Polymer and photosensitive resin composition containing same, copper paste, liquid composition, method for manufacturing semiconductor device, and method for manufacturing copper pillar for semiconductor connection
The method addresses the complexity of semiconductor device manufacturing by using a photosensitive resin composition, copper paste with specific molar ratios, and a coordinating liquid to reduce steps and temperature for copper pillar bonding, improving semiconductor device reliability and efficiency.
Patent Information
- Application Number
- PCT/JP2024/019805
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-30
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional semiconductor device manufacturing methods require numerous steps for miniaturization and increased connection terminals, necessitating high temperature and high pressure for copper pillar bonding, which can lead to thermal stress and bonding defects due to material warping and coefficient differences.
A method involving a photosensitive resin composition, a copper paste with specific molar ratios of basic and acidic groups, and a liquid composition with a coordinating organic compound to reduce the number of manufacturing steps, lower bonding temperatures, and improve filling properties, allowing for copper pillar formation and bonding at reduced temperatures.
This approach reduces the number of manufacturing steps, lowers the bonding temperature for copper pillars, and enhances filling properties, minimizing thermal stress and defects in semiconductor devices.
Smart Images

Figure JP2024019805_05122024_PF_FP_ABST
Abstract
Description
Polymer and photosensitive resin composition containing same, copper paste, liquid composition, method for manufacturing semiconductor device, and method for manufacturing copper pillar for semiconductor connection
[0001] The present embodiment relates to a polymer, a photosensitive resin composition containing the polymer, a copper paste, a liquid composition, a method for manufacturing a semiconductor device, and a method for manufacturing a copper pillar for connecting a semiconductor.
[0002] With the advent of a post-5G and 6G society, there is a rapidly increasing demand for advanced semiconductor technology that can transmit huge amounts of information at high speeds and with low latency in all hardware, from communications infrastructure to edge devices such as smartphones and tablets. Achieving this demand requires miniaturization and an increase in connection terminals as semiconductors become more highly integrated. In the manufacturing process, not only is miniaturization processing in the front-end process important, but packaging technology that integrates multiple semiconductors in three dimensions in the back-end process is also becoming increasingly important. Bonding copper pillars to connect semiconductor chips has traditionally required strict process conditions of high temperature and pressure. Further advances in copper-to-copper direct bonding technology are required to achieve further miniaturization.
[0003] Japanese Patent Application Laid-Open No. 2021-197430
[0004] (1) Conventionally, the manufacture of semiconductor devices has required many steps due to the miniaturization and increased number of connection terminals associated with the high integration of semiconductors. The first object of the present disclosure is to provide a method for manufacturing a semiconductor device that allows for a reduction in the number of steps compared to conventional methods. (2) In the connection between semiconductor chips, a narrower pitch for metal pillars is required to increase density. At the same time, a resist resin that allows for patterning at a narrower pitch is also required. The second object of the present disclosure is to provide a polymer (A) that allows for patterning at a narrower pitch, and a photosensitive resin composition containing the polymer (A). (3) Conventionally, methods that involve patterning with a resist resin and forming pillars by copper plating have required many steps for pillar formation. Furthermore, copper-to-copper bonding between pillars formed by copper plating has required process conditions of high temperature (300 to 400°C) and high pressure. The third object of the present disclosure is to provide a copper paste that allows for a reduction in the number of steps for copper pillar formation and a lower bonding temperature compared to conventional methods. Furthermore, the present disclosure is to provide a copper paste that has excellent filling properties even when the resist openings formed on the semiconductor chip are narrow. (4) Conventionally, as described above, copper-to-copper bonding between pillars formed by copper plating required process conditions of high temperature of 300 to 400°C and high pressure. High bonding temperatures could lead to cracks or poor bonding due to the effects of thermal stress caused by warping of the substrate or differences in the linear expansion coefficients of different materials. A fourth object of the present disclosure is to provide a liquid composition that can lower the bonding temperature compared to conventional methods.
[0005] As a result of intensive research, the present inventors have found that the first problem can be solved by a method for manufacturing a semiconductor device, the method comprising: (1) a step of preparing a structure, the step including: forming a resin layer on a substrate or a semiconductor chip using a resin composition; and patterning the resin layer to form a patterned resin layer having openings; and a step of bonding two or more of the structures using the patterned resin layer. (2) The second problem can be solved by a polymer (A) for producing a resin composition in the method for manufacturing a semiconductor device, the polymer (A) comprising the following monomer units (A1) and (A2). (3) A method for manufacturing a semiconductor device, the method comprising: copper particles; and a dispersion medium containing a basic compound and a reducing organic substance, wherein the molar ratio of the basic group contained in the basic compound to the acidic group contained in the reducing organic substance (basic group / acidic group) is 0.5 to 1.2, and the dispersion medium is resistant to oxidation at 25°C and a shear rate of 10 s as measured with a rheometer. -1 (4) It has been found that the third problem can be solved by a copper paste for manufacturing copper pillars for connecting semiconductors, which has a viscosity of 0.1 to 200 Pa·s at 200°C. (5) It has been found that the fourth problem can be solved by a liquid composition for assisting the joining of pillars for connecting semiconductors, which contains a reducing organic substance, a basic compound, and a coordinating organic compound excluding compounds contained in the basic compound, and the coordinating organic compound has a higher boiling point than the reducing organic substance.
[0006] 9 shows an electron microscope photograph of the solvent-treated copper foil surface of Example 16. FIG. 9 shows an electron microscope photograph of the solvent-treated copper foil surface of Example 17. FIG. 9 shows an electron microscope photograph of the solvent-treated copper foil surface of Comparative Example 9. FIG. 9 shows an electron microscope photograph of the arrangement pattern of the copper bumped Si chip used in Example 29. FIG. 9 shows an electron microscope photograph of the copper bump portion surface of the copper bumped Si chip used in Example 29. FIG. 9 shows an electron microscope photograph of the copper bump portion surface of the solvent-treated Si chip of Example 29. FIG. 9 shows a cross-sectional SEM photograph of the bonded body of Example 30. FIG. 9 shows an enlarged photograph of FIG. 7. FIG. 9 shows a cross-sectional SEM photograph of the bonded body of Example 31.
[0007] This embodiment has the following aspects. <First Embodiment> [1] A method for manufacturing a semiconductor device, comprising: a step of preparing structures, the step including: forming a resin layer on a substrate or a semiconductor chip using a resin composition; and patterning the resin layer to form a patterned resin layer having openings; and a step of bonding two or more of the structures using the patterned resin layer. [2] The method for manufacturing a semiconductor device according to [1], wherein the resin composition is a photosensitive resin composition, and the patterning is performed by exposure to light and development. [3] The method for manufacturing a semiconductor device according to [1] or [2], wherein the pitch between adjacent openings is 80 μm or less. [4] The method for manufacturing a semiconductor device according to any of [1] to [3], wherein the opening width of the openings is less than 40 μm. [5] The method for manufacturing a semiconductor device according to any of [1] to [4], wherein the preparation step includes forming metal pillars in the openings. [6] The method for manufacturing a semiconductor device according to [5], wherein forming the metal pillar comprises filling the opening with a copper paste, the copper paste comprising copper particles and a dispersion medium containing a basic compound and a reducing organic substance, and wherein a molar ratio of a basic group contained in the basic compound to an acidic group contained in the reducing organic substance (basic group / acidic group) is 0.5 to 1.2. [7] The method for manufacturing a semiconductor device according to [5] or [6], further comprising planarizing the surfaces on which the patterns of the metal pillar and the patterning resin layer are present prior to the bonding step. [8] The method for manufacturing a semiconductor device according to [7], wherein the planarization is performed by CMP. [9] The method for manufacturing a semiconductor device according to any one of [5] to [8], wherein the bonding step comprises overlapping two or more of the structures with the metal pillars of the respective structures and bonding them at a temperature of 200°C to 250°C.
[10] The method for manufacturing a semiconductor device according to any one of [5] to [9], wherein the bonding step comprises overlapping two or more of the structures with metal pillars of the respective structures and bonding them at a temperature of less than 200° C.
[11] The method for manufacturing a semiconductor device according to any one of [5] to
[10] , wherein the method comprises applying a liquid composition to the joints of the metal pillars before the bonding step.
[12] The method for manufacturing a semiconductor device according to
[11] , wherein the liquid composition contains a reducing organic substance, a basic compound, and a coordinating organic compound excluding compounds contained in the basic compound, and the coordinating organic compound has a higher boiling point than the reducing organic substance.
[13] The method for manufacturing a semiconductor device according to any one of [1] to
[12] , wherein the resin layer is formed using a polymer (A) containing the following monomer units (A1) and (A2): Monomer unit (A1): a monomer containing an alkali-soluble group, Monomer unit (A2): an aromatic (meth)acrylic acid ester having a phenolic hydroxyl group.
[0008] <Second embodiment>
[14] A polymer (A) for producing the resin composition in the method for producing a semiconductor device, particularly in the method for producing a semiconductor device according to any one of [1] to
[12] , comprising the following monomer units (A1) and (A2): Monomer unit (A1): A monomer containing an alkali-soluble group Monomer unit (A2): An aromatic (meth)acrylic acid ester having a phenolic hydroxyl group
[15] The polymer (A) according to
[14] , further comprising: Monomer unit (A3): An N-substituted maleimide compound;
[16] The polymer (A) according to
[14] or
[15] , further comprising: Monomer unit (A4): A (meth)acrylic acid alkyl ester in which the alkyl group has two or more carbon atoms;
[17] The polymer (A) according to any one of
[14] to
[16] , wherein the proportion of the monomer unit (A1) relative to the total amount (100 mol%) of all monomer units constituting the polymer (A) is 5 to 50 mol%.
[0009] <Third embodiment>
[18] A photosensitive resin composition for a semiconductor device manufacturing method, particularly for the semiconductor device manufacturing method according to any one of [1] to
[12] , the photosensitive resin composition comprising: a polymer (A) containing the following monomer units (A1) and (A2): monomer unit (A1): a monomer containing an alkali-soluble group; monomer unit (A2): an aromatic (meth)acrylic acid ester having a phenolic hydroxyl group; and a solvent (C).
[0010] <Fourth embodiment>
[19] A dispersion medium comprising copper particles and a dispersion medium containing a basic compound and a reducing organic substance, wherein the molar ratio of the basic group contained in the basic compound to the acidic group contained in the reducing organic substance (basic group / acidic group) is 0.5 to 1.2, and the dispersion medium has a viscosity of 25°C at a shear rate of 10 s measured with a rheometer. -1
[20] A copper paste for producing a copper pillar for connecting a semiconductor, wherein the viscosity at 0.1 to 200 Pa·s is 0.1 to 200 Pa·s, wherein the basic compound is a compound represented by the following formula (1): [In formula (1), R a ~R c are the same or different and represent a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and represent at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c cannot be a hydrogen atom at the same time. A double line including a dashed line represents a single bond or a double bond, and if it is a double bond, there is no R. a ~R c
[21] The copper paste according to
[19] or
[20] , wherein the reducing organic compound is at least one organic compound selected from the group consisting of formic acid and oxalic acid.
[22] The copper paste according to [21 ... -1
[23] The copper paste according to any one of
[19] to
[22] , wherein the viscosity at 100°C is 0.1 Pa·s or more and less than 100 Pa·s.
[24] The copper paste according to any one of
[19] to
[23] , wherein the maximum peak temperature in differential thermogravimetric analysis (DTG) at a heating rate of 10°C / min under a nitrogen atmosphere is 100 to 220°C.
[25] The copper paste according to any one of
[19] to
[24] , wherein the volume average particle diameter of the copper particles is 1 nm or more and 500 nm or less.
[26] The copper paste according to any one of
[19] to
[25] , wherein the content of the copper particles in the copper paste is 50 to 85 mass%.
[27] The copper paste according to any one of
[19] to
[26] , wherein the content of the reducing organic substance in the copper paste is 6.0 to 22.0 wt% and the content of the basic compound in the copper paste is 3.0 to 35.0 wt%.
[27] The content of the basic compound is 3.0 to 35.0 wt %, and the weight ratio of the basic compound to the reducing organic substance (basic compound / reducing organic substance) is 0.4 to 5.0.
[19] The copper paste according to any one of
[26] to
[26] .
[0011] <Fifth Embodiment>
[28] A method for manufacturing a semiconductor device, comprising: forming a resin layer on a substrate or a semiconductor chip using a resin composition; patterning the resin layer to form a patterned resin layer having openings; and filling the openings with a copper paste, particularly the copper paste described in any one of
[19] to
[27] , to form copper pillars.
[29] A method for manufacturing a semiconductor device according to
[28] , further comprising bonding the copper pillars to each other after removing the patterned resin layer.
[30] A method for manufacturing a semiconductor device according to
[28] , further comprising bonding the patterned resin layers to each other without removing the patterned resin layer, and metal-bonding the copper pillars to each other.
[31] Use of a copper paste for manufacturing a copper pillar for connecting a semiconductor, comprising: copper particles; and a dispersion medium containing a basic compound and a reducing organic substance, wherein the molar ratio of basic groups contained in the basic compound to acidic groups contained in the reducing organic substance (basic groups / acidic groups) is 0.5 to 1.2.
[0012] <Sixth embodiment>
[32] A liquid composition for assisting bonding of semiconductor connecting pillars, comprising a reducing organic substance, a basic compound, and a coordinating organic compound excluding compounds contained in the basic compound, wherein the coordinating organic compound has a higher boiling point than the reducing organic substance.
[33] The liquid composition according to
[32] , wherein the coordinating organic compound is a compound having a carboxyl group.
[34] The liquid composition according to
[32] or
[33] , wherein the reducing organic substance is at least one organic substance selected from formic acid and oxalic acid.
[35] The liquid composition according to any one of
[32] to
[34] , further comprising a reducing organic substance other than formic acid.
[36] The basic compound is a compound represented by the following formula (1): [In formula (1), R a ~R c are the same or different and represent a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and represent at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c are not simultaneously hydrogen atoms. A double line including a dashed line represents a single bond or a double bond. When it is a double bond, R c does not exist. a ~R c
[37] The liquid composition according to any one of
[32] to
[36] , wherein the basic compound has an ethylenediamine structure or an ethanolamine structure in its molecular structure, and the amino group in the ethylenediamine structure or the ethanolamine structure is a tertiary amino group.
[38] The liquid composition according to any one of
[32] to
[37] , wherein the ratio of the total number of moles of basic groups contained in the basic compound to the total number of moles of acidic groups contained in the reducing organic substance (basic groups / acidic groups) is 0.4 to 2.5.
[39] The liquid composition according to any one of
[32] to
[38] , further comprising a solvent.
[0013] Seventh Embodiment
[40] A method for manufacturing a semiconductor device, comprising applying a liquid composition, particularly the liquid composition according to any one of
[32] to
[39] , to a joining portion before joining semiconductor connecting pillars together.
[41] Use of a liquid composition for assisting joining of semiconductor connecting pillars together, the liquid composition comprising a reducing organic substance, a basic compound, and a coordinating organic compound excluding compounds contained in the basic compound, wherein the coordinating organic compound has a higher boiling point than the reducing organic substance.
[0014] Eighth Embodiment
[42] A method for manufacturing a semiconductor device, comprising: a first step of applying a photosensitive resin composition onto a substrate or a semiconductor chip; a second step of patterning the photosensitive resin composition by photolithography to form copper pillars with a maximum spacing width of 80 μm or less; a third step of filling openings formed by the patterning with copper paste and drying the paste to form copper pillars; a fourth step of planarizing a surface having the copper pillars and the patterning without peeling off the photosensitive resin composition; a step of preparing a set of structures obtained through the first to fourth steps; a fifth step of applying a liquid composition to the planarized surface of at least one of the set of structures; a sixth step of stacking the set of structures so that the copper pillars are in contact with each other; and a seventh step of heating the set of structures at 200° C. or less in an inert atmosphere.
[43] The method for producing a semiconductor device according to
[42] , wherein the photosensitive resin composition comprises a polymer (A) containing the following monomer units (A1) and (A2): monomer unit (A1): a monomer containing an alkali-soluble group; monomer unit (A2): an aromatic (meth)acrylic acid ester having a phenolic hydroxyl group; a photopolymerization initiator (B); and a solvent (C).
[44] The method for producing a semiconductor device according to
[42] or
[43] , wherein the copper paste is the copper paste according to any one of
[19] to
[27] .
[45] The method for producing a semiconductor device according to
[42] , wherein the liquid composition is the liquid composition according to any one of
[32] to
[39] .
[0015] <Ninth embodiment>
[46] A method for manufacturing a semiconductor device, comprising: a first step of applying a thermosetting resin onto a substrate or a semiconductor chip on which metal pillars are formed at a pitch with a maximum spacing of 80 μm or less, a second step of planarizing a surface having the metal pillars and the thermosetting resin, and a step of preparing a set of structures obtained through the first and second steps, a third step of applying a liquid composition to the planarized metal pillar surface of at least one of the set of structures, a fourth step of stacking the set of structures so that the metal pillars are in contact with each other, and a fifth step of heating the set of structures at 200° C. or less in an inert atmosphere.
[47] The method for manufacturing a semiconductor device according to
[46] , wherein the liquid composition is the liquid composition according to any of
[32] to
[39] .
[0016] Tenth Embodiment
[48] A semiconductor device including a semiconductor bonded by a copper pillar and a resin, wherein the copper pillar is present in an opening in the resin, and the interval between the openings is 80 μm or less.
[0017] According to the first embodiment, it is possible to provide a method for manufacturing a semiconductor device that can reduce the number of manufacturing steps for the semiconductor device compared to the conventional method.
[0018] According to the second or third embodiment, it is possible to provide a method for manufacturing a semiconductor device that allows patterning at a narrower pitch, a polymer (A), and a photosensitive resin composition containing the polymer (A).
[0019] According to the fourth or fifth embodiment, the number of steps for forming a copper pillar can be reduced compared to conventional methods. Furthermore, a copper paste for manufacturing a semiconductor connecting pillar and a method for manufacturing a semiconductor device that can lower the bonding temperature can be provided. Furthermore, according to the fourth embodiment, a copper paste that has excellent filling properties even when the resist opening formed on the semiconductor chip is narrow can be provided.
[0020] According to the sixth or seventh embodiment, it is possible to provide a liquid composition and a method for manufacturing a semiconductor device that can further reduce the bonding temperature compared to conventional methods.
[0021] According to the eighth, ninth, and tenth embodiments, it is possible to provide a method for manufacturing a semiconductor device that can reduce the number of manufacturing steps compared to conventional methods and further lower the bonding temperature between structures having metal pillars compared to conventional methods.
[0022] One embodiment of the present invention will be described in detail below. This embodiment is not limited to the following embodiment and can be implemented with appropriate modifications as long as the effects of this embodiment are not impaired. The configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible as appropriate within the scope of the present embodiment. This embodiment is not limited by the embodiment, but is limited only by the claims. Each aspect disclosed in this specification can be combined with any other feature disclosed in this specification. If a specific description of one embodiment also applies to other embodiments, that description may be omitted in other embodiments. In this embodiment, the expression "X to Y" for a numerical range means "X or more and Y or less." Furthermore, when multiple upper and lower limits are specified for a specific parameter, any of these upper and lower limits can be combined to form a suitable numerical range. Furthermore, the lower and / or upper limits of a numerical range described in this disclosure are numerical values within that numerical range and may be replaced with numerical values shown in the examples.
[0023] [Definitions] In this specification, the terms in parentheses below are defined as follows. "Structure" refers to a structure comprising a patterned resin layer having openings on a substrate or semiconductor chip, and metal pillars may be formed in the openings. "Patterned resin layer" refers to a resin layer that has been patterned. The patterned resin layer typically has multiple openings. "Bonding" is a term that encompasses adhesion and bonding. For example, it may include connecting the surfaces of two or more structures comprising a patterned resin layer having openings on a substrate or semiconductor chip, and bonding them by applying heat or pressure. Furthermore, when metal pillars are formed in the openings, it may also include bonding the metal pillars in the openings of two or more structures by applying heat or pressure through metal diffusion. "Opening pitch (spacing)" refers to the distance between the centers of adjacent openings formed in the patterned resin layer. Here, it is the arithmetic average value measured at 10 locations. "Opening width" refers to the longest width of each opening formed in the patterned resin layer. When the shape of the opening is (approximately) circular, it is also referred to as the opening diameter, and the opening diameter refers to the diameter of the opening. Here, it is the arithmetic average of the measurements for 10 openings. "Metal pillar" refers to a columnar (pillar) electrode formed on a substrate or semiconductor chip, whose cross section does not have to be point-symmetric or line-symmetric. "Planarization" refers to the process of flattening the surface on which the metal pillar and patterned resin layer patterns are located. "Permanent resist" refers to a resin formed on a substrate or semiconductor chip that remains without being removed until the finished semiconductor device is produced. "(Meth)acrylate" refers to acrylate and methacrylate.
[0024] [First embodiment: semiconductor device manufacturing method] A first embodiment of the present disclosure relates to a semiconductor device manufacturing method including: a structure preparation step including: forming a resin layer on a substrate or a semiconductor chip using a resin composition; and patterning the resin layer to form a patterned resin layer having openings; and a step of bonding two or more of the structures using the patterned resin layer. The first embodiment makes it possible to reduce the number of manufacturing steps for semiconductor devices compared to conventional methods.
[0025] <Method for manufacturing a semiconductor device> The method for manufacturing a semiconductor device according to this embodiment includes: a step of preparing a structure, the step including forming a resin layer on a substrate or a semiconductor chip using a resin composition, and patterning the resin layer to form a patterned resin layer having openings; and a step of bonding two or more of the structures using the patterned resin layer.
[0026] In one embodiment, the substrate is preferably selected from the group consisting of, for example, a ceramic substrate, a green sheet, an organic substrate, a glass substrate, and a circuit-formed substrate. In one embodiment, the organic substrate is preferably made of, for example, glass epoxy, epoxy resin, phenolic resin, cycloolefin polymer (COP), polyimide, liquid crystal polymer (LCP), polystyrene, modified polyphenylene ether, fluorine-based resin, etc. In one embodiment, the semiconductor chip is preferably selected from the group consisting of, for example, a silicon chip, a compound semiconductor chip, and a semiconductor package chip.
[0027] Examples of the resin composition include a resist resin composition containing a photocurable resin and a resin composition containing a thermosetting resin, and the resin composition may contain one or more selected from these. Examples of the photocurable resin include a photocurable acrylic resin, a photocurable urethane resin, and a photocurable epoxy resin. These may be used alone or in combination of two or more. Examples of the thermosetting resin include an epoxy resin, an acrylic resin, a melamine resin, a maleimide resin, a polyurethane resin, a diallyl phthalate resin, and a silicone resin. These may be used alone or in combination of two or more. In one embodiment, the resin composition preferably contains the polymer (A) described in the second embodiment below from the viewpoint of lowering the bonding temperature. When the polymer (A) is contained, the bonding temperature of the structure can be lowered (e.g., 200°C or lower). In another embodiment, the resin composition may contain the thermosetting resin described in the ninth embodiment below. As a method for forming a pattern having openings on a substrate or a semiconductor chip using the resin composition, it is preferable to form an etching mask by patterning using photolithography. More specifically, the process of forming the etching mask involves applying a resin composition onto a semiconductor chip, drying the resulting coating, exposing the coating through a specified mask (and, if necessary, baking after exposure) to form a latent image pattern, and then developing the coating, thereby forming an etching mask having a highly accurate fine pattern.
[0028] In one embodiment, when forming a pattern having two or more openings on a substrate or a semiconductor chip, the pitch (spacing) between adjacent openings is preferably 80 μm or less, more preferably 40 μm or less, even more preferably 20 μm or less, and particularly preferably 10 μm or less. In one embodiment, when forming a pattern having two or more openings on a substrate or a semiconductor chip, the lower limit of the pitch (spacing) between adjacent openings is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 5 μm or more, and particularly preferably 10 μm. In one embodiment, when a pattern having two or more openings is formed on a substrate or a semiconductor chip, the pitch (spacing) between adjacent openings is preferably one pitch (spacing) selected from the group consisting of 0.1 μm to 80 μm, 1 μm to 80 μm, 5 μm to 80 μm, 10 μm to 80 μm, 0.1 μm to 40 μm, 1 μm to 40 μm, 5 μm to 40 μm, 10 μm to 40 μm, 0.1 μm to 20 μm, 1 μm to 20 μm, 5 μm to 20 μm, 10 μm to 20 μm, 0.1 μm to 10 μm, 1 μm to 10 μm, and 5 μm to 10 μm.
[0029] In one embodiment, the opening width of the opening is preferably less than 40 μm, more preferably 20 μm, and even more preferably 10 μm. The shape of the opening in a plan view is not limited, and examples thereof include a circle, an ellipse, a rectangle, a square, a rectangular, and an irregular shape.
[0030] The photosensitive resin composition can be applied using a conventional coating means such as a spin coater, a dip coater, a roller coater, etc. The thickness of the coating is, for example, 0.1 to 30 μm, preferably 0.3 to 15 μm.
[0031] For exposure, light rays of various wavelengths (for example, ultraviolet rays, X-rays, etc.) can be used. The exposure energy is, for example, 1 to 1000 mJ / cm. 2 is.
[0032] The exposure causes the photopolymerization initiator (B) and the polymer (A) to react with each other to generate alkali-soluble groups (e.g., hydroxyl groups, carboxy groups, etc.). Therefore, when the coating film after exposure is developed with an alkaline developer, the exposed areas of the coating film dissolve in the alkaline developer, while the unexposed areas remain undissolved, thereby forming an etching mask having a predetermined pattern.
[0033] The semiconductor chip is then etched using the etching mask obtained in the above step, and the etching mask is removed after etching to obtain a semiconductor chip on which a wiring pattern is formed. In one embodiment, the method does not necessarily require removing the etching mask. That is, the etching mask formed from the resin composition may be used as a permanent resist. Not removing the etching mask makes it possible to reduce the number of manufacturing steps for a semiconductor device. Furthermore, adjusting the film thickness of the permanent resist is preferable because it also enables patterning at a high aspect ratio.
[0034] In one embodiment, the step of preparing the structure preferably includes forming a metal pillar in the opening. In one embodiment, forming the metal pillar preferably includes filling the opening with a copper paste, and the copper paste preferably includes copper particles and a dispersion medium containing a basic compound and a reducing organic substance, and the molar ratio of the basic group contained in the basic compound to the acidic group contained in the reducing organic substance (basic group / acidic group) is preferably 0.5 to 1.2. By forming the metal pillar including filling the opening with the copper paste, the pillar can be formed more easily. When the copper paste thus contains copper particles and a dispersion medium containing a basic compound and a reducing organic substance and satisfies a predetermined molar ratio (basic group / acidic group), the temperature during bonding of the structure can be lowered (e.g., 200°C or lower).
[0035] In one embodiment, it is preferable to further include planarizing the surfaces on which the patterns of the metal pillar and the patterned resin layer are present prior to the bonding step. By including the planarization, the bonding strength between the bonding surfaces can be further improved, distortion can be reduced inside the semiconductor device, and the possibility of short circuits can be reduced. In one embodiment, the planarization can be performed by a physical polishing method such as a surface planer or a chemical polishing method using chemicals such as etching, but is preferably performed by CMP (Chemical Mechanical Polishing).
[0036] In one embodiment, the bonding step preferably includes bonding two or more of the structures by overlapping the metal pillars of each of the structures (i.e., overlapping the patterned resin layers so that the patterned resin layers are bonded to each other and the metal pillars are bonded to each other) at a temperature of 200°C or higher and 250°C or lower, and more preferably includes bonding at a temperature of less than 200°C.
[0037] In one embodiment, it is preferable to include applying a liquid composition to the joining portion of the metal pillars before the joining step. By including applying a liquid composition to the joining portion of the metal pillars, the joining temperature can be lowered (for example, 200°C or lower). In one embodiment, the liquid composition includes a reducing organic substance, a basic compound, and a coordinating organic compound excluding compounds included in the basic compound, and the coordinating organic compound has a higher boiling point than the reducing organic substance. By using the above liquid composition, the joining temperature can be further lowered.
[0038] [Second embodiment: Polymer (A)] This relates to a polymer (A) for producing the resin composition in a semiconductor device manufacturing method, particularly in the above-described semiconductor device manufacturing method, the polymer (A) comprising the following monomer units (A1) and (A2). Monomer unit (A1): Monomer containing an alkali-soluble group Monomer unit (A2): Aromatic (meth)acrylic acid ester having a phenolic hydroxyl group. The polymer (A) according to the second embodiment can be patterned at a narrower pitch.
[0039] <Monomer Unit (A1)> The polymer (A) according to the first embodiment contains a monomer unit (A1). The monomer unit (A1) is a monomer unit derived from a monomer containing an alkali-soluble group. The monomer unit (A1) has the function of imparting alkali solubility to the polymer (A). By including the monomer unit (A1), the polymer (A) according to the first embodiment can be dissolved in an aqueous alkaline solution (developer) during development. Furthermore, the monomer unit (A1) hardens the polymer (A) during exposure by crosslinking with a crosslinking agent or by reacting with the monomer units (A2) to (A4) present in the polymer (A) molecule, thereby imparting the hardness required for a resist to the resulting film and rendering the polymer (A) alkali-insoluble. In one embodiment, the polymer (A) may be used, in particular, for a negative photoresist.
[0040] The monomer unit (A1) can be introduced into the polymer (A) by copolymerizing a polymerizable unsaturated compound (a1) having an alkali-soluble group with other monomers. The alkali-soluble group may be any group commonly used in the resist field, such as a carboxy group or a phenolic hydroxyl group. Representative examples of the polymerizable unsaturated compound (a1) having an alkali-soluble group include, but are not limited to, unsaturated carboxylic acids or their acid anhydrides, hydroxystyrene or its derivatives, etc. Among these, unsaturated carboxylic acids or their acid anhydrides are particularly preferred.
[0041] Examples of unsaturated carboxylic acids or acid anhydrides thereof include α,β-unsaturated carboxylic acids such as acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, and fumaric acid, and acid anhydrides thereof (maleic anhydride, itaconic anhydride, etc.). Among these, acrylic acid and / or methacrylic acid are particularly preferred. The polymerizable unsaturated compound (a1) having an alkali-soluble group may be used alone or in combination of two or more.
[0042] In one embodiment, the proportion of the monomer unit (A1) relative to the total amount (100 mol%) of all monomer units constituting the polymer (A) is preferably 5 to 50 mol%, more preferably 5 to 40 mol%, and even more preferably 5 to 30 mol%. When the proportion of the monomer unit (A1) is within the above range, the developability is likely to be good and the etching resistance after development is likely to be good.
[0043] <Monomer Unit (A2)> The polymer (A) according to the first embodiment contains a monomer unit (A2). The monomer unit (A2) is a monomer unit derived from an aromatic (meth)acrylic acid ester having a phenolic hydroxyl group. When the polymer (A) according to the first embodiment contains the monomer unit (A2), a pattern with a narrower pitch can be formed. Examples of aromatic (meth)acrylic acid esters having a phenolic hydroxyl group include hydroxyphenyl (meth)acrylate, and p-hydroxyphenyl methacrylate and / or p-hydroxyphenyl acrylate are preferred.
[0044] In one embodiment, the proportion of the monomer units (A2) relative to the total amount (100 mol%) of all monomer units constituting the polymer (A) is preferably 5 to 50 mol%, more preferably 5 to 40 mol%, and even more preferably 5 to 30 mol%. When the proportion of the monomer units (A2) is within the above range, it is easy to stably form a narrow-pitch pattern.
[0045] <Monomer Unit (A3)> The polymer (A) according to the first embodiment preferably further contains a monomer unit (A3). The monomer unit (A3) is a monomer unit derived from an N-substituted maleimide compound. When the polymer (A) according to the second embodiment contains the monomer unit (A3), good heat resistance can be achieved. Examples of the N-substituted maleimide compound include compounds represented by the following formula (1): (In formula (1), R 1 represents an organic group.)
[0046] Examples of the organic group include hydrocarbon groups and heterocyclic groups. Examples of the hydrocarbon group include alkyl groups (e.g., C1-6 alkyl groups) such as methyl, ethyl, propyl, isopropyl, butyl, and hexyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, cyclooctyl, adamantyl, and norbornyl; aryl groups such as phenyl; aralkyl groups such as benzyl; and groups in which two or more of these are bonded together. Examples of the heterocyclic group include 5- to 10-membered heterocycloalkyl and heteroaryl groups containing at least one heteroatom selected from the group consisting of nitrogen, oxygen, and sulfur atoms.
[0047] As the N-substituted maleimide compound, one or more compounds represented by the above formula (1) can be used. Examples include N-alkylmaleimides such as N-methylmaleimide, N-ethylmaleimide, and N-propylmaleimide; N-cycloalkylmaleimides such as N-cyclopentylmaleimide, N-cyclohexylmaleimide, N-cyclooctylmaleimide, N-adamantylmaleimide, and N-norbornylmaleimide; N-arylmaleimides such as N-phenylmaleimide; and N-aralkylmaleimides such as N-benzylmaleimide. The N-substituted maleimide compound may be used alone or in combination of two or more. Among these, N-methylmaleimide, N-phenylmaleimide, and N-cyclohexylmaleimide are preferred, and N-cyclomaleimide is more preferred.
[0048] In one embodiment, the proportion of the monomer unit (A3) relative to the total amount (100 mol%) of all monomer units constituting the polymer (A) is preferably 5 to 60 mol%, more preferably 10 to 50 mol%, and even more preferably 15 to 45 mol%. When the proportion of the monomer unit (A3) is within the above range, good heat resistance is easily achieved.
[0049] <Monomer Unit (A4)> The polymer (A) according to the first embodiment preferably contains a monomer unit (A4). The monomer unit (A4) is a monomer unit derived from a (meth)acrylic acid alkyl ester having an alkyl group with two or more carbon atoms. When the polymer (A) according to the first embodiment contains the monomer unit (A4), good flexibility can be achieved. Examples of the (meth)acrylic acid alkyl ester having an alkyl group with two or more carbon atoms include alkyl (meth)acrylates having an alkyl group with two or more to twelve carbon atoms, such as ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, and hexyl (meth)acrylate. Of these, it is preferable to contain ethyl or ethylhexyl butyl (meth)acrylate, and it is particularly preferable to contain butyl acrylate.
[0050] In one embodiment, the proportion of the monomer unit (A4) relative to the total amount (100 mol%) of all monomer units constituting the polymer (A) is preferably 5 to 60 mol%, more preferably 10 to 50 mol%, and even more preferably 15 to 45 mol%. When the proportion of the monomer unit (A4) is within the above range, good flexibility is easily achieved.
[0051] <Other Monomer Units> In one embodiment, the polymer (A) may contain other monomer units in addition to the aforementioned monomer units (A1) to (A4). Examples of other monomer units include units derived from a monomer having a phenolic hydroxyl group and a polymerizable unsaturated group other than the monomer unit (A2), units derived from a (meth)acrylic acid ester compound other than the monomer unit (A4), units derived from a monomer having a hydroxyalkyl group and a polymerizable unsaturated group, units derived from an acrylamide compound, acrylonitrile units, units derived from a styrene compound, and units derived from a vinyl compound. The polymer (A) may contain one or more of these other monomer units. Specific examples of monomers that can constitute the other monomer units are described below, but are not limited to these.
[0052] Examples of monomers having a phenolic hydroxyl group and a polymerizable unsaturated group other than the monomer unit (A2) include p-hydroxystyrene, α-methyl-p-hydroxystyrene, N-hydroxyphenylmaleimide, N-hydroxyphenylacrylamide, N-hydroxyphenylmethacrylamide, etc. These may be used alone or in combination of two or more.
[0053] Examples of the (meth)acrylic acid ester compound other than the monomer unit (A4) include methyl (meth)acrylate, benzyl (meth)acrylate, naphthyl (meth)acrylate, anthryl (meth)acrylate, anthrylmethyl (meth)acrylate, phenyl (meth)acrylate, glycidyl (meth)acrylate, phenoxyethyi (meth)acrylate, 2,2,2-trifluoroethyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, 2-methoxyethyl (meth)acrylate, and methoxytriethylene glycol (meth)acrylate. , 2-ethoxyethyl (meth)acrylate, 2-aminoethyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-methyl-2-adamantyl (meth)acrylate, 2-propyl-2-adamantyl (meth)acrylate, 8-ethyl-8-tricyclodecyl (meth)acrylate, 8-methyl-8-tricyclodecyl (meth)acrylate, diethylene glycol mono(meth)acrylate, caprolactone-2-(acryloyloxy)ethyl ester, polyethylene glycol ethyl ether (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0054] Examples of monomers having a hydroxyalkyl group and a polymerizable unsaturated group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2,3-dihydroxypropyl (meth)acrylate, glycerin mono(meth)acrylate, 5-acryloyloxy-6-hydroxynorbornene-2-carboxylic-6-lactone, etc. These may be used alone or in combination of two or more.
[0055] Examples of the acrylamide compound include N-methylacrylamide, N-methylmethacrylamide, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N-methoxymethylacrylamide, N-methoxymethylmethacrylamide, N-butoxymethylacrylamide, N-butoxymethylmethacrylamide, etc. These may be used alone or in combination of two or more.
[0056] Examples of the styrene compound include styrenes having no hydroxy group, such as styrene, α-methylstyrene, chlorostyrene, bromostyrene, etc. These may be used alone or in combination of two or more.
[0057] Examples of vinyl compounds include methyl vinyl ether, benzyl vinyl ether, cyclohexyl vinyl ether, vinyl naphthalene, vinyl anthracene, vinyl carbazole, allyl glycidyl ether, 3-ethenyl-7-oxabicyclo[4.1.0]heptane, 1,2-epoxy-5-hexene, and 1,7-octadiene monoepoxide. These may be used alone or in combination of two or more.
[0058] In one embodiment, when the polymer (A) contains one or more other monomer units, the amount of such other monomer units is preferably 40 mol % or less relative to the total amount (100 mol %) of all monomer units constituting the polymer (A).
[0059] In one embodiment, the weight average molecular weight (Mw) of the polymer (A) is not particularly limited, but is preferably, for example, 2,000 to 300,000, more preferably 3,000 to 100,000, and even more preferably 5,000 to 50,000. The molecular weight distribution (ratio of weight average molecular weight to number average molecular weight: Mw / Mn) of the polymer (A) is not particularly limited, but is preferably, for example, 5.0 or less, more preferably 1.2 to 4.5, and even more preferably 1.5 to 4.0. In the present disclosure, the weight average molecular weight (Mw) and number average molecular weight (Mn) can be measured by GPC using polystyrene as a standard substance.
[0060] <Method for producing polymer (A)> The polymer (A) according to the second embodiment can be produced by blending the monomers constituting the above-described monomer units (A1) and (A2) and, if necessary, one or more monomers constituting other monomer units, and copolymerizing them.
[0061] The polymer (A) according to the second embodiment may be copolymerized in the presence of a polymerization initiator. Examples of the polymerization initiator include conventional or known radical polymerization initiators, such as azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), dimethyl-2,2'-azobis(2-methylpropionate), diethyl-2,2'-azobis(2-methylpropionate), and dibutyl-2,2'-azobis(2-methylpropionate); organic peroxides such as benzoyl peroxide, lauroyl peroxide, t-butyl peroxypivalate, and 1,1-bis(t-butylperoxy)cyclohexane; and hydrogen peroxide. When a peroxide is used as the radical polymerization initiator, it may be combined with a reducing agent to form a redox initiator. Of these, azo compounds are preferred, with 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile) and dimethyl-2,2'-azobis(2-methylpropionate) being more preferred.
[0062] The amount of the polymerization initiator used is not particularly limited and can be appropriately selected within a range that does not impair smooth copolymerization. For example, the amount is preferably 1 to 20 parts by weight, more preferably 3 to 15 parts by weight, relative to the total amount (100 parts by weight) of the monomers.
[0063] The polymer (A) according to the second embodiment can be produced by a conventional method used in producing an acrylic polymer or a styrene polymer, such as solution polymerization, bulk polymerization, suspension polymerization, bulk-suspension polymerization, or emulsion polymerization. The above-mentioned monomers and polymerization initiator may be supplied to the reaction system all at once, or a part or all of them may be added dropwise to the reaction system. For example, a method in which a solution of a polymerization initiator dissolved in a polymerization solvent is added dropwise to each monomer or a mixture of a monomer and a polymerization solvent maintained at a constant temperature to polymerize the monomers, or a method in which a solution of a single monomer and a polymerization initiator dissolved in a polymerization solvent is added dropwise to a polymerization solvent maintained at a constant temperature to polymerize the monomers (drop polymerization method), can be used.
[0064] In one embodiment, the polymer (A) is preferably copolymerized in a polymerization solvent. The polymerization solvent can be appropriately selected depending on the monomer composition and the like, and examples thereof include ethers (diethyl ether; chain ethers such as glycol ethers such as ethylene glycol mono- or dialkyl ethers, diethylene glycol mono- or dialkyl ethers, propylene glycol mono- or dialkyl ethers, propylene glycol mono- or diaryl ethers, dipropylene glycol mono- or dialkyl ethers, tripropylene glycol mono- or dialkyl ethers, 1,3-propanediol mono- or dialkyl ethers, 1,3-butanediol mono- or dialkyl ethers, 1,4-butanediol mono- or dialkyl ethers, and glycerin mono-, di-, or tri-alkyl ethers; cyclic ethers such as tetrahydrofuran and dioxane), esters (carboxylic acid esters such as methyl acetate, ethyl acetate, butyl acetate, isoamyl acetate, ethyl lactate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, C5-6 cycloalkanediol mono- or diacetate, and C5-6 cycloalkanedimethanol mono- or diacetate);Ethylene glycol monoalkyl ether acetate, ethylene glycol mono- or diacetate, diethylene glycol monoalkyl ether acetate, diethylene glycol mono- or diacetate, propylene glycol monoalkyl ether acetate, propylene glycol mono- or diacetate, dipropylene glycol monoalkyl ether acetate, dipropylene glycol mono- or diacetate, 1,3-propanediol monoalkyl ether acetate, 1,3-propanediol mono- or diacetate, 1,3-butanediol monoalkyl ether acetate, 1,3-butanediol mono- or diacetate, 1,4-butanediol monoalkyl ether acetate, 1,4-butanediol mono- or diacetate, glycerin mono-, di- or triacetate, glycerin mono- or di-C1 Examples of suitable polymerization solvents include glycol acetates or glycol ether acetates such as propylene glycol mono- or di-acetate, propylene glycol monoalkyl ether acetate, and tripropylene glycol mono- or diacetate; ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, 3,5,5-trimethyl-2-cyclohexene-1-one, and the like); amides (N,N-dimethylacetamide, N,N-dimethylformamide, and the like); sulfoxides (dimethyl sulfoxide, and the like); alcohols (methanol, ethanol, propanol, C5-6 cycloalkanediol, C5-6 cycloalkanedimethanol, and the like); hydrocarbons (aromatic hydrocarbons such as benzene, toluene, xylene, and the like; aliphatic hydrocarbons such as hexane, and alicyclic hydrocarbons such as cyclohexane, and the like); and mixed solvents thereof. While any of these polymerization solvents can be used, in one embodiment, the polymerization solvent is preferably an ester, and more preferably a propylene glycol monoalkyl ether acetate.
[0065] The polymerization temperature can be appropriately selected depending on the type and composition of the monomers, and is not particularly limited, but is preferably, for example, 30 to 150°C.
[0066] The reaction solution containing the polymer (A) obtained by the above method can be purified by precipitation or reprecipitation, if necessary. The solvent used for precipitation or reprecipitation may be either an organic solvent or water, or a mixture thereof. Examples of organic solvents include hydrocarbons (aliphatic hydrocarbons such as pentane, hexane, heptane, and octane; alicyclic hydrocarbons such as cyclohexane and methylcyclohexane; aromatic hydrocarbons such as benzene, toluene, and xylene), halogenated hydrocarbons (halogenated aliphatic hydrocarbons such as methylene chloride, chloroform, and carbon tetrachloride; halogenated aromatic hydrocarbons such as chlorobenzene and dichlorobenzene), nitro compounds (nitromethane and nitroethane), nitriles (acetonitrile and benzonitrile), ethers (chain ethers such as diethyl ether, diisopropyl ether, and dimethoxyethane; cyclic ethers such as tetrahydrofuran and dioxane), ketones (acetone, methyl ethyl ketone, and diisobutyl ketone), esters (ethyl acetate and butyl acetate), carbonates (dimethyl carbonate, diethyl carbonate, ethylene carbonate, and propylene carbonate), alcohols (methanol, ethanol, propanol, isopropyl alcohol, and butanol), carboxylic acids (acetic acid), and mixed solvents containing these solvents.
[0067] [Third embodiment: photosensitive resin composition] A third embodiment of this embodiment relates to a photosensitive resin composition containing the polymer (A) according to the second embodiment, a photopolymerization initiator (B), and a solvent (C). The photosensitive resin composition according to the second embodiment is a resin composition containing the polymer (A) according to the second embodiment as an essential component. According to the third embodiment, patterning at a narrower pitch is possible. Furthermore, since the photosensitive resin composition according to the third embodiment can also be used as a permanent resist, bonding between metal pillars at a narrower pitch can be performed with fewer steps than conventional methods.
[0068] <Photopolymerization initiator (B)> The photosensitive resin composition according to the third embodiment contains a photopolymerization initiator (B) as a curing catalyst. Examples of the photopolymerization initiator (B) include alkylphenone-based photoradical generators, acylphosphine oxide-based photoradical generators, oxime ester-based photoradical generators, and α-hydroxyketone-based photoradical generators.
[0069] Examples of alkylphenone-based photoradical generators include 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, benzophenone, methylbenzophenone, o-benzoylbenzoic acid, benzoyl ethyl ether, 2,2-diethoxyacetophenone, 2,4 -diethylthioxanthone, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, ethyl-(2,4,6-trimethylbenzoyl)phenylphosphinate, 4,4'-bis(diethylamino)benzophenone, 1-hydroxycyclohexyl phenyl ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, and oligomers of 2-hydroxy-1-(4-isopropenylphenyl)-2-methylpropan-1-one. These may be used alone or in combination of two or more.
[0070] Examples of the acylphosphine oxide photoradical generator include diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, ethyl-(2,4,6-trimethylbenzoyl)phenylphosphinate, etc. These may be used alone or in combination of two or more.
[0071] Examples of oxime ester-based photoradical generators include 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(O-benzoyloxime), 1-[6-(2-methylbenzoyl)-9-ethyl-9H-carbazol-3-yl]ethanone O-acetyloxime, 6-[1-(acetyloxyimino)ethyl]-9-ethyl-9H-carbazol-3-yl(2-methylphenyl)ketone, etc. These may be used alone or in combination of two or more.
[0072] Examples of α-hydroxyketone-based photoradical generators include benzoin, benzoin methyl ether, benzoin butyl ether, 1-hydroxycyclohexyl phenyl ketone, 1-phenyl-2-hydroxy-2-methylpropan-1-one, 1-(4-i-propylphenyl)-2-hydroxy-2-methylpropan-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 1-hydroxycyclohexyl phenyl ketone, etc. These may be used alone or in combination of two or more.
[0073] In one embodiment, the proportion of the photopolymerization initiator (B) is preferably 1.0 to 10.0 parts by mass, more preferably 2.0 to 8.0 parts by mass, and even more preferably 2.5 to 6.0 parts by mass, relative to 100 parts by mass of the polymer component including the polymer (A). When the proportion of the photopolymerization initiator (B) is within the above range, poor curing is unlikely to occur.
[0074] <Solvent (C)> The photosensitive resin composition according to the third embodiment contains a solvent (C). Examples of the solvent (C) include ethers (chain ethers such as diethyl ether; ethylene glycol mono- or di-alkyl ethers, diethylene glycol mono- or di-alkyl ethers, propylene glycol mono- or di-alkyl ethers, propylene glycol mono- or diaryl ethers, dipropylene glycol mono- or di-alkyl ethers, tripropylene glycol mono- or di-alkyl ethers, 1,3-propanediol mono- or di-alkyl ethers, 1,3-butanediol mono- or di-alkyl ethers, 1,4-butanediol mono- or di-alkyl ethers, and glycol ethers such as glycerin mono-, di-, or tri-alkyl ethers; and cyclic ethers such as tetrahydrofuran and dioxane), esters (carboxylic acid esters such as methyl acetate, ethyl acetate, butyl acetate, isoamyl acetate, ethyl lactate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, C5-6 cycloalkanediol mono- or di-acetate, and C5-6 cycloalkanedimethanol mono- or di-acetate),Ethylene glycol monoalkyl ether acetate, ethylene glycol mono- or diacetate, diethylene glycol monoalkyl ether acetate, diethylene glycol mono- or diacetate, propylene glycol monoalkyl ether acetate, propylene glycol mono- or diacetate, dipropylene glycol monoalkyl ether acetate, dipropylene glycol mono- or diacetate, 1,3-propanediol monoalkyl ether acetate, 1,3-propanediol mono- or diacetate, 1,3-butanediol monoalkyl ether acetate, 1,3-butanediol mono- or diacetate Glycol acetates or glycol ether acetates such as acetate, 1,4-butanediol monoalkyl ether acetate, 1,4-butanediol mono- or diacetate, glycerin mono-, di-, or triacetate, glycerin mono- or di-C1-4 alkyl ether di- or monoacetate, tripropylene glycol monoalkyl ether acetate, tripropylene glycol mono- or diacetate, etc.), ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, 3,5,5-trimethyl-2-cyclohexene-1-one, etc.), or mixed solvents thereof can be used;
[0075] <Other Polymers> The photosensitive resin composition according to the third embodiment may contain a polymer component (other polymer) other than the polymer (A). Examples of the other polymers include a polyfunctional vinyl compound, a polyfunctional thiol compound, and a polyfunctional epoxy compound.
[0076] The polyfunctional vinyl compound is not particularly limited as long as it is a compound having two or more vinyl groups, and examples thereof include di(meth)acrylates of alkylene glycols such as ethylene glycol and propylene glycol; di(meth)acrylates of polyalkylene glycols such as polyethylene glycol and polypropylene glycol; di(meth)acrylates of polymers hydroxylated at both ends such as both-terminally hydroxylated polybutadiene, both-terminally hydroxylated polyisoprene, and both-terminally hydroxylated polycaprylactone; glycerin, 1,2,4-butanetriol, trimethylol; Examples of the polyfunctional vinyl compound include poly(meth)acrylates of trivalent or higher polyhydric alcohols such as methylalkane, tetramethylolalkane, pentaerythritol, and dipentaerythritol; poly(meth)acrylates of polyalkylene glycol adducts of trivalent or higher polyhydric alcohols; poly(meth)acrylates of cyclic polyols such as 1,4-cyclohexanediol and 1,4-benzenediol; and oligo(meth)acrylates such as polyester(meth)acrylate, epoxy(meth)acrylate, urethane(meth)acrylate, and silicone resin(meth)acrylate. The polyfunctional vinyl compound may be used alone or in combination of two or more.
[0077] The polyfunctional thiol compound is not particularly limited as long as it is a compound having two or more thiol groups, and examples thereof include hexanedithiol, decanedithiol, 1,4-butanediol bisthiopropionate, 1,4-butanediol bisthioglycolate, ethylene glycol bisthioglycolate, ethylene glycol bisthiopropionate, trimethylolpropane tristhioglycolate, trimethylolpropane tristhiopropionate, trimethylolpropane tris(3-mercaptobutyrate), pentaerythritol tetrakisthioglycolate, pentaerythritol tetrakisthiopropionate, trimercaptopropionic acid tris(2-hydroxyethyl)isocyanurate, and 1,4-dimethylmercaptobenzene. , 2,4,6-trimercapto-s-triazine, 2-(N,N-dibutylamino)-4,6-dimercapto-s-triazine, tetraethylene glycol bis-3-mercaptopropionate, trimethylolpropane tris-3-mercaptopropionate, tris(3-mercaptopropynyloxyethyl)isocyanurate, pentaerythritol tetrakis-3-mercaptopropionate, dipentaerythritol tetrakis-3-mercaptopropionate, 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, pentaerythritol tetrakis(3-mercaptobutyrate), etc. The polyfunctional thiol compounds may be used alone or in combination of two or more.
[0078] The polyfunctional epoxy compound is not particularly limited as long as it is a compound having two or more epoxy groups, and examples thereof include glycidyl ether type epoxy compounds [glycidyl ethers produced by reacting polyhydroxy compounds (bisphenols, polyhydric phenols, alicyclic polyhydric alcohols, aliphatic polyhydric alcohols, etc.) with epichlorohydrin (for example, (poly)C2-4 alkylene glycol diglycidyl ethers such as ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, etc.; diglycidyl ethers of polyhydric phenols such as resorcinol and hydroquinone; diglycidyl ethers of alicyclic polyhydric alcohols such as cyclohexanediol, cyclohexanedimethanol, and hydrogenated bisphenols; bisphenols (bis(hydroxyphenyl)alkanes such as 4,4'-dihydroxybiphenyl and bisphenol A, etc.)], or diglycidyl ethers of their C2-3 alkylene oxide adducts), novolac epoxy resins (phenol novolac or cresol novolac epoxy resins, etc.)], glycidyl ester epoxy compounds, alicyclic epoxy compounds (or cycloaliphatic epoxy resins), heterocyclic epoxy resins (triglyceridyl isocyanurate (TGIC), hydantoin epoxy resins, etc.), glycidylamine epoxy compounds [reaction products of amines and epichlorohydrin, for example, N-glycidyl aromatic amines {tetraglycidyldiaminodiphenylmethane (TGDDM), triglycidylaminophenol (TGPAP, TGMAP, etc.), diglycidylaniline (DGA), diglycidyltoluidine (DGT), tetraglycidylxylylenediamine (TGMXA, etc.), etc.}, N-glycidyl alicyclic amines (tetraglycidylbisaminocyclohexane, etc.)]. The polyfunctional epoxy compounds may be used alone or in combination of two or more.
[0079] <Other Components> The photosensitive resin composition according to the third embodiment may contain components other than the above-described components. Examples of the other components include one or more of a resin such as a novolac resin, a phenolic resin, an imide resin, or a carboxyl group-containing resin, a radical polymerization initiator, a curing agent, a curing accelerator, or an additive (such as a filler, an antifoaming agent, a flame retardant, an antioxidant, an ultraviolet absorber, a colorant, a stress reducer, a flexibility imparting agent, a wax, a resin, a crosslinking agent, a halogen trapping agent, a leveling agent, or a wetting improver).
[0080] In the photosensitive resin composition according to the third embodiment, the content of polymer (A) is not particularly limited, but is preferably, for example, 3 to 50% by mass relative to the total mass of the photosensitive resin composition. The weight ratio of the total amount (100% by mass) of the curable components contained in the photosensitive resin composition to polymer (A) is also not particularly limited, but is preferably, for example, 5:1 to 1:10, more preferably 3:1 to 1:8, even more preferably 2:1 to 1:5, and particularly preferably 1:1 to 1:3.
[0081] <Applications> The photosensitive resin composition according to the third embodiment contains the polymer (A) according to the second embodiment, and can be patterned at a narrower pitch. Therefore, the photosensitive resin composition according to the third embodiment can be suitably used for semiconductor devices, particularly as a resin composition for resists of semiconductor devices.
[0082] [Fourth Embodiment: Copper Paste] A fourth embodiment of the present disclosure relates to a copper paste for manufacturing a copper pillar for connecting a semiconductor, comprising: copper particles; and a dispersion medium containing a basic compound and a reducing organic substance, wherein the molar ratio of the basic group contained in the basic compound to the acidic group contained in the reducing organic substance (basic group / acidic group) is 0.5 to 1.2. According to the fourth embodiment, the number of steps for forming the copper pillar can be reduced compared to conventional methods. Furthermore, a copper paste for manufacturing a copper pillar for connecting a semiconductor can be provided, which allows for a lower bonding temperature.
[0083] In the fourth embodiment, the term "copper pillar for semiconductor connection" refers to a columnar (pillar) copper electrode formed on a substrate or semiconductor chip, the cross section of which does not have to be point-symmetric or line-symmetric.
[0084] <Copper Particles> In the copper paste for manufacturing a copper pillar for semiconductor connection according to the fourth embodiment, the term "copper particles" refers to copper or copper oxide (copper oxide (Cu 2 The copper particles may contain metals other than copper and copper oxides and their oxides, but are preferably composed of copper particles alone.
[0085] In one embodiment, the copper particles may have various shapes such as spherical, ellipsoidal flake (flat), fibrous, or irregular shapes, but are preferably spherical or flake in shape from the viewpoint of the coatability and storage stability of the copper paste. These may be used alone or in combination of two or more.
[0086] In one embodiment, the volume average particle diameter (median diameter, D50) of the metal particles is preferably 1 nm to 500 μm, more preferably 1 nm to 400 μm, even more preferably 1 nm to 300 μm, particularly preferably 1 nm to 200 μm, and most preferably 1 nm to 100 nm. The volume average particle diameter of the copper particles can be measured, for example, using a commercially available laser particle size distribution analyzer (e.g., SALD-7000, manufactured by Shimadzu Corporation).
[0087] In one embodiment, when particles of metals other than copper and copper oxides and their oxides (hereinafter also referred to as other metal particles) are used in combination, the weight ratio of copper particles to the total particles (copper particles / total particles) is preferably 0.35 to 0.9, more preferably 0.4 to 0.87, and even more preferably 0.45 to 0.84.
[0088] In one embodiment, the content of the copper particles in the copper paste (the total content when two or more types of copper particles and / or copper particles having two or more particle sizes are contained) is preferably 50 to 85% by weight, more preferably 50 to 80% by weight, even more preferably 50 to 75% by weight, particularly preferably 50 to 70% by weight, and most preferably 50 to 60% by weight.
[0089] <Dispersion Medium> The copper paste for manufacturing a copper pillar for semiconductor connection according to the fourth embodiment contains a dispersion medium containing a basic compound and a reducing organic substance, and the molar ratio of the basic group contained in the basic compound to the acidic group contained in the reducing organic substance (basic group / acidic group) is 0.5 to 1.2.
[0090] <Basic Compound> The basic compound in the present disclosure increases the temperature at which formic acid volatilizes in the copper paste, makes the compatible substance a good dispersion medium, and suppresses corrosion of the copper particle surface by formic acid. In one embodiment, the basic compound is represented by the following formula (1): [In formula (1), R a ~R c are the same or different and represent a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and represent at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c cannot be a hydrogen atom at the same time. A double line including a dashed line represents a single bond or a double bond, and if it is a double bond, there is no R. a ~R c any two of which may be bonded to each other to form a ring together with the adjacent nitrogen atom].
[0091] In one embodiment, R a ~R c Examples of the hydrocarbon group include an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Of these, an aliphatic hydrocarbon group and an alicyclic hydrocarbon group are preferred, and an aliphatic hydrocarbon group is more preferred.
[0092] In one embodiment, examples of the aliphatic hydrocarbon group include a linear or branched alkyl group, a linear or branched alkenyl group, a linear or branched alkynyl group, and a linear or branched alkylidene group, and among these, a linear or branched alkyl group is preferred.
[0093] In one embodiment, the linear or branched alkyl group is preferably a linear alkyl group having 1 to 12 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkyl group having preferably 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples of such groups include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a decyl group, a dodecyl group, a tetradecyl group, an octadecyl group, an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and a 2-ethylhexyl group.
[0094] In one embodiment, the linear or branched alkenyl group is preferably a linear alkenyl group having 2 to 12 carbon atoms, more preferably 2 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkenyl group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms, and examples thereof include a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, and the like. thenyl group, 3-butenyl group, 1-pentenyl group, 2-pentenyl group, 3-pentenyl group, 4-pentenyl group, 1-hexenyl group, 3-hexenyl group, 5-hexenyl group, 1-heptenyl group, 1-octenyl group, 1-nonenyl group, 1-decenyl group, isopropenyl group, 2-methyl-1-propenyl group, methallyl group, 3-methyl-2-butenyl group, 4-methyl-3-pentenyl group, and the like.
[0095] In one embodiment, the linear or branched alkynyl group is preferably a linear alkynyl group having 2 to 12 carbon atoms, more preferably 2 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkynyl group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples include an ethynyl group, a 1-propynyl group, a 2-propynyl group, a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, a 1-pentynyl group, a 2-pentynyl group, a 3-pentynyl group, a 4-pentynyl group, a 1-hexynyl group, a 2-hexynyl group, a 3-hexynyl group, a 4-hexynyl group, a 5-hexynyl group, a 1-heptynyl group, a 1-octynyl group, a 1-nonynyl group, a 1-decynyl group, a trimethylsilylethynyl group, and a triethylsilylethynyl group.
[0096] In one embodiment, the linear or branched alkylidene group is preferably a linear alkylidene group having 1 to 12 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkylidene group having preferably 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples include a methylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a sec-butylidene group, a pentylidene group, an isopentylidene group, an octylidene group, and an isooctylidene group.
[0097] In one embodiment, examples of the alicyclic hydrocarbon group include a cycloalkyl group and a cycloalkenyl group. The cycloalkyl group is preferably a cycloalkyl group having 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 5 to 8 carbon atoms, and examples thereof include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, and a cyclodecyl group. The cycloalkenyl group is preferably a cycloalkenyl group having 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 5 to 8 carbon atoms, and examples thereof include a cyclopentenyl group and a cyclohexenyl group.
[0098] In one embodiment, the aromatic hydrocarbon group is an aryl group preferably having 6 to 18 carbon atoms, more preferably having 6 to 18 carbon atoms, and even more preferably having 6 to 10 carbon atoms, and examples thereof include a phenyl group and a naphthyl group.
[0099] The double line including the dashed line in formula (1) represents a single bond or a double bond. When the double line including the dashed line is a double bond, there is no reaction, and R in formula (1) a and R b The nitrogen atom to which is bonded represents an imino group or an N-substituted imino group.
[0100] In one embodiment, R a ~R cThe total number of amino groups, N-substituted amino groups, and N,N-substituted amino groups that R may have is preferably 0 to 6, more preferably 1 to 4, and even more preferably 1 or 2. a ~R c The total number of imino groups and N-substituted imino groups that R may have is preferably 0 to 4, more preferably 1 to 3, and even more preferably 1 or 2. a ~R c The total number of hydroxyl groups that may be possessed by is preferably 0 to 6, more preferably 1 to 4, and even more preferably 1 or 2.
[0101] In one embodiment, the substituents of the N-substituted amino group, N,N-substituted amino group, and N-substituted imino group are each selected from the group represented by R a ~R c The hydrocarbon groups are the same as those described above.
[0102] In one embodiment, R a ~R c Any two of these may be bonded to each other to form a ring together with the adjacent nitrogen atom. Examples of the ring formed include a pyrrolidine ring, a pyrroline ring, a piperidine ring, a pyrrole ring, an imidazolidine ring, an imidazole ring, a piperazine ring, an imidazolidine ring, a pyridine ring, a diazine ring, and a triazine ring.
[0103] In one embodiment, R a ~R c The hydrocarbon group in the above formula (1) may have a substituent other than an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, or a hydroxyl group. Examples of such a substituent include a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), an oxo group, a substituted oxy group (an alkoxy group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an aralkyloxy group having 7 to 16 carbon atoms, an acyloxy group having 1 to 4 carbon atoms, etc.), a carboxyl group, a substituted oxycarbonyl group (an alkoxycarbonyl group having 1 to 4 carbon atoms, an aryloxycarbonyl group having 6 to 10 carbon atoms, an aralkyloxycarbonyl group having 7 to 16 carbon atoms, etc.), a cyano group, a nitro group, a sulfo group, a mercapto group, and a heterocyclic group.
[0104] In one embodiment, specific examples of the basic compound represented by formula (1) include, for example, R a ~R c an alkylamine in which at least one of R is a linear or branched alkyl group; a , R b is a hydrogen atom, and R c is a linear or branched alkyl group having one hydroxyl group; a is a hydrogen atom, and R b and R c are the same or different and are linear or branched alkyl groups each having one hydroxyl group; a ~R c are the same or different and are a linear or branched alkyl group having one hydroxyl group; a , R b are the same or different and are a hydrogen atom or a linear or branched alkyl group, and R c an aminoalkanediol in which R in formula (1) is a linear or branched alkyl group having two hydroxyl groups; a ~R c a diamine having a total of one amino group; a ~R c a triamine having a total of two amino groups; R in formula (1) a ~R c a diaminoalkanol having a total of one amino group and a total of one hydroxyl group; R in formula (1) a ~R c an imidazole compound in which a ring is formed by incorporating nitrogen atoms of the imino groups, and R in formula (1) a , R b Examples of such compounds include nitrogen-containing aromatic compounds (pyridine compounds, diazine compounds, triazine compounds, etc.) in which the nitrogen atom to which the reactant is bonded is an imino group and a ring is formed containing the imino group.
[0105] In one embodiment, examples of the alkylamine include methylamine, ethylamine, propylamine, butylamine, pentylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, piperidine, trimethylamine, triethylamine, 4-dimethylaminopyridine, 2-aminopyrazine, 2-aminopyrimidine, 3-aminopyridazine, 2-aminotriazine, diazabicyclononene, and diazabicycloundecene.
[0106] In one embodiment, examples of the monoalkanolamine include 2-aminoethanol, 3-aminopropanol, 1-amino-2-propanol, 1-amino-2-methyl-2-propanol, 2-amino-2-methyl-1-propanol, 4-amino-1-butanol, 6-amino-1-hexanol, 10-amino-1-decanol, 12-amino-1-dodecanol, N-methyl-2-aminoethanol, N-ethyl-2-aminoethanol, N-propyl-2-aminoethanol, 2-dimethylaminoethanol, 6-diethylaminohexanol, 1-(2-hydroxyethyl)pyrrolidine, 2-(hydroxymethyl)pyrrolidine, 2-(2-hydroxyethyl)-1-methylpyrrolidine, 1-piperidineethanol, and 1-ethanol-4-propanolpiperidine.
[0107] In one embodiment, examples of the dialkanolamine include diethanolamine, di-n-propanolamine, diisopropanolamine, di-n-butanolamine, and diisobutanolamine.
[0108] In one embodiment, examples of the trialkanolamine include triethanolamine, tri-n-propanolamine, triisopropanolamine, tri-n-butanolamine, and triisobutanolamine.
[0109] In one embodiment, examples of the aminoalkanediol include 1-amino-2,3-propanediol, 4-amino-1,2-butanediol, 4-amino-1,3-butanediol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 1-methylamino-2,3-propanediol, 1-ethylamino-2,3-propanediol, 1-propylamino-2,3-propanediol, 1-butylamino-2,3-propanediol, 3-dimethylamino-1,2-propanediol, and 2-diethylamino-1,3-propanediol.
[0110] In one embodiment, examples of the diamine include 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,5-diamino-2-methylpentane, N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dimethyl-1,3-propanediamine, N,N'-diethyl-1,3-propanediamine, N,N'-dimethyl-1,4-butanediamine, N,N'-diethyl-1,4-butanediamine, and N , N'-dimethyl-1,6-hexanediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N-dimethyl-1,3-propanediamine, N,N-diethyl-1,3-propanediamine (=diethylaminopropylamine), N,N-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N-dimethyl-1,6-hexanediamine, 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, piperazine, N-methylpiperazine, N-ethylpiperazine, N,N'-dimethylpiperazine, homopiperazine, and the like.
[0111] In one embodiment, examples of the triamine include diethylenetriamine, N,N,N',N",N"-pentamethyldiethylenetriamine (=pentamethyldiethylenetriamine), N,N,N',N",N"-pentakis(2-hydroxypropyl)diethylenetriamine, 3,3'-diaminodipropylamine, N-(3-aminopropyl)-N-methyl-1,3-propanediamine, N'-[3-(dimethylamino)propyl]-N,N-dimethyl-1,3-propanediamine, 2,6,10-trimethyl-2,6,10-triazaundecane, N-(2-aminoethyl)piperazine, 1,4,7-triazacyclononane, N,N,N',N",N"-pentakis(2-hydroxypropyl)diethylenetriamine, 1-(2-aminoethyl)-4-methylpiperazine, and 1-(2-dimethylaminoethyl)-4-methylpiperazine.
[0112] In one embodiment, examples of the diaminoalkanol include 1,3-diaminopropan-2-ol, 2-(2-aminoethylamino)ethanol, 2-(2-aminopropylamino)ethanol, 2-(2-aminoethylmethylamino)ethanol, 1-(2-hydroxyethyl)piperazine, 4-methylpiperazine-1-ethanol, and 1,4-bis(2-hydroxyethyl)piperazine.
[0113] In one embodiment, examples of the imidazole compound include imidazole, 2-methylimidazole, 2-propylimidazole, N-methylimidazole (=1-methylimidazole), N-propylimidazole, N-butylimidazole, 1-(2-hydroxyethyl)imidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 1-acetylimidazole, and 2-hydroxybenzimidazole.
[0114] In one embodiment, examples of the nitrogen-containing aromatic compound include pyridine, α-picoline, β-picoline, γ-picoline, 2,6-lutidine, 2,3-lutidine, pyrazine, 2-hydroxypyrazine, pyrimidine, 2-hydroxypyrimidine, 4-hydroxypyrimidine, pyridazine, 3-hydroxypyridazine, 4-hydroxypyridazine, triazine, 2-hydroxytriazine, etc. These can be used alone or in combination of two or more.
[0115] In one embodiment, the molar ratio of the basic groups contained in the basic compound to the acidic groups contained in the reducing organic substance (basic groups / acidic groups) is preferably 0.5 to 1.2, more preferably 0.55 to 1.15, and even more preferably 0.6 to 1.1. If the molar ratio is below 0.5, the storage stability of the copper paste tends to be poor, and if it exceeds 1.20, it tends to be difficult to obtain a sintered body exhibiting good conductivity. The number of moles of basic groups in the basic compound is calculated by multiplying the number of moles of the basic compound by the number of basic groups contained in the basic compound, and the basic group in the imidazole compound is the one attached to the nitrogen atom at position 1.
[0116] <Reducing Organic Substance> The reducing organic substance in the present disclosure is compatible with the basic compound described below to serve as a dispersion medium for metal particles. It also reduces the oxide film on the surface of the metal particles, promoting sintering of the metal particles. To incorporate the reducing organic substance into the dispersion medium of the present disclosure so that the molar ratio (basic group / acidic group) is 0.5 to 1.2, a reducing organic substance or a mixed solution containing the reducing organic substance can be used. In one embodiment, the reducing organic substance is preferably at least one organic substance selected from formic acid and oxalic acid. Among these, a mixed solution containing 50% by weight or more of formic acid is preferred from the viewpoint of ease of handling, and a formic acid-triethylamine azeotropic composition (e.g., formic acid:triethylamine=5:2 (molar ratio)), 98% formic acid, or an 88% formic acid aqueous solution is more preferred.
[0117] In one embodiment, the content of the reducing organic substance in the copper paste is preferably 6.0 to 22.0 wt%, more preferably 6.0 to 20.0 wt%, and even more preferably 6.0 to 15.0 wt%. In one embodiment, the content of the basic compound in the copper paste is preferably 3 to 35 wt%, more preferably 9.0 to 28.0 wt%, even more preferably 9.0 to 25.0 wt%, and particularly preferably 9.0 to 20.0 wt%. In one embodiment, the weight ratio of the basic compound to the reducing organic substance (basic compound / reducing organic substance) is preferably 0.4 to 5.0, more preferably 0.4 to 4.0, and even more preferably 0.4 to 3.0.
[0118] In one embodiment, the dispersion medium, in order to adjust the fluidity (viscosity) and operability, may contain water or an organic solvent other than the mixture of the basic compound and the reducing organic substance (for example, organic acids other than formic acid (acetic acid, propionic acid, n-octanoic acid, etc.); ester-based solvents such as acetates (ethyl acetate, butyl acetate, etc.); ether-based solvents such as dioxane and tetrahydrofuran; ketone-based solvents such as acetone; aromatic solvents such as toluene and xylene; halogen-based solvents such as dichloromethane and chloroform; alcohol-based solvents such as methanol, ethanol, isopropanol, and butanol; nitrile-based solvents such as acetonitrile and benzonitrile), resin components (for example, polymer compounds having a number average molecular weight of 10,000 or more such as ethyl cellulose resin, alkyl cellulose resin, polyvinyl acetal resin, and acrylic resin), basic compounds other than the basic compounds (inorganic bases (sodium hydroxide, potassium hydroxide, ammonia, etc.)), additives (surface conditioners (leveling agents), antifoaming agents, dispersants, thixotropy-imparting agents, etc.), etc.).
[0119] In the copper paste for manufacturing a copper pillar for semiconductor connection according to the fourth embodiment, the dispersion medium can be manufactured through a process of mixing the above-mentioned basic compound and reducing organic substance with other components to make them compatible. The temperature during mixing preferably does not exceed 100°C. Cooling after mixing may be performed to room temperature (e.g., 25°C) or below, and may be performed gradually at room temperature or rapidly by ice cooling or the like.
[0120] In one embodiment of the copper paste, the content of the basic compound, the content of the reducing organic substance, and the weight ratio (basic compound / reducing organic substance) preferably simultaneously satisfy the following ranges, since this facilitates the formation of a sintered body that fills resist openings formed on a semiconductor chip and exhibits good electrical conductivity. The content of the reducing organic substance is preferably 6 to 22 wt%, more preferably 6 to 15 wt%, and even more preferably 6 to 10 wt%, and the content of the basic compound (total content when two or more types are used in combination) is preferably 3 to 35 wt%, more preferably 9 to 28 wt%, even more preferably 9 to 20 wt%, and particularly preferably 9 to 15 wt%. The weight ratio of the basic compound to the reducing organic substance (basic compound / reducing organic substance) is preferably 0.7 to 3.5, more preferably 0.72 to 3.4, and even more preferably 0.74 to 3.3.
[0121] In the copper paste according to one embodiment, the viscosity measured by a rheometer (25°C, shear rate 10 s -l ) is preferably 0.1 to 200 Pa·s, more preferably 0.1 to 100 Pa·s, and even more preferably 0.1 to 95 Pa·s, from the viewpoint of improving the filling ability into narrower resist openings formed on a semiconductor chip. In one embodiment, the viscosity measured by a rheometer (25°C, shear rate 10 s -l) is 0.1 to 100 Pa s, it may be 0.2 to 100 Pa s, for example, 0.3 to 90 Pa s is preferred. Methods for adjusting the viscosity of the copper paste include, for example, adding water or an organic solvent (excluding a mixture of a basic compound and the above-mentioned reducing organic substance) if the viscosity is too high; not adding a resin component or reducing the amount added; blending an alkylamine having at least one linear alkyl group having 1 to 20 carbon atoms (preferably 1 to 15 carbon atoms) together with a chelating basic compound as the basic compound; reducing the content of copper particles, that is, increasing the proportion of the liquid composition (this is particularly effective in liquid compositions with low viscosity); and increasing the size of the copper particles (increasing the size of the copper particles reduces the number of copper particles per weight, that is, the specific surface area decreases, thereby reducing the frequency of collisions between the copper particles).
[0122] In one embodiment of the copper paste, the maximum peak temperature of differential thermogravimetric analysis (DTG), which is the temperature at which the weight loss slope is greatest in thermogravimetric analysis DTG (heating rate 10 ° C. / min, under a nitrogen atmosphere), is preferably 100 to 220 ° C., more preferably 110 to 210 ° C., and even more preferably 120 to 200 ° C.
[0123] <Method for Manufacturing Copper Paste> The copper paste for manufacturing the copper pillar for semiconductor connection according to the fourth embodiment can be manufactured by mixing copper particles with the dispersion medium. Furthermore, the copper paste of the present disclosure can be manufactured by mixing copper particles with the basic compound, the reducing organic substance, and other components. The temperature during mixing preferably does not exceed 100°C. Cooling after mixing may be performed to room temperature (e.g., 25°C) or below, and may be performed gradually at room temperature or rapidly by ice cooling or the like. The total content of water, organic solvents other than the mixture of the basic compound and the reducing organic substance, basic compounds other than the basic compound, additives, etc. in the copper paste of the present disclosure is preferably 10 wt% or less.
[0124] Since the copper paste of the present disclosure has a suitable viscosity as described above, it is not necessary to add a resin component. Even if a resin component is added, the content of the resin component in the copper paste is preferably 10 wt % or less, more preferably 5 wt % or less. If the amount of the resin component added exceeds the above range, ash derived from the resin component generated by firing causes a deterioration in electrical properties, which is not preferable.
[0125] The mixture of the basic compound and the reducing organic substance contained in the copper paste of the present disclosure quickly volatilizes during firing, and the reducing organic substance reduces the surface oxidation of the metal particles, enabling low-temperature bonding of copper pillars (preferably 120 to 320°C, more preferably 150 to 290°C, and even more preferably 180 to 250°C) without a reducing atmosphere. In one embodiment, copper pillars formed using the copper paste can be bonded at a temperature of 200°C or higher and 250°C or lower. In another embodiment, copper pillars formed using the copper paste can be bonded at a temperature below 200°C (more preferably 180°C). Since the reducing organic substance remains, the bonding may be performed in air or in an inert atmosphere (such as a nitrogen, helium, or argon atmosphere). Furthermore, to achieve a more reduced state, the mixture may be fired in an inert atmosphere with an additional reducing agent, or in a reducing atmosphere (e.g., a formic acid gas atmosphere).
[0126] The copper paste for manufacturing a copper pillar for connecting a semiconductor according to the fourth embodiment has the above-described properties, making it suitable for use in manufacturing a copper pillar for connecting a semiconductor. In manufacturing a copper pillar for connecting a semiconductor according to one embodiment, the copper paste has the above-described properties. Therefore, in manufacturing a copper pillar for connecting a semiconductor according to the present disclosure, a substrate is patterned by photolithography using a resist material or laser etching using a thermosetting resin, and the resulting opening is filled with the copper paste of the present disclosure and pre-dried (200°C, 10 minutes) to form a copper pillar. Examples of thermosetting resins include those exemplified in the ninth embodiment described below. In manufacturing a copper pillar for connecting a semiconductor according to one embodiment, the opening width of the opening is 80 μm or less, preferably 40 μm or less, more preferably 20 μm or less, and particularly preferably 10 μm or less. In manufacturing a copper pillar for connecting a semiconductor according to one embodiment, the opening width of the opening is preferably 40 μm or less. Conventionally, a substrate is patterned with a resist resin, and then a pillar is formed by copper plating. The copper paste for manufacturing a copper pillar for semiconductor connection according to the third embodiment allows the copper pillar to be formed without using a copper plating method, making it possible to form the copper pillar more simply and with fewer steps.
[0127] In one embodiment, the copper paste is useful for manufacturing semiconductor devices because it can bond copper pillars for semiconductor connection at temperatures of 200°C to less than 250°C, preferably less than 200°C, and more preferably at a temperature of 180°C. The copper paste for manufacturing copper pillars for semiconductor connection according to the third embodiment eliminates the need for high-temperature, high-pressure process conditions of 300 to 400°C that were required for copper-copper bonding between pillars formed by copper plating, and can lower the bonding temperature of the copper pillars to 180 to 250°C. When bonding copper pillars for semiconductor connection, a liquid composition may be applied to the bonding portion. By applying a liquid composition to the bonding portion, the copper-copper bonding temperature can be further lowered.
[0128] <Applications> The copper pillar according to the fourth embodiment can reduce the number of steps for forming the copper pillar compared to conventional methods and can also lower the bonding temperature, and therefore can be suitably used for semiconductor devices, particularly as a semiconductor device.
[0129] [Fifth Embodiment: Semiconductor Device Manufacturing Method] The fifth embodiment relates to a semiconductor device manufacturing method including: forming a resin layer on a substrate or a semiconductor chip using a resin composition; patterning the resin layer to form a patterned resin layer having openings; and filling the openings with a copper paste, particularly the above-described copper paste, to form copper pillars. According to the fifth embodiment, the number of steps for forming copper pillars can be reduced compared to conventional methods. In addition, a semiconductor device manufacturing method for manufacturing semiconductor connecting pillars can be provided, which allows for a lower bonding temperature.
[0130] In one embodiment, the method may further include bonding the copper pillars together after removing the patterned resin layer. In one embodiment, it is preferable to further include bonding the patterned resin layers together without removing the patterned resin layers, and metal bonding the copper pillars together.
[0131] <Polymer Hybrid Bonding> In one embodiment, the copper paste for manufacturing the copper pillar for semiconductor connection according to the fourth embodiment is useful in the method for manufacturing the semiconductor device according to the first embodiment (hereinafter also referred to as polymer hybrid bonding).
[0132] Sixth Embodiment: Liquid Composition The sixth embodiment of the present disclosure relates to a liquid composition for assisting bonding between semiconductor connecting pillars, the liquid composition comprising a reducing organic substance, a basic compound, and a coordinating organic compound excluding compounds contained in the basic compound, wherein the coordinating organic compound has a higher boiling point than the reducing organic substance. Because the liquid composition contains a reducing organic substance, applying the liquid composition to the surface of the semiconductor connecting pillar can suppress oxidation of the semiconductor connecting pillar surface during firing, even without a reducing atmosphere. Furthermore, because the liquid composition contains a basic compound, it can dissolve the surface of a metal member to remove a metal oxide film. Furthermore, even if the liquid composition is not removed after application to the surface of the semiconductor connecting pillar, corrosion of the semiconductor connecting pillar surface by the reducing organic substance can be suppressed. For these reasons, the liquid composition is suitable as a liquid composition for assisting bonding between semiconductor connecting pillars.
[0133] In the sixth embodiment, the semiconductor connecting pillar means a metal electrode in the form of a fine protruding column (pillar) formed on a semiconductor chip.
[0134] The liquid composition of the sixth embodiment contains a reducing organic substance, a basic compound, and a coordinating organic compound excluding compounds contained in the basic compound, and the coordinating organic compound has a higher boiling point than the reducing organic substance.
[0135] The liquid composition containing the coordinating organic compound facilitates the formation of a metal complex when the surface of the metal member is dissolved, and the formed metal complex is easily converted into metal nanoparticles when it is thermally decomposed or reductively decomposed and precipitated on the surface of the metal member. When metal nanoparticles are present on the surface of the metal member, the influence of surface diffusion increases, making it easier for the metal members to be bonded at lower temperatures.
[0136] <Reducing Organic Substance> Examples of the reducing organic substance contained in the liquid composition of the sixth embodiment include alcohols (lower alcohols such as ethanol, higher alcohols such as palmitol, and aminoalkanols such as ethanolamines), amino acids, organic acids (carboxylic acids, etc.), and aromatic compounds (polyphenols, phenolic acid compounds, etc.). Among these, organic acids (carboxylic acids, etc.) and aromatic compounds are preferred because they exhibit acidity, and carboxylic acids are more preferred because they are liquid at room temperature, easy to handle, and not highly toxic. These may be used alone or in combination of two or more types.
[0137] In one embodiment, examples of the carboxylic acid include formic acid (boiling point 101°C), acetic acid (boiling point 118°C), lactic acid (boiling point 122°C), propionic acid (boiling point 141°C), acrylic acid (boiling point 141°C), malic acid (boiling point 167°C), n-hexanoic acid (boiling point 205°C), succinic acid (boiling point 235°C), n-octanoic acid (boiling point 237°C), tartaric acid (boiling point 275°C), and oxalic acid (boiling point 365°C). Among these, formic acid and oxalic acid are preferred because they are excellent in reducing properties and can easily produce a sintered body having excellent conductivity.
[0138] In one embodiment, the reducing organic substance is preferably formic acid because it has a low boiling point and can be easily used in combination with a coordinating organic substance having a boiling point higher than that of the reducing organic substance. When two or more reducing organic substances containing formic acid are used in combination, the content of the reducing organic substance other than formic acid in the reducing organic substance is preferably 1 molar part or less relative to 1 molar part of formic acid.
[0139] <Basic Compound> The basic compound contained in the liquid composition of the sixth embodiment is not particularly limited as long as it functions as a base and realizes the effects of the present disclosure, and specific examples include hydroxides of alkali metals, alkaline earth metals, etc., nitrogen-containing compounds such as ammonia and amine compounds, phosphorus-containing compounds such as phosphines and phosphites, etc. Among these, nitrogen-containing compounds represented by the following formula (1) are preferred because they make it easier to obtain a sintered body with excellent electrical conductivity: In formula (1), R a ~R care the same or different and represent a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and represent at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c are not hydrogen atoms at the same time. A double line including a dashed line represents a single bond or a double bond. In the case of a double bond, R c does not exist. a ~R c Any two of may be bonded to each other to form a ring together with the adjacent nitrogen atom.
[0140] R a ~R c Examples of the hydrocarbon group include an aliphatic hydrocarbon group, an alicyclic hydrocarbon group, and an aromatic hydrocarbon group. Of these, an aliphatic hydrocarbon group and an alicyclic hydrocarbon group are preferred, and an aliphatic hydrocarbon group is more preferred.
[0141] Examples of the aliphatic hydrocarbon group include a linear or branched alkyl group, a linear or branched alkenyl group, a linear or branched alkynyl group, and a linear or branched alkylidene group, and among these, a linear or branched alkyl group is preferred.
[0142] The linear or branched alkyl group is preferably a linear alkyl group having 1 to 20 carbon atoms, more preferably 1 to 15 carbon atoms, or a branched alkyl group having preferably 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples of the linear or branched alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a decyl group, a dodecyl group, a tetradecyl group, an octadecyl group, an isopropyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, and a 2-ethylhexyl group.
[0143] The linear or branched alkenyl group is preferably a linear alkenyl group having 2 to 12 carbon atoms, more preferably 2 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkenyl group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples thereof include a vinyl group, a 1-propenyl group, a 2-propenyl group, a 1-butenyl group, a 2-butenyl group, a 3-butenyl group, a 1-pentenyl group, a 2-pentenyl group, a 3-pentenyl group, a 4-pentenyl group, a 1-hexenyl group, a 3-hexenyl group, a 5-hexenyl group, a 1-heptenyl group, a 1-octenyl group, a 1-nonenyl group, a 1-decenyl group, an isopropenyl group, a 2-methyl-1-propenyl group, a methallyl group, a 3-methyl-2-butenyl group, and a 4-methyl-3-pentenyl group.
[0144] The linear or branched alkynyl group is preferably a linear alkynyl group having 2 to 12 carbon atoms, more preferably 2 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkynyl group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples of the linear or branched alkynyl group include an ethynyl group, a 1-propynyl group, a 2-propynyl group, a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, a 1-pentynyl group, a 2-pentynyl group, a 3-pentynyl group, a 4-pentynyl group, a 1-hexynyl group, a 2-hexynyl group, a 3-hexynyl group, a 4-hexynyl group, a 5-hexynyl group, a 1-heptynyl group, a 1-octynyl group, a 1-nonynyl group, a 1-decynyl group, a trimethylsilylethynyl group, and a triethylsilylethynyl group.
[0145] The linear or branched alkylidene group is preferably a linear alkylidene group having 1 to 12 carbon atoms, more preferably 1 to 8 carbon atoms, and even more preferably 2 to 4 carbon atoms, or a branched alkylidene group having 3 to 12 carbon atoms, more preferably 3 to 8 carbon atoms, and even more preferably 3 to 6 carbon atoms. Examples of the linear or branched alkylidene group include a methylidene group, a propylidene group, an isopropylidene group, a butylidene group, an isobutylidene group, a sec-butylidene group, a pentylidene group, an isopentylidene group, an octylidene group, and an isooctylidene group.
[0146] Examples of the alicyclic hydrocarbon group include a cycloalkyl group and a cycloalkenyl group.
[0147] The cycloalkyl group is preferably a cycloalkyl group having 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 5 to 8 carbon atoms, and examples thereof include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclononyl group, and a cyclodecyl group.
[0148] The cycloalkenyl group is preferably a cycloalkenyl group having 3 to 12 carbon atoms, more preferably 4 to 10 carbon atoms, and even more preferably 5 to 8 carbon atoms, and examples thereof include a cyclopentenyl group and a cyclohexenyl group.
[0149] The aromatic hydrocarbon group is preferably an aryl group having 6 to 18 carbon atoms, more preferably 6 to 18 carbon atoms, and even more preferably 6 to 10 carbon atoms, and examples thereof include a phenyl group and a naphthyl group.
[0150] In formula (1), the double line including the dashed line represents a single bond or a double bond. When the double line including the dashed line is a double bond, R c does not exist, and R in formula (1) a and R b The nitrogen atom to which is bonded represents an imino group or an N-substituted imino group.
[0151] R a ~R c The total number of amino groups, N-substituted amino groups and N,N-substituted amino groups that may be contained in the alkyl group is preferably 0 to 6, more preferably 1 to 4, and even more preferably 1 or 2.
[0152] R a ~R c The total number of imino groups and N-substituted imino groups that may be contained in the alkyl group is preferably 0 to 4, more preferably 1 to 3, and even more preferably 1 or 2.
[0153] R a ~R c The total number of hydroxyl groups that may be possessed by is preferably 0 to 6, more preferably 1 to 4, and even more preferably 1 or 2.
[0154] The substituents of the N-substituted amino group, N,N-substituted amino group, and N-substituted imino group are the same as those of the above R a ~R c The hydrocarbon groups are the same as those described above.
[0155] R a ~R c Any two of these may be bonded to each other to form a ring together with the adjacent nitrogen atom. Examples of the ring formed include a pyrrolidine ring, a pyrroline ring, a piperidine ring, a pyrrole ring, an imidazolidine ring, an imidazole ring, a piperazine ring, an imidazolidine ring, a pyridine ring, a diazine ring, and a triazine ring.
[0156] R a ~R c The hydrocarbon group in the formula (I) may have a substituent other than an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, or a hydroxyl group. Examples of such a substituent include a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), an oxo group, a substituted oxy group (an alkoxy group having 1 to 4 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an aralkyloxy group having 7 to 16 carbon atoms, an acyloxy group having 1 to 4 carbon atoms, etc.), a carboxyl group, a substituted oxycarbonyl group (an alkoxycarbonyl group having 1 to 4 carbon atoms, an aryloxycarbonyl group having 6 to 10 carbon atoms, an aralkyloxycarbonyl group having 7 to 16 carbon atoms, etc.), a cyano group, a nitro group, a sulfo group, a mercapto group, and a heterocyclic group.
[0157] Specific examples of the basic compound represented by formula (1) include, for example, R a ~R c an alkylamine in which at least one of R in formula (1) is a linear or branched alkyl group; a , R b is a hydrogen atom, and R c is a linear or branched alkyl group having one hydroxyl group; a is a hydrogen atom, and R b and R care the same or different and are linear or branched alkyl groups each having one hydroxyl group; a ~R c are the same or different and are a linear or branched alkyl group having one hydroxyl group; a , R b are the same or different and are a hydrogen atom or a linear or branched alkyl group, and R c an aminoalkanediol in which R in formula (1) is a linear or branched alkyl group having two hydroxyl groups; a ~R c a diamine having a total of one amino group; a ~R c a triamine having a total of two amino groups; a ~R c a diaminoalkanol having a total of one amino group and a total of one hydroxyl group; R in formula (1) a ~R c an imidazole compound containing one imino group in total, and a ring formed by incorporating the nitrogen atoms of the imino groups; a , R b is bonded to an imino group, and a ring is formed containing the imino group (such as a pyridine-based compound, a diazine-based compound, or a triazine-based compound).
[0158] Examples of the alkylamine include methylamine, ethylamine, propylamine, butylamine, pentylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, piperidine, trimethylamine, triethylamine, dimethyldodecylamine, 4-dimethylaminopyridine, 2-aminopyrazine, 2-aminopyrimidine, 3-aminopyridazine, 2-aminotriazine, diazabicyclononene, and diazabicycloundecene.
[0159] Examples of the monoalkanolamine include 2-aminoethanol, 3-aminopropanol, 1-amino-2-propanol, 1-amino-2-methyl-2-propanol, 2-amino-2-methyl-1-propanol, 4-amino-1-butanol, 6-amino-1-hexanol, 10-amino-1-decanol, 12-amino-1-dodecanol, N-methyl-2-aminoethanol, N-ethyl-2-aminoethanol, 1-dimethylamino-2-propanol, N-propyl-2-aminoethanol, 2-dimethylaminoethanol, 6-diethylaminohexanol, 1-(2-hydroxyethyl)pyrrolidine, 2-(hydroxymethyl)pyrrolidine, 2-(2-hydroxyethyl)-1-methylpyrrolidine, 1-piperidineethanol, and 1-ethanol-4-propanolpiperidine.
[0160] Examples of the dialkanolamine include diethanolamine, di-n-propanolamine, diisopropanolamine, di-n-butanolamine, diisobutanolamine, N-methyl-diethanolamine, and N-ethyl-diethanolamine.
[0161] Examples of the trialkanolamine include triethanolamine, tri-n-propanolamine, triisopropanolamine, tri-n-butanolamine, and triisobutanolamine.
[0162] Examples of the aminoalkanediol include 1-amino-2,3-propanediol, 4-amino-1,2-butanediol, 4-amino-1,3-butanediol, 2-amino-1,3-propanediol, 2-amino-2-methyl-1,3-propanediol, 1-methylamino-2,3-propanediol, 1-ethylamino-2,3-propanediol, 1-propylamino-2,3-propanediol, 1-butylamino-2,3-propanediol, 3-dimethylamino-1,2-propanediol, and 2-diethylamino-1,3-propanediol.
[0163] Examples of the diamine include 1,3-propanediamine, 2,2-dimethyl-1,3-propanediamine, 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,5-diamino-2-methylpentane, N,N'-dimethylethylenediamine, N,N'-diethylethylenediamine, N,N'-dimethyl-1,3-propanediamine, N,N'-diethyl-1,3-propanediamine, N,N'-dimethyl-1,4-butanediamine, and N,N'-diethyl-1,4-butanediamine. Examples thereof include hexanediamine, N,N'-dimethyl-1,6-hexanediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N-dimethyl-1,3-propanediamine, N,N-diethyl-1,3-propanediamine, N,N-dimethyl-1,4-butanediamine, N,N-diethyl-1,4-butanediamine, N,N-dimethyl-1,6-hexanediamine, 1,2-cyclohexanediamine, 1,4-cyclohexanediamine, piperazine, N-methylpiperazine, N-ethylpiperazine, N,N'-dimethylpiperazine, and homopiperazine.
[0164] Examples of the triamine include diethylenetriamine, N,N,N',N",N"-pentamethyldiethylenetriamine, N,N,N',N",N"-pentakis(2-hydroxypropyl)diethylenetriamine, 3,3'-diaminodipropylamine, N-(3-aminopropyl)-N-methyl-1,3-propanediamine, N'-[3-(dimethylamino)propyl]-N,N-dimethyl-1,3-propanediamine, 2,6,10-trimethyl-2,6,10-triazaundecane, N-(2-aminoethyl)piperazine, 1,4,7-triazacyclononane, N,N,N',N",N"-pentakis(2-hydroxypropyl)diethylenetriamine, 1-(2-aminoethyl)-4-methylpiperazine, and 1-(2-dimethylaminoethyl)-4-methylpiperazine.
[0165] Examples of the diaminoalkanol include 1,3-diaminopropan-2-ol, 2-(2-aminoethylamino)ethanol, 2-(2-aminopropylamino)ethanol, 2-(2-aminoethylmethylamino)ethanol, 1-(2-hydroxyethyl)piperazine, 4-methylpiperazine-1-ethanol, and 1,4-bis(2-hydroxyethyl)piperazine.
[0166] Examples of the imidazole compound include imidazole, 2-methylimidazole, 2-propylimidazole, N-methylimidazole, N-propylimidazole, N-butylimidazole, 1-(2-hydroxyethyl)imidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 1-acetylimidazole, and 2-hydroxybenzimidazole.
[0167] Examples of the nitrogen-containing aromatic compound include pyridine, α-picoline, β-picoline, γ-picoline, 2,6-lutidine, 2,3-lutidine, pyrazine, 2-hydroxypyrazine, pyrimidine, 2-hydroxypyrimidine, 4-hydroxypyrimidine, pyridazine, 3-hydroxypyridazine, 4-hydroxypyridazine, triazine, and 2-hydroxytriazine.
[0168] The basic compound contained in the liquid composition according to one embodiment is preferably a chelating basic compound having an ethylenediamine structure or an ethanolamine structure in its molecular structure, since this facilitates stabilization of metal ions dissolved in metal oxides on the surface of the semiconductor connecting pillars by chelating coordination. The amino group in the above structure may be any of primary, secondary, and tertiary amino groups, but is preferably a tertiary amino group, since side reactions such as amidation are less likely to occur between the reducing organic substance and the basic compound.
[0169] The content of the basic compound is preferably 0.25 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, and even more preferably 0.75 to 3 parts by weight, per part by weight of the reducing organic substance, from the viewpoint of facilitating adjustment of the molar ratio (basic group / acidic group) described below.
[0170] The basic compound preferably contains, together with the chelating basic compound, an alkylamine having at least one linear alkyl group having 1 to 20 carbon atoms (preferably 1 to 15 carbon atoms), since the basic compound has relatively low polarity and therefore makes it easier to adjust the viscosity and wettability of the liquid composition. The content of the alkylamine is preferably 0.01 to 1 part by weight, more preferably 0.05 to 0.75 parts by weight, and even more preferably 0.1 to 0.5 parts by weight, per part by weight of the reducing organic substance. Only one type of the basic compound may be used, or two or more types may be used.
[0171] In one embodiment of the liquid composition, the ratio of the total number of moles of basic groups contained in the basic compound to the total number of moles of acidic groups contained in the reducing organic substance (basic groups / acidic groups) is preferably 0.4 to 2.5, more preferably 0.45 to 2.4, and even more preferably 0.5 to 2.3. The total number of moles of acidic groups contained in the reducing organic substance is calculated by multiplying the number of moles of the reducing organic substance by the number of acidic groups contained in the reducing organic substance, and the total number of moles of basic groups contained in the basic compound is calculated by multiplying the number of moles of the basic compound by the number of basic groups contained in the basic compound. In one embodiment, the ratio is preferably 0.7 to 2.5, more preferably greater than 1.0 and not greater than 2.5, and even more preferably greater than 1.0 and not greater than 1.5.
[0172] <Coordinating Organic Compound> The coordinating organic compound contained in the liquid composition according to the sixth embodiment is a coordinating organic compound excluding the compounds contained in the basic compound. The coordinating organic compound has a higher boiling point than the reducing organic compound, and therefore is more likely to remain than the reducing organic compound during firing, which makes it easier to suppress contact between the reducing organic compound and the active metal surface, and therefore makes it easier to suppress decomposition of the reducing organic compound.
[0173] Examples of the coordinating organic compound include compounds having a carboxyl group (such as carboxylic acid), compounds having a ketone group (such as diketones such as acetylacetone and β-ketoesters), and compounds having a hydroxyl group, sulfo group, and thiol group. Among these, compounds having a carboxyl group (such as carboxylic acid) are preferred because they facilitate the precipitation of dissolved metal oxides as metal nanoparticles.
[0174] The compound having a carboxyl group is preferably a monovalent or divalent carboxylic acid, and more preferably a monovalent carboxylic acid, since the precipitated metal nanoparticles are easily sintered.
[0175] Examples of the carboxylic acid include acetic acid (boiling point 118°C), lactic acid (boiling point 122°C), propionic acid (boiling point 141°C), acrylic acid (boiling point 141°C), malic acid (boiling point 167°C), n-hexanoic acid (boiling point 205°C), succinic acid (boiling point 235°C), n-octanoic acid (boiling point 237°C), tartaric acid (boiling point 275°C), oxalic acid (boiling point 365°C), 2-ethylhexanoic acid (boiling point 227°C), and caproic acid (boiling point 205°C). Carboxylic acids may function as reducing organic substances or coordinating organic compounds. Therefore, when a carboxylic acid is used as a reducing organic substance, another carboxylic acid having a boiling point higher than that of the carboxylic acid can be used in combination as a coordinating organic compound.
[0176] The boiling point of the carboxylic acid at normal pressure is preferably above 110°C, more preferably 150°C or higher, and even more preferably 200°C or higher, because the carboxylic acid is less likely to volatilize than formic acid (boiling point 101°C).
[0177] The content of the coordinating organic compound in the liquid composition according to one embodiment is preferably 0.05 to 1.00 parts by weight, more preferably 0.10 to 0.75 parts by weight, and even more preferably 0.15 to 0.50 parts by weight, per 1 part by weight of the reducing organic substance. When the content is 0.05 part by weight or more, precipitation of metal nanoparticles is easily obtained, and when it is 1.00 part by weight or less, the liquid composition is less likely to remain after firing.
[0178] In the liquid composition according to one embodiment, the molar ratio of the coordinating organic compound to the basic compound (coordinating organic compound / basic compound) is preferably 0.01 to 1.00, more preferably 0.05 to 0.50, and even more preferably 0.10 to 0.40. If the molar ratio is 0.01 or more, metal nanoparticles are likely to precipitate, and if it is 1.00 or less, the liquid composition is less likely to remain after firing.
[0179] <Solvent> In order to adjust the fluidity (viscosity) and operability, the liquid composition according to one embodiment may contain, in addition to the basic compound, reducing organic substance, and coordinating organic compound, a solvent such as water or an organic solvent. Examples of the organic solvent include ester-based solvents such as acetates (ethyl acetate, butyl acetate, etc.) and ester oils (butyl stearate, hexyl laurate, triethyl citrate, etc.); ether-based solvents such as dioxane and tetrahydrofuran; ketone-based solvents such as acetone; aromatic solvents such as toluene and xylene; halogen-based solvents such as dichloromethane and chloroform; alcohol-based solvents such as methanol, ethanol, isopropanol, and butanol; and nitrile-based solvents such as acetonitrile and benzonitrile. These may be used alone or in combination of two or more.
[0180] The content of the solvent is preferably 0 to 200 parts by weight, more preferably 0.10 to 100 parts by weight, even more preferably 0.20 to 40 parts by weight, particularly preferably 0.50 to 10 parts by weight, and most preferably 1 to 5 parts by weight, relative to 1 part by weight of the reducing organic substance.
[0181] The liquid composition according to one embodiment may contain other components, such as resin components (e.g., polymeric compounds having a number average molecular weight of 10,000 or more, such as ethyl cellulose resin, alkyl cellulose resin, polyvinyl acetal resin, and acrylic resin), additives (surface conditioners, leveling agents, antifoaming agents, dispersants, thixotropy-imparting agents, etc.), etc., within the range that does not impair the effects of the present disclosure. The content of the other components in the liquid composition is, for example, 1% by weight or less (preferably 0.5% by weight or less).
[0182] <Method for producing liquid composition> The liquid composition according to the sixth embodiment can be produced by mixing the basic compound, reducing organic substance, and coordinating organic compound with the solvent and other components. The temperature during mixing preferably does not exceed 100°C. Cooling after mixing may be performed to room temperature (e.g., 25°C) or below, and may be performed gradually at room temperature or rapidly by ice cooling or the like.
[0183] <Method for manufacturing a solvent-treated semiconductor connecting pillar> A solvent-treated semiconductor connecting pillar can be manufactured by applying the liquid composition according to the sixth embodiment to a semiconductor connecting pillar. In the solvent-treated semiconductor connecting pillar, the metal oxide film on the surface is dissolved and removed by the liquid composition. When the solvent-treated semiconductor connecting pillar is used, the liquid composition remaining on the surface during firing allows for the manufacture of a sintered body and a bonded body with excellent conductivity even without a reducing atmosphere.
[0184] Furthermore, by applying the liquid composition according to the sixth embodiment to a semiconductor connecting pillar, the metal oxide film on the surface is dissolved and removed, and a solvent-treated semiconductor connecting pillar having a surface on which metal nanoparticles having a number-average particle size of less than 600 nm (1 nm or more but less than 600 nm, 5 nm or more but less than 100 nm, or 10 nm or more but less than 60 nm) are precipitated can be produced. That is, by using the liquid composition according to the fourth embodiment, a semiconductor connecting pillar having metal nanoparticles on its surface can be produced by applying the liquid composition to the semiconductor connecting pillar, dissolving at least a portion of the surface of the semiconductor connecting pillar to form a metal complex, and then thermally and / or reductively decomposing the formed metal complex to precipitate metal nanoparticles on the surface of the semiconductor connecting pillar. The thermal decomposition and / or reductive decomposition is achieved by heating in the presence of the reducing organic substance. Since the metal component has nanometal particles on its surface, it can be fired at a lower temperature. The number-average particle size of the metal nanoparticles can be calculated by number, for example, by observation with an electron microscope.
[0185] Examples of metals that form the semiconductor connecting pillars include gold, silver, copper, nickel, palladium, tin, aluminum, and alloys thereof. Among these, copper and silver are prone to forming a metal oxide film on their surfaces, and therefore, when the liquid composition is used, the improvement effect of obtaining a sintered body and a bonded body with excellent electrical conductivity is remarkable.
[0186] The shape of the metal particles contained in the aggregate that is the semiconductor connecting pillar may be various shapes such as spherical, ellipsoidal flake (flat), short fiber, etc., or may be irregular. These may be used alone or in combination of two or more types.
[0187] The volume average particle diameter (median diameter, D 50 The average particle size of the metal particles may be, for example, 1 nm to 100 μm, and may be 600 nm or more (600 nm to 100 μm, or 1 to 10 μm) because the metal nanoparticles precipitate when the second liquid composition is applied. The average particle size of the metal particles can be measured, for example, by a laser diffraction / scattering method.
[0188] When manufacturing the above-mentioned solvent-treated semiconductor connecting pillar, the amount of metal nanoparticles that precipitate can be adjusted by separately dissolving a metal compound in the liquid composition of the sixth embodiment and then applying it.
[0189] As the metal compound to be dissolved, a metal compound containing copper is preferred from the viewpoint of precipitating copper nanoparticles that are easily sintered, and copper oxide (II), cuprous oxide (I), and copper hydroxide (II) are more preferred from the viewpoint of easy storage. These may be used alone or in combination of two or more.
[0190] A sintered body can be obtained by heating the solvent-treated semiconductor connecting pillar obtained by the above-mentioned manufacturing method, and a bonded body can be obtained by contacting the solvent-treated metal member with a bonded body and heating it.
[0191] The bonded body may be formed by applying a liquid composition according to the fourth embodiment to an aggregate layer of metal particles formed on the surface of a substrate to form a treated aggregate layer, and then bonding the substrate and the object to be bonded together by bringing the object to be bonded into contact with the treated aggregate layer and heating the layer.
[0192] The heating can be carried out within a temperature range of, for example, 200 to 250° C., preferably less than 200° C. The heating time may be, for example, 1 to 120 minutes (or 5 to 60 minutes). Furthermore, the bonded body (laminate) may be pressurized against the bonding surfaces at a pressure of, for example, 20 MPa or less.
[0193] [Use of Liquid Composition for Aiding Bonding Between Semiconductor Connection Pillars] The liquid composition for aiding bonding between semiconductor connection pillars according to the sixth embodiment has the above-described properties and is therefore suitable for use in aiding bonding between semiconductor connection pillars. In bonding copper pillars for semiconductor connection according to one embodiment, when bonding copper pillars for semiconductor connection, the bonding temperature can be reduced to 200°C by applying the liquid composition for aiding bonding between semiconductor connection pillars according to the sixth embodiment to the bonding portion. In bonding between semiconductor connection pillars according to one embodiment, the opening width is preferably less than 40 μm. Conventionally, for example, copper-copper bonding between pillars formed by copper plating required process conditions of high temperature and high pressure of 300 to 400°C, which significantly affected the warping of the substrate and other components. However, the liquid composition for aiding bonding between semiconductor connection pillars according to the sixth embodiment can reduce the bonding temperature to 200°C, allowing semiconductor devices to be manufactured with minimal warping of the substrate and minimal impact on other components.
[0194] <Polymer Hybrid Bonding> In one embodiment, the liquid composition for manufacturing a copper pillar for semiconductor connection according to the sixth embodiment is useful in the method for manufacturing a semiconductor device according to the first embodiment (hereinafter also referred to as polymer hybrid bonding).
[0195] Eighth Embodiment: Method for Manufacturing a Semiconductor Device An eighth embodiment of the present disclosure relates to a method for manufacturing a semiconductor device, including: a first step of applying a photosensitive resin composition onto a substrate or a semiconductor chip; a second step of patterning the photosensitive resin composition by photolithography to form copper pillars with a maximum spacing width of 80 μm or less; a third step of filling openings formed by the patterning with copper paste and drying the paste to form copper pillars; a fourth step of planarizing the surface having the copper pillars and the patterning without peeling off the photosensitive resin composition; a step of preparing a set of structures obtained through the first to fourth steps; a fifth step of applying a liquid composition to the planarized surface of at least one of the set of structures; a sixth step of stacking the set of structures so that the copper pillars are in contact with each other; and a seventh step of heating the set of structures at 200° C. or less in an inert atmosphere.
[0196] In one embodiment, from the viewpoint of enabling patterning at a narrower pitch, the photosensitive resin composition in the eighth embodiment is preferably the photosensitive resin composition according to the third embodiment.
[0197] In one embodiment, from the viewpoint of lowering the bonding temperature between structures, the copper paste in the eighth embodiment is preferably the copper paste according to the fourth embodiment.
[0198] In one embodiment, from the viewpoint of lowering the bonding temperature between structures, the liquid composition in the eighth embodiment is preferably the liquid composition according to the sixth embodiment.
[0199] [Ninth Embodiment: Semiconductor Device Manufacturing Method] In the embodiments described so far, examples have been described in which metal pillars are formed in openings in a patterned resin layer, but resin may be applied after the metal pillars are formed. A ninth embodiment of the present disclosure relates to a semiconductor device manufacturing method including: a first step of applying a thermosetting resin to a substrate or a semiconductor chip on which metal pillars are formed at a pitch with a maximum spacing of 80 μm or less; a second step of planarizing the surface on which the metal pillars and the thermosetting resin are formed; a step of preparing a set of structures obtained through the first and second steps; a third step of applying a liquid composition to the planarized metal pillar surface of at least one of the set of structures; a fourth step of stacking the set of structures so that the metal pillars are in contact with each other; and a fifth step of heating the set of structures at 200°C or less (preferably 150 to 200°C, for example 200°C) in an inert atmosphere. According to the ninth embodiment, the number of manufacturing steps can be reduced compared to the conventional method (copper pillar formation steps, resin peeling and re-application steps, etc. are no longer necessary), and the bonding temperature between structures having metal pillars can be further reduced compared to the conventional method.
[0200] In one embodiment, from the viewpoint of adhesion to a substrate or a semiconductor chip, the thermosetting resin according to the ninth embodiment is preferably a thermosetting composition containing a compound (A) represented by the following formula (X) and one or more silsesquioxanes (B) selected from the group consisting of random silsesquioxanes (B1) and silsesquioxanes (B2) having a ladder skeleton, and having a structural unit represented by the following formula (Y): [In formula (X), r1 represents an integer of 4 to 20. L represents a group containing one or more groups selected from the group consisting of an epoxy group, an oxetanyl group, and a vinyl ether group. R 11 and R 12 represents a hydrocarbon group which may have a substituent. s1 represents an integer of 1 to 3, t1 represents an integer of 0 to 2, and s1+t1 is 3. R 13 and R 14 represents a hydrogen atom or a hydrocarbon group which may have a substituent.] [R 1 SiO3/2 ] (Y) [In formula (1), R 1 represents a group containing an epoxy group.
[0201] In one embodiment, from the viewpoint of adhesion between the thermosetting resin and the substrate or the semiconductor chip, it is preferable to apply a surface treatment agent to the substrate or the semiconductor chip before applying the thermosetting resin to the substrate or the semiconductor chip.
[0202] In one embodiment, from the viewpoint of lowering the bonding temperature between structures, the liquid composition in the ninth embodiment is preferably the liquid composition according to the sixth embodiment.
[0203] The method for producing the metal pillar in the semiconductor device manufacturing method of this embodiment can be a conventionally known method, but since the patterning spacing is narrow in the manufacturing method of this embodiment, it is preferable to adopt a method of forming the metal pillar using the copper paste for manufacturing the copper pillar for semiconductor connection of the fourth embodiment.
[0204] The present embodiment will be described in more detail below with reference to examples, but the interpretation of the present invention is not limited to these examples.
[0205] (1) Polymer (A) and (2) Photosensitive Resin Composition The following monomers were used in the synthesis of polymer (A): Methacrylic acid (MAA), 4-hydroxyphenyl methacrylate (PQMA), N-cyclohexylmaleimide (CHMI), butyl acrylate (BA), and p-isopropenylphenol (IPP).
[0206] Example 1 Synthesis of Polymer (A) [MAA / PQMA / CHMI / BA=11 / 14 / 40 / 35 wt %, Mw=10,000, NV=30 wt %] An appropriate amount of nitrogen was passed into a 1 L flask equipped with a reflux condenser, a dropping funnel, and a stirrer to create a nitrogen atmosphere, and 201 g of propylene glycol monomethyl ether acetate was placed therein, followed by heating to 80° C. with stirring. Thereafter, a solution of 96 g (0.53 mol) of N-cyclohexylmaleimide, 84 g (0.65 mol) of butyl acrylate, 34 g (0.19 mol) of 4-hydroxyphenyl methacrylate, and 26 g (0.30 mol) of methacrylic acid dissolved in 222 g of propylene glycol monomethyl ether acetate as monomers, and a mixed solution of 22 g of 2,2'-azobis(2,4-dimethylvaleronitrile) and 2 g of 2,2-azobisisobutyronitrile dissolved in 114 g of propylene glycol monomethyl ether acetate were added dropwise using a dropping pump over a period of about 5 hours. After the dropwise addition of the mixed solution was completed, the temperature was maintained at the same temperature for about 3 hours, and then cooled to room temperature to obtain a solution (P-1) of polymer (A) with a solids content of 31.1 wt%. The resulting copolymer had a weight average molecular weight Mw of 10,000, a polydispersity of 1.90, and an acid value of 70 KOHmg / g.
[0207] Preparation of Photosensitive Resin Composition 12.8 g of the solution (P-1) of polymer (A), 6.4 g of polyester acrylate (Aronix M-8060 manufactured by Toagosei), 0.51 g of diphenyl(2,4,6-trimethoxybenzoyl)phosphine oxide, 0.051 g of 6-[1-(acetyloxyimino)ethyl]-9-ethyl-9H-carbazol-3-yl(2-methylphenyl)ketone, and 12.8 g of propylene glycol monomethyl ether acetate were placed in a flask and heated to 40°C with stirring. Thereafter, the mixture was filtered at 0.1 MPa using a propylene filter (10 μm mesh size) in a pressure filter to obtain a photosensitive resin composition (R-1).
[0208] Comparative Example 1 Polymer Synthesis (MAA / IPP / CHMI / BA=11 / 14 / 40 / 35 wt%, Mw=10,000, NV=30 wt%). A suitable amount of nitrogen was passed into a 1 L flask equipped with a reflux condenser, a dropping funnel, and a stirrer to create a nitrogen atmosphere, and 184 g of propylene glycol monomethyl ether acetate was added and heated to 80° C. with stirring. Thereafter, a solution of 106 g of N-cyclohexylmaleimide, 92 g of butyl acrylate, 37 g of p-isopropenylphenol, and 29 g of methacrylic acid dissolved in 214 g of propylene glycol monomethyl ether acetate as monomers, and 2,2′-azobis(2,4- A mixed solution of 22 g of dimethylvaleronitrile and 2 g of 2,2-azobisisobutyronitrile dissolved in 114 g of propylene glycol monomethyl ether acetate was added dropwise using a dropping pump over a period of approximately 5 hours. After the dropwise addition of the mixed solution was completed, the temperature was maintained for approximately 3 hours and then cooled to room temperature, yielding a polymer solution (P-2) with a solids content of 34.3 wt %. The resulting copolymer had a weight average molecular weight Mw of 9,900, a polydispersity of 1.80, and an acid value of 73 KOHmg / g.
[0209] Preparation of Photosensitive Resin Composition 12.8 g of polymer solution (P-2), 6.4 g of polyester acrylate (Aronix M-8060 manufactured by Toagosei), 0.51 g of diphenyl(2,4,6-trimethoxybenzoyl)phosphine oxide, 0.051 g of 6-[1-(acetyloxyimino)ethyl]-9-ethyl-9H-carbazol-3-yl(2-methylphenyl)ketone, and 12.8 g of propylene glycol monomethyl ether acetate were placed in a flask and heated to 40°C with stirring. Thereafter, the mixture was filtered at 0.1 MPa using a propylene filter (10 μm mesh size) in a pressure filter to obtain a photosensitive resin composition (R-2).
[0210] <Patterning Evaluation> The photosensitive resin compositions (R-1) and (R-2) according to Example 1 and Comparative Example 1 were applied onto a semiconductor chip (Si substrate), and patterns with as small an interval as possible were formed by photolithography under the following conditions: The Si substrate coated with the photosensitive resin composition was pre-baked at 120°C for 5 minutes, and then irradiated with broadband light having a central wavelength of 405 nm at an irradiation intensity of 1800 mJ / cm through a predetermined pattern mask. 2 After the exposure, the coating film was brought into contact with a 2.38% by mass aqueous solution of tetramethylammonium hydroxide for 240 seconds, washed with running water, and developed to perform patterning.
[0211] In the case of the photosensitive resin composition (R-1) according to Example 1, the maximum width of the pitch (spacing) between adjacent openings was 20 μm. In the case of the photosensitive resin composition (R-2) according to Comparative Example 1, the maximum width of the pitch (spacing) between adjacent openings was 40 μm. From the above, it was found that by using the polymer (A) according to the second embodiment and the photosensitive resin composition according to the third embodiment, it is possible to form a pattern with a narrower pitch.
[0212] <Adhesion Evaluation> After applying the photosensitive resin composition (R-1) according to Example 1 onto a Si wafer, the wafer was prebaked at 120°C for 5 minutes, and then irradiated with broadband light having a central wavelength of 405 nm at an irradiation intensity of 1800 mJ / cm 2The coating was exposed to light at 1000 K. After exposure, the coating film was contacted with a 2.38% by mass aqueous solution of tetramethylammonium hydroxide for 240 seconds, and the coating film was washed with running water to form a photosensitive resin composition-coated substrate that had been exposed and developed. The photosensitive resin composition-coated substrate was cut into a size of 20 mm x 20 mm using a diamond cutter, and a Si wafer cut into a size of 3 mm x 3 mm was mounted on the resin composition surface of the cut substrate. The substrate was then heated at 250 ° C. for 10 minutes while applying a load of 0.19 MPa to produce a laminate for adhesive evaluation. The heating rate and cooling rate were 10 ° C. / sec. SEM observation of the cross section of the laminate for evaluation revealed no peeling at the interface between the Si wafer and the photosensitive resin composition (R-1), indicating that the photosensitive resin composition (R-1) can be used as an adhesive layer even after exposure and development.
[0213] When a pair of copper bumps according to Example 1 was bonded together, sufficient bonding strength was obtained between the copper bumps. On the other hand, when a pair of copper bumps according to Comparative Example 1 was bonded together, the copper bumps could not be bonded together.
[0214] As described above, by using the polymer (A) according to the second embodiment and the photosensitive resin composition according to the third embodiment, it is possible to form a pattern with a narrower pitch. Furthermore, after patterning, the resist resin can be used as an adhesive layer without peeling it off or using an adhesive layer separate from the resist resin. This has revealed that it is possible to eliminate steps such as peeling the resist resin, applying an adhesive layer separate from the resist resin, and filling with underfiller.
[0215] (3) Copper Paste In the following, unless otherwise specified, the volume average particle diameter (median diameter, D50) of metal particles is a value measured by a laser diffraction / scattering method. The copper particles, formic acid, basic compound, and other additives used are as follows. <Copper particles> TNCu: volume average particle diameter 110 nm (calculated by SEM observation), manufactured by Taiyo Nippon Sanso Corporation CH-0200L1: volume average particle diameter 200 nm, manufactured by Mitsui Mining & Smelting Co., Ltd. 1100Y: volume average particle diameter 1.1 μm, manufactured by Mitsui Mining & Smelting Co., Ltd. <Formic acid> Formic acid: manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. Formic acid / triethylamine (5:2 molar ratio azeotropic composition): manufactured by Tokyo Chemical Industry Co., Ltd. <Basic compounds> Triethanolamine: reagent manufactured by Tokyo Chemical Industry Co., Ltd. 1-methylimidazole: reagent manufactured by Tokyo Chemical Industry Co., Ltd. Pentamethyldiethylenetriamine: reagent manufactured by Tokyo Chemical Industry Co., Ltd. N-ethyldiethanolamine: reagent manufactured by Tokyo Chemical Industry Co., Ltd. Diethanolamine: reagent manufactured by Tokyo Chemical Industry Co., Ltd. <Other additives> Ethylene glycol: reagent manufactured by Tokyo Chemical Industry Co., Ltd. PVP K30: Fujifilm Wako Pure Chemical Industries, Ltd. Water
[0216] <Peak temperature with the steepest weight loss slope (DTG maximum peak temperature)> A differential thermogravimetric (DTG) curve was obtained by differentiating a TG curve measured by thermogravimetry using a thermogravimetric analyzer (TG-DSC STA200, manufactured by Hitachi High-Tech Science Corporation) under conditions of a nitrogen atmosphere (flow rate 200 ml / min) and a heating rate of 10°C / min, and the peak with the largest negative value was determined as the DTG maximum peak.
[0217] <Viscosity of copper paste> The copper paste evaluation sample was measured using a rheometer (MCR302, manufactured by Anton Paar) with a measuring jig CP25-2 at 25°C, with the shear rate varying in logarithmic increments from 0.01 to 1000 s -1 From the obtained viscosity curve, the shear rate was changed from 10 s -1 The shear viscosity at this point was taken as the viscosity of the copper paste. The results are shown in Table 1.
[0218] Example 2: Ethylene glycol and PVP K30 were mixed to the contents listed in Table 1 and stirred at 60°C for 60 minutes to completely dissolve the PVP K30, yielding a resin solution. The resin solution, formic acid, oxalic acid, N-ethyldiethanolamine, and TNCu were then mixed to the contents listed in Table 1 and stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was produced by stirring for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). The molar ratio of formic acid to basic groups was 0.67. The DTG maximum peak temperature was 194°C. The viscosity of the copper paste was 121 Pa·s, and the viscosity did not increase even after storing it under nitrogen atmosphere at 5°C or 25°C for one week, demonstrating good storage stability. Using the photosensitive resin composition (R-1) according to Example 1, a copper pillar fabrication sample (S-1) with a patterning interval of 40 μm and a copper pillar fabrication sample (S-2) with a patterning interval of 20 μm were fabricated in the same manner as in the patterning evaluation in Example 1. The paste of Example 1 was filled into the openings of the pillar fabrication samples (S-1) and (S-2) using an applicator. The copper paste was filled into (S-1), and a copper pillar could be fabricated. The copper paste was not filled into (S-2), and a copper pillar could not be fabricated.
[0219] Example 3 Formic acid, pentamethyldiethylenetriamine, and CH-0200L1 were mixed to the contents listed in Table 1 and stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by this. The molar ratio of formic acid to basic groups was 0.52. The DTG maximum peak temperature was 135°C. The viscosity of the copper paste was 89.7 Pa·s, and the viscosity did not increase even after storing under nitrogen atmosphere at 5°C or 25°C for 1 week, demonstrating good storage stability. Copper pillars were prepared in the same manner as in Example 2 except that the paste of Example 3 was used. Copper pillars were successfully prepared for both (S-1) and (S-2).
[0220] Example 4 Formic acid, pentamethyldiethylenetriamine, N-ethyldiethanolamine, and CH-0200L1 were mixed to the contents listed in Table 1 and stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by this. The molar ratio of formic acid to basic groups was 0.55. The DTG maximum peak temperature was 135°C. The viscosity of the copper paste was 11 Pa·s, and the viscosity did not increase even after storing it under nitrogen for 1 week at 5°C or 25°C, and the storage stability was also good. Copper pillars were prepared in the same manner as in Example 2 except that the paste of Example 4 was used. Copper pillars were successfully prepared for both (S-1) and (S-2).
[0221] Example 5 Ethylene glycol and PVP K30 were mixed to the contents listed in Table 1 and stirred at 60°C for 60 minutes to completely dissolve the PVP K30, resulting in a resin solution. The resin solution, formic acid, oxalic acid, pentamethyldiethylenetriamine, N-ethyldiethanolamine, TNCu, and 1100Y were then mixed to the contents listed in Table 1, and the mixture was stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by stirring for 2 minutes. The molar ratio of formic acid to basic groups was 1.13. The DTG maximum peak temperature was 194°C. The viscosity of the copper paste was 11 Pa·s, and the viscosity did not increase even after storing the paste under nitrogen atmosphere at 5°C or 25°C for one week, demonstrating good storage stability. Copper pillars were prepared using the same method as in Example 2, except that the paste of Example 5 was used. Copper pillars were successfully prepared for both (S-1) and (S-2).
[0222] Example 6 Formic acid, pentamethyldiethylenetriamine 1-methylimidazole, N-ethyldiethanolamine, and CH-0200L1 were mixed to the contents listed in Table 1 and stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by this. The molar ratio of formic acid to basic groups was 1.13. The DTG maximum peak temperature was 135°C. The viscosity of the copper paste was 0.3 Pa·s. Furthermore, the viscosity did not increase even after storing the paste under nitrogen for one week at 5°C or 25°C, and the storage stability was also good. Copper pillars were prepared in the same manner as in Example 2 except that the paste of Example 6 was used. Copper pillars were successfully prepared for both (S-1) and (S-2).
[0223] Comparative Example 2 A paste was prepared by blending a formic acid / triethylamine mixed solvent (5:2 molar ratio azeotropic composition), triethanolamine, and TNCu in the amounts shown in Table 1 and stirring for 5 minutes using a planetary centrifugal mixer (Thinky Corporation). The molar ratio of formic acid to basic groups (basic groups / formic acid) was 0.96. The DTG maximum peak temperature was 130°C. The viscosity of the paste of Example 2 was 239 Pa·s, and the viscosity did not increase even after storing under nitrogen atmosphere at 5°C or 25°C for one week, demonstrating good storage stability. Copper pillars were prepared using the same method as in Example 2 except that the paste of Comparative Example 2 was used. However, the copper paste could not be filled into both (S-1) and (S-2), and no copper pillars could be prepared.
[0224] (Comparative Example 3) Formic acid, 1-methylimidazole, water, and TNCu were mixed to the contents listed in Table 1 and stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by this. The molar ratio of formic acid to basic groups was 1.13. The DTG maximum peak temperature was 135°C. The viscosity of the copper paste was 0.3 Pa·s, and the viscosity did not increase even after storing it under nitrogen for 1 week at 5°C or 25°C, demonstrating good storage stability. Copper pillars were prepared using the same method as in Example 2 except that the paste of Comparative Example 3 was used. However, the copper paste could not be filled into both (S-1) and (S-2), and no copper pillars could be prepared.
[0225] (Comparative Example 4) Formic acid, triethylamine, and TNCu were mixed to the contents shown in Table 1, and the mixture was stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by this. The molar ratio of formic acid to basic groups was 0.4. The DTG maximum peak temperature was 123°C. The viscosity of the copper paste was 66 Pa s. After storing the paste under nitrogen at 5°C or 25°C for 1 week, the viscosity increased significantly and the storage stability was poor. Copper pillars were prepared in the same manner as in Example 2 except that the paste of Comparative Example 4 was used. Copper pillars were successfully prepared for both (S-1) and (S-2).
[0226] Comparative Example 5 Formic acid, 1-methylimidazole, water, and TNCu were mixed to the contents shown in Table 1, and the mixture was stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by this. The molar ratio of formic acid to basic groups was 0.4. The DTG maximum peak temperature was 117°C. The viscosity of the copper paste was 403 Pa s. After storing the paste in a nitrogen atmosphere at 5°C or 25°C for 1 week, the viscosity increased significantly and the storage stability was poor. Copper pillars were prepared using the same method as in Example 2 except that the paste of Comparative Example 5 was used. However, the copper paste could not be filled into both (S-1) and (S-2), and no copper pillars could be prepared.
[0227] Comparative Example 6 Formic acid, 1-methylimidazole, N-ethyldiethanolamine, water, and TNCu were mixed to the contents listed in Table 1 and stirred for 2 minutes using a planetary centrifugal mixer (Thinky Corporation). A copper paste was prepared by this. The molar ratio of formic acid to basic groups was 1.31. The DTG maximum peak temperature was 136°C. The viscosity of the copper paste was 245 Pa·s, and the viscosity did not increase even after storing it under nitrogen for one week at 5°C or 25°C, demonstrating good storage stability. When copper pillars were prepared using the same method as in Example 2 except for using the paste of Comparative Example 3, it was not possible to fill both (S-1) and (S-2) with the copper paste, and no copper pillars could be prepared. As described above, the copper paste according to the fourth embodiment can reduce the number of steps required for copper pillar formation compared to conventional methods. Furthermore, the bonding temperature can be lowered. Furthermore, the copper paste according to the fourth embodiment can provide high filling properties even when the resist opening formed on the semiconductor chip is narrow.
[0228]
[0229] (4) Liquid Composition The reducing organic substance, basic compound, coordinating organic compound, solvent, and metal particles used in preparing the liquid composition are as follows. <Reducing organic substances> Formic acid: Reagent manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. Oxalic acid: Reagent manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. <Basic compounds> MDETA: N-methyldiethanolamine, reagent manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. PMDTA: Pentamethyldiethylenetriamine, reagent manufactured by Tokyo Chemical Industry Co., Ltd. DMAMPZ: 1-(2-dimethylaminoethyl)-4-methylpiperazine, reagent manufactured by Tokyo Chemical Industry Co., Ltd. DMDA: N,N-dimethyldodecylamine, reagent manufactured by Tokyo Chemical Industry Co., Ltd. <Coordinating organic compounds> Acetic acid: Reagent manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. nHxA: n-hexanoic acid, reagent manufactured by Toho Film Industries Co., Ltd. nOcA: n-octanoic acid, reagent manufactured by Tokyo Chemical Industry Co., Ltd. <Solvents> TEC: Triethyl citrate, a reagent manufactured by Tokyo Chemical Industry Co., Ltd. EtOH: Ethanol, a reagent manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0230] (Preparation of Liquid Composition Samples) The reducing organic substance, basic compound, coordinating organic compound, and solvent were weighed and mixed in a screw tube so as to have the contents shown in Tables 2 and 3, and then the mixture was stirred at 2000 rpm for 1 minute using a planetary centrifugal mixer (product name: "Awatori Rentaro", manufactured by Thinky Corporation) to prepare liquid composition samples 1 to 22 used for evaluating the oxide film removal performance, metal nanoparticle precipitation, electrical conductivity, and bondability.
[0231]
[0232]
[0233] Examples 7 to 10, Comparative Examples 7 and 8: Using the liquid composition samples, the "performance of removing oxide films from copper foil surfaces" was evaluated. (Surface Treatment of Copper Foil) A copper foil (product name "C1020P") having a thickness of 100 μm was cut into a square (5 cm × 5 cm) and heated at 200°C for 10 minutes in air using a hot plate to prepare a test piece of oxidation-treated copper foil having an oxide film on its surface.
[0234] Two drops (approximately 40 mg) of the liquid composition sample were dropped onto the center of the oxidation-treated copper foil using a dropper, and the oxidation-treated copper foil test piece was placed on a hot plate in a glove box with a nitrogen atmosphere (oxygen concentration 100 ppm or less).The temperature was increased from room temperature (25°C) to 150°C at a heating rate of 10°C / min and held for 5 minutes, and then increased to 200°C at a heating rate of 10°C / min and held for 10 minutes.Then, the copper foil was allowed to cool naturally to room temperature (25°C), and after cooling, washed with methanol to produce a liquid composition-treated copper foil.
[0235] (Measurement of Oxide Film Thickness on Copper Foil Surface) Using an oxide film / metal film thickness measuring instrument (product name "QC-100", manufactured by ECI TECHNOLOGY), the thickness of the oxide film formed by oxides, etc. on the surface of the treated copper foil was measured by a continuous electrochemical method. The measurement conditions were as follows. The oxide film thickness was determined as the sum of the thicknesses of cuprous oxide (I), copper oxide (II), and copper sulfide obtained from the measurement results. Measurement was performed on the area where the liquid composition droplets remained until the end when the liquid composition evaporated. If measurement was not possible within the 10-minute measurement time, the thickness was considered to be 100 Å or more. The liquid composition samples used and the evaluation results are shown in Table 3. The copper oxide thickness on the copper foil before the oxidation treatment was 35 Å. Measurement range (gasket size): φ3.2 mm Current value: 30 μA / cm 2 Measurement time: Maximum 10 minutes
[0236] (Evaluation Criteria for Oxide Film Removal Performance) The oxide film removal performance on the copper foil surface was evaluated according to the following criteria: ◯ (Good): 30 Å or less Δ (Fair): More than 30 Å and less than 100 Å × (Poor): 100 Å or more
[0237]
[0238] In Examples 7 to 10, it was shown that the oxide film was successfully removed by treatment using the liquid composition of the present disclosure (evaluation: ◯, △). On the other hand, in Comparative Examples 7 and 8, which did not contain a basic compound, it was shown that the oxide film removal performance was poor (evaluation: ×).
[0239] Examples 11 to 20 and Comparative Example 9: Evaluation was made on the "precipitation of metal nanoparticles on the copper foil surface." For the evaluation, the copper foils treated with the liquid composition prepared in the evaluation of the "performance for removing oxide film from the copper foil surface" were used.
[0240] (Surface of Copper Foil) The presence or absence of precipitation of metal nanoparticles was confirmed by observation with an electron microscope. If precipitation of metal nanoparticles was observed, the particle diameters of 100 of the nanoparticles were measured and the average value was calculated to obtain the number average particle diameter. The liquid composition samples used and the evaluation results are shown in Table 9. Also, Figures 1 to 3 show electron microscope photographs of Example 16, Example 17, and Comparative Example 9, respectively (bottom right bar in Figure 1: 1 μm, bottom right bar in Figure 2: 100 nm, bottom right bar in Figure 3: 1 μm).
[0241] A "-" in the particle size column indicates that no particulate deformation was observed on the surface.
[0242] In Examples 11 to 20, copper nanoparticles were shown to precipitate, and in Examples 11 to 13, where a coordinating organic compound was not added, copper particles of over 1000 nm were shown to precipitate. In Examples 14 to 20, where a coordinating organic compound was added, copper particles of 20 to 500 nm were shown to precipitate. By adding a coordinating organic compound, coarsening during nanoparticle generation can be suppressed and the influence of surface diffusion during bonding can be increased, making it easier to bond metal members even at lower temperatures. On the other hand, in Comparative Example 9, where a basic compound was not included, copper particles were shown not to precipitate.
[0243] Examples 21 to 28, Comparative Examples 10 and 11 Using the above liquid composition samples, the "conductivity" of sintered bodies of copper particle aggregates was evaluated. (Preparation of Copper Particle Aggregates) 10.5 g of formic acid, 10.5 g of nOcA, 2.6 g of PMDTA, 10.9 g of MDEtA, and 13.5 g of DMDA were mixed, and then 0.5 g of polyvinyl butyral resin (product name "S-LEC B BL-1", manufactured by Sekisui Chemical Co., Ltd.) was added as a binder resin and mixed uniformly to obtain a dispersion solvent for copper paste.
[0244] 10 g of copper particles CH-0200L1, 10 g of copper particles CT-0500, and 2.4 g of the copper paste dispersion solvent were stirred and mixed at 2000 rpm for 3 minutes using a planetary centrifugal mixer (product name "ARE-310" manufactured by Thinky Corporation). A copper paste was obtained.
[0245] The copper paste was molded and heated in a nitrogen atmosphere at 200°C for 5 minutes to produce copper particle aggregates (strip-shaped, 50 mm long, 10 mm wide, 20 µm thick). The copper particle aggregates were not sintered and did not exhibit electrical conductivity.
[0246] The liquid composition sample was applied to the prepared copper particle aggregate, and the resulting sintered body was fired at 200°C for 30 minutes in a nitrogen atmosphere. The volume resistivity of the resulting sintered body was measured using a resistivity meter (product name "Loresta GP MCP-T610", manufactured by Mitsubishi Chemical Analytech Co., Ltd.). A smaller volume resistivity value indicates better "conductivity." The liquid composition samples used and the evaluation results are shown in Table 6.
[0247] (Evaluation Criteria for Conductivity) Conductivity was evaluated according to the following criteria: ◯ (Good): Volume resistivity is less than 20 μΩ·cm Δ (Fair): Volume resistivity is 20 μΩ·cm or more and less than 100 μΩ·cm × (Poor): Volume resistivity is 100 μΩ·cm or more
[0248] A "-" in the particle size column indicates that no current flowed and no measurement value was obtained.
[0249] In Examples 21 to 28, it was shown that low volume resistivity and good conductivity were obtained (evaluated as ◯ and △). On the other hand, in Comparative Examples 10 and 11, which did not contain a reducing organic substance or a basic compound, it was shown that high volume resistivity and poor conductivity were obtained.
[0250] (Example 29, Microelectrode Bonding) A copper bumped Si chip (trade name "WALTS-TEG CC40", 10 mm x 10 mm, manufactured by Waltz Corporation) with a pattern of 28,224 (168 x 168) copper bumps (height 15 μm, 22 μmφ) arranged at 40 μm intervals within a 10 mm x 10 mm area, and a Si interposer (trade name "WALTS-TEG IP40", manufactured by Waltz Corporation) with copper pads corresponding to the pattern were used. Figure 4 shows an electron microscope photograph of the copper bump arrangement pattern, and Figure 5 shows an electron microscope photograph of the surface of the copper bump portion (bottom right bar in Figure 4: 10 μm, bottom right bar in Figure 5: 100 nm).
[0251] The copper bumped Si chip was heated to 200 ° C. in air using a hot plate for 5 minutes to oxidize the surface of the copper bumps. 5 μL of the liquid composition sample 7 was applied to the oxidized copper bumped Si chip using a micropipette, and then placed on a hot plate in a glove box with a nitrogen atmosphere (oxygen concentration 100 ppm or less). The temperature was increased from room temperature (25 ° C.) to 150 ° C. at a heating rate of 10 ° C. / min, and then held for 5 minutes. The temperature was then increased to 200 ° C. at a heating rate of 10 ° C. / min, and then held for 10 minutes. The temperature was then naturally cooled to room temperature (25 ° C.). After cooling, the Si chip was washed with methanol to obtain a liquid composition-treated Si chip. Figure 7 shows an electron microscope photograph of the copper bump surface of the liquid composition-treated Si chip (bottom right bar in Figure 6: 100 nm). Copper nanoparticles were precipitated on the surface of the copper bumps.
[0252] A liquid composition-coated Si interposer was obtained by applying 5 μL of the liquid composition sample 19 onto the Si interposer using a micropipette. The liquid composition-coated Si interposer and the liquid composition-treated Si chip were stacked together so that the copper pads and copper bumps were positioned to correspond to each other, and then bonded using a flip chip bonder (product name "T-3000-PRO-HF", manufactured by Dr. TRESKY) by heating at 200° C. for 10 minutes under a nitrogen atmosphere and a load of 1 MPa.
[0253] The bond strength of the bonded structure was measured using a universal bond tester (product name "Die Shear Tester SERIES4000", manufactured by Nordson DAGE). The bond strength was 25 MPa, which was sufficient and indicated excellent bondability.
[0254] From the above results, it was found that the liquid composition for assisting bonding of semiconductor connecting pillars according to the sixth embodiment could reduce the bonding temperature of copper pillars to 200° C. In other words, it became unnecessary to use the high temperature and high pressure process conditions of 300 to 400° C. that were required for copper-to-copper bonding of pillars formed by copper plating, and it was possible to manufacture semiconductor devices with reduced warpage of the substrate and minimal impact on other components.
[0255] <Polymer Hybrid Bonding> (Example 30) The photosensitive resin composition (R-1) according to Example 1 was applied by spin coating onto an oxide film-attached Si wafer and prebaked at 120 ° C. for 5 minutes. Thereafter, photolithography was performed under the conditions described in Example 1 to prepare a copper pillar formation substrate with a patterning interval of 20 μm. The copper paste of Example 4 was applied to the copper pillar formation substrate using an applicator, and then the temperature was increased to 150 ° C. at 5 ° C. / min in a nitrogen atmosphere and held for 5 minutes, and then the temperature was increased to 200 ° C. at 5 ° C. / min and held for 10 minutes to form copper pillars. After the copper pillars were formed, they were planarized by CMP to prepare chips with copper pillars. Two chips with copper pillars were prepared and mounted using a flip-chip bonder so that the copper pillars of the chips and the photosensitive resin compositions were in contact with each other. A bonded structure was then produced by thermal bonding at 250°C for 10 minutes under a nitrogen atmosphere with a load of 1.6 MPa. The bond strength of the bonded structure was measured using a universal bond tester and found to be 16 MPa. The semiconductor device manufacturing method according to the fifth embodiment demonstrated superior bondability between bonded structures. Figures 7 and 8 show photographs of the cross section of the bonded structure of Example 30 observed with a scanning electron microscope at 2000x magnification (Figure 7) or 5000x magnification (Figure 8).
[0256] Example 31 DSM-AcHEt (manufactured by Daicel Corporation) was applied by spin coating onto an oxide film-coated Si wafer on which copper pillars were formed at intervals of 20 μm, followed by baking at 100 ° C. for 5 minutes. R2MX1 (manufactured by Daicel Corporation) was applied by spin coating onto the baked wafer, followed by heating at 80 ° C. for 4 minutes and then at 100 ° C. for 2 minutes to remove the solvent. Further, after baking at 130 ° C. for 20 minutes, a chip with copper pillars was produced by planarizing using CMP. A liquid composition-treated chip was produced by applying the liquid composition sample 6 to the surface of the chip with copper pillars. Two chips were prepared and mounted using a flip chip bonder so that the copper pillars of the chips and the photosensitive resin compositions were in contact with each other. Heat bonding was performed at 200 ° C. for 10 minutes under a nitrogen atmosphere while applying a load of 1.6 MPa to produce a bonded body. 9 and 10 show photographs of the cross section of the bonded body of Example 31 observed with a scanning electron microscope at 2000x magnification (FIG. 9) or 10,000x magnification (FIG. 10). Cross-sectional SEM observation of the bonded body confirmed that the copper pillars were bonded to each other, and furthermore, the temperature for copper-copper bonding could be reduced to 200°C. It was found that the semiconductor device manufacturing method according to the ninth embodiment allows bonding of bonded bodies with fewer steps and enables copper-copper bonding at a lower temperature.
[0257] The semiconductor device manufacturing method of this embodiment can bond metal pillars at a narrower pitch in fewer steps than conventional methods, and therefore can be suitably used in semiconductor device manufacturing methods, etc., and has industrial applicability. The polymer of this embodiment and a photosensitive resin composition containing the polymer can enable patterning at a narrower pitch and can be suitably used in semiconductor device manufacturing methods, etc., and has industrial applicability. The copper paste of this embodiment can reduce the number of steps for copper pillar formation compared to conventional methods and can lower the bonding temperature, and can be suitably used in semiconductor device manufacturing methods, etc., and has industrial applicability. The liquid composition of this embodiment can lower the bonding temperature compared to conventional methods and can be suitably used in semiconductor device manufacturing methods, etc., and has industrial applicability.
Claims
1. A dispersion medium containing copper particles and a basic compound and a reducing organic substance, wherein the molar ratio (basic group / acidic group) of the basic group contained in the basic compound to the acidic group contained in the reducing organic substance is 0.5 to 1.2, and the dispersion medium contains copper particles and a basic compound and a reducing organic substance. -1 The copper paste for producing a copper pillar for connecting a semiconductor device has a viscosity of 0.1 to 200 Pa·s at 20° C.
2. The basic compound is represented by the following formula (1): [In formula (1), R a ~R c are the same or different and each represents a hydrogen atom or a hydrocarbon group which may have a substituent. The substituent may be the same or different and is at least one group selected from an amino group, an N-substituted amino group, an N,N-substituted amino group, an imino group, an N-substituted imino group, and a hydroxyl group. a ~R c At the same time, R is not a hydrogen atom. A double line including a dashed line represents a single bond or a double bond, and when it is a double bond, no reaction is present. a ~R c Any two of the nitrogen-containing compounds may be bonded to each other to form a ring together with adjacent nitrogen atoms.
3. The copper paste according to claim 1 or 2, wherein the reducing organic substance is at least one organic substance selected from the group consisting of formic acid and oxalic acid.
4. Measured by a rheometer at 25°C and a shear rate of 10 s -1 The copper paste according to claim 1 or 2, having a viscosity of 0.1 Pa·s or more and less than 100 Pa·s.
5. The copper paste according to claim 1 or 2, which has a maximum peak temperature of 100 to 220°C as measured by differential thermogravimetry (DTG) analysis at a heating rate of 10°C / min in a nitrogen atmosphere.
6. The copper paste according to claim 1 or 2, wherein the volume average particle diameter of the copper particles is 1 nm or more and 500 nm or less.
7. The copper paste according to claim 1 or 2, wherein the content of the copper particles in the copper paste is 50 to 85 mass %.
8. The copper paste according to claim 1 or 2, wherein the content of the reducing organic substance in the copper paste is 6.0 to 22.0% by weight, and the content of the basic compound is 3.0 to 35.0% by weight.
9. The copper paste according to claim 1 or 2, wherein the content of the basic compound is 3.0 to 35.0% by weight, and the weight ratio of the basic compound to the reducing organic substance (basic compound / reducing organic substance) is 0.4 to 5.
0.
10. A method for manufacturing a semiconductor device, comprising: forming a resin layer on a substrate or a semiconductor chip using a resin composition; patterning the resin layer to form a patterned resin layer having an opening; and filling the opening with the copper paste according to claim 1 or 2 to form a copper pillar.
11. The method for producing a semiconductor device according to claim 10, further comprising bonding copper pillars together after removing the patterned resin layer.
12. The method for manufacturing a semiconductor device according to claim 10, further comprising: bonding the patterned resin layers together without removing the patterned resin layers; and metal bonding copper pillars together.
13. A dispersion medium comprising copper particles and a basic compound and a reducing organic substance, wherein the molar ratio (basic group / acidic group) of the basic group contained in the basic compound to the acidic group contained in the reducing organic substance is 0.5 to 1.2, and the dispersion medium is a dispersion medium containing copper particles and a basic compound and a reducing organic substance. -1 Use of a copper paste having a viscosity of 0.1 to 200 Pa·s at 20° C. for producing a copper pillar for connecting a semiconductor.
14. A method for manufacturing a semiconductor device, comprising: a first step of applying a photosensitive resin composition onto a substrate or a semiconductor chip; a second step of patterning the photosensitive resin composition by photolithography to have a maximum spacing width of 80 μm or less; a third step of filling openings formed by the patterning with copper paste and drying to form copper pillars; a fourth step of planarizing a surface having the copper pillars and the patterning without peeling off the photosensitive resin composition; a step of preparing a set of structures obtained through the first to fourth steps; a fifth step of applying a liquid composition to the planarized surface of at least one of the set of structures; a sixth step of stacking the set of structures so that the copper pillars are in contact with each other; and a seventh step of heating the set of structures at 200° C. or less in an inert atmosphere.
15. The method for producing a semiconductor device according to claim 14, wherein the copper paste is the copper paste according to claim 1 or 2.
16. A semiconductor device comprising a semiconductor bonded by a copper pillar and a resin, the copper pillar being present in an opening in the resin, and the spacing between the openings being 80 μm or less.
Citation Information
Patent Citations
Fine pattern connection circuit part and method for forming the same
JP2003174055A
Photosensitive resin composition, film-shaped resin, resin sheet, resin pattern, semiconductor wafer with resin layer, transparent substrate with resin layer, semiconductor device and method for manufacturing semiconductor device
JP2013216804A
Semiconductor device manufacturing method
JP2016178108A
Conductive pillar and method for manufacturing same, and method for manufacturing bonded structure
WO2021145129A1
Dispersion medium for metal particle sintering, and electroconductive paste