Method for forming multilayer coating film

A multi-step coating process with a specific intermediate coating composition addresses the challenge of chipping resistance in multilayer coatings by optimizing aluminum pigment content and resin composition, enhancing both recoat performance and mechanical strength.

WO2024248094A1PCT designated stage expired Publication Date: 2024-12-05NIPPON PAINT AUTOMOTIVE COATINGS +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/019891
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing methods for forming multilayer coatings on automobile bodies face challenges in achieving excellent chipping resistance, particularly in recoated areas, due to inadequate adhesion between layers and the use of aluminum pigments which can affect the appearance and mechanical strength.

Method used

A method involving an intermediate coating composition with a specific ratio of aluminum pigment, acrylic resin, and polyester resin, applied in a multi-step process including electrodeposition, baking, and clear paint application, to achieve optimal crosslinking density and interlayer adhesion, enhancing chipping resistance and recoat performance.

Benefits of technology

The method results in a multilayer coating film with improved chipping resistance and recoat performance, maintaining mechanical strength and appearance by controlling the aluminum pigment content and resin composition, ensuring strong interlayer adhesion and suitable crosslinking density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-M000001
    Figure JPOXMLDOC01-APPB-M000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000045_0000
    Figure 00000045_0000
Patent Text Reader

Abstract

Disclosed is a method for forming a multilayer coating film that has excellent chipping resistance, especially excellent chipping resistance at the time of recoating, the method comprising (1) an intermediate coating material application step in which an uncured intermediate coating film that contains an aluminum pigment is formed directly on an electrodeposition coating film of an object to be coated, (2) a base coating material application step in which an uncured base coating film is formed on the uncured intermediate coating film, (3) a preheating step in which the thus-obtained coating films are dried, (4) a clear coating material application step in which an uncured clear coating film is formed on the uncured base coating film, and (5) a baking step in which the uncured intermediate coating film, the uncured base coating film, and the uncured clear coating film are baked and cured at the same time, wherein: the intermediate coating material composition contains an acrylic resin, a polyester resin, and a curing agent; (mass of aluminum pigment) / (mass of resin solid contents) × 100 is 1.5% by mass to 3% by mass inclusive; and the crosslinking density of a cured coating film of the intermediate coating material composition is 1.76-1.94 mol / ml.
Need to check novelty before this filing date? Find Prior Art

Description

Multi-layer coating film formation method

[0001] The present invention relates to a method for forming a multi-layer coating film.

[0002] When painting automobile bodies, chipping resistance is an important coating property. Chipping refers to damage to the coating caused by collisions with stones or other objects kicked up while the vehicle is moving. To improve chipping resistance, adhesion between coating layers and physical strength are important.

[0003] Furthermore, when painting an automobile body, if a defect occurs in the appearance of the paint film, only the defective part may be repainted. In such a recoating process, it is difficult to ensure sufficient adhesion between the original paint film and the recoated paint film, which can result in a decrease in chipping resistance in the recoated part.

[0004] Aluminum pigments are widely used in automotive paints, and are often blended into base paint compositions primarily for the purpose of achieving aesthetic appeal.

[0005] Patent Document 1 describes blending an aluminum pigment into an intermediate coating, but the purpose of blending the aluminum pigment into the intermediate coating is to obtain a good coating appearance so that the intermediate coating film takes on part of the role that has traditionally been played by the base coating film layer.

[0006] International Publication No. 2015 / 099151

[0007] An object of the present invention is to provide a method for forming a multi-layer coating film that can form a multi-layer coating film that is particularly excellent in chipping resistance, particularly in recoating chipping resistance.

[0008] The present invention relates to a method for forming a multi-layer coating film, comprising the steps of: an intermediate coating application step (1) of applying an intermediate coating containing an aluminum pigment directly onto an electrodeposition coating film formed on an object to form an uncured intermediate coating film; a base coating application step (2) of applying a base coating composition to the uncured intermediate coating film to form an uncured base coating film; a preheating step (3) of drying the resulting uncured intermediate coating film and base coating film; a clear coating application step (4) of applying a clear coating composition to the uncured base coating film to form an uncured clear coating film; and a baking step (5) of simultaneously baking and curing the uncured intermediate coating film, the uncured base coating film, and the uncured clear coating film, wherein the intermediate coating composition comprises an acrylic resin, a polyester resin, and a curing agent, and the content of the aluminum pigment in the intermediate coating composition is 1.5% by mass or more and 3% by mass or less, as calculated by the following formula: mass of aluminum pigment / mass of resin solids×100, The method for forming a multi-layer coating film is such that the crosslink density of the cured coating film of the intermediate coating composition is 1.76 to 1.94 mol / ml.

[0009] The intermediate coating composition preferably contains 3 parts by mass or more of a polyester resin per 100 parts by mass of resin solids. The base coating film is preferably a coating film formed by applying one or more base coating compositions.

[0010] The multilayer coating film preferably has an interlayer adhesion strength of 2.45 kN / m or more between the electrodeposition coating film and the cured intermediate coating film. The base coating composition application step is preferably a step of applying a base coating composition to an uncured intermediate coating film without preheating to form an uncured base coating film. The aluminum pigment preferably has a volume average particle diameter D50 of 5 to 20 μm and an average thickness of 0.01 to 0.3 μm.

[0011] The method for forming a multi-layer coating film of the present invention is effective in improving chipping resistance, particularly in improving chipping resistance at recoated areas.

[0012] Schematic diagram showing a method for measuring peel strength, Schematic diagram showing a method for measuring peel strength, Schematic diagram showing a minimum adhesive strength.

[0013] The multilayer coating film forming method of the present disclosure is characterized by blending a predetermined amount of aluminum pigment in an intermediate coating composition having a specific resin composition. It is believed that the use of such an intermediate coating composition allows the crosslink density to be controlled within a suitable range, resulting in excellent chipping resistance. Furthermore, the interlayer adhesion between the electrodeposition coating film and the intermediate coating film and the physical strength of the intermediate coating film can also be maintained within appropriate ranges, ensuring film strength that can withstand impacts caused by film breakage in the recoated area, resulting in excellent chipping resistance in the recoated area.

[0014] (Intermediate Coating Composition) The intermediate coating composition used in the present invention is characterized by containing an aluminum pigment in a proportion of 1.5% by mass to 3% by mass (resin solids ratio). It has been discovered that by incorporating such a specific amount of aluminum pigment, the desired effects described above can be obtained.

[0015] It is known to incorporate aluminum pigments into intermediate coating compositions at a ratio of 5% by mass or more. However, it is not known to incorporate aluminum pigments at a low ratio of 3% by mass or less. Furthermore, for example, incorporating aluminum pigments at approximately 5% by mass results in undesirable results in that the chipping resistance of the recoated area is insufficient. Furthermore, aluminum pigments have a larger particle size than other color pigments, which affects the appearance of the intermediate coating film.

[0016] If the amount of aluminum pigment is less than 1.5% by mass, the above-mentioned effects cannot be sufficiently obtained, which is undesirable.

[0017] The upper limit of the aluminum pigment content is more preferably 2.9% by mass, and even more preferably 2.8% by mass. The aluminum pigment content here refers to the mass ratio relative to the resin solid content in the paint, and more specifically, it is the mass ratio calculated based on the mass of the components contained in the paint composition using the following formula: Mass of aluminum pigment / mass of resin solid content x 100. Each component blended in the intermediate paint will be described in detail below.

[0018] [Aluminum Pigment] A metallic aluminum pigment is preferably used as the aluminum pigment to be incorporated into the intermediate coating composition. In the present invention, the content of the aluminum pigment contained in the intermediate coating composition is 1.5% by mass or more and 3% by mass or less, based on 100 parts by mass of the resin solids contained in the intermediate coating composition.

[0019] The aluminum pigment incorporated into the intermediate coating preferably has a small particle size, with a volume average particle size D50 of 5 to 20 μm. Having the volume average particle size D50 of the aluminum pigment within this range prevents peeling at the interface between the intermediate coating film and the electrodeposition coating film, making it easier to achieve an excellent sense of depth. A more preferred volume average particle size D50 is 8 to 17 μm. The volume average particle size D50 is the particle size at which the total volume of particles, calculated as a percentage of the total particle volume from the smallest particle size to a certain particle size in the particle size distribution of the aluminum pigment, is 50%. The volume average particle size D50 can be measured using dynamic light scattering, particularly a UPA-150 (Microtrac particle size distribution analyzer manufactured by Nikkiso Co., Ltd.), and an electron microscope.

[0020] Furthermore, the aluminum pigment preferably has a thin film (scale-like) shape and an average thickness of 0.01 to 0.3 μm. By ensuring that the average thickness of the thin film-shaped aluminum pigment falls within this range, peeling at the interface between the intermediate coating film and the electrodeposition coating film can be avoided, resulting in a multilayer coating film with good chipping resistance. Here, the average thickness is determined by measuring the thickness of 100 randomly selected aluminum pigment particles using a scanning electron microscope (SEM) and calculating the number average value. The aluminum pigment also preferably has an aspect ratio (volume average particle size, corresponding to the average major axis, divided by the average thickness of the pigment) of 50 to 300, preferably 100 to 200.

[0021] (Water-Based Intermediate Coating Paint) The intermediate coating paint composition is preferably a water-based intermediate coating paint composition from the viewpoint of reducing the environmental load.

[0022] The intermediate coating composition used in the method of the present invention contains an acrylic resin, a polyester resin, and a curing agent. The acrylic resin preferably contains an acrylic resin emulsion and a water-soluble acrylic resin. The aqueous coating composition preferably further contains a polyurethane resin. Each component is described below.

[0023] (Acrylic Resin Emulsion) The acrylic resin emulsion is preferably a hydroxyl group-containing acrylic resin emulsion. The hydroxyl group-containing acrylic resin emulsion may contain a styrene-based monomer, and can be obtained by emulsion polymerization of a monomer mixture containing a (meth)acrylic acid alkyl ester (I), an acid group-containing ethylenically unsaturated monomer (II), and a hydroxyl group-containing ethylenically unsaturated monomer (III). The compounds exemplified below as components of the monomer mixture may be used alone or in appropriate combination of two or more.

[0024] By blending a styrene-based monomer into the acrylic resin emulsion, the hydrophobic effect thereof can be achieved, which significantly prevents sagging of the resulting water-based primer coating composition during application.

[0025] Examples of the styrene-based monomer include styrene, α-methylstyrene, α-methylstyrene dimer, vinyltoluene, and divinylbenzene. Among these, styrene is particularly preferred from the viewpoints of hydrophobicity, cost, and availability.

[0026] The content of the styrene-based monomer is preferably 1 to 10% by mass, more preferably 2 to 8% by mass, for example 3 to 7% by mass, based on the total amount of monomers used in synthesizing the acrylic resin emulsion. In the present invention, by having the content of the styrene-based monomer within this range, a good hydrophobic effect can be obtained, and sagging of the resulting aqueous intermediate coating composition during application can be suppressed. Furthermore, excellent physical properties can be imparted to the intermediate coating film formed from the resulting aqueous intermediate coating composition.

[0027] By blending the styrene-based monomer in the above content into the acrylic resin emulsion, the water tolerance of the acrylic resin emulsion can be adjusted to 0.2 to 5 (ml), preferably 0.3 to 4 (ml), and the hexane tolerance can be adjusted to 5 to 25 (ml), preferably 6 to 23 (ml). In this specification, the water tolerance is used to evaluate the degree of hydrophilicity, with a higher value indicating higher hydrophilicity, and the hexane tolerance is used to evaluate the degree of hydrophobicity, with a higher value indicating higher hydrophobicity.

[0028] If the water tolerance is less than 0.2 (ml), compatibility will decrease, causing turbidity in the coating film and potentially deteriorating the appearance of the coating film. If the water tolerance exceeds 5 (ml), water resistance may decrease. Therefore, if the water tolerance is within the above range, the storage stability of the aqueous primer coating composition will be improved, and coating workability will be improved.

[0029] If the hexane tolerance is less than 5 ml, compatibility will decrease, causing the coating film to become cloudy and possibly resulting in poor coating film appearance, whereas if the hexane tolerance is more than 25 ml, compatibility will decrease, resulting in problems such as reduced storage stability of the aqueous primer coating composition.

[0030] In this specification, water tolerance is a value that can be measured as follows. The measurement temperature is 20°C, 0.5 g of the resin to be measured is weighed into a 100 ml beaker, 10 ml of acetone is added using a volumetric pipette, and the resin is dissolved in acetone using a magnetic stirrer. Next, deionized water is added dropwise to the acetone solution prepared above using a 50 ml burette, and the amount of water added (ml) at the point where turbidity occurs is taken as the water tolerance. Note that hexane tolerance is the amount of hexane added (ml) measured by replacing the water in the above water tolerance with n-hexane.

[0031] The hydroxyl-containing acrylic resin emulsion used in the present invention is preferably a hydroxyl-containing acrylic resin emulsion having a water tolerance of 0.2 to 5 and a hexane tolerance of 5 to 25. By using such a hydroxyl-containing acrylic resin, sagging of the resulting water-based primer coating composition during application can be significantly prevented, improving the appearance of the coating film.

[0032] The (meth)acrylic acid alkyl ester (I) is used to constitute the main skeleton of the acrylic resin emulsion. Specific examples of the (meth)acrylic acid alkyl ester (I) include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate. The content of the (meth)acrylic acid alkyl ester (I) is preferably 50 to 98% by mass, for example, 65 to 96% by mass, based on the total amount of monomers used in the synthesis of the acrylic resin emulsion. The (meth)acrylic acid alkyl ester (I) may be used alone or in combination. In any embodiment, however, the content is adjusted so that the glass transition temperature, acid value, and hydroxyl value of the resulting acrylic resin fall within the predetermined ranges according to the present invention.

[0033] The acid group-containing ethylenically unsaturated monomer (II) is used to improve the various stabilities of the resulting acrylic resin emulsion, such as storage stability, mechanical stability, and stability against freezing, and to promote the curing reaction with a curing agent such as a melamine resin during coating film formation. The acid group is preferably selected from a carboxyl group, a sulfonic acid group, a phosphoric acid group, etc. A particularly preferred acid group is a carboxyl group, from the viewpoint of improving the various stabilities and promoting the curing reaction.

[0034] Examples of the carboxyl group-containing ethylenically unsaturated monomer include acrylic acid, methacrylic acid, crotonic acid, isocrotonic acid, ethacrylic acid, propylacrylic acid, isopropylacrylic acid, itaconic acid, maleic anhydride, and fumaric acid. Examples of sulfonic acid group-containing ethylenically unsaturated monomers include p-vinylbenzenesulfonic acid, p-acrylamidopropanesulfonic acid, and t-butylacrylamidosulfonic acid. Examples of phosphoric acid group-containing ethylenically unsaturated monomers include Light Ester PM (manufactured by Kyoeisha Chemical Co., Ltd.), such as phosphoric acid monoester of 2-hydroxyethyl acrylate and phosphoric acid monoester of 2-hydroxypropyl methacrylate. The content of the acid group-containing ethylenically unsaturated monomer (II) is preferably 0.1 to 5% by mass, for example, 0.1 to 3% by mass, based on the total amount of monomers used in the synthesis of the acrylic resin emulsion. The acid group-containing ethylenically unsaturated monomer (II) may be used alone or in combination. In any embodiment, however, the content is adjusted so that the glass transition temperature, acid value, and hydroxyl value of the resulting acrylic resin fall within the predetermined ranges according to the present invention.

[0035] The hydroxyl group-containing ethylenically unsaturated monomer (III) is used to impart hydrophilicity based on the hydroxyl group to the acrylic resin emulsion, thereby improving workability and stability against freezing when the emulsion is used as a coating composition, and to impart curing reactivity with the melamine resin and isocyanate-based curing agent. The content of the hydroxyl group-containing ethylenically unsaturated monomer (III) is preferably 1.0 to 32 mass%, for example, 1.0 to 30 mass%, based on the total amount of monomers used in synthesizing the acrylic resin emulsion. The hydroxyl group-containing ethylenically unsaturated monomer (III) may be used alone or in combination. However, in either embodiment, the content is adjusted so that the glass transition temperature, acid value, and hydroxyl value of the resulting acrylic resin fall within the specified ranges according to the present invention.

[0036] Examples of the hydroxyl group-containing ethylenically unsaturated monomer (III) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and ε-caprolactone-modified acrylic monomers.

[0037] Specific examples of the ε-caprolactone-modified acrylic monomer include "PLACCEL FA-1," "PLACCEL FA-2," "PLACCEL FA-3," "PLACCEL FA-4," "PLACCEL FA-5," "PLACCEL FM-1," "PLACCEL FM-2," "PLACCEL FM-3," "PLACCEL FM-4," and "PLACCEL FM-5," ​​manufactured by Daicel Chemical Industries, Ltd.

[0038] The monomer mixture may contain, as another component, at least one monomer selected from the group consisting of (meth)acrylonitrile and (meth)acrylamide.

[0039] The monomer mixture may also contain crosslinkable monomers such as carbonyl group-containing ethylenically unsaturated monomers, hydrolytically polymerizable silyl group-containing monomers, and various polyfunctional vinyl monomers, in which case the resulting acrylic resin emulsion will be self-crosslinking.

[0040] The emulsion polymerization can be carried out by heating the monomer mixture in an aqueous solution in the presence of a radical polymerization initiator and an emulsifier while stirring. The reaction temperature is, for example, about 30 to 100°C, and the reaction time is, for example, about 1 to 10 hours. The reaction temperature can be adjusted by adding the monomer mixture or the monomer pre-emulsion all at once or gradually dropping it into a reaction vessel containing water and an emulsifier.

[0041] As the radical polymerization initiator, known initiators typically used in emulsion polymerization of acrylic resins can be used. Specifically, as a water-soluble free radical polymerization initiator, for example, a persulfate such as potassium persulfate, sodium persulfate, or ammonium persulfate is used in the form of an aqueous solution. Also, so-called redox initiators, which are combinations of an oxidizing agent such as potassium persulfate, sodium persulfate, ammonium persulfate, or hydrogen peroxide with a reducing agent such as sodium hydrogen sulfite, sodium thiosulfate, Rongalite, or ascorbic acid, are used in the form of an aqueous solution.

[0042] The emulsifier used may be an anionic or nonionic emulsifier selected from micellar compounds having a hydrocarbon group with 6 or more carbon atoms and a hydrophilic moiety such as a carboxylate, sulfonate, or sulfate partial ester in the same molecule. Examples of anionic emulsifiers include alkali metal or ammonium salts of sulfuric acid half esters of alkylphenols or higher alcohols; alkali metal or ammonium salts of alkyl or aryl sulfonates; and alkali metal or ammonium salts of sulfuric acid half esters of polyoxyethylene alkyl phenyl ethers, polyoxyethylene alkyl ethers, or polyoxyethylene allyl ethers. Examples of nonionic emulsifiers include polyoxyethylene alkyl phenyl ethers, polyoxyethylene alkyl ethers, and polyoxyethylene allyl ethers. In addition to these general-purpose anionic and nonionic emulsifiers, various anionic and nonionic reactive emulsifiers having a radically polymerizable unsaturated double bond in the molecule, i.e., having an acrylic, methacrylic, propenyl, allyl, allyl ether, maleic acid, or other group, may also be used alone or in combination of two or more types as appropriate.

[0043] Furthermore, during emulsion polymerization, the combined use of an auxiliary agent (chain transfer agent) for adjusting molecular weight, such as a mercaptan compound or a lower alcohol, is often preferable from the viewpoint of advancing the emulsion polymerization and from the viewpoint of promoting smooth and uniform formation of a coating film and improving adhesion to the substrate, and is carried out as appropriate depending on the circumstances.

[0044] The emulsion polymerization may be any polymerization method, such as a conventional single-stage continuous uniform monomer dropping method, a core-shell polymerization method which is a multi-stage monomer feed method, or a power feed polymerization method in which the monomer composition fed during polymerization is continuously changed.

[0045] The hydroxyl group-containing acrylic resin emulsion used in the present invention is prepared in this manner. The weight average molecular weight of the resulting acrylic resin is not particularly limited, but is generally about 50,000 to 1,000,000, for example, about 100,000 to 800,000.

[0046] The glass transition temperature (Tg) of the acrylic resin is preferably -50°C to 50°C, more preferably -30°C to 50°C, and in some embodiments, within the range of -25°C to 40°C, for example, -20°C to 40°C. When the glass transition temperature (Tg) is within this range, when an aqueous intermediate coating composition containing the acrylic resin emulsion is used in a wet-on-wet system, the affinity and / or adhesion with the electrodeposition coating film and the topcoat coating film is good, resulting in good compatibility at the interface with the upper coating film in a wet state and preventing inversion. Furthermore, the final coating film has appropriate flexibility and enhanced chipping resistance. As a result, a multilayer coating film with excellent appearance can be formed.

[0047] In the present invention, if the Tg of the acrylic resin is less than -50°C, the mechanical strength of the coating film may be insufficient, resulting in poor chipping resistance. On the other hand, if the Tg of the resin is greater than 50°C, the coating film may become hard and brittle, resulting in poor impact resistance and poor chipping resistance. The type and amount of each monomer component are selected so that the Tg of the resin falls within the above-mentioned range. Herein, the glass transition temperature (Tg) of the acrylic resin can be calculated from the amounts of various monomers in the monomer mixture used to synthesize the acrylic resin emulsion.

[0048] The acid value of the acrylic resin is preferably 2 to 60 mgKOH / g, more preferably 3 to 50 mgKOH / g, for example, in the range of 5 to 30 mgKOH / g. By maintaining the acid value of the resin within this range, the various stabilities of the resin emulsion and the aqueous primer coating composition using it, such as storage stability, mechanical stability, and stability against freezing, are improved. Furthermore, the curing reaction with the curing agent, such as melamine resin, during coating film formation occurs sufficiently, improving the strength, chipping resistance, and water resistance of the coating film. If the acid value of the resin is less than 2 mgKOH / g, the above-mentioned stabilities may be poor. Furthermore, the curing reaction with the curing agent, such as melamine resin, may not occur sufficiently, resulting in poor coating film strength, chipping resistance, and water resistance. On the other hand, if the acid value of the resin exceeds 60 mgKOH / g, the polymerization stability of the resin may be poor, or the above-mentioned stabilities may be adversely affected, resulting in poor water resistance of the resulting coating film. The type and amount of each monomer component can be selected so that the acid value of the resin falls within the above range. As described above, it is important to use a carboxyl group-containing monomer among the acid group-containing ethylenically unsaturated monomers (II), and the carboxyl group-containing monomer is preferably contained in an amount of 50 mass % or more, for example, 80 mass % or more, of the monomers (II).

[0049] The hydroxyl value of the acrylic resin is preferably 10 to 120 mgKOH / g, more preferably 10 to 70 mgKOH / g. By maintaining the hydroxyl value within this range, the resin has appropriate hydrophilicity, which improves workability and stability against freezing when used in a coating composition containing a resin emulsion, and also ensures sufficient curing reactivity with melamine resins, isocyanate-based curing agents, and the like. In the present invention, if the hydroxyl value is less than 10 mgKOH / g, the curing reaction with the curing agent is insufficient, resulting in weak mechanical properties of the coating film, poor chipping resistance, and poor water resistance and solvent resistance. On the other hand, if the hydroxyl value exceeds 120 mgKOH / g, the water resistance of the resulting coating film may be reduced, and compatibility with the curing agent may be poor, causing distortion in the coating film and uneven curing reactions, resulting in poor coating film strength, particularly chipping resistance, solvent resistance, and water resistance. The type and amount of each of the monomer components can be selected so that the hydroxyl value of the resin falls within the above range.

[0050] A basic compound can be added to the resulting acrylic resin emulsion to neutralize a part or all of the carboxylic acid and maintain the stability of the acrylic resin emulsion. As such a basic compound, ammonia, various amines, alkali metals, etc. are usually used, and these are also used appropriately in the present invention.

[0051] The resin solids content of the acrylic resin emulsion contained in 100 parts by mass of the total resin solids content of the film-forming resin is preferably 3 to 30 parts by mass, more preferably 5 to 20 parts by mass, and even more preferably, for example, 6 to 15 parts by mass. When the film-forming resin contains the acrylic resin emulsion of the present invention in such a range, the various stabilities of the coating film formed from the aqueous intermediate coating composition, such as storage stability, mechanical stability, and stability against freezing, are improved, and the curing reaction with the curing agent, such as melamine resin, during coating film formation occurs sufficiently, improving the strength, chipping resistance, and water resistance of the coating film.

[0052] (Water-soluble acrylic resin) The primer coating of the present invention preferably contains a water-soluble acrylic resin. The content of the water-soluble acrylic resin is preferably 5 to 50 parts by mass, and more preferably 10 to 40 parts by mass, per 100 parts by mass of resin solids. By containing the water-soluble acrylic resin in the above range, there is an advantage in that a good coating appearance can be obtained.

[0053] The water-soluble acrylic resin preferably has a number average molecular weight of 3,000 to 50,000, and more preferably 6,000 to 30,000. If it is less than 3,000, workability and curability are insufficient, while if it exceeds 50,000, the nonvolatile content during application becomes too low, which actually worsens workability.

[0054] The water-soluble acrylic resin preferably has an acid value of 10 to 100 mgKOH / g, more preferably 20 to 80 mgKOH / g; if the acid value exceeds the upper limit, the water resistance of the coating film decreases, and if the acid value is below the lower limit, the water dispersibility of the resin decreases. The water-soluble acrylic resin also preferably has a hydroxyl value of 20 to 180 mgKOH / g, more preferably 30 to 160 mgKOH / g. Having a water washability value within the above range has the advantage of ensuring good water resistance and curability of the coating film.

[0055] This water-soluble acrylic resin can be obtained by solution polymerization of the α,β-ethylenically unsaturated monomer having an acid group, which is described above in the monomer mixture section, as an essential component, together with other α,β-ethylenically unsaturated monomers.

[0056] The water-soluble acrylic resin is usually neutralized with a basic compound, for example, an organic amine such as monomethylamine, dimethylamine, trimethylamine, triethylamine, diisopropylamine, monoethanolamine, diethanolamine, or dimethylethanolamine, and then dissolved in water before use. This neutralization may be carried out on the water-soluble acrylic resin itself, or may be carried out during the production of the undercoat paint described below.

[0057] The aqueous intermediate coating composition preferably contains an acrylic resin emulsion and a water-soluble acrylic resin as the acrylic resin, and the total content of the acrylic resin emulsion and the water-soluble acrylic resin contained in the aqueous intermediate coating composition is preferably 8 to 50 parts by mass, and more preferably 10 to 45 parts by mass, per 100 parts by mass of the resin solids.

[0058] (Polyester Resin) In the present invention, the film-forming resin in the aqueous intermediate coating composition contains a polyester resin. The polyester resin may be a resin commonly used in the art. Preferably, the resin contains a hydroxyl group-containing polyester resin. By including a polyester resin, the viscosity of the coating film after application can be kept appropriate, resulting in a high-quality appearance.

[0059] The solid content of the polyester resin contained in 100 parts by mass of the total resin solid content of the coating film-forming resin is preferably 1 to 55 parts by mass, more preferably 5 to 35 parts by mass, for example 5 to 30 parts by mass, and in one embodiment 5 to 25 parts by mass.

[0060] Examples of hydroxyl-containing polyester resins include oil-free polyester resins obtained by condensing a polyhydric alcohol component with a polybasic acid component, and oil-modified polyester resins obtained by reacting the above-mentioned acid and alcohol components with an oil component such as castor oil, dehydrated castor oil, tung oil, safflower oil, soybean oil, linseed oil, tall oil, palm oil, or one or a mixture of two or more of these fatty acids in addition to the polyhydric alcohol component and polybasic acid component. Polyester resins grafted with acrylic resins or vinyl resins can also be used. Furthermore, urethane-modified polyester resins obtained by reacting a polyester resin obtained by reacting a polyhydric alcohol component with a polybasic acid component with a polyisocyanate compound can also be used.

[0061] The number average molecular weight (Mn) of the hydroxyl group-containing polyester resin is preferably 800 to 10,000, more preferably 1,000 to 8,000. If Mn is less than 800, the stability of the polyester resin when dispersed in water decreases, while if it exceeds 10,000, the viscosity of the resin increases, which may decrease the solids concentration when made into a coating composition, thereby reducing coating workability.

[0062] The hydroxyl value of the hydroxyl-containing polyester resin is preferably 35 to 170 mgKOH / g, more preferably 50 to 150 mgKOH / g. If the hydroxyl value is less than 35 mgKOH / g, the curability of the resulting coating film may be reduced, while if it exceeds 170 mgKOH / g, the chipping resistance of the coating film may be reduced.

[0063] The hydroxyl group-containing polyester resin preferably has an acid value of 15 to 100 mgKOH / g, and more preferably 20 to 80 mgKOH / g. If the acid value is less than 15 mgKOH / g, the aqueous dispersion stability of the polyester resin may be reduced, while if it exceeds 100 mgKOH / g, the water resistance of the resulting coating may be reduced.

[0064] The glass transition temperature of the hydroxyl group-containing polyester resin is preferably −40 to 50° C. If the glass transition temperature is less than −40° C., the hardness of the resulting coating film may decrease, and if it exceeds 50° C., the base hiding ability may decrease. A temperature of −40 to 10° C. is more preferable. The glass transition temperature can be calculated from the amounts of various monomers in the monomer mixture used for synthesis.

[0065] Examples of the polyhydric alcohol component include ethylene glycol, diethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-diethyl-1,3-propanediol, neopentyl glycol, 1,9-nonanediol, 1,4-cyclohexanediol, hydroxypivalic acid neopentyl glycol ester, 2-butyl-2-ethyl-1,3-propanediol, Examples include diols such as 3-methyl-1,5-pentanediol, 2,2,4-trimethylpentanediol, and hydrogenated bisphenol A; trivalent or higher polyol components such as trimethylolpropane, trimethylolethane, glycerin, and pentaerythritol; and hydroxycarboxylic acid components such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutanoic acid, 2,2-dimethylolpentanoic acid, 2,2-dimethylolhexanoic acid, and 2,2-dimethyloloctanoic acid.

[0066] Examples of the polybasic acid component include aromatic polycarboxylic acids and acid anhydrides such as phthalic anhydride, isophthalic acid, terephthalic acid, trimellitic anhydride, tetrabromophthalic anhydride, tetrachlorophthalic anhydride, and pyromellitic anhydride; alicyclic polycarboxylic acids and anhydrides such as hexahydrophthalic anhydride, tetrahydrophthalic anhydride, and 1,4- and 1,3-cyclohexanedicarboxylic acid; and aliphatic polycarboxylic acids and anhydrides such as maleic anhydride, fumaric acid, succinic anhydride, adipic acid, sebacic acid, and azelaic acid, as well as polybasic acid components and anhydrides thereof. If necessary, monobasic acids such as benzoic acid and t-butylbenzoic acid may be used in combination.

[0067] When preparing the polyester resin, further reactive components may be used in combination: monohydric alcohols, monoepoxide compounds such as Cardura E (trade name: manufactured by Shell Chemical), and lactones (β-propiolactone, dimethylpropiolactone, butyrolactone, γ-valerolactone, ε-caprolactone, γ-caprolactone, γ-caprylolactone, crotolactone, δ-valerolactone, δ-caprolactone, etc.). Lactones, in particular, undergo ring-opening addition to the polyester chains of polycarboxylic acids and polyhydric alcohols to form polyester chains themselves, and furthermore, are useful for improving the chipping resistance of aqueous primer coating compositions. These may be present in an amount of 3 to 30%, preferably 5 to 20%, and particularly 7 to 15% of the total mass of all reactive components.

[0068] The hydroxyl group-containing polyester resin can be easily made aqueous by adjusting its acid value and neutralizing the carboxyl groups with a basic substance (e.g., 50% or more). Examples of basic substances that can be used here include ammonia, methylamine, ethylamine, dimethylamine, diethylamine, trimethylamine, triethylamine, dimethylethanolamine, diethanolamine, and triethanolamine, with diethanolamine, dimethylethanolamine, and triethanolamine being preferred. The neutralization rate during the neutralization is not particularly limited and is, for example, 80 to 120%.

[0069] [Urethane Emulsion Resin] The urethane emulsion resin that can be incorporated as the film-forming resin in the intermediate coating composition can be, for example, one obtained as follows. First, a diisocyanate is reacted with a glycol having at least two active hydrogens or a glycol having a carboxylic acid group at an NCO / OH equivalent ratio of 0.5 to 2.0 to produce a urethane prepolymer. Next, the produced urethane prepolymer is neutralized with a neutralizing agent and chain-extended with a chain extender. After that, a cationic, nonionic, or anionic surfactant and ion-exchanged water are added and dispersed to obtain a urethane emulsion resin.

[0070] Examples of the diisocyanate include aliphatic, alicyclic, and aromatic diisocyanates, such as 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, m-phenylene diisocyanate, xylylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, meta-xylene diisocyanate, lysine diisocyanate, 1,4-cyclohexylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 1,5-naphthalene diisocyanate, 1,5-tetrahydronaphthalene diisocyanate, isophorone diisocyanate, and derivatives thereof.

[0071] Examples of the glycol having active hydrogen include low molecular weight glycols such as ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, trimethylene glycol, 1,3-butylene glycol, tetramethylene glycol, hexamethylene glycol, hydrogenated bisphenol A, and ethylene oxide or propylene oxide adducts of bisphenol A; polyoxypropylene glycols; an adduct of polyoxypropylene and glycerin; an adduct of polyoxypropylene and trimethylolpropane; an adduct of polyoxypropylene and 1,2,6-hexanetriol; an adduct of polyoxypropylene and pentaerythritol; an adduct of polyoxypropylene and sorbitol; methylene-bis-phenyl diisocyanate; polytetrafuran polyether chain-extended with hydrazine; and derivatives thereof. Further examples include polyesters and polycaprolactones which are condensation products of adipic acid or phthalic acid with ethylene glycol, propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, diethylene glycol, hexanediol, 1,2,6-hexanetriol, trimethylolpropane, 1,1,1-trimethylolethane, or the like.

[0072] Examples of the glycol having a carboxylic acid group include 2,2-dimethylolpropionic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvaleric acid.

[0073] Examples of the neutralizing agent include amines such as trimethylamine, triethylamine, tri-n-propylamine, tributylamine, and triethanolamine, sodium hydroxide, potassium hydroxide, and ammonia.

[0074] Examples of the chain extender include polyols such as ethylene glycol and propylene glycol; aliphatic, alicyclic, or aromatic diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, tolylenediamine, xylylenediamine, diphenyldiamine, diaminodiphenylmethane, diaminocyclohexylmethane, piperazine, 2-methylpiperazine, 1,2-bis(2-cyanoethylamino)ethane, and isophoronediamine; and water.

[0075] Commercially available products can be used as the urethane emulsion resin. Specific examples include the "Bondic" series and "Hydran" series manufactured by Dai Nippon Ink & Coatings, the "Impranil" series manufactured by Bayer, the "Neolet's" series manufactured by Avecia, such as Neolet's R-940, R-941, R-960, R-962, R-966, R-967, R-962, R-9603, R-9637, R-9618, R-9619, and XR-9624, the "U-Coat," "Uprene," and "Permarin" series manufactured by Sanyo Chemical Industries, Ltd., and the "Adeka Bontitor" series manufactured by ADEKA. These urethane emulsion resins can be used alone or in combination of two or more.

[0076] The content of the urethane emulsion resin is preferably 3 to 30 parts by mass per 100 parts by mass of the resin solids of the intermediate coating composition. If the content of the urethane emulsion resin is less than 3 parts by mass, there is a risk of reduced adhesion, and if it exceeds 30 parts by mass, there is a risk of reduced storage stability of the coating. A content of 3 to 20 parts by mass is particularly preferred.

[0077] [Polyether Polyol] The intermediate coating composition may optionally contain a polyether polyol as a film-forming resin. Polyether polyols that can be incorporated as film-forming resins in intermediate coatings preferably have an average of 0.02 or more primary hydroxyl groups per molecule and a number-average molecular weight of 300 to 3,000. The inclusion of such polyether polyols can improve the flip-flop properties, water resistance, and chipping resistance of the coating film. In this specification, the number-average molecular weight refers to the number-average molecular weight calculated in terms of polystyrene using GPC (gel permeation chromatography).

[0078] If the number of primary hydroxyl groups per molecule of polyether polyol is less than 0.02 on average, the water resistance and chipping resistance of the coating film will be reduced. The number of primary hydroxyl groups per molecule is more preferably 0.04 or more, and even more preferably 1 or more. From the viewpoint of the water resistance and chipping resistance of the coating film, the number of hydroxyl groups, including primary hydroxyl groups, secondary and tertiary hydroxyl groups, per molecule is preferably 2 or more.

[0079] Here, the hydroxyl value of the polyether polyol is preferably 30 to 700 mgKOH / g. If the hydroxyl value is less than 30 mgKOH / g, curability may decrease, resulting in a decrease in the water resistance and chipping resistance of the coating film. If the hydroxyl value exceeds 700 mgKOH / g, the stability of the paint and the water resistance of the coating film may decrease. A particularly preferred hydroxyl value is 50 to 500 mgKOH / g.

[0080] Furthermore, if the number average molecular weight of the polyether polyol is less than 300, the water resistance of the coating film may decrease, and if the number average molecular weight exceeds 3000, the curability and chipping resistance of the coating film may decrease. A particularly preferred number average molecular weight is 400 to 2000.

[0081] When the intermediate coating composition contains a polyether polyol, the content of the polyether polyol in the intermediate coating is preferably 1 to 40 parts by mass, more preferably 3 to 20 parts by mass, per 100 parts by mass of the resin solids of the intermediate coating. Having the polyether polyol content within this range has the advantage of enabling good coating appearance, water resistance, and chipping resistance to be obtained.

[0082] Examples of polyether polyols include compounds in which alkylene oxides are added to active hydrogen-containing compounds such as polyhydric alcohols, polyhydric phenols, and polycarboxylic acids. Examples of active hydrogen-containing compounds include water, polyhydric alcohols (dihydric alcohols such as ethylene glycol, diethylene glycol, trimethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol, 1,4-dihydroxymethylcyclohexane, and cyclohexylene glycol), glycerin, trioxyisobutane, 1,2,3-butanetriol, 1,2,3-pentanetriol, 2-methyl-2-propanol, and the like. ethyl-1,2,3-propanetriol, 2-methyl-2,3,4-butanetriol, 2-ethyl-1,2,3-butanetriol, 2,3,4-pentanetriol, 2,3,4-hexanetriol, 4-propyl-3,4,5-heptanetriol, 2,4-dimethyl-2,3,4-pentanetriol, pentamethylglycerin, pentaglycerin, 1,2,4-butanetriol, 1,2,4-pentanetriol, trimethylolethane, and trimethylolethane. Trihydric alcohols such as methylolpropane, tetrahydric alcohols such as pentaerythritol, 1,2,3,4-pentanetetrol, 2,3,4,5-hexanetetrol, 1,2,4,5-pentanetetrol, 1,3,4,5-hexanetetrol, diglycerin and sorbitan, pentahydric alcohols such as adonitol, arabitol, xylitol and triglycerin, dipentaerythritol, sorbitol, mannitol, iditol, inositol, dulcitol Examples of suitable polyols include hexahydric alcohols such as sucrose, talose, and allose, octahydric alcohols such as sucrose, and polyglycerin; polyhydric phenols [polyhydric phenols (pyrogallol, hydroquinone, phloroglucin, etc.), bisphenols (bisphenol A, bisphenol sulfone, etc.)]; polycarboxylic acids [aliphatic polycarboxylic acids (succinic acid, adipic acid, etc.), aromatic polycarboxylic acids (phthalic acid, terephthalic acid, trimellitic acid, etc.)]; and mixtures of two or more of these.

[0083] Polyether polyols can be obtained by a conventional method by adding an alkylene oxide to the active hydrogen-containing compound in the presence of an alkali catalyst at normal or elevated pressure and at a temperature of 60 to 160°C. Examples of alkylene oxides include ethylene oxide, propylene oxide, and butylene oxide, and these can be used alone or in combination of two or more. When two or more types are used in combination, the addition method can be either block or random.

[0084] Commercially available polyether polyols can be used, such as Primepol PX-1000, Sannix SP-750, PP-400, and GP-1000 (all manufactured by Sanyo Chemical Industries, Ltd.), and PTMG-650 (manufactured by Mitsubishi Chemical Corporation).

[0085] (Curing Agent) The intermediate coating composition used in the present invention contains a curing agent. The curing agent is not particularly limited, and examples thereof include melamine resins and isocyanate compounds. The melamine resin is not particularly limited, as long as it undergoes a curing reaction with the acrylic resin and hydroxyl group-containing polyester resin contained as an emulsion and can be incorporated into the aqueous intermediate coating composition. For example, imino-type methyl / butyl mixed etherified melamine resin, methylol group-type methylated melamine resin, and mixtures thereof can be suitably used.

[0086] The melamine resin can be used as a curing agent, and in one embodiment, the solid content of the melamine resin contained in 100 parts by mass of the total resin solid content of the coating film-forming resin is 10 to 50 parts by mass, for example, 10 to 40 parts by mass, and preferably 20 to 40 parts by mass. By having the solid content of the melamine resin in this range, the curing reaction occurs sufficiently, and the strength, chipping resistance, and water resistance of the coating film are improved.

[0087] As the melamine resin, a commercially available product may be used. Commercially available products include, for example, methylol group / imino type methyl / butyl mixed etherified melamine resins such as "Cymel 202"; imino type methyl / butyl mixed etherified melamine resins such as "Cymel 204", "Cymel 211", "Cymel 250" and "Cymel 254"; fully alkylated methylated melamine resins such as "Cymel 350"; imino group type methylated melamine resins such as "Cymel 325", "Cymel 327", "Cymel 385", "Cymel 701" and "Cymel 712"; methylol group type methylated melamine resins such as "Cymel 370" (all manufactured by Allnex Japan Co., Ltd.); imino type methyl / butyl mixed etherified melamine resins such as "Mycoat 212", "Mycoat 518" and "Mycoat 525"; imino type butylated melamine resins such as "Mycoat 508"; imino group type methylated melamine resins such as "Mycoat 723" and "Mycoat 776"; Examples include methylol group type methyl / isobutyl mixed etherified melamine resins such as "Mycoat 2677" (all manufactured by Mitsui Cytec Co., Ltd.) These may be used alone or in combination of two or more.

[0088] The polyisocyanate is not particularly limited as long as it is a compound having two or more isocyanate groups, and examples thereof include aromatic compounds such as tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate, and metaxylylene diisocyanate; aliphatic compounds such as hexamethylene diisocyanate; alicyclic compounds such as isophorone diisocyanate; and monomers thereof and polymers such as biuret types, isocyanurate types, and adduct types thereof.

[0089] Commercially available polyisocyanates include Duranate 24A-90PX (NCO: 23.6%, trade name, manufactured by Asahi Kasei Corporation), Sumidur N-3200-90M (trade name, manufactured by Sumitomo Bayer Urethanes Co., Ltd.), Takenate D165N-90X (trade name, manufactured by Mitsui Chemicals, Inc.), Sumidur N-3300, Sumidur N-3500 (all trade names, manufactured by Sumitomo Bayer Urethanes Co., Ltd.), Duranate THA-100 (trade name, manufactured by Asahi Kasei Corporation), etc. Blocked isocyanates obtained by blocking the above polyisocyanates can also be used, if necessary.

[0090] [Other Components] The primer coating may contain a pigment other than the aluminum pigment described above. Examples of pigments other than aluminum pigments include color pigments and other pigments other than color pigments. The color pigment is not particularly limited, and any color pigment commonly used in the paint field can be used. In this specification, "color pigment" includes chromatic color pigments and achromatic color pigments. Examples of other pigments include extender pigments. Examples of extender pigments include calcium carbonate, barium sulfate, clay, and talc. Anti-rust pigments can also be used as other pigments.

[0091] The primer paint may also contain a viscosity control agent as an additive to prevent blending with the base paint film (described later), ensure good coating workability, and control the orientation of the aluminum pigment. Viscosity control agents that generally exhibit thixotropy can be used, and examples include crosslinked or non-crosslinked resin particles, polyamide-based agents such as swollen dispersions of fatty acid amides, amide fatty acids, and phosphate salts of long-chain polyaminoamides, polyethylene-based agents such as colloidal swollen dispersions of polyethylene oxide, organic acid smectite clays, organic bentonite-based agents such as montmorillonite, inorganic pigments such as aluminum silicate and barium sulfate, and flat pigments whose viscosity is determined by the shape of the pigment.

[0092] In addition to the above components, the primer coating may also contain additives that are typically added to coatings, such as surface conditioners, thickeners, antioxidants, ultraviolet inhibitors, antifoaming agents, etc. The amounts of these additives added are within the ranges known in the art.

[0093] The method for preparing the intermediate coating material having the above-mentioned composition is not particularly limited, and the intermediate coating material can be prepared by a conventionally known method. Specifically, the intermediate coating material can be prepared by mixing and / or dispersing the above-mentioned components by a method commonly used by those skilled in the art.

[0094] (Crosslink Density) In the method for forming a multi-layer coating film of the present invention, the crosslink density of the cured coating film of the intermediate coating composition must be 1.76 to 1.94 mol / ml. By achieving a crosslink density within this range, it is preferable in that good coating film properties can be obtained as an intermediate coating film.

[0095] In this embodiment, the coating film crosslink density (n) is determined from the following mathematical formula 1 by dynamic viscoelasticity measurement, in which the viscoelasticity is measured while applying minute vibrations to the base coating film as a sample. In mathematical formula 1, E' represents the dynamic Young's modulus, R represents the gas constant, and T represents the absolute temperature. The coating film crosslink density is adjusted by appropriately adjusting the amount of crosslinking agent (a high amount results in a high crosslink density, and a low amount results in a low crosslink density), the molecular weight of the polyol (a low molecular weight results in a high crosslink density, and a high molecular weight results in a low crosslink density), the number of functional groups in one molecule of the polyol or crosslinking agent (a high number of functional groups results in a high crosslink density, and a low number of functional groups results in a low crosslink density), the baking temperature (a high baking temperature results in a high crosslink density, and a low baking temperature results in a low crosslink density), etc. By adjusting the coating film crosslink density within the above range, a multilayer coating film with good coating film performance such as chipping resistance can be obtained.

[0096]

[0097] The coating film used to measure such crosslink density is a single-layer coating film obtained by forming a coating film from an intermediate coating composition in a manner similar to the method for forming a multi-layer coating film, and then subjecting the coating film to a heat treatment similar to the heat history imparted to the coating film when forming the multi-layer coating film.

[0098] (Aqueous Base Coating Composition) The aqueous base composition used in the method of the present invention may be, for example, a coating composition commonly used as an aqueous base coating composition for automobile bodies. Examples include compositions containing a film-forming resin, a curing agent, an aluminum pigment, a pigment such as a coloring pigment or an extender pigment, and various additives dispersed or dissolved in an aqueous medium. Examples of film-forming resins that can be used include polyester resins, acrylic resins, urethane resins, carbonate resins, and epoxy resins. From the standpoints of pigment dispersibility and workability, a combination of an acrylic resin and / or a polyester resin with a melamine resin is preferred. Commonly used curing agents, pigments, and various additives can also be used.

[0099] The pigment concentration (PWC) in the aqueous base coating composition generally has a lower limit of 1% by mass and an upper limit of 60% by mass, for example, a lower limit of 2% by mass and an upper limit of 55% by mass, and more preferably a lower limit of 3% by mass and an upper limit of 55% by mass. If the pigment concentration is less than 1% by mass, the effect of the pigment cannot be obtained, and if it exceeds 60% by mass, the appearance of the resulting coating film may be deteriorated.

[0100] The aqueous base coating composition can be prepared by the same method as the intermediate coating composition. The form of the aqueous base coating composition is not particularly limited as long as it is aqueous, and may be, for example, water-soluble, water-dispersible, aqueous emulsion, or the like.

[0101] The base aqueous coating composition may be a layer of multiple base coatings with different compositions, specifically, a colored base coating film may be formed by applying a glitter base coating containing a glitter pigment onto a colored base coating film containing a colored coating film.

[0102] When two types of aqueous base coating compositions are used in this way, it is preferable to form the coating by applying them successively without providing a curing step.

[0103] (Clear Coating Composition) The clear coating composition used in the method of the present invention may be, for example, a coating composition commonly used as a clear coating composition for automobile bodies. Examples include those containing a film-forming resin, a curing agent, and other additives dispersed or dissolved in a medium. Examples of film-forming resins include acrylic resins, polyester resins, epoxy resins, and urethane resins. These are preferably used in combination with curing agents such as amino resins and / or isocyanate resins. A preferred embodiment of the clear coating composition, from the standpoints of transparency or acid etching resistance, is a combination of an acrylic resin and / or a polyester resin with an amino resin, or an acrylic resin and / or a polyester resin having a carboxylic acid / epoxy curing system. Another preferred embodiment of the clear coating composition is a two-component urethane clear coating composition, from the standpoint of low-temperature curing. An example of a urethane clear coating composition is a clear coating composition containing a hydroxyl-containing resin and an isocyanate compound curing agent. The hydroxyl-containing resin can be any resin that reacts with an isocyanate compound curing agent without any particular limitation. The isocyanate compound as the curing agent is not particularly limited, and examples thereof include aliphatic isocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate (HDI), and trimethylhexamethylene diisocyanate; aliphatic cyclic isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, and 1,2-cyclohexane diisocyanate; aromatic isocyanates such as xylylene diisocyanate (XDI), 2,4-tolylene diisocyanate (TDI), and 2,6-tolylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate (IPDI) and norbornane diisocyanate methyl; and polymers and mixtures thereof, such as biuret and nurate forms thereof.

[0104] The paint form of the clear paint composition may be any of organic solvent-based, aqueous (water-soluble, water-dispersible, emulsion), non-aqueous dispersion, and powder types, and may contain a curing catalyst, surface conditioner, etc. Of these, organic solvent-based paints are most preferred.

[0105] (Method for forming a multi-layer coating film) In the method for forming a multi-layer coating film of the present invention, first, an automobile body having an electrodeposition coating film formed thereon is provided. The electrodeposition coating film is formed by applying an electrodeposition coating composition to the automobile body and baking and curing it. The automobile body to be coated is not particularly limited as long as it is a metal product that can be subjected to cationic electrodeposition coating. Examples include iron, copper, aluminum, tin, zinc, and alloys containing these metals. The electrodeposition coating composition is not particularly limited, and known cationic electrodeposition coating compositions and anionic electrodeposition coating compositions can be used. Furthermore, the electrodeposition coating and baking may be carried out using methods and conditions normally used for electrodeposition coating automobile bodies.

[0106] In one embodiment, a chipping-resistant coating film is formed by applying a chipping-resistant coating film-forming composition onto an electrodeposition coating film. To obtain the desired coating thickness, the chipping-resistant coating film-forming composition is most preferably applied by airless spray coating, which can produce a thick film in a short time. This airless spray coating also includes improved methods such as electrostatic airless spray coating and air-assisted airless spray coating. Application can also be performed using a computer-controlled automatic coating machine or a robotic coating machine.

[0107] The amount of coating applied is adjusted so that the thickness of the cured coating film is 3 to 15 μm, preferably 4 to 10 μm. If the film thickness is less than 3 μm, the chipping resistance of the resulting coating film may decrease, while if it exceeds 20 μm, appearance defects such as sagging during application and pinholes during bake curing may occur.

[0108] Next, an aqueous intermediate coating composition is applied to the automobile body on which the electrodeposition coating film has been formed, or in one embodiment, to the automobile body on which the chipping-resistant coating film has been formed on the electrodeposition coating film.

[0109] The intermediate coating composition can be applied by spraying, for example, using an air electrostatic sprayer commonly known as a "react gun," or a rotary atomizing electrostatic coating machine commonly known as a "micro-microbell (μμbell)," "microbell (μbell)," "metallicbell (metabell)," etc.

[0110] The amount of coating applied is adjusted so that the thickness of the cured coating film is 10 to 40 μm, preferably 15 to 30 μm. If the thickness is less than 10 μm, the appearance and chipping resistance of the resulting coating film may be impaired, while if it exceeds 40 μm, problems such as sagging during application and pinholes during bake curing may occur.

[0111] As mentioned above, in the present invention, the intermediate coating composition may be applied, followed by heat curing, and then the base coating. For example, when the intermediate coating composition is applied, followed by heat curing, and then the base coating is applied, preheating may be performed as necessary. In this case, the preheating temperature and preheating time are not particularly limited, but may be, for example, 60 to 90°C, preferably 70 to 90°C, for 3 to 10 minutes.

[0112] When the intermediate coating composition is applied, followed by heat curing, and then the base coating is applied, the heat curing conditions for the intermediate coating composition are not particularly limited, and the intermediate coating composition can be cured, for example, by heating at a temperature of 120 to 160°C, preferably 130 to 160°C, for 10 to 60 minutes.

[0113] In the method of the present invention, the aqueous base paint composition may be applied immediately after application of the intermediate paint composition, or the aqueous base paint composition may be applied after heat curing. Regardless of which method is used to form the intermediate paint film, effects such as good improvement in adhesion, chipping resistance, and recoat chipping resistance can be obtained.

[0114] The amount of aqueous base coating composition applied is usually adjusted so that the thickness of the coating film after curing is 10 to 20 μm. If the thickness after curing is less than 10 μm, there is a risk of insufficient hiding of the base and uneven color, and if it exceeds 20 μm, there is a risk of sagging during application and pinholes occurring during heat curing.

[0115] After applying the aqueous base paint composition, the coating is preheated for 3 to 10 minutes, preferably at 60 to 90°C, more preferably at 70 to 90°C. By preheating, even if the clear paint composition is applied immediately after the formation of the uncured base paint film, mixing of the two paint film layers (mixing) can be prevented, and the resulting multilayer paint film can have an extremely excellent paint film appearance. Furthermore, according to the present invention, by preheating the aqueous base paint composition under the conditions described in the present invention, sagging of the aqueous base paint composition can be effectively prevented.

[0116] The amount of clear coating composition applied is usually adjusted so that the thickness of the coating film after drying and curing is 15 to 60 μm. If the thickness after curing is less than 15 μm, the appearance such as the gloss of the multi-layer coating film will be reduced, and if it exceeds 60 μm, the clarity will be reduced and problems such as unevenness and running will occur during application.

[0117] Next, the base coating film and the clear coating film are simultaneously baked and cured. If the base coating film and the clear coating film are applied while the intermediate coating film is still in an uncured state, the intermediate coating film will also be cured at the same time by this process.

[0118] Baking is usually carried out by heating to a temperature of 120 to 160°C, preferably 130 to 160°C. This allows for a cured coating film with a high degree of crosslinking to be obtained. If the heating temperature is less than 120°C, curing tends to be insufficient, while if it exceeds 160°C, the resulting coating film may be hard and brittle. The heating time can be set appropriately depending on the temperature, but is, for example, 10 to 60 minutes when the temperature is 130 to 160°C.

[0119] The multilayer coating film obtained by the method of the present invention preferably has an interlayer adhesion strength at the coating interface between the electrodeposition coating film and the intermediate coating film that constitute the multilayer coating film of 0.15 to 0.27 kN / m. The interlayer adhesion strength of the electrodeposition coating film and the intermediate coating film that constitute the multilayer coating film is measured based on the SAICAS method. Here, "SAICAS" stands for Surface and Interfacial Cutting Analysis System. This SAICAS method can measure the peel strength and shear strength of the coating film relative to the adherend. The SAICAS method is a known measurement method, and is described in, for example, "Evaluation of Adhesion Strength of Adherends by the SAICAS Method (1)", Nishiyama, Itsuo, Coating Technology, 34, 4, 123 (1995) and "Evaluation of Adhesion Strength of Adherends by the SAICAS Method (2)", Nishiyama, Itsuo, Coating Technology, Coating Technology, 34, 5, 129 (1995).

[0120] Figure 1 is a schematic diagram showing a method for measuring adhesive strength using the SAICAS method. A cutting blade 5 is pressed against the surface of a coating film 7 formed on a substrate 9 with a predetermined load and moved horizontally relative to the coating surface, causing the cutting blade 5 to cut into the coating film 7. The cutting direction at this time is indicated by 11. After the cutting blade 5 reaches the coating interface, the cutting blade 5 is moved only horizontally to measure the horizontal cutting stress. The interlayer adhesion strength is calculated using the following formula: P = FH / w (P: interlayer adhesive strength (N / m), FH: horizontal cutting stress (N), w: cutting edge width of the cutting blade (m)).

[0121] As described above, the SAICAS method can be used to measure interlayer adhesion. However, when this method is used to measure the interlayer adhesion strength between an electrodeposition coating and an undercoat coating on an automotive paint, the measured values ​​can vary. This is because automotive paint has a relatively thick film thickness, and therefore the tensile stress on the cutting edge side and the strength of the upper layer of the paint film itself that is turned up by cutting affect the horizontal cutting stress. As a result, the measured value includes the force that resists these effects.

[0122] Therefore, in the present invention, we attempted to eliminate the influence of the thickness of the film cut from the surface of the coating film from the measurement value, thereby enabling more accurate measurement of interlayer adhesion strength. For the coating film to be measured, the coating film above the interface between the electrodeposition coating and the intermediate coating film, where interlayer adhesion strength is to be measured, is cut away in advance as shown in Figure 2. Next, a cutting blade is used to make an incision from the cut interface. Once the cutting blade has reached the interface between the electrodeposition coating and the intermediate coating, the cutting blade is moved only horizontally to measure the horizontal cutting stress (arrow in Figure 2). This measurement method is called the two-stage cutting method. The interlayer adhesion strength between coatings in the present invention is measured using this two-stage cutting method. This measurement method enables interlayer adhesion strength measurements to be performed with excellent reproducibility.

[0123] In the present invention, the interlayer adhesion strength (interlayer adhesion) between coating films is further measured by determining the "minimum adhesion strength." Here, "minimum adhesion strength" refers to the strength obtained by determining the lowest numerical value among the measurement results, as shown schematically in FIG. 3 . The adhesion strength of a coating film is generally evaluated by determining the "average adhesion strength," which is the average value of the measured adhesion strengths. On the other hand, the reason for determining the "minimum adhesion strength" in the present invention is that in actual coating films, peeling occurs from the weakest adhesion portion when subjected to impacts such as chipping. By determining the "minimum adhesion strength" between coating films with excellent reproducibility as in the present invention, it is possible to evaluate the peeling of the coating film more closely to the peeling that actually occurs.

[0124] In the present invention, a multilayer coating film in which the interlayer adhesion strength between the electrodeposition coating film and the intermediate coating film is 2.45 kN / m or more is preferred because it has excellent chipping resistance. If the interlayer adhesion strength is less than 2.45 kN / m, the minimum adhesive strength at the interface between the electrodeposition coating film and the intermediate coating film is low, and peeling of the coating film at the interface between the electrodeposition coating film and the intermediate coating film is likely to occur.

[0125] The interlayer adhesion is preferably 10 kN / m or less. If the interlayer adhesion exceeds 10 kN / m, the adhesion strength at the interface between the electrodeposition coating and the intermediate coating is strong, and peeling of the coating is unlikely to occur at the interface between the electrodeposition coating and the intermediate coating. However, there is a risk of a problem in that peeling at other interfaces, such as the substrate / electrodeposition coating interface, is more likely to occur in response to impacts such as chipping. Peeling at such locations is undesirable because it can significantly reduce the durability of the coating after peeling and increase the likelihood of rust, blistering, or peeling of the coating.

[0126] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" means "parts by mass" unless otherwise specified.

[0127] Production Example 1: Preparation of Hydroxyl-Containing Acrylic Resin Emulsion 126.5 parts of deionized water were added to a reaction vessel, and the temperature was raised to 80°C while mixing and stirring in a nitrogen stream. Next, a monomer emulsion consisting of 30 parts of a monomer mixture (containing 6.98 parts of ethyl acrylate, 12.42 parts of butyl acrylate, 4.75 parts of styrene, 2.78 parts of 2-hydroxyethyl methacrylate, and 3.07 parts of methacrylic acid), 0.33 parts of ADEKA Reasoap SR-10 (polyoxyethylene-1-alkoxymethyl-2-(2-propenyloxy)ethyl ether sulfate ester ammonium salt, manufactured by ADEKA Corporation), and 24 parts of deionized water was added dropwise to the reaction vessel over 1.5 hours, in parallel with an initiator solution consisting of 0.09 parts of ammonium persulfate and 3 parts of deionized water. After completion of the dropwise addition, the mixture was aged for 1 hour at the same temperature.

[0128] Next, a monomer emulsion consisting of 70 parts of a monomer mixture (containing 16.28 parts of ethyl acrylate, 28.97 parts of butyl acrylate, 15.25 parts of styrene, 6.5 parts of 2-hydroxyethyl methacrylate, and 3 parts of allyl methacrylate), 0.77 parts of Adeka Reasoap SR-10, and 56 parts of deionized water, and an initiator solution consisting of 0.21 parts of ammonium persulfate and 7 parts of deionized water were added dropwise to the reaction vessel over 1.5 hours in parallel. After completion of the addition, the mixture was aged at the same temperature for 1 hour.

[0129] The mixture was then cooled to 40°C and filtered through a 400-mesh filter. 20 parts of deionized water and 0.32 parts of dimethylaminoethanol were added to the filtrate to adjust the pH to 6.5. This yielded an emulsion of hydroxyl-containing acrylic resin (A1) with a core-shell multilayer structure having an average particle size of 100 nm, a Tg of 27°C, a nonvolatile content of 30%, an acid value of 20 mgKOH / g, and a hydroxyl value of 40 mgKOH / g.

[0130] Production Example 2: Preparation of Hydroxyl Group-Containing Polyester Resin 25.6 parts of isophthalic acid, 22.8 parts of phthalic anhydride, 5.6 parts of adipic acid, 19.3 parts of trimethylolpropane, 26.7 parts of neopentyl glycol, 17.5 parts of ε-caprolactone, and 0.1 parts of dibutyltin oxide were added to a reactor and heated to 170 ° C. with mixing and stirring. Thereafter, the temperature was raised to 220 ° C. over 3 hours, and water produced by the condensation reaction was removed until the acid value reached 8 mg KOH / g. Next, 7.9 parts of trimellitic anhydride was added, and the mixture was reacted at 150 ° C. for 1 hour to obtain a polyester resin with an acid value of 40 mg KOH / g. After further cooling to 100°C, 11.2 parts of butyl cellosolve was added and stirred until uniform. After cooling to 60°C, 98.8 parts of ion-exchanged water and 5.9 parts of dimethylethanolamine were added to obtain a hydroxyl-containing polyester resin with a solid content of 50% by mass, a solid acid value of 40 mgKOH / g, a hydroxyl value of 110 mgKOH / g, a number average molecular weight of 2870, and a glass transition temperature (Tg) of -3°C. The glass transition temperature (Tg) of the hydroxyl-containing polyester resin was calculated from the amounts of the various monomers used in the synthesis.

[0131] Production Example 3: Preparation of pigment dispersion paste 4.5 parts of a commercially available dispersant "Disperbyk 190" (anionic / nonionic dispersant, product name, manufactured by BYK-Chemie), 0.5 parts of an antifoaming agent "BYK-011" (antifoaming agent, manufactured by BYK-Chemie), 22.9 parts of ion-exchanged water, 72.1 parts of rutile titanium dioxide, and 27.2 parts of barium sulfate as an extender pigment were premixed, and then glass bead media was added in a paint conditioner, and the mixture was mixed and dispersed at room temperature until the particle size became 5 μm or less, to obtain a pigment dispersion paste.

[0132] Production Example 4: Production of water-soluble acrylic resin 23.89 parts of tripropylene glycol methyl ether and 16.11 parts of propylene glycol methyl ether were added to a reaction vessel, and the mixture was heated to 105°C while being mixed and stirred in a nitrogen stream. Next, an initiator solution consisting of 100 parts of the following monomer mixture, 10.0 parts of tripropylene glycol methyl ether, and 1 part of tert-butyl peroxy 2-ethylhexanoate was added dropwise to the reaction vessel in parallel over 3 hours. After completion of the dropwise addition, the mixture was aged at the same temperature for 0.5 hours.

[0133] Further, an initiator solution consisting of 5.0 parts of tripropylene glycol methyl ether and 0.3 parts of tertiary butyl peroxy 2-ethylhexanoate was added dropwise to the reaction vessel over 0.5 hours. After the completion of the addition, the mixture was aged at the same temperature for 2 hours.

[0134] Using a solvent remover, 16.1 parts of the solvent was distilled off under reduced pressure (70 torr) at 110°C, and then 204 parts of deionized water and 7.1 parts of dimethylaminoethanol were added to obtain a water-soluble acrylic resin solution. The resulting water-soluble acrylic resin solution had a nonvolatile content of 30%, a solids acid value of 40 mgKOH / g, a hydroxyl value of 50 mgKOH / g, and a viscosity of 140 poise (E-type viscometer, 1 rpm, 25°C).

[0135] Polyurethane Resin A urethane emulsion "Permarine UA-150" (manufactured by Sanyo Chemical Industries, Ltd., polyether-based urethane emulsion, resin solid content 30% by mass) was used.

[0136] Melamine Resin Imino-type melamine resins "Cymel 211" and "Cymel 370" (both manufactured by Allnex Japan Co., Ltd.) were mixed in a resin solids ratio of 1:1 and used.

[0137] Polyether polyol Sannix GP-1000 (manufactured by Sanyo Chemical Industries, Ltd.) was used.

[0138] Example 1: Formation of multi-layer coating film Preparation of aqueous primer coating composition 2.41 parts by mass of hydroxyl-containing acrylic resin emulsion (Em1) prepared in Production Example 1, 5.51 parts by mass of hydroxyl-containing polyester resin prepared in Production Example 2, 1.28 parts by mass of polyurethane resin "Permarine UA-150", 4.35 parts by mass of water-soluble acrylic resin prepared in Production Example 4, 8.42 parts by mass of melamine resin (a 1:1 mixture of resin solids of "Cymel 211" and "Cymel 370") as a curing agent, 2.41 parts by mass of polyether polyol resin 0.42 parts by mass of the pigment dispersion paste prepared in Production Example 3 was mixed with 0.46 parts by mass of lauryl acid phosphate and 0.49 parts by mass (pigment solids) of a brilliant aluminum pigment (manufactured by Toyo Aluminum Co., Ltd., Aluminum Paste WM-2068, volume-average average particle size D50: 15 μm, thickness 0.17 μm, aspect ratio 88) to obtain a water-based intermediate coating composition. The above parts by mass are parts by mass of solids. The volume-average particle size was measured by laser diffraction dispersion.

[0139] Formation of multilayer coating film (three-coat, one-bake coating) A zinc phosphate-treated dull steel plate was electrodeposited with Powernix 1010 (a cationic electrodeposition paint, product name, manufactured by Nippon Paint Automotive Coatings Co., Ltd.) to a dry coating film thickness of 15 μm, and the resulting coating was heat-cured at 170°C for 30 minutes and then cooled to prepare a steel plate substrate. Next, the aqueous primer coating composition prepared as described above was applied to the electrodeposited coated surface of the steel plate substrate by air spray coating to a dry coating film thickness of 20 μm. Thereafter, without going through a preheating step, the base coating composition Aqualex AR-3510 Silver Metallic (a water-based metallic base paint, product name, manufactured by Nippon Paint Automotive Coatings Co., Ltd.) was applied by air spray coating to a dry coating film thickness of 15 μm, and the resulting coating was preheated at 80°C for 3 minutes. Furthermore, a clear coating composition, Polyurexcel O-1200 Clear (two-component clear coating, product name, manufactured by Nippon Paint Automotive Coatings Co., Ltd.), was applied to the coated plate by air spray coating so that the dry coating film thickness was 35 μm, and then the plate was heat-cured at 140° C. for 20 minutes to obtain a test specimen.

[0140] The above water-based intermediate coating composition, water-based base coating composition and clear coating composition were diluted under the following conditions before use in coating.

[0141] Water-based intermediate coating composition Thinner: ion-exchanged water 900 mPa·s / 6 rpm / B-type viscometer The solid content of the coating was 48 mass %.

[0142] Water-based paint composition Thinner: Ion-exchanged water 3000 mPa·s / 6 rpm / B-type viscometer

[0143] Clear coating composition Thinner: EEP (ethoxyethyl propionate) / S-150 (aromatic hydrocarbon solvent, product name, manufactured by Exxon) mixed solvent = 1 / 1 (mass ratio) 30 seconds / No. 4 Ford cup / 20°C

[0144] Examples 2 to 7 and Comparative Examples 1 to 4 Aqueous intermediate coating compositions were prepared in the same manner as in Example 1, except that the amounts of each component were changed as shown in the table below. Using the resulting aqueous coating compositions, multi-layer coating films were formed in the same manner as in Example 1.

[0145] The appearance of the multi-layer coating film obtained after heat curing was evaluated according to the following criteria, and the results are shown in the table below.

[0146] [Chipping Resistance] Using a Gravelotester tester (Suga Testing Machines), a 250 g hexagonal nut M2 (brass material, no surface treatment plating) was impacted at a 45° angle from a distance of 35 cm with an air pressure of 5 kgf / cm2 onto the multilayer coating film formed by the above procedure (three-coat, one-bake coating). After rinsing and drying, the peeled coating pieces were removed using industrial gummed tape (Sliontec No. 3310), and the degree of peeling of the coating film was then visually observed. Chipping resistance was evaluated according to the following evaluation criteria based on the state of peeling of the coating film and zinc plating layer. In the following evaluation, a score of "slight peeling of the coating film" or higher was considered to be acceptable. ◯: No peeling of the coating film or slight peeling of the coating film was observed. △: Scattered peeling of the coating film of 2.5 mm or more was observed. ×: The area of ​​peeling of the coating film was large or the coating film was peeled.

[0147] [Chipping resistance of recoated portion] The chipping resistance of the recoated portion of the three-coat, one-bake coating was evaluated by forming an intermediate coating film / base coating film / clear coating film on the multi-layer coating film formed by the above three-coat, one-bake coating in the same manner as in the above three-coat, one-bake coating. Using test pieces having the resulting recoated multi-layer coating film, evaluation was carried out in the same manner as in the above chipping resistance evaluation, and the evaluation was based on the same criteria. The chipping resistance of the recoated portion of the three-coat, two-bake coating was evaluated by forming an intermediate coating film / base coating film / clear coating film on the multi-layer coating film formed by the above three-coat, two-bake coating in the same manner as in the above three-coat, two-bake coating. Using test pieces having the resulting recoated multi-layer coating film, evaluation was carried out in the same manner as in the above chipping resistance evaluation, and the evaluation was based on the same criteria.

[0148] Measurement of crosslink density of cured intermediate coating film Steel plate substrates having electrodeposition coating films were prepared in the same manner as described for the formation of the multilayer coating film above. The aqueous intermediate coating compositions prepared in the Examples and Comparative Examples were spray-painted onto the electrodeposition-coated surface of the resulting steel plate substrate to a dry film thickness of 20 μm, and then heat-cured at 140° C. for 20 minutes to obtain evaluation test pieces. The resulting intermediate coating film was measured using a dynamic viscoelasticity measuring instrument ("Vibron DDVII", manufactured by Toyo Baldwin Co., Ltd.) that measures viscoelasticity while applying minute vibrations, and the coating film crosslink density (n) was determined according to the above formula 1.

[0149] Measurement of Interlayer Adhesion Strength between Electrodeposited Coating and Cured Interlayer Coating The minimum adhesive strength of the laminated coating film prepared above was measured using a SAICAS CN-100 (manufactured by Daipura Intes Co., Ltd.). The coating film above the electrodeposited coating and interlayer coating, where interlayer adhesive strength was to be measured, was removed by cutting, leaving a portion 10 μm above the interface between the electrodeposited coating and the interlayer coating, as shown in Figure 2. Next, a cut was made with a cutting blade from the cut interface, and at a position 10 μm into the interface, the cutting blade was moved only horizontally to measure the horizontal cutting stress (see arrow in Figure 2). The minimum value of the measured stress was taken as the "minimum adhesive strength" (see Figure 3), and this minimum adhesive strength was taken as the interlayer adhesion strength. The results are shown in the table below.

[0150] Evaluation of the hue of intermediate coating films Steel substrates having electrodeposition coating films were prepared in the same manner as described for the formation of the multilayer coating films above. The aqueous intermediate coating compositions prepared in the Examples and Comparative Examples were air spray painted onto the electrodeposition-coated surfaces of the resulting steel substrates to a dry coating thickness of 15 μm, and then heat cured at 140° C. for 20 minutes to obtain test specimens for evaluation. The resulting test specimens were visually evaluated according to the following criteria. Evaluation criteria: ○: Almost no visible effect of the aluminum pigment △: Visible effect of the aluminum pigment (darkness, brightness, etc.) ×: Visible effect of the aluminum pigment (darkness, brightness, etc.)

[0151]

[0152] The present invention can be used as a method for forming a multi-layer coating film for automobiles.

[0153] 1: Vertical displacement gauge 5: Cutting edge 7: Coating film 9: Workpiece 11: Cutting method 13: Vertical load 15: Horizontal force 21: Upper coating film such as base coat and clear coat 23: Middle coating film 25: Electrodeposition coating film 27: Substrate

Claims

1. A method for forming a multi-layer coating film, comprising the steps of: an intermediate coating coating step (1) of coating an intermediate coating containing an aluminum pigment directly on an electrodeposition coating film formed on an object to be coated to form an uncured intermediate coating film; a base coating coating step (2) of coating a base coating composition on the uncured intermediate coating film to form an uncured base coating film; a preheating step (3) of drying the obtained uncured intermediate coating film and base coating film; a clear coating coating step (4) of coating a clear coating composition on the uncured base coating film to form an uncured clear coating film; and a baking step (5) of baking and curing the uncured intermediate coating film, the uncured base coating film and the uncured clear coating film simultaneously, wherein the intermediate coating composition contains an acrylic resin, a polyester resin and a curing agent, and the content of the aluminum pigment contained in the intermediate coating composition is 1.5% by mass or more and 3% by mass or less, as calculated by the following formula: aluminum pigment mass / resin solids mass×100, The method for forming a multi-layer coating film, wherein the crosslink density of the cured coating film of the intermediate coating composition is 1.76 to 1.94 mol / ml.

2. The method for forming a multi-layer coating film according to claim 1, wherein the intermediate coating composition contains 3 parts by mass or more of polyester resin per 100 parts by mass of resin solids.

3. The method for forming a multi-layer coating film according to claim 1 or 2, wherein the base coating film is a coating film formed by applying one or more base coating compositions.

4. A method for forming a multi-layer coating film according to claim 1 or 2, wherein the interlayer adhesion strength between the electrocoating film and the cured intermediate coating film is 2.45 kN / m or more.

5. The method for forming a multi-layer coating film according to claim 1, wherein the base coating coating step is a step of coating an uncured intermediate coating film with a base coating composition without preheating to form an uncured base coating film.

6. The method for forming a multi-layer coating film according to claim 1 or 2, wherein the aluminum pigment has a volume average particle diameter D50 of 5 to 20 μm and an average thickness of 0.01 to 0.3 μm.

Citation Information

Patent Citations

  • Method for forming brilliant coating film and coated article

    JP2002273329A

  • Method of coating car body and coating material composition used for the same

    JP2005185893A

  • Vehicle and vehicle coating method

    JP2019042720A

  • Multi-layer coating film forming method

    JP2019198861A

  • Multi-layered coating film formation method

    JP2022113338A