Thermally conductive silicone composition and cured product

The thermally conductive silicone composition, featuring phenyl-modified organopolysiloxane and thermally conductive fillers, addresses the limitations of existing materials by providing a heat-resistant and chemically resistant heat dissipation solution with high thermal conductivity for use in ATF environments.

WO2024247771A1PCT designated stage expired Publication Date: 2024-12-05SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/018422
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current heat dissipation materials, such as general-purpose silicone and fluororubber, face challenges in chemical resistance and thermal conductivity, particularly in environments with organic solvents like ATF, where they may swell or deteriorate, and have high viscosity issues when increasing thermal filler content.

Method used

A thermally conductive silicone composition comprising phenyl-modified organopolysiloxane, organohydrogenpolysiloxane, hydrolyzable organopolysiloxane, thermally conductive fillers, a platinum group metal catalyst, and a hydrosilylation reaction control agent, which forms a cured product with excellent heat resistance and chemical resistance, and high thermal conductivity.

Benefits of technology

The composition achieves high thermal conductivity and chemical resistance, enabling effective heat dissipation in organic solvent environments like ATF, while maintaining workability and processability, and exhibits minimal volume change and hardness retention under heat and chemical exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024018422_05122024_PF_FP_ABST
    Figure JP2024018422_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention pertains to: a thermally conductive silicone composition in which a hydrolyzable organopolysiloxane represented by general formula (1) is added to a component (C); and a cured product. Consequently, a thermally conductive silicone composition and a cured product are provided. (In the formula, R1s are independently a C6-C10 monovalent aromatic hydrocarbon group, R2s are independently a C1-C10 alkyl group, and R3 is a C1-C4 alkyl group. a is 2 or 3, m is an integer of 1≤m≤30, and n is an integer of 0≤n≤60, where the range of 3≤m+n≤90 is satisfied. The bonds of the siloxane units in parentheses in general formula (1) may be a block or may be random.)
Need to check novelty before this filing date? Find Prior Art

Description

Thermally conductive silicone composition and cured product

[0001] The present invention relates to a thermally conductive silicone composition and a cured product thereof.

[0002] The performance of electronic components, such as highly integrated circuits like CPUs, is significantly degraded by heat generation during use. To solve this problem, heat-dissipating materials are used, which improve heat transfer efficiency when introduced into the air gap between the heat-generating and cooling components. Silicone heat-dissipating materials, in particular, are used in a wide range of fields due to their high heat resistance, weather resistance, and electrical insulation properties inherent to silicone. In addition, as electronic devices have become increasingly miniaturized and highly integrated in recent years, it is important to more efficiently cool the generated heat, which has led to a demand for heat-dissipating materials with high thermal conductivity.

[0003] In recent years, there has been an increasing use of automotive heat-dissipating materials in oils containing chemicals, such as automatic transmission fluid (ATF), which is a lubricant for engine gears. Therefore, heat-dissipating materials are required to have chemical resistance. However, general-purpose silicone (dimethyl silicone) heat-dissipating materials have the problem of being prone to swelling and degradation in organic solvent environments such as ATF. Furthermore, ATF is often heated to high temperatures, so heat resistance as well as ATF resistance is required.

[0004] As a chemical-resistant heat-dissipating material, a heat-dissipating material using fluororubber, which has a perfluoropolyether structure in the main chain and is a mixture of thermally conductive fillers, has been proposed (Patent Documents 1 to 3). However, this fluororubber has a lower thermal conductivity than dimethyl silicone. When an attempt is made to compensate for this by increasing the thermally conductive filler loading, the composition does not become grease-like or becomes highly viscous, resulting in poor workability and processability. Furthermore, this heat-dissipating material has a high specific gravity and is expensive, so there is a need to develop a new heat-dissipating material that can replace it and has chemical resistance.

[0005] Compared to dimethylsilicone, phenylsilicone has a greater affinity for aromatic solvents such as benzene and toluene, but a lower affinity for saturated hydrocarbons such as automatic transmission fluid (ATF). Phenylsilicone also has a thermal conductivity comparable to that of dimethylsilicone. Furthermore, phenylsilicone is known to have higher heat resistance because it is less susceptible to oxidative degradation than dimethylsilicone (Patent Documents 4 and 5). Therefore, by incorporating phenylsilicone into a heat-dissipating material, it is possible to provide a heat-dissipating material that also has chemical resistance.

[0006] However, a dispersant (wetter) for phenylsilicone and thermally conductive filler has not yet been developed, and there has been little research into compositions using phenylsilicone and their cured products.

[0007] JP 2015-67736 A JP 2015-67737 A JP 2017-082090 A JP 2007-039621 A JP 2004-262919 A

[0008] An object of the present invention is to provide a thermally conductive silicone composition and cured product that exhibit excellent heat resistance and chemical resistance.

[0009] The present invention has been made to solve the above problems, and provides the following thermally conductive silicone composition and cured product.

[0010] That is, the present invention provides a thermally conductive silicone composition comprising the following components (A) to (F): (A) a silicone oil having two or more alkenyl groups per molecule and a kinematic viscosity at 25°C of 100 to 100,000 mm 2 / s: 100 parts by mass; (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups: an amount such that the number of moles of hydrosilyl groups in component (B) is 0.1 to 3 moles per mole of alkenyl groups in component (A); (C) a compound represented by the following general formula (1): (In the formula, R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonding of the siloxane units enclosed in parentheses in general formula (1) may be block or random.) 10 to 300 parts by mass of a hydrolyzable organopolysiloxane represented by the formula (I): (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides: 10 to 97% by mass based on the total mass of the composition; (E) a platinum group metal catalyst: 0.1 to 500 ppm by mass, calculated as platinum group metal atoms, based on the mass of component (A); and (F) a hydrosilylation reaction inhibitor: 0.05 to 5 parts by mass.

[0011] Such a thermally conductive silicone composition can yield a cured product that has excellent heat resistance and chemical resistance.

[0012] The component (C) is preferably represented by the following general formula (2). (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bonding of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bonding of two types of siloxane units enclosed in parentheses with x forms a block polymer.

[0013] Such hydrolyzable organopolysiloxanes have high solubility in phenyl-modified silicones.

[0014] R shown in the above general formula (1) 1 is a phenyl group, and R 2 is preferably a methyl group.

[0015] From the viewpoint of synthesis of hydrolyzable organopolysiloxane, these groups are preferred.

[0016] The thermally conductive silicone composition preferably has an absolute viscosity at 23°C of 1 to 1,000 Pa·s.

[0017] If the absolute viscosity at 23°C of the thermally conductive silicone composition is within the above range, it will be excellent in terms of workability and processability.

[0018] The present invention also provides a thermally conductive silicone cured product obtained by curing the above thermally conductive silicone composition.

[0019] Such thermally conductive silicone cured products are excellent in terms of heat resistance and chemical resistance.

[0020] In this case, the thermally conductive silicone cured product is characterized by having a thermal conductivity of 1.0 W / m·K or higher.

[0021] A thermally conductive silicone cured product that has heat resistance, chemical resistance, and good thermal conductivity can be used as a heat dissipation material in an organic solvent environment such as ATF.

[0022] The thermally conductive silicone composition and cured product of the present invention can be highly thermally conductive with excellent heat resistance and chemical resistance. In particular, the cured product of the thermally conductive silicone composition of the present invention can be used even in environments containing organic solvents such as ATF.

[0023] The present invention is described in detail below, but is not limited to these. As a result of extensive research conducted by the present inventors to achieve the above-mentioned object, they have completed a thermally conductive silicone composition and a cured product thereof that combines heat resistance and chemical resistance by adding a hydrolyzable organopolysiloxane having a specific structure to a thermally conductive silicone composition, which acts as a dispersant (wetter) for the phenylsilicone and thermally conductive filler.

[0024] That is, the present invention provides a thermally conductive silicone composition comprising the following components (A) to (F): (A) a silicone oil having two or more alkenyl groups per molecule and a kinematic viscosity at 25°C of 100 to 100,000 mm 2 / s: 100 parts by mass; (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups: an amount such that the number of moles of hydrosilyl groups in component (B) is 0.1 to 3 moles per mole of alkenyl groups in component (A); (C) a compound represented by the following general formula (1): (In the formula, R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonding of the siloxane units enclosed in parentheses in the above general formula (1) may be block or random.) 10 to 300 parts by mass of a hydrolyzable organopolysiloxane represented by the following formula: (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides: 10 to 97% by mass based on the entire composition; (E) a platinum group metal catalyst: 0.1 to 500 ppm by mass, calculated as platinum group metal atoms, based on the mass of component (A); and (F) a hydrosilylation reaction inhibitor: 0.05 to 5 parts by mass. It is particularly preferred that the component (C) is a hydrolyzable organopolysiloxane represented by the following general formula (2). (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bonding of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bonding of two types of siloxane units enclosed in parentheses with x forms a block polymer.

[0025] The present invention will be described in detail below. In the following, the endpoints of a range of values ​​include all values ​​within that range.

[0026] [(A) Phenyl-modified organopolysiloxane] Component (A) has two or more, preferably 2 to 10, and more preferably 2 to 5 alkenyl groups in the molecule, and has a kinematic viscosity at 25°C of 100 to 100,000 mm 2 The phenyl-modified organopolysiloxane is a phenyl-modified organopolysiloxane having the formula:

[0027] The main chain is generally composed of diorganosiloxane units, but may also have a partially branched structure or may be a cyclic organopolysiloxane. From the viewpoint of the physical properties of the cured product, however, a linear organopolysiloxane is preferred.

[0028] The alkenyl group is preferably an alkenyl group having 2 to 8 carbon atoms, more preferably 2 to 6 carbon atoms. Examples include vinyl, allyl, propenyl, isopropenyl, butenyl, hexenyl, cyclohexenyl, and octenyl groups. Vinyl groups are particularly preferred. The alkenyl group may be bonded to a silicon atom at the terminal of the molecular chain, a silicon atom in the middle of the molecular chain, or both.

[0029] The phenyl-modified organopolysiloxane of component (A) preferably has 0.00001 to 0.01 mol / g, and especially 0.0001 to 0.01 mol / g, of alkenyl groups per molecule.

[0030] Component (A) is also characterized by having phenyl groups. The amount of phenyl groups in one molecule is preferably 10 to 80%, more preferably 20 to 60%, of the number of siloxane units containing phenyl groups per total siloxane units. If the amount of phenyl groups in one molecule is 10% or more of the total siloxane units, compatibility with component (C) will not be significantly reduced. Furthermore, if the amount of phenyl groups in one molecule is 80% or less of the total siloxane units, the viscosity of the composition will not increase more than necessary.

[0031] Furthermore, from the viewpoint of viscosity, the groups other than the alkenyl group and the phenyl group are preferably alkyl groups having 1 to 18 carbon atoms, preferably 1 to 10 carbon atoms, and more preferably 1 to 8 carbon atoms. Examples include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl groups. These alkyl groups in which some of the hydrogen atoms have been substituted with halogen atoms may also be used. As the alkyl group, a methyl group is particularly preferred.

[0032] The phenyl-modified organopolysiloxane of component (A) has a kinematic viscosity at 25°C of 100 to 100,000 mm 2 In the present invention, the kinematic viscosity is a value measured by an Ostwald viscometer described in JIS Z8803:2011. The kinematic viscosity is preferably 300 to 20,000 mm 2 / s, and more preferably 500 to 10,000 mm 2 / s. The kinematic viscosity is 100 mm 2 If the kinematic viscosity is less than 100,000 mm / s, the phenyl modification rate becomes too small, which is not preferable. 2 If the ratio exceeds 1 / s, the composition becomes difficult to handle, which is not preferred. The phenyl-modified organopolysiloxane may be used alone or in combination of two or more kinds.

[0033] Examples of such component (A) include phenyl-modified organopolysiloxanes having a kinematic viscosity at 25°C of 100 to 100,000 mm, such as those represented by the following formula: 2 and dimethylsiloxane-diphenylsiloxane copolymers having both molecular chain terminals blocked with dimethylvinylsiloxy groups, which are represented by the formula (I) / s.

[0034] [(B) Organohydrogenpolysiloxane] Component (B) is an organohydrogenpolysiloxane having two or more hydrosilyl groups per molecule, preferably 2 to 50, more preferably 2 to 20, and even more preferably 2 to 10 hydrosilyl groups.

[0035] Any compound that can undergo an addition reaction with the alkenyl group of the component (A) in the presence of the platinum group metal catalyst (E) described below to form a crosslinked structure can be used.

[0036] The molecular structure of the organohydrogenpolysiloxane is not particularly limited as long as it has the above properties, and examples thereof include a linear structure, a branched structure, a cyclic structure, and a linear structure having a partially branched or cyclic structure. A linear structure or a cyclic structure is preferred. The organohydrogenpolysiloxane preferably has a kinematic viscosity at 25°C of 1 to 1,000 mm 2 / s, more preferably 10 to 100 mm 2 / s. The kinematic viscosity is 1 mm 2 / s or more, there is no risk of the physical properties of the silicone composition being reduced, and 2 If the viscosity is 1 / s or less, there is no risk of the silicone composition having poor extensibility.

[0037] The organic group bonded to the silicon atom of the organohydrogenpolysiloxane preferably contains a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms, and preferably does not contain a hydrosilylation-reactive group such as an alkenyl group or an alkynyl group. Furthermore, the group other than the monovalent aromatic hydrocarbon group is preferably an alkyl group, preferably an alkyl group having 1 to 12 carbon atoms, and more preferably an alkyl group having 1 to 10 carbon atoms. Examples include methyl, ethyl, propyl, butyl, hexyl, and dodecyl groups. These alkyl groups in which some of the hydrogen atoms have been substituted with halogen atoms may also be used. Among these, methyl groups are preferred. The organohydrogenpolysiloxane may be used alone or in combination of two or more types.

[0038] Examples of such component (B) include a methylhydrogensiloxane-diphenylsiloxane copolymer capped at both molecular chain terminals with trimethylsiloxy groups, such as the phenyl-modified organohydrogenpolysiloxane represented by the following formula, and a dimethylsiloxane-methylhydrogensiloxane-diphenylsiloxane copolymer capped at both molecular chain terminals with trimethylsiloxy groups.

[0039] The amount of organohydrogenpolysiloxane in component (B) is such that the ratio of the number of hydrosilyl groups in component (B) to the total number of alkenyl groups in component (A) is 0.1 to 3, preferably 0.7 to 3, and more preferably 1 to 2. If the amount of component (B) is less than the above-mentioned lower limit, the addition reaction will not proceed sufficiently, resulting in insufficient crosslinking. If the amount exceeds the above-mentioned upper limit, the crosslinked structure may become non-uniform and the stability of the composition over time may deteriorate.

[0040] [(C) Hydrolyzable Organopolysiloxane] Component (C) acts as a dispersant (wetter) for the phenylsilicone and thermally conductive filler, and is a hydrolyzable organopolysiloxane represented by the following formula (1). (In the formula, R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonding of the siloxane units enclosed in parentheses in the above general formula (1) may be block or random.

[0041] In the above general formula (1), R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms. 1 Specific examples of include aryl groups such as phenyl, tolyl, xylyl, and mesityl, with the phenyl group being preferred.

[0042] In the above general formula (1), R 2 are independently alkyl groups having 1 to 10 carbon atoms, preferably 1 to 5 carbon atoms, and more preferably 1 to 3 carbon atoms. 2 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a tert-butyl group, a pentyl group, a hexyl group, an octyl group, a nonyl group, and a decyl group, and among these, a methyl group is preferred.

[0043] In the above general formula (1), R 3 are independently an alkyl group having 1 to 4 carbon atoms, and are preferably a methyl group or an ethyl group. 3 Examples of a include methyl, ethyl, propyl, isopropyl, butyl, and tert-butyl groups. Of these, methyl is particularly preferred from the viewpoint of the hydrolysis property of the organopolysiloxane compound of the present invention. In addition, in the above general formula (1), a is 2 or 3, but from the viewpoint of ease of synthesis and economic efficiency, a is preferably 3.

[0044] In the general formula (1), m is typically an integer satisfying 1≦m≦30, preferably 3≦m≦20, and more preferably 5≦m≦18. If m exceeds 30, the viscosity of the organopolysiloxane increases significantly, which is undesirable. Furthermore, in the general formula (1), n ​​is typically an integer satisfying 0≦n≦60, preferably 5≦n≦50, and more preferably 10≦n≦40. Outside the above range, compatibility with the phenyl-modified silicone decreases, which is undesirable. Furthermore, m+n satisfies 3≦m+n≦90, and preferably 6≦m+n≦60. Outside the above range, the composition becomes difficult to handle, which is undesirable.

[0045] The component (C) of the present invention is preferably a hydrolyzable organopolysiloxane having a block structure represented by the following general formula (2). (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bonding of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bonding of two types of siloxane units enclosed in parentheses with x forms a block polymer.

[0046] Examples of such component (C) include hydrolyzable organopolysiloxanes such as dimethylsiloxane-diphenylsiloxane copolymers terminated at one molecular chain end with a trimethoxysiloxy group, as shown in the following formula:

[0047] The blend amount of component (C) is 10 to 300 parts by mass, preferably 15 to 200 parts by mass, and more preferably 20 to 100 parts by mass per 100 parts by mass of component (A). A blend amount of component (C) less than 10 parts by mass is undesirable because it makes it difficult to highly fill the thermally conductive silicone cured product with thermally conductive filler. A blend amount of more than 300 parts by mass is also undesirable because it significantly increases the viscosity of the thermally conductive silicone composition.

[0048] [(D) Thermally Conductive Filler] Component (D) is one or more thermally conductive fillers selected from the group consisting of metal oxides, metal hydroxides, and metal nitrides. Examples include alumina, zinc oxide, magnesium oxide, aluminum oxide, silicon dioxide, cerium oxide, iron oxide, aluminum hydroxide, cerium hydroxide, aluminum nitride, and boron nitride. These fillers can be used alone or in combination of two or more. A combination of particles with different average particle sizes, i.e., a combination of large particle components and small particle components, is preferred. Any two or more types of particles with different average particle sizes can be combined, preferably two, three, or four types of particles with different average particle sizes. Combining particles with different average particle sizes allows for optimal adjustment of the viscosity, processability, uniformity, and other properties of the resulting composition. Hereinafter, when component (D) is a combination of particles with different average particle sizes, the portion composed of components with an average particle size of less than 10 μm will be referred to as the small particle component, and the portion composed of components with an average particle size larger than the average particle size of any of the small particle components will be referred to as the large particle component.

[0049] If the average particle size of the large particle component is 0.1 μm or more, the viscosity of the resulting composition will not increase and the processability will not decrease.If the average particle size of the large particle component is 100 μm or less, the resulting composition will not become non-uniform and there will be no risk of oil bleeding.Therefore, the range of 0.1 to 100 μm, preferably 10 to 75 μm, is preferred.

[0050] Furthermore, if the average particle size of the small particle component (smaller than the average particle size of the large particle component) is 0.01 μm or more, the viscosity of the resulting composition will not increase and the processability will not decrease. On the other hand, if it is 10 μm or less, the resulting composition will not be non-uniform, so the range of 0.01 μm or more and less than 10 μm, preferably 0.1 to 4 μm, is preferable.

[0051] The ratio of large particle components to small particle components is not particularly limited, but when the large particle components have an average particle size of 10 μm or more (preferably 10 μm to 75 μm) and the small particle components have an average particle size of less than 10 μm (preferably 0.01 μm to 10 μm), the ratio of the large particle components to the small particle components is preferably in the range of 9:1 to 1:9 (mass ratio). The shapes of the large particle components and the small particle components are not particularly limited, and may be spherical, irregular, acicular, or the like. The large particle components are preferably spherical, and the small particle components are preferably spherical or irregular. Even if the small particle components have an irregular shape, they can fill the voids between the large particles. The average particle size can be determined, for example, as the volume-based average (or median) diameter in particle size distribution measurement by laser diffraction, and can be determined using a commercially available laser diffraction particle size distribution analyzer such as the MT3000II particle size distribution analyzer (manufactured by Microtrac Bell Corporation).

[0052] The blending amount of component (D) is 10 to 97% by mass, preferably 20 to 95% by mass, more preferably 30 to 95% by mass, and even more preferably 50 to 95% by mass, based on the total mass of the composition. If it is more than 97% by mass, the viscosity of the composition increases and processability decreases. If it is less than 10% by mass, thermal conductivity decreases.

[0053] [(E) Platinum Group Metal Catalyst] Component (E) is a platinum group metal catalyst that functions to promote the addition reaction between the above-mentioned components (A) and (B). Any conventionally known platinum group metal catalyst used in addition reactions can be used. Examples include platinum-based, palladium-based, and rhodium-based catalysts, with platinum or platinum compounds being preferred, as they are relatively readily available. Examples include platinum itself, platinum black, chloroplatinic acid, platinum-olefin complexes, platinum-alcohol complexes, and platinum coordination compounds. Platinum group metal catalysts may be used singly or in combination of two or more.

[0054] The amount of component (E) to be blended is 0.1 to 500 ppm, preferably 1 to 200 ppm, by mass, calculated as platinum group metal atoms relative to the mass of component (A). If the amount of catalyst is less than the lower limit, the catalytic effect may not be obtained. On the other hand, if the amount exceeds the upper limit, the catalytic effect will not increase and it is uneconomical, so it is not preferred.

[0055] [(F) Hydrosilylation Reaction Inhibitor] Component (F) is a reaction inhibitor that suppresses the progress of the hydrosilylation reaction at room temperature and is added to extend shelf life and pot life. This reaction inhibitor can be any known inhibitor used in addition-curable silicone compositions. Examples of such reaction inhibitors include acetylene compounds such as acetylene alcohols (e.g., 3-methyl-1-tridecyn-3-ol, 1-ethynyl-1-cyclohexanol, 3,5-dimethyl-1-hexyn-3-ol), various nitrogen compounds such as tributylamine, tetramethylethylenediamine, and benzotriazole, organophosphorus compounds such as triphenylphosphine, oxime compounds, and organochloro compounds.

[0056] The amount of component (F) blended is 0.05 to 5 parts by mass, and preferably 0.1 to 1 part by mass. If the amount of reaction retarder is less than 0.05 parts by mass, the desired shelf life and pot life may not be achieved, while if it is more than 5 parts by mass, the curability of the silicone composition may decrease.

[0057] Manufacturing Process of Thermally Conductive Silicone Composition A manufacturing method of the thermally conductive silicone composition of the present invention will now be described. The manufacturing method of the thermally conductive silicone composition of the present invention is not particularly limited. Examples of methods include mixing the above-mentioned components (A) to (F) using a mixer such as a rotation-revolution mixer (product name: Awatori Rentaro, manufactured by THINKYO Corporation), a Trimix, a Twinmix, or a Planetary Mixer (all manufactured by Inoue Seisakusho Co., Ltd.), an Ultramixer (Mizuho Kogyo Co., Ltd.), or a Hivis Dispermix (Tokushu Kika Kogyo Co., Ltd.). All of the components to be mixed may be mixed at once, or one or more components may be mixed in several stages. In the present invention, it is preferred to first mix components (A), (C), and (D) at room temperature, and then mix components (E), (B), and (F).

[0058] The phenyl silicone composition of the present invention preferably has an absolute viscosity measured at 23°C of 1 to 1,000 Pa·s, more preferably 20 to 700 Pa·s, and even more preferably 50 to 500 Pa·s. If the absolute viscosity is 1 Pa·s or higher, there is no risk of workability being impaired, such as difficulty in maintaining shape. Furthermore, if the absolute viscosity is 1,000 Pa·s or lower, there is no risk of processability being impaired. The above viscosity can be obtained by adjusting the blending amounts of each of the above-mentioned components. Note that, in the present invention, the absolute viscosity is a value measured using a viscosity / viscoelasticity measuring device. For example, a MARS40 manufactured by Thermo Fisher Scientific Co., Ltd. can be used as the measuring device, and the measurement conditions are 23°C, using parallel plates, a gap of 0.5 mm, and a rotation speed of 10 s. -1 The absolute viscosity can be determined by measuring the viscosity at 1000 kJ / cm2.

[0059] Manufacturing Process for Cured Thermally Conductive Silicone Products The thermally conductive silicone composition of the present invention can be cured by heating typically at 50 to 180°C, preferably 80 to 150°C, and more preferably 100 to 120°C. A cured product of any shape can be obtained by molding the thermally conductive silicone composition of the present invention using a desired method. While there are no particular limitations on the molding method, for example, a cured thermally conductive silicone product can be obtained by pouring the thermally conductive silicone composition prepared in the above-described composition manufacturing process into a mold, sandwiching the mold opening between two sheets of fluorine-treated PET film, and then curing for 10 minutes at 110°C using a press molding machine.

[0060] Thermal Conductivity of Cured Thermally Conductive Silicone Product The thermal conductivity of the cured thermally conductive silicone product of the present invention is 1.0 W / m K or more, preferably 2.0 W / m K or more. Since a higher thermal conductivity is preferable, no upper limit can be determined, but it can be set to, for example, 20 W / m K or less. In the present invention, the thermal conductivity is a value measured by the hot disc method in accordance with ISO 22007-2. This value can be measured, for example, using a hot disc method thermal property measuring device TPS series (such as the TPS 2500S) manufactured by Kyoto Electronics Manufacturing Co., Ltd.

[0061] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0062] Preparation of Thermally Conductive Silicone Composition The components (A) to (F) used in the following examples are shown below. Me represents a methyl group, and Ph represents a phenyl group. In the following formulas, the bonds of the siloxane units enclosed in parentheses may be either block or random. Siloxane units enclosed in square brackets are block polymers. The kinematic viscosity is the value measured at 25°C using an Ostwald viscometer as described in JIS Z8803:2011.

[0063] (A) Component A-1: ​​Represented by the following formula, kinematic viscosity of 700 mm 2 ・s -1 Phenyl-modified organopolysiloxane A-2: Represented by the following formula, kinematic viscosity is 600 mm2 ・s ―1 Organopolysiloxane

[0064] (B) Component B-1: A component having a kinematic viscosity of 20 mm 2 ・s -1 Phenyl-modified organohydrogenpolysiloxane B-2: A kinematic viscosity of 19 mm2, as represented by the following formula: 2 ・s -1 Phenyl-modified organohydrogenpolysiloxane B-3: A kinematic viscosity of 5 mm, represented by the following formula: 2 ・s -1 Organohydrogenpolysiloxane

[0065] Component (C) C-1: Hydrolyzable organosiloxane represented by the following formula: C-2: Hydrolyzable organosiloxane represented by the following formula: C-3: Decyltrimethoxysilane represented by the following formula C-4: Phenyltrimethoxysilane represented by the following formula

[0066] Component (D) The filler particle size (average particle size) of component (D) was measured using a particle size distribution measuring device MT3000II (manufactured by Microtrac Bell Co., Ltd.). D-1: Spherical alumina powder (median diameter: 70 μm) D-2: Spherical alumina powder (median diameter: 45 μm) D-3: Spherical alumina powder (median diameter: 10 μm) D-4: Irregular alumina powder (median diameter: 2 μm)

[0067] Component (E): 5% chloroplatinic acid solution in 2-ethylhexanol

[0068] Component (F): 3-methyl-1-tridecyn-3-ol

[0069] [Manufacturing Method] Components (A), (C), and (D) were mixed as follows to obtain compositions of Examples and Comparative Examples. The plastic containers containing components (A), (C), and (D) were placed in a rotation-revolution mixer (trade name: Awatori Rentaro, manufactured by THINKY Corporation) in the composition ratios (parts by mass) shown in Tables 1 and 2, and mixed at room temperature at 2,000 rpm for 1 minute twice. The resulting mixture was then cooled to room temperature. Component (E) was then added, and the mixture was mixed at 2,000 rpm for 30 seconds twice. The resulting mixture was then cooled to room temperature. A mixture of components (B) and (F) was then added, and the mixture was mixed at 2,000 rpm for 10 seconds twice. The mixture was then cooled to room temperature and degassed using a vacuum pump.

[0070] [Molding method] The prepared thermally conductive silicone composition was poured into a mold measuring 60 mm × 60 mm × 6 mm or 190 mm × 140 mm × 2 mm, the mold opening was sandwiched between two sheets of fluorine-treated PET film, and then the composition was cured in a press molding machine at 110°C for 10 minutes to obtain a cured thermally conductive silicone product.

[0071] [Evaluation Method] [Absolute Viscosity] The obtained composition was measured using a viscosity / viscoelasticity measuring device (trade name: MARS40 (Thermo Fisher Scientific Co., Ltd.)) at a rotation speed of 10 s -1 The measurement conditions were 23°C, parallel plates were used, and the gap was 0.5 mm.

[0072] [Thermal Conductivity] Using two 6 mm thick sheets molded in Examples 1 to 3 and Comparative Examples 1 to 4 below, the thermal conductivity of the cured product was measured with a thermal conductivity meter (TPS 2500S, manufactured by Kyoto Electronics Manufacturing Co., Ltd.) (hot disk method in accordance with ISO 22007-2).

[0073] [Hardness] The hardness of the cured thermally conductive silicone was measured using a durometer (Type A) hardness tester specified in JIS K6253-3: 2012. For products with measured values ​​of less than 20, the hardness was measured using a durometer (Asker C) hardness tester measured in accordance with the method described in Appendix 2 of JIS K7312: 1996.

[0074] [Heat Resistance Test] A 6 mm thick sheet was aged at 180° C. After aging for 90 hours, the sheet was returned to room temperature, and the hardness before and after aging was measured.

[0075] [Chemical Resistance Test] A 2 mm thick, 40 × 40 mm sheet was immersed in a genuine TOYOTA ATF and aged at 150° C. After aging for 250 hours, the sheet was removed from the ATF, and the volume change rate was calculated from the changes in mass and density before and after aging.

[0076] The evaluation results are shown in Tables 1 and 2.

[0077]

[0078] The thermally conductive silicone cured products in Examples 1 to 3, in which the component (C) used was a phenyl-modified hydrolyzable organosiloxane corresponding to the general formula (1) above, had a thermal conductivity of 2.0 W / m·K or higher, and showed almost no change in hardness in a heat resistance test at 180°C. Furthermore, despite the high loading of thermally conductive filler in Examples 2 and 3, the inclusion of the component (C) of the present invention suppressed increases in the viscosity of the composition and the hardness of the cured product, achieving high thermal conductivity. On the other hand, when a hydrolyzable dimethylorganosiloxane (C-2) was used as component (C), as in Comparative Example 1, it was found that a stable cured product could not be obtained. This is thought to be due to the low compatibility between the phenyl-modified organopolysiloxane of component (A) and the dimethylorganosiloxane (C-2), which resulted in separation of (C-2) in the composition. Furthermore, when decyltrimethoxysilane (C-3) or phenyltrimethoxysilane (C-4) was used as component (C), as in Comparative Examples 2 and 3, the hardness after the heat resistance test increased significantly. This is believed to be due to the low molecular weight and high volatility of (C-3) and (C-4). Furthermore, the cured product using the phenyl-modified silicone composition in Example 1 exhibited a volume change of approximately -4% after a 250-hour ATF resistance test. This differs from the result of a cured product using a dimethylsilicone elastomer, as in Comparative Example 4, which swelled by 2.6% under the same conditions. Furthermore, the volume change of the cured product using the phenyl-modified silicone composition after this ATF resistance test showed almost no difference depending on the component (C), which is believed to be a property unique to the phenyl-modified silicone composition. From these results, the thermally conductive silicone cured product of the present invention exhibits relatively high ATF resistance and also has a thermal conductivity of 4.0 W / m·K or greater. Therefore, the thermally conductive silicone composition and cured product of the present invention can be used as a new heat-dissipating material with chemical resistance.

[0079] This specification encompasses the following aspects: [1]: A thermally conductive silicone composition comprising the following (A) to (F): (A) a silicone rubber having two or more alkenyl groups per molecule and a kinematic viscosity at 25°C of 100 to 100,000 mm 2 / s: 100 parts by mass; (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups: an amount such that the number of moles of hydrosilyl groups in component (B) is 0.1 to 3 moles per mole of alkenyl groups in component (A); (C) a compound represented by the following general formula (1): (In the formula, R 1 are independently monovalent aromatic hydrocarbon groups having 6 to 10 carbon atoms, and R 2 are independently alkyl groups having 1 to 10 carbon atoms, and R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonding of the siloxane units enclosed in parentheses in general formula (1) above may be block or random.) 10 to 300 parts by mass of a hydrolyzable organopolysiloxane represented by the formula: (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides: 10 to 97% by mass of the entire composition; (E) a platinum group metal catalyst: 0.1 to 500 ppm by mass, calculated as platinum group metal atoms, relative to the mass of component (A). (F) a hydrosilylation reaction inhibitor: 0.05 to 5 parts by mass. [2]: The thermally conductive silicone composition according to [1], wherein the component (C) is represented by the following general formula (2): (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bond of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bond of two types of siloxane units enclosed in parentheses with x is a block polymer.) [3]: The R in the above general formula (1) 1 is a phenyl group, and the R 2is a methyl group. [4]: ​​The thermally conductive silicone composition according to any one of [1] to [3], wherein the thermally conductive silicone composition has an absolute viscosity of 1 to 1,000 Pa s at 23°C. [5]: A thermally conductive silicone cured product obtained by curing the thermally conductive silicone composition according to any one of [1] to [4]. [6]: The thermally conductive silicone cured product according to [5], wherein the thermal conductivity is 1.0 W / m K or more.

[0080] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and that exhibits similar effects is included within the technical scope of the present invention.

Claims

1. A thermally conductive silicone composition comprising the following (A) to (F): (A) a silicone having two or more alkenyl groups in one molecule and a kinetic viscosity at 25°C of 100 to 100,000 mm 2 (B) an organohydrogenpolysiloxane having two or more hydrosilyl groups: an amount such that the number of moles of hydrosilyl groups in the component (B) is 0.1 to 3 moles per mole of alkenyl groups in the component (A); and (C) a compound represented by the following general formula (1): (In the formula, R 1 are each independently a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms; R 2 are independently an alkyl group having 1 to 10 carbon atoms; R 3 is an alkyl group having 1 to 4 carbon atoms. a is 2 or 3, m is an integer satisfying 1≦m≦30, and n is an integer satisfying 0≦n≦60, provided that the range of 3≦m+n≦90 is satisfied. The bonds of the siloxane units enclosed in parentheses in the above general formula (1) may be in blocks or random. ) a hydrolyzable organopolysiloxane represented by the formula: 10 to 300 parts by mass, (D) one or more thermally conductive fillers selected from the group consisting of metals, metal oxides, metal hydroxides, and metal nitrides: an amount of 10 to 97% by mass based on the entire composition, (E) a platinum group metal catalyst: 0.1 to 500 ppm by mass calculated as platinum group metal atoms based on the mass of the above component (A), and (F) a hydrosilylation reaction inhibitor: 0.05 to 5 parts by mass.

2. The thermally conductive silicone composition according to claim 1, wherein the component (C) is represented by the following general formula (2): (In the formula, R 1 , R 2 , R 3 and a are the same as above, x is an integer of 1≦x≦30, m' is an integer of 1≦m'≦3, and n' is an integer of 0≦n'≦2, provided that m'+n' is 3. The bond of the siloxane units enclosed in parentheses with m' and n' may be block or random, and the bond of two types of siloxane units enclosed in parentheses with x is a block polymer.

3. The R in the general formula (1) 1 is a phenyl group, and the R 2 2. The thermally conductive silicone composition according to claim 1, wherein: is a methyl group.

4. The thermally conductive silicone composition according to claim 1, characterized in that the absolute viscosity of said thermally conductive silicone composition at 23° C. is 1 to 1,000 Pa·s.

5. A thermally conductive silicone cured product obtained by curing the thermally conductive silicone composition according to any one of claims 1 to 4.

6. The thermally conductive cured silicone product according to claim 5, characterized in that it has a thermal conductivity of 1.0 W / m·K or more.

Citation Information

Patent Citations

  • Cosmetic composition containing hydrocarbon oil and silicone oil

    JP2004262919A

  • Heat-conductive silicone oil composition, heat-dissipation agent and electronic device

    JP2007039621A

  • Method for thermoconductive rubber sheet and thermoconductive rubber sheet

    JP2015067736A

  • Thermoconductive resin composition and thermoconductive sheet using the same

    JP2015067737A

  • Heat-conductive fluorine-containing curable composition, cured product of the same, and electric and electronic component

    JP2017082090A

Cited By

  • Thermally conductive composite silicone rubber sheet

    WO2026063215A1

  • Thermally conductive composite silicone sheet

    WO2026079096A1