A) is a calculated value calculated from the charged amounts of each raw material used in the production of the modified (meth)acrylic resin (A), assuming that 100% of the raw materials have reacted. The ethylenically unsaturated group equivalent of the modified (meth)acrylic resin (A) may be calculated from the amount of halogen bonded to the modified (meth)acrylic resin (A). The amount of halogen bonded to the modified (meth)acrylic resin (A) can be evaluated in accordance with JIS K 0070:1992.
[0061] The hydroxyl value of the modified (meth)acrylic resin (A) is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, and even more preferably 15 mgKOH / g or more. The hydroxyl value of the modified (meth)acrylic resin (A) is preferably 200 mgKOH / g or less, more preferably 100 mgKOH / g or less, and even more preferably 50 mgKOH / g or less. Any combination of these lower and upper limits may be used. For example, when the curable resin composition is used in an adhesive layer, a hydroxyl value of 5 mgKOH / g or more will exhibit sufficient adhesiveness. A hydroxyl value of 200 mgKOH / g or less will suppress adhesive residue upon peeling from an adherend. The hydroxyl value of the modified (meth)acrylic resin (A) is a value measured using a mixed indicator of bromothymol blue and phenol red in accordance with JIS K0070:1992. The hydroxyl value of a resin means the mass (mg) of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of the resin is acetylated.
[0062] The glass transition temperature (Tg) of the modified (meth)acrylic resin (A) is preferably -80°C to 0°C, more preferably -70°C to -10°C, and even more preferably -60°C to -30°C. When the glass transition temperature (Tg) is -80°C or higher, the cohesive strength of a photocrosslinkable cured product produced using the modified (meth)acrylic resin (A) is enhanced. For example, when the photocrosslinkable cured product is used in a pressure-sensitive adhesive layer, sufficient strength is obtained and adhesive residue upon peeling after UV irradiation is suppressed. When the glass transition temperature (Tg) is 0°C or lower, sufficient hardness is obtained. Therefore, when a photocrosslinkable cured product produced using the modified (meth)acrylic resin (A) is used in a pressure-sensitive adhesive layer, sufficient adhesive strength to an adherend and sufficient fixation during processing of the adherend are obtained.
[0063] (Isocyanato Group-Containing Ethylenically Unsaturated Compound (a)) The isocyanato group-containing ethylenically unsaturated compound (a) is not particularly limited as long as it is a compound that does not have a hydroxy group or a carboxy group, but has one isocyanato group and an ethylenically unsaturated group. Specific examples include (meth)acryloyloxyalkyl isocyanates such as 2-isocyanatoethyl (meth)acrylate, 2-isocyanatopropyl (meth)acrylate, 3-isocyanatopropyl (meth)acrylate, 2-isocyanato-1-methylethyl (meth)acrylate, 2-isocyanato-1,1-dimethylethyl (meth)acrylate, and 4-isocyanatocyclohexyl (meth)acrylate; 2-(2-isocyanatoethyloxy)ethyl (meth)acrylate; and 1,1-(bis(meth)acryloyloxymethyl)ethyl isocyanate. Among these, from the viewpoint of ease of synthesis of the modified (meth)acrylic resin (A), (meth)acryloyloxyalkyl isocyanate is preferred, and 2-(meth)acryloyloxyethyl isocyanate is more preferred.
[0064] The amount of the isocyanato group-containing ethylenically unsaturated compound (a) used is preferably 0.5 mol or more, more preferably 1 mol or more, and even more preferably 5 mol or more, relative to 100 mol of the raw material monomer group (M) in step (i). The amount of the isocyanato group-containing ethylenically unsaturated compound (a) used is preferably 49 mol or less, more preferably 40 mol or less, and even more preferably 30 mol or less, relative to 100 mol of the raw material monomer group (M) in step (i). Any combination of these lower and upper limits may be used. When the amount of the isocyanato group-containing ethylenically unsaturated compound (a) used is 0.5 mol or more, a sufficient amount of ethylenically unsaturated groups is introduced into the copolymer (A-0), thereby improving the crosslinking efficiency after UV irradiation. When the modified (meth)acrylic resin (A) is used in the pressure-sensitive adhesive layer, better releasability can be obtained when peeling the pressure-sensitive adhesive sheet from an adherend after UV irradiation. When the amount of the isocyanato group-containing ethylenically unsaturated compound (a) used is 49 moles or less, the hydroxy group content of the modified (meth)acrylic resin (A) can be sufficiently ensured, and the curing property during thermal curing can be improved. When the modified (meth)acrylic resin (A) is used in the pressure-sensitive adhesive layer, excellent cohesive strength of the pressure-sensitive adhesive layer can be obtained. In addition, the amount of unreacted isocyanato group-containing ethylenically unsaturated compound (a) can be reduced. Therefore, when the modified (meth)acrylic resin (A) is used in the pressure-sensitive adhesive layer, a pressure-sensitive adhesive sheet with little adhesive residue can be obtained.
[0065] The ratio of the number of moles of the isocyanato group-containing ethylenically unsaturated compound (a) in step (ii) to the number of moles of the hydroxy group-containing (meth)acrylate (m-1) in step (i) is preferably 30% or more, more preferably 50% or more, and even more preferably 60% or more. The ratio of the number of moles of the isocyanato group-containing ethylenically unsaturated compound (a) in step (ii) to the number of moles of the hydroxy group-containing (meth)acrylate (m-1) in step (i) is preferably 99% or less, more preferably 90% or less, and even more preferably 80% or less. Any combination of these lower and upper limits may be used.
[0066] (Catalyst) In the addition reaction in step (ii), a known catalyst can be used, if necessary. Examples of the catalyst include urethanization catalysts such as dibutyltin dilaurate, titanium diisopropoxybis(ethylacetoacetate), tetrakis(2,4-pentanedionato)zirconium, and bismuth tris(2-ethylhexanoate).
[0067] When a catalyst is used in step (ii), the amount of the catalyst used is preferably 0.01 to 10 parts by mass, more preferably 0.02 to 5 parts by mass, and even more preferably 0.03 to 1 part by mass, per 100 parts by mass of the total of the copolymer (A-0) and the isocyanato group-containing ethylenically unsaturated compound (a).
[0068] (Polymerization inhibitor) In the addition reaction in step (ii), a known polymerization inhibitor can be used as necessary. The polymerization inhibitor can be any known one, and is not particularly limited. Examples of the polymerization inhibitor include 4-methoxyphenol, hydroquinone, methoquinone, 2,6-di-t-butylphenol, 2,2'-methylenebis(4-methyl-6-t-butylphenol), and phenothiazine. The polymerization inhibitor may be used alone, or two or more types may be used in combination.
[0069] When a polymerization inhibitor is used in step (ii), the amount of the polymerization inhibitor used is preferably 0.005 to 5 parts by mass, more preferably 0.03 to 3 parts by mass, and even more preferably 0.05 to 1.5 parts by mass, relative to 100 parts by mass of the total of the copolymer (A-0) and the isocyanato group-containing ethylenically unsaturated compound (a). When the amount of the polymerization inhibitor used is 0.005 parts by mass or more, gelation during the addition reaction can be prevented. On the other hand, when the amount of the polymerization inhibitor used is 5 parts by mass or less, sufficient exposure sensitivity of the modified (meth)acrylic resin (A) during UV irradiation can be obtained.
[0070] (Reaction Conditions) The temperature of the addition reaction is preferably 25°C to 130°C, and particularly preferably 40°C to 90°C. When the temperature of the addition reaction is 25°C or higher, a sufficient reaction rate can be obtained. When the temperature of the addition reaction is 130°C or lower, crosslinking of double bonds due to thermal radical polymerization can be prevented, preventing the formation of a gelled product.
[0071] During the addition reaction, a gas having a polymerization inhibitory effect may be introduced into the reaction system. By introducing a gas having a polymerization inhibitory effect into the reaction system, gelation during the addition reaction can be prevented.
[0072] Examples of gases that have a polymerization-inhibiting effect include gases containing oxygen to an extent that does not fall within the explosive range of the substances in the system, such as air.
[0073] It is more preferable to use a gas having a polymerization inhibitor effect in combination with a polymerization inhibitor, since this allows the amount of polymerization inhibitor used to be reduced and the polymerization inhibitor effect to be enhanced.
[0074] [Method for producing curable resin composition] <Step (iii)> The curable resin composition can be produced by a method including step (iii) of mixing a modified (meth)acrylic resin (A), a photopolymerization initiator (B), a crosslinking agent (C), and other components added as needed. The curable resin composition containing the modified (meth)acrylic resin (A) can be suitably used as a pressure-sensitive adhesive composition, and the pressure-sensitive adhesive composition is suitably used for a removable pressure-sensitive adhesive sheet, in particular, a dicing / die-bonding integrated film.
[0075] The method for mixing the components contained in the curable resin composition is not particularly limited, and the mixing can be carried out using, for example, a stirring device equipped with stirring blades such as a homodisper or a paddle blade.
[0076] (Photopolymerization Initiator (B)) Examples of the photopolymerization initiator (B) include benzophenone, benzil, benzoin, ω-bromoacetophenone, chloroacetone, acetophenone, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, 2-chlorobenzophenone, 4,4′-dichlorobenzophenone, 4,4′-bisdiethylaminobenzophenone, Michler's ketone, benzoin methyl ether, and benzoin isopropyl alcohol. butyl ether, benzoin-n-butyl ether, benzyl methyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methylbenzoyl formate, 4'-dimethylaminoacetophenone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, and other carbonyl-based photopolymerization initiators.
[0077] Examples of the photopolymerization initiator (B) include sulfide-based photopolymerization initiators such as diphenyl disulfide, dibenzyl disulfide, tetraethylthiuram disulfide, and tetramethylammonium monosulfide; acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide; quinone-based photopolymerization initiators such as benzoquinone and anthraquinone; sulfochloride-based photopolymerization initiators; and thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, and 2-methylthioxanthone.
[0078] Among these photopolymerization initiators (B), from the viewpoint of solubility in the curable resin composition, carbonyl-based photopolymerization initiators and acylphosphine oxides are preferred, and it is more preferred to use at least one selected from 1-hydroxycyclohexyl phenyl ketone and 2,4,6-trimethylbenzoyldiphenylphosphine oxide.
[0079] The photopolymerization initiator (B) may be used alone or in combination of two or more kinds.
[0080] The amount of the photopolymerization initiator (B) is preferably 0.1 to 5.0 parts by mass, more preferably 0.5 to 2.0 parts by mass, per 100 parts by mass of the modified (meth)acrylic resin (A). When the content of the photopolymerization initiator (B) per 100 parts by mass of the modified (meth)acrylic resin (A) is 0.1 parts by mass or more, the crosslink density of the photocrosslinkable cured product can be improved at a sufficiently fast curing rate upon UV irradiation. Therefore, when the photocrosslinkable cured product is used in the pressure-sensitive adhesive layer, the adhesive strength of the pressure-sensitive adhesive layer after UV irradiation can be sufficiently reduced. When the content of the photopolymerization initiator (B) per 100 parts by mass of the modified (meth)acrylic resin (A) is 5.0 parts by mass or less, the effect of the photopolymerization initiator (B) on the properties of the cured product can be suppressed. For example, when a pressure-sensitive adhesive sheet having a photocrosslinkable cured product as a pressure-sensitive adhesive layer is attached to an adherend and then peeled off, the pressure-sensitive adhesive layer is less likely to remain on the adherend. Even if the content of the photopolymerization initiator (B) exceeds 5.0 parts by mass relative to 100 parts by mass of the (meth)acrylic resin (A), an effect commensurate with the content of the photopolymerization initiator (B) is not observed. Therefore, by setting the content to 5.0 parts by mass or less, the curable resin composition can be produced economically.
[0081] (Crosslinking Agent (C)) The crosslinking agent (C) is a compound that does not have an ethylenically unsaturated bond and has two or more functional groups that react with the hydroxy groups and / or carboxy groups, which are optional functional groups, contained in the modified (meth)acrylic resin (A). By heating, the functional groups of the crosslinking agent (C) react with the hydroxy groups of the modified (meth)acrylic resin (A), thereby curing the curable resin composition and obtaining a photocrosslinkable cured product. When the photocrosslinkable cured product is used in the pressure-sensitive adhesive layer, a pressure-sensitive adhesive sheet that has a good balance between adhesive strength before and after UV irradiation can be obtained.
[0082] The crosslinking agent (C) is not particularly limited, but a compound having two or more functional groups reactive with a hydroxy group is preferred. When the modified (meth)acrylic resin (A) has a carboxy group, a compound having two or more functional groups reactive with a carboxy group may be used. Examples of functional groups reactive with a hydroxy group include an isocyanato group, an epoxy group, a carboxy group, an acid anhydride group, and an aziridinyl group. From the viewpoint of reactivity, an isocyanato group and an epoxy group are preferred, and an isocyanato group is particularly preferred. Examples of functional groups reactive with a carboxy group include an epoxy group, a hydroxy group, and an aziridinyl group. From the viewpoint of reactivity, an epoxy group and an aziridinyl group are preferred.
[0083] Examples of the crosslinking agent (C) include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, hydrogenated tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, isocyanurate of hexamethylene diisocyanate, tetramethylxylylene diisocyanate, 1,5-naphthalene diisocyanate, tetramethylxylylene ... Polyisocyanates such as tolylene diisocyanate adduct of trimethylolpropane, xylylene diisocyanate adduct of trimethylolpropane, triphenylmethane triisocyanate, methylenebis(4-phenylmethane)triisocyanate; 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, bisphenol A-epichlorohydrin type epoxy resin, N,N'-[1,3-phenylenebis(methylene)]bis[bis(oxiran-2-ylmethyl)amine], ethylene glycol polyepoxy compounds such as ethanol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerin diglycidyl ether, glycerin triglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane triglycidyl ether, sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, and diglycerol polyglycidyl ether; Aziridine compounds such as N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), and N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide); melamine compounds such as hexamethoxymethylmelamine, hexaethoxymethylmelamine, hexapropoxymethylmelamine, hexabutoxymethylmelamine, hexapentyloxymethylmelamine, and hexahexyloxymethylmelamine;Examples of aziridinyl compounds include ethylene glycol bis-[3-(2-aziridinyl)propionate], trimethylolpropane tris[3-(2-aziridinyl)propionate], trimethylolpropane tris[3-(1-aziridinyl)propionate], trimethylolpropane tris[3-(2-methyl-1-aziridinyl)propionate], tetramethylolmethane tris[3-(2-aziridinyl)propionate], pentaerythritol tris[3-(1-aziridinyl)propionate], N,N'-diphenylmethane-4,4'-bis(1-aziridinylcarboxamide), and N,N'-hexamethylene-1,6-bis(1-aziridinylcarboxamide);
[0084] Among these crosslinking agents (C), it is preferable to use at least one selected from the group consisting of polyisocyanates and polyepoxy compounds, and it is more preferable to use polyisocyanates, because they have good reactivity with the modified (meth)acrylic resin (A).
[0085] The crosslinking agent (C) may be used alone or in combination of two or more kinds.
[0086] The crosslinking agent (C) is preferably present in an amount of 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, even more preferably 0.1 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the modified (meth)acrylic resin (A). When the content of the crosslinking agent (C) per 100 parts by mass of the modified (meth)acrylic resin (A) is 0.1 parts by mass or more, a three-dimensional crosslinked structure is sufficiently formed in the photocrosslinkable cured product upon UV irradiation. Therefore, when the photocrosslinkable cured product is used as an adhesive, the adhesive strength of the adhesive after UV irradiation can be sufficiently reduced. When the content of the crosslinking agent (C) per 100 parts by mass of the (meth)acrylic resin (A) is 30 parts by mass or less, the properties of the photocrosslinkable cured product and the cured product after UV irradiation are well balanced. When the photocrosslinkable cured product is used as an adhesive, the adhesive strength of the adhesive before UV irradiation is good.
[0087] (Other Components) In the method for producing the curable resin composition, if necessary, components other than the modified (meth)acrylic resin (A), the photopolymerization initiator (B), and the crosslinking agent (C) may be mixed in. Examples of the other components include a tackifier, a solvent, and various additives.
[0088] <<Tackifier>> Conventional known tackifiers can be used without any particular limitation. Examples of tackifiers include terpene-based tackifier resins, phenol-based tackifier resins, rosin-based tackifier resins, aliphatic petroleum resins, aromatic petroleum resins, copolymer-based petroleum resins, alicyclic petroleum resins, xylene resins, epoxy-based tackifier resins, polyamide-based tackifier resins, ketone-based tackifier resins, and elastomer-based tackifier resins. These tackifiers may be used alone or in combination of two or more.
[0089] When a tackifier is mixed, the amount added is preferably 30 parts by mass or less, and more preferably 5 to 20 parts by mass, per 100 parts by mass of the modified (meth)acrylic resin (A).
[0090] <<Solvent>> A solvent can be used to dilute the curable resin composition in order to adjust the viscosity of the curable resin composition. For example, when applying the curable resin composition, the solvent can be used to adjust the viscosity of the curable resin composition to an appropriate value. As the solvent, the solvent used in steps (i) and (ii) may be used as is, or a further solvent may be added to the solvent.
[0091] Examples of the solvent that can be used include organic solvents such as methyl ethyl ketone, methyl isobutyl ketone, acetone, ethyl acetate, propyl acetate, tetrahydrofuran, dioxane, cyclohexanone, hexane, toluene, xylene, n-propanol, isopropyl alcohol, etc. These solvents may be used alone or in combination of two or more.
[0092] <Additives> Examples of additives include plasticizers, surface lubricants, leveling agents, softeners, antioxidants, antiaging agents, light stabilizers, ultraviolet absorbers, polymerization inhibitors, benzotriazole-based light stabilizers and the like, phosphate ester-based and other flame retardants, surfactants, and antistatic agents.
[0093] [Method for Producing Photocrosslinkable Cured Product] <Step (iv)> The photocrosslinkable cured product can be produced by a method including a step (iv) of applying the curable resin composition onto a substrate or a release sheet and thermally curing the composition.
[0094] The curable resin composition obtained in step (iii) may be used as it is, or may be used after adjusting the viscosity by adding a solvent.
[0095] The thermal curing proceeds by, if necessary, performing heat drying and curing during the process of forming a photocrosslinkable cured product. For example, in one embodiment of step (iv), the curable resin composition is applied to a substrate, and if a solvent is contained, the composition is heated and dried to remove the solvent, thereby forming a curable resin composition layer. Thereafter, if necessary, a release sheet is attached to the curable resin composition layer. Furthermore, if necessary, the obtained sheet is cured in an oven for a certain period of time to form a crosslinked structure, thereby obtaining a photocrosslinkable cured product layer.
[0096] According to another embodiment, step (iv) includes step (iv-1) of applying a curable resin composition to a release sheet to obtain a curable resin composition layer, step (iv-2) of thermally curing the curable resin composition layer to obtain a photo-crosslinkable cured product layer, and step (iv-3) of laminating a substrate on the curable resin composition layer or the photo-crosslinkable cured product layer. Step (iv-3) may be performed between step (iv-1) and step (iv-2), or may be performed after step (iv-2). For example, the curable resin composition is applied to a release sheet, and if a solvent is contained, the composition is heated and dried to remove the solvent, thereby forming a curable resin composition layer (step (iv-1)). Thereafter, the release sheet having the curable resin composition layer is placed on a substrate, with the surface of the curable resin composition layer facing the substrate, and the curable resin composition layer is transferred (transferred) onto the substrate (step (iv-3)). Furthermore, the obtained sheet may be cured in an oven for a certain period of time, if necessary, to form a crosslinked structure, thereby obtaining a photocrosslinkable cured material layer (step (iv-2)).
[0097] The curable resin composition can be applied to a substrate (or a release sheet) by a known method, specifically, by using a conventional coater such as a gravure roll coater, a reverse roll coater, a kiss roll coater, a dip roll coater, a bar coater, a knife coater, a spray coater, a comma coater, or a direct coater.
[0098] The conditions for heat-drying the applied curable resin composition are not particularly limited, but are typically 25 to 180°C, preferably 60 to 150°C, for 1 to 20 minutes, preferably 1 to 10 minutes. Heat-drying within the above ranges allows for the removal of the solvent contained in the curable resin composition. The conditions for curing the heat-dried sheet in an oven for a certain period of time are not particularly limited, but are typically 25 to 100°C, preferably 30 to 80°C, for 1 to 30 days, preferably 1 to 14 days. Curing under the above conditions allows for crosslinking of the modified (meth)acrylic resin (A) with the crosslinking agent (C), thereby adjusting the gel fraction of the photocrosslinkable cured product to the desired range.
[0099] The sheet obtained by step (iv) can be used for, for example, optical components, pressure-sensitive adhesive sheets, etc. Pressure-sensitive adhesive sheets can be used as backgrinding tapes, dicing tapes, supporting tapes, etc. when producing electronic components.
[0100] The substrate is not particularly limited and can be appropriately selected depending on the application. Materials include, but are not particularly limited to, paper, plastic, cloth, metal, etc. The substrate may also be a film, woven fabric, or nonwoven fabric.
[0101] When used for optical members, glass substrates, silicon substrates, polycarbonate substrates, polyester substrates, polyamide substrates, polyamideimide substrates, polyimide substrates, aluminum substrates, printed wiring boards, array substrates, etc. can be used as appropriate.
[0102] When used in pressure-sensitive adhesive sheets, resin films are preferred, and examples of resin materials include polyvinyl chloride, polyvinylidene chloride, polyolefin (PO), polyester, polyurethane, polycarbonate, polyether ether ketone, polyimide, polyetherimide, polyamide, wholly aromatic polyamide (aramid), polyphenyl sulfide, fluororesin, cellulose-based resin, and silicone resin. Examples of polyolefins include polyethylene (PE) such as low-density polyethylene, linear polyethylene, medium-density polyethylene, high-density polyethylene, and ultra-low-density polyethylene; polypropylene (PP) such as random copolymer polypropylene, block copolymer polypropylene, and homopolypropylene; polybutene; polymethylpentene; ethylene-vinyl acetate copolymer; ionomer resin; ethylene-(meth)acrylic acid copolymer; ethylene-(meth)acrylic acid ester copolymer; ethylene-butene copolymer; and ethylene-hexene copolymer. Examples of polyesters include polyethylene terephthalate (PET), polyethylene naphthalate, and polybutylene terephthalate (PBT). Among these resin materials, it is particularly preferable to use one or more selected from the group consisting of PE, PP, and PET, since this allows the production of a pressure-sensitive adhesive sheet with appropriate flexibility. The resin material used as the substrate material may be a single material or a mixture of two or more materials. When used as a dicing tape, it is preferable to use polyolefin.
[0103] The substrate may be made of one type of material or two or more types of materials. The substrate may have a single-layer structure or a multi-layer structure. Since the photo-crosslinkable cured product on the substrate is an ultraviolet-curable type, the substrate preferably has ultraviolet transparency. When the substrate is a resin film, the substrate may be a non-stretched film, a uniaxially stretched film, or a biaxially stretched film.
[0104] The substrate may be subjected to a treatment to enhance adhesion, such as a physical treatment such as corona discharge treatment, plasma treatment, sand matting treatment, ozone exposure treatment, flame exposure treatment, high-voltage shock exposure treatment, or ionizing radiation treatment, a chemical treatment such as chromate treatment, or a primer treatment.
[0105] It is preferable to use a PO film as the substrate. PO film has low heat resistance and is not suitable for the above-mentioned heat drying temperature. Therefore, it is preferable to apply a curable resin composition to a release sheet, heat-dry to remove the solvent, and then transfer the curable resin composition layer to the PO film. Specifically, it is preferable to apply a curable resin composition to the release-treated surface of a silicone-based light-release PET film, heat-dry, and then attach the PO film to the curable resin composition layer using a rubber roller so that the corona-treated surface of the PO film adheres to the exposed surface of the curable resin composition layer.
[0106] The release sheet is not particularly limited, and for example, a release sheet generally used for pressure-sensitive adhesives can be used without any restrictions. Specifically, the same resin film as that used for the substrate is preferable, and from the viewpoint of handleability, it is preferable to use a resin film containing one or more selected from PE, PP, and PET.
[0107] The release sheet may be subjected to a release treatment to impart easy releasability, specifically, a silicone release treatment or the like.
[0108] When used in a pressure-sensitive adhesive sheet, the thickness of the photo-crosslinkable cured material layer is preferably 5 to 100 μm, more preferably 10 to 50 μm, and even more preferably 10 to 20 μm. If the thickness of the photo-crosslinkable cured material layer is 5 μm or more, sufficient adhesive properties are exhibited and coating is easy. If the thickness of the photo-crosslinkable cured material layer is 100 μm or less, the generation of bubbles during heat drying and residual solvent can be suppressed.
[0109] [Uses of Photocrosslinkable Cured Product] The photocrosslinkable cured product can be used, for example, as a resist, a transparent material, a surface protector, a temporary fixer, a backgrinding tape, a dicing tape, a dicing and die bonding integrated film, and the like.
[0110] [Uses of Pressure-Sensitive Adhesive Sheets] A sheet having a photocrosslinkable cured product layer can be used, for example, as a pressure-sensitive adhesive sheet. The pressure-sensitive adhesive sheet can be used, for example, as a removable pressure-sensitive adhesive sheet when manufacturing electronic components. Specifically, removable pressure-sensitive adhesive sheets are used in various processes when manufacturing electronic components, such as fixing an adherend and subjecting it to various processing steps, followed by irradiating it with UV (ultraviolet) light to remove it from the adherend. Therefore, the pressure-sensitive adhesive sheet can be used as a backgrinding tape, dicing tape, etc. when processing semiconductor wafers. The pressure-sensitive adhesive sheet can also be used as a support tape for fragile components such as ultrathin glass substrates and components prone to warping such as FPC boards. In particular, the pressure-sensitive adhesive sheet has excellent adhesion to the adhesive layer and excellent releasability after UV irradiation, making it suitable as a dicing tape used when manufacturing a dicing / die-bonding integrated film.
[0111] An exemplary method of using an adhesive sheet as a wafer dicing tape is described below. Before the dicing process, an adhesive sheet is attached to a wafer on which multiple components are formed. Next, the wafer is cut and separated (diced) into individual components to form element pieces (chips). Then, UV light is irradiated onto the adhesive sheet attached to each element piece. This causes UV light to irradiate the adhesive layer (photocrosslinkable cured material layer) through the base material of the adhesive sheet, and the unsaturated bonds in the adhesive form a three-dimensional crosslinked structure and harden. As a result, the adhesive strength of the adhesive layer is reduced. Then, the adhesive sheet is peeled off from each element piece.
[0112] [Method for Producing Dicing Tape] The dicing tape is produced by forming a photocrosslinkable cured material layer on a substrate. The method for forming the photocrosslinkable cured material layer is the same as in step (iv) above.
[0113] The substrate is preferably made of a material suitable for the expanding process, and is preferably a polyolefin film.
[0114] When a polyolefin film is used, heating during the formation of the photocrosslinkable cured material layer may pose a problem in terms of heat resistance. Therefore, it is preferable to perform the following steps in this order: Step (iv-1) of applying a curable resin composition onto a release sheet to obtain a curable resin composition layer; Step (iv-2) of thermally curing the curable resin composition layer to obtain a photocrosslinkable cured material layer; and Step (iv-3) of laminating a substrate on the photocrosslinkable cured material layer, and then, if necessary, curing the obtained sheet in an oven for a certain period of time to form a crosslinked structure, thereby obtaining a dicing tape.
[0115] The thickness of the photo-crosslinkable cured material layer is preferably 5 to 100 μm, more preferably 10 to 50 μm, and even more preferably 10 to 20 μm. When the thickness of the photo-crosslinkable cured material layer is 5 μm or more, sufficient adhesive properties are exhibited and coating is easy. When the photo-crosslinkable cured material layer is 100 μm or less, the generation of bubbles during heat drying and residual solvent can be suppressed. In particular, when the thickness of the photo-crosslinkable cured material layer is 10 to 20 μm, sufficient peelability and severability (cuttability) can be obtained.
[0116] [Method for Producing a Dicing and Die Bonding Integrated Film] The dicing and die bonding integrated film can be obtained by laminating a dicing tape and a die bonding tape. The method for producing the dicing tape is the same as that described above.
[0117] That is, the method for producing a dicing and die bonding integrated film includes the following steps: Step (iv-1) of applying a curable resin composition onto a release sheet to obtain a curable resin composition layer; Step (iv-2) of thermally curing the curable resin composition layer to obtain a photocrosslinkable cured material layer; Step (iv-3) of laminating a substrate on the curable resin composition layer or the photocrosslinkable cured material layer to obtain a dicing tape; and Step (v) of laminating the dicing tape and the die bonding tape. The order of the steps may be reversed, except that Step (iv-1) is performed first and Step (v) is performed last. Step (iv-3) may be performed between Step (iv-1) and Step (iv-2), or after Step (iv-2).
[0118] The thickness of the photo-crosslinkable cured material layer is preferably 5 to 100 μm, more preferably 10 to 50 μm, and even more preferably 10 to 20 μm. When the thickness of the photo-crosslinkable cured material layer is 5 μm or more, sufficient adhesive properties are exhibited and coating is easy. When the thickness of the photo-crosslinkable cured material layer is 100 μm or less, the generation of bubbles during heat drying and residual solvent can be suppressed. In particular, when the thickness of the photo-crosslinkable cured material layer is 10 to 20 μm, sufficient peelability and severability (cuttability) can be obtained.
[0119] Step (v) can be performed, for example, by preparing a die bonding tape and bonding it to a dicing tape. The die bonding tape can be obtained, for example, by applying an adhesive composition to a release sheet and curing it to form an adhesive layer. The bonding temperature is, for example, 30 to 50°C. The bonding pressure (linear pressure) is, for example, 0.1 to 20 kgf / cm.
[0120] As a modified example of the method for producing a dicing and die bonding integrated film, the thermal curing of the curable resin composition may be carried out in two steps, step (iv-2) and step (v). For example, after the thermal curing is allowed to proceed in step (iv-2), the dicing tape and the die bonding tape may be laminated together in step (v), followed by curing to further proceed with the thermal curing (thermal crosslinking) of the photocrosslinkable cured material layer.
[0121] As a modified example of the method for producing a dicing and die-bonding integrated film, the release sheet in step (iv-1) may be replaced with the die-bonding tape in step (v), and the formation of the photocrosslinkable cured material layer and the lamination of the dicing tape and die-bonding tape may be carried out simultaneously. In this case, a dicing and die-bonding integrated film can be obtained by applying a curable resin composition onto the adhesive layer of the die-bonding tape, thermally curing it, and laminating a substrate on it before or after thermal curing.
[0122] [Method for Producing a Cured Product] <Step (vi)> The method for producing a cured product includes a step (vi) of irradiating a photocrosslinkable cured product with UV light to form a crosslinked structure.
[0123] Examples of light sources used for UV irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, xenon lamps, metal halide lamps, chemical lamps, and black lights.
[0124] The amount of UV irradiation applied to the photocrosslinkable cured product is 50 to 3,000 mJ / cm 2 is preferably 100 to 600 mJ / cm 2 It is more preferable that the UV irradiation dose applied to the photocrosslinkable cured product is 50 mJ / cm. 2 If the UV irradiation is more than this, the crosslink density of the photocrosslinkable cured product can be improved at a sufficiently fast curing rate by UV irradiation. Therefore, when the photocrosslinkable cured product is used in an adhesive layer, the adhesive strength of the adhesive layer after UV irradiation can be sufficiently reduced. When the photocrosslinkable cured product is used in a resist, the strength can be improved. The UV irradiation dose irradiated to the photocrosslinkable cured product is 3,000 mJ / cm 2 Even if the UV irradiation dose exceeds 3,000 mJ / cm, no further improvement in crosslink density can be obtained. 2 By doing as follows, it is possible to economically produce a cured product while reducing the effect of UV irradiation on the adherend. Therefore, when the photocrosslinkable cured product is used in a pressure-sensitive adhesive sheet, it can be economically peeled off.
[0125] The present invention will be explained in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0126] The raw materials used in the synthesis of the modified (meth)acrylic resins (A) and (cA) are shown below. Hydroxy group-containing (meth)acrylate (m-1) 2-hydroxyethyl acrylate, Nippon Shokubai Co., Ltd., 2-hydroxyethyl methacrylate, Nippon Shokubai Co., Ltd., 4-hydroxybutyl acrylate, Osaka Organic Chemical Industry Ltd. Alkyl (meth)acrylate (m-2) 2-ethylhexyl acrylate, Osaka Organic Chemical Industry Ltd., n-butyl acrylate, Osaka Organic Chemical Industry Ltd., dodecyl acrylate, Kyoeisha Chemical Co., Ltd., methyl methacrylate, Nippon Shokubai Co., Ltd. RAFT agent: 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, FUJIFILM Wako Pure Chemical Industries, Ltd., 4-cyano-4-[(dodecylsulfanylthiocarbonyl)sulfanyl]pentanoic acid, FUJIFILM Wako Pure Chemical Industries, Ltd. Radical polymerization initiator: 2,4,6-trimethylbenzoyldiphenylphosphine oxide (BASF, trade name: L-TPO), 2,2'-Azobisisobutyronitrile, Fujifilm Wako Pure Chemical Industries, Ltd. Isocyanato group-containing ethylenically unsaturated compound (a): Karenz™ MOI, 2-isocyanatoethyl methacrylate, Resonaq Inc.
[0127] A synthesis example is shown below.
[0128] Synthesis Example 1 (Example 1-1) A reaction apparatus equipped with a stirrer, a temperature controller, a reflux condenser, and a thermometer was charged with 83 parts by mass (75.5 mol) of 2-ethylhexyl acrylate, 17 parts by mass (24.5 mol) of 2-hydroxyethyl acrylate, 0.002 parts by mass of 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, 0.001 parts by mass of 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and 100 parts by mass of ethyl acetate as a solvent. This reaction raw material solution was heated at a wavelength of 385 nm and an illuminance of 1.5 mW / cm. 2The mixture was continuously irradiated with UV and subjected to UV irradiation RAFT polymerization at room temperature (25°C) for 10 hours. After UV irradiation was stopped, the temperature of the reaction mixture was raised to 60°C, and a mixture of 16 parts by mass (17.3 mol) of 2-isocyanatoethyl methacrylate and 0.19 parts by mass of dibutyltin dilaurate as a urethanization catalyst was added dropwise through a dropping funnel. After completion of the dropwise addition, the reaction system was maintained at 70°C for 4 hours to eliminate the isocyanato groups. After completion of the reaction, ethyl acetate was added so that the solids content was 35% by mass. This resulted in a solution with a solids content of 35% by mass containing a modified (meth)acrylic resin (A1) having a weight average molecular weight of 730,000, a glass transition temperature of -50°C, an ethylenically unsaturated group equivalent of 1,123 g / mol, and a hydroxyl value of 20.9 mgKOH / g.
[0129] [Synthesis Examples 2 to 8 (Examples 1-2 to 1-8)] Solutions containing modified (meth)acrylic resins were obtained in the same manner as in Synthesis Example 1, except that the compositions shown in Table 1 were used. Hereinafter, the modified (meth)acrylic resins obtained in Synthesis Examples 2 and 5 to 8 will be referred to as modified (meth)acrylic resins (A2) to (A6), respectively.
[0130] Comparative Synthesis Example 1 (Comparative Example 1-1) A reactor equipped with a stirrer, temperature controller, reflux condenser, and thermometer was charged with 83 parts by mass (75.5 mol) of 2-ethylhexyl acrylate, 17 parts by mass (24.5 mol) of 2-hydroxyethyl acrylate, 0.079 parts by mass of 2-[(dodecylsulfanylthiocarbonyl)sulfanyl]propanoic acid, 0.02 parts by mass of 2,2'-azobisisobutyronitrile, and 100 parts by mass of ethyl acetate as a solvent. The temperature of the reactants was maintained at 80°C, and thermal RAFT polymerization was carried out for 10 hours. The temperature of the reactants was lowered to 60°C, and a mixture of 16 parts by mass (17.3 mol) of 2-isocyanatoethyl methacrylate and 0.19 parts by mass of dibutyltin dilaurate as a urethanization catalyst was added dropwise through a dropping funnel. After completion of the dropwise addition, the reaction system was maintained at 70°C for 4 hours to eliminate the isocyanato groups. After completion of the reaction, ethyl acetate was added so that the solid content became 35% by mass, thereby obtaining a solution having a solid content of 35% by mass and containing a (meth)acrylic resin (cA1) having a weight average molecular weight of 550,000, a glass transition temperature of −50° C., an ethylenically unsaturated group equivalent of 1,123 g / mol, and a hydroxyl value of 20.9 mgKOH / g.
[0131] Comparative Synthesis Examples 2 to 3 (Comparative Examples 1-2 to 1-3) Solutions containing modified (meth)acrylic resins (cA2) to (cA3) were obtained in the same manner as in Comparative Synthesis Example 1, except that the compositions shown in Table 1 were used.
[0132]
[0133] The raw materials used in preparing the curable resin composition are as follows: Photopolymerization initiator (B): TPO: 2,4,6-trimethylbenzoyldiphenylphosphine oxide (BASF, trade name: L-TPO) Crosslinking agent (C): L-45E: tolylene diisocyanate adduct of trimethylolpropane (Tosoh Corporation, trade name: Coronate L-45E)
[0134] [Preparation of Curable Resin Composition] Ethyl acetate, a dilution solvent, was added to each of the solutions containing the modified (meth)acrylic resins (A1) to (A6) and (cA1) to (cA3) obtained in Synthesis Examples 1, 2, and 5 to 8, and Comparative Synthesis Examples 1 to 3, so that the content of each of the modified (meth)acrylic resins (A1) to (A6) and (cA1) to (cA3) was 30 mass%. Using this solution, a curable resin composition was obtained by the method described below.
[0135] In a room shielded from actinic radiation, the modified (meth)acrylic resin (A) or (cA) shown in Table 2, the photopolymerization initiator (B), and the crosslinking agent (C) were added to a plastic container in the amounts (parts by mass) shown in Table 2, and the mixture was stirred to obtain curable resin compositions (D1) to (D6) and (cD1) to (cD3). The numerical values for the modified (meth)acrylic resins (A) and (cA) in Table 2 are the solid contents of the solutions used, i.e., the amounts (parts by mass) of the modified (meth)acrylic resins (A) and (cA) used.
[0136] [Example 2-1] Preparation of Dicing Tape A silicone-based light-release PET film (Toyobo Co., Ltd., product name: E7006, thickness 25 μm) was prepared as a separator. The release-treated surface was coated with the curable resin composition (D1) using an applicator so that the thickness after thermal curing was 20 μm. The film was then dried by heating at 100°C for 2 minutes to form a curable resin composition layer. Next, a 90 μm-thick PO film was prepared as a sheet-like substrate. The PO film was attached to the curable resin composition layer using a rubber roller so that the corona-treated surface of the PO film was adhered to the exposed surface of the curable resin composition layer. The film was then cured in an oven at 40°C for 3 days, and the curable resin composition layer was crosslinked and cured to obtain the dicing tape of Example 2-1.
[0137] [Examples 2-2 to 2-6 and Comparative Examples 2-1 to 2-3] Preparation of adhesive sheets Dicing tapes of Examples 2-2 to 2-6 and Comparative Examples 2-1 to 2-3 were obtained in the same manner as in Example 2-1, except that the curable resin composition shown in Table 2 was used instead of the curable resin composition (D1).
[0138]
[0139] [Preparation of a dicing / die bonding integrated film] The cover film on one side of a die bonding film (FH-D25T-50, Resonac Corporation), in which both sides of the adhesive layer were protected by a cover film, was peeled off to expose the adhesive layer. This adhesive layer was then bonded with a rubber roller to the photocrosslinkable cured material layer of the dicing tapes of Examples 2-1 to 2-6 and Comparative Examples 2-1 to 2-3, in which the light-release PET film had been peeled off to expose the photocrosslinkable cured material layer. This was left at room temperature for one day to obtain a dicing / die bonding integrated film.
[0140] [Evaluation] (1) Measurement of Adhesion Strength (30° Peel Strength) Before UV Irradiation The adhesion strength of the dicing tape according to the Examples and Comparative Examples to the die bonding film was evaluated by measuring the 30° peel strength as follows. A sample measuring 25 mm wide and 100 mm long was cut from the integrated dicing and die bonding film. The cover film on the side of the integrated dicing and die bonding film to which the dicing tape was not attached was peeled off, and the adhesive layer was attached to a polycarbonate plate using double-sided tape to obtain a sample for adhesion measurement. The peel strength of the dicing tape to the die bonding film was measured using a tensile tester (VPA-H200, Kyowa Interface Science Co., Ltd.). The measurement conditions were a peel angle of 30° and a tensile speed of 600 mm / min. The sample storage and peel strength measurement were performed at a temperature of 23°C and a relative humidity of 40%. The results are shown in Table 2.
[0141] (2) Measurement of adhesive strength (30° peel strength) after UV irradiation. The dicing and die bonding integrated film was exposed to an irradiation dose of 300 mJ / cm from the substrate side of the dicing tape. 2 The samples were irradiated with ultraviolet (UV) rays under the conditions of (a) to (c) to obtain samples for measuring adhesive strength after UV irradiation. A conveyor-type UV irradiation device (Eye Graphics Co., Ltd., 2 kW lamp, 80 W / cm) was used for UV irradiation. The peel strength of the dicing tape against the die bonding film was then measured using the same method as for measuring adhesive strength (30° peel strength) before UV irradiation. The results are shown in Table 2.
[0142] (3) Tensile Test (Elongation, Tensile Strength) The dicing tape was cut into a dumbbell shape with a width of 5 mm and a length of 50 mm as shown in Figure 1, and the light release PET film and PO film were peeled off to expose the pressure-sensitive adhesive layer. According to the method of JIS K 7161-1:2014, a tensile test of the pressure-sensitive adhesive layer was performed using a tensile tester (manufactured by Stable MicroSystems) under conditions of a gauge length of 20 mm and a pulling speed of 100 mm / min, and the elongation at break and breaking strength (tensile strength) were measured. The elongation was calculated according to the following formula. Test piece dimensions: Total length: 50 mm Parallel portion length: 25 mm Gauge distance: 20 mm Parallel portion width: 5 mm Thickness: 50 μm Grip width: 20 mm Distance between grippers: 30 mm Elongation: {[(Gauge distance at break) - (Initial gauge distance 20 mm)] / (Initial gauge distance 20 mm)} × 100
[0143] (4) Processability Evaluation (i) Preparation of a Sample for Processability Evaluation A protective tape (BG tape) was attached to the surface of a silicon wafer (diameter: 12 inches, thickness: 775 μm). The silicon wafer was then subjected to stealth dicing. That is, a modified layer was formed inside the silicon wafer by irradiating the surface (back surface) of the silicon wafer opposite to the side where the BG tape was attached with laser light under the following conditions. <Stealth dicing conditions> Stealth dicing device: DFL7361 (Disco Corporation) Laser oscillator type: Q-switched semiconductor-pumped solid-state laser Wavelength: 1342 nm Frequency: 90 kHz Output: 1.7 W Number of passes: 2 Chip size: 10 mm × 10 mm Dicing speed: 700 mm / sec
[0144] The silicon wafer after stealth dicing was polished to a thickness of 30 μm. A grinder polisher (DGP8761, Disco Corporation) was used for polishing. The adhesive layer of a dicing / die bonding integrated film was attached to the polished silicon wafer under the following conditions, with the substrate side of the dicing tape facing the dicing ring. The BG tape was then peeled off from the surface of the silicon wafer. <Attachment conditions> Attachment device: DFM2800 (Disco Corporation) Attachment temperature: 70°C Attachment speed: 10 mm / s Attachment tension level: Level 6
[0145] Next, a die separator (DDS2300, Disco Corporation) was used to cool and expand under the following conditions. Thereafter, the base material layer (PO film) of the dicing-die bonding integrated film was heat-shrunk under the following conditions. Through these processes, the silicon wafer and adhesive layer were singulated into multiple adhesive-piece chips (size 10 mm x 10 mm). <Cooling and expanding conditions> - Cooling temperature: -15°C - Cooling time: 120 seconds - Push-up amount: 12 mm - Push-up speed: 200 mm / sec - Holding time after push-up: 3 seconds <Heat shrinking conditions> - Heater temperature: 220°C - Heater rotation speed: 5° / sec - Push-up amount: 8 mm - Tape cooling waiting time: 10 seconds
[0146] After the silicon wafer and the adhesive layer were separated into individual pieces, the photo-crosslinkable cured material layer was irradiated with ultraviolet light from the surface of the dicing tape facing the substrate under the following conditions. This cured the photo-crosslinkable cured material layer, thereby reducing its adhesive strength to the adhesive layer. <UV Irradiation Conditions> UV Illuminance: 100 mW / cm 2 UV irradiation dose: 150 mJ / cm 2
[0147] (ii) Evaluation of processability <Contamination (DAF skipping)> After cooling expansion and heat shrinking, DAF skipping was evaluated according to the following criteria. The results are shown in Table 2. A: No DAF skipping occurred. B: No DAF skipping occurred, but peeling or lifting was observed at the interface between the adhesive layer and the photo-crosslinkable cured material layer. C: DAF skipping occurred in at least one location.
[0148] <Dicing ability (separability of adhesive layer)> The entire surface of the silicon wafer after dicing was observed under a microscope, and the separability of the adhesive layer was evaluated according to the following criteria. The results are shown in Table 2. A: The adhesive layer was completely separated. C: There was at least one part of the adhesive layer that was not separated.
[0149] <Dicing properties (kerf width)> The spacing (kerf width) between the chips with adhesive pieces after singulation was measured using a microscope. The kerf width in the MD / TD directions was measured at two locations on the outer periphery of the silicon wafer (top, bottom, left, and right) and one location in the center (18 locations in total), and the average value was calculated. Evaluation was based on the following criteria. The results are shown in Table 2. A: The average kerf width was 100 μm or more and less than 150 μm. B: The average kerf width was 70 μm or more and less than 100 μm. C: The average kerf width was 50 μm or more and less than 70 μm.
[0150] <Pickup ability> After carrying out the above evaluation, ultraviolet irradiation was carried out under the above conditions, and 100 chips with adhesive pieces attached were picked up under the following conditions and evaluated according to the following criteria. The results are shown in Table 2. (Pickup conditions) Die bonder: DB-830P (Fasford Technology Co., Ltd.) Push-up pin: EJECTOR NEEDLE SEN2-83-05 (diameter: 0.7 mm, tip shape: hemisphere with radius of 350 μm, Micromechanics Co., Ltd.) Push-up height: 250 μm Push-up speed: 1 mm / sec Number of push-up pins: 9 (Evaluation criteria) A: The pickup success rate was 100%. B: The pickup success rate was 80% or more but less than 100%. C: The pickup success rate was 60% or more but less than 80%.
[0151] According to the present disclosure, a modified (meth)acrylic resin having a narrow molecular weight distribution and a desired weight-average molecular weight can be obtained. Therefore, optimization for improving quality stability, storage stability, and desired performance can be easily achieved. A photocrosslinkable cured material layer produced using the modified (meth)acrylic resin can be particularly preferably used as a pressure-sensitive adhesive layer for dicing tapes and dicing / die-bonding integrated films.
Claims
1. A method for producing a modified (meth)acrylic resin, comprising: a step (i) of performing reversible addition-fragmentation chain transfer (RAFT) polymerization on a reaction raw material liquid containing raw material monomers (M) containing a hydroxyl group-containing (meth)acrylate (m-1) and an alkyl (meth)acrylate (m-2), as well as a radical polymerization initiator and a RAFT agent, while irradiating the reaction raw material liquid with UV light, to obtain a copolymer (A-0); and a step (ii) of adding an isocyanato group-containing ethylenically unsaturated compound (a) to a portion of the side chain hydroxyl groups of the copolymer (A-0), to obtain a modified (meth)acrylic resin (A) having an ethylenically unsaturated group.
2. The method for producing a modified (meth)acrylic resin according to claim 1, wherein the step (i) is carried out by a solution polymerization method, and the total concentration of the components excluding the solvent in the reaction raw material liquid is 30 to 90 mass %.
3. The method for producing a modified (meth)acrylic resin according to claim 1, wherein in the step (i), 0.0002 to 1.7 parts by mass of the radical polymerization initiator and 0.0005 to 10 parts by mass of the RAFT agent are used relative to 100 parts by mass of the raw material monomer group (M).
4. The method for producing a modified (meth)acrylic resin according to claim 1, wherein the RAFT agent is a trithiocarbonate.
5. The method for producing a modified (meth)acrylic resin according to claim 1, wherein in the step (i), the hydroxyl group-containing (meth)acrylate (m-1) is used in an amount of 5 to 50 mol % and the alkyl (meth)acrylate (m-2) is used in an amount of 50 to 95 mol % relative to 100 mol % of the raw material monomer group (M).
6. The method for producing a modified (meth)acrylic resin according to claim 1, wherein the modified (meth)acrylic resin (A) has a weight average molecular weight (Mw) of 7,000 to 1,500,000 and a molecular weight distribution (Mw / Mn) of 1.1 to 3.
0.
7. The method for producing a modified (meth)acrylic resin according to claim 1, wherein 0.5 to 49 moles of the isocyanato group-containing ethylenically unsaturated compound (a) are used in the step (ii) relative to 100 moles of the raw material monomer group (M) in the step (i), and the ratio of the number of moles of the isocyanato group-containing ethylenically unsaturated compound (a) in the step (ii) to the number of moles of the hydroxyl group-containing (meth)acrylate (m-1) in the step (i) is 30 to 99%.
8. In the step (i), the UV irradiance is 1 to 50 mW / cm 2 The method for producing a modified (meth)acrylic resin according to claim 1, wherein the polymerization is carried out under conditions of 10 to 40° C.
9. The method for producing a modified (meth)acrylic resin according to claim 1, wherein in the step (i), the UV irradiation time is 1 to 50 hours.
10. A method for producing a curable resin composition, comprising the step (iii) of mixing a modified (meth)acrylic resin (A) obtained by the production method according to any one of claims 1 to 9, a photopolymerization initiator (B), and a crosslinking agent (C).
11. A method for producing a curable resin composition according to claim 10, wherein the crosslinking agent (C) in step (iii) is at least one selected from the group consisting of polyisocyanates and polyepoxy compounds.
12. A method for producing a photocrosslinkable cured product, comprising the step (iv) of applying the curable resin composition obtained by the method according to claim 10 onto a substrate or a release sheet, and thermally curing the composition.
13. A method for producing a cured product, comprising the step (vi) of irradiating the photocrosslinkable cured product obtained by the method according to claim 12 with UV light to form a crosslinked structure.
14. A method for producing a dicing tape, comprising: a step (iv-1) of applying the curable resin composition obtained by the production method according to claim 10 onto a release sheet to obtain a curable resin composition layer; a step (iv-2) of thermally curing the curable resin composition layer to obtain a photocrosslinkable cured material layer; and a step (iv-3) of laminating a substrate onto the curable resin composition layer or the photocrosslinkable cured material layer.
15. A method for producing a dicing and die bonding integrated film, comprising the step (v) of laminating a dicing tape obtained by the method according to claim 14 and a die bonding tape.
Citation Information
Patent Citations
Living radical polymerization initiator
JP2005112980A
Method for producing temperature-sensitive adhesive
JP2015209448A
Adhesive tape
JP2018138682A
Radiation curable adhesive composition and pressure sensitive adhesive tape
JP2019143022A
Silicone-based graft copolymer, pressure-sensitive adhesive composition, pressure-sensitive adhesive tape, and method for producing semiconductor device
WO2021112173A1