Synthetic leather and method for producing same
By using a polyvinyl chloride resin layer with polycarbonate and silicone resin components and a thicker base fabric, the synthetic leather achieves improved flexibility and feel while maintaining abrasion resistance, addressing the limitations of conventional polyvinyl chloride-based materials.
Patent Information
- Application Number
- PCT/JP2024/019275
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-24
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional polyvinyl chloride-based synthetic leather lacks flexibility and feel while attempting to maintain abrasion resistance, as existing techniques that improve the resin layer structure, such as adding a foamed layer, do not reach the performance level of polyurethane-based synthetic leather.
Incorporating a resin layer primarily made of polyvinyl chloride resin with a main body containing polycarbonate resin or polycarbonate urethane resin, and a surface portion with polycarbonate block-containing resin and silicone resin, along with an adhesive layer and a thicker base fabric layer, to enhance flexibility and feel without compromising abrasion resistance.
The solution improves the flexibility and feel of synthetic leather while maintaining abrasion resistance, allowing for a thinner resin layer and better cushioning properties, comparable to polyurethane-based synthetic leather.
Smart Images

Figure JP2024019275_05122024_PF_FP_ABST
Abstract
Description
Synthetic leather and manufacturing method
[0001] The present invention relates to synthetic leather and a method for producing synthetic leather.
[0002] Synthetic leather is widely used for automobile seats and the like. A typical synthetic leather comprises a base fabric layer containing a fabric and a resin layer containing a resin material, with polyvinyl chloride resin and polyurethane resin being typical resin materials constituting the resin layer. While polyvinyl chloride resin offers cost advantages over polyurethane resin due to differences in raw material costs, it suffers from inferior mechanical properties such as abrasion resistance. Conventional polyvinyl chloride synthetic leathers typically compensate for their inferior mechanical properties by providing a thicker resin layer than polyurethane synthetic leathers, but it has sometimes been difficult to achieve satisfactory performance in all aspects, including mechanical properties, weight, flexibility, touch, and texture.
[0003] In view of the above issues, various techniques have been investigated for forming a foamed resin layer as part of a resin layer in polyvinyl chloride-based synthetic leather. For example, Japanese Patent Laid-Open Publication No. 2020-180191 (Patent Document 1) discloses a foamed resin layer containing a polyvinyl chloride-based resin and a thermoplastic polyurethane elastomer, and synthetic leather containing the foamed resin layer. The technology of Patent Document 1 can provide synthetic leather that is lightweight and has excellent abrasion resistance. Furthermore, Japanese Patent Laid-Open Publication No. 2017-210703 (Patent Document 2) discloses synthetic leather that includes a foamed resin layer containing a vinyl chloride resin and a plasticizer, and a resin layer containing polyurethane. The technology of Patent Document 2 can provide synthetic leather that has excellent abrasion resistance and is less likely to wrinkle.
[0004] Japanese Patent Publication No. 2020-180191 (or US Patent Application Publication No. 2020 / 0340175) Japanese Patent Publication No. 2017-210703 (or Chinese Patent Application Publication No. 107435248)
[0005] However, the techniques of Patent Documents 1 and 2 merely improve the structure of the foamed resin layer, and the improvement effects are limited. In particular, the flexibility and tactile feel of the products do not reach a level comparable to that of polyurethane synthetic leather.
[0006] Thus, there is a demand for improving the softness and feel of polyvinyl chloride synthetic leather without impairing its abrasion resistance.
[0007] The synthetic leather according to the present invention comprises a resin layer, a fabric layer containing a material, and an adhesive layer bonding the resin layer to the fabric layer, wherein the resin layer comprises a main body portion containing polyvinyl chloride resin as a primary component, and a surface portion containing at least one polycarbonate block-containing resin selected from the group consisting of polycarbonate resin and polycarbonate-based urethane resin, and a silicone resin, the main body portion being in contact with the adhesive layer on one side and with the surface portion on the other side.
[0008] The present invention provides a method for producing synthetic leather having a main body portion including a resin layer, a fabric layer containing a material, and an adhesive layer bonding the resin layer and the fabric layer, the resin layer containing a polyvinyl chloride resin as a main component, and a surface portion containing a polycarbonate block-containing resin or a silicone resin as a main component, the main body portion including a resin layer, a fabric-containing base fabric layer, and an adhesive layer bonding the resin layer and the fabric layer together, the main body portion including at least one polycarbonate block-containing resin selected from the group consisting of polycarbonate resin and polycarbonate-based urethane resin, and a silicone resin, the method comprising the steps of: forming the main body portion; forming the adhesive layer on one side of the main body portion; bonding the fabric layer to the adhesive layer; and forming the surface portion on the other side of the main body portion.
[0009] In these structures, abrasion resistance is ensured by providing a surface layer containing a polycarbonate block-containing resin and a silicone resin, instead of the foamed resin layer used in conventional polyvinyl chloride synthetic leathers, making it easier to reduce the thickness of the resin layer, thereby improving the flexibility and feel of the synthetic leather without sacrificing abrasion resistance.
[0010] Preferred embodiments of the present invention will be described below, but the scope of the present invention is not limited to the preferred embodiments described below.
[0011] In one embodiment of the synthetic leather according to the present invention, the polycarbonate block-containing resin is preferably a polycarbonate-based urethane resin.
[0012] According to this configuration, the properties of the surface portion can be easily controlled by adjusting the ratio of the polycarbonate block to the urethane block in the polycarbonate-based urethane resin.
[0013] In one embodiment of the synthetic leather according to the present invention, the fabric has a basis weight of 150 g / m 2 More than 300g / m 2 It is preferable that:
[0014] This structure uses a thicker fabric than the fabric typically used for the base fabric layer in conventional polyvinyl chloride synthetic leather, which tends to improve the feel of the synthetic leather.
[0015] In one embodiment of the synthetic leather according to the present invention, the fabric is preferably raised.
[0016] This configuration makes it easier to improve the cushioning properties of the synthetic leather.
[0017] In one embodiment, the manufacturing method according to the present invention preferably further includes a step of shaping the resin layer by adsorbing the surface portion onto the outer peripheral surface of a support having an uneven outer peripheral surface and a negative pressure inside.
[0018] According to this configuration, the texture is less likely to be visible when the resin layer is shaped, making it easier to add decoration as intended.
[0019] Further features and advantages of the present invention will become more apparent from the following description of exemplary and non-limiting embodiments, which is given with reference to the drawings.
[0020] 1 is a schematic cross-sectional view showing the structure of a synthetic leather according to an embodiment. FIG. 2 is a schematic view showing a shaping device used in a manufacturing method according to an embodiment and a method of using the same.
[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A synthetic leather and a manufacturing method thereof according to an embodiment of the present invention will be described with reference to the accompanying drawings. In the following, an example in which the synthetic leather and manufacturing method according to the present invention are applied to synthetic leather 1 and a manufacturing method thereof will be described.
[0022] [Structure of Synthetic Leather] Synthetic leather 1 according to this embodiment includes a resin layer 2, an adhesive layer 3, and a base fabric layer 4, and the resin layer 2 has a main body portion 5 and a surface portion 6 (Fig. 1). The main body portion 5 is in contact with the adhesive layer 3 on one side and with the surface portion 6 on the other side. Synthetic leather 1 is used, for example, for automobile seats, and the surface of the resin layer 2 is decorated with irregularities. Note that Fig. 1 is a schematic illustration of the layer structure of synthetic leather 1, and the thickness ratios of the various portions in Fig. 1 are not accurate. Furthermore, Fig. 1 does not show the irregularities on the surface of the resin layer 2.
[0023] Of the resin layer 2, the main body portion 5 contains polyvinyl chloride resin as its main component. Here, the term "main component" refers to the material that accounts for the largest weight ratio of the materials constituting the main body portion 5. The main body portion 5 is also generally referred to as a skin layer in the field of synthetic leather. The polyvinyl chloride resin contained in the main body portion 5 may have a degree of polymerization of 1,300 or more and 2,500 or less, for example.
[0024] Of the resin layer 2, the surface portion 6 is called a surface treatment layer and contains a polycarbonate block-containing resin and a silicone resin. The surface portion 6 is mainly composed of a polycarbonate block-containing resin or a silicone resin. Here, the term "main component" refers to the material that accounts for the largest weight ratio of the materials constituting the surface portion 6. The surface portion 6 is also generally called a surface treatment layer in the field of synthetic leather. However, the surface portion 6 may contain components other than the polycarbonate block-containing resin and the silicone resin. Non-limiting examples of such other components include a crosslinking agent and a leveling agent.
[0025] The polycarbonate block-containing resin contained in the surface portion 6 is a polymer having polycarbonate blocks in its molecule, and is not particularly limited as long as it is at least one resin selected from the group consisting of polycarbonate resins and polycarbonate-based urethane resins. For example, the surface portion 6 can be formed using a commercially available polycarbonate-based urethane resin-containing surface treatment agent sold by Stahl, Dainichiseika Color & Chemicals Mfg. Co., Ltd., Seiko Kasei Co., Ltd., etc. Similarly, commercially available surface treatment agents can be used for polycarbonate resins. The content of the polycarbonate block-containing resin in the surface portion 6 is, for example, 10 g / m 2 30g / m or more 2 The surface portion 6 may contain multiple types of polycarbonate block-containing resins, but is not limited to these. In this case, the content of the polycarbonate block-containing resin is specified as the total content of the multiple types of polycarbonate block-containing resins.
[0026] Polycarbonate-based urethane resins are polymers obtained by reacting, for example, a polyol compound containing a polycarbonate block with an isocyanate compound. The physical properties of polycarbonate-based urethane resins are determined by factors such as the number of polymerizations of the polycarbonate block, the number of isocyanate groups in the isocyanate compound, and the molecular structure. For example, the higher the number of polymerizations of the polycarbonate block, the smaller the proportion of urethane bonds in the polymer chain of the polycarbonate-based urethane resin. In this case, hydrogen bonds (involving urethane bonds) between polymer chains are less likely to form, resulting in a relatively soft polycarbonate-based urethane resin. Conversely, a low number of polymerizations of the polycarbonate block results in a relatively hard polycarbonate-based urethane resin. Furthermore, if the number of isocyanate groups in the isocyanate compound is two, the polymer chain of the polycarbonate-based urethane resin will be linear, resulting in a relatively soft polycarbonate-based urethane resin. On the other hand, if the number of isocyanate groups in the isocyanate compound is three or more, the polymer chains of the polycarbonate-based urethane resin will be network-like, resulting in a relatively hard polycarbonate-based urethane resin. In this way, the physical properties of the polycarbonate-based urethane resin can be appropriately controlled by selecting the polyol compound and the isocyanate compound. This can be used to control the physical properties of the surface portion 6.
[0027] The silicone resin contained in the surface portion 6 is not particularly limited. Therefore, commercially available silicone resin-containing surface treatment agents sold by, for example, Nissin Chemical Industry Co., Ltd., Stahl, and Seiko Chemical Co., Ltd. can be used to form the surface portion 6. The surface portion 6 (surface treatment layer) containing a polycarbonate block-containing resin and a silicone resin can be formed, for example, by applying a commercially available surface treatment agent containing a polycarbonate block-containing resin and a commercially available surface treatment agent containing a silicone resin. The surface portion 6 may contain multiple types of silicone resin. In this case, the content of the silicone resin is specified as the total content of the multiple types of silicone resin.
[0028] The silicone resin may be modified or unmodified. When the silicone resin is modified, i.e., when it is a modified silicone resin, it may be, but is not limited to, an amino-modified silicone resin, a dimethyl-modified silicone resin, a carbinol-modified silicone resin, or the like.
[0029] The composition of the surface portion 6 is not limited as long as it contains a polycarbonate block-containing resin or a silicone resin as the main component. Incidentally, "containing a polycarbonate block-containing resin or a silicone resin as the main component" includes cases in which both the polycarbonate block-containing resin and the silicone resin account for the largest weight ratios of the materials constituting the surface portion 6 (i.e., cases in which the content of the polycarbonate block-containing resin and the content of the silicone resin are equal and greater than the content of other components). For example, when the surface portion 6 contains a polycarbonate block-containing resin as the main component, the surface portion 6 may contain 1 to 15 parts by weight of silicone resin per 100 parts by weight of the polycarbonate block-containing resin.
[0030] The weight of the resin layer 2 is not particularly limited, but is, for example, 160 g / m 2 More than 300g / m 2 The surface portion 6 may have a density of, for example, 10 g / m 2 30g / m or more 2 and the main body 5 may be the remainder thereof.
[0031] The adhesive layer 3 may contain an adhesive commonly used in the field of synthetic leather. An example of such an adhesive is an adhesive containing polyvinyl chloride resin. In this case, the polyvinyl chloride resin may have a degree of polymerization of 1000 or more and 1700 or less. The weight of the adhesive layer 3 is not particularly limited, but may be, for example, 65 g / m 2 180g / m or more 2 It can be the following:
[0032] The fabric layer 4 comprises a fabric, which may be, for example, but is not limited to, a woven fabric, a single jersey, a double jersey, a tricot, a raschel, a double raschel, a nonwoven fabric, or the like.
[0033] The fabric contained in the base fabric layer 4 has a basis weight of 150 g / m 2 More than 300g / m 2 It is preferable that the weight of the fabric is 150 g / m or less. 2 When the weight of the fabric is 300 g / m or more, the feel (cushioning property, etc.) of the synthetic leather 1 tends to be good. 2 If it is equal to or less than this, the bending resistance of the synthetic leather 1 tends to be in a range suitable for use in automobile seats.
[0034] The fabric contained in the base fabric layer 4 is preferably brushed. This is preferable because it is easy to enhance the cushioning properties of the synthetic leather. The color of the fabric contained in the base fabric layer 4 is not limited, but it is preferable to use the same color or a similar color as the resin layer 2 (main body portion 5), because this makes the base fabric layer 4 less noticeable in perforations, etc.
[0035] [Method for Manufacturing Synthetic Leather] Next, a method for manufacturing the synthetic leather 1 according to this embodiment will be described. In the manufacturing method according to this embodiment, the manufacturing process of the synthetic leather 1 is carried out in three stages: a first stage, a second stage, and a third stage.
[0036] In the first stage, a first semi-finished product is produced, which is composed of the main body 5, the adhesive layer 3, and the fabric layer 4. The first semi-finished product is produced by sequentially stacking the main body 5, the adhesive layer 3, and the fabric layer 4 on top of a release paper, and finally removing the release paper.
[0037] First, a process for forming the main body portion 5 is performed. Specifically, polyvinyl chloride resin is applied to release paper fed from a release paper supply source (e.g., in roll form) and then dried, forming the main body portion 5 on the release paper. Next, a process for forming an adhesive layer 3 on one side of the main body portion 5 is performed. Specifically, an adhesive is applied to the main body portion 5 formed on the release paper. Subsequently, a process for adhering the base fabric layer 4 to the adhesive layer 3 is performed. Specifically, the base fabric layer 4 is bonded to the main body portion 5 formed on the release paper and the adhesive layer 3. Through these processes, a first semi-finished product with release paper is obtained. Finally, the release paper is peeled from the main body portion 5 of the first semi-finished product, and the release paper and the first semi-finished product are separately collected. There are no particular restrictions on how the release paper and the first semi-finished product are collected, but considering ease of use in the next process, it is preferable that they be collected in a rolled form.
[0038] In the second stage, the body portion 5 of the first semi-finished product is surface-treated to form the surface portion 6, thereby producing a second semi-finished product consisting of the resin layer 2 (surface portion 6 and body portion 5), adhesive layer 3, and fabric layer 4. That is, a step of forming a surface portion on the other side of the body portion 5 is carried out. Specifically, a surface treatment agent containing a polycarbonate block-containing resin and a silicone resin is applied to the first semi-finished product delivered from a supply source of the first semi-finished product (for example, in a roll form), and the applied surface treatment agent is dried to form the surface portion 6 on the body portion 5.
[0039] In the third stage, a concave-convex pattern is formed on the resin layer 2 of the second semi-finished product to decorate it. That is, a process of shaping the resin layer 2 is carried out. The shaping device 10 used in this process includes a heater 11 that heats the second semi-finished product 20, a ceramic roll 12 (an example of a support), and a pressure reducing device (not shown) that creates a negative pressure inside the roll 12 (FIG. 2). Note that FIG. 2 is a schematic diagram of the configuration of the shaping device 10, and the dimensional proportions of the various parts are not accurate.
[0040] The roll 12 is made of ceramic and has voids through which air can pass, so that negative pressure draws air from the outside to the inside of the roll 12. On the outer peripheral surface of the roll 12, irregularities 13 corresponding to the pattern to be transferred to the resin layer 2 are formed.
[0041] The second semi-finished product 20 is heated by the heater 11 and then introduced into the roll 12. This heating is intended to soften the vinyl chloride resin of the resin layer 2 to make it easier to shape. In the roll 12, the resin layer 2 of the second semi-finished product 20 is adsorbed onto the outer peripheral surface of the roll 12 using negative pressure from a pressure reducing device as a driving force. At this time, the irregularities 13 on the outer peripheral surface of the roll 12 are transferred to the resin layer 2, and the resin layer 2 is shaped.
[0042] By using negative pressure as a driving force to shape the resin layer 2, the texture of the fabric layer 4 is less likely to be visible on the surface of the resin layer 2, making it easier to achieve the intended decoration. The problem of the texture of the fabric layer 4 being visible on the surface of the resin layer 2 is more likely to occur when the resin layer 2 is thin (i.e., when the resin layer 2 is light in weight). On the other hand, if the contact force between the roll and the resin layer 2 is reduced to avoid the problem of the texture of the fabric layer 4 being visible on the surface of the resin layer 2, the intended decoration may not be achieved. Therefore, when the resin layer 2 is thin, it is difficult to determine the shaping conditions that prevent the texture of the fabric layer 4 from being visible and allow for sufficient decoration. Using a method using negative pressure as a driving force to shape the resin layer 2 makes it easier to both avoid the texture being visible and achieve sufficient decoration, compared to using a method in which synthetic leather 1 is pressed against a roll. Therefore, when the weight of the resin layer 2 is relatively small, using negative pressure as a driving force to shape the resin layer 2 is particularly advantageous compared to using a method in which synthetic leather 1 is pressed against a roll. In the synthetic leather 1 according to this embodiment, the weight of the resin layer 2 is 160 g / m 2 More than 300g / m 2 However, the preferred range of this basis weight is smaller than the weight of a typical resin layer in conventional polyvinyl chloride synthetic leather. In other words, since the weight of the resin layer 2 in the preferred embodiment of the synthetic leather 1 according to the present embodiment is smaller than the weight of the resin layer in conventional polyvinyl chloride synthetic leather, it is advantageous to shape the resin layer 2 using a method that uses negative pressure as a driving force.
[0043] [Other Embodiments] Finally, other embodiments of the synthetic leather and manufacturing method according to the present invention will be described. Note that the configurations disclosed in the following embodiments can be applied in combination with the configurations disclosed in other embodiments, as long as no contradiction occurs.
[0044] In the above embodiment, synthetic leather 1 including resin layer 2, adhesive layer 3, and fabric layer 4 has been described as an example. However, in the synthetic leather according to the present invention, the presence of other layers is not excluded as long as the resin layer and fabric layer are bonded together by the adhesive layer. Similarly, the presence of other portions is not excluded as long as the resin layer has a main portion including polyvinyl chloride resin and a surface portion including polycarbonate block-containing resin and silicone resin.
[0045] In the above embodiment, a configuration in which the resin layer 2 is shaped using a ceramic roll 12 has been described as an example. However, in the manufacturing method according to the present invention, the step of shaping the resin layer may or may not be included. Furthermore, the method of shaping the resin layer is not limited to the above configuration. For example, a method in which a main body portion is formed on embossed release paper and the unevenness of the release paper is transferred to the main body portion, or a method in which the main body portion is pressed against a roll formed of a material other than ceramic (such as iron) and the unevenness of the roll is transferred can be employed. Note that if the unevenness of the release paper is transferred to the main body portion, the third step of the manufacturing method according to the above embodiment can be omitted.
[0046] Among these methods, when using a roll (regardless of material), a desired pattern can be formed on the resin layer 2 by installing a roll having concaves and convexes corresponding to the desired pattern in equipment available to the user. In contrast, when using release paper, unless the release paper is manufactured in equipment available to the user, the patterns that can be formed on the resin layer 2 are limited to a range of commercially available release papers. Since it is not common for manufacturers of synthetic leather 1 to manufacture release paper, using a roll offers the advantage of greater freedom in shaping and easier design changes than using release paper. Therefore, shaping the resin layer 2 using a method using negative pressure as a driving force is particularly advantageous in that it allows for both the addition of the intended decoration and the freedom of decoration in a preferred embodiment of the synthetic leather 1 according to this embodiment.
[0047] Regarding other configurations, it should be understood that the embodiments disclosed in this specification are illustrative in all respects and that the scope of the present invention is not limited thereby. Those skilled in the art will easily understand that appropriate modifications are possible without departing from the spirit of the present invention. Therefore, other embodiments modified without departing from the spirit of the present invention are naturally included in the scope of the present invention.
[0048] The present invention will be further described below with reference to examples, but the present invention is not limited to these examples.
[0049] [Production of Test Pieces] The method of producing the synthetic resins of the Examples and Comparative Examples will be described below. Unless otherwise specified, the method follows the above embodiment.
[0050] (Example 1) The resin layer is made of polyvinyl chloride resin and has a basis weight of 300 g / m 2 The base fabric layer was made of a double jersey fabric with a basis weight of 250 g / m 2The surface portion was formed using a surface treatment agent containing 100 parts by mass of a polycarbonate-based urethane resin, 9 parts by mass of a first silicone resin, and 3 parts by mass of a second silicone resin (referred to as "PC, Si" in Table 1). The first silicone resin was a dimethyl-modified silicone resin, and the second silicone resin was an amino-modified silicone resin, which also applies to the following examples and comparative examples. The fabric of the base fabric layer was a black, unbrushed material. The resin layer was shaped by adsorption onto a ceramic roll (referred to as "adsorption" in Table 1).
[0051] (Example 2) The resin layer was made of polyvinyl chloride resin and had a basis weight of 300 g / m 2 The base fabric layer was made of a single jersey fabric with a basis weight of 150 g / m 2 The surface portion was formed using a surface treatment agent containing 100 parts by mass of a polycarbonate-based urethane resin, 9 parts by mass of a first silicone resin, and 3 parts by mass of a second silicone resin. The base fabric layer was made of a white, unbrushed material. The resin layer was shaped by transferring the unevenness of the release paper to the main body portion (referred to as "release paper" in Table 1).
[0052] (Example 3) The resin layer was made of polyvinyl chloride resin and had a basis weight of 300 g / m 2 The base fabric layer was made of a single jersey fabric with a basis weight of 150 g / m 2 The surface was formed using a surface treatment agent containing 100 parts by mass of a polycarbonate-based urethane resin, 9 parts by mass of a first silicone resin, and 3 parts by mass of a second silicone resin. The base fabric layer was made of a white, unbrushed fabric. The resin layer was shaped using a method in which the irregularities of an iron roll were transferred to the main body (referred to as "iron" in Table 1), and the pressing force when pressing the synthetic leather against the iron roll was adjusted to a range in which the texture of the base fabric layer did not appear on the surface of the resin layer.
[0053] (Example 4) The resin layer is made of polyvinyl chloride resin and has a basis weight of 300 g / m 2 The base fabric layer was made of a double jersey fabric with a basis weight of 300 g / m 2The surface portion was formed using a surface treatment agent containing 100 parts by mass of a polycarbonate-based urethane resin, 9 parts by mass of a first silicone resin, and 3 parts by mass of a second silicone resin. The fabric of the base fabric layer was a black, brushed fabric. The resin layer was shaped by adsorption onto a ceramic roll.
[0054] (Example 5) The resin layer was made of polyvinyl chloride resin and had a basis weight of 300 g / m 2 The base fabric layer was a single-woven fabric with a basis weight of 200 g / m 2 The surface portion was formed using a surface treatment agent containing 100 parts by mass of a polycarbonate-based urethane resin, 9 parts by mass of a first silicone resin, and 3 parts by mass of a second silicone resin. The fabric of the base fabric layer was a white, brushed fabric. The resin layer was shaped by adsorption onto a ceramic roll.
[0055] (Comparative Example 1) This is an example of conventional polyvinyl chloride synthetic leather. The resin layer is made of polyvinyl chloride resin, and the basis weight is 600 g / m. 2 The base fabric layer was a single-woven fabric with a basis weight of 150 g / m 2 The resin layer was configured to have a surface layer, a main body, and an intermediate layer made of foamed polyvinyl chloride resin, and the intermediate layer was configured to be in contact with the adhesive layer. The surface was formed using a surface treatment agent containing polyurethane resin (referred to as "PU" in Table 1). The fabric of the base fabric layer was unbrushed white. The resin layer was shaped by transferring the unevenness of the release paper to the main body.
[0056] (Comparative Example 2) A synthetic leather according to Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that the resin layer was shaped by transferring the irregularities of an iron roll to the main body. The pressing force used to press the synthetic leather against the iron roll was adjusted within a range such that the texture of the base fabric layer did not appear on the surface of the resin layer.
[0057] (Comparative Example 3) This is an example of conventional polyvinyl chloride synthetic leather without an intermediate layer. The resin layer is made of polyvinyl chloride resin and has a basis weight of 300 g / m. 2 The base fabric layer was a single-woven fabric with a basis weight of 150 g / m 2The surface was formed using a surface treatment agent containing polyurethane resin. The base fabric layer was made of white, unbrushed fabric. The resin layer was formed by adsorbing it onto a ceramic roll.
[0058] (Comparative Example 4) This is an example in which the surface treatment method for a conventional polyvinyl chloride synthetic leather was changed. The resin layer was made of polyvinyl chloride resin, and the basis weight was 600 g / m. 2 The base fabric layer was a single-woven fabric with a basis weight of 150 g / m 2 The surface portion was formed using a surface treatment agent containing 100 parts by mass of a polycarbonate-based urethane resin, 9 parts by mass of a first silicone resin, and 3 parts by mass of a second silicone resin. The fabric of the base fabric layer was unbrushed white. The resin layer was shaped by adsorption onto a ceramic roll.
[0059] (Comparative Example 5) This is an example of conventional polyurethane synthetic leather. The resin layer is made of polyurethane resin, and the basis weight is 150 g / m. 2 The base fabric layer was made of a double jersey fabric with a basis weight of 300 g / m 2 The surface was formed using a surface treatment agent containing polyurethane resin. The base fabric layer was made of a black, brushed fabric. The resin layer was shaped by transferring the unevenness of the release paper to the main body.
[0060] (Comparative Example 6) This is an example of conventional polyurethane synthetic leather. The resin layer is made of polyurethane resin, and the basis weight is 100 g / m. 2 The base fabric layer was made of tricot fabric with a basis weight of 200 g / m 2 The surface was formed using a surface treatment agent containing polyurethane resin. The base fabric layer was a black, unbrushed fabric. The resin layer was shaped by transferring the unevenness of the release paper to the main body.
[0061] [Evaluation of Test Pieces] (Bending Hardness Test) A bending hardness test was conducted by sensory evaluation for each of the Examples and Comparative Examples. A 22 cm × 17 cm test piece was prepared for each Example, placed on a desk with the surface portion 6 facing up, and the tester's hand was placed on top of it. With the thumb spread and the other four fingers closed, the tester removed the palm from the test piece while keeping the fingertips in contact with the test piece, and then gripped the test piece. The bending hardness of the test piece was evaluated based on the resistance felt in the palm and fingers. Comparative Example 6 (conventional polyurethane-based synthetic leather) was used as the standard for the highest rating of "A" and Comparative Example 2 (conventional polyvinyl chloride-based synthetic leather) was used as the standard for the lowest rating of "E," and the tester subjectively selected the bending hardness of the test piece from five levels, A to E.
[0062] (Slipperiness Test) A slipperiness test was conducted by sensory evaluation for each of the Examples and Comparative Examples. A 22 cm × 17 cm test piece was prepared for each Example, placed on a platform balance with the surface portion 6 facing up, and the tester's index, middle, and ring fingertips (beyond the first joint) were brought into contact with the test piece. The tester pressed the test piece with three fingers, maintaining a reading of 300 g on the platform balance, while moving the fingertips back and forth. The slipperiness of the test piece was evaluated based on the resistance felt at the fingertips. Comparative Example 6 (conventional polyurethane-based synthetic leather) was used as the standard for the highest rating of "A," and Comparative Example 2 (conventional polyvinyl chloride-based synthetic leather) was used as the standard for the lowest rating of "E." The tester then subjectively selected the slipperiness of the test piece from five levels, A to E.
[0063] (Indentation Test) A sensory evaluation of indentation test was conducted for each of the Examples and Comparative Examples. A 22 cm x 17 cm test piece was prepared for each Example, placed on a desk with the surface 6 facing up, and the tester pressed the test piece with his or her index finger. The indentation test of the test piece was evaluated based on the rebound sensation felt at the fingertip. Comparative Example 5 (a conventional polyurethane-based synthetic leather with a raised base fabric layer 4) was used as the standard for the highest rating of "A," and Comparative Example 1 (a conventional polyvinyl chloride-based synthetic leather) was used as the standard for the lowest rating of "E." The indentation test of the test piece was subjectively selected from five levels, A to E, by the tester.
[0064] (Visual Test) Each example of the Examples and Comparative Examples was visually observed to confirm the state of the pattern on the surface. The state of the pattern in each example was evaluated on the following two levels of A or E. A: The pattern can be seen even when observed from a distance of 30 cm or more from the test piece. E: The pattern can be seen only when approaching within 30 cm of the test piece.
[0065] (Bending resistance test) For each of the examples and comparative examples, a bending test was carried out based on JIS L 1096:2020 (Bending resistance test method A (45° cantilever method)). The numerical values of the test results for each example are shown in Table 1.
[0066] (Wear Resistance Test) For each of the Examples and Comparative Examples, an abrasion resistance test was conducted in accordance with JASO M403-88 (friction strength method B). However, the load was changed to 3 kgf. The number of abrasion cycles until damage was observed on the surface of the test specimen was recorded as the test result for each example. For test specimens that showed no damage after 28,000 abrasion cycles, the test was terminated at that point. The numerical test results for each example are shown in Table 1.
[0067] (KES Test) For each of the Examples and Comparative Examples, a bending hardness test and a bending recovery test were carried out using KES-FB2-A. The test results for each example are shown in Table 1.
[0068] [Results] The evaluation results for each example of the Examples and Comparative Examples are shown in Table 1. As shown in Table 1, synthetic leathers obtained in Examples 1 to 5 had higher abrasion resistance and were superior in flexibility and tactile feel compared to Comparative Examples 1 and 2, which were conventional polyvinyl chloride-based synthetic leathers. In terms of abrasion resistance and slipperiness, Examples 1 to 5 were comparable to Comparative Examples 5 and 6, which were polyurethane-based synthetic leathers. Furthermore, Examples 4 and 5, which used brushed fabric, exhibited pressability comparable to Comparative Examples 5 and 6.
[0069] Table 1: Examples and Comparative Examples
[0070] The present invention can be used, for example, in car seats.
[0071] REFERENCE SIGNS LIST 1: Synthetic leather 2: Resin layer 3: Adhesive layer 4: Fabric layer 5: Main body 6: Surface 10: Shaping device 11: Heater 12: Roll 13: Concave / convex 20: Second semi-finished product
Claims
1. A synthetic leather comprising a resin layer, a fabric layer including a material, and an adhesive layer bonding the resin layer and the fabric layer, wherein the resin layer has a main body portion including polyvinyl chloride resin as a main component, and a surface portion including at least one polycarbonate block-containing resin selected from the group consisting of polycarbonate resin and polycarbonate-based urethane resin, and a silicone resin, the main body portion being in contact with the adhesive layer on one side and in contact with the surface portion on the other side.
2. The synthetic leather according to claim 1, wherein the polycarbonate block-containing resin is a polycarbonate-based urethane resin.
3. The fabric has a basis weight of 150 g / m 2 More than 300g / m 2 2. The synthetic leather according to claim 1, wherein:
4. The synthetic leather according to any one of claims 1 to 3, wherein the fabric is brushed.
5. A method for producing synthetic leather comprising: a resin layer, a fabric layer containing a material, and an adhesive layer bonding the resin layer and the fabric layer, wherein the resin layer comprises a main body portion containing polyvinyl chloride resin as a main component, and at least one polycarbonate block-containing resin selected from the group consisting of polycarbonate resin and polycarbonate-based urethane resin, and a silicone resin, and a surface portion containing polycarbonate block-containing resin or silicone resin as a main component, the method comprising the steps of: forming the main body portion; forming the adhesive layer on one side of the main body portion; bonding the fabric layer to the adhesive layer; and forming the surface portion on the other side of the main body portion.
6. The manufacturing method according to claim 5, further comprising a step of adsorbing said surface portion onto the outer peripheral surface of a support having an uneven outer peripheral surface and a negative pressure on the inside, thereby shaping said resin layer.
Citation Information
Patent Citations
JP1974010532A
JP1974036804A
Vacuum molding of laminated sheet
JP1996127060A
Synthetic resin leather and method for producing the same
JP2011214191A
Flexible decorative laminate, and production method of flexible decorative laminate
JP2017061051A
Cited By
Synthetic leather and manufacturing method
JP2025177717A
Synthetic leather and manufacturing method
JP7663276B1