Electrode assembly including adhesive insulating coating parts and electrochemical device including same

The electrode assembly with an insulating coating using inorganic particles and binders with varying glass transition temperatures addresses the adhesion issues in lithium secondary batteries, enhancing safety by preventing short circuits and maintaining structural integrity.

WO2024248389A1PCT designated stage expired Publication Date: 2024-12-05LG ENERGY SOLUTION LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/006854
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-26
Filing Date
2024-05-21
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Lithium secondary batteries used in electric and hybrid vehicles face issues with short circuits due to inadequate adhesion between the anode and cathode, leading to safety concerns such as explosions and fires, as existing insulating materials like PVDF-based resins fail to provide sufficient adhesion and are prone to detachment or dissolution by the electrolyte.

Method used

An electrode assembly with an insulating coating around the active material layer, comprising inorganic particles and a binder with two types of adhesive binders having different glass transition temperatures, which enhances the adhesion between the electrode and separator, ensuring wet adhesion of 1 to 20 gf/20 mm and improving the structural integrity of the battery.

Benefits of technology

The proposed solution effectively prevents short circuits and enhances the safety of lithium secondary batteries by maintaining strong adhesion between the electrodes, even when exposed to electrolytes, thereby reducing the risk of explosions and fires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024006854_05122024_PF_FP_ABST
    Figure KR2024006854_05122024_PF_FP_ABST
Patent Text Reader

Abstract

An electrode assembly according to one aspect of the present invention is characterized by comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, and at least one of the positive electrode and the negative electrode comprises: a current collector; an active material layer formed on at least one surface of the current collector; and an insulating coating part formed on the entire outer periphery of one surface of the active material layer, wherein a wet adhesive strength between the positive electrode or the negative electrode provided with the insulating coating portion and the separator is 1 to 20 gf / 20 mm, and the electrode assembly has excellent wet adhesive strength between an electrode and the separator and thereby improves a folding phenomenon of the separator, and accordingly, has an advantage of enhancing safety of an electrochemical device.
Need to check novelty before this filing date? Find Prior Art

Description

Electrode assembly including an adhesive insulating coating portion and an electrochemical device including the same

[0001] The present invention relates to an electrode assembly including an insulating coating portion and an electrochemical device including the same.

[0002] This application claims priority to Korean Patent Application No. 2023-0068575, filed with the Korean Intellectual Property Office on May 26, 2023, the entire disclosure of which is incorporated herein by reference.

[0003] As technological developments and demand for mobile devices increase, the demand for secondary batteries as an energy source is rapidly increasing. Recently, secondary batteries are being used as power sources for electric vehicles (EVs) and hybrid electric vehicles (HEVs). Accordingly, extensive research is being conducted on secondary batteries that can meet diverse needs.

[0004] In particular, demand is high for lithium secondary batteries with high energy density, high discharge voltage, and output stability. Among these, lithium secondary batteries, used as power sources for electric and hybrid electric vehicles, require high-power characteristics capable of delivering large outputs in a short period of time. There is ongoing interest in improving battery safety for these batteries.

[0005] Meanwhile, secondary batteries can be classified into jelly-roll electrode assemblies, stacked electrode assemblies, and stacked / folded electrode assemblies depending on the structure of the electrode assembly, and the electrode assembly basically includes three elements of anode / separator / cathode as basic components.

[0006] Conventional electrode assemblies have a laminated structure with a separator interposed between the anode and cathode, each with a protruding electrode tab on one side. However, this structure presents a problem where, if exposed to an external heat source or an internal short circuit causes the temperature to rise and the separator to shrink, parts of the anode and cathode may come into contact, resulting in a short circuit.

[0007] Accordingly, research is being conducted to address these issues by utilizing insulating materials, such as inserting an insulating layer into portions of the electrode assembly. For example, research is underway to prevent short circuits, lithium precipitation, and ignition by incorporating an insulating layer using PVDF resin into the anode.

[0008] However, the PVDF-based insulating material being researched and developed has been reported to have problems such as detachment due to insufficient adhesiveness, or dissolution by the electrolyte when the electrolyte is poured into the electrode assembly. In addition, there are still reports of a short circuit phenomenon in which the adhesive strength between each component of the electrode assembly is reduced, and the separator is folded without being adhered to the electrode, causing parts of the positive and negative electrodes to come into contact.

[0009] Therefore, the present invention solves the above-described problem,

[0010] The present invention aims to provide an electrode assembly that effectively solves the short-circuit problem between the positive and negative electrodes and an electrochemical device including the same.

[0011] In particular, the electrode assembly of the present invention includes an insulating coating portion, and is intended to provide an electrode assembly having excellent adhesion between the electrode and the separator.

[0012] For example, the electrode assembly of the present invention includes an insulating coating portion, and is intended to provide an electrode assembly having excellent adhesion between the anode and the separator.

[0013] To solve the above problem,

[0014] According to one aspect of the present invention, electrode assemblies of the following embodiments are provided.

[0015] An electrode assembly according to the first embodiment comprises:

[0016] An electrode assembly having an anode, a cathode, and a separator interposed between the anode and the cathode,

[0017] At least one of the positive electrode and the negative electrode comprises a current collector; an active material layer formed on at least one surface of the current collector; and an insulating coating formed around the entire outer periphery of one surface of the active material layer;

[0018] The wet adhesive strength between the positive or negative electrode provided with the insulating coating and the separator is 1 to 20 gf / 20 mm.

[0019] According to the second embodiment, in the first embodiment,

[0020] At least one of the positive electrode and the negative electrode may include an active material layer on each side of the current collector; and an insulating coating formed around the entire outer periphery of one side of each of the active material layers.

[0021] According to the third embodiment, in the first embodiment or the second embodiment,

[0022] The above insulating coating portion includes inorganic particles and a binder,

[0023] The above binder may include two types of adhesive binders having a glass transition temperature (Tg) difference of 100°C or less.

[0024] According to the fourth embodiment, in any one of the first to third embodiments,

[0025] The above insulating coating portion includes inorganic particles and a binder,

[0026] The above binder may include a first adhesive binder having a glass transition temperature (Tg) of 50°C or higher, and a second adhesive binder having a glass transition temperature (Tg) of 20°C or lower.

[0027]

[0028] According to another aspect of the present invention, an insulating coating composition of the following embodiments is provided.

[0029] The composition for insulating coating according to the fifth embodiment is:

[0030] Containing inorganic particles and binders,

[0031] The above binder may include two types of adhesive binders having a difference in glass transition temperature (Tg) of 100°C or less.

[0032] The composition for insulating coating according to the sixth embodiment is:

[0033] Containing inorganic particles and binders,

[0034] The above binder may include a first adhesive binder having a glass transition temperature (Tg) of 50°C or higher, and a second adhesive binder having a glass transition temperature (Tg) of 20°C or lower.

[0035] According to the seventh embodiment, in the sixth embodiment,

[0036] The above first adhesive binder may include an aqueous particulate binder.

[0037] According to the eighth embodiment, in the sixth embodiment or the seventh embodiment,

[0038] The above first adhesive binder may include an aqueous particle-type binder having a particle size of 250 nm or more.

[0039] According to the ninth embodiment, in any one of the sixth to eighth embodiments,

[0040] The second adhesive binder may include an aqueous particle-type binder, a solution-type binder, or a mixture thereof.

[0041] According to the tenth embodiment, in any one of the sixth to ninth embodiments,

[0042] The second adhesive binder may include an aqueous particle-type binder having a particle size of 250 nm or less.

[0043] According to the eleventh embodiment, in any one of the sixth to tenth embodiments,

[0044] The weight ratio of the first adhesive binder and the second adhesive binder may be 1:9 to 9:1.

[0045] According to the 12th embodiment, in any one of the 5th to 11th embodiments,

[0046] The weight ratio of the above-mentioned inorganic particles and the above-mentioned binder may be 7:3 to 9:1.

[0047]

[0048] According to another aspect of the present invention, electrochemical devices of the following embodiments are provided.

[0049] The electrochemical device according to the 13th embodiment,

[0050] An electrode assembly according to any one of the first to fourth embodiments may be housed in a case.

[0051]

[0052] According to another aspect of the present invention, a method for manufacturing an electrode assembly of the following embodiments is provided.

[0053] A method for manufacturing an electrode assembly according to the 14th embodiment is as follows:

[0054] A step of preparing a current collector and an electrode having an active material layer on at least one surface of the current collector,

[0055] A step of forming an insulating coating portion including inorganic particles and a binder around the entire outer periphery of one side of the active material layer, and

[0056] It includes a step of rolling after contacting a separator with a surface on which the insulating coating portion is formed,

[0057] The above electrode is at least one of an anode and a cathode,

[0058] The wet adhesion between the electrode and the separator on which the insulating coating is formed may be 1 to 20 gf / 20 mm.

[0059] An electrode assembly according to one embodiment of the present invention can exhibit the effect of increasing the adhesive strength between the electrode and the separator and suppressing the occurrence of a short between the electrodes by having an adhesive insulating coating portion around the outer periphery of the electrode.

[0060] This can have a beneficial effect on improving safety by reducing the risk of explosion and fire caused by the above paragraph.

[0061] FIG. 1 illustrates an embodiment in which an electrode active material layer (11) is formed on a current collector having a tab portion (1) formed thereon according to one embodiment of the present invention, and an insulating coating portion (20) is formed around the entire outer periphery of one surface of the electrode active material layer.

[0062] FIG. 2 is a side view of one embodiment of an assembly in which an electrode active material layer (11), an insulating coating portion (20), and a separator (30) are sequentially laminated on a current collector (10) having a tab portion (1) formed thereon according to one embodiment of the present invention.

[0063] FIG. 3 is a vertical cross-sectional view of the central portion of one embodiment of an assembly in which an electrode active material layer (11), an insulating coating portion (20), and a separator (30) are sequentially laminated on a current collector (10) on which a tab portion (1) is formed according to one embodiment of the present invention.

[0064] Hereinafter, the present invention will be described in detail.

[0065] In this specification, when a part is said to "include" a certain component, this does not mean that other components are excluded, but rather that other components may be included, unless otherwise specifically stated.

[0066] In this specification, the term “A and / or B” means “A or B, or both.”

[0067] The present invention relates to an electrode assembly and an electrochemical device comprising the same. Examples of the electrochemical device include a primary battery, a secondary battery, a supercapacitor, an electric double layer capacitor, and the like. More specifically, the secondary battery may be a lithium ion secondary battery.

[0068]

[0069] The electrode assembly and electrochemical device of the present invention will be described in more detail with reference to the drawings below.

[0070] An electrode assembly according to one aspect of the present invention has a structure in which a positive electrode, a negative electrode, and a separator are interposed between the positive electrode and the negative electrode. At this time, at least one of the positive electrode and the negative electrode includes a current collector; an active material layer formed on at least one surface of the current collector; and an insulating coating formed around the entire outer periphery of one surface of the active material layer; and a wet adhesive force between the positive electrode or negative electrode provided with the insulating coating and the separator is 1 to 20 gf / 20 mm.

[0071] In one embodiment of the present invention, the positive electrode comprises an active material layer formed on at least one surface of the positive electrode, and an insulating coating formed around the entire outer periphery of one surface of the positive electrode, and the wet adhesive force between the one surface of the positive electrode provided with the insulating coating and the separator may be 1 to 20 gf / 20 mm.

[0072] In another embodiment of the present invention, the negative electrode comprises an active material layer formed on at least one surface of the negative electrode, and an insulating coating formed around the entire outer periphery of one surface of the active material layer, and the wet adhesive force between the negative electrode surface provided with the insulating coating and the separator may be 1 to 20 gf / 20 mm.

[0073] In another embodiment of the present invention, the positive electrode and the negative electrode each include an active material layer formed on at least one surface, and an insulating coating formed around the entire outer periphery of one surface of the active material layer, and the wet adhesive force between one surface of the positive electrode provided with the insulating coating and the separator and / or the wet adhesive force between one surface of the negative electrode provided with the insulating coating and the separator may be 1 to 20 gf / 20 mm.

[0074] Fig. 1 is a schematic diagram of an example of the electrode. Specifically, Fig. 1 shows an embodiment in which an electrode active material layer (11) is formed on a current collector having a tab portion (1) formed thereon according to one embodiment of the present invention, and an insulating coating portion (20) is formed around the entire outer periphery of one surface of the electrode active material layer.

[0075] Referring to Fig. 1, in one embodiment of the present invention, the electrode may have a structure including a current collector, an active material layer (11) formed on at least one surface of the current collector, and an electrode tab (1) extending from the current collector. At this time, the insulating coating portion (20) is formed to surround the entire outer periphery of one surface of the active material layer (11).

[0076] FIG. 2 is a schematic diagram illustrating one embodiment of attaching the electrode and separator. Specifically, FIG. 2 illustrates that, according to one embodiment of the present invention, an electrode active material layer (11) formed on a current collector (10) having a tab portion (1) formed thereon includes an insulating coating portion (20) around the outer periphery thereof, so that the insulating coating portion (20) can be positioned between the electrode active material layer (11) and the separator (30). Accordingly, the adhesive strength between the electrode active material layer and the separator can be improved, and the folding phenomenon of the separator can be improved when manufacturing an electrode assembly.

[0077] In one embodiment of the present invention, the electrode may have an active material layer on each side of the current collector, and may include an insulating coating formed around the entire outer periphery of one side of each of the active material layers. In this case, the electrode may be a positive electrode and / or a negative electrode, and the present invention is not limited thereto.

[0078] Fig. 3 is a schematic diagram illustrating one embodiment of attaching the electrode and separator. Specifically, Fig. 3 shows a vertical cross-sectional view centered on the central portion of the assembly to which the electrode and separator are attached. Referring to Fig. 3, since the insulating coating portion (20) is formed around the outer periphery of the electrode active material layer (11), the insulating coating portion is not included on the inner surface of the electrode active material layer (11). At this time, in order to prevent the phenomenon of the electrode active material layer and the separator not adhering due to the thickness of the insulating coating portion itself, it is preferable that the insulating coating portion is formed thinly so that one surface of the electrode active material layer can sufficiently contact the separator when pressurized between the electrode and the separator during the manufacture of the electrode assembly.

[0079] In one embodiment of the present invention, the insulating coating portion is formed to surround the entire outer periphery of one surface of the electrode active material layer, and may be formed to have a thickness of, for example, 0.5 to 1 ㎛. In the manufacture of a conventional electrode assembly, the electrode active material layer may have a thickness deviation of, for example, about 3 ㎛ or more due to a sliding phenomenon of the electrode slurry, etc. However, according to the present invention, since the insulating coating portion having a thin thickness as described above is formed around the outer periphery of the electrode active material layer, not only can the thickness deviation of the entire electrode be improved, but also the adhesive strength between the electrode and the separator can be improved, thereby improving the folding phenomenon of the separator, thereby exhibiting an advantage of improving the safety of the battery, but the mechanism of the present invention is not limited thereto.

[0080] In one embodiment of the present invention, the insulating coating formed around the entire outer periphery of one side of the electrode active material layer may have an area of, for example, 5 to 50 area%, 10 to 30 area%, or 15 to 20 area% based on the total area of ​​one side of the electrode active material layer. When the insulating coating has an area within the above-described range based on the area of ​​one side of the electrode active material layer, it may be preferable in terms of the energy density of the electrode while maintaining the effect of the insulating coating, but the present invention is not limited thereto.

[0081] In one embodiment of the present invention, the area of ​​the insulating coating portion can be measured by obtaining a top surface image of an electrode on which the insulating coating portion is formed when the current collector, electrode active material layer, and insulating coating portion are laminated in an up-down direction, and then measuring the area occupied by the insulating coating portion relative to the total area of ​​the active material layer. At this time, the top surface image of the electrode is not particularly limited to a photographic image, a microscope image such as an SEM, etc.

[0082] The above electrode assembly exhibits a wet adhesive strength of 1 to 20 gf / 20 mm at the interface between the electrode and the separator provided with the insulating coating, thereby improving the phenomenon of the separator not being attached to the electrode within the electrode assembly and folding, and thus exhibiting an excellent effect of preventing a short circuit phenomenon between the electrodes.

[0083] In this specification, the wet adhesive strength refers to the adhesive strength measured in the presence of an electrolyte so as to be similar to the environment in which the electrode assembly is operated as a battery. Even when the dry adhesive strength between the electrode, such as the positive or negative electrode, and the separator is high, when the electrode assembly comes into contact with the electrolyte and each component of the electrode assembly is wetted by the electrolyte, there may be a problem in that the wet adhesive strength is not sufficiently secured due to a decrease in the frictional force between each component or the dissolution of the adhesive component. In order to solve this problem, according to one aspect of the present invention, an electrode assembly is provided in which the wet adhesive strength between one surface of the electrode provided with the insulating coating portion and the separator is secured in a range of 1 to 20 gf / 20 mm.

[0084] In one embodiment of the present invention, the wet adhesive force between the electrode and the separator may be, for example, 5 to 15 gf / 20 mm or 8 to 12 gf / mm. For example, the wet adhesive force between the electrode and the separator may be 10 gf / mm, but the present invention is not limited thereto. When the wet adhesive force between the electrode and the separator is within the above-described range, it may exhibit an advantageous effect in terms of maintaining the adhesive force of the separator even after the electrolyte is injected into the electrode assembly.

[0085] In the present specification, the wet adhesion can be measured, for example, by the following method, but is not limited thereto. First, an electrode and a separator having the insulating coating formed on the entire periphery of one side of the active material layer are each cut into a size of 25 mm x 60 mm to obtain a sample, and then a heat press is used to apply pressure at 6.5 MPa for 1 second at 60°C to manufacture an electrode-separator sample. After that, the electrode-separator sample is placed in a pouch, 1 g of electrolyte is poured in, and impregnated for 1 day. After that, the electrode-separator sample is taken out from the pouch, mounted on a UTM device (LLOYD Instrument LF Plus), and the 90° peel strength is measured at a speed of 300 mm / min.

[0086] In one embodiment of the present invention, the electrode assembly may be characterized by excellent dry adhesion as well as wet adhesion between the electrode and the separator.

[0087] In one embodiment of the present invention, the dry adhesion between the electrode and the separator may be, for example, 5 to 30 gf / 25 mm, 10 to 28 gf / 25 mm, 15 to 25 gf / 25 mm, or 18 to 23 gf / 25 mm. For example, the dry adhesion between the electrode and the separator may be 20 gf / 25 mm.

[0088] In the present specification, the dry adhesion can be measured, for example, by the following method, but is not limited thereto. After obtaining a sample of an electrode and a separator each having an insulating coating formed around the entire outer periphery of an active material layer, each cut to a size of 25 mm x 60 mm, a heat press is used to apply pressure of 6.5 MPa at 60°C for 1 second to manufacture an electrode-separator sample. Thereafter, the electrode-separator sample is mounted on a UTM device (LLOYD Instrument LF Plus), and the 180° peel strength is measured at a speed of 300 mm / min.

[0089] In one embodiment of the present invention, the electrode assembly may also be characterized by excellent peel strength between the active material layer and the insulating coating portion.

[0090] In this specification, the peel strength refers to the adhesive strength between the insulating coating formed around the entire outer periphery of the active material layer and the active material layer.

[0091] In one embodiment of the present invention, the peel strength between the active material layer and the insulating coating portion may be, for example, 5 to 30 gf / 15 mm, 10 to 30 gf / 15 mm, 15 to 25 gf / 15 mm, or 20 to 25 gf / 15 mm. For example, the peel strength between the active material layer and the insulating coating portion may be 20 gf / 15 mm.

[0092] In this specification, the peel strength can be measured by, for example, the following method, but is not limited thereto. The positive electrode to be measured is cut to a size of 15 mm X 100 mm. A double-sided adhesive tape is attached on a glass plate, and the surfaces of the insulating coating portion and the active material layer of the prepared electrode are attached so as to adhere to the adhesive tape. After that, the end of the attached insulating coating portion is mounted on a UTM device (LLOYD Instrument LF Plus), and a force is applied at 180° at a measuring speed of 300 mm / min to measure the force required for the insulating coating portion and the active material layer to peel off.

[0093] According to one embodiment of the present invention, the insulating coating portion includes inorganic particles and a binder. In this case, in order to exhibit the above-described adhesive strength, the binder includes an adhesive binder.

[0094] In one embodiment of the present invention, the binder included in the insulating coating portion may include two types of binders having different glass transition temperatures (Tg) as adhesive binders.

[0095]

[0096] Hereinafter, a composition for insulating coating according to another aspect of the present invention will be described in detail.

[0097] According to another aspect of the present invention, a composition for insulating coating is provided.

[0098] The above composition for insulating coating can be used to form an insulating coating portion formed on an electrode in the above-described electrode assembly.

[0099] The composition for the insulating coating includes inorganic particles and a binder, and the binder includes a first adhesive binder having a glass transition temperature (Tg) of 50°C or higher, and a second adhesive binder having a glass transition temperature (Tg) of 20°C or lower.

[0100] According to one aspect of the present invention, the composition for insulating coating exhibits an effect of improving the adhesive strength between the positive electrode and the separator by including an adhesive binder. At this time, the binder includes two types of adhesive binders having different glass transition temperature ranges, so that not only is the wet adhesive strength and dry adhesive strength excellent, but also the adhesive strength (peel strength) between the active material layer and the insulating coating portion can exhibit an excellent effect.

[0101] Specifically, the two types of adhesive binders included in the composition for the insulating coating may be sequentially referred to as a first adhesive binder and a second adhesive binder. The first adhesive binder and the second adhesive binder may function to bind inorganic particles to each other within the insulating coating portion, thereby stably maintaining the insulating performance of the insulating coating portion.

[0102] In one embodiment of the present invention, the first adhesive binder may additionally, but not limited to, perform a function of improving the adhesive strength between the insulating coating portion and the separator, specifically, the adhesive strength between the positive electrode and the separator. In addition, the second adhesive binder may additionally, but not limited to, perform a function of improving the adhesive strength between the insulating coating portion and the active material and / or the current collector. As described above, in order to improve the adhesive strength between the positive electrode and the separator and the adhesive strength between the active material layer and the insulating coating portion, the binder may include two types of binders having different glass transition temperatures, but the effects of the present invention are not limited thereto.

[0103] In the present specification, the glass transition temperature (Tg) represents the temperature range in which the glass transition of the binder occurs. The glass transition temperature can be measured by a known method for measuring the glass transition temperature, such as a differential scanning calorimeter (DSC), specific heat measurements, a dilatometer, thermo mechanical analysis (DMA), thermal expansion measurement (TAM), micro-heat-transfer measurement, isothermal compressibility, or heat capacity measurement.

[0104] In the present specification, the glass transition temperature value may represent a value measured by a method of measuring heat flow within a binder sample during a linear temperature rise process, particularly using a differential scanning calorimeter (DSC), and it will be apparent to a person skilled in the art that the numerical value of the glass transition temperature is a value that includes a measurement error range of a predetermined range, for example, a measurement error range of -5% to +5%, based on the described value.

[0105] In one embodiment of the present invention, the binder may include two types of adhesive binders having a glass transition temperature (Tg) difference of 100°C or less. Specifically, the binder may include two types of adhesive binders having a glass transition temperature difference of 90°C or less. More specifically, the binder may include two types of adhesive binders having a glass transition temperature difference of, for example, 50°C to 90°C, 60°C to 80°C, 65°C to 75°C, or 65°C to 70°C.

[0106] In one embodiment of the present invention, the glass transition temperature of the first adhesive binder may be, for example, 50°C to 80°C or 50°C to 70°C.

[0107] In one embodiment of the present invention, the glass transition temperature of the second adhesive binder may be, for example, -50°C to 20°C, -40°C to 0°C, or -30°C to -10°C.

[0108] In one embodiment of the present invention, the first adhesive binder has a glass transition temperature of 50°C or higher and may be an aqueous particle-type binder.

[0109] In this specification, the 'aqueous particle-type binder' collectively refers to a binder that is dispersed in an aqueous solvent such as water (H2O) and exhibits a particle shape. The type of the particle-type binder is not particularly limited as long as it satisfies the above-described characteristics, but may be, for example, an acryl-based polymer, a rubber-based polymer, a cellulose-based polymer, or a mixture thereof. The acryl-based polymer may include, for example, a polyalkyl (meth)acrylate, and the 'alkyl' may be an alkyl having 1 to 5 carbon atoms, but is not particularly limited thereto. The rubber-based polymer may be a rubber-based polymer containing at least one butadiene unit, and examples thereof include, but are not limited to, polybutadiene rubber, styrene-butadiene rubber, nitrile-butadiene rubber, and the like. The above cellulose polymer is a general term for cellulose and cellulose derivatives, and examples thereof include, but are not limited to, cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and phthalic acid hydroxypropyl methyl cellulose.

[0110] In one embodiment of the present invention, the first adhesive binder may include an aqueous particle-type binder, and specifically may be composed solely of an aqueous particle-type binder. In this case, the aqueous particle-type binder of the first adhesive binder may include particles having a larger particle size than the inorganic particles included in the composition for insulating coating, as described below.

[0111] Specifically, the first adhesive binder may be a water-based particle-type binder, but may preferably be larger in size than the inorganic particles of the insulating coating composition so that it does not soak between the inorganic particles within the insulating coating but exists on the surface of the insulating coating to exhibit excellent adhesiveness with the separator.

[0112] In one embodiment of the present invention, the first adhesive binder may be an aqueous particle-type binder having a particle size of 250 nm or more. The first adhesive binder may be an aqueous particle-type binder having a particle size of, for example, 250 nm to 1 μm or 250 nm or 500 nm, but is not limited thereto.

[0113] In this specification, the particle size of the particulate binder may represent a value measured through a PSD (particle size distribution) analysis method, and may represent a value measured using, for example, a Malvern Mastersizer 2000.

[0114] In one embodiment of the present invention, the second adhesive binder can exhibit the effect of improving the bonding strength between inorganic particles in the insulating coating portion and improving the adhesive strength between the active material layer and / or the positive electrode current collector and the insulating coating portion by soaking between the inorganic particles.

[0115] To this end, in one embodiment of the present invention, the second adhesive binder may include an aqueous particle-type binder, a solution-type binder, or a mixture thereof. Alternatively, the second adhesive binder may be composed solely of the aqueous particle-type binder or the solution-type binder.

[0116] In one embodiment of the present invention, when the second adhesive binder includes an aqueous particle-type binder, it may be preferable for the aqueous particle-type binder to include particles having a size equal to or smaller than that of the inorganic particles so that the particles can be impregnated between the inorganic particles in the insulating coating portion.

[0117] In one embodiment of the present invention, the second adhesive binder may be an aqueous particle-type binder having a particle size of 250 nm or less. The second adhesive binder may be an aqueous particle-type binder having a particle size of, for example, 50 nm to 250 nm or 100 nm to 200 nm, but is not limited thereto.

[0118] In one embodiment of the present invention, the second adhesive binder may include a solution-type binder.

[0119] In this specification, the 'solution type binder' is a general term for a binder that can be dissolved in a polar solvent including water (H2O), and may also be referred to as a 'dissolvable binder'. The type of the solution type binder is not particularly limited as long as it satisfies the above-described characteristics, but may include, for example, a PVDF series polymer, polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylamide (PAM), or a mixture of two or more thereof. The PVDF series polymer is a general term for a polymer that includes vinylidene fluoride as a monomer, such as polyvinylidene fluoride (PVDF), polyvinylidene-co-hexafluoropropylene, etc.

[0120] In one embodiment of the present invention, as long as it can exhibit the above-described adhesive strength, there is no particular limitation, but for example, the weight ratio of the first adhesive binder and the second adhesive binder may be 1:9 to 9:1. Specifically, the weight ratio of the first adhesive binder and the second adhesive binder may be 5:5 to 8:2.

[0121] In one embodiment of the present invention, the inorganic particles may be used without particular limitation as long as they can be used in the insulating coating portion of the electrode. The inorganic particles may be, for example, alumina (Al2O3), boehmite (AlOOH), silica (SiO2), titanium dioxide (TiO2), aluminum hydroxide (Al(OH)3), magnesium oxide (MgO), magnesium hydroxide (Mg(OH)2), zinc oxide (ZnO), barium titanate (BaTiO), aluminum nitride (AlN), boron nitride (BN), silicon carbide (SiC), beryllium oxide (BeO), potassium nitrate (KNO3), monoammonium phosphate (NH4H2PO4), or a mixture of two or more thereof, but are not limited thereto. Specifically, the inorganic particles may include alumina (Al2O3), boehmite (AlOOH), silica (SiO2), or a mixture of two or more thereof.

[0122] In one embodiment of the present invention, the inorganic particles may have, for example, an average particle diameter of 250 nm or more. Specifically, the average particle diameter of the inorganic particles may be from 250 nm to 1,000 μm or from 250 nm to 500 μm.

[0123] In this specification, the above 'average particle diameter' is D 50 It may represent the average particle size. The above 'D 50 The 'average particle size' refers to the particle size at the 50% point of the cumulative particle volume distribution according to particle size. The above D 50The average particle size can be measured using laser diffraction. Specifically, the particles to be measured are dispersed in a dispersion medium, and then introduced into a commercially available laser diffraction particle size measuring device. When the particles pass through a laser beam, the difference in diffraction pattern according to particle size is measured, thereby calculating the particle size distribution. The commercially available laser diffraction particle size measuring device may be, for example, Microtrac's S3500, but is not limited thereto.

[0124] In one embodiment of the present invention, the weight ratio of the inorganic particles and the binder is not particularly limited as long as it does not impede the purpose of the present invention, but may be, for example, 9:1 to 1:9. Specifically, the weight ratio of the inorganic particles and the binder may be 7:3 to 9:1, more specifically 8:2. When the weight ratio of the inorganic particles and the binder is within the above-described range, it may exhibit advantageous effects in terms of the insulation of the insulating coating portion, the adhesive strength of the anode, and the adhesive strength of the insulating coating portion, but the present invention is not limited thereto.

[0125]

[0126] Hereinafter, other configurations of an electrode assembly according to one aspect of the present invention will be described in detail.

[0127] anode

[0128] The above positive electrode includes a current collector and an active material layer formed on at least one surface of the current collector, as described above.

[0129] In one embodiment of the present invention, the positive electrode may include: a current collector; an active material layer formed on at least one surface of the current collector; and an insulating coating formed around the entire outer periphery of the active material layer.

[0130] The above-mentioned current collector supports the active material layer, and is not particularly limited as long as it has high conductivity without causing chemical changes in the battery. For example, copper, stainless steel, aluminum, nickel, titanium, palladium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, silver, etc., aluminum-cadmium alloy, etc. can be used.

[0131] The above-mentioned collector can form fine irregularities on its surface to strengthen the bonding strength with the positive electrode active material, and can be used in various forms such as a film, sheet, foil, mesh, net, porous body, foam, and non-woven fabric.

[0132] The above active material layer includes a positive electrode active material and may further include a conductive material, a binder, and additives.

[0133] In one embodiment of the present invention, the positive electrode active material may include, but is not limited to, a lithium transition metal oxide; a lithium metal iron phosphate; a lithium nickel-manganese-cobalt oxide; an oxide in which a portion of the lithium nickel-manganese-cobalt oxide is substituted with another transition metal; or two or more thereof. Specifically, the positive electrode active material may include, but is not limited to, a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; a compound having the chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M x Ni-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 2-xM x Lithium manganese composite oxides represented by O2 (wherein M = Co, Ni, Fe, Cr, Zn or Ta and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein M = Fe, Co, Ni, Cu or Zn); lithium metal phosphate LiMPO4 (wherein M = Fe, CO, Ni or Mn); lithium nickel-manganese-cobalt oxide Li 1+x (Ni a Co b Mn c ) 1-x O2(x = 0 ~ 0.03, a = 0.3 ~ 0.95, b = 0.01 ~ 0.35, c = 0.01 ~ 0.5, a+b+c=1); Lithium nickel-manganese-cobalt oxide partially substituted with aluminum a [Ni b Co c Mn d Al e ] 1-f M1 f O2 (M1 is at least one selected from the group consisting of Zr, B, W, Mg, Ce, Hf, Ta, La, Ti, Sr, Ba, F, P and S, and 0.8≤a≤1.2, 0.5≤b≤0.99, 0 <c<0.5, 0<d<0.5, 0.01≤e≤0.1, 0≤f≤0.1); 리튬 니켈-망간-코발트 산화물에 일부가 다른 전이금속으로 치환된 산화물 Li 1+x (Ni a Co b Mn c M d ) 1-x O2(x = 0 ~ 0.03, a = 0.3 ~ 0.95, b = 0.01 ~ 0.35, c = 0.01 ~ 0.5, d = 0.001 ~ 0.03, a+b+c+d=1, M is any one selected from the group consisting of Fe, V, Cr, Ti, W, Ta, Mg and Mo), disulfide compounds; Fe2(MoO4)3, etc., but are not limited thereto.

[0134] In one embodiment of the present invention, the conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path for electrons to move from the current collector to the positive electrode active material, and any conductive material that is physically distinct from the carbon contained in the sulfur-carbon complex and is a component of the electrode can be used without limitation.

[0135] In one embodiment of the present invention, the conductive material may be, for example, carbon black such as Super-P, Denka black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, carbon black; carbon derivatives such as carbon nanotubes or fullerene; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbon, aluminum, and nickel powder; or conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole, which may be used alone or in combination.

[0136] In one embodiment of the present invention, the content of the conductive material may be 0 to 10 wt%, for example, 1 to 10 wt%, based on the total weight of the active material layer. If the content of the conductive material is less than the above range, electron transfer between the positive electrode active material and the current collector may not be easy, resulting in a decrease in voltage and capacity. Conversely, if the content exceeds the above range, the proportion of the positive electrode active material may relatively decrease, resulting in a decrease in the total energy (charge) of the battery. Therefore, it is preferable to determine an appropriate content within the above-described range.

[0137] In one embodiment of the present invention, the positive electrode active material layer may include a positive electrode active material and a binder polymer, and may not include a conductive material. This has the advantage of allowing the positive electrode to include more positive electrode active material since it does not include a conductive material.

[0138] In one embodiment of the present invention, the positive electrode binder maintains the positive electrode active material on the positive electrode current collector and organically connects the positive electrode active materials to further increase the bonding strength between them, and any binder polymer known in the art can be used.

[0139] In one embodiment of the present invention, the binder in the positive electrode active material layer may be the same as or different from the binder of the insulating coating portion, i.e., the first adhesive binder and / or the second adhesive binder, and may be selected independently of them.

[0140] In one embodiment of the present invention, the binder in the positive electrode active material layer is, for example, a fluororesin binder including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); a rubber binder including styrene butadiene rubber (SBR), acrylonitrile-butidiene rubber, styrene-isoprene rubber, etc.; a cellulose binder including carboxyl methyl cellulose (CMC), starch, hydroxy propyl cellulose, regenerated cellulose, etc.; a polyalcohol binder; a polyolefin binder including polyethylene, polypropylene, etc.; a polyimide binder; a polyester binder; a polyacrylic binder such as polyacrylic acid (PAA); a silane binder; a polyurethane binder; Or it may include a mixture of two or more of these, and further, the binder polymer may include a copolymer having repeating units derived from two or more of these binders.

[0141] In one embodiment of the present invention, the content of the binder polymer may be 0.5 to 30 wt% based on 100 wt% of the total positive electrode active material layer. When the content of the binder polymer satisfies this range, the physical properties of the positive electrode are improved, so that the phenomenon of the active material and conductive material within the positive electrode being detached can be prevented, and the ratio of the active material and conductive material in the positive electrode can be appropriately controlled, so that the battery capacity can be secured.

[0142]

[0143] cathode

[0144] The above negative electrode may include a negative electrode current collector and a negative electrode active material layer applied to one or both surfaces of the negative electrode current collector. Alternatively, the negative electrode may be a lithium metal plate.

[0145] In one embodiment of the present invention, the negative electrode may include: a current collector; an active material layer formed on at least one surface of the current collector; and an insulating coating formed around the entire outer periphery of the active material layer.

[0146] The above negative electrode current collector is for supporting the negative electrode active material layer, as described in the positive electrode current collector.

[0147] The above-mentioned negative electrode active material layer may include a conductive material, a binder, etc. in addition to the negative electrode active material. In this case, the conductive material and the binder follow the above-mentioned.

[0148] The above negative active material is lithium (Li + ) can be reversibly intercalated or deintercalated, a material that can react with lithium ions to form a reversibly lithium-containing compound, or a lithium metal or a lithium alloy.

[0149] The above lithium ion (Li + ) can be reversibly inserted or de-inserted, for example, crystalline carbon, amorphous carbon, or a mixture thereof. The lithium ion (Li +) can be, for example, tin oxide, titanium nitrate or silicon. The lithium alloy can be, for example, an alloy of lithium (Li) and a metal selected from the group consisting of sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al) and tin (Sn).

[0150]

[0151] membrane

[0152] The above separator separates or insulates the positive and negative electrodes from each other and enables lithium ion transport between the positive and negative electrodes. Any separator commonly used in electrochemical devices may be used without particular limitations. For example, the separator may be provided in a film-like shape.

[0153] According to one embodiment of the present invention, the separator may include a porous substrate and a porous coating layer formed on at least one surface of the porous substrate.

[0154] Hereinafter, the composition of the porous substrate and the porous coating layer will be exemplarily described.

[0155] In one embodiment of the present invention, the porous substrate refers to a substrate having a plurality of pores formed therein, which serves as an ion-conducting barrier that allows ions to pass through while blocking electrical contact between the cathode and the anode. The pores are structured to be interconnected, so that gas or liquid can pass from one side of the substrate to the other.

[0156] In one embodiment of the present invention, the porous substrate may be a porous polymer film containing a thermoplastic resin, from the perspective of imparting a shutdown function. Here, the shutdown function refers to a function in which, when the battery temperature rises, the thermoplastic resin melts and closes the pores of the porous substrate, thereby blocking the movement of ions and preventing thermal runaway of the battery.

[0157] In one embodiment of the present invention, a thermoplastic resin having a temperature lower than 200°C may be preferable as the thermoplastic resin used in the porous substrate. In addition, the thermoplastic resin may be used without particular limitation as long as it can be used as a substrate of a separator, for example, polyolefin, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, or a mixture of two or more thereof, but is not limited thereto.

[0158] In one embodiment of the present invention, the porous substrate may be a polyolefin substrate.

[0159] In one embodiment of the present invention, the porous coating layer may include inorganic particles and further include a binder resin, such that the inorganic particles are coated on all or at least a portion of the surface by the binder resin. At this time, the inorganic particles are surface-bonded and / or point-bonded via the binder resin. For example, the inorganic particles and the binder resin in the porous coating layer may be included in a weight ratio of 95:5 to 50:50. The porous coating layer has a structure in which a plurality of micropores are formed therein, and these micropores are interconnected, and has the structural characteristics of a porous layer in which gas or liquid can pass from one side to the other side.

[0160] In one embodiment of the present invention, the porous coating layer may have a porous structure derived from pores formed by the interstitial volume between inorganic particles. The pore size and porosity (pore volume ratio) can be controlled depending on the size and size distribution of the particles. Through this structure, the resistance to metallic foreign substances present in the electrode is increased, and at the same time, shrinkage of the porous polyolefin substrate is suppressed, thereby enhancing the safety of the electrochemical device.

[0161] In one embodiment of the present invention, the porous coating layer comprises a plurality of nodes including the inorganic particles and a binder polymer covering at least a portion of the surface of the inorganic particles; and one or more filaments formed in a thread shape from the binder polymer of the nodes, the filaments having a node connecting portion extending from the nodes and connecting other nodes; and the node connecting portion may have a structure in which a plurality of filaments derived from the binder polymer intersect with each other to form a three-dimensional network structure.

[0162] In one embodiment of the present invention, the porous coating layer may be formed through a safety reinforced separator (SRS) manufacturing method, a ceramic coated separator (CCS) manufacturing method, or another known manufacturing method, but is not limited thereto.

[0163] In one embodiment of the present invention, the inorganic particles can be used without particular limitation as long as they are electrochemically stable. That is, the inorganic particles that can be used in the present invention are not particularly limited as long as they do not undergo oxidation and / or reduction reactions within the operating voltage range of the applied electrochemical device (e.g., 0 to 5 V based on Li / Li+). Non-limiting examples of such inorganic particles include BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC and TiO2, and one or more of these may be included.

[0164] In one embodiment of the present invention, when a binder resin is included in the porous coating layer, the binder resin may include, for example, a polyvinylidene fluoride-based resin (PVdF-based resin). In one embodiment of the present invention, the PVdF-based resin may include at least one of a homopolymer of vinylidene fluoride (i.e., polyvinylidene fluoride), a copolymer of a monomer copolymerizable with vinylidene fluoride, and a mixture thereof. In one embodiment of the present invention, the monomer may include, for example, a fluorinated monomer and / or a chlorinated monomer. Non-limiting examples of the fluorinated monomer include vinyl fluoride; trifluoroethylene (TrFE); chlorofluoroethylene (CTFE); 1,2-difluoroethylene; tetrafluoroethylene (TFE); hexafluoropropylene (HFP); Perfluoro(alkylvinyl) ethers such as perfluoro(methylvinyl) ether (PMVE), perfluoro(ethylvinyl) ether (PEVE), and perfluoro(propylvinyl) ether (PPVE); perfluoro(1,3-dioxole); and perfluoro(2,2-dimethyl-1,3-dioxole) (PDD), and more than one of these may be included.

[0165] In one embodiment of the present invention, the first porous coating layer and the second porous coating layer may have the same composition, but may be formed with different compositions as needed, and the present invention is not limited thereto.

[0166] In one embodiment of the present invention, the binder in the porous coating layer may be the same as or different from the binder of the insulating coating portion, i.e., the first adhesive binder and / or the second adhesive binder, and may be selected independently of them.

[0167]

[0168] According to another aspect of the present invention, an electrochemical device can be provided in which the above-described electrode assembly is housed in a case.

[0169] In one embodiment of the present invention, the case may adopt a conventional battery case, and there are no particular limitations on the external shape depending on the intended use of the battery. For example, the case may be cylindrical, square, pouch-shaped, or coin-shaped, such as using a can.

[0170] Once the electrode assembly as described above is completed, it can be housed and sealed in a case in a conventional manner to manufacture an electrochemical device. At this time, the electrochemical device can be, for example, a lithium secondary battery.

[0171] Meanwhile, an adhesive insulating coating may be provided on the separator to improve the adhesion between the separator and the electrode or to prevent short circuits between the electrodes. However, in this case, when the adhesive insulating coating is provided on the separator, the coating solution may be impregnated into the pores of the separator, thereby blocking the pores of the separator and thus reducing the air permeability of the separator. Accordingly, according to one aspect of the present invention, it is preferable to provide an insulating coating on the active material layer of the electrode in contact with the separator as described above and then laminate the separator.

[0172] According to one embodiment of the present invention, when the above-described coating solution is applied to a separator, the coating solution may be impregnated into the pores of the surface of the separator, thereby reducing the air permeability of the separator, and thus exhibiting an air permeability time exceeding 200 seconds / 100 cc, which may cause a problem in that the separator cannot be used as an electrochemical device separator. Here, the air permeability time may be a value measured using a Gurley densometer according to the ASTM D726-94 standard. Specifically, the air permeability is measured when 100 cc of air is applied to 1 inch of the separator to be measured under a pressure of 12.2 in H2O. 2 The time (in seconds) it takes for a particle to pass through the cross section can be measured as the ventilation time.

[0173] In an electrode assembly manufactured according to one embodiment of the present invention, the separator may exhibit a ventilation time of 200 seconds / 100 cc or less, specifically, 150 seconds / 100 cc or less, or 100 seconds / 100 cc or less, but the present invention is not limited thereto.

[0174] Accordingly, according to another aspect of the present invention, a method for manufacturing the above-described electrode assembly is provided.

[0175] A method for manufacturing an electrode assembly according to another aspect of the present invention is as follows:

[0176] A step of preparing a current collector and an electrode having an active material layer on at least one surface of the current collector,

[0177] A step of forming an insulating coating portion including inorganic particles and a binder around the entire outer periphery of one side of the active material layer, and

[0178] It includes a step of rolling after contacting a separator with a surface on which the insulating coating portion is formed.

[0179] As described above, the electrode on which the insulating coating portion is formed may be at least one of an anode and a cathode.

[0180] In addition, the electrode assembly manufactured as described above can exhibit a wet adhesion between the electrode on which the insulating coating portion is formed and the separator of 1 to 20 gf / 20 mm.

[0181]

[0182] Hereinafter, the present invention will be described in more detail through examples, but the following examples are intended to illustrate the present invention, and the scope of the present invention is not limited to these examples.

[0183] [Preparation of composition for insulating coating]

[0184] Example 1

[0185] Al2O3(D) as inorganic particles in water (H2O) 5080 parts by weight of 500 nm) and 20 parts by weight of binder were added and stirred to prepare a composition for insulating coating.

[0186] The above binder is a first adhesive binder (acrylic, D) having a Tg of 50°C. 50 400 nm) and a second adhesive binder (acrylic, D) with Tg of -20°C 50 A mixture of 200 nm) was used in a weight ratio of 8:2.

[0187]

[0188] Example 2

[0189] An insulating coating composition was prepared according to the same method as Example 1, except that the first adhesive binder was changed to an acrylic binder having a Tg of 70°C, and the second adhesive binder was changed to an acrylic binder having a Tg of -40°C.

[0190]

[0191] Comparative Example 1

[0192] An insulating coating composition was prepared according to the same method as Example 1, except that the first adhesive binder having a Tg of 50°C was used alone as a binder.

[0193]

[0194] Comparative Example 2

[0195] An insulating coating composition was prepared according to the same method as Example 1, except that a second adhesive binder having a Tg of -20°C was used alone as a binder.

[0196]

[0197] Comparative Example 3

[0198] An insulating coating composition was prepared according to the same method as Example 1, except that the first adhesive binder was changed to an acrylic binder having a Tg of 40°C, and the second adhesive binder was changed to an acrylic binder having a Tg of 30°C.

[0199]

[0200] [Manufacturing Example 1. Manufacturing of an Electrode Assembly]

[0201] An electrode assembly was manufactured as follows using the composition for insulating coating manufactured above.

[0202] First, the positive electrode active material (LiNi 0.8 Mn 0.1 Co 0.1 O2), conductive agent (carbon black), dispersant, and binder resin (PVDF-HFP and PVDF mixture) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a positive electrode active material layer having a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to form a positive electrode active material layer (thickness 120 μm). Each of the insulating coating compositions prepared above was applied around the outer periphery of one surface of the manufactured positive electrode active material layer and dried to manufacture a positive electrode having an insulating coating portion (thickness 1 μm) formed around the entire periphery of the outer periphery of the active material layer (the total area of ​​the insulating coating portion was 17 area% based on the total area of ​​one surface of the positive electrode active material layer).

[0203] Graphite (natural graphite and artificial graphite blend), conductive agent (carbon black), dispersant, and binder resin (PVDF-HFP and PVDF blend) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for an anode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of a copper thin film (thickness 10 μm) and dried to manufacture an anode having an anode active material layer (thickness 120 μm).

[0204] An electrode assembly was prepared by positioning the positive and negative electrodes so that they face each other and interposing a polyethylene separator having a thickness of 16 ㎛ and a porosity of 46 vol% between them.

[0205]

[0206] [Adhesion Evaluation]

[0207] For each electrode assembly manufactured above, wet adhesion, dry adhesion, and peel strength were evaluated using the following methods, and the results are shown in Table 1 below. Table 1 also summarizes the glass transition temperature characteristics of the binder used in forming the insulating coating portion.

[0208]

[0209] Wet adhesion

[0210] The positive electrode and separator manufactured above were each cut to a size of 25 mm X 60 mm, and then pressurized at 60°C and 6.5 MPa for 1 second using a heat press. Then, the positive electrode and separator assembly was stored in a pouch-type case, and 1 g of an electrolyte having a composition of 1 M LiPF6 dissolved in a 1,3-dioxolane:dimethoxymethane (DOL:DME 1:1 v / v) mixed solvent was injected, and an aging process and a degassing process were performed for 1 day.

[0211] Afterwards, the positive electrode and separator assembly was removed from the case and mounted on the UTM equipment (LLOYD Instrument LF Plus), and force was applied at a measuring speed of 300 mm / min and 90° to measure the force required to separate the bonded surfaces.

[0212]

[0213] Dry adhesion

[0214] The anode and separator manufactured above were each cut to a size of 25 mm X 60 mm, and then pressurized at 60°C and 6.5 MPa for 1 second using a heat press. Then, they were mounted on a UTM device (LLOYD Instrument LF Plus) and force was applied at a measurement speed of 300 mm / min and 180° to measure the force required to separate the bonded surfaces.

[0215]

[0216] peel strength

[0217] The positive electrode manufactured above was cut to a size of 15 mm X 100 mm. Double-sided adhesive tape was attached on a glass plate and the surfaces of the insulating coating and the active material layer of the prepared positive electrode were attached so that they adhered to the adhesive tape. After that, the end of the bonded insulating coating was mounted on a UTM device (LLOYD Instrument LF Plus) and a force was applied at a measuring speed of 300 mm / min at 180° to measure the force required to peel off the insulating coating and the active material layer.

[0218] Binder compositionWet adhesion(gf / 20mm)Dry adhesion(gf / 25mm)Peel strength(gf / 15mm)Comparative example 1Tg 50℃1 type000Comparative example 2Tg -20℃1 type0030Comparative example 3Tg 40℃ / Tg 30℃2 types mixture035Example 1Tg 50℃ / Tg -20℃2 types mixture102025Example 2Tg 70℃ / Tg -40℃2 types mixture8515

[0219] As shown in the results in Table 1 above, when the insulating coating portion is formed around the entire outer periphery of the positive electrode active material layer, it was confirmed that when two types of a first adhesive binder having a Tg of 50°C or higher and a second adhesive binder having a Tg of 20°C or lower are used, a wet adhesive strength in the range of 1 to 20 gf / 20 mm can be exhibited. In particular, in the case of Example 1 using a glass transition temperature difference of 100°C or lower, it was confirmed to be superior to Comparative Examples 1 to 3 not only in wet adhesive strength but also in dry adhesive strength and peeling strength.

[0220] On the other hand, in the case of Comparative Example 3, which used two types of binders with different glass transition temperatures as the binder of the insulating coating portion (when using those with glass transition temperatures of 40°C and 30°C, respectively), it was confirmed that the adhesive strength (peeling strength) of the insulating coating portion was inferior, and both the wet adhesion and the dry adhesion were inferior. In addition, in the case of Comparative Example 1, which used only one type of binder with a Tg of 50°C, the peel strength, wet adhesion and dry adhesion of the insulating coating portion were inferior, and in the case of Comparative Example 2, which used only one type of binder with a Tg of -20°C, it was confirmed that the adhesive strength of the insulating coating portion was strongly secured, but the wet adhesion and the dry adhesion were not secured. Through this, it was inferred that in the case of Comparative Example 2, the binder was impregnated between the inorganic particles to increase the adhesive strength of the insulating coating portion, but the adhesive strength of the surface of the insulating coating portion was not secured.

[0221]

[0222] [Comparative Manufacturing Example 1. Manufacturing of Electrode Assembly]

[0223] The insulating coating composition of Example 1 manufactured above was used, and the positive electrode, negative electrode, and separator manufactured in Manufacturing Example 1 were prepared in the same manner.

[0224] However, instead of forming an insulating coating portion on the anode, the insulating coating composition of Example 1 was applied to one surface of the separator (thickness 16 ㎛, porosity 46 vol%) in contact with the anode and dried to prepare a separator having an insulating coating portion on one surface.

[0225] An electrode assembly was manufactured by bonding the anode / separator / cathode so that the insulating coating portion of the prepared separator and the anode face each other.

[0226] It was confirmed that the electrode assembly prepared according to Comparative Manufacturing Example 1 could not be used as an electrochemical device due to a significant reduction in the pores of the separator. Specifically, the air permeability of the separator equipped with an insulating coating was evaluated as follows, and it was confirmed that the air permeability time of the separator exceeded 200 s / 100 cc.

[0227]

[0228] Measurement of ventilation (ventilation time)

[0229] The air permeability was measured using a Gurley densometer according to ASTM D726-94. Specifically, the air permeability was measured when 100 cc of air was injected into 1 inch of the membrane under a pressure of 12.2 in H2O. 2 The time (in seconds) it takes for the gas to pass through the cross section was measured as the ventilation time.

[0230]

[0231] Although the present invention has been described with reference to the embodiments and drawings, those skilled in the art will be able to make various applications and modifications within the scope of the present invention based on the above contents.

[0232]

[0233] [Explanation of symbols]

[0234] 1: Electrode tab

[0235] 10: Whole house

[0236] 11: Electrode active material layer

[0237] 20: Insulating coating part

[0238] 30: Membrane

Claims

1. An electrode assembly having a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, At least one of the positive electrode and the negative electrode comprises a current collector; an active material layer formed on at least one surface of the current collector; and an insulating coating formed around the entire outer periphery of one surface of the active material layer; An electrode assembly characterized in that the wet adhesive strength between the positive or negative electrode provided with the insulating coating and the separator is 1 to 20 gf / 20 mm.

2. In claim 1, An electrode assembly characterized in that at least one of the positive electrode and the negative electrode includes an active material layer on each side of the current collector; and an insulating coating formed around the entire outer periphery of one side of each of the active material layers.

3. In claim 1, The above insulating coating portion includes inorganic particles and a binder, An electrode assembly characterized in that the binder comprises two types of adhesive binders having a glass transition temperature (Tg) difference of 100°C or less.

4. In claim 1, The above insulating coating portion includes inorganic particles and a binder, The above binder, A first adhesive binder having a glass transition temperature (Tg) of 50°C or higher, and An electrode assembly characterized by including a second adhesive binder having a glass transition temperature (Tg) of 20°C or less.

5. Contains inorganic particles and binders, An insulating coating composition characterized in that the binder comprises two types of adhesive binders having a difference in glass transition temperature (Tg) of 100°C or less.

6. Contains inorganic particles and binders, The above binder, A first adhesive binder having a glass transition temperature (Tg) of 50°C or higher, and An insulating coating composition characterized by including a second adhesive binder having a glass transition temperature (Tg) of 20°C or less.

7. In claim 6, An insulating coating composition characterized in that the first adhesive binder comprises an aqueous particle-type binder.

8. In claim 7, An insulating coating composition, characterized in that the first adhesive binder comprises an aqueous particle-type binder having a particle size of 250 nm or more.

9. In claim 6, A composition for insulating coating, characterized in that the second adhesive binder comprises an aqueous particle-type binder, a solution-type binder, or a mixture thereof.

10. In claim 9, An insulating coating composition characterized in that the second adhesive binder comprises an aqueous particle-type binder having a particle size of 250 nm or less.

11. In claim 6, An insulating coating composition characterized in that the weight ratio of the first adhesive binder and the second adhesive binder is 1:9 to 9:

1.

12. In claim 5 or claim 6, An insulating coating composition characterized in that the weight ratio of the inorganic particles and the binder is 7:3 to 9:

1.

13. An electrochemical device characterized in that the electrode assembly according to any one of claims 1 to 4 is housed in a case.

14. A step of preparing a current collector and an electrode having an active material layer on at least one surface of the current collector; A step of forming an insulating coating portion including inorganic particles and a binder around the entire outer periphery of one side of the active material layer, and It includes a step of rolling after contacting a separator with a surface on which the insulating coating portion is formed, The above electrode is at least one of an anode and a cathode, A method for manufacturing an electrode assembly, characterized in that the wet adhesive force between the electrode and the separator on which the insulating coating portion is formed is 1 to 20 gf / 20 mm.

Citation Information

Patent Citations

  • Secondary battery

    JP2022134345A

  • Secondary battery having stepped cell structure

    KR1020160046523A

  • Apparatus, method and computer-readable storage medium for providing platform of application service of bicycle based on calculating reduced carbon emission

    KR102360491B1

  • KR20190004158A

  • KR20220021137A