Polyolefin-based resin foam particles and molded body of polyolefin-based resin foam particles
The incorporation of a specific NOR type hindered amine compound in polyolefin resin foam particles addresses the trade-off between moldability and flame retardancy, enabling the production of lightweight, mechanically sound, and flame-retardant foamed particle molded products for diverse applications.
Patent Information
- Application Number
- PCT/JP2024/018389
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-17
- Publication Date
- 2024-12-05
AI Technical Summary
Foamed polyolefin resin particles with added NOR type hindered amine compounds face a trade-off between maintaining good in-mold moldability and achieving stable flame retardancy, as increasing the amount of the flame retardant can compromise moldability, while a low amount may not ensure sufficient flame retardancy.
The use of polyolefin resin foam particles with a specific NOR type hindered amine compound, represented by general formula (I), within a content range of 0.01% to 3% by mass, which maintains excellent in-mold moldability and provides stable flame retardancy, even with a relatively large or small amount of the compound.
The approach allows for the production of foamed particle molded products with a balance of light weight, mechanical properties, and high flame retardancy, suitable for various applications such as vehicle parts and building materials, while preventing deterioration in moldability.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Expanded polyolefin resin beads and expanded polyolefin resin beads molded article
[0001] The present invention relates to expanded polyolefin resin beads containing a flame retardant and to an expanded polyolefin resin bead molding having excellent flame retardancy, which is obtained by molding the expanded polyolefin resin beads in a mold.
[0002] Expanded polyolefin resin bead moldings obtained by molding expanded polyolefin resin beads in a mold are used in various applications, such as packaging materials, vehicle components, and building materials. These expanded bead moldings may be colored with carbon black or the like. Furthermore, in order to make the expanded bead moldings less flammable, a NOR-type hindered amine compound may be added to the expanded polypropylene resin beads as a flame retardant (see, for example, Patent Document 1).
[0003] JP 2004-263033
[0004] Expanded bead moldings with reduced density and reduced weight, and expanded bead moldings containing a large amount of carbon material such as carbon black, tend to be more flammable. Therefore, in order to achieve the desired flame retardancy, it may be necessary to increase the amount of NOR hindered amine compound added to the expanded beads. However, for example, increasing the amount of NOR hindered amine compound described in Patent Document 1 could result in a decrease in the in-mold moldability of the expanded beads. That is, in order to maintain good in-mold moldability of the expanded beads, it is preferable to add a small amount of NOR hindered amine compound. However, when the amount of NOR hindered amine compound added to the expanded beads is kept small in consideration of the effect on in-mold moldability, etc., the expanded bead moldings produced using the expanded beads tend not to consistently exhibit the desired flame retardancy.
[0005] The present invention has been made in view of the above background, and provides expanded polyolefin resin beads that can be used to obtain expanded bead moldings that have excellent in-mold moldability and stably exhibit excellent flame retardancy, and an expanded polyolefin resin bead molding obtained by molding the expanded polyolefin resin beads in a mold.
[0006] The expanded polyolefin resin particles of the present invention have a bulk density of 10 kg / m 3 More than 100kg / m 3 The expanded polyolefin resin beads contain a NOR hindered amine compound, wherein the NOR hindered amine compound is represented by the following general formula (I), and the content of the NOR hindered amine compound in the expanded polyolefin resin beads is 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
[0007] The expanded polyolefin resin bead molding of the present invention has a density of 10 kg / m 3 More than 100kg / m 3 and a polyolefin resin foamed bead molding containing a NOR hindered amine compound, wherein the NOR hindered amine compound is represented by the following general formula (I), and the content of the NOR hindered amine compound in the polyolefin resin foamed bead molding is 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
[0008] According to the present invention, there are provided expanded polyolefin resin beads that have excellent in-mold moldability and can be used to obtain expanded bead moldings that stably exhibit excellent flame retardancy, and expanded polyolefin resin beads molded in-mold using the expanded polyolefin resin beads.
[0009] 1 is a DSC curve obtained according to the method for measuring the heat of transition of plastics described in JIS K7122 (1987) for determining the total heat of fusion and the heat of fusion of the high-temperature peak of the expanded polyolefin resin beads according to one embodiment of the present invention.
[0010] The expanded polyolefin resin beads of the present invention (hereinafter sometimes simply referred to as the expanded beads of the present invention) and the expanded polyolefin resin bead molded article of the present invention (hereinafter sometimes simply referred to as the expanded bead molded article of the present invention) will be described below. In the following description, preferred numerical ranges of the present invention may be indicated as appropriate. In this case, preferred ranges, more preferred ranges, and particularly preferred ranges regarding the upper and lower limits of the numerical ranges can be determined from all combinations of the upper and lower limits.
[0011] The expanded beads of the present invention have a bulk density of 10 kg / m 3 More than 100kg / m 3 and contains a NOR-type hindered amine compound represented by the following general formula (I): In the following description, the NOR-type hindered amine compound represented by the following general formula (I) may be referred to as a specific hindered amine compound. The content of the specific hindered amine compound in the expanded beads of the present invention is adjusted to 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
[0012] The expanded beads of the present invention having the above-described configuration are lightweight, excellent in-mold moldability, and also excellent in flame retardancy. Therefore, the expanded beads of the present invention can provide expanded bead moldings that have low density, excellent fusion between expanded beads, and consistently exhibit excellent flame retardancy. In other words, by using a specific hindered amine compound as a flame retardant, the present invention is less likely to reduce the moldability of the expanded beads even when a relatively large amount of flame retardant is added. Therefore, the present invention can provide polyolefin resin expanded beads that can provide expanded bead moldings exhibiting the desired flame retardancy. Furthermore, the present invention can provide expanded bead moldings exhibiting the desired flame retardancy even when a relatively small amount of flame retardant is added. Therefore, the present invention can provide polyolefin resin expanded beads in which the deterioration of moldability of the expanded beads due to the flame retardant is more suppressed. The expanded beads of the present invention are described in more detail below.
[0013] [Polyolefin Resin] The expanded beads of the present invention use a polyolefin resin as the base resin. In the present invention, the polyolefin resin refers to a homopolymer of an olefin monomer such as ethylene, propylene, butene, or pentene, or a copolymer containing 50 mol% or more of a component derived from an olefin monomer. The polyolefin resin may be composed of one type of polyolefin resin, or may be composed of a mixed resin of two or more types of polyolefin resins.
[0014] The polyolefin resin preferably contains a polyethylene resin and / or a polypropylene resin as its main component. More specifically, the sum of the proportion of the polypropylene resin and the proportion of the polypropylene resin in the polyolefin resin is preferably 60% by mass or more, more preferably 80% by mass or more. Furthermore, when the polyolefin resin contains a polypropylene resin as its main component, the proportion of the polypropylene resin in the polyolefin resin is preferably 60% by mass or more, more preferably 80% by mass or more. Examples of polyethylene resins include resins containing 50 mol% or more of ethylene component units, and specific examples include high-density polyethylene, low-density polyethylene, linear low-density polyethylene, very low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-methyl methacrylate copolymer, and ethylene-ethyl acrylate copolymer. Among these, from the viewpoint of being able to stably produce expanded beads with excellent in-mold moldability, it is preferable that the polyethylene resin contain linear low-density polyethylene as its main component. More specifically, the proportion of linear low-density polyethylene in the polyethylene resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more.
[0015] Furthermore, examples of polypropylene-based resins include resins containing 50 mol% or more of propylene component units. Specific examples include propylene homopolymers, impact-resistant polypropylenes commercially available as block polypropylenes in which a rubber component such as ethylene-propylene rubber is dispersed in polypropylene, propylene-ethylene random copolymers, propylene-ethylene block copolymers, propylene-butene random copolymers, propylene-butene block copolymers, and propylene-ethylene-butene random copolymers. Among these, from the viewpoint of being able to stably produce expanded beads with excellent in-mold moldability, it is preferable that the polypropylene-based resin contains propylene-ethylene random copolymers and / or propylene-ethylene-butene random copolymers as the main components. More specifically, the proportion of propylene-ethylene random copolymers and / or propylene-ethylene-butene random copolymers in the polypropylene-based resin is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 80% by mass or more.
[0016] From the viewpoint of obtaining an expanded bead molding that has an excellent balance between mechanical properties such as compressive strength and light weight and is particularly suitable for applications such as packaging materials, vehicle components, and building materials, it is preferable that the expanded beads in the present invention use a polypropylene-based resin as the base resin. In this case, the melting point of the polypropylene-based resin constituting the expanded beads is preferably 125°C or higher and 160°C or lower, more preferably 130°C or higher and 155°C or lower, and even more preferably 135°C or higher and 150°C or lower. By using a polypropylene-based resin having a melting point within this range as the base resin, it is possible to achieve a good balance between good in-mold moldability of the expanded beads and good compression properties of the expanded bead molding obtained by in-mold molding of the expanded beads.
[0017] The melting point of the polypropylene resin constituting the expanded beads is measured in accordance with JIS K 7121:2012. Specifically, the expanded beads are used as test specimens, and conditioning is performed in accordance with "(2) Measuring the melting temperature after a certain heat treatment" in "3. Conditioning of test specimens" in JIS K 7121:2012. In conditioning, the test specimen is heated from 23°C to 200°C at a heating rate of 10°C / min, maintained at 200°C for 10 minutes, and then cooled to 23°C at a cooling rate of 10°C / min. After conditioning the test specimen in this manner, the test specimen is again heated to 200°C at a heating rate of 10°C / min to obtain a DSC curve. The flow rate of nitrogen gas in the measurement environment is 30 mL per minute. The apex temperature of the melting peak appearing in the DSC curve obtained above is taken as the melting point of the polypropylene resin constituting the expanded beads. When a plurality of melting peaks appear on the DSC curve, the apex temperature of the melting peak having the highest height relative to the baseline is taken as the melting point of the polypropylene resin constituting the expanded beads.
[0018] In addition to the polyolefin-based resin, the expanded beads of the present invention may contain other resins or elastomers other than polyolefin-based resins, as long as the purpose and effects of the present invention are not impaired. Examples of resins other than polyolefin-based resins include thermoplastic resins such as polystyrene-based resins, vinyl acetate resins, thermoplastic polyester resins, acrylic ester resins, methacrylic ester resins, and polyarylene sulfide-based resins. Examples of the elastomers include olefin-based thermoplastic elastomers, styrene-based thermoplastic elastomers, and amide-based thermoplastic elastomers. Resins and elastomers other than olefin-based resins are preferably contained in an amount of 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the polyolefin-based resin. It is particularly preferred that the expanded beads of the present invention are substantially free of other resins or elastomers other than polyolefin-based resins.
[0019] [NOR-Type Hindered Amine Compound] The expanded beads of the present invention contain a NOR-type hindered amine compound represented by the following general formula (I) in a range of 0.01% by mass to 3% by mass. From the viewpoint of being able to exhibit flame retardancy that meets high standards, the expanded beads of the present invention preferably contain the specific hindered amine compound in a range of 0.02% by mass or more, and more preferably in a range of 0.03% by mass or more. Furthermore, from the viewpoint of being able to exhibit high flame retardancy and sufficiently excellent in-mold moldability, the expanded beads of the present invention preferably contain the specific hindered amine compound in a range of 2% by mass or less, and more preferably in a range of 1.5% by mass or less. That is, the expanded beads of the present invention preferably contain the specific hindered amine compound in a range of 0.02% by mass to 2% by mass, and more preferably in a range of 0.03% by mass to 1.5% by mass. When the expanded beads contain two or more specific NOR hindered amine compounds, the total content of these compounds is defined as the content of the specific NOR hindered amine compounds in the expanded beads. A hindered amine compound in which a nitrogen atom in a 2,2,6,6-tetramethyl-4-piperidine structure is bonded to a hydrocarbon group via an oxygen atom, as in the structure represented by the following general formula (I), is called a NOR hindered amine. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
[0020] The content of the NOR type hindered amine compound in the expanded beads can be determined, for example, by measuring the expanded beads using proton nuclear magnetic resonance ( 1 It can be determined by proton nuclear magnetic resonance ( 1When determining the content of the NOR-type hindered amine compound by H-NMR, for example, the following method can be used. First, the freeze-pulverized expanded particles are subjected to Soxhlet extraction using chloroform as a solvent to remove polymer components and the like that are insoluble in chloroform. Next, the chloroform-soluble portion obtained by Soxhlet extraction is mixed with acetone to remove the acetone-insoluble portion. A solid obtained by removing the solvent from the acetone-soluble portion is used as a measurement sample and subjected to proton nuclear magnetic resonance ( 1 The content of the NOR-type hindered amine compound in the expanded beads can be determined from the relationship between the measurement results and those of a standard sample (internal standard sample) with a known concentration. 1 As an apparatus for performing the measurement by H-NMR, for example, an AL-400 model manufactured by JEOL Ltd. can be used. In the measurement, the following measurement conditions can be adopted: solvent: CDCl3, internal standard sample: tetrachloroethane (TCE).
[0021] The specific hindered amine compound used in the present invention differs from other NOR-type hindered amine compounds conventionally used as flame retardants in that X in general formula (I) is an alkanolamine group. The reason why the use of a specific hindered amine compound as a flame retardant improves the flame retardancy of expanded beads while maintaining good in-mold moldability of the expanded beads is unclear. However, the reason why the above-described excellent effects of the present invention are exhibited is presumed to be as follows. That is, it is presumed that X in general formula (I) is an alkanolamine group, and that the —OH group in this X acts as a catalyst to form a synthetic intermediate of a non-flammable gas during combustion of the expanded beads (expanded bead molded article). Therefore, it is presumed that high flame retardancy is exhibited and good in-mold moldability is maintained even when the blending amount of the specific hindered amine compound is reduced. In the above X, the —OH group is brought close to the —NH group, which makes it easier to cause the above-mentioned catalytic action, and from the viewpoint of making it easier to obtain expanded beads that stably exhibit excellent flame retardancy, the number of carbon atoms in X in the above general formula (I) is preferably 1 or more and 8 or less, more preferably 1 or more and 6 or less, and even more preferably 1 or more and 4 or less.
[0022] From the viewpoint of being able to more stably obtain expanded beads that have good moldability in a mold and that exhibit flame retardancy that meets a high standard, R 1 and R 2 The number of carbon atoms in the hydrocarbon group of each of R is preferably 1 or more and 20 or less, more preferably 2 or more and 16 or less, and even more preferably 3 or more and 10 or less. 1 and R 2 From the same viewpoint, the hydrocarbon groups of R in the general formula (I) are preferably alkyl groups or cycloalkyl groups. 3 and R 4 The number of carbon atoms in the hydrocarbon group of each of R is preferably 1 or more and 20 or less, more preferably 2 or more and 10 or less, and even more preferably 3 or more and 8 or less. 3 and R 4The hydrocarbon groups in R in general formula (I) are preferably alkyl groups or cycloalkyl groups. It is more preferable that either of the following aspect 1 or aspect 2 is satisfied, and it is particularly preferable that both are satisfied. Aspect 1: 1 and R 2 and each represent a cyclohexyl group. 3 and R 4 are butyl groups.
[0023] In general formula (I), X is an alkanolamine group, which is a substituent having a hydroxy group and an amino group in an alkane skeleton. The specific hindered amine compound used in the present invention is preferably an ethanolamine group in which the alkane skeleton of X has two carbon atoms, and more preferably an ethanolamine group in which the alkane skeleton of X has two carbon atoms and satisfies the above aspects 1 and 2.
[0024] The melting point of the specific hindered amine compound is preferably 60°C or higher and 100°C or lower, more preferably 70°C or higher and 95°C or lower, and even more preferably 75°C or higher and 90°C or lower. When the melting point of the specific hindered amine compound is within the above range, the hindered amine compound can be easily dispersed well in the base resin, and expanded beads with excellent in-mold moldability can be stably obtained. Furthermore, in expanded bead moldings molded using the expanded beads thus obtained, the hindered amine compound tends to be less likely to migrate to the surface of the molding. As a result, expanded bead moldings that exhibit excellent flame retardancy over a long period of time can be stably obtained. Here, the melting point of the NOR hindered amine compound can be measured by "(1) Visual inspection" in "3. Melting point measurement method" of JIS K 0064:1992. It should be noted that the expanded beads can be measured by proton nuclear magnetic resonance ( 1 The structure of the NOR hindered amine compound contained in the expanded beads may be identified by subjecting the expanded beads to 1H-NMR or the like, and the melting point of the NOR hindered amine compound having such a structure may be measured, thereby determining the melting point of the NOR hindered amine compound contained in the expanded beads.
[0025] The molecular weight of the specific hindered amine compound is preferably 1000 or less, more preferably 900 or less. When the molecular weight of the specific hindered amine compound is within the above range, the hindered amine compound is likely to be well dispersed and present in the base resin, and expanded beads with excellent in-mold moldability can be stably obtained. The lower limit of the molecular weight is approximately 550, and preferably 600. Here, the molecular weight of the NOR type hindered amine compound can be determined as the sum of the atomic weights of the atoms constituting the NOR type hindered amine compound. When the expanded beads are analyzed by proton nuclear magnetic resonance ( 1 The structure of the NOR hindered amine compound contained in the expanded beads may be identified by subjecting the expanded beads to 1H-NMR or the like, and the molecular weight of the NOR hindered amine compound may be determined from the structure.
[0026] The expanded beads of the present invention contain one or more compounds selected from the specific hindered amine compounds represented by the general formula (I) as a flame retardant. Furthermore, the expanded beads of the present invention may contain, in addition to the specific hindered amine compound represented by the general formula (I), other flame retardants other than the specific hindered amine compound, as long as the purpose and effects of the present invention are not impaired. Examples of other flame retardants include NOR-type hindered amine flame retardants other than the specific hindered amine compound, halogen-based flame retardants, phosphorus-based flame retardants, and metal hydroxides. The amount of the flame retardant other than the specific hindered amine compound represented by the general formula (I) is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 20 parts by mass or less, and particularly preferably 10 parts by mass or less, per 100 parts by mass of the specific hindered amine compound in the expanded beads. It is particularly preferred that the expanded beads of the present invention are substantially free of flame retardants other than the specific hindered amine compound.
[0027] [Carbon Material] The expanded beads of the present invention may further contain a carbon material. Generally, expanded bead moldings obtained by molding expanded beads containing a carbon material in a mold tend to be highly flammable. However, the expanded beads of the present invention containing a specific hindered amine compound can exhibit excellent flame retardancy even when containing a carbon material. The amount of carbon material contained in the expanded beads of the present invention is not particularly limited, but from the viewpoint of easily exhibiting excellent flame retardancy, the content of the carbon material in the expanded beads is preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.5% by mass or more and 7% by mass or less, and even more preferably 1% by mass or more and 5% by mass or less.
[0028] Examples of the carbon material include at least one carbon powder selected from the group consisting of carbon black, carbon nanotubes, graphite, graphene, carbon nanofibers, carbon microfibers, carbon microcoils, and carbon nanocoils. Among these, the expanded beads of the present invention containing carbon black in an amount of 1% by mass to 10% by mass, more preferably 1% by mass to 5% by mass, are preferred because they can provide black expanded bead moldings that are excellent in flame retardancy, fusion, surface appearance, and recovery. The expanded beads of the present invention may contain one type of carbon material, or two or more types.
[0029] The carbon black includes gas furnace black, oil furnace black, acetylene black, channel black, roller black, thermal black, ketjen black, and the like.
[0030] The content of the carbon material in the expanded beads can be determined, for example, by a thermogravimetric differential thermal analyzer (i.e., TG-DTA). In this case, the expanded beads are first subjected to measurement based on JIS K7120-1987. Then, the content of the carbon material in the expanded beads can be determined based on the mass loss rate in a predetermined temperature range (e.g., from 400°C to 1000°C) of the TG curve obtained by the measurement.
[0031] [Other Additives] The expanded beads of the present invention may contain any additives within the scope of not impairing the purpose and effects thereof. Examples of the optional additives include one or more additives selected from the group consisting of a flame retardant aid, a cell regulator, a catalyst neutralizer, a lubricant, a crystal nucleating agent, an antistatic agent, a conductivity imparting agent, an antioxidant, an ultraviolet absorber, etc.
[0032] [Fusing Layer] The expanded beads of the present invention may have a fusing layer on their surface to facilitate fusing of the expanded beads together even at lower molding pressures during in-mold molding. The fusing layer may be present on the entire surface of the expanded beads, or on a portion of the surface. Polyolefin resins are preferably used as the resin constituting the fusing layer. Examples of polyolefin resins constituting the fusing layer include polyolefin resins having a melting point lower than that of the polyolefin resin constituting the expanded bead body (core layer), and polyolefin resins that have no melting point and have a softening point lower than that of the polyolefin resin constituting the expanded bead body (core layer). Regarding expanded beads having a fusing layer, the expanded bead body on which the fusing layer is provided may be referred to as the core layer. When the expanded beads have a fusing layer, the proportion of the fusing layer in the expanded beads is generally 0.5% by mass to 20% by mass, preferably 1% by mass to 10% by mass. Furthermore, when the expanded beads have a fusion layer whose base resin is a polyolefin resin having a melting point, the difference between the melting point of the polyolefin resin constituting the expanded bead body and the melting point of the polyolefin resin constituting the fusion layer is generally 1°C or more and 30°C or less, preferably 2°C or more and 25°C or less, and more preferably 5°C or more and 20°C or less. The method for forming the fusion layer on the surface of the expanded bead body is not particularly limited, and examples include a method of foaming resin beads having a fusion layer on their surface, and a method of obtaining expanded beads and then attaching a fusion layer to the surface of the expanded beads. When expanding resin beads having a fusion layer on their surface to obtain expanded beads, it is preferable to use a method in which, when producing resin beads, a molten mixture for forming the core layer and a molten resin for forming the fusion layer are co-extruded using an extrusion device capable of co-extrusion, thereby laminating a fusion layer on the surface of the resin beads.
[0033] [Bulk density of expanded beads] The bulk density of the expanded beads of the present invention is 10 kg / m 3 More than 100kg / m 3 The following is a summary. Generally, as the bulk density of expanded beads decreases, the amount of base resin constituting the expanded beads decreases, and therefore the burning rate of an expanded bead molding molded using expanded beads with a low bulk density tends to increase. However, the expanded beads of the present invention contain a specific hindered amine compound as a flame retardant. As a result, the present invention can adjust the bulk density of the expanded beads to the low range described above, while suppressing an increase in the burning rate of an expanded bead molding molded using the expanded beads. In other words, the expanded beads of the present invention can provide an expanded bead molding that is lightweight and exhibits excellent flame retardancy.
[0034] From the viewpoint of further improving the lightness of the foamed bead molding produced by molding the foamed beads of the present invention in a mold, the bulk density of the foamed beads is 80 kg / m 3 Preferably, it is 60 kg / m or less. 3 More preferably, it is 50 kg / m or less. 3 From the viewpoint of improving the mechanical properties such as compressive strength of the expanded bead molding produced by molding the expanded bead of the present invention in a mold, the bulk density of the expanded bead is more preferably 12 kg / m or less. 3 It is preferable that the viscosity is 15 kg / m or more. 3 More preferably, it is 18 kg / m or more. 3 In other words, the bulk density of the expanded beads of the present invention is 12 kg / m or more. 3 More than 80kg / m 3 It is preferable that the viscosity is 15 kg / m or less. 3 More than 60kg / m 3 More preferably, it is 18 kg / m or less. 3 More than 50kg / m 3 It is more preferable that:
[0035] The bulk density of the expanded beads described above is calculated by the following method. First, the expanded beads to be used for measurement are left to stand for 24 hours or more in an environment of 23°C temperature, 50% relative humidity, and 1 atm. The expanded beads thus obtained are filled into a measuring cylinder with a volume of 1 L or more to a bulk volume of 1 L or more. After the height of the filled expanded beads is stabilized, the bulk volume (unit: L) of the expanded beads is read from the scale of the measuring cylinder. The mass (unit: g) of the expanded beads in the measuring cylinder is then divided by the aforementioned bulk volume and converted into a unit to obtain the bulk density of the expanded beads (unit: kg / m). 3 ) can be obtained.
[0036] [Average Cell Diameter of Expanded Beads] The average cell diameter of expanded beads is preferably 50 μm or more and 250 μm or less, more preferably 55 μm or more and 200 μm or less, even more preferably 60 μm or more and 150 μm or less, and even more preferably 60 μm or more and 120 μm or less. When the average cell diameter of expanded beads is within the above range, expanded beads that exhibit good moldability in a mold and can be used to consistently produce expanded bead moldings exhibiting excellent flame retardancy can be obtained. The average cell diameter of expanded beads can be measured by drawing multiple lines from the outermost surface of an expanded bead through the center to the outermost surface on the opposite side in an enlarged photograph of the cross section of a bisected expanded bead, and dividing the number of cells intersecting each line by the total length of the lines. Specifically, it can be measured by the method described in the Examples.
[0037] [High-Temperature Peak of Expanded Beads] The expanded beads preferably have a crystalline structure in which one or more melting peaks appear higher than the peak of the melting peak inherent to the polyolefin resin in a DSC curve obtained by heat flux differential scanning calorimetry. The melting peak inherent to the polyolefin resin may also be referred to as an "intrinsic peak." The one or more melting peaks appearing higher than the peak of the inherent peak may also be referred to as "high-temperature peaks." By using expanded beads exhibiting high-temperature peaks for in-mold molding, molding conditions for molding an expanded bead molding can be selected from a wide range, and the mechanical properties of the resulting expanded bead molding, such as compressive strength, can be further improved. From this perspective, the heat of fusion of the high-temperature peak is preferably 5 J / g or more, more preferably 8 J / g or more. The heat of fusion of the high-temperature peak is preferably 50 J / g or less, more preferably 40 J / g or less. The heat of fusion of the high-temperature peak may also be referred to as the "high-temperature peak heat." The high-temperature peak calorific value is preferably 5 J / g or more and 50 J / g or less, and more preferably 8 J / g or more and 40 J / g or less.
[0038] The high-temperature peak calorific value of expanded beads can be calculated by the following method. First, a test piece of approximately 3 mg of expanded beads is used, and a DSC curve is obtained when the test piece is heated and melted according to the method for measuring the heat of transition of plastics specified in JIS K7122-1987. The temperature range of the DSC curve is from 23°C to a temperature 30°C higher than the temperature at the end of the melting peak, and the heating rate during heating is 10°C / min. The flow rate of nitrogen gas in the measurement environment is 30 mL per minute. When expanded beads have a high-temperature peak, the DSC curve will show an intrinsic peak a and a high-temperature peak b, which has a peak higher than the peak of intrinsic peak a, as shown in Figure 1. Note that Figure 1 is an example of a DSC curve measured by heat flux differential scanning calorimetry for expanded polyolefin resin beads. Although Figure 1 shows one high-temperature peak b, there may be two or more high-temperature peaks b.
[0039] Next, a line is drawn connecting point I on the DSC curve, which corresponds to 80°C, and point II, which corresponds to the melting end temperature of the expanded beads. The melting end temperature is the high-temperature end point of high-temperature peak b, i.e., the point on the DSC curve where high-temperature peak b returns to the high-temperature baseline.
[0040] Next, as shown in Figure 1, the intersection of a line passing through maximum point III between intrinsic peak a and high-temperature peak b and parallel to the vertical axis of the graph with a line connecting points I and II is designated as point IV. The area enclosed by the line connecting points I and IV, the line connecting points III and IV, and the DSC curve connecting points I and III is designated as the area of intrinsic peak a. The area enclosed by the line connecting points IV and II, the line connecting points III and IV, and the DSC curve connecting points III and II (shaded portion) is designated as the area of high-temperature peak b. The total heat of fusion of the expanded beads is calculated from the sum of the areas of intrinsic peak a and high-temperature peak b determined as described above, and the heat of fusion of high-temperature peak b is calculated from the area of high-temperature peak b.
[0041] In addition, if a DSC curve is obtained by the above-mentioned method, and then the expanded beads are cooled to 23°C at a cooling rate of 10°C / min and heated again at a heating rate of 10°C / min to obtain a DSC curve, only the intrinsic peak a appears in the DSC curve, and the high-temperature peak b disappears from the DSC curve.
[0042] [Polyolefin Resin Expanded Bead Molded Article] Next, the expanded bead molded article of the present invention will be described. The expanded bead molded article of the present invention has a molded article density of 10 kg / m 3 More than 100kg / m 3 and contains a NOR-type hindered amine compound (specific hindered amine compound) represented by the following general formula (I): The content of the specific hindered amine compound in the expanded bead molding is 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
[0043] The expanded bead molding of the present invention, which contains a specific hindered amine compound in a predetermined range of amount, is excellent in balance between light weight and mechanical properties such as compressive strength, and also in flame retardancy. Furthermore, the expanded bead molding of the present invention, produced by molding the expanded beads of the present invention in a mold, is also excellent in fusion property, surface appearance, and recovery property. Therefore, the expanded bead molding of the present invention can be suitably used for various applications such as vehicle components and building materials. The content of the NOR hindered amine compound in the expanded bead molding can be determined, for example, by subjecting the expanded bead molding to proton nuclear magnetic resonance ( 1 The amount of the carbon black can be determined by subjecting the carbon black to spectroscopy (H-NMR) or the like.
[0044] As described above, the density of the expanded bead molding of the present invention is 10 kg / m 3 More than 100kg / m 3 From the viewpoint of achieving a balance between light weight and mechanical properties such as rigidity, and also ensuring flame retardancy, the density is 12 kg / m 3 More than 80kg / m 3 It is preferable that the viscosity is 15 kg / m or less. 3 More than 60kg / m 3 More preferably, it is:
[0045] The density of the expanded bead molding is calculated by dividing the mass of the expanded bead molding by the volume calculated based on the outer dimensions.
[0046] <Flame Retardancy> The flame retardancy of an expanded bead molding can be evaluated based on the position at which combustion ends, the duration of combustion, and the burning distance when a flammability test is carried out in accordance with Federal Motor Vehicle Safety Standard (FMVSS) No. 302. The flammability test method specified in FMVSS No. 302 is specifically as follows.
[0047] First, the expanded beads are molded in a mold, and then the resulting expanded bead molding is cut to prepare a plate-shaped test piece. The test piece is then left for 24 hours in an environment at a temperature of 21°C and a relative humidity of 50% to condition the test piece. After conditioning, a start line is drawn on the test piece at a position 38 mm away from the base end in the longitudinal direction, and an end line is drawn at a position 292 mm away from the base end. The test piece is then attached to the U-shaped frame of a chamber dedicated to FMVSS No. 302.
[0048] Next, the burner is ignited, and the amounts of gas and air are adjusted so that the flame height is 38 mm. In this state, the burner is moved so that the center of the tip of the burner is at the center of the width direction at the base end of the test piece, and the burner flame is brought into contact with the test piece for 15 seconds. Thereafter, the burner flame is removed from the test piece, and the combustion duration is measured from the time the test piece's combustion position reaches the start line until the combustion ends.
[0049] In the present invention, the flame retardancy of an expanded bead molding is evaluated in terms of self-extinguishing property and average burning rate. Specifically, if the test specimen does not ignite, if the burning of the test specimen ends before reaching the initiation line, or if the burning of the test specimen ends within 51 mm from the initiation line and the burning duration is within 60 seconds, the expanded bead molding is judged to have self-extinguishing property. Furthermore, if the test specimen does not have the aforementioned self-extinguishing property, the burning rate is determined by dividing the burning distance from the initiation line by the burning duration. If the burning of the test specimen reaches the end line, the burning rate is determined by dividing the burning distance from the initiation line to the end line by the burning duration from the initiation line to the end line. Ten or more test specimens are prepared, and the burning rates are determined for each specimen. The arithmetic mean of these values is used as the average burning rate.
[0050] As a result of conducting a flammability test specified in FMVSS (Federal Motor Vehicle Safety Standard) No. 302, the burning rate is preferably 102 mm / min or less, more preferably less than 80 mm / min, and even more preferably exhibits self-extinguishing properties. Expanded bead moldings evaluated as having more favorable or even more favorable flammability are suitable for applications requiring particularly high flame retardancy. In particular, expanded bead moldings having self-extinguishing properties are suitable for use as vehicle components, such as automobile bumpers and seat cores.
[0051] The expanded bead molding of the present invention is preferably produced, for example, by in-mold molding of the expanded beads of the present invention. The expanded bead molding of the present invention produced by in-mold molding of the expanded beads of the present invention enjoys the excellent effects of the expanded beads of the present invention described above. For example, the expanded bead molding of the present invention may be produced by in-mold molding of the black expanded beads of the present invention. In this case, the expanded bead molding will not only be black but also exhibit good flame retardancy. From this perspective, when the expanded bead molding contains a carbon material, the content of the carbon material in the expanded bead molding is preferably 0.1% by mass to 10% by mass, more preferably 0.5% by mass to 7% by mass, and even more preferably 1% by mass to 5% by mass. Furthermore, when the expanded bead molding contains carbon black, the content of the carbon black in the expanded bead molding is preferably 1% by mass to 10% by mass, and even more preferably 1% by mass to 5% by mass.
[0052] [Method for Producing Expanded Polyolefin Resin Beads] The method for producing expanded beads of the present invention is not particularly limited as long as it can produce expanded beads having a specific NOR hindered amine compound content within a specific range. Examples of the production method include a method of expanding resin beads containing a specific NOR hindered amine compound and a method of impregnating expanded beads with a specific NOR hindered amine compound. A preferred embodiment of the method for producing expanded beads of the present invention will now be described. The expanded beads of the present invention can be obtained by expanding polyolefin resin beads containing a blowing agent. For example, the expanded beads can be produced by a production method including an expansion step in which polyolefin resin particles containing a blowing agent are released from a pressure vessel together with an aqueous medium under a pressure lower than the pressure inside the pressure vessel to expand them. The polyolefin resin particles contain a polyolefin resin as a base resin. Furthermore, the resin particles preferably contain a specific NOR hindered amine compound.
[0053] In the above-described production method, the expanded particles obtained in the expansion step may be used as expanded particles as they are. Alternatively, as will be described later, the expanded particles obtained in the expansion step may be used as first-stage expanded particles, and the first-stage expanded particles may be used to produce expanded particles by performing a second-stage expansion step. From the viewpoint of obtaining expanded particles with a lower bulk density, it is preferable to perform the second-stage expansion step after the expansion step.
[0054] <Granulation step> The method for producing expanded beads preferably includes a granulation step, prior to the expansion step, in which polyolefin resin particles containing a specific NOR hindered amine compound are produced using a polyolefin resin as a base resin. Hereinafter, the polyolefin resin particles produced in the granulation step will also be simply referred to as resin particles. The method for producing the resin particles in the granulation step is not particularly limited. For example, the polyolefin resin and the specific NOR hindered amine compound are extruded while being kneaded by extrusion molding to produce strands, and the strands are then cut to the desired size using a pelletizer or the like, thereby obtaining the resin particles.
[0055] In the foaming step, resin particles are first supplied into a pressure vessel and dispersed in an aqueous dispersion medium such as water. If necessary, a dispersant, a dispersion aid, a surfactant, or the like may be added to disperse the resin particles in the dispersion medium in the pressure vessel.
[0056] As the dispersant, inorganic fine particles such as aluminum oxide, tricalcium phosphate, magnesium pyrophosphate, zinc oxide, kaolin, mica, etc. can be used. These inorganic fine particles may be used alone or in combination of two or more. As the dispersing aid, for example, aluminum sulfate can be used. Furthermore, as the surfactant, for example, anionic surfactants such as sodium alkylbenzenesulfonate, sodium dodecylbenzenesulfonate, sodium alkanesulfonate, etc. can be used. These surfactants may be used alone or in combination of two or more.
[0057] After sealing the pressure vessel, a foaming agent is added to the vessel. This allows the resin particles to be impregnated with the foaming agent. At this time, the impregnation of the resin particles with the foaming agent can be promoted by heating the inside of the pressure vessel. Alternatively, resin particles that have already been impregnated with the foaming agent may be supplied to the pressure vessel.
[0058] After the resin particles are impregnated with a predetermined amount of blowing agent, the contents of the pressure vessel are released under a pressure lower than the pressure inside the pressure vessel, thereby expanding the resin particles to obtain expanded particles (first-stage expanded particles).
[0059] Any additives such as carbon black can be blended into the resin particles by, for example, kneading them with the base resin in the granulation step.
[0060] Examples of blowing agents used in the foaming step include organic physical blowing agents such as hydrocarbons and halogenated hydrocarbons, and inorganic physical blowing agents such as carbon dioxide, nitrogen, air, and water. Examples of hydrocarbons that can be used as organic physical blowing agents include butane, pentane, and hexane. Examples of halogenated hydrocarbons that can be used as organic physical blowing agents include trichlorofluoromethane, dichlorofluoromethane, and tetrachlorodifluoroethane. As the organic physical blowing agent, the aforementioned substances may be used alone or in combination of two or more. Similarly, as the inorganic physical blowing agent, the aforementioned substances may be used alone or in combination of two or more.
[0061] In the production of expanded beads of the present invention, the blowing agent is preferably an inorganic physical blowing agent, more preferably carbon dioxide. By expanding resin beads using such a blowing agent, expanded beads that can ultimately be used to produce expanded bead moldings with a high expansion ratio and excellent flame retardancy can be easily obtained. Furthermore, since carbon dioxide is non-flammable, using carbon dioxide as the blowing agent can avoid deterioration in the flame retardancy of the expanded bead moldings caused by the blowing agent.
[0062] The amount of foaming agent added can be appropriately set depending on the type of base resin, the type of foaming agent, the desired bulk density of the expanded beads, etc. For example, when carbon dioxide is used as the foaming agent, the amount added is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 15 parts by mass or less, and even more preferably 1 part by mass or more and 10 parts by mass or less, per 100 parts by mass of the resin particles.
[0063] The expansion step may include a step of generating the aforementioned high-temperature peak before expanding the resin particles. A method for generating the high-temperature peak can be, for example, a method of heat-treating resin particles in a pressure vessel while maintaining the resin particles in a dispersion medium within a specific temperature range. The timing of the heat treatment is not particularly limited, and the heat treatment may be performed before, during, or after the impregnation with the blowing agent, or may be performed across two or more of the aforementioned points. This heat treatment can produce expanded beads having a crystalline structure that exhibits a melting peak (intrinsic peak) derived from the crystals inherent to the polyolefin resin and a melting peak (high-temperature peak) located at a higher temperature than the intrinsic peak. Here, the heat treatment can be, for example, a temperature-holding step in which a predetermined temperature is maintained for a predetermined time during a temperature-raising step in which the temperature inside the pressure vessel is increased after the resin particles are introduced into the pressure vessel.
[0064] <Second-Stage Expansion Step> The production method may further include a second-stage expansion step. The second-stage expansion step is carried out, for example, by pressurizing a pressure-resistant container filled with the first-stage expanded beads obtained in the expansion step with air or the like, impregnating the first-stage expanded beads with air or the like to increase the pressure in the cells, and then heating the pressurized first-stage expanded beads to expand them. The heating of the expanded beads in the second-stage expansion step may be carried out in a pressure-resistant container whose pressure is adjusted, or may be carried out after removing them from the pressure-resistant container and under a pressure lower than the pressure in the cells. The first-stage expanded beads used in the second-stage expansion step are preferably those that have been cured at atmospheric pressure after the expansion step is completed.
[0065] In the above-described manufacturing method, by expanding resin particles in two stages, the expansion stage and the second-stage expansion stage, low-density expanded particles can be more easily obtained. Although the two-stage expansion stage has been described here, the expanded particles obtained by the second-stage expansion stage may be further subjected to a three-stage or more expansion stage.
[0066] In this specification, the container used in the foaming step is referred to as a "pressure vessel" and the container used in the second-stage foaming step is referred to as a "pressure-resistant vessel", but either of them may be a container that can be sealed and to which pressure can be applied.
[0067] [Method for producing a foamed bead molded article of polyolefin resin] The method for producing a foamed bead molded article of the present invention is not particularly limited as long as it can produce a foamed bead molded article having the above-described configuration. For example, a preferred embodiment of the method for producing a foamed bead molded article of the present invention is in-mold molding using the foamed beads of the present invention described above. The in-mold molding widely includes known in-mold molding methods using foamed beads. For example, the in-mold molding of the foamed bead molded article of the present invention can be carried out as follows.
[0068] First, the expanded beads of the present invention are filled into a mold having a cavity corresponding to the shape of the desired expanded bead molded article, and the expanded beads filled in the mold are heated by applying a predetermined molding pressure using a heating medium such as steam. Heating the expanded beads in the cavity in this manner further expands them and fuses them together. After heating with steam or the like is completed, the pressure is released, and cooling of the mold and the molded article within the mold is quickly initiated. Cooling is then terminated when it is confirmed that the pressure (surface pressure) generated on the inner surface of the mold has fallen below a predetermined value. The mold is then opened, and the expanded bead molded article is removed from the mold. The cooling method used here is not particularly limited, but examples include water cooling. This series of molding steps results in an expanded bead molded article corresponding to the shape of the cavity.
[0069] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. Tables 1 and 2 show the NOR hindered amine compounds used and the content (% by mass) of the NOR hindered amine compounds relative to 100% by mass of the expanded beads.
[0070] Example 1 Granulation Process A polypropylene resin, carbon black, a NOR-type hindered amine compound, and a cell control agent were fed into an extruder and extruded while kneading them together to produce strands containing these. The resulting strands were then cut using a pelletizer to obtain resin particles with a length-to-diameter ratio (length / diameter) of 2.0 and an average mass of 1.0 mg. The polypropylene resin used was a propylene-ethylene random copolymer with a melting point of 143°C and a melt flow rate of 7 g / 10 min at 230°C and a load of 2.16 kg. Furnace black was used as the carbon black, and was added so that the carbon black content in the expanded particles was 3% by mass. The NOR hindered amine compound used was a compound having the structure of general formula (I) above and showing the structure of chemical formula (II) below (product name: Tinuvin 152, manufactured by BASF, melting point 83°C, molecular weight 757). The NOR hindered amine compound was added so that the content in the expanded beads would be the value shown in Table 1. Zinc borate powder was used as the cell regulator and was added so that the content in the expanded beads would be 0.05% by mass.
[0071] <Foaming Process> A 5 L autoclave (pressure vessel) was charged with 0.3 parts by mass of dispersant, 0.01 parts by mass of dispersant aid, 0.004 parts by mass of surfactant, and 300 parts by mass of dispersion medium per 100 parts by mass of resin particles. The dispersant was kaolin, the dispersion aid was aluminum sulfate, the surfactant was sodium dodecylbenzenesulfonate, and the dispersion medium was water. Next, carbon dioxide was supplied as a foaming agent into the autoclave, and the autoclave was pressurized to a gauge pressure of 1.0 MPa (G). Thereafter, the autoclave was heated to 144°C at a heating rate of 2°C / min while stirring. After the temperature inside the autoclave reached 144°C, this temperature was maintained for 15 minutes while continuing to stir. Next, the autoclave was heated to 149°C at a heating rate of 2°C / min while stirring. After the temperature inside the autoclave reached 149°C, carbon dioxide was supplied into the autoclave to adjust the pressure inside the autoclave to 2.7 MPa (G), while maintaining the temperature at 149°C for 15 minutes. Thereafter, the autoclave was opened and the contents were released under atmospheric pressure. In this way, the resin particles were expanded to a bulk density of 45 kg / m 3 In this specification, the unit of pressure with (G) means gauge pressure, that is, a pressure value based on atmospheric pressure.
[0072] <Second-Stage Expansion Step> The first-stage expanded particles obtained in the expansion step were left to cure for 24 hours in an environment of 23°C, 50% relative humidity, and 1 atm, and then the cured first-stage expanded particles were packed into a pressure vessel. Air was then injected into the pressure vessel, and the pressure in the pressure vessel was increased from atmospheric pressure to 0.60 MPa (G) over 24 hours. This pressure was maintained for 24 hours, allowing the air to penetrate into the cells. The first-stage expanded particles removed from the pressure vessel were then packed into a second-stage expansion machine, and steam was supplied at a pressure of 0.15 MPa (G) to further expand the first-stage expanded particles, yielding second-stage expanded particles. Table 1 shows the bulk density, average cell diameter, and heat of fusion of the high-temperature peak of the obtained second-stage expanded particles.
[0073] The bulk density of the second-stage expanded beads was measured according to the method for measuring the bulk density of expanded beads described above. Specifically, the expanded beads were first left for 24 hours or more in an environment of 23°C temperature, 50% relative humidity, and 1 atm. The expanded beads thus obtained were filled into a graduated cylinder graduated with 1 L markings, and the bottom of the graduated cylinder was lightly tapped on the floor several times to stabilize the expanded beads filled in the graduated cylinder so that the height position of the expanded beads was at the 1 L mark. The mass (unit: g) of the expanded beads thus obtained in the graduated cylinder with a bulk volume of 1 L was measured, and the bulk density (unit: kg / m) of the expanded beads was determined by unit conversion. 3 ) was calculated. The heat of fusion of the high-temperature peak of the second-stage expanded beads was measured according to the method for measuring the heat of fusion of high-temperature peak b described above. The average cell diameter of the second-stage expanded beads was measured as follows: First, 30 expanded beads were randomly selected. Each expanded bead was cut through its center to divide it into two, and an enlarged photograph of one cross section was taken. In each cross-sectional photograph, four line segments were drawn from the outermost surface of the expanded bead through the center to the outermost surface on the opposite side, so that the angles between adjacent two line segments were equiangular. The number of cells intersecting each line segment was counted, and the average cell diameter of each expanded bead was determined by dividing the total length of the four line segments by the total number of cells intersecting the lines. The average cell diameter of each expanded bead was then determined by arithmetically averaging the average cell diameter values of each expanded bead.
[0074] <In-mold molding> The two-stage expanded beads obtained by the above method were filled into a mold capable of molding a flat plate 350 mm long, 250 mm wide, and 50 mm thick, and heated using the following heating method to produce an expanded bead molded article. First, steam was supplied to the mold with the drain valves on both sides of the mold open to perform preheating (exhaust process). Steam was then supplied from one side of the mold to heat it, and then steam was supplied from the other side to heat it. Subsequently, steam was supplied from both sides of the mold at a predetermined molding pressure (molding steam pressure) to heat it (main heating). After the main heating was completed, the pressure was released, and the mold was water-cooled until the pressure generated on the molding surface of the mold was 0.04 MPa (G). The mold was then opened, and the expanded bead molded article was removed. The resulting molded article was cured in an oven at 80°C for 12 hours to obtain an expanded bead molded article. The molding pressure range of the expanded beads was evaluated using the following method.
[0075] (Molding Pressure Range (Range of Molding Steam Pressures Capable of Molding Good Products)) Expanded bead moldings were molded using the in-mold molding method described above, with the molding pressure during in-mold molding being changed in increments of 0.01 MPa. The resulting expanded bead moldings were evaluated for fusion, surface appearance, and recovery, as described below. The molding pressure (molding steam pressure) during in-mold molding that allowed for molding an expanded bead molding that passed all three of the criteria listed below was confirmed, and the range from the lower limit to the upper limit of the molding steam pressure was defined as the molding pressure range. This confirmed the in-mold moldability of the expanded beads used. Note that the wider the range from the lower limit to the upper limit of the molding steam pressure that allows for molding an expanded bead molding that meets the pass criteria, the wider the range of molding steam pressures that allows for molding good products, and is therefore more preferable. Furthermore, the lower the lower limit of the molding steam pressure that allows for molding good products, the more productive the molding process is, since good expanded bead moldings can be obtained even at low molding steam pressures. The range from the lower limit to the upper limit of the molding steam pressure (molding pressure range) at which an expanded bead molding that meets the acceptance standard can be molded is preferably 0.02 MPa or more, more preferably 0.03 MPa or more, and even more preferably 0.04 MPa or more.
[0076] Weldability: The obtained foamed bead molding was bent and broken, and the number of foamed beads present on the fracture surface (C1) and the number of broken foamed beads (C2) were determined. The ratio of the number of broken foamed beads to the total number of foamed beads (C2 / C1) × 100 was calculated as the material failure rate. The measurement was carried out five times using different test pieces, and the material failure rates were calculated for each. The arithmetic mean of the material failure rates was 80% or more, which was considered to be acceptable, and that of less than 80% was considered to be unacceptable.
[0077] Surface appearance: A 100 mm × 100 mm square was drawn in the center of the obtained foamed bead molding, a line was drawn diagonally from one corner of the square, and the number of voids (gaps) of 1 mm × 1 mm or more on the line was counted. A molding with fewer than 5 voids was rated as pass, and any other molding was rated as fail.
[0078] Recovery: The thickness of each of the four corners and the center of a flat expanded bead molding obtained by in-mold molding, measuring 350 mm in length, 250 mm in width, and 50 mm in thickness, was measured. The "near the four corners" refers to the area 10 mm inward from the corner of the expanded bead molding toward the center of the plate surface. The "center" refers to the intersection of a line dividing the expanded bead molding in half longitudinally and a line dividing the expanded bead molding in half transversely. The ratio (%) of the thickness of the center to the thickness of the thickest point near the four corners was then calculated. A ratio of 95% or more was considered acceptable, and a ratio of less than 95% was considered unacceptable.
[0079] (Density) In-mold molding was performed at the lowest molding pressure within the molding pressure range described above to obtain an expanded bead molding. This expanded bead molding was dried in an environment of 80°C for 24 hours, and then the mass (unit: g) of the expanded bead molding was measured. Thereafter, the mass of the expanded bead molding was divided by the volume (unit: L) calculated from the external dimensions of the expanded bead molding, and the density of the molding (unit: kg / m) was calculated by converting the unit. 3 ) was calculated.
[0080] (50% Compression Strength) In-mold molding was performed at the lowest molding pressure within the molding pressure range described above to obtain an expanded bead molding. This expanded bead molding was dried for 24 hours in an environment of 80°C, and then a rectangular parallelepiped test piece measuring 50 mm in length, 50 mm in width, and 25 mm in thickness was taken from the center of the expanded bead molding. A compression test was performed on the test piece at a compression rate of 10 mm / min based on the method specified in JIS K7220:2006, and a stress-strain curve was obtained. The compression test was performed in a laboratory at 23°C. Based on this stress-strain curve, the 50% deformation compressive stress of the test piece was calculated, and this value was used as the 50% compression strength of the molding.
[0081] (FMVSS Test) Flame retardancy was evaluated by a method conforming to the flammability test method specified in FMVSS (Federal Motor Vehicle Safety Standard) No. 302. Specifically, the foamed bead molding was first cut to prepare a test specimen having a plate shape of 350 mm in length, 102 mm in width, and 12.7 mm in thickness, with one of the sides bounded by a 350 mm long side and a 102 mm wide side being a skin surface. A start line was drawn on this test specimen at a position 38 mm away from the base end in the longitudinal direction, and an end line was drawn at a position 292 mm away from the base end. Using this test specimen, a flammability test was performed using the same method as FMVSS No. 302, with the skin surface in contact with the burner flame.
[0082] Average Burning Rate and Self-Extinction Rate: The FMVSS test was performed 10 times, and the average burning rate and self-extinguishing rate were calculated based on the test results. The average burning rate was determined by arithmetically averaging the burning rates measured for each test piece. The burning rate of the test piece was calculated using the following formula (1): [Mathematical Formula 1] B = 60 × D / T (1)
[0083] In the above formula (1), the symbol B represents the burning rate (unit: mm / min), the symbol D represents the distance the flame has traveled (unit: mm), and the symbol T represents the time (unit: seconds) required for the flame to travel D mm. If the test specimen self-extinguished, the burning rate was treated as 0 mm / min. Here, the test specimen was judged to have self-extinguished if "the test specimen did not ignite," "the burning of the test specimen finished before reaching the position where the burning time measurement started (i.e., the above-mentioned start line)" or "the burning of the test specimen finished within 60 seconds after reaching the position where the burning time measurement started, and the distance from the measurement start position to the position where the burning finished was within 51 mm."
[0084] The self-extinguishing rate was calculated by dividing the number of tests that were rated as "self-extinguishing" by the number of tests (10), and expressing the result as a percentage.
[0085] (Examples 2 to 4) First-stage expanded beads and second-stage expanded beads were produced in the same manner as in Example 1, except that the content of the NOR-type hindered amine compound in the expanded beads was changed to the value shown in Table 1. These second-stage expanded beads were used to perform in-mold molding in the same manner as in Example 1 to obtain expanded bead moldings. These were designated Examples 2 to 4, respectively.
[0086] Example 5 First-stage expanded beads and second-stage expanded beads were produced in the same manner as in Example 1, except that resin beads produced by the following method were used. These second-stage expanded beads were used to perform in-mold molding in the same manner as in Example 1 to obtain expanded bead moldings. The polypropylene resin, carbon black, NOR-type hindered amine compound, and cell regulator used in Example 5 to form the core layer were the same as those used in Example 1.
[0087] First, a manufacturing apparatus was prepared, which included an extruder for forming a core layer, a die for forming a multilayer strand attached downstream of the extruder for forming the core layer, and an extruder for forming a fusion layer. The downstream side of the extruder for forming the fusion layer was connected to the die for forming a multilayer strand, and the manufacturing apparatus was configured to enable lamination of the resin melts for forming each layer within the die and to enable co-extrusion.
[0088] As the core layer forming materials, polypropylene resin, carbon black, a specific NOR hindered amine compound, and a cell regulator were fed to a core layer forming extruder and melt-kneaded to form a polypropylene resin melt. At this time, the amounts of each material were adjusted so that the core layer of the resulting expanded beads had a carbon black content of 3% by mass, a specific NOR hindered amine compound content of 0.1% by mass, and a cell regulator content of 0.05% by mass. As the fusion layer forming materials, polypropylene resin, carbon black, and a specific NOR hindered amine compound were fed to a fusion layer forming extruder and melt-kneaded to form a polypropylene resin melt. At this time, the amounts of each material were adjusted so that the fusion layer of the resulting expanded beads had a carbon black content of 3% by mass and a specific NOR hindered amine compound content of 0.1% by mass. The polypropylene resin used to form the adhesive layer was a propylene-ethylene-butene random copolymer having a melting point of 133° C. and a melt flow rate of 6 g / 10 min at 230° C. and a load of 2.16 kg.
[0089] The resin melts for forming each layer formed as described above were introduced into a multilayer strand forming die and merged within the die, and a multilayer strand having a two-layer structure was extruded from the holes in the die attached downstream of the die. The two-layer structure refers to a structure of a fusion layer / core layer. The extruded strand was water-cooled and cut using a pelletizer to obtain polypropylene resin particles with a length / diameter ratio of 2.0 and an average mass of 1.0 mg. The mass ratio of the core layer to the fusion layer was core layer / fusion layer = 95 / 5.
[0090] Example 6 First-stage expanded beads and second-stage expanded beads were produced in the same manner as in Example 1, except that carbon black was not used. These second-stage expanded beads were used to carry out in-mold molding in the same manner as in Example 1 to obtain an expanded bead molding, which was designated Example 6.
[0091] Example 7 The first-stage expanded beads prepared in the manufacturing process of Example 1 were used to carry out in-mold molding in the same manner as in Example 1 to obtain an expanded bead molding.
[0092] Comparative Examples 1 to 4 First-stage expanded beads and second-stage expanded beads were produced in the same manner as in Example 1, except that the NOR-type hindered amine compound used was changed as shown in Table 2. These second-stage expanded beads were used to perform in-mold molding in the same manner as in Example 1 to obtain expanded bead molded articles. These were designated Comparative Examples 1 to 4. In Comparative Examples 1 to 4, a NOR-type hindered amine compound not having the structure of general formula (I) described above was used. Specifically, the NOR hindered amine compound used in Comparative Examples 1 and 2 was "trade name: NOR116FF, manufactured by BASF Corporation, melting point 108°C, molecular weight 2261," the NOR hindered amine compound used in Comparative Example 3 was "trade name: EVERSORB95, manufactured by Everlight Chemical Corporation, liquid at room temperature, molecular weight 737," and the NOR hindered amine compound used in Comparative Example 4 was a polymeric hindered amine compound, "trade name: NOR371FF, manufactured by BASF Corporation, melting point 91°C, molecular weight 2800 to 4000."
[0093] For Examples 2 to 7 and Comparative Examples 1 to 4, the high-temperature peak heat of fusion, bulk density, and average cell diameter of the expanded beads were measured, and the density, molding pressure range, and 50% compression strength of the expanded bead-like molded articles were measured, and the FMVSS test was also carried out, in the same manner as in Example 1. In Example 7, the two-stage expansion step was not carried out, and therefore, first-stage expanded beads were used for the above-mentioned measurements.
[0094]
[0095]
[0096] The present invention described above encompasses the following technical concepts: (1) A bulk density of 10 kg / m 3 More than 100kg / m 3 The expanded polyolefin resin beads contain a NOR hindered amine compound, wherein the NOR hindered amine compound is represented by the following general formula (I), and the content of the NOR hindered amine compound in the expanded polyolefin resin beads is 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2, R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group. (2) The expanded polyolefin resin beads according to (1) above, wherein the NOR hindered amine compound has a melting point of 60°C or higher and 100°C or lower. (3) The expanded polyolefin resin beads according to (1) or (2) above, wherein the NOR hindered amine compound has a molecular weight of 1,000 or lower. (4) The expanded polyolefin resin beads according to any one of (1) to (3) above, wherein X in general formula (I) is an ethanolamine group. (5) The expanded polyolefin resin beads according to any one of (1) to (4) above, wherein the expanded polyolefin resin beads further contain a carbon material. (6) The expanded polyolefin resin beads having a density of 10 kg / m 3 More than 100kg / m 3 1. A foamed polyolefin resin bead molding containing a NOR hindered amine compound, wherein the NOR hindered amine compound is represented by the following general formula (I), and the content of the NOR hindered amine compound in the foamed polyolefin resin bead molding is 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
Claims
1. Bulk density is 10 kg / m 3 More than 100kg / m 3 The expanded polyolefin resin beads contain a NOR type hindered amine compound, the NOR type hindered amine compound being represented by the following general formula (I), and the content of the NOR type hindered amine compound in the expanded polyolefin resin beads is 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
2. The expanded polyolefin resin particles according to claim 1, wherein the melting point of the NOR type hindered amine compound is 60°C or higher and 100°C or lower.
3. The expanded polyolefin resin particles according to claim 1 or 2, wherein the molecular weight of the NOR type hindered amine compound is 1,000 or less.
4. The expanded polyolefin resin particles according to any one of claims 1 to 3, wherein X in the general formula (I) is an ethanolamine group.
5. The expanded polyolefin resin particles according to any one of claims 1 to 4, further comprising a carbon material.
6. Density is 10 kg / m 3 More than 100kg / m 3 1. An expanded polyolefin resin bead molding containing a NOR type hindered amine compound, wherein the NOR type hindered amine compound is represented by the following general formula (I), and the content of the NOR type hindered amine compound in the expanded polyolefin resin bead molding is 0.01% by mass or more and 3% by mass or less. (In general formula (I), R 1 , R 2 , R 3 and R 4 each independently represents a hydrocarbon group, and X represents an alkanolamine group.
Citation Information
Patent Citations
In-mold foam molding of polyolefin-based resin
JP2004263033A
Laminate and decorative sheet
JP2019030998A
Method for producing polypropylene-based resin foam particle, and method for producing polypropylene-based resin in-mold foam molded body
JP2022135455A
Polypropylene resin foamed particle, method for producing polypropylene resin foamed particle, and molded body of polypropylene resin foamed particle
JP2023025507A