Polyvinyl acetal resin film, film laminate, laminate and method for producing same, glazing material, and head-up display device

The use of a polyvinyl acetal resin film with tailored properties in laminated glass for HUD devices addresses the issue of poor image quality by enhancing adhesion and thermal stability, resulting in improved image clarity and reduced distortion.

WO2024247929A1PCT designated stage expired Publication Date: 2024-12-05KURARAY EURO GMBH

Patent Information

Application Number
PCT/JP2024/019240
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-24
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing laminated glass technologies for head-up display (HUD) devices suffer from poor image quality due to inadequate adhesion and thermal properties of the adhesive layers, leading to distortion and degradation of the reflected image.

Method used

A polyvinyl acetal resin film with specific thickness, roughness, and shear storage modulus is used to create a film laminate that improves adhesion and thermal stability, enhancing the image quality by thermocompression bonding with a light-reflecting layer and a translucent base material.

Benefits of technology

The polyvinyl acetal resin film laminate achieves improved adhesion and thermal stability, resulting in higher image quality and reduced distortion for head-up display devices by optimizing the thickness, roughness, and shear storage modulus of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024019240_05122024_PF_FP_ABST
    Figure JP2024019240_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides: a polyvinyl acetal resin film that is suitable as a material of a laminate for a head-up display (HUD) device which includes a translucent base material and a light-reflecting layer and that can improve the image quality of a reflected image reflected on the surface of the light-reflecting layer; and a film laminate and a laminate that use the polyvinyl acetal resin film. This polyvinyl acetal resin film has a polyvinyl acetal resin content of 80-100 mass% and a plasticizer content of 20-0 mass% with respect to 100 mass% of the polyvinyl acetal resin film, a thickness (T) of 5-350 μm, a ten-point average roughness (Rz) of at least one surface of 2-7 μm, and a shear storage modulus at 100°C (G'(100)) of 0.3-0.7 MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Polyvinyl acetal resin film, film laminate, laminate and manufacturing method thereof, glazing material, and head-up display device

[0001] The present disclosure relates to a polyvinyl acetal resin film, a film laminate, a laminate and a manufacturing method thereof, a glazing material, and a head-up display device.

[0002] Laminated glass, which is formed by laminating a pair of glass sheets via an adhesive layer generally called an interlayer, is resistant to breakage, and even if broken, glass fragments do not scatter, providing excellent security and safety, and is therefore used in a variety of applications such as vehicles and buildings. Traditionally, polyvinyl acetal resin films have been widely used as materials for interlayer films for laminated glass because of their excellent transparency, flexibility, impact absorption, and adhesion to glass. In recent years, laminated glass has increasingly been given various functionalities, such as reflectivity, absorption, or shielding of light such as infrared and ultraviolet rays or electron beams; design properties such as coloring; and electrical conductivity, thereby enhancing its functionality.

[0003] Patent Documents 1 and 2 disclose laminated glass in which a functional film having a functional layer and, if necessary, a substrate film such as a polyethylene phthalate (PET) film is disposed between one glass plate and an interlayer (e.g., claims 1, 3, 5, 6, 10, and 11 of Patent Document 1, and claims 1 and 9 of Patent Document 2). In recent years, head-up display (HUD) devices have been developed that display a reflected image (also referred to as a HUD image) reflected on the surface of a light-reflective layer disposed in a vehicle windshield or combiner. In such applications, a P-polarized reflective film is an example of a functional film disposed within the laminated glass to improve the visibility of the reflected image (e.g., claim 9 of Patent Document 2). By disposing a P-polarized reflective film within the laminated glass and changing the polarization state of the reflected image to P-polarized, the visibility of the reflected image when wearing polarized sunglasses can be improved.

[0004] International Publication No. 2018 / 010865 International Publication No. 2020 / 017502

[0005] In Patent Document 1, the objective of which is to provide laminated glass that protects a functional layer from corrosion and the like and has no defects in appearance is to sandwich a functional film between two thermoplastic resin films (e.g., polyvinyl acetal resin films) and to specify the relationship between the thicknesses of these three films (Claim 1, Paragraph 0051, etc.). In Patent Document 1, the functions of the functional layer include absorption of radio waves, infrared rays, or UV rays, conductivity, and coloring (Claim 11). Patent Document 1 does not describe the use of a head-up display (HUD) device, or the physical properties of the light-reflecting layer and thermoplastic resin film other than their thicknesses, and does not disclose any means for improving the image quality of the reflected image (HUD image) reflected on the surface of the light-reflecting layer.

[0006] In Patent Document 2, a functional film is bonded to one of the glass plates via an adhesive layer, and the thickness and softening point of the adhesive layer are specified with the objectives of reducing distortion of the HUD image and enabling degassing during the production of laminated glass (Claim 1, Paragraph 0008, etc.). Polyvinyl butyral and the like are cited as materials for the adhesive layer (Paragraph 0029). Patent Document 2 also states that the storage modulus of the adhesive layer measured at a frequency of 10 Hz in a temperature range of 20°C or less is 1.0 x 10 7 Pa or more, 1.0 × 10 7 However, the inventors have found that even if the storage modulus of the adhesive layer is within the above range, the image quality of the HUD image may be poor.

[0007] The present disclosure aims to provide a polyvinyl acetal resin film that is suitable as a material for a laminate for a head-up display (HUD) device that includes a light-transmitting substrate and a light-reflecting layer, and that can improve the image quality of an image reflected on the surface of the light-reflecting layer, as well as a film laminate and a laminate using the same.

[0008] The present disclosure provides a polyvinyl acetal resin film, a film laminate, a laminate and its manufacturing method, a glazing material, and a head-up display device as set forth in the following [1] to

[15] . [1] A polyvinyl acetal resin film containing one or more polyvinyl acetal resins, wherein, relative to 100% by mass of the polyvinyl acetal resin film, the polyvinyl acetal resin content is 80 to 100% by mass and the plasticizer content is 20 to 0% by mass, the polyvinyl acetal resin film has a thickness (T) of 5 to 350 μm, at least one surface of which has a ten-point average roughness (Rz) of 2 to 7 μm as measured in accordance with JIS B0601-1994, and a shear storage modulus (G'(100)) at 100°C of 0.3 to 0.7 MPa.

[0009] [2] The polyvinyl acetal resin film according to [1], wherein T [μm] and G′(100) [MPa] satisfy the following formula (1): 1.5≦T×G′(100)≦120 (1) [3] A film laminate comprising the polyvinyl acetal resin film according to [1] or [2], and a light-reflecting layer having a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer.

[0010] [4] A film laminate having, on a first resin film consisting of the polyvinyl acetal resin film of [1] or [2], a light-reflecting layer of a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer, and a second resin film, in that order. [5] The film laminate of [4], wherein the second resin film contains one or more resins selected from the group consisting of polyvinyl acetal resin, ionomer resin, ethylene-vinyl acetate copolymer, cycloolefin polymer, and polyurethane. [6] The film laminate of [5], wherein the second resin film is a polyvinyl acetal resin film containing 60 to 80% by mass of polyvinyl acetal resin and 40 to 20% by mass of a plasticizer, relative to 100% by mass of the second resin film. [7] A film laminate having, on the polyvinyl acetal resin film of [1] or [2], a light-reflecting layer having a single-layer structure or a laminate structure that reflects at least a part of light, or a light-reflecting film including the light-reflecting layer, and a hard coat layer in this order.

[0011] [8] A laminate having the film laminate of any one of [4] to [6] and a pair of light-transmitting substrates sandwiching the film laminate. [9] A laminate having, on a light-transmitting substrate, the polyvinyl acetal resin film of [1] or [2], a light-reflecting layer of a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer, and a hard coat layer, in that order.

[10] A glazing material including the laminate of [8] or [9], wherein the light-transmitting substrate includes a glass plate or a glass laminate.

[11] A head-up display device including a windshield or combiner including the glazing material of

[10] .

[0012]

[12] A method for producing a laminate, the method comprising the steps of: (S1) obtaining a temporary laminate having, on a light-transmitting substrate, the polyvinyl acetal resin film of [1] or [2], and a light-reflecting layer of a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer, the temporary laminate being in contact with the light-transmitting substrate without being bonded; and (S2) thermocompression bonding the temporary laminate.

[13] The method for producing a laminate according to

[12] , wherein in step (S1), the light-transmitting substrate is in contact with the surface of the polyvinyl acetal resin film having a ten-point average roughness (Rz) of 2 to 7 μm.

[0013]

[14] The method for producing a laminate according to

[12] or

[13] , wherein step (S2) sequentially comprises: a step (S2-1) of heating the temporary laminate at a temperature of 90 to 110°C to obtain a pre-press-bonded body; and a step (S2-2) of pressurizing and heating the pre-press-bonded body at a temperature higher than the heating temperature of step (S2-1).

[0014]

[15] The method for producing a laminate according to any one of

[12] to

[14] , wherein the step (S1) includes: a step (S1-1) of obtaining a film laminate including the polyvinyl acetal resin film and the light-reflecting film; and a step (S1-2) of stacking a plurality of members including the light-transmitting substrate and the film laminate to obtain the temporary laminate.

[0015] According to the present disclosure, it is possible to provide a polyvinyl acetal resin film that is suitable as a material for a laminate for a head-up display (HUD) device including a light-transmitting substrate and a light-reflecting layer and that can improve the image quality of a reflected image reflected on the surface of the light-reflecting layer, as well as a film laminate and a laminate using the same.

[0016] Fig. 1 is a schematic cross-sectional view of a first film laminate according to an embodiment of the present invention. Fig. 2 is a schematic cross-sectional view of a second film laminate according to an embodiment of the present invention. Fig. 3 is a schematic cross-sectional view of a third film laminate according to an embodiment of the present invention. Fig. 4 is a schematic cross-sectional view of a first laminate according to an embodiment of the present invention. Fig. 5 is a schematic cross-sectional view of a second laminate according to an embodiment of the present invention. Fig. 6 is a schematic cross-sectional view of a head-up display (HUD) device according to a first embodiment of the present invention. Fig. 7 is a schematic cross-sectional view of a head-up display (HUD) device according to a second embodiment of the present invention.

[0017] [Polyvinyl acetal resin film] The polyvinyl acetal resin film of the present disclosure contains one or more polyvinyl acetal resins and, if necessary, may contain one or more plasticizers. The polyvinyl acetal resin film of the present disclosure has a polyvinyl acetal resin content of 80 to 100% by mass, a plasticizer content of 20 to 0% by mass, and a thickness (T) of 5 to 350 μm, and has a ten-point average roughness (Rz) of at least one surface measured in accordance with JIS B0601-1994 of 2 to 7 μm, and a shear storage modulus (G'(100)) at 100°C of 0.3 to 0.7 MPa. Generally, the terms "film" and "sheet" are used for thin film molded products depending on the thickness. Therefore, the term "film" used herein may include "sheet," and the term "sheet" used herein may include "film."

[0018] The polyvinyl acetal resin film of the present disclosure can be used for any application and is suitable as a material for a laminate including a light-transmitting substrate such as a glass plate and a light-reflecting layer or a light-reflecting film containing the same. Specifically, it is suitable as an adhesive material for bonding the light-transmitting substrate and the light-reflecting layer or light-reflecting film in a laminate including the light-transmitting substrate and the light-reflecting layer or light-reflecting film. Bonding between the light-transmitting substrate and the light-reflecting layer or light-reflecting film via the polyvinyl acetal resin film of the present disclosure can be performed by thermocompression bonding, preferably by two-stage thermocompression bonding: preliminary heating at a temperature of 90 to 110°C (preferably heating under reduced pressure), and final heating under pressure at a temperature higher than the preliminary heating.

[0019] A laminate including a translucent substrate and a light-reflecting layer or film can be a glass laminate such as laminated glass. When the laminate including a translucent substrate and a light-reflecting layer or film is laminated glass, the step of adhering the translucent substrate and the light-reflecting layer or film via the polyvinyl acetal resin film of the present disclosure can be included in the laminating step of a pair of glass plates in the manufacturing method of laminated glass. Examples of laminates including a translucent substrate and a light-reflecting layer or film include glazing materials for head-up display (HUD) devices such as vehicle windshields and combiners. The polyvinyl acetal resin film of the present disclosure is particularly suitable as an adhesive material for adhering the translucent substrate and the light-reflecting layer or film in glazing materials for head-up display (HUD) devices.

[0020] (Thickness (T)) The polyvinyl acetal resin film of the present disclosure has a thickness (T) of 5 to 350 μm. The lower limit is preferably 10 μm, more preferably 15 μm, even more preferably 20 μm, particularly preferably 25 μm, and most preferably 50 μm. The upper limit is preferably 300 μm, more preferably 250 μm, even more preferably 200 μm, particularly preferably 150 μm, and most preferably 125 μm.

[0021] If the thickness (T) is less than the lower limit, thermal shrinkage of the polyvinyl acetal resin film of the present disclosure and deformation of the reflective layer or light-reflecting film may occur when laminating the polyvinyl acetal resin film of the present disclosure to a light-reflecting layer or light-reflecting film, or when adhering the polyvinyl acetal resin film of the present disclosure to a light-transmitting substrate via the polyvinyl acetal resin film of the present disclosure. As a result, the bondability (adhesion) between the polyvinyl acetal resin film of the present disclosure to the light-reflecting layer or light-reflecting film and the flatness of the light-reflecting layer may be reduced. Furthermore, the impact absorption properties of the polyvinyl acetal resin film may be insufficient. If the thickness (T) exceeds the upper limit, the in-plane thickness unevenness of the polyvinyl acetal resin film of the present disclosure may increase, and the flatness of the light-reflecting layer laminated to the light-transmitting substrate via the polyvinyl acetal resin film of the present disclosure may be reduced. In the use of a head-up display (HUD) device that displays a reflected image (HUD image) reflected on the surface of a light-reflecting layer, a decrease in the flatness of the light-reflecting layer may lead to a decrease in image quality, such as undulation and blurring of the reflected image (HUD image).

[0022] When the thickness (T) of the polyvinyl acetal resin film of the present disclosure is within the above range, it has good film-forming properties, can provide good adhesion between a translucent substrate and a light-reflecting layer or film, and can exhibit good impact absorption properties. Furthermore, since the in-plane thickness unevenness and thermal shrinkage of the polyvinyl acetal resin film of the present disclosure are suppressed, the flatness of the light-reflecting layer bonded to the translucent substrate via the polyvinyl acetal resin film of the present disclosure can be improved. As a result, in applications such as head-up display (HUD) devices, the image quality of the reflected image (HUD image) reflected on the surface of the light-reflecting layer can be improved. The thicknesses of the polyvinyl acetal resin film of the present disclosure and the second resin film described below can be measured by the method described in the Examples section below.

[0023] (Ten-point average roughness (Rz)) The polyvinyl acetal resin film of the present disclosure has a ten-point average roughness (Rz) of at least one surface of 2.0 to 7.0 μm. The lower limit is preferably 2.2 μm, more preferably 2.4 μm, particularly preferably 3.0 μm, and most preferably 3.2 μm. The upper limit is preferably 6.5 μm, more preferably 6.2 μm, particularly preferably 6.0 μm, and most preferably 5.8 μm.

[0024] If the Rz value is less than the lower limit, adhesion to the translucent substrate, light-reflecting layer, or light-reflecting film in contact with the surface may be too high, resulting in wrinkles in the polyvinyl acetal resin film. Furthermore, air trapped between the translucent substrate, light-reflecting layer, or light-reflecting film in contact with the surface may be difficult to escape, resulting in reduced degassing. If the Rz value exceeds the upper limit, adhesion to the translucent substrate, light-reflecting layer, or light-reflecting film in contact with the surface may be reduced. Furthermore, when laminating the polyvinyl acetal resin film of the present disclosure to the light-reflecting layer or light-reflecting film, or when adhering the translucent substrate to the light-reflecting layer or light-reflecting film via the polyvinyl acetal resin film of the present disclosure, thermal shrinkage of the polyvinyl acetal resin film of the present disclosure and resulting deformation of the light-reflecting layer or light-reflecting film may occur. As a result, the bondability (adhesion) between the polyvinyl acetal resin film of the present disclosure and the light-reflecting layer or light-reflecting film and the flatness of the light-reflecting layer may be reduced.

[0025] When the polyvinyl acetal resin film of the present disclosure has an Rz within the above range, it can provide good adhesion between a translucent substrate and a light-reflecting layer or film. Furthermore, since the thermal shrinkage of the polyvinyl acetal resin film of the present disclosure is suppressed, the flatness of the light-reflecting layer bonded to the translucent substrate via the polyvinyl acetal resin film of the present disclosure can be improved. As a result, in applications such as head-up displays (HUDs), the image quality of the reflected image (HUD image) reflected on the surface of the light-reflecting layer can be improved.

[0026] The ten-point average roughness (Rz) of the polyvinyl acetal resin film of the present disclosure can be adjusted within the above range by the production method and production conditions. The polyvinyl acetal resin film of the present disclosure having a ten-point average roughness (Rz) within the above range can be preferably produced by extrusion molding including embossing. The ten-point average roughness (Rz) can be adjusted within the desired range by adjusting the surface shape and surface material of the cooling roll used in extrusion molding, the press pressure during extrusion molding, the embossing conditions (such as the resin film temperature and the cooling roll surface temperature), and the composition of the polyvinyl acetal resin film. In this specification, the "ten-point average roughness (Rz)" can be measured in accordance with JIS B0601-1994 using a surface roughness meter (preferably a contact-type surface roughness meter) or a laser microscope. For specific measurement methods, see the "Examples" section below.

[0027] (Shear storage modulus (G'(100)) The polyvinyl acetal resin film of the present disclosure has a shear storage modulus (G'(100)) at 100°C of 0.3 to 0.7 MPa. The lower limit is preferably 0.32 MPa, more preferably 0.35 MPa, particularly preferably 0.40 MPa, and most preferably 0.42 MPa. The upper limit is preferably 0.65 MPa, more preferably 0.60 MPa, particularly preferably 0.55 MPa, and most preferably 0.50 MPa. As described above, adhesion between the light-transmitting substrate and the light-reflecting layer or film via the polyvinyl acetal resin film of the present disclosure can be performed by thermocompression bonding, and preferably can be performed by two-stage thermocompression bonding: preliminary compression bonding in which heating is performed at a temperature of 90 to 110°C, and main compression bonding in which heating is performed under pressure at a temperature higher than that of the preliminary compression bonding. 100°C is a typical temperature suitable for preliminary compression bonding.

[0028] If G'(100) is less than the lower limit, the polyvinyl acetal resin film of the present disclosure may deform significantly during pre-bonding, potentially reducing the flatness of the light-reflective layer. If G'(100) is greater than the upper limit, the polyvinyl acetal resin film of the present disclosure may not deform sufficiently during pre-bonding, resulting in uneven thickness of the polyvinyl acetal resin film and reduced flatness of the light-reflective layer. If G'(100) is within the above range, the polyvinyl acetal resin film of the present disclosure may deform appropriately during pre-bonding, reducing uneven thickness, and making it easier to obtain a laminate with a good flatness of the light-reflective layer. As a result, in head-up display (HUD) device applications, the image quality of the reflected image (HUD image) reflected on the surface of the light-reflective layer can be improved. G'(100) can be adjusted within the above range depending on the molecular weight and degree of acetalization of the polyvinyl acetal resin, the content of plasticizer in the polyvinyl acetal resin film, and the like. G'(100) can be measured by the method described in the Examples section below.

[0029] (T×G'(100)) In the polyvinyl acetal resin film of the present disclosure, the product of the thickness (T) [μm] and the shear storage modulus at 100°C (G'(100)) [MPa] preferably satisfies the following formula (1): 1.5≦T×G'(100)≦120 (1) The lower limit is more preferably 2, even more preferably 4, even more preferably 10, particularly preferably 15, and most preferably 20. The upper limit is more preferably 110, even more preferably 100, even more preferably 80, particularly preferably 60, and most preferably 50. When T×G'(100) is within the above range, effects such as improved bondability (adhesion) between the light-transmitting substrate and the light-reflecting layer or light-reflecting film, improved flatness of the light-reflecting layer bonded to the light-transmitting substrate via the polyvinyl acetal resin film of the present disclosure, and improved image quality of the reflected image (HUD image) in head-up display (HUD) device applications can be more favorably obtained.

[0030] In designing the polyvinyl acetal resin film of the present disclosure, the thickness (T) is determined within a preferred range, and then the degree of acetalization of the polyvinyl acetal resin and the plasticizer content, etc., are adjusted to adjust G'(100), preferably G'(100) and T×G'(100), within preferred ranges. Table 1 shows examples of the relationship between the thickness (T), the lower and upper limits of G'(100) for the thickness (T) at which T×G'(100) satisfies the above formula (1), and the relationship between T×G'(100) when G'(100) is the lower limit and T×G'(100) when G'(100) is the upper limit. For example, when T is determined within the range of 5 to 150 μm and G'(100) is 0.3 to 0.7 MPa, T×G'(100) can satisfy the above formula (1). For example, when T is determined to be 200 μm, if G′(100) is 0.3 to 0.6 MPa, T×G′(100) can satisfy the above formula (1).

[0031]

[0032] After determining G'(100) within a suitable range by adjusting the degree of acetalization of the polyvinyl acetal resin and the content of plasticizer, etc., the thickness (T), preferably the thickness (T) and T×G'(100), may be adjusted within a suitable range. Table 2 shows an example of the relationship between G'(100), the lower limit and upper limit of T at which T×G'(100) satisfies the above formula (1), and T×G'(100) when T is the lower limit and T×G'(100) when T is the upper limit. For example, when G'(100) is determined to be 0.3 MPa, if T is 5 to 350 μm, T×G'(100) can satisfy the above formula (1). For example, when G'(100) is determined to be 0.4 MPa, if T is 5 to 300 μm, T×G'(100) can satisfy the above formula (1).

[0033]

[0034] (Polyvinyl acetal resin) The polyvinyl acetal resin film of the present disclosure contains one or more polyvinyl acetal resins. The polyvinyl acetal resin is a resin produced by acetalization of a polyvinyl alcohol-based resin such as polyvinyl alcohol or an ethylene-vinyl alcohol copolymer. The polyvinyl acetal resin film of the present disclosure may contain two or more polyvinyl acetal resins differing in one or more properties selected from the group consisting of viscosity-average polymerization degree, acetalization degree, vinyl acetate unit content, vinyl alcohol unit content, ethylene unit content, molecular weight of the aldehyde used in acetalization, and chain length. In this case, from the viewpoints of ease of melt-forming, deformability during adhesion between a translucent substrate and a light-reflecting layer or film via the polyvinyl acetal resin film of the present disclosure, and prevention of misalignment of the translucent substrate during use of a laminate such as laminated glass, especially at high temperatures, the polyvinyl acetal resin film of the present disclosure preferably contains two or more polyvinyl acetal resins differing in viscosity-average polymerization degree.

[0035] Polyvinyl acetal resins can be produced by known methods, for example, by the following method. First, an aqueous solution of polyvinyl alcohol and / or ethylene-vinyl alcohol copolymer with a concentration of 3 to 30% by mass is maintained at a temperature range of 80 to 100°C and then gradually cooled over 10 to 60 minutes. When the temperature has dropped to -10 to 30°C, an aldehyde and / or ketone compound and an acid catalyst are added, and the acetalization reaction is carried out for 30 to 300 minutes while maintaining the temperature constant. Next, the reaction solution is heated to a temperature of 20 to 80°C over 30 to 200 minutes and maintained at that temperature for 30 to 300 minutes. Next, the reaction solution is filtered as needed, and then neutralized by adding a neutralizing agent such as an alkali. Next, the resulting resin is filtered, washed with water, and dried. In this manner, polyvinyl acetal resins are produced.

[0036] The acid catalyst used in the acetalization reaction is not particularly limited and may be either an organic acid or an inorganic acid. Examples of the acid catalyst include acetic acid, paratoluenesulfonic acid, nitric acid, sulfuric acid, and hydrochloric acid. Among them, hydrochloric acid, sulfuric acid, and nitric acid are preferred from the viewpoints of acid strength and ease of removal during washing.

[0037] From the viewpoint of facilitating the production of a polyvinyl acetal resin having a suitable breaking energy, the aldehyde or ketone compound used in the production of the polyvinyl acetal resin preferably has a linear, branched, or cyclic molecular structure having 2 to 10 carbon atoms, and more preferably a linear or branched molecular structure, thereby obtaining a corresponding linear or branched acetal group.

[0038] One or more aldehyde and / or ketone compounds can be used, and at least one of them is preferably one or more aliphatic unbranched aldehydes having 2 to 10 carbon atoms. As such an aldehyde, n-butylaldehyde and the like are preferred from the viewpoint of facilitating the production of a polyvinyl acetal resin having a suitable breaking energy. The amount of n-butylaldehyde in the one or more aldehyde and / or ketone compounds used for acetalization is preferably 50% by mass or more, more preferably 80% by mass or more, particularly preferably 95% by mass or more, and most preferably 99% by mass or more, and may even be 100% by mass.

[0039] The polyvinyl acetal resin may be produced using a combination of multiple types of polyvinyl alcohol and / or ethylene-vinyl alcohol copolymers having different properties such as viscosity-average polymerization degree or hydrolysis degree. The viscosity-average polymerization degree of the raw material polyvinyl alcohol is not particularly limited, but is preferably 100 or more, more preferably 300 or more, more preferably 400 or more, even more preferably 600 or more, particularly preferably 700 or more, and most preferably 750 or more. When the viscosity-average polymerization degree of the polyvinyl alcohol is equal to or greater than the above-mentioned lower limit, misalignment of the light-transmitting substrate at high temperatures in the resulting laminate, such as laminated glass, is likely to be suppressed. The viscosity-average polymerization degree of the polyvinyl alcohol is preferably 5000 or less, more preferably 3000 or less, even more preferably 2500 or less, particularly preferably 2300 or less, and most preferably 2000 or less. When the viscosity-average polymerization degree of the polyvinyl alcohol is equal to or less than the above-mentioned upper limit, the film-forming properties of the polyvinyl acetal resin are good.

[0040] The viscosity-average degree of polymerization of polyvinyl alcohol can be measured, for example, in accordance with JIS K 6726 "Testing Methods for Polyvinyl Alcohol." Typically, the viscosity-average degree of polymerization of a polyvinyl acetal resin is equal to that of the raw material polyvinyl alcohol, and therefore the preferred viscosity-average degree of polymerization of the polyvinyl alcohol described above is equal to that of the resulting polyvinyl acetal resin. When the polyvinyl acetal resin film of the present disclosure contains two or more polyvinyl acetal resins, it is preferred that the viscosity-average degree of polymerization of at least one polyvinyl acetal resin be equal to or greater than the lower limit and equal to or less than the upper limit.

[0041] The amount of acetyl groups (amount of vinyl acetate units) in the polyvinyl acetal resin can be adjusted by appropriately adjusting the degree of saponification of the raw material polyvinyl alcohol and / or ethylene-vinyl alcohol copolymer. The polarity of the polyvinyl acetal resin changes depending on the amount of acetyl groups, thereby adjusting the compatibility with a plasticizer added as needed and the mechanical strength of the resulting polyvinyl acetal resin film of the present disclosure.

[0042] The amount of acetyl groups in the polyvinyl acetal resin is preferably 0.07 to 14.82 mol%, more preferably 0.15 to 11.12 mol%, even more preferably 0.22 to 7.41 mol%, particularly preferably 0.30 to 5.19 mol%, and most preferably 0.37 to 2.96 mol%, based on the ethylene units in the polyvinyl acetal main chain. The amount of acetyl groups can be adjusted within the above range by appropriately adjusting the saponification degree of the raw material polyvinyl alcohol. When the polyvinyl acetal resin film of the present disclosure contains a polyvinyl acetal resin having an acetyl group amount within the above range, good adhesion and reduced optical distortion are likely to be achieved. When the polyvinyl acetal resin film of the present disclosure contains two or more polyvinyl acetal resins, it is preferable that the amount of acetyl groups in at least one of the polyvinyl acetal resins is within the above range.

[0043] The degree of acetalization of the polyvinyl acetal resin is not particularly limited, but is preferably 40 to 86 mol%, more preferably 45 to 84 mol%, even more preferably 50 to 82 mol%, particularly preferably 60 to 82 mol%, and most preferably 68 to 82 mol%. The degree of acetalization of the polyvinyl acetal resin can be adjusted within the above range by appropriately adjusting the amount of aldehyde and / or ketone compound used when acetalizing the polyvinyl alcohol resin. An acetalization degree within the above range improves the mechanical strength of the polyvinyl acetal resin and its compatibility with plasticizers added as needed. When the polyvinyl acetal resin film of the present disclosure contains two or more polyvinyl acetal resins, it is preferable that the degree of acetalization of at least one polyvinyl acetal resin be within the above range.

[0044] The hydroxyl group content (amount of vinyl alcohol units) of the polyvinyl acetal resin is not particularly limited, and is preferably 8.7 to 37.6 mol%, more preferably 17.3 to 34.7 mol%, particularly preferably 21.7 to 31.8 mol%, and most preferably 26.0 to 30.4 mol%, based on the ethylene units of the polyvinyl acetal main chain. When sound insulation performance is desired in the polyvinyl acetal resin film of the present disclosure, the content is preferably 8.7 to 28.9 mol%, more preferably 11.6 to 26.0 mol%, particularly preferably 14.5 to 21.7 mol%, and most preferably 15.9 to 18.8 mol%. The hydroxyl group content can be adjusted within the above range by adjusting the amount of aldehyde used when acetalizing the polyvinyl alcohol resin. When the hydroxyl group content is within the above range, the refractive index difference between the polyvinyl acetal resin and the second adhesive layer is reduced, making it easier to obtain laminates such as laminated glass with reduced optical irregularities. When the polyvinyl acetal resin film of the present disclosure contains two or more types of polyvinyl acetal resins, it is preferable that the hydroxyl group amount of at least one of the polyvinyl acetal resins is within the above range.

[0045] Polyvinyl acetal resins are usually composed of acetal group-containing units, hydroxyl group-containing units, and acetyl group-containing units, and the amount of each unit can be measured, for example, by JIS K 6728 "Testing Methods for Polyvinyl Butyral" or nuclear magnetic resonance (NMR). When the polyvinyl acetal resin contains units other than those mentioned above, the amount of hydroxyl group-containing units and the amount of acetyl group-containing units are measured, and the amount of these units is subtracted from the amount of acetal group-containing units in a resin containing no other units, thereby calculating the amount of the remaining acetal group-containing units.

[0046] The viscosity average degree of polymerization of the polyvinyl acetal resin is not particularly limited. Unless otherwise specified in this specification, the viscosity of the polyvinyl acetal resin is the viscosity measured using a Brookfield (B-type) viscometer at 20°C and 30 rpm on a solution prepared by adjusting the concentration of the polyvinyl acetal resin to 10% by mass using a mixed solvent of toluene and ethanol in a 1:1 mass ratio. The viscosity of the polyvinyl acetal resin contained in the polyvinyl acetal resin film of the present disclosure is preferably greater than 200 mPa·s, more preferably 210 mPa·s or greater, more preferably 220 mPa·s or greater, even more preferably 230 mPa·s or greater, particularly preferably 240 mPa·s or greater, and most preferably 265 mPa·s or greater. When the viscosity of the polyvinyl acetal resin is greater than 200 mPa·s, displacement of the translucent substrate of a laminate such as laminated glass at high temperatures is easily suppressed. By using a polyvinyl acetal resin produced using a polyvinyl alcohol having a relatively high viscosity average degree of polymerization as a raw material or as part of the raw material, the viscosity of the polyvinyl acetal resin can be adjusted to more than 200 mPa s. When the polyvinyl acetal resin film of the present disclosure contains two or more polyvinyl acetal resins, the viscosity is the viscosity of a mixture of these resins. From the viewpoint of achieving good film formability, the viscosity is usually 1000 mPa s or less, preferably 800 mPa s or less, more preferably 500 mPa s or less, particularly preferably 450 mPa s or less, and most preferably 400 mPa s.

[0047] The polyvinyl acetal resin film of the present disclosure preferably contains a non-crosslinked polyvinyl acetal resin, from the viewpoint of easily obtaining good film-forming properties, or may contain a crosslinked polyvinyl acetal resin. For crosslinking methods of polyvinyl acetal resins, see, for example, EP 1527107 and WO 2004 / 063231 (thermal self-crosslinking of carboxyl group-containing polyvinyl acetal), EP 1606325 (polyvinyl acetal crosslinked with polyaldehyde), and WO 2003 / 020776 (polyvinyl acetal crosslinked with glyoxylic acid). By appropriately adjusting the acetalization reaction conditions, the amount of intermolecular acetal bonds and the degree of blocking of residual hydroxyl groups can also be adjusted.

[0048] (Plasticizer) The polyvinyl acetal resin film of the present disclosure may contain one or more plasticizers as needed. In the polyvinyl acetal resin film of the present disclosure, the polyvinyl acetal resin content (total amount if multiple types are used) is 80 to 100% by mass, and the plasticizer content (total amount if multiple types are used) is 20 to 0% by mass, based on 100% by mass of the polyvinyl acetal resin film. The lower limit of the polyvinyl acetal resin content is preferably 82% by mass, more preferably 84% by mass, even more preferably 86% by mass, even more preferably 88% by mass, even more preferably 90% by mass, particularly preferably 92% by mass, and most preferably 94% by mass. The upper limit is preferably 18% by mass, more preferably 16% by mass, even more preferably 14% by mass, even more preferably 12% by mass, even more preferably 10% by mass, particularly preferably 8% by mass, and most preferably 6% by mass. The upper limit of the polyvinyl acetal resin content is preferably 99% by mass, more preferably 98% by mass. The lower limit of the plasticizer content is preferably 1% by mass, more preferably 2% by mass.

[0049] If the plasticizer content exceeds the above upper limit, the film-forming properties of the polyvinyl acetal resin film of the present disclosure may be reduced. Furthermore, particularly in high-temperature environments, self-adhesion of polyvinyl acetal resin films of the present disclosure may occur, resulting in reduced surface uniformity and deformation. This may affect the optical properties of a laminate including a translucent substrate and a light-reflecting layer or film. When the plasticizer content is within the above range, the polyvinyl acetal resin film of the present disclosure has excellent film-forming properties and handleability. Furthermore, the polyvinyl acetal resin film of the present disclosure deforms appropriately during pre-press bonding, reducing film thickness unevenness and making it easier to obtain a laminate with a favorable flatness of the light-reflecting layer. As a result, in head-up display (HUD) device applications, the image quality of the reflected image (HUD image) reflected on the surface of the light-reflecting layer can be improved. When the polyvinyl acetal resin film of the present disclosure contains a small amount (preferably 1 to 10% by mass) of plasticizer, roll wrinkles can be suppressed during film formation.

[0050] The plasticizer is not particularly limited, and one or more of the following examples (Pa) to (Pe) can be used. (Pa) Esters of polyvalent aliphatic or aromatic acids. Examples of such esters include dialkyl adipates (e.g., dihexyl adipate, di-2-ethylbutyl adipate, dioctyl adipate, di-2-ethylhexyl adipate, hexylcyclohexyl adipate, diheptyl adipate, dinonyl adipate, diisononyl adipate, and heptylnonyl adipate); esters of adipic acid with an alcohol or an alcohol containing an ether structure (e.g., di(butoxyethyl) adipate); di(butoxyethoxyethyl)adipate; dialkyl sebacates (for example, dibutyl sebacate); esters of sebacic acid and alcohols containing an alicyclic structure or an ether structure; esters of phthalic acid (for example, butyl benzyl phthalate and bis-2-butoxyethyl phthalate); esters of alicyclic polycarboxylic acids and aliphatic alcohols (for example, 1,2-cyclohexanedicarboxylic acid diisononyl ester).

[0051] (P-b) Esters or ethers of polyhydric aliphatic or aromatic alcohols or oligoether glycols having one or more aliphatic or aromatic substituents. Examples of such esters or ethers include esters of glycerin, diglycol, triglycol, tetraglycol, or the like with linear or branched aliphatic or alicyclic carboxylic acids. Specific examples include diethylene glycol bis-(2-ethylhexanoate), triethylene glycol bis-(2-ethylhexanoate) (3GO), triethylene glycol bis-(2-ethylbutanoate), tetraethylene glycol bis-n-heptanoate, triethylene glycol bis-n-heptanoate, triethylene glycol bis-n-hexanoate, tetraethylene glycol dimethyl ether, and dipropylene glycol dibenzoate.

[0052] (P-c) Phosphate esters of aliphatic or aromatic alcohols. Examples of such phosphate esters include tris(2-ethylhexyl)phosphate, triethylphosphate, diphenyl-2-ethylhexylphosphate, and tricresylphosphate. (P-d) Esters of citric acid, succinic acid, or fumaric acid. (P-e) Polyesters or oligoesters obtained from polyhydric alcohols and polycarboxylic acids; terminal esterified or etherified products thereof; polyesters or oligoesters obtained from lactones or hydroxycarboxylic acids; terminal esterified or etherified products thereof.

[0053] When both the first resin film and the second resin film described below, which are made of the polyvinyl acetal resin film of the present disclosure, contain a plasticizer, from the viewpoint of suppressing problems such as changes in physical properties over time due to migration of the plasticizer between these films, it is preferable to use the same plasticizer as that contained in the second resin film, or a plasticizer that does not impair the physical properties of the second resin film (e.g., heat resistance, light resistance, transparency, and plasticizing effect). Specifically, triethylene glycol-bis-(2-ethylhexanoate) (3G8), triethylene glycol-bis(2-ethylbutanoate), tetraethylene glycol-bis-(2-ethylhexanoate), and tetraethylene glycol-bisheptanoate are preferred, with triethylene glycol-bis-(2-ethylhexanoate) (3G8) being particularly preferred.

[0054] (Other Additives) The polyvinyl acetal resin film of the present disclosure may contain one or more additives other than plasticizers, if necessary. Examples of other additives include ultraviolet absorbers, antioxidants, adhesion modifiers, (fluorescent) brighteners, stabilizers, processing aids, impact modifiers, flow modifiers, crosslinking agents, colorants such as pigments, dyes, and luminescent materials, refractive index modifiers, heat-shielding materials, organic or inorganic nanoparticles (e.g., nanoparticles having infrared absorption or reflection capabilities), calcined silica, and surfactants.

[0055] [Method for producing polyvinyl acetal resin film] The method for producing the polyvinyl acetal resin film of the present disclosure is not particularly limited, and examples thereof include extrusion, calendaring, pressing, casting, and inflation methods. Of these, extrusion using an extruder equipped with a T-die (also referred to as the T-die method) is preferred. The polyvinyl acetal resin film of the present disclosure has fine surface irregularities on at least one surface with a ten-point average roughness (Rz) of 2 to 7 μm. Methods for forming the surface irregularity structure include embossing roll methods, calendaring roll methods, and profile extrusion methods. Of these, the embossing roll method is preferred because it can easily form a relatively large amount of irregularities.

[0056] The T-die method will be described below. A resin material containing one or more polyvinyl acetal resins, optionally one or more plasticizers, and optionally one or more other additives is melt-kneaded using an extruder and extruded in a molten state from a T-die with a wide discharge port. Examples of extruders include single-screw extruders, twin-screw extruders, multi-screw extruders, and combinations thereof. The resin temperature during extrusion is not particularly limited, but is preferably 150 to 250°C, more preferably 170 to 230°C. If the resin temperature is too high, the polyvinyl acetal resin may decompose, resulting in a large amount of volatile substances. If the resin temperature is too low, the amount of volatile substances may also increase. To efficiently remove the volatile substances, it is preferable to remove the volatile substances by reducing the pressure through a vent port of the extruder.

[0057] To remove foreign matter, the molten resin is preferably melt-filtered using a filter before extrusion. By forming a film using the melt-filtered molten resin, a film with fewer defects caused by foreign matter and gels can be obtained. The filter material is appropriately selected based on the operating temperature, viscosity, filtration accuracy, etc. Examples include nonwoven fabrics made of glass fiber, etc.; sheets made of phenolic resin-impregnated cellulose; sintered metal fiber nonwoven sheets; sintered metal powder sheets; wire mesh; and combinations thereof. Among these, from the viewpoint of heat resistance and durability, a filter formed by stacking multiple sintered metal fiber nonwoven sheets is preferred. The filtration accuracy of the filter is not particularly limited, but is preferably 30 μm or less, more preferably 15 μm or less, and particularly preferably 5 μm or less. To improve the thickness accuracy of the film, a gear pump may be installed in the extrusion molding line to perform film formation.

[0058] The molten resin extruded into a film form from a T-die is cooled using multiple cooling rolls. Examples of cooling rolls include rigid metal rolls and elastic metal rolls. Rigid metal rolls are inelastic rolls made of metal such as stainless steel, and include drilled rolls and spiral rolls. The surface of the rigid metal roll may be a mirror finish or may have a pattern or irregularities. Elastic metal rolls are rolls with an elastic outer cylinder made of a thin metal film on their outer periphery. For example, elastic metal rolls consist of a metal shaft roll made of stainless steel or the like, a thin metal film (elastic outer cylinder) made of stainless steel or the like covering the outer surface of the shaft roll, and a fluid sealed between the shaft roll and the thin metal film (elastic outer cylinder), and can exhibit elasticity in the presence of the fluid. Examples of fluids include water and oil. The thickness of the thin metal film of the elastic metal roll is not particularly limited, but is preferably about 2 to 8 mm. The thin metal film preferably has flexibility and bendability, and preferably has a seamless structure without welded joints. Such a metal elastic roll equipped with a metal thin film is highly durable, and if the metal thin film is mirror-finished, it can be handled in the same way as a normal mirror-finished roll. If a pattern, irregularities, etc., are imparted to the metal thin film, the roll can transfer the shape, making it easy to use. By using a roll having a surface irregularity of appropriate roughness (also called an embossing roll) as one or more cooling rolls, it is possible to produce a polyvinyl acetal resin film of the present disclosure, in which at least one surface has a ten-point average roughness (Rz) of 2 to 7 μm. The film obtained after cooling is taken up by a take-up roll. The above-mentioned extrusion, cooling, and take-up steps are carried out continuously.

[0059] [First Film Laminate] The first film laminate of the present disclosure comprises the polyvinyl acetal resin film of the present disclosure described above, and a light-reflecting layer of a single-layer or laminate structure that reflects at least a portion of light, or a light-reflecting film including this light-reflecting layer. The light-reflecting layer can directionally reflect or diffusely reflect at least a portion of incident light in a specific direction. When the light-reflecting layer reflects directionally, the observer can view a virtual image through the light-reflecting layer. When the light-reflecting layer reflects diffusely, the observer can view a real image on the light-reflecting layer. In applications such as head-up display (HUD) devices, the light-reflecting layer is preferably a semi-transmissive semi-reflective layer (also referred to as a half-mirror layer).

[0060] FIG. 1 shows a schematic cross-sectional view of a first film laminate according to one embodiment of the present invention. In the figure, symbol FL1 represents the first film laminate, symbol 10 represents the polyvinyl acetal resin film of the present disclosure, and symbol 20 represents a light-reflecting layer or a light-reflecting film. The first film laminate of the present disclosure preferably includes the polyvinyl acetal resin film of the present disclosure and a light-reflecting film. Examples of methods for producing the first film laminate of the present disclosure include a method of superposing the polyvinyl acetal resin film of the present disclosure and a light-reflecting film; a method of thermocompression bonding a temporary laminate obtained by this method; and a method of applying a resin solution containing a polyvinyl acetal resin and a solvent onto the light-reflecting layer or the light-reflecting film and then drying and removing the solvent. The first film laminate of the present disclosure includes a temporary laminate before thermocompression bonding in which the polyvinyl acetal resin film of the present disclosure and a light-reflecting film are superimposed; a thermocompression-bonded body obtained by thermocompression bonding this temporary laminate; a laminate of a light-reflecting layer or a light-reflecting film and a coated and dried product of a polyvinyl acetal resin solution; and the like.

[0061] The light-reflecting layer may be an inorganic film having a single layer structure or a multilayer structure, containing one or more inorganic substances selected from the group consisting of metals and metal compounds. Examples of the metal compounds include metal oxides, metal nitrides, and metal oxynitrides. Examples of the metal compounds include oxides, nitrides, and oxynitrides of at least one metal element selected from the group consisting of B, Al, Si, Ti, Cr, Ni, Zn, Ga, Y, Zr, Nb, In, Sn, Hf, Ta, and W. For example, Al 2 O 3 , SiO 2 , TiO 2 , ZnO, Ga 2 O 5 , Y 2 O 3 , ZrO 2 , Nb 2 O 5 , In 2 O 3 , ITO (indium tin oxide), SnO 2 , HfO 2 , Ta 2 O 5 , and W.O. 3 Metal oxides such as AlN, SiN x , and TiN x Examples of the inorganic film include metal nitrides such as SiO2, AlON, SiON, and the like; metal oxynitrides such as AlON and SiON; and combinations thereof. The light-reflecting layer may be formed by doping any of the above metal compounds with any element. The reflectance of the light-reflecting layer can be adjusted by appropriately selecting the type of inorganic material, the thickness of each layer, the number of layers, the total thickness, and the like. Examples of methods for forming the inorganic film include vacuum deposition, sputtering, ion plating, laser ablation, chemical vapor deposition (CVD), and plasma-enhanced chemical vapor deposition (plasma CVD).

[0062] Light-reflective films include substrate-containing types that include a substrate resin film and a light-reflective layer having a single-layer or laminated structure, and substrate-free types that do not include a substrate resin film and consist only of a light-reflective layer having a single-layer or laminated structure. Substrate-containing light-reflective films include those in which a light-reflective layer made of the above-mentioned inorganic film having a single-layer or laminated structure is formed on a substrate resin film containing a thermoplastic resin such as polyethylene terephthalate (PET) or polycarbonate resin (PC). Substrate-free light-reflective films include embossed hologram films, reflective hologram films, and nano-laminate films. Nano-laminate films include reflective polarizing films (such as "DBEF (registered trademark)" manufactured by Sumitomo 3M), metallic gloss / easy-formable films (such as "PICASUS (registered trademark)" manufactured by Toray Industries, Inc.), and ultra-multilayer shrink films (such as "MLF (registered trademark)" manufactured by Teijin DuPont Films). The total thickness of the light-reflecting layer is not particularly limited, but is preferably 50 to 150 nm if it has a single layer structure, and is preferably 200 to 500 nm if it has a laminate structure. The total thickness of the light-reflecting film is not particularly limited, but is preferably 50 to 150 μm, more preferably 80 to 120 μm.

[0063] The first film laminate of the present disclosure may have another functional layer between the polyvinyl acetal resin film of the present disclosure and the light-reflecting layer or light-reflecting film. The function of the functional layer is not particularly limited, and examples thereof include a function of protecting the light-reflecting layer or light-reflecting film from a plasticizer contained in the polyvinyl acetal resin film of the present disclosure, a function of improving adhesion between the polyvinyl acetal resin film of the present disclosure and the light-reflecting layer or light-reflecting film, a function of absorbing or reflecting ultraviolet rays contained in sunlight, a function of absorbing or reflecting infrared rays contained in sunlight, and a function of containing a material with low thermal conductivity and preventing heat propagation to the light-reflecting layer or light-reflecting film.

[0064] [Second Film Laminate] The second film laminate of the present disclosure has, on a first resin film made of the polyvinyl acetal resin film of the present disclosure, a light-reflecting layer having a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including this light-reflecting layer, and a second resin film, in this order.

[0065] Figure 2 shows a schematic cross-sectional view of a second film laminate according to an embodiment of the present invention. The same components as those in Figure 1 are designated by the same reference numerals, and a description thereof will be omitted. In the figure, reference numeral FL2 denotes the second film laminate, and reference numeral 30 denotes the second resin film. The second film laminate of the present disclosure preferably includes, on a first resin film made of the polyvinyl acetal resin film of the present disclosure, a light-reflecting film including a light-reflecting layer that reflects at least a portion of light, and a second resin film, in that order.

[0066] Examples of methods for producing the second film laminate of the present disclosure include a method of superposing a first resin film, a light-reflecting film, and a second resin film, each made of the polyvinyl acetal resin film of the present disclosure; a method of thermocompression bonding a temporary laminate obtained by this method; a method of superposing the first film laminate of the present disclosure and a second resin film; a method of thermocompression bonding a second resin film and a light-reflecting film, and then superposing a first resin film made of the polyvinyl acetal resin film of the present disclosure; a method of applying a resin solution containing the constituent resins of the second resin film and a solvent onto a light-reflecting layer or light-reflecting film, drying and removing the solvent to obtain a film laminate of the light-reflecting layer or light-reflecting film and the second resin film, and then superposing this film laminate with a first resin film made of the polyvinyl acetal resin film of the present disclosure; and a method of thermocompression bonding a temporary laminate obtained by these methods.

[0067] The second film laminate of the present disclosure includes a temporary laminate obtained by superposing a first resin film, a light-reflecting film, and a second resin film, each of which is made of the polyvinyl acetal resin film of the present disclosure; a temporary laminate obtained by superposing the first film laminate of the present disclosure and a second resin film; a temporary laminate obtained by superposing a thermocompression-bonded product of a second resin film and a light-reflecting film and a first resin film made of the polyvinyl acetal resin film of the present disclosure; a temporary laminate obtained by superposing a laminate of a light-reflecting layer or a light-reflecting film and a coated and dried product of a resin solution containing the constituent resin of the second resin film and a first resin film made of the polyvinyl acetal resin film of the present disclosure; and a thermocompression-bonded product obtained by thermocompression-bonding these temporary laminates.

[0068] The second resin film is preferably a resin film for use as an interlayer in laminated glass. The second resin film is preferably a resin film containing one or more resins selected from the group consisting of polyvinyl acetal resin, ionomer resin, ethylene-vinyl acetate copolymer, cycloolefin polymer, and polyurethane. Among these, a polyvinyl acetal resin film containing 60 to 80 mass% of polyvinyl acetal resin and 40 to 20 mass% of plasticizer, relative to 100 mass% of the second resin film, is preferred. The second resin film may contain one or more additives other than the plasticizer, as necessary. The types of other additives and the manufacturing method of the second resin film are the same as those of the polyvinyl acetal resin film of the present disclosure. A commercially available resin film for use as an interlayer in laminated glass may also be used as the second resin film.

[0069] The thickness of the second resin film is not particularly limited and is preferably 100 to 1600 μm. The lower limit is more preferably 350 μm, even more preferably 500 μm, particularly preferably 600 μm, and most preferably 700 μm. The upper limit is more preferably 1200 μm, even more preferably 1000 μm, particularly preferably 900 μm, and most preferably 800 μm. When the thickness of the second resin film is within the above range, excellent penetration resistance is easily obtained. The second resin film may have a wedge-shaped cross section. In this case, the second resin film can have functions such as sound insulation and heat insulation. Furthermore, in applications such as head-up display (HUD) devices, the refractive index can be well controlled, enabling clear image display.

[0070] The ten-point average roughness (Rz) of the surface of the second resin film, measured in accordance with JIS B0601-1994, is not particularly limited, but is preferably 10 to 50 μm, more preferably 20 to 40 μm, from the viewpoint of degassing properties during the production of laminated products such as laminated glass.

[0071] The second film laminate of the present disclosure may have another functional layer between the light-reflecting layer or light-reflecting film and the second resin film. The function of the functional layer is not particularly limited, and examples thereof include a function of protecting the light-reflecting layer or light-reflecting film from a plasticizer that may be contained in the second resin film, a function of improving adhesion between the light-reflecting layer or light-reflecting film and the second resin film, a function of absorbing or reflecting ultraviolet rays contained in sunlight, a function of absorbing or reflecting infrared rays contained in sunlight, and a function of containing a material with low thermal conductivity and preventing heat propagation to the light-reflecting layer or light-reflecting film.

[0072] [Third Film Laminate] The third film laminate of the present disclosure includes, on the polyvinyl acetal resin film of the present disclosure, a light-reflecting layer having a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer, and a hard coat layer, which are arranged in this order. The hard coat layer can function as a scratch-resistant layer that protects the light-reflecting layer or the light-reflecting film from scratches.

[0073] Figure 3 shows a schematic cross-sectional view of a third film laminate according to an embodiment of the present invention. The same components as those in Figure 1 are designated by the same reference numerals, and a description thereof will be omitted. In the figure, reference numeral FL3 denotes the third film laminate, and reference numeral 60 denotes a hard coat layer. The third film laminate according to the present disclosure preferably includes, on a first resin film made of the polyvinyl acetal resin film according to the present disclosure, a light-reflecting film including a light-reflecting layer that reflects at least a portion of light, and a hard coat layer, in that order.

[0074] Examples of methods for producing the third film laminate of the present disclosure include a method of forming a hard coat layer on a light-reflecting layer or a light-reflecting film, and then superposing the obtained light-reflecting film with the hard coat layer on the polyvinyl acetal resin film of the present disclosure described above; a method of thermocompression bonding a temporary laminate obtained by this method; a method of forming a hard coat layer on a light-reflecting layer or a light-reflecting film, and then applying a resin solution containing a polyvinyl acetal resin and a solvent onto the obtained light-reflecting film with the hard coat layer, and then drying and removing the solvent to form the polyvinyl acetal resin film of the present disclosure; and a method of forming a hard coat layer on the first film laminate of the present disclosure described above.

[0075] The third film laminate of the present disclosure includes a temporary laminate obtained by stacking a light reflective film with a hard coat layer and the above-described polyvinyl acetal resin film of the present disclosure; a thermocompression-bonded body obtained by thermocompression-bonding this temporary laminate; a laminate of a light reflective film with a hard coat layer and a coated and dried product of a polyvinyl acetal resin solution; and a first film laminate with a hard coat layer obtained by forming a hard coat layer on the above-described first film laminate of the present disclosure.

[0076] Materials for the hard coat layer include inorganic, organic, organic-inorganic, and silicone materials, and from the viewpoint of productivity, organic and organic-inorganic materials are preferred. The thickness of the hard coat layer is not particularly limited, and is preferably 0.5 to 30 μm, more preferably 1 to 20 μm, and particularly preferably 1.5 to 15 μm.

[0077] The inorganic hard coat layer may be, for example, SiO 2 , Al 2 O3 , TiO 2 , and ZrO 2 The hard coat layer can be formed by depositing an inorganic material such as a metal oxide by vapor-phase deposition, such as vacuum deposition or sputtering. The organic hard coat layer can be formed by applying a curable composition containing one or more curable compounds and curing it by heating or ionizing radiation. Examples of the curable compound include monomers, oligomers, prepolymers, and curable resins. Examples of curable compounds that cure upon heating include thermosetting resins such as polyester resins, epoxy resins, polyurethane resins, aminoalkyd resins, melamine resins, guanamine resins, urea resins, and thermosetting acrylic resins. Examples of curable compounds that cure upon ionizing radiation include oligomers and prepolymers having radically polymerizable unsaturated groups in the molecule. Specific examples include oligomers and prepolymers such as epoxy (meth)acrylates, urethane (meth)acrylates, polyether-based urethane (meth)acrylates, caprolactone-based urethane (meth)acrylates, polyester (meth)acrylates, and polyether (meth)acrylates. Ionizing radiation is electromagnetic waves and charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules, and specific examples include electromagnetic waves such as ultraviolet (UV) rays, electron beams (EB), X-rays, and gamma rays; and charged particle beams such as alpha rays, beta rays, and ion beams.

[0078] The organic hard coat layer can also be formed by a known method using a resin sheet for reinforcing glass. Commercially available resin sheets for reinforcing glass include "Spallshield (registered trademark) CPET sheeting" manufactured by Kuraray Co., Ltd.

[0079] The organic-inorganic hard coat layer can be formed, for example, by applying an ultraviolet-curable hard coat coating material containing inorganic ultrafine particles such as silica ultrafine particles having photopolymerizable functional groups introduced on the surface and a curable organic component, and then polymerizing the curable organic component with the photopolymerizable functional groups of the inorganic ultrafine particles by ultraviolet irradiation. This method results in a network-like crosslinked coating film in which the inorganic ultrafine particles are dispersed in the organic matrix while being chemically bonded to the organic matrix.

[0080] The silicone-based hard coat layer can be formed, for example, by polycondensing partial hydrolysates of carbon functional alkoxysilane, alkyltrialkoxysilane, tetraalkoxysilane, etc., or materials obtained by blending these with colloidal silica.

[0081] Examples of methods for applying the curable composition include dip coating, various roll coating methods such as gravure roll coating, flow coating, rod coating, blade coating, spray coating, die coating, and bar coating.

[0082] The third film laminate of the present disclosure may have another functional layer between the light-reflecting layer or light-reflecting film and the hard coat layer. The function of the functional layer is not particularly limited, and examples thereof include a function of improving adhesion between the light-reflecting layer or light-reflecting film and the hard coat layer, a function of absorbing or reflecting ultraviolet rays contained in sunlight, a function of absorbing or reflecting infrared rays contained in sunlight, a function of containing a material with low thermal conductivity and preventing heat propagation to the light-reflecting layer or light-reflecting film, etc.

[0083] [First Laminate] The first laminate of the present disclosure includes the second film laminate of the present disclosure and a pair of light-transmitting substrates sandwiching the second film laminate. Figure 4 shows a schematic cross-sectional view of a first laminate of one embodiment according to the present invention. The same components as those in Figure 2 are given the same reference numerals, and their explanations will be omitted. In the figure, symbol LB1 denotes the first laminate, symbol 41 denotes the first light-transmitting substrate, and symbol 42 denotes the second light-transmitting substrate.

[0084] From the viewpoints of transparency, weather resistance, and mechanical strength, the translucent substrate is preferably a glass plate or a glass laminate in which one or more layers or elements are formed on at least one surface of a glass plate. Examples of glass plates include inorganic glass (also simply referred to as "glass") and organic glass. The shape of the translucent substrate is not particularly limited, and it may be a flat plate without a curved surface or a plate with a curved surface. Examples of inorganic glass include float glass, tempered glass, semi-tempered glass, chemically strengthened glass, green glass, and quartz glass. Examples of organic glass include methacrylic resin sheets, polycarbonate resin sheets, polystyrene resin sheets, polyester resin sheets, polyimide resin sheets, and polycycloolefin resin sheets. Among these, inorganic glass, methacrylic resin sheets, or polycarbonate resin sheets are preferred, and inorganic glass is particularly preferred. The first laminate of the present disclosure may be laminated glass.

[0085] The first laminate of the present disclosure may have another functional layer between the first light-transmitting substrate and the polyvinyl acetal resin film of the present disclosure, or between the second resin film and the second light-transmitting substrate. The function of the functional layer is not particularly limited, and examples thereof include a function of improving adhesion between the first light-transmitting substrate and the polyvinyl acetal resin film of the present disclosure, or between the second light-transmitting substrate and the second light-transmitting substrate, a function of absorbing or reflecting ultraviolet rays contained in sunlight, a function of absorbing or reflecting infrared rays contained in sunlight, a function of containing a material with low thermal conductivity and preventing heat propagation to the light-reflecting layer or the light-reflecting film, and the like.

[0086] [Second Laminate] The second laminate of the present disclosure has, on a light-transmitting substrate, the polyvinyl acetal resin film of the present disclosure, a light-reflecting layer of a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including this light-reflecting layer, and a hard coat layer, in that order. Figure 5 shows a schematic cross-sectional view of a second laminate of one embodiment according to the present invention. The same components as in Figure 3 are given the same reference numerals, and their descriptions are omitted. In the figure, symbol LB2 denotes the second laminate, and symbol 50 denotes the light-transmitting substrate. The second laminate of the present disclosure preferably has, on a light-transmitting substrate, the polyvinyl acetal resin film of the present disclosure, a light-reflecting film, and a hard coat layer, in that order.

[0087] From the viewpoints of transparency, weather resistance, and mechanical strength, the translucent substrate preferably includes a glass plate or a glass laminate in which any one or more layers or elements are formed on at least one surface of a glass plate. Examples and shapes of the glass plate are the same as those of the glass plate for the translucent substrate of the first laminate of the present disclosure. In the second laminate of the present disclosure, the glass plate may be laminated glass in which a plurality of glass plates are bonded together via an interlayer film.

[0088] The second laminate of the present disclosure may have another functional layer between the light-transmitting substrate and the polyvinyl acetal resin film of the present disclosure. The function of the functional layer is not particularly limited, and examples thereof include a function of improving adhesion between the light-transmitting substrate and the polyvinyl acetal resin film of the present disclosure, a function of absorbing or reflecting ultraviolet rays contained in sunlight, a function of absorbing or reflecting infrared rays contained in sunlight, and a function of containing a material with low thermal conductivity and preventing heat propagation to the light-reflecting layer or the light-reflecting film.

[0089] [Method for manufacturing first and second laminates] The method for manufacturing the first and second laminates of the present disclosure includes the steps of: (S1) obtaining a temporary laminate having, on a light-transmitting substrate, the polyvinyl acetal resin film of the present disclosure; and a light-reflecting layer having a single-layer or laminate structure that reflects at least a portion of light, or a light-reflecting film including this light-reflecting layer, in which the light-transmitting substrate and the polyvinyl acetal resin film are in contact without being bonded; and (S2) thermocompression bonding the temporary laminate. In step (S1), with respect to components other than the light-transmitting substrate that constitute the temporary laminate, adjacent components may be bonded to each other by thermocompression bonding or the like. In step (S1), it is preferable to contact the light-transmitting substrate with a surface of the polyvinyl acetal resin film of the present disclosure having a ten-point average roughness (Rz) of 2 to 7 μm.

[0090] In the method for producing the first laminate of the present disclosure, in step (S1), a temporary laminate is obtained which has, on a first light-transmitting substrate, a polyvinyl acetal resin film of the present disclosure, a light-reflecting layer or film, a second resin film, and a second light-transmitting substrate, in that order, and in which the first light-transmitting substrate and the polyvinyl acetal resin film of the present disclosure are in contact with each other without being bonded.

[0091] In the method for producing the first laminate of the present disclosure, a first aspect of step (S1) can include: a step (S1-1) of thermocompression bonding the polyvinyl acetal resin film and a light reflective film of the present disclosure to obtain the first film laminate of the present disclosure; and a step (S1-2) of stacking a plurality of members including a first light-transmitting substrate, the first film laminate of the present disclosure, a second resin film, and a second light-transmitting substrate to obtain a temporary laminate.

[0092] In the method for producing the first laminate of the present disclosure, a second aspect of step (S1) can include: a step (S1-1) of thermocompression bonding the polyvinyl acetal resin film, the light reflective film, and the second resin film of the present disclosure to obtain the second film laminate of the present disclosure; and a step (S1-2) of stacking a plurality of members including the first light-transmitting substrate, the second film laminate of the present disclosure, and the second light-transmitting substrate to obtain a temporary laminate.

[0093] In the above-described method for producing the second laminate according to the present disclosure, in step (S1), a temporary laminate is obtained which has, on a light-transmitting substrate, the polyvinyl acetal resin film according to the present disclosure, a light-reflecting layer or film, and a hard coat layer, in that order, and in which the light-transmitting substrate and the polyvinyl acetal resin film according to the present disclosure are in contact with each other without being bonded.

[0094] In the method for producing the second laminate of the present disclosure, one aspect of step (S1) can include a step (S1-1) of obtaining the third film laminate of the present disclosure by a method of thermocompression bonding the polyvinyl acetal resin film of the present disclosure and a light reflective film and forming a hard coat layer on the light reflective film, or a method of thermocompression bonding the polyvinyl acetal resin film of the present disclosure and a light reflective film with a hard coat layer, and a step (S1-2) of stacking multiple members including a translucent substrate and the third film laminate of the present disclosure to obtain a temporary laminate. In the method for producing the second laminate of the present disclosure, a protective member such as a cover glass may be placed on the temporary laminate in step (S2).

[0095] In the manufacturing method of the first and second laminates of the present disclosure, it is preferable that step (S2) sequentially includes a step (S2-1) (also referred to as a preliminary pressure-bonding step) of heating the temporary laminate at a temperature of 90 to 110°C to obtain a pre-pressed body, and a step (S2-2) (also referred to as a main pressure-bonding step) of pressurizing and heating the pre-pressed body at a temperature higher than the heating temperature of step (S2-1).

[0096] Preliminary pressure-bonding methods, from the viewpoint of degassing ability and inter-component bonding, include degassing methods under reduced pressure, such as the vacuum bag method, vacuum ring method, and vacuum laminator method; degassing methods using nip rolls; and compression methods at high temperatures. Among these, degassing methods under reduced pressure are preferred. For details on the vacuum bag method and the vacuum ring method, see British Patent No. 1,235,683. The vacuum laminator may include a heatable and evacuable chamber. The absolute pressure in the preliminary pressure-bonding step is preferably 10 to 30 kPa. The heating time is preferably 10 to 60 minutes, more preferably 20 to 60 minutes. In the main pressure-bonding step, for example, the obtained pre-pressurized body can be placed in an autoclave and pressurized and heated at a pressure of 1.0 to 1.5 MPa and a temperature higher than the heating temperature in step (S2-1). The heating temperature is preferably 110 to 150°C, more preferably 120 to 150°C. The heating time is preferably 20 to 40 minutes.

[0097] The polyvinyl acetal resin film of the present disclosure can have the following properties before the step (S2-2) (pressurizing and heating step) is performed: a thickness (T) of 5 to 350 μm, a ten-point average roughness (Rz) of at least one surface of 2 to 7 μm, and a shear storage modulus (G'(100)) at 100°C of 0.3 to 0.7 MPa.

[0098] [Glazing Material] The glazing material of the present disclosure comprises the first or second laminate of the present disclosure. In the use of the glazing material, the translucent substrate comprises a glass plate or a glass laminate. The glazing material of the present disclosure is suitable for applications in vehicles such as trains, electric trains, automobiles, ships, and aircraft; architecture, and the like. The glazing material of the present disclosure is suitable for vehicle window glass such as windshields, rear windows, roof glass, and side glass. In the use of vehicle window glass, when the glazing material comprising the first laminate of the present disclosure is arranged so that the second translucent substrate faces the interior of the vehicle, detachment of the glass on the interior of the vehicle is suppressed, which is advantageous in terms of impact resistance. The glazing material comprising the second laminate of the present disclosure is preferably arranged so that the hard coat layer side faces the interior of the vehicle.

[0099] The glazing material of the present disclosure includes a glazing material and an image display device arranged outside the glazing material, and is suitable as an optical component (specifically, a windshield, combiner, etc.) for a head-up display (HUD) device that displays an image by projecting light from the image display device toward the glazing material and allowing an observer to view the light reflected by a light-reflecting layer within the glazing material.

[0100] [Head-up display device] The head-up display (HUD) device of the present disclosure includes a windshield or combiner including the glazing material of the present disclosure. Figures 6 and 7 show schematic cross-sectional views of head-up display (HUD) devices according to first and second embodiments of the present invention. The same components as those in Figures 4 and 5 are designated by the same reference numerals, and their descriptions will be omitted. In the figures, reference numerals HD1 and HD2 denote head-up display (HUD) devices, reference numeral 70 denotes an image display device such as a liquid crystal display, reference numeral 80 denotes a virtual image, and reference numeral 90 denotes the observer's eye. The head-up display device HD1 includes a glazing material including a first laminate LB1 and an image display device 70 such as a liquid crystal display. The head-up display device HD2 includes a glazing material including a second laminate LB2 and an image display device 70 such as a liquid crystal display. Light emitted from an image display device 70 such as a liquid crystal display is reflected by the surface 20S of the light reflecting layer included in the first laminate LB1 or the second laminate LB2, and enters the viewer's eye 90. The viewer can visually recognize a virtual image 80 beyond the first laminate LB1 or the second laminate LB2. This virtual image is a reflected image that is displayed on the image display device 70 and then reflected by the surface 20S of the light reflecting layer, and is also called a HUD image.

[0101] In the first laminate LB1, a portion of the light incident on the first laminate LB1 undergoes Fresnel reflection at the interface between the second light-transmitting substrate 42 (the light-transmitting substrate on the viewer's side) and air, which may cause the viewer to see light reflected at a surface other than the light-reflecting layer as a ghost image. Therefore, it is preferable to apply a known anti-reflection treatment to the surface of the second light-transmitting substrate 42 (the light-transmitting substrate on the viewer's side), or to convert the light incident on the first laminate LB1 to P-polarized light and allow it to enter the second light-transmitting substrate 42 (the light-transmitting substrate on the viewer's side) at approximately the Brewster angle. In the second laminate LB2, a portion of the light incident on the first laminate LB2 undergoes Fresnel reflection at the interface between the hard coat layer 60 and air. However, because the thickness of the hard coat layer 60 is very thin compared to the light-transmitting substrate, such as a glass plate, the optical path of this Fresnel-reflected light substantially overlaps with the optical path of the light reflected by the surface 20S of the light-reflecting layer, and therefore no ghost image is visible. The quality of the reflected images of the first and second laminates LB1 and LB2 can be measured using the modulation transfer function (MTF). According to the present disclosure, an MTF of 0.2 or more, for example, 0.2 to 0.5, can provide a reflected image with high resolution and visibility. The MTF can be measured by the method described in the Examples section below.

[0102] As described above, the present disclosure can provide a polyvinyl acetal resin film that is suitable as a material for a laminate for a head-up display (HUD) device, which includes a light-transmitting substrate and a light-reflecting layer or a light-reflecting film, and that can improve the image quality of a reflected image reflected on the surface of the light-reflecting layer, as well as a film laminate and a laminate using the same.

[0103] Examples and comparative examples according to the present invention will be described. [Evaluation Items and Evaluation Methods] The evaluation items and evaluation methods are as follows. (Ten-point average roughness (Rz)) Using a stylus surface profiler ("Dektak150" manufactured by ULVAC, Inc.), the surface profile of a polyvinyl acetal resin film was measured under conditions of a stylus pressure of 5 mg, a measurement distance of 5 mm, and a measurement time of 50 seconds, and the ten-point average roughness (Rz) was determined.

[0104] (Thickness) The thickness of the film was measured using a micrometer ("U-shaped steel plate micrometer PMU-MX" manufactured by Mitutoyo Corporation).

[0105] (Shear storage modulus (G'(100)) A circular test piece having a diameter of 8 mm was obtained from the polyvinyl acetal resin film. Using a viscoelasticity measuring device (TA Instruments' "ARES-G2"), viscoelasticity measurement was carried out under conditions in which the test piece was heated from 30°C to 200°C at a heating rate of 5°C / min in a vibration mode at a frequency of 10 Hz, and the shear storage modulus (G'(100)) at 100°C was determined. The average value of G'(100) for a total of three samples was used as data.

[0106] (Image Quality of Reflected Image) As shown in Figures 6 and 7, a liquid crystal display was placed at a -58° angle (see the angle θ in the figure) relative to the normal (VL) to the surface of the light-reflecting layer of the laminate. The distance between the display and the light-reflecting layer was approximately 300 mm. A black-and-white bar chart for MTF measurement (white bar pitch = black bar pitch = 1 / 60° = approximately 0.016°) was displayed on the display. Since image quality cannot be evaluated if there is any reflected light other than that reflected by the surface of the light-reflecting layer, only P-polarized light was emitted from the display. Since the light emitted from the display (P-polarized light) is incident on the laminate at Brewster's angle, it is not reflected at the interface between the air and the laminate, but is reflected only by the surface of the light-reflecting layer. A two-dimensional luminance meter ("ACE" manufactured by HI-LAND) was placed at a +58° angle relative to the normal (VL) to the surface of the light-reflecting layer of the laminate. The distance between the two-dimensional luminance meter and the light-reflecting layer was approximately 550 mm. The luminance distribution of the reflected image (virtual image) of the black and white bar chart reflected on the surface of the light-reflecting layer was measured, and the maximum luminance (white luminance) and minimum luminance (black luminance) were determined. The modulation transfer function (MTF) was calculated based on the following formula. The MTF is in the range of 0 to 1, and the larger the value, the higher the image quality. [MTF] = ([Maximum luminance] - [Minimum luminance]) / ([Maximum luminance] + [Minimum luminance])

[0107] [Materials] The materials used were as follows. <Polyvinyl acetal resins> (PVB1) A polyvinyl butyral resin obtained by acetalizing a polyvinyl alcohol resin with n-butyl aldehyde, "Mowital B60H" manufactured by Kuraray Co., Ltd., with a weight-average molecular weight (Mw) of 50,000 to 60,000, a vinyl alcohol unit content of 26.2 to 30.2 mol%, a vinyl acetate unit content of 0.7 to 3.0 mol%, and a degree of acetalization of 68.9 to 73.6 mol%. (PVB2) A polyvinyl butyral resin obtained by acetalizing a polyvinyl alcohol resin with a viscosity-average degree of polymerization of approximately 1700 with n-butyl aldehyde, with a vinyl alcohol unit content of 29.7 mol%, a vinyl acetate unit content of 0.9 mol%, and a degree of acetalization of 70 mol%. (PVB3) Polyvinyl butyral resin obtained by acetalizing polyvinyl alcohol resin with n-butyl aldehyde, "Mowital B30H" manufactured by Kuraray Co., Ltd., weight average molecular weight (Mw) 18,000 to 28,000, vinyl alcohol unit content 26.2 to 30.2 mol%, vinyl acetate unit content 0.7 to 3.0 mol%, degree of acetalization 68.9 to 73.6 mol%.

[0108] <Plasticizer> (P-1) Triethylene glycol bis(2-ethylhexanoate) (3G8). <Ultraviolet absorber> (U-1) Benzotriazole-based, "Tinuvin (registered trademark) 360" manufactured by BASF. <Antioxidant> (O-1) "Songnox 2450" manufactured by SONGWON.

[0109] Example (E-1) 98 parts by mass of polyvinyl acetal resin (PVB1), 2 parts by mass of plasticizer (P-1), 1.5 parts by mass of ultraviolet absorber (U-1), and 0.073 parts by mass of antioxidant (O-1) were melt-kneaded at 200°C using a twin-screw extruder, extruded into a strand, and pelletized. The resulting pellets were placed in a single-screw vent extruder with a screw diameter of 50 mmφ, melt-kneaded at 200°C, and extruded into a film from a T-die at 210°C. The extruded resin was cooled using multiple cooling rolls including an embossing roll and a mirror-finished roll, and taken up with a pair of take-up rolls. In this manner, a 50 μm-thick first polyvinyl acetal resin film (F1-1) was obtained. The obtained film had one surface which was a mirror finish with a ten-point average roughness (Rz) of 0.6 μm, and the other surface which was an embossed surface with a ten-point average roughness (Rz) of 6.2 μm.

[0110] A 100 μm thick polyethylene terephthalate (PET) film was used as a base resin film, and a SiO 2 film was used as a light reflective layer (half mirror layer) on one surface of the film. 2 layer and TiO 2 A light-reflecting film (R-1) was prepared by vapor-depositing a SiO layer and a SiO layer alternately to a total thickness of about 350 nm. The SiO layer was vapor-deposited so that the reflectance of P-polarized light incident on the surface of the light-reflecting layer (half mirror layer) at an incident angle of 58° (also referred to as the P-polarized light reflectance at an incident angle of 58°) was about 15%. 2 layer and TiO 2 The number of layers and the thickness of each layer were designed. The light-reflecting film (R-1) was overlaid on the polyvinyl acetal resin film (F1-1) so that the mirror surface of the polyvinyl acetal resin film (F1-1) and the PET film were in contact with each other, and these were thermocompression-bonded at 75°C to obtain a first film laminate (FL1-1) as shown in Figure 1.

[0111] 72 parts by mass of polyvinyl acetal resin (PVB2) and 28 parts by mass of plasticizer (P-1) were melt-kneaded at 200°C using a twin-screw extruder, extruded into strands, and pelletized. The resulting pellets were fed into a single-screw vent extruder with a screw diameter of 50 mmφ, melt-kneaded at 200°C, and extruded into a film form from a T-die at 210°C. The extruded resin was cooled using multiple cooling rolls including multiple embossing rolls and taken up with a pair of take-up rolls. In this way, a 760 μm-thick second polyvinyl acetal resin film (F2-1) was obtained. Both sides of the obtained film had embossed surfaces with a ten-point average roughness (Rz) of 32.9 μm.

[0112] The first film laminate (FL1-1), the second polyvinyl acetal resin film (F2-1), and the second glass plate were sequentially stacked on one surface of the first glass plate. In this process, the first glass plate and the embossed surface of the first polyvinyl acetal resin film (F1-1) were abutted against each other. The resulting pre-laminate was placed in a vacuum bag, and the vacuum bag was evacuated at room temperature for 15 minutes using a vacuum pump. The temperature was raised to 100 ° C while maintaining the reduced pressure in the vacuum bag, and heated for 60 minutes (pre-pressure bonding). After cooling to room temperature, the pressure was returned to normal, and the pre-pressure bonded body was removed. Next, the pre-pressure bonded body was placed in an autoclave and pressurized and heated at 140 ° C and 1.2 MPa for 30 minutes (main pressure bonding). In this manner, the first laminate (LB1-1) shown in FIG. 4 was obtained.

[0113] [Example (E-2)] As the light-reflecting film (R-2), a nano-laminate film ("Picasus (registered trademark)" manufactured by Toray Industries, Inc.) having a thickness of approximately 100 μm and consisting of a light-reflecting layer (half-mirror layer) having an alternating laminate structure of a high refractive index polymer layer and a low refractive index polymer layer was prepared. The P-polarized light reflectance of this light-reflecting film at an incident angle of 58° was approximately 15%. The light-reflecting film (R-2) was superimposed on the mirror surface of the polyvinyl acetal resin film (F1-1) obtained in Example (E-1), and these were thermocompression bonded at 75 ° C. to obtain a first film laminate (FL1-2) as shown in FIG. 1. The subsequent steps were the same as in Example (E-1), and a first laminate (LB1-2) was obtained.

[0114] [Examples (E-3) to (E-6)] First polyvinyl acetal resin films (F1-3) to (F1-6) were obtained in the same manner as in Example (E-1), except that the blending composition and / or thickness of the first polyvinyl acetal resin film was changed. The subsequent steps were the same as in Example (E-2), and first laminates (LB1-3) to (LB1-6) were obtained.

[0115] [Example (E-7)] On the surface of the light-reflecting film (R-2) of the first film laminate (FL1-2) obtained in Example (E-2), a hard coat layer of about 3 μm thick made of polyethylene terephthalate (PET) was formed using "Spallshield (registered trademark) CPET sheeting" manufactured by Kuraray Co., Ltd., according to the manufacturer's recommended method. In this way, a film laminate with a hard coat layer (FL1-2H) was obtained. On one surface of a glass plate, the film laminate with a hard coat layer (FL1-2H) and a cover glass were sequentially stacked to obtain a provisional laminate, and preliminary pressure bonding and full pressure bonding were carried out in the same manner as in Example (E-2). The cover glass was peeled off from the obtained laminate, and a second laminate (LB2-1) as shown in FIG. 5 was obtained.

[0116] Comparative Examples (EC-1) to (EC-3) First polyvinyl acetal resin films (FC1-1) to (FC1-3) were obtained in the same manner as in Example (E-1), except that the blending composition and / or thickness of the first polyvinyl acetal resin film was changed. The subsequent steps were the same as in Example (E-2), and first laminates (LC1-1) to (LC1-3) were obtained.

[0117] Comparative Example (EC-4) A first polyvinyl acetal resin film (FC1-4) was obtained in the same manner as in Example (E-1), except that film formation was carried out without using an embossing roll. Both surfaces of the obtained film had a mirror finish with a ten-point average roughness (Rz) of 0.6 μm. The subsequent steps were the same as in Example (E-2), and a first laminate (LC1-4) was obtained.

[0118] [Summary of Results] The main production conditions and evaluation results are shown in Tables 3 and 4. In these tables, conditions not listed in the tables are common conditions. In the tables, "PVB" refers to polyvinyl acetal resin. The blending amount is expressed in parts by mass.

[0119]

[0120]

[0121] In Examples (E-1) to (E-7), the formulation and thickness were appropriately designed, and embossing was performed on at least one surface to obtain a first polyvinyl acetal resin film having a thickness (T) of 5 to 350 μm, an Rz of 2 to 7 μm on at least one surface, a shear storage modulus (G'(100)) at 100 ° C. of 0.3 to 0.7 MPa, and a plasticizer content of 0 to 20% by mass. In these Examples, a temporary laminate was obtained in which the obtained first polyvinyl acetal resin film and a light-reflecting film were sequentially placed on a light-transmitting substrate (specifically, a glass plate), and the light-transmitting substrate and the first polyvinyl acetal resin film were abutted together without bonding. In this process, the light-transmitting substrate and the surface of the first polyvinyl acetal resin film having an Rz of 2 to 7 μm were abutted against each other. The temporary laminate was heated under reduced pressure at a temperature of 90 to 110°C to obtain a pre-bonded body, and then the pre-bonded body was heated under pressure at a higher temperature to obtain a laminate as shown in Figure 4 or Figure 5. When the image quality of the reflected image was evaluated for the laminates obtained in these Examples, the MTF was 0.2 to 0.5, and a reflected image with high resolution and high visibility was obtained.

[0122] The first polyvinyl acetal resin film obtained in Comparative Example 1 had a shear storage modulus (G'(100)) at 100°C of more than 0.7 MPa. The first polyvinyl acetal resin film obtained in Comparative Example 2 had a thickness (T) of more than 350 µm. The first polyvinyl acetal resin film obtained in Comparative Example 3 had a plasticizer content of more than 20 mass%. The first polyvinyl acetal resin film obtained in Comparative Example 4 had Rz of less than 2 µm on both sides. When the image quality of the reflected images of the laminates obtained in these Comparative Examples was evaluated, the MTF was 0.1 or less in all cases, the resolution of the reflected images was low, and the visibility was poor.

[0123] The present invention is not limited to the above-described embodiments and examples, and appropriate design changes are possible without departing from the spirit of the present invention.

[0124] This application claims priority based on Japanese Patent Application No. 2023-087071, filed May 26, 2023, the disclosure of which is incorporated herein by reference in its entirety.

[0125] REFERENCE SIGNS LIST 10 Polyvinyl acetal resin film 20 Light-reflecting layer or light-reflecting film 20S Surface of light-reflecting layer 30 Second resin film 41, 42, 50 Light-transmitting substrate 60 Hard coat layer 70 Image display device 80 Virtual image 90 Observer's eye FL1 to FL3 Film laminate HD1, HD2 Head-up display device LB1, LB2 Laminate

Claims

1. A polyvinyl acetal resin film containing one or more polyvinyl acetal resins, the polyvinyl acetal resin content is 80-100% by mass and the plasticizer content is 20-0% by mass, relative to 100% by mass of the polyvinyl acetal resin film, the thickness (T) is 5-350 μm, at least one surface has a ten-point average roughness (Rz) of 2-7 μm as measured in accordance with JIS B0601-1994, and the shear storage modulus (G'(100)) at 100°C is 0.3-0.7 MPa.

2. The polyvinyl acetal resin film according to claim 1, wherein T [μm] and G'(100) [MPa] satisfy the following formula (1): 1.5≦T×G'(100)≦120 (1) 3. A film laminate comprising the polyvinyl acetal resin film according to claim 1 or 2, and a light-reflecting layer having a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer.

4. A film laminate having, on a first resin film consisting of the polyvinyl acetal resin film according to claim 1 or 2, a light-reflecting layer of a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including said light-reflecting layer, and a second resin film, in that order.

5. The film laminate according to claim 4, wherein the second resin film contains one or more resins selected from the group consisting of polyvinyl acetal resins, ionomer resins, ethylene-vinyl acetate copolymers, cycloolefin polymers, and polyurethanes.

6. The film laminate described in claim 5, wherein the second resin film is a polyvinyl acetal resin film containing 60 to 80 mass % of polyvinyl acetal resin and 40 to 20 mass % of plasticizer relative to 100 mass % of the second resin film.

7. A film laminate having, on the polyvinyl acetal resin film according to claim 1 or 2, a light-reflecting layer of a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer, and a hard coat layer in that order.

8. A laminate comprising the film laminate according to any one of claims 4 to 6 and a pair of light-transmitting substrates that sandwich the film laminate.

9. A laminate having, on a light-transmitting substrate, the polyvinyl acetal resin film according to claim 1 or 2, a light-reflecting layer having a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer, and a hard coat layer, in that order.

10. A glazing material comprising the laminate according to claim 8 or 9, wherein the light-transmitting substrate comprises a glass sheet or a glass laminate.

11. A head-up display device comprising a windshield or combiner comprising the glazing material of claim 10.

12. A method for producing a laminate comprising, on a light-transmitting substrate, a polyvinyl acetal resin film according to claim 1 or 2, a light-reflecting layer having a single-layer structure or a laminate structure that reflects at least a portion of light, or a light-reflecting film including the light-reflecting layer, the method comprising the steps of: (S1) obtaining a provisional laminate in which the light-transmitting substrate and the polyvinyl acetal resin film are in contact with each other without being bonded; and (S2) thermocompression bonding the provisional laminate.

13. A method for producing a laminate as described in claim 12, wherein in step (S1), the light-transmitting substrate is brought into contact with the surface of the polyvinyl acetal resin film having a ten-point average roughness (Rz) of 2 to 7 μm.

14. A method for producing a laminate according to claim 12 or 13, wherein step (S2) sequentially comprises: a step (S2-1) of heating the provisional laminate at a temperature of 90 to 110°C to obtain a pre-pressure-bonded body; and a step (S2-2) of pressurizing and heating the pre-pressure-bonded body at a temperature higher than the heating temperature of step (S2-1).

15. A method for producing a laminate described in any one of claims 12 to 14, wherein step (S1) comprises: a step (S1-1) of obtaining a film laminate including the polyvinyl acetal resin film and the light-reflecting film; and a step (S1-2) of stacking a plurality of members including the light-transmitting substrate and the film laminate to obtain the provisional laminate.

Citation Information

Patent Citations

  • Laminated film and its manufacturing method

    JP2023027939A

  • Intermediate film for laminated glasses, laminated glass, and method for manufacturing head up display system

    WO2019189741A1

  • Polyvinyl acetal resin film and film roll thereof, and layered product

    WO2020067184A1

  • Intermediate laminate, method for manufacturing same, laminate, and glazing material

    WO2020067338A1

  • Interlayer film for laminated glass, and laminated glass

    WO2021246506A1

Cited By

  • Resin sheet and method for producing same