Composition, polymer-based portion, foldable apparatus containing the same, and methods of making
A composition of low and high refractive index acrylates with a hydroxyl-containing acrylate and urethane-acrylate oligomer addresses the poor impact and puncture resistance issues in foldable displays by enhancing the polymer-based portion's glass-transition temperature and flexibility, achieving improved performance and environmental sustainability.
Patent Information
- Application Number
- PCT/US2024/027936
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-06
- Publication Date
- 2024-12-05
AI Technical Summary
Conventional foldable displays and protective covers face challenges with poor impact and puncture resistance due to small minimum bend radii, and existing polymer-based solutions impair flexibility and bending performance when subjected to high bending strains.
A composition comprising a low refractive index acrylate, a high refractive index acrylate, and a hydroxyl-containing acrylate, along with a urethane-acrylate oligomer, is used to create a polymer-based portion with a glass-transition temperature below operating ranges, enabling consistent properties and improved bending performance and impact resistance, while being solvent-free to enhance curing rates and reduce environmental impact.
The resulting polymer-based portion exhibits improved impact resistance, puncture resistance, and flexibility, allowing for small minimum bend radii while maintaining optical clarity and mechanical integrity, thus addressing the limitations of existing foldable display technologies.
Smart Images

Figure US2024027936_05122024_PF_FP_ABST
Abstract
Description
ATTORNEY DOCKET NO. SP23-121 COMPOSITION, POLYMER-BASED PORTION, FOLDABLE APPARATUS CONTAINING THE SAME, AND METHODS OF MAKING CROSS-REFERENCETORELATEDAPPLICATION
[0001] This application claims the benefit of priority under 35 U.S.C. § 119 of U.S. Provisional Application Serial No.63 / 469119 filed on May 26, 2023, the content of which is relied upon and incorporated herein by reference in its entirety. FIELD
[0002] The present disclosure relates generally to compositions, polymer- based portions, foldable apparatus containing polymer-based portions, and methods of making the same and, more particularly, to compositions comprising a hydroxyl- containing acrylate, polymer-based portions comprising an acrylate-based polymer, foldable apparatus containing the same, and methods of making the same from a hydroxyl-containing acrylate. BACKGROUND
[0003] Glass-based substrates are commonly used, for example, in display devices, for example, liquid crystal displays (LCDs), electrophoretic displays (EPD), organic light-emitting diode displays (OLEDs), plasma display panels (PDPs), or the like.
[0004] There is a desire to develop foldable versions of displays as well as foldable protective covers to mount on foldable displays. Foldable displays and covers should have good impact and puncture resistance. At the same time, foldable displays and covers should have small minimum bend radii (e.g., about 10 millimeters (mm) or less).
[0005] However, plastic displays and covers with small minimum bend radii tend to have poor impact and / or puncture resistance. Furthermore, conventional wisdom suggests that ultra-thin glass-based sheets (e.g., about 75 micrometers (µm or microns) or less thick) with small minimum bend radii tend to have poor impactand / or puncture resistance. Furthermore, thicker glass-based sheets (e.g., greater than 125 micrometers) with good impact and / or puncture resistance tend to have relatively large minimum bend radii (e.g., about 30 millimeters or more).
[0006] Moreover, adhesives and / or polymer-based portions can impair the flexibility and bending performance of the foldable display and / or foldable protective cover if the bending strain exceeds the ultimate elongation of the polymer-based portion.
[0007] There is a desire for foldable apparatus, for example, as foldable displays or foldable protective covers to mount on foldable displays. Foldable apparatus should have good impact and puncture resistance. At the same time, foldable displays and foldable covers should have small minimum bend radii (e.g., about 10 millimeters (mm) or less). Additionally, there is a need to develop foldable substrates (e.g., glass-based substrates, ceramic-based substrates) and polymer-based portions for foldable apparatus that have high transparency, low haze, low minimum bend radii, and good impact and puncture resistance. Consequently, there is a need to develop foldable apparatus and / or polymer-based portions that have low minimum bend radii and good impact and puncture resistance. SUMMARY
[0008] There are set forth herein compositions, polymer-based portions, foldable apparatus comprising the same, and methods of making polymer-based portions and foldable apparatus comprising the same. Polymer-based portions can comprise a high refractive index acrylate, a low refractive index acrylate, a hydroxyl- containing acrylate, and an oligomer. Providing a low refractive index acrylate and a high refractive index acrylate can enable a predetermined refractive index of the resulting polymer-based portion to be obtained. Providing a refractive index for the polymer-based portion from about 1.48 to about 1.55 or from 1.49 to 1.52 can reduce an absolute difference of refractive index (e.g., about 0.05 or less, about 0.01 or less) between the polymer-based portion and components that can be adjacent to the polymer-based portion in an application, which can reduce optical distortions.
[0009] Providing a polymer-based portion with a glass-transition temperature (e.g., about -20°C or less) outside of an operating range (e.g., from about 0°C to about 40°C, from about -10°C to about 50°C) can enable consistent properties across the operating range. Providing a glass-transition temperature (e.g., about -20°C or less)below the operating range e.g., from about 0°C to about 40°C, from about -10°C to about 50°C) can enable the polymer-based portion to operate in the rubbery plateau, where low storage moduli (E’) and low elastic modulus (E”) can be observed. Providing a low (e.g., about 1 MPa or less, or from about 0.1 MPa to about 1 MPa) storage modulus (E’) at 25°C can enable the strain between layers adjacent to the polymer-based portion to be decoupled, which can improve bending performance (e.g., parallel plate distance and / or cycles withstood to a parallel plate distance) and / or improve impact resistance. Providing a low (e.g., about 0.15 MPa or less, or from about 0.0.05 MPa to about 0.15 MPa) storage modulus (E”) at 25°C can increase an amount of recoverable strain, for example, by decreasing an amount of viscous dissipation (e.g., during bending and / or impact). Further, providing a ratio of the storage modulus (E’) at 25°C to the loss modulus (E”) at 25°C of about 2.5 or more (i.e., E” / E’ of about 0.4 or less) can increase an amount of recoverable strain, for example, by decreasing an amount of viscous dissipation (e.g., during bending and / or impact).
[0010] Providing a precursor viscosity in a range from about 0.1 Pa-s to about 10 Pa-s can enable the precursor solution to be coated on a target substrate (e.g., foldable substrate) using a variety of techniques. In aspects, a predetermined precursor viscosity can be obtained by partially curing the composition to obtain the precursor solution that can be coated before being further cured to produce the polymer-based portion. In aspects, the composition can comprise a linear polymer that enables the composition to achieve a predetermined viscosity.
[0011] Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can increase the curing rate of the composition, which can decrease processing time. Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can reduce (e.g., decrease) the use of additives, for example, rheology modifiers, and increase composition homogeneity, which can improve the quality of the resulting polymer-based portion (e.g., increased transmittance, decreased haze, increased mechanical properties). Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can reduce a volume change as a result of curing (e.g., shrinkage). In aspects, the composition and / or the polymer- based portion can be substantially free of fluorine-based compounds and / or free of fluorine-based compounds, which can reduce an environmental impact of the polymer-based portion and / or reduce a cost to produce the polymer-based portion.
[0012] The foldable substrate can comprise glass-based and / or ceramic-based portions, which can provide good dimensional stability, reduced incidence of mechanical instabilities, good impact resistance, and / or good puncture resistance. The foldable substrate can comprise glass-based and / or ceramic-based portions comprising one or more compressive stress regions, which can further provide increased impact resistance and / or increased puncture resistance. By providing a foldable substrate comprising a glass-based and / or ceramic-based substrate, the substrate can also provide increased impact resistance and / or puncture resistance while simultaneously facilitating good folding performance. In aspects, the substrate thickness can be sufficiently large (e.g., from about 70 micrometers (microns or µm) to about 2 millimeters) to further enhance impact resistance and puncture resistance. Providing foldable substrates comprising a central portion comprising a central thickness that is less than a substrate thickness (e.g., first thickness of the first portion and / or second thickness of the second portion) (e.g., by about 10 µm or more) can enable a small parallel plate distance (e.g., about 10 millimeters or less) based on the reduced thickness in the central portion, which can enable the foldability and / or rollability of the foldable substrate and / or foldable apparatus.
[0013] In aspects, the foldable apparatus and / or foldable substrates can comprise one or more recesses, for example, a first central surface area recessed from a first major surface by a first distance and / or a second central surface area recessed from a second major surface by a second distance. Providing a first recess opposite a second recess can provide a central thickness that is less than a substrate thickness. Further, providing a first recess opposite a second recess can reduce a maximum bend-induced strain of the foldable apparatus, for example, between a central portion and a first portion and / or second portion since the central portion comprising the central thickness can be closer to a neutral axis of the foldable apparatus and / or foldable substrates than if only a single recess was provided. Additionally, providing the first distance substantially equal to the second distance can reduce the incidence of mechanical instabilities in the central portion, for example, because the foldable substrate is symmetric about a plane comprising a midpoint in the substrate thickness and the central thickness. Moreover, providing a first recess opposite a second recess can reduce a bend-induced strain of a material positioned in the first recess and / or second recess compared to a single recess with a surface recessed by the sum of the first distance and the second distance. Providing a reduced bend-induced strain of amaterial positioned in the first recess and / or the second recess can enable the use of a wider range of materials because of the reduced strain requirements for the material. For example, stiffer and / or more rigid materials can be positioned in the first recess, which can improve impact resistance, puncture resistance, abrasion resistance, and / or scratch resistance of the foldable apparatus. Additionally, controlling properties of a first material positioned in a first recess and a second material positioned in a second recess can control the position of a neutral axis of the foldable apparatus and / or foldable substrates, which can reduce (e.g., mitigate, eliminate) the incidence of mechanical instabilities, apparatus fatigue, and / or apparatus failure.
[0014] Some example aspects of the disclosure are described below with the understanding that any of the features of the various aspects may be used alone or in combination with one another.
[0015] Aspect 1. A composition comprising, as wt% of the composition: from about 65 wt% to about 75 wt% of a low refractive index acrylate comprising a refractive index less than 1.5 and at least one of an alkyl acrylate or an ether acrylate; from about 10 wt% to about 25 wt% of a high refractive index acrylate comprising a refractive index greater than 1.5; from about 10 wt% to about 25 wt% of a hydroxyl-containing acrylate; and from greater than 0 wt% to about 1 wt% of a urethane-acrylate oligomer.
[0016] Aspect 2. The composition of aspect 1, wherein the composition comprises from about 17 wt% to about 20 wt% of the high refractive index acrylate.
[0017] Aspect 3. The composition of any one of aspects 1-2, wherein the high refractive index acrylate is an aromatic acrylate.
[0018] Aspect 4. The composition of any one of aspects 1-3, wherein the high refractive index acrylate comprises biphenyl methyl acrylate.
[0019] Aspect 5. The composition of any one of aspects 1-4, wherein the low refractive index acrylate comprises two or more compounds.
[0020] Aspect 6. The composition of any one of aspects 1-5, wherein the low refractive index acrylate comprises at least 2-(2-ethoxyethoxy)ethyl acrylate.
[0021] Aspect 7. The composition of any one of aspects 1-6, wherein the low refractive index acrylate comprises at least 2-ethylhexyl acrylate.
[0022] Aspect 8. The composition of any one of aspects 1-7, wherein the composition comprises from about 68 wt% to about 70 wt% of the low refractive index acrylate.
[0023] Aspect 9. The composition of any one of aspects 1-8, wherein the composition comprise from about from about 17 wt% to about 20 wt% of the hydroxyl-containing acrylate.
[0024] Aspect 10. The composition of any one of aspects 1-9, wherein the composition comprises from about 0.4 wt% to about 0.8 wt% of the urethane-acrylate oligomer.
[0025] Aspect 11. The composition of any one of aspects 1-10, wherein the composition comprises a refractive index from about 1.43 to about 1.47.
[0026] Aspect 12. The composition of any one of aspects 1-11, further comprising, by superaddition: from about 0.1 wt% to about 0.5 wt% of a photoinitiator; and from 0 wt% to about 0.25 wt% of a tackifier.
[0027] Aspect 13. A composition comprising, as wt% of the composition: from about 50 wt% to about 85 wt% of a low refractive index alkyl acrylate comprising a refractive index less than 1.5; from greater than 0 wt% to about 25 wt% of a high refractive index acrylate comprising a refractive index greater than 1.5; from about 5 wt% to about 20 wt% of a hydroxyl-containing acrylate; from about 0.5 wt% to about 30 wt% of a linear polymer; and from greater than 0 wt% to about 1 wt% of a urethane-acrylate oligomer.
[0028] Aspect 14. The composition of aspect 13, wherein the linear polymer comprises a copolymer of ethylene and vinyl acrylate.
[0029] Aspect 15. The composition of any one of aspects 13-14, wherein the linear polymer comprises one or more of poly(ethylene-co-vinyl acrylate), poly(vinyl acrylate-co-vinyl alcohol-co-ethylene) poly(vinyl methyl ketone), poly(vinyl formal), or combinations thereof.
[0030] Aspect 16. The composition of any one of aspects 13-15, wherein the composition comprises from about 1 wt% to 20 wt% of the linear polymer.
[0031] Aspect 17. The composition of any one of aspects 13-16, wherein the composition further comprises a viscosity from about 0.1 Pascal-second to about 10 Pascal-seconds at 25°C.
[0032] Aspect 18. The composition of any one of aspects 13-17, wherein the composition comprises from about 17 wt% to about 20 wt% of the high refractive index acrylate.
[0033] Aspect 19. The composition of any one of aspects 13-18, wherein the high refractive index acrylate is an aromatic acrylate.
[0034] Aspect 20. The composition of any one of aspects 13-19, wherein the high refractive index acrylate comprises biphenyl methyl acrylate.
[0035] Aspect 21. The composition of any one of aspects 13-20, wherein the low refractive index alkyl acrylate comprises two or more compounds.
[0036] Aspect 22. The composition of any one of aspects 13-21, wherein the low refractive index acrylate comprises at least 2-ethylhexyl acrylate.
[0037] Aspect 23. The composition of any one of aspects 13-22, wherein the composition comprises from 65 wt% to 75 wt% of the low refractive index alkyl acrylate.
[0038] Aspect 24. The composition of any one of aspects 13-23, wherein the composition comprises from about 0.4 wt% to about 0.8 wt% of the urethane-acrylate oligomer.
[0039] Aspect 25. The composition of any one of aspects 13-23, wherein the linear polymer comprises a hydroxyl functional group at an end of the linear polymer.
[0040] Aspect 26. The composition of aspect 25, further comprising from greater than 0 wt% to less than 0.5 wt% of a cross-linker comprising functional groups selected from acrylate, isocyanate, and compositions thereof.
[0041] Aspect 27. The composition of aspect 26, wherein the composition comprises from 0.02 wt% to 0.1 wt% of the cross-linker.
[0042] Aspect 28. The composition of any one of aspects 13-27, further comprising, by superaddition: from about 0.1 wt% to about 0.5 wt% of a photoinitiator; and from 0 wt% to about 0.25 wt% of a tackifier.
[0043] Aspect 29. A polymer-based portion comprising a product of curing the composition of any one of aspects 1-12.
[0044] Aspect 30. A polymer-based portion comprising a product of curing the composition of any one of aspects 13-28.
[0045] Aspect 31. The polymer-based portion of any one of aspects 29-30, further comprising:a glass-transition temperature (Tg) of about -20°C or less; a storage modulus (E’) at 25°C from about 0.1 MegaPascals to about 1 MegaPascals; and a refractive index from about 1.47 to about 1.51.
[0046] Aspect 32. A polymer-based portion comprising: an acrylate-based polymer; a glass-transition temperature (Tg) of about -20°C or less; a storage modulus (E’) at 25°C from about 0.1 MegaPascals to about 1 MegaPascals; and a refractive index from about 1.47 to about 1.51.
[0047] Aspect 33. The polymer-based portion of any one of aspects 31-32, wherein the storage modulus (E’) is from about 0.1 MegaPascals to about 0.5 MegaPascals.
[0048] Aspect 34. The polymer-based portion of any one of aspects 21-33, further comprising a loss modulus (E”) at 25°C of about 0.2 MegaPascals or less.
[0049] Aspect 35. The polymer-based portion of aspect 34, wherein the loss modulus (E”) is from about 0.05 MegaPascals to about 0.16 MegaPascals.
[0050] Aspect 36. The polymer-based portion of any one of aspects 31-35, wherein the glass-transition temperature is from -50°C to -20°C.
[0051] Aspect 37. The polymer-based portion of any one of aspects 29-36, further comprising a strain recovery of about 50% or more of an applied strain of 300%.
[0052] Aspect 38. The polymer-based portion of aspect 37, wherein the strain recovery is from about 60% to about 90% of the applied strain.
[0053] Aspect 39. The polymer-based portion of any one of aspects 29-38, further comprising a peel adhesion of about 0.6 N / cm or more after a 15 minute dwell time.
[0054] Aspect 40. The polymer-based portion of aspect 39, wherein the peel adhesion is from about 0.65 N / cm to about 10 N / cm after the 15 minute dwell time.
[0055] Aspect 41. The polymer-based portion of any one of aspects 39-40, wherein the peel adhesion after the 15 minute dwell time is less than another peel adhesion after a 24 hour dwell time.
[0056] Aspect 42. The polymer-based portion of any one of aspects 29-38, further comprising a peel adhesion is about 1 N / cm or more after a 24 hour dwell time.
[0057] Aspect 43. The polymer-based portion of aspect 42, wherein the peel adhesion is from about 3 N / cm to about 15 N / cm after the 24 hour dwell time.
[0058] Aspect 44. The polymer-based portion of any one of aspects 29-43, wherein the polymer-based portion can withstand 3,000 folding cycles to a parallel plate distance of 3 millimeters.
[0059] Aspect 45. The polymer-based portion of any one of aspects 29-44, wherein the polymer-based portion can withstand being held at a parallel plate distance of 3 millimeters at -20°C for 10 days.
[0060] Aspect 46. The polymer-based portion of any one of aspects 29-45, wherein the polymer-based portion comprises a gel fraction of about 70% or more.
[0061] Aspect 47. The polymer-based portion of aspect 46, wherein the gel fraction is from about 75% to about 90%.
[0062] Aspect 48. A foldable apparatus comprising: the polymer-based portion of any one of aspects 29-47; a foldable substrate comprising a first major surface; and a device substrate, wherein the polymer-based portion is positioned between and contacts the first major surface of the foldable substrate and the device substrate, and a minimum thickness of the polymer-based portion is from about 5 micrometers to about 30 micrometers.
[0063] Aspect 49. The foldable apparatus of aspect 48, wherein the foldable substrate comprises a glass-based material or a ceramic-based material.
[0064] Aspect 50. The foldable apparatus of any one of aspects 48-49, wherein the device substrate comprises an elastic modulus of about 1 GigaPascal or more.
[0065] Aspect 51. The foldable apparatus of any one of aspects 48-50, wherein the foldable substrate comprises a central portion comprising a first central surface area recessed from the first major surface by 5 micrometers or more, and the polymer-based portion further contacting the first central surface area.
[0066] Aspect 52. A method of forming a foldable apparatus comprising:providing a precursor solution comprising a viscosity from about 0.1 Pascal- second to about 10 Pascal-seconds at 25°C; disposing the precursor solution on a foldable substrate; and curing the precursor solution to form a polymer-based portion on the foldable substrate, wherein the polymer-based portion comprises: an acrylate-based polymer; a glass-transition temperature (Tg) of about -20°C or less; a storage modulus (E’) at 25°C from about 0.1 MegaPascals to about 1 MegaPascals; and a refractive index from about 1.47 to about 1.51.
[0067] Aspect 53. The method of aspect 50, wherein the precursor solution is formed by partially curing a mixture comprising, as a wt% of the mixture: from about 65 wt% to about 75 wt% of a low refractive index acrylate comprising a refractive index less than 1.5; from about 10 wt% to about 25 wt% of a high refractive index acrylate comprising a refractive index greater than 1.5; from about 10 wt% to about 25 wt% of a hydroxyl-containing acrylate; and from greater than 0 wt% to about 1 wt% of a urethane-acrylate oligomer.
[0068] Aspect 54. The method of aspect 53, wherein the mixture comprises from about 17 wt% to about 20 wt% of the high refractive index acrylate.
[0069] Aspect 55. The method of any one of aspects 53-54, wherein the low refractive index acrylate comprises at least 2-(2-ethoxyethoxy)ethyl acrylate.
[0070] Aspect 56. The method of any one of aspects 53-55, wherein the mixture comprises from about 68 wt% to about 70 wt% of the low refractive index acrylate.
[0071] Aspect 57. The method of any one of aspects 53-56, wherein the mixture comprises from about from about 17 wt% to about 20 wt% of the hydroxyl- containing acrylate.
[0072] Aspect 58. The method of any one of aspects 53-57, wherein the mixture comprises a photoinitiator and the precursor solution comprises more of the photoinitiator (in terms of wt% of the mixture) than the mixture.
[0073] Aspect 59. The method of aspect 51, wherein the precursor solution comprises:from about 50 wt% to about 85 wt% of a low refractive index acrylate comprising a refractive index less than 1.5; from greater than 0 wt% to about 25 wt% of a high refractive index acrylate comprising a refractive index greater than 1.5; from about 5 wt% to about 20 wt% of a hydroxyl-containing acrylate; from about 0.5 wt% to about 30 wt% of a linear polymer; and from greater than 0 wt% to about 1 wt% of a urethane-acrylate oligomer.
[0074] Aspect 60. The method of aspect 59, wherein the linear polymer comprises a copolymer of ethylene and vinyl acrylate.
[0075] Aspect 61. The method of any one of aspects 59-60, wherein the linear polymer comprises one or more of poly(ethylene-co-vinyl acrylate), poly(vinyl acrylate-co-vinyl alcohol-co-ethylene) poly(vinyl methyl ketone), poly(vinyl formal), or combinations thereof.
[0076] Aspect 62. The method of any one of aspects 59-61, wherein the composition comprises from about 17 wt% to about 20 wt% of the high refractive index acrylate.
[0077] Aspect 63. The method of any one of aspects 59-62, wherein the composition comprises from 65 wt% to 75 wt% of the refractive index alkyl acrylate.
[0078] Aspect 64. The method of any one of aspects 59-63, wherein the linear polymer comprises a hydroxyl functional group at an end of the linear polymer.
[0079] Aspect 65. The method of aspect 64, further comprising from greater than 0 wt% to less than 0.5 wt% of a cross-linker comprising functional groups selected from acrylate, isocyanate, and compositions thereof.
[0080] Aspect 66. The method of any one of aspects 59-65, wherein the low refractive index acrylate is an alkyl acrylate.
[0081] Aspect 67. The method of any one of aspects 59-65 inclusive, wherein the precursor solution further comprises, by superaddition: from about 0.1 wt% to about 0.5 wt% of a photoinitiator; and from 0 wt% to about 0.25 wt% of a tackifier.
[0082] Aspect 68. The method of aspect 53, wherein the precursor solution comprises from about 0.5 wt% to about 30 wt% of a linear polymer.
[0083] Aspect 69. The method of any one of aspects 59-67, wherein the composition comprises from about 1 wt% to 20 wt% of the linear polymer.
[0084] Aspect 70. The method of any one of aspects 53-67, wherein the high refractive index acrylate is an aromatic acrylate.
[0085] Aspect 71. The method of any one of aspects 53-66 or 70 inclusive, wherein the high refractive index acrylate comprises biphenyl methyl acrylate.
[0086] Aspect 72. The method of any one of aspects 53-66 or 70-71 inclusive, wherein the low refractive index acrylate comprises two or more compounds.
[0087] Aspect 73. The method of aspect 72, wherein the curing comprises impinging the precursor solution with light comprising an optical wavelength.
[0088] Aspect 74. The method of aspect 73, wherein the optical wavelength is in a range from about 100 nm to about 400 nm.
[0089] Aspect 75. The method of any one of aspects 52-74, wherein the low refractive index acrylate comprises at least 2-(2-ethoxyethoxy)ethyl acrylate.
[0090] Aspect 76. The method of any one of aspects 52-74, wherein the low refractive index acrylate comprises at least 2-ethylhexyl acrylate.
[0091] Aspect 77. The method of any one of aspects 52-76, wherein the storage modulus (E’) is from about 0.1 MegaPascals to about 0.5 MegaPascals.
[0092] Aspect 78. The method of any one of aspects 52-77, wherein the polymer-based portion further comprises a loss modulus (E”) at 25°C of about 0.2 MegaPascals or less.
[0093] Aspect 79. The method of aspect 78, wherein the loss modulus (E”) is from about 0.05 MegaPascals to about 0.16 MegaPascals.
[0094] Aspect 80. The method of any one of aspects 52-79, wherein the glass- transition temperature is from -50°C to -20°C.
[0095] Aspect 81. The method of any one of aspects 52-80, wherein the polymer-based portion further comprises a strain recovery of about 50% or more of an applied strain of 300%.
[0096] Aspect 82. The method of aspect 81, wherein the strain recovery is from about 60% to about 90% of the applied strain.
[0097] Aspect 83. The method of any one of aspects 52-82, wherein the polymer-based portion further comprises a peel adhesion of about 0.6 N / cm or more after a 15 minute dwell time.
[0098] Aspect 84. The method of aspect 83, wherein the peel adhesion is from about 0.65 N / cm to about 10 N / cm after the 15 minute dwell time.
[0099] Aspect 85. The method of any one of aspects 52-84, wherein the peel adhesion after the 15 minute dwell time is less than another peel adhesion after a 24 hour dwell time.
[0100] Aspect 86. The method of any one of aspects 52-82, wherein the polymer-based portion further comprises a peel adhesion of about 1 N / cm or more after a 24 hour dwell time.
[0101] Aspect 87. The method of aspect 86, wherein the peel adhesion is from about 3 N / cm to about 15 N / cm after the 24 hour dwell time.
[0102] Aspect 88. The method of any one of aspects 52-87, wherein the polymer-based portion can withstand 3,000 folding cycles to a parallel plate distance of 3 millimeters.
[0103] Aspect 89. The method of any one of aspects 52-88, wherein the polymer-based portion can withstand being held at a parallel plate distance of 3 millimeters at -20°C for 10 days.
[0104] Aspect 90. The method of any one of aspects 52-88, wherein the polymer-based portion comprises a gel fraction of about 70% or more.
[0105] Aspect 91. The method of aspect 90, wherein the gel fraction is from about 75% to about 90%. BRIEF DESCRIPTION OF THE DRAWINGS
[0106] The above and other features and advantages of aspects of the present disclosure are better understood when the following detailed description is read with reference to the accompanying drawings, in which:
[0107] FIG.1 is a schematic view of an example foldable apparatus in a flat configuration according to aspects, wherein a schematic view of the folded configuration may appear as shown in FIG.5;
[0108] FIGS. 2-4 are cross-sectional views of the foldable apparatus along line 2-2 of FIG.1 including a foldable substrate according to aspects;
[0109] FIG.5 is a schematic view of example foldable apparatus of aspects of the disclosure in a folded configuration wherein a schematic view of the flat configuration may appear as shown in FIG.1;
[0110] FIG. 6 is a cross-sectional view of a testing apparatus to determine the minimum parallel plate distance of an example foldable substrate along line 7-7 of FIG.5;
[0111] FIG. 7 is a cross-sectional view of another testing apparatus to determine the minimum parallel plate distance of an example modified foldable apparatus along line 7-7 of FIG.5;
[0112] FIG. 8 is a cross-sectional view of a testing apparatus to determine the minimum parallel plate distance of an example foldable substrate along line 7-7 of FIG.5;
[0113] FIG. 9 is a cross-sectional view of another testing apparatus to determine the minimum parallel plate distance of an example modified foldable apparatus along line 7-7 of FIG.5;
[0114] FIG. 10 is a schematic plan view of an example consumer electronic device according to aspects;
[0115] FIG. 11 is a schematic perspective view of the example consumer electronic device of FIG.10;
[0116] FIG.12 is a flow chart illustrating example methods making foldable apparatus in accordance with aspects of the disclosure; and
[0117] FIGS. 13-18 schematically illustrate steps in methods of making a foldable apparatus.
[0118] Throughout the disclosure, the drawings are used to emphasize certain aspects. As such, it should not be assumed that the relative size of different regions, portions, and substrates shown in the drawings are proportional to its actual relative size, unless explicitly indicated otherwise. DETAILEDDESCRIPTION
[0119] Aspects will now be described more fully hereinafter with reference to the accompanying drawings in which example aspects are shown. Whenever possible, the same reference numerals are used throughout the drawings to refer to the same or like parts.
[0120] The polymer-based portions of aspects of the disclosure can be used, for example, in a foldable apparatus 101, 301, 401, 701, and 901 illustrated in FIGS. 2-4, 7, and 9. However, it is to be understood that the polymer-based portions are not limited to such applications and can be used in other applications. Unless otherwise noted, a discussion of features of aspects of one polymer-based portion and / or foldable apparatus can apply equally to corresponding features of any aspect of the disclosure. For example, identical part numbers throughout the disclosure can indicate that, in some aspects, the identified features are identical to one another andthat the discussion of the identified feature of one aspect, unless otherwise noted, can apply equally to the identified feature of any other aspect of the disclosure.
[0121] Aspects of the disclosure can comprise a polymer-based portion (e.g., first polymer-based portion 289 and / or second polymer-based portion 299). As shown in FIGS. 2-3, a first polymer-based portion 289 can comprise a first contact surface 283 and a second contact surface 285 opposite the first contact surface 283. In aspects, as shown, the first contact surface 283 can comprise a planar surface. As shown in FIGS. 2-4, a second polymer-based portion 299 can comprise a third contact surface 293 and a fourth contact surface 295 opposite the third contact surface 293. In aspects, as shown, the fourth contact surface 295 can comprise a planar surface.
[0122] As used herein, the refractive index is measured in accordance with ASTM E1967-19 at a wavelength of 589 nanometers (nm). In aspects, the polymer- based portion 289 and / or 299 can be optically clear and / or comprise a first refractive index. In aspects, a refractive index of the polymer-based portion 289 and / or 299 may be about 1.47 or more, about 1.48 or more, about 1.49 or more, about 1.495 or more, about 1.50 or more, about 1.55 or less, about 1.54 or less, about 1.53 or less, about 1.52 or less, about 1.51 or less, or about 1.505 or less. In aspects, the refractive index of the polymer-based portion 289 and / or 299 can be in a range from about 1.47 to about 1.55, from about 1.47 to about 1.54, from about 1.47 to about 1.53, from about 1.47 to about 1.52, from about 1.47 to about 1.51, from about 1.48 to about 1.51, from about 1.49 to about 1.51, from about 1.495 to about 1.505, from about 1.50 to about 1.505, or any range or subrange therebetween. Providing a refractive index for the polymer-based portion within one or more of the above-mentioned ranges can reduce an absolute difference of refractive index between the polymer-based portion and components (e.g., substrate, adhesive, hard-coating) that can be adjacent to the polymer-based portion in an application, which can reduce optical distortions.
[0123] As used herein, “optically transparent” or “optically clear” means an average transmittance of 70% or more in the wavelength range of 400 nm to 700 nm through a 1.0 mm thick piece of material, wherein the thickness is measured along the path length of light travelling through the piece of material. As used herein, an average transmittance of a material is measured by averaging over optical wavelengths in a range from 400 nm to 700 nm through a 1.0 mm thick piece of the material, which comprises measuring the transmittance of whole number wavelengthsfrom about 400 nm to about 700 nm and averaging the measurements. Unless specified otherwise, “transmittance” of a material refers to the average transmittance of the material. In aspects, an “optically transparent material” or an “optically clear material” may have an average transmittance of 75% or more, 80% or more, 85% or more, 89% or more, or 90% or more, 92% or more, 94% or more, 96% or more in the wavelength range of 400 nm to 700 nm through a 1.0 mm thick piece of the material. In aspects, the polymer-based portion 289 and / or 299 can be optically transparent. In further aspects, the polymer-based portion 289 and / or 299 can comprise an average transmittance measured over optical wavelengths in a range from 400 nm to 700 nm of about 85% or more, 89% or more, about 90% or more, about 91% or more, about 92% or more, about 93% or more, 94% or more, 95% or more, 100% or less, about 98% or less, about 96% or less, or about 94% or less. In further aspects, the polymer- based portion can comprise an average transmittance measured over optical wavelengths in a range from 400 nm to 700 nm in a range from about 89% to 100%, from about 90% to about 98%, from about 91% to about 98%, from about 92% to about 98%, from about 92% to about 96%, from about 92% to about 94%, from about 93% to about 94%, or any range or subrange therebetween. As used herein, “minimum transmittance” refers to the lowest transmittance value for any optical wavelength within a specified range of optical wavelengths. In aspects, the polymer- based portion 289 and / or 299 can comprise a minimum transmittance for optical wavelengths from 400 nm to 750 nm can be about 85% or more, about 87% or more, about 88% or more, about 89% or more, about 90% or more, about 91% or more, or about 92% or more. As shown in the Examples below, polymer-based portions exhibit an average transmittance (measured over optical wavelengths in a range from 400 nm to 700 nm) of 85% or more, 90% or more, or 95% or more.
[0124] The polymer-based portion 289 and / or 299 can comprise a haze as a function of an angle of illumination relative to a direction normal to a surface of the polymer-based portion. As used herein, haze refers to transmission haze that is measured in accordance with ASTM E430. Haze can be measured using a haze meter supplied by BYK Gardner under the trademark HAZE-GUARD PLUS, using an aperture over the source port. The aperture has a diameter of 8 mm. A CIE D65 illuminant is used as the light source for illuminating the foldable apparatus. Unless indicated otherwise, haze is measured at about 10° relative to an angle of incidence normal to a surface of the polymer-based portion. In aspects, the haze at about 0°and / or 10° relative to an angle of incidence normal to the surface of the polymer- based portion measured through a 1.0 millimeter (mm) thick piece of the polymer- based portion can be about 1% or less, about 0.5% or less, about 0.2% or less, about 0.15% or less, about 0.1% or less, or about 0.01% or more, about 0.02% or more, about 0.05% or more, or about 0.08% or more. In aspects, the haze at about 0° and / or 10° relative to an angle of incidence normal to the surface of the polymer-based portion measured through a 1.0 mm thick piece of the polymer-based portion can be in a range from 0% to about 1%, from 0% to 0.5%, from about 0.01% to about 0.2%, from about 0.02% to about 0.15%, from about 0.05% to about 0.1%, or any range or subrange therebetween. In aspects, the haze at about 20° relative to an angle of incidence normal to the surface of the polymer-based portion can be within one or more of the ranges specified above for 0° and / or 10°. Providing a polymer-based portion comprising low haze can enable good visibility through the polymer-based portion.
[0125] The polymer-based portion 289 and / or 299 can comprise a glass- transition (Tg) temperature. As used herein, the glass-transition temperature, a storage modulus (E’) at a range of temperatures, a storage modulus (e.g., at a rubbery plateau), and a loss modulus (E”) (e.g., at a rubbery plateau) are measured using Dynamic Mechanical Analysis (DMA) with an instrument, for example, the DMA 850 from TA Instruments. The samples for the DMA analysis comprise a film secured by a tension clamp. As used herein, the storage modulus refers to the in-phase component of a response of the polymer-based material to the dynamic testing. Throughout the disclosure, the modulus of elasticity of a polymer-based material refers to the storage modulus of the polymer-based material because, without wishing to be bound by theory, the in-phase component of the response is attributed to the elastic portion of a viscoelastic material. As used herein, the loss modulus refers to the out-of-phase component of a response to the polymer-based material during the dynamic testing. Without wishing to be bound by theory, the loss modulus can correspond to the viscous component of a viscoelastic material. As used herein, the glass-transition temperature corresponds to a maximum value of a tan delta, which is a ratio of the loss modulus to the storage modulus.
[0126] In aspects, the polymer-based portion can exhibit a single glass- transition temperature (as opposed to multiple glass-transition temperatures in a range from -120°C to 100°C or from -40°C to 0°C). In aspects, the glass-transitiontemperature (Tg) of the polymer-based portion can be about -20°C or less, about - 21°C or less, about -22°C or less, about -25°C or more, or about -30°C or less, about - 50°C or more, about -45°C or less, about -40°C or less, about -35°C or less, about - 32°C or less, or about -30°C or less. In aspects, the glass-transition temperature (Tg) of the polymer-based portion can be in a range from about -20°C to about -50°C, from about -21°C to about -45°C, from about -22°C to about -40°C, from about -25°C to about -35°C, from about -25°C to about -30°C, or any range or subrange therebetween. Providing a polymer-based portion with a glass-transition temperature outside of an operating range (e.g., from about 0°C to about 40°C, from about -10°C to about 50°C) can enable consistent properties across the operating range.
[0127] In aspects, the storage modulus (E’) of the polymer-based portion at 25°C can be about 0.1 MegaPascals (MPa) or more, about 0.2 MPa or more, about 0.25 MPa or more, about 0.3 MPa or more, about 0.35 MPa or more, about 1 MPa or less, about 0.8 MPa or less, about 0.6 MPa or less, about 0.5 MPa or less, about 0.45 MPa or less, about 0.4 MPa or less, or about 0.35 MPa or less. In aspects, the storage modulus (E’) of the polymer-based portion at 25°C can be in a range from about 0.1 MPa to about 1 MPa, from about 0.1 to about 1 MPa, from about 0.1 to about 0.8 MPa, from about 0.1 MPa to about 0.6 MPa, from about 0.1 MPa to about 0.5 MPa, from about 0.2 MPa to about 0.5 MPa, from about 0.25 MPa to about 0.45 MPa, from about 0.3 MPa to about 0.4 MPa, or any range or subrange therebetween. Providing a low (e.g., about 1 MPa or less) storage modulus (E’) at 25°C can enable the strain between layers adjacent to the polymer-based portion to be decoupled, which can improve bending performance (e.g., parallel plate distance and / or cycles withstood to a parallel plate distance) and / or improve impact resistance.
[0128] In aspects, the storage modulus (E’) of the polymer-based portion at -20°C can be about 1 MPa or more, about 1.5 MPa or more, about 2 MPa or more, about 2.5 MPa or more, about 3 MPa or more, about 4 MPa or more, about 5 MPa or more, about 10 MPa or less, about 9 MPa or less, about 8 MPa or less, or about 6 MPa or less. In aspects, the storage modulus (E’) of the polymer-based portion at -20°C can be in a range from about 1 MPa to about 10 MPa, from about 1.5 MPa to about 9 MPa, from about 2 MPa to about 8 MPa, from about 2.5 MPa to about 6 MPa, from about 3 MPa to about 6 MPa, or any range or subrange therebetween.
[0129] In aspects, the loss modulus (E”) of the polymer-based portion at 25°C can be about 0.05 MPa or more, about 0.08 MPa or more, about 0.1 MPa ormore, about 0.11 MPa or more, about 0.12 MPa or more, about 0.15 MPa or less, about 0.14 MPa or less, about 0.13 MPa or less, about 0.12 MPa or less, or about 0.1 MPa or less. In aspects, the loss modulus (E”) of the polymer-based portion at 25°C can be in a range from about 0.05 MPa to about 0.15 MPa, from about 0.08 MPa to about 0.14 MPa, from about 0.1 MPa to about 0.13 MPa, or any range or subrange therebetween. Providing a low (e.g., about 0.15 MPa or less) storage modulus (E”) at 25°C can increase an amount of recoverable strain, for example, by decreasing an amount of viscous dissipation (e.g., during bending and / or impact).
[0130] In aspects, the loss modulus (E”) of the polymer-based portion at - 20°C can be about 0.5 MPa or more, about 0.6 MPa or more, about 0.8 MPa or more, about 1 MPa or more, about 2 MPa or more, about 3 MPa or more, about 50 MPa or less, about 30 MPa or less, about 10 MPa or less, about 7 MPa or less, or about 5 MPa or less. In aspects, the loss modulus (E”) of the polymer-based portion at -20°C can be in a range from about 0.5 MPa to about 50 MPa, from about 0.6 MPa to about 30 MPa, from about 0.8 MPa to about 10 MPa, from about 1 MPa to about 7 MPa, from about 2 MPa to about 5 MPa, or any range or subrange therebetween.
[0131] In aspects, a ratio of the storage modulus (E’) at 25°C to the loss modulus (E”) at 25°C can be greater than 1 or more, about 1.8 or more, about 2 or more, about 2.1 or more, about 2.2 or more, about 2.5 or more, about 20 or less, about 10 or less, about 5 or less, about 4 or less, or about 3 or less. In aspects, a ratio of the storage modulus (E’) at 25°C to the loss modulus (E”) at 25°C can be in a range from greater than 1 to about 20, from about 1.8 to about 10, from about 2 to about 5, from about 2.1 to about 4, from about 2.2 to about 4, from about 2.5 to about 3, or any range or subrange therebetween. As presented in the Examples, below, the reverse ratio (E” / E’) at 25°C can be about 0.5 or less, about 0.45 or less, about 0.42 or less, about 0.41 or less, about 0.4 or less, about 0.33 or less, about 0.05 or more, about 0.1 or more, about 0.15 or more, about 0.2 or more, about 0.25 or more, or about 0.3 or more, for example, in a range from about 0.1 to about 0.5, from about 0.15 to about 0.45, from about 0.2 to about 0.42, from about 0.25 to about 0.41, from about 0.3 to about 0.4, or any range or subrange therebetween. Providing a ratio of the storage modulus (E’) at 25°C to the loss modulus (E”) at 25°C of about 2.5 or more (i.e., E” / E’ of about 0.4 or less) can increase an amount of recoverable strain, for example, by decreasing an amount of viscous dissipation (e.g., during bending and / or impact).
[0132] Throughout the disclosure, an elastic modulus (i.e., Young’s modulus) of the polymer-based portion 289 and / or 299 is measured using ASTM D4065-20. In aspects, an elastic modulus of the polymer-based portion can be within one or more of the ranges discussed above for the storage modulus (E’).
[0133] Throughout the disclosure, tension set of a sample is measured using ASTM D-412 as the strain at zero stress after the sample is stretched to a specified strain. In aspects, the polymer-based portion 289 and / or 299 can comprise a tension set after being extended to a strain of 10% at a strain rate of 10% strain per minute at 23°C. In further aspects, the tension set can be about 2% or less, about 1% or less, about 0.5% or less, or 0% or more. In further aspects, the tension set can be in a range from 0% to about 2%, from 0% to about 1%, from 0% to about 0.5%, or any range or subrange therebetween. In further aspects, the polymer-based portion can fully recover after being extended to a strain of 10% at a strain rate of 10% strain per minute at 23°C. In aspects, the polymer-based portion can fully recover after being extended to a strain of 10% at a strain rate of 10% strain per minute at 0°C. In aspects, the polymer-based portion can comprise a tension set after 200 cycles extending the polymer-based portion to a strain of 10% at a strain rate of 10% strain per minute at 23°C. In further aspects, the tension set can be about 2% or less, about 1% or less, about 0.5% or less, or 0% or more. In further aspects, the tension set can be in a range from 0% to about 2%, from 0% to about 1%, from 0% to about 0.5%, or any range or subrange therebetween.
[0134] Throughout the disclosure, strain recovery of a sample is measured by inducing a shear strain of 300% on the sample from an applied force, holding the 300% shear strain for 10 minutes, and then removing the applied force and allowing the sample to relax for 10 minutes. A recovered strain is measured after the sample is allowed to relax. The strain recovery is reported as a ratio of the recovered strain divided by the imposed strain as a percentage (i.e., 100% * εrecovered / εimposed, where εimposed = 300%). Consequently, a strain recovery of 100% means that the sample recovered to its original shape while 0% strain recovery means that the sample stayed in the configuration with the induced shear strain of 300% after the applied force was removed. Unless otherwise indicated, the dimensions of the sample used to measure strain recovery was a circular disk with a diameter of 8 mm and a thickness of 500 µm that was placed in a parallel plate rheometer (e.g., DHR-3 rheometer available from TA Instruments) with the plates imposing a normal force of 1 N on the sample beforeimparting the shear strain at 25°C. The values reported for the Examples (below) are the average of at least three samples. In aspects, the polymer-based portion can exhibit a strain recovery of about 50% or more, about 55% or more, about 60% or more, about 65% or more, about 70% or more, about 75% or more, about 80% or more, about 85% or more, about 99% or less, about 95% or less, about 90% or less, about 90% or less, about 88% or less, or about 85% or less. In aspects, the polymer- based portion can exhibit a strain recovery in a range from about 50% to about 99%, from about 55% to about 95%, from about 60% to about 90%, from about 65% to about 90%, from about 70% to about 90%, from about 75% to about 88%, from about 80% to about 85%, or any range or subrange therebetween.
[0135] As used herein, peel adhesion is measured for the polymer-based portion via a 180° peel adhesion test in accordance with ASTM D3330 Test Method D with a 76 micron (0.003 inch) thick PET pressed onto the polymer-based portion and Corning Gorilla Glass substrate with 2.04 kgf (4.5 lbf) at a constant speed of 305 mm / min (12 inch / min). Unless otherwise indicated, peel adhesion was measured using an Poweroll PR-1000 (IMASS). In aspects, after a 15-minute dwell time following pressing the PET and substrate into the polymer-based portion, the peel adhesion of the polymer-based portion can be about 0.6 Newtons per centimeter (N / cm) or more, about 0.65 N / cm or more, about 0.7 N / cm or more, about 0.8 N / cm or more, about 1 N / cm or more, about 15 N / cm or less, about 10 N / cm or less, about 8 N / cm or less, about 6 N / cm or less, about 4 N / cm or less, or about 2 N / cm or less. In aspects, after a 15-minute dwell time following pressing the PET and substrate into the polymer-based portion, the peel adhesion of the polymer-based portion can be in a range from about 0.6 N to about 15 N / cm, from about 0.65 N / cm to about 10 N / cm, from about 0.65 N / cm to about 8 N / cm, from about 0.7 N / cm to about 6 N / cm, from about 0.8 N / cm to about 4 N / cm, from about 1 N / cm to about 2 N / cm, or any range or subrange therebetween. In aspects, after a 24-hour dwell time following pressing the PET and substrate into the polymer-based portion, the peel adhesion of the polymer- based portion can be about 0.6 Newtons per centimeter (N / cm) or more, about 1 N / cm or more, about 2 N / cm or more, about 3 N / cm or more, about 4 N / cm or more, about 15 N / cm or less, about 12 N / cm or less, about 10 N / cm or less, about 8 N / cm or less, or about 6 N / cm or less. In aspects, after a 24-hour dwell time following pressing the PET and substrate into the polymer-based portion, the peel adhesion of the polymer- based portion can be in a range from about 1 N / cm to about 15 N / cm, from about 2N / cm to about 12 N / cm, from about 3 N / cm to about 10 N / cm, from about 4 N / cm to about 8 N / cm, or any range or subrange therebetween. In aspects, a peel adhesion after a 15-minute dwell time can be greater than a peel adhesion after a 24-hour dwell time.
[0136] As used herein, “gel fraction” refers to a ratio of a non-extractable weight to a total weight of the polymer-based portion as percentage (i.e., 100% x wnon-extractable / wtotal). The non-extractable weight refers to a weight of the polymer- based portion that remains after soaking in ethyl acetate for 24 hours. Without wishing to be bound by theory, a higher gel fraction corresponds to a higher degree of cross-linking, and thus, a higher extent of reaction for the curing in the polymer-based portion. In aspects, a gel fraction of the polymer-based portion can be about 70% or more, about 75% or more, about 80% or more, about 85% or more, about 95% or less, about 92% or less, about 90% or less, about 88% or less, or about 85% or less. In aspects, the gel fraction of the polymer-based portion can be in a range from about 70% to about 95%, from about 75% to about 92%, from about 80% to about 90%, from about 85% to about 88%, or any range or subrange therebetween.
[0137] As used herein, “foldable” includes complete folding, partial folding, bending, flexing, or multiple capabilities. As used herein, the terms “fail,” “failure” and the like refer to breakage, destruction, delamination, or crack propagation. Likewise, a foldable apparatus achieves a parallel plate distance of “X,” or has a parallel plate distance of “X,” or comprises a parallel plate distance of “X” if it resists failure when the foldable apparatus is held at a parallel plate distance of “X” for 24 hours at about 85°C and about 85% relative humidity. In aspects, the foldable substrate and / or the foldable apparatus can be rollable. As used herein, a foldable substrate or a foldable apparatus is “rollable” if it can achieve a threshold parallel plate distance over a length of the corresponding foldable substrate and / or foldable apparatus that is the greater of 10 mm or 10% of the length of the corresponding foldable substrate and / or foldable apparatus.
[0138] For determining the parallel plate distance or the minimum parallel plate distance of the polymer-based portion, with reference to FIG. 8, a first contact surface 283 of the polymer-based portion 289 is attached to a glass-based substrate 803 with a thickness of 30 µm and a second contact surface 285 of the polymer-based portion 289 is attached to a 50 µm thick sheet of poly(ethylene terephthalate) (PET) 707 that is formed into a foldable apparatus by hot pressing at 180°C for 1 hour. Fordetermining a parallel plate distance for a polymer-based portion, the 30 µm thick glass-based material comprising Composition 1, nominally, in mol% of: 69.1 SiO2; 10.2 Al2O3; 15.1 Na2O; 0.01 K2O; 5.5 MgO; 0.09 SnO2. As shown in FIG.8, The test foldable apparatus 801 formed from the polymer-based portion 289 is configured with the 50 µm thick sheet 707 of PET contacting the pair of parallel rigid stainless-steel plates 603 and 605 of a parallel plate apparatus 601 such that an outer surface 807 of the glass-based substrate 803 faces itself. The distance 811 between the parallel plates is reduced at a rate of 50 µm / second until the parallel plate distance is equal to the “parallel plate distance” to be tested. Then, the parallel plates are held at the parallel plate distance to be tested for 24 hours at about 60°C and about 90% relative humidity. As used herein, the “minimum parallel plate distance” is the smallest parallel plate distance that the foldable apparatus can withstand without failure under the conditions and configuration described above.
[0139] In aspects, the polymer-based portion can achieve a parallel plate distance of about 10 millimeters (mm), 7 mm, 5 mm, 4 mm, 3 mm, 2 mm, or 1 mm. In aspects, the polymer-based portion can comprise a minimum parallel plate distance in a range from about 0.5 mm to about 10 mm, from about 1 mm to about 5 mm, from about 2 mm to about 3 mm, or any range or subrange therebetween. In further aspects, the polymer-based portion can achieve a parallel plate distance of 3 mm at 25°C. In further aspects, the polymer-based portion can achieve a parallel plate distance of 3 mm at -20°C. In aspects, the polymer-based portion cured on and bonded to a glass- based substrate can withstand being held at a parallel plate distance of 3mm at -20°C for 10 days without delamination from the glass-based substrate or other failure. In aspects, the polymer-based portion can withstand 3,000 folding cycles of bending to a parallel plate distance of 3 mm at 25°C and 40% relative humidity. In aspects, the polymer-based portion can withstand 20,000 folding cycles of bending to a parallel plate distance of 3 mm at 25°C and 40% relative humidity. In aspects, the polymer- based portion can withstand 200,000 folding cycles of bending to a parallel plate distance of 3 mm at 25°C and 40% relative humidity. As used herein, each folding cycle lasted 1.82 seconds.
[0140] The polymer-based portion 289 and / or 299 may have an impact resistance defined by the capability of a test apparatus including the polymer-based portion to avoid failure at a pen drop height (e.g., 5 centimeters (cm) or more, 8 cm or more, 10 centimeters or more, 12 cm or more, 15 cm or more), when measuredaccording to the “Pen Drop Test for Polymer.” For the polymer-based portion, the test apparatus for the Pen Drop Test for Polymer is formed by (1) hot pressing the polymer-based portion to a 30 µm thick glass-based substrate (comprising Composition 1) at 180°C for 1 hour. Then, the polymer-based portion and glass-based substrate is attached to a 50 µm thick sheet of PET using a 25 µm thick adhesive having an elastic modulus of 10 MPa contacting the polymer-based portion and the 50 µm sheet of PET. As such, the test apparatus has the 50 µm thick sheet of PET disposed on the 25 µm thick adhesive that is in turn disposed on the polymer-based portion that is in turn disposed on the 30 µm thick glass-based substrate. As used herein, the “Pen Drop Test for Polymer” is conducted such that the test apparatus is tested with the load (i.e., from a pen dropped from a certain height) imparted to an outer surface of the PET sheet. During testing, the foldable apparatus bonded to the PET sheet is placed on an aluminum plate (6063 aluminum alloy, as polished to a surface roughness with 400 grit paper) with the glass-based substrate in contact with the aluminum plate. No tape is used on the side of the sample resting on the aluminum plate. A tube is used for the Pen Drop Test for Polymer to guide a pen to the outer surface of the PET sheet of the test apparatus so that the longitudinal axis of the tube is substantially perpendicular to the outer major surface with the longitudinal axis of the tube extending in the direction of gravity. The tube has an outside diameter of 1 inch (2.54 cm), an inside diameter of nine-sixteenths of an inch (1.4 cm), and a length of 90 cm. An acrylonitrile butadiene (ABS) shim is employed to hold the pen at a predetermined height for each test. After each drop, the tube is relocated relative to the test apparatus to guide the pen to a different impact location on the test apparatus. The pen employed in Pen Drop Test is a BIC Easy Glide Pen, Fine, having a tungsten carbide ballpoint tip of 0.7 mm (0.68 mm) diameter, and a weight of 5.73 grams (g) including the cap. The pen is dropped with the cap attached to the top end (i.e., the end opposite the tip) so that the ballpoint can interact with the test apparatus. In a drop sequence according to the Pen Drop Test for Polymer, one pen drop is conducted at an initial height of 1 cm, followed by successive drops in 0.5 cm increments up to 20 cm, and then after 20 cm, 2 cm increments until failure of the test apparatus. After each drop is conducted, the presence of any observable fracture, failure, or other evidence of damage to the test apparatus is recorded along with the particular pen drop height. Using the Pen Drop Test, multiple test apparatus can be tested according to the same drop sequence to generate a population with improved statistical accuracy. For thePen Drop Test, the pen is to be changed to a new pen after every 5 drops, and for each new test apparatus tested. In addition, all pen drops are conducted at random locations on the test apparatus at or near the center of the test apparatus, with no pen drops near or on the edge of the test apparatus. For purposes of the Pen Drop Test for Polymer, “failure” means the formation of a visible mechanical defect in a laminate. The mechanical defect may be a crack or plastic deformation (e.g., surface indentation). The crack may be a surface crack or a through crack. The crack may be formed on an interior or exterior surface of a laminate. The crack may extend through all or a portion of the glass-based substrate or the test apparatus. A visible mechanical defect has a minimum dimension of 0.2 mm or more.
[0141] In aspects, the polymer-based portion 289 and / or 299 can resist failure for a pen drop in the Pen Drop Test for Polymer at a pen drop height of 5 cm or more, 8 cm or more, 9 cm or more, 10 cm or more, 11 cm or more, 12 cm or more, 13 cm or more, 14 cm or more, 15 cm or more, or 20 cm. In aspects, a maximum pen drop height that the polymer-based portion 289 and / or 299 withstand without failure in the Pen Drop Test for Polymer may be about 10 cm or more, about 11 cm or more, about 12 cm or more, about 13 cm or more, about 14 cm or more, about 15 cm or more, or about 20 cm or more.
[0142] The polymer-based portion can exhibit a puncture resistance as measured in a Quasi-Static Puncture Test for Polymer. For the “Quasi-Static Puncture Test for Polymer”, a test apparatus identical to the test apparatus discussed above for the Pen Drop Test for Polymer is used. As such, the test apparatus has the 50 µm thick sheet of PET disposed on the 25 µm thick adhesive that is in turn disposed on the polymer-based portion that is in turn disposed on the 30 µm thick glass-based substrate. In the Quasi-Static Puncture Test for Polymer, a tungsten carbide ball with a predetermined diameter is placed on the outer surface of the PET sheet and a load is applied to the tungsten carbide ball at a rate of 0.1 kilogram-force (kgf) per minute until failure. In aspects, the polymer-based portion can withstand a load of about 0.5 kgf or more, about 0.8 kgf or more, about 0.9 kgf or more, about 1 kgf or more, about 1.1 kgf or more, about 1.2 kgf or more applied through a 0.25 millimeter diameter tungsten carbide ball in the Quasi-Static Puncture Test for Polymer. In aspects, the polymer-based portion can withstand a load of about 0.5 kgf or more, about 1 kgf or more, about 1.5 kgf or more, about 1.8 kgf or more, about 1.9 kgf or more, about 2 kgf or more, about 2.1 kgf or more, about 2.2 kgf or more, about 2.5 kgf or moreapplied through a 0.5 millimeter diameter tungsten carbide ball in the Quasi-Static Puncture Test for Polymer.
[0143] In aspects, the polymer-based portion 289 and / or 299 can optionally include one or more adhesion promoter (e.g., acrylate functionalized silane coupling agent, epoxy functionalized silane coupling agent), photoinitiator, and / or antioxidant. An amount of the one or more adhesion promoter, photoinitiator, and / or antioxidant can be within one or more of the corresponding ranges discussed below. For example, the polymer-based portion can comprise a photoinitiator from about 0.5 parts-per-hundred (pph) to about 3 pph, the polymer-based portion can comprise an adhesion promoter (e.g., acrylate functionalized silane coupling agent, epoxy functionalized silane coupling agent) from about 0.5 parts-per-million (ppm) to about 50 ppm or from about 0.1 pph to about 10 pph (e.g., from about 0.5 pph to about 5 pph), and / or the polymer-based portion can comprise the antioxidant from about 0.1 pph to about 1 pph. In aspects, the polymer-based portion 289 and / or 299 can be substantially free of fluorine-based compounds. As used herein, the composition can be substantially free of fluorine-based compounds while containing a trace amount of fluorine in a minor component (e.g., about 5 wt% or less of a photoinitiator) of the composition corresponding to an overall wt% of fluorine of about 0.25 wt% or less (resulting 0.0125 wt% fluorine). In further aspects, the composition can be free of fluorine-based compounds.
[0144] Throughout the disclosure, contents of the polymer-based portion can be determined through differential scanning calorimetry (DSC), infrared (IR) spectroscopy, X-ray photoelectron spectroscopy (XPS), electron paramagnetic resonance (EPR), and / or nuclear magnetic resonance (NMR). For example, a fraction of organic material (e.g., epoxy, acrylate, urethane-acrylate oligomer) as opposed to inorganic material (e.g., silsesquioxanes, inorganic nanoparticles) can be determined using DSC since mass associated with organic material is typically lost by 300°C while organic material is usually not. For example, IR spectroscopy can be used to determine the presence and / or amount of certain functional groups (e.g., epoxy, ether, acrylate, urethane) based on the existence and / or an intensity of absorbances at characteristic wavenumbers. The fine-structure detected by XPS can indicate a bonding structure of the material. In aspects, the polymer-based portion can comprise a fraction of organic material, based on a total weight of the polymer-based portion,can be about 66% or more, about 75% or more, about 85% or more, about 90% or more, about 95% or more, or about 98% or more.
[0145] In aspects, the polymer-based portion 289 and / or 299 comprises an acrylate-based polymer. In further aspects, the acrylate-based polymer contains urethane-acrylate oligomers. In aspects, the polymer-based portion 289 and / or 299 is cross-linked, for example, with bridging oxygens between polymer chains. In aspects, the polymer-based portion 289 and / or 299 can further comprise a linear polymer, as discussed below. As used herein, the “main chain” of a polymer is the longest chain of atoms in the polymer that linearly (i.e., continuously and sequentially) extends from one end of the polymer to another end of the polymer. As used herein, a linear polymer contains fewer than 5 (e.g., 0) covalently bonded repeat units deviating from the main chain.
[0146] The polymer-based portion described above can be formed as the product of curing a composition. Methods of forming the polymer-based portion described above will now be described.
[0147] Methods of forming the polymer-based portion comprises creating a composition. The composition comprises at least a low refractive index acrylate, a high refractive index acrylate, and a hydroxyl-containing acrylate. As used herein, the “low refractive index acrylate” has a refractive index less than 1.5. As used herein, the “high refractive index acrylate” has a refractive index greater than 1.5. As used herein, “acrylate” includes methacrylates and other functional groups containing acrylate functionality, unless otherwise indicated. In aspects, acrylates and / or urethane-acrylate oligomers can exclude methacrylates. In aspects, the polymer-based portion can optionally further comprise one or more of a urethane-acrylate oligomer, a linear polymer, a photoinitiator, an adhesion promoter, a tackifier, or combinations thereof. Providing a low refractive index acrylate and a high refractive index acrylate can enable a predetermined refractive index of the resulting polymer-based portion to be obtained.
[0148] In aspects, the low refractive index acrylate comprises two or more different compounds. In aspects, at least one of the low refractive index acrylates comprises an alkyl acrylate or an ether acrylate. In further aspects, all of the low refractive index acrylates comprise an alkyl acrylate or an ether acrylate. Exemplary aspects of the low refractive index acrylate includes 2-(2-ethoxyethoxy)ethyl acrylate (available from BASF) and 2-ethylhexyl acrylate (available from BASF). In aspects,an alkyl acrylate for the low refractive index acrylate can comprise 2-(2- ethoxyethoxy)ethyl acrylate (available from BASF), 2-ethylhexyl acrylate (available from BASF), 2-propylheptyl acrylate (available from BASF), ethyl acrylate (available from BASF), n-butyl acrylate (available from BASF), iso-butyl acrylate (available from BASF), tert-butyl acrylate (available from BASF), n-hexyl acrylate (available from BASF), dodecyl acrylate (available as Miramer M122 (Miwon)), isodecyl acrylate (available as Miramer M130 (Miwon)), heptadecyl acrylate (available from BASF), or combinations thereof. In aspects, the ether acrylate can comprise 2-(2- ethoxyethoxy)ethylacrylate (available as Miramer M170 (Miwon)). Additionally, in aspects, the low refractive index acrylate can comprise acrylic acid in addition to at least one alkyl acrylate, ether acrylate, or combinations thereof. In aspects, an amount of the low refractive index acrylate, as a wt% of the composition, can be about 50 wt% or more, about 55 wt% or more, about 60 wt% or more, about 65 wt% or more, about 68 wt% or more, about 85 wt% or less, about 80 wt% or less, about 75 wt% or less, or about 70 wt% or less. In aspects, an amount of the low refractive index acrylate, as a wt% of the composition, can be in a range from about 50 wt% to about 85 wt%, from about 55 wt% to about 80 wt%, from about 60 wt% to about 80 wt%, from about 65 wt% to about 75 wt%, from about 68 wt% to about 70 wt%, or any range or subrange therebetween.
[0149] In aspects, the high refractive index acrylate comprises an aromatic acrylate. In further aspects, the high refractive index acrylate comprises an aromatic methacrylate. An exemplary aspect of a high refractive index acrylate is biphenyl methyl acrylate (BPMA). In aspects, the high refractive index acrylate comprises a thiol functional group. In aspects, the high refractive index acrylate can be biphenyl methyl acrylate (BPMA), a phenyl epoxy acrylate (available as Miramer PE110 (Miwon)), benzyl acrylate (available as Miramer M1182 (Miwon)), an aromatic polyether (e.g., Miramer M140 or Miramer M142 available from Miwon), a thiol acrylate (e.g., phenyl thiol acrylate such as 2-(phenylthio)ethyl acrylate (available as M1162 (Miwon))), or combinations thereof. In aspects, an amount of the high refractive index acrylate, as a wt% of the composition, can be greater than 0 wt% or more, about 5 wt% or more, about 10 wt% or more, about 13 wt% or more, about 15 wt% or more, about 17 wt% or more, about 25 wt% or less, about 24 wt% or less, about 23 wt% or less, about 22 wt% or less, about 21 wt% or less, or about 20 wt% or less. In aspects, an amount of the high refractive index acrylate, as a wt% of thecomposition, can be in a range from greater than 0 wt% to about 25 wt%, from about 5 wt% to about 24 wt%, from about 10 wt% to about 23 wt%, from about 13 wt% to about 22 wt%, from about 15 wt% to about 21 wt%, from about 17 wt% to about 20 wt%, or any range or subrange therebetween.
[0150] In aspects, the hydroxyl-containing acrylate can comprise a hydroxy alkyl acrylate. Exemplary aspects of the hydroxyl-containing acrylate include 4- hyrdoxybutyl acrylate (available from BASF), 2-hydroxy-3-phenoxypropyl acrylate(available from BASF), caprolactone acrylate (available as Miramer M100D (Miwon)), and combinations thereof. In aspects, an amount of the hydroxyl- containing acrylate, as a wt% of the composition, can be about 5 wt% or more, about 10 wt% or more, about 13 wt% or more, about 15 wt% or more, about 17 wt% or more, about 30 wt% or less, about 25 wt% or less, about 23 wt% or less, or about 20 wt% or less. In aspects, an amount of the hydroxyl-containing acrylate, as a wt% of the composition, can be in a range from about 5 wt% to about 30 wt%, from about 10 wt% to about 25 wt%, from about 13 wt% to about 23 wt%, from about 15 wt% to about 20 wt%, from about 17 wt% to about 20 wt%, or any range or subrange therebetween.
[0151] In aspects, the urethane-acrylate oligomer can comprise a difunctional urethane-acrylate oligomer. In aspects, the difunctional urethane-acrylate oligomer can comprise one or more of the following products in the Miramer product line available from Miwon: PU210, PU256, PU2050, PU2100, PU2300C, PU2560, SC2404, and / or SC2565. In aspects, the difunctional urethane-acrylate oligomer can comprise one or more of the following products in the Photomer product line available from IGM Resins: 6009, 6063, 6210, 6215, 6230, 6620, 6630, 6638, 6643, 6644, 6645, 6891, 6579, 6581, 6582, and / or 6581. In aspects, the difunctional urethane-acrylate oligomer can comprise the following products available from Arkema (Sartomer): PRO13944, PRO14213, CN8881, CN90004, CN9009, CN9030, CN9031, CN964, CN966J75, CN981, CN991, and / or CN 962. In aspects, the difunctional urethane-acrylate oligomer can comprise the following products from Dymax (Bomar): BR-344, BR-345, BR-374, BR-3042, BR-3747AE, BR-541S, BR- 543, BR-543TF, BR-571, BR-641E, BR-744BT, BR-744SD, and / or BR-771F. In aspects, the difunctional urethane-acrylate oligomer can comprise a polyether urethane acrylate. In aspects, the difunctional urethane-acrylate oligomer can comprise difunctional aliphatic urethane acrylate. An exemplary aspect of adifunctional urethane-acrylate oligomer is Bomar BR-543 (Dymax). In aspects, an amount of the difunctional urethane-acrylate oligomer, as a wt% of the composition, can be 0 wt% or more, greater than 0 wt%, about 0.2 wt% or more, about 0.4 wt% or more, about 1 wt% or less, about 0.8 wt% or less, or about 0.6 wt% or less. In aspects, an amount of the difunctional urethane-acrylate oligomer, as a wt% of the composition, can be in a range from 0 wt% to about 1 wt%, from greater than 0 wt% to about 1 wt%, from about 0.2 wt% to about 0.8 wt%, from about 0.4 wt% to about 0.6 wt%, or any range or subrange therebetween.
[0152] In aspects, the composition can optionally include a cross-linker. As used herein, a “cross-linker” is a compound with at least two reactive functional groups at ends of the compound. In further aspects, the cross-linker can be a monomer. In further aspects, the cross-linker can be difunctional (e.g., difunctional monomer). Alternatively, the cross-linker can have more than two reactive functional groups (e.g., tri-functional). Exemplary functional groups for the cross-linker include acrylate, isocyanate, and combinations thereof. An exemplary aspect of a crosslinker is H12MDI is hydrogenated methylene diphenyl isocyanate available from Millipore Sigma.
[0153] In aspects, the composition can comprise a photoinitiator. As used herein a photoinitiator is a compound sensitive to one or more wavelengths that upon absorbing light comprising the one or more wavelengths undergoes a reaction to produce one or more radicals or ionic species that can initiate a polymerization reaction. In further aspects, the photoinitiator may be sensitive to one or more wavelengths of ultraviolet (UV) light. Example aspects of photoinitiators sensitive to UV light include without limitation benzoin ethers, benzil ketals, dialkoxyacetophenones, hydroxyalkylphenones, aminoalkylphenones, acylphosphine oxides, thioxanthones, hydroxyalkylketones, and thoxanthanamines. In further aspects, the photoinitiator may be sensitive to one or more wavelengths of visible light. Example aspects of photoinitiators sensitive to visible light include without limitation 5,7-diiodo-3-butoxy-6-fluorone, bis (4-methoxybenzoyl) diethylgermanium, bis(2,4,6-trimethylbenzoyl)-phenylphosphineoxide, 3-methyl-4- aza-6-helicene, and thiocyanide borates. In further aspects, the photoinitiator may be sensitive to a wavelength that other components of the polymer-based portion and / or composition are substantially transparent at. As used herein, a compound (e.g., component of the composition) is substantially transparent at a predeterminedwavelength if it comprises an average transmittance of 75% or more (e.g., 80% or more, 85% or more, or 90% or more, 92% or more, 94% or more, 96% or more) through a 1.0 mm thick piece of the compound at the predetermined wavelength. Providing a photoinitiator can enable controlled activation of curing of the composition. Providing a photoinitiator can enable uniform curing of the composition.
[0154] In further aspects, the photoinitiator may produce one or more ions. Example aspects of photoinitiators producing one or more ions include without limitation triarylsulfonium hexfluoroantimonate, triphenylsulfonium hexafluoroantimonate, and bis(4-tert-butylphenyl)iodonium perfluoro-1- butanesulfonate. Commercially available photoinitiators include without limitation the Irgacure product line from BASF. Exemplary aspects of photoinitiators include acetophenone-based compounds, for example, dimethoxyphenyl acetophenone. In further aspects, the photoinitiator may produce one or more radicals (e.g., free radicals). Example aspects of photoinitiators producing one or more radicals include acetophenone, anisoin, anthraquinone, benzene, benzil, benzoin, benzoin ethyl ether, benzoin isobutyl ether, benzoin methyl ether, benzophenone, hydroxycyclohexyl phenyl ketone, 4-benzoylbiphernyl, camphorquinone, 2-chlorothioxanthen-9-one, bibezosuberenone, 2-,2-diethyoxyacetophenone, dimethylbenzil, ferrocene, ethylanthraquinone, hydroxyacetophenone, hydroxybenzophenone, thioxanthene-9- one, diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, and phophineoxide. In even further aspects, the photoinitiator can comprise ethyl (2,4,6-trimethylbenzoyl) phenylphosphinate. As used herein, “superaddition” refers to an additional material added to a composition with the reference 100 wt% of the composition excluding the material added by superaddition. Throughout the disclosure, one “part-per-hundred” (pph) and 10,000 “parts-per-million” (ppm) refers to an amount equal to 1 wt% of the composition excluding materials added by superaddition. It is to be understood that compositions stated in terms of components added by superaddition can be converted to compositions without one or more of the components stated as superaddition by renormalizing the wt% of the composition to include the one or more components. In aspects, the composition can comprise an amount of the photoinitiator added by superaddition of about 0.1 pph or more, about 0.5 pph or more, about 1 pph or more, about 1.5 pph or more, about 5 pph or less, about 3 pph or less, about 2 pph or less, or about 1.5 pph or less, for example, from about 0.1 pph to about 5 pph, from about 0.5 pph to about 3, from about 1 to about 2, or any range or subrange therebetween.
[0155] In aspects, the polymer-based portion and / or composition can comprise a catalyst. Without wishing to be bound by theory, a catalyst can increase a rate of the curing (e.g., polymerization, reaction), and the catalyst may avoid permanent chemical change as a result of the curing. In aspects, the catalyst can comprise one or more platinum group metals, for example, ruthenium, rhodium, palladium, osmium, iridium, and / or platinum. In aspects, the catalyst can comprise a platinum-based Karstedt’s catalyst solution. Exemplary aspects of platinum-based catalysts include chloroplatinic acid, platinum-fumarate, colloidal platinum, metallic platinum, and / or platinum-nickel nanoparticles.
[0156] In aspects, the composition can comprise a silane coupling agent. In further aspects, the silane coupling agent can comprise a mercapto silane, an acrylate silane, and / or an epoxy silane. In even further aspects, the silane coupling agent can comprise an acrylate silane. Exemplar aspects of mercapto silanes include 3- mercaptopropylmethyldimethoxysilane (e.g., SIM6474.0 (Gelest), 3-mercaptopropyl- trimethoxysilane (e.g., SIM6476.0 (Gelest)), 3-mercaptopropylmethyldiethoxysilane, 3-mercaptopropyltriethoxysilane (e.g., SIM6475.0 (Gelest)), 11-mercaptoundecyl- trimethoxysilane (e.g., SIM6480.0 (Gelest)), (mercaptomethyl)methyldiethoxysilane (e.g., SIM6473.0 (Gelest)), and / or 3-mercaptopropylmethyldimethoxysilane (e.g., SIM6474.0 (Gelest)). Exemplary aspects of acrylate silanes include 3-acryloxypropyltrimethoxysilane (e.g., SIA0200.0 (Gelest)), 3-acryloxypropyl- triethoxysilane, 3-arcyloxypropyldimethylmethoxysilane (e.g., SIA0190.0 (Gelest)), 3-acryloxypropyldimethylethoxysilane, 3-acryloxypropylmethyl-diethoxysilane (e.g., SIA0197.0 (Gelest)), 3-acryloxypropylmethyldimethoxysilane (e.g., SIA0198.0 (Gelest)), N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltrimethoxysilane, N-(3-acryloxy-2-hydroxypropyl)-3-aminopropyltriethoxysilane (e.g., SIA0180.0 (Gelest)), acryloxy-methyltrimethoxysilane (e.g., SIA0182.0 (Gelest)), acryloxymethyltriethoxysilane, acryloxymethylphenethyltrimethoxysilane (e.g., SIA0184.0 (Gelest), and acryloxy-methylphenethyltriethoxysilane. In aspects, the composition can comprise an amount of the silane coupling agent added by superaddition of about 0.5 ppm or more, about 5 ppm or more about 20 ppm or more, about 0.1 pph or more, about 0.5 pph or more, about 1 pph or more, about 2 pph or more, about 5 pph or more, about 10 pph or less, about 5 pph or less, about 3 pph or less, about 1 pph or less, about 0.1 pph or less, about 1,000 ppm or less, or about 50 ppm or less. In aspects, the composition can comprise an amount of the silanecoupling agent added by superaddition from about 0.5 ppm to about 10 pph, from about 0.1 pph to about 10 pph, from about 0.5 pph to about 5 pph, from about 1 pph to about 3 pph, from about 2 pph to about 3 pph, or any range or subrange therebetween. Alternatively, aspects, the composition can comprise less than 1 pph of the silane coupling agent added by superaddition, for example, in a range from 0.5 ppm to about 0.1 pph, from about 5 ppm to about 1,000 ppm or less, from about 20 ppm to about 50 ppm, or any range or subrange therebetween.
[0157] In aspects, the polymer-based portion and / or composition can comprise an antioxidant. In further aspects, the antioxidant can comprise a phenolic- based compound or a phosphite-based compound. Exemplary aspects of antioxidants comprising phenolic-based compounds available include pentaerythritol tetrakis(3- (3,5-di-tert-butyl-4-hydroxyphenyl)propionate (e.g., Irganox 1010 (BASF)), thiodiethylene bis[3-(3,5-di-ter-butyl-4-hydroxy-phenyl)]propionate (e.g., Irganox 1035 (BASF)), octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate (e.g., Irganox 1076 (BASF)), benzenepropanoic acid (e.g., Irganox 1135 (BASF)), 3,3’,3’,5,5’,5’-hexa-tert-butyl-a,a’,a’-(mesitylene-2,4,6-triyl)tri-p-cresol (e.g., Irganox 1330 (BASF)), (1,1-di-tert-butyl)-4-hydroxyphenyl)methyl)ethylphosphonate (e.g., Irganox 1425 (BASF)), 4,6-bis[octylthiomethyl]-o-crsol (e.g., Irganox 1520 (BASF)), 1,3,5-tris[3,5-di-tert-butyl-4-hydroxybenzyl)-1,3,5-triazine-2,4,5(1H,3H,5H)-trione (e.g., Irganox 3114 (BASF)), 2,6-di-tert-butyl-4-(4,6-bis(octothiol)-1,3,5-triazin-2- ylamino)phenol (e.g., Irganox 565 (BASF)), and 2’,3-bis[3-(3,5-di-tert-butyl-4- hydroxyphenyl)propionyl] propionohydrazine (e.g., Irganox MD-1024 (BASF)). Exemplary aspects of antioxidants comprising phosphite-based compounds include 2,2’,2’’-nitrolo(triethyl-tris[3,3’,5,5’-terta-tert-butyl-1,1’-biphenyl-2,2’- diyl])phosphile (e.g., Irgafos 12 BASF), bis[2,4,-di-tert-butylphenol]pentaerythritol diphosphate (e.g., Irgafos 126 (BASF), tris[2,4-ditert-butylphenyl]phosphite (e.g., Irgafos 168 (BASF)), bis[2,4-di-tert-butyl-6-methylphenyl]-ethyl-phosphite (e.g., Irgafos 38 (BASF)), trisnonylphenyl phosphite (e.g., Weston 399 (Addivant)), 3,9- bis(octadecyloxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiroundecane (e.g., Weston 618 (Addivant)) [1,3,2-dioxaphosphorinane, 5-butyl-5-ethyle-2-(2,4,6-tris[1,1- dimethylethyl]phenoxy)-1,3,2-dioxaphosphinane] (e.g., Ultranox 641 (SI Group)), 2,2’-ethyidene-bis[4,6,-di-tert-butylphenyl]fluorophosphate (e.g., Ethenox 398 (SI Group)), and 2,2’-Methylene-bis[4,6-di-tert-butylphenyl]-2-ethylhexyl phosphite (e.g., ADK STAB HP-10 (Adeka)). In aspects, the composition can comprise anamount of the antioxidant added by superaddition of about 0.01 pph or more, about 0.1 pph or more, about 0.2 pph or more, about 0.4 pph or more, about 5 pph or less, about 1 pph or less, about 0.8 pph or less, or about 0.6 pph or less, for example, in a range from about 0.01 pph to about 5 pph, from about 0.1 pph to about 1 pph, from about 0.2 pph to about 0.8 pph, from about 0.4 pph to about 0.6 pph, or any range or subrange therebetween. Providing an antioxidant can improve a color of the polymer- based portion and / or foldable apparatus, for example by decreasing yellowing as the polymer-based portion and / or foldable apparatus.
[0158] In aspects, the composition can comprise a linear polymer. As used herein, a linear polymer contains fewer than 5 (e.g., 0) covalently bonded repeat units deviating from the main chain. In aspects, the linear polymer can comprise a homopolymer or a monomer. In further aspects, the linear polymer can comprise a copolymer of ethylene, vinyl alcohol, and / or vinyl acrylate (e.g., poly(ethylene-co- vinyl acetate) (EVA), poly(vinyl acrylate-vinyl alcohol-co-ethylene)). Exemplary aspects of the linear polymer include poly(ethylene-co-vinyl acrylate), poly(vinyl acrylate-co-vinyl alcohol-co-ethylene) poly(vinyl methyl ketone), poly(vinyl formal), or combinations thereof. In aspects, the linear polymer can comprise a hydroxyl functional group at an end of the linear polymer. For example, the linear polymer can be partially hydrolyzed, which can enable the linear polymer to react with the other components in the composition. In aspects, an amount of the linear polymer, as a wt% of the composition and / or the resulting polymer-based portion, can be about 0.5 wt% or more, about 1 wt% or more, about 3 wt% or more, about 5 wt% or more, about 10 wt% or more, about 30 wt% or less, about 20 wt% or less, about 15 wt% or less, about 10 wt% or less, or about 5 wt% or less. In aspects, the amount of the linear polymer, as a wt% of the composition and / or the resulting polymer-based portion, can be in a range from about 0.5 wt% to about 30 wt%, from about 1 wt% to about 20 wt%, from about 3 wt% to about 15 wt%, from about 5 wt% to about 10 wt%, or any range or subrange therebetween. In aspects, the amount of the linear polymer, as a wt% of the composition and / or the resulting polymer-based portion, can be less than 5 wt%, for example, in a range from about 0.5 wt% to about 5 wt%, from about 1 wt% to about 3 wt%, or any range or subrange therebetween. Providing the linear polymer can enable a predetermined viscosity to be achieved, which can facilitate coating using a predetermined technique.
[0159] In aspects, the composition can be substantially solvent-free, solvent- free, and / or entirely solvent-free. As used herein, a composition is entirely solvent- free if it only contains components that participate in the curing reaction and / or are considered an inorganic filler, a photoinitiator, a catalyst, a silane coupling agent, or an antioxidant based on the above discussion. As used herein, a composition is solvent-free if it contains 99.5 wt% or more components that participate in the curing reaction and / or are considered a photoinitiator, a catalyst, or an antioxidant based on the above discussion. As used herein a composition is substantially solvent-free if it contains 98 wt% or more components that participate in the curing reaction and / or are considered a photoinitiator, a catalyst, or an antioxidant based on the above discussion. For example, water and octanol are considered solvents. Solvents can comprise one or more of a polar solvent (e.g., water, an alcohol, an acetate, acetone, formic acid, dimethylformamide, acetonitrile, dimethyl sulfoxone, nitromethane, propylene carbonate, poly(ether ether ketone)) or a non-polar solvent (e.g., pentane, 1,4-dioxane, chloroform, dichloromethane, diethyl ether, hexane, heptane, benzene, toluene, xylene). For example, a composition comprising up to 0.5 wt% solvent is considered to be both substantially solvent-free and solvent-free. Likewise, a composition containing no solvent is considered to be substantially solvent-free, solvent-free, and entirely solvent-free. Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can increase the curing rate of the composition, which can decrease processing time. Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can reduce (e.g., decrease, eliminate) the use of additives, for example, rheology modifiers, and increase composition homogeneity, which can improve the quality of the resulting polymer- based portion (e.g., increased transmittance, decreased haze, increased mechanical properties). Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can reduce a volume change as a result of curing (e.g., shrinkage). In aspects, the composition and / or the polymer-based portion can be substantially free of fluorine-based compounds and / or free of fluorine-based compounds, which can reduce an environmental impact of the polymer-based portion and / or reduce a cost to produce the polymer-based portion.
[0160] Example composition ranges of polymer-based portions and / or compositions including an acrylate and / or a urethane-acrylate oligomer in accordance with aspects of the disclosure are presented in Tables 1-2. Table 1 presents ranges R1-R6 of compositions without a linear polymer while Table 2 presents Ranges R7-R13 with a non-zero amount of a linear polymer. R1 and R7 are the broadest of the ranges in the respective tables. Ranges R1, R3-R4, R7, and R10-R11 can be free of the urethane-acrylate oligomer. Ranges 1-13 can be free of a cross-linker while Ranges R1, R6-R7, R10-R11, and R13 can include a cross-linker. Ranges R7, R10, and R12 can be free of a photoinitiator. Ranges R1, R4, R7, R10, and R12 can be free of a silane coupling agent. Ranges R1, R5, R7, R9, and R12 can be free of an antioxidant. Ranges R1-R13 comprise a low refractive index acrylate, a high refractive index acrylate, and a hydroxyl-containing acrylate. Again, it is to be understood that other ranges or subranges discussed above for these components can be used in combination with any of the ranges presented in Table 1. Table 1: Composition ranges (wt%) R1-R6 of aspects of polymer-based portionsTable 2: Composition ranges (wt%) R7-R13 of aspects of polymer-based portions
[0161] Methods of forming the polymer-based portion, for example, as part of making a foldable apparatus, will now be discussed with reference to the flow chart shown in FIG.12 and the example steps illustrated in FIGS.13-18.
[0162] A first set of methods of forming the polymer-based portion, for example from compositions within ranges R1-R6, will now be discussed. Methods can start at step 1201 comprising providing the composition within one or more of the compositional ranges discussed above. In aspects, components of the composition can be provided by purchase, synthesis, or combinations thereof. In aspects, the components can be mixed together to form a composition (e.g., composition 1301 in FIG. 13). In further aspects, less than all of the photoinitiator (e.g., from about 20 wt% to about 80 wt%, from about 30 wt% to about 70 wt%, of from about 40 wt% to about 60 wt% of the total amount of photoinitiator to be used in making the polymer- based portion) can be included in the composition. In further aspects, the composition in step 1201 may not include a silane coupling agent and / or an anti-oxidant even if these components are to be included in the resulting polymer-based portion. In further aspects, as for ranges R1-R6, the composition can be free of a linear polymer.
[0163] After step 1201, as shown in FIG. 13, methods can proceed to step 1203 comprising partially curing the composition to form a precursor solution. In aspects, as shown, the composition 1301 can be in a container 1311. In further aspects, the composition 1301 can be mixed, for example by rotating (arrow 1305) an impeller 1307 about a shaft 1303, during step 1203 and / or step 1201. Mixing the composition during step 1203 can provide a more homogenous precursor solution. In aspects, as shown, the partially curing can comprise impinging the composition 1301 with radiation 1315 emitted from a radiation source 1313 (e.g., light source). In further aspects, the impinging can comprise impinging the composition with at least one wavelength of light that the photoinitiator is sensitive to. In further aspects, the irradiating can comprise impinging the composition with a light beam emitted from aradiation source with a predetermined fluence. In even further aspects, the radiation source 1313 can be configured to emit a light beam comprising an ultra-violet (UV) wavelength or a visible wavelength. In still further aspects, the wavelength of the light beam can be in a range from about 10 nm to about 400 nm, from about 100 nm to about 400 nm, from about 200 nm to about 400 nm, from about 10 nm to about 300 nm, from about 100 nm to about 300 nm, from about 200 nm to about 300 nm, from about 10 nm to about 200 nm, from about 100 nm to about 200 nm, or any range or subrange therebetween. In still further aspects, an operating wavelength range of the radiation source 1313 may be over a range of optical wavelengths from about 315 nm to about 400 nm, from about 280 nm to about 315 nm, from about 100 nm to about 280 nm, or from 122 nm to about 200 nm. In even further aspects, the wavelength of the light beam can be in a range from about 300 nm to about 1,000 nm, from about 350 nm to about 900 nm, from about 400 to about 800 nm, from about 500 nm to about 700 nm, or any range or subrange therebetween. In still further aspects, the wavelength of the light beam can be about 365 nm, about 415 nm, or about 590 nm. In further aspects, the predetermined fluence can be about 0.05 milliJoule per centimeter squared (mJ / cm2) or more, about 0.1 mJ / cm2or more, about 0.3 mJ / cm2or more, about 0.5 mJ / cm2or more, about 2 mJ / cm2or less, about 1.5 mJ / cm2or less, or about 1 mJ / cm2or less. In further aspects, the predetermined fluence can range from about 0.05 mJ / cm2to about 2 mJ / cm2, from about 0.1 mJ / cm2to about 2 mJ / cm2, from about 0.3 mJ / cm2to about 1.5 mJ / cm2, from about 0.5 mJ / cm2to about 1 mJ / cm2, or any range or subrange therebetween. Alternatively, although not shown, the partially curing can comprise heating the composition at a temperature for a time. As used herein, heating a composition “at a temperature” means that the composition is exposed to the temperature, for example, by being placed in an oven. In further aspects, the temperature can be about 80°C or more, about 100°C or more, about 120°C or more, about 140°C or more, about 250°C or less, about 200°C or less, about 180°C or less, or about 160°C or less. In further aspects, the temperature can be in a range from about 80°C to about 250°C, from about 80°C to about 200°C, from about 100°C to about 200°C, from about 100°C to about 180°C, from about 120°C to about 180°C, from about 120°C to about 160°C, from about 140°C to about 160°C, or any range or subrange therebetween. In further aspects, the time can be about 15 minutes or more, about 30 minutes or more, 1 hour or more about 12 hours or less, about 6 hours or less, about 3 hours or less, or about 2 hours or less. In further aspects, thetime can be in a range from about 15 minutes to about 12 hours, from about 15 minutes to about 6 hours, from about 15 minutes to about 3 hours, from about 30 minutes to about 3 hours, from about 1 hour to about 3 hours, from about 1 hour to about 2 hours, or any range or subrange therebetween.
[0164] As used herein, “partially cured” refers to an extent of reaction of the acrylate functional groups of less than 70%. An extent of reaction can be monitored and / or determined using spectroscopy. Unless otherwise indicated, an extent of reaction is determined using infrared (IR) spectroscopy to monitor the intensity of absorbance associated with the unreacted acrylate group. In aspects, at the end of step 1203, an extent of reaction of the acrylate functional groups in the precursor solution can be about 10% or more, about 15% or more, about 20% or more, about 25% or more, about 30% or more, about 70% or less, about 60% or less, about 50% or less, about 40% or less, about 33% or less, or about 25% or less. In aspects, at the end of step 1203, an extent of reaction of the acrylate functional groups in the precursor solution can be in a range from about 5% to about 70%, from about 5% to about 60%, from about 10% to about 50%, from about 15% to about 40%, from about 20% to about 33%, or any range or subrange therebetween. In aspects, at the end of step 1203, a gel fraction (defined above) of the precursor solution can be about 30% or less, about 25% or less, about 20% or less, about 15% or less, or about 10% or less.
[0165] The partially curing the composition 1301 in step 1203 produces the precursor solution 1401 (compare FIGS. 13-14). In aspects, the precursor solution 1401 has a precursor viscosity that is greater than a viscosity of the composition 1301. As used herein, a viscosity of a liquid is measured at 25°C using a rotational rheometer (e.g., CAP2000 viscometer from Brookfield Engineering) at a shear rate of 1.66 1 / second (i.e., 100 revolutions per minute (rpm)). In aspects, the precursor viscosity of the precursor solution 1401 at the end of step 1203 can be about 0.1 Pascal-seconds (Pa-s) or more, about 0.2 Pa-s or more, about 0.3 Pa-s or more, about 0.4 Pa-s or more, about 0.5 Pa-s or more, about 10 Pa-s or less, about 8 Pa-s or less, about 5 Pa-s or less, about 3 Pa-s or less, about 1 Pa-s or less, or about 0.8 Pa-s or less. In aspects, the precursor viscosity of the precursor solution 1401 at the end of step 1203 can be in a range from about 0.1 Pa-s to about 10 Pa-s, from about 0.1 Pa-s to about 8 Pa-s, from about 0.2 Pa-s to about 5 Pa-s, from about 0.3 Pa-s to about 3 Pa-s, from about 0.4 Pa-s to about 1 Pa-s, from about 0.5 Pa-s to about 0.8 Pa-s, or any range or subrange therebetween. Providing a precursor viscosity in a range fromabout 0.1 Pa-s to about 10 Pa-s can enable the precursor solution to be coated on a target substrate (e.g., foldable substrate) using a variety of techniques.
[0166] After step 1203, as shown in FIG. 14, methods can proceed to step 1205 comprising mixing the precursor solution 1401 with one or more additional components (e.g., solution 1423). In aspects, as shown, the precursor solution 1401 can be in the container 1311. In further aspects, the precursor solution 1401 can be mixed, for example by rotating (arrow 1305) an impeller 1307 about a shaft 1303, during step 1205. In aspects, as shown, a solution 1423 (i.e., one or more components) can be dispensed from a container 1421 (e.g., conduit, flexible tube, micropipette, or syringe) and mixed with the precursor solution 1401. In further aspects, the one or more additional components can include a portion of the photoinitiator held back from the composition 1301 (see FIG.13 and step 1201) as well as additives, for example, a silane coupling agent and / or an anti-oxidant. Adding the additional components (e.g., additional photoinitiator) to the precursor solution can enable a high cure state (e.g., measured by gel fraction) of the resulting polymer-based portion while allowing a predetermined precursor viscosity to be obtained.
[0167] After step 1205, as shown in FIGS.15 and 17, methods can proceed to step 1207 comprising disposing the precursor solution on a foldable substrate 201. In aspects, as shown, the precursor solution can be dispensed from a container 1501 or 1701 (e.g., conduit, flexible tube, micropipette, or syringe) to form a layer 1503 or 1703 of the precursor solution on the foldable substrate 201. In aspects, as shown, the layer 1503 or 1703 of the precursor solution can be at least partially positioned (e.g., positioned in) a recess (e.g., first recess 211, second recess 241) of the foldable substrate 201. In further aspects, although not shown, disposing the precursor solution can further comprise drawing an applicator bar across the a central surface area (e.g., second central surface are 243 in FIG. 17) and / or a major surface (e.g., first major surface 203 in FIG. 15 or second major surface 205 in FIG. 17) to achieve a layer of a predetermined thickness, by controlling a height of the applicator bar. In even further aspects, a predetermined thickness of the layer can be within one or more of the ranges discussed below with reference to the polymer-based portion 289 and / or 299. In aspects, as shown by comparing FIGS. 15-16, the layer 1503 can extend beyond a recess (e.g., first recess 211). In aspects, as shown by comparing FIGS. 15- 16, a layer of another material (e.g., device substrate or release liner 271) can be disposed on the layer 1503 before proceeding to step 1209.
[0168] After step 1207, as shown in FIG. 17, methods can proceed to step 1209 comprising curing the precursor solution to form a polymer-based portion. In aspects, as shown, the curing can comprise impinging the layer 1503 (see FIG.15) of the precursor solution with radiation 1603 from a radiation source 1601 to form the polymer-based portion (e.g., second polymer-based portion 299). In further aspects, the impinging can comprise impinging the composition with at least one wavelength of light that the photoinitiator is sensitive to. In further aspects, the irradiating can comprise impinging the composition with a light beam emitted from a radiation source with a predetermined fluence. In even further aspects, the radiation source 1601 can be configured to emit a radiation 1603 (e.g., light beam) comprising an ultra-violet (UV) wavelength or a visible wavelength, for example, within one or more of the wavelength ranges discussed above for step 1203. In further aspects, the predetermined fluence can be about 1 milliJoule per centimeter squared (mJ / cm2) or more, about 2 mJ / cm2or more, about 2.5 mJ / cm2or more, about 5 mJ / cm2or less, about 4 mJ / cm2or less, about 3 mJ / cm2or less, or about 2.5 mJ / cm2or less. In further aspects, the predetermined fluence can range from about 1 mJ / cm2to about 5 mJ / cm2, from about 2 mJ / cm2to about 4 mJ / cm2, from about 2.5 mJ / cm2to about 3 mJ / cm2, or any range or subrange therebetween. Alternatively, although not shown, the partially curing can comprise heating the composition at a temperature for a time. As used herein, heating a composition “at a temperature” means that the composition is exposed to the temperature, for example, by being placed in an oven at a temperature within one or more of the corresponding ranges discussed above for step 1203 and / or a period of time within one or more of the corresponding ranges discussed above for step 1203. In aspects, as shown, the curing can form the polymer-based portion (e.g., second polymer-based portion 299) disposed on and / or attached to the foldable substrate 201, for example, contacting a central surface area (e.g., first central surface area 213) and / or a major surface (e.g., first major surface 203) of the foldable substrate 201. In further aspects, as shown, the curing can further form the polymer- based portion (e.g., second polymer-based portion 299) attached to another material (e.g., device substrate or release liner 271) that was disposed on the layer before the curing, for example, such that the polymer-based portion attaches the foldable substrate 201 to the another material (e.g., device substrate or release liner 271).
[0169] At the end of step 1209, the polymer-based portion can comprise any one or more of the aspects discussed above for the polymer-based portion. Forexample, the polymer-based portion can be an acrylate-based polymer with a glass- transition temperature (Tg) of about -20°C or less, a storage modulus (E’) at 25°C from about 0.1 MegaPascals to about 1 MegaPascals, a refractive index from about 1.47 to about 1.51.
[0170] In aspects, curing the precursor solution in step 1209 to form the polymer-based portion (e.g., polymer-based material) can result in a volume change of the polymer-based portion relative to a volume of the precursor solution. In further aspects, a magnitude of a difference of the volume of the polymer-based portion relative to the volume of the precursor solution as a percentage of the volume of the precursor solution can be about 5% or less, about 2% or less, about 1% or less, about 0.5% or less, about 0.1% or less, about 0.01% or more, about 0.1% or more, about 0.5% or more, about 1% or more. In further aspects, a magnitude of a difference of the volume of the polymer-based portion relative to the volume of the precursor solution as a percentage of the volume of the composition can be in a range from 0% to about 5%, from 0% to about 2%, from 0% to about 1%, from 0.01% to about 1%, from about 0.1% to about 1%, from about 0.5% to about 1%, from about 0.01% to about 5%, from about 0.01% to about 2%, from about 0.1% to about 2%, from about 0.5% to about 2%, or any range or subrange therebetween.
[0171] In aspects, after step 1209, as shown in FIGS. 17-18, methods can proceed to step 1211 comprising assembling a foldable apparatus. In aspects, as shown in FIGS. 17-18, step 1211 can comprise assembling the foldable apparatus by disposing another polymer-based portion (e.g., first polymer-based portion 289) over the foldable substrate 201, although it is to be understood that other materials (e.g., an adhesive layer, and / or a coating) can be disposed on the foldable substrate additionally or alternatively. In further aspects, as shown in FIG. 17, another precursor solution 1703 can be disposed on the foldable substrate 201 (e.g., opposite the polymer-based portion formed in step 1209), for example, by dispensing the another precursor solution 1703 from a container 1701 (e.g., conduit, flexible tube, micropipette, or syringe) that can be cured to form another polymer-based portion (e.g., second polymer-based portion). Curing the another precursor solution 1703 can comprise heating the another precursor solution 1703, irradiating the another precursor solution 1703 with ultraviolet (UV) radiation, and / or waiting a predetermined amount of time (e.g., from about 30 minutes to 24 hours, from about 1 hour to about 8 hours). In further aspects, as shown in FIG.18, an adhesive layer 261can be disposed over and / or disposed on the second major surface 205 (e.g., the second surface area 225 and the fourth surface area 235) and / or the additional polymer-based portion (e.g., second polymer-based portion 299). For example, the adhesive layer 261 can comprise one or more sheets of an adhesive material. In aspects, although not shown, at least a portion of the adhesive layer can be disposed in the second recess. In aspects, a release liner (e.g., see device substrate or release liner 271 in FIGS. 2-4) or a display device may be disposed on the adhesive layer 261 (e.g., second contact surface 265).
[0172] After step 1209 or 1211, methods can proceed to step 1213, where methods of making the polymer-based portion (or foldable substrate and / or the foldable apparatus) can be complete. In aspects, methods can proceed along steps 1201, 1203, 1205, 1207, 1209, 1211, and 1213 of the flow chart in FIG. 12 sequentially, as discussed above. In aspects, methods can follow arrow 1202 from step 1201 to step 1207, for example, if the precursor solution with the precursor viscosity is already present at the end of step 1201. In aspects, methods can follow arrow 1204 from step 1203 to step 1207, for example, if there are no additional components to be added to the precursor solution between the partial curing to form the precursor solution and disposing the precursor solution on the foldable substrate. In aspects, methods can follow arrow 1206 from step 1209 to step 1213, for example, if methods are complete at the end of step 1209. Any of the above options may be combined to make a polymer-based portion (or a foldable apparatus) in accordance with the embodiments of the disclosure.
[0173] A second set of methods of forming the polymer-based portion, for example from compositions within ranges R7-R13 comprising the linear polymer, will now be discussed. Methods can start at step 1201 comprising providing the precursor within one or more of the compositional ranges discussed above. In aspects, components of the composition can be provided by purchase, synthesis, or combinations thereof. In aspects, the components can be mixed together to form the precursor solution 1401 (see FIG.14). In aspects, as shown in FIG.14, step 1201 can comprise adding one or more components (e.g., linear polymer) shown as a solution 1423. In further aspects, a solution 1423 (i.e., one or more components) can be dispensed from a container 1421 (e.g., conduit, flexible tube, micropipette, or syringe) and mixed with the precursor solution 1401. In aspects, step 1201 can comprise mixing the precursor solution 1401 with one or more additional components (e.g.,solution 1423) in the container 1311, where the precursor solution 1401 can be mixed, for example by rotating (arrow 1305) an impeller 1307 about a shaft 1303, during step 1205. At the end of step 1201, the precursor solution 1401 comprising the linear polymer can comprise a precursor viscosity within one or more of the ranges discussed above for the precursor solution at the end of step 1203 (e.g., from about 0.1 Pa-s to about 10 Pa-s, from about 0.2 Pa-s to about 5 Pa-s, from about 0.3 Pa-s to about 3 Pa-s, from about 0.4 Pa-s to about 1 Pa-s, from about 0.5 Pa-s to about 0.8 Pa- s). Providing a precursor viscosity in a range from about 0.1 Pa-s to about 10 Pa-s can enable the precursor solution to be coated on a target substrate (e.g., foldable substrate) using a variety of techniques.
[0174] After step 1201, as shown in the flow chart in FIG.12 and in FIGS. 15 and 17, methods can follow arrow 1202 to step 1207, comprising disposing the precursor solution on a foldable substrate 201. In aspects, step 1207 of this second set of methods can comprise one or more of the aspects discussed above for step 1207 with reference to the first set of methods. In aspects, step 1207 of this second set of methods can be identical to step 1207 discussed above with reference to the first set of methods.
[0175] After step 1207, as shown in FIG. 17, methods can proceed to step 1209 comprising curing the precursor solution to form a polymer-based portion. In aspects, step 1209 of this second set of methods can comprise one or more of the aspects discussed above for step 1209 with reference to the first set of methods. In aspects, step 1209 of this second set of methods can be identical to step 1209 discussed above with reference to the first set of methods. At the end of step 1209, the polymer-based portion can comprise any one or more of the aspects discussed above for the polymer-based portion. For example, the polymer-based portion can be an acrylate-based polymer with a glass-transition temperature (Tg) of about -20°C or less, a storage modulus (E’) at 25°C from about 0.1 MegaPascals to about 1 MegaPascals, a refractive index from about 1.47 to about 1.51.
[0176] In aspects, after step 1209, as shown in FIGS. 17-18, methods can proceed to step 1211 comprising assembling a foldable apparatus, which can include one or more of the aspects discussed above with reference to step 1211 of the first set of methods and / or be identical to step 1211 discussed above. After step 1209 or 1211, methods can proceed to step 1213, where methods of making the polymer-based portion (or foldable substrate and / or the foldable apparatus) can be complete. Inaspects, methods can proceed along steps 1201, 1207, 1209, 1211, and 1213 of the flow chart in FIG. 12 sequentially, as discussed above. In aspects, methods can follow arrow 1206 from step 1209 to step 1213, for example, if methods are complete at the end of step 1209. Any of the above options may be combined to make a polymer-based portion (or a foldable apparatus) in accordance with the embodiments of the disclosure.
[0177] Aspects will now be described more fully hereinafter with reference to the accompanying drawings in which example aspects are shown. Whenever possible, the same reference numerals are used throughout the drawings to refer to the same or like parts. FIGS. 1-4, 7, and 9 illustrate views of foldable apparatus 101, 301, 401, 701, and 901 comprising a foldable substrate 201 in accordance with aspects of the disclosure. Unless otherwise noted, a discussion of features of aspects of one foldable apparatus can apply equally to corresponding features of any aspects of the disclosure. For example, identical part numbers throughout the disclosure can indicate that, in some aspects, the identified features are identical to one another and that the discussion of the identified feature of one aspect, unless otherwise noted, can apply equally to the identified feature of any of the other aspects of the disclosure.
[0178] FIGS. 2-4 schematically illustrate example aspects of foldable apparatus 101, 301, and 401 comprising the foldable substrate 201 in accordance with aspects of the disclosure in an unfolded (e.g., flat) configuration while FIGS.7 and 9 illustrate example aspects of a foldable apparatus 701 and 901 comprising the foldable substrate 201 in accordance with aspects of the disclosure in a folded configuration. The foldable apparatus 101, 301, and 401 and the foldable substrate 201 comprise a first portion 221, a second portion 231, and a central portion 281 positioned between the first portion 221 and the second portion 231. In aspects, as shown in FIGS. 2 and 4, the foldable apparatus 101 and 401 can comprise a device substrate or release liner 271 although other substrates (e.g., cover substrate 371, a glass-based substrate and / or a ceramic-based substrate discussed throughout the application) or coatings (e.g., coating 251) may be used in further aspects rather than with the illustrated device substrate or release liner 271. In aspects, as shown in FIG. 3, the foldable apparatus 301 can comprise a cover substrate 371. In aspects, as shown in FIG. 2 and 7, the foldable apparatus 101 and 701 can comprise a coating 251. In aspects, as shown in FIGS. 2-3, the foldable apparatus 101 and 301 can comprise an adhesive layer 261. In aspects, as shown in FIGS. 2-4, 7, and 9, foldable apparatus101, 301, 401, 701, and 901 comprise a polymer-based portion 289 and / or 299. As shown in FIGS. 2-4, the foldable substrate 201 can comprise a first recess 211. In aspects, as shown in FIGS. 2-3, the foldable substrate 201 can further comprise a second recess 241. It is to be understood that any of the foldable apparatus of the disclosure can comprise a second substrate (e.g., a glass-based substrate and / or a ceramic-based substrate), a device substrate or release liner 271, a cover substrate 371, a display device, a coating 251, an adhesive layer 261, and / or a polymer-based portion 289 and / or 299.
[0179] Throughout the disclosure, with reference to FIG. 1, the width 103 of the foldable apparatus 101, 301, 401, 501, 701, and / or 901 is considered the dimension of the foldable apparatus taken between opposed edges of the foldable apparatus in a direction 104 of a fold axis 102 of the foldable apparatus, wherein the direction 104 also comprises the direction of the width 103. Furthermore, throughout the disclosure, the length 105 of the foldable apparatus is considered the dimension of the foldable apparatus taken between opposed edges of the foldable apparatus in a direction 106 perpendicular to the fold axis 102 of the foldable apparatus. It is to be understood that the direction 104 of the width 103 and / or the direction 106 of the length 105 can correspond to corresponding directions in the foldable substrate 201. In aspects, as shown in FIGS. 1-2, the foldable apparatus of any aspects of the disclosure can comprise a fold plane 109 that includes the fold axis 102 when the foldable apparatus is in the flat configuration (see FIG. 2). In further aspects, as shown in FIG. 2, the fold plane 109 can extend along the fold axis 102 and in a direction of the substrate thickness 207 when the foldable apparatus is in the flat configuration (see FIG.2). The fold plane 109 may comprise a central axis 107 of the foldable apparatus. In aspects, the foldable apparatus can be folded in a direction 111 (see FIG.1) about the fold axis 102 extending in the direction 104 of the width 103 to form a folded configuration (see FIGS.5, 7, and 9). As shown, the foldable apparatus and / or the foldable substrate may include a single fold axis to allow the foldable apparatus and / or the foldable substrate to comprise a bifold wherein, for example, the foldable apparatus and / or the foldable substrate may be folded in half. In further aspects, the foldable apparatus and / or the foldable substrate may include two or more fold axes with each fold axis including a corresponding central portion similar or identical to the central portion 281 discussed herein. For example, providing two fold axes can allow the foldable apparatus and / or the foldable substrate to comprise atrifold wherein, for example, the foldable apparatus and / or the foldable substrate may be folded with the first portion 221, the second portion 231, and a third portion similar or identical to the first portion or second portion with the central portion 281 and another central portion similar to or identical to the central portion positioned between the first portion and the second portion and between the second portion and the third portion, respectively.
[0180] The foldable substrate 201 can comprise a glass-based substrate and / or a ceramic-based substrate having a pencil hardness of 8H or more, for example, 9H or more. As used herein, pencil hardness is measured using ASTM D3363-20 with standard lead graded pencils. Providing a glass-based foldable substrate and / or a ceramic-based foldable substrate can enhance puncture resistance and / or impact resistance. Throughout the disclosure, an elastic modulus (e.g., Young’s modulus) is measured using ISO 527-1:2019. In aspects, the foldable substrate 201 can comprise an elastic modulus in a range from about 10 GPa to about 150 GPa, from about 40 GPa to about 100 GPa, from about 60 GPa to about 80 GPa, or any range or subrange therebetween.
[0181] In aspects, the foldable substrate 201 can comprise a glass-based substrate. As used herein, “glass-based” includes both glasses and glass-ceramics, wherein glass-ceramics have one or more crystalline phases and an amorphous, residual glass phase. A glass-based material (e.g., glass-based substrate) may comprise an amorphous material (e.g., glass) and optionally one or more crystalline materials (e.g., ceramic). Amorphous materials and glass-based materials may be strengthened. As used herein, the term “strengthened” may refer to a material that has been chemically strengthened, for example, through ion exchange of larger ions for smaller ions in the surface of the substrate, as discussed below. However, other strengthening methods, for example, thermal tempering, or utilizing a mismatch of the coefficient of thermal expansion between portions of the substrate to create compressive stress and central tension regions, may be utilized to form strengthened substrates. Exemplary glass-based materials, which may be free of lithia or not, comprise soda lime glass, alkali aluminosilicate glass, alkali-containing borosilicate glass, alkali-containing aluminoborosilicate glass, alkali-containing phosphosilicate glass, and alkali-containing aluminophosphosilicate glass. In aspects, glass-based material can comprise an alkali-containing glass or an alkali-free glass, either of which may be free of lithia or not. In aspects, the glass material can be alkali-freeand / or comprise a low content of alkali metals (e.g., R2O of about 10 mol% or less, wherein R2O comprises Li2O Na2O, K2O, or the more expansive list provided below). In one or more aspects, a glass-based material may comprise, in mole percent (mol %): SiO2in a range from about 40 mol % to about 80%, Al2O3in a range from about 5 mol % to about 30 mol %, B2O3 in a range from 0 mol % to about 10 mol %, ZrO2 in a range from 0 mol% to about 5 mol %, P2O5 in a range from 0 mol % to about 15 mol %, TiO2in a range from 0 mol % to about 2 mol %, R2O in a range from 0 mol % to about 20 mol %, and RO in a range from 0 mol % to about 15 mol %. As used herein, R2O can refer to an alkali-metal oxide, for example, Li2O, Na2O, K2O, Rb2O, and Cs2O. As used herein, RO can refer to MgO, CaO, SrO, BaO, and ZnO. “Glass- ceramics” include materials produced through controlled crystallization of glass. In aspects, glass-ceramics have about 1% to about 99% crystallinity. Examples of suitable glass-ceramics may include Li2O-Al2O3-SiO2 system (i.e., LAS-System) glass-ceramics, MgO-Al2O3-SiO2system (i.e., MAS-System) glass-ceramics, ZnO × Al2O3 × nSiO2 (i.e., ZAS system), and / or glass-ceramics that include a predominant crystal phase including β-quartz solid solution, β-spodumene, cordierite, petalite, and / or lithium disilicate. The glass-ceramic substrates may be strengthened using the chemical strengthening processes. In one or more aspects, MAS-System glass- ceramic substrates may be strengthened in Li2SO4 molten salt, whereby an exchange of 2Li+for Mg2+can occur.
[0182] In aspects, the foldable substrate 201 can comprise a ceramic-based substrate. As used herein, “ceramic-based” includes both ceramics and glass- ceramics, wherein glass-ceramics have one or more crystalline phases and an amorphous, residual glass phase. Ceramic-based materials may be strengthened (e.g., chemically strengthened). In aspects, a ceramic-based material can be formed by heating a glass-based material to form ceramic (e.g., crystalline) portions. In further aspects, ceramic-based materials may comprise one or more nucleating agents that can facilitate the formation of crystalline phase(s). In aspects, ceramic-based materials can comprise one or more oxides, nitrides, oxynitrides, carbides, borides, and / or silicides. Example aspects of ceramic oxides include zirconia (ZrO2), zircon (ZrSiO4), titania (TiO2), hafnium oxide (Hf2O), yttrium oxide (Y2O3), iron oxides, beryllium oxides, vanadium oxide (VO2), fused quartz, cristobalite, mullite (a mineral comprising a combination of aluminum oxide and silicon dioxide), and spinel (MgAl2O4). Example aspects of ceramic nitrides include silicon nitride (Si3N4),aluminum nitride (AlN), gallium nitride (GaN), beryllium nitride (Be3N2), boron nitride (BN), tungsten nitride (WN), vanadium nitride, alkali earth metal nitrides (e.g., magnesium nitride (Mg3N2)), nickel nitride, and tantalum nitride. Example aspects of oxynitride ceramics include silicon oxynitride, aluminum oxynitride, and a SiAlON (a combination of alumina and silicon nitride and can have a chemical formula, for example, Si12-m-nAlm+nOnN16-n, Si6-nAlnOnN8-n, or Si2-nAlnO1+nN2-n, where m, n, and the resulting subscripts are all non-negative integers).
[0183] In aspects, the foldable substrate 201 can be optically transparent. As used herein, “optically transparent” or “optically clear” means an average transmittance of 70% or more in the wavelength range of 400 nm to 700 nm through a 1.0 mm thick piece of a material. In aspects, the foldable substrate 201 may have an average transmittance of 75% or more, 80% or more, 85% or more, or 90% or more, 92% or more, 94% or more, 96% or more in the wavelength range of 400 nm to 700 nm through a 1.0 mm thick piece of the material. The average transmittance in the wavelength range of 400 nm to 700 nm is calculated by measuring the transmittance of whole number wavelengths from about 400 nm to about 700 nm and averaging the measurements.
[0184] As shown in FIGS. 2-4, the foldable apparatus 101, 301, and 401 comprise the foldable substrate 201 comprising a first major surface 203 and a second major surface 205 opposite the first major surface 203. As shown in FIGS. 2-4, the first major surface 203 can extend along a first plane 204a. The second major surface 205 can extend along a second plane 206a. In aspects, as shown, the second plane 206a can be parallel to the first plane 204a. As used herein, a substrate thickness 207 can be defined between the first major surface 203 and the second major surface 205 as a distance between the first plane 204a and the second plane 206a. In aspects, the substrate thickness 207 can be about 10 micrometers (µm) or more, about 25 µm or more, about 50 µm or more, about 70 µm or more, about 80 µm or more, about 90 µm or more, about 100 µm or more, about 125 µm or more, about 150 µm or more, about 200 µm or more, about 300 µm or more, about 2 millimeters (mm) or less, about 1 mm or less, about 800 µm or less, about 500 µm or less, about 300 µm or less, about 200 µm or less, about 180 µm or less, or about 160 µm or less. In aspects, the substrate thickness 207 can range from about 10 µm to about 2 mm, from about 25 µm to about 2 mm, from about 50 µm to about 2 mm, from about 70 µm to about 2 mm, from about 70 µm to about 1 mm, from about 70 µm to about 800 µm, fromabout 80 µm to about 500 µm, from about 90 µm 500 µm, from about 100 µm to about 200 µm, from about 125 µm to about 200 µm, from about 150 µm to about 200 µm, or any range or subrange therebetween.
[0185] As shown in FIGS.2-4, the first portion 221 of the foldable substrate 201 can comprise a first surface area 223 and a second surface area 225 opposite the first surface area 223. The first portion 221 will now be described with reference to the foldable apparatus 101 of FIG. 2 with the understanding that such description of the first portion 221, unless otherwise stated, can also apply to any aspects of the disclosure, for example, the foldable apparatus 301, 401, 701, and / or 901 illustrated in FIGS.3-4, 7, and 9. In aspects, as shown, the first surface area 223 can comprise a planar surface, and / or the second surface area 225 of the first portion 221 can comprise a planar surface. In further aspects, as shown, the second surface area 225 can be parallel to the first surface area 223. In aspects, as shown, the first major surface 203 can comprise the first surface area 223 and the second major surface 205 can comprise the second surface area 225. In further aspects, the first surface area 223 can extend along the first plane 204a. In further aspects, the second surface area 225 can extend along the second plane 206a. In aspects, the substrate thickness 207 can correspond to the distance between the first surface area 223 of the first portion 221 and the second surface area 225 of the first portion 221. In aspects, the substrate thickness 207 can be substantially uniform across the first surface area 223. In aspects, a first thickness defined between the first surface area 223 and the second surface area 225 can be within one or more of the ranges discussed above with regards to the substrate thickness 207. In further aspects, the first thickness can comprise the substrate thickness 207. In further aspects, the first thickness of the first portion 221 may be substantially uniform between the first surface area 223 and the second surface area 225 across its corresponding length (i.e., in the direction 106 of the length 105 of the foldable apparatus) and / or its corresponding width (i.e., in the direction 104 of the width 103 of the foldable apparatus).
[0186] As shown in FIGS. 2-4, the second portion 231 of the foldable substrate 201 can comprise a third surface area 233 and a fourth surface area 235 opposite the third surface area 233. The second portion 231 will now be described with reference to the foldable apparatus 101 of FIG. 2 with the understanding that such description of the second portion 231, unless otherwise stated, can also apply to any aspects of the disclosure, for example, the foldable apparatus 301, 401, 701,and / or 901 illustrated in FIGS. 3-4, 7, and 9. In aspects, as shown, the third surface area 233 of the second portion 231 can comprise a planar surface, and / or the fourth surface area 235 of the second portion 231 can comprise a planar surface. In further aspects, the third surface area 233 of the second portion 231 can be in a common plane with the first surface area 223 of the first portion 221. In further aspects, as shown, the fourth surface area 235 can be parallel to the third surface area 233. In further aspects, the fourth surface area 235 of the second portion 231 can be in a common plane with the second surface area 225 of the first portion 221. A second thickness can be defined between the third surface area 233 of the second portion 231 and the fourth surface area 235 of the second portion 231. In aspects, the second thickness can be within the range discussed above with regards to the substrate thickness 207. In further aspects, the second thickness can comprise the substrate thickness 207 and / or be substantially equal to the substrate thickness 207 (e.g., first thickness). In aspects, the second thickness of the second portion 231 may be substantially uniform between the third surface area 233 and the fourth surface area 235.
[0187] As shown in FIGS. 2-4, the foldable substrate 201 can comprise a central portion 281 positioned between the first portion 221 and the second portion 231. The central portion 281 comprises a first central surface area 213 and a second central surface area 243 opposite the first central surface area 213. As shown, the first central surface area 213 can be positioned between the first surface area 223 and the third surface area 233. In further aspects, the first central surface area 213 can correspond to a central region 248 of the central portion 281. In further aspects, as shown, the first central surface area 213 can extend along a third plane 204b when the foldable apparatus 101, 301, and / or 401 is in a flat configuration. A first recess 211 can be defined between the first central surface area 213 (e.g., third plane 204b) and the first plane 204a.
[0188] In aspects, the third plane 204b can be substantially parallel to the first plane 204a and / or the second plane 206a. In further aspects, as shown in FIGS. 2-3, the first central surface area 213 can be recessed from the first major surface 203 by a first distance 219. In further aspects, the first distance 219 that the first central surface area 213 is recessed from the first plane 204a can be about 5 µm or more, about 10 µm or more, about 25 µm or more, about 40 µm or more, about 80 µm or more, about 100 µm or more, about 125 µm or more, about 150 µm or more, about 1mm or less, about 800 µm or less, about 500 µm or less, about 300 µm or less, about 200 µm or less, about 180 µm or less, or about 150 µm or less. In further aspects, the first distance 219 can range from about 5 µm to about 1 mm, from about 5 µm to about 500 µm, from about 10 µm to about 300 µm, from about 25 µm to about 200 µm, from about 40 µm to about 200 µm, from about 80 µm to about 200 µm, from about 100 µm to about 180 µm, from about 125 µm to about 150 µm, or any range or subrange therebetween. In further aspects, the first distance 219, as a percentage of the substrate thickness 207, can be about 1% or more, about 5% or more, about 10% or more, about 15% or more, about 20% or more, about 25% or more, about 75% or less, about 60% or less, about 50% or less, about 40% or less, about 35% or less, or about 30% or less. In further aspects, the first distance 219, as a percentage of the substrate thickness 207, can range from about 1% to about 75%, from about 1% to about 60%, from about 5% to about 60%, from about 10% to about 50%, from about 15% to about 45%, from about 20% to about 35%, from about 25% to about 30%, or any range or subrange therebetween.
[0189] As shown in FIGS. 2-4, the second central surface area 243 of the central portion 281 is positioned between the second surface area 225 and the fourth surface area 235. In aspects, as shown in FIGS. 2-3, the second central surface area 243 can extend along a fourth plane 206b when the foldable apparatus 101 and / or 301 is in a flat configuration. In further aspects, a second recess 241 is defined between the second central surface area 243 (e.g., fourth plane 206b) and the second plane 206a. As shown in FIG.4, the second central surface area 243 can extend along the second plane 206a.
[0190] In aspects, as shown in FIGS. 2-3, the second central surface area 243 can be recessed from the second major surface 205 by a second distance 249. In further aspects, the second distance 249 can be within one or more of the ranges discussed above for the first distance 219. In further aspects, the first distance can be greater than the second distance. In even further aspects, the second distance 249 that the second central surface area 243 is recessed from the second plane 206a, as a percentage of the substrate thickness 207, can be about 1% or more, about 2% or more, about 5% or more, about 10% or more, about 12% or more, about 30% or less, about 25% or less, about 20% or less, about 18% or less, or about 15% or less. In even further aspects, the second distance 249, as a percentage of the substrate thickness 207, can range from about 1% to about 30%, from about 2% to about 25%, fromabout 5% to about 20%, from about 10% to about 18%, from about 12% to about 15%, or any range or subrange therebetween. In further aspects, as shown in FIG. 2, the first distance 219 can be substantially equal to the second distance 249. Providing the first distance substantially equal to the second distance can further reduce the incidence of mechanical instabilities in the central portion, for example, because the foldable substrate is symmetric about a plane comprising a midpoint in the substrate thickness and the central thickness. In further aspects, as shown in FIG.4, the second central surface area 243 can be coplanar with the second surface area 225 and / or the fourth surface area 235, for example, forming a planar second major surface 205 extending along the second plane 206a.
[0191] A central thickness 209 can be defined between the first central surface area 213 and the second central surface area 243 as the distance between the third plane 204b and the fourth plane 206b. In aspects, the central thickness 209 can be about 10 µm or more, about 25 µm or more, about 40 µm or more, about 120 µm or less, about 100 µm or less, about 80 µm or less, about 60 µm or less, or about 50 µm or less. In aspects, the central thickness 209 can range from about 10 µm to about 120 µm, from about 10 µm to about 100 µm, from about 25 µm to about 80 µm, from about 40 µm to about 60 µm, or any range or subrange therebetween. In aspects, the central thickness 209 can be less than the substrate thickness 207 by about 10 µm or more, about 20 µm or more, about 30 µm or more, about 40 µm or more, about 50 µm or more, or about 60 µm or more. In aspects, the central thickness 209 as a percentage of the substrate thickness 207 can be about 0.5% or more, about 1% or more, about 2% or more, about 5% or more, about 40% or less, about 30% or less, about 20% or less, about 13% or less, about 10% or less, or about 8% or less. In aspects, the central thickness 209 as a percentage of the substrate thickness 207 can range from about 0.5% to about 40%, from about 0.5% to about 20%, from about 1% to about 13%, from about 2% to about 10%, from about 5% to about 8%, or any range or subrange therebetween. In aspects, the central region 248 of the central portion 281 can correspond to a region comprising the central thickness 209. By providing the first central surface area 213 of the central portion 281 extending along the third plane 204b parallel to the second central surface area 243 of the central portion 281 extending along the fourth plane 206b, a uniform central thickness 209 may extend across the central portion 281 that can provide enhanced folding performance at a predetermined thickness for the central thickness 209. A uniform central thickness209 across the central portion 281 can improve folding performance by preventing stress concentrations that would occur if a portion of the central portion 281 was thinner than the rest of the central portion 281.
[0192] In aspects, as shown in FIGS. 2-4, the central portion 281 of the foldable substrate 201 can comprise a first transition region 212 comprising a first transition surface area 215 extending between the first surface area 223 and the first central surface area 213. In further aspects, as shown, a width (e.g., first transition width 214) of the first transition region 212 corresponding to the minimum distance in a direction 106 of the length 105 (see FIG. 1) between a portion of the first central surface area 213 extending along the third plane 204b and a portion of the first surface area 223. In even further aspects, the first transition width 214 of the first transition region 212 can be about 0.15 mm or more, about 0.3 mm or more, about 0.5 mm or more, about 0.6 mm or more, about 0.7 mm or more, about 0.8 mm or more, about 2 mm or less, about 1.8 mm or less, about 1.5 mm or less, about 1.2 mm or less, about 1 mm or less, about 0.8 mm or less, about 0.7 mm or less, or about 0.5 mm or less. In even further aspects, the first transition width 214 of the first transition region 212 can range from about 0.15 mm to about 2 mm, from about 0.3 mm to about 2 mm, from about 0.5 mm to about 1.8 mm, from about 0.6 mm to about 1.5 mm, from about 0.7 mm to about 1.2 mm, from about 0.8 mm to about 1 mm, or any range or subrange therebetween. In aspects, as shown in FIGS. 2-3, the first transition region 212 can comprise a second transition surface area 245 extending between the second surface area 225 and the second central surface area 243. A width of the second transition surface area 245 corresponding to the minimum distance in a direction 106 of the length 105 (see FIG. 1) between a portion of the second central surface area 243 extending along the fourth plane 206b and a portion of the second surface area 225 can be within one or more of the ranges discussed above for the first transition width 214 and / or substantially equal to the first transition width 214.
[0193] In aspects, as shown in FIGS. 2-4, a thickness of the first transition region 212 can decrease between the substrate thickness 207 of the first portion 221 and the central thickness 209 of the central portion 281. In further aspects, as shown, a thickness of the first transition region 212 can smoothly decrease, monotonically decrease, and / or smoothly and monotonically decrease between the substrate thickness 207 of the first portion 221 and the central thickness 209 of the central portion 281. As used herein, a thickness decreases smoothly if changes in the cross-sectional area are smooth (e.g., gradual) rather than abrupt (e.g., step) changes in thickness. As used herein, a thickness decreases monotonically in a direction if the thickness decreases for a portion and for the rest of the time either stays the same, decreases, or a combination thereof (i.e., the thickness decreases but never increases in the direction). A smooth shape of the first transition region and / or the second transition region can reduce optical distortions.
[0194] In aspects, as shown in FIGS. 2-4, the first transition surface area 215 can comprise a linearly inclined surface extending between the first central surface area 213 and the first surface area 223. In aspects, although not shown, the first transition surface area can comprise a concave up shape, for example, with a local slope of the first transition surface area smoothly transitioning to a slope of the first central surface area 213 while a local slope of the first transition surface area is substantially different from a slope of the first surface area 223. In aspects, although not shown, the first transition surface area can comprise a sigmoid shape. In aspects, although not shown, a local slope of the first transition surface area can be greater at a midpoint of the first transition surface area than where the first transition surface area meets the first central surface area 213 and where the first transition surface area meets the first surface area 223. In aspects, although not shown, the first transition surface area can comprise a convex up shape, for example, with a local slope of the first transition surface area smoothly transitioning to a slope of the first surface area 223 while a local slope of the first transition surface area is substantially different from a slope of the first central surface area 213. In aspects, the second transition surface area can comprise one of the shapes or properties discussed above in this paragraph for the first transition surface area. For example, as shown in FIG. 2, the second transition surface area 245 can comprise a linearly inclined surface extending between the second central surface area 243 and the second surface area 225.
[0195] In aspects, as shown in FIGS. 2-4, a thickness of the first transition region 212 can decrease at a constant rate (e.g., linearly change) from the substrate thickness 207 to the central thickness 209. In aspects, although not shown, a thickness of the first transition region can decrease slower where the first transition surface area meets the first central surface area 213 than at a midpoint of the first transition region and / or than where the first transition surface area meets the first surface area 223 (e.g., first portion 221). In aspects, although not shown, a thickness of the first transition region can decrease faster where the first transition surface area meets thefirst central surface area 213 than at a midpoint of the first transition region and / or than where the first transition surface area meets the first surface area 223. Providing a non-uniform slope of a surface area of the first transition region and / or the second transition region can reduce an amount of the corresponding transition region comprising intermediate thicknesses, for example, comprising a chemical strengthening induced expansion strain less than a portion of the corresponding transition region closer to the first central surface area and / or the second central surface area and / or than the first central surface area and / or the second central surface area.
[0196] Throughout the disclosure, an average angle of a transition surface area relative to a central surface area is measured as an angle between a transition surface area and a central surface area. An angle is calculated for a location on the corresponding transition surface area relative to the corresponding central surface area with the location of the corresponding central surface area approximated as a plane fitted from measurements at 20 locations evenly spaced over the corresponding central surface area in the direction 106 of the length 105. The angle measured is an external angle for the foldable substrate, meaning that it extends from the plane fitted to the corresponding central surface area to the location on the corresponding transition surface area without passing through the material of the foldable substrate other than an incidental amount at the endpoints. The average angle is calculated from 10 locations on the corresponding transition surface area that are located in a region comprising 80% of a distance that the corresponding central surface area is recessed from the corresponding major surface with the region centered at the midpoint between the corresponding central surface area and the corresponding major surface in the direction 202 of the thickness (e.g., substrate thickness 207, central thickness 209). In aspects, as shown in FIGS. 2-4, the first transition surface area 215 of the first transition region 212 extends between the first surface area 223 and the first central surface area 213 with a first average angle 282 relative to the first central surface area 213. As described above, the first average angle 282 is an external angle because it does not pass through the material of the foldable substrate 201 other than an incidental amount at the endpoints. In further aspects, the first average angle 282 can be about 160° or more, about 162° or more, about 165° or more, about 167° or more, about 170° or more, about 171° or more, about 172° or more, about 179° or less, about 176° or less, about 175° or less, about 174° or less, or about 173° or less.In further aspects, the first average angle 282 can range from about 160° to about 179°, from about 162° to about 176°, from about 165° to about 176°, from about 167° to about 175°, from about 170° to about 175°, from about 171° to about 174°, from about 172° to about 173°, or any range or subrange therebetween. For example, a first transition surface comprising a linear (e.g., planar) surface area with a first transition width of 500 µm and height (i.e., a difference between the first central surface area 213 and the first major surface 203 corresponding to the first distance 219) of 30 µm corresponds to a first average angle of about 176.6°.
[0197] In aspects, as shown in FIGS. 2-4, the third transition surface area 217 of the second transition region 218 extends between the third surface area 233 and the first central surface area 213 with a third average angle 286 relative to the first central surface area 213. In further aspects, the third average angle 286 can be within one or more of the ranges discussed above for the first average angle 282. In further aspects, the first average angle 282 can be substantially equal to the third average angle 286.
[0198] In aspects, as shown in FIGS. 2-4, the central portion 281 of the foldable substrate 201 can comprise a second transition region 218 comprising a third transition surface area 217 extending between the third surface area 233 and the first central surface area 213. In further aspects, as shown, a width (e.g., second transition width 216) of the second transition region 218 can be measured as the minimum distance in a direction 106 of the length 105 (see FIG. 1) between a portion of the first central surface area 213 extending along the third plane 204b and a portion of the third surface area 233. In even further aspects, the second transition width 216 of the second transition region 218 can be within one or more of the ranges discussed above for the first transition width 214. In still further aspects, the second transition width 216 of the second transition region 218 can be substantially equal to (e.g., equal to) the first transition width 214.
[0199] In aspects, as shown in FIGS. 2-3, the second transition region 218 can comprise a fourth transition surface area 247 extending between the fourth surface area 235 and the second central surface area 243. In further aspects, a width of the fourth transition surface area 247 can be measured as the minimum distance in a direction 106 of the length 105 (see FIG. 1) between a portion of the second central surface area 243 extending along the fourth plane 206b and a portion of the fourth surface area 235. In even further aspects, the width of the fourth transition surfacearea 247 can be substantially equal to (e.g., equal to) the second transition width 216. In aspects, as shown in FIGS.2-3, a thickness of the second transition region 218 can decrease between the substrate thickness 207 of the second portion 231 and the central thickness 209 of the central portion 281. In further aspects, as shown, a thickness of the first transition region 212 can smoothly decrease, monotonically decrease, or smoothly and monotonically decrease between the substrate thickness 207 of the second portion 231 and the central thickness 209 of the central portion 281. In aspects, as shown in FIG. 4, the portion of the second transition region 218 extending between the fourth surface area 235 and the second central surface area 243 can be coplanar with one or both surface areas.
[0200] In aspects, as shown in FIGS. 2-4, the third transition surface area 217 can comprise a linearly inclined surface extending between the first central surface area 213 and the third surface area 233. In aspects, the third transition surface area 217 and / or the fourth transition surface area 247 can comprise one of the shapes or properties discussed above with reference to the first transition surface area. In aspects, the fourth transition surface area 247 can comprise one of the shapes or properties discussed above in this paragraph for the first transition surface area. For example, as shown in FIGS.2-4, the fourth transition surface area 247 can comprise a linearly inclined surface extending between the second central surface area 243 and the fourth surface area 235. In aspects, as shown in FIGS. 2-4, a thickness of the second transition region 218 can decrease at a constant rate (e.g., linearly change) from the substrate thickness 207 to the central thickness 209. In aspects, although not shown, a thickness of the second transition region can decrease slower where the third transition surface area meets the first central surface area 213 than at a midpoint of the second transition region and / or than where the third transition surface area meets the third surface area 233 (e.g., first portion 221). In aspects, although not shown, a thickness of the second transition region can decrease faster where the third transition surface area meets the first central surface area 213 than at a midpoint of the second transition region and / or than where the third transition surface area meets the third surface area 233.
[0201] In aspects, as shown in FIGS. 2-3, the second transition surface area 245 of the first transition region 212 extends between the second surface area 225 and the second central surface area 243 with a second average angle 284 relative to the second central surface area 243. In further aspects, the second average angle 284 canbe within one or more of the ranges discussed above for the first average angle 282 and / or substantially equal to the first average angle 282. Providing an average angle within one of the above-mentioned ranges can provide reduced visibility of the transition region. In aspects, as shown in FIGS.2-3, the fourth transition surface area 247 of the second transition region 218 extends between the fourth surface area 235 and the second central surface area 243 with a fourth average angle 288 relative to the second central surface area 243. In further aspects, the fourth average angle 288 can be within one or more of the ranges discussed above for the second average angle 284. In further aspects, the second average angle 284 can be substantially equal to the fourth average angle 288. In further aspects, the first average angle 282 and / or the third average angle 286 can be substantially equal to the fourth average angle 288.
[0202] As used herein, if a first layer and / or component is described as “disposed over” a second layer and / or component, other layers may or may not be present between the first layer and / or component and the second layer and / or component. Furthermore, as used herein, “disposed over” does not refer to a relative position with reference to gravity. For example, a first layer and / or component can be considered “disposed over” a second layer and / or component, for example, when the first layer and / or component is positioned underneath, above, or to one side of a second layer and / or component. As used herein, a first layer and / or component described as “bonded to” a second layer and / or component means that the layers and / or components are bonded to each other, either by direct contact and / or bonding between the two layers and / or components or via an adhesive layer. As used herein, a first layer and / or component described as “contacting” or “in contact with” a second layer and / or components refers to direct contact and includes the situations where the layers and / or components are bonded to each other.
[0203] As shown in FIGS. 2-3, the foldable apparatus 101 can comprise an adhesive layer 261. As shown, the adhesive layer 261 can comprise a first contact surface 263 and a second contact surface 265 that can be opposite the first contact surface 263. In aspects, as shown in FIGS.2-3, the second contact surface 265 of the adhesive layer 261 can comprise a planar surface. In aspects, as shown in FIGS. 2-3, the first contact surface 263 of the adhesive layer 261 can comprise a planar surface. An adhesive thickness 267 of the adhesive layer 261 can be defined as a minimum distance between the first contact surface 263 and the second contact surface 265. In aspects, the adhesive thickness 267 of the adhesive layer 261 can be about 1 µm ormore, about 5 µm or more, about 10 µm or more, about 100 µm or less, about 60 µm or less, about 30 µm or less, or about 20 µm or less. In aspects, the adhesive thickness 267 of the adhesive layer 261 can range from about 1 µm to about 100 µm, from about 5 µm to about 60 µm, from about 10 µm to about 30 µm, from about 10 µm to about 20 µm, or any range or subrange therebetween.
[0204] In aspects, as shown in FIGS.2-3, the second contact surface 265 of the adhesive layer 261 can face and / or contact the first major surface 273 of a device substrate or release liner 271 (described below). In aspects, as shown, the first contact surface 263 of the adhesive layer 261 can face and / or contact the second surface area 225 of the first portion 221. In aspects, as shown, the first contact surface 263 of the adhesive layer 261 can face and / or contact the fourth surface area 235 of the second portion 231. In aspects, as shown in FIG. 2, the first contact surface 263 of the adhesive layer 261 can face the second central surface area 243 of the central portion 281. In aspects, as shown in FIG.2, the first contact surface 263 of the adhesive layer 261 can face the second central surface area 243 of the central portion 281. In further aspects, although not shown, the first contact surface 263 of the adhesive layer 261 can contact the second central surface area 243 of the central portion 281, for example by filling the region (e.g., second recess 241) indicated as occupied by the second polymer-based portion 299 in FIG. 2. In aspects, although not shown, the second recess may not be totally filled, for example, to leave room for electronic devices and / or mechanical devices. In aspects, although not shown, the foldable substrate 201 of FIG. 4 can be configured with the adhesive layer 261 contacting the second major surface 205 rather than the first major surface 203 while the second polymer-based portion 299 or a coating 251 in place of the second polymer-based portion 299 can be positioned at least partially in the first recess 211.
[0205] In aspects, the adhesive layer 261 can comprise one or more of a polyolefin, a polyamide, a halide-containing polymer (e.g., polyvinylchloride or a fluorine-containing polymer), an elastomer, a urethane, phenolic resin, parylene, polyethylene terephthalate (PET), and polyether ether ketone (PEEK). Example aspects of polyolefins include low molecular weight polyethylene (LDPE), high molecular weight polyethylene (HDPE), ultrahigh molecular weight polyethylene (UHMWPE), and polypropylene (PP). Example aspects of fluorine-containing polymers include polytetrafluoroethylene (PTFE), polyvinylfluoride (PVF), polyvinylidene fluoride (PVDF), perfluoropolyether (PFPE), perfluorosulfonic acid(PFSA), a perfluoroalkoxy (PFA), fluorinated ethylene propylene (FEP) polymers, and ethylene tetrafluoro ethylene (ETFE) polymers. Example aspects of elastomers include rubbers (e.g., polybutadiene, polyisoprene, chloroprene rubber, butyl rubber, nitrile rubber) and block copolymers (e.g., styrene-butadiene, high-impact polystyrene, poly(dichlorophosphazene)). In further aspects, the adhesive layer 261 can comprise an optically clear adhesive. In even further aspects, the optically clear adhesive can comprise one or more optically transparent polymers: an acrylic (e.g., polymethylmethacrylate (PMMA)), an epoxy, silicone, and / or a polyurethane. Examples of epoxies include bisphenol-based epoxy resins, novolac-based epoxies, cycloaliphatic-based epoxies, and glycidylamine-based epoxies. In even further aspects, the optically clear adhesive can comprise, but is not limited to, acrylic adhesives, for example, 3M 8212 adhesive, or an optically transparent liquid adhesive, for example, a LOCTITE optically transparent liquid adhesive. Exemplary aspects of optically clear adhesives comprise transparent acrylics, epoxies, silicones, and polyurethanes. For example, the optically transparent liquid adhesive could comprise one or more of LOCTITE AD 8650, LOCTITE AA 3922, LOCTITE EA E- 05MR, LOCTITE UK U-09LV, which are all available from Henkel.
[0206] Throughout the disclosure, a tensile strength, ultimate elongation (e.g., strain at failure), and yield point of a polymeric material (e.g., adhesive, polymer-based portion) is determined using ASTM D638 using a tensile testing machine, for example, an Instron 3400 or Instron 6800, at 23°C and 50% relative humidity with a type I dogbone shaped sample. In aspects, the adhesive layer 261 can comprise an elastic modulus of about 0.001 MegaPascals (MPa) or more, about 0.01 MPa or more, about 0.1 MPa or more, about 0.5 MPa or more, about 50 MPa or less, about 20 MPa or less, about 10 MPa or less, about 5 MPa or less, about 1 MPa or less, about 0.5 MPa or less, about 0.1 MPa or less, or about 0.05 MPa or less. In aspects, the adhesive layer 261 can comprise an elastic modulus in a range from about 0.001 MPa to about 50 MPa, from about 0.001 MPa to about 20 MPa, from about 0.01 MPa to about 10 MPa, from about 0.1 MPa to about 5 MPa, from about 0.5 MPa to about 1 MPa, or any range or subrange therebetween.
[0207] As shown in FIGS. 2-4, at least a portion of the polymer-based portion 289 and / or 299 of the foldable apparatus 101 can be positioned between the first portion 221 and the second portion 231. In aspects, as shown, the polymer-based portion can comprise a first polymer-based portion 289 at least partially positioned inand / or filling the first recess 211. In aspects, as shown in FIGS. 2-3, the polymer- based portion can comprise a second polymer-based portion 299 at least partially positioned in and / or filling the second recess 241. In aspects, as shown in FIG. 4, the polymer-based portion can comprise a second polymer-based portion 299 at least partially positioned in and / or filling the first recess 211. In aspects, although not shown, the second recess may not be totally filled, for example, to leave room for electronic devices and / or mechanical devices.
[0208] As shown in FIGS. 2-3, the first polymer-based portion 289 can comprise a second contact surface 285 opposite the first contact surface 283. In aspects, as shown, the first contact surface 283 can comprise a planar surface, for example, parallel to (FIGS. 2-3) and / or substantially coplanar (e.g., extend along a common plane, first plane 204a) (FIG.2) with the first surface area 223 and the third surface area 233. In aspects, as shown in FIG. 3, the first contact surface 283 can extend over (e.g., cover) at least a portion of the first major surface 203 (e.g., with a minimum thickness 367 of about 5 µm or more for the first polymer-based portion 289 over the first major surface 203). In aspects, as shown in FIG.2, the fourth major surface 255 of the coating 251 can face and / or contact the first contact surface 283 of the first polymer-based portion 289. In aspects, the second contact surface 285 can comprise a planar surface, for example, substantially coplanar (e.g., extend along a common plane, third plane 204b) with the first central surface area 213. In further aspects, the second contact surface 285 can contact the first central surface area 213, the first transition surface area 215, and / or the third transition surface area 217.
[0209] As shown in FIGS. 2-4, the second polymer-based portion 299 can comprise a fourth contact surface 295 opposite the third contact surface 293. In further aspects, as shown in FIGS. 2-3, the third contact surface 293 can contact the second central surface area 243, the second transition surface area 245, and / or the fourth transition surface area 247. In aspects, as shown in FIGS.2-3, the third contact surface 293 can comprise a planar surface, for example, being substantially coplanar (e.g., extend along a common plane with the fourth plane 206b) with the second central surface area 243. In aspects, as shown in FIGS.2-4, the fourth contact surface 295 can comprise a planar surface, for example, being parallel to (FIGS. 2-4) and / or substantially coplanar (e.g., extend along a common plane with the second plane 206a) (FIGS.2-3) with the second surface area 225 and the fourth surface area 235.
[0210] In aspects, as shown in FIG. 4, the third contact surface 293 can contact the first central surface area 213, the first transition surface area 215, and / or the third transition surface area 217. In aspects, as shown in FIG. 4, the third contact surface 293 can comprise a planar surface, for example, being substantially coplanar (e.g., extend along a common plane with the third plane 204b) with the first central surface area 213. In aspects, as shown, the third contact surface 293 can comprise a planar surface, for example, substantially coplanar (e.g., extend along a common plane with the third plane 204b) with the first central surface area 213. In aspects, as shown in FIG.4, the fourth contact surface 295 can be parallel to the first plane 204a that the first major surface 203 extends along. Although not shown in FIG. 4, as discussed above with reference to FIGS. 2-3, the fourth contact surface 295 can be substantially coplanar (e.g., extend along a common plane with the first plane 204a) with the first surface area 223 and the third surface area 233. In aspects, as shown in FIGS. 3-4, the first contact surface 263 of the adhesive layer 261 can face and / or contact the fourth contact surface 295 of the second polymer-based portion 299. In aspects, as shown in FIG. 4, the fourth contact surface 295 can extend over (e.g., cover) at least a portion of the first major surface 203 (e.g., with a minimum thickness 467 of about 5 µm or more for the second polymer-based portion 299 over the first major surface 203).
[0211] The polymer-based materials disclosed above for the first polymer- based portion 289 and / or the second polymer-based portion 299 can fulfil the functions of both a “fill polymer” and either a “pressure sensitive adhesive” or an “optical clear adhesive.” For example, the first polymer-based portion 289 including a portion positioned in the first recess 211 in addition to a portion with a minimum thickness 367 over the first major surface of 5 µm or more (e.g., extending beyond the first plane 204a) can occupy the space corresponding to the second polymer-based portion 299 and the adhesive layer 261.
[0212] The polymer-based portion 289 and / or 299 comprises a polymer (e.g., optically transparent polymer). In aspects, the first polymer-based portion 289 and / or the second polymer-based portion 299 can comprise one or more of the materials discussed above for the polymer-based portion 289 and / or 299 (e.g., acrylate-based polymers, for example, made from compositions within ranges R1- R13). In further aspects, the first polymer-based portion 289 can comprise one or more of the materials discussed above for the polymer-based portion 289 and / or 299while the second polymer-based portion 299 can comprise one or more of the materials discussed below in this paragraph. In further aspects, the second polymer- based portion 299 can comprise one or more of the materials discussed above for the polymer-based portion 289 and / or 299 while the first polymer-based portion 289 can comprise one or more of the materials discussed below in this paragraph. In further aspects, one of the first polymer-based portions (e.g., second polymer-based portion 299) can comprise one or more of an optically transparent: an acrylic (e.g., polymethylmethacrylate (PMMA)), an epoxy, a silicone, and / or a polyurethane. Examples of epoxies include bisphenol-based epoxy resins, novolac-based epoxies, cycloaliphatic-based epoxies, and glycidylamine-based epoxies. In further aspects, the polymer-based portion 289 and / or 299 comprise one or more of a polyolefin, a polyamide, a halide-containing polymer (e.g., polyvinylchloride or a fluorine- containing polymer), an elastomer, a urethane, phenolic resin, parylene, polyethylene terephthalate (PET), and polyether ether ketone (PEEK). Example aspects of elastomers include rubbers and block copolymers, for example, comprising one or more of polystyrene, polydichlorophosphazene, and poly(5-ethylidene-2-norbornene). In aspects, the polymer-based portion can comprise a sol-gel material. Example aspects of polyurethanes comprise thermoset polyurethanes, for example, Dispurez 102 available from Incorez and thermoplastic polyurethanes, for example, KrystalFlex PE505 available from Huntsman. In even further aspects, the second portion can comprise an ethylene acid copolymer. An exemplary aspect of an ethylene acid copolymer includes SURLYN available from Dow (e.g., Surlyn PC-2000, Surlyn 8940, Surlyn 8150). An additional exemplary aspect for the second portion comprises Eleglass w802-GL044 available from Axalta with from 1wt% to 2wt% cross-linker. In aspects, the polymer-based portion 289 and / or 299 can further comprise nanoparticles, for example, carbon black, carbon nanotubes, silica nanoparticles, or nanoparticles comprising a polymer. In aspects, the polymer-based portion can further comprise fibers to form a polymer-fiber composite.
[0213] In aspects, the polymer-based portion 289 and / or 299 can be within one or more of the ranges discussed above for the elastic modulus of the polymer- based portion 289 and / or 299. In aspects, the polymer-based portion 289 and / or 299 can comprise an elastic modulus of about 0.01 MegaPascals (MPa) or more, about 0.1 MPa or more, about 1 MPa or more, about 10 MPa or more, about 20 MPa or more, about 100 MPa or more, about 200 MPa or more, about 1,000 MPa or more, about5,000 MPa or less, about 3,000 MPa or less, about 1,000 MPa or less, about 800 MPa or less, about 500 MPa or less, or about 200 MPa or less. In aspects, the polymer- based portion 289 and / or 299 can comprise an elastic modulus in a range from about 0.01 MPa to about 5,000 MPa, from about 0.1 MPa to about 3,000 MPa, from about 1 MPa to about 1,000 MPa, from about 10 MPa to about 800 MPa, from about 20 MPa to about 500 MPa, from about 100 MPa to about 200 MPa, or any range or subrange therebetween. In aspects, the adhesive layer 261 comprises an elastic modulus greater than or less than the elastic modulus of the polymer-based portion 289 and / or 299.
[0214] In aspects, as shown in FIG. 3, the foldable apparatus 301 can comprise a cover substrate 371 disposed over the first major surface 203, the first central surface area 213, and / or the first polymer-based portion 289. In further aspects, the cover substrate 371 can comprise a glass-based material, a ceramic-based material, or a polymer-based material (e.g., PET, PMMA). The cover substrate 371 can comprise a cover thickness 377 defined between a fifth major surface 373 and a sixth major surface 375 opposite the fifth major surface 373, which can be within one or more of the ranges discussed above for the central thickness 209. In further aspects, an elastic modulus of the cover substrate 371 can be about 5 GPa or more, about 10 GPa or more, about 20 GPa or more, about 50 GPa or more, about 70 GPa or more, about 200 GPa or less, about 150 GPa or less, about 100 GPa or less, about 90 GPa or less, about 50 GPa or less, or about 20 GPa or less, for example, in a range from about 5 GPa to about 200 GPa, from about 10 GPa to about 150 GPa, from about 20 GPa to about 100 GPa, from about 50 GPa to about 90 GPa, or any range or subrange therebetween. In further aspects, as shown, the sixth major surface 375 can contact and / or be bonded to the first polymer-based portion 289, for example, if the first polymer-based portion 289 extends over (e.g., covers) the first major surface 203.
[0215] In aspects, as shown in FIG. 2, a coating 251 can be disposed over the first major surface 203 of the foldable substrate 201. In further aspects, the coating 251 can be disposed over the first portion 221, the second portion 231, and the central portion 281. In aspects, the coating 251 can comprise a third major surface 253 and a fourth major surface 255 opposite the third major surface 253. In further aspects, the coating 251 (e.g., fourth major surface 255) can contact the foldable substrate 201 (e.g., first major surface 203). In further aspects, although not shown, at least a part of the coating 251 can be positioned in the first recess 211. In even further aspects, the coating 251 can fill the first recess 211. In further aspects, although not shown, asecond adhesive layer can be positioned between the first major surface 203 and the coating 251. In further aspects, the coating 251 can comprise a coating thickness 257 defined between the third major surface 253 and the fourth major surface 255. In further aspects, the coating thickness 257 can be about 0.1 µm or more, about 1 µm or more, about 5 µm or more, about 10 µm or more, about 20 µm or more, about 25 µm or more, about 40 µm or more, about 80 µm or more, about 200 µm or less, about 100 µm or less, or about 50 µm or less, about 25 µm or less, about 20 µm or less, about 20 µm or less, about 15 µm or less, or about 10 µm or less. In aspects, the coating thickness 257 can range from about 0.1 µm to about 200 µm, from about 1 µm to about 100 µm, from about 10 µm to about 50 µm, from about 20 µm to about 50 µm, or any range or subrange therebetween.
[0216] In aspects, the coating 251 can comprise a polymeric hard coating. In further aspects, the polymeric hard coating can comprise one or more of an ethylene- acid copolymer, a polyurethane-based polymer, an acrylate resin, and a mercapto- ester resin. Example aspects of ethylene-acid copolymers include ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, and ethylene-acrylic- methacrylic acid terpolymers (e.g., Nucrel, manufactured by DuPont), ionomers of ethylene acid copolymers (e.g., Surlyn, manufactured by DuPont), and ethylene- acrylic acid copolymer amine dispersions (e.g., Aquacer, manufactured by BYK). Example aspects of polyurethane-based polymers include aqueous modified polyurethane dispersions (e.g., Eleglas®, manufactured by Axalta). Example aspects of acrylate resins that can be UV curable include acrylate resins (e.g., Uvekol® resin, manufactured by Allinex), cyanoacrylate adhesives (e.g., Permabond® UV620, manufactured by Krayden), and UV radical acrylic resins (e.g., Ultrabond windshield repair resin, for example, Ultrabond (45CPS)). Example aspects of mercapto-ester resins include mercapto-ester triallyl isocyanurates (e.g., Norland optical adhesive NOA 61). In further aspects, the polymeric hard coating can comprise ethylene- acrylic acid copolymers and ethylene-methacrylic acid copolymers, which may be ionomerized to form ionomer resins through neutralization of the carboxylic acid residue with typically alkali-metal ions, for example, sodium and potassium, and also zinc. Such ethylene-acrylic acid and ethylene-methacrylic acid ionomers may be dispersed in water and coated onto the substrate to form an ionomer coating. Alternatively, such acid copolymers may be neutralized with ammonia which, after coating and drying liberates the ammonia to reform the acid copolymer as the coating.By providing a coating comprising a polymeric coating, the foldable apparatus can comprise low energy fracture.
[0217] In aspects, the coating can comprise a polymeric hard coating comprising an optically transparent polymeric hard-coat layer. Suitable materials for an optically transparent polymeric hard-coat layer include but are not limited to a cured acrylate resin material, an inorganic-organic hybrid polymeric material, an aliphatic or aromatic hexafunctional urethane acrylate, a siloxane-based hybrid material, and a nanocomposite material, for example, an epoxy and urethane material with nanosilicate. In aspects, an optically transparent polymeric hard-coat layer may consist essentially of one or more of these materials. In aspects, an optically transparent polymeric hard-coat layer may consist of one or more of these materials. As used herein, “inorganic-organic hybrid polymeric material” means a polymeric material comprising monomers with inorganic and organic components. An inorganic-organic hybrid polymer is obtained by a polymerization reaction between monomers having an inorganic group and an organic group. An inorganic-organic hybrid polymer is not a nanocomposite material comprising separate inorganic and organic constituents or phases, for example, inorganic particulates dispersed within an organic matrix. More specifically, suitable materials for an optically transparent polymeric (OTP) hard-coat layer include, but are not limited to, a polyimide, a polyethylene terephthalate (PET), a polycarbonate (PC), a poly methyl methacrylate (PMMA), organic polymer materials, inorganic-organic hybrid polymeric materials, and aliphatic or aromatic hexafunctional urethane acrylates. In aspects, an OTP hard- coat layer may consist essentially of an organic polymer material, an inorganic- organic hybrid polymeric material, or aliphatic or aromatic hexafunctional urethane acrylate. In aspects, an OTP hard-coat layer may consist of a polyimide, an organic polymer material, an inorganic-organic hybrid polymeric material, or aliphatic or aromatic hexafunctional urethane acrylate. In aspects, an OTP hard-coat layer may include a nanocomposite material. In aspects, an OTP hard-coat layer may include a nano-silicate at least one of epoxy and urethane materials. Suitable compositions for such an OTP hard-coat layer are described in U.S. Pat. Pub. No.2015 / 0110990, which is hereby incorporated by reference in its entirety by reference thereto. As used herein, “organic polymer material” means a polymeric material comprising monomers with only organic components. In aspects, an OTP hard-coat layer may comprise an organic polymer material manufactured by Gunze Limited and having a hardness of9H, for example Gunze’s “Highly Durable Transparent Film.” As used herein, “inorganic-organic hybrid polymeric material” means a polymeric material comprising monomers with inorganic and organic components. An inorganic-organic hybrid polymer is obtained by a polymerization reaction between monomers having an inorganic group and an organic group. An inorganic-organic hybrid polymer is not a nanocomposite material comprising separate inorganic and organic constituents or phases, for example, inorganic particulates dispersed within an organic matrix. In aspects, the inorganic-organic hybrid polymeric material may include polymerized monomers comprising an inorganic silicon-based group, for example, a silsesquioxane polymer. A silsesquioxane polymer may be, for example, an alkyl- silsesquioxane, an aryl-silsesquioxane, or an aryl alkyl-silsesquioxane having the following chemical structure: (RSiO1.5)n, where R is an organic group for example, but not limited to, methyl or phenyl. In aspects, an OTP hard-coat layer may comprise a silsesquioxane polymer combined with an organic matrix, for example, SILPLUS manufactured by Nippon Steel Chemical Co., Ltd. In aspects, an OTP hard-coat layer may comprise 90 wt% to 95 wt% aromatic hexafunctional urethane acrylate (e.g., PU662NT (Aromatic hexafunctional urethane acrylate) manufactured by Miwon Specialty Chemical Co.) and 10 wt% to 5 wt% photoinitiator (e.g., Darocur 1173 manufactured by BASF) with a hardness of 8H or more. In aspects, an OTP hard-coat layer composed of an aliphatic or aromatic hexafunctional urethane acrylate may be formed as a stand-alone layer by spin-coating the layer on a polyethylene terephthalate (PET) substrate, curing the urethane acrylate, and removing the urethane acrylate layer from the PET substrate. In aspects, an OTP hard-coat layer may be an aliphatic or aromatic hexafunctional urethane acrylate material layer having a thickness within one or more of the thickness ranges discussed above for the coating thickness 257.
[0218] In aspects, the coating 251, if provided, may also comprise one or more of an easy-to-clean coating, a low-friction coating, an oleophobic coating, a diamond-like coating, a scratch-resistant coating, or an abrasion-resistant coating. A scratch-resistant coating may comprise an oxynitride, for example, aluminum oxynitride or silicon oxynitride with a thickness of about 500 micrometers or more. In such aspects, the abrasion-resistant layer may comprise the same material as the scratch-resistant layer. In aspects, a low friction coating may comprise a highly fluorinated silane coupling agent, for example, an alkyl fluorosilane with oxymethylgroups pendant on the silicon atom. In such aspects, an easy-to-clean coating may comprise the same material as the low friction coating. In other aspects, the easy-to- clean coating may comprise a protonatable group, for example an amine, for example, an alkyl aminosilane with oxymethyl groups pendant on the silicon atom. In such aspects, the oleophobic coating may comprise the same material as the easy-to-clean coating. In aspects, a diamond-like coating comprises carbon and may be created by applying a high voltage potential in the presence of a hydrocarbon plasma.
[0219] In aspects, as shown in FIGS. 2 and 4, the foldable apparatus 101 can comprise the device substrate or release liner 271 although other substrates (e.g., glass-based substrate and / or ceramic-based substrate discussed throughout the application) may be used in further aspects rather than the illustrated device substrate or release liner 271. In further aspects, as shown, the device substrate or release liner 271 can be disposed over the adhesive layer 261. In even further aspects, as shown, the release liner 271 can directly contact the second contact surface 265 of the adhesive layer 261. Although not shown for the foldable apparatus 101, 301, and 401, as shown in FIG. 16, the device substrate or release liner 271 can directly contact a surface of the polymer-based portion (e.g., fourth contact surface 295 of the second polymer-based portion 299) and / or attached to the foldable substrate 201 by the polymer-based portion (e.g., second polymer-based portion 299). The device substrate or release liner 271 can comprise a first major surface 273 and a second major surface 275 opposite the first major surface 273. As shown in FIGS. 2 and 4, the device substrate or release liner 271 can be disposed on the adhesive layer 261 by attaching the second contact surface 265 of the adhesive layer 261 to the first major surface 273 of the device substrate or release liner 271. In aspects, as shown, the first major surface 273 of the device substrate or release liner 271 can comprise a planar surface. In aspects, as shown, the second major surface 275 of the device substrate or release liner 271 can comprise a planar surface. When the device substrate or release liner 271 is a release liner, the release liner can comprise a paper and / or a polymer, for example polyesters (e.g., polyethylene terephthalate (PET)) and polyolefins. For example, the release liner can be configured to be removed to present a surface of a polymer-based portion or an adhesive layer that an electronic device (e.g., consumer electronic device, display device) can be attached thereto. When the device substrate or release liner 271 is a device substrate, the device substrate can comprise a polymerwith an elastic modulus of 5 GPa or more or a glass-based portion that can be similar and / or identical to the cover substrate 371.
[0220] Aspects of the disclosure can comprise a consumer electronic product. The consumer electronic product can comprise a front surface, a back surface, and side surfaces. The consumer electronic product can further comprise electrical components at least partially within the housing. The electrical components can comprise a controller, a memory, and a display. The display can be at or adjacent to the front surface of the housing. The display can comprise liquid crystal display (LCD), an electrophoretic displays (EPD), an organic light-emitting diode (OLED) display, or a plasma display panel (PDP). The consumer electronic product can comprise a cover substrate disposed over the display. In aspects, at least one of a portion of the housing or the cover substrate comprises the foldable apparatus discussed throughout the disclosure. The consumer electronic product can comprise a portable electronic device, for example, a smartphone, a tablet, a wearable device, or a laptop.
[0221] The foldable apparatus disclosed herein may be incorporated into another article, for example, an article with a display (or display articles) (e.g., consumer electronics, including mobile phones, tablets, computers, navigation systems, wearable devices (e.g., watches), and the like), architectural articles, transportation articles (e.g., automotive, trains, aircraft, sea craft, etc.), appliance articles, or any article that may benefit from some transparency, scratch-resistance, abrasion resistance or a combination thereof. An exemplary article incorporating any of the foldable apparatus disclosed herein is shown in FIGS. 10-11. Specifically, FIGS. 10-11 show a consumer electronic device 1000 including a housing 1002 having front 1004, back 1006, and side surfaces 1008. Although not shown, the consumer electronic device can comprise electrical components that are at least partially inside or entirely within the housing. For example, electrical components include at least a controller, a memory, and a display. As shown in FIGS. 10-11, the display 1010 can be at or adjacent to the front surface of the housing 1002. The consumer electronic device can comprise a cover substrate 1012 at or over the front surface of the housing 1002 such that it is over the display 1010. In aspects, at least one of the cover substrate 1012 or a portion of housing 1002 may include any of the foldable apparatus disclosed herein, for example, the foldable substrate.
[0222] In aspects, the foldable substrate 201 comprising a glass-based substrate and / or a ceramic-based substrate, and the first portion 221, the second portion 231, and / or the central portion 281 can comprise one or more compressive stress regions. In aspects, a compressive stress region may be created by chemically strengthening. Chemically strengthening may comprise an ion exchange process, where ions in a surface layer are replaced by–or exchanged with–larger ions having the same valence or oxidation state. Methods of chemically strengthening will be discussed later. Without wishing to be bound by theory, chemically strengthening the first portion 221, the second portion 231, and / or the central portion 281 can enable good impact and / or puncture resistance (e.g., resists failure for a pen drop height of about 15 centimeters (cm) or more, about 20 cm or more, about 50 cm or more). Without wishing to be bound by theory, chemically strengthening the first portion 221, the second portion 231, and / or the central portion 281 can enable small (e.g., smaller than about 10 mm or less) parallel plate distance because the compressive stress from the chemical strengthening can counteract the bend-induced tensile stress on the outermost surface of the substrate. A compressive stress region may extend into a portion of the first portion and / or the second portion for a depth called the depth of compression (DOC). As used herein, depth of compression means the depth at which the stress in the chemically strengthened substrates and / or portions described herein changes from compressive stress to tensile stress. Depth of compression may be measured by a surface stress meter or a scattered light polariscope (SCALP, wherein values reported herein were made using SCALP-5 made by Glasstress Co., Estonia) depending on the ion exchange treatment and the thickness of the article being measured. Where the stress in the substrate and / or portion is generated by exchanging potassium ions into the substrate, a surface stress meter, for example, the FSM-6000 (Orihara Industrial Co., Ltd. (Japan)), is used to measure depth of compression. Unless specified otherwise, compressive stress (including surface CS) is measured by surface stress meter (FSM) using commercially available instruments, for example the FSM-6000, manufactured by Orihara. Surface stress measurements rely upon the accurate measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. Unless specified otherwise, SOC is measured according to Procedure C (Glass Disc Method) described in ASTM standard C770-16, entitled “Standard Test Method for Measurement of Glass Stress-Optical Coefficient,” the contents of which are incorporated herein by reference in their entirety. Where thestress is generated by exchanging sodium ions into the substrate, and the article being measured is thicker than about 400 µm, SCALP is used to measure the depth of compression and central tension (CT). Where the stress in the substrate and / or portion is generated by exchanging both potassium and sodium ions into the substrate and / or portion, and the article being measured is thicker than about 400 µm, the depth of compression and CT are measured by SCALP. Without wishing to be bound by theory, the exchange depth of sodium may indicate the depth of compression while the exchange depth of potassium ions may indicate a change in the magnitude of the compressive stress (but not the change in stress from compressive to tensile). The refracted near-field (RNF; the RNF method is described in U.S. Patent No.8,854,623, entitled “Systems and methods for measuring a profile characteristic of a glass sample”, which is incorporated herein by reference in its entirety) method also may be used to derive a graphical representation of the stress profile. When the RNF method is utilized to derive a graphical representation of the stress profile, the maximum central tension value provided by SCALP is utilized in the RNF method. The graphical representation of the stress profile derived by RNF is force balanced and calibrated to the maximum central tension value provided by a SCALP measurement. As used herein, “depth of layer” (DOL) means the depth that the ions have exchanged into the substrate and / or portion (e.g., sodium, potassium). Throughout the disclosure, DOL is measured in accordance with ASTM C-1422. Without wishing to be bound by theory, a DOL is usually greater than or equal to the corresponding DOC. Through the disclosure, when the maximum central tension cannot be measured directly by SCALP (as when the article being measured is thinner than about 400 µm) the maximum central tension can be approximated by a product of a maximum compressive stress and a depth of compression divided by the difference between the thickness of the substrate and twice the depth of compression, wherein the compressive stress and depth of compression are measured by FSM.
[0223] In aspects, the first portion 221 may comprise a first compressive stress region at the first surface area 223 extending to a first depth of compression from the first surface area 223 and / or a second compressive stress region at the second surface area 225 extending to a second depth of compression from the second surface area 225. In aspects, the first depth of compression and / or the second depth of compression, as a percentage of the substrate thickness 207, can be about 5% or more, about 10% or more, about 12% or more, about 15% or more, about 30% or less, about25% or less, about 22% or less, about 20% or less, about 17% or less, or about 15% or less. In aspects, the first depth of compression and / or the second depth of compression, as a percentage of the substrate thickness 207, can range from about 5% to about 30%, from about 10% to about 25%, from about 10% to about 22%, from about 12% to about 20%, from about 15% to about 17%, or any range or subrange therebetween. In aspects, the first depth of compression and / or the second depth of compression can be about 1 µm or more, about 10 µm or more, about 15 µm or more, about 20 µm or more, about 25 µm or more, about 30 µm or more, about 200 µm or less, about 150 µm or less, about 100 µm or less, about 60 µm or less, about 45 µm or less, about 30 µm or less, or about 20 µm or less. In aspects, the first depth of compression and / or the second depth of compression can range from about 1 µm to about 200 µm, from about 1 µm to about 150 µm, from about 10 µm to about 100 µm, from about 15 µm to about 60 µm, from about 20 µm to about 45 µm, from about 20 µm to about 30 µm, or any range or subrange therebetween. By providing a first portion comprising a first glass-based and / or ceramic-based portion comprising a first depth of compression and / or a second depth of compression in a range from about 1% to about 30% of the first thickness, good impact and / or puncture resistance can be enabled.
[0224] In aspects, the first compressive stress region can comprise a first maximum compressive stress, and / or the second compressive stress region can comprise a second maximum compressive stress. In further aspects, the first maximum compressive stress and / or the second maximum compressive stress can be about 100 MegaPascals (MPa) or more, about 300 MPa or more, 400 MPa or more, about 500 MPa or more, about 600 MPa or more, about 700 MPa or more, about 1,500 MPa or less, about 1,200 MPa or less, about 1,000 MPa or less, or about 800 MPa or less. In further aspects, the first maximum compressive stress and / or the second maximum compressive stress can range from about 100 MPa to about 1,500 MPa, from about 300 MPa to about 1,500 MPa, from about 400 MPa to about 1,200 MPa, from about 500 MPa to about 1,000 MPa, from about 600 MPa to about 900 MPa, from about 700 MPa to about 800 MPa, or any range or subrange therebetween. By providing a first maximum compressive stress and / or a second maximum compressive stress in a range from about 100 MPa to about 1,500 MPa, good impact and / or puncture resistance can be enabled.
[0225] The first portion 221 may comprise a first tensile stress region positioned between the first compressive stress region and the second compressive stress region. In aspects, the first tensile stress region can comprise a first maximum tensile stress of about 10 MPa or more, about 20 MPa or more, about 30 MPa or more, about 100 MPa or less, about 80 MPa or less, or about 60 MPa or less. In further aspects, the first maximum tensile stress can range from about 10 MPa to about 100 MPa, from about 20 MPa to about 80 MPa, from about 30 MPa to about 60 MPa, or any range or subrange therebetween. Providing a first maximum tensile stress in a range from about 10 MPa to about 100 MPa can enable good impact and / or puncture resistance while providing low energy fractures, as discussed below.
[0226] In aspects, the second portion 231 may comprise a third compressive stress region at the third surface area 233 extending to a third depth of compression from the third surface area 233, and / or the second portion 231 may comprise a fourth compressive stress region at the fourth surface area 235 extending to a fourth depth of compression from the fourth surface area 235. In aspects, the third depth of compression and / or the fourth depth of compression, as a percentage of the substrate thickness 207, can be within one or more of the ranges discussed above for the first depth of compression and / or the second depth of compression. In further aspects, the third depth of compression can be substantially equal to the fourth depth of compression. The third compressive stress region can comprise a third maximum compressive stress, and / or the fourth compressive stress region can comprise a fourth maximum compressive stress. In aspects, the third maximum compressive stress and / or the fourth maximum compressive stress can be within one or more of the ranges discussed above for the first maximum compressive stress and / or the second maximum compressive stress. The second portion 231 may comprise a second tensile stress region positioned between the third compressive stress region and the fourth compressive stress region. In aspects, the second tensile stress region can comprise a second maximum tensile stress that can be within one or more of the ranges discussed above for the first maximum tensile stress. In further aspects, the first maximum tensile stress can be substantially equal to the second maximum tensile stress.
[0227] In aspects, the first depth of compression can be substantially equal to the third depth of compression. In aspects, the second depth of compression can be substantially equal to the fourth depth of compression. In aspects, the first maximum compressive stress can be substantially equal to the third maximum compressivestress. In aspects, the second maximum compressive stress can be substantially equal to the fourth maximum compressive stress. In aspects, the first depth of layer of one or more alkali-metal ions can be substantially equal to the third depth of layer of one or more alkali-metal ions. In aspects, the second depth of layer of one or more alkali- metal ions can be substantially equal to the fourth depth of layer of one or more alkali-metal ions.
[0228] In aspects, the central portion 281 can comprise a first central compressive stress region at the first central surface area 213 extending to a first central depth of compression from the first central surface area 213, and / or the central portion 281 can comprise a second central compressive stress region at the second central surface area 243 extending to a second central depth of compression from the second central surface area 243. In further aspects, the first central depth of compression and / or the second central depth of compression, as a percentage of the central thickness 209, can be within one or more of the ranges discussed above for the first depth of compression and / or the second depth of compression, as a percentage of the substrate thickness 207. In further aspects, the first central depth of compression and / or the second central depth of compression as a percentage of the central thickness 209 can be about 1% or more, about 2% or more, about 5% or more, about 8% or more, about 10% or more, about 12% or more, about 25% or less, about 20% or less, about 17% or less, about 15% or less, about 12% or less, about 10% or less, about 7% or less, or about 5% or less. For example, the first central depth of compression and / or the second central depth of compression as a percentage of the central thickness 209 can range from about 1% to about 25%, from about 2% to about 20%, from about 5% to about 17%, from about 7% to about 12%, or any range or subrange therebetween. In further aspects, the first central depth of compression can be substantially equal to the second central depth of compression. In further aspects, the first central depth of compression and / or the second central depth of compression can be within one or more of the ranges discussed above for the first depth of compression and / or the second depth of compression. In further aspects, the first central depth of compression and / or the second central depth of compression can be about 1 µm or more about 2 µm or more, about 4 µm or more, about 6 µm or more, about 20 µm or less, about 15 µm or less, about 10 µm or less, or about 8 µm or less. For example, the first central depth of compression and / or the second central depth of compression can range from about 1 µm to about 20 µm, from about 2 µm to about 15µm, from about 4 µm to about 10 µm, from about 6 µm to about 8 µm, or any range or subrange therebetween. By providing a central portion comprising a glass-based and / or ceramic-based portion comprising a first central depth of compression and / or a second central depth of compression in a range from about 1% to about 25% of the central thickness, good impact and / or puncture resistance can be enabled.
[0229] The first central compressive stress region can comprise a first central maximum compressive stress, and / or the second central compressive stress region can comprise a second central maximum compressive stress. In aspects, the first central maximum compressive stress and / or the second central maximum compressive stress can be within one or more of the ranges discussed above for the first maximum compressive stress and / or the second maximum compressive stress. By providing a first central maximum compressive stress and / or a second central maximum compressive stress in a range from about 100 MPa to about 1,500 MPa, good impact and / or puncture resistance can be enabled.
[0230] The central portion 281 may comprise a central tensile stress region positioned between the first central compressive stress region and the second central compressive stress region. In aspects, the central tensile stress region can comprise a central maximum tensile stress of about 25 MPa or more, about 50 MPa or more, about 75 MPa or more, about 100 MPa or more, about 150 MPa or more, about 375 MPa or less, about 300 MPa or less, about 250 MPa or less, or about 200 MPa or less. In further aspects, the central maximum tensile stress can range from about 25 MPa to about 375 MPa, from about 50 MPa to about 300 MPa, from about 75 MPa to about 250 MPa, from about 100 MPa to about 250 MPa, from about 150 MPa to about 200 MPa, or any range or subrange therebetween. Providing a central maximum tensile stress in a range from about 125 MPa to about 375 MPa can enable low minimum parallel plate distance.
[0231] In aspects, the polymer-based portion 289 and / or 299 can be optically clear and / or comprise a first refractive index within one or more of the ranges discussed above for the polymer-based portion 289 and / or 299. In aspects, the foldable substrate 201 can comprise a second refractive index of about 1.4 or more, about 1.45 or more, about 1.49 or more, about 1.7 or less, about 1.6 or less, or about 1.55 or less. In aspects, the second refractive index of the foldable substrate 201 can range from about 1.4 to about 1.7, from about 1.4 to about 1.6, from about 1.45 to about 1.55, from about 1.49 to about 1.55, or any range or subrange therebetween. Inaspects, a differential equal to the absolute value of the difference between the second refractive index of the foldable substrate 201 and the first refractive index of the polymer-based portion 289 and / or 299 can be about 0.1 or less, about 0.07 or less, about 0.05 or less, about 0.001 or more, about 0.01 or more, or about 0.02 or more. In aspects, the differential is in a range from about 0.001 to about 0.1, from about 0.01 to about 0.07, from about 0.02 to about 0.05, or any range or subrange therebetween. In aspects, the second refractive index of the foldable substrate 201 may be greater than the first refractive index of the polymer-based portion 289 and / or 299. In aspects, the second refractive index of the foldable substrate 201 may be less than the first refractive index of the polymer-based portion 289 and / or 299.
[0232] In aspects, the adhesive layer 261 can comprise a third refractive index that can be within one or more of the ranges discussed above with regards to the first refractive index of the polymer-based portion 289 and / or 299. In aspects, a differential equal to the absolute value of the difference between the third refractive index of the adhesive layer 261 and the first refractive index of the polymer-based portion 289 and / or 299 can be within one or more of the ranges discussed above for the differential between the second refractive index and the first refractive index. In aspects, the third refractive index of the adhesive layer 261 may be greater than the first refractive index of the polymer-based portion 289 and / or 299. In aspects, the third refractive index of the adhesive layer 261 may be less than the first refractive index of the polymer-based portion 289 and / or 299. In aspects, a differential equal to the absolute value of the difference between the third refractive index of the adhesive layer 261 and the second refractive index of the foldable substrate 201 can be within one or more of the ranges discussed above for the differential between the second refractive index and the first refractive index. In aspects, the third refractive index of the adhesive layer 261 may be greater than the second refractive index of the foldable substrate 201. In aspects, the third refractive index of the adhesive layer 261 may be less than the second refractive index of the foldable substrate 201.
[0233] In aspects, the coating 251 can comprise a fourth refractive index. In aspects, the fourth refractive index of the coating 251 can be within one or more of the ranges discussed above with regards to the first refractive index of the polymer- based portion 289 and / or 299. In aspects, a differential equal to the absolute value of the difference between the fourth refractive index of the coating 251 and the first refractive index of the polymer-based portion 289 and / or 299 can be within one ormore of the ranges discussed above for the differential between the second refractive index and the first refractive index. In aspects, the fourth refractive index of the coating 251 may be greater than the first refractive index of the polymer-based portion 289 and / or 299. In aspects, the fourth refractive index of the coating 251 may be less than the first refractive index of the polymer-based portion 289 and / or 299. In aspects, a differential equal to the absolute value of the difference between the fourth refractive index of the coating 251 and the second refractive index of the foldable substrate 201 can be within one or more of the ranges discussed above for the differential between the second refractive index and the first refractive index. In aspects, the fourth refractive index of the coating 251 may be greater than the second refractive index of the foldable substrate 201. In aspects, the fourth refractive index of the coating 251 may be less than the second refractive index of the foldable substrate 201. In aspects, a differential equal to the absolute value of the difference between the fourth refractive index of the coating 251 and the third refractive index of the adhesive layer 261 can be within one or more of the ranges discussed above for the differential between the second refractive index and the first refractive index. In aspects, the fourth refractive index of the coating 251 may be greater than the third refractive index of the adhesive layer 261. In aspects, the fourth refractive index of the coating 251 may be less than the third refractive index of the adhesive layer 261.
[0234] FIGS. 7 and 9 schematically illustrate aspects of a foldable apparatus 701 and / or 901 in accordance with aspects of the disclosure in a folded configuration. As shown in FIG. 6, the foldable apparatus 501 is folded such that the second major surface 205 of the foldable substrate 201 is on the inside of the folded foldable apparatus 501, for example, foldable apparatus 301 can be folded to form foldable apparatus 501. For example, a display could be located on the side of the second major surface 205, and a viewer would view the display from the side of the first major surface 203. Alternatively, a display could be located on the side of the first major surface 203, and a viewer would view the display from the side of the second major surface 205. For example, a display could be located on the side of the second major surface 205, and a viewer would view the display from the side of the first major surface 203. Alternatively, a display could be located on the side of the first major surface 203, and a viewer would view the display from the side of the second major surface 205.
[0235] As shown in FIG. 7, the foldable apparatus 101 shown in FIG. 1 (modified as described in the Parallel Plate Test below) is folded to form folded foldable apparatus 701 such that the first major surface 203 of the foldable substrate 201 is on the inside of the folded foldable apparatus 701. In FIG. 7, a user would view a display device in place of the 50 µm sheet 707 of PET through the foldable substrate 201 and, thus, would be positioned on the side of the first major surface 203. In aspects, as shown in FIG.7, the foldable apparatus 701 can comprise a coating 251 disposed over the foldable apparatus 701 (e.g., second major surface 205). In further aspects, a user would view a display device in place of the 50 µm sheet 707 of PET through the coating 251. In aspects, as shown in FIG. 7, the polymer-based portion 289 and / or 299 can be disposed over the foldable substrate 201. In further aspects, although not shown, an additional substrate (e.g., glass-based substrate and / or ceramic-based substrate in place of release liner 271 or 50 µm sheet 707 of PET), and the additional substrate can be disposed over a display device. As shown in FIG. 9, the foldable apparatus 401 shown in FIG. 4 (modified as described in the Parallel Plate Test below) is folded to form folded foldable apparatus 901 such that the first major surface 203 of the foldable substrate 201 is on the inside of the folded foldable apparatus 901. In FIG. 9, a user would view a display device in place of the 50 µm sheet 707 of PET through the foldable substrate 201 and, thus, would be positioned on the side of the first major surface 203. In aspects, as shown in FIG. 9, the second polymer-based portion 299 can be disposed over the foldable substrate 201 (e.g., in the first recess 211). In further aspects, although not shown, an additional substrate (e.g., glass-based substrate and / or ceramic-based substrate in place of release liner 271 or 50 µm sheet 707 of PET), and the additional substrate can be disposed over a display device. It is to be understood that the foldable apparatus can be designed to fold such that the display device is on the inside of the bend, on the outside of the bend, or such that the foldable apparatus can be folded in either direction.
[0236] As used herein, the “parallel plate distance” of a foldable apparatus and / or foldable substrate is measured with the following test configuration and process using a parallel plate apparatus 601 (see FIGS. 6-7 and 9) that comprises a pair of parallel rigid stainless-steel plates 603, 605 comprising a first rigid stainless- steel plate 603 and a second rigid stainless-steel plate 605. When measuring the “parallel plate distance” for the foldable substrate 201 (e.g., the foldable apparatus 301 shown in FIG. 3 consisting of foldable substrate 201), as shown in FIG. 6, thefoldable substrate 201 is placed between the pair of plates 603 and 605 such that the first major surface 203 is in contact with the pair of plates 603 and 605. When measuring the “parallel plate distance” for a foldable apparatus resembling the foldable apparatus 101 and 401 shown in FIGS. 2 and 4, respectively, the adhesive layer 261 is removed and is replaced by a test adhesive layer 709 comprises a thickness of 50 µm. Further, the test is conducted with a 50 µm thick sheet 707 of polyethylene terephthalate (PET) rather than with the release liner 271 of FIGS. 2 and 4. Thus, during the test to determine the “parallel plate distance” of a configuration of a foldable apparatus, the foldable apparatus 701 is produced by using the 50 µm thick sheet 707 of polyethylene terephthalate (PET) rather than with the release liner 271 of FIGS.2 and 4.
[0237] When preparing the foldable apparatus 701, the 50 µm thick sheet 707 of polyethylene terephthalate (PET) is attached to the test adhesive layer 709 in an identical manner that the release liner 271 is attached to the second contact surface 265 of the adhesive layer 261 as shown in FIG. 2. To test the foldable apparatus 701 of FIG.7, the test adhesive layer 709 and the 50 µm sheet 707 of PET can likewise be installed as shown in the configuration of FIG. 7 to conduct the test on the foldable apparatus 701. The foldable apparatus 701 is placed between the pair of parallel rigid stainless-steel plates 603 and 605 such that the foldable substrate 201 will be on the inside of the bend, similar to the configuration shown in FIG. 7. Similarly, when preparing the foldable apparatus 901, the foldable apparatus 401 shown in FIG. 4 is prepared for testing by replacing the adhesive layer 261 and the release liner 271 with the test adhesive layer 709 and the 50 µm thick sheet 707 of PET. For determining a “parallel plate distance”, the distance between the parallel plates is reduced at a rate of 50 µm / second until the parallel plate distance 611 or 711 is equal to the “parallel plate distance” to be tested. Then, the parallel plates are held at the “parallel plate distance” to be tested for 24 hours at about 85°C and about 85% relative humidity. As used herein, the “minimum parallel plate distance” is the smallest parallel plate distance that the foldable apparatus can withstand without failure under the conditions and configuration described above.
[0238] In aspects, the foldable apparatus 101, 301, 401, 701, 801, and / or 901 and / or foldable substrate 201 can achieve a parallel plate distance of 100 mm or less, 50 mm or less, 20 mm or less, 10 mm or less, 5 mm or less, or 3 mm or less. In further aspects, the foldable apparatus and / or foldable substrate can achieve a parallelplate distance of 50 millimeters (mm), or 20 mm, or 10 mm, of 5 mm, or 3 mm. In aspects, the foldable apparatus and / or foldable substrate can comprise a minimum parallel plate distance of about 40 mm or less, about 20 mm or less, about 10 mm or less, about 5 mm or less, about 3 mm or less, about 1 mm or less, about 1 mm or more, about 3 mm or more, about 5 mm or more, or about 10 mm or more. In aspects, the foldable apparatus and / or foldable substrate can comprise a minimum parallel plate distance in a range from about 1 mm to about 40 mm, from about 1 mm to about 20 mm, from about 1 mm to about 10 mm, from about 1 mm to about 5 mm, from about 1 mm to about 3 mm. In aspects, the foldable apparatus and / or foldable substrate can achieve a minimum parallel plate distance in a range from about 2 mm to about 40 mm, from about 2 mm to about 20 mm, from about 3 mm to about 10 mm, from about 3 mm to about 5 mm, or any range or subrange therebetween.
[0239] A width 287 of the central portion 281 of the foldable substrate 201 is defined between the first portion 221 and the second portion 231 in the direction 106 of the length 105. In aspects, the width 287 of the central portion 281 of the foldable substrate 201 can extend from the first portion 221 to the second portion 231. A width 210 of the first central surface area 213 and the second central surface area 243 of the foldable substrate 201 is defined between the first transition region 212 and the second transition region 218, for example, as the portion comprising the central thickness 209, in the direction 106 of the length 105. In aspects, the width 287 of the central portion 281 of the foldable substrate 201 and / or the width 210 of the first central surface area 213 of the foldable substrate 201 can be about 1.4 times or more, about 1.6 times or more, about 2 times or more, about 2.2 times or more, about 3 times or less, or about 2.5 times or less the minimum parallel plate distance. In aspects, the width 287 of the central portion 281 of the foldable substrate 201 and / or the width 210 of the first central surface area 213 of the foldable substrate 201 as a multiple of the minimum parallel plate distance can range from about 1.4 times to about 3 times, from about 1.6 times to about 2.5 times, from about 2 times to about 2.5 times, from about 2.2 times to about 2.5 times, or any range or subrange therebetween. Without wishing to be bound by theory, the length of a bent portion in a circular configuration between parallel plates can be about 1.6 times the parallel plate distance. Without wishing to be bound by theory, the length of a bend portion in an elliptical configuration between parallel plates can be about 2.2 times the parallel plate distance. In aspects, the width 287 of the central portion 281 and / or the width210 of the first central surface area 213 as a percentage of the length 105 of the foldable apparatus can be about 30% or more, about 35% or more, about 40% or more, about 45% or more, about 70% or less, about 60% or less, about 55% or less, or about 50% or less. In aspects, the width 287 of the central portion 281 and / or the width 210 of the first central surface area 213 as a percentage of the length 105 of the foldable apparatus can range from about 30% to about 70%, from about 35% to about 60%, from about 40% to about 55%, from about 45% to about 50%, or any range or subrange therebetween. In aspects, the width 287 of the central portion 281 of the foldable substrate 201 and / or the width 210 of the first central surface area 213 of the foldable substrate 201 can be about 1 mm or more, about 3 mm or more, about 5 mm or more, about 8 mm or more, about 10 mm or more, about 15 mm or more, about 20 mm or more, about 60 mm or less, about 50 mm or less, about 40 mm or less, about 35 mm or less, about 30 mm or less, or about 25 mm or less. In aspects, the width 287 of the central portion 281 of the foldable substrate 201 and / or the width 210 of the first central surface area 213 of the foldable substrate 201 can range from about 1 mm to about 100 mm, from about 3 mm to about 60 mm, from about 5 mm to about 50 mm, from about 8 mm to about 40 mm, from about 10 mm to about 40 mm, from about 15 mm to about 35 mm, from about 20 mm to about 30 mm, or any range of subrange therebetween. In aspects, the width 287 of the central portion 281 of the foldable substrate 201 and / or the width 210 of the first central surface area 213 of the foldable substrate 201 can be about 2.8 mm or more, about 6 mm or more, about 9 mm or more, about 60 mm or less, about 40 mm, or less, or about 24 mm or less. In aspects, the width 287 of the central portion 281 of the foldable substrate 201 and / or the width 210 of the first central surface area 213 of the foldable substrate 201 can range from about 2.8 mm to about 40 mm, from about 6 mm to about 24 mm, or any range of subrange therebetween. In aspects, the first central surface area 213, the central portion 281 (e.g., centerline of the central portion 281), and / or the fold plane 109 can correspond to a midpoint between opposing ends of the foldable substrate and / or the foldable apparatus in the direction 106 of the length 105. By providing a width within the above-noted ranges for the central portion, folding of the foldable apparatus without failure can be facilitated.
[0240] The foldable apparatus 101, 301, 401, 701, 801, and / or 901 may have an impact resistance defined by the capability of a region of the foldable apparatus (e.g., a region comprising the first portion 221, a region comprising thesecond portion 231, a region comprising the polymer-based portion 289 and / or 299 and / or central portion 281) to avoid failure at a pen drop height (e.g., 5 centimeters (cm) or more, 10 centimeters or more, 20 cm or more), when measured according to the “Pen Drop Test.” As used herein, the “Pen Drop Test” is conducted such that samples of foldable apparatus are tested with the load (i.e., from a pen dropped from a certain height) imparted to an outer surface of the PET sheet with the foldable apparatus configured as in the parallel plate test with 50 µm thick sheet 707 of PET attached to the test adhesive layer 709 having a thickness of 50 µm instead of the release liner 271 shown in FIG. 2. During testing, the foldable apparatus bonded to the PET sheet is placed on an aluminum plate (6063 aluminum alloy, as polished to a surface roughness with 400 grit paper) with the outer surface opposite the PET sheet in contact with the aluminum plate. No tape is used on the side of the sample resting on the aluminum plate.
[0241] A tube is used for the Pen Drop Test to guide a pen to an outer surface of the foldable apparatus. For the foldable apparatus 101, 301, 401, 701, 801, and / or 901 in FIGS. 2-4 and 7-9, the pen is guided to the outer surface of the PET sheet, and the tube is placed in contact with the outer surface of the PET sheet so that the longitudinal axis of the tube is substantially perpendicular to the outer major surface with the longitudinal axis of the tube extending in the direction of gravity. The tube has an outside diameter of 1 inch (2.54 cm), an inside diameter of nine-sixteenths of an inch (1.4 cm), and a length of 90 cm. An acrylonitrile butadiene (ABS) shim is employed to hold the pen at a predetermined height for each test. After each drop, the tube is relocated relative to the sample to guide the pen to a different impact location on the sample. The pen employed in Pen Drop Test is a BIC Easy Glide Pen, Fine, having a tungsten carbide ballpoint tip of 0.7 mm (0.68 mm) diameter, and a weight of 5.73 grams (g) including the cap.
[0242] For the Pen Drop Test, the pen is dropped with the cap attached to the top end (i.e., the end opposite the tip) so that the ballpoint can interact with the test sample. In a drop sequence according to the Pen Drop Test, one pen drop is conducted at an initial height of 1 cm, followed by successive drops in 0.5 cm increments up to 20 cm, and then after 20 cm, 2 cm increments until failure of the test sample. After each drop is conducted, the presence of any observable fracture, failure, or other evidence of damage to the sample is recorded along with the particular pen drop height. Using the Pen Drop Test, multiple samples can be tested according to the samedrop sequence to generate a population with improved statistical accuracy. For the Pen Drop Test, the pen is to be changed to a new pen after every 5 drops, and for each new sample tested. In addition, all pen drops are conducted at random locations on the sample at or near the center of the sample, with no pen drops near or on the edge of the samples.
[0243] For purposes of the Pen Drop Test, “failure” means the formation of a visible mechanical defect in a laminate. The mechanical defect may be a crack or plastic deformation (e.g., surface indentation). The crack may be a surface crack or a through crack. The crack may be formed on an interior or exterior surface of a laminate. The crack may extend through all or a portion of the foldable substrate 201 and / or coating. A visible mechanical defect has a minimum dimension of 0.2 mm or more.
[0244] In aspects, the foldable apparatus can resist failure for a pen drop in a region comprising the first portion 221 or the second portion 231 at a pen drop height of 10 centimeters (cm), 12 cm, 14 cm, 16 cm, or 20 cm. In aspects, a maximum pen drop height that the foldable apparatus can withstand without failure over a region comprising the first portion 221 or the second portion 231 may be about 10 cm or more, about 12 cm or more, about 14 cm or more, about 16 cm or more, about 40 cm or less, or about 30 cm or less, about 20 cm or less, about 18 cm or less. In aspects, a maximum pen drop height that the foldable apparatus can withstand without failure over a region comprising the first portion 221 or the second portion 231 can range from about 10 cm to about 40 cm, from about 12 cm to about 30 cm, from about 14 cm to about 20 cm, from about 16 cm to about 20 cm, from about 18 cm to about 20 cm, or any range or subrange therebetween.
[0245] In aspects, the foldable apparatus can resist failure for a pen drop in a region (e.g., central portion 281) comprising the polymer-based portion 289 and / or 299 between the first portion 221 and the second portion 231 in the Pen Drop Test at a pen drop height of 5 cm or more, 8 cm or more, 9 cm or more, 10 cm or more, 11 cm or more, 12 cm or more, 13 cm or more, 14 cm, 15 cm or more, or 20 cm. In aspects, a maximum pen drop height that the foldable apparatus can withstand without failure over a region comprising the polymer-based portion 289 and / or 299 between the first portion 221 and the second portion 231 in the Pen Drop Test may be of 5 cm or more, 8 cm or more, 9 cm or more, 10 cm or more, 11 cm or more, 12 cm or more, 13 cm or more, 14 cm or more, 15 cm or more, 20 cm or less, 15 cm or less, or 13 cm or less. Inaspects, a maximum pen drop height that the foldable apparatus can withstand without failure over a region comprising the polymer-based portion 289 and / or 299 between the first portion 221 and the second portion 231 in the Pen Drop Test can range from about 5 cm to about 20 cm, from about 10 cm to about 15 cm, from about 11 cm to about 13 cm, or any range or subrange therebetween.
[0246] The foldable apparatus can exhibit a puncture resistance in a portion comprising the polymer-based portion 289 and / or 299 as measured in a Quasi-Static Puncture Test. For the “Quasi-Static Puncture Test”, a test apparatus identical to the test apparatus discussed above for the Pen Drop Test is used, where the foldable apparatus is configured with 50 µm thick sheet 707 of PET attached to the test adhesive layer 709 having a thickness of 50 µm instead of the release liner 271 shown in FIG.2. During testing, the foldable apparatus bonded to the PET sheet is placed on an aluminum plate (6063 aluminum alloy, as polished to a surface roughness with 400 grit paper) with the outer surface opposite the PET sheet in contact with the aluminum plate. No tape is used on the side of the sample resting on the aluminum plate. In the Quasi-Static Puncture Test, a tungsten carbide ball with a predetermined diameter is placed on the outer surface of PET sheet in a portion of the foldable apparatus comprising the polymer-based portion 289 and / or 299 and a load is applied to the tungsten carbide ball at a rate of 0.1 kilogram-force (kgf) per minute until failure. In aspects, the foldable apparatus can withstand a load of about 0.5 kgf or more, about 0.8 kgf or more, about 0.9 kgf or more, about 1 kgf or more, about 1.1 kgf or more, about 1.2 kgf or more applied through a 0.25 millimeter diameter tungsten carbide ball in the Quasi-Static Puncture Test. In aspects, the foldable apparatus can withstand a load of about 0.5 kgf or more, about 1 kgf or more, about 1.5 kgf or more, about 1.8 kgf or more, about 1.9 kgf or more, about 2 kgf or more, about 2.1 kgf or more, about 2.2 kgf or more, about 2.5 kgf or more applied through a 0.5 millimeter diameter tungsten carbide ball in the Quasi-Static Puncture Test.
[0247] Methods of making the foldable apparatus in accordance with aspects of the disclosure can include any of the aspects discussed above with reference to the flow chart in FIG.12 and example method steps illustrated in FIGS.13-18. EXAMPLES
[0248] Various aspects will be further clarified by the following examples. Tables 3-4 present compositions of Examples 1-11, AA, and EE-KK, and Tables 5-7 present properties of Examples 1-11 and AA-KK. Tables 8-11 present compositionsof Examples 12-28, LL-ZZ, and A1-A5, and Tables 12-15 present properties of Examples 12-28, LL-ZZ, and A1-A3. In Tables 3-4 and 8-11, EB230 is Ebecryl 230 (Sartomer), which is a urethane-acrylate oligomer. 2-EHA is 2-ethylhexylacrylate (available from BASF), 2-PHA is 2-propylhexylacrylate, M122 is dodecyl acrylate available as Miramer M122 (Miwon), M130 is isodecyl acrylate available as Miramer M130 (Miwon), C17A is heptadecyl acrylate, and AA is acrylic acid (available from BASF). M170 is 2-(2-ethoxyethoxy)ethylacrylate available as Miramer M170 (Miwon). 2-EHA, 2-PHA, M122, M130, M170, C17A, and AA are low refractive index acrylates. 2-EHA, 2-PHA, M122, M130, and C17A are alkyl acrylates with a low refractive index. M170 is an ether acrylate with a low refractive index. BPMA is biphenyl methyl acrylate available as Miramer M1190 (Miwon), which is a high refractive index acrylate. HBA is 4-hyrdoxybutyl acrylate, and HPPA is 2-hydroxy-3- phenoxypropyl acrylate. HBA and HPPA each have one acrylate functionality and one hydroxyl functionality. D1173 is 2-hydroxy-2-methylpropiophenone available as Darocur 1173 (BASF), which is a photoinitiator. PentA is Pentalyn A (Eastman), which is a tackifier. EVA-40 is poly(ethylene-co-vinyl acetate) (EVA) as a 40 wt% solution in vinyl acetate available from Millipore Sigma, VMK is poly(vinyl methyl ketone) available from Millipore Sigma, and HP-EVA is a partially hydrolyzed EVA made from EVA 40. EVA-40, VMK, and HP-EVA are linear polymers. EVA-40 and HP-EVA are linear copolymers, and HP-EVA can react with other components in the composition. H12MDI is hydrogenated methylene diphenyl isocyanate available from Millipore Sigma, which is a cross-linking agent. Examples BB-DD correspond to CEF3502 (3M) and CEF360 (3M), and NCF0962 (LINTEC). Tables 3-4 and 8-11 present the compositions as wt% with all components adding up to 100%, but it is to be understood that the photoinitiator, tackifier, (and any silane coupling agent and / or antioxidant) can be represented as pph, as discussed above. For compositions,that a component was not present. For properties, “-” means that the property was not measured.
[0249] As shown in Table 3, Example AA comprises a single low refractive index acrylate (2-EHA), a single high refractive index acrylate (BPMA), a hydroxyl- containing acrylate (HBA), a urethane-acrylate oligomer (EB230), and photoinitiator (D1173). Examples 1-8 comprised two or more low refractive index acrylates (e.g., 2- EHA, M170, AA). Examples 5 and 7 include a tackifier (PentaA). As shown in Table 4, Examples 9-11 also include two or more low refractive index acrylates (e.g., M170,C17, AA). Example 11 includes a tackifier (PentA). In contrast, Examples EE-KK did not include a high refractive index acrylate. Table 3: Composition (wt%) of Examples AA and 1-8Table 4: Composition (wt%) of Examples 9-11 and EE-KK
[0250] Tables 5-7 present the properties of Examples 1-11 and AA-KK. As discussed above, Examples 1-11 can be partially cured with half of the photoinitiator to achieve a precursor solution with a predetermined precursor viscosity before adding the remainder of the photoinitiator and optionally any additives (e.g., tackifier, anti-oxidant, silane coupling agent) before further curing. The properties of Examples 1-11 correspond to those of the composition at the end of the curing process. Examples 1-11 and AA-KK were cured using UV light from two Ushio F15T8BLBblacklight bulbs to form the precursor solution from the composition followed by UV light from eight Sylvania F40 / 350BI / ECO blacklight bulbs. Table 5: Properties of Examples 1-9Table 6: Properties of Examples 10-11 and EE-KKTable 7: Properties of Examples BB-DD
[0251] As shown in Tables 5-6, Examples 1-11 comprised a storage modulus (E’) at 25°C from 0.1 MPa to 1 MPa (e.g., from 0.1 MPa to 0.5 MPa, or from 0.2 MPa to 0.5 MPa), and Examples 1-11 comprised a storage modulus (E’) at - 20°C from 1 MPa to about 40 MPa (e.g., from about 1 MPa to about 20 MPa, or from about 1.5 MPa to about 15 MPa). In contrast, as shown in Table 7, Example DD had a storage modulus (E’) at 25°C greater than 1 MPa (e.g., greater than 2 MPa) and a storage modulus (E’) at -20°C greater than 40 MPa (e.g., greater than 50 MPa, about 60 MPa). Likewise, Example HH have an elastic modulus (E’) at -20°C greater than 40 MPa. At the same time, Examples BB, EE-GG, and II-JJ have an elastic modulus (E’) at -20°C less than 1 MPa, which is lower than any of Examples 1-11.
[0252] Examples 1-11 comprised a loss modulus (E”) at 25°C of less than 1 MPa (e.g., less than 0.5 MPa, or from 0.1 MPa to about 0.5 MPa), and Examples 1-9 comprised a loss modulus (E”) at 25°C of less than 0.2 MPa (e.g., from about 0.1 MPa to about 0.2 MPa). Examples 1-11 comprised a loss modulus (E”) at -20°C of less than 30 MPa (e.g., from about 0.4 MPa to about 30 MPa, or from about 1 MPa to about 26 MPa), and Examples 1-5 and 9-10 comprised a loss modulus (E”) at -20°C of less than 20 MPa (e.g., less than 10 MPa, less than 5 MPa, from 1 MPa to 10 MPa, or from 2 MPa to 5 MPa). In contrast, as shown in Table 7, Examples DD and HH comprised a loss modulus (E”) at 25°C greater than 0.2 MPa (e.g., about 0.5 MPa or more, about 0.6 MPa or more, or about 0.7 MPa or more) and a loss modulus (E”) at - 20°C greater than 30 MPa (e.g., greater than 40 MPa, or greater than 50 MPa). At the same time, Examples FF and II-JJ have loss modulus (E”) at 25°C less than 0.1 MPa. Examples EE-GG and II comprised a loss modulus (E”) at -20°C less than 1 MPa.
[0253] Examples 1-11 comprised a ratio of E” / E’ (e.g., tan delta) at 25°C of about 0.5 or less (e.g., from about 0.2 to about 0.5 or from about 0.25 to about 0.47), and Examples 1-4 and 7-11 comprised a ratio of E” / E’ (e.g., tan delta) at 25°C of about 0.4 or less (e.g., from about 0.3 to about 0.4). In contrast, Examples AA-BB andJJ-KK comprised a ratio of E” / E’ at 25°C greater than 0.4 (e.g., greater than 0.45 for Examples AA-BB), and Examples BB and KK comprised a ratio of E” / E’ at 25°C greater than 0.5 (e.g., greater than 0.6, and greater than 0.7).
[0254] As shown in Tables 5-6, Examples 1-11 comprised a glass transition temperature (Tg) less than -19°C (e.g., less than about -20°C, from about -45°C to about -20°C). Examples HH and JJ are labeled as n / a because they did not contain a single, well-defined peak in tan delta that could be used to identify a single Tg and this is associated with phase separation (as discussed below). Examples 1-11 comprises a 300% strain recovery greater than 35% (i.e., recovering greater than 105% of the 300% imposed strain). Examples 1-7 and 11 comprised a 300% strain recovery greater than 50%. Examples 1-3, 5-7, and 11 comprised a 300% strain recovery greater than 60% (e.g., from about 60% to about 93%). In contrast, as shown in Table 7, Example DD comprised a 300% strain recovery of less than 30% (e.g., less than 25%). Examples 1-11 comprised a peel adhesion (after a 15 minute dwell time) of greater than 0.6 N / cm (e.g., greater than 1 N / cm, from about 1 N / cm to about 5 N / cm). Examples 1-5 and 7-11 comprised a peel adhesion (after a 15 minute dwell time) of greater than 1.4 N / cm (e.g., from about 1.4 N / cm to about 5 N / cm).
[0255] Examples 1-11 comprised a liquid refractive index from about 1.46 to about 1.48. Example 6 comprised a cured refractive index of 1.5008 (i.e., within 0.01 of 1.5). The multiple low-refractive index acrylates in Examples 1-1 enable the refractive index of the resulting polymer-based portion to be tuned without significantly impacting mechanical properties, as demonstrated by Example 6 being within 0.01 of 1.5 while Examples BB-CC, FF, and KK comprised a cured refractive index of about 1.47. Likewise, the lack of a high refractive index acrylate in Examples EE-KK is associated with a lower liquid refractive index (e.g., less than 1.46, or less than 1.45).
[0256] Tables 8-11 present the compositions for Examples 12-28, LL-ZZ, and A1-A5 that include a linear polymer. Examples 12-28, LL-XX, and A4 include EVA-40 as the linear polymer. Examples YY-ZZ and A1-A3 include PVMK as the linear polymer. Example A5 includes PH-EVA as the linear polymer. Examples 12-28 include at least 50 wt% of low refractive index acrylate(s) (e.g., 2-EHA, M130, M170), a high refractive index acrylate (BPMA), a urethane-acrylate oligomer (EB230), a hydroxy-containing acrylate (e.g., HBA, HPPA), linear polymer (e.g., EVA-40), and a photoinitiator (D1173). Examples A4-A5 comprise a cross-linkingagent (H12MDI). In Examples A4-A5, it is possible for the linear polymer to be incorporated into the polymer formed from those compositions by either the cross- linker reacting with the linear polymer and an acrylate or by a hydroxyl group in the hydrolyzed polymer reacting with an acrylate. Consequently, the urethane acrylate oligomer was omitted from Examples A4-A5. In Examples 12-28, LL-ZZ, and A1- A3, it is expected that the linear polymers are not physically bonded to the acrylate polymer. Examples VV-ZZ comprise HPPA instead of HBA as the hydroxyl- containing acrylate. Examples A1-A3 comprise less than 50 wt% (i.e., 10 wt%) of low refractive index acrylates; instead, Examples A1-A3 comprise greater than 50 wt% (e.g., greater than 70 wt%) of the hydroxyl-containing acrylate (e.g., HBA). Examples LL-ZZ do not contain a high refractive index acrylate. Table 8: Composition (wt%) of Examples 12-20Table 9: Composition (wt%) of Examples 21-28Table 10: Composition (wt%) of Examples LL-UUTable 11: Composition (wt%) of Examples VV-ZZ and A1-A5
[0257] Tables 12-15 present the properties of Examples 12-28, LL-ZZ, and A1-A3. Examples 12-13 and 16-26 comprised a storage modulus (E’) at 25°C less than 1 MPa (e.g., from about 0.1 MPa to about 1 MPa, or from 0.4 MPa to 0.6 MPa). Examples 12-13 and 16-26 comprised a storage modulus (E’) at -20°C from about 1 MPa to about 10 MPa (e.g., from about 3 MPa to about 10 MPa). In contrast, Examples A3 has a storage modulus (E’) at 25°C greater than 3 MPa, and Examples YY-ZZ and A1-A3 comprised a storage modulus (E’) at -20°C greater than 10 MPa (e.g., greater than 40 MPa). Examples 12-13 and 16-26 comprised a loss modulus (E”) at 25°C of less than 0.3 MPa (e.g., from about 0.1 MPa to about 0.3 MPa, or from about 0.15 MPa to about 0.25 MPa). Examples 12-13 and 16-26 comprised a loss modulus (E”) at -20°C from about 1 MPa to about 20 MPa (e.g., from about 3 MPa to about 11 MPa). Examples 12-13 and 16-28 comprised a ratio of E” / E’ at 25°C less than about 0.4 (e.g., from about 0.3 to about 0.4). In contrast, Examples QQ-SS and YY comprised a ratio E” / E’ at 25°C less than 0.3. Example A3 comprised a ratio of E” / E’ at 25°C greater than 0.4 (e.g., greater than 0.5, greater than 0.6, or greater than 0.7).
[0258] Examples 12-13 and 16-28 comprised a (single) glass-transition temperature less of about -20°C or less (e.g., from about -20°C to about -40°C). In contrast, Examples YY-ZZ and A1-A3 comprise a glass transition temperature above-20°C, which may be a result of the elevated amounts of the hydroxyl-containing acrylate in those Examples. Examples LL-SS and WW-XX comprised more than one glass-transition temperature, which is associated with phase separation. Table 12: Properties of Examples 12-20Table 13: Properties of Examples 21-28Table 14: Properties of Examples LL-UUTable 15: Properties of Examples VV-ZZ and A1-A5
[0259] As shown in Tables 12-13, Examples 12-13, 16-20, and 22-26 comprised a 300% strain recovery greater than 40%, Examples 12-13, 16-20, 22, and 24-26 comprised a 300% strain recovery greater than 50%, and Examples 12-13, 16- 20, and 25-26 comprised a 300% strain recovery greater than 60%. In contrast, as shown in Tables 14-16, Examples QQ-UU and YY-ZZ comprised a 300% strain recovery less than 40%. As shown in Tables 12-13, Examples 13-28 comprised a peel adhesion after a 15 minute dwell time of about 2 N / cm or more, and Examples 21-26 comprised a peel adhesion after a 15 minute dwell time of about 3 N / cm or more. Examples 12-13, 16-20, and 27-28 comprised a peel adhesion after a 24 hour dwell time of about 3 N / cm or more. For Examples 12, 20, and 25-28, the peel adhesion after the 24 hour dwell time was greater than the peel adhesion after the 15 minute dwell time. In contrast, as shown in Table 16, Examples YY-ZZ had peel adhesion after a 15 minute dwell time and after a 24 hour dwell time less than 1 N / cm.
[0260] Examples 12-16 have different amounts of linear polymer and low refractive index acrylate with the amount of oligomer and hydroxyl-containing acrylate held constant. Examples 13-16 had coatable viscosities from 0.8 Pa-s to about 4 Pa-s. Since Example 16 had the lowest amount of linear polymer and still produced a coatable viscosity, Examples 17-20 explored compositions with similar linear polymer loadings with different amounts of the urethane-acrylate oligomer. Examples 17 and 20 had coatable viscosities from 0.7 Pa-s to about 2 Pa-s. Examples 21-28 have linear polymer loadings from 1 wt% to 5 wt% with small adjustments in the amount of the high refractive index monomer and the choice of hydroxyl-containing acrylate. Examples 21-28 had lower viscosities than Examples 13-16.
[0261] As shown in Tables 12-13, Examples 21-26 comprised an average transmittance greater than 80% (e.g., about 85% or more) after 400 seconds of UV exposure, and Examples 21-22 and 25-26 comprised an average transmittance greater than 90% (e.g., about 95% or more) after 400 seconds of UV exposure. Likewise, Examples 21-26 comprised an average transmittance greater than 80% (e.g., greaterthan 85%, greater than 90%, about 95% or more) after 700 seconds of UV exposure. In contrast, as shown in Table 15, Examples A1-A3 comprised an average transmittance of less than 80% after 400 seconds of UV exposure and an average transmittance of less than 85% after 700 seconds of UV exposure. Examples 21-26 comprised a gel fraction greater than 75% (e.g., from about 75% to about 90%, or from about 77% to about 88%). Examples YY-ZZ and A1-A3 comprised a gel fraction of about 90% or more while Examples TT-UU comprised a gel fraction less than 70% (e.g., less than 65%).
[0262] Table 16 presents the performance of Examples 23, AA, TT, UU, ZZ, and A3 after 1000 cycles (as described above). Examples 23, AA, TT, and UU withstood the 1000 cycles without creasing, delamination, or other signs of failure. Example ZZ had residual creasing that wave visible with the naked eye after cycling. Example A3 separated from (i.e., delaminated from) the PET layer (as part of the test apparatus described above). Table 16: Cycling Performance of Examples 23, AA, TT, UU, ZZ, and A3
[0263] The above observations can be combined to provide compositions, polymer-based portions, foldable apparatus comprising the same, and methods of making polymer-based portions and foldable apparatus comprising the same. Polymer-based portions can comprise a high refractive index acrylate, a low refractive index acrylate, a hydroxyl-containing acrylate, and an oligomer. Providing a low refractive index acrylate and a high refractive index acrylate can enable a predetermined refractive index of the resulting polymer-based portion to be obtained. Providing a refractive index for the polymer-based portion from about 1.48 to about 1.55 or from 1.49 to 1.52 can reduce an absolute difference of refractive index (e.g., about 0.05 or less, about 0.01 or less) between the polymer-based portion andcomponents that can be adjacent to the polymer-based portion in an application, which can reduce optical distortions.
[0264] Providing a polymer-based portion with a glass-transition temperature (e.g., about -20°C or less) outside of an operating range (e.g., from about 0°C to about 40°C, from about -10°C to about 50°C) can enable consistent properties across the operating range. Providing a glass-transition temperature (e.g., about -20°C or less) below the operating range e.g., from about 0°C to about 40°C, from about -10°C to about 50°C) can enable the polymer-based portion to operate in the rubbery plateau, where low storage moduli (E’) and low elastic modulus (E”) can be observed. Providing a low (e.g., about 1 MPa or less, or from about 0.1 MPa to about 1 MPa) storage modulus (E’) at 25°C can enable the strain between layers adjacent to the polymer-based portion to be decoupled, which can improve bending performance (e.g., parallel plate distance and / or cycles withstood to a parallel plate distance) and / or improve impact resistance. Providing a low (e.g., about 0.15 MPa or less, or from about 0.0.05 MPa to about 0.15 MPa) storage modulus (E”) at 25°C can increase an amount of recoverable strain, for example, by decreasing an amount of viscous dissipation (e.g., during bending and / or impact). Further, providing a ratio of the storage modulus (E’) at 25°C to the loss modulus (E”) at 25°C of about 2.5 or more (i.e., E” / E’ of about 0.4 or less) can increase an amount of recoverable strain, for example, by decreasing an amount of viscous dissipation (e.g., during bending and / or impact).
[0265] Providing a precursor viscosity in a range from about 0.1 Pa-s to about 10 Pa-s can enable the precursor solution to be coated on a target substrate (e.g., foldable substrate) using a variety of techniques. In aspects, a predetermined precursor viscosity can be obtained by partially curing the composition to obtain the precursor solution that can be coated before being further cured to produce the polymer-based portion. In aspects, the composition can comprise a linear polymer that enables the composition to achieve a predetermined viscosity.
[0266] Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can increase the curing rate of the composition, which can decrease processing time. Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can reduce (e.g., decrease) the use of additives, for example, rheology modifiers, and increase composition homogeneity, which can improve the quality of the resulting polymer-based portion (e.g., increasedtransmittance, decreased haze, increased mechanical properties). Providing a composition that is substantially solvent-free (e.g., entirely solvent-free) can reduce a volume change as a result of curing (e.g., shrinkage). In aspects, the composition and / or the polymer-based portion can be substantially free of fluorine-based compounds and / or free of fluorine-based compounds, which can reduce an environmental impact of the polymer-based portion and / or reduce a cost to produce the polymer-based portion.
[0267] The foldable substrate can comprise glass-based and / or ceramic- based portions, which can provide good dimensional stability, reduced incidence of mechanical instabilities, good impact resistance, and / or good puncture resistance. The foldable substrate can comprise glass-based and / or ceramic-based portions comprising one or more compressive stress regions, which can further provide increased impact resistance and / or increased puncture resistance. By providing a foldable substrate comprising a glass-based and / or ceramic-based substrate, the substrate can also provide increased impact resistance and / or puncture resistance while simultaneously facilitating good folding performance. In aspects, the substrate thickness can be sufficiently large (e.g., from about 70 micrometers (microns or µm) to about 2 millimeters) to further enhance impact resistance and puncture resistance. Providing foldable substrates comprising a central portion comprising a central thickness that is less than a substrate thickness (e.g., first thickness of the first portion and / or second thickness of the second portion) (e.g., by about 10 µm or more) can enable a small parallel plate distance (e.g., about 10 millimeters or less) based on the reduced thickness in the central portion, which can enable the foldability and / or rollability of the foldable substrate and / or foldable apparatus.
[0268] In aspects, the foldable apparatus and / or foldable substrates can comprise one or more recesses, for example, a first central surface area recessed from a first major surface by a first distance and / or a second central surface area recessed from a second major surface by a second distance. Providing a first recess opposite a second recess can provide a central thickness that is less than a substrate thickness. Further, providing a first recess opposite a second recess can reduce a maximum bend-induced strain of the foldable apparatus, for example, between a central portion and a first portion and / or second portion since the central portion comprising the central thickness can be closer to a neutral axis of the foldable apparatus and / or foldable substrates than if only a single recess was provided. Additionally, providingthe first distance substantially equal to the second distance can reduce the incidence of mechanical instabilities in the central portion, for example, because the foldable substrate is symmetric about a plane comprising a midpoint in the substrate thickness and the central thickness. Moreover, providing a first recess opposite a second recess can reduce a bend-induced strain of a material positioned in the first recess and / or second recess compared to a single recess with a surface recessed by the sum of the first distance and the second distance. Providing a reduced bend-induced strain of a material positioned in the first recess and / or the second recess can enable the use of a wider range of materials because of the reduced strain requirements for the material. For example, stiffer and / or more rigid materials can be positioned in the first recess, which can improve impact resistance, puncture resistance, abrasion resistance, and / or scratch resistance of the foldable apparatus. Additionally, controlling properties of a first material positioned in a first recess and a second material positioned in a second recess can control the position of a neutral axis of the foldable apparatus and / or foldable substrates, which can reduce (e.g., mitigate, eliminate) the incidence of mechanical instabilities, apparatus fatigue, and / or apparatus failure.
[0269] Directional terms as used herein—for example, up, down, right, left, front, back, top, bottom—are made only with reference to the figures as drawn and are not intended to imply absolute orientation.
[0270] It will be appreciated that the various disclosed aspects may involve features, elements, or steps that are described in connection with that aspect. It will also be appreciated that a feature, element, or step, although described in relation to one aspect, may be interchanged or combined with alternate aspects in various non- illustrated combinations or permutations.
[0271] It is also to be understood that, as used herein the terms “the,” “a,” or “an,” mean “at least one,” and should not be limited to “only one” unless explicitly indicated to the contrary. For example, reference to “a component” comprises aspects having two or more such components unless the context clearly indicates otherwise. Likewise, a “plurality” is intended to denote “more than one.”
[0272] As used herein, the term “about” means that amounts, sizes, formulations, parameters, and other quantities and characteristics are not and need not be exact, but may be approximate and / or larger or smaller, as desired, reflecting tolerances, conversion factors, rounding off, measurement error and the like, and other factors known to those of skill in the art. Ranges can be expressed herein asfrom “about” one particular value, and / or to “about” another particular value. When such a range is expressed, aspects include from the one particular value and / or to the other particular value. Similarly, when values are expressed as approximations, by use of the antecedent “about,” it will be understood that the particular value forms another aspect. Whether or not a numerical value or endpoint of a range in the specification recites “about,” the numerical value or endpoint of a range is intended to include two aspects: one modified by “about,” and one not modified by “about.” It will be further understood that the endpoints of each of the ranges are significant both in relation to the other endpoint and independently of the other endpoint.
[0273] The terms “substantial,” “substantially,” and variations thereof as used herein are intended to note that a described feature is equal or approximately equal to a value or description. For example, a “substantially planar” surface is intended to denote a surface that is planar or approximately planar. Moreover, as defined above, “substantially similar” is intended to denote that two values are equal or approximately equal. In aspects, “substantially similar” may denote values within about 10% of each other, for example, within about 5% of each other, or within about 2% of each other.
[0274] Unless otherwise expressly stated, it is in no way intended that any method set forth herein be construed as requiring that its steps be performed in a specific order. Accordingly, where a method claim does not actually recite an order to be followed by its steps or it is not otherwise specifically stated in the claims or descriptions that the steps are to be limited to a specific order, it is in no way intended that any particular order be inferred.
[0275] While various features, elements, or steps of particular aspects may be disclosed using the transitional phrase “comprising,” it is to be understood that alternative aspects, including those that may be described using the transitional phrases “consisting of” or “consisting essentially of,” are implied. Thus, for example, implied alternative aspects to an apparatus that comprises A+B+C include aspects where an apparatus consists of A+B+C and aspects where an apparatus consists essentially of A+B+C. As used herein, the terms “comprising” and “including”, and variations thereof shall be construed as synonymous and open-ended unless otherwise indicated.
[0276] The above aspects, and the features of those aspects, are exemplary and can be provided alone or in any combination with any one or more features of other aspects provided herein without departing from the scope of the disclosure.
[0277] It will be apparent to those skilled in the art that various modifications and variations can be made to the present disclosure without departing from the spirit and scope of the disclosure. Thus, it is intended that the present disclosure cover the modifications and variations of the aspects herein provided they come within the scope of the appended claims and their equivalents.
Claims
What is claimed is:
1. A foldable apparatus comprising: a polymer-based portion comprising: a glass-transition temperature (Tg) of about -20°C or less; a storage modulus (E’) at 25°C from about 0.1 MegaPascals to about 1 MegaPascals; and a refractive index from about 1.47 to about 1.51; a foldable substrate comprising a first major surface; and a device substrate, wherein the polymer-based portion is positioned between and contacts the first major surface of the foldable substrate and the device substrate, and a minimum thickness of the polymer-based portion is from about 5 micrometers to about 30 micrometers.
2. The polymer-based portion of claim 1, further comprising a loss modulus (E”) at 25°C of about 0.2 MegaPascals or less.
3. The polymer-based portion of any one of claims 1-2, further comprising a strain recovery of about 50% or more of an applied strain of 300%.
4. The polymer-based portion of any one of claims 1-3, further comprising a peel adhesion of about 6 N / cm or more after a 15 minute dwell time.
5. The polymer-based portion of any one of claims 1-4, wherein the peel adhesion after the 15 minute dwell time is less than another peel adhesion after a 24 hour dwell time.
6. The polymer-based portion of any one of claims 1-5, wherein the polymer- based portion can withstand 3,000 folding cycles to a parallel plate distance of 3 millimeters.
7. The polymer-based portion of any one of claims 1-6, wherein the polymer- based portion comprises a gel fraction of about 70% or more.
8. A composition comprising, as wt% of the composition: from about 65 wt% to about 75 wt% of a low refractive index acrylate comprising a refractive index less than 1.5 and at least one of an alkyl acrylate or an ether acrylate; from about 10 wt% to about 25 wt% of a high refractive index acrylate comprising a refractive index greater than 1.5; from about 10 wt% to about 25 wt% of a hydroxyl-containing acrylate; and from greater than 0 wt% to about 1 wt% of a urethane-acrylate oligomer.
9. The composition of claim 8, wherein the high refractive index acrylate is an aromatic acrylate.
10. The composition of any one of claims 8-9, wherein the high refractive index acrylate comprises biphenyl methyl acrylate.
11. The composition of any one of claims 8-10, wherein the low refractive index acrylate comprises two or more compounds.
12. The composition of any one of claims 8-11, wherein the low refractive index acrylate comprises at least one of 2-(2-ethoxyethoxy)ethyl acrylate or 2-ethylhexyl acrylate.
13. The composition of any one of claims 8-12, wherein the composition comprises a refractive index from about 1.43 to about 1.
47.
14. The composition of any one of claims 8-13, further comprising, by superaddition: from about 0.1 wt% to about 0.5 wt% of a photoinitiator; and from 0 wt% to about 0.25 wt% of a tackifier.
15. The composition of claim 14, further comprising from greater than 0 wt% to less than 0.5 wt% of a cross-linker comprising functional groups selected from acrylate, isocyanate, and compositions thereof.
16. A method of forming a foldable apparatus comprising: providing a precursor solution comprising a viscosity from about 0.1 Pascal- second to about 10 Pascal-seconds at 25°C; disposing the precursor solution on a foldable substrate; and curing the precursor solution to form a polymer-based portion on the foldable substrate, wherein the polymer-based portion comprises: an acrylate-based polymer; a glass-transition temperature (Tg) of about -20°C or less; a storage modulus (E’) at 25°C from about 0.1 MegaPascals to about 1 MegaPascals; and a refractive index from about 1.47 to about 1.
51.
17. The method of claim 16, wherein the precursor solution is formed by partially curing a mixture comprising, as a wt% of the mixture: from about 65 wt% to about 75 wt% of a low refractive index acrylate comprising a refractive index less than 1.5; from about 10 wt% to about 25 wt% of a high refractive index acrylate comprising a refractive index greater than 1.5; from about 10 wt% to about 25 wt% of a hydroxyl-containing acrylate; and from greater than 0 wt% to about 1 wt% of a urethane-acrylate oligomer.
18. The method of any one of claims 16-17, wherein the mixture comprises a photoinitiator and the precursor solution comprises more of the photoinitiator (in terms of wt% of the mixture) than the mixture.
Citation Information
Patent Citations
Methods and Apparatus Providing A Substrate and Protective Coating Thereon
US20150110990A1
Systems and methods for measuring a profile characteristic of a glass sample
US8854623B2
Polymer-based portion, adhesive, foldable apparatus, and methods of making
WO2021076434A1
Polymer-based portion, foldable apparatus, and methods of making
WO2023081350A1