Decorative film
The decorative film with a UV ink-based, sequentially laminated structure addresses the limitations of conventional methods by ensuring high peel strengths and eliminating copper plates and organic solvents, offering enhanced design freedom and environmental sustainability.
Patent Information
- Application Number
- PCT/KR2024/003844
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-06-02
- Filing Date
- 2024-03-27
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional methods for manufacturing decorative films are limited by high production costs and time due to the need for copper plates, safety risks, and environmental concerns from organic solvent-based inks, with insufficient compatibility and peeling issues from digital printing.
A decorative film with a sequentially laminated structure comprising a base layer, a digital printing layer using UV ink composition, a first primer layer, and a transparent layer, ensuring peel strengths of at least 3.0 kgf/inch between layers to prevent cracking and peeling, and eliminating the need for copper plates and organic solvents.
This solution reduces production costs and time, enhances design freedom, and improves environmental sustainability by enabling eco-friendly production with improved adhesion and formability, suitable for various applications without the limitations of traditional methods.
Smart Images

Figure PCTKR2024003844-APPB-IMG-000001 
Figure PCTKR2024003844-APPB-IMG-000002 
Figure PCTKR2024003844-APPB-IMG-000003
Abstract
Description
Decorative film
[0001] The present invention relates to a decorative film having a high degree of design freedom and excellent formability.
[0002]
[0003] Decorative films, such as interior films, have been manufactured by forming a printing layer on a conventional PET, PVC, or other sheet using a printing method such as offset printing, gravure printing, or flexo printing, and various technologies for manufacturing decorative films using these methods have been proposed. For example, Patent Publication No. 2021-0077834 discloses an interior film and a manufacturing method thereof, including an adhesive layer comprising an acrylic copolymer, water, a tackifier, and an additive; a substrate layer comprising a heat stabilizer and a PVC resin; and a printing layer comprising a solvent having a boiling point of 120°C or lower.
[0004] Conventional methods require the production of copper plates (printing rolls) to implement a design onto a product. This process is expensive and time-consuming, limits the ability to vividly express images, and increases the risk of safety accidents and time-consuming process changes. Furthermore, the production of copper plates for design changes is expensive and time-consuming. Furthermore, because inks containing organic solvents are used, volatile organic compounds (VOCs) are emitted into the atmosphere during the ink drying process, degrading the work environment and contributing to environmental problems.
[0005] To address these issues, digital printers have been used. However, conventional ink compositions lack sufficient compatibility with film materials, print resolution, and peel strength. Consequently, cracks and film peeling occur when applied to products, resulting in poor formability. Therefore, there is a need for the development of decorative films that offer both high design freedom and superior formability.
[0006]
[0007] The present invention provides a decorative film having a high degree of design freedom and excellent formability.
[0008]
[0009] The present invention provides a decorative film comprising a sequentially laminated substrate layer, a printed layer formed by digital printing, a first primer layer, and a transparent layer, wherein the printed layer is formed of a UV ink composition, and the peel strength between the substrate layer and the printed layer is 3.0 kgf / inch or more, and the peel strength between the printed layer and the transparent layer is 3.0 kgf / inch or more.
[0010]
[0011] The present invention provides a decorative film that has a high degree of design freedom and excellent formability. According to the present invention, since there is no need to produce a printing plate, production costs and time can be reduced, thereby accelerating product development. Furthermore, since ink containing organic solvents is not used, products can be manufactured in an environmentally friendly manner. The decorative film of the present invention can be applied to interior films, home appliance films, deco films, lamination films, VCM (Vinyl Coated Metal), LVT (Luxury Vinyl Tile), and flooring (floor coverings).
[0012]
[0013] The present invention will be described in detail below. However, it is not limited to the following description, and each component may be modified or selectively mixed as needed. Therefore, it should be understood that all modifications, equivalents, and alternatives included within the spirit and technical scope of the present invention are included.
[0014] The “weight average molecular weight” used herein is measured by a conventional method known in the art, and can be measured, for example, by a gel permeation chromatography (GPC) method. The “glass transition temperature” is measured by a conventional method known in the art, and can be measured, for example, by a differential scanning calorimetry (DSC) method. The “particle size (D50)” is measured by a conventional method known in the art, and can be measured, for example, by a laser light scattering (LLS) method.
[0015] The decorative film of the present invention comprises a sequentially laminated substrate layer, a printed layer formed by digital printing, a first primer layer, and a transparent layer, wherein the printed layer is formed of a UV ink composition, and the peel strength between the substrate layer and the printed layer is 3.0 kgf / inch or more, and the peel strength between the printed layer and the transparent layer is 3.0 kgf / inch or more. Therefore, the decorative film of the present invention does not cause cracks or film peeling when applied to a product, and thus can be applied to products requiring high formability.
[0016] The above peel strength is the strength at which delamination occurs between layers when some layers are peeled off from the laminated layers, or at which a portion of a specific layer is torn off and peeled off.
[0017] The peel strength between the printed layer and the transparent layer refers to the peel strength at the point where peeling or partial separation of the transparent layer occurs during the process of peeling the printed layer from the transparent layer. When the substrate layer, the printed layer, the first primer layer, and the transparent layer are sequentially laminated, peeling between the printed layer and the transparent layer may occur between the printed layer and the first primer layer and / or between the first primer layer and the transparent layer, and for example, may occur between the printed layer and the first primer layer.
[0018] The peel strength between the substrate layer and the print layer refers to the peel strength at the point where peeling or partial separation of the print layer occurs during the process of peeling the print layer from the substrate layer. When the substrate layer, the second primer layer, the print layer, the first primer layer, and the transparent layer are sequentially laminated, peeling between the substrate layer and the print layer may occur between the substrate layer and the second primer layer and / or between the second primer layer and the print layer, and for example, between the second primer layer and the print layer.
[0019] For example, the peel strength can be measured by 180°Peeling using a Universal Testing Machine (UTM).
[0020] The peel strength between the substrate layer and the printed layer may be 3.0 kgf / inch or more, for example, 3.0 to 10 kgf / inch, another example, 3.5 to 8.0 kgf / inch, and another example, 5.0 to 6.0 kgf / inch. The peel strength between the printed layer and the transparent layer may be 3.0 kgf / inch or more, for example, 3.0 to 10 kgf / inch, another example, 3.5 to 8.0 kgf / inch, and another example, 5.0 to 6.0 kgf / inch.
[0021]
[0022] Substrate layer
[0023] A decorative film according to the present invention includes a substrate layer. The substrate layer serves as a support for the decorative film.
[0024] There is no particular limitation on the type of substrate constituting the above-mentioned substrate layer, but general materials used as substrate layers in decorative films for walls, floor tiles, wallpaper, etc. can be used. The substrate layer can be composed of a resin containing polyvinyl chloride (PVC), polyethylene terephthalate (PET), or a mixture thereof, or an inorganic substrate such as paper, a wood-based substrate, or a ceramic-based substrate, and these can be used alone or in combination of two or more. The substrate layer is usually in the form of a board, but can have various forms depending on the intended use of the decorative film, and the thickness, etc. can also be appropriately selected depending on the intended use. For example, when the substrate layer is composed of a resin containing PVC, PET, or a mixture thereof, the processability of the decorative film can be further improved.
[0025] The resin constituting the above-mentioned base layer may further include a thermoplastic resin used in the relevant technical field in addition to PVC and PET. The thermoplastic resin may include polyethylene terephthalate glycol resin (PETG resin), nylon, polybutylene terephthalate resin (PBT resin), acrylonitrile-butadiene-styrene resin (ABS resin), acrylonitrile-styrene-acrylic acid ester resin, acrylic resin, polyolefin resin, polycarbonate resin, etc., and these may be used alone or in combination of two or more.
[0026]
[0027] Print layer
[0028] The decorative film according to the present invention includes a printing layer on the substrate layer. The printing layer is formed by digital printing using a UV ink composition.
[0029] The printed layer can be formed using digital printing. The method of forming the digital print layer is not particularly limited, and can be formed using any known digital printing method. Digital printing is a known printing method that utilizes an electric signal-controlled ink discharge method, a non-contact printing method. It is advantageous for small and large-scale production of a variety of products, and it offers excellent design freedom and quality. When applying digital printing, full-width designs that cannot be achieved with gravure printing can be realized. Unlike gravure printing, there is no limit to the number of colors that can be realized, so multi-colors can be realized using various colors. Furthermore, digital printing can produce delicate soft tones that are difficult to achieve with gravure printing, and can also implement 3D effects. Furthermore, digital printing allows for precise focus alignment and can maximize the realism of natural materials such as fabric and wood.
[0030] Digital printing is typically performed using water-based inks, but the present invention utilizes UV inks. While water-based inks are limited in their application to media (e.g., paper and fabric) that can withstand the surface tension and drying temperature of water-based inks, UV inks enable printing on all media that cannot utilize water-based inks, including PVC, PET, acrylic, glass, polycarbonate, and corroflasks. For example, the UV ink of the present invention enables direct printing on PVC.
[0031] The above UV ink composition comprises a dispersion, an oligomer, a monomer and an initiator.
[0032] The dispersion may be a black dispersion, a cyan dispersion, a magenta dispersion, a yellow dispersion, or a mixture thereof, depending on the color to be realized. The average particle size (D50) of the dispersion may be 50 to 200 nm, and the viscosity change over time at room temperature may be less than ±30% compared to the initial value. If the average particle size (D50) of the dispersion is outside the above-mentioned range, the pigment dispersion stability may be reduced, resulting in poor ink stability. The dispersion may be included in an amount of 5 to 30 wt% based on the total weight of the UV ink composition.
[0033] The oligomers mentioned above may include polyester oligomers, urethane oligomers, epoxy oligomers, and acrylic oligomers. These may be used alone or in combination of two or more. The oligomers may have a functional group number of 1 to 6 and a weight average molecular weight of 100 to 10,000 g / mol. If the number of functional groups of the oligomer exceeds the above-mentioned range, the hardness of the ink printing surface may increase, resulting in reduced flexibility and breakage. In addition, if the molecular weight of the oligomer exceeds the above-mentioned range, the ink output stability may deteriorate during inkjet printing. The oligomer may be included in an amount of 1 to 30 wt% based on the total weight of the UV ink composition.
[0034] The above monomer controls the viscosity of the UV ink composition, thereby enabling easier coating. The monomer may be an acrylate monomer having a molecular weight of 100 to 1,000 g / mol and a glass transition temperature of -100 to 150°C. If the molecular weight of the monomer is less than the above-mentioned range, it may cause under-curing of the UV ink, and if it exceeds the above-mentioned range, it may cause over-curing, which may increase the hardness of the coating film and make it vulnerable to external impact. In addition, if the glass transition temperature of the monomer exceeds the above-mentioned range, the adhesion with the primer may decrease, resulting in a decrease in peel strength.
[0035] As the monomers, monofunctional monomers such as cyclic trimethylol propane formal acrylate (CTFA), phenoxy ethyl acrylate (PHEA), ethoxy ethoxy ethyl acrylate (EOEOEA), isobornyl acrylate (IBOA), and hydroxy propyl acrylate (HPA) can be used; bifunctional monomers such as hexanediol diacrylate (HDDA), diethylene glycol diacrylate (DEGDA), tripropylene glycol diacrylate (TPGDA), dipropylene glycol diacrylate (DPGDA), triethylene glycol diacrylate (TEGDA), neopentyl glycol diacrylate (NPGDA), and polyethylene glycol diacrylate (PEGDA) can be used; and multifunctional monomers such as trimethylol propane triacrylate (TMPTA), pentaerythritol triacrylate (PETA), and dipentaerythritol hexaacrylate (DPHA) can be used. These may be used alone or in combination of two or more. The monomer may be included in an amount of 10 to 80 wt% based on the total weight of the UV ink composition.
[0036] Examples of the initiator include trioxanthine, monoacylphosphine, phenyl acylphosphine, α-amino ketone, and α-hydroxy ketone. These may be used alone or in combination of two or more. The initiator may be included in an amount of 0.1 to 15 wt% based on the total weight of the UV ink composition.
[0037]
[0038] First primer layer
[0039] The decorative film according to the present invention comprises a first primer layer on a printed layer. The first primer layer serves to improve the adhesion between the printed layer and the transparent layer, maintain the smoothness of the fabric, uniformly print color, and increase the tensile strength, thereby improving workability.
[0040] The first primer layer is formed of a first primer composition. The first primer composition may be a solvent-based primer composition or a UV-curable primer composition.
[0041] The above first primer composition is a solvent-based primer composition and may be a polyurethane primer composition or a polyester primer composition.
[0042] For example, the first primer composition may be a polyurethane primer composition comprising 8 to 40 wt% of a polyurethane resin, 0.1 to 6 wt% of a curing agent, and 55 to 90 wt% of a solvent.
[0043] The polyurethane resin allows the printed layer to adhere more strongly to the transparent layer. Any known polyurethane resin can be used as the polyurethane resin without particular limitation, and for example, a reaction product of a polyol and an isocyanate can be used. The polyol can be polyester polyol, polyether polyol, or polycarbonate polyol, and polyester polyol is preferred, but is not limited thereto.
[0044] The weight average molecular weight of the polyurethane resin may be 5,000 to 100,000 g / mol, and the glass transition temperature may be -30 to 60°C. If the weight average molecular weight of the polyurethane resin is less than the aforementioned range, the interlayer adhesiveness with the transparent layer may be reduced, and if it exceeds the aforementioned range, the viscosity of the coating solution may be high, which may cause unevenness of the coating surface after high-speed gravure roll coating. In addition, if the glass transition temperature of the polyurethane resin is less than the aforementioned range, the solvent resistance may be reduced, causing swelling by UV ink and peeling of the surface, and if it exceeds the aforementioned range, the resin layer may become hard, which may reduce the adhesion with the transparent layer.
[0045] As the above hardener, hexamethylene diisocyanate trimer (HDI trimer), isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), diphenyl methane diisocyanate (MDI), xylene diisocyanate (XDI), etc. can be used.
[0046] The solvent may be a quick-drying solvent such as methyl ethyl ketone, acetone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methanol, ethanol, propanol, toluene, and the like, and may include, for example, 40 to 61 wt% of methyl ethyl ketone and 15 to 29 wt% of ethyl acetate.
[0047] As another example, the first primer composition may be a polyester primer composition comprising 8 to 40 wt% of a polyester resin, 0.1 to 6 wt% of a curing agent, and 55 to 90 wt% of a solvent.
[0048] The weight average molecular weight of the polyester resin may be 5,000 to 100,000 g / mol, and the glass transition temperature may be -25 to 65°C. If the weight average molecular weight of the polyester resin is less than the aforementioned range, the interlayer adhesiveness with the transparent layer may be reduced, and if it exceeds the aforementioned range, the viscosity of the coating solution may be high, which may cause unevenness of the coating surface after high-speed gravure roll coating. In addition, if the glass transition temperature of the polyester resin is less than the aforementioned range, the solvent resistance may be reduced, causing swelling by UV ink and peeling of the surface, and if it exceeds the aforementioned range, the resin layer may become hard, which may reduce the adhesion with the transparent layer.
[0049] As the above hardener, hexamethylene diisocyanate trimer (HDI trimer), isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), diphenyl methane diisocyanate (MDI), xylene diisocyanate (XDI), etc. can be used.
[0050] The solvent may be a quick-drying solvent such as methyl ethyl ketone, acetone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methanol, ethanol, propanol, toluene, and the like, and may include, for example, 40 to 61 wt% of methyl ethyl ketone and 15 to 29 wt% of ethyl acetate.
[0051] The first primer composition may be a UV-curable primer composition. The UV-curable primer may include an oligomer, a monomer, and an initiator. For example, the first primer composition may include 10 to 60 wt% of the oligomer, 10 to 80 wt% of the monomer, and 0.1 to 15 wt% of the initiator, based on the total weight of the first primer composition.
[0052] The oligomers mentioned above may include polyester oligomers, urethane oligomers, epoxy oligomers, and acrylic oligomers. These may be used alone or in combination of two or more. The oligomers may have a functional group number of 2 to 6 and a molecular weight of 100 to 10,000 g / mol. If the functional group number of the oligomer is less than the above-mentioned range, UV curing may be difficult and adhesion performance may be reduced, and if it exceeds the above-mentioned range, the hardness of the primer layer may increase, causing the primer layer to break or crack, which may affect the quality of the finished product.
[0053] The above monomer controls the viscosity of the primer composition, thereby enabling easier coating. The monomer may be an acrylate monomer having a molecular weight of 100 to 1,000 g / mol and a glass transition temperature of -100 to 150°C. If the molecular weight of the monomer is less than the above-mentioned range, problems may occur in UV curing, and if it exceeds the above-mentioned range, the hardness of the primer layer may increase, resulting in breakage or cracking of the primer layer. In addition, if the molecular weight is outside the above-mentioned range, the peel strength may be reduced. On the other hand, if the glass transition temperature of the monomer is outside the above-mentioned range, the peel strength may be reduced.
[0054] As the monomers, monofunctional monomers such as cyclic trimethylol propane formal acrylate (CTFA), phenoxy ethyl acrylate (PHEA), ethoxy ethoxy ethyl acrylate (EOEOEA), isobornyl acrylate (IBOA), and hydroxy propyl acrylate (HPA) can be used; bifunctional monomers such as hexanediol diacrylate (HDDA), diethylene glycol diacrylate (DEGDA), tripropylene glycol diacrylate (TPGDA), dipropylene glycol diacrylate (DPGDA), triethylene glycol diacrylate (TEGDA), neopentyl glycol diacrylate (NPGDA), and polyethylene glycol diacrylate (PEGDA) can be used; and multifunctional monomers such as trimethylol propane triacrylate (TMPTA), pentaerythritol triacrylate (PETA), and dipentaerythritol hexaacrylate (DPHA) can be used. These can be used alone or in combination of two or more.
[0055] Trioxanthine, monoacylphosphine, phenyl acylphosphine, α-amino ketone, α-hydroxy ketone, etc. can be used as the above initiator. These can be used alone or in combination of two or more.
[0056] The above first primer layer may be formed with a thickness of 2 to 5 μm. If the thickness of the above first primer layer is less than the above-mentioned range, adhesion and heat resistance may be reduced, and if it exceeds the above-mentioned range, workability may be reduced due to poor drying, etc.
[0057]
[0058] transparent layer
[0059] The decorative film according to the present invention includes a transparent layer on a first primer layer. The transparent layer serves to protect the printed layer or the first primer layer, and maintains the durability, chemical resistance, wear resistance, etc. of the final product. The transparent layer may be formed of a known material such as PVC (Poly Vinyl Chloride), but is not limited thereto. The thickness of the transparent layer is not particularly limited, and may range from 0.05 to 1.0 mm, for example.
[0060]
[0061] Second primer layer
[0062] The decorative film according to the present invention may further include a second primer layer between the substrate layer and the printing layer. The second primer layer serves to improve the adhesion between the substrate layer and the printing layer, to make the printing surface uniform, to increase the roll fabric leading stability, thereby improving printing quality, and to increase the tensile strength, thereby improving workability.
[0063] The second primer layer is formed of a second primer composition. The second primer composition may be a solvent-based primer composition or a UV-curable primer composition.
[0064] The above second primer composition is a solvent-based primer composition, and may be a polyurethane primer composition or a polyester primer composition.
[0065] For example, the second primer composition may be a polyurethane primer composition comprising 8 to 40 wt% of a polyurethane resin, 0.1 to 6 wt% of a curing agent, and 55 to 90 wt% of a solvent.
[0066] The polyurethane resin allows the printed layer to adhere more strongly to the substrate layer. Any known polyurethane resin can be used as the polyurethane resin without particular limitation. For example, a reaction product of a polyol and an isocyanate can be used. Polyester polyol, polyether polyol, or polycarbonate polyol can be used as the polyol, and polyester polyol is preferred, but is not limited thereto.
[0067] The weight average molecular weight of the polyurethane resin may be 5,000 to 100,000 g / mol, and the glass transition temperature may be -30 to 60°C. If the weight average molecular weight of the polyurethane resin is less than the aforementioned range, the interlayer adhesiveness with the printing layer may be reduced, and if it exceeds the aforementioned range, the viscosity of the coating solution may be high, which may cause unevenness of the coating surface after high-speed gravure roll coating. In addition, if the glass transition temperature of the polyurethane resin is less than the aforementioned range, the solvent resistance may be reduced, causing swelling by UV ink and peeling of the surface, and if it exceeds the aforementioned range, the resin layer may become hard, which may reduce the adhesion with the printing layer.
[0068] As the above hardener, hexamethylene diisocyanate trimer (HDI trimer), isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), diphenyl methane diisocyanate (MDI), xylene diisocyanate (XDI), etc. can be used.
[0069] The solvent may be a quick-drying solvent such as methyl ethyl ketone, acetone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methanol, ethanol, propanol, toluene, and the like, and may include, for example, 40 to 61 wt% of methyl ethyl ketone and 15 to 29 wt% of ethyl acetate.
[0070] As another example, the second primer composition may be a polyester primer composition comprising 8 to 40 wt% of a polyester resin, 0.1 to 6 wt% of a curing agent, and 55 to 90 wt% of a solvent.
[0071] The weight average molecular weight of the polyester resin may be 5,000 to 100,000 g / mol, and the glass transition temperature may be -25 to 65°C. If the weight average molecular weight of the polyester resin is less than the above-mentioned range, the interlayer adhesiveness with the printing layer may be reduced, and if it exceeds the above-mentioned range, the viscosity of the coating solution may be high, which may cause unevenness of the coating surface after high-speed gravure roll coating. In addition, if the glass transition temperature of the polyester resin is less than the above-mentioned range, the solvent resistance may be reduced, causing swelling by UV ink and peeling of the surface, and if it exceeds the above-mentioned range, the resin layer may become hard, which may reduce the adhesion with the printing layer.
[0072] As the above hardener, hexamethylene diisocyanate trimer (HDI trimer), isophorone diisocyanate (IPDI), toluene diisocyanate (TDI), diphenyl methane diisocyanate (MDI), xylene diisocyanate (XDI), etc. can be used.
[0073] The solvent may be a quick-drying solvent such as methyl ethyl ketone, acetone, methyl isobutyl ketone, ethyl acetate, butyl acetate, methanol, ethanol, propanol, toluene, and the like, and may include, for example, 40 to 61 wt% of methyl ethyl ketone and 15 to 29 wt% of ethyl acetate.
[0074] The second primer composition may be a UV-curable primer composition. The UV-curable primer may include an oligomer, a monomer, and an initiator. For example, the second primer composition may include 10 to 60 wt% of the oligomer, 10 to 80 wt% of the monomer, and 0.1 to 15 wt% of the initiator, based on the total weight of the second primer composition.
[0075] The oligomers mentioned above may include polyester oligomers, urethane oligomers, epoxy oligomers, and acrylic oligomers. These may be used alone or in combination of two or more. The oligomers may have a functional group number of 2 to 6 and a molecular weight of 100 to 10,000 g / mol. If the functional group number of the oligomer is less than the above-mentioned range, UV curing may be difficult and adhesion performance may be reduced, and if it exceeds the above-mentioned range, the hardness of the primer layer may increase, causing the primer layer to break or crack, which may affect the quality of the finished product.
[0076] The above monomer controls the viscosity of the primer composition, thereby enabling easier coating. The monomer may be an acrylate monomer having a molecular weight of 100 to 1,000 g / mol and a glass transition temperature of -100 to 150°C. If the molecular weight of the monomer is less than the above-mentioned range, problems may occur in UV curing, and if it exceeds the above-mentioned range, the hardness of the primer layer may increase, resulting in breakage or cracking of the primer layer. In addition, if the molecular weight is outside the above-mentioned range, the peel strength may be reduced. On the other hand, if the glass transition temperature of the monomer is outside the above-mentioned range, the peel strength may be reduced.
[0077] As the monomers, monofunctional monomers such as cyclic trimethylol propane formal acrylate (CTFA), phenoxy ethyl acrylate (PHEA), ethoxy ethoxy ethyl acrylate (EOEOEA), isobornyl acrylate (IBOA), and hydroxy propyl acrylate (HPA) can be used; bifunctional monomers such as hexanediol diacrylate (HDDA), diethylene glycol diacrylate (DEGDA), tripropylene glycol diacrylate (TPGDA), dipropylene glycol diacrylate (DPGDA), triethylene glycol diacrylate (TEGDA), neopentyl glycol diacrylate (NPGDA), and polyethylene glycol diacrylate (PEGDA) can be used; and multifunctional monomers such as trimethylol propane triacrylate (TMPTA), pentaerythritol triacrylate (PETA), and dipentaerythritol hexaacrylate (DPHA) can be used. These can be used alone or in combination of two or more.
[0078] Trioxanthine, monoacylphosphine, phenyl acylphosphine, α-amino ketone, α-hydroxy ketone, etc. can be used as the above initiator. These can be used alone or in combination of two or more.
[0079] The second primer layer may be formed to a thickness of 1 to 3 μm. If the thickness of the second primer layer is less than the aforementioned range, adhesion and heat resistance may be reduced, and if it exceeds the aforementioned range, workability may be reduced due to poor drying, etc.
[0080]
[0081] Hereinafter, the present invention will be described in more detail through examples. However, the following examples are intended only to aid understanding of the present invention and are not intended to limit the scope of the present invention in any way.
[0082]
[0083] [Manufacturing Example 1: Preparation of primer composition]
[0084] According to Table 1 below, each primer composition was prepared.
[0085]
[0086]
[0087] PUD resin: Modified polyurethane resin (weight average molecular weight 10,000 g / mol, glass transition temperature 51 ℃, hydroxyl value 70 mgKOH / g)
[0088] PE resin: Unsaturated polyester resin (weight average molecular weight 51,000 g / mol, glass transition temperature 62 ℃, hydroxyl value 80 mgKOH / g)
[0089] Curing agent: hexamethylene diisocyanate trimer
[0090] Solvent: methyl ethyl ketone
[0091]
[0092] [Manufacturing Example 2: Preparation of UV ink composition]
[0093] According to Table 2 below, each ink composition was prepared.
[0094]
[0095]
[0096] Dispersion: Pigment (Color Black S160) 15 wt%, dispersant (BYK-9152) 7 wt%, solvent (ethoxy ethoxy ethyl acrylate (EOEOEA)) 78 wt%
[0097] Oligomer: Bifunctional Aliphatic Urethane Acrylate (weight average molecular weight 1,000 g / mol, viscosity (25℃) 11,430 cps)
[0098] HDDA: 1,6-Hexanediol diacrylate
[0099] THFA: Tetrahydrofurfuryl acrylate
[0100] PHEA: 2-Phenoxyethyl acrylate
[0101] EOEOEA: 2-(2-Ethoxyethoxy) Ethyl Acrylate
[0102] TPO: 2,4,6-trimethylbenzoyldiphenyl phosphine oxide
[0103]
[0104] [Experimental Example 1-22]
[0105] A second primer composition was applied to the upper surface of the substrate sheet to form a second primer layer (thickness 2-3 ㎛), a printed layer was formed by digital printing using a UV ink composition, a first primer composition was applied to form a first primer layer (thickness 2-3 ㎛), and a transparent layer was laminated. By the above method, a decorative film for each experimental example was manufactured in which the substrate layer / second primer layer / printed layer / first primer layer / transparent layer having the configuration of Table 3-5 were laminated in that order.
[0106]
[0107]
[0108]
[0109]
[0110] A-1: Primer composition of manufacturing example 1 (A-1)
[0111] A-2: Primer composition of manufacturing example 1 (A-2)
[0112] A-3: Primer composition of manufacturing example 1 (A-3)
[0113] A-4: Primer composition of manufacturing example 1 (A-4)
[0114] B-1: UV ink composition of manufacturing example 2 (B-1)
[0115] B-2: UV ink composition of manufacturing example 2 (B-2)
[0116] B-3: Water-based latex ink (LX100, MIMAKI)
[0117] B-4: Oil-based ink (SS21, MIMAKI)
[0118]
[0119] [Physical property evaluation]
[0120] The physical properties of the decorative film manufactured in each experimental example were measured using the following method, and the results are shown in Table 6-8 below.
[0121]
[0122] Peel strength
[0123] Using a tensile tester (Universal Testing Machine, manufacturer: SALT, model number: ST-1003), the 180° peel strength between the substrate layer and the printed layer of the decorative film for each experimental example and the 180° peel strength between the printed layer and the transparent layer were measured.
[0124]
[0125]
[0126]
[0127] As shown in Table 3-8 above, the decorative film of Experimental Examples 1-17 includes a substrate layer, a printed layer formed with a UV ink composition through digital printing, a first primer layer, and a transparent layer, and the peel strength between the substrate layer and the printed layer and the peel strength between the printed layer and the transparent layer were both 3.0 kgf / inch or more. In particular, in the case of the decorative film including the substrate layer, the second primer layer, the printed layer, the first primer layer, and the transparent layer (Experimental Examples 5-8, 13-17), the peel strength between the substrate layer and the printed layer and the peel strength between the printed layer and the transparent layer were both 4.0 kgf / inch or more, which were even better.
[0128] On the other hand, in Experimental Example 18, which does not include the first primer layer and the second primer layer, and in Experimental Examples 19-22, which form the printed layer using water-based latex ink (B-3) or oil-based ink (B-4) instead of UV ink and do not include the first primer layer, the peel strength between the substrate layer and the printed layer and the peel strength between the printed layer and the transparent layer were both less than 3.0 kgf / inch.
[0129]
[0130] The present invention provides a decorative film having a high degree of design freedom and excellent formability.
[0131]
Claims
1. It includes a sequentially laminated substrate layer, a printed layer formed by digital printing, a first primer layer, and a transparent layer, The above printing layer is formed with a UV ink composition, The peel strength between the above substrate layer and the above printing layer is 3.0 kgf / inch or more, A decorative film having a peel strength of 3.0 kgf / inch or more between the printed layer and the transparent layer.
2. A decorative film further comprising a second primer layer between the substrate layer and the printing layer in the first paragraph.
3. In the second paragraph, the second primer layer is formed of a second primer composition, The above second primer composition is a solvent-based primer composition or a UV-curable primer composition, The above solvent-based primer composition is a polyurethane primer composition or a polyester primer composition, The above polyurethane primer composition comprises 8 to 40 wt% of polyurethane resin, 0.1 to 6 wt% of curing agent, and 55 to 90 wt% of solvent, A decorative film comprising the polyester primer composition comprising 8 to 40 wt% of a polyester resin, 0.1 to 6 wt% of a curing agent, and 55 to 90 wt% of a solvent.
4. In the first paragraph, the first primer layer is formed of a first primer composition, The above first primer composition is a solvent-based primer composition or a UV-curable primer composition, The above solvent-based primer composition is a polyurethane primer composition or a polyester primer composition, The above polyurethane primer composition comprises 8 to 40 wt% of polyurethane resin, 0.1 to 6 wt% of curing agent, and 55 to 90 wt% of solvent, A decorative film comprising the polyester primer composition comprising 8 to 40 wt% of a polyester resin, 0.1 to 6 wt% of a curing agent, and 55 to 90 wt% of a solvent.
5. In the third or fourth paragraph, the weight average molecular weight of the polyurethane resin is 5,000 to 100,000 g / mol and the glass transition temperature is -30 to 60 ℃, A decorative film having a weight average molecular weight of the polyester resin of 5,000 to 100,000 g / mol and a glass transition temperature of -25 to 65°C.
6. In the first paragraph, the UV ink composition comprises a dispersion, an oligomer, a monomer and an initiator, The average particle size (D50) of the above dispersion is 50 to 200 nm, and the change in viscosity over time at room temperature is less than ± 30% compared to the initial value, The number of functional groups of the above oligomer is 1 to 5, and the weight average molecular weight is 100 to 10,000 g / mol, A decorative film comprising an acrylate monomer having a molecular weight of 100 to 1,000 g / mol and a glass transition temperature of -100 to 150°C.
Citation Information
Patent Citations
Hydraulic transferring film and hydraulically transferred body
JP2006051672A
Water pressure transfer method, coating agent for water pressure transfer film, and water pressure transfer article
KR1020140020992A
Lens assembly and camera module including the same
KR1020220024343A
Water dispensing apparatus
KR1020220098535A
Rebar Support Integrated Insert
KR102460772B1