Thermally conductive two-component addition-curable silicone composition, cured product, and sheet
The thermally conductive two-component addition-curing silicone composition addresses the challenge of achieving high thermal conductivity and preventing filler separation by using a specific combination of organopolysiloxanes, organohydrogenpolysiloxanes, and aluminum hydroxide powders, resulting in enhanced thermal performance and equipment durability.
Patent Information
- Application Number
- PCT/JP2024/018285
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-01
- Filing Date
- 2024-05-17
- Publication Date
- 2024-12-05
AI Technical Summary
Existing thermally conductive two-component addition-curing silicone compositions face challenges in achieving high thermal conductivity while maintaining low viscosity and preventing filler separation and sedimentation, which affects the abrasion resistance of coating equipment and storage stability.
A thermally conductive two-component addition-curing silicone composition is developed, comprising an organopolysiloxane with alkenyl groups, an organohydrogenpolysiloxane, aluminum hydroxide powder with specific particle sizes, and a thermally conductive filler, along with a silane coupling agent and a hydrosilylation reaction platinum catalyst, to enhance thermal conductivity and prevent filler separation.
The composition achieves high thermal conductivity, low viscosity, and improved productivity with reduced abrasion on coating equipment, effectively suppressing filler separation and sedimentation, ensuring stable storage and handling properties.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Thermally conductive two-component addition-curable silicone composition, cured product, and sheet
[0001] The present invention relates to a thermally conductive two-component addition-curable silicone composition, a cured product and sheet, and methods for producing the same.
[0002] It is widely known that heat-generating electronic components generate heat during use, resulting in a decrease in performance. Various heat dissipation technologies are used to address this issue. Generally, heat is dissipated by placing a cooling component (such as a heat sink) near the heat-generating component, placing them in close contact, and efficiently removing heat from the cooling component. In this case, if there is a gap between the heat-generating component and the cooling component, air with poor thermal conductivity is trapped, reducing thermal conductivity and preventing the temperature of the heat-generating component from dropping sufficiently. To prevent this phenomenon, heat-dissipating materials with good thermal conductivity and conformability to the surface of the component, such as thermal grease and thermal dissipation sheets, are used.
[0003] An example of a heat-generating component is an on-board battery charger (OBC), which automatically adjusts the current and voltage when charging a battery, generating a large amount of heat energy during power conversion and charging. Therefore, in order to keep the operating temperature low and maintain high performance, the heat dissipation material used as a heat countermeasure must have high heat dissipation performance. Furthermore, in environments where insulation is required, such as OBCs, it is necessary to use heat dissipation materials filled with insulating fillers.
[0004] Additionally, examples of insulating and highly thermally conductive fillers used in thermally conductive materials include aluminum oxide and aluminum nitride. However, aluminum oxide and aluminum nitride have a high Mohs hardness of 8 or more, raising concerns about abrasion of dispenser components made of stainless steel or silicon carbide (SiC). In particular, two-component additive-curing thermally conductive materials are generally applied using a metering and dispensing device, where a constant volume is dispensed, followed by mixing the two components in a static mixer. However, abrasion attacks on dispenser components that are metered and dispensed are often problematic, resulting in a decrease in the accuracy of the metering and dispensing components during use. In contrast, aluminum hydroxide has a low Mohs hardness of 3, raising little concern about abrasion attacks on dispenser components.
[0005] However, aluminum hydroxide has a lower thermal conductivity than aluminum oxide or aluminum nitride, and therefore, to obtain a thermally conductive composition with high thermal conductivity, the amount of thermally conductive filler must be increased. However, simply increasing the aluminum hydroxide content increases the viscosity of the composition, making it difficult to discharge. Conversely, reducing the viscosity of the composition to improve workability increases oil separation due to the difference in specific gravity between the organopolysiloxane in the base oil and the thermally conductive filler, resulting in the issue of sedimentation and separation of the filler during storage. Therefore, using aluminum hydroxide with a larger particle size is considered as a way to increase thermal conductivity with the same filling amount, but there are no specific examples of using large particle size aluminum hydroxide to fill a thermally conductive filler at 90% by mass or more.
[0006] Patent Document 1 exemplifies a thermally conductive silicone composition using aluminum hydroxide particles with an average particle size of 50 μm or less. While using a thermally conductive filler with a large average particle size is considered to increase the thermal conductivity of the silicone composition, there are no examples using aluminum hydroxide with an average particle size exceeding 50 μm.
[0007] Patent No. 5940325
[0008] In view of the above circumstances, an object of the present invention is to provide a thermally conductive two-part addition-cure silicone composition, a cured product, a sheet, and a production method that have a low viscosity and excellent productivity, reduce wear on application equipment, and are capable of suppressing separation and sedimentation of the thermally conductive filler in the composition over time, while increasing the proportion of thermally conductive filler in the composition to achieve high thermal conductivity.
[0009] As a result of intensive research by the present inventors to solve the above problems, they have discovered a method for producing a thermally conductive filler composition comprising (A) an organopolysiloxane having, in one molecule, at least two alkenyl groups bonded to silicon atoms, (B) an organohydrogenpolysiloxane having, in one molecule, at least two hydrogen atoms bonded to silicon atoms, (C) aluminum hydroxide powders having different average particle sizes, and a thermally conductive filler having an average particle size of 0.1 μm or more and less than 5 μm, blended in specific amounts and specific ratios, and (D) a silane carbonate. The present inventors have discovered that the above-mentioned problems can be solved by providing a thermally conductive two-part addition-curable silicone composition comprising a first part and a second part, the first part containing the following (A), (C), (D), and (E) but not containing (B), and the second part containing the following (A), (B), (C), and (D) but not containing (E), thereby completing the present invention.
[0010] Accordingly, the present invention provides the following inventions: 1. A thermally conductive two-part addition-curable silicone composition consisting of a first part and a second part, wherein the first part contains the following components (A), (C), (D), and (E) but does not contain component (B), and the second part contains the following components (A), (B), (C), and (D) but does not contain component (E): (A) an organopolysiloxane having, in each molecule, at least two alkenyl groups bonded to silicon atoms; (B) an organohydrogenpolysiloxane having, in each molecule, at least two hydrogen atoms bonded to silicon atoms; (C) an aluminum hydroxide powder (C-1) having an average particle size of 40 to 100 μm; an aluminum hydroxide powder (C-2) having an average particle size of 5 μm or more and less than 40 μm; and a thermally conductive filler (C-3) having an average particle size of 0.1 μm or more and less than 5 μm, wherein the total amount of (C-1) and (C-2) in component (C) is 40 to 70 mass% and the amount of (C-3) in component (C) is 30 to 60 mass%: a thermally conductive two-part addition-curable silicone composition comprising a first part and a second part combined, in which the total amount of component (C) is 90 to 95 mass%; (D) a silane coupling agent and a compound represented by the following general formula (1): (In the formula, R 1 are independently monovalent hydrocarbon groups, and R 2are independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group, a is 5 to 100, and b is 1 to 3.), and (E) a platinum catalyst for a hydrosilylation reaction. 2. The thermally conductive two-component addition-curable silicone composition according to 1, wherein the content of component (D) is 10 to 500 parts by mass per 100 parts by mass of the total of components (A) and (B) in the thermally conductive two-component addition-curable silicone composition consisting of the first and second components combined. 3. The thermally conductive two-component addition-curable silicone composition according to 1 or 2, wherein component (C-3) is aluminum oxide. 4. The thermally conductive two-component addition-curable silicone composition according to any one of 1 to 3, wherein the mass ratio of components (C-1) to (C-2) is 2:8 to 8:2. 5. 5. The thermally conductive two-component addition-curable silicone composition according to any one of 1 to 4, wherein the entire thermally conductive two-component addition-curable silicone composition comprising the first and second components together contains 100 to 700 parts by mass of component (C-1), 50 to 500 parts by mass of component (C-2), and 150 to 800 parts by mass of component (C-3), relative to 100 parts by mass of the total of components (A), (B), (D), and (E). 6. The density measured by the underwater displacement method according to JIS K 6268 is 3.0 g / cm. 3 6. A thermally conductive two-component addition-curable silicone composition according to any one of 1 to 5, which has a thermal conductivity of 3.0 W / m K or more as measured by the hot disk method in accordance with ISO 22007-2. 7. A cured product of the thermally conductive two-component addition-curable silicone composition according to any one of 1 to 6. 8. A thermally conductive sheet comprising a cured product of the thermally conductive two-component addition-curable silicone composition according to any one of 1 to 6. 9. A method for producing the thermally conductive two-component addition-curable silicone composition according to any one of 1 to 6, which comprises the step of mixing (C-1), (C-2), and (C-3) above.
[0011] According to the present invention, it is possible to provide a thermally conductive two-component addition-cure silicone composition, a cured product, a sheet, and a production method which increase the proportion of thermally conductive filler in the composition to obtain high thermal conductivity, while at the same time achieving low viscosity and excellent productivity, thereby reducing wear on application equipment and preventing separation and sedimentation of the thermally conductive filler in the composition over time.
[0012] The present invention will be described in detail below. The "thermally conductive two-component addition-curable silicone composition" of the present invention may also be referred to simply as the "two-component silicone composition." [Component (A)] Component (A) of the present invention is the main component (base polymer) of the composition. Component (A) is an organopolysiloxane having at least two silicon-bonded alkenyl groups per molecule, and may be used alone or in combination of two or more. Component (A), for example, is an organopolysiloxane represented by the following average composition formula (2) and having at least two silicon-bonded alkenyl groups per molecule (hereinafter sometimes referred to as "silicon-bonded alkenyl groups"). At least two silicon-bonded alkenyl groups are present per molecule, preferably 2 to 50, and more preferably 2 to 20. These silicon-bonded alkenyl groups may be bonded to a silicon atom at a molecular chain terminal, a silicon atom at a non-terminal position (i.e., other than the molecular chain terminal), or a combination thereof. 3 c R 4 d SiO (4-c-d) / 2 (2) (wherein, R 3 are independently an alkenyl group, and R 4 are independently unsubstituted or substituted monovalent hydrocarbon groups having no aliphatic unsaturated bonds, c is 0.0001 to 0.2, d is 1.7 to 2.2, and c+d is a number that satisfies the range of 1.9 to 2.4.
[0013] Examples of the alkenyl group include those having 2 to 6 carbon atoms, such as a vinyl group, an allyl group, an isopropenyl group, a 1-butenyl group, a 1-pentenyl group, and a 1-hexenyl group. Of these, an alkenyl group having 2 to 4 carbon atoms is preferred, and a vinyl group is more preferred.
[0014] The remaining organic group bonded to the silicon atom, that is, the unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bond, can be one having 1 to 12 carbon atoms, with monovalent hydrocarbon groups having 1 to 6 carbon atoms being preferred. Specific examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, and dodecyl; aryl groups such as phenyl, 1-naphthyl, 2-naphthyl, and tolyl; aralkyl groups such as benzyl and 2-phenylethyl; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, chlorine, and bromine, such as chloromethyl and 3,3,3-trifluoropropyl. From the viewpoint of ease of synthesis, etc., the methyl, phenyl, and 3,3,3-trifluoropropyl groups are preferred.
[0015] c is 0.0001 to 0.2, and preferably 0.0005 to 0.1. d is 1.7 to 2.2, and preferably 1.9 to 2.0. c+d is a number that satisfies the range of 1.9 to 2.4, and preferably a number that satisfies the range of 1.95 to 2.05.
[0016] The kinematic viscosity of component (A) at 25°C measured using an Ostwald meter is 10 to 100,000 mm 2 / s is preferred, and 100 to 50,000 mm 2 / s is more preferable. 2 When the ratio is 1 / s, the resulting cured product has better strength, fluidity and workability.
[0017] Examples of organopolysiloxanes of component (A) that satisfy the above requirements include those represented by the following general formula (3): (In the formula, R 5 are independently unsubstituted or substituted monovalent hydrocarbon groups, e is a number from 10 to 2,000, and R 5 At least two of the groups are selected to be alkenyl groups.
[0018] In this formula (3), R 5 The unsubstituted or substituted monovalent hydrocarbon group represented by the R 3 (alkenyl group), and R4 (an unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bonds), and the number of carbon atoms, specific examples, etc. are also the same. 5 At least two, preferably 2 to 50, and more preferably 2 to 20 of these groups are selected to be alkenyl groups. By setting the number of alkenyl groups to at least the above-mentioned lower limit, curing becomes easier, while by setting the number of alkenyl groups to no more than the above-mentioned upper limit, the cured product becomes more stable. Furthermore, e is preferably 40 to 1,200, and more preferably 50 to 600. By setting it within this range, a two-component silicone composition with a more suitable viscosity can be obtained, which makes it easier to handle and work with and gives a stronger cured product.
[0019] Specific examples of organopolysiloxanes represented by the above formula (3) include dimethylpolysiloxanes capped at both molecular chain terminals with dimethylvinylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with trimethylsiloxy groups, dimethylsiloxane-methylvinylsiloxane copolymers capped at one molecular chain terminal with a trimethylsiloxy group and one terminal with a dimethylvinylsiloxy group, dimethylsiloxane-methylvinylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxy groups, and dimethylsiloxane-diphenylsiloxane copolymers capped at both molecular chain terminals with dimethylvinylsiloxy groups, etc. Component (A) is produced by a conventionally known method.
[0020] The content of component (A) in the entire thermally conductive two-component addition-curable silicone composition, consisting of the first and second components combined, is preferably 0.5 to 8.0 mass %, and more preferably 0.8 to 5.0 mass %.
[0021] [Component (B)] Component (B) of the present invention is an organohydrogenpolysiloxane having at least two silicon-bonded hydrogen atoms (hereinafter sometimes referred to as "silicon-bonded hydrogen atoms") per molecule, and can be used alone or in combination of two or more. The number of silicon-bonded hydrogen atoms per molecule of this organohydrogenpolysiloxane is preferably 2 to 100, more preferably 2 to 50, and even more preferably 2 to 20. By setting the number of silicon-bonded hydrogen atoms at or above the above-mentioned lower limit, curing becomes easier, while by setting it at or below the above-mentioned upper limit, greater flexibility is achieved and voids due to dehydrogenation during storage and curing can be more effectively prevented. The silicon-bonded hydrogen atoms may be located at the molecular chain terminals, in the middle of the molecular chain, or both.
[0022] Examples of the component (B) include those represented by the following average composition formula (4). (In the formula, R 6 are independently hydrogen atoms or monovalent hydrocarbon groups having no aliphatic unsaturated bonds, and f is 8 to 1,000. 6 and f are selected so that there are at least two hydrogen atoms bonded to silicon atoms in one molecule. Note that the order of bonding of the siloxanes in the organopolysiloxane formula is not important.
[0023] In the above formula (4), R 6 are independently hydrogen atoms or monovalent hydrocarbon groups that do not contain aliphatic unsaturated bonds. The monovalent hydrocarbon groups preferably have 1 to 12 carbon atoms, and more preferably have 1 to 6 carbon atoms. 6Specific examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclohexyl, octyl, and dodecyl; aryl groups such as phenyl, 1-naphthyl, 2-naphthyl, and tolyl; aralkyl groups such as benzyl and 2-phenylethyl; and groups in which some or all of the hydrogen atoms in these groups have been substituted with halogen atoms such as fluorine, chlorine, and bromine, such as a chloromethyl group or a 3,3,3-trifluoropropyl group. Of these, from the viewpoint of ease of synthesis, the methyl group, the phenyl group, and the 3,3,3-trifluoropropyl group are preferred.
[0024] f is 8 to 1,000, and is preferably 10 to 500, more preferably 15 to 100, from the viewpoint of improving the handling properties of the composition and the properties of the resulting cured product. When the degree of polymerization is within the above range, a two-component silicone composition with a more suitable viscosity is obtained, which is easy to handle and produces a stronger cured product. However, 6 and f are appropriately selected so that each molecule contains at least two silicon-bonded hydrogen atoms. The number of silicon-bonded hydrogen atoms is at least two, and preferably 2 to 20. By setting the number within the above range, a two-component silicone composition with a more suitable viscosity can be obtained. The molecular structure of the organohydrogenpolysiloxane of component (B) is not particularly limited as long as it satisfies the above requirements. Component (B) is produced by a conventionally known method.
[0025] The viscosity of the organohydrogenpolysiloxane of component (B) is preferably 1 to 10,000 mPa·s, more preferably 3 to 2,000 mPa·s, and even more preferably 10 to 1,000 mPa·s. It is preferably liquid at room temperature (25°C). The viscosity of component (B) is measured using a BM-type viscometer (for example, manufactured by Tokyo Keiki Co., Ltd.). The rotor, rotation speed, and rotation time are selected appropriately according to the viscosity, using standard methods.
[0026] The content of component (B) in the entire thermally conductive two-component addition-curable silicone composition comprising the first and second components is preferably an amount such that the number of silicon-bonded hydrogen atoms (SiH groups) in component (B) per alkenyl group in component (A) in the entire composition is 0.1 to 5.0, more preferably 0.2 to 2.0, and even more preferably 0.5 to 1.5. If the content of component (B) is too low, the effect of improving storage stability may be insufficient, and if the content is too high, the physical properties of the resulting thermally conductive silicone cured product may be unstable.
[0027] Note that component (B) is used in component 2, but is not contained in component 1. When component (B) is used in component 1, component 1 thickens and hardens over time at room temperature, making it impossible to maintain the viscosity of the two-component silicone composition at the time of production.
[0028] [Component (C)] Component (C) of the present invention comprises aluminum hydroxide powder (C-1) having an average particle size of 40 to 100 μm, aluminum hydroxide powder (C-2) having an average particle size of 5 μm or more and less than 40 μm, and thermally conductive filler (C-3) having an average particle size of 0.1 μm or more and less than 5 μm, wherein the total proportion of (C-1) and (C-2) in component (C) is 40 to 70 mass%, and the proportion of (C-3) in component (C) is 30 to 60 mass%, and each of these thermally conductive fillers can be used alone or in combination of two or more.
[0029] The average particle size in the present invention can be measured using a laser diffraction / scattering particle size distribution analyzer, for example, the "Microtrac MT3300EX" manufactured by Nikkiso Co., Ltd. The average particle size is determined by multiplying the measured particle size value by the relative particle amount (difference %) and dividing the result by the total relative particle amount (100%). The average particle size is the average diameter of the particles.
[0030] The average particle size of component (C-1) is 40 to 100 μm, preferably 50 to 90 μm. If the average particle size of component (C-1) is greater than 100 μm, it may cause wear on the kneader and stirring blades, increase the material thickness during packaging, and increase the unevenness of the sheet surface, resulting in an increased thermal resistivity. The aluminum hydroxide powder of component (C-1) may be of one type, or two or more types with different average particle sizes may be used in combination.
[0031] The average particle size of component (C-2) is 5 μm or more but less than 40 μm, preferably 10 to 30 μm. The aluminum hydroxide powder of component (C-2) may be a single type or a combination of two or more types with different average particle sizes.
[0032] The average particle size of the thermally conductive filler (C-3) is 0.1 μm or more but less than 5 μm, preferably 0.5 to 3 μm. If the average particle size is less than 0.1 μm, the particle surface area increases, increasing the interface area between the particles and the resin. This increases interfacial thermal resistance, tending to reduce thermal conductivity and also resulting in a significant increase in the viscosity of the two-component silicone composition. Preferred thermally conductive fillers include aluminum oxide powder, magnesium oxide powder, aluminum hydroxide powder, zinc oxide powder, and aluminum nitride powder, with aluminum oxide being preferred from the perspective of packing properties. While both spherical and irregular shapes are usable, irregular shapes are more preferred because spherical particles result in point contact between fillers, reducing the contact area between fillers. Shapes other than spherical are considered irregular. The thermally conductive filler (C-3) may be a single type or a combination of two or more types with different average particle sizes.
[0033] The content of component (C) in the entire thermally conductive two-component addition-curable silicone composition consisting of the first and second components combined is 90 to 95% by mass, and preferably 91 to 94% by mass. If the content is less than 90% by mass, the thermal conductivity of the two-component silicone composition will be insufficient, and if it exceeds 95% by mass, handling will be impaired when filling component (C).
[0034] In the entire thermally conductive two-part addition-curable silicone composition consisting of the first and second parts, the total amount of (C-1) and (C-2) in component (C) is 40 to 70% by mass, preferably 45 to 75% by mass, and the amount of component (C-3) is 30 to 60% by mass, preferably 35 to 55% by mass.
[0035] If the combined proportion of components (C-1) and (C-2) is less than 40% by mass (if the proportion of component (C-3) exceeds 60% by mass), wear on the kneader and stirring blades may increase, and separation and sedimentation of the thermally conductive filler in the composition will become more pronounced over time. If the combined proportion of components (C-1) and (C-2) exceeds 70% by mass (if the proportion of component (C-3) is less than 30% by mass), the thermal conductivity of the two-component silicone composition will be insufficient, and sedimentation and separation of the thermally conductive filler in the composition will become more pronounced over time.
[0036] The mass ratio of component (C-1) to component (C-2) is preferably 2:8 to 8:2, and more preferably 2.5:7.5 to 7.5:2.5. This range improves filling properties and reduces separation and sedimentation of the thermally conductive filler in the composition over time.
[0037] More specifically, in the entire thermally conductive two-component addition-curable silicone composition consisting of the first and second components, the content of component (C-1) is preferably 100 to 700 parts by mass, more preferably 200 to 600 parts by mass, and even more preferably 300 to 500 parts by mass, per 100 parts by mass of the total of components (A), (B), (D), and (E). By setting the content of component (C-1) to be equal to or greater than the above-mentioned lower limit, filling properties are improved and thermal conductivity is further increased. On the other hand, by setting the content of component (C-1) to be equal to or less than the above-mentioned upper limit, filling properties are improved and the viscosity of the two-component silicone composition can be set within a more suitable range.
[0038] More specifically, in the entire thermally conductive two-component addition-curable silicone composition consisting of the first and second components, the content of component (C-2) is preferably 50 to 500 parts by mass, more preferably 75 to 400 parts by mass, and even more preferably 100 to 300 parts by mass, per 100 parts by mass of the total of components (A), (B), (D), and (E). By keeping the content of component (C-2) within this range, dense filling of component (C) becomes possible, the thermal conductivity becomes higher, and the viscosity of the two-component silicone composition can be set within a more suitable range.
[0039] In the entire thermally conductive two-component addition-curable silicone composition consisting of the first and second components, the content of component (C-3) is preferably 150 to 800 parts by mass, more preferably 200 to 700 parts by mass, and even more preferably 300 to 600 parts by mass, per 100 parts by mass of the total of components (A), (B), (D), and (E). By setting the content of component (C-2) at or above the lower limit, dense packing of component (C) is possible, and oil separation can be suppressed. By setting the content of component (C-2) at or below the upper limit, thermal conductivity is increased, and the viscosity of the two-component silicone composition can be set within a more suitable range.
[0040] The component (C) is used in both the first liquid and the second liquid, and the ratio of the component (C) used in the first liquid and the second liquid is not particularly limited as long as the mixing ratio of the first liquid and the second liquid is approximately the same mass ratio.
[0041] [Component (D)] The component (D) of the present invention is a compound represented by the following general formula (1): (In the formula, R 1 are independently monovalent hydrocarbon groups, and R 2 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group, a is 5 to 100, and b is 1 to 3.) These organopolysiloxanes can be used alone or in combination of two or more. The incorporation of component (D) has the effect of lowering the viscosity of the resulting two-component silicone composition.
[0042] Examples of silane coupling agents include vinyl-based silane coupling agents, epoxy-based silane coupling agents, acrylic-based silane coupling agents, and long-chain alkyl-based silane coupling agents. Specific examples include hexyltrimethoxysilane, decyltrimethoxysilane, hexadecyltrimethoxysilane, decylmethyldimethoxysilane, decyldimethylmethoxysilane, decyltriethoxysilane, 7-octenyltrimethoxysilane, and phenyltrimethoxysilane. Among these, decyltrimethoxysilane is preferred.
[0043] In the above formula (1), R 1 are independently monovalent hydrocarbon groups, which may be unsubstituted or substituted. The number of carbon atoms is preferably 1 to 10, more preferably 1 to 6, and even more preferably 1 to 3. Specific examples include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, and dodecyl; aryl groups such as phenyl; and groups in which some or all of the hydrogen atoms have been substituted with halogen atoms such as fluorine, chlorine, and bromine, or with cyano groups, such as chloromethyl, 3,3,3-trifluoropropyl, and cyanoethyl. R 1 As the alkyl group, a methyl group, a phenyl group, and a 3,3,3-trifluoropropyl group are preferred.
[0044] In the above formula (1), R 2 are independently an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group. Examples of alkyl groups include R 1 Examples of the alkoxyalkyl group include the same straight-chain alkyl group, branched-chain alkyl group, and cyclic alkyl group as those exemplified in 1. Examples of the alkoxyalkyl group include a methoxyethyl group and a methoxypropyl group, and those having 2 to 10 carbon atoms are preferred. Examples of the alkenyl group include a vinyl group, an allyl group, an isopropenyl group, a 1-butenyl group, a 1-pentenyl group, and a 1-hexenyl group, and those having 1 to 8 carbon atoms are preferred. Examples of the acyl group include an acetyl group and an octanoyl group, and those having 2 to 10 carbon atoms are preferred. R 2is preferably an alkyl group, more preferably a methyl group or an ethyl group.
[0045] a is an integer of 5 to 100, preferably 8 to 50, and b is an integer of 1 to 3, preferably 3.
[0046] Specific examples of suitable organopolysiloxanes of component (D) include the following: (In the formula, Me is a methyl group. The same applies hereinafter.)
[0047] The viscosity of the organopolysiloxane of component (D) at 25°C measured with an Ostwald meter is usually 0.01 to 1,000 mm 2 / s, 0.1 to 100 mm 2 / s is preferable. 2 If the viscosity is less than 1,000 mm / s, the oil of component (D) may easily bleed out from the silicone composition. 2 By adjusting the viscosity to be equal to or less than 1 / 2 s, a two-component silicone composition having a more suitable viscosity can be obtained, and application workability can be further improved.
[0048] In the present invention, when component (D) is used, it is preferably prepared into a heat-treated mixture together with the above-mentioned component (C) or components (A) to (C) at a temperature of 70°C or higher, more preferably 80 to 180°C.
[0049] When component (D) is used in the present invention, the aforementioned component (C) can also be pretreated with component (D). Treating component (C) with component (D) can further reduce the viscosity of the resulting two-component silicone composition. In this case, the surface treatment of component (C) with component (D) can be performed using a spraying method using a fluid nozzle, a stirring method that applies shear force, a dry method using a ball mill or mixer, or a wet method using an aqueous or organic solvent system. Stirring is performed to a temperature that does not destroy the thermally conductive filler. In the dry method, the system temperature or the drying temperature after treatment is determined appropriately depending on the type of surface treatment agent within a range that does not cause the surface treatment agent to volatilize or decompose, but is, for example, 80 to 180°C.
[0050] The content of component (D) in the entire thermally conductive two-component addition-curable silicone composition (combining the first and second components) is preferably 10 to 500 parts by weight, more preferably 25 to 450 parts by weight, and even more preferably 100 to 400 parts by weight, per 100 parts by weight of the total of components (A) and (B). By maintaining the content within this range, component (D) can more effectively reduce the viscosity of the two-component silicone composition. In two-component addition-curable materials, dehydrogenation of the organohydrogenpolysiloxane occurs due to the thermally conductive filler during storage at room temperature. Therefore, if the content of component (D) is too low, it may be difficult to suppress the deterioration over time, i.e., the decrease in hardness during storage at room temperature. On the other hand, by keeping the content of component (D) below the upper limit, separation and sedimentation of the thermally conductive filler in the composition over time can be further suppressed. The content of component (D) in the entire thermally conductive two-component addition-curable silicone composition, consisting of the first and second components, is preferably 0.9 to 10.0% by mass, and more preferably 2.0 to 8.0% by mass.
[0051] When component (D) is used, it can be used in both the first liquid and the second liquid, or in either one of them. The ratio of component (D) used in the first liquid and the second liquid is not particularly limited, but for example, it can be used in equal amounts in the first liquid and the second liquid.
[0052] [Component (E)] Component (E) of the present invention is a platinum catalyst for hydrosilylation reaction, which is a catalyst that promotes the addition reaction between the alkenyl group in component (A) and the hydrogen atom bonded to the silicon atom in component (B).Examples include chloroplatinic acid, alcohol-modified chloroplatinic acid, coordination compounds of chloroplatinic acid with olefins, aldehydes, vinylsiloxanes or acetylene compounds, tetrakis(triphenylphosphine)palladium, chlorotris(triphenylphosphine)rhodium, etc.Platinum catalysts are preferred, and coordination compounds of chloroplatinic acid with vinylsiloxane are more preferred.
[0053] The content of component (E) may be a catalytic amount, but from the viewpoint of appropriate curing, it is preferably an amount equivalent to 0.1 to 500 ppm (by mass), and more preferably 1 to 100 ppm, of platinum group metals relative to the entire thermally conductive two-component addition-curable silicone composition consisting of components 1 and 2. Note that component (E) is used in component 1, but is not contained in component 2.
[0054] In addition to the components (A) to (E) described above, the composition of the present invention can contain various other known components (additives) as other compounding agents, provided that the purpose of the present invention is not impaired. When an additive is contained, the content of the additive is preferably 1.0% by mass or less, more preferably 0.5% by mass or less, and may even be 0% by mass, based on the total thermally conductive two-part addition-curable silicone composition consisting of the first and second parts combined.
[0055] For example, reaction inhibitors for adjusting the curing rate and storage stability, specifically acetylene alcohols such as triallyl isocyanate alkyl maleate, ethynyldecylmethylcarbinol, and ethynylcyclohexanol, and silanes thereof, siloxane-modified products, hydroperoxide, tetramethylethylenediamine, colorants such as ferrous oxide and ferric oxide, either alone or in combination, and fumed silica as a thixotropic agent can be blended.
[0056] [Production Method] The composition of the present invention is a thermally conductive two-part addition-curable silicone composition comprising a first part containing the above-mentioned components (A), (C), (D), and (E) but not the above-mentioned component (B), and a second part containing the above-mentioned components (A), (B), (C), and (D) but not the above-mentioned component (E). These can be obtained by mixing the respective components.
[0057] The method for producing the composition of the present invention simply involves mixing the components of the first and second liquids. The (C) thermally conductive filler preferably includes a step of mixing (C-1), (C-2), and (C-3). Specifically, examples of the production method include the following steps: For the first liquid, the steps are: mixing components (A), (C), and (D) and heat-treating them at a temperature of 70°C or higher to obtain a heated mixture; cooling the heated mixture obtained above to room temperature (25°C) or lower, and then adding component (E), a reaction inhibitor, a colorant, and a thixotropic agent. For the second liquid, the steps are: mixing components (A), (C), and (D) and heat-treating them at a temperature of 70°C or higher to obtain a heated mixture; cooling the heated mixture obtained above to room temperature (25°C) or lower, and then adding component (B), a reaction inhibitor, a colorant, and a thixotropic agent.
[0058] The heating temperature in the heat treatment step is preferably 70°C or higher, more preferably 70 to 180°C. The heating time is not particularly limited, and is preferably 1 hour or longer, more preferably 1 to 3 hours. When an additive is added, it may be added in any step, but it is preferably added after the heated mixture has been cooled. As a mixing device for preparing the first and second liquids, known mixers such as a static mixer, a planetary mixer, a paddle mixer, etc. can be used.
[0059] In the composition of the present invention, the mixing ratio of the first liquid to the second liquid is preferably approximately equal by mass, and specifically, the ratio of the first liquid to the second liquid is preferably in the range of 1:0.5 to 1:2, more preferably 1:0.75 to 1:1.25, even more preferably 1:0.9 to 1:1.1, and particularly preferably 1:0.95 to 1:1.05. The device for mixing the first liquid and the second liquid is not limited to a static mixer such as a static mixer, and may be a known mixer such as a planetary mixer or a paddle mixer.
[0060] [Thermal Conductive Two-Part Addition-Curable Silicone Composition] The viscosity of the first and second parts of the thermally conductive two-part addition-curable silicone composition of the present invention at 25°C is preferably 30 to 800 Pa·s, more preferably 60 to 500 Pa·s, and even more preferably 90 to 300 Pa·s. Setting the viscosity at or above the lower limit improves shape retention, while setting the viscosity at or below the upper limit improves workability. The viscosity can be adjusted mainly by adjusting the content and blending ratio of component (C) within the range specified above. The viscosity can be measured using a spiral viscometer, for example, a Malcom viscometer (Type PC-10AA, rotation speed 10 rpm).
[0061] The thermal conductivity of the first and second parts of the thermally conductive two-part addition-curable silicone composition of the present invention is preferably 3.0 W / m·K or higher, and more preferably 3.3 W / m·K or higher, from the viewpoint of heat dissipation performance of heat-generating electronic components. The upper limit of the thermal conductivity can be set to 5.2 W / m·K or lower, or even 4.2 W / m·K or lower. The thermal conductivity can be adjusted mainly by adjusting the content and blending ratio of component (C) within the range specified above. The thermal conductivity is measured by the hot disk method in accordance with ISO 22007-2.
[0062] The thermally conductive two-component addition-curable silicone composition of the present invention has a density of 2.0 g / cm3 for the first and second components. 3 More than 2.2 g / cm is preferred. 3 The upper limit of the density is preferably 3.0 g / cm3 from the viewpoint of reducing the weight of the material and parts using the material. 3 Preferably, 2.8 g / cm or less 3 The following is more preferable. The density can be adjusted mainly by adjusting the content and blending ratio of component (C) within the range specified above. The density is measured by the underwater displacement method in accordance with JIS K 6268.
[0063] [Cured Product] The curing conditions for the thermally conductive two-component addition-curable silicone composition are not particularly limited and may be the same as those for known addition-reaction-curable silicone compositions. For example, the composition will cure sufficiently at room temperature, but may be heated if necessary. When heated, the curing conditions may be 40 to 180°C for 1 to 60 minutes.
[0064] The hardness of the cured product is preferably 10 to 90, more preferably 20 to 80, on a Shore OO hardness scale as specified in ASTM D 2240-05. A hardness equal to or greater than the lower limit mentioned above reduces the possibility that the heat dissipation material will shift or fall off from its mounted position due to impacts such as vibration. Furthermore, a hardness equal to or less than the upper limit mentioned above reduces the stress applied to electronic components, thereby extending the solder life. The measurement methods and preferred ranges for the thermal conductivity and density of the cured product are the same as those for the thermally conductive two-component addition-curable silicone composition described above.
[0065] [Sheet] The shape of the cured product is not particularly limited, but a sheet is preferred. The properties of the thermally conductive sheet are not particularly limited, but examples include gel, low-hardness rubber, and high-hardness rubber. Of these, low-hardness rubber is preferred. In this case, low hardness refers to a range of 10 to 90 in terms of the hardness of the cured product. The thickness of the sheet is not particularly limited, but is preferably 100 μm or more, and, considering the size of the electronic components to be mounted, is preferably 5 mm or less.
[0066] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the following formulas, Me is a methyl group, Vi is a vinyl group, and the order of the siloxane bonds does not matter.
[0067] The raw materials are shown below. The kinematic viscosity of component (A) is measured at 25°C using an Ostwald meter. Component (A) A-1: Dimethylpolysiloxane terminated at both molecular chain ends with dimethylvinylsiloxy groups (kinematic viscosity 400 mm 2 / s, amount of Vi group per 100 g is 0.0185 mol, e in general formula (3) is 146)
[0068] Component (B) B-1: Trimethylsiloxy-blocked methylhydrogen-dimethylpolysiloxane represented by formula (5) (Si—H content: 0.00128 mol / g) B-2: Trimethylsiloxy-blocked methylhydrogen-dimethylpolysiloxane represented by formula (6) (Si—H content: 0.00190 mol / g) B-3: Dimethylhydrogensiloxy-blocked dimethylpolysiloxane represented by formula (7) (Si—H content: 0.00130 mol / g)
[0069] (C) Component C-1-1: crushed aluminum hydroxide (average particle size 90 μm, density 2.42 g / cm 3 C-1-2: crushed aluminum hydroxide (average particle size 53 μm, density 2.42 g / cm 3 ) C-2-1: crushed aluminum hydroxide (average particle size 12 μm, density 2.42 g / cm 3 C-2-2: crushed aluminum hydroxide (average particle size 8 μm, density 2.42 g / cm 3 ) C-3-1: crushed aluminum oxide (average particle size 2 μm, density 3.98 g / cm 3 )
[0070] Component (D) D-1: organopolysiloxane represented by formula (8) Component (E) E-1: vinylsiloxane complex of chloroplatinic acid (Pt content 1% by mass)
[0071] First Liquid: Components (A), (C), and (D) were added to a 5 L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. in the mass mixing ratios shown in Tables 1 to 3, and mixed, followed by heat treatment and mixing at 150°C for 1 hour to obtain Mixture 1. Next, after this Mixture 1 was sufficiently cooled to room temperature (25°C), component (E) was added in the mass mixing ratios shown in Tables 1 to 3 below, and the mixture was mixed uniformly at room temperature (25°C) for 20 minutes to obtain a first liquid.
[0072] Liquid 2: Components (A), (C), and (D) were added to a 5L planetary mixer manufactured by Inoue Seisakusho Co., Ltd. in the mass mixing ratios shown in Tables 1 to 3, and then heated and mixed at 150°C for 1 hour to obtain Mixture 2. Mixture 2 was then sufficiently cooled to room temperature (25°C), after which component (B) was added in the mass mixing ratios shown in Tables 1 to 3 below, and the mixture was mixed uniformly at room temperature (25°C) for 20 minutes to obtain Liquid 2.
[0073] [Viscosity] The viscosity of each of the first and second liquids in each example was measured at 25° C. using a spiral viscometer: Malcom viscometer (type PC-10AA, rotation speed: 10 rpm).
[0074] The first and second parts of each example were mixed uniformly at a mass ratio of 1:1 using a static mixer MXA6.3-21 (manufactured by Noritake Co., Ltd.) at room temperature (25°C), discharged, thoroughly degassed under vacuum, and then poured into a mold that would result in a thickness of 6 mm after curing. The mixture was cured at 25°C for 24 hours to obtain a sheet-like cured product. The thermal conductivity of the resulting cured product at 25°C was measured using a hot disc method thermal property measuring device TPS 2500 S (manufactured by Kyoto Electronics Manufacturing Co., Ltd.) (hot disc method in accordance with ISO 22007-2).
[0075] [Density] The first and second parts of each example were mixed uniformly at a mass ratio of 1:1 using a static mixer MXA6.3-21 (manufactured by Noritake Co., Ltd.) at room temperature (25°C), discharged, thoroughly degassed under vacuum, and then poured into a mold that would result in a thickness of 6 mm after curing. The mixture was cured at 25°C for 24 hours to obtain a sheet-like cured product. The density of the resulting cured product was measured by the underwater displacement method specified in JIS K 6268, and the value was used.
[0076] [Confirmation of Separation and Sedimentation of Thermally Conductive Filler] 800 g of the first and second liquids of each example were filled into a 350 mL cylindrical container and left to stand at room temperature for one month. After that, a ruler was immersed in the material. If the ruler touched the bottom of the container, it was marked as "Good", and if it touched a hard part of the material before touching the bottom and did not reach the bottom, it was marked as "Poor".
[0077] The results of the above viscosity, thermal conductivity, density, and separation and sedimentation confirmation are also shown in Tables 1 to 3.
[0078]
[0079]
[0080]
[0081] The above results show that the thermally conductive two-component addition-curable silicone compositions of Examples 1 to 8 of the present invention had a thermal conductivity of 3.0 W / m K or higher, and prevented separation and sedimentation of the thermally conductive filler in the composition over time. 3 or less. A thermally conductive silicone composition and its cured product were obtained that exhibited high thermal conductivity, low density, and excellent workability and storage stability. Comparative Examples 1 to 3 demonstrated that when component (C-1), component (C-2), or component (C-3) was not included and a thermally conductive filler was blended in the same proportion, the viscosity became so high that it became impossible to measure the viscosity. Comparative Examples 4 and 5 demonstrated that when the total blend amount of components (C-1) and (C-2) in component (C) and the blend amount of component (C-3) were not within the specified ranges, separation and sedimentation over time worsened, and caking was confirmed after leaving the composition to stand for one month.
[0082] The thermally conductive two-component addition-curable silicone composition of the present invention has excellent thermal conductivity, is easy to handle, has appropriate viscosity, and is low in abrasion. As a result, it can be used to dissipate heat and protect electronic components such as power devices, transistors, thyristors, CPUs (central processing units), and GPUs (graphics processing units), and is also expected to have the effect of reducing abrasion to coating equipment.
Claims
1. A thermally conductive two-part addition-curable silicone composition consisting of a first part and a second part, wherein the first part contains the following components (A), (C), (D), and (E) but does not contain component (B), and the second part contains the following components (A), (B), (C), and (D) but does not contain component (E). (A) an organopolysiloxane having at least two alkenyl groups bonded to silicon atoms in one molecule, (B) an organohydrogenpolysiloxane having at least two hydrogen atoms bonded to silicon atoms in one molecule, (C) an aluminum hydroxide powder (C-1) having an average particle size of 40 to 100 μm, an aluminum hydroxide powder (C-2) having an average particle size of 5 μm or more and less than 40 μm, and a thermally conductive filler (C-3) having an average particle size of 0.1 μm or more and less than 5 μm, wherein the total ratio of (C-1) and (C-2) in component (C) is 40 to 70 mass%, and the ratio of (C-3) in component (C) is 30 to 60 mass%: a thermally conductive two-part addition curable silicone composition comprising a first liquid and a second liquid together has a total of 90 to 95 mass% of component (C), (In the formula, R 1 are independently monovalent hydrocarbon groups; R 2 each independently represents an alkyl group, an alkoxyalkyl group, an alkenyl group, or an acyl group, a is 5 to 100, and b is 1 to 3; (E) a platinum catalyst for hydrosilylation reaction 2. A thermally conductive two-component addition curable silicone composition according to claim 1, wherein the content of component (D) is 10 to 500 parts by mass per 100 parts by mass of the total of components (A) and (B) in the entire thermally conductive two-component addition curable silicone composition consisting of the first and second components combined.
3. The thermally conductive two-part addition-curable silicone composition according to claim 1, wherein component (C-3) is aluminum oxide.
4. The thermally conductive two-part addition curable silicone composition according to claim 1, wherein the mass ratio of components (C-1) and (C-2) is 2:8 to 8:
2.
5. The thermally conductive two-component addition curable silicone composition according to claim 1, wherein the entire thermally conductive two-component addition curable silicone composition consisting of the first and second components combined contains 100 to 700 parts by mass of component (C-1), 50 to 500 parts by mass of component (C-2), and 150 to 800 parts by mass of component (C-3) per 100 parts by mass combined of components (A), (B), (D), and (E).
6. The density measured by the underwater displacement method specified in JIS K 6268 is 3.0 g / cm 3 2. The thermally conductive two-part addition curable silicone composition according to claim 1, wherein the composition has a thermal conductivity of 3.0 W / m·K or more as measured by a hot disk method in accordance with ISO 22007-2.
7. A cured product of the thermally conductive two-part addition curable silicone composition according to any one of claims 1 to 6.
8. A thermally conductive sheet comprising a cured product of the thermally conductive two-part addition curing type silicone composition according to any one of claims 1 to 6.
9. A method for producing the thermally conductive two-part addition curable silicone composition according to any one of claims 1 to 6, comprising the step of mixing (C-1), (C-2) and (C-3) above.
Citation Information
Patent Citations
Thermally conductive silicone composition
JP5940325B2
Thermally conductive silicone composition and thermally conductive silicone molding using the same
JP2011016923A
Heat conductive silicone composition and cured product of the same
JP2011089079A
Heat conductive silicone composition and cured product of the same
JP2011178821A
Heat-conductive silicone composition, heat-conductive silicone sheet, and method of manufacturing the same
JP2020002236A