Potassium ferrate composite environmental remediation material, and preparation method therefor and use thereof
The preparation of potassium ferrate composite environmental remediation material has solved the problems of limited oxidation capacity and poor stability, and has achieved efficient pollutant removal and antibacterial functions, making it suitable for the remediation of polluted water bodies and soil.
Patent Information
- Application Number
- PCT/CN2026/090968
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-04-16
- Publication Date
- 2026-11-12
AI Technical Summary
Existing environmental remediation materials have limited oxidation capacity and a single scope of application. Potassium ferrate has poor stability and a complex preparation process, making it difficult to achieve large-scale application.
Potassium ferrate composite environmental remediation material is used. The preparation process involves combining potassium ferrate with a porous carrier and a stabilizer. The process includes the synthesis of potassium ferrate by sodium hypochlorite oxidation, carrier modification and calcination, forming stable porous composite particles.
The stability and oxidation capacity of potassium ferrate have been improved, enabling broad-spectrum removal of pollutants and simultaneous antibacterial function, extending the shelf life of the material, and making it suitable for the remediation of polluted water bodies and soil.
Abstract
Description
A potassium ferrate composite environmental remediation material, its preparation method and application Technical Field
[0001] This invention belongs to the field of environmental functional materials technology, specifically relating to a composite environmental remediation material with potassium ferrate (K2FeO4) as the core component, its preparation method and application, which is suitable for the synergistic treatment of heavy metals, organic pollutants and microorganisms in polluted water bodies and soil. Background Technology
[0002] Traditional environmental remediation materials (such as activated carbon, zero-valent iron, and Fenton's reagent) have drawbacks such as limited oxidation capacity, easy generation of secondary pollution, and limited scope of action. For example, activated carbon only has adsorption function and cannot degrade pollutants; zero-valent iron is easily passivated and deactivated, producing secondary pollution of iron sludge; Fenton's reagent requires strict pH control and produces a large amount of iron-containing sludge.
[0003] Although potassium ferrate has strong oxidizing properties (oxidation potential up to +2.2V) and flocculation function, its long-term effectiveness is easily reduced when used alone due to poor stability and rapid reaction. Its decomposition half-life at room temperature is only 2-3 hours.
[0004] In addition, existing potassium ferrate preparation processes are complex and have low yields. The traditional ferric chloride method has a yield of less than 40%, making it difficult to achieve large-scale application.
[0005] Therefore, there is an urgent need to develop environmental remediation materials that combine high stability, strong removal capacity, and feasibility for large-scale production. Summary of the Invention
[0006] To address the aforementioned issues, this invention provides a potassium ferrate composite environmental remediation material, its preparation method, and its application. This composite environmental remediation material, with potassium ferrate (K2FeO4) as its core component, solves the technical problems of limited oxidation capacity, limited scope of action, and poor stability of potassium ferrate when used alone in existing environmental remediation materials. It improves the stability of potassium ferrate (shelf life ≥ 6 months) and simplifies the preparation process.
[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0008] On the one hand, this invention proposes a potassium ferrate composite environmental remediation material, comprising the following components and their mass percentages:
[0009] Potassium ferrate 40-70%;
[0010] Porous carrier 20-50%;
[0011] Stabilizer 5-10%;
[0012] The functions and mechanisms of each component are as follows:
[0013] Potassium ferrate: a hexavalent iron salt with strong oxidizing properties, can treat a variety of pollutants (phenols, drugs, toxins, etc.) and microorganisms (viruses, bacteria, etc.) through oxidation, disinfection and flocculation, with guaranteed safety, short reaction time and no secondary pollution.
[0014] Porous carrier: High specific surface area and controllable pore size distribution can optimize mass transfer rate and ensure the continuous and stable oxidation of potassium ferrate. At the same time, the porous carrier has adsorption effect, which can synergistically enhance the decontamination ability of potassium ferrate.
[0015] Stabilizer: Adding stabilizers effectively reduces the natural decomposition rate of potassium ferrate and improves its service life.
[0016] In a further technical solution, the porous carrier is one of activated carbon, zeolite, and biochar; the stabilizer is sodium silicate or polyvinyl alcohol.
[0017] On the other hand, the present invention also proposes a method for preparing the potassium ferrate composite environmental remediation material as described above, comprising the following processes:
[0018] S1: Potassium ferrate synthesis: Potassium ferrate was synthesized by sodium hypochlorite oxidation method;
[0019] S2: Modification of porous carrier: After acid washing and activation, the porous carrier is immersed in a stabilizer solution and then dried for later use;
[0020] S3: Composite Loading: The potassium ferrate powder obtained in step S1 is mixed with the modified porous carrier in the above proportion, then a binder is added, the mixture is ball-milled for a period of time, pressed into tablets, and then calcined in an inert atmosphere to obtain porous composite particles, i.e., the environmental remediation material.
[0021] In a further technical solution, step S1 specifically involves: mixing an iron salt solution with a strong alkaline solution, slowly adding sodium hypochlorite dropwise at low temperature, reacting to generate K2FeO4 precipitate, centrifuging and then vacuum drying.
[0022] In a further technical solution, the iron salt is FeCl3 or Fe(NO3)3, the strongly alkaline solution is a mixed solution of NaOH and KOH, and the low-temperature condition is 0-5℃. The relevant reaction process for step S1 is as follows:
[0023] 1. Synthesis of sodium ferrate (Na2FeO4)
[0024] Under strongly alkaline conditions, sodium hypochlorite (NaClO) oxidizes ferric compounds (such as FeCl3 or Fe(NO3)3) to sodium ferrate in the presence of a co-catalyst, as shown in the following reaction:
[0025] 3NaClO+2FeCl3+10NaOH→2Na2FeO4+9NaCl+5H2O
[0026] or
[0027] 3NaClO+2Fe(NO3)3+10NaOH→2Na2FeO4+3NaCl+6NaNO3+5H2O
[0028] Key point: Fe 3+ Oxidized to Fe 6+ NaClO is used as the oxidant; the reaction needs to be carried out in an alkaline medium, NaOH provides OH⁻ and neutralizes acidic byproducts, and the auxiliary catalyst promotes the forward reaction and improves the reaction yield in the formation of potassium ferrate; the auxiliary catalyst is nano-TiO₂ or Fe₃O₄.
[0029] 2. Conversion to potassium ferrate (K2FeO4)
[0030] Sodium ferrate reacts with potassium hydroxide (KOH) via a metathesis reaction to produce potassium ferrate.
[0031] Na₂FeO₄ + 2KOH → K₂FeO₄ + 2NaOH
[0032] Key point: This reaction is a double displacement reaction. Because the solubility product (Ksp) of K₂FeO₄ is less than that of Na₂FeO₄, it precipitates more easily at low temperatures. In actual production, temperature, concentration, and other conditions need to be controlled to improve the yield.
[0033] In a further technical solution, in step S2, the porous carrier is activated by acid washing with 5% HNO3 and dried at a temperature of 60-80℃.
[0034] In a further technical solution, the adhesive is hydroxymethyl cellulose.
[0035] In a further technical solution, the ball milling time in step S3 is 2-4 hours, the inert atmosphere is N2 atmosphere, and the calcination process is: calcination at 300-400℃ for 1-2 hours.
[0036] Thirdly, this invention also proposes the application of the above-mentioned potassium ferrate composite environmental remediation material in the remediation of polluted water bodies and soil.
[0037] This invention discloses a potassium ferrate composite environmental remediation material and its preparation method. Through a carrier modification-stabilizer composite-calcination strengthening process, potassium ferrate is loaded onto a porous carrier to form a stable composite environmental remediation material, which has the following beneficial effects:
[0038] (1) By using composite carriers and stabilizers, the stability and sustained-release properties of potassium ferrate are improved.
[0039] (2) Develop a low-cost, high-purity one-step synthesis process and optimize reaction conditions and post-processing procedures;
[0040] (3) Achieve broad-spectrum removal of pollutants (heavy metals, antibiotics, petroleum hydrocarbons, etc.) and simultaneous antibacterial function.
[0041] The enhanced stability of potassium ferrate in this invention is due to the stabilizer and porous carrier (such as sodium silicate) reducing the decomposition rate of potassium ferrate in the environment. When potassium ferrate is typically used in soil and water, sodium silicate, after dissolving in water, exhibits strong alkalinity, maintaining high alkalinity and reducing potassium ferrate decomposition. Silicate ions can form a buffer system with hydroxide ions, mitigating pH fluctuations and thus delaying decomposition. The silica colloids generated from the hydrolysis of sodium silicate can adsorb onto the surface of potassium ferrate particles, forming a physical barrier that isolates water molecules. Furthermore, silicate ions can form stable complexes with impurities such as iron ions, reducing the catalytic effect of these ions on the decomposition of potassium ferrate.
[0042] Compared to traditional remediation materials, potassium ferrate has the highest redox potential of 2.2V and the strongest oxidizing ability. It can oxidize pollutants that traditional oxidants cannot treat. When carried with a porous carrier, it can achieve long-lasting oxidation and prevent pollution recurrence.
[0043] The increased yield of potassium ferrate in the process of this invention is due to the presence of an auxiliary catalyst, which generates more sodium ferrate, which is then replaced by potassium hydroxide to generate more potassium ferrate.
[0044] In summary, the composite structure of this invention's potassium ferrate composite environmental remediation material delays the decomposition of potassium ferrate, extending the material's shelf life to over 6 months. The porous carrier provides adsorption sites, synergistically enhancing pollutant removal rates through oxidation-adsorption. The calcination process strengthens the material's mechanical strength, making it suitable for injection into flowing water bodies or deep soil. Detailed Implementation
[0045] To make the objectives, technical solutions, and advantages of this invention clearer, the technical solutions of this invention will be described in detail below. Obviously, the described embodiments are merely some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other implementation methods obtained by those skilled in the art without creative effort are within the scope of protection of this invention.
[0046] Example 1: A method for preparing a potassium ferrate composite environmental remediation material, the process is as follows:
[0047] Step 1: Synthesis of potassium ferrate: Mix 2 mol of 0.5 mol / L Fe(NO3)3 solution with 18 mol of 6 mol / L strong alkaline solution (NaOH / KOH), where NaOH is 12 mol and KOH is 6 mol. Add an auxiliary catalyst (nano TiO2). Slowly add 12% sodium hypochlorite (NaClO) at low temperature (1℃). The reaction produces K2FeO4 precipitate, which is separated by centrifugation and then vacuum dried.
[0048] Step 2: After activating the porous support by acid washing with 5% HNO3, it is immersed in a stabilizer solution (concentration 10wt%) and dried at 60℃ for later use.
[0049] Step 3: Composite Loading. Potassium ferrate powder and modified carrier are mixed in the following proportion, 2% carboxymethyl cellulose is added, ball milling is performed for 3 hours, and after being pressed into tablets, they are calcined at 400°C for 2 hours in an inert atmosphere (N2) to obtain porous composite particles, which are the environmental remediation material.
[0050] Material composition (by mass percentage):
[0051] Potassium ferrate (K2FeO4): 63%
[0052] Porous support (activated carbon): 30%
[0053] Stabilizer (sodium silicate): 7%.
[0054] Example 2: A method for preparing a potassium ferrate composite environmental remediation material, the process is as follows:
[0055] Step 1: Synthesis of potassium ferrate: Mix 2 mol of 0.5 mol / L FeCl3 solution with 21 mol of 6 mol / L strong alkaline solution (NaOH / KOH), where NaOH is 13 mol and KOH is 8 mol. Add an auxiliary catalyst (nano TiO2). Slowly add 12% sodium hypochlorite (NaClO) at low temperature (0℃). The reaction produces K2FeO4 precipitate, which is separated by centrifugation and then vacuum dried.
[0056] Step 2: After activating the porous support by acid washing with 5% HNO3, it is immersed in a stabilizer solution (concentration 10wt%) and dried at 80℃ for later use.
[0057] Step 3: Composite Loading. Potassium ferrate powder and modified carrier are mixed in the following proportion, 2% carboxymethyl cellulose is added, ball milling is performed for 2 hours, and after being pressed into tablets, they are calcined at 300°C for 1 hour in an inert atmosphere (N2) to obtain porous composite particles, which are the environmental remediation material.
[0058] Material composition (by mass percentage):
[0059] Potassium ferrate (K2FeO4): 57%
[0060] Porous support (activated carbon): 35%
[0061] Stabilizer (sodium silicate): 8%.
[0062] Application Example 1: Synergistic Removal of Cr(VI) and Tetracycline from Water
[0063] 1g of the environmental remediation material prepared in Example 1 was added to simulated wastewater containing Cr(VI) (50mg / L) and tetracycline (20mg / L), the pH was adjusted to 7, and the reaction was carried out for 60 minutes:
[0064] Test results: Cr(VI) not detected (ICP-MS), tetracycline residue <1 mg / L (HPLC).
[0065] Cr(VI) removal rate > 99% (reduced to Cr(III) and adsorbed); tetracycline degradation rate > 95% (mainly through oxidative decomposition pathway).
[0066] Application Example 2: Remediation of Oil-Contaminated Soil
[0067] The environmental remediation material prepared in Example 1 was mixed into soil containing petroleum hydrocarbons (5000 mg / kg) at a mass ratio of 2%, and after 30 days of curing:
[0068] Petroleum hydrocarbon degradation rate >85%, soil microbial diversity restored to 90% of clean soil.
[0069] Comparative Application Example 1 (using existing environmental remediation materials)
[0070] Add 0.5g of ferrous sulfate and 0.5g of activated carbon to simulated wastewater containing Cr(VI) (50mg / L) and tetracycline (20mg / L), adjust the pH, and react for 60 minutes:
[0071] Detection results: Cr(VI) residue 23 mg / L, tetracycline residue >12 mg / L (HPLC).
[0072] Cr(VI) removal rate 54% (reduction to Cr(III)); tetracycline degradation rate <40% (adsorption).
[0073] Comparative Application Example 2 (using existing environmental remediation materials)
[0074] When Fenton's reagent is mixed at a 2% mass ratio into soil containing petroleum hydrocarbons (5000 mg / kg), and cured for 30 days:
[0075] The degradation rate of petroleum hydrocarbons was 61%, and the soil microbial diversity was restored to 77% of that of clean soil.
[0076] As can be seen from the comparison, the environmental remediation material of this invention has better removal and remediation effects than existing environmental remediation materials (such as activated carbon, zero-valent iron, Fenton's reagent, etc.) in the synergistic removal of Cr(VI) and tetracycline in wastewater and in the remediation of petroleum-contaminated soil. Regarding the removal of Cr(VI) and tetracycline in wastewater, it has an oxidizing effect on tetracycline; the amide bond and benzene ring in tetracycline are easily oxidized by potassium ferrate, generating small molecule intermediates. The reduction of hexavalent chromium is due to: the hydrolysis of potassium ferrate to generate trivalent iron, which reduces hexavalent chromium to trivalent chromium; simultaneously, trivalent chromium is adsorbed by the flocculating ferric hydroxide generated after hydrolysis by potassium ferrate.
[0077] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A potassium ferrate composite environmental remediation material, characterized in that, Includes the following components and their mass percentages: Potassium ferrate 40-70%; Porous carrier 20-50%; Stabilizer 5-10%; The porous carrier is one of activated carbon, zeolite, and biochar; the stabilizer is sodium silicate or polyvinyl alcohol.
2. The preparation method of the potassium ferrate composite environmental remediation material as described in claim 1, characterized in that, The following processes are included: S1: Potassium ferrate synthesis: Potassium ferrate was synthesized by sodium hypochlorite oxidation method; S2: Modification of porous carrier: After acid washing and activation, the porous carrier is immersed in a stabilizer solution and then dried for later use; S3: Composite Loading: The potassium ferrate powder obtained in step S1 is mixed with the modified porous carrier in a certain proportion, then a binder is added, the mixture is ball-milled for a period of time, pressed into tablets, and then calcined in an inert atmosphere to obtain porous composite particles, i.e., the environmental remediation material.
3. The preparation method of a potassium ferrate composite environmental remediation material according to claim 2, characterized in that, Step S1 specifically involves mixing an iron salt solution with a strong alkaline solution, slowly adding sodium hypochlorite dropwise at low temperature, reacting to generate K2FeO4 precipitate, centrifuging and then vacuum drying.
4. The method for preparing a potassium ferrate environmental remediation material according to claim 3, characterized in that, The iron salt is FeCl3 or Fe(NO3)3, the strongly alkaline solution is a mixed solution of NaOH and KOH, and the low temperature condition is 0-5℃.
5. The method for preparing a potassium ferrate environmental remediation material according to claim 4, characterized in that, The specific process for step S1 is as follows: (1) Synthesis of sodium ferrate: Under strongly alkaline conditions, sodium hypochlorite oxidizes iron salts to sodium ferrate in the presence of an auxiliary catalyst. (2) Conversion to potassium ferrate: Sodium ferrate reacts with potassium hydroxide in a metathesis reaction to produce potassium ferrate; The auxiliary catalyst is nano-TiO2 or Fe3O4.
6. The method for preparing a potassium ferrate environmental remediation material according to claim 2, characterized in that, In step S2, the porous support is activated by acid washing with 5% HNO3 by mass, and the drying temperature is 60-80℃.
7. The method for preparing a potassium ferrate environmental remediation material according to claim 2, characterized in that, The adhesive is hydroxymethyl cellulose.
8. The method for preparing a potassium ferrate environmental remediation material according to claim 2, characterized in that, In step S3, the ball milling time is 2-4 hours, the inert atmosphere is N2 atmosphere, and the calcination process is: calcination at 300-400℃ for 1-2 hours.
9. The application of the potassium ferrate composite environmental remediation material as described in claim 1 in the remediation of polluted water bodies and soil.