Soluble calcium salts from calcium-containing material

A process and system for recovering soluble calcium salts from slags by leaching and precipitation effectively addresses the need for novel uses of industrial waste streams, producing high-purity calcium salts suitable for various applications.

WO2026234329A1PCT designated stage Publication Date: 2026-11-12TAPOJÄRVI OY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/FI2026/050240
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-05-08
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

There is a need for novel methods to utilize industrial side streams, particularly slags, as raw materials for producing valuable products within the concept of a circular economy, as they are often treated as waste.

Method used

A process and system for recovering soluble calcium salts from calcium-containing materials like slags by leaching with acid, separating residues, precipitating silicon compounds into a gelled cake, and producing a dilute calcium salt solution with controlled temperature and pH, followed by optional concentration and crystallization to obtain high-purity calcium salts.

Benefits of technology

This method efficiently produces soluble calcium salts with high solubility in water, enabling the recovery of valuable products from industrial waste streams, promoting a circular economy by utilizing slags as a resource.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FI2026050240_12112026_PF_FP_ABST
    Figure FI2026050240_12112026_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a process and a system for recovering a soluble calcium salt from calcium-containing material The process comprises leaching the calcium-containing material, separating residue from calcium-containing leachate, precipitating silicon compounds from calcium-containing leachate into a gelled silicon cake, and separating the gelled silicon cake from the calcium-containing leachate.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Soluble calcium salts from calcium-containing material

[0002] Technical field

[0003] The invention is related to systems and processes for recovering soluble calcium salts from calcium-containing material, such as slag.

[0004]

[0005] Many industrial processes produce co-products and side products, or side streams, in addition to the main product of the process. Some side streams of these processes may have conventionally even been treated as waste.

[0006] With the increasing environmental concern, there is an increasing demand for sustainable products and circular economy processes. Industrial side streams previously considered as waste are continuously explored for novel uses.

[0007] Slags are an example of industrial side streams that show potential for novel uses. Slags are a class of materials obtained as by-products or co-products in metallurgical processes. Composition of slags varies by the exact metallurgical process in question. Slags often comprise mixtures of metal oxides and silicon dioxide. Slags may also contain metal sulfides and elemental metals. The major components of slags include the oxides of calcium, magnesium, silicon, iron, and aluminium, with lesser amounts of manganese, phosphorus, and others depending on the specifics of the raw materials used.

[0008] Slags are conventionally used in construction industry (e.g., in concretes), landfilling applications and agriculture (e.g., as a liming material). Slags may also be used as a raw material for producing certain metal compounds. However, novel methods for utilizing slags are needed. Slags, being byproducts or co-products of metallurgical processes, serve as a promising raw material for various applications within the concept of circular economy.Summary

[0009] An object of the invention is to reduce or even eliminate the drawbacks found in the prior art.

[0010] Particularly, an object of the presented invention is to provide novel uses for industrial side streams.

[0011] A further object of the invention is to provide processes for producing calcium salts that utilize industrial side streams as a raw material.

[0012] The invention is defined by what is recited in the independent claims. Embodiments or examples of the invention are presented in the dependent claims.

[0013] Any embodiments or examples of the invention presented herein that are specified with the open term ‘comprise’ may be further limited with a closed term ‘consisting of’.

[0014] All embodiments or examples of the invention are mutually freely combinable, unless otherwise indicated. The presented embodiments and examples of the invention are applicable to all aspects of the invention, both the process and the system.

[0015] Particularly, a process for recovering a soluble calcium salt from calcium-containing material is provided. The process comprises or consists of

[0016] a. leaching the calcium-containing material using an acid in a leaching reactor to dissolve calcium from the calcium-containing material, thus producing a process stream comprising a calcium- containing leachate and a residue;

[0017] b. separating the residue from the calcium-containing leachate; c. precipitating silicon compounds from the calcium-containing leachate into a gelled silicon cake; and

[0018] d. separating the gelled silicon cake from the calcium-containing leachate to produce a dilute calcium salt solution having a calcium salt concentration in the range of 1-15 wt-%, preferably in the range of 5-10 wt-% of the total weight of the dilute calciumsalt solution, whereby the gelled silicon cake has a dry mass content in the range of 10-25 wt-% of the total weight of the gelled silicon cake.

[0019] Unless otherwise indicated, the process steps a. to d. are performed in the order specified herein. In other words, the leaching at a. is the first step in the process, followed subsequently by separating the residue at b., precipitating the silicon compounds at c., and separating the producing the dilute calcium salt solution at d.

[0020] A system for recovering a soluble calcium salt from calcium-containing material is further provided. The system comprises or consists of

[0021] - a leaching reactor configured to leach the calcium-containing material using an acid to dissolve calcium from the calcium- containing material, thus configured to produce a process stream comprising a calcium-containing leachate and a residue;

[0022] - a means for separating the residue from the calcium-containing leachate;

[0023] - a means for precipitating silicon compounds from the calcium- containing leachate into a gelled silicon cake; and

[0024] - a means for separating the gelled silicon cake from the calcium- containing leachate configured to produce a dilute calcium salt solution having a calcium salt concentration in the range of 1-15 wt-% of the total weight of the dilute calcium salt solution, whereby the gelled silicon cake has a dry mass content in the range of IQ- 25 wt-% of the total weight of the gelled silicon cake.

[0025] The presented process and system both utilize calcium-containing material as a starting material. Calcium-containing material should be in the course of this specification understood as a material having a calcium content high enough to facilitate profitable calcium salt production. Suitable calcium-containing materials may have a calcium content as calcium oxide (CaO) in the range of 20-60 wt-%, preferably in the range of 25-60 wt-%, more preferably in the range of 30-60 wt-%, calculated as weight percentage of calcium oxide of the total weight of the material. The calcium content of 20-60 wt-% as CaO corresponds to approx. 13-40 wt-% of the total weight of the material as pure calcium. Correspondingly, the 25-60 wt-% as CaO corresponds to approx. 17-40 wt-% as pure calcium, and the 30-60 wt-% as CaO corresponds to approx.

[0026] 20-40 wt-% as pure calcium, of the total weight of the calcium-containing material.

[0027] The presented process and system are suitable for producing soluble calcium salts from calcium-containing material. The term ‘soluble’ should be understood as solubility in water. Solubility of the calcium salt in water should be at least 10 g / 100 ml at 20°C. In other words, the soluble calcium salt is a calcium salt having a solubility in water of at least 10 g / 100 ml at 20°C, such as 10-300 g / 100 ml at 20°C.

[0028] The term ‘solution’ should be in the course of this specification understood as aqueous solution.

[0029] Brief description of the drawings

[0030] Fig. 1 presents the process and system of the invention.

[0031] Fig. 2 presents process steps of the process and equipment of the system according to embodiments of the invention.

[0032] Figs. 3a-b present process steps and equipment of the system according to embodiments of the invention for recovering a silicon product.

[0033] Detailed description

[0034] The following reference numberswill be used in the course of this specification.

[0035] 100 system

[0036] 101 leaching reactor

[0037] 102 means for separating a residue from calcium-containing leachate 103 means for precipitating silicon compounds from calcium-containing leachate into a gelled silicon cake

[0038] 104 means for separating gelled silicon cake from calcium-containing leachate

[0039] 105 means for concentrating dilute calcium salt solution

[0040] 106 means for recovering solid calcium salt

[0041] 107 means for drying gelled silicon cake

[0042] 108 means for grinding dried silicon cake109 means for dissolving remaining calcium from gelled silicon cake or from ground silicon cake

[0043] 110 means for separating Ca-depleted silicon cake from calcium salt solution

[0044] 200 calcium-containing material

[0045] 202 calcium-containing leachate

[0046] 204 residue

[0047] 206 dilute calcium salt solution

[0048] 208 concentrated calcium salt solution

[0049] 210 solid calcium salt

[0050] 300 gelled silicon cake

[0051] 302 dried silicon cake

[0052] 304 ground silicon cake

[0053] 306 calcium salt solution

[0054] 308 Ca-depleted silicon cake

[0055] 310 silicon product

[0056] A soluble calcium salt may be produced by the presented process. Solubility of the soluble calcium salt in water should be at least 10 g / 100 ml at 20°C, such as at least 12, at least 14, or at least 16 g / 100 ml at 20°C. Solubility of the soluble calcium salt in water may be in the range of 10-300 g / 100 ml, preferably 12-300, 14-300, or 16-300 g / 100 ml at 20°C.

[0057] The presented process may be a batch process or a continuous process. However, precipitation of the silicon compounds into the gelled silicon cake at c. is most conveniently arranged as a batch process even in an otherwise continuous process.

[0058] Referring to Figure 1, the presented process may comprise leaching the calcium-containing material 200 using an acid at a. in a leaching reactor 101. The calcium-containing material 200 is leached in order to dissolve calcium from the calcium-containing material 200. Thus, a process stream comprising a calcium-containing leachate 202 and a residue 204 are produced. Correspondingly, the presented system 100 may comprise a leaching reactor configured to leach the calcium-containing material 200 using an aqueous acidsolution 201 to dissolve calcium from the calcium-containing material 200. The leaching reactor 101 is thus configured to produce a process stream comprising a calcium-containing leachate 202 and a solid residue 204.

[0059] The calcium-containing material 200 suitable for the present invention may originate from different sources, provided that the calcium content in the material is suitable for the presented process. For example, materials comprising calcium as silicates, hydroxides, carbonates, or combinations thereof may be suitable for the present invention. For example slags, particularly pyrometallurgical slags may be suitable materials for the invention. Examples of suitable slags include, but are not limited to bauxite slag, copper slag, steel slag, stainless steel slag, carbon steel slag, and any combinations thereof. For clarity, slag should be understood as slag formed in the manufacturing process of a certain metal or metal alloy. For example, steel slag should be understood as slag formed in the manufacturing process of steel. Likewise, stainless steel slag and carbon steel slag refer to slags formed in the manufacturing process of stainless steel and carbon steel, respectively. The slag may originate from different kinds of metallurgical processes, or different process stages of metallurgical processes, e.g., basic oxygen furnace slag (BOF slag), oxygen decarburization slag (OD slag), or electric arc furnace slag (EAF slag).

[0060] The calcium-containing material may also be combined with other industrial side streams to be used as a starting material for the presented process. For example, combinations of calcium-containing material and silicon-rich industrial side streams, such as lime kiln dust (LKD), may be used as a starting material for the presented process. The silicon-rich industrial side stream may be used to increase the silicon content of the calcium-containing material used as a starting material for the presented process. Thus, the calcium-containing material 200 may be a silicon-enriched calcium containing material. Silicon-enriched calcium-containing material may be particularly compatible with processes that comprise recovering a silicon product from the gelled silicon cake 300 at d., as described below.

[0061] The acid used for leaching at a. may be selected from the group comprising inorganic acids, organic acids, and any combination thereof. In cases where the acid is an inorganic acid, it may be selected from the group comprisingnitric acid, hydrochloric acid, and any combination thereof. In cases where the acid is an organic acid, it may be selected from the group comprising formic acid, acetic acid, propanoic acid, lactic acid, and any combination thereof. In particularly preferred processes, the acid is formic acid. The acid may be used in a form of aqueous acid solution.

[0062] The acid used for the leaching at a. provides the anion for the soluble calcium salt produced by the presented method. Therefore, the produced calcium salt may be selected from the group comprising calcium nitrate, calcium chloride, calcium formate, calcium acetate, calcium propanoate, calcium lactate, or any combination thereof. In particularly preferred processes, the calcium salt is calcium formate, i.e., calcium methanoate.

[0063] The acid 201 may be added in stoichiometric excess compared to the amount of the calcium salt to be recovered from the calcium-containing material 200. The acid 201 may be added in a weight ratio in the range of 1.5:1 to 10:1 to the weight of calcium in the calcium-containing material, preferably in a weight ratio in the range of 2: 1 to 5: 1 to the weight of calcium in the calcium-containing material.

[0064] The amount of the acid 201 added may alternatively or in addition be determined in comparison to the weight of the calcium-containing material 200 to be leached. The acid 201 may be added in a weight ratio in the range of 1:1 to 1 :5 to the weight of the calcium-containing material, preferably in a weight ratio of 1 :1 to 1 :2 to the weight of the calcium-containing material.

[0065] Referring to Figure 1, the leaching reactor 101 at a. may be a continuous reactor. A calculated dwell time of the calcium-containing material in the continuous reactor may be in the range of 0.5-30 min. Preferably, the dwell time is in the range of 1-10 min, more preferably in the range of 3-8 min, even more preferably in the range of 4-6 min. The selected dwell time may enable an efficient or even complete leaching of the slag in the leaching reactor without compromising process economy in terms of, e.g., energy usage. Moreover, the dwell time contributes to the efficiency of separation of the residue 204 at b. (see below).Alternatively, the leaching reactor 101 may be a batch reactor. In alteration to a single batch reactor, the leaching reactor may be arranged as a plurality of batch reactors connected in series, such as two, three, or four batch reactors connected in series. A reaction time in the batch reactor or the plurality of batch reactors may be in the range of 0.5-30 min. Preferably, the reaction time is in the range of 1-10 min, more preferably in the range of 3-8 min, even more preferably in the range of 4-6 min.

[0066] The dwell time (in a continuous reactor) or the reaction time (in the batch reactor or plurality of batch reactors) as specified herein may be selected to obtain optimal leaching. Dwell times or reaction times shorter than specified above may lead to incomplete or insufficient leaching of the calcium, thus leaving an unacceptably high calcium concentration in the residue 204. Dwell times or reaction times longer than specified above may, in the other hand, lead to warming of the leachate, which may in turn lead to poor formation of the gelled silicon cake 300 or at least increase the need to cool the calcium-containing leachate 202 (see below). Too long dwell times or reaction times may also lead to leaching of impurities or undesired elements from the calcium-containing material 200. Also, the precipitation of the silicon compounds (i.e., formation of the gelled silicon cake) may start to take place too early if the dwell time or the reaction time is too long, thus hindering the separation of the residue 204 at b. Thus, the dwell times or reaction times as specified above ensure an optimal and selective leaching of calcium from the calcium-containing material 200.

[0067] The presented process may comprise controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 at a. such that the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 is in the range of 0-25°C, preferably in the range of 0-20°C. The system 100 may correspondingly comprise a means for controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 at a.

[0068] As mentioned above, controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 may comprise cooling the acid entering the leaching reactor 101 such that the temperature of the acid is in the range of 0-15°C when entering the leaching reactor 101. Controlling thetemperature of the acid entering the leaching reactor 101 may have an indirect effect on the residue separation at b. through optimization of energy streams in the process. Cooling the acid entering the leaching reactor 101 may assist in controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101. Since the leaching is an exothermic reaction, temperature of the calcium-containing material will increase during leaching. When the acid entering the leaching reactor is properly cooled within the specified temperature range, it will be easier to control the temperature of the leachate exiting the leaching reactor. In other words, cooling the acid entering the leaching reactor will make it easier to control the temperature of the leachate exiting the reactor within its specified temperature range. Correspondingly, the system 100 may comprise a means for cooling the acid entering the leaching reactor 101 at a.

[0069] Controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 may further comprise cooling the leaching reactor 101 during the leaching at a. Cooling the leaching reactor 101 may comprise, e.g., conducting heat away from the reactor via its outer housing. Correspondingly, the system 100 may comprise a means for cooling the leaching reactor 101 during the leaching at a.

[0070] In an efficient leaching process, most or even essentially all calcium compounds originally contained in the calcium-containing material 200 are dissolved into the calcium-containing leachate 202. In materials suitable for the present invention, calcium may be present as, e.g., calcium silicates, calcium hydroxides, calcium oxides, and combinations thereof. The calcium-containing leachate may further comprise silicon compounds originating for example from the calcium silicates or from the silicon enrichment (see above). The residue 204 comprises components of the calcium-containing material 200 that are not soluble in the used acid, e.g., metals originally present in the calcium-containing material 200.

[0071] Controlling the temperature of the calcium-containing leachate 202 exiting the leaching reactor 101 may comprise cooling the calcium-containing leachate 202 exiting the leaching reactor 101, cooling the acid entering the leaching reactor 101, cooling the leaching reactor 101 during the leaching process, or any combination thereof.pH of the calcium-containing leachate 202 may be controlled during the leaching at a. in order to facilitate efficient separation of the residue 204 at b. In preferred processes, pH of the calcium-containing leachate 202 exiting the leaching reactor 101 may be in the range of 2-7, preferably in the range of 4-5. The pH value may be controlled directly or indirectly. Direct controlling of the pH value may comprise adding an acid or a base. Indirect controlling the pH value may comprise adjusting any other process parameters that have an impact on the pH during the leaching. The most important process parameter that may be adjusted to affect the pH of the calcium-containing leachate 202 is the dwell time (in a continuous reactor) or the reaction time (in a batch reactor). In other words, the dwell time or reaction time used for the leaching at a. may be controlled to prevent the pH from increasing above the specified values.

[0072] In preferred processes, the leaching at a. may comprise controlling the temperature and pH of the calcium-containing leachate 202 exiting the leaching reactor 101 together. Controlling the temperature and pH together may comprise controlling the temperature of the calcium-containing leachate (202) exiting the leaching reactor such that its temperature is in the range of 0-10°C, preferably in the range of 0-5°C; and / or controlling the temperature of the acid (201) entering the leaching reactor (101) such that its temperature is in the range of 0-5°C; while simultaneously controlling pH of the calcium-containing leachate (202) at exit from the leaching reactor (101) such that its pH is in the range of 3-6, preferably in the range of 3-5, more preferably in the range of 4-4.9.

[0073] Precise control of the temperature and / or pH of the calcium-containing leachate 202 exiting the leaching reactor 101 may enable efficient residue separation at b (see below). If either the temperature, the pH, or the combination of the temperature and pH of the calcium-containing leachate 202 exiting the leaching reactor 101 is too high, the silicon compounds originally contained in the calcium-containing material start to precipitate already before the residue 204 is separated from the calcium-containing leachate 202 at b. In other words, precipitation of the silicon compounds may occur too early if either the temperature or the pH of the calcium-containing leachate exiting the leaching reactor is too high. This may in turn make the residue separation atb. inefficient or even practically impossible. Thus, precise control of the temperature and / or pH of the calcium-containing leachate 202 exiting the leaching reactor 101 may facilitate efficient separation of the residue 204 at b. , also contributing to the purity of the obtained calcium salt product.

[0074] Referring to Figure 1, the presented process may comprise separating the residue 204 from the calcium-containing leachate 202 at b. The separating is preferably performed by filtering. More preferably, the filtering is performed using a continuous filter, such as a belt filter or a drum filter. Continuous filtering may provide efficient separation of the residue 204 from the calcium-containing leachate 202, which may in turn improve the processability of the calcium-containing leachate 202 later in the process. The system 100 may correspondingly comprise a means 102 for separating the residue 204 from the calcium-containing leachate 202 at b. Preferably, the means 102 for separating the residue 204 from the calcium-containing leachate 202 is a filter, more preferably a continuous filter. In particularly preferred systems, the means 102 for separating the residue 204 from the calcium-containing leachate 202 is a belt filter or a drum filter.

[0075] Still referring to Figure 1, the presented method may comprise precipitating silicon compounds from the calcium-containing leachate 202 into a gelled silicon cake 300 at c. The system 100 correspondingly comprises a means 103 for precipitating silicon compounds from the calcium-containing leachate 202 into a gelled silicon cake 300 at c.

[0076] The precipitation at c. may be performed by stirring the calcium-containing leachate 202 to precipitate any silicon compounds into the gelled silicon cake 300. The stirring should be intensive enough to enable efficient formation of the gelled silicon cake 300. Correspondingly, the means 103 for precipitating silicon compounds from the calcium-containing leachate 202 into a gelled silicon cake 300 at c may be a container equipped with a stirrer or a mixer. The precipitation at c. may be arranged as a batch process. Respectively, the means 103 for precipitating the silicon compounds may be a batch precipitation container equipped with a stirrer or a mixer.

[0077] The precipitation, such as the stirring, at c. may be carried out for 0.5-10 hours, preferably 1-5 hours, more preferably 2-3 hours. The specified time mayenable an efficient or even essentially complete precipitation of silicon from the calcium-containing leachate 202 into the gelled silicon cake 300. In other words, a majority or even essentially all silicon originally present in the calcium-containing leachate 202 may be precipitated from the leachate into the gelled silicon cake 300, enabling the production of a high purity calcium salt product.

[0078] The precipitation at c. may be performed at ambient temperature. Alternatively, the precipitation at c. may be performed at an elevated temperature. The precipitation at c. may be performed at a temperature in the range of 20-80°C, preferably in the range of 30-50°C. Using an elevated temperature may increase the precipitation rate of the gelled silicon cake, i.e. , fasten the gelled silicon cake 300 formation. Thereby, it may be possible to reduce the time used for the stirring at c. The process may further comprise heating the calcium-containing leachate 202 to the specified temperature. Temperatures higher than specified here do not further remarkably increase the precipitation reaction rate. Thus, it may be beneficial in terms of energy usage to keep the temperatures within the above-specified limits. Correspondingly, the system 100 may comprise a means for heating the calcium-containing leachate 202 to the specified temperature.

[0079] Referring to Figure 1, the presented process may comprise separating the gelled silicon cake 300 from the calcium-containing leachate 202 at d. Thus, a dilute calcium salt solution 206 having a calcium salt concentration in the range of 1-15 wt-% is produced. In preferred processes, the dilute calcium salt solution 206 may have a calcium salt concentration in the range of 5-10 wt-% of the total weight of the dilute calcium salt solution. The dry mass content of the gelled silicon cake 300 after the separation at d. may be in the range of 10-25 wt-% of the total weight of the gelled silicon cake. Essentially all silicon originally dissolved in the calcium-containing leachate 202 may be precipitated into the gelled silicon cake 300 at c. and separated from the remaining calcium-containing leachate 202, i.e., the dilute calcium salt solution 206, at d. The gelled silicon cake 300 may still contain dissolved calcium due to the rather high water content after the separation. However, the separation may ensure that essentially no silicon is present in the dilute calcium salt solution 206. Efficient separation of the gelled silicon cake 300 from the remaining calcium-containing leachate 202 is important for obtaining a high purity calcium salt product. Correspondingly, the system 100 may comprise a means 104 forseparating the gelled silicon cake 300 from the calcium-containing leachate 202.

[0080] Separating the gelled silicon cake 300 from the calcium-containing leachate 202 at d. may comprise filtering, such as pressure filtering, or sedimentation, such as centrifuging. Correspondingly, the means 104 for separating the gelled silicon cake 300 from the calcium-containing leachate 202 may be a filter, preferably a pressure filter, or a sedimental separator, such as a centrifuge.

[0081] The dilute calcium salt solution 206 obtained at d. may be utilized further as is. In other words, the calcium salt recovered from calcium-containing material 200 using the presented process may be the dilute calcium salt solution 202. Alternatively, the dilute calcium salt solution 206 may be processed further by concentrating at e. and / or by recovering a solid calcium salt at f. (see below). Thus, the calcium salt recovered from the calcium-containing material 200 may be the dilute calcium salt solution 206, the concentrated calcium salt solution 208, or the solid calcium salt 210.

[0082] Referring to Figure 2, the process may further comprise, at e., concentrating the dilute calcium salt solution 206 obtained at d. Thus, a concentrated calcium salt solution 208 having a calcium salt concentration in the range of 10-20 wt-% of the total weight of the concentrated calcium salt solution may be produced. In preferred processes, the concentrated calcium salt solution 208 may have a calcium salt concentration in the range of 12-16 wt-% of the total weight of the concentrated calcium salt solution. Concentrating the dilute calcium salt solution 206 may facilitate easier and more energy efficient recovery of a solid calcium salt 210 product later in the process at f. (see below). Furthermore, in cases where the calcium salt is used further in the form of a calcium salt solution, it may be beneficial to concentrate the solution for, e.g., transport purposes. Correspondingly, the system 100 may comprise a means 105 for concentrating the dilute calcium salt solution 206 configured to produce the concentrated calcium salt solution 208.

[0083] Concentrating the dilute calcium salt solution 206 at e. may be performed, e.g., by reverse osmosis, electrodialysis, membrane distillation, or by distillation. Reverse osmosis and electrodialysis may be particularly suitable methods for concentrating the dilute calcium salt solution 206 due to their smaller energyconsumption when compared to, e.g., thermal methods such as distillation. Correspondingly, the means 105 for concentrating the dilute calcium salt solution 206 may be a reverse osmosis membrane, an electrodialysis equipment, a membrane distillation equipment, or a distillation equipment.

[0084] Still referring to Figure 2, the process may further comprise, at f. , recovering a solid calcium salt 210 from the dilute calcium salt solution 206 or the concentrated calcium salt solution 208 . The solid calcium salt 210 may further be packaged and transported for further use. Preferably, recovering the solid calcium salt 210 is performed by crystallizing and / or by evaporating. Recovering the solid calcium salt by crystallizing may have the advantage of increased product purity compared to other recovery methods. For example, when compared to evaporation where possible impurities remain in the solid phase after evaporation of the solvent, crystallization may produce a very high-quality product with a reduced impurity content, since the possible impurities are remained in the solvent phase. Furthermore, crystallizing may be more energy efficient compared to other recovery methods. To obtain even improved product purities, the crystallization may be repeated one or several times. The process may comprise separating the produced calcium salt crystals from the remainder of the dilute calcium salt solution 206 or the concentrated calcium salt solution 208. The separating may comprise, e.g., filtering or sedimentation, such as centrifuging. Correspondingly, the system 100 may comprise a means 106 for recovering the solid calcium salt 210, preferably a crystallization equipment or an evaporation equipment. The crystallization equipment may comprise, e.g., a crystallizer and a separator, such as a filter or a sedimental separator, such as a centrifuge.

[0085] Referring to Figures 3a and 3b, the presented process may further comprise, at g., recovering a silicon product 310 from the gelled silicon cake 300 separated at d. The silicon product may be obtained in a form of amorphic, impure silicon oxide. The silicon product may have a silicon dioxide content in the range of 60-100 wt-%, such as in the range of 70-95 wt-% or in the range of 75-90 wt-% of the total dry weight of the silicon product. Materials suitable for the presented process typically comprise remarkable concentrations of silicon, e.g., as calcium silicates. Silicon may as a co-product have uses in construction, for example. Correspondingly, the system 100 may comprise a means for recovering the silicon product 310 from the gelled silicon cake 300.Still referring to Figures 3a and 3b, recovering the silicon product 310 at g. may comprise dissolving any remaining calcium from the gelled silicon cake 300 by adding water to produce a calcium salt solution 306 and a Ca-depleted silicon cake 308 at g.3. The calcium dissolution at g.3 may also be termed washing of the gelled silicon cake 300. Upon addition of water, the gelled silicon cake 300 at least partly dissolves in the water, thus dissolving or releasing any calcium ions trapped in the gelled silicon cake 300. The calcium dissolution at g.3 may be beneficial both for the purity of the silicon product, and for the recovery efficiency, or product yield, of the produced calcium salt. Correspondingly, the system 100 may comprise a means 109 for dissolving any remaining calcium from the gelled silicon cake 300 or from a ground silicon cake 304 (see below), thus being configured to produce the calcium salt solution 306 and the Ca-depleted silicon cake 308. The means 109 for dissolving remaining calcium from the gelled silicon cake 300 or the ground silicon cake 304 may comprise, e.g., a washing equipment configured to add water to the gelled silicon cake 300 or to the ground silicon cake 304.

[0086] The process may further comprise separating the Ca-depleted silicon cake 308 from the calcium salt solution 306 at g.4. In preferred processes, the separating at g.4 comprises filtering, preferably through a pressure filter, or sedimentation, such as centrifuging. Thus, the silicon product 310 may be obtained as the filtrate or the supernatant. The separation at g.4 may further increase the dry mass content of the Ca-depleted silicon cake 308. Correspondingly, the system 100 may comprise a means 110 for separating the Ca-depleted silicon cake 308 from the calcium salt solution 306. The means 110 for separating the Ca-depleted silicon cake 308 from the calcium salt solution 306 may be a filter, preferably a pressure filter, or a sedimental separator, such as a centrifuge.

[0087] The presented process may further comprise combining the calcium salt solution 306 obtained at g.4 with the dilute calcium salt solution 206 obtained at d. By combining the calcium salt solution 306 obtained at g.4 with the dilute calcium salt solution 206 obtained at d., the product yield of the recovered calcium salt may be increased. In other words, recovery efficiency of the calcium salt product may be increased. The combination of the calcium salt solution 306 and the dilute calcium salt solution 206 may optionally then beconducted to the concentration at e. and / or to the solid calcium salt recovery at f.

[0088] Referring to Figure 3b, recovering the silicon product 310 may further comprise drying the gelled silicon cake 300 at g.1. A dried silicon cake 302 having a dry mass content in the range of 70-100 wt-% of the total weight of the dried silicon cake may thus be produced. The drying at g.1 may be performed by thermal drying, e.g., by a fluid bed drier or a paddle drier. In preferred processes, the dried silicon cake 302 has a dry mass content in the range of 80-90 wt-% of the total weight of the dried silicon cake. Correspondingly, the system 100 may comprise a means 107 for drying the gelled silicon cake 300, thus configured to produce the dried silicon cake 302. The means 107 for drying the gelled silicon cake 300 may, e.g., be a fluid bed drier or a paddle drier.

[0089] The process may further comprise grinding the dried silicon cake 302 at g.2, thus producing a ground silicon cake 304. The drying at g.1 and grinding at g.2 may conveniently take place prior to the calcium dissolution at g.3, whereby the remaining calcium is dissolved at g.3 from the ground silicon cake 304 obtained at g.2. The silicon cake may be ground to a grain size in the range of 25 pm or less, such as 0.01-25 pm. The grain size may be defined as a statistical average of 25 pm or less, such as 0.01-25 pm, i.e., 95% of all measured grains are present in this size range. Correspondingly, the system 100 may further comprise a means 108 for grinding the dried silicon cake 302, being configured to produce the ground silicon cake 304.

[0090] Drying (at g.1) and grinding (at g.2) the silicon cake prior to the calcium dissolution may provide the advantage of improving the solubility of the calcium salt at the dissolution at g.3. As a consequence, both the purity of the silicon product as well as the calcium salt product may be increased. Furthermore, the improved solubility of the calcium salt at the dissolution at g.3 further improves the recovery efficiency, i.e., product yield, of the recovered calcium salt.Examples

[0091] Example 1

[0092] a. Leaching

[0093] 6 grams of formic acid (98 wt-%) was added to 100 ml of water in a beaker under magnetic stirring, thus producing a formic acid solution. The beaker was placed in an ice bath. The formic acid solution was cooled to 10°C.

[0094] 10 g of stainless steel slag (grain size <250 pm) was added. The mixture was leached and stirred for 30 s while monitoring the pH and the temperature of the mixture. After the 30 s of leaching, the mixture had a pH of 4.4 and a temperature of 21 °C.

[0095] Immediately after the leaching, the mixture was filtered by vacuum filtration.

[0096] The filtrate was collected in a beaker, and pH of the filtrate was adjusted to 7 by adding 0.4 g of calcium hydroxide Ca(OH)2. After the pH adjustment, the solution was heated to 40°C while stirring. The stirring was continued for approx. 10 min, after which the silicon compounds precipitated out of the solution forming a gel-like precipitate, i.e. , a gelled silicon cake.

[0097] The gelled silicon cake was separated from the calcium formate solution by vacuum filtration.

[0098] Calcium formate was recovered from the obtained calcium formate solution by evaporating the solvent. Elemental composition of the obtained solid calcium formate was characterized using inductively coupled plasma optical emission spectroscopy (ICP-OES). Calcium content of the obtained calcium formate was determined by titration. Elemental composition of the calcium formate is presented in Table 1.Table 1. Elemental composition of calcium formate determined by ICP-OES and titration (Ca).

[0099] Element Al B Ba Ca Cd Co Cr Cu Fe Unit PPm PPm PPm % PPm PPm PPm PPm PPm

[0100]

[0101] Result 272 < 100 80 30,2 <2 <10 <10 <25 <25 Element Mg Mn Na Nb Ni Pb Ti V Zn Unit PPm PPm PPm PPm PPm PPm PPm PPm PPm

[0102]

[0103] Result 3463 399 1056 <10 <10 <25 15 <25 <25

[0104] Example 2

[0105] 48.4 g of formic acid (80 wt-%) was diluted with 380 ml of water and cooled to 4.5°C. The obtained formic acid solution was stirred using a magnetic stirrer in a beaker. pH and temperature of the formic acid solution was constantly monitored.

[0106] 54 g of stainless steel slag (grain size <250 pm) was added. The mixture was leached and stirred for 70 s. After the 70 s of leaching, the mixture had a pH of 4.3 and a temperature of 26.8°C.

[0107] Immediately after the leaching, the solution was filtered by vacuum filtration.

[0108] The filtrate was collected in a beaker. The filtrate was stirred at room temperature for 2 h, whereby silicon compounds precipitated forming a gel-like precipitate, i.e. , the gelled silicon cake.

[0109] The gelled silicon cake was separated from the calcium formate solution by vacuum filtering. After the filtering, the silicon cake was washed with 100 ml of water.

[0110] Calcium formate was recovered from the obtained calcium formate solution by evaporating the solvent. Elemental composition of the obtained solid calcium formate was characterized using inductively coupled plasma optical emission spectroscopy (ICP-OES). Calcium content of the obtained calcium formatewas determined by titration. Elemental composition of the calcium formate is presented in Table 2.

[0111] Table 2. Elemental composition of calcium formate obtained in Example 2 determined by ICP-OES and titration.

[0112] Element Al B Ba Ca Cd Co Cr Cu Fe Unit PPm PPm PPm PPm PPm PPm PPm PPm PPm

[0113]

[0114] Result 1 ,6 35 20 33 000 < 0,001 0,02 18 0,6 15 Element Mg Mn Na Sn Ni Pb Se V Zn Unit PPm PPm PPm PPm PPm PPm PPm PPm PPm

[0115]

[0116] Result 1300 35 20 0,01 0,20 <0,10 0,09 2,6 15

[0117] The washed silicon cake was dried in an oven for 24 hours, after which it was milled for 60 s using a swing mill.

[0118] The dried and milled silicon cake sample was purified by washing with water. In the washing, the silicon cake sample was mixed with 150 ml of water and stirred for 15 minutes, after which the purified silicon cake was separated from the washing solution by vacuum filtration.

[0119] Composition of the silicon cake was characterized by X-ray fluorescence (XRF). Composition of the silicon cake is presented in Table 3.

[0120] Table 3. Composition of the silicon product obtained in Example 2 determined by XRF.

[0121] Compound SiO2P2O5 BaO CaO K2O TiO2Cr2O3 ZnO Fe2O3 Unit % % % % % % % % %

[0122]

[0123] Result 88,73 0,01 0 5,41 0,02 0,64 0,112 0,01 0,199 Compound MgO MnO Na Nb Ni Pb F AI2O3

[0124] Unit % % % % % % % %

[0125]

[0126] Result 0,137 0,03 0,03 0,02 0 0,01 1 ,41 2,45

Claims

Claims:

1. A process for recovering a soluble calcium salt from calcium-containing material (200), the process comprisinga. leaching the calcium-containing material (200) using an acid in a leaching reactor (101) to dissolve calcium from the calcium- containing material, thus producing a process stream comprising a calcium-containing leachate (202) and a residue (204); b. separating the residue (204) from the calcium-containing leachate (202);c. precipitating silicon compounds from the calcium-containing leachate (202) into a gelled silicon cake (300);d. separating the gelled silicon cake (300) from the calcium- containing leachate (202) to produce a dilute calcium salt solution (206) having a calcium salt concentration in the range of 1-15 wt-%, preferably in the range of 5-10 wt-% of the total weight of the dilute calcium salt solution, whereby the gelled silicon cake has a dry mass content in the range of 10-25 wt-% of the total weight of the gelled silicon cake.

2. The process according to claim 1 , wherein the acid used for leaching at a. is selected from the group comprising inorganic acids, organic acids, and any combination thereof, preferably wherein the inorganic acid is selected from the group comprising nitric acid, hydrochloric acid, and any combination thereof, and / or wherein the organic acid is selected from the group comprising formic acid, acetic acid, propanoic acid, lactic acid, and any combination thereof, more preferably wherein the acid is formic acid.

3. The process according to claim 1 or 2, wherein the leaching reactor (101) at a. is a continuous reactor; or wherein the leaching reactor (101 ) at a. is a batch reactor, or a plurality of batch reactors connected in series, such as two, three, or four batch reactors connected in series.

4. The process according to claim 3, wherein a calculated dwell time of the calcium-containing material (200) in the continuous reactor or a reaction time in the batch reactor or the plurality of batch reactors is in the range of 0.5-30min, preferably in the range of 1-10 min, more preferably in the range of 3-8 min, even more preferably in the range of 4-6 min.

5. The process according to any of the preceding claims, wherein the leaching at a. further comprises controlling the temperature of the calcium-containing leachate (202) exiting the leaching reactor (101) such that its temperature is in the range of 0-25°C, preferably in the range of 0-20°C; preferably wherein controlling the temperature of the calcium-containing leachate (202) comprises cooling the acid entering the leaching reactor (101) such that its temperature is in the range of 0-15°C when entering the leaching reactor (101 ), or wherein controlling the temperature of the calcium-containing leachate (202) comprises cooling the leaching reactor (101) during the leaching at a.

6. The process according to any of the preceding claims, wherein the leaching at a. further comprises controlling the pH of the calcium-containing leachate (202) exiting the leaching reactor (101) such that its pH is in the range of 2-7, preferably in the range of 4-5.

7. The process according to any of the preceding claims, wherein the separating at b. is performed by filtering, preferably wherein the filtering is performed using a continuous filter, such as a belt filter or a drum filter.

8. The process according to any of the preceding claims, wherein the precipitation at c. is carried out for 0.5-10 hours, preferably 1-5 hours, more preferably 2-3 hours; and / or wherein the precipitation at c. is performed at a temperature in the range of 20-80°C, preferably in the range of 30-50°C.

9. The process according to any of the preceding claims, wherein separating the gelled silicon cake (300) from the calcium-containing leachate (202) at d. comprises filtering, more preferably pressure filtering.

10. The process according to any of the preceding claims, further comprising, after separating the gelled silicon cake (300) from the calcium-containing leachate (202) at d., one or more ofe. concentrating the dilute calcium salt solution (206) obtained at d., to provide a concentrated calcium salt solution (208) having a calcium salt concentration in the range of 10-20 wt-%, preferably in therange of 15-17 wt-%, of the total weight of the concentrated calcium salt solution; andf. recovering a solid calcium salt (210) from the dilute calcium salt solution (206) or the concentrated calcium salt solution (208), preferably by crystallizing and / or by evaporating.

11. The process according to any of the preceding claims, further comprising g. recovering a silicon product (310) from the gelled silicon cake (300) separated at d., comprisingg.

3. dissolving remaining calcium from the gelled silicon cake (300) by adding water to produce a calcium salt solution (306) and a Ca-depleted silicon cake (308); and g.

4. separating the Ca-depleted silicon cake (308) from the calcium salt solution (306) to provide the silicon product (310).

12. The process according to claim 11 , further comprising combining the calcium salt solution (306) obtained at g.4 with the dilute calcium salt solution (206) obtained at d.

13. The process according to claim 11 or 12, further comprising, prior to the dissolving at g.3,g.

1. drying the gelled silicon cake (300) to produce a dried silicon cake (302) having a dry mass content in the range of 70-100 wt-%, preferably in the range of 80-90 wt-%, of the total weight of the dried silicon cake; andg.

2. grinding the dried silicon cake, thus producing a ground silicon cake (304),wherein the remaining calcium is dissolved at g.3 from the ground silicon cake (304) instead of the gelled silicon cake (300).

14. A system (100) for recovering a soluble calcium salt from calcium-containing material (200) according to the process of any of claims 1 to 13, wherein the system (100) comprises- a leaching reactor (101) configured to leach the calcium-containing material (200) using an acid to dissolve calcium from the calcium- containing material (200), thus configured to produce a processstream comprising a calcium-containing leachate (202) and residue (204);- a means (102) for separating the a residue (204) from the calcium- containing leachate (202);- a means (103) for precipitating silicon compounds from the calcium- containing leachate (202) into a gelled silicon cake (300); and - a means (104) for separating the gelled silicon cake (300) from the calcium-containing leachate (202) configured to produce a dilute calcium salt solution (206) having a calcium salt concentration in the range of 1-15 wt-% of the total weight of the dilute calcium salt solution, whereby the gelled silicon cake has a dry mass content in the range of 10-25 wt-% of the total weight of the gelled silicon cake.

15. The system according to claim 14, further comprising one or more of - a means for controlling the temperature of the calcium-containing leachate (202) exiting the leaching reactor (101) at a.;- a means (105) for concentrating the dilute calcium salt solution (206), thus configured to provide a concentrated calcium salt solution (208) having a calcium salt concentration in the range of 10-20 wt-% of the total weight of the concentrated calcium salt solution;- a means (106) for recovering a solid calcium salt (210) from the dilute calcium salt solution (206) or the concentrated calcium salt solution (208);- a means (107) for drying the gelled silicon cake (300), thus configured to produce a dried silicon cake (302) having a dry mass content in the range of 70-100 wt-% of the total weight of the dried silicon cake;- a means (108) for grinding the dried silicon cake (302), thus configured to produce a ground silicon cake (304);- a means (109) for dissolving remaining calcium from the gelled silicon cake (300) or from the ground silicon cake (304), configured to produce a calcium salt solution (306) and a Ca-depleted silicon cake (308); and- a means (110) for separating the Ca-depleted silicon cake (308) from the calcium salt solution (306), thus configured to provide a silicon product (310).