Packaging material, packaging bag, and package
The laminated packaging material with a polyolefin resin base film and heat-sealable layers addresses the challenges of multifunctionality and environmental impact, offering improved gas barrier and sealing performance while ensuring recyclability and microwave safety.
Patent Information
- Application Number
- PCT/JP2024/019829
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-31
- Filing Date
- 2024-05-30
- Publication Date
- 2024-12-05
AI Technical Summary
Current packaging materials face challenges in achieving multifunctionality, such as gas barrier properties, heat sealability, and environmental friendliness, particularly in the design of monomaterial packaging bags that are recyclable and suitable for microwave use.
A laminated packaging material comprising a polyolefin resin-based base film with a gas barrier layer, a heat-sealable film, and specific resin layers, including a linear low-density polyethylene resin and propylene copolymer, to achieve low environmental impact, high sealing strength, and improved gas barrier performance.
The solution provides a packaging material with enhanced gas barrier properties, heat sealability, and a firm feel, while maintaining environmental sustainability and convenience, by optimizing the composition and structure of the resin layers.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Packaging material, packaging bag, and packaging body
[0001] The present invention relates to a laminated packaging material, a packaging bag, and a package used in the packaging fields of foods, medicines, industrial products, etc.
[0002] In recent years, regulations aimed at reducing the use of disposable plastics have been strengthened in Europe and other countries around the world. Behind these trends are growing international awareness of resource recycling and the worsening waste problems in emerging countries. Therefore, environmentally friendly products are being sought from the perspective of the 3Rs (Recycle, Reuse, Reduce) for plastic packaging materials required for food, pharmaceuticals, etc.
[0003] One possibility for making packaging materials more environmentally friendly is to make them from the same recyclable material, i.e., to make them mono-material. For example, polyester-based or polyolefin-based materials are being developed as mono-materials.
[0004] While there is a demand for packaging materials with a low environmental impact, as described above, the current situation is that the properties required of packaging materials themselves are becoming increasingly multifunctional for convenience. In particular, packaging bags that do not use aluminum foil and can be used in microwave ovens are required to simultaneously provide gas barrier properties, heat resistance, toughness (bag tear resistance, pinhole resistance, and firmness), and high sealability, etc., in a single packaging bag. To achieve this, it is necessary to bond different materials, each with different functions, together. A typical bag structure is at least three layers, with a vapor-deposited polyester film on the outside, a polyamide film in the middle, and a polyolefin-based heat-sealable film on the inside (contents side), dry-laminated with an adhesive. While this structure may achieve the desired performance, bonding different materials together makes it less recyclable, which is a problem that makes it less environmentally friendly as described above.
[0005] Taking these points into consideration, research is underway to see if it is possible to design bags with the aforementioned multifunctionality using the same material that can be made into a monomaterial.
[0006] In the design of polyester-based monomaterial packaging materials, a polyester-based sealant with improved low adsorption and heat resistance has been disclosed as an alternative to conventional polyolefin-based sealants (see, for example, Patent Document 1). The polyester-based sealant in Patent Document 1 separates a layer with heat-sealability from other layers, and achieves both heat-sealability and heat resistance by separately controlling the raw material compositions of these layers. However, there is a problem in that the heat-sealability is inferior to the seal strength of polyolefin-based sealants.
[0007] On the other hand, polyolefin-based monomaterial packaging design allows for the use of polyolefin-based heat-sealing resins as sealants, offering the advantage of ensuring sufficient heat-sealing properties compared to the aforementioned polyester-based sealants. Polyolefin-based sealants require a certain thickness to achieve sufficient sealing properties, and they account for a large proportion of the package. This is another major reason for the promotion of polyolefin-based monomaterial packaging design. However, polyolefin-based sealants have the problem of inferior gas barrier performance compared to conventional packaging with barrier properties. While polypropylene film has water vapor barrier properties, its performance is not sufficient compared to, for example, transparent inorganic vapor-deposited polyester film, which is generally considered to have excellent water vapor barrier properties, and its oxygen barrier properties are also very poor.
[0008] In response to this, films have been used in which a polypropylene film is laminated with a polymer resin composition generally considered to have relatively high oxygen barrier properties, such as polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinylidene chloride resin, or polyacrylonitrile (see, for example, Patent Documents 2 to 4). However, gas barrier coated films made using the above-mentioned polymer resin compositions, such as polyvinyl alcohol or ethylene-vinyl alcohol copolymer, are highly humidity-dependent, resulting in a decrease in gas barrier properties under high humidity conditions. Furthermore, while polyvinylidene chloride resin and polyacrylonitrile have low humidity dependency, they have problems such as insufficient absolute barrier values and a high risk of generating hazardous substances during disposal or incineration. Furthermore, the polypropylene film used has insufficient heat resistance, and heating during coating, printing, lamination, and sterilization processes can cause the film to expand and contract, resulting in wrinkles in appearance and reduced performance.
[0009] Regarding the improvement of the gas barrier properties of polypropylene films, attempts have been made to achieve stable gas barrier performance independent of humidity by laminating an inorganic thin film (e.g., Patent Document 5). However, there were problems such as inferior absolute values of gas barrier performance (particularly oxygen barrier performance) compared to conventional polyester vapor-deposited films and vulnerability to physical damage compared to the aforementioned coated barrier films. Barrier materials in which polyolefin sealants are vapor-deposited have also been investigated (e.g., Patent Document 6), but although water vapor barrier performance is achieved, there were problems such as insufficient oxygen barrier performance.
[0010] Furthermore, when designing polyolefin-based mono-material packaging, the heat resistance of the film that forms the outer and middle layers of the bag is low, so if the heat sealing temperature is high, wrinkles will form, resulting in a poor appearance and poor gas barrier properties, and if the heat sealing temperature is low, sufficient seal strength cannot be obtained.
[0011] In contrast, it is known that by using a substrate with a low heat shrinkage rate and a melting point 10°C or more higher than that of the sealant, the laminate does not distort due to heat during bag production, and packaging bags with no dimensional deviation can be obtained even when bag production is carried out at high speed (for example, Patent Document 7). However, in order to obtain sufficient heat seal strength using a polypropylene-based sealant, it is necessary to increase the heat seal temperature, which poses problems such as increased production costs and the risk of burns. Furthermore, the polypropylene-based sealant in Patent Document 7 also has the problem of poor stiffness.
[0012] On the other hand, the use of a polyethylene-based sealant can lower the heat-sealing temperature (see, for example, Patent Document 8). However, when attempting to develop a polyolefin-based monomaterial packaging material into a pouch or the like, it is necessary to consider the handling characteristics during the bag-making process. Compared to polypropylene-based sealants, polyethylene-based sealants have lower rigidity, so there is a risk that the necessary firmness during the bag-making process cannot be ensured, resulting in a poor finish.
[0013] Japanese Patent Application Laid-Open No. 2017-165059 Japanese Patent Application Laid-Open No. 2000-52501 Japanese Patent Application Laid-Open No. 4-359033 Japanese Patent Application Laid-Open No. 2003-231221 WO2017 / 221781 Japanese Patent No. 3318479 Japanese Patent Application Laid-Open No. 2022-191722 Japanese Patent Application Laid-Open No. 2021-123042
[0014] In the above Patent Documents 1 to 8, it was difficult to achieve both mono-material packaging materials and various performances required of packaging materials, particularly gas barrier properties, sheet sealability, and firmness, and it was not possible to design environmentally friendly and convenient packaging materials.
[0015] The present invention was made in light of the problems of the prior art. That is, an object of the present invention is to provide a packaging material, a packaging bag, and a package that are made of a resin that has a low environmental impact and that have all three properties of gas barrier property, heat sealability, and firmness.
[0016] The present inventors have discovered that gas barrier performance can be significantly improved by forming a laminate film in which a predetermined gas barrier layer tailored to the required performance is laminated on a base film, and that by further bonding a resin layer that has excellent low-temperature heat sealing properties and stiffness to the above-mentioned base film as the heat-sealable film, it is possible to provide an environmentally friendly and highly convenient packaging material, which has led to the completion of the present invention.
[0017] That is, the present invention has the following configuration: 1. A packaging material having at least one base film mainly composed of a polyolefin resin and a heat-sealable film, at least one of the base films being a laminated base film having a gas barrier layer, and when the surfaces of the heat-sealable films of the packaging material are heat-sealed together at 120°C, 0.1 MPa, for 1 second, the sealing strength is 10 N / 15 mm or more, the loop stiffness is 22 mN / 25 mm or more, and the oxygen permeability at 23°C x 65% RH is 50 ml / m 2 ・d・MPa or less and water vapor permeability at 40℃ × 90% RH is 3.0 g / m 2d or less. 2. The packaging material according to 1., wherein the total thickness of the packaging material is 140 μm or less. 3. The packaging material according to 1. or 2., wherein the gas barrier layer is an inorganic thin film layer selected from the group consisting of aluminum, aluminum oxide, silicon oxide, and a composite oxide of silicon oxide and aluminum oxide. 4. The packaging material according to any one of 1. to 3., wherein the gas barrier layer is a coating layer containing, as a constituent, a resin selected from the group consisting of polyvinyl alcohol resin, polyester resin, and polyurethane resin. 5. The packaging material according to 4., further containing an inorganic layered compound. 6. The packaging material according to any one of 1. to 5., wherein an anchor coat layer is laminated between the base film and the gas barrier layer. 7. The packaging material according to any one of 1. to 6., wherein a protective layer is laminated on the gas barrier layer. 8. The packaging material according to any one of 1. to 7., wherein the heat-sealable film has a heat-seal layer containing a linear low-density polyethylene resin and a propylene copolymer. 9. The packaging material according to 8., wherein the linear low-density polyethylene resin has a flexural modulus of 200 MPa or less. 10. The packaging material according to 8. or 9., wherein the heat-sealable film comprises, in addition to the heat-seal layer, an intermediate layer and a laminate layer, the heat-seal layer, the intermediate layer and the laminate layer being laminated in this order. 11. The packaging material according to 10., wherein the intermediate layer and the laminate layer comprise a propylene copolymer. 12. The packaging material according to any of 1. to 11., wherein the base film comprises a base layer and a surface layer, the base layer comprising a propylene homopolymer having a mesopentad fraction of 96% or more. 13. The packaging material according to 12., wherein the propylene homopolymer comprises a propylene homopolymer having an MFR of 5 g / 10 min or less and a propylene homopolymer having an MFR of more than 5 g / 10 min. 14. The packaging material according to any of 1. to 13., wherein two or more of the base films are used. 15. A packaging material according to any one of 1. to 14., which is used for microwave heating. 16. A packaging bag made of the packaging material according to any one of 1. to 15. 17. A package in which an item to be packaged is packaged in the packaging material according to any one of 1. to 15.18. A package in which an item is packaged in the packaging bag according to 16.
[0018] According to the present invention, it is possible to provide packaging materials, packaging bags, and packaging bodies that are made of resins that have a low environmental impact and that have gas barrier properties, heat sealability, and a firm feel.
[0019] The packaging material of the present invention is a packaging material having at least one base film mainly composed of a polyolefin resin and a heat-sealable film, wherein at least one of the base films is a laminated base film having a gas barrier layer, and when the surfaces of the heat-sealable films of the packaging material are heat-sealed together at 120°C, 0.1 MPa, for 1 second, the sealing strength is 10 N / 15 mm or more, the loop stiffness is 22 mN / 25 mm or more, and the oxygen permeability at 23°C x 65% RH is 50 ml / m 2 ・d・MPa or less and water vapor permeability at 40℃ × 90% RH is 3.0 g / m 2 The term "main component" as used herein means that the component accounts for 50% by mass or more of the total components.
[0020] The present invention will be described in detail below. [Base Film] The packaging material of the present invention comprises a base film primarily composed of a polyolefin resin. The base film is preferably a base film primarily composed of a polypropylene resin (hereinafter referred to as a polypropylene film), and more preferably a stretched polypropylene film. The stretched polypropylene film used as the base film in the present invention is preferably a biaxially stretched polypropylene film. Any known biaxially stretched polypropylene film can be used as the biaxially stretched polypropylene film, and the raw materials, blend ratio, etc. are not particularly limited. The polypropylene resin may be, for example, a polypropylene homopolymer (propylene homopolymer), a propylene copolymer (preferably a propylene random copolymer or a propylene block copolymer) containing propylene as the main component with one or more α-olefins selected from ethylene, butene, pentene, hexene, etc., or a mixture of two or more of these polymers. The propylene homopolymer and the propylene copolymer may each be used singly or in combination of two or more. For the purpose of improving physical properties, known additives such as antioxidants, antistatic agents, plasticizers, etc. may be added, and for example, petroleum resins, terpene resins, etc. may be added.
[0021] In the present invention, the polypropylene-based resin constituting the base film is preferably a propylene homopolymer that does not substantially contain comonomers other than propylene (preferably ethylene, propylene, or butene), and the comonomer amount is preferably 0 mol % to 0.5 mol %, more preferably 0 mol % to 0.3 mol %, and even more preferably 0 mol % to 0.1 mol %. Within the above range, crystallinity is improved, and the rigidity of the film is improved. Note that a trace amount of comonomer may be contained within a range that does not significantly reduce crystallinity.
[0022] In the present invention, as a means for improving the laminate strength of the substrate film and the interfacial adhesive strength with an inorganic thin film layer, a coating agent, or the like, a mixture of two or more polypropylene resins with different melt flow rates (MFR) may be used as the polypropylene resin constituting the surface layer of the substrate film. Each polypropylene resin may be a propylene homopolymer containing no copolymerization component, or a polypropylene resin copolymerized with ethylene and / or an α-olefin having 4 to 10 carbon atoms at a concentration of more than 0.5 mol% and not more than 5.0 mol%. The copolymerized polypropylene resin preferably contains 1.0 to 4.0 mol%, more preferably 1.5 to 3.5 mol%, and even more preferably 2.0 to 3.5 mol% of the copolymerization component. Examples of α-olefins having 4 to 10 carbon atoms include 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. Polar maleic acid or the like may also be used as another copolymerization component. Among these, the propylene copolymer used for the base film is preferably a propylene-ethylene copolymer, a propylene-butene copolymer, or a propylene-ethylene-butene copolymer, and more preferably a propylene-ethylene copolymer. The propylene copolymer may be a block copolymer or a random copolymer.
[0023] From a practical standpoint, the xylene soluble content of the polypropylene resin constituting the base film is preferably 0.1 to 7 mass %, more preferably 0.1 to 6 mass %, and even more preferably 0.1 to 5 mass %. Within this range, crystallinity is improved, and the rigidity of the film is improved.
[0024] The substrate film preferably comprises a substrate layer and a surface layer, and the substrate layer preferably contains a propylene homopolymer having a mesopentad fraction of 96% or more. The mesopentad fraction of the propylene homopolymer is more preferably 97 to 99.9%, even more preferably 97.5 to 99.9%, and even more preferably 98 to 99.9%. When the mesopentad fraction is within the above range, the crystallinity of the polypropylene resin is high, and a substrate film having predetermined rigidity and heat resistance can be obtained. When the mesopentad fraction is less than 96%, wrinkles may form in part of the packaging material, deteriorating the appearance of the seal. The mesopentad fraction is calculated according to the method described in Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973), and can be calculated using, for example, 13 It can be measured using C-NMR. 13 As a condition for C-NMR measurement, for example, an AVANCE 500 manufactured by BRUKER is used, and 200 mg of a sample is dissolved in a mixed solution of o-dichlorobenzene and deuterated benzene at a ratio of 8:2 at 135°C, and measurement is performed at 110°C.
[0025] In the present invention, the melt flow rate (MFR) (230°C, 2.16 kgf) of the polypropylene resin is preferably 0.5 g / 10 min to 20 g / 10 min, more preferably 1.0 g / 10 min to 17 g / 10 min, even more preferably 2.0 g / 10 min to 16 g / 10 min, and even more preferably 4.0 g / 10 min to 15 g / 10 min. Within the above range, the mechanical load is small, and extrusion and stretching are easy. Furthermore, within the above range, stretching is easy, thickness unevenness is small, the stretching temperature and heat setting temperature can be easily increased, crystallinity is improved, and the rigidity of the film is improved.
[0026] The propylene homopolymer preferably contains a propylene homopolymer having an MFR of 5 g / 10 min or less and a propylene homopolymer having an MFR of more than 5 g / 10 min, more preferably a propylene homopolymer having an MFR of 0.5 to 5 g / 10 min and a propylene homopolymer having an MFR of more than 5 g / 10 min and 10 g / 10 min or less, and even more preferably a propylene homopolymer having an MFR of 1.0 to 5 g / 10 min and a propylene homopolymer having an MFR of more than 5 g / 10 min and 9 g / 10 min or less. Using multiple propylene homopolymers with different MFRs can increase the interfacial adhesive strength with other layers.
[0027] The polypropylene resin may have a predetermined mass average molecular weight, and the mass average molecular weight of the polypropylene resin is preferably 200,000 to 500,000, more preferably 210,000 to 450,000, and even more preferably 220,000 to 400,000. When the mass average molecular weight is within the above range, the stretching temperature can be increased, and stretching tends to be easier.
[0028] The polypropylene resin may have a predetermined number-average molecular weight, and the number-average molecular weight of the polypropylene resin is preferably 30,000 to 100,000, more preferably 40,000 to 90,000, and even more preferably 50,000 to 85,000. When the number-average molecular weight is within the above range, the stretching temperature can be increased, and stretching tends to be easier.
[0029] The molecular weight distribution (mass average molecular weight / number average molecular weight) of the polypropylene resin is preferably 2 to 10, more preferably 2.5 to 9, even more preferably 2.7 to 8, and even more preferably 3 to 7. When the polypropylene resin has a molecular weight distribution within the above range, a low molecular weight polypropylene resin and a high molecular weight polypropylene resin are contained in a balanced manner, and a film with high crystallinity can be obtained. The mass average molecular weight, number average molecular weight, and molecular weight distribution of the polypropylene resin are calculated using gel permeation chromatography (GPC).
[0030] The polypropylene-based resin may have a predetermined DSC melting peak temperature, and the DSC melting peak temperature of the polypropylene-based resin is, for example, 100 to 175° C., preferably 110 to 170° C., more preferably 120 to 167° C., even more preferably 140 to 165° C., and still more preferably 150 to 164° C. When the polypropylene-based resin has a DSC melting peak temperature in the above range, heat sealing at high temperatures becomes possible.
[0031] The polypropylene resin may have a predetermined DSC melting peak area, for example, 50 to 120 J / g, preferably 55 to 110 J / g, more preferably 60 to 100 J / g, and even more preferably 70 to 100 J / g. When the polypropylene resin has a DSC melting peak area within the above range, a substrate film with a high degree of crystallinity can be obtained. The DSC melting peak temperature and DSC melting peak area are both calculated according to the method described in the Examples below.
[0032] From the viewpoint of film rigidity, the content of the polyolefin resin constituting the base film is preferably 70 to 100 mass%, more preferably 80 to 100 mass%, even more preferably 90 to 100 mass%, still more preferably 95 to 100 mass%, and particularly preferably 100 mass%, relative to 100 mass% of the resin composition constituting the base film.
[0033] When the polyolefin resin constituting the substrate film contains a propylene homopolymer (A) having an MFR of 5 g / 10 min or less and a propylene homopolymer (B) having an MFR of more than 5 g / 10 min, the content of the propylene homopolymer (A) having an MFR of 5 g / 10 min or less is preferably 15 to 85 mass%, more preferably 20 to 80 mass%, and even more preferably 25 to 75 mass%, based on 100 mass% of the resin composition constituting the substrate film. The content of the propylene homopolymer (B) having an MFR of more than 5 g / 10 min is preferably 15 to 85 mass%, more preferably 20 to 80 mass%, and even more preferably 25 to 75 mass%, based on 100 mass% of the resin composition constituting the substrate film. When the substrate film has multiple layers, it is sufficient that any one or each of the multiple layers satisfy the above range.
[0034] The substrate film (preferably a biaxially oriented polypropylene film) used in the present invention may be a single-layer film or a laminate film. However, to achieve the objects of the present invention, a laminate film is preferred. The type of laminate, the number of layers, and the lamination method are not particularly limited and can be selected from known methods. However, it is preferable to improve the lamination strength and the adhesive strength of coating agents by controlling the surface roughness and flexibility of the substrate film surface. Examples of the structure of the laminate film include surface layer / substrate layer, surface layer / substrate layer / surface layer, and surface layer / substrate layer / substrate layer / surface layer. An adhesive layer may be provided between the surface layer and the substrate layer, but it is preferable not to provide an adhesive layer from the standpoint of productivity, etc. In particular, the substrate film preferably has a structure of surface layer / substrate layer / surface layer.
[0035] The surface layer and the base layer preferably contain at least a propylene homopolymer, and more preferably contain multiple propylene homopolymers or propylene homopolymers and propylene copolymers. The base layer more preferably contains 10 to 50% by mass (preferably 20 to 40% by mass) of a propylene homopolymer having an MFR of 5 g / 10 min or less and 50 to 90% by mass (preferably 60 to 80% by mass) of a propylene homopolymer having an MFR of more than 5 g / 10 min. The surface layer more preferably contains 50 to 90% by mass (preferably 60 to 80% by mass) of a propylene homopolymer having an MFR of 5 g / 10 min or less and 10 to 50% by mass (preferably 20 to 40% by mass) of a propylene homopolymer having an MFR of more than 5 g / 10 min. The surface layer more preferably contains 40 to 80% by mass (preferably 45 to 75% by mass) of a propylene homopolymer having an MFR of 5 g / 10 min or less and 20 to 60% by mass (preferably 25 to 55% by mass) of a propylene copolymer having an MFR of more than 5 g / 10 min. In the surface layer / base layer / surface layer configuration, the surface layers may have the same configuration or different configurations, but it is preferable that they have the same configuration.
[0036] From the viewpoint of heat resistance, the substrate film may be a uniaxially stretched film in the longitudinal direction (MD direction) or the transverse direction (TD direction), but is preferably a biaxially stretched film. In the present invention, the rigidity can be improved by stretching at least uniaxially, and by using the above-mentioned preferred raw materials, a film with high heat resistance can be obtained, with less dimensional change upon heating than would be expected with conventional polypropylene films. Examples of stretching methods include simultaneous biaxial stretching and sequential biaxial stretching, but sequential biaxial stretching is preferred from the viewpoint of improving flatness, dimensional stability, thickness unevenness, etc.
[0037] In the sequential biaxial stretching method, a polypropylene resin is heated and melted in a single-screw or twin-screw extruder so that the resin temperature is preferably 200 to 280°C (more preferably 210 to 270°C, and even more preferably 220 to 260°C), formed into a sheet from a T-die, and extruded onto a chill roll having a temperature of preferably 10 to 100°C (more preferably 20 to 80°C, and even more preferably 25 to 60°C) to obtain an unstretched sheet. Next, the film is roll-stretched in the machine direction (MD direction) preferably at 120 to 165°C (more preferably 120 to 150°C, even more preferably 120 to 140°C) and preferably 3.0 to 8.0 times (more preferably 3.5 to 7.0 times, even more preferably 4.0 to 6.5 times), and subsequently, after preheating in a tenter, it can be stretched in the transverse direction (TD direction) preferably at 150 to 175°C (more preferably 152 to 170°C, even more preferably 154 to 165°C, even more preferably 155 to 164°C, particularly preferably 156 to 164°C) and preferably 4.0 to 20.0 times (more preferably 5.0 to 15 times, even more preferably 6.0 to 14 times, even more preferably 7.0 to 10 times). Furthermore, after biaxial stretching, heat setting can be carried out at a temperature of preferably 165 to 175°C (more preferably 165 to 172°C, even more preferably 165 to 169°C) while allowing relaxation of preferably 1 to 15% (more preferably 2 to 12%, even more preferably 3 to 10%).
[0038] The substrate film of the present invention is preferably produced by the following method. First, the stretching temperature in the longitudinal direction (MD) is preferably the film melting point (Tm) -20 to -7°C, more preferably Tm -20 to -10°C, and even more preferably Tm -20 to -12°C. Within the above range, the heat elongation rate is easily reduced, and the film is less likely to melt onto the stretching rolls and be difficult to stretch, resulting in little deterioration in quality. Note that the stretching in the longitudinal direction may be performed in two or more stages using three or more pairs of stretching rolls.
[0039] Furthermore, the film produced by the above process can be wound into a roll and then annealed offline.
[0040] In order to improve handleability (e.g., windability after lamination), the substrate film used in the present invention preferably contains particles in the film (preferably the surface layer) to form protrusions on the film surface. Examples of particles to be contained in the film (preferably the surface layer) include inorganic particles such as silica, kaolinite, talc, calcium carbonate, zeolite, and alumina, and heat-resistant polymer particles such as acrylic, PMMA, nylon, polystyrene, polyester, benzoguanamine-formalin condensate, and silicone. Among these, silica and silicone are preferred. From the viewpoint of transparency, the particle content in the film is preferably low, for example, preferably 1 to 4,000 ppm, and more preferably 50 to 3,500 ppm, relative to the total mass of the film (preferably the surface layer). The average particle diameter of the particles is preferably 1.0 to 3.0 μm, more preferably 1.0 to 2.7 μm. The average particle diameter here is measured by taking a photograph using a scanning electron microscope and measuring the Feret's diameter in the horizontal direction using an image analyzer, and expressing the average value. Furthermore, from the viewpoint of transparency, it is preferable to select particles having a refractive index close to that of the resin to be used. In addition, the substrate film may contain, as necessary, antioxidants, ultraviolet absorbers, antistatic agents, dyes, lubricants, nucleating agents, adhesives, antifogging agents, flame retardants, antiblocking agents, inorganic or organic fillers, etc., in order to impart various functions thereto.
[0041] In addition to the polypropylene resin used in the present invention, other resins can be used within the scope of the present invention for the purposes of improving the mechanical properties of the base film, improving adhesion to an ink layer or adhesive layer laminated on the gas barrier coating layer, reducing environmental load, etc. Examples of such resins include polyethylene resins, polypropylene resins different from the above, random copolymers which are copolymers of propylene with ethylene and / or an α-olefin having 4 to 10 carbon atoms, and various elastomers.
[0042] The polyethylene resin that can be used for the substrate film in the present invention is a resin containing ethylene as a primary component. For example, any ethylene homopolymer such as high-pressure low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, or high-density polyethylene can be used. In addition, crystalline or low-crystalline or amorphous random or block copolymers with monomers such as α-olefins such as propylene, butene-1, pentene-1, hexene-1,3-methylbutene-1,4-methylpentene-1, and octene-1, vinyl acetate, (meth)acrylic acid, or (meth)acrylic acid esters, or mixtures thereof, can also be used. The content of the polyethylene resin is preferably 0 to 25% by mass, more preferably 1 to 25% by mass, even more preferably 5 to 20% by mass, even more preferably 8 to 18% by mass, and particularly preferably 8 to 15% by mass, based on 100% by mass of the total polypropylene resin and polyethylene resin that constitute the substrate. When the content exceeds 0% by mass, heat seal strength, blocking resistance, and anti-fogging properties are improved. When the content is 25% by mass or less, rigidity is easily maintained. The melting point of the polyethylene resin is preferably in the range of 100 to 135°C, more preferably 105 to 130°C, from the viewpoints of heat resistance, transparency, mechanical properties, and film-forming properties. The melting point is measured, for example, using a differential scanning calorimeter. The density is measured in accordance with JIS K7112 and is 0.90 to 0.94 g / cm. 3 is preferably 0.91 to 0.94 g / cm 3The melt flow rate (MFR) (190°C, 2.16 kgf) of the polyethylene resin is preferably 0.5 g / 10 min to 20 g / 10 min, more preferably 1 g / 10 min to 15 g / 10 min, and even more preferably 2 g / 10 min to 10 g / 10 min, from the viewpoint of stable moldability.
[0043] In the present invention, the thickness of the substrate film is set arbitrarily according to the intended application, but is preferably 2 to 130 μm, more preferably 3 to 125 μm, even more preferably 4 to 120 μm, even more preferably 5 to 100 μm, and particularly preferably 10 to 50 μm. A thin film reduces the rigidity of the film, making it difficult to handle. On the other hand, a thick film not only creates cost problems, but also makes it prone to poor flatness due to curling when wound into a roll and stored. When the substrate film includes a surface layer and a substrate layer, the total thickness of the surface layer and the substrate layer should be within the above range. The thickness of the substrate layer is, for example, 2 to 40 μm, preferably 3 to 35 μm, more preferably 4 to 30 μm, and even more preferably 5 to 25 μm. The thickness of the surface layer is, for example, 0.5 to 10 μm, preferably 0.7 to 7 μm, and more preferably 0.9 to 5 μm.
[0044] The substrate film of the present invention preferably has transparency from the viewpoint of visibility of contents, and the haze of the substrate film is specifically preferably 0.1 to 6%, more preferably 0.5 to 5%, and even more preferably 1 to 4%. Haze tends to deteriorate, for example, when the stretching temperature or heat setting temperature is too high, when the cooling roll (CR) temperature is high and the cooling rate of the stretched raw sheet is slow, or when there is too much low molecular weight, so it can be controlled within the above range by adjusting these.
[0045] Furthermore, the substrate film in the present invention may be subjected to corona discharge treatment, glow discharge treatment, flame treatment, surface roughening treatment, or known anchor coat treatment, printing, decoration, etc., as long as the object of the present invention is not impaired. Generally, it is preferable to use a resin with good adhesiveness such as polyurethane or polyester for the anchor coat, and the anchor coat layer for improving the barrier layer in the present invention will be described later.
[0046] The packaging material of the present invention includes at least one substrate film having a gas barrier layer. However, using two or more substrate films and laminating them together is more preferable, as this is expected to improve the toughness and gas barrier performance of the packaging material. In terms of toughness, using two polypropylene-based biaxially oriented films, which generally have high puncture strength, enables a packaging material design that is comparable to, for example, a configuration using two sheets of different materials, such as polyester film and polyamide film, which are widely used as packaging materials. In terms of gas barrier performance, using two substrate films makes the intermediate film less susceptible to the influences of the external environment, such as temperature and humidity and external bending, and allows for more stable gas barrier performance. In this sense, when two substrate films are used, it is particularly preferable that the coating layer or inorganic thin film layer having gas barrier performance is laminated to the intermediate film.
[0047] [Gas barrier layer] In the present invention, at least one of the substrate films is a laminated substrate film having a gas barrier layer. As the gas barrier layer, either a coating layer (A) mainly composed of an organic substance or an inorganic thin film layer (B) mainly composed of an inorganic substance, as described below, is laminated. Furthermore, in order to enhance the barrier properties of the gas barrier layer, an anchor coat (C) or a protective layer (D), as described below, can also be laminated in combination.
[0048] [Coating layer (A)] In the present invention, it is preferable to provide a coating layer (A) as a gas barrier layer. However, in the present invention, it is necessary to design the coating layer (A) with due consideration given to the environmental impact, such as increased costs due to the additional steps and difficulty in recycling depending on the coating layer's thickness.
[0049] The gas barrier layer is preferably a coating layer containing, as a constituent component, a resin selected from the group consisting of polyvinyl alcohol resin, polyester resin, and polyurethane resin. Among these, polyvinyl alcohol resin is desirable as the resin used for the coating layer (A). Polyvinyl alcohol resins are primarily composed of vinyl alcohol units, and are expected to significantly improve barrier performance due to their high cohesion properties resulting from a hydrogen-bonded structure. The polymerization degree and saponification degree of the polyvinyl alcohol resin are determined based on the desired gas barrier properties and the viscosity of the coating aqueous solution. The polymerization degree is preferably 100 to 2600, more preferably 200 to 2000, and even more preferably 300 to 1500, from the viewpoint of coating workability. A saponification degree of less than 90% does not provide sufficient oxygen gas barrier properties under high humidity conditions, while a saponification degree of more than 99.7% makes it difficult to prepare the aqueous solution and is prone to gelation, making it unsuitable for industrial production. Therefore, the saponification degree is preferably 90 to 99.7%, more preferably 93 to 99%. In the present invention, various copolymerized or modified polyvinyl alcohol resins, such as polyvinyl alcohol resins copolymerized with ethylene and silanol-modified polyvinyl alcohol resins, can also be used within the range that does not impair processability or productivity.
[0050] The coating layer (A) of the present invention may further contain an inorganic layered compound. The presence of the inorganic layered compound can be expected to provide a labyrinth effect against gases, improving gas barrier properties. Furthermore, the addition of the inorganic layered compound can suppress humidity dependency of gas barrier properties. Examples of materials include clay minerals (including synthetic products thereof) such as smectite, kaolin, mica, hydrotalcite, and chlorite. Specific examples include montmorillonite, beidellite, saponite, hectorite, sauconite, stevensite, kaolinite, nacrite, dickite, halloysite, hydrated halloysite, tetrasilylic mica, sodium taeniolite, muscovite, margarite, phlogopite, talc, antigorite, chrysotile, pyrophyllite, vermiculite, xanthophyllite, and chlorite. Furthermore, scaly silica and the like can also be used as an inorganic layered compound. These may be used alone or in combination of two or more. Among these, smectite (including synthetic products thereof) is particularly preferred because it has a high effect of improving the water vapor barrier property.
[0051] Furthermore, inorganic layered compounds containing metal ions, particularly iron ions, having redox properties are preferred. Among these, montmorillonite, a type of smectite, is preferred from the viewpoint of coating suitability and gas barrier properties. As montmorillonite, known compounds that have been conventionally used in gas barrier agents can be used. For example, compounds represented by the following general formula: (X, Y) 2~3 Z4O 10 (OH)mHO(Wω) (In the formula, X represents Al, Fe(III), or Cr(III). Y represents Mg, Fe(II), Mn(II), Ni, Zn, or Li. Z represents Si or Al. W represents K, Na, or Ca. HO represents interlayer water. m and ω represent positive real numbers.) Among these, those in which W in the formula is Na are preferred because they cleave in an aqueous medium.
[0052] The size and shape of the inorganic layered compound are not particularly limited, but the particle size (major axis) is preferably 1 to 5 μm, more preferably 1 to 4 μm, and even more preferably 1 to 3 μm. If the particle size is larger than 5 μm, dispersibility will be poor, which may result in deterioration of the coatability and coat appearance of the coating layer (A). On the other hand, the aspect ratio is preferably 50 to 5,000, more preferably 100 to 4,000, and even more preferably 200 to 3,000.
[0053] The blending ratio of the resin composition to the inorganic layered compound in the coating layer of the present invention (resin composition / inorganic layered compound) is preferably 75 / 25 to 35 / 65 (mass %), more preferably 70 / 30 to 40 / 60 (mass %), and even more preferably 65 / 35 to 45 / 55 (mass %). If the blending ratio of the inorganic layered compound is less than 25% by mass, the barrier performance may be insufficient. On the other hand, if it is more than 65% by mass, dispersibility may be poor, which may result in poor coatability and poor adhesion.
[0054] In order to improve the cohesive strength of the film and the heat-and-moisture resistant adhesion, various crosslinking agents may be blended into the coating layer (A) of the present invention, as long as they do not impair gas barrier properties or productivity. Examples of crosslinking agents include silicon-based crosslinking agents, oxazoline compounds, carbodiimide compounds, epoxy compounds, isocyanate compounds, etc. Among them, by blending a silicon-based crosslinking agent, a crosslinking reaction can be caused with a resin composition having a hydroxyl group or an inorganic thin film layer, and from the viewpoint of improving water-resistant adhesion, silicon-based crosslinking agents are particularly preferred. Commonly used silicon-based crosslinking agents include metal alkoxides and silane coupling agents. Metal alkoxides are represented by the general formula M(OR) n(M: metal, such as Si or Al; R: alkyl group, such as CH3 or CH5; n is 1 to 4). Specific examples include tetraethoxysilane [Si(OC2H5)4] and triisopropoxyaluminum [Al[OCH(CH3)2]3]. Examples of silane coupling agents include those with epoxy groups, such as 3-glycidoxypropyltrimethoxysilane; those with amino groups, such as 3-aminopropyltrimethoxysilane; those with mercapto groups, such as 3-mercaptopropyltrimethoxysilane; those with isocyanate groups, such as 3-isocyanatopropyltriethoxysilane; and tris-(3-trimethoxysilylpropyl)isocyanurate. Other crosslinking agents, such as oxazoline compounds, carbodiimide compounds, and epoxy compounds, may also be used in combination. However, when recyclability is important, the amount of crosslinker used must be carefully considered.
[0055] When a crosslinking agent is incorporated, its amount in the composition constituting the coating layer is preferably 0.05 to 4.00% by mass, more preferably 0.10 to 3.50% by mass, and even more preferably 0.15 to 3.00% by mass. By maintaining the amount in this range, the film hardens and the cohesive strength improves, resulting in a film with excellent water-resistant adhesion. If the amount of crosslinking agent exceeds 4.00% by mass, the amount of uncrosslinked portions increases, or the film hardens due to excessive hardening, which may result in a decrease in adhesion. On the other hand, if the amount of crosslinking agent is less than 0.05% by mass, sufficient cohesive strength may not be obtained.
[0056] In the present invention, the haze of the film after lamination of the coating layer (A) is preferably 1 to 20%, more preferably 1 to 18%, and even more preferably 1 to 16%, from the viewpoint of visibility of the contents. If the haze is greater than 20%, transparency will be significantly reduced and there is a concern that it may also affect the surface irregularities, which may lead to poor appearance in subsequent printing processes, etc. The haze can be adjusted by the composition ratio of the coating layer (A), solvent conditions, film thickness, etc. Here, the haze is evaluated in accordance with JIS K7136 using a turbidity meter (NDH2000, manufactured by Nippon Denshoku Co., Ltd.).
[0057] The coating amount of the coating layer (A) is 0.10 to 0.70 g / m2 It is preferable to set the density to 0.15 to 0.65 g / m 2 , more preferably 0.20 to 0.60 g / m 2 , and even more preferably 0.25 to 0.55 g / m 2 The coating amount of the coating layer (A) is 0.70 g / m 2 If the coating thickness exceeds 0.10 g / m, the gas barrier property is improved, but the cohesive force inside the coating layer becomes insufficient and the uniformity of the coating layer is also reduced, which may result in unevenness (increased haze, whitening) or defects in the coat appearance, or in insufficient gas barrier property and adhesiveness. In terms of processability, there is also a risk of blocking occurring due to the thick film thickness. Furthermore, there is a concern that this may have an adverse effect on the recyclability of the film, and the amount of raw materials, solvents, etc. used will increase, which will increase the environmental load. On the other hand, if the coating thickness of the coating layer (A) is 0.10 g / m, 2 If it is less than this, there is a risk that sufficient gas barrier properties and interlayer adhesion may not be obtained.
[0058] The coating method for the resin composition for the coating layer is not particularly limited as long as it is a method that can coat the surface of a film to form a layer, and for example, a conventional coating method such as gravure coating, reverse roll coating, wire bar coating, or die coating can be used.
[0059] When forming the coating layer (A), it is preferable to apply the resin composition for the coating layer, pre-dry it at a relatively low temperature to volatilize the solvent, and then dry it at a high temperature, as this will result in a uniform film. The pre-drying temperature is preferably 80 to 110°C, more preferably 85 to 105°C, and even more preferably 90 to 100°C. If the pre-drying temperature is less than 80°C, the coating layer may not be sufficiently dried. If the pre-drying temperature is higher than 110°C, the coating layer may dry before it has spread, resulting in a poor appearance.
[0060] On the other hand, the main drying temperature is preferably 110 to 140°C, more preferably 115 to 135°C, and even more preferably 120 to 130°C. If the main drying temperature is less than 110°C, film formation of the coating layer (A) will not proceed, resulting in a decrease in cohesive strength and adhesiveness, which may adversely affect the barrier properties. If the temperature exceeds 140°C, the film may be subjected to too much heat, making it brittle and causing large wrinkles due to heat shrinkage.
[0061] The preferred drying time for preliminary drying is 3.0 to 10.0 seconds, more preferably 3.5 to 9.5 seconds, and even more preferably 4.0 to 9.0 seconds. The preferred drying time for main drying is 3.0 to 10.0 seconds, more preferably 3.5 to 9.5 seconds, and even more preferably 4.0 to 9.0 seconds. However, care must be taken because the drying conditions vary depending on the type of heat transfer medium and the intake and exhaust conditions of the drying furnace. Furthermore, additional heat treatment for 1 to 4 days at a temperature as low as possible, specifically a temperature range of 40 to 60°C, separate from drying, is also more effective in promoting the formation of the coating layer (A).
[0062] [Inorganic Thin Film Layer (B)] In the present invention, it is preferable to provide an inorganic thin film layer (B) on the surface of the substrate film as a gas barrier layer. The inorganic thin film layer (B) is preferably a thin film made of a metal or an inorganic oxide. There are no particular limitations on the material forming the inorganic thin film layer as long as it can be formed into a thin film. From the viewpoint of gas barrier properties, preferred examples include metals such as aluminum, and inorganic oxides such as silicon oxide (silica), aluminum oxide (alumina), and mixtures of silicon oxide and aluminum oxide. That is, the gas barrier layer is preferably an inorganic thin film layer made of any one of aluminum, aluminum oxide, silicon oxide, or a composite oxide of silicon oxide and aluminum oxide, and more preferably an inorganic thin film layer made of any one of aluminum, silicon oxide, or a composite oxide of silicon oxide and aluminum oxide. In particular, a composite oxide of silicon oxide and aluminum oxide is preferred from the viewpoint of achieving both flexibility and density of the thin film layer. In this composite oxide, the mixing ratio of silicon oxide to aluminum oxide is preferably in the range of 20 to 70 mass % Al, more preferably in the range of 25 to 65 mass %, and even more preferably in the range of 30 to 60 mass %, as the mass ratio of the metal content (Al / (Al+Si)×100). If the Al ratio is less than 20 mass %, the water vapor barrier property may be reduced. On the other hand, if the Al ratio exceeds 70 mass %, the inorganic thin film layer tends to become hard, and there is a risk that the film will be destroyed during secondary processing such as printing or lamination, resulting in a reduction in gas barrier property. Note that silicon oxide referred to here means various silicon oxides such as SiO and SiO2 or mixtures thereof, and aluminum oxide means various aluminum oxides such as AlO and Al2O3 or mixtures thereof.
[0063] The thickness of the inorganic thin film layer (B) is usually 1 to 100 nm, preferably 5 to 50 nm. If the thickness of the inorganic thin film layer (B) is less than 1 nm, it may be difficult to obtain satisfactory gas barrier properties. On the other hand, even if the thickness is excessively thick, exceeding 100 nm, the corresponding improvement in gas barrier properties is not obtained, and it is actually disadvantageous in terms of flex resistance and manufacturing costs. In particular, the thickness of the aluminum layer is, for example, 10 to 100 nm, preferably 15 to 90 nm, more preferably 20 to 80 nm, and even more preferably 25 to 70 nm. The thickness of the silicon oxide layer is, for example, 10 to 80 nm, preferably 15 to 70 nm, and more preferably 20 to 60 nm. The thickness of the silicon oxide and aluminum oxide layers is, for example, 5 to 60 nm, preferably 7 to 50 nm, and more preferably 10 to 40 nm.
[0064] The method for forming the inorganic thin film layer (B) is not particularly limited, and any known vapor deposition method may be appropriately employed, such as physical vapor deposition (PVD) methods such as vacuum deposition, sputtering, and ion plating, or chemical vapor deposition (CVD). A typical method for forming the inorganic thin film layer (B) will be described below, taking silicon oxide / aluminum oxide-based thin films as an example. For example, when using vacuum deposition, a mixture of SiO and AlO, or a mixture of SiO and Al, is preferably used as the vapor deposition source. These vapor deposition sources are typically particles, and the particle size is preferably such that the pressure during vapor deposition does not change, with a preferred particle diameter being 1 to 5 mm. Heating methods such as resistance heating, high-frequency induction heating, electron beam heating, and laser heating can be employed. Furthermore, reactive vapor deposition using reactive gases such as oxygen, nitrogen, hydrogen, argon, carbon dioxide, and water vapor, or ozone addition or ion-assisted deposition can also be employed. Furthermore, the film formation conditions can be changed as desired by applying a bias to the deposition target (substrate film to be subjected to deposition), heating or cooling the deposition target, etc. The deposition material, reactive gas, bias, heating / cooling, etc. of the deposition target can be changed in the same way when sputtering or CVD is employed.
[0065] [Anchor Coat Layer (C)] In the present invention, an anchor coat layer may be laminated between the substrate film and the gas barrier layer (preferably the inorganic thin film layer) as an auxiliary layer to ensure sufficient gas barrier properties and adhesiveness when the gas barrier layer is laminated. The provision of the anchor coat layer can suppress the exposure of oligomers and antiblocking agents from the polypropylene resin. Furthermore, when laminating other layers on the anchor coat layer (C), it can also enhance the adhesion between layers. In particular, when forming an inorganic thin film layer, not only is adhesion improved, but the smoothing of the surface can also be expected to promote the formation of the inorganic layer and improve gas barrier properties. Additionally, by using a material with a certain level of gas barrier properties for the anchor coat layer (C) itself, the gas barrier performance of the film when the gas barrier layer is laminated can be significantly improved. Furthermore, the anchor coat layer (C) prevents hot water from penetrating the substrate, thereby reducing film whitening after boiling or retorting.
[0066] The gas barrier properties of the film when only the anchor coat layer (C) is laminated are such that the oxygen permeability in an environment of 23°C x 65% RH is 1 to 10,000 ml / m 2 MPa is preferable in terms of exhibiting good gas barrier properties after laminating the gas barrier layer, and more preferably 2 to 9000 ml / m 2 d MPa, more preferably 3 to 8000 ml / m 2 ・d・MPa. Oxygen permeability is 10000 ml / m 2 If the modulus exceeds d·MPa, sufficient barrier performance cannot be obtained even after laminating the gas barrier layer, making it difficult to use in applications where high gas barrier properties are required.
[0067] In the present invention, the amount of the anchor coat layer (C) deposited is 0.10 to 0.60 g / m 2This allows the anchor coat layer (C) to be uniformly controlled during coating, resulting in a film with fewer coating irregularities and defects. Furthermore, the anchor coat layer (C) contributes to suppressing oligomer exposure, stabilizing haze after wet heat treatment. The amount of anchor coat layer (C) deposited is more preferably 0.15 to 0.50 g / m 2 , more preferably 0.20 to 0.45 g / m 2 , more preferably 0.35 to 0.40 g / m 2 The amount of the anchor coat layer (C) deposited was 0.60 g / m 2 If the thickness exceeds 0.10 g / m, the gas barrier property is improved, but the cohesive force inside the anchor coat layer becomes insufficient and the uniformity of the anchor coat layer is also reduced, resulting in unevenness and defects in the coat appearance. In terms of processability, a thick film thickness may cause blocking or increase production costs. Furthermore, there is a concern that it may have a negative effect on the recyclability of the film, and the amount of raw materials, solvents, etc. used will increase, resulting in a greater environmental impact. On the other hand, if the thickness of the anchor coat layer (C) is 0.10 g / m, 2 If it is less than this, there is a risk that sufficient gas barrier properties and interlayer adhesion may not be obtained.
[0068] Resin compositions used in the anchor coat layer (C) of the present invention include urethane-based, polyester-based, acrylic-based, titanium-based, isocyanate-based, imine-based, and polybutadiene-based resins to which epoxy-based, isocyanate-based, and melamine-based curing agents have been added. They may also contain crosslinking agents such as silicon-based crosslinkers, oxazoline compounds, carbodiimide compounds, and epoxy compounds. Urethane-based resins are particularly preferred because they offer barrier properties due to the high cohesive properties of the urethane bond itself, as well as the interaction of polar groups with the inorganic thin film layer and flexibility due to the presence of amorphous portions, thereby reducing damage even when subjected to bending loads. Polyester resins are also suitable because they are expected to have similar effects. In the present invention, polyurethanes containing polyester-based resins and isocyanate-based curing agents as constituent components are particularly preferred. Furthermore, the addition of a silicon-based crosslinking agent is even more preferred from the viewpoint of improving adhesion.
[0069] In terms of gas barrier properties, the urethane resin used in the anchor coat layer (C) of the present invention is preferably a urethane resin containing an aromatic or araliphatic diisocyanate component as a main constituent. Among these, it is particularly preferable to use a metaxylylene diisocyanate component. By using such a resin, the cohesive strength of the urethane bond can be further enhanced due to the stacking effect between aromatic rings, resulting in good gas barrier properties.
[0070] In the present invention, the proportion of aromatic or araliphatic diisocyanate in the urethane resin used in the anchor coat layer (C) is preferably 50 mol% or more (50 to 100 mol%) relative to 100 mol% of the polyisocyanate component. The total proportion of aromatic or araliphatic diisocyanate is more preferably 60 to 100 mol%, even more preferably 70 to 100 mol%, and even more preferably 80 to 100 mol%. If the total proportion of aromatic or araliphatic diisocyanate is less than 50 mol%, good gas barrier properties may not be obtained.
[0071] The urethane resin used in the anchor coat layer (C) of the present invention may be blended with various crosslinking agents in order to improve the cohesive strength of the film and improve the adhesion resistance to wet heat.As crosslinking agents, for example, silicon-based crosslinking agents, oxazoline compounds, carbodiimide compounds, epoxy compounds, etc. can be exemplified.Among them, silicon-based crosslinking agents are particularly preferred, because by blending silicon-based crosslinking agents, they can improve the water-resistant adhesion with inorganic thin film layers in particular.Other crosslinking agents may also be used in combination with oxazoline compounds, carbodiimide compounds, epoxy compounds, etc.
[0072] As the silicon-based crosslinking agent, a silane coupling agent is preferred from the viewpoint of crosslinking between an inorganic substance and an organic substance. Examples of the silane coupling agent include hydrolyzable alkoxysilane compounds, such as halogen-containing alkoxysilanes (chloro C2-4 alkyl tri C1-4 alkoxysilanes such as 2-chloroethyltrimethoxysilane, 2-chloroethyltriethoxysilane, 3-chloropropyltrimethoxysilane, and 3-chloropropyltriethoxysilane), and alkoxysilanes having an epoxy group (2-glycidyloxyethyltrimethoxysilane, 2-glycidyloxyethyltriethoxysilane, 3-glycidyloxypropyltriethoxysilane, and the like). trimethoxysilane, glycidyloxy C2-4 alkyltri C1-4 alkoxysilanes such as 3-glycidyloxypropyltriethoxysilane, glycidyloxydi C2-4 alkyldi C1-4 alkoxysilanes such as 3-glycidyloxypropylmethyldimethoxysilane and 3-glycidyloxypropylmethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-(3,4-epoxycyclohexyl)propyl (epoxycycloalkyl)C2-4 alkyltriC1-4 alkoxysilanes such as 2-aminoethyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, etc.], alkoxysilanes having an amino group (aminoC2-4 alkyltriC1-4 alkoxysilanes such as 2-aminoethyltrimethoxysilane, 3-aminopropyltriethoxysilane, etc., aminodiC2-4 alkyldiC1-4 alkoxysilanes such as 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, etc.), 2-[N-(2-aminoethyl)amino] (2-aminoC2-4 alkyl)aminoC2-4 alkyltriC1-4 alkoxysilanes such as 3-[N-(2-aminoethyl)amino]ethyltrimethoxysilane, 3-[N-(2-aminoethyl)amino]propyltrimethoxysilane, and 3-[N-(2-aminoethyl)amino]propyltriethoxysilane; (aminoC2-4 alkyl)aminodiC2-4 alkyldiC1-4 alkoxysilanes such as 3-[N-(2-aminoethyl)amino]propylmethyldimethoxysilane and 3-[N-(2-aminoethyl)amino]propylmethyldiethoxysilane;Alkoxysilanes having a mercapto group (mercapto C2-4 alkyltri C1-4 alkoxysilanes such as 2-mercaptoethyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, etc.; mercaptodi C2-4 alkyldi C1-4 alkoxysilanes such as 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropylmethyldiethoxysilane, etc.); alkoxysilanes having a vinyl group (vinyltri C1-4 alkoxysilanes such as vinyltrimethoxysilane, vinyltriethoxysilane, etc.); ethylene Examples of suitable silane coupling agents include alkoxysilanes having a radically unsaturated bond group [(meth)acryloxyC2-4 alkyltriC1-4 alkoxysilanes such as 2-(meth)acryloxyethyltrimethoxysilane, 2-(meth)acryloxyethyltriethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, and 3-(meth)acryloxypropyltriethoxysilane; and (meth)acryloxydiC2-4 alkyldiC1-4 alkoxysilanes such as 3-(meth)acryloxypropylmethyldimethoxysilane and 3-(meth)acryloxypropylmethyldiethoxysilane]. These silane coupling agents can be used alone or in combination of two or more. Of these silane coupling agents, silane coupling agents having an amino group are preferred, (2-aminoC2-4 alkyl)aminoC2-4 alkyltriC1-4 alkoxysilanes are more preferred, and 3-[N-(2-aminoethyl)amino]propyltrimethoxysilane is even more preferred.
[0073] The silicon-based crosslinking agent is preferably added in an amount of 0.05 to 4.00% by mass to the composition constituting the coating layer, more preferably 0.10 to 3.50% by mass, and even more preferably 0.15 to 3.00% by mass. The addition of the silicon-based crosslinking agent promotes film hardening and improves cohesive strength, resulting in a film with excellent water-resistant adhesion and also expected to prevent oligomer exposure. If the amount added exceeds 4.00% by mass, the film hardens and improves cohesive strength, but some unreacted portions may occur, potentially reducing interlayer adhesion. On the other hand, if the amount added is less than 0.05% by mass, sufficient cohesive strength may not be obtained.
[0074] The polyester resin used in the anchor coat layer (C) of the present invention is produced by polycondensation of a polycarboxylic acid component and a polyhydric alcohol component. The molecular weight of the polyester resin is not particularly limited as long as it can provide sufficient film toughness, coatability, and solvent solubility for use as a coating material, but the number-average molecular weight is preferably 1,000 to 50,000, more preferably 1,500 to 30,000. The functional group at the polyester end is also not particularly limited; it may be an alcohol end, a carboxylic acid end, or both. However, when an isocyanate-based curing agent is used in combination, it is necessary to use a polyester polyol that is predominantly alcohol-terminated.
[0075] The Tg of the polyester resin used in the anchor coat layer (C) of the present invention is preferably 10°C or higher. If the temperature is lower than this, the resin will become tacky after the coating operation, making blocking more likely to occur and making the winding operation after coating more difficult. If the Tg is less than 10°C, it will be difficult to prevent blocking even under conditions where the pressure near the winding core is high, even with the addition of an anti-blocking agent. The Tg is more preferably 15 to 70°C, and even more preferably 20 to 60°C.
[0076] The polyester resin used in the anchor coat layer (C) of the present invention is a polycondensate of a polycarboxylic acid component and a polyhydric alcohol component. The polycarboxylic acid component of the polyester resin used in the present invention includes at least one ortho-oriented aromatic dicarboxylic acid or its anhydride. Ortho-orientation improves solubility in solvents, enabling uniform coating on the substrate. A uniformly coated film reduces variation in barrier performance, thereby contributing to the suppression of whitening caused by oligomers. Furthermore, ortho-orientation results in a film with excellent flexibility and improved interfacial adhesion, thereby reducing damage to the substrate due to wet heat treatment and leading to the suppression of oligomers. Examples of aromatic polycarboxylic acids or anhydrides in which carboxylic acids are substituted at the ortho positions include orthophthalic acid or its anhydride, naphthalene 2,3-dicarboxylic acid or its anhydride, naphthalene 1,2-dicarboxylic acid or its anhydride, anthraquinone 2,3-dicarboxylic acid or its anhydride, and 2,3-anthracenecarboxylic acid or its anhydride. These compounds may have a substituent on any carbon atom of the aromatic ring. Examples of the substituent include a chloro group, a bromo group, a methyl group, an ethyl group, an i-propyl group, a hydroxyl group, a methoxy group, an ethoxy group, a phenoxy group, a methylthio group, a phenylthio group, a cyano group, a nitro group, an amino group, a phthalimide group, a carboxyl group, a carbamoyl group, an N-ethylcarbamoyl group, a phenyl group, or a naphthyl group. Furthermore, polyester polyols having a content of these in an amount of 70 to 100 mol % relative to 100 mol % of the total polycarboxylic acid components are particularly preferred because they have a high effect of improving barrier properties and excellent solvent solubility, which is essential for a coating material.
[0077] In the present invention, other polycarboxylic acid components may be copolymerized within the range that does not impair the effects of the present invention. Specifically, examples of aliphatic polycarboxylic acids include succinic acid, adipic acid, azelaic acid, sebacic acid, and dodecanedicarboxylic acid; examples of unsaturated bond-containing polycarboxylic acids include maleic anhydride, maleic acid, and fumaric acid; examples of alicyclic polycarboxylic acids include 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid; examples of aromatic polycarboxylic acids include terephthalic acid, isophthalic acid, pyromellitic acid, trimellitic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, naphthalic acid, biphenyldicarboxylic acid, diphenic acid and its anhydride, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, and anhydrides or ester-forming derivatives of these dicarboxylic acids; and ... p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid, and ester-forming derivatives of these dihydroxycarboxylic acids. These polybasic acids can be used alone or in mixtures of two or more. Among these, succinic acid, 1,3-cyclopentanedicarboxylic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalic acid, and diphenic acid are preferred from the viewpoint of organic solvent solubility and gas barrier properties.
[0078] The polyhydric alcohol component of the polyester used in the anchor coat layer (C) of the present invention is not particularly limited as long as it can synthesize a polyester that exhibits gas barrier filling performance, but it is preferable for it to contain a polyhydric alcohol component containing at least one selected from the group consisting of ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol, cyclohexanedimethanol, and 1,3-bishydroxyethylbenzene. Among these, it is most preferable to use ethylene glycol as the main component, because it is presumed that the fewer the number of carbon atoms between oxygen atoms, the less flexible the molecular chain becomes and the more difficult oxygen permeates.
[0079] In the present invention, it is preferable to use the polyhydric alcohol component described above, but other polyhydric alcohol components may also be copolymerized within the scope of not impairing the effects of the present invention. Specific examples of diols include 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, methylpentanediol, dimethylbutanediol, butylethylpropanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, and tripropylene glycol. Examples of trihydric or higher alcohols include glycerol, trimethylolpropane, trimethylolethane, tris(2-hydroxyethyl)isocyanurate, 1,2,4-butanetriol, pentaerythritol, and dipentaerythritol. Polyesters containing glycerol and tris(2-hydroxyethyl)isocyanurate in combination are particularly preferred, as they have a moderately high crosslinking density due to their branched structure, resulting in good solubility in organic solvents and excellent barrier function.
[0080] Examples of catalysts that can be used in the reaction to obtain the polyester of the present invention include tin-based catalysts such as monobutyltin oxide and dibutyltin oxide, titanium-based catalysts such as tetraisopropyltitanate and tetrabutyltitanate, and acid catalysts such as zirconia-based catalysts such as tetrabutylzirconate. It is preferable to use a combination of the above-mentioned titanium-based catalysts, such as tetraisopropyltitanate and tetrabutyltitanate, which have high activity in esterification reactions, with the above-mentioned zirconia catalyst. The amount of the catalyst is preferably 1 to 1,000 ppm, more preferably 10 to 100 ppm, based on the total mass of the reaction raw materials used. If the amount is less than 1 ppm, it is difficult to obtain the catalytic effect, and if it exceeds 1,000 ppm, problems such as inhibition of the urethanization reaction may occur when an isocyanate curing agent is used.
[0081] In the present invention, when a polyester resin is used as the main component of the coating agent constituting the anchor coat layer (C), it is particularly preferable to use an isocyanate-based curing agent to form a urethane resin. In this case, the coating layer becomes crosslinked, which has the advantage of improving heat resistance, abrasion resistance, and rigidity. On the other hand, there is the problem that the liquid cannot be reused after mixing with the curing agent, and a curing (aging) process is required after coating. Examples of advantages include the fact that, as a simple overcoat varnish, there is no risk of thickening of the coating liquid, coating production is easy to manage, the coating liquid can be diluted and reused, and a curing process (so-called aging process) is not required. In this case, the polyester used can be terminated with a polyol, a polycarboxylic acid, or a mixture of these without any problems. On the other hand, since the resin of the coating layer is linear, problems such as insufficient heat resistance and abrasion resistance may occur.
[0082] When a curing agent is used in the coating layer, since it is a coating on a film, an isocyanate-based curing agent is preferred from the standpoint of the film's heat resistance; in this case, the resin component of the coating material must be polyester polyol. On the other hand, when an epoxy-based compound is used as the curing agent, it must be polyester polycarboxylic acid. In these cases, the coating layer becomes crosslinked, which has the advantage of improving heat resistance, abrasion resistance, and rigidity. On the other hand, there are problems with this method, such as the liquid not being reusable after mixing with the curing agent, and the need for a curing (aging) process after application.
[0083] When the polyester has hydroxyl groups, the polyisocyanate compound used in the present invention reacts at least partially to form a urethane structure, thereby becoming highly polar as a resin component and further enhancing the gas barrier function by causing aggregation between polymer chains. Furthermore, when the resin of the coating material is a linear resin, crosslinking with a trivalent or higher polyisocyanate can impart heat resistance and abrasion resistance. The polyisocyanate compound used in the present invention may be a diisocyanate, a trivalent or higher polyisocyanate, a low-molecular-weight compound, or a high-molecular-weight compound, but it is preferable to contain an aromatic ring or an aliphatic ring as part of the skeleton from the viewpoint of improving the gas barrier function. Examples of isocyanates having an aromatic ring include toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and naphthalene diisocyanate; examples of isocyanates having an aliphatic ring include hydrogenated xylylene diisocyanate, hydrogenated toluene diisocyanate, isophorone diisocyanate, and norbornane diisocyanate, as well as trimers of these isocyanate compounds, and compounds containing terminal isocyanate groups obtained by reacting an excess amount of these isocyanate compounds with low-molecular-weight active hydrogen compounds such as ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, ethylenediamine, monoethanolamine, diethanolamine, and triethanolamine, or high-molecular-weight active hydrogen compounds such as various polyester polyols, polyether polyols, and polyamides. The polyisocyanate compound may be an adduct, allophanate, or biuret. Among these, it is preferable to use a trimethylolpropane adduct of metaxylylene diisocyanate as the polyisocyanate compound.
[0084] The method for forming the anchor coat layer (C) is not particularly limited, and conventionally known methods such as coating methods can be used. Among coating methods, offline coating and in-line coating methods are preferred. For example, in the case of an in-line coating method carried out in the process of producing a substrate film, the conditions for drying and heat treatment during coating depend on the coat thickness and the conditions of the equipment, but it is preferable to feed the film to a stretching process in the perpendicular direction immediately after coating and dry it in the preheating zone or stretching zone of the stretching process. In such cases, it is usually preferable to use a temperature of about 50 to 250°C.
[0085] The method for applying the resin composition for the anchor coat layer (C) is not particularly limited as long as it is a method that can apply the resin composition to the surface of a film to form a layer. For example, conventional coating methods such as gravure coating, reverse roll coating, wire bar coating, and die coating can be used.
[0086] When forming the anchor coat layer (C), it is preferable to apply the resin composition for the anchor coat layer and then heat-dry it. The drying temperature is preferably 100 to 145°C, more preferably 110 to 140°C, and even more preferably 110 to 130°C. If the drying temperature is less than 100°C, the anchor coat layer may not be sufficiently dried. On the other hand, if the drying temperature exceeds 145°C, the film may be overheated, becoming brittle or shrinking, resulting in poor processability. In particular, volatilizing the solvent at a relatively low temperature of 80 to 110°C immediately after application and then drying at 120°C or higher is particularly preferable, as this results in a uniform film. In addition to drying, additional heat treatment at as low a temperature as possible is also more effective in promoting the formation of the anchor coat layer.
[0087] [Protective Layer (D)] In the present invention, a protective layer may be laminated on the gas barrier layer, or a protective layer (D) may be laminated on the inorganic thin film layer that is the gas barrier layer. An inorganic thin film layer made of a metal or metal oxide layer is not a completely dense film, but has minute defects scattered therein. By forming a protective layer by applying a specific resin composition for a protective layer (described below) onto a metal oxide layer, the resin in the resin composition for a protective layer penetrates into the defects in the metal oxide layer, resulting in the effect of stabilizing the barrier properties of the gas barrier layer. In addition, using a material with gas barrier properties for the protective layer itself also improves the gas barrier performance of the laminate film.
[0088] In the present invention, the amount of the protective layer (D) deposited is 0.10 to 0.40 g / m 2 It is preferable to set the density to 0.13 to 0.37 g / m 2 , and more preferably 0.16 to 0.34 g / m 2 , and even more preferably 0.19 to 0.31 g / m 2 This allows the protective layer to be uniformly controlled during coating, resulting in a film with fewer coating irregularities and defects. Furthermore, the cohesive force of the protective layer (D) itself is improved, and the adhesion between the inorganic thin film layer and the protective layer is also strengthened. The protective layer (D) deposition amount is 0.40 g / m 2 If the coating weight of the protective layer (D) exceeds 0.10 g / m, the gas barrier property is improved, but the cohesive force inside the protective layer becomes insufficient and the uniformity of the protective layer is also reduced, which may result in unevenness or defects in the coat appearance and insufficient gas barrier property and adhesiveness. 2 If it is less than this, there is a risk that sufficient gas barrier properties and interlayer adhesion may not be obtained.
[0089] The resin composition used for the protective layer (D) of the present invention can be a polyvinyl alcohol-based, urethane-based, polyester-based, acrylic-based, titanium-based, isocyanate-based, imine-based, polybutadiene-based resin, or the like, and a curing agent such as an epoxy-based, isocyanate-based, melamine-based, or silanol-based curing agent can be added. It can also contain a crosslinking agent such as a silicon-based crosslinking agent, an oxazoline compound, a carbodiimide compound, or an epoxy compound. In particular, the protective layer is preferably composed of a composition containing a polyvinyl alcohol-based resin and a silicon-based crosslinking agent. Examples of the polyvinyl alcohol-based resin and the silicon-based crosslinking agent include those similar to those described above.
[0090] The method for applying the resin composition for the protective layer is not particularly limited as long as it is a method that can apply the resin composition for the protective layer to the surface of a film to form a layer. For example, a conventional coating method such as gravure coating, reverse roll coating, wire bar coating, or die coating can be used.
[0091] When forming the protective layer (D), it is preferable to apply the protective layer resin composition and then heat-dry it. The drying temperature is preferably 100 to 160°C, more preferably 110 to 150°C, and even more preferably 120 to 140°C. Drying temperatures below 100°C can result in insufficient drying of the protective layer, or the formation of the protective layer cannot proceed, resulting in reduced cohesive strength and water-resistant adhesion, and consequently reduced barrier properties and hand-tearability. On the other hand, drying temperatures above 160°C can result in excessive heat being applied to the film, making it brittle and reducing puncture strength, or shrinking and reducing processability. It is particularly preferable to volatilize the solvent immediately after application of the protective layer at a relatively low temperature of 90 to 110°C, followed by drying at 130°C or higher, as this results in a uniform and transparent film. In addition to drying, additional heat treatment at as low a temperature as possible can be even more effective in promoting the formation of the protective layer.
[0092] [Other Films] In the present invention, the packaging material may contain other films in addition to the base film mainly composed of a polyolefin resin, as long as the monomaterial ratio described below is satisfied. The other films used in the present invention are, for example, films obtained by melt-extruding a plastic and, as necessary, stretching it in the longitudinal direction and / or the width direction, cooling, and heat setting. Examples of plastics include polyamides typified by nylon 4.6, nylon 6, nylon 6.6, and nylon 12, polyesters typified by polyethylene terephthalate, polybutylene terephthalate, and polyethylene-2,6-naphthalate, as well as polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene vinyl alcohol, wholly aromatic polyamide, polyamideimide, polyimide, polyetherimide, polysulfone, polystyrene, and polylactic acid.
[0093] The other films in the present invention can be of any thickness depending on the desired purpose, such as mechanical strength and transparency. The thickness of the other films is not particularly limited, but is usually recommended to be 5 to 250 μm, and when used as a packaging material, it is desirable to be 10 to 60 μm. However, it is necessary to take into consideration the mono-material ratio of the packaging material, which will be described later.
[0094] The other film in the present invention may be a laminated film of one or more types of plastic films. When a laminated film is used, the type of laminate, the number of layers, the lamination method, etc. are not particularly limited, and can be arbitrarily selected from known methods depending on the purpose.
[0095] [Heat-sealable film] The heat-sealable film of the present invention includes at least a laminate layer and a heat-sealable layer. The laminate layer and the heat-sealable layer will be described in detail below.
[0096] (Heat seal layer) The heat seal layer in the present invention is preferably made of a resin composition mainly composed of a mixture of polypropylene resin and polyethylene resin. Here, "main component" means that the mixture of polypropylene resin and polyethylene resin accounts for 90% by mass or more of the resin composition, more preferably 95% by mass or more, even more preferably 97% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass.
[0097] (Polypropylene-Based Resin) The polypropylene-based resin in the heat-seal layer is a resin containing propylene as a main component, and examples thereof include propylene homopolymers, propylene copolymers (propylene random copolymers, block copolymers) of propylene with an α-olefin such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1. The term "main component" means that propylene accounts for 90% by mass or more of the polypropylene resin, more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 99% by mass or more. Of these, the polypropylene-based resin constituting the heat-seal layer is preferably a propylene copolymer, more preferably a propylene-ethylene copolymer, a propylene-butene copolymer, or a propylene-ethylene-butene copolymer, even more preferably a propylene-ethylene-butene copolymer, and even more preferably a propylene-ethylene-butene random copolymer.
[0098] The melt flow rate of the polypropylene resin constituting the heat seal layer is preferably 0.1 g / 10 min to 9 g / 10 min, more preferably 0.5 g / 10 min to 8 g / 10 min, and even more preferably 1 g / 10 min to 7 g / 10 min. The melting point of the polypropylene resin constituting the heat seal layer is preferably 120 to 150°C, more preferably 125 to 150°C, and even more preferably 130 to 140°C. The polypropylene resin constituting the heat seal layer may have a predetermined flexural modulus. From the viewpoint of loop stiffness, the flexural modulus of the polypropylene resin is preferably 300 to 1500 MPa, more preferably 400 to 1200 MPa, and even more preferably 500 to 900 MPa. The flexural modulus is measured, for example, according to JIS K7171.
[0099] The polypropylene-based resin constituting the heat seal layer preferably contains 80 to 100% by mass of a propylene copolymer, more preferably 85 to 100% by mass, even more preferably 90 to 100% by mass, still more preferably 95 to 100% by mass, and particularly preferably 100% by mass.
[0100] From the viewpoint of loop stiffness, the content of the polypropylene-based resin constituting the heat seal layer is preferably 30 to 90 mass%, more preferably 35 to 85 mass%, and even more preferably 35 to 80 mass%, relative to 100 mass% of the resin composition constituting the heat seal layer.
[0101] (Polyethylene Resin) The polyethylene resin in the heat seal layer is preferably primarily composed of a linear low-density polyethylene resin (straight-chain low-density polyethylene resin). In addition to linear low-density polyethylene, at least one ethylene homopolymer selected from the group consisting of high-pressure low-density polyethylene, medium-density polyethylene, and high-density polyethylene can be used. Furthermore, random or block copolymers containing ethylene as the main component and copolymerized with other monomers such as α-olefins (e.g., propylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1), vinyl acetate, (meth)acrylic acid, and (meth)acrylic acid esters, or mixtures thereof, can also be used. These may be crystalline, low-crystalline, or amorphous.
[0102] The polyethylene resin constituting the heat seal layer has a melt flow rate (190°C, 2.16 kgf) of, for example, 0.1 to 9 g / 10 min, preferably 0.5 to 8 g / 10 min, more preferably 1 to 7 g / 10 min. The polyethylene resin constituting the heat seal layer has a melting point of, for example, 100 to 140°C, preferably 105 to 135°C, more preferably 110 to 130°C.
[0103] The polyethylene resin constituting the heat seal layer may have a predetermined flexural modulus, and the flexural modulus of the linear low-density polyethylene resin is preferably 200 MPa or less, more preferably 10 to 190 MPa, even more preferably 20 to 180 MPa, still more preferably 30 to 170 MPa, and particularly preferably 40 to 160 MPa. When the flexural modulus of the linear low-density polyethylene resin is within the above range, the seal strength can be increased.
[0104] The polyethylene resin constituting the heat seal layer preferably contains 90% by mass or more of a straight-chain linear polyethylene resin, more preferably 95% by mass or more, even more preferably 97% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass.
[0105] From the viewpoint of heat sealability, the content of the polyethylene resin constituting the heat seal layer is preferably 10 to 70 mass%, more preferably 15 to 65 mass%, and even more preferably 20 to 65 mass%, relative to 100 mass% of the resin composition constituting the heat seal layer.
[0106] From the viewpoint of improving both the heat sealability and the loop stiffness, the heat sealable film more preferably has a heat seal layer containing a linear low-density polyethylene resin and a propylene copolymer.
[0107] The polypropylene resin content is preferably 1 to 90% by mass, more preferably 5 to 90% by mass, relative to 100% by mass of the mixture of polypropylene resin and polyethylene resin constituting the heat seal layer. When the polypropylene resin content is 1% by mass or more, the rigidity is excellent. Furthermore, the polyethylene resin content is preferably 10 to 99% by mass, more preferably 20 to 90% by mass. When the polyethylene resin content is 10% by mass or more, the low-temperature sealability is excellent.
[0108] The difference in melting point between the polypropylene resin and polyethylene resin constituting the heat-seal layer is preferably 15 to 25°C, more preferably 16 to 25°C, even more preferably 17 to 25°C, even more preferably 18 to 25°C, and particularly preferably 19 to 25°C. When the difference in melting point between the polypropylene resin and polyethylene resin is 15°C or more, low-temperature sealability is improved, the polypropylene resin and polyethylene resin are well mixed, and variation in heat-seal strength is reduced. Furthermore, the arithmetic mean melting point of the polypropylene resin and polyethylene resin constituting the heat-seal layer is preferably 100 to 130°C, more preferably 112 to 130°C, even more preferably 115 to 130°C, even more preferably 116 to 130°C, and particularly preferably 121 to 130°C. If the arithmetic mean melting point of the polypropylene-based resin and polyethylene-based resin is 100°C or higher, the boiling suitability as a packaging material is improved, if it is 116°C or higher, the semi-retort suitability is improved, and if it is 121°C or higher, the high-retort suitability is improved.
[0109] (Anti-blocking agent) The resin composition in the heat seal layer may contain, as an anti-blocking agent, inorganic particles such as synthetic silica, diatomaceous earth, talc, or mica, or organic particles such as silicone particles, acrylic particles, nylon particles, or polyethylene particles (preferably ultra-high molecular weight polyethylene particles). Among these, the anti-blocking agent is preferably synthetic silica or ultra-high molecular weight polyethylene. The average particle size of the particles used in the present invention is preferably 2 to 20 μm, more preferably 3 to 15 μm, and even more preferably 5 to 10 μm.
[0110] The particle content of the resin composition in the heat seal layer is preferably 0.1 to 2% by mass, more preferably 0.3 to 1.5% by mass, and even more preferably 0.4 to 1.0% by mass, relative to the heat seal layer of the film. If the particle content is less than 0.1% by mass, it becomes difficult to achieve a surface roughness Ra of 0.1 μm or more on at least one surface layer, making it difficult to obtain anti-blocking properties and slip properties. Furthermore, if the particle content exceeds 2% by mass, the number of surface protrusions increases, resulting in poor appearance and poor abrasion resistance.
[0111] (Organic Lubricant) The resin composition in the heat seal layer preferably contains 0.01 to 2.0% by mass of an organic lubricant (preferably a fatty acid amide), more preferably 0.05 to 1.5% by mass, and particularly preferably 0.1 to 1.0% by mass. If the amount of organic lubricant is less than 0.01% by mass, blocking between films will be severe, resulting in unsatisfactory film handleability. If the amount of organic lubricant is 2.0% by mass or more, the seal strength will decrease. Examples of fatty acid amides include erucic acid amide, ethylene bisoleic acid amide, and behenic acid amide, and these may be used in combination. Note that, since sufficient bag-making suitability is achieved if the antiblocking agent and organic lubricant are contained on the outermost layer side of the packaging material, i.e., on the heat seal layer side, it is preferable from a cost perspective to contain them only in the heat seal layer.
[0112] The closer the melt flow rates of the resin compositions or raw resins constituting the heat seal layer, the better the appearance. The ratio of the melt flow rates of the raw resins mixed in the seal layer is preferably 0.5 to 2.0, more preferably 0.8 to 1.8, and even more preferably 1.0 to 1.6. When the melt flow rate ratio is within this range, poor appearance such as layer misalignment, blemishes, and unevenness is less likely to occur.
[0113] The heat-sealable film preferably includes an intermediate layer and a laminate layer in addition to the heat-sealable layer, and the heat-sealable layer, the intermediate layer, and the laminate layer are laminated in this order. The intermediate layer and the laminate layer preferably contain a propylene copolymer.
[0114] (Laminate Layer) The laminate layer in the present invention is preferably made of a resin composition mainly composed of a polypropylene resin. The term "main component" means that the proportion of polypropylene resin in the resin composition is 90% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, even more preferably 99% by mass or more, and particularly preferably 100% by mass. By making the laminate layer of a resin composition mainly composed of a polypropylene resin, the rigidity required to ensure firmness can be obtained. Loop stiffness evaluation as an index of firmness will be described later.
[0115] (Polypropylene-Based Resin) The polypropylene-based resin in the laminate layer is a resin containing propylene as the main component, and examples thereof include propylene homopolymers, propylene copolymers (preferably propylene random copolymers and block copolymers) of propylene with α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1. Among these, random copolymers and / or block copolymers of propylene with α-olefins such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1 are preferred. The term "main component" means that propylene accounts for 90% or more by mass of the polypropylene resin, with 95% or more being more preferred, 97% or more being even more preferred, and 99% or more being even more preferred. When propylene accounts for 90% or more by mass of the polypropylene resin, a film with excellent rigidity can be obtained. Among these, the polypropylene-based resin constituting the laminate layer is preferably a propylene copolymer, more preferably a propylene-ethylene copolymer, a propylene-butene copolymer, or a propylene-ethylene-butene copolymer, even more preferably a propylene-ethylene-butene copolymer, even more preferably a propylene-ethylene-butene random copolymer, and particularly preferably a propylene-ethylene-butene random copolymer.
[0116] The polypropylene resin constituting the laminate layer preferably has a melt flow rate (230°C, 2.16 kgf) of 0.1 g / 10 min to 9 g / 10 min, more preferably 0.5 g / 10 min to 8 g / 10 min, and even more preferably 1 g / 10 min to 7 g / 10 min. The polypropylene resin constituting the laminate layer preferably has a melting point (JIS K7121) of 120 to 160°C, more preferably 125 to 155°C, and even more preferably 130 to 150°C. The polypropylene resin constituting the laminate layer may have a predetermined flexural modulus, and from the viewpoint of loop stiffness, the flexural modulus of the polypropylene resin is preferably 400 to 1500 MPa, more preferably 500 to 1300 MPa, and even more preferably 600 to 1100 MPa.
[0117] The polypropylene-based resin constituting the laminate layer preferably contains 80 to 100% by mass of a propylene copolymer, more preferably 85 to 100% by mass, even more preferably 90 to 100% by mass, still more preferably 95 to 100% by mass, and particularly preferably 100% by mass.
[0118] From the viewpoint of loop stiffness, the content of the polypropylene resin constituting the laminate layer is preferably 50 to 100 mass%, more preferably 60 to 100 mass%, even more preferably 70 to 100 mass%, still more preferably 80 to 100 mass%, particularly preferably 90 to 100 mass%, and most preferably 100 mass%, relative to 100 mass% of the resin composition constituting the laminate layer.
[0119] In addition to polypropylene-based resins, the resin composition of the laminate layer can also include at least one ethylene homopolymer selected from the group consisting of high-pressure low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene. Furthermore, random or block copolymers containing ethylene as the main component and copolymerized with other monomers, such as α-olefins such as propylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1, vinyl acetate, (meth)acrylic acid, and (meth)acrylic acid esters, or mixtures thereof, can also be used. These may be crystalline, low-crystalline, or amorphous.
[0120] The melt flow rate (190°C, 2.16 kgf) of the polyethylene resin constituting the laminate layer is preferably 0.1 g / 10 min to 9 g / 10 min, more preferably 0.5 g / 10 min to 8 g / 10 min, and even more preferably 1 g / 10 min to 7 g / 10 min. The melting point (JIS K7121) of the polyethylene resin constituting the laminate layer is preferably 100 to 140°C, more preferably 105 to 135°C, and even more preferably 110 to 130°C. The melting point of the polyethylene resin may show two or more melting endothermic peaks, and the peak with the largest melting endothermic amount is defined as the main peak.
[0121] (Anti-blocking Agent) The resin composition in the laminate layer may contain, as an anti-blocking agent, inorganic particles such as synthetic silica, diatomaceous earth, talc, or mica, or organic particles such as silicone particles, acrylic particles, nylon particles, or polyethylene particles. The average particle size of the particles used in the present invention is preferably 2 to 20 μm, more preferably 3 to 15 μm, and even more preferably 5 to 10 μm.
[0122] The particle content of the resin composition in the laminate layer is preferably 0.1 to 2% by mass, more preferably 0.3 to 1.5% by mass, and even more preferably 0.4 to 1.0% by mass, relative to the seal layer of the film. If the particle content is less than 0.1% by mass, it becomes difficult to achieve a surface roughness Ra of 0.1 μm or more on at least one surface layer, making it difficult to obtain anti-blocking properties and slip properties. On the other hand, if the particle content exceeds 2% by mass, the number of protrusions on the surface increases, resulting in poor appearance and poor abrasion resistance.
[0123] (Organic Lubricant) The resin composition in the laminate layer preferably contains 0.01 to 2.0% by mass of an organic lubricant (preferably a fatty acid amide), more preferably 0.05 to 1.5% by mass, and particularly preferably 0.1 to 1.0% by mass. If the amount of organic lubricant is less than 0.01% by mass, blocking between films will be severe, resulting in unsatisfactory film handling. If the amount of organic lubricant is 2.0% by mass or more, the seal strength will decrease. Examples of fatty acid amides include erucic acid amide, ethylene bisoleic acid amide, and behenic acid amide, and these may be used in combination.
[0124] The closer the melt flow rates of the resin compositions or raw resins that make up the laminate layer, the better the appearance. The ratio of the melt flow rates of the raw resins mixed in the laminate layer is preferably 0.5 to 2.0, more preferably 0.8 to 1.8, and even more preferably 1.0 to 1.6. When the melt flow rate ratio is within this range, poor appearance such as layer misalignment, blemishes, and unevenness is less likely to occur.
[0125] (Intermediate layer) The heat-sealable film of the present invention may include an intermediate layer between the laminate layer and the seal layer. The intermediate layer in the present invention is preferably made of a resin composition mainly composed of a polypropylene resin. The term "main component" means that the proportion of the polypropylene resin in the resin composition is 90% by mass or more, more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 99% by mass or more.
[0126] (Polypropylene-Based Resin) The polypropylene-based resin in the intermediate layer is a resin containing propylene as a main component, and examples thereof include propylene homopolymers and propylene copolymers (preferably propylene random copolymers and block copolymers) of propylene and an α-olefin such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, or octene-1. Of these, random copolymers of propylene and an α-olefin such as ethylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, or octene-1 are preferred. Of these, the polypropylene-based resin constituting the laminate layer is more preferably a propylene-ethylene copolymer, a propylene-butene copolymer, or a propylene-ethylene-butene copolymer, even more preferably a propylene-ethylene-butene copolymer, and even more preferably a propylene-ethylene-butene random copolymer. The term "main component" means that propylene accounts for 90% by mass or more of the polypropylene resin, preferably 95% by mass or more, more preferably 97% by mass or more, and even more preferably 99% by mass or more.
[0127] The polypropylene resin constituting the intermediate layer preferably has a melt flow rate (230°C, 2.16 kgf) of 0.1 g / 10 min to 9 g / 10 min, more preferably 0.5 g / 10 min to 8 g / 10 min, and even more preferably 1 g / 10 min to 7 g / 10 min. The polypropylene resin constituting the intermediate layer preferably has a melting point of 120 to 160°C, more preferably 125 to 150°C, and even more preferably 130 to 140°C. The polypropylene resin constituting the intermediate layer may have a predetermined flexural modulus, and the flexural modulus of the polypropylene resin is preferably 300 to 1200 MPa, more preferably 400 to 1100 MPa, and even more preferably 500 to 1000 MPa.
[0128] The polypropylene-based resin constituting the intermediate layer preferably contains 80 to 100 mass %, more preferably 85 to 100 mass %, even more preferably 90 to 100 mass %, still more preferably 95 to 100 mass %, and particularly preferably 100 mass % of a propylene copolymer.
[0129] The content of the polypropylene resin constituting the intermediate layer is preferably 50 to 100 mass%, more preferably 60 to 100 mass%, even more preferably 70 to 100 mass%, still more preferably 80 to 100 mass%, particularly preferably 90 to 100 mass%, and most preferably 100 mass%, based on 100 mass% of the resin composition constituting the intermediate layer.
[0130] In addition to polypropylene-based resins, the resin composition for the intermediate layer can be, for example, at least one ethylene homopolymer selected from the group consisting of high-pressure low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, and high-density polyethylene. Furthermore, random or block copolymers containing ethylene as the main component and copolymerized with other monomers such as α-olefins such as propylene, butene-1, pentene-1, hexene-1, 3-methylbutene-1, 4-methylpentene-1, and octene-1, vinyl acetate, (meth)acrylic acid, and (meth)acrylic acid esters, or mixtures thereof, can also be used. These may be crystalline, low-crystalline, or amorphous.
[0131] The polyethylene resin constituting the intermediate layer preferably has a melt flow rate (190°C, 2.16 kgf) of 0.1 g / 10 min to 9 g / 10 min, more preferably 0.5 g / 10 min to 8 g / 10 min, and even more preferably 1 g / 10 min to 7 g / 10 min. The polyethylene resin constituting the intermediate layer preferably has a melting point of 100 to 140°C, more preferably 105 to 135°C, and even more preferably 110 to 130°C.
[0132] (Anti-blocking Agent) The resin composition in the intermediate layer may contain an anti-blocking agent used in the seal layer or laminate layer.
[0133] (Organic Lubricant) The resin composition in the intermediate layer may contain an organic lubricant used in the seal layer or laminate layer.
[0134] The closer the melt flow rates of the resin composition or raw resins constituting the intermediate layer, the better the appearance. The ratio of the melt flow rates of the raw resins mixed in the seal layer is preferably 0.5 to 2.0, more preferably 0.8 to 1.8, and even more preferably 1.0 to 1.6. When the melt flow rate ratio is within this range, poor appearance such as layer misalignment, blemishes, and unevenness is less likely to occur.
[0135] (Layer Structure) The layer structure of the heat-sealable film of the present invention may be laminate layer / heat-seal layer, laminate layer / intermediate layer / heat-seal layer, or laminate layer / intermediate layer 1 / intermediate layer 2 / heat-seal layer. An intermediate layer is preferably provided between the laminate layer and the heat-seal layer, as this reduces peeling between the laminate layer and the heat-seal layer and facilitates the use of recycled raw materials. The raw material composition of the intermediate layer is preferably intermediate between the laminate layer and the heat-seal layer to reduce peeling between the laminate layer and the heat-seal layer. The thickness of the heat-sealable film is, for example, 5 to 100 μm, preferably 10 to 80 μm, and more preferably 20 to 60 μm. The thickness of the laminate layer and the heat-seal layer is, for example, 1 to 30 μm, preferably 2 to 15 μm, and more preferably 3 to 10 μm. The thickness of the intermediate layer is, for example, 5 to 50 μm, preferably 7 to 40 μm, and more preferably 9 to 30 μm.
[0136] The greater the difference in melt flow rates between the raw resins of adjacent layers and / or the greater the difference in melt flow rates between the raw resins mixed in each layer, the more defective the appearance becomes. The ratio of the melt flow rates of the raw resins of adjacent layers is preferably 0.5 to 2.0. A melt flow rate ratio within this range is less likely to cause poor appearance, such as layer misalignment, blemishes, or unevenness. Furthermore, the main peak of the melting point of the heat-sealable film of the present invention is preferably 121°C or higher, more preferably 130°C or higher, even more preferably 140°C or higher, even more preferably 150°C or higher, and particularly preferably 160°C or higher. When the main peak of the melting point of the heat-sealable film is 121°C or higher, the high retort suitability is further improved.
[0137] (Method for producing heat-sealable film) The method for producing the heat-sealable film of the present invention will be described in detail below, but is not limited thereto. The resin composition of the laminate layer and the heat-sealable layer may be prepared by blending the above-mentioned resin raw materials and, if necessary, various additives in a mixer such as a Henschel mixer, a Banbury mixer, or a tumbler mixer, and then pelletizing the mixture using a single- or twin-screw extruder before molding into a film. Alternatively, the components may be blended together and fed to a film molding machine.
[0138] (Melt Extrusion Process) The mixed resin composition is melted, for example, at a resin temperature of 110 to 300°C, melt-extruded into a sheet from, for example, a T-die, cast onto a chill roll, and cooled and solidified to obtain an unstretched sheet. A preferred specific method for this is casting onto a chill roll. Multilayering can be achieved using a multilayering device such as a multilayer feed block, a static mixer, or a multi-manifold die. For example, resins delivered from different flow paths using two or more extruders are laminated into multiple layers using a multilayer feed block or a multi-manifold die. Examples of methods include melt-extruding a melt-kneaded laminated resin composition sheet and forming it into a film using a T-die method or an inflation method. However, the T-die method is particularly preferred because it allows for a high resin melt temperature.
[0139] (Cooling and Solidification Process) For example, a sheet melt-extruded from a T-die is preferably cast onto a chill roll and cooled. The chill roll temperature is preferably 10 to 70°C. Temperatures below this range are undesirable, as not only may the crystallization-suppressing effect saturate, but also may cause problems such as condensation. Temperatures above this range are undesirable, as crystallization progresses and transparency deteriorates. Furthermore, when the chill roll temperature is within the above range, it is preferable to reduce the humidity of the environment near the chill roll to prevent condensation. During casting, the surface temperature of the chill roll rises due to contact of the hot resin with the surface. Typically, chill rolls are cooled by flowing cooling water through piping inside. However, it is necessary to minimize the temperature difference across the width of the chill roll surface by ensuring a sufficient amount of cooling water, optimizing the piping arrangement, and performing maintenance to prevent sludge from adhering to the piping. In this case, the thickness of the unstretched sheet is preferably in the range of 3 to 130 μm. The thickness of the film is preferably in the range of 5 to 125 μm, more preferably 10 to 120 μm. When the film thickness is 3 μm or more, the film can have the rigidity necessary to ensure firmness, and when it is 130 μm or less, the film is not too firm and is easy to process, and a suitable package can be easily produced.
[0140] [Adhesive Layer] In the packaging material of the present invention, the substrate film and the heat-sealable film can be laminated by a dry lamination method using an adhesive. The adhesive layer used in the present invention can be a general-purpose laminating adhesive. For example, (solvent-free), aqueous, or hot-melt adhesives containing poly(ester)urethane, polyester, polyamide, epoxy, poly(meth)acrylic, polyethyleneimine, ethylene-(meth)acrylic acid, polyvinyl acetate, (modified) polyolefin, polybutadiene, wax, or casein as the main component can be used. Among these, urethane or polyester adhesives are preferred in terms of heat resistance and flexibility that can adapt to dimensional changes in each substrate. The adhesive layer can be applied by, for example, direct gravure coating, reverse gravure coating, kiss coating, die coating, roll coating, dip coating, knife coating, spray coating, fountain coating, or other methods. To achieve sufficient adhesion, a coating weight after drying of 1 to 8 g / m is required. 2 is preferable, and more preferably 2 to 7 g / m 2 , more preferably 3 to 6 g / m 2 The coating amount is 1 g / m 2 If the thickness is less than 8 g / m, it becomes difficult to bond the entire surface, and the adhesive strength decreases. 2 If the thickness exceeds 100 μm, it takes a long time for the film to completely cure, unreacted material is likely to remain, and adhesive strength decreases. The thickness of the adhesive layer is, for example, 0.1 to 10 μm, preferably 0.5 to 7 μm, and more preferably 1 to 5 μm.
[0141] [Printed Layer] Furthermore, in the packaging material of the present invention, at least one printed layer may be laminated between the base film layer and the heat-sealable film or on the outer side thereof.
[0142] As the printing ink for forming the printing layer, aqueous and solvent-based resin-containing printing inks are preferably used. Examples of resins used in printing inks include acrylic resins, urethane resins, polyester resins, vinyl chloride resins, vinyl acetate copolymer resins, and mixtures thereof. The printing ink may contain known additives such as antistatic agents, light-blocking agents, ultraviolet absorbers, plasticizers, lubricants, fillers, colorants, stabilizers, lubricants, defoamers, crosslinking agents, anti-blocking agents, and antioxidants. The printing method for forming the printing layer is not particularly limited, and known printing methods such as offset printing, gravure printing, and screen printing can be used. To dry the solvent after printing, known drying methods such as hot air drying, heat roll drying, and infrared drying can be used.
[0143] [Characteristics of Packaging Material] The packaging material of the present invention can have any laminate structure. From the viewpoint of environmental impact, a structure in which one substrate film having a barrier layer and a heat-sealable film are laminated together is preferred, as it requires the fewest materials and the fewest number of lamination steps. On the other hand, as mentioned above, from the viewpoint of improving toughness and gas barrier performance, a laminate in which, for example, a film having a gas barrier layer is sandwiched between a substrate film not having a gas barrier layer and a thermoplastic copolymer having a heat-sealable film is also cited as a preferred structure. In this case, by laminating a printing layer on the front-side substrate film, there is also the advantage that it is not necessary to print on the film having a gas barrier layer. Other suitable structures include laminating the material with a white substrate film or heat-sealable film to improve concealing properties, or laminating it with an ultraviolet-blocking film to provide light-blocking properties.
[0144] The packaging material of the present invention may include a coating layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, an inorganic thin film layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, an inorganic thin film layer / anchor coat layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, a protective layer / inorganic thin film layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, a protective layer / inorganic thin film layer / anchor coat layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, a coating layer / surface layer / substrate layer / surface layer / adhesive layer /
[0043] The preferred configurations are inorganic thin film layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, coating layer / surface layer / substrate layer / surface layer / adhesive layer / inorganic thin film layer / anchor coat layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, inorganic thin film layer / surface layer / substrate layer / surface layer / adhesive layer / inorganic thin film layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, inorganic thin film layer / surface layer / substrate layer / surface layer / adhesive layer / inorganic thin film layer / anchor coat layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, inorganic thin film layer / surface layer / substrate layer / surface layer / adhesive layer / inorganic thin film layer / anchor coat layer / surface layer / substrate layer / surface layer / adhesive layer / laminate layer / intermediate layer / heat seal layer, and the like.
[0145] The packaging material of the present invention must have a seal strength of 10 N / 15 mm or more in the MD or TD direction when heat-sealed at 120°C, 0.1 MPa, and 1 second. Having a heat seal strength within the above range at a low heat seal temperature of 120°C can improve bag-making processability. The heat seal strength is preferably 10 N / 15 mm to 40 N / 15 mm, more preferably 12 N / 15 mm to 35 N / 15 mm, even more preferably 14 N / 15 mm to 30 N / 15 mm, and particularly preferably 15 N / 15 mm to 30 N / 15 mm. For general packaging bags, etc., where the mass of the contents is large and a relatively high heat seal strength is required, a heat seal strength of 15 N / 15 mm or more is required. Details of the heat seal strength measurement method are provided in the Examples below, but it can be measured, for example, based on JIS Z1707.
[0146] In the present invention, the heat sealing temperature is preferably 60 to 180° C., more preferably 70 to 170° C., and even more preferably 80 to 160° C. The lower limit of the heat sealing temperature is preferably 20° C. or more lower than the lowest melting point of the polyethylene resin and / or polypropylene resin in the seal layer of the heat-sealable film, and the upper limit is preferably 10° C. or more higher than the highest melting point of the polyethylene resin and / or polypropylene resin in the laminate layer.
[0147] The packaging material of the present invention preferably has an excellent appearance after heat sealing. Specifically, it is preferable that the sealed portion does not wrinkle and the bag does not distort. In order to maintain the appearance after sealing, it is possible to set the difference in melting point between the polyethylene-based resin and the polypropylene-based resin in the seal layer of the heat-sealable film within the above-mentioned specified range.
[0148] The packaging material of the present invention must have a loop stiffness value of 22 mN / 25 mm or more. Loop stiffness refers to the resilience of a loop measured when a film cut into strips of predetermined dimensions is formed and the loop is crushed by a predetermined amount in the radial direction, and is an index of the film's rigidity. By setting the loop stiffness value within the above range, it is possible to ensure, for example, the firmness required during bag manufacturing. The loop stiffness value is preferably 23 mN / 25 mm to 800 mN / 25 mm, more preferably 25 mN / 25 mm to 750 mN / 25 mm, and even more preferably 27 mN / 25 mm to 700 mN / 25 mm. If the loop stiffness value is less than 22 mN / 25 mm, sufficient firmness may not be obtained during bag manufacturing, resulting in a poor finish. If the loop stiffness value is greater than 800 mN / 25 mm, the firmness may be too strong, making bag manufacturing difficult. Details of the method for measuring loop stiffness are provided in the Examples below, but it may be measured, for example, using a loop stiffness tester. The loop stiffness value can be achieved by adjusting the type and thickness of the polypropylene-based resin and polyethylene-based resin in the laminate layer and seal layer that make up the heat-sealable film. However, care must be taken because increasing the thickness is undesirable from the perspective of volume reduction and leads to increased costs. Regarding the relationship between loop stiffness and thickness, for example, the value of (loop stiffness value) / (total thickness) is preferably 0.10 to 8.00, more preferably 0.15 to 7.50, even more preferably 0.20 to 7.00, even more preferably 0.50 to 3.0, and particularly preferably 0.53 to 2.0.
[0149] The packaging material of the present invention has an oxygen transmission rate of 60 ml / m under conditions of 23°C x 65% RH. 2 In order to achieve good gas barrier properties, it is preferable that the gas barrier strength is 0.5 to 50 ml / m. 2 d MPa, more preferably 1.0 to 40 ml / m 2 d MPa, more preferably 1.5 to 35 ml / m 2・d・MPa. Oxygen permeability is 60 ml / m 2 If the pressure exceeds 0.5 MPa, it becomes difficult to use the film in applications that require high gas barrier properties. 2 If the pressure is less than d MPa, the barrier performance will be excellent, but the residual solvent will be less likely to permeate to the outside of the bag, which is undesirable because there is a risk that the amount of oxygen transferred to the contents will increase relatively. The oxygen permeability is measured, for example, based on JIS K7126B.
[0150] The packaging material of the present invention has a water vapor permeability of 3.0 g / m under conditions of 40°C x 90% RH. 2 In order to achieve good gas barrier properties, it is preferable that the thickness is 0.1 to 2.5 g / m or less. Furthermore, by providing a barrier layer on each film, it is possible to obtain a thickness of 0.1 to 2.5 g / m. 2 d, more preferably 0.2 to 2.0 g / m 2 ・d. The water vapor permeability is 3.0 g / m 2 If the value of d exceeds 0.1 g / m, it becomes difficult to use the film in applications that require high gas barrier properties. 2 If the water vapor permeability is less than 100%, the barrier performance will be excellent, but the residual solvent will be less likely to permeate to the outside of the bag, which is undesirable because there is a risk that the amount of water vapor that migrates to the contents will relatively increase. The water vapor permeability is measured, for example, in accordance with JIS K7129B.
[0151] As an evaluation criterion for the mono-material nature of the packaging material of the present invention, when the ratio of the thickness of the polyolefin-based material to the total thickness of each film and adhesive is calculated as the mono-material (mono-mate) ratio, the mono-material ratio is preferably 70% or more, more preferably 80% or more, and even more preferably 90% or more. By setting the mono-material ratio within this range, a packaging material configuration that is easy to recycle can be achieved. If the mono-material ratio is less than 70%, recycling may be difficult due to foreign matter from other materials. As mentioned above, it is preferable to use a polypropylene-based resin as the polyolefin-based resin that constitutes the base film, but using a polypropylene-based resin in the heat-sealable film can also make the configuration easier to recycle. If all the polyolefin-based materials used are polypropylene-based resins, the configuration can be made even easier to recycle.
[0152] In the present invention, the total thickness of the packaging material (each film and adhesive) is, for example, 140 μm or less, preferably 20 to 140 μm, more preferably 25 to 135 μm, and even more preferably 30 to 130 μm. By setting the total thickness of the packaging material within this range, a package can be obtained that exhibits the necessary physical properties, such as firmness, toughness, and barrier performance, required for the packaging material. If the total thickness is less than 20 μm, the bag will not have enough firmness and will not stand on its own. On the other hand, if the total thickness exceeds 140 μm, a high heat-sealing temperature is required to exhibit sufficient heat-sealing strength, which may result in poor appearance such as wrinkles and distortion. Furthermore, this increases the cost of the package, which is economically undesirable.
[0153] As described above, the packaging material of the present invention has excellent gas barrier properties, heat sealing properties, firmness, and visibility, and can be used as various types of packaging. In particular, the packaging material of the present invention is preferably used for heating in a microwave oven. When the packaging material of the present invention is heated in a microwave oven, the film surface remains unchanged and no wrinkles or the like are formed.
[0154] The form of the package using the packaging material of the present invention is not particularly limited and can take various forms, such as a three-sided or four-sided pouch, a standing pouch, a spout pouch, etc.
[0155] The present invention also encompasses a package in which an item to be packaged is packaged in a packaging material. The contents filled in a packaging bag using the packaging material of the present invention are not particularly limited, and may be liquid, powder, or gel. The contents may also be food or non-food.
[0156] This application claims the benefit of priority based on Japanese Patent Application No. 2023-090244, filed on May 31, 2023. The entire contents of the specification of Japanese Patent Application No. 2023-090244, filed on May 31, 2023, are incorporated herein by reference.
[0157] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples. Various evaluations were carried out by the following measurement methods.
[0158] (1) Thickness of Various Films The thickness was measured using a dial gauge in accordance with JIS K7130-1999 Method A.
[0159] (2) Mesopentad fraction ([mmmm] unit: %) The mesopentad fraction was measured by 13 The mesopentad fraction was calculated according to the method described in "Zambelli et al., Macromolecules, Vol. 6, p. 925 (1973)". 13 C-NMR measurement was performed using an AVANCE 500 manufactured by BRUKER at 110°C by dissolving 200 mg of a sample in a mixed solution of o-dichlorobenzene and deuterated benzene at a volume ratio of 8:2 at 135°C.
[0160] (3) Melt flow rate ([MFR] g / 10 min) Measured in accordance with JIS K7210 at a temperature of 230°C and a load of 2.16 kgf. In the case of raw resin, the required amount of pellets (powder) was weighed out and used. In the case of film, the required amount was cut out and then cut into approximately 5 mm square samples.
[0161] (4) Molecular Weight and Molecular Weight Distribution The molecular weight and molecular weight distribution of the raw resin and film were determined using gel permeation chromatography (GPC) with monodisperse polystyrene as the standard. The measurement conditions for the column, solvent, etc. used in the GPC measurement are as follows: Solvent: 1,2,4-trichlorobenzene Column: TSKgel GMHHR-H(20)HT x 3 Flow rate: 1.0 ml / min Detector: RI Measurement temperature: 140°C
[0162] The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) are defined by the following equations, where Mn is the molecular weight (Mi) at each elution position of the GPC curve obtained via the molecular weight calibration curve, and Ni is the number of molecules. Number average molecular weight: Mn = Σ(Ni·Mi) / ΣNi Weight average molecular weight: Mw = Σ(Ni·Mi) 2 ) / Σ(Ni·Mi) Molecular weight distribution: Mw / Mn When the baseline was unclear, the baseline was set in the range up to the lowest point of the high molecular weight base of the elution peak on the high molecular weight side closest to the elution peak of the standard substance.
[0163] (5) Melting Peak Temperature (°C) and Melting Peak Area (J / g) Measurements were performed using a differential scanning calorimeter (DSC) manufactured by SII, with a sample weight of 10 mg and a heating rate of 20°C / min. The melting endothermic peak temperature and the melting peak area were determined from the DSC curve.
[0164] (6) Composition and Thickness of Inorganic Thin Film Layer (B) on Substrate Film The laminate films (after thin film lamination) obtained in Examples and Comparative Examples were measured for thickness composition using a fluorescent X-ray analyzer (Rigaku Corporation, "Supermini 200") based on a pre-prepared calibration curve. The excitation X-ray tube conditions were 50 kV and 4.0 mA.
[0165] (7) Amount of adhesion of coating layer (A), anchor coat layer (C), and protective layer (D) on substrate film In each example and comparative example, each laminated film obtained at the stage where a predetermined coating layer (A), anchor coat layer (C), and protective layer (D) were laminated on a substrate film was used as a sample, and a test piece of 100 mm x 100 mm was cut out from this sample, and the coating layer was wiped off with either water, ethanol, or acetone, and the amount of adhesion was calculated from the change in mass of the film before and after wiping.
[0166] [Preparation of packaging material] (8) Preparation of packaging material for evaluation When there was one substrate film, a polyurethane adhesive (TM569 / cat 10L manufactured by Toyo-Morton Co., Ltd.) was applied to the gas barrier layer side of the substrate film described in the Examples and Comparative Examples so that the thickness after drying at 80°C would be 3 μm, and then various heat-sealable films described below were dry-laminated on a metal roll heated to 60°C, and aging was performed at 40°C for 2 days (48 hours) to obtain a packaging material that was a laminate for evaluation. On the other hand, when there were two substrate films, a polyurethane adhesive (TM569 / cat 10L manufactured by Toyo-Morton Co., Ltd.) was applied to the substrate film described in the Examples and Comparative Examples so that the thickness after drying at 80°C would be 3 μm, and then another substrate film was dry-laminated on a metal roll heated to 60°C to form a take-up roll. The same adhesive was applied to this roll so that the thickness after drying at 80°C would be 3 μm, and then a heat-sealable film described below was dry-laminated on a metal roll heated to 60°C, and aging was carried out at 40°C for 2 days (48 hours) to obtain a packaging material for evaluation.
[0167] (9) Evaluation method for oxygen transmission rate (OTR) of packaging material The oxygen transmission rate of the packaging material prepared in (4) above was measured in accordance with JIS-K7126 Method B using an oxygen transmission rate measuring device (OX-TRAN (registered trademark) 2 / 22 manufactured by MOCON Corporation) under an atmosphere of a temperature of 23°C and a humidity of 65% RH. The measurement of oxygen transmission rate was carried out in the direction in which oxygen permeated from the base film side of the packaging material to the heat-sealable film side.
[0168] (10) Method for evaluating water vapor transmission rate (WVTR) of packaging material The water vapor transmission rate of the packaging material prepared in (4) above was measured in accordance with JIS-K7129 Method B using a water vapor transmission rate measuring device ("PERMATRAN-W 3 / 33MG" manufactured by MOCON) under an atmosphere of a temperature of 40°C and a humidity of 90% RH. The water vapor transmission rate was measured in the direction in which water vapor permeated from the base film side of the packaging material to the heat-sealable film side.
[0169] (11) Method for Evaluating Heat-Seal Strength of Packaging Materials The heat-seal strength of the packaging materials prepared in (8) above was measured in accordance with JIS Z1707. The specific procedure is as follows: Using a heat sealer (semi-automatic mouthpiece sealing machine, manufactured by Seibu Kikai Co., Ltd., TYB-300), the heat-sealed surfaces of the samples were bonded perpendicular to the MD direction. The heat-sealing conditions were an upper bar temperature of 120°C, a lower bar temperature of 30°C, a pressure of 0.1 MPa, and a time of 1 second. The bonded samples were cut to a seal width of 15 mm. Peel strength was measured in the MD direction at a tensile speed of 200 mm / min using a universal tensile tester "DSS-100" (manufactured by Shimadzu Corporation). The heat-seal strength was expressed as the strength per 15 mm (N / 15 mm). A total of three measurements were performed, and the average value was taken as the heat-seal strength. The appearance of the seal (finish) was evaluated relatively as follows: ◯: seal without wrinkles, △: partial wrinkles, and ×: wrinkles over the entire surface.
[0170] (12) Loop Stiffness of Packaging Material The loop stiffness of the packaging material prepared in (8) above was measured. A strip of film measuring 25 mm wide and 110 mm long was cut out, and the longitudinal direction of the strip of film was aligned with the direction of the object being measured. The cut strip of film was set in a loop stiffness tester manufactured by Toyo Seiki Seisakusho, and the repulsive force was measured. The measurement frequency was 50 Hz. The repulsive force value (mN / 25 mm) obtained by the measurement was taken as the loop stiffness value.
[0171] (13) Evaluation Criteria for Mono-Materialization: Mono-Material Ratio For the packaging materials prepared in (8) above, the ratio of the thickness of the olefin-based material to the total thickness of each film and adhesive was calculated as the mono-material ratio as the evaluation criterion for mono-materialization.
[0172] (14) Evaluation Criteria for Visibility and Microwave Suitability Regarding the packaging materials prepared in (8) above, the evaluation criteria for visibility and microwave suitability were rated as ◯ when the packaging was transparent and did not use aluminum foil or aluminum vapor deposition for the barrier layer.
[0173] The substrate films used in the present examples and comparative examples are described below. [Preparation of substrate films] Details of the polypropylene-based resin raw materials used in the preparation of polyolefin substrate films OPP-1 to OPP-6, the film forming conditions, and the raw material blending ratios are shown in Tables 1 to 4.
[0174]
[0175]
[0176]
[0177]
[0178] (OPP-1) For the base layer (A), a blend of 30 mass% of a propylene homopolymer having Mn=81,000, Mw=320,000, MFR=2.2 g / 10 min, and mesopentad fraction [mmmm]=99.2% (PP "FS2012" manufactured by Sumitomo Chemical Co., Ltd.: copolymerization monomer amount: 0.0 mol%; hereinafter abbreviated as "PP-2") and 70 mass% of a propylene homopolymer having Mn=65,000, Mw=240,000, MFR=7.5 g / 10 min, and mesopentad fraction [mmmm]=98.9% (PP "FLX80E4" manufactured by Sumitomo Chemical Co., Ltd.: copolymerization monomer amount: 0.0 mol%; hereinafter abbreviated as "PP-3") shown in Table 1 was used. For the surface layer (B), a mixture of 24.8 mass% of a propylene polymer having Mn=55,000, Mw=300,000, MFR=5.6 g / 10 min, and mesopentad fraction [mmmm]=98.4% (Novatec (registered trademark) PP "FL4" manufactured by Japan Polypropylene Corporation, abbreviated as "PP-5"), 72.2 mass% of a propylene polymer having Mn=59,000, Mw=310,000, MFR=5.3 g / 10 min, and mesopentad fraction [mmmm]=93.8% (Prime Polypropylene "F300SP" manufactured by Prime Polymer Co., Ltd., abbreviated as "PP-6"), and 3.0 mass% of the masterbatch A shown in Table 2 was used. The base layer (A) was extruded using a 45 mm extruder, the surface layer (B) using a 25 mm extruder, and the second surface layer (B) (surface layer (C)) using a 20 mm extruder. The raw resins were melted at 250 ° C. and co-extruded into a sheet from a T-die. The surface layer (B) was cooled and solidified so that it came into contact with a 40 ° C. cooling roll, and then stretched 4.5 times in the machine direction (MD) at 125 ° C. Next, in a tenter, both ends of the film width direction (TD) were clamped with clips, preheated at 167 ° C., stretched 8.2 times in the width direction (TD) at 163 ° C., and then heat-set at 169 ° C. while relaxing 6.7% in the width direction (TD). The film formation conditions at this time were designated film formation conditions a. In this way, a biaxially oriented polypropylene film having a configuration of surface layer (B) / base layer (A) / second surface layer (B) (surface layer (C)) was obtained.The surface of the surface layer (B) of the biaxially oriented polypropylene film was subjected to corona treatment using a corona treatment machine manufactured by Softal Corona & Plasma GmbH under the condition of an applied current value of 0.75 A, and then wound up with a winder. The thickness of the obtained film was 20 μm (thickness of surface layer (B) / base layer (A) / second surface layer (B) was 1.0 μm / 18.0 μm / 1.0 μm). Details of this configuration are shown in Table 4.
[0179] (OPP-2) A 20 μm biaxially oriented polypropylene film was obtained under the same conditions as OPP-1, except that the base layer (A) was made of 100% by mass of a propylene homopolymer (PP "FL203D" manufactured by Japan Polypropylene Corporation; copolymerization monomer amount: 0.0 mol%; hereafter abbreviated as "PP-1") having Mn=56,000, Mw=310,000, MFR=2.5 g / 10 min, and mesopentad fraction [mmmm]=94.8% as shown in Table 1, and the surface layer (B) was made of a blend of 95.2% by mass of PP-1 and 4.8% by mass of masterbatch B, and the film was formed under the conditions of b in Table 3. Details of this configuration are shown in Table 4.
[0180] (OPP-3) The surface layer (C) was prepared by blending 52.0% by mass of a propylene-ethylene copolymer (Wintec (registered trademark) PP "WFX4M" manufactured by Japan Polypropylene Corporation, abbreviated as "PP-4") having Mn = 80,000, Mw = 220,000, and MFR = 7.0 g / 10 min shown in Table 1, 45.0% by mass of PP-6, and 3.0% by mass of Masterbatch A shown in Table 2. Furthermore, a 20 μm biaxially oriented polypropylene film was obtained under the same conditions as OPP-1, except that the surface of the surface layer (C) of the biaxially oriented polypropylene film was subjected to a corona treatment using a corona treater manufactured by Softal Corona & Plasma GmbH at an applied current of 0.75 A. Details of this configuration are shown in Table 4.
[0181] (Other substrate films) (Vapor-deposited PET) Transparent vapor-deposited polyester film ("VE707-12 μm" manufactured by Toyobo Co., Ltd.) (NY) Biaxially oriented polyamide film ("N1100-15 μm" manufactured by Toyobo Co., Ltd.)
[0182] (Coating Layer (A)) Details of the coating liquid for forming the coating layer (A) used in the examples and comparative examples are described below.
[0183] [Polyvinyl alcohol resin (a)] 10 parts by mass of a fully saponified polyvinyl alcohol resin (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name: G Polymer OKS8049Q (saponification degree 99.0% or more, average polymerization degree 450)) was added to 90 parts by mass of purified water, and the mixture was heated to 80°C with stirring and then stirred for about 1 hour. The mixture was then cooled to room temperature, thereby obtaining a nearly transparent polyvinyl alcohol solution (PVA solution) with a solids content of 10%.
[0184] [Inorganic layered compound dispersion (b)] 5 parts by mass of montmorillonite (trade name: Kunipia F, manufactured by Kunimine Industries Co., Ltd.), an inorganic layered compound, was added to 95 parts by mass of purified water with stirring, and the mixture was thoroughly dispersed using a homogenizer at a setting of 1500 rpm. Thereafter, the mixture was kept at 23°C for 1 day to obtain an inorganic layered compound dispersion having a solid content of 5%.
[0185] [Coating Liquid 1 Used for Coating Layer 1] A coating liquid (resin composition for coating layer) was prepared by mixing the materials in the following blending ratio: Ion-exchanged water 15.00% by mass, Isopropyl alcohol 15.00% by mass, Polyvinyl alcohol resin (a) 30.00% by mass, Inorganic layer compound dispersion (b) 40.00% by mass.
[0186] [Coating Liquid 2 Used for Coating Layer 2] A coating liquid (resin composition for coating layer) was prepared by mixing the materials in the following blending ratio: Ion-exchanged water 15.00% by mass, Isopropyl alcohol 15.00% by mass, Polyvinyl alcohol resin (a) 70.00% by mass.
[0187] (Coating of the coating liquid onto a film (lamination of a coating layer)) The coating liquid prepared above was applied onto the corona-treated surface of a substrate film by gravure roll coating, pre-dried at 90°C for 4 seconds, and then fully dried at 120°C for 4 seconds to obtain a coating layer. The coating layer adhesion amount at this time was 0.30 g / m 2Thereafter, a post-heat treatment was carried out at 40° C. for 2 days (48 hours). In this manner, a laminated film having either the coating layer 1 or 2 was prepared.
[0188] (Inorganic Thin Film Layer (B)) The method for producing the inorganic thin film layer (B) used in each example and comparative example is described below. (Formation of Inorganic Thin Film Layer 1) As inorganic thin film layer 1 (vapor deposition 1), a complex oxide layer of silicon dioxide and aluminum oxide was formed on a substrate film or anchor coat layer by electron beam vapor deposition. Particulate SiO2 (purity 99.9%) and Al2O3 (purity 99.9%) measuring approximately 3 mm to 5 mm were used as the vapor deposition source. The thickness of the inorganic thin film layer (SiO2 / Al2O3 complex oxide layer) in the inorganic thin film layer / substrate film thus obtained was 13 nm. The composition of this complex oxide layer was SiO2 / Al2O3 (mass ratio) = 70 / 30.
[0189] (Formation of Inorganic Thin Film Layer 2) As the inorganic thin film layer 2 (deposition 2), silicon oxide was deposited on the substrate film or the anchor coat layer. -3 After reducing the pressure to below 1 Pa, silicon oxide was placed in a Nilaco evaporation source B-110 from below the substrate and evaporated by heating to form a silicon oxide film with a thickness of 30 nm on the substrate film.
[0190] (Formation of Inorganic Thin Film Layer 3) As the inorganic thin film layer 3 (deposition 3), metallic aluminum was deposited on the substrate film or the anchor coat layer. -3 After reducing the pressure to below 1 Pa, aluminum foil with a purity of 99.9% was placed in a Nilaco evaporation source CF-305W from below the substrate, and metallic aluminum was heated and evaporated to form a metallic aluminum film with a thickness of 30 nm on the substrate film.
[0191] (Anchor Coat Layer (C)) The method for producing the anchor coat layer (C) used in each example and comparative example is described below. [Polyester Resin (a)] As the polyester component, polyester polyol (DF-COAT GEC-004C manufactured by DIC Corporation: solid content 30%) was used.
[0192] [Polyisocyanate Crosslinking Agent (b)] As the polyisocyanate component, a trimethylolpropane adduct of metaxylylene diisocyanate ("Takenate D-110N" manufactured by Mitsui Chemicals, Inc.: solid content 75%) was used.
[0193] [Silane Coupling Agent (c)] As the silane coupling agent, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane ("KBM-603" manufactured by Shin-Etsu Chemical Co., Ltd.) was used.
[0194] [Urethane Resin (d)] As the urethane resin, a polyester urethane resin dispersion (HYDRAN (registered trademark) AP-201 manufactured by DIC Corporation; solid content 23%) was used.
[0195] [Coating Liquid 1 for Anchor Coat Layer 1] A solution (15% by mass) of silane coupling agent (c) dissolved in acetone and isocyanate (b) were mixed in the following ratio and stirred for 10 minutes using a magnetic stirrer. The resulting mixture was diluted with methyl ethyl ketone and 1-methoxy-2-propanol (hereinafter referred to as PGM), and polyester resin (a) was then added to obtain the target coating liquid 1. The mixing ratio is shown below: Polyester resin (a) 10.62% by mass Isocyanate (b) 4.07% by mass Silane coupling agent (c) *acetone diluted solution 1.73% by mass Methyl ethyl ketone 69.55% by mass PGM 14.03% by mass
[0196] [Coating Liquid 2 for Anchor Coat Layer 2] The following coating materials were mixed to prepare Coating Liquid 2: Water 43.91% by mass, Isopropanol 30.00% by mass, Urethane resin (d) 26.09% by mass
[0197] (Coating of coating liquid onto film (lamination of anchor coat layer)) Coating liquid 1 or coating liquid 2 was applied onto the corona-treated surface of the substrate film by gravure roll coating, pre-dried at 95°C for 4 seconds, and then fully dried at 115°C for 4 seconds to obtain an anchor coat layer. The adhesion amount of the anchor coat layer at this time was 0.40 g / m 2 Thereafter, a post-heat treatment was carried out at 40° C. for 4 days (96 hours) to obtain the desired laminated film.
[0198] (Protective Layer (D)) [Coating Liquid 1 Used for Protective Layer (D)] A solution obtained by hydrolyzing tetraethoxysilane with 0.02 mol / L hydrochloric acid was added to a 5 mass% aqueous solution of polyvinyl alcohol resin (PVA) having a saponification degree of 99% and a polymerization degree of 2400 in a mass ratio of SiO2 / PVA = 60 / 40 to prepare a protective layer solution (coating liquid 1).
[0199] (Coating of Coating Liquid on Film (Laminating of Protective Layer)) The above-mentioned Coating Liquid 1 was applied onto the inorganic thin film layer of the substrate film by gravure roll coating, and dried in a dry oven at 120°C for 10 seconds to obtain Protective Layer 1. The adhesion amount of the protective layer at this time was 0.30 g / m 2 Thereafter, a post-heat treatment was carried out at 40° C. for 2 days (48 hours). In this manner, a laminated film provided with a protective layer was produced.
[0200] [Preparation of Heat-Sealable Film CPP1] Table 5 shows the details of the polypropylene-based resin raw materials and polyethylene-based resin raw materials used in the preparation of the heat-sealable films CPP-1 to CPP-5, as well as the blending ratios of the raw materials.
[0201]
[0202] (Propylene-based copolymers) 1) FL8115A (manufactured by Sumitomo Chemical Co., Ltd., Noblen (registered trademark), propylene-ethylene-butene random copolymer, melting point 148°C, melt flow rate 7.0 g / 10 min, flexural modulus 1,000 MPa) 2) FL6745A (manufactured by Sumitomo Chemical Co., Ltd., Noblen (registered trademark), propylene-ethylene-butene random copolymer, melting point 130°C, melt flow rate 6.0 g / 10 min, flexural modulus 700 MPa)
[0203] (Polyethylene polymers) 1) FV401 (manufactured by Sumitomo Chemical Co., Ltd., Sumikathene (registered trademark) E, linear low-density polyethylene resin, melting point 112°C, melt flow rate 3.8 g / 10 min, flexural modulus 80 MPa) 2) FV405 (manufactured by Sumitomo Chemical Co., Ltd., Sumikathene (registered trademark) E, linear low-density polyethylene resin, melting point 118°C, melt flow rate 3.8 g / 10 min, flexural modulus 220 MPa) (Anti-blocking agents) 1) Synthetic silica: KMP130 (average particle size 4 μm, Shin-Etsu Chemical Co., Ltd.) 2) Ultra-high molecular weight polyethylene particles: Mipelon (registered trademark) PM200 (average particle size 10 μm, manufactured by Mitsui Chemicals, Inc.)
[0204] (Organic lubricants) 1) Erucic acid amide: Brand name Diamid L-200 (melting point 81°C, manufactured by Mitsubishi Chemical Corporation) 2) Behenic acid amide: Brand name D1007 (melting point 110°C, manufactured by Tokyo Chemical Industry Co., Ltd.)
[0205] (Masterbatches) 1) Silica masterbatch: Silica (KMP-130, manufactured by Shin-Etsu Chemical Co., Ltd., average particle size 4 μm) was mixed with Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. to prepare a masterbatch containing 12% by mass of silica. 2) Ultra-high molecular weight polyethylene particle masterbatch: Ultra-high molecular weight polyethylene particles (Mipelon PM200, manufactured by Mitsui Chemicals, Inc., average particle size 10 μm) were mixed with Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. to prepare a masterbatch containing 10% by mass of ultra-high molecular weight polyethylene particles. 3) Erucic acid amide masterbatch: Erucic acid amide was mixed with Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. to prepare a masterbatch containing 5% by mass of erucic acid amide. 4) Behenic acid amide masterbatch: Behenic acid amide was mixed with Noblen (registered trademark) FL6745A manufactured by Sumitomo Chemical Co., Ltd. to prepare a masterbatch containing 2% by mass of behenic acid amide.
[0206] (CPP-1) The laminate layer was made from FL8115A, the intermediate layer from FL6745A, and the seal layer from the resins and additives shown in Table 5. The resins were melted at 240 ° C. in three extruders, filtered through a sintered filter with a filtration accuracy of 60 μm, and then co-extruded into a sheet from a T-die. The thickness ratio of the laminate layer, intermediate layer, and seal layer was melt-extruded to be 25:50:25 vol.%, cooled and solidified on a cooling roll at 30 ° C., and then wound up into a roll at a speed of 20 m / min. A heat-sealable film with a total thickness of 30 μm (laminate layer thickness 7.5 μm, intermediate layer thickness 15 μm, seal layer thickness 7.5 μm), and a laminate layer wet tension of 45 mN / m was obtained. The content ratio of polypropylene resin and polyethylene resin in each layer is relative to the total of polypropylene resin and polyethylene resin.
[0207] (CPP-2 to 5) Heat-sealable films of CPP-2 to 5 were prepared in the same manner using the blending ratios shown in Table 5.
[0208] In this manner, packaging materials were prepared which had a coating layer, an anchor coat layer, an inorganic thin film layer, or a protective layer on each film, and further had a heat-sealable film.
[0209] In each example and comparative example, each film was used and bonded by dry lamination using the adhesive described above to obtain a packaging material having the configuration shown in Table 6A. Various evaluations were also carried out on the resulting packaging materials. The results are shown in Table 6B.
[0210]
[0211]
[0212] According to the present invention, a laminate film is formed by laminating a predetermined gas barrier layer tailored to the required performance on a base film, thereby greatly improving gas barrier performance, and by further laminating a resin layer with excellent low-temperature heat sealing properties as a heat-sealable film to the above-mentioned base film, it is possible to provide an environmentally friendly and highly convenient packaging material. Moreover, the packaging material of the present invention can be easily produced with few processing steps, so it is excellent in both economy and production stability, and it is possible to provide a gas barrier package with uniform properties.
Claims
1. A packaging material having at least one base film mainly composed of a polyolefin resin and a heat-sealable film, at least one of the base films being a laminated base film having a gas barrier layer, and when the faces of the heat-sealable films of the packaging material are heat-sealed together at 120°C, 0.1 MPa, for 1 second, the seal strength is 10 N / 15 mm or more, the loop stiffness is 22 mN / 25 mm or more, and the oxygen permeability at 23°C x 65% RH is 50 ml / m 2 ・d・MPa or less and water vapor transmission rate at 40℃×90%RH is 3.0g / m 2 A packaging material, characterized in that the thickness is d or less.
2. The packaging material according to claim 1, wherein the total thickness of the packaging material is 140 μm or less.
3. The packaging material according to claim 1, wherein the gas barrier layer is an inorganic thin film layer selected from the group consisting of aluminum, aluminum oxide, silicon oxide, and composite oxides of silicon oxide and aluminum oxide.
4. The packaging material according to claim 1, wherein the gas barrier layer is a coating layer containing, as a constituent component, a resin selected from the group consisting of polyvinyl alcohol resins, polyester resins, and polyurethane resins.
5. The packaging material according to claim 4, further comprising an inorganic layered compound.
6. The packaging material according to claim 1, wherein an anchor coat layer is laminated between the base film and the gas barrier layer.
7. The packaging material according to claim 1, wherein a protective layer is laminated on the gas barrier layer.
8. The packaging material according to claim 1, wherein said heat sealable film has a heat seal layer comprising a linear low density polyethylene resin and a propylene copolymer.
9. The packaging material according to claim 8, wherein the linear low-density polyethylene resin has a flexural modulus of 200 MPa or less.
10. The packaging material according to claim 8, wherein the heat-sealable film comprises, in addition to the heat-sealing layer, an intermediate layer and a laminate layer, the heat-sealing layer, the intermediate layer and the laminate layer being laminated in this order.
11. The packaging material of claim 10, wherein said intermediate layer and said laminate layer comprise a propylene copolymer.
12. The packaging material according to claim 1, wherein the base film is composed of a base layer and a surface layer, and the base layer contains a propylene homopolymer having a mesopentad fraction of 96% or more.
13. The packaging material according to claim 12, wherein the polypropylene homopolymer comprises a propylene homopolymer having an MFR of 5 g / 10 min or less and a propylene homopolymer having an MFR of more than 5 g / 10 min.
14. The packaging material according to claim 1, wherein two or more sheets of the base film are used.
15. The packaging material according to claim 1, which is used for microwave heating.
16. A packaging bag made of the packaging material according to any one of claims 1 to 15.
17. A package comprising an item packaged in the packaging material according to any one of claims 1 to 15.
18. A package comprising an item packaged in the packaging bag according to claim 16.
Citation Information
Patent Citations
Biaxially oriented laminated polypropylene film
JP2023013959A
Laminate, pouch, and lid member
WO2021199637A1
Laminated film and packaging material
WO2022030361A1
Sealant film
WO2023074754A1