Method for producing polysaccharide-containing article having improved thermal stability
The method of absorbing an aqueous medium with reactive compounds into polysaccharide articles to adjust the aqueous medium ratio addresses the low thermal stability of polysaccharides, ensuring uniform thermal stability and preventing color issues, enhancing their performance in applications like resin compositions.
Patent Information
- Application Number
- PCT/JP2024/018974
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Polysaccharides like cellulose have low thermal stability, leading to deformation and discoloration when heated, resulting in poor performance and appearance issues in products such as cellulose fiber-containing resin compositions, and existing methods to improve stability, such as using polyhydric alcohol or boric acid, often result in uneven thermal stability and surface precipitation.
A method involving the absorption of an aqueous medium containing a compound that reacts with the reducing end or hydroxyl group of polysaccharides, with the aqueous medium ratio adjusted to 10-1000% by mass before drying, to enhance thermal stability uniformly across articles.
The method achieves uniformly improved thermal stability, preventing coloration and color unevenness when heated, and reduces the heating weight loss rate of polysaccharide-based articles, making them suitable for use in various applications including resin modifiers and reinforcing materials.
Smart Images

Figure JP2024018974_05122024_PF_FP_ABST
Abstract
Description
Method for producing polysaccharide-containing articles with improved thermal stability
[0001] The present invention relates to a method for making polysaccharide-containing articles having improved thermal stability.
[0002] Polysaccharides, such as cellulose, starch, and hemicellulose, are used in a variety of products. For example, in industry, they are used in a wide range of fields, including food, cosmetics, toiletries, oral care, pharmaceuticals, adhesives, papermaking, medicine, and mining. Polysaccharides used in these fields are generally prepared in the form of powder, fiber, film, or the like. Furthermore, because most polysaccharides are naturally occurring polymeric substances, they are attracting attention as biomass-derived materials with low environmental impact.
[0003] In recent years, in response to growing environmental awareness, biomass-derived polysaccharide powders and fibers have been used as resin modifiers and reinforcing materials (see, for example, Patent Document 1). However, polysaccharides such as cellulose have low thermal stability, and heating can cause deformation and discoloration of the appearance, resulting in performance degradation. Therefore, for example, in cellulose fiber-containing resin compositions, when preparing the resin composition or when obtaining a molded article from the resin composition, the cellulose fibers can become discolored by heating, resulting in poor appearance.
[0004] As a method for improving the thermal stability of polysaccharides such as cellulose, for example, Patent Document 2 proposes a method in which an aqueous solution of a polyhydric alcohol is dropped onto cellulose filter paper, followed by drying for 24 hours in an oven at 105° C. Furthermore, Patent Document 3 proposes a method for producing cellulose in which boric acid water is added to fine cellulose powder, followed by heat treatment at 105° C. for 24 hours or more, thereby suppressing yellowing and blackening at temperatures of 300° C. or less.
[0005] JP 2018-024967 A JP 2010-159364 A JP 2008-163053 A
[0006] In the examples of Patent Documents 2 and 3, 15 to 70 times the amount of the aqueous solution or boric acid solution is dropped onto 100 parts by mass of cellulose filter paper or cellulose fine powder, and a drying process is carried out in this state. The inventors of the present application have found that the methods described in Patent Documents 2 and 3 may result in uneven improvement in thermal stability, such as precipitation of boric acid on the surface of the article or dark coloration of parts of the surface of the article. Therefore, an object of the present invention is to provide a method for producing an article containing a polysaccharide, which can produce an article with uniformly improved thermal stability.
[0007] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by having a polysaccharide-containing article absorb an aqueous medium containing a compound (A) capable of reacting with a reducing end or a hydroxyl group of a polysaccharide, and then adjusting the amount of aqueous medium coexisting with the article to a certain value or less before drying, thereby completing the present invention. That is, the present invention has the following aspects: [1] A method for producing a polysaccharide-containing article having improved thermal stability, comprising: allowing the article to absorb an aqueous medium containing a compound (A) capable of reacting with a reducing end or a hydroxyl group of the polysaccharide (step (I)); adjusting the proportion of the aqueous medium to be 10 to 1,000 mass% relative to the total mass of the article before absorbing the aqueous medium (step (II)); and drying the article (step (III)). [2] The method for producing an article containing a polysaccharide according to [1], wherein the compound (A) comprises at least one compound selected from a glycosylating agent (a1) for a reducing end of the polysaccharide and an esterifying agent (a2) for a hydroxyl group of the polysaccharide. [3] The method for producing an article containing a polysaccharide according to [2], wherein the glycosylating agent (a1) comprises a monohydric or higher alcohol, and the esterifying agent (a2) comprises boric acid. [4] The method for producing an article containing a polysaccharide according to any one of [1] to [3], wherein the article is a fibrous material, and the step (I) comprises absorbing 100 parts by mass or more of the aqueous medium per 100 parts by mass of the fibrous material, and the step (II) comprises adjusting the proportion of the aqueous medium to 10 to 200% by mass with respect to the total mass of the fibrous material before absorbing the aqueous medium. [5] The method for producing an article containing a polysaccharide according to any one of [1] to [3], wherein the article is a powder of 10 mesh or larger, and the step (II) includes adjusting the proportion of the aqueous medium to 30 to 500 mass% with respect to the total mass of the powder before absorbing the aqueous medium.[6] The method for producing an article containing a polysaccharide according to any one of [1] to [3], wherein the article is a plate-like article or a film, wherein step (I) comprises absorbing 50 parts by mass or more of the aqueous medium per 100 parts by mass of the plate-like article or the film, and step (II) comprises adjusting the proportion of the aqueous medium to 20 to 200% by mass with respect to the total mass of the plate-like article or the film before absorbing the aqueous medium. [7] The method for producing an article containing a polysaccharide according to any one of [1] to [3], wherein the article is a cotton-like article, wherein step (I) comprises absorbing 100 parts by mass or more of the aqueous medium per 100 parts by mass of the cotton-like article, and step (II) comprises adjusting the proportion of the aqueous medium to 30 to 800% by mass with respect to the total mass of the cotton-like article before absorbing the aqueous medium. [8] The method for producing an article containing a polysaccharide according to any one of [1] to [7], wherein step (III) comprises drying the article at room temperature to 300°C. [9] The method for producing an article containing a polysaccharide according to any one of [1] to [8], wherein the concentration of the compound (A) in the aqueous medium in the step (I) is 0.1 to 50% by mass.
[0008] According to the present invention, a method for producing an article containing a polysaccharide can be provided, which allows the production of an article having uniformly improved thermal stability.
[0009] 1 is a photograph of the regenerated cellulose fibers of Examples 1 to 2 and Comparative Examples 1 to 3 after annealing. 2 is a graph showing the results of measuring the rate of weight loss upon heating by TG-DTA for Examples 9 to 16 and Comparative Example 1.
[0010] An embodiment of the present disclosure will be described in detail below. However, the scope of the present disclosure is not limited to the embodiment described herein, and various modifications can be made without departing from the spirit of the present disclosure. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. Furthermore, when multiple upper and lower limits are described for a particular parameter, any of these upper and lower limits can be combined to form a suitable numerical range. Furthermore, the lower and / or upper limits of a numerical range described in this disclosure are numerical values within that range and may be replaced with numerical values shown in the examples. The expression "X to Y" indicating a numerical range means "X or more and Y or less." If a specific description described for one embodiment also applies to other embodiments, that description may be omitted in other embodiments.
[0011] The configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible as appropriate without departing from the spirit of the present disclosure. The present disclosure is not limited to the embodiments. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification.
[0012] [Method for producing an article containing a polysaccharide] This embodiment relates to a method for producing an article containing a polysaccharide having improved thermal stability, the method comprising: allowing the article to absorb an aqueous medium containing a compound (A) capable of reacting with the reducing end or hydroxyl group of the polysaccharide (step (I)); adjusting the proportion of the aqueous medium to be 10 to 1,000 mass% relative to the total mass of the article before absorbing the aqueous medium (step (II)); and drying the article (step (III)). In this specification, the "reducing end of a polysaccharide" refers to the end of the molecular chain of the polysaccharide at which a glycosidic hydroxy group is present.
[0013] <Polysaccharides> Polysaccharides are a general term for long chains of monosaccharides such as glucose and mannose, and in a broad sense refer to carbohydrates obtained by the bonding of 10 or more monosaccharides. Polysaccharides contained in the article according to this embodiment typically include cellulose, but other examples include starch (e.g., amylose, amylopectin, etc.), hemicellulose (e.g., xylan, glucomannan, galactan, etc.), mannan, chitin, chitosan, etc. Furthermore, the article according to this embodiment may contain one type of these polysaccharides alone or two or more types. Of these, it is preferable to contain cellulose, which is highly versatile.
[0014] Cellulose is a plant-derived polysaccharide found in, for example, wood, cotton, hemp, ramie, linen, hemp, jute, Manila hemp, sisal, etc. When the article according to the present embodiment contains cellulose, the cellulose may be natural cellulose or regenerated cellulose. When regenerated cellulose is used, the method for producing it is not particularly limited, and examples thereof include solvent-based regenerated cellulose such as viscose rayon, lyocell, cupra, and ionic liquid.
[0015] According to the manufacturing method of this embodiment, an article with uniformly improved thermal stability can be manufactured. In this specification, the term "polysaccharide-containing article" refers to any article containing polysaccharides as a main component of the components constituting the article. Furthermore, the term "containing polysaccharides as a main component" means that the polysaccharides account for more than 50% by mass of the total amount (100% by mass) of all components constituting the article. This proportion may be 60% by mass or more, 70% by mass or more, 80% by mass or more, or 90% by mass or more.
[0016] <Step (I)> The production method according to this embodiment includes allowing an article containing a polysaccharide to absorb an aqueous medium containing a compound (A) capable of reacting with the reducing end or hydroxyl group of a polysaccharide (step (I)). The production method according to this embodiment includes allowing the article to absorb the aqueous medium containing the compound (A), thereby causing a reaction between the reducing end or hydroxyl group of the polysaccharide in the article and the compound (A). Note that "allowing the article to absorb the aqueous medium" includes not only taking in the aqueous medium into voids within the article (water absorption), but also the article absorbing the aqueous medium and swelling. Furthermore, in the final article, the compound (A) may have reacted with the reducing end or hydroxyl group of the polysaccharide in the article, or may be immobilized on the surface of the article.
[0017] (Aqueous medium) The aqueous medium may be an aqueous solution of the compound (A), or an emulsion (dispersion) in which the compound (A) is dispersed. The water component contained in the aqueous medium may be pure water, ion-exchanged water, tap water, industrial water, or a mixture thereof. From the viewpoint of cost, the water component is preferably tap water or industrial water.
[0018] (Compound (A) Reactive with Reducing End or Hydroxyl Group of Polysaccharide) The aqueous medium contains a compound (A) reactive with a reducing end or hydroxyl group of a polysaccharide. The compound (A) may have a structure capable of chemically reacting with the reducing end or hydroxyl group of the polysaccharide, or may be a compound having a structure capable of physically reacting with the reducing end or hydroxyl group of the polysaccharide. The position of the reducing end or hydroxyl group of the polysaccharide that can react with the compound (A) is not particularly limited. Among these, from the viewpoint of the effect of improving thermal stability, it is preferable to contain at least one compound selected from a glycosylating agent (a1) for the reducing end of the polysaccharide and an esterifying agent (a2) for the hydroxyl group of the polysaccharide.
[0019] Glycosylating Agent (a1) In one embodiment, compound (A) can contain a glycosylating agent (a1) for the reducing end of a polysaccharide. The term "glycosylating agent" refers to any compound capable of glycosylating the reducing end of a polysaccharide. The glycosylating agent (a1) is not particularly limited as long as it is a compound capable of glycosylating the reducing end of a polysaccharide. However, from the viewpoint of facilitating glycosylation of the reducing end, it is preferable that the glycosylating agent (a1) contains a monohydric or higher alcohol.
[0020] Examples of the monohydric or higher alcohol include, for example, alcohols having 1 to 20 carbon atoms. Specific examples include monohydric alcohols such as methanol, ethanol, propanol, isopropanol, butanol, ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, benzyl alcohol, and phenethyl alcohol; linear polyhydric alcohols such as mannitol, glycerin, erythritol, pentaerythritol, xylitol, glucitol, and ethylene glycol; and phenols such as phenol, para-cresol, meta-cresol, ortho-cresol, ethylphenol, guaiacol, and catechol. These may be used alone or in combination of two or more. Among these, from the viewpoint of more effectively glycosylating the reducing end, glycerin, mannitol, pentaerythritol, methanol, or ethylene glycol is preferred, and glycerin, mannitol, or pentaerythritol is more preferred.
[0021] When a glycosylating agent (a1) is used as compound (A), the ratio of the glycosylating agent (a1) to the total mass of the aqueous medium (the concentration of the glycosylating agent (a1)) is preferably 0.1 to 50% by mass, more preferably 0.5 to 20% by mass, and particularly preferably 1 to 15% by mass. In one embodiment, the concentration of the glycosylating agent (a1) may be 0.1 to 5% by mass, 0.1 to 3% by mass, or 0.1 to 1% by mass. By having an article absorb an aqueous medium having a glycosylating agent (a1) concentration within the above range, the thermal stability of the article is likely to be improved.
[0022] Esterifying Agent (a2) In one embodiment, the compound (A) can contain an esterifying agent (a2) for the hydroxyl groups of a polysaccharide. The term "esterifying agent" refers to any compound capable of esterifying the hydroxyl groups of a polysaccharide. The esterifying agent (a2) is not particularly limited as long as it is a compound capable of esterifying the hydroxyl groups of a polysaccharide. However, from the viewpoint of avoiding destruction of the internal structure of the polysaccharide by the esterifying agent (a2), it is preferable for the esterifying agent (a2) to contain a weak acid such as acetic acid, boric acid, or a boric acid compound, more preferably boric acid or a boric acid compound, and even more preferably boric acid.
[0023] Examples of the boric acid compound include borate salts such as alkali metal salts, alkaline earth metal salts, and metal salts; metaboric acid and its salts; polyboric acid and its salts; etc. These boric acid compounds may be used alone or in combination of two or more.
[0024] When the esterifying agent (a2) is used as the compound (A), the proportion of the esterifying agent (a2) relative to the total mass of the aqueous medium (the concentration of the esterifying agent (a2)) is preferably 0.1 to 50 mass%, more preferably 0.5 to 20 mass%, and particularly preferably 1 to 15 mass%. By having the article absorb an aqueous medium having an esterifying agent (a2) concentration within the above range, the thermal stability of the article is likely to be improved.
[0025] In one embodiment, from the viewpoint of the efficiency of improving thermal stability, the compound (A) preferably contains an esterifying agent (a2), more preferably boric acid. In one embodiment, from the viewpoint of easily reducing the rate of weight loss upon heating of the article, the compound (A) may contain boric acid as the esterifying agent (a2). From the same viewpoint, the compound (A) may contain a glycosylating agent (a1), which may contain glycerin, pentaerythritol, or mannitol.
[0026] The compound (A) may contain other compounds in addition to the glycosylation agent (a1) and the esterification agent (a2). Examples of the other compounds include aluminum hydroxide, calcium hydroxide, dolomite, hydrotalcite, calcium hydroxide, barium hydroxide, basic magnesium carbonate, zirconium hydroxide, and metal hydrates such as tin oxide hydrate. The other compounds may be used alone or in combination of two or more.
[0027] In step (I), the method for absorbing the aqueous medium containing compound (A) into the article is not particularly limited, and any method can be adopted depending on the form of the article. For example, the article may be immersed in a container containing the aqueous medium (immersion method), or the aqueous medium may be dripped onto the article (including spraying method) (dropping method). Since the production method according to this embodiment includes step (II) of adjusting the ratio of aqueous medium to the article, the amount of aqueous medium absorbed in step (I) is not particularly limited. However, from the viewpoint of enhancing the thermal stability improving effect, it is preferable to set the amount of aqueous medium absorbed in the range of 10 to 1,000 parts by mass per 100 parts by mass of the article. Furthermore, it is more preferable to adjust the amount of aqueous medium absorbed depending on the form of the article. Preferred embodiments depending on the form of the article will be described later.
[0028] The temperature of the aqueous medium can be set depending on the solubility of compound (A) in the water component. For example, in the case of boric acid, the saturated aqueous solution concentration at 20°C is less than 5% by mass. Therefore, for example, to prepare a 9% by mass aqueous solution, it is preferable to set the temperature of the aqueous medium to 50°C or higher.
[0029] When the immersion method is employed in step (I), since polysaccharides basically easily absorb water, the time for immersing the article in the aqueous medium can be set to 1 minute or less for articles other than cotton-like articles. In the case of cotton-like articles, it is necessary to thoroughly remove the air trapped inside, so it is preferable to release the air inside the cotton-like article as bubbles to the outside while immersing the cotton-like article in the aqueous medium.
[0030] In the case of the dropping method, any speed and amount of dropping can be set within the range in which the amount of aqueous medium absorbed into the article is the aforementioned preferred amount, but for example, the amount of dropping per second per gram of article is preferably 1 to 500 drops / second, more preferably 1 to 350 drops / second, and even more preferably 10 to 200 drops / second. In one embodiment, the amount of dropping may be 0.005 to 25 mL / second, 0.05 to 25 mL / second, 0.05 to 17.5 mL / second, or 0.5 to 10 mL / second.
[0031] In a preferred embodiment, step (I) may include allowing the article to absorb an aqueous medium to adhere compound (A) to the article. The concentration of compound (A) and the amount of absorbed aqueous medium may be adjusted so that the amount of adhered compound (A) is 0.1 to 20 parts by mass, more preferably 0.3 to 15 parts by mass, per 100 parts by mass of the article. By adhering compound (A) to the article, preferably to at least a portion of the surface of the article, the thermal stability improvement effect tends to be uniform. In a preferred embodiment, the amount of adhered compound (A) may be 0.01 to 20 parts by mass, 0.01 to 10 parts by mass, or 0.03 to 5 parts by mass, per 100 parts by mass of the article. This embodiment is preferably performed when the article includes a fibrous material and compound (A) includes boric acid or a glycosylation agent (a1) (preferably glycerin, pentaerythritol, or mannitol). In this case, an article with a lower rate of weight loss upon heating is more likely to be obtained.
[0032] <Step (II)> The manufacturing method according to this embodiment includes adjusting the proportion of the aqueous medium to 10 to 1,000 mass% relative to the total mass of the article before the aqueous medium is absorbed (step (II)). In this way, by absorbing an aqueous medium containing compound (A) into the article and then adjusting the amount of aqueous medium relative to the article within a certain range, an article with uniformly improved thermal stability can be manufactured regardless of the shape of the article. As mentioned above, the "total mass of the article" in step (II) refers to the total mass of the article before the aqueous medium is absorbed. Hereinafter, the "proportion of the aqueous medium relative to the total mass of the article before the aqueous medium is absorbed" will be referred to as the "aqueous medium ratio." The amount of compound (A) adhering to the article can be adjusted by controlling the concentration of compound (A) in the aqueous medium and the aqueous medium ratio.
[0033] According to this embodiment, if the aqueous medium ratio is less than 10% by mass, the effect of improving the thermal stability of the resulting article is insufficient. On the other hand, if the aqueous medium ratio exceeds 1,000% by mass, the drying efficiency in step (III) deteriorates. Furthermore, the effect of improving thermal stability becomes non-uniform, so the aqueous medium ratio must be 1,000% by mass or less. In one embodiment, the aqueous medium ratio is preferably 10 to 800% by mass, more preferably 10 to 700% by mass, even more preferably 20 to 600% by mass, and particularly preferably 30 to 500% by mass.
[0034] Step (II) preferably includes dehydrating the article that has absorbed the aqueous medium (step (II-1)) and calculating the aqueous medium ratio of the article after dehydration (step (II-2)). Depending on the form of the article, it is preferable to adjust the aqueous medium ratio to a more preferable range within the range of 10 to 1,000 mass % before carrying out step (III). By adjusting the aqueous medium ratio to a more preferable range, the uniformity of the thermal stability improving effect tends to be improved. Therefore, it is preferable to calculate the aqueous medium ratio after carrying out the dehydration treatment (step (II-1)). The preferable range of the aqueous medium ratio depending on the form of the article will be described later.
[0035] The dehydration treatment (step (II-1)) is not particularly limited as long as it is a method capable of dehydrating excess aqueous medium from the article, but generally, compression dehydration, centrifugal dehydration, vibration dehydration, etc. can be used. Any conditions for the dehydration treatment can be used depending on the form of the article. Furthermore, a plurality of dehydration methods may be combined.
[0036] The method for calculating the aqueous medium ratio in step (II-2) is to first measure the weight (W1) of the article before performing step (I). Then, step (I) is performed, and the weight (W2) of the article after absorbing the aqueous medium is measured. When step (I) is performed by the immersion method, the article may be temporarily recovered from the container containing the aqueous medium and the weight (W2) may be measured, or the aqueous medium may be drained from the container and the weight (W2) may be measured. When step (I) is performed by the dropping method, the aqueous medium may be dropped into the article to allow it to absorb the aqueous medium, and then the weight (W2) of the article may be measured without performing any treatment such as recovery. Alternatively, the weight (W2) of the article may be calculated by adding the amount of dripping to the weight (W1) of the article. When step (II-1) is performed, the weight of the article after the dehydration treatment is calculated as the weight (W2) of the article. The weight of the article measured above (weight of the article before step (I) is performed: W1, weight of the article after step (I) is performed: W2) is applied to the following formula (1) to calculate the aqueous medium ratio. Aqueous medium ratio = (W2 - W1) / W1 × 100 (1)
[0037] The aqueous medium ratio may be calculated from the formula (1) before step (I). In other words, in another embodiment, step (II) may involve calculating the aqueous medium ratio under set conditions in advance and adjusting the aqueous medium ratio within the range during actual production. Such a step is preferable, for example, when the production method according to this embodiment is applied to continuous production.
[0038] The weight of the article (W2) is the sum of the weight of the article itself (W1 above) plus the aqueous medium absorbed by the article, the aqueous medium incorporated into the voids of the article, and the aqueous medium present in contact with and around the article. To improve the overall thermal stability of an article containing a polysaccharide, it is believed that absorbing an appropriate amount of aqueous medium into the article increases the reaction efficiency with compound (A). However, it has been found that drying in the presence of an excess amount of aqueous medium (aqueous medium ratio exceeding 1,000% by mass) results in an uneven improvement in the thermal stability of the resulting article. This is thought to be due to precipitation and segregation of compound (A) during the drying process. Furthermore, if compound (A) contained in the aqueous medium precipitates on the surface of the article, the article must be washed to remove the precipitated compound (A), which is undesirable from the perspective of production costs. It has also been found that even if the concentration of compound (A) in the aqueous medium is low, drying in the presence of an excess amount of aqueous medium is likely to cause the above phenomenon.
[0039] The present inventors have discovered that by adjusting the amount of aqueous medium within the article and the amount of aqueous medium around the article so that the aqueous medium ratio calculated from the above formula (1) is within the range of 10 to 1,000 mass%, and then performing step (III), precipitation of compound (A) can be suppressed and the thermal stability of the article can be uniformly improved. Because the amount of aqueous medium absorbed varies depending on the type of polysaccharide and the form of the article, the aqueous medium ratio of the article after performing step (I) may be within the range of 10 to 1,000 mass%. In such cases, step (II-2) can be performed without performing step (II-1), and then step (III) can be performed. In this case, step (II-2) (calculating the aqueous medium ratio) may simply involve measuring the weight (W2) of the article. That is, step (II) may include steps (II-1) and (II-2), or may include only step (II-2). Whether to perform step (II-1) may be determined by visual inspection of the article after performing step (I).
[0040] In step (II-2), if the aqueous medium ratio calculated from formula (1) is less than 10% by mass, the aqueous medium ratio is adjusted to 10% by mass or more. A preferred method for adjusting the aqueous medium ratio to 10% by mass or more is to perform step (I) again. If the aqueous medium ratio exceeds 1,000% by mass, the aqueous medium ratio is adjusted to 10 to 1,000% by mass. A preferred method for adjusting the aqueous medium ratio to 10 to 1,000% by mass is to perform step (II-1) again.
[0041] <Step (III)> The manufacturing method according to this embodiment further includes drying the article after steps (I) and (II). The drying method is not particularly limited, and any method can be adopted depending on the form of the article. It is preferable to carry out step (III) until the weight (W3) of the article after drying is approximately the same as the weight (W1) before carrying out step (I). Specifically, it is more preferable to carry out step (III) until the value calculated from the following formula (2) is 10 mass % or less. (W3 - W1) / W1 × 100 (%) ... (2)
[0042] The drying temperature can be set arbitrarily depending on the form of the article. In one embodiment, the drying temperature is preferably room temperature to 300°C, more preferably 20 to 260°C. The drying temperature may also be 100 to 260°C, or 150 to 200°C.
[0043] The manufacturing method according to this embodiment may be carried out in a batch manner or continuously. When the article is a powder, it is preferably carried out in a batch manner. When the article is a fibrous material, a cotton-like material, a plate-like material, or a film, it may be carried out continuously. In the case of a continuous method, the basis weight (g / m 2 Steps (I) to (III) may be carried out continuously while measuring the weight (W2) of the article from the fiber size (w) and fineness (denier), or a pre-calculated aqueous medium ratio may be used.
[0044] The manufacturing method of this embodiment can produce an article with uniformly improved thermal stability. Here, "uniformly improved thermal stability" includes the fact that the article is less likely to discolor and less likely to develop uneven color due to discoloration, even when heated at 200 to 300°C. Furthermore, "improved thermal stability" can also include the fact that the rate of weight loss on heating measured by TG-DTA is lower than that of the article before the thermal stability improvement.
[0045] <Form> The form of the article according to the present embodiment is not particularly limited, but is preferably a fibrous material, a powder, a plate-like material, a film, or a cotton-like material. Preferred embodiments according to the form of the article will be described below.
[0046] (Fibrous material) In this specification, "fibrous material" means a fiber obtained from a raw material containing a polysaccharide as a main component, and may be a short fiber or a long fiber. Furthermore, the fibrous material may be a spun fiber or a spun fiber. Furthermore, it may be a natural fiber or a regenerated fiber. The average fiber diameter, average fiber length, etc. of the fibrous material are not particularly limited. A preferred method for producing a fibrous material containing a polysaccharide will be described below.
[0047] Step (I) When the article is a fibrous material, the fibrous material is allowed to absorb an aqueous medium containing the compound (A) in an amount of preferably 100 parts by mass or more, more preferably 150 parts by mass or more, and even more preferably 200 parts by mass or more, per 100 parts by mass of the fibrous material. By allowing the fibrous material to absorb a relatively large amount of the aqueous medium, the thermal stability of the entire fibrous material is likely to be uniformly improved.
[0048] When the article is a fibrous material, at least one compound selected from the glycosylating agent (a1) and the esterifying agent (a2) described above can be preferably used as the compound (A). Among these, from the viewpoint of reaction efficiency and the ease of obtaining an article with a low rate of weight loss on heating, it is more preferable to include an esterifying agent (a2), and even more preferable to include boric acid. Furthermore, from the viewpoint of the ease of obtaining an article with a low rate of weight loss on heating, the glycosylating agent (a1) may contain glycerin, pentaerythritol, or mannitol. The concentration of the compound (A) in the aqueous medium can be adjusted as desired within the aforementioned preferred range. In a preferred embodiment, the concentration of the compound (A) in the aqueous medium can be 1 to 15% by mass.
[0049] The method for absorbing the aqueous medium into the fibrous material can be the immersion method or the dropping method described above, or a combination of these. The immersion method is preferred from the viewpoint of swelling the fibrous material and facilitating absorption of a large amount of the aqueous medium. The temperature and time of the aqueous medium can be adjusted as desired within the preferred ranges described above.
[0050] Step (II): Due to their structure, fibrous materials tend to absorb large amounts of aqueous medium and swell. Furthermore, color unevenness is likely to occur due to variations in the thermal stability improvement effect depending on the aqueous medium ratio. Therefore, it is preferable to perform a dehydration treatment after step (I) and then calculate the aqueous medium ratio. That is, it is preferable to include steps (II-1) and (II-2). In one embodiment, from the viewpoint of efficiency and workability, the fibrous material that has absorbed the aqueous medium is preferably compressed and dehydrated using a roll, and more preferably compressed and dehydrated at a speed of 10 to 1,000 m / min. When the article is a fibrous material, the aqueous medium ratio is preferably adjusted to 10 to 200% by mass, more preferably 10 to 150% by mass, even more preferably 20 to 150% by mass, and particularly preferably 20 to 100% by mass, within the range of 10 to 1,000% by mass.
[0051] Step (III) When the article is a fibrous material, the drying temperature for the fibrous material is preferably room temperature to 300° C., more preferably room temperature to 280° C., and even more preferably room temperature to 260° C. In one embodiment, the drying may be performed at 100 to 260° C., or 150 to 200° C.
[0052] (Powder) In this specification, the term "powder" refers to an aggregate of fine particles obtained from a raw material containing a polysaccharide as a main component, and the particle size and average particle diameter thereof are not particularly limited. From the viewpoint of the surface area, which is closely related to the reaction efficiency, a powder having a particle size of 10 mesh or more is preferable. The upper limit of the particle size can be 1,000 mesh or less.
[0053] Step (I): When the article is a powder of 10 mesh or larger, the amount of aqueous medium absorbed by the powder can be adjusted to a range of more than 10 parts by mass and not more than 1,000 parts by mass per 100 parts by mass of the powder. In one embodiment, the amount may be 300 to 1,000 parts by mass per 100 parts by mass of the powder. Since it is difficult to use an immersion method for powders, it is preferable to absorb the aqueous medium into the powder by a dropping method. The temperature and time of the aqueous medium can be adjusted as desired within the aforementioned preferred ranges.
[0054] When the article is a powder, at least one compound selected from the aforementioned glycosylating agent (a1) and esterifying agent (a2) can be preferably used as compound (A). Among these, from the viewpoint of reaction efficiency, it is more preferable to include esterifying agent (a2), and even more preferable to include boric acid. The concentration of compound (A) in the aqueous medium can be adjusted as desired within the aforementioned preferred range. In a preferred embodiment, the concentration of compound (A) in the aqueous medium can be 1 to 15% by mass.
[0055] Step (II): Compared to fibrous materials, powders with a mesh size of 10 or larger are less likely to exhibit variations in the thermal stability improvement effect due to the amount of aqueous medium absorbed, so the aqueous medium ratio may be calculated without dehydration. Furthermore, the aqueous medium ratio of the powder is preferably adjusted to 30 to 500% by mass, more preferably 50 to 400% by mass, and even more preferably 80 to 300% by mass, within the range of 10 to 1,000% by mass. In the case of powders, adjusting the aqueous medium ratio within the above range for reasons of uniformity makes it easier to consistently obtain powders with improved thermal stability.
[0056] Step (III) When the article is a powder, the drying temperature of the powder is preferably room temperature to 300° C., more preferably room temperature to 280° C., and even more preferably room temperature to 260° C. Note that step (III) is preferably carried out until the value calculated from the above formula (2) becomes 20 mass% or less.
[0057] (Plate or Film) In this specification, the term "plate" refers to a wide strip or similar object having a certain thickness (more than 100 μm) obtained from a raw material containing polysaccharides as the main component. The term "film" refers to a wide strip or similar object having a thickness of 100 μm or less obtained from a raw material containing polysaccharides as the main component.
[0058] Step (I): When the article is a plate-like material or a film, the plate-like material or film is allowed to absorb an aqueous medium in an amount of preferably 50 parts by mass or more, more preferably 100 parts by mass or more, and even more preferably 150 parts by mass or more, per 100 parts by mass of the plate-like material or film. If the amount of aqueous medium absorbed by the plate-like material or film is 50 parts by mass or more, the thermal stability of the entire plate-like material or film is likely to be uniformly improved.
[0059] When the article is a plate or film, at least one compound selected from the aforementioned glycosylating agent (a1) and esterifying agent (a2) can be preferably used as compound (A). Among these, from the viewpoint of reactivity, it is more preferable to include esterifying agent (a2), and even more preferable to include boric acid. The concentration of compound (A) in the aqueous medium can be adjusted as desired within the aforementioned preferred range. In a preferred embodiment, the concentration of compound (A) in the aqueous medium can be 1 to 15% by mass.
[0060] The method for absorbing the aqueous medium into the plate or film is preferably an immersion method or a spray method, and the temperature and time of the aqueous medium can be adjusted as desired within the above-mentioned preferred ranges.
[0061] Step (II): When an immersion method is employed in step (I), it is preferable to carry out steps (II-1) and (II-2). From the viewpoint of shape retention, step (II-1) is preferably compression dehydration using a roll. On the other hand, when a spraying method is employed in step (I), the amount of aqueous medium absorbed can be controlled to some extent, and therefore only step (II-2) can be included. The aqueous medium content of the plate-like material or film is preferably adjusted to 20 to 200% by mass, more preferably 30 to 150% by mass, and even more preferably 50 to 150% by mass, within a range of 10 to 1,000% by mass.
[0062] Step (III) When the article is a plate-like material or a film, the drying temperature of the plate-like material or film is preferably room temperature to 300° C., more preferably room temperature to 280° C., and even more preferably room temperature to 260° C. Furthermore, step (III) is preferably carried out until the value calculated from the above formula (2) becomes 15 mass% or less.
[0063] (Cotton-like material) In this specification, the term "cotton-like material" refers to a material obtained by crimping monofilaments obtained from a raw material containing a polysaccharide as a main component, cutting the monofilaments to a desired fiber length, and assembling the crimped monofilaments. The cotton-like material has an appearance similar to that of cotton (a group of fibers covering a seed). The average fiber diameter, average fiber length, etc. of the cotton-like material are not particularly limited.
[0064] Step (I): When the article is a cotton-like material, the cotton-like material is allowed to absorb an aqueous medium in an amount of preferably 100 parts by mass or more, more preferably 150 parts by mass or more, and even more preferably 200 parts by mass or more, per 100 parts by mass of the cotton-like material. When the amount of aqueous medium absorbed by the cotton-like material is 100 parts by mass or more, the thermal stability of the entire cotton-like material is easily improved uniformly.
[0065] When the article is a cotton-like material, at least one compound selected from the aforementioned glycosylating agent (a1) and esterifying agent (a2) can be preferably used as compound (A). Among these, from the viewpoint of reaction efficiency, it is more preferable to include esterifying agent (a2), and even more preferable to include boric acid. The concentration of compound (A) in the aqueous medium can be adjusted as desired within the aforementioned preferred range. In a preferred embodiment, the concentration of compound (A) in the aqueous medium can be 1 to 15% by mass.
[0066] As a method for absorbing an aqueous medium into a cotton-like material, the immersion method is preferred from the viewpoint of water absorption efficiency. Furthermore, as described above, it is preferred to release the air inside the cotton-like material as bubbles to the outside while immersing the cotton-like material in the aqueous medium. The temperature and time of the aqueous medium can be adjusted as desired within the preferred ranges described above.
[0067] Step (II) The aqueous medium ratio of the cotton-like material is adjusted to preferably 30 to 800% by mass, more preferably 30 to 500% by mass, and even more preferably 50 to 300% by mass, within the range of 10 to 1,000% by mass.
[0068] Step (III): When the article is a cotton-like material, the drying temperature for the cotton-like material is preferably room temperature to 300° C., more preferably room temperature to 280° C., and even more preferably room temperature to 260° C. In addition, step (III) is preferably carried out until the value calculated from the above formula (2) becomes 15 mass % or less.
[0069] [Uses] Articles containing polysaccharides obtained by the production method according to this embodiment have uniformly improved thermal stability. That is, they are less likely to develop discoloration or uneven color even when heated at 200 to 300°C. Therefore, they can be suitably used in fields where poor appearance due to discoloration or uneven color is a problem, as well as in fields such as reinforcing materials and modifiers for resins. Furthermore, articles containing polysaccharides (preferably fibrous materials) obtained by the production method according to this embodiment have a smaller rate of weight loss upon heating compared to before the improvement of thermal stability. Such articles (preferably fibrous materials, more preferably cellulose fibers, and even more preferably regenerated cellulose fibers) can be suitably used, for example, as fillers (reinforcing agents) for thermoplastic resins and thermosetting resins.
[0070] Other preferred aspects of the manufacturing method according to this embodiment are as follows. <1> A method for manufacturing a polysaccharide-containing article having improved thermal stability, wherein the article is a fibrous material, powder, plate-like material, film, or cotton-like material, the manufacturing method comprising: allowing the article to absorb an aqueous medium containing a compound (A) capable of reacting with a reducing end or a hydroxyl group of the polysaccharide within the range of the following condition (1) depending on the shape of the article (step (i)); adjusting the aqueous medium ratio within the range of the following condition (2) depending on the shape of the article (step (ii)); and drying the article (step (iii)). (Condition (1)) When the article is the fibrous material or the cotton-like material, 100 parts by mass or more of the aqueous medium is absorbed per 100 parts by mass of the fibrous material or the cotton-like material. When the article is a powder of 10 mesh or larger, more than 10 parts by mass and not more than 1,000 parts by mass of the aqueous medium is absorbed per 100 parts by mass of the powder. When the article is a plate-like material or a film, the aqueous medium is absorbed in an amount of 50 parts by mass or more per 100 parts by mass of the plate-like material or the film. (Condition (2)) When the article is a fibrous material, the aqueous medium ratio is adjusted to 10 to 200% by mass. When the article is a powder, the aqueous medium ratio is adjusted to 30 to 500% by mass. When the article is a plate-like material or a film, the aqueous medium ratio is adjusted to 20 to 200% by mass. When the article is a cotton-like material, the aqueous medium ratio is adjusted to 30 to 800% by mass. <2> The production method according to <1>, wherein the compound (A) comprises at least one compound selected from a glycosylating agent (a1) for a reducing end of the polysaccharide and an esterifying agent (a2) for a hydroxyl group of the polysaccharide. <3> The method according to <2>, wherein the glycosylating agent (a1) contains a monohydric or higher alcohol, and the esterifying agent (a2) contains boric acid. <4> The method according to any one of <1> to <3>, wherein the step (iv) comprises drying the article at room temperature to 300° C. <5> The method according to any one of <1> to <4>, wherein the concentration of the compound (A) in the aqueous medium in the step (i) is 0.1 to 50 mass%.<6> The manufacturing method according to any one of <1> to <5>, wherein the article comprises regenerated cellulose fibers. <7> The manufacturing method according to any one of <1> to <6>, wherein the compound (A) comprises boric acid, glycerin, pentaerythritol, or mannitol.
[0071] The present disclosure will be explained in more detail below by showing examples, but interpretation of the present disclosure is not limited to these examples.
[0072] [Materials] The following materials were used in the examples and comparative examples. <Articles containing polysaccharides> Regenerated cellulose fiber: regenerated cellulose fiber (lyocell) obtained by a solvent method (552 tex, 2700 filaments, average fiber diameter: 11 μm). Wood flour: cedar wood flour (particle size: 40 mesh). Pulp (plate-like material): manufactured by Nippon Paper Industries Co., Ltd., product name "LDPT". Cotton (cotton-like material): average fiber diameter: 15 μm. Ramie (cotton-like material): average fiber diameter: 40 μm. <Compound (A)> Esterifying agent (a2): boric acid.
[0073] Example 1: 100 parts by mass (W1: approximately 0.4 g) of regenerated cellulose fibers, the weight (W1) of which had been measured in advance, were immersed in an aqueous medium containing boric acid (6.0% by mass boric acid solution, aqueous medium temperature 23°C) for 5 seconds to absorb at least 200 parts by mass of the aqueous medium. The fibers were then sandwiched between paper towels and compressed for dehydration to remove the aqueous medium, after which the weight (W2) was measured and the aqueous medium ratio calculated using the above formula (1). The resulting aqueous medium ratio was 68% by mass. The regenerated cellulose fibers containing the aqueous medium were then dried at 23°C for 240 hours to obtain regenerated cellulose fibers with improved thermal stability. The amount of boric acid (the amount of compound (A) attached to the article) per 100 parts by mass of the resulting regenerated cellulose fibers was 5.7 parts by mass.
[0074] [Examples 2 to 4 and Examples 7 to 8] In Examples 2 to 4, regenerated cellulose fibers with improved thermal stability were obtained in the same manner as Example 1, except that the amount of aqueous medium absorbed in step (I), the concentration of compound (A) in the aqueous medium, the temperature of the aqueous medium, and the aqueous medium ratio were set as shown in Table 1. In Examples 7 to 8, cotton and ramie with improved thermal stability were obtained in the same manner as Example 1, except that the type of article, the concentration of compound (A) in the aqueous medium, the temperature of the aqueous medium, and the aqueous medium ratio were set as shown in Table 1. The W1 of the cotton in Example 7 was approximately 0.2 g, and the W1 of the ramie in Example 8 was approximately 0.2 g.
[0075] Example 5: An aqueous medium containing boric acid (2.0% by mass boric acid water, aqueous medium temperature 23°C) was added dropwise to 100 parts by mass (W1: approximately 1 g) of wood flour, the weight (W1) of which had been measured in advance, to allow the wood flour to absorb 270 parts by mass of the aqueous medium. The weight (W2) of the wood flour was measured without dehydration, and the aqueous medium ratio was calculated using the above formula (1). As a result, the aqueous medium ratio was 270% by mass. Next, the powder containing the aqueous medium was dried at 23°C for 480 hours to obtain wood flour with improved thermal stability. The amount of boric acid (amount of compound (A) adhered to the article) per 100 parts by mass of the obtained wood flour was 6.2 parts by mass.
[0076] [Example 6] Pulp with improved thermal stability was obtained in the same manner as in Example 5, except that the type of article, the amount of aqueous medium absorbed in step (I), the concentration of compound (A), the temperature of the aqueous medium, and the aqueous medium ratio were as shown in Table 1. The W1 of the pulp in Example 6 was approximately 1 g.
[0077] [Comparative Examples 1 to 10] Each article was obtained in the same manner as in Example 1 or Example 5, except that the type of article, the amount of aqueous medium absorbed in step (I), the concentration of compound (A), the temperature of the aqueous medium, and the aqueous medium ratio were as shown in Table 2. Comparative Example 1 is an example of regenerated cellulose fiber that was not subjected to a thermal stability improvement treatment. Comparative Examples 2, 3, 6, 8, and 10 are examples in which the article was immersed in an aqueous medium and then further aqueous medium was added dropwise to adjust the aqueous medium ratio to more than 1,000 mass%. Comparative Examples 4, 5, 7, and 9 are examples in which the article was immersed in an aqueous medium that did not contain compound (A). The W1 of the article in each comparative example was the same as in Examples 1 and 5 to 8.
[0078] The thermal stability of the articles obtained in each example was evaluated under the following conditions. <Evaluation of Thermal Stability> The articles obtained in each example were annealed under the following conditions. - Regenerated cellulose fiber, cotton, ramie: heated in a 240°C oven for 10 minutes. - Wood flour, pulp: heated in a 1200W toaster oven for 10 minutes. The discoloration level of the annealed articles was evaluated according to the following criteria. The discoloration level was determined as Level 1 for the article that was not annealed (Blank 1), and Level 4 for the regenerated cellulose of Comparative Example 1 (not subjected to the thermal stability improvement treatment) and the articles of Comparative Examples 4, 5, 7, and 9 (treated with an aqueous medium containing no compound (A) and then annealed; Blank 2). The degree of discoloration was compared. The uniformity of the thermal stability improvement effect was also evaluated based on the discoloration level and color unevenness. The results are shown in Tables 1 and 2. (Discoloration Level) Level 1: Similar color to Blank 1. Level 2: Slightly more discolored than Blank 1. Level 3: More colored than level 2. Level 4: The entire article is colored to the same extent as blank 2. (Evaluation criteria) A: The coloring level is level 1, and there is no color unevenness. B: The coloring level is level 2, but there is no color unevenness throughout the article. C: The coloring level is level 2 or higher, and there is color unevenness throughout the article. In addition, the presence or absence of boric acid precipitation on the article after annealing was also evaluated.
[0079]
[0080]
[0081] Example 9: 100 parts by mass (W1: approximately 0.2 g) of regenerated cellulose fibers, the weight (W1) of which had been measured in advance, were immersed in an aqueous medium containing boric acid (0.1% by mass boric acid solution, aqueous medium temperature 25°C) for 15 minutes to absorb at least 100 parts by mass of the aqueous medium. The fibers were then sandwiched between paper towels and compressed for dehydration, after which the weight (W2) was measured and the aqueous medium ratio calculated using the above formula (1). The resulting aqueous medium ratio was 80% by mass. The regenerated cellulose fibers containing the aqueous medium were then dried at 170°C for 30 minutes to obtain regenerated cellulose fibers with improved thermal stability. The amount of boric acid (the amount of compound (A) attached to the article) per 100 parts by mass of the resulting regenerated cellulose fibers was 0.08 parts by mass.
[0082] [Examples 10 to 16] Regenerated cellulose fibers with improved thermal stability were obtained in the same manner as in Example 9, except that the type of compound (A) and the amount of compound (A) attached per 100 parts by mass of regenerated cellulose fibers were as shown in Table 3.
[0083] <TG-DTA Measurement> The thermal weight loss rates of the regenerated cellulose fibers obtained in Examples 9 to 16 and the regenerated cellulose fiber of Comparative Example 1 (untreated product) were measured by TG-DTA. The results are shown in Figure 2. Table 3 shows the thermal weight loss rates (%) when heated at 230°C for 30 minutes. Note that the thermal weight loss rates in Figure 3 and Table 3 represent the ratio (%) of the weight after heating to the weight before heating (100%). (Measurement conditions) Measuring equipment: Hitachi High-Tech Science Corporation, product name "STA200RV" Starting temperature: 30°C Heating rate: 50°C / min Holding temperature: 220°C Holding time: 30 minutes Carrier gas: Air Carrier gas flow rate: 200 mL / min
[0084]
[0085] FIG. 1 shows photographs of the regenerated cellulose fibers obtained in Examples 1 and 2 and Comparative Examples 1 to 3. As is clear from FIG. 1, the articles (regenerated cellulose fibers) obtained by the manufacturing method according to this embodiment had uniformly improved thermal stability, and no discoloration or color unevenness due to the annealing treatment occurred. On the other hand, in Comparative Example 1, which was not subjected to the thermal stability improvement treatment, the regenerated cellulose fibers turned brown upon annealing. Furthermore, the regenerated cellulose fibers of Comparative Examples 2 and 3, which were obtained by drying in the presence of a large amount of aqueous medium (aqueous medium ratio exceeding 1,000% by mass), developed discoloration and color unevenness upon annealing, and large amounts of boric acid precipitated on the fiber surface. Similarly, the articles obtained by the manufacturing method according to this embodiment showed reduced discoloration and color unevenness due to the annealing treatment, whereas Comparative Examples 8 and 10, which were dried with an aqueous medium ratio adjusted to exceed 1,000% by mass, developed discoloration and color unevenness upon annealing, and boric acid precipitated on the surface. In Comparative Example 6, although there was no color unevenness and little coloring, precipitation of boric acid was confirmed on the surface. From the above results, it was confirmed that the manufacturing method according to the present embodiment can manufacture an article with uniformly improved thermal stability.
[0086] Figure 2 and Table 3 show the results of Examples 9 to 16 and Comparative Example 1. As shown, the regenerated cellulose fibers of Examples 9 to 16 had a lower rate of weight loss on heating than the regenerated cellulose fiber of Comparative Example 1. That is, when the regenerated cellulose fiber of Comparative Example 1 (untreated) was heated at 230°C for 30 minutes, the weight after heating was reduced by approximately 1.0% compared to the weight before heating, whereas the regenerated cellulose fibers of Examples 9 to 16 had a weight loss rate of approximately 0.5 to 0.6% under the same conditions. These results also confirmed that the manufacturing method according to this embodiment can produce articles with improved thermal stability.
[0087] The article obtained by the manufacturing method according to the present embodiment has uniformly improved thermal stability, and is therefore less likely to develop discoloration or uneven color even when heated. Such articles can also be suitably used as modifiers or reinforcing materials for resins.
Claims
1. A method for producing an article containing a polysaccharide having improved thermal stability, comprising the steps of: allowing the article to absorb an aqueous medium containing a compound (A) capable of reacting with a reducing end or a hydroxyl group of the polysaccharide (step (I)); adjusting the proportion of the aqueous medium to be 10 to 1,000 mass% relative to the total mass of the article before absorbing the aqueous medium (step (II)); and drying the article (step (III)).
2. The method for producing an article containing a polysaccharide according to claim 1, wherein the compound (A) comprises at least one compound selected from a glycosylating agent (a1) for the reducing end of the polysaccharide and an esterifying agent (a2) for the hydroxyl group of the polysaccharide.
3. The method for producing an article comprising a polysaccharide according to claim 2, wherein the glycosylating agent (a1) comprises a monohydric or higher alcohol and the esterifying agent (a2) comprises boric acid.
4. A method for producing an article containing the polysaccharide according to any one of claims 1 to 3, wherein the article is a fibrous material, the step (I) comprises absorbing 100 parts by mass or more of the aqueous medium per 100 parts by mass of the fibrous material, and the step (II) comprises adjusting the proportion of the aqueous medium to 10 to 200% by mass with respect to the total mass of the fibrous material before absorbing the aqueous medium.
5. A method for producing an article containing the polysaccharide according to any one of claims 1 to 3, wherein the article is a powder of 10 mesh or more, and the step (II) includes adjusting the proportion of the aqueous medium to 30 to 500 mass % based on the total mass of the powder before absorbing the aqueous medium.
6. A method for producing an article containing the polysaccharide according to any one of claims 1 to 3, wherein the article is a plate-like article or a film, the step (I) comprises absorbing 50 parts by mass or more of the aqueous medium per 100 parts by mass of the plate-like article or the film, and the step (II) comprises adjusting the proportion of the aqueous medium to 20 to 200% by mass with respect to the total mass of the plate-like article or the film before absorbing the aqueous medium.
7. A method for producing an article containing the polysaccharide according to any one of claims 1 to 3, wherein the article is a cotton-like material, the step (I) comprises absorbing 100 parts by mass or more of the aqueous medium per 100 parts by mass of the cotton-like material, and the step (II) comprises adjusting the proportion of the aqueous medium to 30 to 800% by mass relative to the total mass of the cotton-like material before absorbing the aqueous medium.
8. A method for producing an article comprising the polysaccharide according to any one of claims 1 to 3, wherein step (III) comprises drying the article at room temperature to 300°C.
9. A method for producing an article containing a polysaccharide according to any one of claims 1 to 3, wherein the concentration of the compound (A) in the aqueous medium in step (I) is 0.1 to 50 mass%.
Citation Information
Patent Citations
Method for controlling depolymerization of polysaccharides
JP2008163053A
Fine fibrous cellulose-containing material
JP2017057291A
Absorbent article
WO2017099078A1