Coating composition, method for producing coated article, coated article, and silsesquioxane derivative

The silsesquioxane derivative with a polyhedral structure and multiple alkyl groups addresses the limitations of existing AO resistance methods by offering improved solubility and AO resistance for spacecraft materials, enhancing their durability and applicability in space environments.

WO2024247487A1PCT designated stage expired Publication Date: 2024-12-05JAPAN AEROSPACE EXPLORATION AGENCY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013881
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-04-04
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current methods for improving atomic oxygen (AO) resistance in spacecraft materials, such as polyimide films, are either complex in synthesis or have limitations like cracking and require photocuring, which are not practical for widespread use.

Method used

A coating composition containing a silsesquioxane derivative with a polyhedral structure and multiple alkyl groups bonded to silicon atoms, which enhances AO resistance and solubility, allowing for a simpler and more effective application on polyimide films and other substrates.

Benefits of technology

The silsesquioxane derivative provides high AO resistance, improved solubility, and outgassing properties, making it suitable for space applications with reduced surface defects and enhanced durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided are: a coating composition which has enhanced coatability and solubility in solvents and contains POSS with alkyl groups introduced; a method for producing a coated article using the coating composition; and a produced coated article. The present invention relates to a coating composition containing a silsesquioxane derivative which has a silsesquioxane skeleton having a polyhedral structure and in which a plurality of alkyl groups having different numbers of carbon atoms are bonded to silicon atoms. The coating composition can be applied to a substrate to produce a coated article. This produced coated article has a substrate and a coating, formed on the surface of the substrate, that contains a silsesquioxane derivative which has a silsesquioxane skeleton having a polyhedral structure and in which a plurality of alkyl groups having different numbers of carbon atoms are bonded to silicon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Coating composition, method for producing coated article, coated article and silsesquioxane derivative

[0001] The present invention relates to a coating composition, a method for producing a coated article, a coated article, and a silsesquioxane derivative.

[0002] Spacecraft such as artificial satellites, space shuttles, and space stations fly in low Earth orbit (LEO) environments at altitudes of 100 to 700 km. It is known that the LEO environment contains large amounts of atomic oxygen (AO), which is formed when atmospheric oxygen molecules are dissociated into atoms by ultraviolet rays from the sun. It is also known that multi-layer insulation (MLI) used to insulate spacecraft can be eroded and damaged by collisions with AO.

[0003] The outermost layer of the MLI is a polyimide film, which has excellent heat resistance, radiation resistance, and UV resistance. To prevent AO corrosion of this polyimide film (to improve AO resistance), a method of introducing a polysiloxane structure into the polyimide resin that constitutes the film has been investigated (Patent Document 1).

[0004] Although polyimide resins having a polysiloxane structure as described in Patent Document 1 can improve the AO resistance of films, they are not practical because their resin structure is complex and requires multi-stage synthesis. Methods under consideration for more simply improving AO resistance include forming an aluminum-containing film on the surface of a polyimide film (Patent Document 2) and forming a cured film of polysiloxane into which curable functional groups such as epoxy groups or acryloyl groups have been introduced (Patent Document 3, Non-Patent Document 1).

[0005] It has been reported that physical defects occur in cured films of polysiloxanes into which curable functional groups have been introduced due to collisions with AO (Non-Patent Document 2).

[0006] JP 2003-113264 A JP 2004-225006 A JP 2011-042755 A

[0007] Kimoto et al., “Development of space-qualified photocurable-silsesquioxane-based polyimide films”, Journal of Spacecraft and Rockets, 53.6 (2016), pp. 1028-1034Goto et al., “Property changes in materials due to atomic oxygen in the low Earth orbit”, CEAS Space Journal, 13.3 (2021), pp. 415-432

[0008] By providing an AO-resistant coating such as those described in Patent Document 2, Patent Document 3, and Non-Patent Document 1, it is expected that the AO resistance of a polyimide film can be improved without the need for a complicated manufacturing process. Furthermore, it is expected that such a coating can improve the AO resistance of not only the polyimide film but also other components. However, metal coatings such as those described in Patent Document 2 are prone to cracking upon impact with AO and cannot prevent erosion of the polyimide film by AO that penetrates through the cracks. Furthermore, curable polysiloxanes such as those described in Patent Document 3 and Non-Patent Document 1 require photocuring after application, making the formation of the coating time-consuming, and also fail to provide sufficiently high AO resistance as described in Non-Patent Document 2.

[0009] In response to this, the present inventors have discovered that a coating with high AO resistance can be formed by applying a silsesquioxane derivative, in which an octyl group has been introduced into a cage-type silsesquioxane (Polyhedral Oligomeric Silsesquioxane: POSS, hereinafter also referred to simply as "POSS"), to a polyimide film or a silicon substrate. However, this silsesquioxane derivative has low solubility in solvents, and even when dissolved, its coatability to polyimide film, silicon, etc. is poor.

[0010] POSS is a compound that is expected to be used in a variety of applications. Therefore, if the solubility and coatability of POSS with alkyl groups can be improved, it is expected that it will be easier to expand into applications other than AO-resistant coatings.

[0011] The present invention has been made in view of the above problems, and an object of the present invention is to provide a coating composition containing POSS having an alkyl group introduced therein, which has improved solubility in solvents and coatability, a method for producing a coated article using the coating composition, the produced coated article, and the POSS (silsesquioxane derivative).

[0012] One aspect of the present invention for solving the above problems relates to coating compositions according to the following [1] to [3]. [1] A coating composition comprising a silsesquioxane derivative having a silsesquioxane skeleton with a polyhedral structure, in which a plurality of alkyl groups with different carbon numbers are bonded to the silicon atom. [2] The coating composition according to [1], which is used for coating spacecraft. [3] The coating composition according to [1] or [2], in which the concentrations of the polymerizable compound and the resin are 0% by mass or more and 10% by mass or less, based on the total mass of the solid content of the coating composition.

[0013] Another aspect of the present invention for solving the above problems relates to a method for producing a coated article according to the following item [4]: ​​[4] A method for producing a coated article, comprising a step of applying the coating composition according to any one of items [1] to [3] to a substrate.

[0014] Another aspect of the present invention for solving the above problems relates to the coated articles of [5] to [6] below. [5] A coated article comprising: a substrate; and a coating formed on the surface of the substrate, the coating containing a silsesquioxane derivative having a silsesquioxane skeleton with a polyhedral structure, in which a plurality of alkyl groups with different carbon numbers are bonded to a silicon atom. [6] The coated article according to [5], which is a component to be placed on a surface of a spacecraft exposed to the outside of the vehicle.

[0015] One embodiment of the present invention for solving the above problems relates to a silsesquioxane derivative according to the following item [7]: [7] A silsesquioxane derivative having a silsesquioxane skeleton with a polyhedral structure, in which a plurality of alkyl groups having different carbon numbers are bonded to the silicon atom.

[0016] According to the present invention, there are provided a coating composition containing POSS having an alkyl group introduced therein, which has improved solubility in solvents and coatability, a method for producing a coated article using the coating composition, the produced coated article, and the POSS (silsesquioxane derivative).

[0017] One embodiment of the present invention relates to a coating composition containing POSS having an alkyl group introduced therein.

[0018] The coating composition contains a silsesquioxane derivative having a silsesquioxane skeleton with a polyhedral structure, in which a plurality of alkyl groups having different carbon numbers are bonded to the silicon atom.

[0019] [Silsesquioxane Derivative] The silsesquioxane derivative has a silsesquioxane skeleton with a polyhedral structure, and a plurality of alkyl groups with different carbon numbers are bonded to the silicon atom.

[0020] The type of silsesquioxane skeleton having a polyhedral structure is not limited, and the number of Si atoms arranged at the vertices of the polyhedron is 8. 8 (general formula (1)), or T 10 or a polyhedron having 12 Si atoms at its vertices. 12 may be.

[0021]

[0022] In general formula (1), R represents an alkyl group having 1 to 32 carbon atoms. However, in this embodiment, R includes a plurality of alkyl groups having different numbers of carbon atoms.

[0023] As explained in the explanation of general formula (1), the silsesquioxane derivative has multiple alkyl groups with different carbon numbers bonded to the silicon atom. It is believed that the silsesquioxane derivative thus achieves both high AO resistance due to the POSS to which the alkyl groups are bonded and good solubility in solvents due to weakened intermolecular interactions. Furthermore, the silsesquioxane derivative exhibits excellent outgassing properties for films formed therefrom. Specifically, the amount of gaseous material released is low (low TML in outgassing property tests), the released gaseous material is less likely to adhere to other materials (low CVCM in outgassing property tests), and outgassing other than water vapor is low (low RML in outgassing property tests). Therefore, the silsesquioxane derivative is suitable for use in space applications.

[0024] The plurality of alkyl groups may all be linear or branched chain alkyl groups, all may have an alicyclic structure, or may be a combination of a chain alkyl group and an alkyl group having an alicyclic structure. The plurality of alkyl groups may also be two types of alkyl groups with different carbon numbers, or three or more types of alkyl groups with different carbon numbers. The upper limit of the number of alkyl groups with different carbon numbers can be 12 or less, 10 or less, or 8 or less, depending on the type of silsesquioxane skeleton. From the viewpoint of ensuring solubility in solvents, it is preferable that at least one of the plurality of alkyl groups be linear. Two or more of the plurality of alkyl groups may be linear, or all of the alkyl groups may be linear.

[0025] The plurality of alkyl groups are not particularly limited as long as they have from 1 to 32 carbon atoms, but preferably include an alkyl group having from 2 to 30 carbon atoms, more preferably include an alkyl group having from 3 to 25 carbon atoms, even more preferably include an alkyl group having from 4 to 22 carbon atoms, and particularly preferably include an alkyl group having from 5 to 20 carbon atoms. In this case, it is sufficient that at least one of the plurality of alkyl groups has a carbon number within the above-mentioned preferred range, but two or more of the alkyl groups may have a carbon number within the above-mentioned preferred range, or all of the alkyl groups may have a carbon number within the above-mentioned preferred range.

[0026] Furthermore, the difference in the number of carbon atoms among the multiple alkyl groups, between the alkyl group with the largest number of carbon atoms and the alkyl group with the smallest number of carbon atoms, is preferably 2 or more and 32 or less, more preferably 4 or more and 20 or less, and even more preferably 4 or more and 8 or less.

[0027] Furthermore, with regard to the multiple alkyl groups, the molar ratio (AR2 / AR1) of the alkyl group (AR1) contained in the silsesquioxane derivative in the largest number to the alkyl group (AR2) contained in the silsesquioxane derivative in the second largest number is preferably 0.1 or more and 1 or less, more preferably 0.3 or more and 1 or less, even more preferably 0.5 or more and 1 or less, and particularly preferably 0.7 or more and 1 or less.

[0028] In the silsesquioxane derivative, it is preferred that a plurality of alkyl groups having different carbon numbers are randomly bonded to silicon atoms. "Randomly bonded" means that alkyl groups having different carbon numbers are not specifically arranged on specific silicon atoms (for example, only on adjacent silicon atoms), but are randomly arranged. The random bonding of alkyl groups having different carbon numbers can be confirmed by a combination of mass spectrometry and nuclear magnetic resonance measurement.

[0029] Of the above-mentioned alkyl groups, one or more of the alkyl groups may be substituted with a halogen atom (for example, fluorine), but it is preferable that they are unsubstituted.

[0030] In addition, the silsesquioxane derivative may have functional groups or atomic groups other than alkyl groups bonded to one or more silicon atoms.The type of the functional group or atomic group is not particularly limited, but may be a polymerizable group such as (meth)acryloyl group, vinyl group, allyl group, oxetanyl group, epoxy group, or an atomic group having the same, an atomic group having an amide group, an ester group, an ether group, a urethane group, or an aromatic group such as a phenyl group, or an atomic group having the same, an amino group, a hydroxyl group, a mercapto group, or an atomic group having the same, an atomic group having an ethylene oxide group, a propylene oxide group, a silanol group, or an atomic group having the same, a halogen atom such as a fluorine atom, or an atomic group having the same, etc.The number of silicon atoms to which these functional groups or atomic groups other than alkyl groups are bonded is preferably less than half the number of silicon atoms contained in the silsesquioxane derivative, more preferably 3 or less, even more preferably 2 or less, even more preferably 1 or less, and particularly preferably 0. The silsesquioxane derivative may have silicon atoms to which hydrogen atoms are bonded without being substituted with alkyl groups during synthesis.

[0031] The silsesquioxane derivative can be synthesized by reacting a silsesquioxane (hereinafter referred to as "H-POSS") having a polyhedral structure in which a hydrogen atom is bonded to every silicon atom with two types of alkenes having different numbers of carbon atoms. During the reaction, other compounds for introducing the functional group or atomic group may be used in combination, if necessary.

[0032] Specifically, H-POSS and two or more alkenes having different carbon numbers are dissolved in a solvent such as toluene, in which the number of equivalents of the alkenes is preferably 8 to 100, more preferably 8 to 10, relative to the equivalent of H-POSS.

[0033] Next, the resulting solution is treated with a Karstedt catalyst or a Speier's catalyst (H 2 PtCl 6) is added and heated to 60°C to 110°C in an inert atmosphere such as nitrogen and argon. The heating time is not particularly limited, but can be from 5 hours to 24 hours. When an alkyl group having a small carbon number is bonded to a silicon atom, heating may be performed in a gas atmosphere such as ethylene, propylene, or butene (in this case, one type of alkene or two or more types of alkenes may be dissolved in the solution).

[0034] The mixture is then cooled to room temperature, and the synthesized silsesquioxane derivative is extracted. Extraction can be performed by silica column chromatography using hexane as a developing solvent, but other methods may also be used as appropriate. After extraction, removal of unreacted alkenes and by-product alkanes, purification of the silsesquioxane derivative, and other steps may be performed as needed.

[0035] [Coating Composition, Method for Producing Coated Article, and Coated Article] The coating composition contains the above-mentioned silsesquioxane derivative and a solvent that dissolves it.

[0036] The solvent is not particularly limited, and examples of the solvent that can be used include: water, halogen-based solvents such as dichloromethane, chloroform, carbon tetrachloride, 1,2-dichloroethane, and percrene; hydrocarbon solvents such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, cyclopentane, cyclohexane, methylcyclopentane, methylcyclohexane, benzene, toluene, xylene, ethylene chloride, chlorobenzene, dichloromethane, trichloromethane, and tetrachloromethane; ether-based solvents such as tetrahydrofuran, diethyl ether, and dibutyl ether; ester-based solvents such as propylene glycol monomethyl ether acetate, ethyl acetate, and butyl acetate; ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; alcohols such as methanol, ethanol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, and glycerin; and propylene glycol monomethyl ether, N-methylpyrrolidone, dimethylformamide, and dimethyl sulfoxide. Of these, chloroform is preferred as a solvent because it provides good solubility to the silsesquioxane derivative and enables uniform surface coating.

[0037] The concentration of the silsesquioxane derivative in the coating composition is not particularly limited and can be 1% by mass or more and 20% by mass or less relative to the total mass of the coating composition. From the viewpoint of forming a coating with a uniform and sufficient thickness, the concentration can be 3% by mass or more and 15% by mass or less, and preferably 5% by mass or more and 10% by mass or less.

[0038] Silsesquioxane derivatives having a single alkyl group have very low solubility in chloroform, but the above silsesquioxane derivatives having multiple alkyl groups with different carbon numbers can also be dissolved in chloroform at a concentration of 10 mass % or more.

[0039] In addition to the silsesquioxane derivative, the coating composition may contain other additives such as monomers (polymerizable compounds), polymerization initiators, polymerization inhibitors, resins, and optionally their curing agents, antioxidants, UV absorbers, leveling agents, fillers, metal fine particles, and pigments. Since the coating composition can be formed into a film using only the silsesquioxane derivative, it is not necessary to blend monomers, resins, their polymerization initiators, and curing agents. For example, the concentration of the monomers and resins can be 0% by mass or more and 10% by mass or less, preferably 0% by mass or more and 5% by mass or less, and more preferably 0% by mass or more and 1% by mass or less, based on the total mass of the solid content of the coating composition.

[0040] The coating composition can be used to form a coating by applying it to a substrate and optionally removing the solvent.

[0041] The substrate can be a variety of substrates, including polymer resins such as polyimide film, silicon, glass, and metals such as aluminum. These substrates may be pretreated, for example, by washing or ozone treatment, as necessary. According to the findings of the present inventors, good film formation is possible on substrates made of resins such as polyimide, even without pretreatment.

[0042] The application method is not particularly limited, and various methods such as roll coating, spin coating, spray coating, dipping, screen printing, and ink jet printing can be used.

[0043] After application, the solvent may be removed by a method such as heating. The method for removing the solvent can be appropriately selected depending on the type of solvent used. Furthermore, when the solvent can be removed during application, such as when the coating composition is applied to a substrate by spin coating, removal of the solvent is not necessary.

[0044] The thickness of the coating is not particularly limited and may be selected depending on the intended use. For example, the thickness of the coating is preferably 50 nm or more and 2500 nm or less, more preferably 100 nm or more and 2000 nm or less, and even more preferably 200 nm or more and 1500 nm or less.

[0045] The coating composition can form a smooth coating with a small difference in surface elevation. For example, the coating formed using the coating composition can have a surface elevation difference of 100 nm or less. The difference in elevation is a value measured using a known tactile step thickness meter (for example, Alpha-Step IQ manufactured by KLA-Tencor Corporation).

[0046] Furthermore, the coating composition can form a highly transparent coating. The coating formed from the coating composition can have an absorptance of less than 0.05 for sunlight with a wavelength of 250 to 2500 nm. The height difference is a value measured using a known solar absorptance measuring device (for example, a spectrophotometer U-4100 manufactured by Hitachi High-Tech Corporation equipped with a Spectralon integrating sphere).

[0047] The coating thus formed has the same composition as the coating composition, except for the volatile components such as the solvent. For example, the concentration of the resin component in the coating is the same as the concentration of the monomers and resin relative to the total mass of the solids in the coating composition.

[0048] [Applications] Coated articles produced in this manner, in which a coating is formed on the surface of a substrate, can be used in a variety of applications, such as spacecraft components, mobile equipment components such as automobiles, trucks, trains, ships, and airplanes, residential exteriors, electronic components, electrical components, optical components, and medical components. Specifically, the coated articles can be solar cell devices, electric wires, antennas, thermal control material sheets, and heat insulating films, in which the coating is formed on the outer surfaces thereof. When used as spacecraft components, the silsesquioxane derivative can be used on components that are placed on surfaces exposed to the outside of the spacecraft, with the coating facing outward, thereby imparting high AO resistance to the components. These coated articles can be used in outer space, on Earth, or on planets or satellites other than Earth, such as the surface of the Moon, Mars, or an asteroid.

[0049] In addition to being used in coating compositions, the silsesquioxane derivatives can also be used as heat resistance imparting agents, flame retardants, abrasion resistance imparting agents, crosslinking agents, viscosity modifiers, binder resins, and the like.

[0050] [Other Embodiments] It goes without saying that the above-described embodiments are exemplary embodiments of the present invention, and the present invention may include embodiments other than the above-described embodiments within the scope of its core technical concept.

[0051] The present invention will be described in detail based on examples, but the present invention is not limited to these examples.

[0052] 1. Synthesis of silsesquioxane derivatives 1-1. C 8 C 10 C 12 C 14Synthesis of H-POSS: H-POSS (a compound having the structure shown in general formula (1) where all R's are hydrogen atoms; 85 mg, 0.20 mmol) containing 8 Si atoms, 1-octene (49 mg, 0.44 mmol), 1-decene (62 mg, 0.44 mmol), 1-dodecene (74 mg, 0.44 mmol), and 1-tetradecene (86 mg, 0.44 mmol) were placed in a screw tube and dissolved in 2 mL of toluene. Then, 120 μL of Karstedt's catalyst (up to 2% in xylene) was added, and the mixture was heated at 80°C overnight under a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature, and the resulting compounds were eluted using silica column chromatography (developing solvent: hexane). The solution containing the target product was concentrated under reduced pressure, and the raw alkene and by-product alkanes were distilled off under reduced pressure (125°C, 5 Torr) using a Kugelrohr apparatus. The compound was purified again using silica column chromatography (developing solvent: hexane), and the solvent was distilled off under reduced pressure to obtain 180 mg of the target product as a white solid. 1 H NMR (400 MHz, CDCl 3 ): δ 1.46-1.26 (m, 150H), 0.88 (t, J=6.8Hz, 24H), 0.60 (t, J=8.4Hz, 16H).

[0053] 1-2. C 8 C 16 Synthesis of H-POSS: H-POSS (85 mg, 0.20 mmol), 1-octene (99 mg, 0.88 mmol), and 1-hexadecene (198 mg, 0.88 mmol) were placed in a screw tube and dissolved in 2 mL of toluene. Then, 120 μL of Karstedt's catalyst (approximately 2% in xylene) was added, and the mixture was heated overnight at 80°C under a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature, and the resulting compounds were eluted using silica column chromatography (developing solvent: hexane). The solution containing the target product was concentrated under reduced pressure, and the raw alkene and by-product alkanes were distilled off under reduced pressure (125°C, 5 Torr) using a Kugelrohr apparatus. The compound was purified again using silica column chromatography (developing solvent: hexane), and the solvent was distilled off under reduced pressure to obtain 206 mg of the target product as a white solid. 1H NMR (400 MHz, CDCl 3 ): δ 1.43-1.25 (m, 154H), 0.88 (t, J=7.2Hz, 24H), 0.60 (t, J=8.0Hz, 16H).

[0054] 1-3. C 8 C 12 C 16 Synthesis of H-POSS: H-POSS (85 mg, 0.20 mmol), 1-octene (67 mg, 0.60 mmol), 1-dodecene (100 mg, 0.60 mmol), and 1-hexadecene (135 mg, 0.60 mmol) were placed in a screw tube and dissolved in 2 mL of toluene. Then, 120 μL of Karstedt's catalyst (approximately 2% in xylene) was added, and the mixture was heated overnight at 80°C under a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature, and the resulting compounds were eluted using silica column chromatography (developing solvent: hexane). The solution containing the target product was concentrated under reduced pressure, and the raw alkene and by-product alkanes were distilled off under reduced pressure (125°C, 5 Torr) using a Kugelrohr apparatus. The compound was purified again using silica column chromatography (developing solvent: hexane), and the solvent was distilled off under reduced pressure to obtain 222 mg of the target product as a white solid. 1 H NMR (400MHz, CDCl 3 ): δ 1.46-1.25 (m, 156H), 0.88 (t, J=6.8Hz, 24H), 0.60 (t, J=8.0Hz, 16H).

[0055] 1-4. C 6 C 16Synthesis of H-POSS: H-POSS (85 mg, 0.20 mmol), cyclohexane (72 mg, 0.88 mmol), and 1-hexadecene (197 mg, 0.88 mmol) were added to a screw tube and dissolved in 2 mL of toluene. Then, 120 μL of Karstedt's catalyst (approximately 2% in xylene) was added and heated overnight at 75°C under a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature, and the resulting compounds were eluted using silica column chromatography (developing solvent: hexane). The solution containing the target product was concentrated under reduced pressure, and the raw alkene and by-product alkanes were distilled off under reduced pressure (125°C, 5 Torr) using a Kugelrohr apparatus. The compound was purified again using silica column chromatography (developing solvent: hexane), and the solvent was distilled off under reduced pressure to obtain 157 mg of the target product as a white solid. 1 H NMR (400MHz, CDCl 3 ): δ 1.82-1.62 (m, 5H), 1.46-1.18 (m, 201H), 0.87 (t, J=6.4Hz, 21H), 0.78-0.69 (m, 1H), 0.67-0.53 (m, 14H).

[0056] 1-5. C 2 C 16 Synthesis of H-POSS: H-POSS (85 mg, 0.20 mmol) and 1-hexadecene (198 mg, 0.88 mmol) were added to a small autoclave and dissolved in 2 mL of toluene. Then, 120 μL of Karstedt's catalyst (approximately 2% in xylene) was added, and the mixture was heated overnight at 80°C under ethylene gas pressure. After the reaction, the mixture was cooled to room temperature, and the resulting compounds were eluted using silica column chromatography (developing solvent: hexane). The solution containing the target product was concentrated under reduced pressure, and the raw alkene and by-product alkanes were distilled off under reduced pressure (125°C, 5 Torr) using a Kugelrohr apparatus. The compound was purified again using silica column chromatography (developing solvent: hexane), and the solvent was distilled off under reduced pressure to obtain the target product as a white solid.

[0057] 1-6. C 8Synthesis of H-POSS: H-POSS (100 mg, 0.24 mmol) and 1-octene (0.33 mL, 2.1 mmol) were placed in a screw tube and dissolved in 2 mL of toluene. Then, 140 μL of Karstedt's catalyst (up to 2% in xylene) was added, and the mixture was heated overnight at 80°C under a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature and concentrated under reduced pressure. The compound was purified using silica column chromatography (developing solvent: hexane), and the solvent was distilled off under reduced pressure to obtain 187 mg of the target product as a white solid. 1 H NMR (400MHz, CDCl 3 ): δ 1.42-1.26 (m, 96H), 0.88 (t, J=6.8Hz, 24H), 0.60 (t, J=8.0Hz, 16H).

[0058] 1-7. C 16 Synthesis of H-POSS: H-POSS (100 mg, 0.24 mmol) and 1-hexadecene (450 mg, 2.0 mmol) were placed in a screw tube and dissolved in 2 mL of toluene. Then, 140 μL of Karstedt's catalyst (up to 2% in xylene) was added, and the mixture was heated overnight at 80°C under a nitrogen atmosphere. After the reaction, the mixture was cooled to room temperature and concentrated under reduced pressure. The compound was purified using silica column chromatography (developing solvent: hexane), and the solvent was distilled off under reduced pressure. Further recrystallization using hexane yielded 257 mg of the target product as a white solid. 1 H NMR (400MHz, CDCl 3 ): δ 1.43-1.25 (m, 224H), 0.88 (t, J=6.8Hz, 24H), 0.60 (t, J=8.0Hz, 16H).

[0059] 2. Evaluation 1 (film-forming ability) C 8 C 10 C 12 C 14 -POSS, C 8 C 16 -POSS, C 8 -POSS and C 16 The following evaluations were carried out using four types of POSS derivatives.

[0060] The four POSS derivatives were dissolved in hexane and chloroform at room temperature to a concentration of 10% by mass. If sufficient dissolution was not observed, the solution was heated to 60°C to confirm whether it could be dissolved.

[0061] Based on these results, the solubility was evaluated according to the following criteria: ○ Sufficiently soluble in hexane, tetrahydrofuran, and chloroform at room temperature, and solutions with a concentration of 5% by mass or more can be prepared. × Solutions with a concentration of 5% by mass or more cannot be prepared in chloroform, tetrahydrofuran, or hexane at room temperature, but can be prepared by raising the temperature.

[0062] 2-2. Wettability to substrate surface C 8 C 10 C 12 C 14 -POSS and C 8 C 16 -POSS chloroform solution (concentration 10% by mass), and C 8 -POSS and C 16 A tetrahydrofuran solution of POSS (concentration 2.5% by mass) was filtered through a filter. A silicon substrate, which had been washed with toluene, acetone, water, and 2-propanol, dried, and then treated with ozone to remove surface contamination, and a polyimide film that had not been pretreated were prepared as substrates. 20 to 100 μL of each filtered solution was applied to a spin coater (MS-A100, manufactured by Misaka Co., Ltd.) for 10 minutes. 8 C 10 C 12 C 14 -POSS and C 8 C 16 -POSS chloroform solution was heated at 4000 rpm, C 8 -POSS and C 16 The tetrahydrofuran solution of -POSS was rotated at 1500 rpm to form a film on the surface of the silicon substrate and the polyimide film.

[0063] However, C 8 -POSS and C 16Since it was not possible to form a film of sufficient thickness (100 nm or more) using a tetrahydrofuran solution of -POSS, a hexane solution (dissolved at 60°C, concentration 10% by mass) was dropped onto a silicon substrate heated to 50°C and spin-coated at 4500 rpm.

[0064] The formed films were observed and their wettability was evaluated according to the following criteria: ◯ With either solution, a film could be formed on both the silicon substrate and the polyimide film at room temperature without exposing the substrate △ When a film was formed at room temperature using a low-concentration solution of 5 mass % or less, a film was formed that exposed the substrate, but by using a high-concentration solution of 5 mass % or more prepared by heating to 50°C or higher, a film of sufficient thickness could be formed without exposing the substrate × With either solution, a film of sufficient thickness could not be formed, and the substrate was partially exposed

[0065] 2-3. Uniformity of the film In the above-mentioned wettability test on the substrate surface, 8 C 10 C 12 C 14 -POSS and C 8 C 16 - A film formed using a chloroform solution of POSS, and C 16 The surface unevenness of the film formed using the hexane solution of -POSS was measured using a tactile step thickness meter (Alpha-Step IQ, manufactured by KLA-Tencor Corporation).

[0066] Based on the measured height difference of the surface irregularities, the uniformity of the film was evaluated according to the following criteria: ◯: The height difference of the surface irregularities was less than 100 nm. ×: The height difference of the surface irregularities was 100 nm or more.

[0067] The evaluation results are shown in Table 1.

[0068]

[0069] As shown in Table 1, POSS derivatives having a plurality of alkyl groups with different carbon numbers exhibited good solubility in common organic solvents, good wettability to substrates, and good film uniformity.

[0070] In addition, C 8 C10 C 12 C 14 -POSS and C 8 C 16 The thickness of the film formed using a chloroform solution of C-POSS was 400 to 1000 nm, and the height difference of the surface irregularities was several tens of nm. 8 The thickness of the film formed using a tetrahydrofuran solution of C-POSS was several tens of nanometers, and the substrate was exposed, making it impossible to measure the height difference of the surface irregularities. 16 The thickness of the film formed using a hexane solution of -POSS was 1000 to 2000 nm, and the height difference of the surface unevenness was 500 to 1000 nm. It is clear that POSS derivatives having multiple alkyl groups with different carbon numbers can form good films.

[0071] 3. Evaluation 2 (Transparency, AO resistance) C 8 C 10 C 12 C 14 -POSS and C 8 C 16 The following evaluations were carried out using test pieces prepared by forming a film (thickness: 1 μm) on the surface of a polyimide film using a chloroform solution of -POSS.

[0072] 3-1. Transparency Using a solar absorptance measuring device (Hitachi High-Tech Corporation, spectrophotometer U-4100 equipped with a Spectralon integrating sphere), the solar absorptance of the polyimide film before film formation and the solar absorptance of the film-formed surface of the test piece were measured. Measurement conditions: Measurement wavelength: 250 to 2500 nm Scanning width: 1 nm Detector: Photomultiplier tube / lead sulfide element

[0073] The solar absorptance of the polyimide film before film formation was subtracted from the solar absorptance of the film-formed surface, and the transparency of the film was evaluated based on the calculation results obtained using the following criteria: ○ The difference in solar absorptance was less than 0.05 × The difference in solar absorptance was 0.05 or more

[0074] 3-2. AO Resistance (Mass Loss) The coating surface of the test piece was irradiated with atomic oxygen (AO) under the following conditions: Irradiation conditions: AO speed: 8 km / s Irradiation time: 41 hours Average AO flux: 4.2 × 10 15 atoms・cm -2 ・s -1 ・Irradiation amount: 6×10 20 atoms・cm -2 ・Irradiation area: 3.14cm 2 ・Irradiation temperature: Room temperature ・Degree of vacuum during irradiation: Approximately 2×10 -2 Pa

[0075] The test pieces before and after AO irradiation were left to stand for 6 hours or more in an environment with a humidity of 23±3°C and a relative humidity of 50±5%. Thereafter, the mass of each test piece was measured using an electronic balance capable of measuring to the μg level (Mettler Toledo, Microbalance XP6).

[0076] Three test pieces were subjected to AO irradiation and mass measurement, and the mass after AO irradiation was subtracted from the mass before AO irradiation for each test piece. The subtracted amount (mg) was calculated based on the area (mm 2 Based on the calculation results, the AO resistance (mass loss) of the film was evaluated according to the following criteria: ○ Mass loss is 2 × 10 -4 mg / mm 2 The mass loss was less than 2 × 10 -4 mg / mm 2 That was all

[0077] 3-3. AO Resistance (Crack Resistance) In the above AO resistance (mass loss) test, the surface of the test piece irradiated with AO was observed using a scanning electron microscope (JEOL Ltd., JSM-7900F). Based on the observation results, the AO resistance (crack resistance) of the film was evaluated according to the following criteria: ○ No defects (cracks) with a width of 1 μm or more were found on the film surface × Defects (cracks) with a width of 1 μm or more were found on the film surface

[0078] 3-4. AO resistance (change in transparency) Using a solar absorptance measuring device (Hitachi High-Technologies Corporation, spectrophotometer U-4100 equipped with a Spectralon integrating sphere), the solar absorptance of the surface of the test piece irradiated with AO and the solar absorptance of the film surface before AO irradiation were measured for the above AO resistance (mass loss). Measurement conditions: Measurement wavelength: 250 to 2500 nm Scanning width: 1 nm Detector: Photomultiplier tube / lead sulfide element

[0079] The solar absorptance of the film surface before AO irradiation was subtracted from the solar absorptance of the film surface after AO irradiation, and the transparency of the film was evaluated based on the calculation results obtained according to the following criteria: ○ The difference in solar absorptance was less than 0.05 × The difference in solar absorptance was 0.05 or more

[0080] The evaluation results are shown in Table 2.

[0081]

[0082] As shown in Table 2, the POSS derivatives having a plurality of alkyl groups with different carbon numbers had good transparency and excellent AO resistance.

[0083] 4. Evaluation 3 (outgassing characteristics) C 8 C 10 C 12 C 14 -POSS and C 8 C 16 The outgassing characteristics were evaluated using test pieces prepared by forming a film on the surface of a 25 μm thick polyimide film substrate by spin coating using a chloroform solution of C-POSS (concentration: 10 mass %). 8 C 10 C 12 C 14 -POSS: 500-900 nm, C 8 C 16 -POSS was 300 to 500 nm.

[0084] The outgassing characteristics were measured in accordance with ASTM E595-93:1999 under the following conditions: (Measurement conditions) Vacuum degree: 7×10 -3Pa or less Material heating temperature: 125±1°C Emission gas cooling temperature: 24±1°C Holding time: 24 hours Measurement items: TML, CVCM, RML Initial sample weight: 210-220 mg

[0085] The mass loss ratio (TML) was calculated by {(sample weight before test - sample weight after test) / sample weight before test} × 100. The recondensable matter ratio (CVCM) was calculated by {(collector plate weight after test - collector plate weight before test) / sample weight before test} × 100. The weight of the test specimen after storage at 23±1°C / 50% RH for 24 hours was defined as the post-moisture absorption sample mass, and the water resorption ratio (WVR) was calculated by {(sample weight after moisture absorption - sample weight after test) / sample weight before test} × 100. The corrected mass loss ratio (RML) was calculated by (TML - WVR).

[0086] For TML, CVCM and RML, if TML was 1% or less, CVCM was 0.1% or less and RML was 1% or less, it was judged as pass (◯), and if otherwise it was judged as fail (×).

[0087] The evaluation results are shown in Table 3.

[0088]

[0089] As shown in Table 3, POSS derivatives having multiple alkyl groups with different carbon numbers have good outgassing properties and are suitable for use in space applications.

[0090] This application claims priority from Japanese Patent Application No. 2023-089767, filed May 31, 2023. The entire disclosure and claims of that application as originally filed are incorporated herein by reference.

[0091] The coating compositions according to the present invention are applicable to a variety of applications.

Claims

1. A coating composition comprising a silsesquioxane derivative having a silsesquioxane skeleton with a polyhedral structure, in which a plurality of alkyl groups having different carbon numbers are bonded to a silicon atom.

2. The coating composition according to claim 1, which is used for coating a spacecraft.

3. The coating composition according to claim 1 or 2, wherein the concentration of the polymerizable compound and the resin is from 0% by mass to 10% by mass based on the total mass of the solid content of the coating composition.

4. A method for producing a coated article, comprising the step of applying the coating composition according to any one of claims 1 to 3 to a substrate.

5. A coated article comprising: a substrate; and a coating formed on a surface of the substrate, the coating comprising a silsesquioxane derivative having a silsesquioxane skeleton with a polyhedral structure, in which a plurality of alkyl groups having different carbon numbers are bonded to silicon atoms.

6. The coated article according to claim 5, which is a component placed on a surface of a spacecraft that is exposed to the outside of the spacecraft.

7. A silsesquioxane derivative having a polyhedral silsesquioxane skeleton in which multiple alkyl groups with different carbon numbers are bonded to the silicon atom.

Citation Information

Patent Citations

  • Polyorganosilsesquioxane and its production

    JP1993125187A

  • Flexible heat control material

    JP2015063118A