Heat-insulating material

The heat insulating material combines a porous structure with infrared shielding and organic hollow particles to effectively suppress heat transfer across various modes, achieving superior thermal insulation and flexibility at high temperatures.

WO2024247724A1PCT designated stage expired Publication Date: 2024-12-05SUMITOMO RIKO CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/017908
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-15
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing heat insulating materials fail to provide sufficient flexibility and resilience at high temperatures, and they often compromise on heat insulation properties due to the limitations of hollow silica particles and hollow latex particles, which either lack flexibility or have poor thermal insulation at elevated temperatures.

Method used

A heat insulating material comprising a porous structure with infrared shielding particles and organic hollow particles, where the infrared shielding particles are 10-30% by mass and organic hollow particles are 5-30% by mass, allowing for effective suppression of conduction, convection, and radiation heat transfer, while maintaining flexibility and resilience.

Benefits of technology

The material achieves high heat insulation properties at both room temperature and high temperatures (up to 500°C) with enhanced flexibility and resilience, preventing heat transfer paths and maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

This heat-insulating material comprises: a porous structure in which a plurality of particles are connected to form a skeleton, and which has pores in the skeleton; infrared ray shielding particles; and organic hollow particles. When the mass of the heat-insulating material is expressed as 100 mass%, the content of the infrared ray shielding particles in the heat-insulating material is 10-30 mass%. When the mass of the heat-insulating material is expressed as 100 mass%, the content of the organic hollow particles is 5-30 mass%. The heat-insulating material has high heat insulating properties even at high temperatures, and has excellent flexibility and restorability with respect to compression.
Need to check novelty before this filing date? Find Prior Art

Description

insulation

[0001] The present disclosure relates to a thermal insulation material using a porous structure such as an aerogel.

[0002] Various insulating materials have traditionally been used in automotive components, residential building materials, industrial equipment, and the like to control heat flow. Silica aerogel, which has low thermal conductivity, is a well-known insulating material. For example, in battery packs installed in hybrid vehicles and electric vehicles, insulating materials are placed between adjacent battery cells. These insulating materials are required to have high insulating properties, particularly at high temperatures, so as to suppress heat transfer and prevent thermal runaway when the battery cells abnormally generate heat. In addition, in battery packs, a battery module formed by stacking multiple battery cells is housed in a housing while being fixed on both sides in the stacking direction by fastening members. Battery cells expand and contract with charging and discharging. Therefore, it is desirable for insulating materials placed between battery cells to be able to deform in response to external pressure and the expansion and contraction of the battery cells, thereby maintaining their insulating properties.

[0003] For example, Patent Document 1 describes an aerogel composite containing an aerogel component and hollow silica particles as an aerogel composite having heat insulating properties and flexibility. Patent Document 2 describes a product containing nanoporous particles and hollow latex particles, in which the hollow latex particles are directly bonded to each other to form a continuous matrix, and the nanoporous particles are dispersed in the continuous matrix of the hollow latex particles.

[0004] International Publication No. 2017 / 038646 Special Publication No. 2013-543036

[0005] According to the aerogel composite described in Patent Document 1, flexibility is improved by adding hollow silica particles to the aerogel component. However, the hollow silica particles have a hollow structure but are made of a hard inorganic material. Therefore, the resulting flexibility is insufficient. Furthermore, Patent Document 1 merely provides flexibility for the purpose of improving the handleability of the aerogel. Therefore, even if the aerogel composite can be compressed and deformed by external pressure, it cannot be said that it has the ability to return to its original shape after removal of the load. Furthermore, Patent Document 1 does not take into account thermal insulation properties at high temperatures.

[0006] On the other hand, the hollow latex particles described in Patent Document 2 are made of a polymer and serve as a binder that binds the nanoporous particles together. As described in Patent Document 2, the hollow latex particles are directly bonded to each other to form a continuous network structure (matrix), and the nanoporous particles are dispersed in the continuous matrix of hollow latex particles. Therefore, in the product described in Patent Document 2, the continuous hollow latex particles act as a heat transfer path, resulting in a decrease in thermal insulation. In addition, when the product is used at high temperatures, the matrix may be decomposed, deteriorated, or otherwise lost, causing the product to lose its shape. Furthermore, paragraph

[0044] of Patent Document 2 states that "the concentration of additional additives, such as infrared attenuators and reflective particles, is 5 wt% or less of the total weight of the product." Even if infrared-shielding particles are added as additional additives, a small amount of 5% by mass or less of the total product provides little effect in blocking radiant heat, and the heat insulation at high temperatures is insufficient.

[0007] The present disclosure has been made in consideration of the above-described circumstances, and aims to provide a thermal insulating material that uses a porous structure and has high thermal insulating properties even at high temperatures, and is excellent in flexibility and recovery against compression.

[0008] (1) In order to solve the above-mentioned problems, the heat insulating material of the present disclosure is a heat insulating material having a porous structure in which a plurality of particles are linked to form a skeleton and the skeleton has pores between the skeletons, infrared-shielding particles, and organic hollow particles, wherein the content of the infrared-shielding particles is 10% by mass or more and 30% by mass or less, when the mass of the heat insulating material is 100% by mass, and the content of the organic hollow particles is 5% by mass or more and 30% by mass or less, when the mass of the heat insulating material is 100% by mass.

[0009] The porous structure can achieve a high thermal insulation effect by suppressing mainly conduction and convection among the three forms of heat transfer (conduction, convection, and radiation). Here, radiation is a phenomenon in which heat is transferred by electromagnetic waves, and the higher the temperature, the greater the radiant energy emitted. Therefore, in high-temperature atmospheres, radiation is the main cause of heat transfer. Therefore, at high temperatures, it is difficult to achieve the desired thermal insulation using only the porous structure, and it is effective to use infrared-shielding particles in combination, which can suppress heat transfer due to radiation. However, when a large amount of infrared-shielding particles is incorporated, the infrared-shielding particles are connected to each other to form a heat transfer path, which increases heat transfer due to conduction and may result in a decrease in thermal insulation. According to the thermal insulation material of the present disclosure, by specifying the content of infrared-shielding particles, both radiative and conductive heat transfer can be suppressed, thereby achieving high thermal insulation not only at room temperature but also at high temperatures of 500°C or higher.

[0010] The thermal insulation material of the present disclosure contains organic hollow particles in addition to infrared-shielding particles. The organic hollow particles are particles formed from an organic material and have internal voids. The organic hollow particles impart flexibility, allowing deformation under compressive loads, and recovery after removal of the load. The organic hollow particles are arranged between porous inorganic particles. In the thermal insulation material of the present disclosure, the content of organic hollow particles is relatively low, so the organic hollow particles are less likely to connect to each other, and many of them are arranged discontinuously. Thus, in the thermal insulation material of the present disclosure, the porous structure forms a matrix, and the organic hollow particles are scattered between the porous structures. Therefore, even though the thermal insulation material of the present disclosure contains organic hollow particles, which are an organic component, heat transfer paths are less likely to be formed. Therefore, the organic hollow particles are less likely to disappear even at high temperatures, and high thermal insulation properties can be maintained.

[0011] (2) In the above configuration, the porous structure may have an average particle diameter of 1 μm or more and 1000 μm or less. With this configuration, the porous structure is likely to exhibit an effect of improving heat insulation, and the infrared-shielding particles are likely to exhibit an effect of blocking radiant heat.

[0012] (3) In any of the above configurations, the average particle diameter of the infrared-shielding particles may be 0.3 μm or more and 22 μm or less. With this configuration, the infrared-shielding particles are likely to exhibit a radiant heat blocking effect. Furthermore, the infrared-shielding particles fill gaps in the porous structure, suppressing bonding between the infrared-shielding particles and other components, making it difficult for heat transfer paths to be formed, and therefore the heat insulating properties are less likely to be reduced.

[0013] (4) In any of the above configurations, the organic hollow particles may have an average particle diameter of 1 μm or more and 1000 μm or less. This configuration makes it possible to achieve desired heat insulation, flexibility, and restorability.

[0014] (5) In any of the above configurations, the elastic modulus of the organic hollow particles may be 1 MPa or more and 30 MPa or less. With this configuration, desired flexibility and restorability can be achieved.

[0015] (6) In any of the above configurations, the organic hollow particles may be composed of one or more materials selected from the group consisting of natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, ethylene-propylene-diene rubber, chloroprene rubber, urethane rubber, silicone rubber, ethylene-vinyl acetate rubber, epichlorohydrin rubber, acrylic rubber, styrene-based thermoplastic elastomers, vinyl chloride-based thermoplastic elastomers, olefin-based thermoplastic elastomers, polyester, crosslinked polyacrylonitrile, crosslinked polymethyl methacrylate, and crosslinked polybutyl methacrylate. This configuration facilitates the production of particles having a hollow structure, and the elastic modulus of the resulting hollow particles can be easily adjusted. This allows for the desired flexibility and resilience to be achieved.

[0016] (7) In any of the above configurations, the infrared shielding particles may comprise at least one of particles selected from silicon carbide, kaolinite, montmorillonite, titanium oxide, silicon nitride, mica, aluminum oxide (alumina), aluminum nitride, boron carbide, iron oxide, magnesium oxide, tin oxide, zinc oxide, tantalum oxide, manganese ferrite, manganese oxide, nickel oxide, nickel, silver oxide, silver, bismuth oxide, carbon black, graphite, titanium, iron titanium oxide, zirconium, zirconia, zirconium silicate, barium titanate, manganese dioxide, chromium oxide, titanium carbide, tungsten carbide, tungsten oxide, niobium oxide, indium tin oxide, and cerium oxide, or a mixture of two or more particles selected from these. According to this configuration, the infrared shielding particles have a relatively large heat capacity, so the particles themselves do not heat up easily. In addition, the infrared shielding particles also have high heat resistance. This is advantageous for improving heat insulation at high temperatures.

[0017] (8) In any of the above configurations, the porous structure may have a silica aerogel having a skeleton formed by a plurality of silica particles linked together. The silica aerogel has a good balance between the skeleton size and the pore size, and exhibits excellent heat insulating properties.

[0018] (9) Any of the above configurations may further comprise at least one of a processing aid and inorganic fibers. The processing aid may be used appropriately depending on the manufacturing method, from the viewpoint of facilitating the manufacturing of the insulating material. For example, when water is used as a solvent for the composition for manufacturing the insulating material, selecting a component with a dispersing function or a thickening function makes it easier for the powder of the porous structure or the like to mix with the water. When the powder of the porous structure or the like is compression molded, selecting a thermoplastic component improves moldability. Furthermore, the presence of inorganic fibers is effective in improving the mechanical strength of the insulating material and preventing the porous structure from falling off.

[0019] (10) In any of the above configurations, the organic hollow particles may be discontinuously present between the porous structures. In this configuration, most of the organic hollow particles, which are the organic component, are not continuous but are scattered. Therefore, heat transfer paths are unlikely to be formed by the organic hollow particles, and high thermal insulation properties can be maintained.

[0020] (11) In any of the above configurations, a configuration may be adopted in which a binder that binds the porous structure, the infrared shielding particles, and the organic hollow particles is not included. Generally, an organic material is used as a binder, and the presence of a binder may result in the formation of a heat transfer path through the binder. In this configuration, the absence of a binder allows for high thermal insulation at high temperatures.

[0021] (12) In any of the above configurations, the organic hollow particles may be monovoid particles having a single internal cavity. In the monovoid particles, only the outermost shell portion is made of an organic material, and the rest of the particles are made of voids. Therefore, this configuration makes it easy to reduce the density of the heat insulating material and adjust its flexibility.

[0022] (13) In any of the above configurations, the organic hollow particles may be multi-void particles having multiple voids therein. In the case of multi-void particles, the multiple voids are arranged within the particle body made of an organic material. That is, in multi-void particles, the organic material is present not only in the outermost layer but also inside the particle. Therefore, this configuration makes it easy to adjust the restorability of the heat insulating material.

[0023] The heat insulating material of the present disclosure can achieve high heat insulating properties not only at room temperature but also at high temperatures of 500° C. or higher. The heat insulating material of the present disclosure can achieve flexibility that allows deformation under compressive load and restoring ability after the load is removed.

[0024] The heat insulating material of the present disclosure is described in detail below. The heat insulating material of the present disclosure is not limited to the following forms, and can be embodied in various forms including modifications and improvements that can be made by a person skilled in the art, without departing from the gist of the present disclosure.

[0025] <Thermal Insulation Material> The thermal insulation material of the present disclosure includes a porous structure, infrared shielding particles, and organic hollow particles.

[0026] [Porous Structure] The porous structure has a skeleton formed by connecting multiple particles, with pores between the skeletons. The diameter of the particles (primary particles) forming the skeleton is preferably approximately 2 to 5 nm, and the size of the pores formed between the skeletons is preferably approximately 10 to 50 nm. If most of the pores are so-called mesopores with a size of 50 nm or less, the mesopores are smaller than the mean free path of air, restricting air convection and impeding heat transfer. The shape of the porous structure is not particularly limited, and may be spherical or irregularly shaped, but a chamfered or spherical shape is preferred. This improves the dispersibility of the porous structure, facilitating the preparation of a composition for producing a thermal insulating material (hereinafter referred to as "thermal insulating material composition"). Furthermore, the gaps between the porous structures can be reduced, allowing for a higher filling amount, which also suppresses the connection of infrared-shielding particles and organic hollow particles, thereby improving thermal insulation. The porous structure may be used as produced, or it may be further pulverized before use. The pulverization process can be carried out using a pulverizer such as a jet mill or a spheroidizing device. The pulverization process removes the corners of the particles, giving them a rounded shape. This makes the surface of the insulation smooth and less prone to cracks.

[0027] The average particle diameter of the porous structure is desirably 1 μm or more and 1000 μm or less. If the average particle diameter of the porous structure is less than 1 μm, the filling property of the porous structure decreases and the gaps between the porous structures increase, making it difficult to obtain the effect of improving thermal insulation. On the other hand, if the particle diameter of the porous structure is greater than 1000 μm, the infrared-shielding particles fill the gaps between the porous structures, which may increase the area where the infrared-shielding particles are not present. In this case, the frequency with which infrared rays emitted from the heat source hit the infrared-shielding particles may decrease, which may reduce the radiant heat blocking effect. For example, the average particle diameter of the porous structure is desirably 8 μm or more, or even 50 μm or more. Furthermore, taking into consideration the stability and ease of application of the heat insulating material composition, it is desirably 500 μm or less, or even 300 μm or less. The average particle diameter of the porous structure is determined by the median diameter (D ) calculated from the volume-based particle size distribution measured by laser diffraction / scattering method. 50If a commercially available product is used, the catalog value may be used.

[0028] When the particle diameters of the porous structures are different, the small-diameter porous structures will fill the gaps between the large-diameter porous structures. This facilitates close packing, allowing for a larger porous structure loading. Furthermore, the small-diameter porous structures can inhibit the linkage of infrared-shielding particles and organic hollow particles. This further enhances the effect of improving heat insulation. From this perspective, it is desirable to use porous structures with a wide particle size distribution or to use two or more types with different average particle sizes in combination. Furthermore, during the manufacturing process of the heat insulating material, the stirring conditions of the materials may be adjusted so that some of the large-diameter particles are pulverized into small-diameter particles.

[0029] From the viewpoint of improving heat insulation, the content of the porous structure is desirably 40% by mass or more, and more preferably 50% by mass or more, when the mass of the entire heat insulating material is taken as 100% by mass. On the other hand, in consideration of the balance between heat insulation, flexibility, and restorability, and prevention of falling off, the content of the porous structure is desirably 75% by mass or less, and more preferably 70% by mass or less, when the mass of the entire heat insulating material is taken as 100% by mass.

[0030] It is desirable for the porous structure to have hydrophobic sites on at least the surface of the outer surface and the interior (pore-forming surface). Having hydrophobic sites on the surface can prevent moisture and other substances from penetrating the pores, thereby maintaining the porous structure and preventing loss of heat insulation. For example, surface treatment with a silane coupling agent or the like can impart hydrophobic properties to the surface of the porous structure. Furthermore, by using specific materials as raw materials for the porous structure, a porous structure having hydrophobic sites can be manufactured, or a hydrophobic treatment such as adding hydrophobic groups can be performed during the manufacturing process of the porous structure.

[0031] The type of porous structure is not particularly limited. Examples of primary particles include inorganic particles such as silica, alumina, zirconia, and titania. Among these, porous structures whose primary particles are silica are preferred due to their excellent chemical stability. For example, silica aerogel, in which a skeleton is formed by linking multiple silica particles, is suitable because it has a good balance between the skeleton size and the pore size. Also suitable are cohesive structures in which nanoparticles with a particle diameter of less than 1 μm are linked to form a skeleton. Examples of nanoparticles include fumed silica, wet silica, and those obtained by crushing or dispersing these, as well as those produced from nanoparticle sols such as colloidal silica and colloidal alumina.

[0032] The method for producing aerogel is not particularly limited, and the drying process may be performed at normal pressure or supercritical pressure. For example, drying at normal pressure allows for easy and low-cost production. Depending on the drying method used to produce aerogel, aerogels dried at normal pressure are sometimes called "xerogels" and aerogels dried under supercritical conditions are sometimes called "aerogels." In this specification, however, the term "aerogels" is used to refer to both aerogels.

[0033] [Infrared Shielding Particles] Infrared shielding particles absorb heat from a heat source and re-emit it from the surface on the heat source side, thereby blocking radiant heat from the heat source and contributing to improved thermal insulation, particularly at high temperatures. The content of the infrared shielding particles is set to 10% by mass or more, where the total mass of the thermal insulation material is taken as 100% by mass, from the viewpoint of fully exerting the effect of suppressing heat transfer due to radiation. At 15% by mass or more, the effect of blocking radiant heat is further enhanced. On the other hand, from the viewpoint of suppressing bonding between the infrared shielding particles and other components and making it difficult for a heat transfer path to be formed, the content of the infrared shielding particles is set to 30% by mass or less, where the total mass of the thermal insulation material is taken as 100% by mass. A content of 20% by mass or less is more preferable.

[0034] From the viewpoint of filling the gaps between the porous structures and suppressing the bonding of the infrared-shielding particles with each other or with other components, making it difficult to form a heat transfer path, it is desirable that the particle diameter of the infrared-shielding particles be relatively small. However, if the particle diameter is too small, infrared rays are less likely to hit the particles, and further, the scattering of the infrared rays is insufficient, making it difficult to achieve the radiant heat blocking effect. From this viewpoint, the average particle diameter of the infrared-shielding particles is preferably 0.3 μm or more and 22 μm or less. The shape of the infrared-shielding particles is not particularly limited, and may be spherical, flat, or the like. As with the porous structures, the average particle diameter of the infrared-shielding particles is also determined by the median diameter (D) calculated from the volume-based particle size distribution measured by a laser diffraction / scattering method. 50 ) can be used, and when using a commercially available product, the catalog value can be used.

[0035] Examples of infrared-shielding particles include particles of one kind selected from silicon carbide, kaolinite, montmorillonite, titanium oxide, silicon nitride, mica, alumina, aluminum nitride, boron carbide, iron oxide, magnesium oxide, tin oxide, zinc oxide, tantalum oxide, manganese ferrite, manganese oxide, nickel oxide, nickel, silver oxide, silver, bismuth oxide, carbon black, graphite, titanium, iron titanium oxide, zirconium, zirconia, zirconium silicate, barium titanate, manganese dioxide, chromium oxide, titanium carbide, tungsten carbide, tungsten oxide, niobium oxide, indium tin oxide, and cerium oxide, or particles of a mixture of two or more kinds selected from these. Among these, from the viewpoint of enhancing the radiant heat blocking effect, it is desirable that the infrared-shielding particles have a high emissivity of 0.6 or more in the infrared wavelength region. Examples of high-emissivity particles include silicon carbide, kaolinite, silicon nitride, mica, alumina, zirconia, aluminum nitride, zirconium silicate, cerium oxide, boron carbide, manganese oxide, tin oxide, and iron oxide. Furthermore, from the viewpoint of scattering incident infrared rays and enhancing the radiant heat blocking effect, a form having particles with a high refractive index in the infrared wavelength range is also effective. For example, high-refractive-index particles with a refractive index of 2.0 or more in the visible light wavelength range are suitable. Examples of high-refractive-index particles include silicon carbide, titanium oxide, zirconia, silicon nitride, aluminum nitride, zinc oxide, tantalum oxide, tungsten oxide, niobium oxide, cerium oxide, manganese oxide, tin oxide, bismuth oxide, iron oxide, and barium titanate.

[0036] For example, silicon carbide, titanium oxide, silicon nitride, mica, alumina, aluminum nitride, boron carbide, iron oxide, magnesium oxide, etc. have a relatively large specific heat capacity, and therefore the particles themselves do not heat up easily. In this respect, they also contribute to improving the heat insulating properties of the heat insulating material. In addition, they have high heat resistance, which also contributes to improving the heat resistance of the heat insulating material. Silicon carbide is particularly suitable because its thermal conductivity does not increase much even in a high-temperature atmosphere of about 800°C.

[0037] [Organic hollow particles] From the viewpoint of imparting flexibility and resilience to the heat insulating material, the content of the organic hollow particles is set to 5% by mass or more, with the total mass of the heat insulating material taken as 100% by mass. 10% by mass or more, and even 15% by mass or more are more preferable. On the other hand, from the viewpoint of increasing the content of components that contribute to heat insulation to enhance heat insulating properties and suppressing bonding between the organic hollow particles and other components to make it difficult to form heat transfer paths, the content of the organic hollow particles is set to 30% by mass or less, with the total mass of the heat insulating material taken as 100% by mass. 20% by mass or less is more preferable.

[0038] If the particle size of the organic hollow particles is too small, it becomes difficult to obtain the effect of improving flexibility and recovery. Therefore, the average particle size of the organic hollow particles is preferably 1 μm or more, and more preferably 10 μm or more. On the other hand, if the particle size is too large, the infrared heat shielding particles arranged together may become separated from each other, which may result in a decrease in heat insulation properties at high temperatures. Therefore, the average particle size of the organic hollow particles is preferably 1000 μm or less, and more preferably 500 μm or less, or 200 μm or less. The shape of the organic hollow particles is not particularly limited, and may be spherical, flat, or the like. As with the porous structure, the average particle size of the organic hollow particles is determined based on the median diameter (D ) calculated from the volume-based particle size distribution measured by laser diffraction / scattering method. 50 ) can be used, and when using a commercially available product, the catalog value can be used.

[0039] Organic hollow particles are particles that have a void inside, and the void may be one or more. The former, monovoid particles, are also called balloon structures and have a shell formed from an organic material and one void disposed inside the shell. The latter, multivoid particles, have a particle body formed from an organic material and multiple voids disposed therein. Multivoid particles are a concept that includes porous particles. As organic hollow particles, either monovoid particles or multivoid particles may be used, or both may be used in combination. Organic hollow particles can be produced, for example, by foaming organic particles or pulverizing organic foams.

[0040] The organic material is not particularly limited. Suitable materials include, for example, crosslinked rubbers such as natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, ethylene-propylene-diene rubber, chloroprene rubber, urethane rubber, silicone rubber, ethylene-vinyl acetate rubber, epichlorohydrin rubber, and acrylic rubber; thermoplastic elastomers such as styrene-based, vinyl chloride-based, and olefin-based elastomers; and resins such as polyester, crosslinked polyacrylonitrile, crosslinked polymethyl methacrylate, and crosslinked polybutyl methacrylate. The surfaces of the organic hollow particles may be subjected to a surface treatment or may have inorganic particles or the like attached thereto in order to suppress dusting and improve handleability, improve flame retardancy, or the like. Furthermore, to improve flame retardancy, a flame retardant or the like may be contained in the organic material.

[0041] From the viewpoint of imparting the desired restoring property to the heat insulating material, the elastic modulus of the organic hollow particles is desirably 1 MPa or more, and more preferably 2.5 MPa or more. On the other hand, from the viewpoint of imparting the desired flexibility against compression to the heat insulating material, the elastic modulus of the organic hollow particles is desirably 30 MPa or less, and more preferably 20 MPa or less.

[0042] In this specification, the elastic modulus of the organic hollow particles is determined by the value calculated from the results of the following compression test. First, a powder of organic hollow particles is placed in a cylindrical container made of SUS with a diameter of 11.3 mm. Next, a cylindrical SUS pressing tool with a diameter of 11.2 mm is inserted into the cylindrical container, and the powder of organic hollow particles is pressed into the container by the pressing tool's own weight (load of 2 N). This process is repeated until the initial filling height of the organic hollow particle powder is adjusted to 14 mm, and the pressing tool is placed in the cylindrical container while still inserted in the container on a compression test machine. Then, a compression test is performed using a Tensilon universal material testing machine "RTF1350" manufactured by A&D Co., Ltd., in which the pressing tool repeatedly presses the top surface of the filled powder. The compression test conditions are as follows: pressing tool speed: 6 mm / min; upper limit of compressive stress: 3 MPa; number of pressings: 10 times.

[0043] After the compression test, a stress-compression curve is created based on the obtained data, with the horizontal axis representing the compression ratio and the vertical axis representing the compressive stress. The compression ratio on the horizontal axis is a value calculated using the following formula (I): Compression ratio (%) = Pressurization amount of pressing jig (mm) / 14 [Initial filling height of organic hollow particle powder] (mm) × 100 (I) Then, on the stress-compression curve after the 10th pressing, a straight line is drawn between the point where the compressive stress is 0 MPa and the point where the compressive stress is 3 MPa, and the value obtained by multiplying the slope of the resulting line by 100 is the elastic modulus of the organic hollow particles.

[0044] The organic hollow particles are arranged between the porous structures. From the viewpoint of preventing the formation of a heat transfer path through the organic hollow particles, it is desirable that most of the organic hollow particles are arranged discontinuously, in other words, in a scattered form. For example, when a heat insulating material is manufactured in a sheet shape and the thickness direction is the direction of heat transfer, the organic hollow particles do not form a matrix and are not continuous in the thickness direction, so that they are unlikely to impair the heat insulating properties.

[0045] [Other Components] In addition to the porous structure, infrared-shielding particles, and organic hollow particles, the heat insulating material of the present disclosure may contain other components such as processing aids, inorganic fibers, reinforcing inorganic particles, flame retardants, organic fibers, inorganic hollow particles, and organic binders, as long as the effects achieved by the present disclosure are not impaired. The presence of a binder that binds constituent materials such as the porous structure may result in the formation of a heat transfer path via the binder. Therefore, from the perspective of suppressing the formation of a heat transfer path and achieving high heat insulation at high temperatures, it is desirable for the heat insulating material to be binder-free.

[0046] (1) Processing Aids Porous structures having hydrophobic sites on the surface or inside are poorly compatible with water. In particular, silica aerogels and fumed silica aggregate structures have a low specific gravity and therefore tend to float in water. From the viewpoint of facilitating production, such as improving the water suspendability of the porous structure and making it easier to disperse the porous structure when preparing a heat insulating material composition using water as a solvent, it is desirable to incorporate a processing aid depending on the production method of the heat insulating material. Examples of processing aids include surfactants, thickeners, and suspending agents.

[0047] Surfactants include ionic surfactants (cationic surfactants, anionic surfactants, and amphoteric surfactants) and nonionic surfactants. For example, the use of ionic surfactants can increase the viscosity of insulation compositions and stabilize the dispersion of materials such as porous structures in the insulation composition, even in relatively small amounts. Examples of ionic surfactants include sodium carboxymethylcellulose (CMC-Na), polycarboxylic acid amine salts, polycarboxylic acid ammonium salts, polycarboxylic acid sodium salts, and TEMPO-oxidized cellulose nanofiber (CNF-Na). The use of nonionic surfactants facilitates the incorporation of materials such as porous structures into the solvent when preparing the insulation composition. Furthermore, when these materials aggregate or separate in the insulation composition, they are more easily redispersed, and the solvent is more easily removed when the insulation material is dried and formed. Examples of nonionic surfactants include polyethylene oxide (PEO) and polyvinyl alcohol (PVA). The combined use of nonionic and ionic surfactants is advantageous because it allows the aforementioned effects of each surfactant to be adjusted as desired. For example, PEO does not have a particularly high water retention capacity. Therefore, when preparing the heat insulating composition, water is less likely to enter the gaps between the porous structures, and voids are less likely to occur when water evaporates during drying. As a result, the gaps between the porous structures are more easily filled with infrared shielding particles and organic hollow particles. Also, the gaps between the large-diameter porous structures are more easily filled with small-diameter porous structures.

[0048] If a processing aid is present on the surface or in gaps of a material such as a porous structure, there is a risk that a heat transfer path will be formed through the processing aid. Therefore, from the viewpoint of suppressing the formation of a heat transfer path, it is desirable that the content of the processing aid be 10% by mass or less, and more preferably 7% by mass or less, when the total mass of the thermal insulation material is taken as 100% by mass.

[0049] (2) Inorganic Fibers Inorganic fibers are physically entangled around the porous structure, thereby improving the mechanical strength of the thermal insulation material and preventing the porous structure from falling off. The type of inorganic fiber is not particularly limited, but ceramic fibers such as glass fiber and alumina fiber are preferred in consideration of heat resistance, mechanical strength, etc. The content of inorganic fibers, when the total mass of the thermal insulation material is taken as 100% by mass, should be 5% by mass or more in terms of achieving a reinforcing effect. It should be 15% by mass or less in terms of preventing the formation of a heat transfer path. The length of the inorganic fibers is preferably 16 mm or less, taking into consideration both the reinforcing effect and the prevention of the formation of a heat transfer path.

[0050] (3) Reinforcing inorganic particles In order to improve the mechanical strength of the heat insulating material, reinforcing inorganic particles may be blended into the heat insulating material. The type of reinforcing inorganic particles is not particularly limited, and for example, particles having a relatively large hardness and specific surface area, such as precipitated silica, gel silica, fused silica, wollastonite, potassium titanate, magnesium silicate, glass flakes, calcium carbonate, and barium sulfate, can be used.

[0051] (4) Flame Retardant Adding a flame retardant can impart flame retardancy to the heat insulating material. Known flame retardants, such as halogen-based, phosphorus-based, and metal hydroxide-based flame retardants, may be used. Considering the environmental impact, it is desirable to use a phosphorus-based flame retardant. Examples of phosphorus-based flame retardants include ammonium polyphosphate, red phosphorus, and phosphate esters. Among these, those that are insoluble in water or coated with a water-resistant resin are preferred because they are less likely to leak even when in contact with moisture during use. For example, ammonium polyphosphate and resin-coated ammonium polyphosphate are preferred.

[0052] <Method for manufacturing a thermal insulating material> The thermal insulating material of the present disclosure can be manufactured by pressure molding a material containing a porous structure, infrared shielding particles, organic hollow particles, etc. Alternatively, the thermal insulating material can be manufactured by applying a liquid (including a slurry) composition for a thermal insulating material to a substrate and drying, or by pressure molding a clay-like composition for a thermal insulating material.

[0053] The thickness of the heat insulating material may be determined appropriately depending on the application. For example, from the viewpoint of heat insulating properties, it is desirable to set it to 0.1 mm or more, 0.5 mm or more, or even 1 mm or more. If the heat insulating material is too thick, not only will it be costly, but it will also be difficult to install the heat insulating material in a narrow space. Therefore, for example, a thickness of 10 mm or less, or 8 mm or less is preferable. In particular, from the viewpoint of thinning and increasing flexibility, it is desirable to set it to 5 mm or less, or even 3 mm or less. The density of the heat insulating material is 0.4 g / cm 3 It is desirable to do the following:

[0054] <Use form of thermal insulation material> The thermal insulation material of the present disclosure may be used alone or together with a substrate that supports the thermal insulation material, an exterior material that houses the thermal insulation material, or the like. The substrate may be arranged on only one side of the thermal insulation material in the thickness direction, or may be arranged on both sides so as to sandwich the thermal insulation material. Alternatively, the thermal insulation material may be covered with a single substrate, and the substrate may be used as an exterior material. An adhesive layer may be interposed between the thermal insulation material and the substrate. The adhesive layer may contain a flame retardant in addition to an adhesive component.

[0055] Examples of substrate materials include cloth, resin, paper, and steel plate. Examples of fibers constituting the cloth include glass fiber, rock wool, ceramic fiber, alumina fiber, silica fiber, carbon fiber, metal fiber, polyimide fiber, aramid fiber, and polyphenylene sulfide (PPS) fiber. Examples of ceramic fibers include refractory ceramic fiber (RCF), polycrystalline alumina fiber (Polycrystalline Wool: PCW), and alkaline earth silicate (AES) fiber. Among these, AES fiber is biosoluble and therefore more safe. Examples of resins include polyethylene terephthalate (PET), polyimide, polyamide, and PPS. Examples of paper include pulp and composites of pulp and magnesium silicate. Examples of steel plates include Galvalume Steel Plate (registered trademark), galvanized sheet, stainless steel (SUS) plate, iron plate, and titanium plate. The shape of the substrate is not particularly limited, and examples include woven fabric, nonwoven fabric, film, and sheet. The substrate may be a single layer or a laminate of two or more layers of the same or different materials.

[0056] For example, fabrics (woven fabrics) and nonwoven fabrics made from inorganic fibers such as glass fibers and metal fibers, such as glass cloth, and fire-resistant insulating paper made as a composite of pulp and magnesium silicate, have relatively low thermal conductivity and high shape retention even in high-temperature environments. Furthermore, the use of a highly heat-resistant substrate allows the insulating material of the present disclosure to be applied to applications requiring high heat resistance, thereby broadening its applications. Furthermore, the use of a fire-resistant substrate further improves safety. The highly heat-resistant substrate may be made from glass fiber, rock wool, ceramic fiber, polyimide, PPS, etc., and specific examples include glass fiber nonwoven fabric, glass cloth, aluminum glass cloth, AES wool paper, and polyimide fiber nonwoven fabric.

[0057] Next, the present disclosure will be described more specifically with reference to examples.

[0058] <Production of Insulating Material Samples> Insulating material samples were produced with the compositions shown in Table 1 below. For the samples of Examples 1 to 3, water was first weighed into a resin container, a surfactant was added as a processing aid, and the mixture was stirred for 60 minutes at 800 rpm using an air-driven blade mixer to dissolve the surfactant in the water. After stirring was stopped, silicon carbide (SiC) powder as infrared heat-shielding particles and a powder of organic hollow particles were added, and stirring was continued for an additional 15 minutes at 800 rpm. While continuing stirring, silica aerogel powder as a porous structure was added and completely wetted in the liquid. Then, glass fiber as inorganic fiber was added and stirred for 30 minutes at 800 rpm. After that, additional stirring was continued for 10 minutes at 1000 rpm to produce a clay-like insulating material composition.

[0059] For the samples of Comparative Examples 1 to 3, no powder of organic hollow particles was blended; instead, an organic binder was blended in the sample of Comparative Example 2, and a powder of organic solid particles was blended in the sample of Comparative Example 3. Except for this, heat insulating compositions were produced in the same manner as for the samples of Examples 1 to 3.

[0060] Details of the materials used are as follows: Silica aerogel powder: pulverized "Aerogel Particles P200" manufactured by Cabot Corporation, average particle size 100 μm. Silicon carbide powder: "Fuji Random GC #4000" manufactured by Fuji Manufacturing Co., Ltd., average particle size 5 μm. Organic hollow particle powder: microballoons made of acrylonitrile copolymer, "Matsumoto Microsphere (registered trademark) MFL-HD60CA" manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., average particle size 50 to 70 μm, elastic modulus 17 MPa. Surfactant: polyethylene oxide "PEO-8" manufactured by Sumitomo Seika Chemicals Co., Ltd., viscosity average molecular weight 1.7 million to 2.2 million. Glass fiber: "ECS03-615" manufactured by Central Glass Fiber Co., Ltd., length 3 mm, fiber diameter 9 μm. Organic binder: silicone emulsion, "Siltech E-2152" manufactured by Siltech Co., Ltd. Organic solid particle powder: acrylic rubber powder, "XM-TM-1" manufactured by Matsumoto Yushi Seiyaku Co., Ltd., average particle size 30 μm.

[0061] Next, a base was prepared by stacking a first spacer plate made of stainless steel on top of glass fiber paper. The first spacer plate was 7 mm thick and had a 150 mm square injection hole formed in the center. The prepared heat insulating material composition was filled into the injection hole of the first spacer plate and formed into a plate. Next, the first spacer plate was removed, and glass fiber paper was placed on top, followed by a second spacer plate on top of that, to produce a laminate consisting of "glass fiber paper / heat insulating layer composition / glass fiber paper / second spacer plate." The second spacer plate was 6 mm thick and, like the first spacer plate, had a 150 mm square injection hole formed in the center. The previously formed heat insulating layer composition was placed in the injection hole of the second spacer plate. Separately, a 5 mm thick, 320 mm square aluminum first plate and a 1 mm thick, 320 mm square aluminum second plate were prepared. Multiple grooves were formed on one side of the first plate. The multiple grooves were each linear, 2.5 mm wide, 3 mm deep, and 200 mm long, and were formed parallel to each other at 5 mm intervals. The second plate had 1 mm diameter punched holes formed throughout at 2 mm intervals. The second plate was placed on one side of the first plate, and the laminate was then placed on top of it. The second plate was then placed on top of the laminate, and the first plate was then placed on top of it, with the side with the grooves facing the second plate. In this state, pressure drying was performed using a hot press at a temperature of 165°C and a load of approximately 980 kN for 10 minutes. The sample was then allowed to cool to room temperature (20°C ± 5°C), and the first plate, second plate, second spacer plate, and upper and lower glass fiber papers were removed to obtain a 6 mm thick plate-shaped insulation sample. The density of the resulting insulation sample was measured using a submerged displacement density / specific gravity meter "DSG-1" manufactured by Toyo Seiki Seisakusho Co., Ltd.

[0062] <Method for evaluating thermal insulation properties> (1) Measurement of thermal conductivity at room temperature The thermal conductivity of the produced insulation material samples at room temperature (20°C ± 5°C) was measured using a "non-steady state method thermal conductivity tester Quick Lambda HC-10" manufactured by Eiko Seiki Co., Ltd.

[0063] (2) Measurement of thermal conductivity at high temperatures The thermal conductivity of the manufactured insulation samples at 800°C was measured using a "Quick Thermal Conductivity Meter QTM-700" and a "High-Temperature Probe PD-31N" manufactured by Kyoto Electronics Manufacturing Co., Ltd., as follows. First, three insulation samples were stacked to prepare two 18 mm thick laminates. These laminates were placed one above the probe and one below the probe, sandwiching the probe. A weight of approximately 5 kg was placed on top of the laminate to prevent it from being crushed, and the laminate was placed in an electric furnace. Then, the temperature in the electric furnace was raised to 800°C, and after the temperature in the furnace stabilized, the thermal conductivity was measured.

[0064] (3) Evaluation criteria With regard to heat insulation at room temperature, a thermal conductivity of 0.050 W / m K or less was deemed to be a pass (indicated by a circle in Table 1 below), and a thermal conductivity of more than 0.050 W / m K was deemed to be a fail (indicated by an x ​​in the same table). With regard to heat insulation at high temperatures, a thermal conductivity of less than 0.30 W / m K at 800°C was deemed to be a pass (indicated by a circle in the same table), and a thermal conductivity of 0.30 W / m K or more was deemed to be a fail (indicated by an x ​​in the same table).

[0065] <Method for Evaluating Flexibility and Resilience> A compression test was conducted using a Tensilon universal material testing machine "RTF1350" manufactured by A&D Co., Ltd., in which the center of the manufactured insulation sample (a square plate measuring 150 mm in length, 150 mm in width, and 6 mm in thickness) was pressed with a 60 mm diameter compression terminal. The compression test was conducted by moving the compression terminal back and forth at a speed of 1 mm / min with an upper limit of compressive stress of 1.0 MPa. Three cycles were repeated, with one cycle being the period during which the compressive stress changed from 0.02 MPa to 1.0 MPa to 0.02 MPa. Based on the data obtained from the compression test, a stress-compression curve was created with the horizontal axis representing the compression ratio and the vertical axis representing the compressive stress. The compression ratio on the horizontal axis was calculated using the following formula (II): Compression rate (%) = Push-in distance (mm) of compression terminal after the compressive stress reaches 0.01 MPa during the first pressing cycle / Thickness (mm) of insulation sample when the compressive stress reaches 0.01 MPa during the first pressing cycle × 100 (II)

[0066] [Flexibility] In the stress-compression curve for the second cycle, a straight line was drawn between the point where the compressive stress at the start of the cycle was 0.02 MPa and the point where the compressive stress was 1.0 MPa, and the slope of the resulting line was multiplied by 100 to obtain the flexibility index value of the insulating material sample. That is, the flexibility index value was calculated using the following formula (III): Flexibility index value=(1.0-0.02) / (a-b)×100 (III) [a: compressibility (%) at a compressive stress of 1.0 MPa, b: compressibility (%) at the start of the cycle was 0.02 MPa] In this example, a flexibility index value of 4.0 or less was considered to be pass (indicated by a circle in Table 1 below), and a flexibility index value of more than 4.0 was considered to be fail (indicated by an x ​​in the same table).

[0067] [Resilience] In the stress-compression curve of the second cycle, the value obtained by subtracting the compressibility when the compressive stress was 0.02 MPa at the end of the cycle from the compressibility when the compressive stress was 1.0 MPa was used as the index value of the resilience of the insulating material sample. In this example, a resilience index value of 25% or more was considered to be pass (indicated by a circle in Table 1 below), and a value of less than 25% was considered to be fail (indicated by an x ​​in the same table).

[0068] <Evaluation Results of Heat Insulation, Flexibility, and Restoration> Table 1 shows the composition, density, and evaluation results of each property of the heat insulating material samples.

[0069] As shown in Table 1, the samples of Examples 1 to 3, which contain a predetermined proportion of organic hollow particles, were confirmed to have excellent heat insulating properties at both room temperature and high temperatures. The samples of Examples 1 to 3 were also confirmed to satisfy both flexibility and recovery. In contrast, the samples of Comparative Examples 1 to 3, which do not contain organic hollow particles, were found to be inferior in both flexibility and recovery. Furthermore, the sample of Comparative Example 2, which contained an organic binder, and the sample of Comparative Example 3, which contained organic solid particles instead of organic hollow particles, showed reduced heat insulating properties at high temperatures.

[0070] The heat insulating material of the present disclosure is suitable for use as a heat insulating material for vehicles, houses, electronic devices, and hot / cold insulation containers, etc. In particular, the heat insulating material is suitable for use as a heat insulating material for battery packs that require heat insulation at high temperatures, and as a heat insulating mat that requires cushioning properties.

Claims

1. A thermal insulation material having a porous structure in which a plurality of particles are linked to form a skeleton and pores are present between the skeleton, infrared shielding particles, and organic hollow particles, wherein the content of the infrared shielding particles is 10% by mass or more and 30% by mass or less when the mass of the thermal insulation material is taken as 100% by mass, and the content of the organic hollow particles is 5% by mass or more and 30% by mass or less when the mass of the thermal insulation material is taken as 100% by mass.

2. The heat insulating material according to claim 1, wherein the average particle diameter of the porous structure is 1 μm or more and 1000 μm or less.

3. The heat insulating material according to claim 1, wherein the average particle diameter of the infrared shielding particles is 0.3 μm or more and 22 μm or less.

4. The heat insulating material according to claim 1, wherein the average particle diameter of the organic hollow particles is 1 μm or more and 1000 μm or less.

5. The heat insulating material according to claim 1, wherein the elastic modulus of the organic hollow particles is 1 MPa or more and 30 MPa or less.

6. The heat insulating material according to claim 1, wherein the organic hollow particles are made of one or more materials selected from the group consisting of natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, ethylene-propylene-diene rubber, chloroprene rubber, urethane rubber, silicone rubber, ethylene-vinyl acetate rubber, epichlorohydrin rubber, acrylic rubber, styrene-based thermoplastic elastomer, vinyl chloride-based thermoplastic elastomer, olefin-based thermoplastic elastomer, polyester, polyacrylonitrile crosslinked body, polymethyl methacrylate crosslinked body, and polybutyl methacrylate crosslinked body.

7. The heat insulating material according to claim 1, wherein the infrared shielding particles comprise at least one of particles selected from silicon carbide, kaolinite, montmorillonite, titanium oxide, silicon nitride, mica, alumina, aluminum nitride, boron carbide, iron oxide, magnesium oxide, tin oxide, zinc oxide, tantalum oxide, manganese ferrite, manganese oxide, nickel oxide, nickel, silver oxide, silver, bismuth oxide, carbon black, graphite, titanium, iron titanium oxide, zirconium, zirconia, zirconium silicate, barium titanate, manganese dioxide, chromium oxide, titanium carbide, tungsten carbide, tungsten oxide, niobium oxide, indium tin oxide, and cerium oxide, and particles of a mixture of two or more types selected from these.

8. The heat insulating material according to claim 1, wherein the porous structure has a silica aerogel in which a plurality of silica particles are linked to form a skeleton.

9. The heat insulating material according to claim 1, further comprising at least one of a processing aid and inorganic fibers.

10. The heat insulating material according to claim 1, wherein the organic hollow particles are present discontinuously between the porous structures.

11. The heat insulating material according to claim 1, which does not have a binder that binds the porous structure, the infrared shielding particles, and the organic hollow particles.

12. The heat insulating material according to claim 1, wherein the organic hollow particles are uni-void particles having one void inside.

13. The heat insulating material according to claim 1, wherein the organic hollow particles are multi-pore type particles having a plurality of pores therein.

Citation Information

Patent Citations

  • Heat insulating metal door

    JP2001280029A

  • Binder composition and its use

    JP2021512181A

  • Thermal insulation material

    WO2023276441A1