Pre-doping agent for power storage device and method for producing same

The use of lithium iron oxide with specific composition and structure as a pre-doping agent in power storage devices addresses the challenges of high manufacturing costs and electrolyte instability, achieving high irreversible capacity and energy density by pre-doping lithium ions at lower voltages.

WO2024247498A1PCT designated stage expired Publication Date: 2024-12-05TAYCA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014407
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-04-09
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing pre-doping methods for power storage devices, such as lithium-ion batteries and capacitors, face challenges including increased manufacturing costs, reduced energy density, and instability due to the use of metal foils and fine particles of metallic lithium, as well as high irreversible capacity and electrolyte decomposition at high charging voltages.

Method used

A pre-doping agent composed of lithium iron oxide with specific composition and structure, represented by the formula Li5Fe_xO_y, where x satisfies 0.6≦x<1.0 and y satisfies 3.4≦y<4.0, is used, which allows for lithium ion pre-doping at a lower charging voltage, suppressing electrolyte decomposition and achieving a high irreversible capacity of 712 mAh/g or more while maintaining a low intensity ratio of diffraction peaks, thereby enhancing energy density and reducing costs.

Benefits of technology

The lithium iron oxide pre-doping agent enables efficient lithium ion pre-doping at a lower voltage, reducing electrolyte decomposition and increasing the irreversible capacity of power storage devices, thereby improving energy density and lowering manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014407_05122024_PF_FP_ABST
    Figure JP2024014407_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a pre-doping agent for a power storage device, the pre-doping agent being mainly composed of a lithium iron oxide represented by formula (1), wherein the intensity ratio (I16.7 / I23.6) of a diffraction peak intensity (I16.7) at a diffraction angle (2θ) of 16.7±0.5° to a diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 40% as measured by X-ray diffraction. Accordingly, a pre-doping agent for a power storage device having a very large irreversible capacity is provided, wherein it is possible to suppress a decrease in the energy density of the power storage device and reduce the manufacturing cost, and electrolyte decomposition can be suppressed because lithium ion pre-doping can be carried out at a lower charging voltage. (1): Li5FexOy [In formula (1), x satisfies 0.6≤x<1.0, and y satisfies 3.4≤y<4.0.]
Need to check novelty before this filing date? Find Prior Art

Description

Pre-dopant for power storage device and method for producing same

[0001] The present invention relates to a pre-dopant used in electricity storage devices such as lithium ion batteries, lithium ion capacitors, and electric double layer capacitors.

[0002] In power storage devices such as lithium-ion batteries, lithium-ion capacitors, and electric double-layer capacitors, it is known that pre-doping the negative electrode with lithium ions can counteract the potential drop of the negative electrode and the irreversible capacity of the negative electrode during the initial charge, thereby enabling the battery to have a higher capacity.

[0003] Patent Literature 1 proposes a method of pre-doping lithium ions into the negative electrode via an electrolyte by using a metal foil having a plurality of through-holes as a current collector and disposing a metal lithium foil in an electrode in which a large number of positive electrodes and negative electrodes are stacked. However, there are problems in that the use of a metal foil having a plurality of through-holes and a metal lithium foil as a current collector increases the manufacturing cost and further reduces the volumetric energy density of the electricity storage device.

[0004] Another pre-doping method that has been proposed is to react fine particles of metallic lithium with the negative electrode active material in a dry or wet manner before coating the electrode. However, handling highly reactive fine particles of metallic lithium places a heavy burden on the battery manufacturing process, and there are significant technical and cost challenges.

[0005] In Patent Document 2, Li 6 MnO 4A method for manufacturing a lithium ion secondary battery is described, which comprises: a pre-dope agent formed by combining a lithium-manganese-based oxide having a basic composition with a carbon material; a positive electrode having a positive electrode active material; a negative electrode; and an electrolyte; and an initial charge of the battery, thereby occluding lithium ions released from the positive electrode active material and the pre-dope agent into the negative electrode active material and generating manganese oxide from the pre-dope agent. The method for manufacturing a lithium ion secondary battery is described, in which the positive electrode potential during the initial charge is 4.5 V (based on a Li counter electrode) or higher. According to this method, by combining the carbon material and the lithium-manganese-based oxide, many conductive paths to the lithium-manganese-based oxide are formed, facilitating decomposition of the lithium-manganese-based oxide during charging. The pre-dope agent described in Patent Document 2 is said to have a large irreversible capacity. However, since the positive electrode potential during the initial charge is 4.5 V (based on a Li counter electrode) or higher, the pre-dope agent undergoes oxidative decomposition in a typical electrolyte, making it difficult to apply to power storage devices such as lithium ion batteries and lithium ion capacitors.

[0006] In Patent Document 3, Li x FeO y The pre-dope agent for an electricity storage device is described as being made of a lithium iron oxide represented by the formula (3.5≦x≦7.0, 3.1≦y≦5.0), characterized in that in X-ray diffraction measurement, the half-width of a diffraction peak at a diffraction angle (2θ) of 23.6±0.5° is 0.06 to 0.17°, and the intensity ratio (I44.6 / I23.6) of the diffraction peak intensity (I44.6) at a diffraction angle (2θ) of 44.6±0.5° to the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 8%. According to this, it is said that a pre-dope agent can be provided which can suppress decomposition of the electrolyte because lithium ions can be pre-doped at a lower charging voltage, has a high depth of charge, a high discharge capacity, and can suppress the occurrence of a short circuit phenomenon. Furthermore, Patent Document 4 describes Li 5 FeO 4 and the Li 5 FeO 4 and a carbon film covering the surface of the carbon-coated Li 5FeO 4 and the BET specific surface area is 2 to 5.4 m 2 / g of carbon-coated Li 5 FeO 4 According to this, it is said that a carbon-coated lithium iron oxide that exhibits sufficient capacity can be provided. A pre-dopant having a higher irreversible capacity at a lower charging voltage of 4.3 V or less has been desired.

[0007] Patent No. 5220510, Patent No. 6217990, WO2022 / 172881, Patent No. 6922672

[0008] The present invention has been made to solve the above problems, and aims to provide a pre-dopant for an electricity storage device that can suppress a decrease in the energy density of the electricity storage device, can reduce manufacturing costs, can pre-dope lithium ions at a lower charging voltage, thereby suppressing decomposition of the electrolyte, and has a very large irreversible capacity.

[0009] The above-mentioned problem is solved by providing a pre-dope agent for an electricity storage device, which contains as a main component a lithium iron oxide represented by the following formula (1), characterized in that in X-ray diffraction measurement, the intensity ratio (I16.7 / I23.6) of the diffraction peak intensity (I16.7) at a diffraction angle (2θ) of 16.7±0.5° to the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 40%. Li 5 Fe x O y (1) [In formula (1), x satisfies 0.6≦x<1.0, and y satisfies 3.4≦y<4.0.]

[0010] The above-mentioned problem can also be solved by providing a pre-dope agent for an electricity storage device containing, as a main component, a lithium iron oxide represented by the following formula (1), characterized in that the pre-dope agent for an electricity storage device has an irreversible capacity of 712 mAh / g or more and 1100 mAh / g or less at a voltage of 3.0 to 4.3 V (based on a Li reference electrode) during initial charging. 5 Fe x O y(1) [In formula (1), x satisfies 0.6≦x<1.0, and y satisfies 3.4≦y<4.0.]

[0011] In this case, in X-ray diffraction measurement, it is a preferred embodiment that the intensity ratio (I43.5 / I23.6) between the diffraction peak intensity (I43.5) at a diffraction angle (2θ) of 43.5±0.5° and the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 10%.

[0012] The space group of the crystal structure is Pbca, and the ratios of the crystal lattice constants a, b, and c are preferably a / c=0.99410 or less and b / c=1.00170 or less, respectively. The tap density is preferably 1.0 to 1.5 g / ml. 3 The content is preferably 5,000 ppm or less.

[0013] A positive electrode for an electricity storage device containing the pre-dopant and a positive electrode active material is a preferred embodiment, and an electricity storage device having the positive electrode as a constituent element is also a preferred embodiment.

[0014] The above-mentioned problems are also solved by providing a method for producing a pre-dope agent for an electricity storage device containing, as a main component, lithium iron oxide obtained by mixing an iron raw material and a lithium raw material and firing the mixture, the method comprising: mixing the iron raw material and the lithium raw material; performing a first firing step of firing the mixture at 350 to 650 ° C. for 2 to 100 hours in an inert gas atmosphere having an oxygen concentration of 1 to 52000 ppm; pulverizing the powdered product that is the first fired product; performing a second firing step of firing the pulverized powder at 700 to 1050 ° C. for 2 to 100 hours in an inert gas atmosphere having an oxygen concentration of 1 to 52000 ppm; and pulverizing the powdered product that is the second fired product, thereby obtaining lithium iron oxide.

[0015] According to the present invention, it is possible to suppress the decrease in energy density of an electricity storage device and reduce manufacturing costs, and since lithium ions can be pre-doped at a lower charging voltage, decomposition of the electrolyte can be suppressed, and a pre-dope agent for an electricity storage device having a very large irreversible capacity can be provided.

[0016] 1 is a diagram showing an XRD pattern of a pre-dope agent obtained in Example 1. FIG. 2 is a diagram showing an XRD pattern of a pre-dope agent obtained in Example 2. FIG. 3 is a diagram showing an XRD pattern of a pre-dope agent obtained in Comparative Example 2.

[0017] The pre-dope agent for an electricity storage device of the present invention (hereinafter, sometimes abbreviated as "pre-dope agent") is characterized in that it contains, as a main component, a lithium iron oxide represented by the following formula (1), and in X-ray diffraction measurement, the intensity ratio of the diffraction peak intensity (I16.7) at a diffraction angle (2θ) of 16.7±0.5° to the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 40%. Li 5 Fe x O y (1) [In formula (1), x satisfies 0.6≦x<1.0, and y satisfies 3.4≦y<4.0.] The pre-dopant of the present invention, which satisfies the constitution that the intensity ratio (I16.7 / I23.6) is less than 40%, has a large distortion in the crystal structure of the lithium iron oxide represented by the above formula (1), and a certain amount of Fe is doped into the lithium oxide.

[0018] In the present invention, the term "mainly composed of" indicates that the content of the lithium iron oxide represented by the formula (1) constituting the pre-dope agent for an electricity storage device is 80 mass % or more, and means that Li compounds other than the lithium iron oxide represented by the formula (1) may be present. Examples of such compounds include LiOH, Li 2 CO 3 Lithium iron oxide (LiFeO) with a low Li content 2 The content of the lithium iron oxide represented by the above formula (1) is preferably 90% by mass or more, and more preferably 95% by mass or more.

[0019] As a result of intensive research by the present inventors, it has been found that a pre-dope agent for an electricity storage device having a very large irreversible capacity can be obtained by using a lithium iron oxide having a specific composition, in which, in X-ray diffraction measurement, the intensity ratio (I16.7 / I23.6) between the diffraction peak intensity (I16.7) at a diffraction angle (2θ) of 16.7±0.5° and the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 40%. That is, a preferred embodiment of the pre-dope agent of the present invention is one in which the irreversible capacity at a voltage of 3.0 to 4.3 V (based on a Li reference electrode) during initial charging is 712 mAh / g or more and 1100 mAh / g or less. The pre-dope agent of the present invention can be subjected to a pre-doping treatment even at a low charging voltage, can suppress decomposition of the electrolyte, and has a very large irreversible capacity, so that the amount of pre-dope agent used when applied to a positive electrode can be reduced. Therefore, the proportion of the positive electrode active material can be increased, and the capacity of the electricity storage device can be increased. The irreversible capacity of the pre-dopant of the present invention is more preferably 720 mAh / g or more, even more preferably 750 mAh / g or more, particularly preferably 800 mAh / g or more, even more preferably 820 mAh / g or more, and most preferably 850 mAh / g or more. On the other hand, the irreversible capacity is more preferably 1050 mAh / g or less, and even more preferably 980 mAh / g or less.

[0020] The pre-dope agent of the present invention is mainly composed of lithium iron oxide represented by the above formula (1), and x satisfies 0.6≦x<1.0. In the lithium iron oxide represented by the above formula (1), x indicates the amount of Fe doped into the lithium oxide. When x is 1.0 or more, the amount of Li relative to Fe is small, resulting in a shortage of lithium pre-doped into the negative electrode, and a pre-dope agent having a high irreversible capacity of 712 mAh / g or more cannot be obtained. When x is less than 0.6, the amount of Fe doped is small, approaching the properties of lithium oxide, making it difficult to release lithium accompanied by an oxidation reaction during charging at a low voltage of 4.3 V or less. Therefore, as the charge capacity decreases, a pre-dope agent having a high irreversible capacity of 712 mAh / g or more cannot be obtained.

[0021] Furthermore, when lithium iron oxide represented by the above formula (1) is combined with a lithium iron oxide that has been adjusted only in composition, i.e., lithium oxide that is not doped with Fe, the intensity ratio (I16.7 / I23.6) does not become less than 40%, and a high irreversible capacity of 712 mAh / g or more cannot be obtained. Here, "lithium iron oxide doped with Fe" refers to a lithium iron oxide having a structure in which part of the Li in the lithium oxide is replaced with Fe. In addition, if lithium oxide that is not doped with Fe remains, the coating slurry thickens and gels when finished into an electrode, so it is essential that a certain amount of Fe be doped into the lithium oxide.

[0022] In the lithium iron oxide represented by the formula (1), y satisfies 3.4≦y<≦4.0. If y is less than 3.4, unreacted lithium and iron raw materials may remain. y is preferably 3.5 or more, more preferably 3.6 or more, and even more preferably 3.7 or more. If y exceeds 4.0, the iron in the lithium iron oxide may be in a highly oxidized state, resulting in a decrease in charge capacity. y is preferably 3.9 or less, more preferably 3.8 or less.

[0023] As long as the intensity ratio (I16.7 / I23.6) satisfies the condition of less than 40%, the lithium iron oxide represented by the above formula (1) may be further doped with a metal element M other than Fe. Examples of the other metal element M include Ni, Co, Mn, Ti, Al, V, Zr, and Nb. The doping amount z of the other metal element M must satisfy 0.6≦x<1.0 for Fe, but it is preferable that 0.01≦z≦0.4. A lithium iron oxide represented by the following formula (2) is a preferred embodiment. Li 5 Fe x M z O y (2) [In formula (2), M is a metal element other than Fe, x satisfies 0.6≦x<1.0, y satisfies 3.4≦y<4.0, and z satisfies 0.01≦z≦0.4]

[0024] As is clear from the comparison between the Examples and Comparative Examples described below, even when the lithium iron oxide represented by the above formula (1) has a specific composition ratio, it was confirmed that a high irreversible capacity of 712 mAh / g or more cannot be obtained in Comparative Examples 1 to 3, in which the intensity ratio (I16.7 / I23.6) does not satisfy the requirement of less than 40%. In contrast, it was confirmed that a pre-dope agent with a very large irreversible capacity of 712 mAh / g or more can be obtained in Examples 1 to 11, in which the intensity ratio (I16.7 / I23.6) is less than 40%. Therefore, it can be seen that there is great significance in adopting a configuration in which the intensity ratio (I16.7 / I23.6) is less than 40%. Furthermore, the pre-dope agent of the present invention makes it possible to reduce manufacturing costs, and since lithium ions can be pre-doped at a lower charging voltage, decomposition of the electrolyte can be suppressed, and since the irreversible capacity is very large, it is possible to reduce the amount of pre-dope agent used when applied to a positive electrode. Therefore, the ratio of the positive electrode active material can be increased, and the capacity of the energy storage device can be increased.

[0025] In X-ray diffraction measurement, the pre-dopant of the present invention preferably has a half-width of 0.06 to 0.17° of a diffraction peak at a diffraction angle (2θ) of 23.6±0.5°. If the half-width is less than 0.06°, the resulting powder product may be hard and difficult to pulverize. In addition, the particles after pulverization may be coarse, making application to an electrode difficult. The half-width is more preferably 0.07° or more, even more preferably 0.09° or more, and particularly preferably 0.10° or more. If the half-width exceeds 0.17°, polymorphous lithium iron oxide may be formed, resulting in a reduced irreversible capacity. The half-width is more preferably 0.16° or less, even more preferably 0.15° or less, particularly preferably 0.14° or less, and most preferably 0.13° or less.

[0026] In X-ray diffraction measurement, the pre-dope agent of the present invention preferably has an intensity ratio (I43.5 / I23.6) of the diffraction peak intensity (I43.5) at a diffraction angle (2θ) of 43.5±0.5° to the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° of less than 10%. If the intensity ratio (I43.5 / I23.6) is 10% or more, the pre-dope agent may have a low irreversible capacity. The intensity ratio (I43.5 / I23.6) is more preferably 8% or less, even more preferably 6% or less, particularly preferably 4% or less, and most preferably 2% or less. The intensity ratio (I43.5 / I23.6) is usually 0% or more.

[0027] In addition, in X-ray diffraction measurement, the pre-dopant of the present invention preferably has an intensity ratio (I44.6 / I23.6) of the diffraction peak intensity (I44.6) at a diffraction angle (2θ) of 44.6±0.5° to the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° of less than 8%. If the intensity ratio (I44.6 / I23.6) is 8% or more, there is a risk of a short circuit phenomenon occurring in the power storage device, and it is more preferably 5% or less, even more preferably 3% or less, and particularly preferably 1% or less. The intensity ratio (I44.6 / I23.6) is usually 0% or more.

[0028] In the pre-dope agent of the present invention, it is preferable that the space group of the crystal structure is Pbca, and the crystal lattice constants a, b, and c satisfy 9.15000 Å≦a≦9.15300 Å, 9.21900 Å≦b≦9.22200 Å, and 9.20600 Å≦c≦9.20800 Å, respectively. Furthermore, in the pre-dope agent of the present invention, it is preferable that the space group of the crystal structure is Pbca, and the ratios of the crystal lattice constants a, b, and c are an a / c ratio of 0.99300 to 0.99410 and a b / c ratio of 1.00100 to 1.00170, respectively. Based on studies by the present inventors, the present inventors have inferred that in the present pre-dope agent in which Fe is partially removed from the lithium iron oxide, the crystal structure of the lithium iron oxide is distorted, making it easier for lithium to be released.

[0029] In the pre-dope agent of the present invention, the volume resistivity is 1.0×10 1~9.0 x 10 15 It is preferable that the volume resistivity is 1.0×10 1 If the volume resistivity is less than Ω cm, electrons preferentially move to the pre-dopant in the electricity storage device system, and only the positive electrode active material near the pre-dopant is utilized, which may result in a local reaction and a decrease in capacity. 2 It is preferable that the resistance is Ω cm or more, and 1.0 × 10 3 As will be described later, it is a preferred embodiment that the pre-dopant of the present invention is coated with a carbonaceous material or the like, but from the viewpoint of controlling the volume resistivity to a certain level or higher while maintaining the irreversible capacity to a certain level or higher, it is also a preferred embodiment that the pre-dopant does not contain a carbonaceous material. From this viewpoint, the volume resistivity is 9.0 × 10 4 It is preferable that the resistance is Ω cm or more, and 9.0 × 10 5 More preferably, it is 9.0×10 Ω cm or more. 6 More preferably, it is 9.0×10 Ω cm or more. 7 It is particularly preferable that the resistance is Ω cm or more, and 9.0 × 10 8 On the other hand, it is most preferable that the volume resistivity is 9.0×10 15 If the volume resistivity exceeds Ω cm, the movement of electrons is hindered, lithium is not sufficiently released from the pre-dopant, and the irreversible capacity may be reduced. 12 More preferably, it is 9.0×10 Ω cm or less. 11 More preferably, it is 9.0×10 Ω cm or less. 10 It is particularly preferable that the resistivity is Ω·cm or less.

[0030] In the pre-dope agent of the present invention, the specific surface area is 0.05 to 5.0 m 2 It is preferable that the specific surface area is 0.05 m / g. 2 If the specific surface area is less than 0.1 m / g, the reaction area is small, lithium is not sufficiently released from the pre-dopant, the charge capacity decreases, and the irreversible capacity may decrease. 2 / g or more, and 0.2m 2 / g or more, and more preferably 0.5m 2 It is particularly preferable that the specific surface area is 5.0 m / g or more. 2 If the specific surface area exceeds 4.0 m / g, there is a risk of side reactions occurring. 2 / g or less is more preferable, and 3.0m 2 / g or less, and more preferably 2.0m 2 / g or less is particularly preferred, and 1.5m 2 / g or less, and more preferably 1.4m 2 / g or less is most preferred.

[0031] In the pre-dopant of the present invention, the average particle diameter (D50) is preferably 1 to 60 μm. The average particle diameter (D50) is more preferably 2 μm or more, even more preferably 3 μm or more, particularly preferably 4 μm or more, and most preferably 5 μm or more. On the other hand, if the average particle diameter (D50) exceeds 60 μm, it may be difficult to suppress the occurrence of a short circuit phenomenon in an electrical storage device. The average particle diameter (D50) is more preferably 50 μm or less, even more preferably 40 μm or less, particularly preferably 30 μm or less, and most preferably 25 μm or less. In the present invention, the average particle diameter (D50) refers to the median diameter obtained by measuring the particle size distribution using a laser diffraction particle size distribution measuring device (Microtrac MT-3000, manufactured by Nikkiso Co., Ltd.).

[0032] In the pre-dope agent of the present invention, the particle size distribution index D10 / D50 is preferably 0.1 to 0.4, more preferably 0.12 to 0.4, and the particle size distribution index D90 / D50 is preferably 2.0 to 4.0, more preferably 2.2 to 4.0.

[0033] In the pre-dope agent of the present invention, the tap density is preferably 1.0 to 1.5 g / ml. When the tap density is in this range, the energy density is improved and a pre-dope agent with a very large irreversible capacity is obtained. The tap density is more preferably 1.05 g / ml or more, even more preferably 1.08 g / ml or more, particularly preferably 1.12 g / ml or more, and most preferably 1.18 g / ml or more. On the other hand, the tap density is more preferably 1.4 g / ml or less.

[0034] In the pre-dopant of the present invention, SO 3 The content is preferably 5,000 ppm or less. 3 If the content exceeds 5,000 ppm, lithium sulfide is generated as an impurity, which may result in a decrease in charge capacity, so the content is more preferably 4,500 ppm or less, even more preferably 3,500 ppm or less, particularly preferably 2,500 ppm or less, and most preferably 1,500 ppm or less. 3 The content is usually 1 ppm or more.

[0035] In the pre-dope agent of the present invention, the amount of Li ion elution is preferably 15 mg / kg or less. If the amount of Li ion elution exceeds 15 mg / kg, lithium compounds are contained as impurities, and there is a risk that the charge capacity will decrease or the slurry stability will be poor during electrode preparation. Therefore, it is more preferably 13 mg / kg, even more preferably 12 mg / kg or less, particularly preferably 11 mg / kg or less, and most preferably 10 mg / kg.

[0036] In the pre-dopant of the present invention, the powder color L value is preferably 20 to 90. When the powder color L value is less than 20, the unreacted iron raw material and the low-order lithium iron oxide LiFeO 2The powder color L value is more preferably 30 or more, even more preferably 40 or more, particularly preferably 50 or more, even more preferably 60 or more, and most preferably 70 or more. On the other hand, when the powder color L value exceeds 90, the powder contains a lithium compound and the charge capacity may be reduced, so the powder color L value is more preferably 88 or less, even more preferably 86 or less, particularly preferably 84 or less, and most preferably 82 or less.

[0037] The method for producing the pre-dope agent of the present invention is not particularly limited. A method for producing a pre-dope agent for an electrical storage device mainly composed of lithium iron oxide obtained by mixing and firing an iron raw material and a lithium raw material, the iron raw material and the lithium raw material are mixed (hereinafter sometimes abbreviated as "mixing step"), and a first firing step is performed in which the mixture is fired at 350 to 650 ° C. for 2 to 100 hours in an inert gas atmosphere having an oxygen concentration of 1 to 52000 ppm (hereinafter sometimes abbreviated as "first firing step"), the powdered product obtained as the first fired product is pulverized, and the pulverized powder is fired at 700 to 1050 ° C. for 2 to 100 hours in an inert gas atmosphere having an oxygen concentration of 1 to 52000 ppm (hereinafter sometimes abbreviated as "second firing step"), and a method for obtaining lithium iron oxide by pulverizing the powdered product obtained as the second fired product is preferably adopted.

[0038] The inventors' studies have revealed that a pre-dope agent for an energy storage device containing the lithium iron oxide of the present invention as a main component, which has a very high irreversible capacity, can be obtained by performing a first firing step in which the iron raw material and the lithium raw material are mixed and fired in an inert atmosphere with a specific oxygen concentration at a low temperature for a specific time, followed by a second firing step in which the material is fired in an inert atmosphere with a specific oxygen concentration at a high temperature for a specific time. The inventors speculate that the crystal structure is distorted by performing the first firing step at a low temperature, and then the crystal structure is doped with the minimum amount of Fe by performing the second firing step at a high temperature. As is clear from a comparison between the examples and comparative examples described below, it was confirmed that a pre-dope agent with a high irreversible capacity could not be obtained in Comparative Example 2, in which the first firing step was not performed and the second firing step was performed at 850°C in a nitrogen atmosphere with an oxygen concentration of 500 ppm. Therefore, a method of obtaining lithium iron oxide by performing both the first firing step and the second firing step is preferably adopted. The oxygen concentration in the first and second firing steps is more preferably 5 ppm or more, even more preferably 30 ppm or more, particularly preferably 100 ppm or more, and most preferably 300 ppm or more, while the oxygen concentration is more preferably 50,000 ppm or less, even more preferably 35,000 ppm or less, particularly preferably 28,000 ppm or less, and most preferably 10,000 ppm or less.

[0039] The iron raw material used in the present invention is not particularly limited, and suitable examples include iron(III) oxide hydroxide, iron(II) oxide, iron(III) oxide, ferrous(II) sulfate, ferric(III) sulfate, iron(II) hydroxide, iron(III) hydroxide, etc. Among these, at least one selected from the group consisting of iron(III) oxide hydroxide and iron(III) oxide is more suitable.

[0040] The lithium raw material used in the present invention is not particularly limited, and lithium hydroxide, lithium carbonate, lithium acetate, lithium nitrate, lithium oxide, etc. are preferably used. These may be hydrated or anhydrous. Of these, lithium hydroxide is more preferably used.

[0041] In the mixing step, the iron raw material and the lithium raw material are mixed. A carbon raw material may be further mixed with the iron raw material and the lithium raw material. Mixing may be performed by a dry method or a wet method, but mixing by a dry method is preferred. Among these, mixing the iron raw material and the lithium raw material in a powder state is a preferred embodiment, and when a carbon raw material is further included, mixing the iron raw material, the lithium raw material, and the carbon raw material in a powder state is a preferred embodiment. When mixing the iron raw material and the lithium raw material, the Li / Fe (molar ratio) is preferably 1.0 to 8.0.

[0042] In the mixing step, it is a preferred embodiment that the particle size and / or bulk density of the raw materials are within a certain range. This allows the iron raw material and the lithium raw material to react uniformly, and the fired product can be easily recovered after the first firing step. Furthermore, in X-ray diffraction measurement, it is possible to control the intensity ratio (I16.7 / I23.6) between the diffraction peak intensity (I16.7) at a diffraction angle (2θ) of 16.7±0.5° and the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° and / or the intensity ratio (I43.5 / I23.6) between the diffraction peak intensity (I43.5) at a diffraction angle (2θ) of 43.5±0.5° and the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° to a certain level.

[0043] From this viewpoint, the particle size of the iron raw material is preferably 30 μm or less, more preferably 28 μm or less, even more preferably 25 μm or less, particularly preferably 22 μm or less, and most preferably 18 μm or less. On the other hand, the particle size of the iron raw material is preferably 0.5 μm or more. The particle size of the iron raw material is determined as the median diameter obtained by measuring the particle size distribution using a laser diffraction particle size distribution measuring device (Microtrac MT-3000, manufactured by Nikkiso Co., Ltd., iron (III) oxide particle refractive index: 2.94, iron (III) oxide hydroxide particle refractive index: 2.26). In this case, ion-exchanged water was used as the medium. The bulk density of the iron raw material was 0.90 g / cm. 3Preferably, 0.88 g / cm or less 3 More preferably, 0.85 g / cm 3 More preferably, 0.82 g / cm 3 The following is particularly preferred: 0.78 g / cm 3 On the other hand, the bulk density of the iron raw material is preferably 0.1 g / cm or less. 3 or more is preferable. The bulk density of the iron raw material is determined by filling a 20 ml measuring cylinder with the iron raw material and measuring the weight of the filled iron raw material. The particle diameter of the lithium raw material is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less, particularly preferably 50 μm or less, and most preferably 40 μm or less. On the other hand, the particle diameter of the lithium raw material is preferably 1 μm or more. The particle diameter of the lithium raw material is determined by the median diameter obtained by measuring the particle size distribution using a laser diffraction particle size distribution measuring device (Microtrac MT-3000, manufactured by Nikkiso Co., Ltd., particle refractive index 1.46). In this case, isopropyl alcohol with a water content of 2000 ppm or less by the Karl Fischer method was used as the medium.

[0044] A preferred embodiment is to carry out a first firing step after the mixing step. In the first firing step, a method of firing for a specific time at a low temperature in an inert gas atmosphere with an oxygen concentration of 1 to 52,000 ppm is preferably employed. Nitrogen, argon, helium, neon, krypton, or the like is preferably used as the inert gas. The firing temperature in the first firing step is preferably 350 to 650°C. If the firing temperature is below 350°C, unreacted raw materials may remain, potentially preventing the production of the lithium iron oxide represented by formula (1). The firing temperature is more preferably 380°C or higher, even more preferably 420°C or higher, particularly preferably 450°C or higher, and most preferably 500°C or higher. On the other hand, if the firing temperature exceeds 650°C, sublimation or solidification of the lithium source may occur, potentially preventing the lithium and iron from reacting uniformly. Therefore, a firing temperature of 620°C or lower is more preferable, even more preferably 600°C or lower, and particularly preferably 580°C or lower is particularly preferable.

[0045] The firing time in the first firing step is preferably 2 to 100 hours. If the firing time is less than 2 hours, unreacted raw materials may remain, and the lithium iron oxide represented by the above formula (1) may not be obtained. The firing time is more preferably 3 hours or more, and even more preferably 4 hours or more. On the other hand, if the firing time exceeds 100 hours, productivity may decrease. The firing time is more preferably 90 hours or less.

[0046] A preferred embodiment is to pulverize the powdered product obtained in the first firing step. For pulverization, at least one pulverizer selected from the group consisting of a ball mill, a planetary mill, a mortar and pestle mill, a jet mill, and a pin mill is preferably used, and at least one pulverizer selected from the group consisting of a ball mill and a planetary mill is more preferably used. In particular, from the viewpoint of improving reactivity in the second firing step, a preferred embodiment is to pulverize the powdered product obtained in the first firing step so that the average particle size (D50) of the powdered product obtained in the first firing step is within a certain range. The average particle size (D50) of the powdered product obtained in the first firing step is preferably 15 μm or less. When the average particle size (D50) of the powdered product is 15 μm or less, the reactivity in the second firing step is improved, and the lithium iron oxide represented by the above formula (1) is obtained. The average particle size (D50) of the powdered product obtained in the first firing step is more preferably 10 μm or less, and even more preferably 8 μm or less. On the other hand, the powdered product obtained by the first firing step preferably has an average particle size (D50) of 1 μm or more. The average particle size (D50) refers to the median diameter obtained by measuring the particle size distribution using a laser diffraction particle size distribution analyzer (Microtrac MT-3000, manufactured by Nikkiso Co., Ltd.).

[0047] A preferred embodiment involves a second calcination step to obtain lithium iron oxide. In the second calcination step, calcination is preferably performed for a specific period of time at a high temperature in an inert gas atmosphere with an oxygen concentration of 1 to 52,000 ppm. Nitrogen, argon, helium, neon, krypton, or the like is preferably used as the inert gas. The calcination temperature in the second calcination step is preferably 700 to 1,050°C. If the calcination temperature is lower than 700°C, unreacted raw materials may remain, potentially preventing the production of the lithium iron oxide represented by formula (1). The calcination temperature is more preferably 720°C or higher, even more preferably 750°C or higher, particularly preferably 780°C or higher, and most preferably 820°C or higher. On the other hand, if the calcination temperature exceeds 1,050°C, the resulting particles may become coarse, making application to an electrode difficult. Therefore, the calcination temperature is preferably 1,000°C or lower, even more preferably 980°C or lower, and particularly preferably 950°C or lower.

[0048] The firing time in the second firing step is preferably 2 to 100 hours. If the firing time is less than 2 hours, unreacted raw materials may remain, and the lithium iron oxide represented by the above formula (1) may not be obtained. The firing time is more preferably 3 hours or more, and even more preferably 4 hours or more. On the other hand, if the firing time exceeds 100 hours, productivity may decrease. The firing time is more preferably 90 hours or less.

[0049] It is also a preferred embodiment to pulverize the lithium iron oxide powder obtained by the second firing step. As a pulverization method, the same method as that used when pulverizing after the first firing step is preferably adopted. The average particle diameter (D50) of the pre-dope agent is preferably within the range described above. In addition, it is also a preferred embodiment to magnetically separate the pre-dope agent obtained after pulverization to remove magnetic substances.

[0050] From the viewpoint of imparting electrical conductivity and moisture resistance to the pre-dope agent, slurry stability during electrode preparation, and reducing interface resistance when applied to an all-solid-state battery, it is a preferred embodiment that the pre-dope agent is coated with at least one coating material selected from the group consisting of an organosilicon compound, a fatty acid, lithium carbonate, a niobium compound, a zirconium compound, and a carbonaceous material (hereinafter, sometimes referred to as a "coated pre-dope agent" or a "surface-treated pre-dope agent"). That is, it is a preferred embodiment that the pre-dope agent is at least one pre-dope agent for an electrical storage device selected from the group consisting of silica-coated lithium iron oxide, fatty acid-coated lithium iron oxide, lithium carbonate-coated lithium iron oxide, lithium niobate-coated lithium iron oxide, lithium zirconate-coated lithium iron oxide, and carbonaceous material-coated lithium iron oxide. It is preferable that the entire surface of the pre-dope agent is coated, but it is also acceptable that there are portions of the surface of the pre-dope agent that are not coated. In the present invention, the term "coated" means that when the elements C, O, Si, Fe, Nb, and Zr are specified and measured using an X-ray photoelectron analyzer, the element concentration of C, Si, Nb, or Zr from the outermost surface of the pre-dopant to a depth of 1 nm is a certain level or higher. The element concentration is preferably 1% or higher, more preferably 5% or higher, even more preferably 12% or higher, even more preferably 15% or higher, particularly preferably 20% or higher, and most preferably 25% or higher. The element concentration is usually 45% or lower. Among these, the element concentration of C is preferably 12% or higher, more preferably 15% or higher. The element concentration of Si is preferably 1% or higher, more preferably 3% or higher. The element concentration of Nb is preferably 1% or higher, more preferably 5% or higher. The element concentration of Zr is preferably 1% or higher, more preferably 5% or higher. X-ray photoelectron analysis was performed using an X-ray photoelectron spectrometer "ESCA3400" manufactured by Shimadzu Corporation. Correction was made using the C1s binding energy of 284.6 eV. The measurement conditions were as follows: (Measurement conditions) X-ray source: Mg-Kα ray Filament voltage-current: 12 kV-15 mA Degree of vacuum: 1.0 x 10 -6 Less than Pa Measurement range: 150 to 180 eV Measurement step: 0.1 eV Number of accumulations: 3

[0051] As described above, it is a preferred embodiment that the pre-dope agent is coated with the coating material, but the powder color L value of the coated pre-dope agent may decrease due to the influence of the coating material such as a carbonaceous material. From this viewpoint, the powder color L value of the coated pre-dope agent is preferably 10 to 90, more preferably 12 to 88, and even more preferably 14 to 86.

[0052] The organosilicon compound is not particularly limited as long as it can coat the surface of the pre-dopant with silica. Suitable examples include tetramethoxysilane, tetraethoxysilane, tetrabutoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, triethoxycaprylylsilane, and vinyltriethoxysilane. Suitable examples of the fatty acid include higher fatty acids having 10 to 24 carbon atoms, such as lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid, oleic acid, and behenic acid. Suitable examples of the niobium compound include pentaethoxyniobium, pentapropoxyniobium, and pentabutoxyniobium. Suitable examples of the zirconium compound include tetraethoxyzirconium, tetrapropoxyzirconium, and tetrabutoxyzirconium. Suitable examples of the carbonaceous material include activated carbon, acetylene black, polyvinyl alcohol, carbon nanotubes, carbon nanofibers, graphene, hard carbon, soft carbon, and Ketjen black.

[0053] The method for coating the pre-dope agent is not particularly limited, and the coating can be performed by mixing the coating material and the pre-dope agent and, if necessary, performing baking or the like. The baking temperature is preferably 300 to 600°C, and the baking time is preferably 0.5 to 24 hours. As a method for coating the pre-dope agent using a fatty acid, a method in which the fatty acid and the pre-dope agent are wet-mixed and then coated by vacuum distillation or the like instead of baking is preferably used. As a method for coating the pre-dope agent using lithium carbonate, a method in which the pre-dope agent is baked at 300 to 600°C in a carbon dioxide atmosphere with an oxygen concentration of 1 to 52,000 ppm, or a method in which the pre-dope agent is bubbled with carbon dioxide gas in an organic solvent is preferably used. As a method for coating the pre-dope agent using a niobium compound, a method is preferably adopted in which a niobium compound, the pre-dope agent, and optionally a lithium compound such as lithium methoxide, lithium ethoxide, lithium isopropoxide, or lithium tert-butoxide are mixed, and the mixture is heat-treated at 300 to 600 ° C. As a method for coating the pre-dope agent using a zirconium compound, a method is preferably adopted in which a zirconium compound, the pre-dope agent, and optionally a lithium compound such as lithium methoxide, lithium ethoxide, lithium isopropoxide, or lithium tert-butoxide are mixed, and the mixture is heat-treated at 300 to 600 ° C. The pre-dope agent thus coated is preferably pulverized as appropriate, and a method similar to the pulverization method for the powdered product is preferably adopted.

[0054] By using the lithium iron oxide obtained as described above as the pre-doping agent for the energy storage device of the present invention, pre-doping can be performed without using a metallic lithium foil, which prevents a decrease in the volumetric energy density of the energy storage device and reduces manufacturing costs. Since lithium ions can be pre-doped at a lower charging voltage, decomposition of the electrolyte can be suppressed, and an energy storage device with a very large irreversible capacity can be provided. Among these, a preferred embodiment is a positive electrode for an energy storage device that includes the pre-dope agent of the present invention and a positive electrode active material. Materials used in lithium ion batteries and lithium ion capacitors can be used as the positive electrode active material, such as layered rock salt lithium oxides containing transition metal elements selected from Ni, Co, Mn, and Al; spinel lithium oxides containing transition metal elements selected from Ni, Co, Mn, Ti, Fe, Cr, Zn, and Cu; and LiFePO 4 and carbon-based materials such as activated carbon, acetylene black, ketjen black, and graphene sheets. As the layered rock salt type lithium oxide, LiNiO 2 , LiCoO 2 , Li 2 MnO 3 , Li(Ni 1/3 Co 1/3 Mn 1/3 ) O 2 , Li(Ni 0.5 Co 0.2 Mn 0.3 ) O 2 , Li(Ni 0.6 Co 0.2 Mn 0.2 ) O 2 , Li(Ni 0.8 Co 0.1 Mn 0.1 ) O 2 , Li(Ni 0.8 Co 0.15 Al 0.05 ) O 2 The spinel-type lithium oxides include LiMn 2 O 4 , LiMn 1.5 Ni 0.5 O4 Examples include:

[0055] In the positive electrode, the content of the pre-dope agent is preferably 1 to 60 wt% relative to the total weight of the pre-dope agent and the positive electrode active material. If the content of the pre-dope agent is less than 1 wt%, the irreversible capacity is small and the potential of the negative electrode, such as graphite or silicon, may not be able to be lowered. Therefore, the content of the pre-dope agent is more preferably 2 wt% or more, and even more preferably 5 wt% or more. On the other hand, if the content of the pre-dope agent exceeds 60 wt%, the energy density may decrease due to a decrease in the content of the positive electrode active material. Therefore, the content of the pre-dope agent is more preferably 55 wt% or less, and even more preferably 45 wt% or less.

[0056] In the present invention, a more preferred embodiment is an electricity storage device having the positive electrode as a constituent element. As the negative electrode in the electricity storage device, carbon-based materials such as graphite and activated carbon, silicon-based materials such as silicon and silicon monoxide, metal materials such as tin, aluminum and germanium, and sulfur can be suitably used. Furthermore, as the electrolyte in the electricity storage device, LiPF 6 , LiBF 4 , LiClO 4 Suitable examples of the electric storage device include an electrolytic solution (liquid electrolyte) in which a lithium salt such as lithium ion battery is dissolved in an organic solvent, and a solid electrolyte. The type of the electric storage device is not particularly limited, and at least one type of electric storage device selected from the group consisting of a lithium ion battery, an all-solid-state battery, a lithium ion capacitor, and an electric double layer capacitor is suitable. Among these, at least one type of electric storage device selected from the group consisting of a lithium ion battery and a lithium ion capacitor is more suitable. Among lithium ion capacitors, a graphite-based lithium ion capacitor using graphite in the negative electrode is a more suitable embodiment.

[0057] The pre-dope agent of the present invention can exert its effect as a pre-dope agent if it is present between the positive electrode and the negative electrode. For example, it can be applied to the positive electrode surface, applied to the separator surface, or incorporated into the separator. When applying it to the separator surface to form a pre-dope agent layer, a slurry prepared by mixing the pre-dope agent, a solvent, and a binder can be applied to the separator using a coater, and the solvent can be removed by drying. The pre-dope agent layer can be formed on either side of the separator, but is preferably formed closer to the positive electrode active material layer. Specifically, when the positive electrode and the negative electrode are arranged with the separator interposed therebetween, it is preferable to form the pre-dope agent layer on the surface facing the positive electrode. The pre-dope agent layer can be formed on both sides of the separator, not just on one side.

[0058] The present invention will be explained in more detail below using examples.

[0059] [Preparation of iron(III) hydroxide oxide] A ferric sulfate solution (manufactured by Jujo Synthetic Chemical Laboratory Co., Ltd.) was used to prepare 1.5 L of a 0.5 mol / L aqueous solution of ferric sulfate. 500 g of 24 wt % aqueous ammonia was added to the prepared solution, and the mixture was stirred for 30 minutes at 50° C. to obtain a suspension. The suspension was then filtered, washed with water, and dried overnight at 80° C. to obtain iron(III) hydroxide oxide.

[0060] [Preparation of Iron (III) Oxide] The iron (III) oxide hydroxide was subjected to a heat treatment in the air at 650° C. for 2 hours to obtain iron (III) oxide.

[0061] [Preparation of pre-dopant (LFO)] (Example 1) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 18 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as a first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the obtained first calcined product so that the Li / Fe = 5.2 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 5 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours, and the obtained powdered product as a second calcined product was pulverized to obtain lithium iron oxide (Li / Fe = 5.2 (molar ratio)), which is the pre-dope agent of Example 1.

[0062] (Example 2) Prepared iron (III) oxide (pulverized to a particle size of 16 μm, bulk density of 0.73 g / cm 3 ) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 18 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as the first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the first calcined product so that the Li / Fe = 5.6 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 6 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours, and the obtained powdered product as the second calcined product was pulverized to obtain lithium iron oxide (Li / Fe = 5.6 (molar ratio)), which is the pre-dope agent of Example 2.

[0063] (Example 3) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 22 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as a first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the obtained first calcined product so that the Li / Fe = 6.0 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 3 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours to obtain a powdered product as a second calcined product, to obtain a lithium iron oxide (Li / Fe = 6.0 (molar ratio)) as a pre-dope agent of Example 3.

[0064] (Example 4) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3 ) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 18 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as the first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the first calcined product so that the Li / Fe = 7.0 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 5 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours to obtain the powdered product as the second calcined product. Lithium iron oxide (Li / Fe = 7.0 (molar ratio)) was obtained as the pre-dope agent of Example 4.

[0065] (Example 5) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 18 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as the first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the first calcined product so that the Li / Fe = 8.0 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 5 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours to obtain the powdered product as the second calcined product, thereby obtaining lithium iron oxide (Li / Fe = 8.0 (molar ratio)), which is the pre-dope agent of Example 5.

[0066] (Example 6) Prepared iron (III) oxide (pulverized to a particle size of 5 μm, bulk density 0.28 g / cm 3 ) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 20 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as the first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the first calcined product so that the Li / Fe = 5.6 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 4 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours, and the obtained powdered product as the second calcined product was pulverized to obtain lithium iron oxide (Li / Fe = 5.6 (molar ratio)), which is the pre-dope agent of Example 6.

[0067] (Example 7) Prepared iron (III) oxide (pulverized to a particle size of 2 μm, bulk density 0.16 g / cm 3) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 21 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as the first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the first calcined product so that the Li / Fe = 5.6 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 4 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours, and the obtained powdered product as the second calcined product was pulverized to obtain lithium iron oxide (Li / Fe = 5.6 (molar ratio)), which is the pre-dope agent of Example 7.

[0068] (Example 8) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3 ) 100 g, and 184 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 7 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as a first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the obtained first calcined product so that the Li / Fe = 5.6 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 5 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours, and the obtained powdered product as a second calcined product was pulverized to obtain lithium iron oxide (Li / Fe = 5.6 (molar ratio)), which is the pre-dope agent of Example 8.

[0069] (Example 9) Prepared iron (III) oxide hydroxide (pulverized to a particle size of 14 μm, bulk density of 0.68 g / cm 3) 100 g, and 165 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 18 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as the first calcined product (Li / Fe = 3.5 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the first calcined product so that the Li / Fe = 5.6 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 5 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours, and the obtained powdered product as the second calcined product was pulverized to obtain lithium iron oxide (Li / Fe = 5.6 (molar ratio)), which is the pre-dope agent of Example 9.

[0070] (Example 10) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3 ) 100 g, and 53 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm pulverized to 18 μm) were dry mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550 ° C. for 4 hours to obtain a powdered product as the first calcined product (Li / Fe = 1.0 (molar ratio)). Next, anhydrous lithium hydroxide was added to the powdered product as the first calcined product so that the Li / Fe = 5.6 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture of the first calcined product (particle diameter 4 μm) was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900 ° C. for 4 hours, and the obtained powdered product as the second calcined product was pulverized to obtain lithium iron oxide (Li / Fe = 5.6 (molar ratio)), which is the pre-dope agent of Example 10.

[0071] (Example 11) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3100 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.; particle size 285 μm pulverized to 18 μm) was dry-mixed using a mixer. The resulting dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 550°C for 4 hours to obtain a powdered product (Li / Fe = 5.0 (molar ratio)). Next, anhydrous lithium hydroxide was added to the resulting powdered product (first calcined product) so that the Li / Fe ratio became 5.6 (molar ratio), and the mixture was pulverized and mixed using a dry bead mill. The obtained pulverized mixture (particle diameter 5 μm) of the first fired product was fired in a firing furnace in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900° C. for 4 hours, and the obtained powdery product, which was the second fired product, was pulverized to obtain lithium iron oxide (Li / Fe=5.6 (molar ratio)) which was the pre-dopant of Example 11.

[0072] (Example 12) In a dry room maintained at a dew point of -30 ° C., 50 g of the lithium iron oxide produced in Example 9 and 5 g of tetraethoxysilane (KBM-04, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed for 20 minutes using a tabletop blender (Iwatani Corporation, Labo Mill Surplus), and the resulting treated powder was dried in a dryer at 150 ° C. for 3 hours. The resulting dried product was pulverized using a mortar to obtain a surface-treated lithium iron oxide (Li / Fe = 5.6 (molar ratio)) which is the pre-dope agent of Example 12. When the amount of Si in the pre-dope agent of Example 12 was determined using an X-ray fluorescence analyzer (Rigaku Corporation, Supermini), the Si / Fe (molar ratio) was 0.066. When the element concentration from the outermost surface to a depth of 1 nm in the pre-dope agent of Example 12 was determined using an X-ray photoelectron analyzer, the element concentration of Si was 3%.

[0073] (Example 13) In a dry room maintained at a dew point of -30 ° C., 50 g of the lithium iron oxide prepared in Example 9 was added to a 500 mL polypropylene container containing 10 mm and 5 mm zirconia balls, and 3 g of acetylene black (Denka Black, manufactured by Denka Co., Ltd.) was added. The mixture was pulverized and mixed for 3 hours on a pot mill rotating table (ANZ-100S, manufactured by Nitto Kagaku Co., Ltd.), thereby obtaining a surface-treated lithium iron oxide (Li / Fe = 5.6 (molar ratio)) which is the pre-dope agent of Example 13. Using a carbon content analyzer (J Science Lab Co., Ltd., JMA-1000), the carbon content of the pre-dope agent of Example 13 was determined, and the carbon content was 5.9 wt%. Using an X-ray photoelectron analyzer, the element concentration from the outermost surface to a depth of 1 nm of the pre-dope agent of Example 13 was determined, and the element concentration of C was 20%.

[0074] (Example 14) In a dry room maintained at a dew point of -30 ° C., 50 g of the lithium iron oxide prepared in Example 9, 1.1 g of lithium ethoxide (manufactured by Sigma-Aldrich), and 6.7 g of pentaethoxy niobium (manufactured by Kanto Chemical Co., Ltd.) were mixed for 20 minutes using a benchtop blender (manufactured by Iwatani Corporation, Labo Mill Surplus), and the resulting treated powder was dried in a dryer at 400 ° C. for 0.5 hours. The resulting dried product was pulverized using a mortar to obtain a surface-treated lithium iron oxide (Li / Fe = 5.7 (molar ratio)) which is the pre-dope agent of Example 14. Using a fluorescent X-ray analyzer (manufactured by Rigaku Corporation, Supermini), the amount of Nb in the pre-dope agent of Example 14 was determined, and the Nb / Fe (molar ratio) was 0.065. The element concentration of the pre-dopant of Example 14 from the outermost surface to a depth of 1 nm was determined using an X-ray photoelectron analyzer, and the element concentration of Nb was found to be 6%.

[0075] (Comparative Example 1) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3100 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size of 285 μm was pulverized to 18 μm) and 263 g of lithium hydroxide monohydrate were dry-mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900° C. for 4 hours using a calcination furnace, and the obtained powdery product was pulverized to obtain lithium iron oxide (Li / Fe=5.0 (molar ratio)) as a pre-dopant of Comparative Example 1.

[0076] (Comparative Example 2) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3 100 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size 285 μm was pulverized to 18 μm) and 273 g of lithium hydroxide monohydrate were dry-mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900° C. for 4 hours using a calcination furnace, and the obtained powdery product was pulverized to obtain lithium iron oxide (Li / Fe=5.2 (molar ratio)) as a pre-dopant of Comparative Example 2.

[0077] (Comparative Example 3) Prepared iron (III) oxide (pulverized to a particle size of 15 μm, bulk density of 0.70 g / cm 3 100 g of lithium hydroxide monohydrate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., particle size of 285 μm was pulverized to 18 μm) and 294 g of lithium hydroxide monohydrate were dry-mixed using a mixer. The obtained dry mixture was calcined in a nitrogen atmosphere with an oxygen concentration of 500 ppm at 900° C. for 4 hours using a calcination furnace, and the obtained powdery product was pulverized to obtain lithium iron oxide (Li / Fe=5.6 (molar ratio)) as a pre-dopant of Comparative Example 3.

[0078] [Evaluation of Pre-dopant] In the evaluation of the pre-dopant below, unless otherwise specified, measurements were carried out in a dry room with a dew point of −20° C. or less or in an inert gas atmosphere of nitrogen or argon.

[0079] (Composition Analysis) By ICP optical emission spectroscopy, the molar ratio of Li / Fe and SO were measured for each pre-dopant obtained in the examples and comparative examples using a plasma optical emission analyzer "SPECTRO ARCOS" manufactured by Hitachi High-Tech Science Corporation. 3The content was measured, and the results are shown in Table 2.

[0080] (Calculation of crystal lattice constant, lattice volume, half-width and peak intensity ratio) Using an XRD device "Empyrean" manufactured by Malvern Panalytical, the peak position and half-width of each pre-dopant obtained in the examples and comparative examples were measured using Cu Kα radiation. The measurement was carried out under atmospheric pressure using a dome-shaped sample holder for air-sensitive samples manufactured by Malvern Panalytical. At this time, Si powder (manufactured by Katayama Chemical Industry Co., Ltd.) was used as an internal standard substance, and the measurement was carried out by mixing it with each pre-dopant at a weight ratio of 5 wt%. The crystal lattice constant and lattice volume were refined using analysis software (HighScore Plus). The analysis was carried out by correcting the peak position based on the peak of Si (111), and then Li 5 FeO 4 (ICSD: 01-075-1253) was used as an approximate structural model, and Rietveld analysis (<Phase fit> Default Rietveld) was performed to calculate the crystal lattice constant and lattice volume V. The results are shown in Table 2.

[0081] (Method for measuring specific surface area) The specific surface area of ​​each pre-dope agent obtained in Examples and Comparative Examples was measured by the BET method using a fully automatic specific surface area measuring device (Macsorb HM model-1208, manufactured by Mountec Co., Ltd.). The degassing process was carried out under the conditions of 150°C and 20 minutes. The results are shown in Table 3.

[0082] (Method for measuring volume resistivity) The volume resistivity of each pre-dope agent obtained in Examples and Comparative Examples was measured using a high resistivity meter (Hilester UX, manufactured by Mitsubishi Chemical Analytech Co., Ltd.). The results were calculated based on the resistance value at 5 kN. The results are shown in Table 3.

[0083] (Method of measuring particle size distribution) The average particle diameter (D50) of each pre-dope agent obtained in Examples and Comparative Examples was measured using a particle size distribution measuring device (Microtrac MT-3000, manufactured by Nikkiso Co., Ltd.). At this time, isopropyl alcohol with a water content of 2000 ppm or less by the Karl Fischer method was used as a medium, and the measurement was performed in a dispersed state by irradiating ultrasonic waves with an output of 40 W for 30 seconds. The results are shown in Table 3.

[0084] (Particle size distribution index D10 / D50 and D90 / D50) The particle diameters D10, D50 and D90 of each pre-dope agent obtained in the examples and comparative examples were measured using a particle size distribution measuring device (Microtrac MT-3000, manufactured by Nikkiso Co., Ltd.). At this time, isopropyl alcohol with a water content of 2000 ppm or less by the Karl Fischer method was used as the medium, and the measurement was performed in a dispersed state by irradiating ultrasonic waves with an output of 40 W for 30 seconds. From the obtained particle diameters D10, D50 and D90 values, the particle size distribution indexes D10 / D50 and D90 / D50 were calculated. The results are shown in Table 3.

[0085] (Tap density) In order to examine the powder density of each pre-dope agent obtained in Examples and Comparative Examples, the pre-dope agent was filled into a 20 ml measuring cylinder, and tapped 200 times using a TAP DENSER, KYT-4000 manufactured by Seishin Enterprise Co., Ltd. The filling volume after tapping was read, and the tap density was calculated from this volume and the weight of the filled pre-dope agent. The results are shown in Table 3.

[0086] [Evaluation of Energy Storage Devices] (Preparation of Coin-Type Batteries for Electrochemical Evaluation) Each pre-dope agent obtained in the Examples and Comparative Examples was dissolved in N-methylpyrrolidone to prepare a slurry containing 58 wt% of the pre-dope agent obtained in each of the Examples and Comparative Examples, 30 wt% of acetylene black (Denka Black manufactured by Denka Co., Ltd.) as a conductive additive, and 12 wt% of polyvinylidene fluoride (PVDF, KF Polymer manufactured by Kureha Corporation) as a binder. The slurry was applied to an etched aluminum foil (JCC-20CB manufactured by Nippon Capacitor Industrial Co., Ltd.) as a current collector and dried at 120 ° C. for 5 minutes. The dried sheet was punched with a punching machine to prepare an electrode (positive electrode) for evaluation. Metallic lithium was used as the counter electrode, and a punched lithium foil was used. A polypropylene separator was sandwiched between the electrode for evaluation and the counter electrode to form an electrode, which was then placed in a coin-type battery container. Then, 1M LiPF was added to a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC = 1:1. 6 After injecting an electrolyte solution in which the above was dissolved, the battery container was sealed to produce a coin-type battery for electrochemical evaluation.

[0087] (Charge / Discharge Test) Using the coin-type battery prepared above, constant current charging was performed at a current density of 11.7 mA / g (per weight of pre-dope agent) until the end-of-charge voltage reached 4.3 V, followed by constant voltage charging (end condition: current value of 3.25 mA / g (per weight of pre-dope agent)). Then, a resting step was performed for 3 minutes. Next, constant current discharging was performed at a current density of 13.0 mA / g (per weight of pre-dope agent) until the voltage reached 3.0 V. The obtained charge capacity, discharge capacity, and irreversible capacity values ​​are shown in Table 3.

[0088] (Amount of Metal Ions Dissolved in Electrolyte) 2.0 g of each pre-dopant obtained in Examples and Comparative Examples was dissolved in a 1 M LiPF solution in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC = 1:1. 6The solution was added to 18.0 g of an electrolyte solution containing the above dissolved ammonium hydroxide and stored in a thermostatic chamber at 50°C for one week. The electrolyte solution was then recovered using a membrane filter, dried in an alumina crucible at 100°C for 24 hours, and then fired at 800°C for 12 hours. Next, 3 mL of 35% hydrochloric acid was added to the alumina crucible and allowed to stand for 30 minutes or more, and ion-exchanged water was added to bring the total volume to 20 mL. This was then diluted 1000 times to obtain 100 mL of test solution. The iron ion concentration in the test solution was measured using ICP atomic emission spectroscopy, and the proportion of iron ions eluted from the pre-dopant was calculated as the iron ion elution rate using the following formula. The results are shown in Table 3. Iron ion elution rate % = iron ion concentration in test solution [mg / L] x 0.1 [L] x 1000 x 100 / (2.0 [g] x 1000 [mg / g])

[0089] (Amount of eluted lithium ions) 1.0 g of each pre-dope agent obtained in the examples and comparative examples and 20 ml of N-methyl-2-pyrrolidone were added to a 30 mL screw tube, and the mixture was stirred overnight at 1000 rpm and 20 ° C. using a stirrer. Thereafter, the solution was recovered using a 0.2 μm membrane filter, and 5 ml of the recovered solution was diluted 10 times with 2-propanol. The lithium ion concentration in the diluted solution was measured by ion chromatography (ICS-2100 manufactured by Dionex), and the amount of lithium ions eluted from the pre-dope agent was calculated. The results are shown in Table 3.

[0090] (Measurement of powder color L value in Lab color system) Each pre-dope agent obtained in Examples and Comparative Examples was molded into pellets using a press, and the powder color L value was measured when regular reflection light was removed using a spectrophotometer (CM-2500d manufactured by Konica Minolta, Inc.). The pellet was prepared by filling 4 g of each pre-dope agent into a 35φ aluminum ring, and pressing it with a force of 50 kN for 30 seconds. The results are shown in Table 3.

[0091] (Fabrication of Lithium Ion Battery and Pre-Doping Treatment) Using the pre-doping agents obtained in Examples and Comparative Examples, lithium ion batteries were fabricated and pre-doped. In the fabrication process of the lithium ion battery, unless otherwise specified, the batteries were fabricated in a dry room with a dew point of -20°C or less or in an inert gas atmosphere of nitrogen or argon.

[0092] (Preparation Example 1) (Preparation of Positive Electrode) First, Li (Ni) was used as a positive electrode active material. 0.5 Co 0.2 Mn 0.3 ) O 2 (manufactured by Hosen Co., Ltd.), the pre-dope agent of Example 1 as a pre-dope agent, acetylene black ("Denka Black" manufactured by Denka Co., Ltd.) as a conductive assistant, and polyvinylidene fluoride (PVDF, "KF Polymer" manufactured by Kureha Corporation) as a binder were dissolved in N-methylpyrrolidone to prepare a positive electrode paint. The content of the pre-dope agent at this time was adjusted to 10% with respect to the total mass of the positive electrode active material and the pre-dope agent, as shown in the following calculation formula. Pre-dope agent content (%) = [mass of pre-dope agent / (mass of positive electrode active material + mass of pre-dope agent)] × 100 Furthermore, the mass ratio of the total of the positive electrode active material and the pre-dope agent / conductive assistant / binder was adjusted to 90 / 5 / 5. In other words, the mass ratio of the positive electrode active material / pre-dope agent / conductive assistant / binder was adjusted to 81 / 9 / 5 / 5. Finally, the prepared positive electrode paint was applied to an etched aluminum foil ("JCC-20CB" manufactured by Nippon Capacitor Industrial Co., Ltd.) as a current collector, dried at 120 ° C for 5 minutes, and then cut into a size of 3 cm × 4 cm to prepare a positive electrode. The design capacity at this time was 15.6 mAh.

[0093] (Preparation of negative electrode) A spherulitic graphite electrode ("HS-LIB-N-Gr-001" manufactured by Hosen Co., Ltd., nominal capacity: 1.6 mAh / cm 2 The negative electrode was fabricated by cutting out a piece of the battery having a size of 3.3 cm x 4.3 cm. The design capacity of the battery was 22.7 mAh.

[0094] (Fabrication of Lithium-ion Battery) The cathode and anode fabricated above and a polyethylene separator were stacked and then housed in an aluminum laminate case. 6The lithium ion battery of the preparation example was fabricated by injecting EC:DEC (v / v = 1 / 1) (Japan Carlit Co., Ltd.) into the battery and then vacuum sealing the battery. The positive electrode capacity of the lithium ion battery of the preparation example was 15.6 mAh, the negative electrode capacity was 22.7 mAh, and the capacity ratio of the positive and negative electrodes (negative electrode / positive electrode) was 1.5.

[0095] (Pre-doping Treatment) Next, the lithium ion battery of Preparation Example 1 was measured for charge / discharge current of 0.02 mA / cm in an environment of 25° C. using a charge / discharge measuring device (manufactured by Hokuto Denko Corporation). 2 The battery was then charged at a constant current up to 4.3 V at a current density of 0.007 mA / cm. 2 A current value of 1000 V was applied to the battery. Then, a rest period of 3 minutes was carried out. Then, the battery was discharged to 3.0 V to carry out a pre-doping treatment.

[0096] (Evaluation of Battery Characteristics) The lithium ion batteries of the above Preparation Example and Comparative Preparation Example were evaluated for battery characteristics. Specifically, using a charge / discharge measuring device (manufactured by Hokuto Denko Corporation), charge / discharge was performed in a range of 3.0 to 4.3 V in an environment of 25°C. The charge / discharge rate was 1 C per weight of positive electrode active material. The current density at a charge / discharge rate of 1 C was 160 mA / g (per weight of active material). To evaluate the battery characteristics, 10 batteries were produced for each condition. The short-circuit rate was calculated from the number of short-circuited cells out of the 10 measured cells, and is shown in Table 3.

[0097]

[0098]

[0099]

Claims

1. A pre-dope agent for an electric storage device, the main component of which is lithium iron oxide represented by the following formula (1), characterized in that in X-ray diffraction measurement, the intensity ratio (I16.7 / I23.6) between the diffraction peak intensity (I16.7) at a diffraction angle (2θ) of 16.7±0.5° and the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 40%. Li 5 Fe x O y (1) [In formula (1), x satisfies 0.6≦x<1.0, and y satisfies 3.4≦y<4.0.] 2. A pre-dope agent for an electric storage device, the main component of which is lithium iron oxide represented by the following formula (1), characterized in that the irreversible capacity at a voltage of 3.0 to 4.3 V (based on a Li reference electrode) during initial charging is 712 mAh / g or more and 1100 mAh / g or less. 5 Fe x O y (1) [In formula (1), x satisfies 0.6≦x<1.0, and y satisfies 3.4≦y<4.0.] 3. A pre-dopant described in claim 1 or 2, in which in X-ray diffraction measurement, the intensity ratio (I43.5 / I23.6) between the diffraction peak intensity (I43.5) at a diffraction angle (2θ) of 43.5±0.5° and the diffraction peak intensity (I23.6) at a diffraction angle (2θ) of 23.6±0.5° is less than 10%.

4. A pre-dopant according to any one of claims 1 to 3, wherein the space group of the crystal structure is Pbca, and the ratios of the crystal lattice constants a, b and c are a / c=0.99410 or less and b / c=1.00170 or less, respectively.

5. The pre-dopant according to any one of claims 1 to 4, which has a tap density of 1.0 to 1.5 g / ml.

6. SO 3 The pre-dopant according to any one of claims 1 to 5, wherein the content is 5,000 ppm or less.

7. A positive electrode for an electricity storage device, comprising the pre-dopant according to any one of claims 1 to 6 and a positive electrode active material.

8. An electricity storage device comprising the positive electrode according to claim 7 as a constituent element.

9. A method for producing a pre-dope agent for an electric storage device, the main component of which is lithium iron oxide obtained by mixing and firing an iron raw material and a lithium raw material, comprising: mixing the iron raw material and the lithium raw material; carrying out a first firing step of firing the mixture at 350 to 650 ° C. for 2 to 100 hours in an inert gas atmosphere having an oxygen concentration of 1 to 52,000 ppm; pulverizing the powdered product obtained as the first fired product; carrying out a second firing step of firing the pulverized powder at 700 to 1,050 ° C. for 2 to 100 hours in an inert gas atmosphere having an oxygen concentration of 1 to 52,000 ppm; and pulverizing the powdered product obtained as the second fired product to obtain lithium iron oxide. The method for producing a pre-dope agent for an electric storage device according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Energy storage devices

    JP5220510B2

  • Pre-doping agent, positive electrode, lithium-ion secondary battery and method for manufacturing the same

    JP6217990B2

  • Carbon-coated Li5FeO4

    JP6922672B2

  • Pre-doping agent for power storage device and manufacturing method thereof

    JP2020167187A

  • Pre-doping agent for power storage device and method for manufacturing pre-doping agent

    WO2021029357A1