Polyolefin resin foamed particles and polyolefin resin foamed particle molded article

By applying magnesium silicate to the surface of polyolefin resin foam particles and optimizing the structural dimensions of the through-holes, the issue of inconsistent expansion ratio and density in polyolefin resin foam particles is resolved, leading to more consistent and mechanically enhanced foamed particle molded products.

WO2024247859A1PCT designated stage expired Publication Date: 2024-12-05JSP CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/018918
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-31
Filing Date
2024-05-22
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Polyolefin resin foam particles with through-holes exhibit significant variations in expansion ratio and molded product density, making it difficult to produce consistent quality foamed particle molded articles.

Method used

Incorporating magnesium silicate on the surface of polyolefin resin foam particles, with a proportion of 0.1% or more, to control the expansion ratio and density variations, and optimizing the average pore diameter, outer diameter, and wall thickness of the through-holes to achieve consistent foam properties.

Benefits of technology

The presence of magnesium silicate suppresses variations in expansion ratio and density, resulting in foamed particle molded products with improved consistency and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The purpose of the present invention is to provide polyolefin resin foamed particles with through-holes, having small variation in expansion ratio, and to provide a foamed particle molded article having low variation in density of the molded article. Polyolefin resin foamed particles according to the present invention have through-holes, contain magnesium silicate present on the surface of the foamed particles, and have an abundance ratio of magnesium silicate on the surface of the foamed particles of 0.1% by mass to 1% by mass inclusive.
Need to check novelty before this filing date? Find Prior Art

Description

Expanded polyolefin resin beads and expanded polyolefin resin beads molded article

[0001] The present invention relates to expanded polyolefin resin beads and a molded article made from expanded polyolefin resin beads.

[0002] BACKGROUND ART Expanded polyolefin resin particles such as expanded polypropylene resin particles having through holes have been known (Patent Document 1).

[0003] Japanese Patent Application Laid-Open No. 2022-096231

[0004] Expanded beads having through holes have a problem in that the expansion ratio varies widely within and between production lots. Furthermore, when the expansion ratio of expanded beads varies widely, the density of the resulting expanded bead moldings also varies widely, making it difficult to produce expanded bead moldings of consistent quality.

[0005] In view of the above-mentioned problems, the present invention aims to provide expanded polyolefin resin beads having through holes with small variations in expansion ratio and to provide expanded bead moldings with small variations in molding density.

[0006] According to the present invention, there are provided the following expanded polyolefin resin beads and expanded polyolefin resin bead molded articles. [1] Expanded polyolefin resin beads having through holes, characterized in that magnesium silicate is present in the surface portion of the expanded beads, and the magnesium silicate content in the surface portion of the expanded beads is 0.1 mass % or more. [2] Expanded polyolefin resin beads according to [1] above, in which the average pore size d of the through holes is 0.1 mm or more and 5 mm or less. [3] Expanded polyolefin resin beads according to [2] above, in which the average pore size d of the through holes is 0.1 mm or more and less than 1 mm, and the ratio d / D of the average pore size d to the average outer diameter D of the expanded polyolefin resin beads is 0.4 or less. [4] Expanded polyolefin resin beads according to [3] above, in which the average outer diameter D of the expanded polyolefin resin beads is 2 mm or more and 5 mm or less, and the average wall thickness t is 1.2 mm or more and 2 mm or less. [5] The expanded polyolefin resin beads according to any one of [1] to [4] above, wherein the length L of the through-holes in the penetration direction of the expanded polyolefin resin beads is 2 mm or more and 6 mm or less. [6] The expanded polyolefin resin beads according to any one of [1] to [5] above, wherein the moisture content of the expanded polyolefin resin beads is 0.1 mass % or more and 2.5 mass % or less. [7] The expanded polyolefin resin beads according to any one of [1] to [6] above, wherein the expanded polyolefin resin beads have a polyolefin resin foam layer and a polyolefin resin coating layer, and the coating layer covers all or part of the foam layer. [8] A polyolefin resin foamed bead molded product obtained by molding the expanded beads according to any one of [1] to [7] above in a mold.

[0007] According to the present invention, by allowing magnesium silicate to be present on the surface of expanded polyolefin resin beads, expanded beads having a small variation in expansion ratio can be obtained, and expanded bead moldings having a small variation in molding density can be obtained.

[0008] The expanded polyolefin resin beads and the expanded polyolefin resin bead molded article of the present invention will be described in detail below in this order.

[0009] In this specification, when multiple types of numerical ranges are defined as numerical values ​​for "items defined using numerical values ​​(referred to as numerically defined items (NM)") such as numerical values ​​corresponding to specific attributes or amounts of addition, for each numerically defined item (NM), the upper limit and lower limit values ​​in the combinations defining each numerical range may be independently combined in any combination. In this specification, a combination defining a numerical range refers to a combination of an upper limit and a lower limit value. Note that a numerical range defined by any combination of an upper limit and a lower limit value includes the upper limit value, the lower limit value, and values ​​between the upper limit value and the lower limit value (i.e., the numerical range is equal to or greater than the lower limit value and equal to or less than the upper limit value). For example, when a target numerically defined item (NM) (particular When the numerical value for a specific compound (such as density or amount of a specific compound) is between MA1 and MB1, preferably between MA2 and MB2, and more preferably between MA3 and MB3, the lower limit of the target numerical specification item (NM) may be any value (selected lower limit) selected from the group consisting of MA1, MA2, and MA3 (a group refers to a collection of multiple elements (a set of numerical values, etc.)), and the upper limit of the target numerical specification item (NM) may be any value (selected upper limit) selected from the group consisting of MB1, MB2, and MB3. Furthermore, the numerical range of the target numerical specification item (NM) may be a numerical range (selected numerical range) that is between the "selected lower limit" and the "selected upper limit." Note that MA1, MA2, MA3, MB1, MB2, and MB3 represent numerical values.

[0010] Furthermore, unless otherwise specified, even when different numerically prescribed items (NM) are combined, the upper limit value of each numerically prescribed item (NM) may be individually set as the "selected upper limit value." This also applies to the lower limit value and numerical range of the numerically prescribed item (NM).

[0011] The present invention relates to expanded polyolefin resin particles having through-holes (hereinafter simply referred to as expanded particles), and the expanded particles include expanded particles consisting of a single polyolefin resin foam layer (single-layer expanded particles) and multi-layer expanded particles having a polyolefin resin foam layer and a polyolefin resin coating layer (multi-layer expanded particles). In this specification, the polyolefin resin foam layer may be referred to as the "foam layer," and the polyolefin resin coating layer may be referred to as the "coating layer."

[0012] Next, the resin constituting the expanded beads of the present invention will be described. When the expanded beads are single-layered expanded beads, the resin constituting the expanded beads is a polyolefin-based resin, and when the expanded beads are multi-layered expanded beads, the resin constituting the foam layer is a polyolefin-based resin. In this specification, polyolefin-based resin refers to a homopolymer of an olefin-based monomer such as ethylene, propylene, butene, or pentene, or a copolymer containing 50 mol % or more of a component derived from an olefin-based monomer.

[0013] Examples of the polyolefin resin include polyethylene resin, ethylene ionomer, polypropylene resin, polybutene, polypentene, and copolymers of olefin monomers and monomers copolymerizable with olefin monomers such as styrene monomers. Among these, the type of polyolefin resin used is preferably polypropylene resin and / or polyethylene resin, and particularly preferably polypropylene resin. Note that, as the polyolefin resin, polyolefin resins derived from post-consumer recycled materials (PCR) or automobile recycled materials (ASR) can also be used.

[0014] Examples of the polyethylene resin include an ethylene copolymer containing 50 mol % or more of a component derived from an ethylene monomer, etc. Examples of the ethylene copolymer containing 50 mol % or more of a component derived from an ethylene monomer include high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, ethylene-propylene random copolymer, ethylene-propylene block copolymer, ethylene-butene block copolymer, ethylene-butene random copolymer, ethylene-vinyl acetate copolymer, and ethylene-methyl methacrylate copolymer.

[0015] Examples of the polypropylene-based resin include propylene homopolymers such as isotactic polypropylene, syndiotactic polypropylene, and atactic polypropylene; and propylene-based copolymers containing 50 mol% or more of a component derived from a propylene-based monomer, such as a propylene-ethylene random copolymer, a propylene-ethylene block copolymer, a propylene-butene random copolymer, a propylene-butene block copolymer, a propylene-ethylene-butene terpolymer, a propylene-acrylic acid copolymer, and a propylene-maleic anhydride copolymer.

[0016] When the expanded beads are composed of a polypropylene-based resin, the melting point (Tmc) thereof is preferably 120°C or higher and 160°C or lower. In this case, an expanded bead molded article having an excellent balance between the in-mold moldability of the expanded beads and the mechanical properties of the resulting molded article can be stably obtained. From the viewpoint of improving the mechanical properties of the resulting molded article, the melting point (Tmc) of the polypropylene-based resin constituting the expanded beads is preferably 130°C or higher, more preferably 135°C or higher. Furthermore, from the viewpoint of improving in-mold moldability under low molding pressure conditions, the melting point (Tmc) of the polypropylene-based resin constituting the expanded beads is preferably 155°C or lower, more preferably 153°C or lower. The numerical range of the melting point (Tmc) of the polypropylene-based resin constituting the expanded beads can be, for example, a range having a lower limit of any one value from the group consisting of 120°C, 130°C, and 135°C, and an upper limit of any one value from the group consisting of 160°C, 155°C, and 153°C (a numerical range not lower than the lower limit and not higher than the upper limit).

[0017] In this specification, the melting point of a polypropylene-based resin is determined based on JIS K7121:1987. Specifically, the conditioning is performed in the manner of "(2) Measuring the melting temperature after a certain heat treatment," and the conditioned test piece is heated from 30°C to 200°C at a heating rate of 10°C / min to obtain a DSC curve, and the apex temperature of the melting peak is taken as the melting point. When multiple melting peaks appear in the DSC curve, the apex temperature of the melting peak with the largest area is taken as the melting point.

[0018] Furthermore, the polyolefin resin constituting the expanded beads of the present invention may contain other resins, such as other resins or elastomers, as long as the purpose and effects of the present invention are not impaired. Examples of resins other than polyolefin resins include thermoplastic resins such as polystyrene resins, polyamide resins, and polyester resins. Examples of elastomers other than polyolefin resins include olefin thermoplastic elastomers and styrene thermoplastic elastomers. The content of the other resins or elastomers in the polyolefin resin is preferably 20% by mass or less, more preferably 10% by mass or less, even more preferably 5% by mass or less, and particularly preferably 0% by mass or less, i.e., the polyolefin resin does not contain the other resins or elastomers.

[0019] Next, the through holes formed in the expanded beads of the present invention will be described. The expanded beads of the present invention have through holes. Expanded beads having through holes have different physical properties and breathability than expanded beads without through holes. Examples of the cross-sectional shape of the expanded beads having through holes include (A) a hollow circular (doughnut) shape, (B) a hollow triangular shape, (C) a hollow hexagonal shape, (D) a shape with a partition inside a hollow circle, (E) a shape with two hollow circles arranged side by side, (F) a shape with three hollow circles arranged side by side and touching each other, (G) a hollow circular shape with a partial break, and (H) a hollow rectangular shape with a partial break. Examples of the through holes include a cylindrical shape with a constant diameter from one open end to the other open end, and a tapered hole.

[0020] The average pore diameter d of the through holes is preferably 0.1 mm or more and 5 mm or less. From the viewpoint of further improving the appearance of the molded article, further improving the compressive strength, and further improving the secondary expandability of the expanded beads, the average pore diameter d of the expanded beads is preferably less than 1 mm, more preferably 0.9 mm or less, even more preferably 0.85 mm or less, even more preferably 0.8 mm or less, and particularly preferably 0.7 mm or less. From the viewpoint of ease of production, the lower limit of the average pore diameter d of the expanded beads is approximately 0.1 mm, preferably 0.3 mm, more preferably 0.4 mm, and even more preferably 0.5 mm. The numerical range of the average pore diameter d of the through holes can be, for example, a range in which the lower limit is any one value from the group consisting of 0.1 mm, 0.3 mm, 0.4 mm, and 0.5 mm, and the upper limit is any one value from the group consisting of 5 mm, 1 mm, 0.9 mm, 0.85 mm, 0.8 mm, and 0.7 mm (a numerical range not less than the lower limit and not more than the upper limit).

[0021] The average pore diameter d of the through holes can be determined by the following method: 50 or more expanded beads randomly selected from a group of expanded beads are cut perpendicular to the penetration direction of the through holes at the position where the cross-sectional area is maximum. Photographs of the cut surfaces of each expanded bead are taken, the cross-sectional areas of the through holes (specifically, the opening areas) are determined, and the diameters of imaginary circles having the same area are calculated. The arithmetic mean of these diameters is taken as the average pore diameter d of the through holes.

[0022] The average outer diameter D of the expanded beads is preferably 2 mm or more, more preferably 2.5 mm or more, and even more preferably 3 mm or more. On the other hand, the average outer diameter D is preferably 6 mm or less, more preferably 5 mm or less, and even more preferably 4 mm or less. When the average outer diameter D is within the above range, the ability of the expanded beads to fill the mold during in-mold molding is improved, and the rigidity of the molded product is increased. The numerical range of the average outer diameter D of the expanded beads can be, for example, a range having a lower limit of any one value from the group consisting of 2 mm, 2.5 mm, and 3 mm, and an upper limit of any one value from the group consisting of 6 mm, 5 mm, and 4 mm (a numerical range not less than the lower limit and not more than the upper limit).

[0023] The ratio d / D of the average pore diameter d to the average outer diameter D of the expanded beads is preferably 0.8 or less. Furthermore, from the viewpoints of improving the appearance of the molded article, preventing a decrease in strength during compression, and preventing a decrease in the secondary expandability of the expanded beads during in-mold molding, the ratio d / D of the average pore diameter d to the average outer diameter D of the expanded beads is preferably 0.4 or less. From the viewpoints of improving the appearance of the molded article, improving the compressive strength, and improving the secondary expandability, the ratio d / D is more preferably 0.35 or less, even more preferably 0.3 or less, even more preferably 0.25 or less, and particularly preferably less than 0.2. On the other hand, if the ratio d / D is too small, production may become difficult, so it is preferably 0.1 or more. The numerical range of the ratio d / D can be, for example, a range having a lower limit of 0.1 and an upper limit of any one of the group consisting of 0.8, 0.4, 0.35, 0.3, and 0.25 (a numerical range not less than the lower limit and not more than the upper limit). The numerical range of the ratio d / D may also be a range not less than 0.1 and less than 0.2.

[0024] The average outer diameter D of expanded beads can be determined by the following method. At least 50 expanded beads randomly selected from a group of expanded beads are cut perpendicular to the penetration direction of the through-holes at the position where the cross-sectional area is greatest. A photograph of the cut surface of each expanded bead is taken, the cross-sectional area of ​​the expanded bead (specifically, the cross-sectional area including the openings of the through-holes) is determined, and the diameter of an imaginary perfect circle having the same area as that area is calculated. The diameter of the imaginary perfect circle is calculated for each expanded bead. The value obtained by arithmetically averaging these diameter values ​​calculated for each expanded bead is defined as the average outer diameter D of the expanded beads.

[0025] The average wall thickness t of the expanded beads is preferably 0.5 mm or more and 2 mm or less. Furthermore, from the viewpoint of ensuring that the expanded beads have a sufficiently large wall thickness and further improving secondary foaming properties during in-mold molding, the average wall thickness t of the expanded beads is preferably 0.9 mm or more and 2 mm or less. Furthermore, from the viewpoint of making the expanded beads more resistant to crushing by external forces and further improving the compressive stress of the molded article, the average wall thickness t of the expanded beads is more preferably 1.0 mm or more, even more preferably 1.2 mm or more, and particularly preferably 1.4 mm or more. The numerical range of the average wall thickness t of the expanded beads can be, for example, a range having a lower limit of any one of the group consisting of 0.5 mm, 0.9 mm, 1.0 mm, 1.2 mm, and 1.4 mm and an upper limit of 2 mm (a numerical range not less than the lower limit and not more than the upper limit).

[0026] The wall thickness t of the expanded beads is the distance from the surface portion (i.e., the outer surface portion) of the expanded beads to the outer edge of the through-hole (i.e., the inner surface portion of the expanded beads), and is a value calculated by the following formula (1): t=(D−d) / 2 (1)

[0027] In the above formula (1), d and D are values ​​corresponding to the following: d: average pore diameter of the through holes (mm), D: average outer diameter of the expanded beads (mm).

[0028] The ratio t / D of the average wall thickness t of the expanded beads to the average outer diameter D is preferably 0.1 or more and 0.5 or less. From the viewpoint of ensuring good filling properties of the expanded beads and further improving secondary foaming properties during in-mold molding of the expanded beads, the ratio t / D of the average wall thickness t of the expanded beads to the average outer diameter D of the expanded beads is preferably 0.35 or more and 0.5 or less. If the ratio t / D is within the above range, a molded product with excellent rigidity can be produced at a lower molding heating temperature.

[0029] In the expanded polyolefin resin beads of the present invention, it is preferable that the average pore diameter d of the through holes is 0.1 mm or more and less than 1 mm, and the ratio d / D is 0.4 or less. When the average pore diameter d is a relatively small value within a predetermined range and the ratio of the average pore diameter d to the average outer diameter D is small enough to satisfy 0.4 or less, it is easy to achieve a situation in which "the through holes are maintained before secondary expansion of the expanded beads and are filled during secondary expansion of the expanded beads during molding," resulting in excellent moldability of the expanded beads and the effects of improving the appearance and physical properties of the molded articles. To further enhance these effects, the expanded polyolefin resin beads of the present invention preferably have an average pore diameter d of 0.1 mm or more and less than 1 mm, and a ratio d / D of 0.4 or less. Furthermore, to ensure good secondary expansion of the expanded beads, it is preferable that the average outer diameter D of the expanded polyolefin resin beads is 2 mm or more and 5 mm or less, and the average wall thickness t is 0.9 mm or more and 2 mm or less.

[0030] The length L of the through-hole in the penetration direction (the length of the through-hole along the penetration direction of the through-hole) is 2 mm or more, more preferably 2.5 mm or more, and even more preferably 3 mm or more, from the viewpoint of shortening the cooling time when producing an expanded bead molding using the expanded beads. From the viewpoint of further reducing the moisture content of the expanded beads and the molding and further improving the strength of the expanded bead molding, the length L of the through-hole in the penetration direction is preferably 6 mm or less, preferably 5 mm or less, and even more preferably 4 mm or less. Note that the numerical range of the length L of the through-hole in the penetration direction can be, for example, a range in which the lower limit is any one value from the group consisting of 2 mm, 2.5 mm, and 3 mm, and the upper limit is any one value from the group consisting of 6 mm, 5 mm, and 4 mm (a numerical range not less than the lower limit and not more than the upper limit).

[0031] The length L of the through holes in the penetration direction can be determined by the following method. At least 50 expanded beads are randomly selected from a group of expanded beads, and the expanded beads are cut parallel to the penetration direction of the through holes, thereby exposing all of the through holes in the penetration direction to the surface. Photographs of the cut surfaces of each expanded bead are taken, and the length of the through holes in the penetration direction of each expanded bead is measured. The values ​​obtained by arithmetically averaging the lengths of the through holes measured for each expanded bead in the penetration direction are used as the length L of the through holes in the penetration direction.

[0032] When through holes are formed in expanded beads, the expansion ratio of each expanded bead tends to vary widely. The reason for this is thought to be as follows: Water used during the production of expanded beads is likely to remain in the through holes. Furthermore, the amount of water remaining in the through holes is likely to be large and fluctuate. This is thought to result in unstable expansion conditions and large variations in the expansion ratio of each expanded bead. The present inventors have found that by allowing a specific amount of magnesium silicate to be present in the surface portion of the expanded beads, water can be effectively prevented from remaining in the through holes, thereby reducing variations in the expansion ratio of the resulting expanded beads. In general, the expansion ratio (unit: times) of expanded beads is a value directly related to the bulk density of the expanded beads. More specifically, the expansion ratio of expanded beads is determined by the density (kg / m) of the resin constituting the expanded beads. 3 ) is the bulk density of the expanded particles (kg / m 3 ) In other words, when the density (bulk density) of the expanded beads varies widely, the expansion ratio of the expanded beads varies widely, and when the density of the expanded beads varies little, the expansion ratio of the expanded beads varies little.

[0033] The expanded beads of the present invention contain magnesium silicate on their surface. Since the surface free energy of magnesium silicate is extremely low, the surface free energy of the expanded beads is kept low. As a result, the wettability of the expanded beads is maintained low, and it is thought that water is less likely to remain in the expanded beads, particularly in the through-holes.

[0034] In this specification, the presence of magnesium silicate on the surface portion of the expanded beads means that it includes an embodiment in which magnesium silicate is attached to the surface of the expanded beads, an embodiment in which the resin on the surface portion of the expanded beads contains magnesium silicate, and an embodiment in which magnesium silicate is attached and the resin on the surface portion of the expanded beads also contains magnesium silicate.

[0035] Specifically, it is preferable to deposit magnesium silicate on the surface of expanded beads, so that magnesium silicate is present on the surface of single-layer or multi-layer expanded beads. A preferred method for depositing magnesium silicate on the surface of expanded beads is the dispersion medium release foaming method described below, in which magnesium silicate is used as a dispersant, and the magnesium silicate functions as a dispersant while also depositing magnesium silicate on the surface of expanded beads. However, in the present invention, the method for depositing magnesium silicate on the surface of expanded beads is not limited to the dispersion medium release foaming method, and other methods may be used as long as magnesium silicate can be present on the surface of expanded beads. Examples of such methods include applying a dispersion liquid containing magnesium silicate to the expanded beads to deposit magnesium silicate on the surface of expanded beads, adding magnesium silicate to the resin constituting the expanded beads to incorporate it into the expanded beads, and incorporating magnesium silicate into the coating layer of multi-layer expanded beads.

[0036] The surface portion of the expanded beads refers to the portion of the expanded beads corresponding to the range from the outer surface portion to a position 20 μm inward, and when magnesium silicate is attached to the surface of the expanded beads, the magnesium silicate attached to the surface of the expanded beads is also included in the magnesium silicate present in the surface portion. It is believed that the presence of magnesium silicate in the above range, which is the surface portion of the expanded beads, allows the expanded beads to exhibit hydrophobicity and enables the production of expanded beads with small variations in expansion ratio.

[0037] In the present invention, the proportion of magnesium silicate present in the surface portion of the expanded beads is a value calculated as the sum of the adhesion proportion and content of magnesium silicate relative to the expanded beads, and is 0.1% by mass or more relative to 100% by mass of the expanded bead body. If this proportion is too low, the effects of the present invention may not be obtained. From this perspective, the proportion of magnesium silicate present is preferably 0.15% by mass or more, more preferably 0.2% by mass or more, and even more preferably 0.3% by mass or more. The upper limit of this proportion is approximately 3% by mass or less, and from the viewpoint of preventing a decrease in the fusibility of the expanded beads, it is preferably 2% by mass or less, more preferably 1% by mass or less, and most preferably 0.8% by mass or less. The numerical range of the abundance ratio of magnesium silicate in the surface portion of the expanded beads (abundance ratio (mass %) relative to 100 mass % of the expanded bead body) can be, for example, a range having a lower limit of any one value from the group consisting of 0.15 mass %, 0.2 mass %, and 0.3 mass % and an upper limit of any one value from the group consisting of 3 mass %, 2 mass %, 1 mass %, and 0.8 mass % (a numerical range not less than the lower limit and not more than the upper limit).

[0038] The proportion of magnesium silicate present on the surface of expanded beads in the present invention can be measured, for example, by the following method. For example, in the case where magnesium silicate is attached to expanded beads, the ash content (A1: wt%) of the expanded beads and the ash content (A2: wt%) of the resin particles before the expanded bead production process are measured, and the ash content (A2: wt%) of the resin particles is subtracted from the ash content (A1: wt%) of the expanded beads to determine the proportion of magnesium silicate present on the surface of the expanded beads. Alternatively, the ash content (A1: wt%) of the expanded beads and the ash content (A3: wt%) of the expanded beads from which the attached content (the magnesium silicate attached content) has been physically or chemically removed are measured, and the ash content (A3: wt%) of the expanded beads from which the attached content (the magnesium silicate attached content) has been removed is subtracted from the ash content (A1: wt%) of the expanded beads to determine the proportion of magnesium silicate present on the surface of the expanded beads. The ash content includes inorganic components other than magnesium silicate, but the amount of magnesium silicate attached can be measured by separately determining the proportion of magnesium silicate present in the ash by X-ray fluorescence analysis or the like.

[0039] (Measurement of the Amount of Talc Present on the Surface Portion of Expanded Beads) When magnesium silicate that forms talc is used as the magnesium silicate, talc may be present on the surface portion of the expanded beads of the present invention. In this case, the amount of talc present (the amount of talc attached to the surface of the expanded beads and / or contained in the surface portion of the expanded beads (referred to as the amount of talc present on the surface)) can be measured as follows. For example, a calibration curve for talc is measured in advance using attenuated total reflectance spectroscopy (ATR), and the amount of talc present on the surface of the expanded beads (the amount of talc present on the surface of the expanded beads) can be measured based on this calibration curve.

[0040] Furthermore, when the expanded beads contain talc, the content of talc present in the surface portion of the expanded beads can be measured, for example, by the following method. First, a resin test piece with a known talc content is prepared. Next, the surface portion of the resin test piece is measured by total internal reflection spectroscopy (ATR method) using an infrared spectrophotometer to obtain an infrared light absorption spectrum of the resin test piece. Next, the peak wavelength attributable to talc is confirmed from the infrared light absorption spectrum of the resin test piece, and the absorption intensity of the peak wavelength is obtained. Specifically, the peak wavelength attributable to talc is 1000 cm -1 , 650 cm -1 A calibration curve is prepared from the relationship between the talc content in the resin test piece and the absorption intensity at the peak wavelength attributable to talc, allowing the talc content present in the surface portion of the expanded beads to be calculated.

[0041] Separately, the expanded beads to be measured are cut into two equal parts. The cut surface of the expanded beads (i.e., the interior of the expanded beads) is used as the measurement target and similarly measured by the ATR method to obtain an infrared absorption spectrum of the cut surface. Then, based on the infrared absorption spectrum of the cut surface, the absorption intensity at the same wavelength as the peak wavelength (the wavelength identified from the infrared absorption spectrum of the resin test piece as the peak wavelength derived from talc) is obtained. If talc is contained on the surface of the expanded beads, it is preferable to use the expanded beads to be measured as a sample for measurement by the ATR method after pre-treating them, such as by wiping off any inorganic matter adhering to the surface. If talc is adhering to the surface of the expanded beads, it is preferable to use the expanded beads to be measured as is as a sample.

[0042] Next, the surface of the expanded beads is measured by attenuated total reflection spectroscopy (ATR) to obtain an infrared absorption spectrum of the surface of the expanded beads, and the absorption intensity of the peak wavelength derived from talc is measured based on the infrared absorption spectrum of the surface of the expanded beads.

[0043] The difference between the absorption intensity based on the infrared absorption spectrum of the surface portion of the expanded beads and the absorption intensity based on the infrared absorption spectrum of the cut surface is calculated.

[0044] The content of talc present in the surface portion of the expanded beads can be calculated from the relationship between the calculated difference value and the calibration curve.

[0045] The difference value may be determined based on the difference spectrum (difference spectrum) between the infrared absorption spectrum of the surface portion of the expanded beads and the infrared absorption spectrum of the cut surface. That is, after obtaining the difference spectrum, the absorption intensity at the same wavelength as the wavelength determined from the infrared absorption spectrum of the resin test piece as the peak wavelength attributable to talc may be read based on the difference spectrum, and the read absorption intensity may be used as the difference value.

[0046] In the present invention, a preferred method for causing magnesium silicate to be present on the surface of expanded beads is to use magnesium silicate as a dispersant in the dispersion medium release foaming method described below, in which magnesium silicate functions as a dispersant and, in addition, magnesium silicate is attached to the surface of resin particles described below, and then the resin particles are foamed.

[0047] Next, the moisture content of the expanded beads will be described. The moisture content of the expanded beads of the present invention is preferably 0.1% by mass or more and 2.5% by mass or less. If the moisture content is within this range, the variation in the expansion ratio of the resulting expanded beads can be reduced. From this perspective, the lower limit of the moisture content is more preferably 0.2% by mass, and even more preferably 0.4% by mass. Meanwhile, the upper limit of the moisture content is more preferably 2.3% by mass, and even more preferably 2.1% by mass. The moisture content of the expanded beads can be, for example, a range having a lower limit of any one value from the group consisting of 0.1% by mass, 0.2% by mass, and 0.4% by mass, and an upper limit of any one value from the group consisting of 2.5% by mass, 2.3% by mass, and 2.1% by mass (a numerical range not less than the lower limit and not more than the upper limit).

[0048] In addition, when the moisture content of the expanded beads is high, the moisture content of each expanded bead tends to vary greatly. In such cases, the weight of each expanded bead varies, making it difficult to stably fill a mold with a constant amount of expanded beads, which results in a large variation in the molding density of the expanded bead molding after in-mold molding. While the above problem (the problem of variation in molding density) can be solved by reducing the moisture content of the expanded beads, adding a drying step leads to a deterioration in production efficiency.

[0049] The moisture content is measured as follows. In the present invention, the moisture content of expanded beads can be measured using a halogen moisture meter. A specific example of a measuring device for measuring the moisture content of expanded beads is a halogen moisture meter (HX204) manufactured by METTLER TOLEDO, which measures moisture content based on halogen lamp heating. The moisture content of expanded beads can be measured specifically by the following method. First, the expanded beads obtained by the expansion process and after curing are weighed to prepare a measurement sample. Next, using the halogen moisture meter, the measurement sample is heated to 100°C and maintained at 100°C for 60 seconds until no weight change occurs. Then, the measurement sample is further heated to 160°C and maintained at 160°C for 90 seconds until no weight change occurs, thereby vaporizing the moisture inside the measurement sample. The weight loss due to heating is divided by the weight of the expanded beads before heating and converted to a percentage to calculate the moisture content (%).

[0050] Next, the inclusion of carbons in the expanded beads will be described. The expanded beads of the present invention preferably contain carbons from the viewpoint of improving the appearance by coloring them black.

[0051] When the expanded beads are single-layer expanded beads, the content of carbons in the expanded beads is preferably 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 4% by mass, and even more preferably 1% by mass to 3% by mass. On the other hand, when the expanded beads are multi-layer expanded beads, it is preferable that at least the coating layer contains carbons. The content of carbons in the coating layer is preferably 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 4% by mass, and even more preferably 1% by mass to 3% by mass. Furthermore, the foam layer may also contain carbons. In this case, the content of carbons in the foam layer is preferably 0.1% by mass to 5% by mass, more preferably 0.5% by mass to 4% by mass, and even more preferably 1% by mass to 3% by mass. When the expanded beads are single-layer expanded beads, the numerical range of the carbon content in the expanded beads can be, for example, a range having a lower limit of any one value from the group consisting of 0.1 mass%, 0.5 mass%, and 1 mass%, and an upper limit of any one value from the group consisting of 5 mass%, 4 mass%, and 3 mass%, (a numerical range not less than the lower limit and not more than the upper limit). When the expanded beads are multi-layer expanded beads, the numerical range of the carbon content in the coating layer, and when the expanded beads are multi-layer expanded beads, the numerical range of the carbon content in the foam layer can be the same as the numerical range of the carbon content in the expanded beads when the expanded beads are single-layer expanded beads.

[0052] The carbon content of expanded beads and their molded articles can be quantified by TG-DTA. Specifically, a sample cut from the expanded beads or molded articles is used as a measurement sample, and the weighed measurement sample is heated from 40°C to 600°C in a nitrogen atmosphere. The heating temperature of the measurement sample is then lowered to 400°C, the atmospheric gas is changed from nitrogen to air, and the measurement sample is heated to 800°C. The weight loss of the measurement sample when heated to 600°C in a nitrogen atmosphere is taken as the organic matter content, and the weight loss of the measurement sample when heated to 800°C in an air atmosphere is taken as the carbon content. When measuring the content of the coating layer, a measurement sample can be prepared by scraping off the target portion and measuring in the same manner.

[0053] Examples of the carbons include at least one type of carbon powder selected from carbon black, carbon nanotubes, graphite, graphene, carbon nanofibers, carbon microfibers, carbon microcoils, and carbon nanocoils, and examples of usable carbons include channel black, roller black, furnace black, thermal black, acetylene black, SWCNT (single-walled carbon nanotube), MWCNT (multi-walled carbon nanotube), branched MWCNT, etc. Among these, furnace black is preferred as the carbon to be used for the expanded beads because it has an excellent balance between dispersibility in polypropylene-based resins and material costs.

[0054] When carbons are contained in the expanded beads of the present invention, the mass ratio (CB / magnesium silicate amount) of the amount of magnesium silicate present in the surface portion of the expanded beads (magnesium silicate amount) to the content of carbons (CB) in the expanded beads is preferably 2.5 to 100, more preferably 3 to 50. Therefore, the numerical range of the mass ratio (CB / magnesium silicate amount) can be, for example, a range having a lower limit of any one of the group consisting of 2.5 and 3 and an upper limit of any one of the group consisting of 100 and 50 (a numerical range not less than the lower limit and not more than the upper limit).

[0055] (Other Additives) The expanded beads of the present invention may contain additives. Specific examples of additives include flame retardants, flame retardant auxiliaries, cell regulators, antioxidants, weathering agents, and crystal nucleating agents. The additives may be contained in the entire single-layer expanded beads, the entire multi-layer expanded beads, or only in the coating layer of the multi-layer expanded beads.

[0056] Next, the bulk density, average cell diameter, and crystalline structure of the expanded beads of the present invention will be described. (Bulk Density of Expanded Beads) The bulk density of the expanded beads is 10 kg / m 3 More than 500kg / m 3 If the bulk density is within this range, the resulting molded article will have a good balance between light weight and rigidity. From this viewpoint, the bulk density of the expanded beads is preferably 15 kg / m or less. 3 More than 100kg / m 3 More preferably, it is 18 kg / m or less. 3 More than 50kg / m 3 Therefore, the range of the bulk density of the expanded beads is, for example, 10 kg / m or less. 3 , 15 kg / m 3 and 18 kg / m 3 and 500 kg / m 3 , 100 kg / m 3 and 50 kg / m 3 The range can be any one of the values ​​in the group consisting of the above as the upper limit (a numerical range not less than the lower limit and not more than the upper limit).

[0057] The bulk density of expanded beads is measured by the following method. First, a plurality of expanded beads (expanded beads) to be measured are left for 24 hours or more in an environment of 23°C temperature, 50% relative humidity, and 1 atm. Then, a mass W (unit: g) of expanded beads is filled into a measuring cylinder, and the bottom of the measuring cylinder is lightly tapped against the floor several times to stabilize the filling height of the expanded beads in the measuring cylinder. The bulk volume V (unit: L) of the expanded beads indicated on the measuring cylinder scale is read, and the mass W of the expanded beads is divided by the bulk volume V of the expanded beads (i.e., W / V). The value obtained in this way is kg / m 3The same measurement is repeated for different samples, and the average of the converted values ​​obtained for each sample is calculated to obtain the bulk density (unit: kg / m) of the expanded beads. 3 ) can be obtained.

[0058] (Average Cell Diameter of Expanded Beads) The average cell diameter of expanded beads is preferably 100 μm or more and 300 μm or less. If the cell diameter is within this range, the range of molding conditions (specifically, molding temperature and molding pressure) under which a good molded article can be obtained when the expanded beads are used to produce a molded article can be widened. From this perspective, the average cell diameter is more preferably 150 μm or more and 280 μm or less, and even more preferably 160 μm or more and 250 μm or less. Therefore, the numerical range of the average cell diameter of expanded beads can be, for example, a range having a lower limit of any one value in the group consisting of 100 μm, 150 μm, and 160 μm, and an upper limit of any one value in the group consisting of 300 μm, 280 μm, and 250 μm (a numerical range not less than the lower limit and not more than the upper limit).

[0059] Next, the crystalline structure of the expanded beads of the present invention analyzed by differential scanning calorimetry (DSC) will be described. (High-Temperature Peak) The expanded beads preferably have a crystalline structure in which a melting peak specific to the polypropylene resin (i.e., the resin-specific peak) and one or more melting peaks (i.e., high-temperature peaks) appear on the higher temperature side of the DSC curve obtained when a test sample is heated from 23°C to 200°C at a heating rate of 10°C / min. The DSC curve is obtained by differential scanning calorimetry (DSC) in accordance with JIS K7121:1987 using 1 to 4 mg of expanded beads as a test sample. The resin-specific peak is an endothermic peak due to the melting of crystals specific to the polypropylene resin constituting the expanded beads, and is thought to be due to the endothermic heat generated when crystals typically melt in polypropylene resins. On the other hand, the endothermic peak on the higher temperature side of the resin-specific peak (i.e., the high-temperature peak) is an endothermic peak that appears on the higher temperature side of the resin-specific peak on the DSC curve. When this high-temperature peak appears, it is presumed that a high-melting secondary crystalline component is present in the resin. In addition, in the DSC curve obtained by heating a test sample from 23°C to 200°C at a heating rate of 10°C / min (i.e., the first heating), cooling the test sample from 200°C to 23°C at a cooling rate of 10°C / min, and then heating the test sample again from 23°C to 200°C at a heating rate of 10°C / min (i.e., the second heating), only an endothermic peak due to the melting of crystals specific to the polypropylene resin constituting the expanded beads is observed, making it possible to distinguish between the resin-specific peak and the high-temperature peak. The peak temperature of this resin-specific peak may differ slightly between the first and second heatings, but the difference is usually within approximately 5°C.

[0060] From the viewpoint of further improving the moldability of the expanded beads and obtaining molded articles with superior rigidity, the heat of fusion of the high-temperature peak of the expanded beads is preferably 5 J / g to 40 J / g, more preferably 7 J / g to 30 J / g, and even more preferably 10 J / g to 20 J / g. The total heat of fusion of the expanded beads is preferably 25 J / g to 150 J / g, more preferably 35 J / g to 100 J / g, and even more preferably 50 J / g to 90 J / g. Therefore, the numerical range of the heat of fusion of the high-temperature peak of the expanded beads can be, for example, a range having a lower limit of any one value from the group consisting of 5 J / g, 7 J / g, and 10 J / g, and an upper limit of any one value from the group consisting of 40 J / g, 30 J / g, and 20 J / g (a numerical range not less than the lower limit and not more than the upper limit). The numerical range of the total heat of fusion of the expanded beads can be, for example, a range having a lower limit of any one of the groups consisting of 25 J / g, 35 J / g, and 50 J / g and an upper limit of any one of the groups consisting of 150 J / g, 100 J / g, and 90 J / g (a numerical range not less than the lower limit and not more than the upper limit).

[0061] (Method for Measuring High-Temperature Peaks) The heat of fusion of each peak in the DSC curve of expanded beads is determined as follows. First, approximately 1 to 4 mg of expanded beads are sampled from a group of expanded beads after conditioning. Using these expanded beads as test specimens, a DSC curve is obtained by heating the test specimen from 23°C to 200°C at a heating rate of 10°C / min using a differential scanning calorimeter. Note that multiple expanded beads may be used as test specimens. The DSC curve exhibits a resin-specific peak ΔH1 and a high-temperature peak ΔH2, which peaks higher than the peak of the resin-specific peak ΔH1. Next, a line L1 is obtained by connecting point α at a temperature of 80°C on the DSC curve with point β at the melting end temperature T of the expanded beads. Next, a line L2 parallel to the vertical axis of the graph is drawn from point γ on the DSC curve, which corresponds to the valley between the resin-specific peak ΔH1 and the high-temperature peak ΔH2, and the point where lines L1 and L2 intersect is designated δ. The point γ can also be said to be a maximum point existing between the resin-specific peak ΔH1 and the high-temperature peak ΔH2. The area of ​​the resin-specific peak ΔH1 is the area of ​​the portion surrounded by the curve of the resin-specific peak ΔH1 portion of the DSC curve, the line segment α-δ, and the line segment γ-δ, and this is the heat of fusion of the resin-specific peak. The area of ​​the high-temperature peak ΔH2 is the area of ​​the portion surrounded by the curve of the high-temperature peak ΔH2 portion of the DSC curve, the line segment δ-β, and the line segment γ-δ, and this is the heat of fusion of the high-temperature peak (i.e., the high-temperature peak heat quantity). The area of ​​the total melting peak is the area of ​​the portion surrounded by the curve of the resin-specific peak ΔH1 portion of the DSC curve, the curve of the high-temperature peak ΔH2 portion, and the line segment α-β (i.e., the straight line L1), and this is the heat of fusion of the total melting peak (total heat of fusion).

[0062] Next, in the present invention, multilayer expanded beads can also be used as the expanded beads. The multilayer expanded beads have a polyolefin resin foam layer (sometimes referred to as the foam layer) and a polyolefin resin coating layer (sometimes referred to as the coating layer), and the coating layer has a structure in which the foam layer is coated in whole or in part. That is, the multilayer expanded beads are composed of a foam layer made of the above-mentioned polyolefin resin and a coating layer that coats the foam layer in whole or in part, and as a whole, a so-called sheath-core structure is formed. When a sheath-core structure is formed, even if the amount of magnesium silicate attached to the surface of the expanded beads is large, the resin of the coating layer can have excellent fusion properties, thereby preventing a decrease in fusion properties between the expanded beads.

[0063] The coating layer is composed of a foamed or non-foamed polyolefin resin. The coating layer is preferably substantially non-foamed. "Substantially non-foamed" means that almost no or no cellular structure is formed. When the coating layer is non-foamed, the amount of resin on the surface of the expanded beads increases, and the fusion between the expanded beads can be further improved.

[0064] Next, the coating layer constituting the multilayer foamed beads will be described. Examples of resins constituting the coating layer include polyolefin-based resins. Examples of polyolefin-based resins include polyethylene-based resins such as linear low-density polyethylene, low-density polyethylene, and high-density polyethylene; polypropylene-based resins such as propylene-ethylene copolymers, propylene-butene copolymers, and propylene-ethylene-butene copolymers; and mixtures thereof. From the viewpoint of excellent adhesion between the coating layer and the foamed layer, the polyolefin-based resin constituting the coating layer is preferably a polypropylene-based resin and / or a polyethylene-based resin, and more preferably a polypropylene-based resin. It is more preferable that the resin constituting the coating layer is at least one selected from a propylene-ethylene copolymer, a propylene-butene copolymer, and a propylene-ethylene-butene copolymer. Furthermore, by forming a coating layer made of a polypropylene-based resin and / or a polyethylene-based resin on the foamed beads, adhesion between the foamed layer and the coating layer can be further improved, and molded articles with good mechanical properties can be consistently obtained. The resin composed of at least one selected from the group consisting of a propylene-ethylene copolymer, a propylene-butene copolymer, and a propylene-ethylene-butene copolymer may be composed of a single copolymer or a mixture of multiple copolymers. Furthermore, from the viewpoint of improving the fusion properties between the expanded beads and improving the adhesion between the foam layer and the coating layer, it is preferable that the resin constituting the coating layer is obtained using a metallocene polymerization catalyst.

[0065] When the resin constituting the coating layer is a polyolefin-based resin, the melting point Tms (°C) of the polyolefin-based resin is preferably lower than, for example, the melting point Tmc (°C) of the polypropylene-based resin constituting the foam layer. That is, it is preferable that Tms < Tmc. In this case, the fusion property between the foamed particles during molding is improved, and a molded product with excellent fusion property can be produced at low temperatures (specifically, low steam pressures) during in-mold molding. From the viewpoint of further improving this effect, it is preferable that Tmc - Tms ≧ 1 (°C), more preferably Tmc - Tms ≧ 3 (°C), and even more preferably Tmc - Tms ≧ 5 (°C). From the viewpoint of further suppressing peeling between the foamed layer and the coating layer and adhesion of the resin to the molding die during in-mold molding, it is preferable that Tmc - Tms ≦ 30 (°C), more preferably Tmc - Tms ≦ 25 (°C), and even more preferably Tmc - Tms ≦ 20 (°C). Therefore, the numerical range of Tmc-Tms can be, for example, a range having a lower limit of any one value from the group consisting of 1 (°C), 3 (°C), and 5 (°C) and an upper limit of any one value from the group consisting of 30 (°C), 25 (°C), and 20 (°C) (a numerical range not less than the lower limit and not more than the upper limit).

[0066] From the viewpoint of easily suppressing adhesion of the resin to the molding die, the melting point Tms of the polyolefin resin constituting the coating layer is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher. On the other hand, from the viewpoint of easily increasing the fusion property of the expanded beads during molding, the melting point Tms of the polyolefin resin constituting the coating layer is preferably 150°C or lower, more preferably 145°C or lower, and even more preferably 140°C or lower. The melting point of the polyolefin resin constituting the coating layer is determined based on JIS K7121:1987. Specifically, the melting point of the polyolefin resin constituting the coating layer can be determined under the same conditions and methods as those that can be used to determine the melting point of the polypropylene resin constituting the single-layer expanded beads described above. The numerical range of the melting point Tms of the polyolefin resin constituting the coating layer can be, for example, a range having a lower limit of any one value from the group consisting of 100°C, 110°C, and 120°C, and an upper limit of any one value from the group consisting of 150°C, 145°C, and 140°C (a numerical range not less than the lower limit and not more than the upper limit).

[0067] When the expanded beads of the present invention are multilayer expanded beads, the proportion of the coating layer in the expanded beads is preferably 0.5% by mass or more and 10% by mass or less. In this case, it is possible to stably obtain expanded bead molded articles having excellent mechanical properties while improving the in-mold moldability of the expanded beads. From the viewpoint of improving the effect of excellent balance between in-mold moldability and mechanical properties, the mass proportion of the coating layer in the multilayer expanded beads is more preferably 1% by mass or more and 8% by mass or less, and even more preferably 2% by mass or more and 6% by mass or less. Therefore, the numerical range of the mass proportion of the coating layer in the multilayer expanded beads can be, for example, a range having a lower limit of any one value from the group consisting of 0.5% by mass, 1% by mass, and 2% by mass and an upper limit of any one value from the group consisting of 10% by mass, 8% by mass, and 6% by mass (a numerical range at least the lower limit and at most the upper limit).

[0068] Next, an example of a method for producing expanded beads of the present invention will be described. The expanded beads can be produced, for example, by a so-called dispersion medium release foaming method. In the dispersion medium release foaming method, resin particles (single-layer resin particles or multi-layer resin particles) are produced (resin particle production step), the resulting resin particles are dispersed in a dispersion medium (e.g., water) (dispersion step), the resin particles are impregnated with a blowing agent (foaming agent impregnation step), and the expandable resin particles containing the blowing agent are released together with the dispersion medium under low pressure (foaming step), thereby producing expanded beads.

[0069] (Resin Particle Manufacturing Process) When forming single-layer resin particles, the resin particles are manufactured, for example, as follows. First, a polyolefin resin and, if necessary, additives such as a bubble nucleating agent are fed into an extruder, heated, and kneaded to form a resin melt kneaded product. The resin melt kneaded product is then extruded through a small hole in a die attached to the tip of the extruder to form a tubular strand having through-holes. The extruded strand is then cooled and cut to obtain resin particles. The tubular strand having through-holes is formed by passing the molten resin kneaded product through a die attached to the tip of the extruder, which has a flow path formed by a metal fitting attached to the flow path of the die, having a cross-sectional shape corresponding to the cross-sectional shape of the resin particles having through-holes. The extruded product is then cut using, for example, a pelletizer. The cutting method can be selected from a strand cutting method, a hot cutting method, an underwater cutting method, etc. Cylindrical single-layer resin particles having through-holes can be obtained in this manner. When forming multilayer resin particles, a resin melt blend of each raw material is obtained using an extruder for forming a foam layer and an extruder for forming a coating layer, and each melt blend is introduced into a die. The melt blends are then merged in the die to form a sheath-core composite molten resin blend consisting of a non-foamed, cylindrical molten resin blend for forming the foam layer and a non-foamed molten resin blend for forming the coating layer, which coats the outer surface of the molten resin blend for forming the foam layer. The composite molten resin blend is then extruded through the holes in a nozzle attached to the tip of the extruder in the form of a strand with through holes, thereby forming an extrudate. The extrudate is then cooled and cut, thereby obtaining multilayer resin particles.

[0070] When magnesium silicate is contained in the expanded resin particles, it is preferable that magnesium silicate is added to the resin for forming the expanded layer of the single-layer resin particles or the resin for forming the coating layer of the multi-layer expanded resin particles in the manufacturing process of the resin particles.

[0071] The particle diameter of the resin particles is preferably 0.1 mm to 3.0 mm, more preferably 0.3 mm to 1.5 mm. The length / outer diameter ratio of the resin particles is preferably 0.5 to 5.0, more preferably 1.0 to 3.0. The average mass of each resin particle (calculated from the mass of 200 randomly selected resin particles) is preferably 0.1 mg to 20 mg, more preferably 0.2 mg to 10 mg, even more preferably 0.3 mg to 5 mg, and particularly preferably 0.4 mg to 2 mg. The mass ratio of the foam layer to the coating layer in the multilayer resin particles (specifically, foam layer mass:coating layer mass) is preferably 99.5:0.5 to 90:10, more preferably 99:1 to 92:8, and even more preferably 98:2 to 94:6. The mass ratio is expressed as the mass of the foam layer:the mass of the coating layer. Therefore, the numerical range of the particle diameter of the resin particles can be, for example, a range having a lower limit of any one of the values ​​in the group consisting of 0.1 mm and 0.3 mm and an upper limit of any one of the values ​​in the group consisting of 3.0 mm and 1.5 mm (a numerical range not less than the lower limit and not more than the upper limit). The numerical range of the length / outer diameter ratio of the resin particles can be, for example, a range having a lower limit of any one of the values ​​in the group consisting of 0.5 and 1.0 and an upper limit of any one of the values ​​in the group consisting of 5.0 and 3.0 (a numerical range not less than the lower limit and not more than the upper limit). The numerical range of the average mass of one resin particle can be, for example, a range having a lower limit of any one of the values ​​in the group consisting of 0.1 mg, 0.2 mg, 0.3 mg, and 0.4 mg and an upper limit of any one of the values ​​in the group consisting of 20 mg, 10 mg, 5 mg, and 2 mg (a numerical range not less than the lower limit and not more than the upper limit). When the total mass of the foam layer and the coating layer in the multilayer resin particles is taken as 100, the numerical range of the mass of the coating layer can be, for example, a range in which the lower limit is any one value from the group consisting of 0.5, 1, and 2, and the upper limit is any one value from the group consisting of 10, 8, and 6 (a numerical range not less than the lower limit and not more than the upper limit).

[0072] If necessary, additives such as a bubble regulator, a crystal nucleating agent, a colorant, a flame retardant, a flame retardant auxiliary, a plasticizer, an antistatic agent, an antioxidant, an ultraviolet inhibitor, a light stabilizer, a conductive filler, and an antibacterial agent may be added to the resin particles. Examples of the bubble regulator include inorganic powders such as mica, zinc borate, calcium carbonate, silica, titanium oxide, gypsum, zeolite, borax, aluminum hydroxide, and carbon; and organic powders such as phosphoric acid-based nucleating agents, phenol-based nucleating agents, amine-based nucleating agents, and polyethylene fluoride-based resin powder. When a bubble regulator is added to the resin particles, the content of the bubble regulator is preferably 0.01 parts by mass or more and 1 part by mass or less relative to 100 parts by mass of the polypropylene-based resin.

[0073] (Dispersion Step) The dispersion step is a step of dispersing resin particles in an aqueous medium. As the resin particles, the above-mentioned single-layer resin particles or the above-mentioned multi-layer resin particles are used.

[0074] An aqueous medium is used as a dispersion medium (specifically, a liquid) for dispersing the single-layer resin particles or multilayer resin particles in a sealed container. The aqueous medium is a dispersion medium (specifically, a liquid) containing water as a main component. The proportion of water in the aqueous medium is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. Examples of dispersion media other than water in the aqueous medium include ethylene glycol, glycerin, methanol, and ethanol.

[0075] When magnesium silicate is to be attached to the expanded beads, it is preferable to add and disperse magnesium silicate in an aqueous medium so that the amount of magnesium silicate is 0.1 to 15 parts by mass per 100 parts by mass of resin particles. The magnesium silicate dispersed in the aqueous medium not only acts as an inorganic dispersant, but also adheres to the resin particles in the dispersion step. Furthermore, when the resin particles are expanded in the expansion step described below, the magnesium silicate remains on the surface of the expanded beads, resulting in expanded beads with magnesium silicate uniformly attached to their surface. Note that when the resin particles contain magnesium silicate on their surface and it is not necessary to attach magnesium silicate to the expanded beads, it is not necessary to use magnesium silicate as an inorganic dispersant.

[0076] In the dispersion step, in addition to magnesium silicate as described above, other inorganic dispersants can be added to the aqueous medium within a range that does not impair the intended effects of the present invention, so as to prevent the resin particles heated in the sealed container from fusing together. Examples of other inorganic dispersants include inorganic fine particles such as aluminum oxide, tricalcium phosphate, magnesium pyrophosphate, and zinc oxide. These inorganic fine particles may be used alone, or two or more types of inorganic fine particles may be used in combination. It is preferable to add the other inorganic dispersants in an amount of 0.001 to 5 parts by mass per 100 parts by mass of resin particles.

[0077] In addition to the inorganic dispersant, additives such as a dispersing aid and a surfactant may be added. Examples of the dispersing aid include aluminum sulfate. Examples of the surfactant include anionic surfactants such as sodium alkylbenzenesulfonate, sodium dodecylbenzenesulfonate, and sodium alkanesulfonate. The surfactant may be used alone, or two or more surfactants may be used in combination. The amount of the dispersing aid added is preferably 0.001 to 1 part by mass per 100 parts by mass of the resin particles.

[0078] (Foaming Agent Impregnation Step) The foaming agent impregnation step is a step of impregnating resin particles with a foaming agent. The foaming agent impregnation step may be performed after the dispersion step, or the foaming agent impregnation step may be performed partly or entirely overlapping with the dispersion step.

[0079] In the blowing agent impregnation step, for example, a container containing resin particles is sealed, and a blowing agent is added to the sealed container to impregnate the resin particles with the blowing agent. This allows for the production of expandable resin particles containing a blowing agent. Examples of the blowing agent include physical blowing agents. The physical blowing agent can be added to the sealed container at any time before the resin particles are expanded. The blowing agent may be added to the aqueous medium together with the resin particles during the dispersion step, and then the resin particles may be impregnated with the blowing agent by heating or the like. Alternatively, gaseous blowing agent may be pressure-injected into the sealed container during or after the dispersion step to impregnate the resin particles with the blowing agent. For example, when carbon dioxide is used as a physical blowing agent, a solid blowing agent (e.g., dry ice) may be added to the aqueous medium together with the resin particles during the dispersion step, or gaseous carbon dioxide may be pressure-injected into the sealed container during or after the dispersion step. When the resin particles are impregnated with the blowing agent, the contents of the sealed container (e.g., the resin particles and the aqueous medium) can be heated and / or pressurized to promote the impregnation of the resin particles with the blowing agent.

[0080] The temperature of the aqueous medium in the sealed container is increased at a rate of 1° C. / min to 5° C. / min, and a holding step is provided during the temperature increase.

[0081] (Retention Step) In the retention step, the expanded beads in the sealed container are maintained at a predetermined temperature, thereby adjusting the crystalline state of the expanded beads. The retention step is carried out by adjusting the temperature rise rate of the space inside the sealed container, or by adjusting the retention temperature and / or retention time of the space inside the sealed container, in the dispersion step and / or the blowing agent impregnation step. In an example where the expanded beads are multilayer expanded beads, the crystalline state of the expanded beads is adjusted so that, in a DSC curve obtained by measuring the expanded beads using a heat flux differential scanning calorimeter, an endothermic peak (i.e., a high-temperature peak) appears at a higher temperature than the endothermic peak (i.e., a resin-specific peak) of the main component of the resin constituting the foam layer of the multilayer expanded beads (i.e., the resin constituting the expanded beads in the case of single-layer expanded beads). Adjusting the high-temperature peak to adjust the crystalline state of the expanded beads can broaden the range of molding conditions (specifically, molding temperature and molding pressure) under which a good molded article can be obtained, thereby improving the compressive strength of the resulting molded article.

[0082] The high-temperature peak is generally adjusted as follows. In the holding step, the temperature increase is stopped at a temperature Ta within the range of at least 15°C lower than the resin melting point Tm of the resin particles and lower than the melting end temperature Te of the resin particles. The temperature Ta is then held for a sufficient time, preferably 10 to 60 minutes, to expand the resin particles that have formed secondary crystals. This allows the high-temperature peak to be adjusted. The high-temperature peak can also be adjusted in the expansion step described below. In this case, the temperature Tb is adjusted to a temperature within the range of (Tm - 5°C) to (Te + 5°C), and the resin particles are released from the container into a low-pressure region at that temperature for expansion, thereby obtaining expanded beads. The calorific value of the high-temperature peak of the expanded beads tends to increase as the temperature Ta or Tb is lower within the temperature range and / or the holding time (the time during which the resin particles are held at temperature Ta) is longer. Typically, the temperature increase rate in the expansion step is 0.5 to 5°C / min. By taking these points into consideration and repeating preliminary experiments (experiments in which the holding step and / or the expansion step are carried out with various values ​​for the temperature Ta, holding time, and temperature Tb to produce expanded beads), it is possible to easily and accurately determine the production conditions for expanded beads that exhibit the desired high-temperature peak calorific value.

[0083] (Blowing Agent) The blowing agent is appropriately selected from among the common blowing agents used to obtain expanded particles. As the blowing agent, a physical blowing agent is preferred. As the physical blowing agent, an inorganic physical blowing agent and / or an organic physical blowing agent can be used. Examples of inorganic physical blowing agents include carbon dioxide, air, nitrogen, helium, argon, water, etc. Examples of organic physical blowing agents include aliphatic hydrocarbons such as propane, butane, and hexane; alicyclic hydrocarbons such as cyclopentane and cyclohexane; and halogenated hydrocarbons such as 2,3,3,3-tetrafluoropropene, trans-1,3,3,3-tetrafluoropropene, and trans-1-chloro-3,3,3-trifluoropropene.

[0084] These physical foaming agents may be used alone, or two or more physical foaming agents may be used in combination. Among these foaming agents, foaming agents containing an inorganic physical foaming agent such as carbon dioxide, nitrogen, or air as a main component are preferably used, and carbon dioxide is more preferably used. In this specification, "containing an inorganic physical foaming agent as a main component" means that the physical foaming agent contains 50 mol% or more of the inorganic physical foaming agent. The physical foaming agent preferably contains 70 mol% or more, more preferably 90 mol% or more of the inorganic physical foaming agent, and even more preferably consists of only the inorganic physical foaming agent.

[0085] The amount of physical foaming agent added is determined appropriately depending on the type of resin constituting the resin particles, the type of foaming agent, the desired bulk density of the expanded particles, etc. It is particularly preferable to determine the amount of physical foaming agent added depending on the desired bulk density. For example, when carbon dioxide is used as the physical foaming agent, the amount of carbon dioxide added is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, per 100 parts by mass of the multilayer resin particles. Therefore, when carbon dioxide is used as the physical foaming agent, the numerical range of the amount of carbon dioxide added, in parts by mass per 100 parts by mass of the multilayer resin particles, can be, for example, a range (numerical range at least the lower limit and at most the upper limit) with a lower limit of any one of the group consisting of 0.1 parts by mass, 0.5 parts by mass, and 1 part by mass, and an upper limit of any one of the group consisting of 30 parts by mass, 15 parts by mass, and 10 parts by mass.

[0086] (Expansion Process) In the expansion process, resin particles containing a blowing agent (i.e., expandable resin particles) are released from a container together with an aqueous medium and expanded to produce expanded particles. Specifically, the expandable resin particles are expanded by releasing the expandable resin particles together with the aqueous medium under a pressure lower than the internal pressure of the sealed container. This expansion method makes it possible to easily obtain expanded particles with a low bulk density.

[0087] The internal pressure of the sealed container during expansion is preferably 0.5 MPa (G: gauge pressure) or more. On the other hand, the internal pressure of the sealed container is preferably 4.0 MPa (G) or less, and more preferably 3.0 MPa (G) or less. Within this range, expanded beads can be produced safely without risk of damage or explosion of the sealed container.

[0088] The bulk density of the expanded beads can be adjusted, for example, by appropriately changing the expansion conditions, such as the temperature and pressure, inside the sealed container when releasing the contents of the sealed container during the expansion process. Furthermore, to produce expanded beads with a lower bulk density, a multi-stage expansion process, such as a two-stage expansion process, is preferably performed. In the two-stage expansion process, the expanded beads (first-stage expanded beads) obtained by the dispersion medium release foaming method described above are first stored in a pressurizable sealed container. A gas such as air is then injected into the sealed container to apply a pressure treatment. This increases the pressure inside the cells of the expanded beads (i.e., the internal pressure). The expanded beads with increased internal pressure are then removed from the sealed container and heated with steam or hot air to expand the expanded beads. By performing this two-stage expansion process, expanded beads (second-stage expanded beads) with a lower bulk density can be obtained. Furthermore, compared to a method of obtaining expanded beads with a low bulk density through a single expansion process, a method of obtaining expanded beads with a low bulk density through a two-stage expansion process makes it easier to increase the cell diameter of the final expanded beads. Expanded bead moldings produced using expanded beads obtained by the second-stage expansion process can further suppress the occurrence of uneven color tone. Therefore, when producing expanded beads containing a colorant, it is preferable to obtain expanded beads by performing the second-stage expansion process. In the present invention, if the first-stage expanded beads satisfy the configuration of the present invention, the variation in expansion ratio of the second-stage expanded beads will also be small, and further, when an expanded bead molding is obtained using these second-stage expanded beads, the variation in expansion ratio of the expanded bead molding will also be small.

[0089] In the resin bead production process, the average diameter d of the through holes of the resulting expanded beads can be adjusted by adjusting the diameter dr of the through holes of the resin beads. The diameter dr of the through holes can be adjusted, for example, by changing the diameter of the small holes at the die outlet for forming the through holes. Furthermore, the average outer diameter and average wall thickness of the expanded beads can be adjusted to fall within the desired ranges by adjusting the particle diameter and average mass of the resin beads.

[0090] The average pore diameter dr of the through holes of the resin particles is preferably less than 0.8 mm, and more preferably less than 0.2 mm. Furthermore, if the average pore diameter dr is less than 0.2 mm, the average pore diameter d of the through holes is 1 mm or less, and further, expanded beads having a ratio d / D of the average pore diameter d to the average outer diameter D of 0.4 or less can be more reliably produced. The average pore diameter dr of the through holes of the resin particles is preferably 0.1 mm or more. If the average pore diameter dr is within this range, the production stability of resin particles having through holes is ensured. Therefore, the numerical range of the average pore diameter dr can be, for example, a numerical range that is 0.1 mm or more and less than any one value of the group consisting of 0.8 mm and 0.2 mm.

[0091] For the same reasons as those described above for the preferred range of the ratio d / D of the average pore diameter d to the average outer diameter D of the expanded beads, the ratio dr / D of the average pore diameter dr to the average outer diameter Dr of the resin particles is preferably 0.4 or less, more preferably 0.3 or less, even more preferably 0.25 or less, and particularly preferably 0.2 or less. The ratio dr / D of the average pore diameter dr to the average outer diameter Dr of the resin particles is preferably 0.1 or more. Therefore, the numerical range of the ratio dr / Dr can be, for example, a numerical range that is 0.1 or more and equal to or less than any one value in the group consisting of 0.4, 0.3, 0.25, and 0.2.

[0092] The average pore diameter dr of the through holes of the resin particles is determined as follows. For each of a plurality of resin particles, the resin particle is cut perpendicular to the penetration direction of the through holes at a position where the cross-sectional area of ​​the resin particle is approximately maximum. Then, a photograph of the cut surface of each resin particle is taken. For each resin particle, the cross-sectional area of ​​the through hole portion (specifically, the opening area) is determined, and the diameter of a virtual perfect circle having the same area is calculated, which is used as the measured value for the pore diameter of the through holes of one resin particle. This operation is performed on 50 or more resin particles randomly selected from a large number of resin particles (a group of resin particles), and the arithmetic mean value of the measured values ​​(measured values ​​for the pore diameter of the through holes) obtained for each resin particle is used as the average pore diameter dr. Note that if the size of the through holes of each resin particle is not uniform in the penetration direction, the pore diameter of the through holes of each resin particle is determined by measurement at a position where the cross-sectional area of ​​the resin particle is approximately maximum, as described above.

[0093] The average outer diameter Dr of the resin particles is determined as follows. For each of the plurality of resin particles, one resin particle is cut perpendicular to the penetration direction of the through holes at a position where the cross-sectional area is approximately maximum. A photograph of the cut surface of each resin particle is taken to determine the cross-sectional area of ​​the resin particle (specifically, the cross-sectional area including the opening of the through holes). The diameter of a virtual circle having the same area as the cross-sectional area is calculated, and this is used as the measured value for the outer diameter of one resin particle. This operation is performed on 50 or more resin particles randomly selected from the expanded particle group, and the arithmetic mean value of the measured values ​​(measured values ​​for the outer diameter of the resin particles) obtained for each resin particle is used as the average outer diameter Dr. Note that if the outer diameter of each resin particle is not uniform in the penetration direction, the outer diameter of each resin particle is determined by measurement at a position where the cross-sectional area of ​​the resin particle in the direction perpendicular to the penetration direction is approximately maximum, as described above.

[0094] In the strand cutting method (strand cutting system), the particle diameter, length / outer diameter ratio, and average mass of the resin particles can be adjusted by appropriately changing the extrusion speed of the strand extruded from the small holes in the die, the take-up speed of the extruded strand, and the cutter speed when cutting the strand in the resin particle production process.

[0095] The expanded polyolefin resin bead molding of the present invention (hereinafter also referred to simply as expanded bead molding or molding) is obtained by in-mold molding using the expanded polyolefin resin beads, and is composed of a large number of expanded beads fused together.

[0096] Specifically, in-mold molding is performed as follows: First, foamed beads are filled into a mold having a cavity corresponding to the shape of the desired molded article. Next, a heating medium such as steam is introduced into the mold to heat the foamed beads filled in the mold. The foamed beads in the cavity further expand due to the heating and also fuse together. This integrates the foamed beads, resulting in a molded article corresponding to the shape of the cavity.

[0097] The density of the expanded bead molding is 10 kg / m 3 More than 100kg / m 3 If the density of the molded body is within this range, the light weight and rigidity of the molded body can be improved in a well-balanced manner. In order to further improve the rigidity of the molded body, the density of the molded body is preferably 20 kg / m or less. 3 In order to make the compact lighter, the compact density of the compact is preferably 80 kg / m or more. 3 More preferably, it is 50 kg / m or less. 3 Therefore, the range of the molding density of the expanded bead molding is, for example, 10 kg / m or less. 3 and 20 kg / m 3 Any one value of the group consisting of 100 kg / m or more 3 , 80 kg / m 3 and 50 kg / m 3 Numerical ranges that are equal to or less than any one value of the group consisting of:

[0098] The density of the compact (kg / m 3 ) is the volume (cm ) calculated from the weight (g) of the molded body and the external dimensions of the molded body. 3) and convert the unit. In cases where it is not easy to determine the volume from the external dimensions of the molded body, for example, because the molded body has a complex shape as a whole or in parts, the volume of the molded body can be determined by the submersion method.

[0099] As described above, the expanded bead molding of the present invention has magnesium silicate present on the surface thereof, and therefore the variation in apparent density is small.

[0100] The foamed bead molding of the present invention is obtained by molding foamed beads having through-holes in a mold, and can be used for various purposes such as packaging materials, automotive parts, and cushioning materials.

[0101] The present invention will now be described in more detail with reference to examples, although the present invention is not limited to these examples.

[0102] In the examples and comparative examples, the following raw materials were used.

[0103] (Polypropylene Resin) (1) Abbreviation "Resin 1": Ethylene-propylene random copolymer (ethylene content 3.1% by mass, melting point 151°C, density 900 kg / m 3 , melt flow rate 5 g / 10 min. (230 ° C, load 2.16 kg)) (2) Abbreviation "Resin 2": ethylene-propylene-butene random copolymer (ethylene content 3.8 mass%, butene content 3.8 mass%, melting point 135 ° C, density 900 kg / m 3 , melt flow rate 5 g / 10 min. (230 ° C, load 2.16 kg)) (3) Abbreviation "Resin 3": ethylene-propylene random copolymer (ethylene content 4.5 mass%, melting point 133 ° C, density 900 kg / m 3 , Melt flow rate 24g / 10min. (230°C, load 2.16kg)

[0104] The melt flow rates of the ethylene-propylene random copolymers indicated by the abbreviations "Resin 1" to "Resin 3" above are values ​​measured under conditions of 230°C and a load of 2.16 kg based on JIS K7210-1:2014.

[0105] The ethylene content and butene content of the ethylene-propylene random copolymers designated by the abbreviations "Resin 1" to "Resin 3" above are all values ​​determined by a known method using IR spectroscopy. Specifically, the ethylene content and butene content are determined by the method described in "Polymer Analysis Handbook" (edited by the Polymer Analysis Research Forum of the Japan Society for Analytical Chemistry, published in January 1995, published by Kinokuniya Shoten, pages 615-616 "II.2.3 2.3.4 Propylene / ethylene copolymer" and 618-619 "II.2.3 2.3.5 Propylene / butene copolymer"), in other words, by a method of quantifying the ethylene content and butene content based on the relationship between the absorbance of ethylene and butene corrected by a predetermined coefficient and the thickness of a film-like test piece.

[0106] (Dispersant: inorganic compound) (1) Abbreviated name "Dispersant 1": magnesium silicate; "Fine powder talc SG-90" manufactured by Nippon Talc Co., Ltd. (average particle size 3.0 μm, silicon dioxide content 62% by mass) (2) Abbreviated name "Dispersant 2": kaolin; "Kaolin ASP-200" manufactured by BASF Japan (average particle size 2.6 μm)

[0107] (Apparatus for Producing Multilayer Resin Particles) A ​​twin-screw extruder with an inner diameter of 50 mm was used as the extruder for forming a cylindrical foam layer (foam layer-forming extruder), and a single-screw extruder with an inner diameter of 30 mm was used as the extruder for forming a coating layer. The production apparatus was configured so that the two extruders were each connected to a multilayer strand-forming die, and co-extrusion of the foam layer-forming resin melt-kneaded material and the coating layer-forming resin melt-kneaded material was possible in a laminated state within the die. A metal fitting was attached to the tip of the outlet of the die flow path so that through holes could be formed in the strand extruded through the multilayer strand-forming die. Furthermore, the tip of the outlet of the die flow path was formed with a shape corresponding to the cross-sectional shape having the through holes (the cross-sectional shape of the multilayer resin particles).

[0108] Examples 1 to 5, Comparative Example 1, Reference Example 1 A polypropylene resin of the type shown in the "Core layer" column of Table 1, 0.05 mass% zinc borate (cell regulator), and 2.6 mass% furnace black were supplied to an extruder for forming a foam layer, and melt-kneaded to prepare a resin melt-kneaded product for forming a foam layer.

[0109] A polypropylene resin of the type shown in the "Coating layer" column in Table 1 and 2.6 mass % of furnace black were fed to the extruder for forming the coating layer, and melt-kneaded to prepare a resin melt-kneaded product for forming the coating layer.

[0110] The resin melt mixtures for forming each layer were introduced into a multilayer strand forming die and merged within the die, with the output rates of each extruder (foam layer forming extruder and coating layer forming extruder) adjusted so that the foam layer:coating layer ratio was 95:5. The foam layer forming resin melt mixture and the coating layer forming resin melt mixture were extruded through the die holes located downstream of the die, thereby obtaining multilayer strands having a two-layer structure (a sheath-core structure consisting of a cylindrical foam layer forming resin and a coating layer forming resin). The extruded strands were water-cooled and cut using a pelletizer to obtain resin particles (multilayer resin particles) with an average mass of 1.5 mg per particle.

[0111] (Production of Multilayer Expanded Beads) The amount of multilayer resin particles shown in the "Resin Particles" column in Table 1 and the amount of water shown in Table 1 were supplied into a sealed container with an internal volume of 400 L. Furthermore, relative to 100 parts by mass of the multilayer resin particles, an inorganic dispersant of the type and amount shown in the "Dispersant Type" column and the "Dispersant Blend Amount" column in Table 1, respectively, and a surfactant (trade name: NEOGEN S-20F, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., aqueous solution of sodium dodecylbenzenesulfonate) in the amount shown in Table 1 were each added to the sealed container.

[0112] Next, carbon dioxide as a blowing agent was injected into the sealed container at room temperature, and the pressure was increased to 1.0 MPa (G) in gauge pressure. In this specification, pressures marked with (G) refer to gauge pressures, i.e., pressure values ​​based on atmospheric pressure. The sealed container was then heated at a temperature increase rate of 2°C / min while stirring to the foaming temperature shown in Table 1, and carbon dioxide was injected into the sealed container and pressurized to the equilibrium vapor pressure shown in Table 1 in gauge pressure, and the inside of the sealed container was maintained at the same temperature for 6 minutes. The state of the resin particles in the sealed container was adjusted so that the resulting expanded beads would have a high-temperature peak in the endothermic curve measured by DSC.

[0113] Thereafter, the contents of the sealed container (expandable resin particles and water) were released under atmospheric pressure to obtain first-stage expanded particles (specifically, first-stage expanded particles). The production conditions for producing the first-stage expanded particles are as shown in the column of first-stage expanded particle production conditions in Table 1.

[0114]

[0115] The first-stage expanded beads obtained as described above were left to stand for 24 hours in an environment of 23°C temperature, 50% relative humidity, and 1 atm to cure the first-stage expanded beads. The cured first-stage expanded beads were then filled into a pressurizable sealed container, and the pressure inside the sealed container was increased from atmospheric pressure to pressurize the first-stage expanded beads. The pressurized state of the first-stage expanded beads was maintained, increasing the pressure inside the cells of the first-stage expanded beads, and the expanded beads were removed from the sealed container to obtain expanded beads for second-stage expansion production in which the internal pressure of the cells of the first-stage expanded beads had been pressurized. The internal pressure of the expanded beads is shown in the column for second-stage expanded bead production conditions (the column for expanded bead internal pressure) in Table 2.

[0116] The expanded beads (expanded beads for second-stage expansion production) with increased internal pressure of the cells of the first-stage expanded beads were then fed into a second-stage expansion device. Steam was supplied into this device to expand the expanded beads for second-stage expansion production. The steam pressure used to heat the first-stage expanded beads to obtain second-stage expanded beads is shown in the column for second-stage expansion conditions (heating pressure) in Table 2. The obtained expanded beads were dried at 23°C for 12 hours to obtain second-stage expanded beads. Various physical properties were measured using the second-stage expanded beads obtained by second-stage expansion, and they were further used to produce expanded bead moldings, etc. The physical properties of the obtained second-stage expanded beads are shown in Table 2.

[0117] (Production of Expanded Bead Moldings) The second-stage expanded beads were filled into a pressurizable sealed container, and the pressure inside the sealed container was increased from normal pressure to pressurize the second-stage expanded beads. The pressurized state of the second-stage expanded beads was maintained for 24 hours to increase the pressure inside the cells of the second-stage expanded beads. The second-stage expanded beads were then removed from the sealed container, and expanded beads with an internal cell pressure of 0.1 MPa (G) were obtained. These expanded beads (second-stage expanded beads with an internal cell pressure of 0.1 MPa (G)) were filled into a molding die having a molding cavity capable of molding a plate-shaped molded body measuring 300 mm long x 250 mm wide x 60 mm high, and molding was performed using the following heating method. Steam was supplied to the mold with the drain valves on both sides of the mold open to perform preheating (exhaust process). Steam was then supplied from one side of the mold to heat it, and then steam was supplied from the other side to heat it. Subsequently, steam was supplied from both sides of the mold to heat it. After heating, the pressure was released and the molded product was water-cooled until the surface pressure due to the foaming force of the molded product reached 0.04 MPa (G), after which the mold was opened and the molded product was removed. This molded product was cured in an oven at 80°C for 12 hours and then slowly cooled to room temperature to obtain a plate-like molded product. The physical properties of the obtained molded product are shown in Table 2.

[0118]

[0119] Examples 1 to 5 are examples in which expanded beads were produced under the same conditions except for varying the amount of magnesium silicate used as a dispersant. Comparing Examples 1 to 5, it was shown that the water content decreased as the amount of magnesium silicate increased, and that the variation in the expansion ratio of the resulting expanded beads was small, which in turn resulted in small variation in the density of the resulting molded body.

[0120] In Reference Example 1, expanded beads were produced in the same manner as in Example 3, except that kaolin was used as a dispersant and no through-holes were formed. Since no through-holes were formed, it was clear that no variation in the compact density occurred even in the absence of magnesium silicate. In Comparative Example 1, expanded beads were produced in the same manner as in Example 3, except that kaolin was used as a dispersant. The moisture content of the resulting first-stage expanded beads was high, and the compact densities of the resulting compacts varied greatly.

[0121] The bulk density, high temperature peak calorific value, moisture content and residual magnesium silicate ratio of the first-stage expanded beads in Table 1 were measured by the methods described above.

[0122] The bulk density, average outer diameter D, average pore diameter d, average wall thickness t, and length in the penetration direction L of the second-stage expanded beads in Table 2 were measured by the methods described above.

[0123] The average cell diameter of the expanded beads in Table 2 was measured as follows. (Average Cell Diameter) An expanded bead was roughly divided into two halves passing through the center of the expanded bead, and a photograph of the cross section was taken using a scanning electron microscope. In the obtained cross-sectional photograph, four line segments were drawn at equal angles from the outermost surface of the expanded bead through the center to the outermost surface on the opposite side. The number of cells intersecting each line segment was counted, and the total length of the four line segments was divided by the total number of cells intersecting the lines to obtain the average cell diameter of one expanded bead. This procedure was performed on 10 randomly selected expanded beads, and the arithmetic mean of the values ​​obtained for each expanded bead was used as the average cell diameter of the two-stage expanded beads in this specification.

[0124] The lower limit molding pressure in Table 2 was determined based on the following definition. The following evaluation criteria were adopted for the moldable pressure range and water cooling time evaluation in Table 2. The physical properties of the molded body, such as fusion and moldability (density variation of the molded body), were evaluated based on the following criteria.

[0125] (Moldable pressure range) Using the above-mentioned molding method, molding pressure (molding heating steam pressure) is increased by 0.02 MPa in a wide molding pressure range, molding is carried out at each molding pressure.The obtained molded body is evaluated from the viewpoint of secondary foaming property, fusion property and recovery property, and the molding pressure that can obtain a molded body that passes all the criteria is defined as moldable pressure, and this moldable pressure is evaluated as A (very good) when it is 2 points or more, B (good) when it is 1 point, and C (bad) when it is not within the range, and these are listed in the column of moldable pressure range in Table 1.

[0126] (Lower Limit Molding Pressure) The lowest molding pressure within the above moldable pressure range was defined as the lower limit molding pressure. The values ​​of the lower limit molding pressure are as shown in Table 2.

[0127] (Evaluation of Water-Cooling Time) The evaluation of water-cooling time was based on the water-cooling time at the above-mentioned lower limit molding pressure. The evaluation of water-cooling time was based on the following criteria. That is, a water-cooling time of 80 seconds or less was evaluated as A (excellent), more than 80 seconds but less than 100 seconds was evaluated as B (excellent), and 100 seconds or more was evaluated as C (poor). The evaluation results are as shown in Table 2.

[0128] (Fusing Property) A cut was made along the edge of the obtained molded article to approximately the center of the molded article with a sharp blade, and the cut portion was then broken by hand. The total number of foamed beads and the number of broken foamed beads present on the broken surface were counted. The ratio (%) of the number of broken foamed beads to the total number of foamed beads was calculated. The calculated value was taken as the broken foamed bead ratio. The fusing property was evaluated based on the broken foamed bead ratio. In the evaluation of the broken foamed bead ratio, a ratio of 90% or more was evaluated as A (very good), a ratio of more than 70% but less than 90% was evaluated as B (good), and a ratio of 70% or less was evaluated as C (poor). The evaluation results are as shown in Table 2.

[0129] (Moldability (density variation of compacted body)) Moldability (density variation of compacted body) was evaluated based on the variation in density of the compacted body when the molding method was performed multiple times. Specifically, molding was performed repeatedly (10 times) using the molding method and the conditions of the lower limit molding pressure. The density of each of the 10 compacts obtained by the 10 molding operations was measured, and the average value of the 10 compacts was calculated. For the evaluation of moldability (density variation of compacted body), those whose densities were all within the range of ±5% or less of the average value were evaluated as A (very good), those whose densities were "more than ±5% and less than ±10%" of the average value were evaluated as B (good), and those whose densities were "more than ±10% and more than ±5%" of the average value were evaluated as C (poor). The evaluation results are as shown in Table 2.

[0130] Table 2 shows the magnesium silicate content and water content of the surface portion of the expanded beads, as well as an evaluation of the variation in expansion ratio.

[0131] (Ratio of Magnesium Silicate in Surface Portions) The ratio of magnesium silicate in the surface portions of expanded beads was measured by the following method. First, the multilayer resin particles used in the production of the multilayer expanded beads and the resulting multilayer expanded beads were prepared. The composition of the particles themselves was not changed in the process of obtaining multilayer expanded beads from the multilayer resin particles. Furthermore, magnesium silicate was attached to the surfaces of the multilayer expanded beads during the dispersion process. Therefore, the ash content (A1: wt%) of the multilayer expanded beads and the ash content (A2: wt%) of the multilayer resin particles before dispersion in an aqueous medium were measured, and the ash content (A2: wt%) of the multilayer expanded beads was subtracted from the ash content (A1: wt%) of the multilayer expanded beads to calculate the amount of magnesium silicate attached to the surface portions of the expanded beads, which was defined as the ratio of magnesium silicate present in the surface portions of the expanded beads.

[0132] The ash content was measured in accordance with JIS K 6226-2. A LECO TGA701 thermogravimetric analyzer was used. Approximately 5 g of foamed particles were collected as a measurement sample and placed in a crucible. A nitrogen gas flow was applied to the heating furnace. (1) Under a nitrogen atmosphere, the temperature of the heating furnace was increased from room temperature to 105°C at a heating rate of 10°C / min. The foamed particles were then heated at 105°C until the measured weight reached equilibrium. (2) The foamed particles were then maintained at 105°C until the measured weight reached equilibrium. (3) The foamed particles were then heated from 105°C to 450°C at a heating rate of 10°C / min. (4) The foamed particles were maintained at 450°C until the measured weight reached equilibrium. (5) The furnace air flow was changed from nitrogen to air, and the foamed particles were then heated from 450°C to 950°C at a heating rate of 10°C / min. (6) The weight W1 of the combustion residue after 10 minutes at 950°C was determined. (7) The combustion residue was then cooled to room temperature. The weight W1 of the combustion residue was divided by the weight of the measurement sample placed in the crucible, and the resulting value was multiplied by 100 to obtain the ash content A1 (wt%) in the expanded beads. The ash content A2 (wt%) in the resin beads was also measured in the same manner, and the proportion As of magnesium silicate present in the surface portion of the expanded beads was calculated using the following formula (2): A2 - A1 = As (wt%) (2)

[0133] (Moisture Content) The moisture content of expanded beads was measured by the following method. Expanded beads produced by the expansion process or two-stage expansion process and immediately after curing were weighed to prepare a measurement sample. Next, using a halogen moisture meter (HX204) manufactured by METTLER TOLEDO, the measurement sample was heated to a temperature of 100°C and maintained at 100°C for 60 seconds until no weight change occurred. Then, the measurement sample was further heated to 160°C and maintained at 160°C for 90 seconds until no weight change occurred, thereby vaporizing the moisture inside the measurement sample. The weight loss due to heating was divided by the weight of the expanded beads before heating and converted to a percentage to calculate the moisture content (%).

[0134] (Evaluation of Variation in Expansion Ratio) The variation in expansion ratio for each of the first-stage expanded beads and the second-stage expanded beads was evaluated based on the magnitude of variation in the bulk density of the resulting expanded beads. The bulk density of the expanded beads was measured by the following method. First, the expanded beads to be measured were left for 24 hours or more in an environment of 23°C temperature, 50% relative humidity, and 1 atm. Then, a mass W (unit: g) of expanded beads was filled into a measuring cylinder, and the bottom of the measuring cylinder was lightly tapped against the floor several times to stabilize the filling height of the expanded beads in the measuring cylinder. The bulk volume V (unit: L) of the expanded beads indicated by the graduations on the measuring cylinder was read, and the mass W of the expanded beads was divided by the bulk volume V of the expanded beads (i.e., W / V). The value obtained in this manner was expressed as kg / m 3 The same measurement was repeated 10 times for different samples, and the average was calculated to obtain the bulk density (unit: kg / m) of the expanded beads. 3 ) was obtained.

[0135] The evaluation of the variation in expansion ratio was carried out by rating A (very good) if all ten measurements were within the range of ±5% of the average value of the obtained ten measurements, B (good) if any of the ten measurements were within the range of "more than ±5% and ±10%" of the average value, and C (poor) if any of the ten measurements were within the range of ±10% of the average value. The evaluation results of the variation in expansion ratio are as shown in Tables 1 and 2.

[0136] In Examples 1 to 5, talc was used as "Dispersant 1." That is, magnesium silicate that forms talc was used as the magnesium silicate. In Examples 1 to 5, the amount of talc present on the surface of the second-stage expanded particles was measured. Specifically, the amount of talc present was determined using the following method.

[0137] (Amount of talc present on the surface of expanded beads (amount of talc present on the surface)) (Procedure 1) Preparation of a calibration curve A calibration curve defining the relationship between the amount of talc present and the absorption intensity described below was established as follows. First, in order to prepare the calibration curve, a solid sheet (a sheet of polypropylene resin with a known talc content) (thickness of the solid sheet: 50 μm) was prepared by kneading a predetermined amount of talc into polypropylene resin. The kneader used to prepare the solid sheet was an MC-15HT manufactured by Xplore. Talc and polypropylene resin were kneaded using the kneader under conditions of 200°C, 50 rpm, and 3 minutes to obtain polypropylene pellets. The polypropylene pellets were then formed into a solid sheet at 200°C using a heat press, and further cooled to room temperature to prepare a sheet with a thickness of approximately 50 μm. The sheet surface of this "solid sheet in which talc is kneaded into a polypropylene-based resin" was brought into close contact with a prism and measured by the ATR method using an infrared spectrophotometer, and the infrared absorption spectrum of the solid sheet was obtained. Based on the infrared absorption spectrum of the solid sheet, a peak attributable to talc was observed at a wavelength of 1000 cm -1 A peak recognized around the wavelength of 650 cm (referred to as the first absorption peak) -1 A peak recognized near the first absorption peak (referred to as the second absorption peak) was identified. Based on the infrared absorption spectrum of the solid sheet, two types of calibration curves were created that define the relationship between the absorption intensity (absorbance value) at these absorption peaks and the amount of talc added to the solid sheet (amount of talc present). The two types of calibration curves define the relationship between the absorption intensity at the first absorption peak and the amount of talc present (wavelength 1000 cm). -1 The first calibration curve is based on an absorption peak near the wavelength of 650 cm. The second calibration curve defines the relationship between the absorption intensity at the second absorption peak and the amount of talc present. -1 (Procedure 2) Measurement of Samples The expanded beads prepared in each step were subjected to a pressure of 340 kg / cm on the surface of the expanded beads of the measurement sample under the following measurement conditions. 2The expanded beads were pressed tightly against the prism with a pressing force of 0.05 sq. m, and infrared light was incident on them. The totally reflected light was measured, and an infrared absorption spectrum (without ATR correction) was obtained. The expanded beads were used as they were as the measurement specimens. Each expanded bead was cut into approximately two equal halves passing through its center so that the volumes were roughly equal, to obtain measurement specimens. The cut surface of the measurement specimen was pressed tightly against the prism, and infrared light was incident on it in the same manner as above, and the totally reflected light was measured, and an infrared absorption spectrum (without ATR correction) was obtained. The difference spectrum between the two spectra was the infrared absorption spectrum corresponding to the talc present on the surface of the expanded beads. (Procedure 3) Calculation of the amount of talc present on the surface of the expanded beads. The 1000 cm wavelength was used as the calibration curve prepared in Procedure 1. -1 The first calibration curve was created using a peak near the wavelength of 650 cm. -1 The amount of talc present on the surface of the expanded beads was calculated from the difference spectrum measured in step 2, i.e., the infrared absorption spectrum corresponding to the talc present on the surface of the expanded beads, using the second calibration curve prepared by employing the peaks around the wavelength of 1000 cm mentioned above. -1 The amount of talc present on the surface of the expanded beads was calculated using the first calibration curve created by using a peak in the vicinity of the wavelength of 1000 cm. -1 If an accurate difference spectrum around 650 cm cannot be determined, -1 The amount of talc present on the surface of the expanded beads was calculated using a second calibration curve prepared using a peak in the vicinity of the wavelength of 1000 cm. -1 When an accurate difference spectrum cannot be determined in the vicinity of the wavelength of 1000 cm, for example, when determining the infrared absorption spectrum (difference spectrum) of the surface portion of the expanded beads measured in (Procedure 2), -1 This may occur when the absorbance of a peak in the vicinity is equal to or greater than the upper limit detectable by measurement using an infrared spectrophotometer. <Measurement conditions> Prism: zinc selenide Incident angle of infrared light: 45° Number of accumulations: 512 Resolution: 4 cm -1 Detector: TGS (Triglycine sulfate) Measurement wave number range: 600 to 4000 cm -1Number of reflections: 1 Measurement area: Area up to 20 μm from the surface Apparatus: FT / IR-4600 type A (ATR PRO450-S type) manufactured by JASCO Corporation

Claims

1. A polyolefin resin expanded bead having through holes, characterized in that magnesium silicate is present on the surface portion of the expanded bead, and the proportion of magnesium silicate present on the surface portion of the expanded bead is 0.1 mass% or more.

2. The expanded polyolefin resin beads according to claim 1, wherein the average pore diameter d of the through holes of the expanded polyolefin resin beads is 0.1 mm or more and 5 mm or less.

3. The polyolefin resin expanded particles according to claim 2, wherein the average pore diameter d of the through holes of the polyolefin resin expanded particles is 0.1 mm or more and less than 1 mm, and the ratio d / D of the average pore diameter d to the average outer diameter D of the polyolefin resin expanded particles is 0.4 or less.

4. The polyolefin resin expanded beads according to claim 3, wherein the average outer diameter D of the polyolefin resin expanded beads is 2 mm or more and 5 mm or less, and the average wall thickness t is 0.9 mm or more and 2 mm or less.

5. The expanded polyolefin resin beads according to any one of claims 1 to 4, wherein the length L of the through holes in the expanded polyolefin resin beads in the penetration direction is 2 mm or more and 6 mm or less.

6. The expanded polyolefin resin particles according to any one of claims 1 to 5, wherein the water content of the expanded polyolefin resin particles is from 0.1% by mass to 2.5% by mass.

7. The polyolefin resin expanded particles according to any one of claims 1 to 6, wherein the polyolefin resin expanded particles have a polyolefin resin foamed layer and a polyolefin resin coating layer, and the coating layer covers all or a part of the foamed layer.

8. A polyolefin resin foamed bead molding obtained by molding the foamed beads according to any one of claims 1 to 7 in a mold.

Citation Information

Patent Citations

  • Manufacture of foam molded body with skin and foam molded body with skin

    JP1999207759A

  • Method for producing molded article of foamed polyolefin resin particle and foamed polyolefin resin particle for in-mold molding

    JP2012082307A

  • Method of manufacturing composite thermoplastic resin particle, foaming composite thermoplastic resin particle, composite thermoplastic resin foamed particle, and composite thermoplastic resin foamed particle molding

    JP2012102201A

  • Polypropylene-based resin foam particle, and foam particle molding

    JP2022096231A

  • Foamed particle and method for producing the same

    JP2022127578A