Oriented polyester film and manufacturing method therefor

The development of a stretched polyester film with optimized crystallinity through specific heat treatments allows for efficient recycling without separation from PET containers, addressing the inefficiencies in current recycling processes and maintaining heat shrinkability for packaging applications.

WO2024248463A1PCT designated stage expired Publication Date: 2024-12-05SK CHEMICALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/007248
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-28
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

The recycling process of waste plastic containers is inefficient due to the need for pretreatment to separate polyester films from PET bottles, as the difference in crystallinity between the polyester film and PET container materials prevents their simultaneous recycling.

Method used

A stretched polyester film with enhanced crystallinity is developed by polymerizing a diol component and a dicarboxylic acid component, followed by primary and secondary heat treatments, allowing it to be recycled without separation from PET bottles by achieving a specific melting temperature ratio and heat of fusion, thereby optimizing crystallinity and heat shrinkability.

Benefits of technology

The enhanced crystallinity of the polyester film enables it to be recycled without separation from PET containers, increasing the efficiency of the recycling process and maintaining excellent heat shrinkability, making it suitable for packaging and labeling while improving recycling efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024007248_05122024_PF_FP_ABST
    Figure KR2024007248_05122024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an oriented polyester film and a manufacturing method therefor. The oriented polyester film comprises a polyester resin in which a diol component and a dicarboxylic acid component are polymerized. When analyzed by differential scanning calorimetry (DSC) after first heat treatment and second heat treatment, the oriented polyester film exhibits a first melting temperature (Tm1) and a second melting temperature (Tm2), and shows not less than 0.1 in the ratio (H2 / H1) of a second heat of fusion (H2) at the second melting temperature (Tm2) to a first heat of fusion (H1) at the first melting temperature (Tm1). The oriented polyester film according to the present invention can be usefully utilized as a heat shrinkable film applied as a label and / or packaging of a plastic container, and in particular, has very excellent crystallinity, thereby increasing recycling process efficiency of a waste plastic container.
Need to check novelty before this filing date? Find Prior Art

Description

Polyester stretch film and method for producing the same

[0001] The present invention relates to a polyester stretch film having excellent crystallinity while having heat shrinkage properties, thereby increasing the efficiency of a recycling process, and a method for producing the polyester stretch film.

[0002] Among polymers, polyester resins are widely used in various fields due to their superior mechanical strength, heat resistance, transparency, and gas barrier properties. In particular, heat-shrinkable films manufactured using polyester resins exhibit high heat resistance and an appropriate heat shrinkage rate, making them suitable for packaging and / or labeling plastic containers such as PET bottles.

[0003] Meanwhile, while the use of plastic containers makes everyday life more convenient, their indiscriminate disposal and excessive use are causing serious environmental problems. Consequently, various measures are being developed to recycle used plastic containers.

[0004] The process of recycling the above waste plastic containers can be divided into a physical recycling process, such as washing and crushing, and a chemical recycling process, such as depolymerization. However, these recycling processes require preprocessing to separate the waste plastic by plastic type, which reduces the efficiency of the recycling process. For example, to recycle a PET bottle with a polyester film bonded as a label, the polyester film must be separated (removed) from the PET bottle. This is because the difference in crystallinity between the polyester resin contained in the polyester film and the PET contained in the PET bottle makes recycling impossible if the PET bottle is recycled while the polyester film is still bonded.

[0005] Therefore, in order to increase the efficiency of the recycling process, it is necessary to develop a technology that can omit the preprocessing work of separating (removing) polyester film from plastic containers such as PET bottles.

[0006] [Prior Art Literature]

[0007] [Patent Document]

[0008] (Patent Document 1) Republic of Korea Patent Publication No. 2009-0062882

[0009] In order to solve the above-mentioned conventional problems, the inventors of the present invention have conducted various studies, and as a result, it has been confirmed that the crystallinity of a polyester stretch film manufactured using a polyester resin can be maximized, and a polyester stretch film that can be recycled without separating (removing) from a waste plastic container can be obtained.

[0010] Accordingly, the object of the present invention is to provide a polyester stretch film having excellent crystallinity and a method for producing the same.

[0011] In order to solve the above problem, the present invention comprises a polyester resin in which a diol component and a dicarboxylic acid component are polymerized, and when analyzed by differential scanning calorimetry (DSC) after the first heat treatment and the second heat treatment, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) represents the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) provides a polyester stretched film having a ratio of second heat of fusion (H2) (H2 / H1) of 0.1 or more.

[0012] In addition, the present invention provides a polyester stretched film comprising a polyester resin polymerized with a diol component and a dicarboxylic acid component, wherein the polyester stretched film is first heat-treated at 70° C., pre-heat-treated at 160° C., and then cut into 1 cm × 1 cm pieces to obtain a polyester stretched film sample, and a polyethylene terephthalate (PET) sample obtained by passing a PET container through a sieve with a diameter of 12.5 mm, are mixed in a weight ratio of 97:3, heat-treated at 195° C. for 90 minutes, and then the heat-treated mixed sample is passed through the sieve, and when evaluating the crystallinity of the polyester stretched film, the polyester stretched film has a crystal fraction represented by the following Formula 2 of 30% or more:

[0013] [Formula 2]

[0014] Crystalline fraction (%) = (F T / F m )×100

[0015] In the above equation 2,

[0016] F above T is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed samples, the weight (S) of the sample passing through a 12.5 mm mesh sieve s ) ratio ((S s / M T ) × 100, %),

[0017] F above m is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed sample remaining on a 12.5 mm mesh sieve (C s ) ratio ((C s / M T ) × 100, %).

[0018] In addition, the present invention includes a step of manufacturing a polyester resin by polymerizing a diol component and a dicarboxylic acid component; a step of manufacturing a polyester stretched sheet from the polyester resin; and a step of heat-setting the stretched sheet, and after the first heat treatment and the second heat treatment, when analyzed by differential scanning calorimetry (DSC), the first melting temperature (T m1 ) and the second melting temperature (T m2 ) represents the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) provides a method for manufacturing a polyester stretched film, wherein the ratio (H2 / H1) of the second heat of fusion (H2) in the film is 0.1 or more.

[0019] The polyester stretch film according to the present invention has a plurality of melting temperatures (T) when heat-treated two or more times under specific conditions. m ) and by satisfying a specific range of heat of fusion ratio, it is possible to maximize crystallinity while exhibiting excellent heat shrinkage.

[0020] Therefore, the polyester stretch film according to the present invention can be usefully used as a heat shrinkable film applied as a packaging and / or label for a plastic container (e.g., a PET bottle).

[0021] Furthermore, the polyester stretch film according to the present invention, due to its high crystallinity, enables recycling of waste plastic containers without separating the polyester stretch film (waste plastic containers can be recycled while still attached to the polyester stretch film). Accordingly, the present invention can increase the efficiency of the recycling process compared to conventional methods.

[0022] Figure 1 is a graph showing the results of DSC analysis of a polyester stretch film manufactured in Example 6 of the present invention.

[0023] Hereinafter, the present invention will be described in detail. Herein, the present invention is not limited to the contents described below, and may be modified in various forms as long as the gist of the invention is not changed.

[0024] The word "comprising" or "including" in this specification is intended to specify particular features, regions, steps, processes, elements and / or components, and does not exclude the presence or addition of other features, regions, steps, processes, elements and / or components, unless specifically stated to the contrary.

[0025] In this specification, terms such as first, second, etc. are used to describe various components, and the components are not limited to these terms. These terms are used to distinguish one component from another.

[0026] All numbers and expressions indicating the amounts of components, reaction conditions, etc. described in this specification can be understood to be modified by the term “about” in all cases unless otherwise specified.

[0027]

[0028] Generally, the melting temperature (T) of polymer resins m ) is the crystallization temperature (T ), which is the temperature at which the crystalline portion of the polymer resin begins to melt. c ) is defined as the limit of the melting temperature (T m ) means that a large amount of heat is required to melt the crystalline portion of the polymer resin, which can be interpreted as the crystallinity of the polymer resin being maximized.

[0029] Based on these points, the polyester stretch film of the present invention including a polyester resin, which is a polymer resin, can be produced at a number of melting temperatures (T) through primary heat treatment and secondary heat treatment under specific conditions. m ) and exhibits high crystallinity by having a ratio of heat of fusion at the above multiple melting temperatures that satisfies a specific range.

[0030] In particular, the polyester stretched film according to one embodiment can shrink the polyester stretched film through a first heat treatment and improve the crystallinity of the polyester stretched film through a second heat treatment.

[0031] In addition, by variously adjusting the secondary heat treatment conditions, the crystallinity of the polyester stretched film can be optimized, and due to this optimized crystallinity, it can be usefully used as a heat shrinkable film applied as a packaging and / or label for a plastic container (e.g., a PET bottle), and further, it has a technical significance in that the recycling process of waste plastic containers (waste plastic containers can be fed into the recycling process with the polyester stretched film bound to it) is possible without separating the polyester stretched film (polyester film), thereby significantly improving the efficiency of the recycling process.

[0032] To explain this in detail, it is as follows.

[0033]

[0034] Polyester stretch film

[0035] According to one embodiment, a polyester stretch film includes a polyester resin in which a diol component and a dicarboxylic acid component are polymerized, and when analyzed by differential scanning calorimetry (DSC) after the first heat treatment and the second heat treatment, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) represents the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) has a ratio (H2 / H1) of the second heat of fusion (H2) of 0.1 or more.

[0036] Specifically, the polyester stretched film is a stretched film containing a polyester resin, and can realize excellent heat shrinkage properties by heat-treating at a first heat treatment temperature, and by heat-treating the heat-shrinked polyester stretched film again at a second heat treatment temperature, the crystallinity of the heat-shrinked polyester stretched film can be optimally improved, thereby providing a heat-shrinkable film having improved crystallinity while maintaining excellent heat shrinkage properties.

[0037] The crystallinity of the above polyester stretched film can be an indicator of recyclability and recyclability process efficiency. That is, the higher the crystallinity of the above polyester stretched film, the higher the recyclability and the better the recycling fixation efficiency.

[0038] According to one embodiment, a polyester stretched film can have its crystallinity optimally improved through two or more heat treatment processes, so that even if a recycling process is performed while the polyester stretched film is bonded to a waste plastic container, fusion with the waste plastic container is reduced, so that a recycling process of the waste plastic container can be performed without going through a process of separating (removing) the polyester stretched film from the waste plastic container, thereby increasing the efficiency of the recycling process.

[0039] Meanwhile, the polyester stretched film according to the present invention may be a polyester film manufactured by heat-treating a stretched film manufactured from a polyester resin twice or more.

[0040] Specifically, the polyester stretched film according to the present invention may be a polyester film manufactured by heat-treating a stretched film manufactured from a polyester resin at a first heat-treatment temperature and then heat-treating it again at a second heat-treatment temperature. In addition, the polyester film may be manufactured by heat-treating it once or twice or more in the second heat-treatment temperature.

[0041] For example, the polyester stretched film may be a polyester film manufactured by heat treating at least twice, specifically two to three times. Specifically, the polyester stretched film may be a polyester film manufactured by, for example, first heat treatment and second heat treatment, or pre-heat treatment of the first heat treatment and second heat treatment.

[0042] In this specification, the polyester stretched film may include a film obtained by melting the polyester resin into a sheet and then stretching the sheet.

[0043] Specifically, the polyester stretched film may be a stretched film obtained through a melting and casting process, a stretching process, and / or a heat setting process of the polyester resin. The specific process method of the polyester stretched film is as described below.

[0044] According to one embodiment, the first heat treatment temperature may be 60 to 105 °C, and specifically 62 to 104 °C, 62 to 103 °C, 65 to 102 °C, 68 to 100 °C, 70 to 100 °C, 70 to 98 °C, 70 to 97 °C, or 70 to 96 °C.

[0045] The above first heat treatment is a shrinkage process of the polyester stretched film, and when the first heat treatment temperature satisfies the above range, the polyester stretched film can realize excellent heat shrinkage properties at the desired level.

[0046] Additionally, the secondary heat treatment temperature may be 140 to 220°C, specifically 141 to 219°C, 142 to 218°C, 143 to 217°C, 144 to 216°C, 145 to 215°C, 145 to 214°C, 146 to 213°C, or 150 to 210°C.

[0047] The above secondary heat treatment is a crystallization process of the polyester stretched film shrunk by the above primary heat treatment, and when the secondary heat treatment temperature satisfies the above range, the polyester stretched film can realize excellent crystallinity at the desired level.

[0048] That is, by performing primary and secondary heat treatments on the polyester stretched film, excellent heat shrinkage properties and high crystallinity can be achieved simultaneously.

[0049] In particular, since the first and second heat treatment temperatures each satisfy the above ranges, the polyester stretched film can have excellent heat shrinkage properties while having a high crystallinity at the required level.

[0050] Additionally, crystallinity can be controlled by varying the secondary heat treatment conditions.

[0051] For example, the second heat treatment may be performed after the first heat-treated polyester stretched film is pre-heat-treated (pre-heat treatment of the second heat treatment).

[0052] Specifically, the secondary heat treatment may include a step of pre-heat treating the first heat-treated polyester stretched film, and a step of second-heat treating the pre-heat-treated polyester stretched film.

[0053] The above pre-heat treatment can be performed at the same or similar temperature range as the above secondary heat treatment. For example, the pre-heat treatment temperature can be 140 to 220°C, and specifically, 141 to 219°C, 142 to 218°C, 143 to 217°C, 144 to 216°C, 145 to 215°C, 145 to 214°C, 146 to 213°C, or 150 to 210°C for 1 to 30 minutes, 1 to 20 minutes, 5 to 30 minutes, 5 to 25 minutes, 5 to 20 minutes, 5 to 15 minutes, 6 to 25 minutes, 6 to 20 minutes, 6 to 15 minutes, or 6 to 13 minutes.

[0054] In the case where the pre-heat treatment is performed within the above range during the above secondary heat treatment, the polyester stretched film shrunk by the first heat treatment is crystallized through the pre-heat treatment, and the crystallinity of the polyester stretched film can be maximized to an optimal range through the second heat treatment, thereby further improving the efficiency of the recycling process.

[0055] Meanwhile, after the first heat treatment and the second heat treatment, the differential scanning calorimetry (DSC) for analyzing the polyester stretched film may be specifically modulated DSC (MDSC), and more specifically, temperature-modulated DSC (TMDSC). When analyzing with the differential scanning calorimetry (DSC), a heating rate condition of, for example, 10°C / min from room temperature to 280°C may be applied.

[0056] According to one embodiment, the first melting temperature (T) that appears during the first heat treatment and the second heat treatment m1 ) and the second melting temperature (T m2 ) are not particularly limited, but may be 150 to 230 ℃, respectively, and at this time, the first melting temperature (Tm1 ) and the second melting temperature (T m2 ) may be different from each other. Specifically, the first melting temperature (T m1 ) is the second melting temperature (T m2 ) may be lower.

[0057] That is, after the first heat treatment, the first melting temperature (T m1 ) may be 150 to 230°C, specifically 152 to 230°C, 154 to 220°C, 156 to 220°C, 158 to 215°C, 160 to 215°C, 162 to 215°C, or 162 to 210°C.

[0058] Additionally, after the first heat treatment, at least one first melting temperature (T m1 ) can be expressed.

[0059] That is, after the first heat treatment, one or more first melting temperatures (T m1 ) can be represented, and the plurality of first melting temperatures (T m1 ) may exhibit different melting temperatures within the above range.

[0060] Also, the second melting temperature (T m2 ) may be 150 to 230°C, specifically 155 to 230°C, 170 to 230°C, 175 to 229°C, 180 to 229°C, 185 to 228°C, 190 to 228°C, or 195 to 228°C.

[0061] Specifically, after the second heat treatment, the second melting temperature (T m2 ) is 150 ℃ to 230 ℃ and may have crystallinity. In addition, after the second heat treatment, the desired melting temperature (T m2 ) and can have enthalpy at the corresponding temperature.

[0062] At this time, the first melting temperature (T m1) and the second melting temperature (T m2 ) may be different from each other.

[0063] In addition, after the second heat treatment, one or more second melting temperatures (T m2 ) can be expressed.

[0064] That is, after the above secondary heat treatment, one or more second melting temperatures (T m2 ) can be represented, and the plurality of second melting temperatures (T m2 ) may exhibit different melting temperatures within the above range.

[0065] The first and second melting temperatures (T m1 , T m2 ) As each range is within the above range, the polyester stretch film according to the present invention can have high crystallinity at the required level while improving heat shrinkage, heat resistance and durability.

[0066] In addition, when the polyester stretched film was pre-heat treated after the first heat treatment and before the second heat treatment, the second-p melting temperature (T) was analyzed by differential scanning calorimetry (DSC). m2-p ) represents the second-p melting temperature (T m2-p ) may be 150 to 230°C, specifically 155 to 230°C, 156 to 230°C, 157 to 229°C, 160 to 229°C, 160 to 228°C or 160 to 225°C.

[0067] In addition, when the polyester stretched film subjected to the first heat treatment is pre-heat treated before the second heat treatment, and then analyzed by differential scanning calorimetry (DSC), one or more of the second-p melting temperatures (T m2-p ) can be expressed.

[0068] That is, after the pre-heat treatment of the first heat-treated polyester stretched film, one or more second-p melting temperatures (T m2-p) can be represented, and the plurality of second-p melting temperatures (T m2-p ) may exhibit different melting temperatures within the above range.

[0069] The above 2-p melting temperature (T m2-p ) is satisfied within the above range, the crystallinity of the polyester stretch film can be maximized, and the heat shrinkage, heat resistance and durability can be further improved.

[0070] Meanwhile, according to one embodiment, the first melting temperature (T m1 ) and the second melting temperature (T m2 ) can each have a specific range of heat of fusion (heat of fusion or delta H). The heat of fusion refers to the amount of heat required for a substance to melt, and by controlling the heat of fusion and the ratio of the heat of fusion, the crystallinity can be controlled within the desired range.

[0071] Specifically, after the first heat treatment, the first melting temperature (T m1 ) may be 1.0 J / g or more, 1.5 J / g or more, 2.0 J / g or more, 40.0 J / g or less, 35.0 J / g or less, 30.0 J / g or less, 28.0 J / g or less, or 27.0 J / g or less. More specifically, after the first heat treatment, the first melting temperature (T m1) is, for example, 1.0 J / g to 40.0 J / g, 1.0 J / g to 30.0 J / g, 1.0 J / g to 28.0 J / g, 2.0 J / g to 40.0 J / g, 2.0 J / g to 30.0 J / g, 2.0 J / g to 28.0 J / g, 3.0 J / g to 40.0 J / g, 3.0 J / g to 30.0 J / g, 3.0 J / g to 28.0 J / g, 4.0 J / g to 40.0 J / g, 4.0 J / g to 30.0 J / g, 4.0 J / g to 28.0 J / g, 4.8 J / g to 40.0 J / g, 4.8 J / g It may be from 4.8 J / g to 28.0 J / g, or from 30.0 J / g to 30.0 J / g.

[0072] After the first heat treatment, the first melting temperature (T m1 ) satisfies the above range, it may be advantageous to satisfy the desired heat shrinkage rate and crystallinity. In particular, the polyester stretched film according to the present invention is manufactured from a stretched film containing a polyester resin, wherein the stretched film exhibits excellent heat shrinkage properties through primary heat treatment, and the polyester stretched film manufactured therefrom has excellent heat shrinkage properties.

[0073] In addition, after the first heat treatment, at least one first melting temperature (T m1 ) represents the total heat of fusion (H 1T ) may be 1.0 J / g or more, 1.5 J / g or more, 2.0 J / g or more, 40.0 J / g or less, 35.0 J / g or less, 30.0 J / g or less, 25.0 J / g or less, or 20.0 J / g or less. More specifically, after the first heat treatment, the total sum of the heat of fusion (H 1T) is, for example, 1.0 J / g to 40.0 J / g, 1.0 J / g to 30.0 J / g, 1.0 J / g to 28.0 J / g, 2.0 J / g to 40.0 J / g, 2.0 J / g to 30.0 J / g, 2.0 J / g to 28.0 J / g, 3.0 J / g to 40.0 J / g, 3.0 J / g to 30.0 J / g, 3.0 J / g to 28.0 J / g, 4.0 J / g to 40.0 J / g, 4.0 J / g to 30.0 J / g, 4.0 J / g to 28.0 J / g, 4.8 J / g to 40.0 J / g, 4.8 J / g to 30.0 J / g, or It can be from 4.8 J / g to 28.0 J / g.

[0074] The total sum of the above heats of fusion (H 1T ) may be more advantageous in achieving the desired effect if it satisfies the above range.

[0075] In addition, after the second heat treatment, the second melting temperature (T m2 ) may be more than 0.0 J / g, more than 0.1 J / g, more than 0.5 J / g, more than 1.0 J / g, more than 1.5 J / g, less than 50.0 J / g, less than 45.0 J / g, less than 40.0 J / g, less than 35.0 J / g, or less than 30.0 J / g. More specifically, after the second heat treatment, the second melting temperature (T m2) is, for example, more than 0.0 J / g to less than 50.0 J / g, 0.1 J / g to 49.0 J / g, 0.1 J / g to 45.0 J / g, 0.1 J / g to 40.0 J / g, 0.5 J / g to 49.0 J / g, 0.5 J / g to 45.0 J / g, 0.5 J / g to 40.0 J / g, 0.5 J / g to 33.0 J / g, 0.5 J / g to 30.0 J / g, 1.0 J / g to 49.0 J / g, 1.0 J / g to 45.0 J / g, 1.0 J / g to 40.0 J / g, 1.0 J / g to 33.0 J / g, 1.0 J / g to 30.0 J / g, 1.5 J / g to 49.0 J / g, 1.5 J / g to 45.0 J / g, 1.5 J / g to 40.0 J / g, 1.5 J / g to 33.0 J / g, or 1.5 J / g to 30.0 J / g.

[0076] After the above second heat treatment, the second melting temperature (T m2 ) satisfies the above range, it may be more advantageous to satisfy the desired heat shrinkage rate and crystallinity.

[0077] After the above secondary heat treatment, one or more second melting temperatures (T m2 ) represents the total heat of fusion (H 2T ) may be 1.0 J / g or more, 1.5 J / g or more, less than 50.0 J / g, 49.0 J / g or less, 45.0 J / g or less, 40.0 J / g or less, 35.0 J / g or less, or 30.0 J / g or less. More specifically, the total sum of the heats of fusion of the above 2 (H 2T) may be, for example, 1.0 J / g to 49.0 J / g, 1.0 J / g to 45.0 J / g, 1.0 J / g to 40.0 J / g, 1.0 J / g to 33.0 J / g, 1.0 J / g to 30.0 J / g, 1.5 J / g to 49.0 J / g, 1.5 J / g to 45.0 J / g, 1.5 J / g to 40.0 J / g, 1.5 J / g to 33.0 J / g, or 1.5 J / g to 30.0 J / g.

[0078] The total sum of the above heats of fusion (H 2T ) may be more advantageous in achieving the desired effect if it satisfies the above range.

[0079] In addition, the polyester stretch film is pre-heat treated after the first heat treatment and before the second heat treatment, and then the second-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) may be 1.0 J / g or more, 1.5 J / g or more, 2.0 J / g or more, 40.0 J / g or less, 35.0 J / g or less, or 33.0 J / g or less. More specifically, the second-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) is, for example, 1.0 J / g to 40.0 J / g, 1.0 J / g to 38.0 J / g, 1.0 J / g to 35.0 J / g, 2.0 J / g to 40.0 J / g, 2.0 J / g to 38.0 J / g, 2.0 J / g to 35.0 J / g, 3.0 J / g to 40.0 J / g, 3.0 J / g to 38.0 J / g, 3.0 J / g to 35.0 J / g, 4.0 J / g to 40.0 J / g, 4.0 J / g to 38.0 J / g, 4.0 J / g to 35.0 J / g, 4.7 J / g to 40.0 J / g, 4.7 J / g to 38.0 J / g, or It can be from 4.7 J / g to 35.0 J / g.

[0080] After the pre-heat treatment of the first heat-treated polyester stretched film, the second-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) satisfies the above range, the crystallinity of the film is maximized, thereby further improving the efficiency of the recycling process.

[0081] In addition, the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) The crystallinity of the polyester stretched film may vary depending on the ratio (H2 / H1) of the second heat of fusion (H2).

[0082] Specifically, the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) may be 0.1 or more in the ratio (H2 / H1) of the second heat of fusion (H2), for example, 0.1 to 10.0, 0.2 to 9.5, 0.3 to 9.0, 0.3 to 8.5, 0.3 to 8.0, 0.3 to 7.0, 0.3 to 6.0, 0.3 to 5.0, 0.3 to 4.0, 0.3 to 3.8, 0.3 to 3.5, 0.3 to 3.0, 0.3 to 2.9, 0.3 to 2.5, 1.0 to 3.5, 1.0 to 3.4, or 1.0 to 3.0.

[0083] The above first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) when the ratio (H2 / H1) of the second heat of fusion (H2) satisfies the above range, excellent heat shrinkage can be satisfied while improving crystallinity.

[0084] According to an embodiment, the polyester stretched film can exhibit an increase in the sum of the heat of fusion after the first heat treatment, the pre-heat treatment, and the second heat treatment. In particular, the film exhibited a number of elevated melting temperatures after the second heat treatment compared to before the heat treatment. This indicates that the pre-heat treatment initiates crystallization, thereby further enhancing crystallinity after the second heat treatment.

[0085] In addition, the total sum of the heat of fusion after the above secondary heat treatment (H 2T ) after the first heat treatment, the total heat of fusion (H 1T ) ratio (H 1T / H 2T ) may be 0.1 or more, for example, 0.1 to 10.0, 0.1 to 9.5, 0.1 to 9.0, 0.2 to 8.5, 0.2 to 8.0, 0.3 to 7.0, 0.3 to 6.0, 0.3 to 5.0, 0.3 to 4.0, 0.3 to 3.8, 0.3 to 3.5, or 0.3 to 3.0.

[0086] In addition, the second-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) for the second melting temperature (T m2 ) the ratio of the second heat of fusion (H2) (H2 / H 2-p ) may be 0.1 or more, for example, 0.1 to 10.0, 0.2 to 9.5, 0.3 to 9.0, 0.3 to 8.5, 0.3 to 8.0, 0.3 to 7.0, 0.3 to 6.0, 0.3 to 5.0, 0.3 to 4.0, 0.3 to 3.8, 0.3 to 3.5, 0.3 to 3.3, 0.3 to 3.2, 0.35 to 3.0, 0.35 to 2.8, or 0.35 to 2.5.

[0087] The above 2-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) for the second melting temperature (T m2) the ratio of the second heat of fusion (H2) (H2 / H 2-p ) When the above range is satisfied, excellent heat shrinkage properties can be satisfied while simultaneously maximizing crystallinity.

[0088] Meanwhile, the polyester stretch film may have a heat shrinkage rate of 40% or more as expressed by the following formula 1-1.

[0089]

[0090] In the above equation 1-1,

[0091] L 25 is the initial transverse direction (TD) length of the polyester stretched film sample at 25 ℃,

[0092] L 80 is the transverse direction (TD) length of the polyester stretched film sample after immersion in hot water at 80°C for 10 seconds.

[0093] Specifically, the polyester stretched film may have a heat shrinkage ratio in the main shrinkage direction represented by the above formula 1-1 of 40% or more, and more specifically, 42% or more, 44% or more, 46% or more, 48% or more, 50% or more, 52% or more, 55% or more, or 60% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 80°C may be 40 to 70%, 41 to 65%, 42 to 60%, 43 to 60%, 44 to 58%, or 45 to 56%.

[0094] In addition, the polyester stretch film may have a heat shrinkage rate of 50% or more as expressed by the following formula 1-2.

[0095]

[0096] In the above equation 1-2,

[0097] L 25 is the initial transverse direction (TD) length of the polyester stretched film sample at 25 ℃,

[0098] L90 is the transverse direction (TD) length of the polyester stretched film sample after immersion in hot water at 90°C for 10 seconds.

[0099] Specifically, the polyester stretched film may have a heat shrinkage ratio in the main shrinkage direction represented by the above formula 1-2 of 50% or more, specifically 51% or more, 52% or more, 54% or more, 56% or more, 60% or more, 63% or more, or 65% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 90°C may be 50 to 80%, 51 to 80%, 52 to 80%, 53 to 79%, 54 to 79%, or 55 to 78%.

[0100] Meanwhile, when applying a polyester label including the polyester stretch film to a plastic container, specifically a polyethylene terephthalate (PET) container, the crystalline fraction may be 30% or more.

[0101] According to an embodiment, a polyester stretched film comprising a polyester resin polymerized with a diol component and a dicarboxylic acid component, wherein the polyester stretched film is first heat-treated at 70° C., pre-heat-treated at 160° C., and then cut into 1 cm × 1 cm pieces to obtain a polyester stretched film sample, and a polyethylene terephthalate (PET) sample obtained by passing a PET container through a sieve with a diameter of 12.5 mm, are mixed in a weight ratio of 97:3, heat-treated at 195° C. for 90 minutes, and then the heat-treated mixed sample is passed through the sieve to evaluate the crystallinity of the polyester stretched film, and the crystallinity fraction represented by the following Equation 2 is 30% or more:

[0102] [Formula 2]

[0103] Crystalline fraction (%) = (F T / F m )×100

[0104] In the above equation 2,

[0105] F above T is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed samples, the weight (S) of the sample passing through a 12.5 mm mesh sieve s ) ratio ((S s / M T ) × 100, %),

[0106] F above m is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed sample remaining on a 12.5 mm mesh sieve (C s ) ratio ((C s / M T ) × 100, %).

[0107] Additionally, the agglomerated sample remaining on the 12.5 mm mesh sieve among the above heat-treated mixed samples can be defined as a polyester stretch film sample (agglomerated sample) fused with the PET sample after heat treatment.

[0108] Among the above heat-treated mixed samples, a sample that passes through a 12.5 mm mesh sieve is defined as a polyester stretch film sample separated from a PET sample after heat treatment.

[0109] For example, the crystalline fraction represented by the above formula 2 may be 40% or more, 45% or more, 47% or more, 50% or more, 52% or more, 60% or more, 65% or more, 67% or more, 70% or more, 80% or more, 90% or more, 95% or more, or 100%.

[0110] The above polyester stretch film sample can be cut after the first heat treatment and the pre-heat treatment. That is, the above polyester stretch film sample can be cut after the pre-heat treatment and before the second heat treatment.

[0111] The crystallinity fraction represented by the above formula 2 can be an indicator for evaluating the degree of recyclability and recycling process efficiency.

[0112] Specifically, when the above crystallinity fraction satisfies the above range or more, recyclability and recycling process efficiency can be excellent.

[0113] Specifically, the polyester stretched film according to this embodiment has excellent heat shrinkability and high crystallinity, and thus can be usefully applied as a heat shrinkable film for packaging or labeling plastic containers. In particular, the polyester stretched film according to the present invention has a crystallinity similar to or equivalent to that of a plastic container (e.g., a PET bottle) having high crystallinity by undergoing the first heat treatment and the second heat treatment (or the second heat treatment after the pre-heat treatment) processes (specifically, has a crystallinity similar to or equivalent to that of the polyethylene terephthalate (PET) component, which is a component of the PET bottle), and thus, in the recycling process of the used waste plastic container, no fusion occurs with the plastic container, and thus the recycling process of the waste plastic container can be performed without undergoing a process of separating (removing) the polyester stretched film from the waste plastic container. Therefore, the present invention can increase the efficiency of the recycling process of the waste plastic container compared to the related art.

[0114] Meanwhile, the polyester resin included in the polyester stretch film according to the present invention may be a polyester resin in which a diol component and a dicarboxylic acid component are polymerized.

[0115] According to the present invention, the diol component may be a commonly known diol component. Specifically, the above diol component is bis-2-hydroxyethyl terephthalate, isosorbide, neopentyl glycol, ethylene glycol, cyclohexanedimethanol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl It may include at least one selected from the group consisting of 4-(hydroxymethyl)cyclohexanecarboxylate (CHDM derivative), 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol (CHDM derivative), recycled cyclohexanedimethanol, recycled ethylene glycol, recycled bis-2-hydroxyethyl terephthalate, and recycled diethylene glycol. Preferably, when considering the crystallinity, heat shrinkage, economic efficiency, etc. of the polyester stretched film, the diol component may include two or more (specifically, three or more, four or more, or five or more) selected from the group consisting of bis-2-hydroxyethyl terephthalate, isosorbide, ethylene glycol, cyclohexanedimethanol, neopentyl glycol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, and recycled bis-2-hydroxyethyl terephthalate.

[0116] For example, the diol component may include at least one (specifically, at least two, at least three, or at least four) selected from the group consisting of ethylene glycol and, as a comonomer, bis-2-hydroxyethyl terephthalate, isosorbide, cyclohexanedimethanol, neopentyl glycol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl 4-(hydroxymethyl)cyclohexanecarboxylate, 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, and recycled bis-2-hydroxyethyl terephthalate.

[0117] When the diol component includes the ethylene glycol and the comonomer, the amounts of these components used are not particularly limited, but based on the total weight of the diol component, the amount of ethylene glycol used may be 10 to less than 100 wt%, 15 to 90 wt%, 20 to 85 wt%, 30 to 85 wt%, or 50 to 85 wt%, and the amount of the comonomer used may be more than 0 to 90 wt%, more than 0 to 85 wt%, 1 to 90 wt%, 1 to 50 wt%, 2 to 50 wt%, 10 to 85 wt%, 15 to 80 wt%, 15 to 70 wt%, or 15 to 50 wt%. In particular, when diethylene glycol is used as the comonomer, the amount of diethylene glycol used may be 0 to 50 wt%, 1 to 50 wt%, 2 to 50 wt%, 3 to 45 wt%, 4 to 40 wt%, or 5 to 35 wt%, based on the total weight of the diol component. Accordingly, the polyester resin according to the present invention may contain a structural unit derived from diethylene glycol in an amount of 0 to 50 wt%, 1 to 50 wt%, 2 to 50 wt%, 3 to 45 wt%, 4 to 40 wt%, or 5 to 35 wt%, based on the total weight of the polyester resin.

[0118] According to the present invention, the dicarboxylic acid component may be a commonly known dicarboxylic acid component. Specifically, the dicarboxylic acid component may include at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, diphenyl dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, dimethyl 1,4-cyclohexane dicarboxylate, dimethyl 1,3-cyclohexane dicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, azelaic acid, regenerated isophthalic acid, regenerated terephthalic acid, regenerated dimethyl isophthalate, and regenerated dimethyl phthalate. Preferably, when considering the crystallinity and heat shrinkage properties of the polyester stretch film, the dicarboxylic acid component may include at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl phthalate, and dimethyl isophthalate.

[0119] According to the present invention, the polyester resin may have an intrinsic viscosity (IV) at 35°C of 0.5 to 1.2 dl / g, specifically 0.52 to 1.15 dl / g, 0.55 to 1.13 dl / g, 0.58 to 1.1 dl / g, 0.6 to 0.9 dl / g, 0.62 to 0.88 dl / g, 0.65 to 0.85 dl / g, 0.68 to 0.83 dl / g, or 0.7 to 0.8 dl / g. As the intrinsic viscosity is within the above range, the processability of the polyester resin can be secured.

[0120]

[0121] Method for manufacturing polyester stretch film

[0122] According to one embodiment, a method for manufacturing the above-described polyester stretch film is provided.

[0123] Specifically, a method for manufacturing a polyester stretched film according to one embodiment includes a step (S-1) of manufacturing a polyester resin by polymerizing a diol component and a dicarboxylic acid component; a step (S-2) of manufacturing a polyester stretched sheet from the polyester resin; and a step (S-3) of heat-setting the stretched sheet, and after the first heat treatment and the second heat treatment, when analyzed by differential scanning calorimetry (DSC), a first melting temperature (T m1 ) and the second melting temperature (T m2 ) represents the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) may have a ratio (H2 / H1) of the second heat of fusion (H2) of 0.1 or more.

[0124] In addition, a method for manufacturing a polyester stretch film according to one embodiment comprises: a step (S-1) of manufacturing a polyester resin by polymerizing a diol component and a dicarboxylic acid component; a step (S-2) of manufacturing a polyester stretch sheet from the polyester resin; And a step (S-3) of heat-treating the stretched sheet, and a polyester stretched film sample obtained by first heat-treating the polyester stretched film at 70° C., pre-heat-treating it at 160° C., and then cutting it into 1 cm × 1 cm pieces, and a polyethylene terephthalate (PET) sample obtained by passing a PET container through a sieve with a diameter of 12.5 mm, are mixed in a weight ratio of 97:3, heat-treated at 195° C. for 90 minutes, and then passing the heat-treated mixed sample through the sieve to evaluate the crystallinity of the polyester stretched film, the crystallinity fraction represented by the above formula 2 may be 30% or more.

[0125]

[0126] To explain this in detail, it is as follows.

[0127]

[0128] Step (S-1): Polyester resin manufacturing

[0129] The above step (S-1) is a step of manufacturing a polyester resin (copolymer) by polymerizing a diol component and a dicarboxylic acid component.

[0130] Descriptions of each of the diol component and the dicarboxylic acid component for the polymerization are the same as described above and are therefore omitted.

[0131] The polymerization of the above diol component and the above dicarboxylic acid component can be carried out by a conventionally known method (e.g., liquid phase polymerization, solid phase polymerization, etc.), and a batch reactor or a continuous reactor can be used for the polymerization reaction. Specifically, the polymerization reaction can include an esterification reaction (esterification exchange reaction) in which the diol component and the dicarboxylic acid component are reacted to produce an oligomer, and a polycondensation reaction of the oligomer.

[0132] The temperature at which the esterification reaction takes place is not particularly limited, but considering the properties of the polyester resin and the polyester stretched film, it may be 230 to 270°C, 235 to 268°C, 240 to 265°C, or 240 to 260°C. In addition, the time at which the esterification reaction takes place is not particularly limited, but may be 1 to 24 hours, 2 to 22 hours, 3 to 20 hours, or 4 to 18 hours. In addition, the pressure at which the esterification reaction takes place is not particularly limited, but may be 0 to 5.0 kgf / cm. 2 , 0.1 to 4.5 kgf / cm 2 , 0.1 to 4.0 kgf / cm 2 , or 0.1 to 3.0 kgf / cm 2 It could be.

[0133] The temperature at which the polycondensation reaction takes place is not particularly limited, but considering the properties of the polyester resin and the polyester stretched film, it may be 245 to 290°C, 250 to 285°C, 255 to 280°C, or 255 to 270°C. In addition, the time at which the polycondensation reaction takes place is not particularly limited, but may be 1 to 24 hours, 2 to 24 hours, 5 to 22 hours, or 7 to 20 hours.

[0134] Meanwhile, an additive including at least one selected from the group consisting of a catalyst, a stabilizer, a coloring agent, a crystallizer, an antioxidant, and a branching agent may be added to the polymerization reaction.

[0135] The catalyst is not particularly limited, but specifically, methylates of sodium and magnesium; acetates, borates, fatty acid salts, or carbonates of Zn, Cd, Mn, Co, Ca, Ba, etc.; oxides or hydrates of Mg, Pb, Mn, Ti, Zn, Sb, Ge, etc. can be used. For example, the catalyst can be tetraethyl titanate, acetyltripropyl titanate, tetrapropyl titanate, tetrabutyl titanate, 2-ethylhexyl titanate, octylene glycol titanate, triethanolamine titanate, acetylacetonate titanate, ethylacetoacetic ester titanate, isostearyl titanate, titanium dioxide, germanium dioxide, germanium tetrachloride, germanium ethyleneglycoxide, germanium acetate, or a combination thereof.

[0136] The above stabilizer is not particularly limited, but phosphorus compounds such as phosphoric acid, trimethyl phosphate, and triethyl phosphate can be used.

[0137] The above coloring agent is not particularly limited, but organic compounds such as cobalt compounds, anthraquionone compounds, perinone compounds, azo compounds, and methine compounds (e.g., cobalt acetate, cobalt propionate, Clarient's Polysynthren Blue RLS toner, Clarient's Solvaperm Red BB toner) can be used.

[0138] The above crystallizer is not particularly limited, but a crystal nucleating agent, an ultraviolet absorber, a polyolefin resin, a polyamide resin, etc. can be used.

[0139]

[0140] The above antioxidant is not particularly limited, but hindered phenol compounds, phosphite compounds, thioether compounds, etc. can be used.

[0141] The above branching agent is not particularly limited, but trimellitic anhydride, trimellitic propane, trimellitic acid, etc. can be used.

[0142]

[0143] Step (S-2): Manufacturing of polyester stretch sheet

[0144] The above step (S-2) is a step for manufacturing a polyester stretched sheet from the polyester resin obtained in the above step (S-1). The manufacturing of the stretched sheet can be carried out by a conventionally known method, and specifically, the stretched sheet can be manufactured through a melting and casting process of the polyester resin, a uniaxial or biaxial stretching process, and / or a heat setting process.

[0145] The melting and casting process of the polyester resin may be performed through an extruder, and at this time, the melting temperature is not particularly limited, but may be 180 to 310°C, 200 to 310°C, 230 to 310°C, 240 to 300°C, or 250 to 290°C. By performing this process, an unstretched sheet may be obtained, and the obtained unstretched sheet may be passed to a stretching process. The unstretched sheet may be preheated to a predetermined temperature (e.g., 90 to 120°C) before undergoing the stretching process.

[0146] The above-described uniaxial or biaxial stretching process can be performed by stretching the unstretched sheet obtained through the above-described melting and casting process in the machine direction (MD), the transverse direction (TD), or both directions. The stretching in the machine direction can be performed at a stretching ratio of 1 to 5 times, or 1.1 to 4.5 times, at a temperature of 55 to 180°C or 60 to 170°C. In addition, the stretching in the transverse direction can be performed at a stretching ratio of 1.5 to 6 times, or 2.5 to 5.5 times, at a temperature of 55 to 180°C or 60 to 170°C.

[0147] The polyester stretched film manufactured through this stretching process may have a heat shrinkage ratio in the main shrinkage direction of 40% or more at 80°C, and more specifically, 42% or more, 44% or more, 46% or more, 48% or more, 50% or more, 52% or more, 55% or more, or 60% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 80°C may be 40 to 70%, 41 to 65%, 42 to 60%, 43 to 60%, 44 to 58%, or 45 to 56%.

[0148] In addition, the polyester stretched film manufactured through the stretching process may have a heat shrinkage ratio in the main shrinkage direction of 50% or more at 90°C, and specifically, may be 51% or more, 52% or more, 54% or more, 56% or more, 60% or more, 63% or more, or 65% or more. For example, the heat shrinkage ratio in the main shrinkage direction at 90°C may be 50 to 80%, 51 to 80%, 52 to 80%, 53 to 79%, 54 to 79%, or 55 to 78%.

[0149]

[0150] Step (S-3): Open fixation

[0151] The above step (S-3) is a step of heat-setting the stretched sheet obtained in the above step (S-2). The temperature at which the stretched sheet is heat-set is not particularly limited, but may be similar to or higher than the stretching process temperature. Specifically, the heat-setting temperature may be 60 to 200°C, 65 to 190°C, 65 to 180°C, or 65 to 170°C. As the heat-setting temperature is within the above range, a polyester stretched film with increased crystallinity and mechanical strength can be manufactured.

[0152]

[0153] Meanwhile, the polyester stretch film may further include a heat treatment process. The heat treatment may be performed two or more times.

[0154] Step (S-4): Primary heat treatment

[0155] The above step (S-4) is a step of first heat treating the polyester stretch film obtained in the above step (S-3).

[0156] The above first heat treatment temperature is not particularly limited, but may be 60 to 105°C, and specifically, 62 to 104°C, 62 to 103°C, 65 to 102°C, 68 to 100°C, 70 to 100°C, 70 to 98°C, 70 to 97°C, or 70 to 96°C. For example, the first heat treatment may be performed by immersing the polyester stretch film manufactured in the step (S-3) in hot water having the temperature range for less than 1 minute, specifically less than 50 seconds, less than 40 seconds, less than 30 seconds, less than 20 seconds, specifically 5 to 60 seconds, 5 to 50 seconds, 5 to 40 seconds, 5 to 30 seconds, 5 to 20 seconds, or 5 to 15 seconds.

[0157]

[0158] Step (S-5): Secondary heat treatment

[0159] The above step (S-5) is a step of secondarily heat-treating the polyester stretched film that was first heat-treated in the above step (S-4). The temperature of the second heat treatment is not particularly limited, but may be 140 to 220°C, and specifically, 141 to 219°C, 142 to 218°C, 143 to 217°C, 144 to 216°C, 145 to 215°C, 145 to 214°C, 146 to 213°C, or 150 to 210°C. For example, the secondary heat treatment may be performed by placing the polyester stretch film that was first heat-treated in the step (S-4) into an oven and applying the temperature range described above, and storing it for less than 4 hours, specifically, 200 minutes or less, 180 minutes or less, 150 minutes or less, 120 minutes or less, 100 minutes or less, for example, 10 to 200 minutes, 10 to 180 minutes, 20 to 150 minutes, 30 to 120 minutes, 40 to 120 minutes, 60 to 120 minutes, or 70 to 100 minutes.

[0160] Additionally, according to one embodiment, the step (S-5) may further include a step of pre-heat-treating the polyester stretch film that has been first heat-treated in the step (S-4) before the second heat treatment.

[0161] Specifically, the secondary heat treatment may be performed after the primary heat-treated polyester stretched film is pre-heat-treated.

[0162] The above pre-heat treatment can be performed at the same or similar temperature range as the above secondary heat treatment. For example, the pre-heat treatment temperature can be 140 to 220°C, and specifically, 141 to 219°C, 142 to 218°C, 143 to 217°C, 144 to 216°C, 145 to 215°C, 145 to 214°C, 146 to 213°C, or 150 to 210°C for 1 to 30 minutes, 1 to 20 minutes, 5 to 30 minutes, 5 to 25 minutes, 5 to 20 minutes, 5 to 15 minutes, 6 to 25 minutes, 6 to 20 minutes, 6 to 15 minutes, or 6 to 13 minutes.

[0163] For example, the step (S-5) may include a step of pre-heat-treating the polyester stretched film that has been first heat-treated in the step (S-4) at 140 to 220°C for 1 to 30 minutes, then cooling it to room temperature for 1 to 30 minutes, and then secondarily heat-treating the pre-heat-treated polyester stretched film again at 140 to 220°C for 10 to 200 minutes.

[0164] In addition, the step (S-5) may include a step of pre-heat-treating the polyester stretched film that has been first heat-treated in the step (S-4) at 150 to 210°C for 1 to 30 minutes, then cooling it to room temperature for 1 to 30 minutes, and then secondarily heat-treating the pre-heat-treated polyester stretched film again at 150 to 210°C for 10 to 180 minutes.

[0165] In this way, the present invention can control crystallinity to be high while having an excellent heat shrinkage rate by heat-treating a polyester stretched film obtained through the above stretching process.

[0166] Specifically, the polyester stretched film can shrink through primary heat treatment, and can improve the crystallinity of the polyester stretched film through secondary heat treatment.

[0167] In addition, when a pre-heat treatment is performed after the first heat treatment and before the second heat treatment, the polyester stretched film shrunk by the first heat treatment can be crystallized, and the crystallinity of the polyester stretched film can be maximized to an optimal range through the second heat treatment, thereby further improving the efficiency of the recycling process.

[0168] If the heat treatment of the polyester stretched film is performed only once (once), the crystallinity of the film does not increase to the desired level, so it is preferable that the heat treatment of the polyester stretched film be performed multiple times (more than twice) including the first and second (twice) treatments, or the first, pre-heat treatment, and the second treatment, as in the present invention.

[0169] Meanwhile, the polyester stretch film of the present invention manufactured through these steps has a first melting temperature (T) when analyzed by the differential scanning calorimetry (DSC) described above after the first heat treatment and the second heat treatment. m1 ) and the second melting temperature (T m2 ) represents the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) so that the ratio (H2 / H1) of the second heat of fusion (H2) satisfies a specific range, the crystallinity can be very high while the heat shrinkage, heat resistance, and durability can be excellent.

[0170] The heat treatment temperature and time of the first and second heat treatments are as described above.

[0171] Additionally, the temperature and time of the pre-heat treatment described below are as described above.

[0172] According to another embodiment, after the first heat treatment, after the pre-heat treatment before the second heat treatment, and after the second heat treatment, the first melting temperature (T) described above is analyzed by the differential scanning calorimetry (DSC) described above. m1 ), the second-p melting temperature (T m2-p ) and the second melting temperature (T m2 ) represents the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) the ratio of the second heat of fusion (H2) (H2 / H1) and / or the second-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) for the second melting temperature (T m2 ) the ratio of the second heat of fusion (H2) (H2 / H 2-p ) can be maximized by satisfying a specific range, and due to this high crystallinity, the recycling process of waste plastic containers can be performed without separating the polyester stretch film during the recycling process of used waste plastic containers (the waste plastic container can be fed into the recycling process with the polyester stretch film attached). Accordingly, the present invention can increase the efficiency of the recycling process compared to the prior art.

[0173]

[0174] article

[0175] The present invention provides an article comprising a polyester stretch film.

[0176] According to one embodiment, a polyester stretched film comprising a polyester resin, wherein the polyester stretched film comprises a polyester resin in which a diol component and a dicarboxylic acid component are polymerized, and when analyzed by differential scanning calorimetry (DSC) after a first heat treatment and a second heat treatment, a first melting temperature (T m1 ) and the second melting temperature (T m2 ) represents the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) can provide a product having a ratio of the second heat of fusion (H2) (H2 / H1) of 0.1 or more.

[0177] In addition, the above article may include a polyester stretched film (polyester film) manufactured by subjecting the stretched film to the above-described first heat treatment and second heat treatment, or the first heat treatment, pre-heat treatment, and second heat treatment processes.

[0178] In addition, the above article can be obtained by molding the polyester resin by a molding method such as extrusion or injection, and can be a film (or sheet) or a component used in the fields of automobiles, electricity, electronics, etc.

[0179] In addition, the above-mentioned article may include labels, cap seals, or packaging materials for various containers such as plastic.

[0180]

[0181] The present invention is described in more detail through the following examples. However, the following examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention.

[0182] [Example 1]

[0183] 1) Manufacturing of polyester resin (copolymer)

[0184] Terephthalic acid (TPA, 7693.0 g), isosorbide (ISB, 96.7 g), ethylene glycol (EG, 2601.3 g), 1,4-cyclohexanedimethanol (CHDM, 1557.1 g), diethylene glycol (DEG, 1213.7 g), Ge catalyst (GeO2, 1.0 g), Ti catalyst 1.0 g), phosphoric acid (phosphoric acid, 1.5 g), blue toner (0.01 g), and red toner (0.005 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 265 ℃, and an esterification reaction (ES) was performed at 265 ℃ under a pressure of 2 kgf / cm2 to obtain a transparent reactant.

[0185] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 270°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.77 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0186] 2) Manufacturing of polyester stretch sheet

[0187] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0188] 3) Open fixation

[0189] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0190] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in warm water at 70°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 160°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 160°C for 90 minutes to pre-heat treat it a second time.

[0191]

[0192] [Example 2]

[0193] 1) Manufacturing of polyester resin (copolymer)

[0194] Into a 10 L reactor connected to a column and a water-cooled condenser, terephthalic acid (TPA, 7663.2 g), ethylene glycol (EG, 3345.5 g), 1,4-cyclohexanedimethanol (CHDM, 1255.7 g), neopentyl glycol (NPG, 106.7 g), diethylene glycol (DEG, 978.7 g), cyclohexanedimethanol derivative (CHDM derivative, 247.4 g), Ti catalyst (1.0 g), blue toner (0.01 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 255 ℃, and an esterification reaction (ES) was performed at 255 ℃ under a pressure of 1 kgf / ㎠ to obtain a transparent reactant.

[0195] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.65 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0196] 2) Manufacturing of polyester stretch sheet

[0197] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0198] 3) Open fixation

[0199] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0200] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in warm water at 90°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 175°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 175°C for 90 minutes to pre-heat treat it a second time.

[0201]

[0202] [Example 3]

[0203] 1) Manufacturing of polyester resin (copolymer)

[0204] Into a 10 L reactor connected to a column and a water-cooled condenser, regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 1202.9 g), terephthalic acid (TPA, 7075.2 g), ethylene glycol (EG, 3488.9 g), 1,4-cyclohexanedimethanol (CHDM, 1363.9 g), diethylene glycol (DEG, 1063.0 g), Ti catalyst (1.0 g), blue toner (0.02 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 255 ℃, and an esterification reaction (ES) was performed at 255 ℃ under a pressure of 0.5 kgf / ㎠ to obtain a transparent reactant.

[0205] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.70 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0206] 2) Manufacturing of polyester stretch sheet

[0207] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0208] 3) Open fixation

[0209] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0210] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in warm water at 95°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 155°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 155°C for 90 minutes to pre-heat treat it a second time.

[0211]

[0212] [Example 4]

[0213] 1) Manufacturing of polyester resin (copolymer)

[0214] Terephthalic acid (TPA, 7918.3 g), ethylene glycol (EG, 4080.5 g), 1,4-cyclohexanedimethanol (CHDM, 1068.5 g), diethylene glycol (DEG, 832.8 g), Ge catalyst (GeO2, 1.0 g), blue toner (0.05 g), and red toner (0.02 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 260 °C, and an esterification reaction (ES) was performed at 260 °C under a pressure of 1 kgf / cm2 to obtain a transparent reactant.

[0215] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 275°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.78, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0216] 2) Manufacturing of polyester stretch sheet

[0217] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0218] 3) Open fixation

[0219] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0220] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in warm water at 95°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 165°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 165°C for 90 minutes to pre-heat treat it a second time.

[0221]

[0222] [Example 5]

[0223] 1) Manufacturing of polyester resin (copolymer)

[0224] Terephthalic acid (TPA, 7878.5 g), isosorbide (ISB, 494.9 g), ethylene glycol (EG, 4076.7 g), 1,4-cyclohexanedimethanol (CHDM, 1139.1 g), diethylene glycol (DEG, 887.8 g), Mn catalyst (Mn(II) acetate tetrahydrate, 1.5 g), Sb catalyst (Sb2O3, 1.8 g), and cobalt acetate (cobalt acetate, 0.8 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 240 ℃, and an esterification reaction (ES) was performed at 240 ℃ under a pressure of 0.1 kgf / ㎠ to obtain a transparent reactant.

[0225] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 255°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.85, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0226] 2) Manufacturing of polyester stretch sheet

[0227] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0228] 3) Open fixation

[0229] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0230] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in warm water at 95°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 175°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 175°C for 90 minutes to pre-heat treat it a second time.

[0231]

[0232] [Example 6]

[0233] 1) Manufacturing of polyester resin (copolymer)

[0234] Terephthalic acid (TPA, 8279.3 g), ethylene glycol (EG, 4432.3 g), neopentyl glycol (NPG, 864.5 g), Ge catalyst (GeO2, 1.0 g), cobalt acetate (0.4 g), blue toner (0.03 g), and red toner (0.01 g) were added to a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 250 °C, and an esterification reaction (ES) was performed at 250 °C under a pressure of 1 kgf / cm2 to obtain a transparent reactant.

[0235] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.70 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0236] 2) Manufacturing of polyester stretch film

[0237] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0238] 3) Open fixation

[0239] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0240] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in warm water at 95°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 160°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 160°C for 90 minutes to pre-heat treat it a second time.

[0241]

[0242] [Example 7]

[0243] 1) Manufacturing of polyester resin (copolymer)

[0244] In a 10 L reactor connected to a column and a water-cooled condenser, regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 2288.5 g), terephthalic acid (TPA, 5982.5 g), ethylene glycol (EG, 739.3 g), 1,4-cyclohexanedimethanol (CHDM, 1441.6 g), neopentyl glycol (NPG, 1301.4 g), diethylene glycol (DEG, 1123.6 g), Ge catalyst (GeO2, 1.0 g), blue toner (0.03 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 265 ℃, and an esterification reaction (ES) was performed at 265 ℃ under a pressure of 2 kgf / cm2 to obtain a transparent reactant.

[0245] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 270°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.78 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0246] 2) Manufacturing of polyester stretch sheet

[0247] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0248] 3) Open fixation

[0249] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0250] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in hot water at 100°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 210°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 210°C for 90 minutes to pre-heat treat it a second time.

[0251]

[0252] [Example 8]

[0253] 1) Manufacturing of polyester resin (copolymer)

[0254] In a 10 L reactor connected to a column and a water-cooled condenser, regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 2509.9 g), terephthalic acid (TPA, 6561.3 g), ethylene glycol (EG, 3281.5 g), 1,4-cyclohexanedimethanol (CHDM, 790.5 g), diethylene glycol (DEG, 616.1 g), Ti catalyst (1.0 g), blue toner (0.01 g), and red toner (0.01 g) were charged. Next, the temperature of the reactor was raised to 263 ℃, and an esterification reaction (ES) was performed at 263 ℃ under a pressure of 1 kgf / cm2 to obtain a transparent reactant.

[0255] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 275°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.70 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0256] 2) Manufacturing of polyester stretch sheet

[0257] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0258] 3) Open fixation

[0259] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0260] Afterwards, the polyester stretched film was subjected to a first heat treatment by immersing it in warm water at 80°C for 10 seconds to shrink it. Next, in order to improve the crystallinity of the polyester stretched film, the polyester stretched film subjected to the first heat treatment was stored in an oven at 170°C for 10 minutes to pre-heat treat it, and then cooled to room temperature for 30 minutes. Then, the polyester stretched film subjected to the pre-heat treatment was stored in an oven at 170°C for 90 minutes to pre-heat treat it a second time.

[0261]

[0262] [Comparative Example 1]

[0263] 1) Manufacturing of polyester resin (copolymer)

[0264] Regenerated bis-2-hydroxyethyl terephthalate (r-BHET, 2256.8 g), terephthalic acid (TPA, 5899.6 g), ethylene glycol (EG, 824.5 g), 1,4-cyclohexanedimethanol (CHDM, 2487.8 g), diethylene glycol (DEG, 1939.0 g), Ge catalyst (GeO2, 1.0 g), blue toner (0.01 g), and red toner (0.01 g) were charged into a 10 L reactor connected to a column and a water-cooled condenser. Next, the temperature of the reactor was raised to 273 ℃, and an esterification reaction (ES) was performed at 273 ℃ under a pressure of 0.5 kgf / ㎠ to obtain a transparent reactant.

[0265] Next, the reactants were transferred to a polycondensation reactor, and a polycondensation reaction (PA) was performed at 285°C while maintaining the pressure of the polycondensation reactor lower than atmospheric pressure. When the intrinsic viscosity (IV) of the reactants inside the polycondensation reactor reached 0.80 dl / g, the reactants were discharged outside the polycondensation reactor to form strands, which were then solidified with a cooling liquid and granulated to an average weight of about 12 to 14 mg, thereby manufacturing polyester resin (copolymer) chips.

[0266] 2) Manufacturing of polyester stretch sheet

[0267] The above polyester resin chips were fed into an extruder and melt-extruded at a temperature of 180 to 310°C and cast at a temperature of 20 to 70°C to produce an unstretched polyester sheet. Subsequently, the unstretched sheet was heated to 75 to 90°C and stretched only in the transverse direction (TD) at a stretch ratio of 5 times to produce an stretched polyester sheet.

[0268] 3) Open fixation

[0269] A polyester stretch film having a thickness of 50 ㎛ was manufactured by heat-setting the above polyester stretch sheet at 60 to 220°C.

[0270] Thereafter, the polyester stretched film was subjected to a primary heat treatment by immersing it in warm water at 110°C for 10 seconds. Then, the polyester stretched film subjected to the primary heat treatment was subjected to a secondary heat treatment by storing it in an oven at 225°C for 30 minutes.

[0271]

[0272] [Example 1]

[0273] In Examples 1 to 8 and Comparative Example 1, each of the polyester stretched films after the first heat treatment, after the pre-heat treatment, and after the second heat treatment was analyzed by differential scanning calorimetry (DSC) to determine the melting temperature (T m ) was confirmed to appear, and the results are shown in Table 1 and Figure 1 (Example 6). The DSC analysis of the polyester stretched film was performed as follows.

[0274] DSC analysis device: Mettler Toledo's DSC 1 model was used.

[0275] Sample preparation: About 6 to 10 mg of primary and secondary, or primary, pre-heat-treated and secondary heat-treated polyester oriented films were taken and filled into an aluminum pan.

[0276] Scan conditions: DSC curves were obtained by heating from room temperature to 280 ℃ at a rate of 10 ℃ / min and annealing at 280 ℃ for 3 minutes.

[0277] Melting temperature verification: The temperature at which an endothermic peak appears during the heating process in the obtained DSC curve was defined as the melting temperature.

[0278] As can be seen in Fig. 1, different analysis results were observed after the first heat treatment, after the pre-heat treatment, and after the second heat treatment of the polyester stretched film of Example 6.

[0279] Specifically, the polyester stretched film of Example 6 showed an increase in the sum of the heat of fusion after the first heat treatment, the pre-heat treatment, and the second heat treatment, and in particular, showed a number of increased melting temperatures after the second heat treatment compared to before the heat treatment. This indicates that crystallization can be initiated by the pre-heat treatment, and that crystallinity can be further improved after the second heat treatment.

[0280]

[0281] [Example 2]

[0282] The heat shrinkage rate of the polyester stretched film after the first heat treatment in Examples 1 to 8 and Comparative Example 1 was evaluated as follows, and the results are shown in Table 1 below.

[0283] Sample preparation: Polyester stretch film was cut into 5 cm × 5 cm pieces and stored at room temperature (25 ℃).

[0284] Heat shrinkage at 80°C: A polyester stretch film sample was immersed in hot water at 80°C for 10 seconds, and the change in length in the transverse direction (TD), which is the main shrinkage direction, was calculated by applying the following equation 1-1.

[0285] Heat shrinkage at 90°C: A polyester stretch film sample was immersed in hot water at 90°C for 10 seconds, and the change in length in the transverse direction (TD), which is the main shrinkage direction, was calculated by applying the following equation 1-2.

[0286]

[0287] In the above equation 1-1,

[0288] L 25 is the initial transverse direction (TD) length of the polyester stretched film sample at 25 ℃,

[0289] L80 is the transverse direction (TD) length of the polyester stretched film sample after immersion in hot water at 80°C for 10 seconds.

[0290]

[0291] In the above equation 1-2,

[0292] L 25 is the initial transverse direction (TD) length of the polyester stretched film sample at 25 ℃,

[0293] L 90 is the transverse direction (TD) length of the polyester stretched film sample after immersion in hot water at 90°C for 10 seconds.

[0294]

[0295] [Example 3]

[0296] The recyclability (crystalline fraction) of each of the pre-heat-treated polyester stretch films obtained in Examples 1 to 8 and Comparative Example 1 before the secondary heat treatment was evaluated as follows, and the results are shown in Table 1 below.

[0297] Sample preparation: The pre-heat-treated polyester stretch films obtained in Examples 1 to 8 and Comparative Example 1 before the secondary heat treatment were cut into 1 cm × 1 cm pieces to prepare polyester stretch film samples (flakes).

[0298] In addition, a polyethylene terephthalate (PET) container was crushed in a crusher and passed through a sieve with a mesh diameter of 12.5 mm to prepare a PET sample (flakes) of the above size in which the polyethylene terephthalate (PET) was crushed.

[0299] After mixing the above polyester stretch film sample (flakes) and PET sample (flakes), the mixed sample was heat-treated at 195°C for 90 minutes.

[0300] Thereafter, the heat-treated mixed sample (mixed flakes) was passed through a sieve with a mesh diameter of 12.5 mm to obtain an aggregated sample remaining on the sieve. This was defined as a polyester stretch film sample fused with a PET sample after heat treatment.

[0301] In addition, the heat-treated mixed sample (mixed flakes) was passed through a sieve with a mesh diameter of 12.5 mm to obtain a sample that passed through the sieve. This was defined as a polyester stretched film sample separated from the PET sample after heat treatment.

[0302] The weight of each of the above samples was measured, and the crystalline fraction (%) expressed by Equation 2 below was calculated using this.

[0303] [Formula 2]

[0304] Crystalline fraction (%) = (F T / F m )×100

[0305] In the above equation 2,

[0306] F above T is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed samples, the weight (S) of the sample passing through a 12.5 mm mesh sieve s ) ratio ((S s / M T ) × 100, %),

[0307] F above m is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed sample remaining on a 12.5 mm mesh sieve (C s ) ratio ((C s / M T ) × 100, %).

[0308]

[0309]

[0310] Referring to Table 1 above, two or more melting temperatures (T) as in the present invention m1 , T m2-p, T m2 ) having the first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) the ratio of the second heat of fusion (H2) (H2 / H1), and the second-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) for the second melting temperature (T m2 ) the ratio of the second heat of fusion (H2) (H2 / H 2-p ) It can be confirmed that the polyester stretch films of Examples 1 to 8 that satisfy this specific range have a high heat shrinkage rate depending on temperature and an improved crystallinity fraction, thereby ensuring recyclability.

[0311] On the other hand, it was confirmed that the polyester stretch film of Comparative Example 1 having a melting temperature of 1 had a significantly reduced crystalline fraction of 27%.

[0312] Meanwhile, it can be confirmed that the polyester stretch film of Example 8, which has a low usage amount of a comonomer (e.g., diethylene glycol), has a somewhat lower heat shrinkage rate.

[0313] Therefore, the polyester stretch film according to the present invention can be usefully used as a heat shrinkable film applied as a packaging and / or label for a plastic container.

[0314] Furthermore, it was confirmed that the polyester stretch film according to the present invention, due to its high crystallinity, enables the recycling process of waste plastic containers without separating the polyester stretch film (the waste plastic container can be fed into the recycling process with the polyester stretch film attached), thereby increasing the efficiency of the recycling process compared to the prior art.

Claims

1. Contains a polyester resin polymerized with a diol component and a dicarboxylic acid component, After the first and second heat treatments, when analyzed by differential scanning calorimetry (DSC), the first melting temperature (T m1 ) and the second melting temperature (T m2 ) represents, The above first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) A polyester stretched film having a ratio of the second heat of fusion (H2) (H2 / H1) of 0.1 or more.

2. In paragraph 1, The above polyester stretched film was subjected to a pre-heat treatment before the second heat treatment after the first heat treatment, and when analyzed by differential scanning calorimetry (DSC), the second-p melting temperature (T m2-p ) represents, The above 2-p melting temperature (T m2-p ) in the second-p heat of fusion (H 2-p ) for the second melting temperature (T m2 ) the ratio of the second heat of fusion (H2) (H2 / H 2-p ) is 0.1 or more, polyester stretched film.

3. In paragraph 1, After the above first heat treatment, at least one first melting temperature (T m1 ) represents the total heat of fusion (H 1T ) is 1.0 J / g or more, a polyester stretched film.

4. In paragraph 1, After the above secondary heat treatment, one or more second melting temperatures (T m2 ) represents the total heat of fusion (H 2T ) is 1.0 J / g or more, a polyester stretched film.

5. In paragraph 1, The total heat of fusion after the above secondary heat treatment (H 2T ) after the first heat treatment, the total heat of fusion (H 1T ) ratio (H 1T / H 2T ) is 0.1 or more, polyester stretched film.

6. In paragraph 1, After the above second heat treatment, the second melting temperature (T m2 ) is 150 ℃ to 230 ℃, and has crystallinity, polyester stretch film.

7. A polyester stretch film comprising a polyester resin polymerized with a diol component and a dicarboxylic acid component, A polyester stretched film sample obtained by first heat-treating the polyester stretched film at 70°C, pre-heat-treating it at 160°C, and then cutting it into 1 cm × 1 cm, and a polyethylene terephthalate (PET) sample obtained by passing a PET container through a sieve with a diameter of 12.5 mm, mixed in a weight ratio of 97:3, heat-treating it at 195°C for 90 minutes, and then passing the heat-treated mixed sample through the sieve to evaluate the crystallinity of the polyester stretched film, wherein the polyester stretched film has a crystallinity fraction of 30% or more, as expressed by the following formula 2: [Formula 2] Crystalline fraction (%) = (F T / F m )×100 In the above equation 2, F above T is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed samples, the weight (S) of the sample passing through a 12.5 mm mesh sieve s ) ratio ((S s / M T ) × 100, %), Above F m is the total weight (M) of the above heat-treated mixed sample T ) of the above heat-treated mixed sample remaining on a 12.5 mm mesh sieve (C s ) ratio ((C s / M T ) × 100, %).

8. In paragraph 1 or paragraph 7, A polyester stretch film having a heat shrinkage rate of 40% or more, as expressed by the following formula 1-1: In the above equation 1-1, L 25 is the initial transverse direction (TD) length of the polyester stretched film sample at 25 ℃, L 80 is the transverse direction (TD) length of the polyester stretched film sample after immersion in hot water at 80°C for 10 seconds.

9. In paragraph 1 or paragraph 7, The above diol component is bis-2-hydroxyethyl terephthalate, isosorbide, neopentyl glycol, ethylene glycol, cyclohexanedimethanol, 1,2-propanediol, 1,3-propanediol, 2-methyl-1,3-propanediol, 2-methylene-1,3-propanediol, 2-ethyl-1,3-propanediol, 2-isopropyl-1,3-propanediol, 2,2-dimethyl-1,3-propanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,5-pentanediol, 3-methyl-2,4-pentanediol, 1,6-hexanediol, 1,2-cyclohexanediol, 1,4-cyclohexanediol, diethylene glycol, 4-(hydroxymethyl)cyclohexylmethyl A polyester stretched film comprising at least one selected from the group consisting of 4-(hydroxymethyl)cyclohexanecarboxylate, 4-(4-(hydroxymethyl)cyclohexylmethoxymethyl)cyclohexylmethanol, recycled cyclohexanedimethanol, recycled ethylene glycol, recycled bis-2-hydroxyethyl terephthalate, and recycled diethylene glycol.

10. In paragraph 1 or paragraph 7, A polyester stretched film, wherein the dicarboxylic acid component comprises at least one selected from the group consisting of isophthalic acid, terephthalic acid, dimethyl isophthalate, phthalic acid, dimethyl phthalate, phthalic anhydride, 2,6-naphthalene dicarboxylic acid, dimethyl 2,6-naphthalene dicarboxylate, diphenyl dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, 1,3-cyclohexane dicarboxylic acid, dimethyl 1,4-cyclohexane dicarboxylate, dimethyl 1,3-cyclohexane dicarboxylate, sebacic acid, succinic acid, isodecylsuccinic acid, maleic acid, maleic anhydride, fumaric acid, adipic acid, glutaric acid, azelaic acid, recycled isophthalic acid, recycled terephthalic acid, recycled dimethyl isophthalate, and recycled dimethyl phthalate.

11. In paragraph 1 or paragraph 7, A polyester stretch film, wherein the intrinsic viscosity (IV) of the polyester resin is 0.5 to 1.2 dl / g.

12. A step of manufacturing a polyester resin by polymerizing a diol component and a dicarboxylic acid component; A step of manufacturing a polyester stretch sheet from the above polyester resin; and Including a step of opening and fixing the above-mentioned extension sheet, After the first and second heat treatments, when analyzed by differential scanning calorimetry (DSC), the first melting temperature (T m1 ) and the second melting temperature (T m2 ) represents, The above first melting temperature (T m1 ) for the second melting temperature (T) in the first heat of fusion (H1) m2 ) A method for manufacturing a polyester stretched film, wherein the ratio of the second heat of fusion (H2) (H2 / H1) is 0.1 or more.

13. In paragraph 12, A method for manufacturing a polyester stretched film, wherein the above primary heat treatment is performed at 60 to 105°C for less than 1 minute.

14. In paragraph 12, A method for manufacturing a polyester stretched film, wherein the above secondary heat treatment is performed at 140 to 220°C for less than 4 hours.

15. In paragraph 12, A method for manufacturing a polyester stretched film, wherein the above secondary heat treatment is performed after the above primary heat-treated polyester stretched film is pre-heat-treated at 140 to 220°C for 1 to 30 minutes.

Citation Information

Patent Citations

  • A heat shrinkable stacked film and a heat shrinkable label using the same as substrate

    KR1020090062882A

  • Recycled polyester staple fiber using waste polyester and method thereof

    KR1020110109533A

  • Low shrinkage protective film

    KR1020120082153A

  • Lithium free battery and preparing method of the same

    KR1020210136830A

  • Power down detection circuit and semiconductor storage apparatus

    KR102469891B1