Phototransistor having perovskite dielectric layer, and manufacturing method therefor

By using a phototransistor with a wide-bandgap organic-inorganic hybrid perovskite dielectric layer and an organic semiconductor channel layer, the problem of high fabrication cost in existing technologies has been solved, realizing low-cost and high-efficiency ultraviolet/deep ultraviolet light detection, which is suitable for large-scale production and commercial applications.

WO2026232715A1PCT designated stage Publication Date: 2026-11-12HUNAN UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2025/115965
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-07
Filing Date
2025-08-20
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing ultraviolet/deep ultraviolet phototransistors using wide-bandgap metal oxides or III-V compound semiconductor materials are expensive and complex to fabricate, making it difficult to achieve low-cost, high-efficiency ultraviolet/deep ultraviolet light detection.

Method used

A phototransistor was fabricated using a wide-bandgap organic-inorganic hybrid perovskite as the dielectric layer and an organic semiconductor as the channel layer, through solution spin coating and low-temperature annealing, and then combined with dry transfer technology to form a bottom gate structure.

Benefits of technology

It achieves low-cost, large-scale production of ultraviolet/deep ultraviolet light detection, and the device operates normally at extremely low voltage, exhibiting good versatility and sensitive light response performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2025115965_12112026_PF_FP_ABST
    Figure CN2025115965_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a phototransistor having a perovskite dielectric layer, and a manufacturing method therefor. The phototransistor has a bottom-gate structure, and comprises a gate electrode, a dielectric layer, a channel layer, a source electrode, and a drain electrode; the dielectric layer comprises wide-bandgap organic-inorganic hybrid perovskite; the channel layer comprises an organic semiconductor; and the channel layer is on the dielectric layer. The phototransistor of the present invention can be manufactured by a simple solution spin-coating method; a manufacturing process that can be implemented by using only one spin coater is simpler, is compatible with a flexible substrate, and is suitable for large-scale commercial applications; in addition, the phototransistor can work normally at an extremely low voltage (<2 V); and the phototransistor has good versatility and low-voltage operation characteristics, so that the phototransistor has a broad application prospect in the field of ultraviolet / deep-ultraviolet photodetection.
Need to check novelty before this filing date? Find Prior Art

Description

A phototransistor with a perovskite dielectric layer and its fabrication method Technical Field

[0001] This invention belongs to the field of organic-inorganic hybrid perovskite field-effect transistors, and more specifically, relates to field-effect transistors using perovskite as the dielectric layer. Background Technology

[0002] Ultraviolet / deep ultraviolet photodetectors are crucial in fields such as communications, missile early warning, astronomy, weather forecasting, fire detection, marine pollution monitoring, and biomedicine, and have received considerable attention in recent years. Among these detectors, phototransistors have advantages over photodiodes due to their signal amplification capabilities, low noise, and excellent switching characteristics. Most phototransistors rely on semiconductors with a bandgap greater than 3 eV as the channel layer to detect ultraviolet / deep ultraviolet light. These semiconductor materials mainly include metal oxides (such as Ga2O3 and SnO2). x These materials include group IgZO and III-V compounds (such as ZnSe, AlN, and BN). However, the preparation of these materials typically requires expensive equipment and stringent conditions (such as vacuum or high temperature), which is not conducive to large-scale production and cost reduction.

[0003] In contrast, metal halide perovskites (MHPs) possess high absorption coefficients, enabling strong light absorption even in very thin films. Their long carrier diffusion lengths also facilitate efficient charge extraction, reducing losses. The solution-processable nature of MHPs significantly reduces manufacturing costs, making them suitable for mass production. By adjusting their composition, the optical bandgap can be adjusted from 1.5 eV to over 3 eV, demonstrating great potential in ultraviolet / deep ultraviolet phototransistors. However, using wide-bandgap MHPs as transistor channel layers faces challenges in charge injection and transport, hindering the achievement of high-performance devices and limiting their widespread application in ultraviolet / deep ultraviolet phototransistors. Summary of the Invention

[0004] The purpose of this invention is to overcome the above-mentioned problems and provide a novel phototransistor concept to achieve low-cost and high-efficiency ultraviolet / deep ultraviolet light detection.

[0005] Therefore, in the first aspect, the present invention solves the technical problem by adopting the following technical solution: a perovskite dielectric layer phototransistor, characterized in that the transistor has a bottom gate structure, the transistor includes a gate electrode, a dielectric layer, a channel layer, a source electrode, and a drain electrode; the dielectric layer is a wide-bandgap organic-inorganic hybrid perovskite; the channel layer is an organic semiconductor; and the channel layer is on the dielectric layer.

[0006] Furthermore, the wide-bandgap organic-inorganic hybrid perovskite is a quasi-two-dimensional perovskite with a bandgap greater than 3.0 eV.

[0007] Furthermore, the quasi-two-dimensional perovskite is A2MZ4 (A = (PEA)). x (BA) y M = Pb x Sn y Z = Br x Cl y (x+y=1).

[0008] Furthermore, the thickness of the perovskite dielectric layer ranges from 80 nm to 200 nm. If the dielectric layer is too thin, leakage current will increase significantly, while if it is too thick, capacitance will decrease, increasing the operating voltage to some extent and thus increasing device power consumption.

[0009] Correspondingly, the present invention provides a method for fabricating a phototransistor with a perovskite dielectric layer, wherein the transistor has a bottom gate structure, and the fabrication method includes the following steps:

[0010] 1) Prepare a wide-bandgap organic-inorganic hybrid perovskite solution.

[0011] 2) A wide-bandgap organic-inorganic hybrid perovskite solution is spin-coated onto a substrate containing electrodes and then annealed at low temperature to form a dielectric layer.

[0012] 3) An organic semiconductor is deposited onto the dielectric layer to form a channel layer.

[0013] Furthermore, the electrodes are gate electrodes, source electrodes, and drain electrodes.

[0014] Furthermore, the electrode is a gate electrode, and a source electrode and a drain electrode are fabricated on the channel layer.

[0015] Furthermore, the wide-bandgap organic-inorganic hybrid perovskite is a quasi-two-dimensional perovskite with a bandgap greater than 3.0 eV.

[0016] Furthermore, the quasi-two-dimensional perovskite is A2MZ4 (A = (PEA)). x (BA) y M = Pb x Sn y Z = Br x Cl y (x+y=1).

[0017] Furthermore, the trench layer deposition method is a dry transfer method. Dry transfer can protect the dielectric layer from solvent damage that could lead to leakage.

[0018] Furthermore, the spin coating speed of the perovskite precursor solution is 4000-6000 rpm, and the annealing temperature is 100 ℃-150 ℃. If the spin coating speed or annealing temperature deviates from the above range, it is easy to cause poor crystallinity of the perovskite film, which may cause the device to break down during operation.

[0019] Organic semiconductors can be replaced with other semiconductors that can be deposited by transfer methods, such as two-dimensional semiconductors, oxide semiconductors, perovskite semiconductors, etc.

[0020] The above technical solution has the following technical effects:

[0021] (1) This invention proposes a phototransistor with a perovskite dielectric layer. Current ultraviolet / deep ultraviolet light detection typically requires the fabrication of wide-bandgap metal oxides or III-V compound semiconductors as the channel layer, and the fabrication processes for these materials are expensive and complex. Our proposed novel structure solves this problem, as it can be fabricated using a simple solution spin-coating method and operates normally at extremely low voltages (<2V).

[0022] (2) The perovskite dielectric layer phototransistor fabrication method provided by the present invention is simple. The perovskite dielectric layer is formed by spin coating the corresponding solution and then annealing at low temperature. The semiconductor layer is also formed on the PDMS substrate by spin coating and then transferred to the perovskite dielectric layer. This fabrication process, which can be carried out using only one spin coater, is simpler and compatible with flexible substrates, making it suitable for large-scale commercial applications.

[0023] (3) The perovskite dielectric layer phototransistor provided by the present invention can be fabricated over a large area, exhibiting good versatility and low voltage operation characteristics, making it a promising candidate for application in the field of ultraviolet / deep ultraviolet photodetection. Attached Figure Description

[0024] Figure 1 is a schematic diagram of a phototransistor with a perovskite dielectric layer in Embodiment 1 of the present invention;

[0025] Figure 2 shows the phototransistor transfer characteristics of the perovskite dielectric layer in Embodiment 1 of the present invention.

[0026] Figure 3 shows the transfer characteristics of the phototransistor with the perovskite dielectric layer in Embodiment 1 of the present invention under ultraviolet light irradiation.

[0027] Figure 4 shows the ultraviolet light response time of the phototransistor with the perovskite dielectric layer in Embodiment 1 of the present invention;

[0028] Figure 5 shows the phototransistor transfer characteristic curve of the perovskite dielectric layer in Embodiment 2 of the present invention.

[0029] Figure 6 shows the transfer characteristic curves of the perovskite dielectric layer phototransistor in Embodiment 2 of the present invention under deep ultraviolet light irradiation.

[0030] Figure 7 shows the deep ultraviolet light response time of the phototransistor with the perovskite dielectric layer in Embodiment 2 of the present invention;

[0031] Figure 8 is a flowchart of the phototransistor fabrication process of the perovskite dielectric layer in Embodiment 3 of the present invention. Embodiments of the present invention

[0032] To more clearly illustrate the purpose and advantages of the present invention, the following embodiments, in conjunction with the accompanying drawings, will provide a more detailed description of the invention. The specific embodiments described below are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0033] Example 1

[0034] A phototransistor with a perovskite dielectric layer is provided. Using PEA2PbBr4 as the dielectric layer, a phototransistor that responds to 405 nm ultraviolet light can be made using an organic semiconductor that has no photoresponse.

[0035] Referring to Figure 1, a perovskite dielectric layer phototransistor, from bottom to top, consists of a gate electrode (Si... ++ It consists of a 140 nm perovskite dielectric layer (PEA2PbBr4), a 100 nm organic semiconductor channel layer (PDVT-10), and 100 nm source (Ag) and drain (Ag) electrodes.

[0036] Referring to Figure 2, the electrical test of the perovskite dielectric layer phototransistor shows that it exhibits good transistor transfer characteristics at room temperature, and the device can operate at extremely low voltages (<2V).

[0037] Referring to Figures 3 and 4, the transfer characteristic curves under illumination show that the perovskite dielectric layer phototransistor achieves a power density of 0.05 mW / cm². 2 Under 405 nm ultraviolet light irradiation, the device exhibits strong photoresponse behavior, with the device current increasing with increasing light intensity; at the same time, the rise time and decay time of the response are 22 ms and 23 ms, respectively, demonstrating sensitive photodetection performance.

[0038] Example 2

[0039] A phototransistor with a perovskite dielectric layer is provided. Taking PEA2PbCl4 as the dielectric layer as an example, a phototransistor that responds to 265 nm deep ultraviolet light can be made using an organic semiconductor that has no photoresponse.

[0040] A perovskite dielectric layer phototransistor, from bottom to top, has a gate electrode (Si) ++ It consists of an 80 nm perovskite dielectric layer (PEA2PbCl4), a 100 nm organic semiconductor channel layer (PDVT-10), and 100 nm source (Ag) and drain (Ag) electrodes.

[0041] Referring to Figure 5, the electrical tests of the perovskite dielectric layer phototransistor show that it exhibits the standard P-type transistor transfer characteristic curve at room temperature, and the device can also operate at extremely low voltages (<2V).

[0042] Referring to Figures 6 and 7, the device demonstrates its photodetection performance under 265 nm illumination. Under illumination from a 265 nm light source at different power densities, the device exhibits distinct photoresponse characteristics, with photoresponse times all around 23 ms, demonstrating extremely sensitive deep ultraviolet light detection capabilities.

[0043] Example 3

[0044] Correspondingly, this embodiment provides a method for fabricating a phototransistor with a perovskite dielectric layer. Taking a bottom-gate top-electrode transistor as an example, PEA2PbBr4 and PDVT-10 are used as the dielectric layer and semiconductor layer, respectively, to fabricate the phototransistor.

[0045] 1) Preparation of PEA2PbBr4 perovskite dielectric layer solution: Dissolve PEABr / PbBr2 in DMF at a molar ratio of 2:1 to prepare a 0.1 M concentration PEA2PbBr4 precursor solution. Then heat on a hot plate at 70 °C for two hours until fully dissolved to obtain the PEA2PbBr4 perovskite dielectric layer solution. Other perovskite dielectric layer precursor solutions can be prepared similarly. For example, PEACl / SnCl2 or PEACl / PbCl2 can be dissolved in DMF or DMSO at a molar ratio of 2:1 to prepare 0.1 M concentration PEA2SnCl4 and PEA2PbCl4 precursor solutions, respectively. Then heat on a hot plate at 70 °C for two hours until fully dissolved to obtain the corresponding perovskite solution.

[0046] 2) Spin-coating a wide-bandgap organic-inorganic hybrid perovskite solution onto a substrate containing electrodes and then annealing at low temperature to form a dielectric layer: This involves placing a heavily doped silicon wafer (Si...) on the substrate. ++The substrate (with gate electrode) was ultrasonically cleaned sequentially with deionized water, acetone, and isopropanol for 1 min, and then dried with an argon gun. The substrate was then transferred to an ozone treatment device for 15 min to alter the wettability of the substrate surface, which is beneficial for subsequent thin film deposition. The PEA2PbBr4 perovskite dielectric layer solution prepared in step 1 was spin-coated onto the treated substrate at 4000 rpm for 30 s, followed by annealing at 100 °C for 5 min to form the dielectric layer.

[0047] 3) Depositing organic semiconductors onto the dielectric layer to form a channel layer: Dissolve PDVT-10 in chlorobenzene solvent at a concentration of 5 g / L, heat at 60 °C to dissolve and form a PDVT-10 semiconductor solution, and then spin-coat the PDVT-10 semiconductor solution onto the PDMS substrate. No annealing treatment of the semiconductor layer is required. Press the side with PDVT-10 directly onto the annealed perovskite film, and then lift the PDMS to transfer PDVT-10 onto the perovskite to form a channel layer.

[0048] 4) Fabricate source and drain electrodes on the channel layer: deposit 100 nm of Ag on the channel layer using a mask as source and drain electrodes to complete the fabrication of the phototransistor with the perovskite dielectric layer.

[0049] The above specific examples illustrate the present invention and are merely for the purpose of aiding understanding, not limiting the scope of the invention. Those skilled in the art can make various simple deductions, modifications, or substitutions based on the concept of the present invention. These deductions, modifications, or substitutions also fall within the scope of the claims of this invention.

Claims

1. A phototransistor with a perovskite dielectric layer, characterized in that, The transistor has a bottom-gate structure and includes a gate electrode, a dielectric layer, a channel layer, a source electrode, and a drain electrode. The dielectric layer is a wide-bandgap organic-inorganic hybrid perovskite. The channel layer is an organic semiconductor. The channel layer is located on the dielectric layer.

2. The phototransistor with a perovskite dielectric layer according to claim 1, characterized in that, The wide-bandgap organic-inorganic hybrid perovskite is a quasi-two-dimensional perovskite with a bandgap greater than 3.0 eV.

3. A phototransistor with a perovskite dielectric layer according to claim 2, characterized in that, The quasi-two-dimensional perovskite is A2MZ4 (A = (PEA)). x (BA) y M = Pb x Sn y Z = Br x Cl y (x+y=1).

4. A phototransistor with a perovskite dielectric layer according to any one of claims 1-3, characterized in that, The thickness of the perovskite dielectric layer ranges from 80 nm to 200 nm.

5. A method for fabricating a phototransistor with a perovskite dielectric layer, characterized in that, The transistor has a bottom-gate structure, and the fabrication method includes the following steps: 1) Preparation of wide-bandgap organic-inorganic hybrid perovskite solution; 2) A wide-bandgap organic-inorganic hybrid perovskite solution is spin-coated onto a substrate containing electrodes and then annealed at low temperature to form a dielectric layer; 3) An organic semiconductor is deposited onto the dielectric layer to form a channel layer.

6. The method for fabricating a phototransistor with a perovskite dielectric layer according to claim 5, characterized in that, The electrode is a gate electrode, a source electrode, or a drain electrode; or the electrode is a gate electrode, and the source electrode and drain electrode are fabricated on the channel layer.

7. A method for fabricating a phototransistor with a perovskite dielectric layer according to any one of claims 5-6, characterized in that, The wide-bandgap organic-inorganic hybrid perovskite is a quasi-two-dimensional perovskite with a bandgap greater than 3.0 eV.

8. The method for fabricating a phototransistor with a perovskite dielectric layer according to claim 7, characterized in that, The quasi-two-dimensional perovskite is A2MZ4 (A = (PEA)). x (BA) y M = Pb x Sn y Z = Br x Cl y (x+y=1).

9. A method for fabricating a phototransistor with a perovskite dielectric layer according to any one of claims 5-8, characterized in that, The channel layer deposition method is a dry transfer method.

10. A method for fabricating a phototransistor with a perovskite dielectric layer according to any one of claims 5-9, characterized in that, The spin coating speed of the perovskite precursor solution is 4000-6000 rpm, and the annealing temperature is 100 ℃-150 ℃.