Strengthened glass and methods thereof

The chemical etching process using specific etchant blends strengthens glass while preserving optical clarity, addressing the challenge of glass fracture and optical property degradation in existing methods, achieving enhanced strength and clarity without thermal or ion-exchange treatments.

WO2024249547A1PCT designated stage expired Publication Date: 2024-12-05LEHIGH UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/US2024/031541
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-31
Filing Date
2024-05-30
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Glass in various applications is prone to fracture during normal use, and existing methods to strengthen glass often compromise its optical properties, such as clarity and transparency.

Method used

A method involving a chemical etching process using an etchant blend comprising HF, HF:NH4F, HF:H2SO4, HF:NH4F:H2SO4, HF:HCl, or HF:Acetic Acid, applied at specific temperatures and times to strengthen glass without compromising its optical clarity, followed by the application of a mirror coating to the etched glass surface.

Benefits of technology

The process enhances the strength of glass significantly, achieving at least 195 MPa without degrading its optical properties, and can be completed within 60 minutes or less at room temperature, potentially replacing traditional tempering or ion-exchange methods, while maintaining superior dimensional stability and clarity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure US2024031541_05122024_PF_FP_ABST
    Figure US2024031541_05122024_PF_FP_ABST
Patent Text Reader

Abstract

Described herein is a method of strengthening a glass body comprising forming an etchant blend comprising an etchant and a carrier liquid, contacting an initial glass body with the etchant blend for a period of etching time at an etching temperature to form an etched glass body; wherein the etchant is selected from one or more of HF, HF:NH4F, HF:H2SO4, HF:NH4F:H2SO4, HF:HCl, HF:HNO3, HF:Acetic Acid, wherein the etching temperature ranges from about 20 °C to about 30 °C, and wherein the period of etching time ranges from about 10 min to about 60 min, and wherein the initial glass body has a first major surface opposite a second major surface and a side surface extending between the first major surface and the second major surface, wherein the etchant blend contacts at least the first major surface of the initial glass body.
Need to check novelty before this filing date? Find Prior Art

Description

Attorney Docket No. LEH-1096-PCT STRENGTHENED GLASS AND METHODS THEREOF CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims priority to U.S. Provisional Application Nos. 63 / 505,118, filed May 31, 2023, which is incorporated by reference in its entirety BACKGROUND

[0002] Glass in many applications may be subject to fracture during normal use. Therefore, a need exists for strengthened glass. Previous attempts to strengthen glass undermine the optical properties of the resulting article. Therefore, a need exists for strengthened glass that does not also undermine optical clarity. BRIEF SUMMARY

[0003] According to some embodiments, the present invention is directed to a method of strengthening a glass body comprising i) forming an etchant blend comprising an etchant and a carrier liquid, ii) contacting an initial glass body with the etchant blend for a period of etching time at an etching temperature to form an etched glass body; wherein the etchant is selected from one or more of HF, HF:NH4F, HF:H2SO4, HF:NH4F:H2SO4, HF:HCl, HF:HNO3, HF:Acetic Acid, wherein the etching temperature ranges from about 20 °C to about 30 °C, and wherein the period of etching time ranges from about 10 min to about 60 min, and wherein the initial glass body has a first major surface opposite a second major surface and a side surface extending between the first major surface and the second major surface, wherein the etchant blend in step ii) contacts at least the first major surface of the initial glass body.

[0004] Other embodiments of the present invention include a mirrored article comprising the previously mentioned etched glass substrate and a mirror coating applied to the etched glass substrate.

[0005] Other embodiments of the present invention include a strengthened mirrored article comprising: an acid-etched glass body comprising a first major surface opposite a second major surface and a side surface extending between the first and second major surface, wherein at least one of the first major surface and the second major surface is an acid-etched surface; and a mirror coating applied to the etched glass body, wherein the acid-etched surface is substantially free of pitting.Attorney Docket No. LEH-1096-PCT

[0006] Other embodiments of the present invention include a method of forming a strengthened mirrored article, i) providing an initial glass body having as a first major surface opposite a second major surface and a side surface extending between the first major surface and the second major surface; ii) contacting at least the first major surface of the initial glass body with an etchant blend for a period of etching time at an etching temperature to form an etched glass body, the etchant blend comprising an etchant and a carrier; iii) applying a mirror composition to one of the first major surface or the second major surface of the etched glass body; wherein the etchant is selected from one or more of HF, HF:NH4F, HF:H2SO4, HF:NH4F:H2SO4, HF:HCl, HF:HNO3, HF:Acetic Acid; and wherein no ion-exchange process is applied to the initial glass substrate or the etched glass substrate between steps ii) and iii).

[0007] Further areas of applicability of the present invention will become apparent from the detailed description provided hereinafter. It should be understood that the detailed description and specific examples, while indicating the preferred embodiment of the invention, are intended for purposes of illustration only and are not intended to limit the scope of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] The present invention will become more fully understood from the detailed description and the accompanying drawings, wherein:

[0009] FIG. 1 is top perspective view of a mirrored article according to the present invention;

[0010] FIG. 2 is a cross-sectional view of the mirrored article according to the present invention, the cross-sectional view being along the A-A line set forth in FIG. 1;

[0011] FIG. 3 is top perspective view of a mirrored article according to the present invention;

[0012] FIG. 4 is a cross-sectional view of the mirrored article according to the present invention, the cross-sectional view being along the A-A line set forth in FIG. 1; and

[0013] FIG.5 is flow-chart representing the glass-strengthening and mirror manufacturing method according to the present invention. DETAILED DESCRIPTION

[0014] The following description of the preferred embodiment(s) is merely exemplary in nature and is in no way intended to limit the invention, its application, or uses.

[0015] As used throughout, ranges are used as shorthand for describing each and every value that is within the range. Any value within the range can be selected as the terminus of the range. InAttorney Docket No. LEH-1096-PCT addition, all references cited herein are hereby incorporated by referenced in their entireties. In the event of a conflict in a definition in the present disclosure and that of a cited reference, the present disclosure controls.

[0016] Unless otherwise specified, all percentages and amounts expressed herein and elsewhere in the specification should be understood to refer to percentages by volume. The amounts given are based on the active volume of the material.

[0017] The description of illustrative embodiments according to principles of the present invention is intended to be read in connection with the accompanying drawings, which are to be considered part of the entire written description. In the description of embodiments of the invention disclosed herein, any reference to direction or orientation is merely intended for convenience of description and is not intended in any way to limit the scope of the present invention. Relative terms such as “lower,” “upper,” “horizontal,” “vertical,” “above,” “below,” “up,” “down,” “top,” and “bottom” as well as derivatives thereof (e.g., “horizontally,” “downwardly,” “upwardly,” etc.) should be construed to refer to the orientation as then described or as shown in the drawing under discussion. These relative terms are for convenience of description only and do not require that the apparatus be constructed or operated in a particular orientation unless explicitly indicated as such.

[0018] Terms such as “attached,” “affixed,” “connected,” “coupled,” “interconnected,” and similar refer to a relationship wherein structures are secured or attached to one another either directly or indirectly through intervening structures, as well as both movable or rigid attachments or relationships, unless expressly described otherwise. Moreover, the features and benefits of the invention are illustrated by reference to the exemplified embodiments. Accordingly, the invention expressly should not be limited to such exemplary embodiments illustrating some possible non- limiting combination of features that may exist alone or in other combinations of features; the scope of the invention being defined by the claims appended hereto.

[0019] According to the present application, the term “about” means + / - 1% of the reference value. According to the present application, the term “substantially free” less than about 0.1 wt. % based on the total of the referenced value.

[0020] Referring to FIGS.1 and 2, embodiments of the present invention include a mirrored article 10 comprising a glass body 100 and a mirror coating 200 applied to the glass body 100. Some embodiments of the present invention may include just the glass body 100.Attorney Docket No. LEH-1096-PCT

[0021] The mirrored article 10 may comprise a first exposed major surface 11 opposite a second exposed major surface 12. The mirrored article 10 may further comprise a side surface 13 extending between the first exposed major surfaces 11 opposite a second exposed major surface 12 of the mirrored article 10.

[0022] The mirrored article 10 may have an article thickness tA as measured between the first exposed major surface 11 and the second exposed major surface 12 of the mirrored article 10. The article thickness tAmay range from about 1.0 mm to about 2.5 mm – including all thickness and sub-ranges there-between. In some embodiments, the article thickness tA may range from about 1 mm to about 2.0 mm – including all thickness and sub-ranges there-between. In some embodiments, the article thickness tAmay be about 1.8 mm.

[0023] The glass body 100 may be a strengthened glass body 100 formed by a chemical strengthening process. The chemical strengthening process may be an etching process. The etching process may be a wet chemical etching process. The glass body 100 may be also referred to as the “strengthened glass body” or the “etched glass body” – which may be used interchangeably herein. The strengthened glass body 100 may also exhibit superior optical properties in the form of no or little to no pitting in the major surfaces.

[0024] The etched glass body 100 may comprise a first major surface 111 opposite a second major surface 112 and a side surface 113 extending between the first and second major surfaces 111, 112 of the etched glass body 100. The etched glass body 100 may have a glass thickness tG1 as measured between the first major surface 111 and the second major surface 112 of the etched glass body 100. The glass thickness tG1may range from about 0.5 mm to about 2.5 mm – including all thickness and sub-ranges there-between. In some embodiments, the glass thickness tG1 may range from about 1 mm to about 2 mm – including all thickness and sub-ranges there-between. In some embodiments, the glass thickness tG1may be about 1.8 mm.

[0025] According to the embodiments directed to the mirrored article 10, the mirror coating 200 may comprise a first major surface 211 opposite a second major surface 212 and a side surface 213 extending between the first and second major surfaces 211, 212 of the mirror coating 200. The mirror coating 200 may have a mirror thickness tM as measured between the first major surface 211 and the second major surface 212 of the mirror coating 200. In a non-limiting embodiment, the mirror thickness tMmay range from about 5 nm to about 200 nm – including all thickness and sub-ranges there-between.Attorney Docket No. LEH-1096-PCT

[0026] The etched glass body 100 may be formed of silicon dioxide (SiO2). The etched glass body 100 may be substantially transparent. The term “substantially transparent” refers to no discernable degradation in clarity when viewing between the first major surface 111 to the second major surface 112 of the etched glass body 100.

[0027] According to the embodiments directed to the mirrored article 10, the mirror coating 200 may be applied to the etched glass body 100. The mirror coating 200 may be applied directly to the etched glass body 100. The mirror coating 200 may be applied to the second major surface of the etched glass body 100. The first major surface 211 of the mirror coating 200 may be adjacent to the second major surface 112 of the etched glass body 100. The first major surface 211 of the mirror coating 200 may directly contact the second major surface 112 of the etched glass body 100.

[0028] The mirror coating 200 may comprise one or more of silver, aluminum, and combinations thereof. The mirror coating 200 may be applied to the second major surface 112 of the etched glass body 200 such that the first exposed major surface 11 of the mirrored article 10 forms a substantially reflective surface.

[0029] Referring now to FIGS. 3-5, in some embodiments, the present invention may comprise a method of forming the strengthened glass body 100. The method may comprises step 0), which comprises forming an initial glass substrate 300. The initial glass substrate 300 may comprise a first major surface 311 opposite a second major surface 312 and a side surface 313 extending between the first and second major surfaces 311, 312 of the initial glass body 100.

[0030] The initial glass body 300 may be formed by a float glass process. The first major surface 311 of the initial glass body 300 may be the tin side formed during the float glass process and the second major surface 312 may be the air side formed during the float glass process. The “air side” refers to the side of the float glass that was up or exposed to the “air” when it was manufactured and the “tin side” refers to the side of the float glass contacting the liquid tin bath while floating during such production.

[0031] Although not shown, in other embodiments, the first major surface 311 of the initial glass body 300 may be the air side formed during the float glass process and the second major surface 312 may be the tin side formed during the float glass process.

[0032] According to some embodiments of the present invention, the etching process may strengthen the air side of the initial glass body 300. According to other embodiments of the presentAttorney Docket No. LEH-1096-PCT invention, the etching process may strengthen the tin side of the initial glass body 300. According to other embodiments of the present invention, the etching process may strengthen both of the air side and the tin side of the initial glass body 300.

[0033] The method of forming the strengthened glass body 100 may further comprise step i), which is forming an etchant blend. The etchant blend may comprise an etchant and a liquid carrier. Non-limiting examples of etchant may be selected from one or more of HF, HF:NH4F, HF:H2SO4, HF:NH4F:H2SO4, HF:HCl, HF:HNO3, HF:Acetic Acid; as well as combinations thereof. In some embodiments, the etchant may be HF:Acetic Acid.

[0034] The etchant may be present in a concentration ranging from about 1 wt. % to about 50 wt. %.

[0035] In some embodiments, the etchant is a blend of HF:Acetic Acid. The HF may be present at a concentration of about 3 wt. % and the acetic acid may be present at a concentration of about 3 wt. %. The HF:Acetic Acid may be present in a volume ratio ranging from about 6:1 to about 10:1 – including all ratios and sub-ranges there-between. In some embodiments, the HF:Acetic Acid may be present in a volume ratio of about 8:1.

[0036] In some embodiments, the etchant is HF at a concentration ranging from about 1 wt. % to about 48 wt. % - including all percentages and sub-ranges there-between. In some embodiments, the etchant is HF at a concentration of about 1 wt. %. In some embodiments, the etchant is HF at a concentration of about 2 wt. %. In some embodiments, the etchant is HF at a concentration of about 3 wt. %. In some embodiments, the etchant is HF at a concentration of about 5 wt. %. In some embodiments, the etchant is HF at a concentration of about 10 wt. %. In some embodiments, the etchant is HF at a concentration of about 48 wt. %.

[0037] In some embodiments, the etchant is a blend of HF:NH4F. In a non-limiting embodiment the HF may be present in a concentration of about 48 wt. % and the NH4F may be present in a concentration of ranging from about 3 wt. % to about 40 wt. %. In some embodiments, the HF may be present in a concentration of about 48 wt. % and the NH4F may be present in a concentration of about 40 wt. %. The HF:NH4F may be present in a volume ratio ranging from about 1:7 to about 1:80 – including all ratios and sub-ranges there-between. In some embodiments, the HF:NH4F may be present in a volume ratio of about 1:7. In some embodiments, the HF:NH4F may be present in a volume ratio of about 1:8. In some embodiments, the HF:NH4F may be present in a volume ratio of about 1:20. In some embodiments, the HF:NH4F may be present in a volumeAttorney Docket No. LEH-1096-PCT ratio of about 1:50. In some embodiments, the HF:NH4F may be present in a volume ratio of about 1:80.

[0038] In some embodiments, the etchant is a blend of HF:H2SO4. In some embodiments, the HF may be present in a concentration of about 48 wt. % and the H2SO4may be present in a concentration ranging from about 1 wt. % to about 98 wt. %. In some embodiments, the HF may be present in a concentration of about 48 wt. % and the H2SO4 may be present in a concentration of about 3 wt. %. In some embodiments, the HF may be present in a concentration of about 48 wt. % and the H2SO4 may be present in a concentration of about 5 wt. %. In some embodiments, the HF may be present in a concentration of about 48 wt. % and the H2SO4 may be present in a concentration of about 10 wt. %. In some embodiments, the HF may be present in a concentration of about 48 wt. % and the H2SO4may be present in a concentration of about 98 wt. %. The HF:H2SO4 may be present in a volume ratio ranging from about 1:10 to about of about 10:1 – including all ratios and sub-ranges there-between. In some embodiments, the HF:H2SO4 may be present in a volume ratio of about 1:10. In some embodiments, the HF:H2SO4may be present in a volume ratio of about 1:7. In some embodiments, the HF:H2SO4 may be present in a volume ratio of about 8:1. In some embodiments, the HF:H2SO4 may be present in a volume ratio of about 10:1.

[0039] In some embodiments, the etchant is a blend of HF:NH4F:H2SO4.In some embodiments, the HF may be present in a concentration of about 48 wt. %, the NH4F may be present in a concentration of about 40 wt. %, and the H2SO4 may be present in a concentration of about 98 wt. %. In some embodiments, the HF:NH4F:H2SO4may be present in a volume ratio of about 2:8:70.

[0040] In some embodiments, the etchant is a blend of HF:HCl. In some embodiments, the HF may be present in a concentration of about 3 wt. % and the HCl may be present in a concentration of about at a concentration ranging from about 3 wt. %. In some embodiments, the HF:HCl may be present in a volume ratio of about 8:1.

[0041] In some embodiments, the etchant is a blend of HF:HNO3. In some embodiments, the HF may be present in a concentration of about 3 wt. % and the HNO3 may be present in a concentration of about 3 wt. %. In some embodiments, the HF:HNO3may be present in a volume ratio of about 8:1.

[0042] In some embodiments, step 0) may occur prior to step i). In some embodiments, step 0) and step i) may at least partially overlap. In some embodiments, step i) may occur prior to step 0).Attorney Docket No. LEH-1096-PCT

[0043] The method of forming the strengthened glass body 100 may further comprise step ii) which is contacting the initial glass body 300 with the etchant blend. In some embodiments, the first major surface 311 of the initial glass body 300 may be contacted with the etchant blend. In some embodiments, the second major surface 312 of the initial glass body 300 may be contacted with the etchant blend. In some embodiments, the side surface 313 of the initial glass body 300 may be contacted with the etchant blend. In some embodiments, the first major surface 311 and the second major surface 312 of the initial glass body 300 may be contacted with the etchant blend. In some embodiments, the first major surface 311, the second major surface 312, and the third major surface 313 of the initial glass body 300 may be contacted with the etchant blend.

[0044] During step ii), the contact of the etchant blend with the initial glass body 300 causing an etching reaction to occur such that the surface exposed to the etching blend to be etched.

[0045] The initial glass body 300 and the etchant blend may be contacted for a period of etching time. The period of etching time may range from about 1 minutes to about 60 minutes – including all times and sub-ranges there-between. In some embodiments, the period of etching time may range from about 10 minutes to about 50 minutes – including all times and sub-ranges there- between. In some embodiments, the period of etching time may range from about 20 min to about 40 minutes – including all times and sub-ranges there-between. In some embodiments, the period of etching time may range from about 25 minutes to about 35 minutes – including all times and sub-ranges there-between. The period of etching time may be about 30 min.

[0046] The initial glass body 300 and the etchant blend may be contacted at an etching temperature. The etching temperature may range from about 10 °C to about 40 °C – including all temperatures and sub-ranges there-between. In some embodiments, the etching temperature may range from about 20 °C to about 30 °C – including all temperatures and sub-ranges there-between. In some embodiments, the etching temperature may be room temperature (i.e., about 20 °C) – also referred to as “RT.”

[0047] Subsequent to the etching of step ii), the initial glass body 300 may be transformed into the etched glass body 100 such that the first major surface 311 of the initial glass body 300 forms the first major surface 111 of the etched glass body 100, the second major surface 312 of the initial glass body 300 forms the second major surface 112 of the etched glass body 100, and the side surface 313 of the initial glass body 300 forms the side surface 113 of the etched glass body 100.Attorney Docket No. LEH-1096-PCT

[0048] Subsequently, according to the embodiments further comprising a method of forming a strengthened mirrored article, the present invention may further comprise step iii) of applying the mirror coating 200 to the etched glass body 100. Specifically, step iii) may comprise applying the mirror coating 200 to the second major surface 112 of the etched glass body 100.

[0049] In a non-limiting embodiment, the second major surface 312 of the initial glass body 300 may be contacted with the etching blend, thereby etching the second major surface 312 of the initial glass body 300 to form the second major surface 112 of the etched glass body 100 – whereby the second major surface 312 of the initial glass body 300 is the air side formed during the float glass process. In such embodiment, the chemical strengthening process of the present invention may enhance the strength of the air side of the initial glass body 300 as it is transformed into the etched glass body 100 – whereby the etched air side of the initial glass body 300 (forming the second major surface 112 of the etched glass body 100) is subsequently coated with the mirror coating 200.

[0050] In some embodiments, the first major surface 311 of the initial glass body 300 may be contacted with the etching blend, thereby etching the first major surface 311 of the initial glass body 300 to form the first major surface 111 of the etched glass body 100 – whereby the first major surface 311 of the initial glass body 300 is the tin side formed during the float glass process. In such embodiment, the chemical strengthening process of the present invention may enhance the strength of the tin side of the initial glass body 300 as it is transformed into the etched glass body 100 – whereby the etched tin side of the initial glass body 300 (forming the first major surface 111 of the etched glass body 100) subsequently forms the first exposed major surface 11 of the mirrored article 10.

[0051] In a non-limiting alternative embodiment, the second major surface 312 of the initial glass body 300 may be contacted with the etching blend, thereby etching the second major surface 312 of the initial glass body 300 to form the second major surface 112 of the etched glass body 100 – whereby the second major surface 312 of the initial glass body 300 is the tin side formed during the float glass process. In such embodiment, the chemical strengthening process of the present invention may enhance the strength of the tin side of the initial glass body 300 as it is transformed into the etched glass body 100 – whereby the etched tin side of the initial glass body 300 (forming the second major surface 112 of the etched glass body 100) is subsequently coated with the mirror coating 200.Attorney Docket No. LEH-1096-PCT

[0052] In some embodiments, the first major surface 311 of the initial glass body 300 may be contacted with the etching blend, thereby etching the first major surface 311 of the initial glass body 300 to form the first major surface 111 of the etched glass body 100 – whereby the first major surface 311 of the initial glass body 300 is the air side formed during the float glass process. In such embodiment, the chemical strengthening process of the present invention may enhance the strength of the air side of the initial glass body 300 as it is transformed into the etched glass body 100 – whereby the etched air side of the initial glass body 300 (forming the first major surface 111 of the etched glass body 100) subsequently forms the first exposed major surface 11 of the mirrored article 10.

[0053] Referring now to FIG. 3 in particular, the method of forming the strengthened glass body 100 may comprise steps 0), i), and ii). Each step may be separated by a transition stage. In some embodiments, step 0) and step i) may be entirely separated by a first separation stage 80. In some embodiments, step i) and step ii) may be entirely separated by a second separation stage 81.

[0054] According to the embodiments comprising the method of producing a strengthened mirror article 10, step ii) and step iii) may be entirely separated by a third separation stage 81.

[0055] The first and second separation stages 80, 81 may comprise one or more sub-steps of additional processing steps that may occur during the initial formation of the float glass sheet and the formation of the etchant blend before the etching of step ii). In a non-limiting example, the first separation stage 80 and second separation stage 81 may include cutting to size the initial glass body 300 from a continuous sheet formed from the float glass process. In another non-limiting example, the first separation stage 80 and second separation stage 81 may include transporting the initial glass body 300 from a float glass plant to a separate etching facility.

[0056] In some embodiments, the first separation stage 80 and the second separation stage 81 may each be free of ion-exchange treatment of the initial glass body 300. Stated otherwise, the glass formed by the float glass process may not undergo any ion-exchange treatment during the span from the initial formation of the float glass and prior to etching – i.e., during steps 0) and i).

[0057] In some embodiments, step ii) may be free of ion-exchange treatment of the initial glass body 300.

[0058] In some embodiments, the first separation stage 80 and the second separation stage 81 may each be free of thermal treatment (e.g., annealing or tempering) of the initial glass body 300. Stated otherwise, the glass formed by the float glass process may not undergo any thermal treatmentAttorney Docket No. LEH-1096-PCT during the span from the initial formation of the float glass and prior to etching – i.e., during steps 0) and i).

[0059] In some embodiments, step ii) may be free of thermal treatment of the initial glass body 300.

[0060] The third separation stage 82 may comprise one or more sub-steps of additional processing steps that may occur after the etching process and before application of the mirror coating of step iii). In a non-limiting example, the third separation stage 82 may include cutting to size the etched glass body 100 and / or transporting the etched glass body 100 from an etching facility to a separate mirroring facility.

[0061] In some embodiments, the third separation stage 82 may be free of ion-exchange treatment of the etched glass body 100. Stated otherwise, the etched glass body 100 formed by the etching process may not subsequently undergo any ion-exchange treatment during the span from the etching and prior to mirroring – i.e., during steps ii) and iii).

[0062] In some embodiments, step iii) may be free of ion-exchange treatment of the initial glass body 300.

[0063] In some embodiments, the third separation stage 82 may be free of thermal treatment of the etched glass body 100. Stated otherwise, the etched glass body 100 formed by the etching process may not subsequently undergo any thermal treatment during the span from the etching and prior to mirroring – i.e., during steps ii) and iii).

[0064] In some embodiments, step iii) may be free of thermal treatment of the initial glass body 300.

[0065] In some embodiments, step 0), first separation stage 80, step i), second separation stage 81, step ii), third separation stage 82, and step iii) may be free of an ion-exchange treatment.

[0066] In some embodiments, step 0), first separation stage 80, step i), second separation stage 81, step ii), third separation stage 82, and step iii) may be free of a thermal treatment.

[0067] According to the present invention, the step i) forming the etching blend and step ii) of contacting the initial glass body 300 with the etchant blend has unexpectedly results in an improved method of not only increasing the strength of the resulting strengthened glass body 100, but also may do so without sacrifice of optical properties (such as clarity and transparency of the etched glass body 100 as well as superior dimensional stability) as well as may be done so within a period of etching time that is surprisingly fast – i.e., etching times of 60 minutes or less – while at anAttorney Docket No. LEH-1096-PCT etching temperature ranging from about 20 °C to about 30 °C – and can replace tempering of glass by thermal treatment, or strengthening by ion-exchange methods. It can also be integrated with these methods for further strengthening of glass.

[0068] Physical improvements in the strengthened glass body 100 may exhibit a strength of at least 195 MPa. In some embodiments, the strengthened glass body 100 may exhibit a strength of at least 200 MPa. In some embodiments, the strengthened glass body 100 may exhibit a strength ranging from about 200 MPa to about 250 MPa – including all MPa and sub-ranges there-between.

[0069] According to the present invention, the step i) forming the etching blend and step ii) of contacting the initial glass body 300 with the etchant blend has unexpectedly results in an improved method of not only increasing the strength of the resulting strengthened glass body 100, but also may do so without sacrifice of optical properties (such as clarity and transparency of the etched glass body 100) as well as may be done so within a period of etching time that is surprisingly fast – i.e., etching times of about 30 minutes or less – while at an etching temperature ranging from about 20 °C to about 30 °C – without the need for any thermal or ion-exchange treatment.

[0070] In a non-limiting embodiment, the etchant blend may comprise Acetic Acid (3%): HF (3%), at a vol. % (1:8) – whereby the etching temperature is room temperature (i.e., about 20 °C) for an etching period of time of about 30 minutes. In such embodiment, the chemical strengthening process has been surprisingly discovered to achieve the minimum strength improvement of at least 195 MPa without degradation of the optical properties necessary for the final application as a mirrored article. Examples

[0071] A number of experiments were conducted to test the glass strengthening process and resulting strengthened glass of the present invention.

[0072] Experiment 1 – HF Etchant

[0073] Table 1 below refers to an experiment based on an etchant blend using HF as the etchant in water – whereby the concentration, etching temperature, period of etching time, and resulting glass topography are listed. The term “RT” refers to room temperature.

[0074] The pitting amount is assigned a grade of 1-5. A grade of 1 refers to no pitting at all (passing grade). A grade of 2 refers to minor pitting (passing grade). A grade of 3 refers to medium pitting (failing grade). A grade of 4 refers to the majority of the glass having pitting (failing grade). A grade of 5 refers to the entirety of the glass having pitting (failing grade).Attorney Docket No. LEH-1096-PCT Table 1 Etchant Temp PeriodPittingAmount

[0075] As demonstratedy a e , e ower e concen ra on o F the less pitting in the final etched body.

[0076] Experiment 2 – HF:NH4F Etchant

[0077] Table 2 below refers to an experiment based on an etchant blend using HF:NH4F as the etchant in water – whereby the concentration, etching temperature, period of etching time, and resulting glass topography are listed. Table 2 Etchant Temp PeriodPittingAmountAttorney Docket No. LEH-1096-PCT

[0078] As demonstrated by Table 2, it has been discovered using the HF:NH4F etchant may provide superior anti-pitting properties after etchant for periods of an hour or less.

[0079] Experiment 3 – HF:H2SO4 Etchant

[0080] Table 3 below refers to an experiment based on an etchant blend using HF:H2SO4as the etchant in water –concentration, etching temperature, period of etching time, and resulting glass topography are listed. Table 3 Etchant Temp PeriodPittingAmount

[0081] As demonstrated by Table 3, it has been discovered using the HF:H2SO4 etchant may provide superior anti-pitting properties at a ratio of 1:1 up to 1:10 for a period of less than 30 minutes.

[0082] Experiment 4 – Additional EtchantsAttorney Docket No. LEH-1096-PCT

[0083] Table 4 below refers to an experiment based on a number of successful etchant blends in water – whereby the concentration, etching temperature, period of etching time, and resulting glass topography are listed. Table 4 Etchant Temp PeriodPittingAmount

[0084] As demonstrated by Table 4, additional etchants have been discovered to provide anti- pitting properties for periods of 30 minutes or less.

[0085] Experiment 5 – Strength Evaluations

[0086] Another experiment was performed to evaluate the strength of various etched samples. Each sample was evaluated for equibiaxial strength – as calculated using the below formula:

[0087] Whereby theDf – Equibiaxial strength (MPa) F – Breaking load (N) E – Modulus of elasticity (MPa) DS – Support ring diameter (mm) DL – Load ring diameter (mm) V – Poisson’s ration D – Test specimen diameter (mm)Attorney Docket No. LEH-1096-PCT

[0088] The results of each sample are provided below in Table 5. Table 5 EquibiaxiaPitting Sample lStrength (MPa)Grade

[0089] Table 5, certain etched mirrors have also exhibited superior strengthening properties – exceeding a equibiaxial strength threshold while also receiving a passing pitting grade – for instance, the etched glass bodies of Examples 4, 8, 9, 10, 11, 12, 13, 14, 15, 23, 26, 27, 28, 29, and 30.

Claims

Attorney Docket No. LEH-1096-PCT CLAIMS WHAT IS CLAIMED IS:

1. A method of strengthening a glass body comprising: i) forming an etchant blend comprising an etchant and a carrier liquid; ii) contacting an initial glass body with the etchant blend for a period of etching time at an etching temperature to form an etched glass body; wherein the etchant is selected from one or more of HF, HF:NH4F, HF:H2SO4, HF:NH4F:H2SO4, HF:HCl, HF:HNO3, HF:Acetic Acid; wherein the etching temperature ranges from about 20 °C to about 30 °C, and wherein the period of etching time ranges from about 10 min to about 60 min; wherein the initial glass body has a first major surface opposite a second major surface and a side surface extending between the first major surface and the second major surface, wherein the etchant blend in step ii) contacts at least the first major surface of the initial glass body.

2. The method according to claim 1, wherein prior to step a), the initial glass body is formed from a float glass process.

3. The method according to any one of claims 1 to 2, wherein the etchant blend in step ii) contacts the second major surface of the initial glass body.

4. The method according to claim 3, wherein the etchant blend in step ii) contacts the side surface of the initial glass body.

5. The method according to any one of claims 3 to 4, wherein the initial glass body has an initial thickness as measured between the first major surface and the second major surface, the initial thickness ranging from about 1.0 mm to about 2.0 mm.

6. The method according to any one of claims 1 to 5, wherein the period of etching time ranges from about 20 minutes to about 40 minutes.Attorney Docket No. LEH-1096-PCT 7. The method according to claim 6, wherein the period of etching time ranges from about 25 minutes to about 35 minutes.

8. The method according to any one of claims 1 to 7, wherein the etchant is a blend of HF:Acetic Acid, the HF at a concentration of about 3 wt. % and the Acetic Acid at a concentration of about 3 wt. %, whereby the HF:Acetic Acid are present in a volume ratio of about 8:

1.

9. The method according to any one of claims 1 to 7, wherein the etchant is HF at a concentration ranging from about 1 wt. % to about 48 wt. %.

10. The method according to any one of claims 1 to 7, wherein the etchant is HF:NH4F, the HF at a concentration of about 48 wt. % and the NH4F at a concentration of about 40 wt. %, and the HF:NH4F at a volume ratio ranging from about 1:7 to about 1:

80.

11. The method according to any one of claims 1 to 7, wherein the etchant is HF:NH4F, the HF at a concentration of about 3 wt. % and the NH4F at a concentration of about 3 wt. %, and the HF:NH4F at a volume ratio ranging from about 8:

1.

12. The method according to any one of claims 1 to 7, wherein the etchant is HF:H2SO4, the HF at a concentration of about 1 wt. % to about 48 wt. % and the H2SO4at a concentration ranging from about 1 wt. % to about 98 wt. %, and the HF:H2SO4at a volume ratio ranging from about 1:10 to about 10:

1.

13. The method according to claim 12, wherein the concentration of HF is about 1 wt. % and the concentration of H2SO4 is about 1 wt. % and the volume ratio of HF:H2SO4 is about 1:

1.

14. The method according to any one of claims 1 to 7, wherein the etchant is HF:H2SO4, the HF at a concentration of about 1 wt. % to 48 wt. % and the H2SO4 at a concentration ranging from about 1 wt. % to about 98 wt. %, and the HF:H2SO4 at a volume ratio ranging from about 1:10 to about 10:1.Attorney Docket No. LEH-1096-PCT 15. The method according to claim 14, wherein the concentration of HF is about 1 wt. % and the concentration of H2SO4 is about 1 wt. % and the volume ratio of HF:H2SO4 is about 1:

1.

16. The method according to any one of claims 1 to 7, wherein the etchant is HF:NH4F:H2SO4,and the HF is present in a concentration of about 48 wt. %, the NH4F is present in a concentration of about 40 wt. %, the H2SO4 is present in a concentration of about 98 wt. %, and the HF:NH4F:H2SO4 is present in a volume ratio of about 2:8:

70.

17. The method according to any one of claims 1 to 7, wherein the etchant is HF:HCl, the HF present in a concentration of about 3 wt. %, the HCl present in a concentration of about 3 wt. %, and the HF:HCl present in a volume ratio of about 8:

1.

18. The method according to any one of claims 1 to 7, wherein the etchant is HF:HNO3, the HF present in a concentration of about 3 wt. %, the HNO3present in a concentration of about 3 wt. %, and the HF:HNO3 present in a volume ratio of about 8:

1. .

19. The method according to any one of claims 1 to 18, wherein the initial glass body of step ii) has not been treated by an ion-exchange process.

20. The method according to any one of claims 1 to 19, wherein the first major surface of the initial glass body forms a first major surface of the etched glass body, the second major surface of the initial glass body forms a second major surface of the etched glass body, and the side surface of the initial glass body forms a side surface of the etched glass body.

21. A method of forming a strengthened mirrored article, wherein the subsequent to step ii) of claim 16, further comprising step iii) applying a mirror composition to one of the first major surface or the second major surface of the etched glass body.

22. The method of forming a strengthened mirrored article according to claim 21, wherein no ion- exchange process is applied to the initial glass substrate or the etched glass substrate between steps ii) and iii).Attorney Docket No. LEH-1096-PCT 23 A mirrored article comprising: the etched glass body formed by the method according to any one of claims 1 to 22; and a mirror coating applied to the etched glass body.

24. A mirrored article comprising: an acid-etched glass body comprising a first major surface opposite a second major surface and a side surface extending between the first and second major surface, wherein at least one of the first major surface and the second major surface is an acid-etched surface; and a mirror coating applied to the etched glass body; wherein the acid-etched surface is substantially free of pitting.

25. The mirrored article according to claim 24, wherein the acid-etched surface is free of ion- exchange treatment.

26. The mirrored article according to any one of claims 24 to 25, wherein the acid-etched surface comprising a content of silicon (Si), oxygen (O), sodium (Na), calcium (Ca), and magnesium (Mg); and wherein a first ratio of the O / Si ranges from about 2.5:1 to about 2.8:

1.

27. The mirrored article according to claim 26, wherein a second ratio of Na / Si ranges from about 0.35:1 to about 0.55:

1.

28. The mirrored article according to any one of claims 26 to 27, wherein a third ratio of Mg / Si ranges from about 0.05:1 to about 0.13:

1.

29. The mirrored article according to any one of claims 26 to 28, wherein the Si is present in the acid-etched surface in an amount ranging from about 21.9 wt. % to about 22.9 wt. %.

30. The mirrored article according to any one of claims 26 to 29, wherein the O is present in the acid-etched surface in an amount ranging from about 59.3 wt. % to about 60.4 wt. %Attorney Docket No. LEH-1096-PCT 31. A method of forming a strengthened mirrored article, i) providing an initial glass body having as a first major surface opposite a second major surface and a side surface extending between the first major surface and the second major surface; ii) contacting at least the first major surface of the initial glass body with an etchant blend for a period of etching time at an etching temperature to form an etched glass body, the etchant blend comprising an etchant and a carrier; iii) applying a mirror composition to one of the first major surface or the second major surface of the etched glass body; wherein the etchant is selected from one or more of HF, HF:NH4F, HF:H2SO4, HF:NH4F:H2SO4, HF:HCl, HF:HNO3, HF:Acetic Acid; and wherein no ion-exchange process is applied to the initial glass substrate or the etched glass substrate between steps ii) and iii).

32. The method according to claim 31, wherein the etching temperature ranges from about 20 °C to about 30 °C.

33. The method according to any one of claims 31 to 32, wherein the period of etching time ranges from about 10 min to about 50 min.

34. The method according to any one of claims 31 to 33, wherein the initial glass body is formed from a float glass process.

35. The method according to any one of claims 31 to 34, wherein the etchant blend in step ii) contacts the second major surface of the initial glass body.

36. The method according to claim 35, wherein the etchant blend in step ii) contacts the side surface of the initial glass body.

37. The method according to any one of claims 31 to 36, wherein the initial glass body has an initial thickness as measured between the first major surface and the second major surface, the initial thickness ranging from about 1.0 mm to about 2.0 mm.Attorney Docket No. LEH-1096-PCT 38. The method according to any one of claims 33 to 37, wherein the period of etching time ranges from about 20 minutes to about 40 minutes.

39. The method according to claim 38, wherein the period of etching time ranges from about 25 minutes to about 35 minutes.

40. The method according to any one of claims 31 to 39, wherein the etchant is a blend of HF:Acetic Acid, the HF at a concentration of about 3 wt. % and the Acetic Acid at a concentration of about 3 wt. %, whereby the HF:Acetic acid are present in a volume ratio of about 8:

1.

41. The method according to any one of claims 31 to 39, wherein the etchant is HF at a concentration ranging from about 1 wt. % to about 48 wt. %.

42. The method according to any one of claims 31 to 39, wherein the etchant is HF:NH4F, the HF at a concentration of about 48 wt. % and the NH4F at a concentration of about 40 wt. %, and the HF:NH4F at a volume ratio ranging from about 1:7 to about 1:

80.

43. The method according to any one of claims 31 to 39, wherein the etchant is HF:H2SO4, the HF at a concentration of about 48 wt. % and the H2SO4at a concentration ranging from about 1 wt. % to about 98 wt. %, and the HF:H2SO4at a volume ratio ranging from about 1:10 to about 10:

1.

44. The method according to any one of claims 31 to 39, wherein the etchant is HF:NH4F:H2SO4, and the HF is present in a concentration of about 48 wt. %, the NH4F is present in a concentration of about 40 wt. %, the H2SO4 is present in a concentration of about 98 wt. %, and the HF:NH4F:H2SO4 is present in a volume ratio of about 2:8:

70.

45. The method according to any one of claims 31 to 39, wherein the etchant is HF:HCl, the HF present in a concentration of about 3 wt. %, the HCl present in a concentration of about 3 wt. %, and the HF:HCl present in a volume ratio of about 8:1.Attorney Docket No. LEH-1096-PCT 46. The method according to any one of claims 31 to 39, wherein the etchant is HF:HNO3,the HF present in a concentration of about 3 wt. %, the HNO3 present in a concentration of about 3 wt. %, and the HF:HNO3 present in a volume ratio of about 8:1.

Citation Information

Patent Citations

  • Glass etchant liquid, glass etching method, glass substrate for flat panel display and flat panel display

    JP2005179132A

  • Method for extracting sodium elements from glass surface

    US20010040143A1

  • Method of manufacturing glass substrate for magnetic recording media

    US20120100786A1

  • Alkali-free glass substrate and method for reducing thickness of alkali-free glass substrate

    US20150072130A1

  • Glass mirror apparatus and methods of manufacturing a glass mirror apparatus

    US20160004033A1