Sintered silicon nitride
The silicon nitride sintered body with optimized grain boundary consistency and sintering aids addresses the thermal conductivity challenge in power modules, enhancing heat dissipation and preventing malfunctions by reducing phonon scattering, thus ensuring improved thermal management in power modules.
Patent Information
- Application Number
- PCT/JP2024/018193
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-16
- Publication Date
- 2024-12-05
AI Technical Summary
The increasing heat generation density in power modules due to denser electronic equipment and semiconductor devices leads to thermal conductivity issues in silicon nitride sintered bodies, causing cracks and malfunctions, necessitating a higher thermal conductivity in heat dissipation substrates.
A silicon nitride sintered body with grain boundaries characterized by an average reciprocal value of lattice spacing consistency between 0 to 0.5, achieved through specific firing conditions and the use of sintering aids like yttria and carbonitride compounds, enhancing the consistency and abundance of grain interfaces for improved thermal conductivity.
The resulting silicon nitride sintered body exhibits enhanced thermal conductivity, effectively addressing the heat dissipation challenges by reducing phonon scattering at grain boundaries, thereby improving the reliability of heat dissipation substrates.
Smart Images

Figure JP2024018193_05122024_PF_FP_ABST
Abstract
Description
Silicon nitride sintered body
[0001] The present invention relates to a silicon nitride sintered body.
[0002] Silicon nitride sintered bodies have attracted attention as ceramic materials in various industrial fields due to their excellent properties, such as high thermal conductivity, high insulation, and high strength, and are used, for example, as heat dissipation substrates for power modules for automotive and semiconductor applications. When used as a heat dissipation substrate, the substrate's thermal conductivity must be high to prevent malfunctions and component cracking due to heat generation. Therefore, silicon nitride sintered bodies with high thermal conductivity are in demand.
[0003] For example, Patent Document 1 discloses a method for producing a silicon nitride sintered body, which comprises preparing silicon nitride powder having an oxygen content of 1.5 mass% or less, filling the silicon nitride powder into a sintering mold, and continuously applying a pulsed direct current having a voltage of 1 V or more but less than 10 V and an output current of 500 A or more and 40,000 A or less to the gaps between the particles of the raw material powder under a pressure of 70 MPa or more to sinter the silicon nitride powder. It also describes that when the silicon nitride sintered body is used as a heat dissipation substrate for a power module, it can efficiently release (radiate) heat generated from the power module.
[0004] Japanese Patent Application Laid-Open No. 2019-6673
[0005] However, in recent years, the heat generation density of power modules has increased due to the increasing density and power output of electronic devices and semiconductor devices. The temperature rise in power modules can lead to cracking of the substrate and malfunction of the elements. Therefore, heat dissipation substrates are required to have higher heat dissipation properties than before, and the thermal conductivity of the silicon nitride sintered bodies used in heat dissipation substrates needs to be improved.
[0006] SUMMARY OF THE INVENTION It is therefore an object of the present invention to provide a silicon nitride sintered body having high thermal conductivity.
[0007] The present inventors have conducted extensive research to achieve the above object, and as a result have found that the above-mentioned problems can be solved by a silicon nitride sintered body having grain boundaries in which, in a transmission electron microscope (TEM) image of the silicon nitride sintered body, the average reciprocal value (1 / M) of the degree of interplanar alignment (M), which indicates the alignment of the grain boundaries, is 0 to 0.5, and have completed the present invention.
[0008] The gist of the present invention is the following [1] to [4]. [1] A silicon nitride sintered body characterized by having grain boundaries in which, in a transmission electron microscope (TEM) image of the silicon nitride sintered body, the average value of the reciprocal value (1 / M) of the degree of interplanar spacing matching (M), which indicates the alignment of the grain boundaries, is 0 to 0.5. [2] The silicon nitride sintered body according to the above [1], in which the average grain size of silicon nitride crystal grains is 1 to 5 μm. [3] The silicon nitride sintered body according to the above [1] or [2], in which the proportion of grain boundaries showing the reciprocal value (1 / M) of the degree of interplanar spacing matching (M) of 0 to 0.2 is 20% or more. [4] The silicon nitride sintered body according to any of the above [1] to [3], which is a heat dissipation substrate.
[0009] According to the present invention, it is possible to provide a silicon nitride sintered body having high thermal conductivity.
[0010] 1 is a diagram illustrating a cross section of a silicon nitride sintered body observed with a scanning electron microscope, and FIG. 2 is a diagram illustrating the degree of interplanar spacing matching (M).
[0011] [Silicon nitride sintered body] The silicon nitride sintered body of the present invention is a silicon nitride sintered body characterized by having grain boundaries in which, in a transmission electron microscope (TEM) image, the average value of the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M), which indicates the alignment of the grain boundaries, is 0 to 0.5.
[0012] <Face spacing coincidence (M)> The silicon nitride sintered body of the present invention has grain boundaries in which the average value of the reciprocal value (1 / M) of the face spacing coincidence (M), which indicates the alignment of the grain boundaries, is 0 to 0.5. When the average value of the reciprocal value (1 / M) of the face spacing coincidence (M) exceeds 0.5, the thermal conductivity of the silicon nitride sintered body decreases. The reason for this is unclear, but is presumed as follows. The reciprocal value (1 / M) of the face spacing coincidence (M) approaches 0 as the difference in the crystal lattice spacing at the grain boundaries between adjacent silicon nitride crystal grains decreases, and increases (up to 2) as the difference in the crystal lattice spacing increases. When the average value of the reciprocal value (1 / M) of the face spacing coincidence (M) exceeds 0.5, this means that the difference in the crystal lattice spacing at the grain boundaries is large, and the alignment of the grain boundaries is low. The thermal conductivity of silicon nitride sintered bodies, which are insulators, is due to lattice vibrations (phonons), and grain boundaries with poor alignment are thought to act as a source of phonon scattering, which inhibits thermal conduction. On the other hand, when the average value of the reciprocal value (1 / M) of the degree of interplanar spacing agreement (M) is 0 to 0.5, it means that the difference in the crystal lattice spacing on the grain boundaries is small and there are many grain boundaries with high interplanar spacing agreement. In this case, it is estimated that there are few phonon scattering sources (factors that inhibit thermal conduction) and the thermal conductivity is high.
[0013] In the present invention, having grain boundaries having an average reciprocal value (1 / M) of the degree of interplanar spacing agreement (M) of 0 to 0.5 means that the reciprocal value (1 / M) of the degree of interplanar spacing agreement (M) is measured at 50 arbitrarily selected grain boundary surfaces by the method described below, and the average value of the 50 points is 0 to 0.5. The degree of interplanar spacing agreement (M) will be described in detail below.
[0014] Generally, silicon nitride sintered bodies are obtained by firing silicon nitride powder, the raw material, at high temperatures. During firing, the silicon nitride crystal grains that make up the silicon nitride powder undergo grain growth and densification to form a silicon nitride sintered body. The interface between adjacent silicon nitride crystal grains in the sintered body is referred to as a grain boundary. For example, FIG. 1 shows a schematic image of a cross section of a silicon nitride sintered body observed with a scanning electron microscope. Silicon nitride sintered body 10 contains multiple silicon nitride crystal grains (e.g., silicon nitride crystal grains A and B) that have grown into grains. The interface between silicon nitride crystal grains A and B is referred to as a grain boundary (grain boundary S in the figure). Note that silicon nitride sintered body 10 contains multiple silicon nitride crystal grains other than silicon nitride crystal grains A and B, and therefore, many grain boundaries other than grain boundary S are also present.
[0015] The degree of lattice spacing agreement (M) in the present invention indicates the consistency of grain boundaries in a transmission electron microscope (TEM) image of a silicon nitride sintered body. As shown in Figure 2, for example, by observing the vicinity of the grain boundary S between adjacent silicon nitride crystal grains A and B with a TEM, the crystal lattice spacing d A and the crystal lattice spacing d on the grain boundary surface S of the silicon nitride crystal grain B. B Then, the reciprocal value (1 / M) of the surface spacing agreement (M) is calculated based on the following formula (1).
[0016] In formula (1), in adjacent silicon nitride crystal grains A and B, the crystal lattice spacing at the grain boundary of silicon nitride crystal grain A is d A and the crystal lattice spacing on the grain boundary of the silicon nitride crystal particle B is d B In formula (1), |d A -d B | is d A -d B In the present invention, the reciprocal value (1 / M) of the degree of interplanar spacing agreement (M) is calculated for each of 50 arbitrarily selected grain boundary surfaces and the reciprocal values (1 / M) of the degree of interplanar spacing agreement (M) are averaged.
[0017] crystal lattice spacing d A and the crystal lattice spacing d B The smaller the difference between the two, the larger the value of M, and the degree of lattice spacing agreement (M) is in the range of 0.5 to infinity. On the other hand, 1 / M, which is the reciprocal of M, is in the range of 0 to 2. The closer 1 / M is to 0, the smaller the crystal lattice spacing d A and the crystal lattice spacing d B The closer 1 / M is to 2, the smaller the difference between A and the crystal lattice spacing d B As described above, the silicon nitride sintered body of the present invention is thought to have high thermal conductivity due to the small difference in crystal lattice spacing on the grain boundaries and the large number of highly coherent grain boundaries.
[0018] The reciprocal value (1 / M) of the degree of interplanar matching (M) is measured as follows. First, a TEM image satisfying the following requirements (1) to (3) is obtained by TEM observation of a cross section of a silicon nitride sintered body. Requirement (1): Two silicon nitride crystal particles (silicon nitride crystal particle A, silicon nitride crystal particle B) are directly bonded via a grain boundary. Requirement (2): The grain boundary of requirement (1), silicon nitride crystal particle A, and silicon nitride crystal particle B are included in the same field of view. However, it is not necessary to include the entire grain boundary, and it is not necessary to include the entire silicon nitride crystal particle A and silicon nitride crystal particle B. Requirement (3): Crystal lattice fringes reaching the grain boundary of requirement (1) are observed in both silicon nitride crystal particle A and silicon nitride crystal particle B.
[0019] Next, from the obtained TEM image, the acute angle θ formed between the crystal lattice fringes of the silicon nitride crystal particles A and the grain boundary surface is A , and the acute angle θ between the crystal lattice fringes of the silicon nitride crystal grain B and the grain boundary surface B Furthermore, selected area electron diffraction images of silicon nitride crystal particle A and silicon nitride crystal particle B are obtained and indexed, and the Miller indices (hkl) are determined for each crystal lattice fringe observed in requirement (3), and the crystal lattice spacing d A0 and the crystal lattice spacing d of the silicon nitride crystal particles B B0However, if multiple sets of crystal lattice fringes are observed in silicon nitride crystal particle A and silicon nitride crystal particle B, the crystal lattice fringe with the largest interplanar spacing is determined as d A0 , d B0 Adopted as.
[0020] The crystal lattice spacing d A0 , d B0 From the above, the crystal lattice spacing d on the grain boundary surface is calculated as follows: A and d B Find the answer. A = d A0 / sin(θ A ) d B = d B0 / sin(θ B ) The d obtained in this way A and d B From this, the reciprocal value (1 / M) of the surface spacing agreement (M) can be calculated based on the above-mentioned formula 1.
[0021] As described above, the silicon nitride sintered body of the present invention has grain boundaries in which, in a transmission electron microscope (TEM) image, the average value of the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M), which indicates the integrity of the grain boundaries, is 0 to 0.5. From the viewpoint of further increasing the thermal conductivity of the silicon nitride sintered body, the average value of the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M) is preferably 0 to 0.45, more preferably 0 to 0.35, and even more preferably 0 to 0.30. The lower limit of the average value of the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M) is ideally 0, but the average value of the reciprocal value (1 / M) may be, for example, 0.1 or more.
[0022] The silicon nitride sintered body of the present invention preferably has a grain boundary surface presence rate of 20% or more, where the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M) is 0 to 0.2. A grain boundary surface presence rate of 20% or more facilitates the improvement of the thermal conductivity of the silicon nitride sintered body. From the viewpoint of further improving the thermal conductivity, the grain boundary surface presence rate is more preferably 22% or more, even more preferably 24% or more, and even more preferably 30% or more. The upper limit of the grain boundary surface presence rate is not particularly limited, but ideally 100%. The grain boundary surface presence rate where the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M) is 0 to 0.2 is determined by calculating the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M) at 50 arbitrarily selected grain boundary surfaces in a transmission electron microscope (TEM) image of the silicon nitride sintered body, and among the measured reciprocal values (1 / M) at those 50 surfaces, the reciprocal value (1 / M) is the proportion of grain boundary surfaces where the reciprocal value (1 / M) is in the range of 0 to 0.2.
[0023] The method for adjusting the average value of the reciprocal value (1 / M) of the degree of interplanar spacing coincidence (M) and the abundance rate of grain boundary surfaces where the reciprocal value (1 / M) is 0 to 0.2 is not particularly limited. For example, they can be adjusted by the firing conditions when producing the silicon nitride sintered body and the amount of sintering aid used during firing.
[0024] <Average particle size> The average particle size of the silicon nitride crystal particles in the silicon nitride sintered body of the present invention is not particularly limited, but is preferably 1 to 5 μm, more preferably 2 to 5 μm, and even more preferably 3 to 5 μm. If the average particle size of the silicon nitride crystal particles is equal to or greater than these lower limits, the thermal conductivity of the sintered body tends to be high. If the average particle size of the silicon nitride crystal particles is equal to or less than these upper limits, the mechanical strength of the sintered body tends to be high.
[0025] The average particle size of silicon nitride crystal grains in a silicon nitride sintered body is the volume-based average particle size and is measured as follows: A cross section of the silicon nitride sintered body is observed with a scanning electron microscope (SEM), and images of 300 or more grains are analyzed with an image analyzer to determine the area-equivalent circle diameter of each grain. The volume-based average particle size of the area-equivalent circle diameter is then calculated.
[0026] <Thermal Conductivity> The thermal conductivity of the silicon nitride sintered body of the present invention is preferably 85 W / (m·K) or more, more preferably 90 W / (m·K) or more, from the viewpoint of improving heat dissipation when used as a heat dissipation substrate. The higher the thermal conductivity, the better, but it is, for example, 150 W / (m·K) or less, and in practical use, 100 W / (m·K) or less. The thermal conductivity can be measured by the method described in the examples.
[0027] [Method for Producing Sintered Silicon Nitride] The sintered silicon nitride of the present invention can be obtained by firing silicon nitride powder, preferably by firing a mixed raw material containing silicon nitride powder and a sintering aid.
[0028] The silicon nitride sintered body of the present invention has many highly coherent grain boundaries. Highly coherent grain boundaries have few dangling bonds and low grain boundary energy. It is believed that if an environment is created in which silicon nitride particles can move freely during sintering, they will be stabilized in a low-energy state, making it easier to form highly coherent grain boundaries. Methods for creating an environment in which silicon nitride particles can move freely include appropriately selecting the amount of sintering aid, sintering temperature, and sintering time, as described below. Note that other methods than those described above can also be applied as long as an environment in which silicon nitride particles can move freely can be created. Below, the raw materials and sintering conditions for producing a silicon nitride sintered body are explained.
[0029] (Silicon nitride powder) The average particle size of the silicon nitride powder contained in the mixed raw material is not particularly limited, but from the viewpoint of setting the average particle size of silicon nitride crystal particles in the silicon nitride sintered body in the desired range described above, it is preferably 0.5 to 3 μm, more preferably 0.5 to 2 μm. The average particle size of the silicon nitride powder can be measured using a laser diffraction / scattering particle size distribution analyzer, and a volume frequency distribution curve is obtained with the horizontal axis representing particle size (μm) and the vertical axis representing volume frequency. The average particle size of the silicon nitride powder means the particle size (D50) at which the cumulative curve of the measured volume-based particle size distribution reaches 50%.
[0030] Silicon nitride powder can be produced by known methods. Examples of methods for producing silicon nitride powder include a reduction-nitridation method in which silica powder is used as a raw material and nitrogen gas is passed through in the presence of carbon powder to produce silicon nitride, a direct nitridation method in which silicon powder is reacted with nitrogen at high temperatures, and an imide decomposition method in which silicon halide is reacted with ammonia. Silicon nitride powder can also be produced by combustion synthesis, a direct nitridation method that utilizes self-combustion. Combustion synthesis allows for stable production of silicon nitride powder without incurring energy costs.
[0031] The combustion synthesis method uses silicon powder as a raw material, forcibly ignites a portion of the raw material powder under a nitrogen atmosphere, and synthesizes silicon nitride by self-heating of the raw material compound. The combustion synthesis method is a known method, and reference can be made to, for example, JP 2000-264608 A and WO 2019 / 167879 A.
[0032] (Sintering Aid) It is preferable to use a metal oxide as the sintering aid. By using a metal oxide as the sintering aid, the sintering of the silicon nitride powder is facilitated, and a denser and stronger sintered body is more likely to be obtained. As the metal oxide, yttria (Y 2 O 3 ), ceria (CeO), magnesia (MgO), etc. Among these, yttria is preferable. One type of metal oxide may be used alone, or two or more types may be used in combination.
[0033] As the sintering aid, it is preferable to use an oxygen-free compound together with the metal oxide. By using these in combination, the reciprocal value (1 / M) of the interplanar spacing matching ratio (M) is easily reduced. Furthermore, by using an oxygen-free compound as a sintering aid, the amount of oxygen dissolved in silicon nitride due to the sintering aid can be reduced. As a result, a silicon nitride sintered body with high thermal conductivity can be obtained. Examples of oxygen-free compounds include carbonitride-based compounds containing rare earth elements and carbonitride-based compounds containing magnesium. Among these, from the viewpoint of reducing the reciprocal value (1 / M) of the interplanar spacing matching ratio (M) of the resulting silicon nitride sintered body, it is preferable to use a carbonitride-based compound containing magnesium as the oxygen-free compound, and it is preferable to use both a carbonitride-based compound containing rare earth elements and a carbonitride-based compound containing magnesium.
[0034] Examples of carbonitride compounds containing rare earth elements include Y 2 Si 4 N 6 C, Yb 2 Si 4 N 6 C, Ce 2 Si 4 N 6 Among these, Y is preferred from the viewpoint of easily obtaining a silicon nitride sintered body having a high thermal conductivity. 2 Si 4 N 6 C, Yb 2 Si 4 N 6 C is preferred, and Y 2 Si 4 N 6 C is more preferable. Examples of carbonitride compounds containing magnesium include MgSi 4 N 6 Examples include C.
[0035] When both a metal oxide and an oxygen-free compound are used as the sintering aid, the mass ratio of the oxygen-free compound contained in the sintering aid to the metal oxide (oxygen-free compound / metal oxide) is preferably 2.2 to 10, more preferably 2.5 to 5, and even more preferably 3 to 4.5. Within such a range, a denser silicon nitride sintered body with higher thermal conductivity can be more easily obtained.
[0036] The content of the sintering aid in the mixed raw material (total content of the sintering aid) is preferably 8 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 13 parts by mass or more, per 100 parts by mass of silicon nitride powder. By adjusting the content of the sintering aid to be higher, a large amount of liquid phase is present during firing, allowing silicon nitride particles to move freely and stabilize in a low-energy state. As a result, it is believed that the alignment of the grain boundaries is improved, making it easier to lower the reciprocal value (1 / M) of the interplanar spacing coincidence (M). The upper limit of the content of the sintering aid (total content of the sintering aid) is not particularly limited, but from the viewpoint of improving the physical properties of the sintered body, such as thermal conductivity and mechanical strength, the content of the sintering aid per 100 parts by mass of silicon nitride powder is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less.
[0037] From the viewpoint of reducing the reciprocal value (1 / M) of the interplanar spacing conformity (M) of the silicon nitride sintered body, the content of the magnesium-containing carbonitride-based compound in the mixed raw material is preferably 5 to 20 parts by mass, more preferably 5 to 15 parts by mass, and even more preferably 6 to 10 parts by mass, per 100 parts by mass of silicon nitride powder. By using a relatively large amount of the magnesium-containing carbonitride-based compound, it becomes easier to reduce the reciprocal value (1 / M) of the interplanar spacing conformity (M). Furthermore, the magnesium-containing carbonitride-based compound volatilizes during firing at a relatively high temperature for a long period of time, and therefore does not adversely affect the physical properties of the fired body.
[0038] (Firing conditions) The silicon nitride sintered body of the present invention can be obtained by firing a mixed powder containing the above-mentioned silicon nitride powder and sintering aid. The mixed powder can be press-molded into a compact and then fired. The press-molding is typically uniaxial press-molding, but a method in which uniaxial press-molding is followed by CIP (cold isostatic pressing) molding is preferably used.
[0039] The firing temperature (firing temperature) can be, for example, 1500 to 1900°C. However, from the viewpoint of reducing the reciprocal value (1 / M) of the interplanar spacing coincidence (M) of the resulting silicon nitride sintered body, it is preferable to set the maximum firing temperature to 1750 to 1800°C and hold the temperature for 8 to 30 hours. By increasing the maximum temperature and lengthening the holding time, an environment in which silicon nitride particles can move freely can be established, making it easier to obtain a silicon nitride sintered body of the present invention with a reciprocal value (1 / M) of the interplanar spacing coincidence (M) within the specified range. The maximum firing temperature is preferably 1755 to 1790°C, more preferably 1760 to 1780°C. The holding time at the maximum temperature is preferably 9 to 25 hours, more preferably 10 to 20 hours.
[0040] The firing is preferably carried out in an inert gas atmosphere. Examples of the inert gas atmosphere include a nitrogen atmosphere and an argon atmosphere, with a nitrogen atmosphere being preferred. The firing may be carried out at normal pressure or under pressure.
[0041] As described above, the silicon nitride sintered body of the present invention has high grain boundary alignment and excellent thermal conductivity, making it suitable for use as a variety of heat dissipation substrates.
[0042] EXAMPLES The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0043] [Measurement Methods] Various physical properties in the examples and comparative examples were measured by the following methods.
[0044] <Average Value of Reciprocal Value (1 / M) of Planar Spacing Conformity (M)> (i) Preparation of TEM Observation Samples For the plate-shaped silicon nitride sintered bodies (thickness approximately 0.3 mm) produced in each Example and Comparative Example, both surfaces were mechanically polished until the thickness was approximately 0.1 mm, and then 6 keV argon ions were irradiated until perforations were formed using an ion slicer "EM-09100IS" manufactured by JEOL Ltd., to prepare TEM observation samples. (ii) TEM Observation Using a transmission electron microscope "JEM-2100" manufactured by JEOL Ltd., an acceleration voltage of 200 kV and an observation magnification of 500,000 times were used to obtain TEM images satisfying the above requirements (1) to (3) at 50 locations per sample. For the 50 grain boundaries, the reciprocal value (1 / M) of the planar spacing conformity (M) was calculated based on the following formula. The reciprocal values (1 / M) of the 50 locations were averaged to obtain the average value of the reciprocal value (1 / M) of the planar spacing conformity (M).
[0045] In formula (1), when adjacent silicon nitride crystal particles are silicon nitride crystal particle A and silicon nitride crystal particle B, and the grain boundary between these adjacent silicon nitride crystal particles is grain boundary surface S, the crystal lattice spacing on the grain boundary surface S of silicon nitride crystal particle A is d A and the crystal lattice spacing on the grain boundary surface S of the silicon nitride crystal grain B is d B d A and d B is calculated by the following formula: A = d A0 / sin(θ A ) d B = d B0 / sin(θ B ) θ A is the acute angle between the crystal lattice fringe of silicon nitride crystal particle A and the grain boundary surface S, and θ B is the acute angle θ between the crystal lattice fringe of silicon nitride crystal particle B and the grain boundary surface S. B Also, d A0 is the crystal lattice spacing of the silicon nitride crystal particle A, and d B0 is the crystal lattice spacing of the silicon nitride crystal particles B.
[0046] <Rate of Presence of Grain Boundary Surfaces Where the Reciprocal Value (1 / M) of the Interplanar Spacing Matching Degree (M) is 0 to 0.2> This is the rate of the number of grain boundary surfaces where the reciprocal value (1 / M) is within the range of 0 to 0.2, among the reciprocal values (1 / M) of the interplanar spacing matching degree (M) at 50 grain boundary surfaces obtained as described above. In other words, if the number of grain boundary surfaces where the reciprocal value (1 / M) is within the range of 0 to 0.2 is X, the rate of presence of grain boundary surfaces where the reciprocal value (1 / M) is 0 to 0.2 can be calculated by the following formula: Rate of Presence (%)=100×(X / 50)
[0047] <Average Particle Diameter of Silicon Nitride Crystal Particles> (i) Preparation of SEM Observation Samples The cross sections of the plate-shaped silicon nitride sintered bodies produced in each Example and Comparative Example were mechanically polished to a mirror finish to prepare SEM observation samples. (ii) SEM Observation Using a JEOL scanning electron microscope "JCM-7000" at an acceleration voltage of 15 kV and an observation magnification of 5000x, five fields of view per sample were observed to obtain particle images of 300 or more silicon nitride crystal particles. The 300 or more particle images were analyzed using an image analyzer attached to the SEM device to determine the area circle diameter of each particle. The volume-based average particle diameter of the area circle equivalent diameter was then calculated. The volume-based average particle diameter can be calculated based on the following formula: Volume-based average particle diameter = Σ(area circle equivalent diameter ^4) / Σ(area circle equivalent diameter ^3)
[0048] <Thermal Conductivity> The thermal conductivity was measured by a laser flash method using a thermal conductivity measuring instrument "LFA467" manufactured by Netsch.
[0049] The following materials were used as raw materials for producing sintered silicon nitride: <Silicon nitride powder> Silicon nitride powder: silicon nitride powder with an average particle size of 0.95 μm produced by combustion synthesis.
[0050] <Sintering aid> Metal oxide: yttria (Y 2 O 3 ) Carbonitride compounds containing rare earth elements: Y 2 Si 4 N 6 C It was prepared by thermal synthesis using the following reaction formula: 8Si 3 N 4 +6Y 2 O 3+15C+2N 2 →6Y 2 Si 4 N 6 C+9CO 2 Carbonitride compounds containing magnesium element: MgSi 4 N 6 C was prepared by thermal synthesis using the following reaction formula: Si 3 N 4 + MgSiN 2 + C → MgSi 4 N 6 C
[0051] Example 1: 100 parts by mass of silicon nitride powder was mixed with Y as a sintering aid. 2 O 3 3 parts by mass of Y 2 Si 4 N 6 2 parts by mass of C, MgSi 4 N 6 Six parts by mass of C were added and mixed in a planetary ball mill to obtain a mixed raw material. Next, the mixed raw material was subjected to uniaxial press molding and CIP molding to produce a molded body, which was then fired in a nitrogen atmosphere at atmospheric pressure to obtain a silicon nitride sintered body. The firing was carried out at a maximum temperature of 1760°C and a holding time at the maximum temperature of 10 hours. The results of various evaluations of the produced silicon nitride sintered body are shown in Table 1.
[0052] Examples 2 to 5, Comparative Examples 1 to 4 Silicon nitride sintered bodies were produced in the same manner as in Example 1, except that the composition of the mixed raw materials and the firing conditions were changed as shown in Table 1. Table 1 shows the results of various evaluations of the produced silicon nitride sintered bodies.
[0053]
[0054] The silicon nitride sintered bodies of the Examples, in which the average value of the reciprocal value (1 / M) of the degree of interplanar spacing agreement (M) was within the range of 0 to 0.5, had high thermal conductivity and excellent heat dissipation. On the other hand, the silicon nitride sintered bodies of the Comparative Examples, in which the average value of the reciprocal value (1 / M) of the degree of interplanar spacing agreement (M) was greater than 0.5, had lower thermal conductivity and inferior heat dissipation compared to the Examples.
[0055] 10 Silicon nitride sintered body A Silicon nitride crystal grain B Silicon nitride crystal grain S Grain boundary surface
Claims
1. A silicon nitride sintered body characterized in that the grain boundaries have an average reciprocal value (1 / M) of the degree of interplanar alignment (M), which indicates the alignment of the grain boundaries, of 0 to 0.5 in a transmission electron microscope (TEM) image of the silicon nitride sintered body.
2. The silicon nitride sintered body according to claim 1, wherein the average particle size of the silicon nitride crystal grains is 1 to 5 μm.
3. The silicon nitride sintered body according to claim 1, wherein the rate of grain boundaries exhibiting a reciprocal value (1 / M) of the degree of coincidence of the interplanar spacing (M) of 0 to 0.2 is 20% or more.
4. The silicon nitride sintered body according to any one of claims 1 to 3, which is a heat dissipation substrate.
Citation Information
Patent Citations
Highly head conductive silicon nitride sintered compact and its production
JP1998194842A
Circuit board excellent in high strength / high heat conductivity
JP2004231513A
Micro processor and risc processor
JP2009206527A
METHOD FOR MANUFACTURING SiC FIBER-REINFORCED SiC COMPOSITE MATERIAL
JP2010070421A