Laser machining method and wafer manufacturing method
The laser processing method with specific scanning patterns and a trailing beam addresses the issue of depth variations in the modified layer, improving wafer peeling efficiency and manufacturing efficiency by forming a consistent peeling layer.
Patent Information
- Application Number
- PCT/JP2024/017303
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-29
- Filing Date
- 2024-05-09
- Publication Date
- 2024-12-05
AI Technical Summary
The existing wafer production methods using laser processing face variations in the formation depth of the modified layer, leading to peeling defects and reduced manufacturing efficiency due to irregularities on the peeled surface.
A laser processing method involving laser scanning with a transparent laser beam to form a modified layer at a predetermined depth, where the laser beam is moved in a specific pattern to create linear irradiation marks, and a trailing beam is used to enhance the formation of a peeling layer with reduced variations in depth.
This method effectively suppresses variations in the formation depth of the modified layer, improving the peeling process efficiency and reducing material loss during grinding or polishing, thereby enhancing the overall manufacturing efficiency.
Smart Images

Figure JP2024017303_05122024_PF_FP_ABST
Abstract
Description
Laser processing method and wafer manufacturing method CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application is based on Japanese Patent Application No. 2023-87816, filed on May 29, 2023, the contents of which are incorporated herein by reference.
[0002] The present disclosure relates to a laser processing method for a processing object made of a semiconductor material, and a wafer manufacturing method using the same.
[0003] Patent Document 1 provides a wafer production method that can efficiently produce wafers from an ingot. Specifically, the wafer production method described in Patent Document 1 includes a separation origin formation step and a wafer peeling step. In the separation origin formation step, a focal point of a laser beam having a wavelength that is transparent to a hexagonal single crystal ingot is positioned at a depth from the surface corresponding to the thickness of the wafer to be produced, and the focal point and the ingot are moved relative to each other to irradiate the laser beam onto the surface. This forms a peeling layer inside the ingot, including a modified layer and cracks extending from the modified layer. In the wafer peeling step, a plate-like object corresponding to the thickness of the wafer is peeled off from the ingot at the peeling layer serving as a separation origin, thereby producing a hexagonal single crystal wafer.
[0004] Patent No. 6482389
[0005] In the wafer production method described in Patent Document 1, variations in the depth of the modified layer may occur. Variations in the depth of the modified layer can result in unevenness on the peeled surface, which increases the amount of grinding or polishing required, or can cause peeling defects, resulting in reduced manufacturing efficiency. The present disclosure has been made in consideration of the circumstances exemplified above. That is, the present disclosure provides a technology for suppressing variations in the depth of the modified layer or peeled layer, for example. Note that in each section of the application documents, each element may be assigned a reference symbol in parentheses. In this case, the reference symbol merely indicates an example of the correspondence between the element and the specific configuration described in the embodiment described below. Therefore, the present disclosure is not limited in any way by the reference symbols.
[0006] According to one aspect of the present disclosure, a laser processing method is a method of irradiating a laser beam onto an object to be processed made of a semiconductor material, and includes modified layer formation, in which a modified layer is formed at a predetermined depth from the surface by irradiating the laser beam, which is transparent to the surface of the object to be processed; the modified layer formation includes performing laser scanning, in which the irradiation position of the laser beam on the surface is moved along a first direction along the surface, while irradiating the laser beam onto the surface, multiple times while changing the position in a second direction on the surface that is perpendicular to the first direction and along the surface, to form multiple irradiation trajectories along the second direction, each consisting of linear irradiation marks of the laser beam along the first direction; and in one laser scan, the laser beam is moved relative to the object to be processed along the first direction and irradiated intermittently, thereby forming the irradiation marks at each of the multiple irradiation positions, and irradiating the subsequent laser beam onto the irradiation marks formed by irradiation of the preceding laser beam. According to another aspect of the present disclosure, a wafer manufacturing method is a method for obtaining a wafer from an ingot, comprising: forming a delamination layer from a surface at one end side in a height direction of the ingot by irradiating the surface with a transparent laser beam, thereby forming a delamination layer from the surface to a depth corresponding to a thickness of the wafer; the delamination layer formation includes: performing laser scanning, in which the irradiation position of the laser beam on the surface is moved along a first direction along the surface, while irradiating the surface with the laser beam, multiple times while changing the position in a second direction on the surface that is perpendicular to the first direction and along the surface, thereby forming multiple irradiation trajectories along the second direction, each consisting of linear irradiation marks of the laser beam along the first direction, to form the delamination layer; and in one laser scanning, the laser beam is moved relative to the ingot along the first direction and irradiated intermittently, thereby forming the irradiation marks at each of the multiple irradiation positions, and irradiating the subsequent laser beam onto the irradiation marks formed by irradiation of the preceding laser beam.According to yet another aspect of the present disclosure, a laser processing method is a method of irradiating a laser beam onto an object to be processed made of a semiconductor material, and includes modified layer formation, in which a modified layer is formed at a predetermined depth from the surface by irradiating the laser beam, which is transparent to the surface of the object to be processed; the modified layer formation includes performing laser scanning, in which the irradiation position of the laser beam on the surface is moved along a first direction along the surface, while irradiating the laser beam onto the surface multiple times while changing the position in a second direction on the surface that is perpendicular to the first direction and along the surface, to form multiple irradiation locus lines along the second direction, each consisting of linear irradiation marks of the laser beam along the first direction; and in one laser scan, the laser beam is moved relative to the object to be processed along the first direction and irradiated intermittently, thereby forming the irradiation marks at each of the multiple irradiation positions, and a trailing beam, which is the laser beam that follows, is irradiated between a pair of irradiation marks formed by irradiation of a leading beam, which is the laser beam that follows, and arranged in the first direction.According to yet another aspect of the present disclosure, a wafer manufacturing method is a method for obtaining a wafer from an ingot, comprising: forming a delamination layer from a surface at one end side in a height direction of the ingot by irradiating the surface with a transparent laser beam, thereby forming a delamination layer from the surface to a depth corresponding to a thickness of the wafer; the delamination layer formation includes: performing laser scanning, in which the irradiation position of the laser beam on the surface is moved along a first direction along the surface, while irradiating the surface with the laser beam, multiple times while changing the position in a second direction on the surface that is perpendicular to the first direction and along the surface, thereby forming multiple irradiation locus lines consisting of linear irradiation marks of the laser beam along the first direction, along the second direction, to form the delamination layer; and the laser scanning is performed once to form the irradiation marks at each of the multiple irradiation positions by intermittently irradiating the laser beam while moving the laser beam relative to the ingot along the first direction, and irradiating a trailing beam, which is the trailing laser beam, between a pair of irradiation marks formed by irradiation of a leading beam, which is the leading laser beam, and arranged in the first direction.
[0007] 1 is a side view showing an outline of a wafer manufacturing method according to an embodiment of the present disclosure; FIG. 2 is a process diagram showing an outline of the wafer manufacturing method; FIG. 3 is a side view showing an outline of a separation layer formation step shown in FIG. 2 , i.e., a laser processing method according to an embodiment of the present disclosure; FIG. 4 is a plan view showing a schematic configuration of an ingot that has undergone the separation layer formation step shown in FIGS. 2 and 3 ; FIG. 5 is a diagram showing a state of formation of an irradiation mark when a laser beam is scanned in a direction perpendicular to the off-angle direction in the wafer manufacturing method of Comparative Example 1; FIG. 6 is a diagram showing a state of formation of an irradiation mark when a laser beam is scanned in a direction perpendicular to the off-angle direction in the wafer manufacturing method of Comparative Example 1; FIG. 7 is a diagram showing a state of formation of an irradiation mark when a laser beam is scanned in the off-angle direction in the wafer manufacturing method of Comparative Example 2; FIG. 8 is a diagram showing a state of formation of an irradiation mark when a laser beam is scanned in the off-angle direction in the wafer manufacturing method of Comparative Example 2; FIG. 9 is a diagram showing a state of formation of an irradiation mark when a laser beam is scanned in the off-angle direction in the wafer manufacturing method of Comparative Example 2; FIG. 1 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 2 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 3 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 4 is a diagram showing how irradiation marks are formed in a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 5 is an optical microscope photograph showing an enlarged view of a modified layer formed by a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 6 is a schematic diagram showing an enlarged view of a modified layer formed by a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 7 is an enlarged plan view showing an example of a two-dimensional scanning pattern of a laser beam in a laser processing method and a wafer manufacturing method according to an embodiment of the present disclosure. FIG. 8 is an enlarged plan view showing another example of a two-dimensional scanning pattern of a laser beam in the laser processing method and a wafer manufacturing method. FIG. 9 is an enlarged plan view showing yet another example of a two-dimensional scanning pattern of a laser beam in the laser processing method and a wafer manufacturing method. FIG. 10 is a process diagram showing an outline of a wafer manufacturing method according to another embodiment of the present disclosure.13 is a plan view showing an example of a setting mode of a measurement position in the wafer optical measurement process shown in FIG. 11. FIG. 14 is a plan view showing scanning of the measurement position in the wafer optical measurement process shown in FIG. 11. FIG. 15 is a graph showing changes in the absorption coefficient calculated from the transmittance measured at the measurement position shown in FIG. 13 depending on the measurement position. FIG. 16 is a side cross-sectional view showing differences in transmittance at the modified layer generation position in the laser slicing process, i.e., the separation layer formation process, shown in FIG. 11. FIG. 17 is a side cross-sectional view showing differences in transmittance at the modified layer generation position in the laser slicing process, i.e., the separation layer formation process, shown in FIG. 11. FIG. 18 is a side cross-sectional view for explaining an example of a method for setting laser beam irradiation conditions in the laser slicing process, i.e., the separation layer formation process, shown in FIG. 11. FIG. 19 is a plan view for explaining a method for deriving the amount of change in absorption coefficient shown in equation (2). FIG. 19 is a graph showing changes in the absorption coefficient in the depth direction of the ingot at the in-plane center position shown in FIG. 17. FIG. 19 is a graph showing changes in the absorption coefficient in the depth direction of the ingot at the first end position shown in FIG. 17 is a graph showing the change in absorption coefficient in the depth direction of the ingot at the second end position shown in FIG. 17. FIG. 18 is a graph for explaining an example of a method for deriving an absorption coefficient. FIG. 19 is a side view showing a first product body and a second product body generated for setting the laser beam irradiation conditions in the laser slicing process, i.e., the peeling layer formation process, shown in FIG. 11. FIG. 19 is a graph showing an area in which the measurement pitch is made finer in the wafer optical measurement process shown in FIG. 11. FIG. 19 is a diagram showing the formation of irradiation marks in a laser processing method and a wafer manufacturing method according to still another embodiment of the present disclosure. FIG. 19 is an enlarged plan view showing a modified example of the two-dimensional irradiation and scanning mode of the laser beam shown in FIG. 10. FIG. 20 is a diagram showing the formation of irradiation marks when the laser beam shown in FIG. 3 has an annular beam shape. FIG. 21 is a diagram showing the formation of irradiation marks when a laser beam having a beam shape different from the beam shape shown in FIG. 24 is used. FIG. 21 is a diagram showing an example of energy distribution in the beam diameter direction of the annular laser beam shown in FIG. 24.Fig. 25 is a diagram showing another example of energy distribution in the beam diameter direction of the annular laser beam shown in Fig. 24. Fig. 26 is a diagram showing the state of formation of irradiation marks in a laser processing method and a wafer manufacturing method according to a modified example.
[0008] (Embodiments) Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. It should be noted that if various modified examples applicable to one embodiment are introduced in the middle of a series of explanations related to the embodiment, it may hinder understanding of the embodiment. Therefore, the modified examples will not be introduced in the middle of a series of explanations related to the embodiment, but will be explained together after the series of explanations.
[0009] 1, a wafer 1 manufactured by the wafer manufacturing method according to this embodiment is obtained by slicing an ingot 2 that is substantially cylindrical in side view along a plane substantially perpendicular to the height direction, and is formed into a thin plate that is substantially circular in plan view. Note that, in order to simplify the illustration and description, so-called orientation flats that are normally provided on the wafer 1 and ingot 2 are not shown or described in this specification as appropriate.
[0010] 1, for ease of explanation, the wafer 1 and the ingot 2 are illustrated as being arranged coaxially along a central axis L that is parallel to the thickness direction of the wafer 1 and the height direction of the ingot 2. That is, the wafer 1 has an end face that is approximately cylindrical and surrounds the central axis L. Similarly, the ingot 2 has a side face that is approximately cylindrical and surrounds the central axis L. The central axis L is a virtual straight line that is parallel to the approximately cylindrical side or end face of the wafer 1 or the ingot 2 and passes through the axial center of the wafer 1 or the ingot 2.
[0011] In this embodiment, the ingot 2 is a single-crystal SiC ingot having a c-axis Lc and a (0001) plane Pc that are orthogonal to each other, and has an off-angle θ exceeding 0 degrees. The c-axis Lc is a crystal axis indicated by a direction index as
[0001] . The (0001) plane Pc is a crystal plane that is orthogonal to the c-axis Lc and is called a "C-plane" in the strict sense of crystallography. The off-angle θ is the angle between the central axis L of the wafer 1 or ingot 2 and the c-axis Lc, and is, for example, approximately 1 to 4 degrees. That is, the c-axis Lc of the wafer 1 and the ingot 2 is tilted at an off-angle θ exceeding 0 degrees toward the off-angle direction Dθ. The off-angle direction Dθ is the direction of movement of a point on the central axis L located on the laser-irradiated surface when the central axis L is rotated toward the c-axis Lc around the intersection of the central axis L and the c-axis Lc. The laser irradiated surface is the upper surface or top surface of the wafer 1 or ingot 2 in the drawing.
[0012] For simplicity of explanation, a right-handed XYZ coordinate system is set as shown in FIG. 1 . In this right-handed XYZ coordinate system, the off-angle direction Dθ and the positive X-axis direction are assumed to be the same direction. The X-axis and Y-axis are assumed to be parallel to the main surfaces of the wafer 1 and the ingot 2. The "main surface" is a surface perpendicular to the thickness direction of a plate-like object, and may also be referred to as the "top surface," "bottom surface," or "plate surface." Alternatively, the "main surface" is a surface perpendicular to the height direction of a columnar object such as the ingot 2, and may also be referred to as the "top surface" or "bottom surface." Furthermore, the thickness direction of the wafer 1 and the height direction of the ingot 2 are assumed to be parallel to the Z-axis. Hereinafter, any direction perpendicular to the Z-axis may be referred to as the "in-plane direction."
[0013] The wafer 1 has a pair of main surfaces, a wafer C-face 11 and a wafer Si-face 12. In this embodiment, the wafer 1 is formed so that the wafer C-face 11, which is the top surface, is inclined at an off angle θ with respect to the (0001) plane Pc. Similarly, the ingot 2 has a pair of main surfaces, an ingot C-face 21 and an ingot Si-face 22. The ingot 2 is formed so that the ingot C-face 21, which is the top surface, is inclined at an off angle θ with respect to the (0001) plane Pc. Note that in FIG. 1 , the direction in which the wafer C-face 11 and the ingot C-face 21 face is shown as the positive direction of the Z axis.
[0014] (Outline of Wafer Manufacturing Method) The wafer manufacturing method according to this embodiment is a method for obtaining a wafer 1 from an ingot 2 using laser processing. FIG. 2 is a process diagram showing a typical example of a wafer manufacturing method according to this embodiment. Below, an outline of each process in this wafer manufacturing method will be described. Note that the term "process" can also be referred to as a "procedure" or "treatment." Furthermore, the term "process" does not only refer to an independent process, but also includes cases where it is difficult or impossible to clearly distinguish from other processes once the intended purpose of the process has been achieved. The same applies to the terms "treatment" and "procedure."
[0015] (1) Separation Layer Formation Step As shown in Figure 3, a laser beam B having a predetermined degree of transparency for the ingot 2 is irradiated onto an ingot C-face 21, which is the main surface at one end in the height direction of the ingot 2. As a result, a separation layer 23 is formed from the ingot C-face 21 to a depth corresponding to the thickness of the wafer 1. Here, the "predetermined degree of transparency" refers to a degree of transparency that allows a focal point BP of the laser beam B to be formed inside the ingot 2 at a depth corresponding to the thickness of the wafer 1. The "depth corresponding to the thickness of the wafer 1" is a dimension obtained by adding a thickness corresponding to a predetermined processing allowance in a wafer flattening step or the like, which will be described later, to the target thickness of the wafer 1 as a finished product, and may also be referred to as the "depth corresponding to the thickness of the wafer 1."
[0016] (2) Wafer Peeling Process The wafer precursor 24, which is the portion between the ingot C-face 21 (laser irradiated surface) and the peeling layer 23, is peeled from the ingot 2 at the peeling layer 23. As in the expression "wafer peeling process" above, the plate-like object obtained by peeling the wafer precursor 24 from the ingot 2 may be commonly referred to as a "wafer." However, to distinguish it from the wafer 1 as a finished product having an epi-ready mirror-finished main surface, such a plate-like object will hereinafter be referred to as a "peeled body 30."
[0017] The peeled body 30 has a pair of main surfaces, a non-peeled surface 31 and a peeled surface 32. The non-peeled surface 31 is the surface on the side that did not form the peeled layer 23 before the wafer peeling process, and corresponds to the ingot C-face 21 before the peeled layer forming process and the wafer peeling process. The peeled surface 32 formed the peeled layer 23 before the wafer peeling process, and is a surface that was newly formed by the wafer peeling process. The peeled surface 32 has rough irregularities that require grinding or polishing due to variations in the depth of the peeled layer 23 and peeling during the wafer peeling process.
[0018] (3) Wafer Planarization Process At least the peeled surface 32 of the non-peeled surface 31 and the peeled surface 32, which are the main surfaces of the peeler 30, is planarized to obtain the wafer 1 as a finished product. In the wafer planarization process, in addition to general grinding stone polishing and CMP, ECMG and ECMP can be used. Note that CMP is an abbreviation for Chemical Mechanical Polishing. ECMG is an abbreviation for Electro-Chemical Mechanical Grinding. ECMP is an abbreviation for Electro-Chemical Mechanical Polishing. The wafer planarization process can be performed by using these multiple types of planarization processes alone or in appropriate combination.
[0019] (4) Ingot Planarization Process The top surface of the ingot 2 newly formed by peeling off the wafer precursor 24 at the peeling layer 23 is planarized, i.e., mirror-finished, so that it can be reused in the peeling layer formation process. In the ingot planarization process, in addition to general grinding stone polishing and CMP, ECMG and ECMP can also be used. The ingot planarization process can also be performed by using these multiple types of planarization processes alone or in appropriate combination.
[0020] 2, the peeled body 30 peeled from the ingot 2 through the peeling layer forming step and the wafer peeling step is finished into an epi-ready wafer 1 through the following steps: Rough grinding of the peeled surface 32 that will become the wafer Si surface 12; ECMG grinding of the peeled surface 32 after rough grinding; ECMP polishing of the peeled surface 32 after ECMG grinding; and Cleaning.
[0021] Furthermore, the ingot 2 remaining after the peeled body 30 has been peeled off from the ingot 2 through the peeling layer forming step and the wafer peeling step can be subjected to the peeling layer forming step again through the following steps: Rough grinding of the ingot C-face 21 newly generated by the wafer peeling step; Finish grinding of the ingot C-face 21 after rough grinding; and Cleaning.
[0022] (Details of the peeling layer forming step) Hereinafter, details of the peeling layer forming step corresponding to the laser processing method of the present disclosure will be described with reference to Figure 3 and the like in addition to Figures 1 and 2. It is assumed that the right-handed XYZ coordinate system shown in Figure 3 and the like is set to match the right-handed XYZ coordinate system shown in Figure 1. As shown in Figure 3, the peeling layer forming step is a step of forming a peeling layer 23 inside an ingot 2, which is an object to be processed and made of a semiconductor material, by irradiating the ingot 2 with a laser beam B that has transparency.
[0023] In this embodiment, the peeling layer formation process involves performing laser scanning parallel to the off-angle direction Dθ multiple times while changing the position in the line feed direction Df shown in FIG. 4 . Laser scanning refers to irradiating the ingot C-face 21 with the laser beam B while moving an irradiation position PR on the ingot C-face 21, which is the laser irradiation surface, along the off-angle direction Dθ along the ingot C-face 21. Thus, laser scanning refers to irradiation of the laser beam B over the entire width of the ingot C-face 21 in the off-angle direction Dθ. Here, the "irradiation position PR" refers to the center position of the laser beam B on the ingot C-face 21. Note that the "irradiation position PR" includes not only the position on the ingot C-face 21 that is actually irradiated with the laser beam B, but also positions that are scheduled to be irradiated with the laser beam B and positions that have been irradiated in the past. In this embodiment, a pulsed laser beam B is intermittently irradiated at discrete irradiation positions PR while moving the laser beam B relative to the ingot 2 along the off-angle direction Dθ in a single laser scan, thereby forming irradiation marks RM at each of the multiple irradiation positions PR. Therefore, "moving the irradiation position PR" refers to moving the position of the intermittently irradiated laser beam B on the ingot C-face 21 almost discontinuously or discretely. The line feed direction Df is a direction perpendicular to the off-angle direction Dθ and along the ingot C-face 21, and corresponds to the second direction in the present disclosure.
[0024] As shown in FIG. 4 , the peeling layer 23 is formed by forming a plurality of irradiation loci Ls in the line feed direction Df, each of which is composed of irradiation marks RM of the laser beam B arranged in a linear, dotted line parallel to the off-angle direction Dθ. That is, the irradiation loci Ls are an arrangement of linear, dotted irradiation marks RM formed by a single laser scan. The spacing between adjacent irradiation loci Ls in the peeling layer 23 in the line feed direction Df is hereinafter referred to as the "line pitch." The line pitch is larger than the irradiation pitch. The irradiation pitch is the spacing between adjacent irradiation marks RM included in one irradiation locus Ls. The irradiation marks RM are formed by a modified layer RA and cracks C, as shown in FIG. 5A and other figures. The modified layer RA is a modified region formed by separating SiC into silicon and carbon by irradiation with the laser beam B. Therefore, the peeling layer formation process can also be referred to as a modified layer formation process. As a result of the formation of the modified layer RA, cracks C are generated starting from the modified layer RA and propagate along the (0001) plane Pc. That is, as shown in Fig. 5A, the propagation direction of the cracks C is inclined by the off angle θ with respect to the in-plane direction parallel to the ingot C-plane 21.
[0025] As described above, the laser beam B has a predetermined degree of transparency with respect to the ingot 2. Therefore, the focal point BP is formed at a predetermined depth from the ingot C-face 21, which is the laser irradiation surface. Therefore, the modified layer RA is formed at a predetermined depth from the ingot C-face 21, which corresponds to the focal point BP. By performing laser scanning across substantially the entire width of the ingot 2 in the line feed direction Df and forming multiple irradiation trajectory lines Ls along the line feed direction Df, a peeling layer 23 is formed at a predetermined depth from the ingot C-face 21. As a result, a wafer precursor 24, which will eventually become the wafer 1, is formed on the ingot C-face 21 side of the peeling layer 23.
[0026] 5A and 5B show the formation of irradiation marks RM by a wafer manufacturing method of Comparative Example 1, which corresponds to the technology disclosed in Japanese Patent Application Laid-Open No. 2016-111143. In Comparative Example 1, laser scanning is performed not in the off-angle direction Dθ but in an in-plane direction perpendicular thereto, i.e., the line feed direction Df in FIG. 4 . According to Comparative Example 1, cracks C significantly propagate in the off-angle direction Dθ between adjacent laser scans in the off-angle direction Dθ. As a result, as shown in FIG. 5B , the processing allowance region W, which is the width in the depth direction of the irradiation marks RM, increases. The processing allowance region W corresponds to the thickness of the peeling layer 23 shown in FIG. 3 and constitutes the processing allowance in the wafer flattening process and the ingot flattening process after the wafer peeling process. In other words, the material portion removed and discarded from the peeled body 30 or the ingot 2 by grinding or polishing in the wafer flattening process and the ingot flattening process is at least equal to the processing allowance region W. Therefore, Comparative Example 1 experienced significant material loss.
[0027] On the other hand, Figures 6A to 6D show the formation of irradiation marks RM according to Comparative Example 2, in which the laser scanning direction is simply changed to a direction parallel to the off-angle direction Dθ in order to address the above-mentioned issues. When laser scanning is performed in the scanning direction Ds parallel to the off-angle direction Dθ, as shown in Figures 6A and 6B, the next irradiation mark RM is formed before the progression of the crack C in the previously formed irradiation mark RM along the off-angle direction Dθ becomes sufficiently large. In other words, the progression of the crack C in the previously formed irradiation mark RM is suppressed by the subsequently formed irradiation mark RM. Therefore, the progression of the crack C along the off-angle direction Dθ in each of the multiple irradiation marks RM arranged in the scanning direction Ds can be suppressed more than in the cases of Figures 5A and 5B.
[0028] Here, let us assume a situation in which no irradiation mark RM exists around the irradiation position PR in the in-plane direction. In such a situation, irradiation of the laser beam B tends to cause the irradiation mark RM to occur at a depth near the focal point BP. However, in reality, the laser beam B moves in the scanning direction Ds while generating irradiation marks RM one after another. Therefore, the above situation mainly occurs when forming the irradiation mark RM corresponding to the starting point of the irradiation locus line Ls, which is formed first in a single laser scan. Therefore, in most situations during laser scanning, a situation occurs in which the irradiation mark RM exists around the irradiation position PR in the in-plane direction.
[0029] That is, as shown in Figures 6B and 6C, at least a crack C in the previously formed irradiation mark RM is usually present at the in-plane position corresponding to the current irradiation position PR. This increases the absorption rate of the laser beam B in the irradiation mark RM. Furthermore, the crack C is formed along the (0001) plane Pc. Therefore, as shown in Figure 6C, the formation positions of the modified layer RA and the irradiation mark RM tend to progress along the (0001) plane Pc as the laser scans.
[0030] As the irradiation mark RM progresses along the (0001) plane Pc in the scanning direction Ds, it is formed at increasingly deeper positions, gradually moving away from the depth of the original focal point BP. This results in a situation where, at the depth corresponding to the previously formed irradiation mark RM, the applied energy density of the currently irradiated laser beam B is not high enough to generate a new modified layer RA. When this situation occurs, as shown in FIG. 6D , the newly formed modified layer RA is formed at a depth near the focal point BP of the currently irradiated laser beam B. This results in a step between the previously formed irradiation mark RM and the currently formed irradiation mark RM. Therefore, the processing allowance region W, which is the width of the irradiation mark RM in the depth direction, becomes larger. Therefore, even in Comparative Example 2, significant material loss occurs. FIG. 6E is an optical microscope photograph showing an enlarged irradiation trajectory line Ls in Comparative Example 2. As shown in Figure 6E, in the irradiation trajectory line Ls in comparison example 2, due to the variation in the formation depth of the modified layer RA in the X-axis direction, i.e., the scanning direction Ds, as described above, there are areas where the modified layer RA is in focus and areas where it is not.
[0031] Therefore, in this embodiment, the linear, i.e., one-dimensional, laser scanning direction, i.e., the traveling direction of the laser beam B or the irradiation position PR, is parallel to the off-angle direction Dθ, and the irradiation position PR of the laser beam B in this traveling direction is multi-pointed. That is, multiple laser beams B spaced apart from each other in the traveling direction can be simultaneously irradiated and scanned in a direction parallel to the off-angle direction Dθ. Then, the trailing laser beam B is irradiated onto the irradiation mark RM formed by the irradiation of the leading laser beam B in the traveling direction. Specifically, the leading laser beam B forms a small modified layer RA, and the trailing laser beam B is irradiated onto the modified layer RA to enlarge the modified layer RA.
[0032] Laser scanning in this embodiment will be described in more detail below with reference to Figures 7A to 7D. In these figures, the traveling direction is indicated as the scanning direction Ds. The leading laser beam B in the scanning direction Ds is referred to as the leading beam B1, and the trailing laser beam B is referred to as the trailing beam B2. The distance between the leading beam B1 and the trailing beam B2 in the scanning direction Ds is N times the irradiation pitch, where N is a positive integer and N≥2. The irradiation position PR corresponding to the leading beam B1 is referred to as the leading irradiation position PR1, and the irradiation position PR corresponding to the trailing beam B2 is referred to as the trailing irradiation position PR2.
[0033] First, as shown in FIG. 7A , the advance beam B1 forms an irradiation mark RM at a position corresponding to the advance irradiation position PR1. The advance beam B1 is output with lower energy, i.e., pulse energy, than when a laser beam B is irradiated once at one irradiation position PR as in the comparative examples. Note that the "single irradiation" in this case may include multiple pulsed irradiations. Thus, the modified layer RA formed by the irradiation of the relatively low-energy advance beam B1 and the amount of crack C propagation from such modified layer RA are smaller than in the comparative examples. Therefore, as shown in FIG. 7B , the focal point BP of the next advance beam B1 can be formed at a position where the irradiation mark RM formed immediately before it does not interfere. This allows the modified layers RA formed by the advance beam B1 to be formed at approximately the same depth. Therefore, as shown in FIGS. 7B and 7C , the multiple modified layers RA formed by the advance beam B1 do not propagate along the (0001) plane Pc, but rather along the same plane substantially parallel to the ingot C-face 21.
[0034] As shown in FIG. 7C , the trailing beam B2 is irradiated onto the modified layer RA formed by irradiation with the leading beam B1. As a result, the modified layer RA thickens and cracks C propagate in the line feed direction Df. Like the leading beam B1, the trailing beam B2 is output with lower energy than when a laser beam B is irradiated once at one irradiation position PR as in each comparative example. The output energy of the leading beam B1 and the trailing beam B2 may be the same or different. Specifically, for example, the output energies of the leading beam B1 and the trailing beam B2 can be appropriately adjusted depending on the transmittance of the laser beam B through the ingot 2, etc.
[0035] According to this embodiment, as shown in FIG. 7D , by sequentially irradiating the trailing beam B2 onto multiple modified layers RA formed at approximately the same depth by the leading beam B1, the irradiation marks RM progress along the same plane approximately parallel to the ingot C-face 21. This effectively suppresses variations in the depth of the modified layers RA and the irradiation marks RM. That is, it is possible to form the peeling layer 23 as thin as possible. FIG. 7E is an optical microscope photograph showing an enlarged view of the irradiation trajectory Ls in this embodiment. As shown in FIG. 7E , the irradiation trajectory Ls in this embodiment is entirely focused on the modified layer RA, regardless of its position in the X-axis direction, i.e., the scanning direction Ds. Therefore, the processing allowance region W, which results in material loss, is effectively reduced, and the process time can be minimized. Therefore, this embodiment can provide a wafer manufacturing method with higher manufacturing efficiency than conventional methods. FIG. 7F is a schematic diagram showing an enlarged view of the irradiation trajectory Ls in this embodiment. In FIG. 7F, the maximum width of the modified layer RA in the Y-axis direction, i.e., the line feed direction Df, is defined as the maximum width DY. Furthermore, the distance between adjacent modified layers RA at positions corresponding to the maximum width of the modified layer RA in the X-axis direction, i.e., the scanning direction Ds, is defined as the maximum spacing DP. The average value of the maximum width DY is defined as DYave, and the average value of the maximum spacing DP is defined as DPave. In this case, according to this embodiment, laser scanning enables the formation of an irradiation locus line Ls, i.e., a peeling layer 23, such that DYave / DPave≦5. Furthermore, it is preferable that DYave / DPave≦2. Furthermore, as in the example of FIG. 7E, it is preferable to perform laser scanning so that DYave / DPave is approximately 0.7 to 1.3.
[0036] (Line Feed Pattern) FIG. 8 shows an example of a two-dimensional scanning pattern of the laser beam B. In FIG. 8, the movement trajectory or planned movement trajectory of the laser beam B or the irradiation position PR is shown as a first scanning line Sc1 and a second scanning line Sc2. The first scanning line Sc1 and the second scanning line Sc2 are both parallel to the off-angle direction Dθ. The first scanning line Sc1 and the second scanning line Sc2 are arranged alternately and at equal intervals in the line feed direction Df. The distance D1 between adjacent first scanning lines Sc1 and second scanning lines Sc2 in the line feed direction Df is the same as the line pitch. The distance D2 between two adjacent first scanning lines Sc1 in the line feed direction Df is twice the line pitch. Similarly, the distance D2 between two adjacent second scanning lines Sc2 in the line feed direction Df is twice the line pitch. Scanning of the laser beam B on the first scanning line Sc1 is referred to as a first laser scan. Similarly, scanning of the laser beam B on the second scanning line Sc2 will be referred to as a second laser scan. The same applies to examples of scanning modes shown in Figs. 9 and 10, which will be described later.
[0037] In the scanning mode shown in Figure 8, the relative movement direction between the laser beam B and the ingot 2 is opposite between one laser scan and the next laser scan. That is, in this scanning mode, the scanning direction Ds, which is the movement direction of the irradiation position PR in the first laser scan, is the same as the off-angle direction Dθ, while the scanning direction Ds in the second laser scan is opposite to the off-angle direction Dθ. Then, the first laser scan and the second laser scan, in which the scanning directions Ds are opposite to each other, are performed alternately. In other words, the laser scan is performed in a zigzag pattern. The scanning direction Ds corresponds to the first direction in this disclosure.
[0038] As described above, the crack C propagates along the (0001) plane Pc upon irradiation with the laser beam B. Here, the propagation in the off-angle direction Dθ can be limited to approximately the irradiation pitch due to the formation of a modified layer RA by the leading beam B1 prior to the irradiation of the trailing beam B2. On the other hand, the propagation in the line feed direction Df is not particularly limited unless a preceding irradiation locus Ls is formed. Therefore, in the scanning mode shown in FIG. 8 , particularly when a small line pitch is set, a situation may occur in which the crack C extending from the previously formed irradiation locus Ls reaches the current irradiation position PR. If this situation occurs, the laser beam B will be irradiated onto the area where the crack C exists. As described above, the absorption rate at the location where the crack C occurs may increase, resulting in a variation in the depth of the modified layer RA. Alternatively, the crack C may reflect the laser beam B, causing the focal point BP to occur at a shallower depth than expected, resulting in the modified layer RA occurring at a shallower position than usual. Therefore, if the above situation occurs, the processing allowance area W will become larger, and there is a concern that material loss will increase.
[0039] Therefore, in the scanning mode shown in FIG. 9 , second laser scanning is performed between irradiation loci Ls formed by first laser scanning on adjacent first scanning lines Sc1 in the line feed direction Df. Specifically, as shown in FIG. 9 , the multiple first scanning lines Sc1 are numbered Sc11, Sc12, Sc13, ... Sc1m, Sc1n from top to bottom in the figure. m and n are integers of 1 or greater indicating ordinal numbers, and for the sake of simplicity, n = m + 1 is used. Similarly, the multiple second scanning lines Sc2 are numbered Sc21, Sc22, Sc23, ... Sc2m from top to bottom in the figure. In this scanning mode, an m-th first laser scanning and the subsequent n-th first laser scanning are performed, followed by an m-th second laser scanning. In this manner, in this scanning mode, a second laser scan is performed between adjacent irradiation trajectory lines Ls in the line feed direction Df, which are formed by a first laser scan performed at a pitch twice the line pitch in the line feed direction Df.
[0040] According to this scanning mode, when the first laser scan is performed, it is easy to realize a situation in which the crack C extending from the previously formed irradiation locus line Ls does not reach the corresponding first scan line Sc1. Therefore, in the first laser scan, the laser beam B is not interfered with by the crack C, and the modified layer RA can be formed to a substantially uniform depth across the entire width of the ingot 2 in the scanning direction Ds. Therefore, according to this scanning mode, material loss due to variations in the formation depth of the modified layer RA can be effectively suppressed.
[0041] The order in which the multiple first laser scans and the multiple second laser scans are performed is not particularly limited. That is, for example, the first laser scan may be performed over the entire width of the ingot 2 in the line feed direction Df, followed by the second laser scan. That is, the first laser scan may be completed first, and then the second laser scan may be performed. In this case, the scanning directions Ds of the multiple first laser scans may all be the same, or may be set alternately between the same direction as the off-angle direction Dθ and the opposite direction. The same applies to the scanning directions Ds of the multiple second laser scans. Alternatively, after the first and second first laser scans are performed, the second laser scans and the first laser scans may be performed alternately, for example, as in Sc11, Sc12, Sc21, Sc13, Sc22, Sc14, Sc23, ...
[0042] (Simultaneous Multipoint Irradiation in the Line Feed Direction) Figure 10 shows a scanning mode in which, in a single laser scan, multiple laser beams B, each at a different position in at least the line feed direction Df, are irradiated onto the ingot C-face 21, thereby simultaneously forming multiple irradiation loci Ls. Specifically, Figure 10 shows an example in which, in a single laser scan, a total of six laser beams B are scanned in the scanning direction Ds, two in the scanning direction Ds and three in the line feed direction Df. Note that the positions in the scanning direction Ds of the three laser beams B or irradiation positions PR arranged in the line feed direction Df may be set to be offset by a predetermined amount as shown in Figure 10, or may be the same position. In other words, the three laser beams B or irradiation positions PR arranged in the line feed direction Df may be arranged parallel to the line feed direction Df.
[0043] In this specific example, the multiple first scanning lines Sc1 arranged in the line feed direction Df are divided into groups of three, starting from the top in the drawing, as follows: Sc11a, Sc11b, Sc11c, Sc12a, Sc12b, Sc12c, Sc13a, Sc13b, Sc13c.... The multiple second scanning lines Sc2 are also divided into groups of three, starting from the top in the drawing, as follows: Sc21a, Sc21b, Sc21c, Sc22a, Sc22b, Sc22c, Sc23a, Sc23b, Sc23c.... The first laser scanning is then performed simultaneously on Sc11a, Sc11b, and Sc11c, and then the first laser scanning is performed simultaneously on the scanning lines Sc12a, Sc12b, and Sc12c, and so on, with the first laser scanning being performed on each group of three first scanning lines Sc1. Thereafter, the second laser scan is performed on each of the three grouped second scan lines Sc2 in the same manner, thereby achieving the same effect as the scanning modes shown in Fig. 8 and Fig. 9, but with a shorter cycle time.
[0044] Second Embodiment A second embodiment will be described below. In the description of this embodiment, differences from the first embodiment will be mainly described. In addition, the same reference numerals are used for identical or equivalent parts between the first embodiment and this embodiment. Therefore, in the following description of this embodiment, for components having the same reference numerals as those in the first embodiment, the description of the first embodiment may be used as appropriate unless there is a technical contradiction or a special additional explanation. The same applies to a third embodiment described below.
[0045] In this embodiment, the irradiation conditions of the laser beam B are controlled based on the measurement results of the transmittance of the laser beam B through the semiconductor material constituting the ingot 2 in the first embodiment. Specifically, in this embodiment, the optical characteristics, i.e., the transmittance and refractive index, of the obtained wafer 1 or peeled body 30 are measured at multiple positions in the scanning direction Ds and the line feed direction Df, and the irradiation conditions of the next laser beam B are controlled based on the measurement results. The irradiation conditions include, for example, the irradiation energy and the irradiation distance.
[0046] FIG. 11 shows an outline of the wafer manufacturing method according to this embodiment. In FIG. 11, "Loading / Unloading" refers to the loading and unloading steps of the workpiece, i.e., the peeled body 30 or the ingot 2. "Laser Slicing" refers to the peeled layer formation step. "Rough Grinding" refers to the rough grinding step of the main surface of the ingot 2 or the peeled body 30. For example, a grinding material with a grit size of about #800 can be used for rough grinding. "Finish Grinding" refers to the finish grinding step of the surface. For example, a grinding material with a grit size of about #30000 can be used for finish grinding. "Wafer Beveling" refers to the chamfering of the corners of the outer edge of the peeled body 30 in the radial direction. The "radial direction" here refers to the direction extending radially from the center of the peeled body 30 in the in-plane direction. "Wafer Optical Measurement" refers to the process of measuring the optical characteristics of the peeled body 30 after finish grinding at multiple positions in the scanning direction Ds and the line feed direction Df. "Ingot cleaning" refers to a process of cleaning the ingot 2 after finish grinding. The arrows on the left side of the blocks indicating each process indicate the processing flow of the ingot 2. The arrows on the right side of the blocks indicating each process indicate the processing flow of the wafer 1 or the peeled body 30, which may be commonly referred to as a "wafer."
[0047] Referring to FIG. 11 , first, an ingot 2 is loaded into a wafer manufacturing apparatus. Next, the loaded ingot 2 is subjected to a separation layer forming process by laser slicing, i.e., irradiation with a laser beam B. Subsequently, in a wafer separation process, a separation body 30 is separated from the ingot 2 that has undergone the separation layer forming process. The top surface of the ingot 2 newly generated in the ingot 2 that has undergone the wafer separation process is flattened by rough grinding and finish grinding. Thereafter, the ingot 2 is cleaned and then subjected to the separation layer forming process again. Note that the ingot 2 that has undergone the separation layer forming process or the ingot cleaning process is ejected from the wafer manufacturing apparatus if its height falls below a predetermined value.
[0048] The peeled body 30 peeled from the ingot 2 in the wafer peeling process is subjected to beveling, rough grinding, and finish grinding, and then optical measurement. The measurement results are used to determine the irradiation conditions of the laser beam B in the next peeling layer formation process. That is, based on the optical measurement results for each location in the in-plane direction of the wafer 1, the irradiation conditions for each location in the in-plane direction of the ingot C-face 21 in the next peeling layer formation process are controlled. This enables fine-tuned changes to the irradiation conditions to accommodate variations in optical properties from location to location in the in-plane direction, thereby reducing material loss. Note that only one of the transmittance and refractive index may be measured. Alternatively, the transmittance and refractive index may be measured on the finally obtained epi-ready wafer 1. Depending on the rough grinding conditions, finish grinding may not be necessary. That is, rough grinding and finish grinding may be integrated.
[0049] FIG. 12 shows an example of how optical measurement positions are set in a generator 100. The generator 100 is the target of optical measurement, and corresponds to a wafer 1 or a peeled body 30 whose surface has been flattened to a predetermined degree after being peeled from an ingot 2. In this example, the optical measurement positions are set at a constant measurement pitch in each of the X-axis direction and the Y-axis direction. The measurement pitch is, for example, about 1 mm. The X-axis direction is parallel to the scanning direction Ds shown in FIG. 8 and the like. The Y-axis direction is parallel to the line feed direction Df shown in FIG. 8 and the like.
[0050] Here, FIG. 14 shows how the absorption coefficient of laser beam B changes with the change in measurement position when optical measurements are performed at multiple measurement positions on the measurement line Lx, as shown in FIG. 13. The measurement line Lx is a virtual line that passes through the center of the generator 100 in the in-plane direction and is parallel to the X-axis. In FIG. 14, the horizontal axis indicates the measurement position, measured in mm, when the center of the generator 100 in the in-plane direction is set as the origin, i.e., "0." As shown in FIG. 14, the absorption coefficient is not constant in the in-plane direction but changes with the change in measurement position. The absorption coefficient is obtained, i.e., calculated, using the following equation (1). In the following equation (1), α represents the absorption coefficient, D represents the workpiece thickness, i.e., the thickness of the generator 100, and T represents the transmittance.
[0051] This embodiment is particularly effective when the wafer 1 or ingot 2 has a facet region RF as shown in FIGS. 12 and 13 . The facet region RF may also be referred to as a “facet portion.” Regions other than the facet region RF are hereinafter referred to as non-facet regions RN. The non-facet region RN may also be referred to as a “non-facet portion.” It is known that the intensity of the laser beam B reaching the focal point BP is stronger in the non-facet region RN than in the facet region RF. Specifically, the region with a high absorption coefficient on the right side in FIG. 14 corresponds to the facet region RF. Furthermore, as shown in FIG. 14 , even the non-facet region RN, which has a lower absorption coefficient than the facet region RF, may have a distribution in the in-plane direction, i.e., the radial direction. The “radial direction” refers to the direction extending radially from the center of the in-plane direction of the generator 100 along the in-plane direction.
[0052] 15A to 15C show how the location where the modified layer RA occurs changes with changes in transmittance, i.e., absorption coefficient. In the figures, the density of the hatching on the ingot 2 corresponds to the transmittance or absorption coefficient. That is, the darker the hatching, the lower the transmittance and, therefore, the higher the absorption coefficient. The location where the modified layer RA occurs is the position where the laser beam B is focused, and can be indicated by the dimension in the depth direction of the ingot 2 from the ingot C-face 21, which is the laser irradiation surface. Here, the depth direction of the ingot 2 is a direction parallel to the height direction of the ingot 2, and more specifically, the direction from the ingot C-face 21 toward the ingot Si-face 22. In the figures, the circle drawn with a dashed line next to the modified layer RA indicates the focused state, i.e., the beam diameter, of the laser beam B at the location where the modified layer RA occurs.
[0053] First, referring to FIG. 15A , as the laser beam B travels through the ingot 2 in the depth direction, it is focused while attenuating according to the absorption coefficient. When the energy density increases to a predetermined level due to the focusing, it reaches the processing threshold, and a modified layer RA is formed. Here, when the transmittance is low, i.e., when the absorption coefficient is high, the amount of attenuation is large. As a result, the energy density corresponding to the processing threshold is reached at a deep position where the focusing cross-sectional area is smaller, as shown in FIG. 15B, and the modified layer RA is generated. On the other hand, when the transmittance is high, the amount of attenuation is small. As shown in FIG. 15C, the energy density corresponding to the processing threshold is reached even at a shallow position where the focusing cross-sectional area is larger, and the modified layer RA is generated. Thus, if the position where the modified layer RA is generated varies due to differences in transmittance, i.e., absorption coefficient, the surface of the product 100 after peeling becomes rough, and the amount of processing required for grinding and polishing, i.e., material loss, increases.
[0054] Therefore, in this embodiment, the transmittance is measured at multiple positions in the in-plane direction, and the irradiation conditions of the laser beam B at each of the multiple positions in the in-plane direction are controlled based on the measurement results. Specifically, this embodiment acquires, i.e., calculates, the absorption coefficient based on the transmittance measured for the product 100 generated in the past, including the previous generation. Then, this embodiment acquires the trend of change in the absorption coefficient in the height direction, i.e., the depth direction, of the ingot 2 for each different position in the plane, and determines the irradiation energy of the laser beam B based on this. That is, for example, the lower the transmittance, the higher the irradiation energy.
[0055] A specific example of controlling the next irradiation conditions of the laser beam B from the optical measurement results of the product 100 obtained previously will be described below. First, the transmittance etc. of the product 100 obtained previously is measured using a transmittance meter. At this time, the workpiece thickness, which is the thickness of the product 100, is also measured. The absorption coefficient is calculated based on the measured transmittance, workpiece thickness and the above formula (1). Then, the input energy, which is the irradiation energy of the laser beam B, is derived using the following formula (2). In the following formula (2) and in FIG. 16, I 0 indicates the input energy, I indicates the processing threshold, i.e., the minimum applied energy required for modification, z indicates the depth, and k indicates the amount of change in the absorption coefficient in the depth direction, i.e., the change tendency of the absorption coefficient in the depth direction of the ingot 2.
[0056] A method for deriving the amount of change in the absorption coefficient will be described below. As shown in Figure 17, the central position of the ingot 2 in the in-plane direction is defined as the in-plane central position Ma. Furthermore, the position on a measurement line Lx that passes through the in-plane central position Ma and is parallel to the X-axis and is an end position of the ingot 2 located within the facet region RF is defined as the first end position Mb. Furthermore, the position on this measurement line Lx that is opposite to the first end position Mb is defined as the second end position Mc. The second end position Mc is a position that is approximately symmetrical to the first end position Mb with respect to the in-plane central position Ma.
[0057] Figure 18A shows how the absorption coefficient changes in the depth direction of the ingot 2 at the in-plane center position Ma. Figure 18B shows how the absorption coefficient changes in the depth direction of the ingot 2 at the first end position Mb. Figure 18C shows how the absorption coefficient changes in the depth direction of the ingot 2 at the second end position Mc. As shown in Figures 18A to 18C, it can be seen that the change in the absorption coefficient in the depth direction of the ingot 2 has a certain tendency and differs for each in-plane position. Based on this tendency of change in the absorption coefficient in the depth direction for each in-plane position, the amount of change in the absorption coefficient can be derived, and this value can be added to or multiplied by the absorption coefficient obtained previously and used to determine the input energy for the next processing.
[0058] For example, as shown in FIG. 19, the previously acquired absorption coefficient α n-1 and the absorption coefficient α obtained two times previously n-2 Based on the amount of change in the absorption coefficient, the estimated value α n Specifically, for example, the previously acquired absorption coefficient α n-1 and the absorption coefficient α obtained two times previously n-2 The difference between the previous absorption coefficient α n-1 The absorption coefficient estimate α n Then, the absorption coefficient estimate α n Based on this, it is possible to determine the irradiation energy of the laser beam B. When calculating the amount of change in the absorption coefficient, statistical processing using a so-called "smoothing filter" or the like may be performed.
[0059] 20 , a first product 101 and a second product 102 are produced. The first product 101 is a product 100 obtained from one end of the ingot 2 in the height direction, i.e., the ingot C-face 21 side. The second product 102 is a product 100 obtained from the other end of the ingot 2 in the height direction, i.e., the ingot Si-face 22 side. Next, a first absorption coefficient, which is the absorption coefficient in the first product 101, and a second absorption coefficient, which is the absorption coefficient in the second product 102, are obtained. Then, the higher of the first absorption coefficient and the second absorption coefficient can be set as the upper limit of the absorption coefficient to determine the irradiation conditions of the laser beam B, i.e., the irradiation energy. In other words, the absorption coefficient obtained from the product 100 with the higher absorption coefficient, i.e., the wafer 1, can be set as the upper limit and not changed any further.
[0060] The measurement pitch for optical measurement may be uniform as shown in FIG. 12 , but can be changed as appropriate. That is, for example, different pitches may be used in the X-axis direction and the Y-axis direction. Alternatively, the measurement pitch may be finer in a region where the change in absorption coefficient is greater than in other regions, such as the region surrounded by the dashed-dotted rectangle in FIG. 21 . Specifically, such a region is, for example, the boundary between the non-facet region RN and the facet region RF. That is, the measurement pitch may be finer in such a boundary region than in other regions. The region in which the measurement pitch is finer may include the entire facet region RF. More specifically, referring to FIG. 21 , for example, the measurement pitch may be finer in a region to the right of the measurement position 40 mm than in a region to the left of the measurement position 40 mm. In other words, the measurement pitch may be finer in a predetermined region formed by the non-facet region RN and the boundary between the non-facet region RN and the facet region RF than in a region outside such a predetermined region.
[0061] (Third Embodiment) This embodiment is a partial modification of the irradiation and scanning modes of the laser beam B in the first embodiment. That is, in the first embodiment, the spacing between the leading beam B1 and the trailing beam B2 in the scanning direction Ds is N times, i.e., an integer multiple, of the irradiation pitch of the leading beam B1. However, during actual processing, the leading irradiation position PR1, which is the irradiation position by the leading beam B1, and the trailing irradiation position PR2, which is the irradiation position by the trailing beam B2, do not necessarily coincide perfectly, and errors may occur in the in-plane direction. Furthermore, the disclosure corresponding to the first embodiment irradiates the trailing beam B2 onto the irradiation mark RM formed by irradiation with the leading beam B1, and perfect coincidence of the leading irradiation position PR1 and the trailing irradiation position PR2 in the in-plane direction is not a necessary requirement. Therefore, the spacing between the leading beam B1 and the trailing beam B2 may not be an integer multiple of the irradiation pitch of the leading beam B1 (for example, (N+0.1) times, etc.). Although these matters are obviously obvious to those skilled in the art, we would like to add that these matters are within the scope of the disclosure in Japanese Patent Application No. 2023-87816 filed on May 29, 2023.
[0062] In this embodiment, as shown in FIG. 22 , the trailing beam B2 is irradiated between a pair of irradiation marks RM formed by irradiation of the leading beam B1 and arranged along the scanning direction Ds. That is, the distance between the leading beam B1 and the trailing beam B2 is a non-integer multiple of the irradiation pitch of the leading beam B1, specifically, N+δ. δ is typically 0.5 or a value close to it (i.e., approximately 0.4 to 0.6). In this embodiment, the leading beam B1 and the trailing beam B2 are irradiated so that the irradiation marks RM formed by irradiation of the leading beam B1 and the irradiation marks RM formed by irradiation of the trailing beam B2 are combined. Here, it does not matter whether the trailing beam B2 is irradiated onto the irradiation marks RM formed by the leading beam B1. Furthermore, the applied energy of the leading beam B1 and the trailing beam B2 can be set to a value larger than that in the first embodiment described above, depending on the size of the irradiation pitch, but may also be approximately the same. According to this embodiment, by irradiating the trailing beam B2 between multiple irradiation marks RM formed by the leading beam B1 at approximately the same depth, the irradiation marks RM formed by the irradiation of the leading beam B1 and the irradiation marks RM formed by the irradiation of the trailing beam B2 are combined. This can achieve the same effect as the first embodiment. Note that if the trailing beam B2 is not irradiated onto the modified layer RA formed by the leading beam B1, the influence of reflection by the cracks C as described above may be a concern. Therefore, in this case, the irradiation interval of the leading beam B1 in the scanning direction Ds can be set so that the trailing beam B2 is irradiated into the gaps between the cracks C formed by the leading beams B1 adjacently arranged along the scanning direction Ds.
[0063] (Modifications) The present disclosure is not limited to the above-described embodiment. Therefore, the above-described embodiment can be modified as appropriate. Representative modifications will be described below. In the following description of the modifications, differences from the above-described embodiment will be mainly described. Furthermore, the same reference numerals are used for parts that are identical or equivalent to each other in the above-described embodiment and the modifications. Therefore, in the following description of the modifications, the description of the above-described embodiment can be used as appropriate for components that have the same reference numerals as the above-described embodiment, unless there is a technical contradiction or special additional explanation.
[0064] The present disclosure is not limited to the specific configurations shown in the above embodiments. That is, for example, there are no particular limitations on the outer diameter or planar shape (e.g., the presence or absence of a so-called orientation flat) of the wafer 1, i.e., the ingot 2. There are also no particular limitations on the magnitude of the off-angle θ. Furthermore, in the above embodiments, the wafer C-plane 11 and the ingot C-plane 21 do not coincide with the C-plane in the strict crystallographic sense, i.e., the (0001) plane Pc. However, even in such cases, the term "C-plane" is used because it is generally accepted. However, the present disclosure is not limited to such an embodiment. That is, the wafer C-plane 11 and the ingot C-plane 21 may coincide with the C-plane in the strict crystallographic sense, i.e., the (0001) plane Pc. In other words, the off-angle θ may be 0 degrees.
[0065] In the above embodiment, the peeling layer 23 is formed on the ingot C-face 21 side by "C-face side irradiation" in which the laser beam B is irradiated onto the ingot C-face 21. However, the present disclosure is not limited to this embodiment. That is, the present disclosure is also applicable to "Si-face side irradiation" in which the laser beam B is irradiated onto the ingot Si-face 22 to form the peeling layer 23 on the ingot Si-face 22 side.
[0066] Depending on the irradiation conditions and scanning conditions of the laser beam B, the peeled surface 32 may have a surface condition that allows it to be satisfactorily ground or polished even if it is subjected to the ECMG or ECMP process as is. Therefore, the rough grinding process of the peeled surface 32 shown in Fig. 2 may be omitted. The same applies to the rough grinding of the top surface of the ingot 2 after the wafer peeling process. The same applies to the rough grinding process shown in Fig. 11.
[0067] There is no particular limitation on the number of laser beams B arranged in the scanning direction Ds, i.e., the off-angle direction Dθ, that are scanned by one laser scan. In other words, although two laser beams B, the leading beam B1 and the trailing beam B2, are arranged in the scanning direction Ds in the above embodiment, three or more laser beams may be arranged. In other words, in the first embodiment, the irradiation mark RM, i.e., the modified layer RA, may be gradually enlarged by irradiating one irradiation position PR with the laser beam B three or more times. The number of laser beams B arranged in the line feed direction Df that are scanned by one laser scan and the arrangement in the scanning direction Ds may also be changed as appropriate from the specific examples shown in the above embodiment.
[0068] 10 is an example in which a total of six laser beams B, two in the scanning direction Ds and three in the line feed direction Df, are scanned in the scanning direction Ds. Furthermore, the positions of the three laser beams B or irradiation positions PR arranged in the line feed direction Df in the scanning direction Ds are set to be offset by a predetermined amount as they move in the line feed direction Df. However, as described above, the present disclosure is not limited to this arrangement.
[0069] That is, for example, a scanning example such as that shown in FIG. 23 is also possible. In this scanning example, three groups of laser beams B, namely, a first beam group BG1, a second beam group BG2, and a third beam group BG3, are arranged in this order in the line feed direction Df. The second beam group BG2 is positioned protruding further in the scanning direction Ds than the first beam group BG1 and the third beam group BG3. That is, the first beam group BG1, the second beam group BG2, and the third beam group BG3 are arranged in a substantially V-shape. This effectively prevents the processing device configuration from becoming bulky due to the expansion of the irradiation area of the multiple laser beams B that are simultaneously scanned. Note that the first beam group BG1 to the third beam group BG3 are each a group of multiple laser beams B aligned along the scanning direction Ds, but the number of laser beams B included therein is not limited to two as shown in FIG. 23 and may be three or more. Furthermore, the number of beam groups such as the first beam group BG1 is not limited to three as shown in FIG. 23, but may be two, or may be four or more.
[0070] Adjusting the beam characteristics of the laser beam B, such as the beam shape, can further improve the processing characteristics. Specifically, for example, as shown in FIG. 24 , the laser beam B may have a beam shape that is annular, i.e., hollow, in front of the focal point BP, but is focused into a point shape at the focal point BP. Such annular laser beam B and devices that generate and irradiate such laser beam B onto a workpiece were already publicly known at the time of filing of this application (see, for example, Japanese Patent Application Laid-Open Nos. 2006-130691 and 2014-147946). Therefore, detailed descriptions of devices and methods for generating such laser beam B are omitted in this specification. FIG. 24 shows how an irradiation mark RM is formed by such an annular laser beam B. On the other hand, FIG. 25 shows how an irradiation mark RM is formed by a non-annular, i.e., solid, laser beam B.
[0071] As shown in FIG. 25 , when a solid laser beam B is used, a modified layer RA formed by the separation of SiC into Si and C due to irradiation with the laser beam B may occur at a depth different from the focal point BP. Therefore, the depth of the modified layer RA and the irradiation mark RM consisting of cracks C propagating from the modified layer RA may also be different from the focal point BP. Specifically, for example, at a position shallower than the focal point BP, the applied energy density due to irradiation with the laser beam B may be increased to a level that can generate the modified layer RA. As a result, the modified layer RA may occur at a position shallower than the focal point BP. The depth at which the modified layer RA occurs may vary due to variations in the irradiation energy of the laser beam B, variations in the refractive index of the ingot 2, variations in the optical system of the laser beam B focusing device, etc. The region where the modified layer RA may occur is shown in the figure as a modifiable range RC.
[0072] In contrast, when an annular laser beam B is used, as shown in FIG. 24, the laser beam B advances at a relatively low energy density until it reaches a depth near the focal point BP, and the energy density rises sharply at the confluence occurring at a depth near the focal point BP. Therefore, the energy application density due to irradiation of the laser beam B increases to a level sufficient to generate a modified layer RA only to a depth near the focal point BP. That is, for example, as in the case of using a solid laser beam B, it is difficult to increase the energy application density due to irradiation of the laser beam B to a level sufficient to generate a modified layer RA at a position shallower than the focal point BP. Therefore, unlike the case of using a solid laser beam B, the modifiable range RC is limited to a narrow depth range centered on the depth of the focal point BP. Therefore, the modified layer RA is stably generated at a depth near the focal point BP. This effectively suppresses the variation in the depth at which the modified layer RA is generated. In other words, it is possible to form the release layer 23 as thin as possible, and the amount of processing required for grinding and polishing after release can be effectively reduced. Therefore, according to this embodiment, it is possible to improve manufacturing efficiency compared to the conventional method.
[0073] Here, the energy distribution in the beam diameter direction of the annular laser beam B shown in Fig. 24 may be the normal Gaussian distribution shown in Fig. 26, but it is preferable to use a top-hat shape shown by the solid line in Fig. 27. Such a top-hat energy distribution can be realized by removing the base of the Gaussian distribution shown by the dashed line in the figure using an optical system or the like. Such a top-hat energy distribution makes it possible to further narrow the modifiable range RC shown in Fig. 24.
[0074] In the above-described embodiments and specific examples, the propagation direction of the crack C is inclined by the off-angle θ with respect to the in-plane direction parallel to the ingot C-face 21. However, in reality, cracks C having an inclination different from this inclination can also be generated by irradiating the laser beam B. Specifically, as shown in FIG. 28 , in addition to the first-type crack C1 inclined by the off-angle θ with respect to the in-plane direction, a second-type crack C2 having a different inclination can also be generated. Such second-type crack C2 is a crack C that is nearly horizontal along the in-plane direction. In other words, the second-type crack C2 has an inclination closer to horizontal than the first-type crack C1. Note that "horizontal" here refers to being parallel to the ingot C-face 21. The generation mode of the crack C shown in FIG. 28 can be effectively achieved by irradiating the laser beam B as described in the above-described embodiments.
[0075] It goes without saying that the elements constituting the above-described embodiments are not necessarily essential unless expressly stated as essential or clearly considered essential in principle. Furthermore, when numerical values such as the number, amount, and range of components are mentioned, the present disclosure is not limited to those specific numerical values unless expressly stated as essential or clearly limited to specific numerical values in principle. Similarly, when the shape, direction, positional relationship, etc. of components are mentioned, the present disclosure is not limited to those shapes, directions, positional relationships, etc., unless expressly stated as essential or clearly limited to specific shapes, directions, positional relationships, etc. in principle.
[0076] The modified examples are not limited to the above examples. For example, other than those exemplified above, multiple embodiments may be combined with each other as long as there is no technical contradiction. Similarly, multiple modified examples may be combined with each other as long as there is no technical contradiction.
[0077] (Viewpoints of the Present Disclosure) As is clear from the above description of the embodiment and modified examples, the above-described present disclosure can be understood from the following viewpoints, for example.
[0078] [Viewpoint 1-1] A laser processing method for irradiating a laser beam (B) onto an object (2) made of a semiconductor material, the method including modified layer formation in which a modified layer (RA) is formed at a predetermined depth from the surface by irradiating the surface (21) of the object with the laser beam that is transparent to the surface, the modified layer formation comprising: performing laser scanning in which the laser beam is irradiated onto the surface while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) on the surface that is perpendicular to the first direction and along the surface, to form a plurality of irradiation locus lines (Ls) along the second direction, the irradiation locus lines being linear irradiation marks of the laser beam along the first direction; and forming the irradiation marks at each of the plurality of irradiation positions by intermittently irradiating the laser beam while moving the laser beam relative to the object along the first direction in one laser scan, and irradiating the laser beam with the laser beam at a predetermined depth from the surface, the modified layer formation comprising: performing laser scanning in which the laser beam is irradiated onto the surface while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) along the surface that is perpendicular to the first direction, the laser beam [Aspect 1-2] The laser processing method according to Aspect 1-1, wherein the laser scanning is performed between the irradiation locus lines adjacent to each other in the second direction. [Aspect 1-3] The laser processing method according to Aspect 1-1 or 1-2, wherein the object to be processed is single crystal SiC having a c-axis (Lc) and a C-plane (Pc) perpendicular to each other, the c-axis is inclined with respect to a central axis (L) perpendicular to the surface at an off-angle angle (θ) exceeding 0 degrees in an off-angle direction (Dθ), and the first direction is parallel to the off-angle direction. [Aspect 1-4] The laser processing method according to any one of Aspects 1-1 to 1-3, wherein the direction of relative movement is opposite between one laser scanning and the next laser scanning. [Aspect 1-5] The laser processing method according to any one of Aspects 1-1 to 1-4, wherein a plurality of the laser beams having different irradiation positions in at least the second direction are irradiated onto the surface in one laser scanning, thereby forming a plurality of irradiation locus lines.[Aspect 1-6] The laser processing method according to any one of Aspects 1-1 to 1-5, wherein the irradiation conditions of the laser beam are controlled based on a measurement result of the transmittance of the laser beam in the semiconductor material. [Aspect 1-7] The laser processing method according to Aspect 1-6, wherein a change trend in the depth direction of the absorption coefficient of the laser beam in the semiconductor material is obtained based on the measurement result, and the irradiation conditions are determined based on the obtained change trend. [Aspect 1-8] The laser processing method according to Aspect 1-6 or 1-7, wherein the measurement pitch of the transmittance is narrower in a boundary portion between a facet region (RF) and a non-facet region (RN) than in other portions. [Aspect 1-9] The laser processing method according to any one of Aspects 1-1 to 1-8, wherein the object to be processed is a single crystal SiC ingot. [Aspect 1-10] The laser processing method according to any one of Aspects 1-1 to 1-9, wherein the maximum width of the modified layer in the second direction is DY, the maximum spacing that is the spacing between adjacent modified layers at positions in the first direction that correspond to the maximum width of the modified layer is DP, the average value of the maximum widths is DYave, and the average value of the maximum spacings is DPave, wherein the laser scanning is performed so that DYave / DPave≦5. [Aspect 1-11] The laser processing method according to Aspect 1-10, wherein the laser scanning is performed so that DYave / DPave≦2. [Aspect 1-12] The laser processing method according to Aspect 1-11, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.3. [Aspect 1-13] The laser processing method according to any one of Aspects 1-1 to 1-12, wherein a single laser scan moves two laser beams, a leading beam (B1) and a trailing beam (B2), which are different in position in the first direction, relative to the object to be processed. [Aspect 1-14] The laser processing method according to Aspect 1-13, wherein the leading beam and the trailing beam can be irradiated simultaneously.[Aspect 1-15] The laser processing method according to any one of Aspects 1-1 to 1-14, wherein the irradiation marks are formed by modified areas (RA) that are generated by modification of the semiconductor material by irradiation with the laser beam, and cracks (C) that are generated starting from the modified areas, and the cracks include first-type cracks that have progressed in a direction inclined by an off-angle (θ) relative to the surface, and second-type cracks that are closer to the surface in inclination than the first-type cracks.
[0079] [Viewpoint 2-1] A wafer manufacturing method for obtaining a wafer (1) from an ingot (2), comprising: forming a peeling layer (23) from a surface (21) on one end side in a height direction of the ingot by irradiating the surface with a laser beam (B) having transparency, thereby forming a peeling layer (23) from the surface to a depth corresponding to a thickness of the wafer; the peeling layer formation includes: performing laser scanning, in which the irradiation position (PR) of the laser beam on the surface is moved along a first direction (Ds) along the surface, while irradiating the surface with the laser beam, multiple times while changing the position in a second direction (Df) on the surface that is perpendicular to the first direction and along the surface; and forming multiple irradiation locus lines (Ls) consisting of linear irradiation marks (RM) of the laser beam along the first direction, along the second direction, to form the peeling layer; A wafer manufacturing method, in which, in a single laser scan, the laser beam is intermittently irradiated while moving relatively to the ingot along the first direction to form the irradiation mark at each of a plurality of the irradiation positions, and the subsequent laser beam is irradiated onto the irradiation mark formed by irradiation of the preceding laser beam. [Aspect 2-2] The wafer manufacturing method according to Aspect 2-1, in which the laser scanning is performed between adjacent irradiation trajectories in the second direction. [Aspect 2-3] The wafer manufacturing method according to Aspect 2-1 or 2-2, in which the ingot is a single crystal SiC ingot having a c-axis (Lc) and a C-plane (Pc) that are orthogonal to each other, the c-axis is tilted at an off-angle angle (θ) exceeding 0 degrees with respect to a central axis (L) that is orthogonal to the surface in an off-angle direction (Dθ), and the first direction is parallel to the off-angle direction. [Aspect 2-4] The wafer manufacturing method according to any one of Aspects 2-1 to 2-3, wherein the direction of the relative movement is opposite between one laser scan and the next laser scan. [Aspect 2-5] The wafer manufacturing method according to any one of Aspects 2-1 to 2-4, wherein a plurality of the laser beams having different irradiation positions in at least the second direction are irradiated onto the surface in one laser scan, thereby forming a plurality of the irradiation locus lines.[Aspect 2-6] The wafer manufacturing method according to any one of Aspects 2-1 to 2-5, controlling the irradiation conditions of the laser beam based on measurement results of the transmittance of the laser beam in the material constituting the ingot. [Aspect 2-7] The wafer manufacturing method according to Aspect 2-6, obtaining a change trend in the height direction of the absorption coefficient of the laser beam in the material based on the measurement results, and determining the irradiation conditions based on the obtained change trend. [Aspect 2-8] The wafer manufacturing method according to Aspect 2-6 or 2-7, narrowing the measurement pitch of the transmittance in a boundary portion between a facet region (RF) and a non-facet region (RN) compared to other portions. [Aspect 2-9] The wafer manufacturing method according to any one of Aspects 2-1 to 2-8, wherein the laser scanning is performed so that DYave / DPave≦5, where DY is the maximum width in the second direction of a modified layer (RA) formed inside the ingot by irradiation with the laser beam, DP is the maximum spacing between adjacent modified layers in the first direction at a position corresponding to the maximum width of the modified layer, DYave is the average value of the maximum widths, and DPave is the average value of the maximum spacings. [Aspect 2-10] The wafer manufacturing method according to Aspect 2-9, wherein the laser scanning is performed so that DYave / DPave≦2. [Aspect 2-11] The wafer manufacturing method according to Aspect 2-10, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.3. [Aspect 2-12] The wafer manufacturing method according to any one of Aspects 2-1 to 2-11, wherein a single laser scan moves two laser beams, a leading beam (B1) and a trailing beam (B2), which are different in position in the first direction, relative to the object to be processed. [Aspect 2-13] The wafer manufacturing method according to Aspect 2-12, wherein the leading beam and the trailing beam can be irradiated simultaneously.[Aspect 2-14] The wafer manufacturing method according to any one of Aspects 2-1 to 2-13, wherein the irradiation marks are formed by modified areas (RA) that are generated by modification of the semiconductor material by irradiation with the laser beam, and cracks (C) that are generated starting from the modified areas, and the cracks include first-type cracks that propagate in a direction inclined by an off-angle (θ) relative to the surface, and second-type cracks that are inclined closer to the surface than the first-type cracks.
[0080] [Aspect 3-1] A laser processing method for irradiating a laser beam (B) onto a processing object (2) made of a semiconductor material, comprising modified layer formation, in which the laser beam, which is transparent to a surface (21) of the processing object, is irradiated to form a modified layer (RA) at a predetermined depth from the surface, wherein the modified layer formation is performed by performing laser scanning, in which the laser beam is irradiated onto the surface while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) on the surface that is perpendicular to the first direction and along the surface, to form a plurality of irradiation locus lines (Ls) along the second direction, each consisting of a linear irradiation mark of the laser beam along the first direction; A laser processing method in which the laser scanning is performed once to form the irradiation marks at each of a plurality of irradiation positions by intermittently irradiating the laser beam while moving the laser beam relatively to the workpiece along the first direction, and a trailing beam (B2) that is the trailing laser beam is irradiated between a pair of irradiation marks that are formed by irradiating a leading beam (B1) that is the leading laser beam and that are arranged along the first direction. [Aspect 3-2] The laser processing method according to Aspect 3-1, in which the laser scanning is performed once to irradiate the leading beam and the trailing beam so that the irradiation mark formed by irradiating the leading beam and the irradiation mark formed by irradiating the trailing beam are combined. [Aspect 3-3] The laser processing method according to Aspect 3-1 or 3-2, in which the laser scanning is performed between the irradiation locus lines that are adjacent in the second direction. [Aspect 3-4] The laser processing method according to any one of Aspects 3-1 to 3-3, wherein the object to be processed is single crystal SiC having a c-axis (Lc) and a C-plane (Pc) that are orthogonal to each other, the c-axis is provided with a central axis (L) that is orthogonal to the surface tilted in an off-angle direction (Dθ) by an off-angle (θ) that exceeds 0 degrees, and the first direction is parallel to the off-angle direction. [Aspect 3-5] The laser processing method according to any one of Aspects 3-1 to 3-4, wherein the direction of the relative movement is opposite between one laser scan and the next laser scan.[Aspect 3-6] The laser processing method according to any one of Aspects 3-1 to 3-5, wherein a plurality of the preceding beams and the following beams having different irradiation positions in the second direction are irradiated onto the surface in a single laser scan, thereby forming a plurality of irradiation trajectories. [Aspect 3-7] The laser processing method according to any one of Aspects 3-1 to 3-6, wherein the irradiation conditions of the laser beam are controlled based on a measurement result of the transmittance of the laser beam in the semiconductor material. [Aspect 3-8] The laser processing method according to Aspect 3-7, wherein a change trend in the depth direction of the absorption coefficient of the laser beam in the semiconductor material is obtained based on the measurement result, and the irradiation conditions are determined based on the obtained change trend. [Aspect 3-9] The laser processing method according to Aspect 3-7 or 3-8, wherein the measurement pitch of the transmittance is narrower in a boundary portion between a facet region (RF) and a non-facet region (RN) than in other portions. [Aspect 3-10] The laser processing method according to any one of Aspects 3-1 to 3-9, wherein the object to be processed is a single crystal SiC ingot. [Aspect 3-11] The laser processing method according to any one of Aspects 3-1 to 3-10, wherein the laser scanning is performed so that DYave / DPave≦5, where DY is the maximum width of the modified layer in the second direction, DP is the maximum spacing between adjacent modified layers at positions corresponding to the maximum widths of the modified layers in the first direction, DYave is the average value of the maximum widths, and DPave is the average value of the maximum spacings. [Aspect 3-12] The laser processing method according to Aspect 3-11, wherein the laser scanning is performed so that DYave / DPave≦2. [Aspect 3-13] The laser processing method according to Aspect 3-12, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.3. [Aspect 3-14] The laser processing method according to any one of Aspects 3-1 to 3-13, wherein one laser scan moves the leading beam and the trailing beam, which are two laser beams that are at different positions in the first direction, relative to the object to be processed.[Aspect 3-15] The laser processing method according to Aspect 3-14, wherein the preceding beam and the following beam can be irradiated simultaneously. [Aspect 3-16] The laser processing method according to any one of Aspects 3-1 to 3-15, wherein the irradiation marks are formed by a modified area (RA) generated by modification of the semiconductor material by irradiation with the laser beam and cracks (C) that occur from such modified area as a starting point, and the cracks include first type cracks that propagate in a direction inclined by an off angle (θ) with respect to the surface, and second type cracks that are inclined closer to the surface than the first type cracks.
[0081] [Viewpoint 4-1] A wafer manufacturing method for obtaining a wafer (1) from an ingot (2), comprising: forming a peeling layer (23) from a surface (21) on one end side in a height direction of the ingot by irradiating the surface with a laser beam (B) having transparency, thereby forming a peeling layer (23) from the surface to a depth corresponding to a thickness of the wafer; the peeling layer formation includes: performing laser scanning, in which the laser beam is irradiated onto the surface while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) on the surface that is perpendicular to the first direction and along the surface, to form a plurality of irradiation locus lines (Ls) along the second direction, each consisting of a linear irradiation mark (RM) of the laser beam along the first direction, thereby forming the peeling layer; A wafer manufacturing method, in which a single laser scan forms the irradiation marks at each of a plurality of the irradiation positions by intermittently irradiating the laser beam while moving the laser beam relatively to the ingot along the first direction, and a trailing beam (B2) that is the trailing laser beam is irradiated between a pair of irradiation marks formed by irradiation of a leading beam (B1) that is the leading laser beam and arranged along the first direction. [Aspect 4-2] The wafer manufacturing method according to Aspect 4-1, in which a single laser scan irradiates the leading beam and the trailing beam so that the irradiation mark formed by irradiation of the leading beam and the irradiation mark formed by irradiation of the trailing beam are combined. [Aspect 4-3] The wafer manufacturing method according to Aspect 4-1 or 4-2, in which the laser scanning is performed between the irradiation locus lines that are adjacent in the second direction. Aspect 4-4 The wafer manufacturing method according to any one of Aspects 4-1 to 4-3, wherein the ingot is a single crystal SiC ingot having a c-axis (Lc) and a C-plane (Pc) that are orthogonal to each other, the c-axis is inclined at an off-angle (θ) exceeding 0 degrees in an off-angle direction (Dθ) relative to a central axis (L) that is orthogonal to the surface, and the first direction is parallel to the off-angle direction.[Aspect 4-5] The wafer manufacturing method according to any one of Aspects 4-1 to 4-4, wherein the direction of relative movement is opposite between one laser scan and the next laser scan. [Aspect 4-6] The wafer manufacturing method according to any one of Aspects 4-1 to 4-5, wherein a plurality of the preceding beams and the following beams, which have different irradiation positions in the second direction, are irradiated onto the surface in one laser scan, thereby forming a plurality of irradiation trajectories. [Aspect 4-7] The wafer manufacturing method according to any one of Aspects 4-1 to 4-6, wherein the irradiation conditions of the laser beam are controlled based on a measurement result of the transmittance of the laser beam in a material constituting the ingot. [Aspect 4-8] The wafer manufacturing method according to Aspect 4-7, wherein a change trend in the height direction of the absorption coefficient of the laser beam in the material is obtained based on the measurement result, and the irradiation conditions are determined based on the obtained change trend. [Aspect 4-9] The wafer manufacturing method according to Aspect 4-7 or 4-8, wherein the transmittance measurement pitch is narrower in a boundary portion between a facet region (RF) and a non-facet region (RN) than in other portions. [Aspect 4-10] The wafer manufacturing method according to any one of Aspects 4-1 to 4-9, wherein the laser scanning is performed so that DYave / DPave≦5, where DY is the maximum width in the second direction of a modified layer (RA) formed inside the ingot by irradiation with the laser beam, DP is the maximum spacing between adjacent modified layers in the first direction at positions corresponding to the maximum widths of the modified layers, and DYave is the average value of the maximum widths. [Aspect 4-11] The wafer manufacturing method according to Aspect 4-10, wherein the laser scanning is performed so that DYave / DPave≦2. [Aspect 4-12] The wafer manufacturing method according to Aspect 4-11, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.3.[Aspect 4-13] The wafer manufacturing method according to any one of Aspects 4-1 to 4-12, wherein one laser scan moves the two laser beams, the leading beam and the trailing beam, which are at different positions in the first direction, relative to the object to be processed. [Aspect 4-14] The wafer manufacturing method according to Aspect 4-13, wherein the leading beam and the trailing beam can be irradiated simultaneously. [Aspect 4-15] The wafer manufacturing method according to any one of Aspects 4-1 to 4-14, wherein the irradiation marks are formed by modified regions (RA) generated by modification of the semiconductor material by irradiation with the laser beam and cracks (C) generated with the modified regions as origins, and the cracks include first type cracks that propagate in a direction inclined by an off angle (θ) with respect to the surface, and second type cracks that are inclined closer to the surface than the first type cracks.
[0082] [Aspect 5-1] A laser processing method for irradiating a laser beam (B) onto a processing object (2) made of a semiconductor material, comprising modified layer formation, in which a modified layer (RA) is formed at a predetermined depth from a surface (21) of the processing object by irradiating the laser beam, which is transparent to the surface (21) of the processing object, wherein the modified layer formation is performed by performing laser scanning, in which the laser beam is irradiated onto the surface while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) on the surface orthogonal to the first direction and along the surface, to form a plurality of irradiation locus lines (Ls) along the second direction, each consisting of a linear irradiation mark of the laser beam along the first direction; A laser processing method in which a single laser scan forms the irradiation marks at each of a plurality of the irradiation positions by intermittently irradiating the laser beam while moving the laser beam relatively along the first direction with respect to the object to be processed, and by irradiating a trailing beam (B2) that is the trailing laser beam between a pair of irradiation marks that are formed by irradiating a leading beam (B1) that is the leading laser beam and arranged along the first direction, the irradiation marks formed by irradiating the leading beam and the irradiation marks formed by irradiating the trailing beam are combined. [Aspect 5-2] The laser processing method according to Aspect 5-1, in which the laser scanning is performed between the irradiation locus lines that are adjacent in the second direction. [Aspect 5-3] The laser processing method according to Aspect 5-1 or 5-2, wherein the object to be processed is single crystal SiC having a c-axis (Lc) and a C-plane (Pc) that are orthogonal to each other, the c-axis is provided with a central axis (L) that is orthogonal to the surface tilted in an off-angle direction (Dθ) by an off-angle (θ) that exceeds 0 degrees, and the first direction is parallel to the off-angle direction. [Aspect 5-4] The laser processing method according to any one of Aspects 5-1 to 5-3, wherein the direction of the relative movement is opposite between one laser scan and the next laser scan.[Aspect 5-5] The laser processing method according to any one of Aspects 5-1 to 5-4, wherein a plurality of the preceding beams and the following beams having different irradiation positions in the second direction are irradiated onto the surface in a single laser scan, thereby forming a plurality of irradiation trajectories. [Aspect 5-6] The laser processing method according to any one of Aspects 5-1 to 5-5, wherein the irradiation conditions of the laser beam are controlled based on a measurement result of the transmittance of the laser beam in the semiconductor material. [Aspect 5-7] The laser processing method according to Aspect 5-6, wherein a change trend in the depth direction of the absorption coefficient of the laser beam in the semiconductor material is obtained based on the measurement result, and the irradiation conditions are determined based on the obtained change trend. [Aspect 5-8] The laser processing method according to Aspect 5-6 or 5-7, wherein the measurement pitch of the transmittance is narrower in a boundary portion between a facet region (RF) and a non-facet region (RN) than in other portions. [Aspect 5-9] The laser processing method according to any one of Aspects 5-1 to 5-8, wherein the processing object is a single crystal SiC ingot. [Aspect 5-10] The laser processing method according to any one of Aspects 5-1 to 5-9, wherein the laser scanning is performed so that DYave / DPave≦5, where DY is the maximum width of the modified layer in the second direction, DP is the maximum spacing between adjacent modified layers at positions corresponding to the maximum width of the modified layer in the first direction, DYave is the average value of the maximum widths, and DPave is the average value of the maximum spacings. [Aspect 5-11] The laser processing method according to Aspect 5-10, wherein the laser scanning is performed so that DYave / DPave≦2. [Aspect 5-12] The laser processing method according to Aspect 5-11, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.3. [Aspect 5-13] The laser processing method according to any one of Aspects 5-1 to 5-12, wherein one laser scan moves the leading beam and the trailing beam, which are two laser beams that are at different positions in the first direction, relative to the object to be processed.[Aspect 5-14] The laser processing method according to Aspect 5-13, wherein the preceding beam and the following beam can be irradiated simultaneously. [Aspect 5-15] The laser processing method according to any one of Aspects 5-1 to 5-14, wherein the irradiation marks are formed by a modified area (RA) generated by modification of the semiconductor material by irradiation with the laser beam and cracks (C) generated from the modified area, and the cracks include first type cracks that propagate in a direction inclined by an off angle (θ) with respect to the surface, and second type cracks that are inclined closer to the surface than the first type cracks.
[0083] [Viewpoint 6-1] A wafer manufacturing method for obtaining a wafer (1) from an ingot (2), comprising: forming a peeling layer (23) from a surface (21) on one end side in a height direction of the ingot by irradiating the surface with a laser beam (B) having transparency, thereby forming a peeling layer (23) from the surface to a depth corresponding to a thickness of the wafer; the peeling layer formation includes: performing laser scanning, in which the laser beam is irradiated onto the surface while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) on the surface that is perpendicular to the first direction and along the surface, to form a plurality of irradiation locus lines (Ls) along the second direction, each consisting of a linear irradiation mark (RM) of the laser beam along the first direction, thereby forming the peeling layer; a laser beam (B1) that is a leading laser beam and a trailing beam (B2) that is a trailing laser beam are irradiated between a pair of irradiation marks that are formed by irradiation of a leading beam (B1) that is a leading laser beam and are arranged along the first direction, thereby combining the irradiation marks formed by irradiation of the leading beam and the irradiation marks formed by irradiation of the trailing beam. [Aspect 6-2] The wafer manufacturing method according to Aspect 6-1, wherein the laser scanning is performed between the irradiation locus lines that are adjacent in the second direction. [Aspect 6-3] The wafer manufacturing method according to Aspect 6-1 or 6-2, wherein the ingot is a single crystal SiC ingot having a c-axis (Lc) and a C-plane (Pc) that are orthogonal to each other, the c-axis is tilted at an off-angle (θ) exceeding 0 degrees in an off-angle direction (Dθ) with respect to a central axis (L) that is orthogonal to the surface, and the first direction is parallel to the off-angle direction. [Aspect 6-4] The wafer manufacturing method according to any one of Aspects 6-1 to 6-3, wherein the direction of the relative movement is opposite between one laser scan and a next laser scan.[Aspect 6-5] The wafer manufacturing method according to any one of Aspects 6-1 to 6-4, wherein a plurality of the preceding beams and the following beams having different irradiation positions in the second direction are irradiated onto the surface in a single laser scan, thereby forming a plurality of irradiation trajectories. [Aspect 6-6] The wafer manufacturing method according to any one of Aspects 6-1 to 6-5, wherein the irradiation conditions of the laser beam are controlled based on a measurement result of the transmittance of the laser beam in the material constituting the ingot. [Aspect 6-7] The wafer manufacturing method according to Aspect 6-6, wherein a change trend in the height direction of the absorption coefficient of the laser beam in the material is obtained based on the measurement result, and the irradiation conditions are determined based on the obtained change trend. [Aspect 6-8] The wafer manufacturing method according to Aspect 6-6 or 6-7, wherein the measurement pitch of the transmittance is narrower in a boundary portion between a facet region (RF) and a non-facet region (RN) than in other portions. [Aspect 6-9] The wafer manufacturing method according to any one of Aspects 6-1 to 6-8, wherein the laser scanning is performed so that DYave / DPave≦5, where DY is the maximum width in the second direction of a modified layer (RA) formed inside the ingot by irradiation with the laser beam, DP is the maximum spacing between adjacent modified layers in the first direction at a position corresponding to the maximum width of the modified layer, DYave is the average value of the maximum widths, and DPave is the average value of the maximum spacings. [Aspect 6-10] The wafer manufacturing method according to Aspect 6-9, wherein the laser scanning is performed so that DYave / DPave≦2. [Aspect 6-11] The wafer manufacturing method according to Aspect 6-10, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.3. [Aspect 6-12] The wafer manufacturing method according to any one of Aspects 6-1 to 6-11, wherein a single laser scan moves the leading beam and the trailing beam, which are two laser beams at different positions in the first direction, relative to the ingot. [Aspect 6-13] The wafer manufacturing method according to Aspect 6-12, wherein the leading beam and the trailing beam can be irradiated simultaneously.[Aspect 6-14] The wafer manufacturing method according to any one of Aspects 6-1 to 6-13, wherein the irradiation marks are formed by modified areas (RA) that are generated by modification of the semiconductor material by irradiation with the laser beam and cracks (C) that are generated from the modified areas, and the cracks include first-type cracks that propagate in a direction inclined by an off-angle (θ) relative to the surface, and second-type cracks that are inclined closer to the surface than the first-type cracks.
Claims
1. A laser processing method for irradiating a laser beam (B) onto a processing object (2) made of a semiconductor material, the method including modified layer formation in which the laser beam, which is transparent to a surface (21) of the processing object, is irradiated to form a modified layer (RA) at a predetermined depth from the surface, the modified layer formation comprising: performing a laser scan in which the laser beam is irradiated onto the surface while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) perpendicular to the first direction on the surface and along the surface, thereby forming a plurality of irradiation locus lines (Ls) consisting of linear irradiation marks of the laser beam along the first direction, and irradiating the laser beam intermittently while moving the laser beam relative to the processing object along the first direction in one laser scan, thereby forming the irradiation marks at each of the plurality of irradiation positions, and irradiating the laser beam to the irradiation marks formed by irradiation of the preceding laser beam.
2. The laser processing method according to claim 1, wherein the laser scanning is performed between adjacent irradiation trajectory lines in the second direction.
3. The laser processing method according to claim 1, wherein the object to be processed is single crystal SiC having a c-axis (Lc) and a C-plane (Pc) perpendicular to each other, the c-axis is arranged with a central axis (L) perpendicular to the surface tilted at an off angle (θ) exceeding 0 degrees in an off-angle direction (Dθ), and the first direction is parallel to the off-angle direction.
4. The laser processing method according to claim 2, wherein the direction of the relative movement is reversed between one laser scan and the next laser scan.
5. The laser processing method according to claim 1, wherein a plurality of the irradiation trajectories are formed by irradiating the surface with a plurality of the laser beams having different irradiation positions in at least the second direction in a single laser scan.
6. The laser processing method according to claim 1, further comprising controlling irradiation conditions of the laser beam based on a measurement result of a transmittance of the laser beam through the semiconductor material.
7. The laser processing method according to claim 6, further comprising the steps of: obtaining a change trend in the absorption coefficient of the laser beam in the semiconductor material in the depth direction based on the measurement results; and determining the irradiation conditions based on the obtained change trend.
8. The laser processing method according to claim 6, wherein the measurement pitch of the transmittance is narrower in a boundary portion between the facet region (RF) and the non-facet region (RN) than in other portions.
9. The laser processing method according to claim 1, wherein the object to be processed is a single crystal SiC ingot.
10. A wafer manufacturing method for obtaining a wafer (1) from an ingot (2), comprising forming a peeling layer (23) from a surface (21) at one end side in a height direction of the ingot with a transparent laser beam (B), to form a peeling layer (23) from the surface to a depth corresponding to a thickness of the wafer, the peeling layer formation being performed by moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, and performing laser scanning in which the laser beam is irradiated onto the surface multiple times while changing the position in a second direction (Df) perpendicular to the first direction on the surface and along the surface, to form multiple irradiation trajectories (Ls) consisting of linear irradiation marks (RM) of the laser beam along the first direction along the second direction, thereby forming the peeling layer; a laser beam is intermittently irradiated onto the ingot while moving the laser beam relatively to the ingot along the first direction in a single laser scan, thereby forming the irradiation mark at each of a plurality of irradiation positions, and a subsequent laser beam is irradiated onto the irradiation mark formed by irradiation of a preceding laser beam.
11. The wafer manufacturing method according to claim 10, wherein the laser scanning is performed between the irradiation trajectory lines adjacent to each other in the second direction.
12. A wafer manufacturing method as described in claim 10, wherein the ingot is a single crystal SiC ingot having a c-axis (Lc) and a C-plane (Pc) perpendicular to each other, the c-axis is arranged with a central axis (L) perpendicular to the surface tilted at an off angle (θ) exceeding 0 degrees in an off-angle direction (Dθ), and the first direction is parallel to the off-angle direction.
13. The wafer manufacturing method according to claim 11, wherein the direction of the relative movement is reversed between one laser scan and the next laser scan.
14. The wafer manufacturing method according to claim 10, wherein a plurality of the irradiation trajectories are formed by irradiating the surface with a plurality of the laser beams having different irradiation positions in at least the second direction in a single laser scan.
15. The wafer manufacturing method according to claim 10, further comprising controlling irradiation conditions of the laser beam based on a measurement result of a transmittance of the laser beam through a material constituting the ingot.
16. The wafer manufacturing method according to claim 15, further comprising: obtaining a trend of change in the absorption coefficient of the laser beam in the material in the height direction based on the measurement results; and determining the irradiation conditions based on the obtained trend of change.
17. A wafer manufacturing method according to claim 15, further comprising the step of narrowing the measurement pitch of the transmittance in a boundary portion between a facet region (RF) and a non-facet region (RN) compared to other portions.
18. A laser processing method according to claim 1, wherein the laser scanning is performed so that DYave / DPave≦5, where DY is the maximum width of the modified layer in the second direction, DP is the maximum interval between adjacent modified layers at a position in the first direction corresponding to the maximum width of the modified layer, DYave is the average value of the maximum widths, and DPave is the average value of the maximum intervals.
19. The laser processing method according to claim 18, wherein the laser scanning is performed so that DYave / DPave≦2.
20. The laser processing method according to claim 19, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.
3.
21. A wafer manufacturing method as described in claim 10, wherein the laser scanning is performed so that DYave / DPave≦5, where DY is the maximum width in the second direction of a modified layer (RA) formed inside the ingot by irradiation with the laser beam, DP is the maximum interval between adjacent modified layers in the first direction at a position corresponding to the maximum width of the modified layer, DYave is the average value of the maximum width, and DPave is the average value of the maximum intervals.
22. The wafer manufacturing method according to claim 21, wherein the laser scanning is performed so that DYave / DPave≦2.
23. The wafer manufacturing method according to claim 22, wherein the laser scanning is performed so that DYave / DPave=0.7 to 1.
3.
24. A laser processing method for irradiating a laser beam (B) onto a processing object (2) made of a semiconductor material, the method including forming a modified layer (RA) at a predetermined depth from a surface (21) of the processing object by irradiating the surface with the laser beam having transparency, the modified layer formation includes performing laser scanning for irradiating the surface with the laser beam while moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, while changing the position in a second direction (Df) perpendicular to the first direction on the surface and along the surface, to form a plurality of irradiation trajectories (Ls) along the second direction, the irradiation trajectories being made of linear irradiation marks of the laser beam along the first direction, A laser processing method in which the laser scanning once is performed to form the irradiation marks at each of a plurality of irradiation positions by intermittently irradiating the laser beam while moving the laser beam relatively to the workpiece along the first direction, and a trailing beam (B2) which is the trailing laser beam is irradiated between a pair of the irradiation marks which are formed by irradiating a leading beam (B1) which is the preceding laser beam and are arranged along the first direction.
25. The laser processing method according to claim 24, wherein each laser scan irradiates the leading beam and the trailing beam so that the irradiation mark formed by irradiation of the leading beam and the irradiation mark formed by irradiation of the trailing beam are combined.
26. The laser processing method according to claim 24, wherein a single laser scan moves the leading beam and the trailing beam, which are two laser beams having different positions in the first direction, relative to the object to be processed.
27. The laser processing method according to claim 26, wherein the leading beam and the trailing beam can be irradiated simultaneously.
28. The laser processing method according to claim 24, wherein a plurality of the irradiation trajectories are formed by irradiating the surface with a plurality of the preceding beams and the following beams having different irradiation positions in the second direction in a single laser scan.
29. A laser processing method as described in claim 1 or 24, wherein the irradiation marks are formed by a modified area (RA) caused by modification of the semiconductor material by irradiation with the laser beam and cracks (C) generated from the modified area, and the cracks include a first type crack that propagates in a direction inclined by an off angle (θ) relative to the surface, and a second type crack that is inclined closer to the surface than the first type crack.
30. A wafer manufacturing method for obtaining a wafer (1) from an ingot (2), comprising forming a peeling layer (23) from a surface (21) at one end side in a height direction of the ingot with a transparent laser beam (B), to form a peeling layer (23) from the surface to a depth corresponding to a thickness of the wafer, the peeling layer formation being performed by moving an irradiation position (PR) of the laser beam on the surface along a first direction (Ds) along the surface, and performing laser scanning in which the laser beam is irradiated onto the surface multiple times while changing the position in a second direction (Df) on the surface perpendicular to the first direction and along the surface, to form multiple irradiation trajectories (Ls) consisting of linear irradiation marks (RM) of the laser beam along the first direction along the second direction, thereby forming the peeling layer; A wafer manufacturing method in which the laser scan is performed once to form the irradiation marks at each of a plurality of irradiation positions by intermittently irradiating the laser beam while moving the laser beam relatively to the ingot along the first direction, and a trailing beam (B2) which is the trailing laser beam is irradiated between a pair of the irradiation marks which are formed by irradiation of a leading beam (B1) which is the preceding laser beam and are arranged along the first direction.
31. A wafer manufacturing method as described in claim 30, wherein a single laser scan irradiates the leading beam and the trailing beam so that the irradiation mark formed by irradiation of the leading beam and the irradiation mark formed by irradiation of the trailing beam are combined.
32. The wafer manufacturing method according to claim 30, wherein one laser scan moves the leading beam and the trailing beam, which are two laser beams having different positions in the first direction, relative to the ingot.
33. The wafer manufacturing method according to claim 32, wherein the preceding beam and the trailing beam can be irradiated simultaneously.
34. The wafer manufacturing method according to claim 30, wherein a plurality of the irradiation trajectories are formed by irradiating the surface with a plurality of the preceding beams and the following beams having different irradiation positions in the second direction in a single laser scan.
35. A wafer manufacturing method as described in claim 10 or 30, wherein the irradiation marks are formed by a modified area (RA) caused by modification of the semiconductor material by irradiation with the laser beam and cracks (C) generated from the modified area, and the cracks include a first type crack (C1) that propagates in a direction inclined by an off angle (θ) relative to the surface, and a second type crack (C2) that is inclined closer to the surface than the first type crack.
Citation Information
Patent Citations
Method and apparatus for dividing and cutting fragile material
JP2006130691A
Laser machining device and laser machining method
JP2014147946A
Generation method of wafer
JP2016111143A
Supercharging device
JP2023087816A
Wafer production method
JP6482389B2