Electrocatalysts for gas evolution reactions

A surface-stabilized ruthenium dioxide electrocatalyst with transition metals addresses the inefficiencies of RuO2 by enhancing stability and activity in gas evolution reactions, particularly in acidic and alkaline environments.

WO2026234576A1PCT designated stage Publication Date: 2026-11-12KING ABDULLAH UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2026/054459
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-05
Filing Date
2026-05-05
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

The slow kinetics and instability of existing electrocatalysts, particularly ruthenium dioxide (RuO2), in gas evolution reactions such as oxygen and chlorine evolution, limit their efficiency and practicality, especially in acidic conditions, leading to degradation and high costs.

Method used

A surface-stabilized ruthenium dioxide electrocatalyst is developed by incorporating transition metals like manganese, chromium, or vanadium on the exterior surface of RuO2 particles, enhancing stability and activity without bulk substitution, thus maintaining catalytic performance.

Benefits of technology

The surface-stabilized RuO2 electrocatalyst improves long-term stability and activity in acidic and alkaline conditions, reducing Ru dissolution and maintaining catalytic performance in oxygen and chlorine evolution reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2026054459_12112026_PF_FP_ABST
    Figure IB2026054459_12112026_PF_FP_ABST
Patent Text Reader

Abstract

An electrode includes: an electrocatalyst including: a plurality of ruthenium dioxide- containing particles, each of the plurality of ruthenium dioxide-containing particles having an exterior surface; and a surface stabilizer predominantly disposed on and coupled to the exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of transition-metal atoms including at least one transition metal selected from one of Manganese, Chromium, Tantalum, and Vanadium.
Need to check novelty before this filing date? Find Prior Art

Description

2025-061-02 ELECTROCATALYSTS FOR GAS EVOLUTION REACTIONSCROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application claims the benefit of and priority to U.S. provisional application 63 / 799,892, titled “ELECTROCATALYSTS FOR OXYGEN EVOLUTION REACTION WITH LONG TERM ACTIVITY AND STABILITY”, filed May 5, 2025, the contents of which are incorporated by reference herein.TECHNICAL FIELD

[0002] The subject matter disclosed herein relates broadly to electrochemistry, electrode technologies, and catalytic materials, and more particularly to electrodes and catalysts for electrochemical water splitting.BACKGROUND

[0003] Gas evolution reactions are electrochemical reactions in which a gaseous species is generated at an electrode-electrolyte interface during operation of an electrochemical cell. Such reactions include, for example, the oxygen evolution reaction (OER), in which water or hydroxide species are oxidized at an anode to form oxygen gas, and the chlorine evolution reaction (CER), in which chloride ions are oxidized at an anode to form chlorine gas. Gas evolution reactions are relevant to electrolyzers, chlor-alkali processes, seawater electrolysis, and other electrochemical conversion systems, and their performance may depend on electrode composition, electrolyte composition, applied potential, and pH. Electrochemical oxygen evolution reaction (OER) is a process in generating protons and electrons from water to supply for reductive processes at the cathode, ultimately leading to the effective utilization of renewable energy sources. However, the inherently slow kinetics of OER, stemming from a complex four-proton-coupled electron transfer process, poses a fundamental challenge to the efficiency and practicality of crucial reactions such as hydrogen (H2) evolution and carbon dioxide reduction. This urgently requires the development of advanced electrocatalysts capable of accelerating these reactions, reducing energy consumption, and ensuring reliable operation under the OER’s2025-061-02 demanding conditions, including high oxidative overpotentials and corrosive electrolytes across a wide pH range.

[0004] The effectiveness of these OER electrocatalysts is particularly critical in acidic proton-exchange membrane water electrolysis (PEMWE) and alkaline water electrolysis (AWE) systems, which provide deployable approaches for large-scale production of sustainable, fuelgrade H2. TO date, the quest for efficient and stable OER electrocatalysts, specifically for acidic PEMWE, remains a formidable challenge, arising from even more sluggish reaction kinetics and severe corrosion in strong acids and oxidizing conditions. Iridium (Ir)-based catalysts like IrO2 are predominantly used for OER in acidic media mainly because of the stability reasons, yet their widespread adoption is constrained by high costs and scarce availability. Ruthenium dioxide (RUO2), with its lower cost, greater earth abundance, and superior OER activity, has emerged as a compelling alternative, drawing fast-growing research attention. Despite these advantages, the stability of pure Ru02 in OER is limited due to its susceptibility to overoxidation over a wide pH range, forming volatile RuO4 or soluble RuOs2-, and accelerating the degradation through the demetallation of surface Ru sites.SUMMARY

[0005] According to one aspect, an electrode includes: an electrocatalyst including: a plurality of ruthenium dioxide-containing particles, each of the plurality of ruthenium dioxidecontaining particles having an exterior surface; and a surface stabilizer predominantly disposed on and coupled to the exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of transition-metal atoms including at least one transition metal selected from one of Manganese, Chromium, Tantalum, and Vanadium.

[0006] According to another aspect, a method for forming an electrocatalyst includes: impregnating a plurality of ruthenium dioxide-containing particles with a solution to form a mixture, wherein the solution includes a transition-metal precursor and a liquid, wherein the transition-metal precursor includes at least one transition metal selected from manganese, chromium, tantalum, and vanadium, and wherein a weight ratio of the plurality of ruthenium dioxide-containing particles to the transition-metal precursor in the mixture ranges from 10: 1 to2025-061-02 25: 1; drying the mixture to form a dried mixture including a catalyst; and optionally thermally treating the dried mixture.

[0007] According to another aspect, an electrochemical apparatus for a gas evolution reaction includes: a cathode; an anode including an electrocatalyst, wherein the electrocatalyst includes: a plurality of ruthenium dioxide-containing particles, each of the plurality of ruthenium dioxide-containing particles having an exterior surface, and a surface stabilizer predominantly disposed on and coupled to the exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of transition-metal atoms including at least one transition metal selected from one of Manganese, Chromium, Tantalum, and Vanadium; and an electrical energy source electrically coupled to the cathode and the anode.BRIEF DESCRIPTION OF THE DRAWINGS

[0008] FIG. 1A illustrates electrocatalyst 162, according to some embodiments.

[0009] FIG. IB illustrates electrochemical apparatus 100, according to some embodiments.

[0010] FIG. 2 illustrates method 200 for forming a catalyst, according to some embodiments.

[0011] FIG. 3A illustrates a process for preparing a Mn(SA) / RuO2 catalyst, according to some embodiments.

[0012] FIG. 3B illustrates a transmission electron microscopy (TEM) image of a Mn(SA) / RuO2 catalyst, according to some embodiments.

[0013] FIG. 3C illustrates a particle size analysis corresponding to the transmission electron microscopy image of FIG. 3B, according to some embodiments.

[0014] FIG. 3D illustrates an aberration-corrected high-angle annular dark-field scanning transmission electron microscopy image of a Mn(SA) / RuO2 catalyst, according to some embodiments.

[0015] FIG. 3E illustrates a fast Fourier transform pattern corresponding to the image of FIG. 3D, according to some embodiments.

[0016] FIG. 3F illustrates an annular dark-field scanning transmission electron microscopy image showing single-atom manganese within a RuCh matrix, according to some embodiments.2025-061-02

[0017] FIG. 3G illustrates a low-magnification high-angle annular dark-field image and corresponding elemental mapping results showing distribution of manganese, oxygen, and ruthenium, according to some embodiments.

[0018] FIG. 3H illustrates an X-ray photoelectron spectroscopy sweep scan pattern showing manganese, oxygen, and ruthenium peaks, according to some embodiments.

[0019] FIG. 4A illustrates an Mn 2p X-ray photoelectron spectroscopy spectrum of RuCh and Mn(SA) / RuO2 catalyst, according to some embodiments.

[0020] FIG. 4B illustrates a Ru 3d X-ray photoelectron spectroscopy spectrum of RuCh and Mn(SA) / RuO2 catalyst, according to some embodiments.

[0021] FIG. 4C illustrates a valence-band X-ray photoelectron spectroscopy profile of RUO2and Mn(SA) / RuO2 catalyst, according to some embodiments.

[0022] FIG. 4D illustrates a Ru K-edge X-ray absorption near-edge structure spectrum of RUO2and Mn(SA) / RuO2 catalyst, according to some embodiments.

[0023] FIG. 4E illustrates a Ru K-edge Fourier transformed extended X-ray absorption fine-structure spectrum of RuCh and Mn(SA) / RuO2 catalyst, according to some embodiments.

[0024] FIG. 4F illustrates an Mn K-edge X-ray absorption near-edge structure spectrum of Mn(SA) / RuO2 catalyst and reference materials, according to some embodiments.

[0025] FIG. 4G illustrates an Mn K-edge Fourier transformed extended X-ray absorption fine-structure spectrum of Mn(SA) / RuO2 catalyst and reference materials, according to some embodiments.

[0026] FIG. 4H illustrates a plot of fitted oxidation states of ruthenium and manganese for Mn(SA) / RuO2 catalyst, according to some embodiments.

[0027] FIG. 41 illustrates a wavelet-transform extended X-ray absorption fine-structure analysis of the Mn K-edge for reference materials and Mn(SA) / RuO2 catalyst, according to some embodiments.

[0028] FIG. 5A illustrates a linear sweep voltammetry curve comparing oxygen evolution reaction activity of RuCh and MnsA) / RuO2, according to some embodiments.

[0029] FIG. 5B illustrates a corresponding Tafel slope plot for the oxygen evolution reaction activity of RuCh and MnsA) / RuO2, according to some embodiments.2025-061-02

[0030] FIG. 5C illustrates a double-layer capacitance plot obtained from cyclic voltammetry curves for RuCh and MnsA) / RuO2, according to some embodiments.

[0031] FIG. 5D illustrates a chronopotentiometric curve at a current density of 10 mA cm2for RUO2and MnsA) / RuO2 on a glassy carbon rotating disk electrode in 0.5 M H2SO4, according to some embodiments.

[0032] FIG. 5E illustrates a plot of dissolved Ru and Mn ion concentrations in 0.5 M H2SO4 for MnsA) / RuO2 on carbon paper during an oxygen evolution reaction test at 10 mA cm2, according to some embodiments.

[0033] FIG. 5F illustrates a chronopotentiometric curve at 10 mA cm2in 0.5 M H2SO4 for MnsA) / RuO2 on carbon paper, according to some embodiments.

[0034] FIG. 5G illustrates a chronopotentiometric curve at 10 mA cm2in 1 M KOH for MnsA) / RuO2 on carbon paper, according to some embodiments.

[0035] FIG. 6A illustrates a schematic diagram of a proton exchange membrane water electrolysis cell using water as a reactant, according to some embodiments.

[0036] FIG. 6B illustrates an I-V curve for proton exchange membrane water electrolysis cells, according to some embodiments.

[0037] FIG. 6C illustrates a chronopotentiometric curve for proton exchange membrane water electrolysis cells at a current density of 1 A cm'2with a membrane, according to some embodiments.

[0038] FIG. 6D illustrates a chronopotentiometric curve for a proton exchange membrane water electrolysis cell with a MnsA) / RuO2-based anode using a membrane, according to some embodiments.

[0039] FIG. 6E illustrates a schematic diagram of an alkaline water electrolysis cell using 1 M KOH as an electrolyte, according to some embodiments.

[0040] FIG. 6F illustrates an I-V curve for alkaline water electrolysis cells, according to some embodiments.

[0041] FIG. 6G illustrates a chronopotentiometric curve at 1 A cm'2for alkaline water electrolysis cells, according to some embodiments.2025-061-02

[0042] FIG. 7A illustrates a computed free-energy diagram for each step of an oxygen evolution reaction process via an adsorbate-evolving mechanism pathway, according to some embodiments.

[0043] FIG. 7B illustrates a plot of energies for surface ruthenium demetallation over simulated RuCh and MnsA) / RuO2 surfaces, according to some embodiments.

[0044] FIG. 7C illustrates an iR-corrected cyclic voltammetry curve of RuCh and MnsA) / RuO2 on glassy carbon rotating disk electrode in 1 M KOH, according to some embodiments.

[0045] FIG. 7D illustrates a set of in situ Raman spectra obtained over Ru02 on carbon paper at oxygen evolution reaction overpotentials of 0 to 1.53 V vs. RHE in 0.5 M H2SO4, according to some embodiments.

[0046] FIG. 7E illustrates a set of in situ Raman spectra obtained over MnSA) / RuO2 on carbon paper at oxygen evolution reaction overpotentials of 0 to 1.53 V vs. RHE in 0.5 M H2SO4, according to some embodiments.

[0047] FIG. 8A illustrates an X-ray diffraction pattern of Cr-RuCh and RuCh, according to some embodiments.

[0048] FIG. 8B illustrates a TEM image for Cr-RuCh, according to some embodiments.

[0049] FIG. 8C illustrates an HRTEM image for Cr-RuCh, according to some embodiments.

[0050] FIG. 8D illustrates a corresponding FFT pattern for FIG. 8C, according to some embodiments.

[0051] FIG. 8E illustrates HAADF-STEM with EDS elemental mapping results for Cr-RUO2, according to some embodiments.

[0052] FIG. 8F illustrates Cr 2p XPS spectra of RuCh and Cr-RuCh, according to some embodiments.

[0053] FIG. 8G illustrates Ru 3d XPS spectra of RuCh and Cr-RuCh, according to some embodiments.

[0054] FIG. 8H illustrates CER overpotentials of metal-modified RuCh at various current densities, according to some embodiments.2025-061-02

[0055] FIG. 9 illustrates a linear sweep voltammetry curve on a glassy carbon rotating disk electrode for chlorine evolution reaction of RuCh and Cr-RuCh, according to some embodiments.

[0056] FIG. 10 illustrates a linear sweep voltammetry curve for chlorine evolution reaction before and after 10,000 cycles of cyclic voltammetry tests of RuCE and Cr-RuCE, according to some embodiments.

[0057] FIG. 11 illustrates a chronopotentiometric curve at 10 mA cm2for chlorine evolution reaction of Cr-RuCE on carbon paper, according to some embodiments.

[0058] FIG. 12 illustrates a chlorine evolution selectivity plot for RuCE and Cr-RuCE, according to some embodiments.

[0059] FIG. 13 A illustrates an X-ray diffraction pattern of an as-prepared Cr-RuCE / Ti electrode, according to some embodiments.

[0060] FIG. 13B illustrates an SEM image for a Cr-RuCE / Ti electrode according to some embodiments.

[0061] FIG. 13C illustrates an SEM image for a Cr-RuCE / Ti electrode according to some embodiments.

[0062] FIG. 13D illustrates an SEM image for a Cr-RuCE / Ti electrode according to some embodiments.

[0063] FIG. 13E illustrates SEM-EDX mapping results for a Cr-RuCE / Ti electrode according to some embodiments.

[0064] FIG. 14 A illustrates a linear sweep voltammetry curve of RuCh / Ti and Cr-RuCE / Ti electrodes for chlorine evolution reaction, according to some embodiments.

[0065] FIG. 14B illustrates an electrochemical impedance spectroscopy curve of RuCE / Ti and Cr-RuCE / Ti electrodes for chlorine evolution reaction, according to some embodiments.

[0066] FIG. 15 illustrates chronopotentiometric stability test and corresponding CL selectivity over multiple 12 h cycles, where arrows indicate electrolyte replacement to maintain CER-dominant conditions, according to some embodiments.

[0067] FIG. 16 A illustrates LSV curves for a comparison of Cr-RuCE / Ti electrode before and after long-term operation, according to some embodiments.

[0068] FIG. 16B illustrates SEM-EDX survey spectra for a comparison of Cr-RuCE / Ti electrode before and after long-term operation, according to some embodiments.2025-061-02DETAILED DESCRIPTION

[0069] Embodiments of the present disclosure provide electrocatalysts, electrochemical apparatuses, and methods for forming electrocatalysts having improved activity and / or stability during electrochemical gas evolution reactions. In some embodiments, the electrocatalyst includes ruthenium oxide-containing particles and a surface stabilizer disposed on exterior surfaces and / or near-surface regions of the ruthenium oxide-containing particles. In some embodiments, the surface stabilizer is predominantly surface disposed rather than substituted throughout a bulk RuCE lattice, thereby allowing the electrocatalyst to retain desirable RuCE catalytic activity while improving durability. The disclosed electrocatalysts may be used, for example, in oxygen evolution reactions, chlorine evolution reactions, water electrolysis, proton exchange membrane water electrolysis, alkaline water electrolysis, and chlor-alkali electrolysis.

[0070] FIG. 1A illustrates electrocatalyst 162, according to some embodiments.Electrocatalyst 162 can be used for electrochemical reactions. Electrocatalyst 162 includes ruthenium, oxygen, and a surface stabilizer (“SS”). In some embodiments, electrocatalyst 162 includes a plurality of ruthenium oxide-containing particles and the surface stabilizer. In some embodiments, electrocatalyst 162 includes a ruthenium oxide-containing titanium mesh and the surface stabilizer. The surface stabilizer can be disposed on the ruthenium oxide-containing particles. Each ruthenium dioxide-containing particle may include an exterior surface, and the surface stabilizer may be predominantly disposed on, coupled to, coordinated with, adsorbed to, anchored to, and / or otherwise associated with the exterior surface. In one non-limiting example, the surface stabilizer is predominantly disposed on the exterior surface of the plurality of ruthenium oxide-containing particles. In some embodiments, the surface stabilizer can be disposed on and coupled to the exterior surface of the ruthenium dioxide-containing particles, meaning that transition-metal atoms or transition-metal-containing species are anchored to, bonded to, coordinated with, adsorbed on, or otherwise retained by the exterior surfaces of the ruthenium dioxide-containing particles. For example, the coupling (e.g., direct coupling) may include metal-oxygen bonding. In one example, manganese atoms of the surface stabilizer are coordinated with oxygen atoms and lack substantial manganese-manganese bonding, indicating isolated manganese species directly associated with the RuCE surface.2025-061-02

[0071] The plurality of ruthenium oxide-containing particles can include one or more oxide forms of ruthenium. In some embodiments, the plurality of ruthenium oxide-containing particles include a plurality of ruthenium dioxide-containing particles. The plurality of ruthenium dioxidecontaining particles can be in the form of stoichiometric RuCh or non-stoichiometric RuCh. In some embodiments, the ruthenium dioxide-containing particles include rutile RuCh particles. The ruthenium dioxide-containing particles can include at least 90 wt%, at least 95 wt%, or at least 98 wt% rutile RuCh.

[0072] The ruthenium dioxide-containing particles of electrocatalyst 162 may have an average particle size selected to provide a high density of catalytically accessible surface sites while maintaining structural integrity during gas evolution reactions. In some embodiments, the average particle size ranges from about 5 nm to about 200 nm, about 10 nm to about 100 nm, about 15 nm to about 75 nm, about 20 nm to about 50 nm, about 25 nm to about 40 nm, or about 28 nm to about 35 nm. In some embodiments, the ruthenium dioxide-containing particles have an average particle size of about 30 nm. The particle size may be determined by transmission electron microscopy, scanning electron microscopy, or another suitable particle-size characterization method. In some embodiments, introduction of the surface stabilizer does not substantially change the particle size of the underlying ruthenium dioxide-containing particles.

[0073] In some embodiments, the surface stabilizer includes at least one of 3d transition metals (i.e., V, Cr, Mn, Fe, Co, Ni, Cu, Zn), 4d metals (i.e., Zr, Nb, Mo), 5d metals (i.e., Ta, W), and rare-earth lanthanides (i.e., La, Ce). In some embodiments, the surface stabilizer used for electrocatalysts utilized in CER includes at least one 3d transition metal (i.e., V, Cr, Mn, Fe, Co, Ni, Cu, Zn), at least one 4d metal (i.e., Zr, Nb, Mo), at least one 5d metal (i.e., Ta, W), and / or at least one rare-earth lanthanide (i.e., La, Ce).

[0074] In some embodiments, the surface stabilizer includes a plurality of transition-metal atoms. The transition-metal atoms may include one or more of manganese, chromium, tantalum, and vanadium. For example, the surface stabilizer may include manganese atoms, chromium atoms, tantalum atoms, vanadium atoms, or any combination thereof. In some embodiments, the surface stabilizer includes manganese and is configured to improve oxygen evolution reaction activity and stability of the ruthenium dioxide-containing particles. In some embodiments, the surface stabilizer includes chromium and is configured to improve chlorine evolution reaction2025-061-02 activity and stability of the ruthenium dioxide-containing particles. In some embodiments, the surface stabilizer includes tantalum or vanadium and is configured to restructure the RuCh surface and enhance its chemical robustness.

[0075] In some embodiments, the surface stabilizer (e.g., the transition-metal atoms of the surface stabilizer) is predominantly located at an exterior surface or near-surface region of the ruthenium dioxide-containing particles. For example, at least 50 wt%, at least 60 wt%, at least 70 wt%, at least 80 wt%, at least 90 wt%, or substantially all of the surface stabilizer may be disposed at or adjacent to the exterior surface of the ruthenium dioxide-containing particles. In one non-limiting example, such surface-arranged atoms may stabilize catalytically active sites while avoiding a bulk compositional change that would otherwise reduce the intrinsic activity of RuCh. In some embodiments, the surface stabilizer suppresses Ru dissolution and maintains catalytic performance without requiring a bulk crystal-doped material.

[0076] In some embodiments, the surface stabilizer is not provided as a bulk substitutional dopant in a lattice of the ruthenium dioxide-containing particles (e.g., bulk crystal-doped material). For example, the electrocatalyst 162 may be distinguished from a bulk crystal-doped material in which transition-metal atoms replace ruthenium atoms throughout a RuCh crystal lattice to follow the formula MvRu / xCh. Instead, the surface stabilizer (e.g., including transitionmetal atoms) may be introduced after formation of the ruthenium dioxide-containing particles and may function predominantly as a surface stabilizer. In some embodiments, X-ray diffraction of electrocatalyst 162 indicates retention of a rutile RuCh crystal structure without formation of a separate detectable bulk transition-metal oxide phase. Accordingly, in some embodiments, the introduced transition metal atoms can function predominantly as a surface stabilizer, rather than as a uniformly lattice-substituting dopant throughout the RuCh crystal. The surface stabilization of the present disclosure suppresses over-oxidation and dissolution of Ru under anodic conditions, while preserving the activity of RuCh.

[0077] In some embodiments, the surface stabilizer may include atoms that are disposed on an exterior surface, coordinated with surface oxygen atoms, incorporated into a near-surface coordination environment, or partially embedded within the ruthenium dioxide-containing particles. In some embodiments, such near-surface positioning does not require the surface stabilizer to be uniformly distributed throughout the bulk RuCh lattice. Accordingly, in some2025-061-02 embodiments, the presence of the surface stabilizer in a surface-adjacent lattice position or oxygen-coordination site may still correspond to a surface stabilizer that is predominantly disposed on and coupled to the exterior surface of the ruthenium dioxide-containing particles.

[0078] In some embodiments, the surface stabilizer includes a plurality of isolated transition-metal atoms. As used herein, an isolated transition-metal atom may refer to a transition-metal atom that is separated from adjacent transition-metal atoms such that the transition-metal atoms do not form a bulk transition-metal oxide phase or a continuous transition-metal oxide coating detectable by one or more conventional characterization techniques. In some embodiments, the isolated transition-metal atoms are single atoms coordinated with oxygen atoms at or near the exterior surface of a ruthenium dioxide-containing particle.

[0079] The surface stabilizer may be present relative to the ruthenium dioxide-containing particles at a molar atomic ratio selected to provide surface stabilization without excessive coverage of active sites. In some embodiments, a molar atomic ratio of surface stabilizer (e.g., transition-metal atoms) to ruthenium dioxide-containing particles ranges from about 1 :5 to about 1:150, about 1:10 to about 1:100, about 1:15 to about 1:70, about 1:20 to about 1:60, about 1:25 to about 1:50, about 1:30 to about 1:45, or about 1:35 to about 1:40. In some embodiments, the molar atomic ratio ranges from about 1:15 to about 1:70. In one non-limiting example, lower transit! on- metal loadings (e.g., less than 1:70) may provide insufficient stabilization, leading to decreased activity / stability, whereas higher transition-metal loadings (e.g., greater than 1:15) may block catalytically active RuCh sites, reduce conductivity, and / or introduce undesired phases / aggregates after treatment, which can negatively affect catalytic performance.

[0080] In manganese-containing embodiments, the mass ratio of manganese atoms to the ruthenium dioxide-containing particles may range from about 1:20 to about 1:250, about 1:30 to about 1:200, about 1:40 to about 1:160, about 1:50 to about 1:140, about 1:60 to about 1:120, about 1:60 to about 1:100, or about 1:60 to about 1:80. In some embodiments, the mass ratio of manganese atoms to the ruthenium dioxide-containing particles ranges from about 1:40 to about 1:160. In some embodiments, manganese loadings of the present disclosure balances activity and conductivity.2025-061-02

[0081] In chromium-containing embodiments, the mass ratio of chromium atoms to the ruthenium dioxide-containing particles may range from about 1:20 to about 1:100, about 1:30 to about 1:80, about 1:35 to about 1:70, about 1:40 to about 1:60, about 1:45 to about 1:55, or about 1:50. In some embodiments, the mass ratio of chromium atoms to the ruthenium dioxide-containing particles ranges from about 1:40 to about 1:60. Chromium-containing electrocatalyst 162 may be particularly suitable for chloride- containing electrolytes, brines, seawater, or chloralkali environments. Chromium species on or near the RuCE surface may improve resistance to surface degradation during chlorine evolution.

[0082] In some embodiments, the surface stabilizer is present in electrocatalyst 162 at a weight percentage selected to provide surface stabilization while preserving accessible RuCE catalytic sites. For example, the surface stabilizer may be present in an amount ranging from about 0.05 wt% to about 15 wt%, about 0.1 wt% to about 10 wt%, about 0.25 wt% to about 7.5 wt%, about 0.5 wt% to about 5 wt%, about 0.75 wt% to about 3 wt%, about 1 wt% to about 2 wt%, or values therebetween, based on a total weight of the electrocatalyst 162. In manganese-containing embodiments, the manganese atoms may be present at about 1-2 wt%. In some embodiments, a transition-metal weight percentage below a weight range of the present disclosure may provide insufficient coverage or stabilization of exterior RuCE surface sites, whereas a transition-metal weight percentage above a weight range of the present disclosure may block active RuCE sites or reduce conductivity.

[0083] Electrocatalyst 162 may be configured for oxygen evolution reaction. In some embodiments, the oxygen evolution reaction is performed in an acidic electrolyte, neutral electrolyte, alkaline electrolyte, solid polymer electrolyte, or combinations thereof. For example, electrocatalyst 162 may be used in sulfuric acid, potassium bicarbonate, potassium hydroxide, water, or another water-containing electrolyte. In some embodiments, electrocatalyst 162 provides lower charge-transfer resistance, improved long-term stability, and suppressed Ru dissolution relative to RuCE particles lacking the surface stabilizer.

[0084] Electrocatalyst 162 may be configured for chlorine evolution reaction. In some embodiments, the chlorine evolution reaction is performed in a chloride-containing electrolyte, such as sodium chloride solution, potassium chloride solution, brine, seawater, acidic brine, and / or another chloride-containing medium. In some embodiments, chromium-containing2025-061-02 electrocatalyst 162 provides improved chlorine evolution activity, improved stability during repeated cycling, improved selectivity, and charge redistribution compared to a RuCE electrocatalyst lacking chromium-containing surface stabilization.

[0085] FIG. IB illustrates electrochemical apparatus 100, according to some embodiments. Electrochemical apparatus 100 includes at least one of a reservoir 110, electrical energy source 120, cathode 130, anode 140, and electrolyte 150. Electrochemical apparatus 100 may further include a separator, such as a diaphragm or membrane. The cathode 130 and the anode 140 can be at least partially disposed in the electrolyte 150 and are electrically coupled to the electrical energy source 120. The electrical energy source 120 may be configured to apply a voltage between the cathode 130 and the anode 140 to drive electrochemical reactions at the respective electrodes. For example, reduction may occur at the cathode 130, and oxidation may occur at the anode 140, such that a gas 132 may be generated at the cathode 130 and / or a gas 142 may be generated at the anode 140.

[0086] The reservoir 110 may define an interior volume configured to receive and retain the electrolyte 150 during operation of the electrochemical apparatus 100. Reservoir 110 may be a tank, tube, or piping sufficient for holding, storing, and / or placing the electrolyte 150 in contact with the cathode 130 and / or the anode 140. The reservoir 110 may be formed from any material chemically compatible with the electrolyte 150 and with gases generated during operation, including glass, polymeric materials, ceramic materials, metals, coated metals, or combinations thereof. In some embodiments, the reservoir 110 may include one or more ports, covers, seals, vents, gas outlets, fluid inlets, fluid outlets, sensors, baffles, or other structures configured to introduce electrolyte 150, remove electrolyte 150, collect gas products, control temperature, or otherwise facilitate operation of the electrochemical apparatus 100. The reservoir 110 may be a single-chamber reservoir or may define multiple chambers, for example, where portions of the reservoir 110 are separated by a diaphragm, membrane, or other separator.

[0087] The electrical energy source 120 may be electrically coupled to the cathode 130 and the anode 140 and may be configured to apply an electrical potential, voltage, or other electrical input between the cathode 130 and the anode 140. The electrical energy source 120 may include, for example, a direct-current power supply, battery, photovoltaic source, power converter, or other source of electrical energy. During operation, the electrical energy source 120 may drive2025-061-02 reduction at the cathode 130 and oxidation at the anode 140, thereby converting electrical energy into chemical products.

[0088] The cathode 130 may be at least partially disposed in the electrolyte 150 and electrically connected to a negative terminal of the electrical energy source 120. Cathode 130 may include a substrate. The substrate may include a conducting surface. In one example, the substrate includes one or more of titanium, nickel, stainless steel, lead, aluminum, and carbon. In another example, the substrate includes a conducting material selected from oxide-free titanium and oxide-free stainless steel. Oxide-free titanium and oxide- free stainless steel substrates may be cleaned by bath sonication and dried prior to catalyst addition. In yet another example, the catalyst is coated on conducting titanium, stainless steel, carbon paper, carbon cloth, and / or carbon felt. Carbon substrates may be acid-treated to improve hydrophilicity.

[0089] The anode 140 may be at least partially disposed in the electrolyte 150 and electrically connected to a positive terminal of the electrical energy source 120. Anode 140 can include or be in contact with electrocatalyst 162. Anode 140 may include a substrate 160. The substrate 160 may include a conducting surface. In one example, the substrate 160 includes one or more of titanium, nickel, stainless steel, lead, aluminum, and carbon. In another example, the substrate 160 includes a conducting material selected from oxide-free titanium and oxide-free stainless steel. In some embodiments, and as shown in FIG. IB, electrocatalyst 162 can be added in contact with an exterior surface of substrate 160. In some embodiments, electrocatalyst 162 is dispersed within substrate 160. In some embodiments, electrocatalyst 162 is coated on substrate 160.

[0090] The electrolyte 150 may be disposed in the reservoir 110 and may provide ionic conductivity between the cathode 130 and the anode 140. The electrolyte 150 may include water, an aqueous electrolyte, an acidic electrolyte, an alkaline electrolyte, a neutral electrolyte, a chloride-containing electrolyte, brine, seawater, and / or a solid polymer electrolyte. The electrolyte 150 may be disposed in the reservoir 110 and may be acidic, alkaline, solid oxide, or ceramic. In some embodiments, the electrolyte 150 may include an alkaline solution, such as potassium hydroxide or sodium hydroxide, as used in alkaline water electrolysis, where electrodes operate in a liquid alkaline electrolyte. The electrolyte 150 may be placed in contact with one or more of the cathode 130 and the anode 140. In other embodiments, the electrolyte2025-061-02 150 may include or be provided by a solid polymer electrolyte, such as a proton exchange membrane, that conducts protons between the anode and cathode while separating product gases and electrically insulating the electrodes.

[0091] The electrochemical apparatus 100 may further include a separator, such as a diaphragm, porous separator, ion-exchange membrane, proton exchange membrane, anion exchange membrane, solid polymer electrolyte, or other ionically conductive and electrically insulating structure. The separator may be positioned between the cathode 130 and the anode 140 and may be configured to permit ionic conduction while inhibiting electrical shorting and / or mixing of gases generated at the cathode 130 and the anode 140. In alkaline water electrolysis, electrodes may be separated by a diaphragm or separator that allows ionic transport and helps separate hydrogen and oxygen product gases. In PEM water electrolysis, the separator may be a solid polymer electrolyte membrane that conducts ions, separates product gases, and electrically insulates the electrodes. In some embodiments, the separator may be a component distinct from the electrolyte 150; in other embodiments, the separator may be at least partially integrated with, or may itself define, the electrolyte 150.

[0092] Electrochemical apparatus 100 can be used for gas evolution reactions. In some embodiments, electrochemical apparatus 100 is an electrochemical water splitter.Electrochemical water splitting includes an oxygen evolution reaction (OER) and a hydrogen evolution reaction (HER), which may occur simultaneously. The main reaction for electrochemical water splitting is shown as Equation 1 below, and a reaction for the cathode 130 (Equation 2) and the anode 140 (Equation 3) are also shown below. In one example, the cathode 130 is negatively charged, and the anode 140 is positively charged. Electrons from the cathode 130 may be used to form hydrogen gas. Electrons may be transferred from the cathode 130 to the anode 140 to complete the circuit. Therefore, hydrogen gas (e.g., gas 132) and oxygen gas (e.g., gas 142) may be produced from water and / or an electrolyte using electrical energy source 120.2H2O + electric energy — 2H2+ O2(Equation 1)2H2O + 2e" — > H2+ 2OH' (Equation 2)2OH' O2+ H2O + 2e’ (Equation 3)

[0093] The electrode(s) of the present disclosure and / or the electrochemical water splitting system (such as electrochemical apparatus 100) may be sufficient for alkaline water electrolysis2025-061-02 (AWE). The AWE system may include one or more of an electrical energy source (such as electrical energy source 120), a cathode (such as cathode 130), an anode (such as anode 140), an electrolyte (such as electrolyte 150), and a reservoir (such as reservoir 110). Alkaline conditions may provide a wide range of applications. In one example, alkaline water electrolysis utilizes two electrodes in a liquid alkaline electrolyte. The liquid alkaline electrolyte (e.g., electrolyte 150) may include an alkali, such as hydroxides of lithium, sodium, potassium, rubidium, and cesium. In one example, the liquid alkaline electrolyte solution includes one or more of potassium hydroxide, lithium hydroxide, sodium hydroxide, and water. For example, this base may have a molarity ranging from about 0.2 M to about 12 M. In another example, the base may have a molarity ranging from about 1 M to about 9 M. In yet another example, the base may have a molarity ranging from about 1 M to about 6 M.

[0094] The alkaline electrolyte may have a pH greater than 7. The alkaline electrolyte may be combined with water to alter the pH. In one example, the pH of the alkaline electrolyte ranges from about 7 to about 14. In another example, the pH of the alkaline electrolyte ranges from about 8 to about 12. In yet another example, the pH of the alkaline electrolyte ranges from about 10 to about 14. AWE may be performed at moderate temperatures and pressures, such as at a temperature ranging from about 20 °C to 120 °C, 50 °C to 100 °C, or 70 °C to 100 °C. The operating pressure during AWE may range from about 1 bar to about 40 bar. In another example, the operating pressure during AWE may range from about 2 bar to about 10 bar.

[0095] The electrode(s) of the present disclosure and / or the electrochemical water splitting system (such as electrochemical apparatus 100) may be sufficient for acidic conditions. The water splitting system may be operated in an acidic solution / electrolyte, such as a solution of sulfuric acid. For example, sulfuric acid may be 0.5 M sulfuric acid. The acidic condition may include one or more of sulfuric acid, hydrochloric acid, phosphoric acid, acetic acid, citric acid, and nitric acid. The electrochemical water splitting system may be operated in a liquid with a pH ranging from 0 to about 7. In one example, the liquid may have a pH ranging from about 2 to about 7. The liquid may have a pH of less than 7, less than 6, less than 5, or less than 4. In another example, the liquid may have a pH ranging from about 3 to about 6. Accordingly, electrochemical apparatus 100 may be utilized at various pH ranges from acidic to basic2025-061-02 conditions (0 to 14 pH). The electrode of the present disclosure and / or the electrochemical water splitting system (such as electrochemical apparatus 100) may be sufficient for PEM.

[0096] In a PEM-based electrolysis cell, water splitting is performed under acidic conditions (such as the pH of the present paragraph) using the proton exchange membrane, sufficient to produce hydrogen from water. The PEM system may include one or more of an electrical energy source (such as electrical energy source 120), a cathode (such as cathode 130), an anode (such as anode 140), an electrolyte (such as electrolyte 150), and a membrane. The membrane may be a polymer membrane and / or may separate the cathode and the anode. The membrane may be a solid polymer electrolyte. Protons may be transported across the membrane to be reduced to hydrogen. In one example, the operating temperature for PEM ranges from about 20 °C to about 120 °C.

[0097] In some embodiments, electrochemical apparatus 100 can be used to perform the chlorine evolution reaction (CER) at anode 140. Chlorine evolution is an anodic reaction used in chlor-alkali electrolysis for producing chlorine. For example, where the electrolyte 150 includes chloride ions, such as in a brine, seawater, sodium chloride solution, potassium chloride solution, or other chloride-containing electrolyte, the electrical energy source 120 may apply an anodic potential sufficient to oxidize chloride ions at or adjacent to the anode 140 to form chlorine gas (e.g., gas 142) (Equation 4).2Cl~ + electric energy — Cl2+ 2e~ (Equation 4)Accordingly, in some embodiments, electrochemical apparatus 100 is a chlor-alkali electrolyzer (e.g., diaphragm or membrane cell) using aqueous brine (NaCl) or molten salt cells. Chromium-containing electrocatalyst 162 may be particularly suitable for chloride-containing electrolytes, brines, seawater, or chlor-alkali environments. Chromium species on or near the RuCE surface can improve resistance to surface degradation during chlorine evolution.

[0098] FIG. 2 illustrates method 200 for forming a catalyst, according to some embodiments. In some embodiments, method 200 includes mixing 210 a plurality of ruthenium oxide-containing particles with a solution to form a mixture, drying 220 the mixture to form a dried mixture including a catalyst, and optionally thermally treating 230 the dried mixture.Method 200 can form electrocatalyst 162.2025-061-02

[0099] At mixing 210, the plurality of ruthenium oxide-containing particles (e.g., ruthenium dioxide) are mixed with the solution to form the mixture. The solution may include a transition-metal precursor of the present disclosure dissolved or dispersed in a solvent, such as one or more of water, ethanol, methanol, and isopropanol. Mixing 210 may include contacting, wetting, dispersing, suspending, immersing, soaking, impregnating, stirring, agitating, sonicating, drop-casting, spray-coating, or any combination thereof. In some embodiments, mixing 210 includes contacting the exterior surfaces of the ruthenium di oxide-containing particles with the solution such that a transition-metal precursor is distributed on, or adjacent to, surface regions of the ruthenium dioxide- containing particles.

[0100] In some embodiments, mixing 210 includes impregnating the ruthenium dioxidecontaining particles with the solution such that the transition-metal precursor is deposited onto exterior surfaces or near-surface regions of the ruthenium dioxide-containing particles upon subsequent drying 220. In some embodiments, mixing 210 includes stirring a suspension of the ruthenium dioxide-containing particles in the solution for a time sufficient to promote wetting of the particle surfaces by the solution. In some embodiments, mixing 210 includes drop-casting or otherwise applying the solution onto ruthenium dioxide-containing particles that are already disposed on a conductive substrate, such as titanium mesh, carbon paper, carbon cloth, glassy carbon, stainless steel, nickel, or another conductive substrate.

[0101] The transition-metal precursor can include at least one of a Manganese-containing precursor, a Chromium-containing precursor, a Vanadium-containing precursor, and a Tantalum-containing precursor. The transition-metal precursor can include a transition-metal containing salt. Accordingly, in some embodiments, the transition metal containing salt includes at least one of a Manganese-containing salt, a Chromium-containing salt, a Vanadium-containing salt, and a Tantalum-containing salt. Examples of salts include nitrate salts, chloride salts, and acetate salts. For example, the transition-metal precursor may include manganese acetate, chromium chloride, tantalum chloride, vanadium chloride, vanadium nitrate, chromium nitrate, manganese nitrate, tantalum acetate, or combinations thereof.

[0102] The weight ratio of the ruthenium dioxide-containing particles to the transitionmetal precursor in the mixture may range from about 5:1 to about 50:1, about 8:1 to about 35:1, about 10:1 to about 25:1, about 12:1 to about 20:1, about 14:1 to about 18:1, or about 16:1 to2025-061-02 about 17: 1. In some embodiments, the amount of transition-metal precursor is selected so that, after drying 220 and any optional thermally treating 230, the transition-metal atoms provide sufficient surface stabilization without blocking an excessive number of catalytically active RuCh surface sites.

[0103] At drying 220, the mixture is dried to form a dried mixture including a catalyst. Drying 220 may remove at least a portion of the liquid and may anchor, deposit, concentrate, or otherwise position the transition-metal precursor or transition-metal species on exterior surfaces of the ruthenium dioxide-containing particles. In some embodiments, drying 220 is performed at a temperature ranging from about 20 °C to about 150 °C, about 40 °C to about 130 °C, about 60 °C to about 120 °C, about 65 °C to about 100 °C, about 70 °C to about 90 °C, or about 70 °C to about 80 °C.

[0104] Drying 220 may be performed for about 0.5 hours to about 48 hours, about 1 hour to about 24 hours, about 4 hours to about 20 hours, about 6 hours to about 18 hours, or about 12 hours to about 16 hours. Drying 220 may be conducted in air, vacuum conditions, nitrogen, or argon. In one example, a RuCh and manganese acetate mixture may be dried at about 70 °C for about 12 hours. In another example, a RuCh and chromium chloride mixture may be dried at about 70 °C for about 16 hours. In another example, a RuCh and tantalum chloride mixture may be dried at about 75 °C for about 18 hours. In another example, a RuCh and vanadium chloride mixture may be dried at about 80 °C for about 6 hours.

[0105] The dried mixture is optionally thermally treated 230. Thermally treating 230 may remove residual solvent, improve coupling between transition-metal atoms and exterior surfaces of the ruthenium dioxide-containing particles, modify the electronic structure of surface Ru species, or improve and / or promote resistance of the catalyst to electrochemical degradation. In some embodiments, thermally treating 230 includes annealing at a temperature ranging from about 200 °C to about 700 °C, about 250 °C to about 650 °C, about 300 °C to about 600 °C, about 350 °C to about 550 °C, about 400 °C to about 500 °C, or about 450 °C. Thermally treating 230 may be performed for about 0.1 hours to about 10 hours, about 0.5 hours to about 4 hours, about 0.75 hours to about 2 hours, or about 1 hour to about 1.5 hours.

[0106] Thermally treating 230 may be conducted in air, nitrogen, argon, an oxygen-containing gas, or another controlled atmosphere. In one example, a chromium-modified RuCh2025-061-02 catalyst may be annealed at about 450 °C for about 1 hour under argon. In another example, a vanadium- modified RuCh catalyst may be annealed at about 450 °C for about 1.5 hours under nitrogen. In some embodiments, thermally treating 230 is omitted, for example, where impregnation and drying are sufficient to provide the desired surface-stabilized electrocatalyst.

[0107] In one example, method 200 can include providing or fabricating a RuCh-coated titanium (Ti) mesh as the base dimensionally stable anode (DSA) electrode. Subsequently, Chromium can be introduced by adding a Cr-containing precursor solution (e.g., mixing 210), followed by thermal treatment (e.g., thermally treating 230) to achieve incorporation.

[0108] In another example, method 200 includes providing or synthesizing a RuCh substrate, optionally in the form of a powder, thin film, or a conductive support coated with RuCh; Impregnating the RuCh substrate with a solution including one or more transition metal salts selected from nitrates, chlorides, or acetates of transition metals, including but not limited to manganese (Mn), chromium (Cr), tantalum (Ta), and vanadium (V). Suitable examples include vanadium nitrate, chromium chloride, tantalum chloride, manganese acetate, and similar compounds; drying the impregnated substrate at a temperature ranging from 60 °C to 120 °C for a duration of 1 to 24 hours to remove solvent and anchor the metal salts on the RuCh surface; and optionally subjecting the dried material to thermal treatment at a temperature of 300 °C to 600 °C in air or inert atmosphere (e.g., nitrogen or argon) for 0.5 to 4 hours. This process promotes the incorporation of metal species, modifies surface electronic structure, and enhances resistance to electrochemical degradation.

[0109] In some embodiments, electrocatalyst 162 is formed using pre-synthesized or commercially available RuCh, rather than by co-forming a bulk doped oxide in one pot.Accordingly, in some embodiments, electrocatalyst 162 can be formed by impregnation, rather than complex hydrothermal synthesis. Additionally, method 200 can be conducted using ruthenium dioxide powders and ruthenium dioxide coated titanium mesh. Method 200 delivers a significant improvement in long-term activity and stability. In particular, the surface stabilizer can suppress Ru dissolution and maintain catalytic performance without requiring a bulk crystaldoping process.Example 1 - Mnts.v / RuCh electrocatalyst2025-061-02

[0110] FIG. 3A illustrates a process for preparing a Mn(SA) / RuO2 catalyst, according to some embodiments. The Mn(SA) / RuO2 catalyst was prepared via a direct impregnation method, where freshly synthesized RuCh nano powder was immersed in an Mn3+solution, followed by solvent evaporation. X-ray diffraction (XRD) patterns show that the tetragonal crystal structure of rutile RuCh (JCPDS 70-2662) remained unchanged after Mn adhesion. FIG.3B illustrates a transmission electron microscopy (TEM) image of a Mn(SA) / RuO2 catalyst, according to some embodiments. FIG. 3C illustrates a particle size analysis corresponding to the transmission electron microscopy image of FIG. 3B, according to some embodiments. Transmission electron microscopy (TEM) images reveal that both RuCh and Mn(SA) / RuO2 catalysts have an average size of approximately 30 nm, indicating that Mn incorporation did not significantly alter the particle size.

[0111] FIG. 3D illustrates an aberration-corrected high-angle annular dark-field scanning transmission electron microscopy image of a Mn(SA) / RuO2 catalyst, according to some embodiments. FIG. 3E illustrates a fast Fourier transform pattern corresponding to the image of FIG. 3D, according to some embodiments. Aberration-corrected high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) images captured through

[0111] zone axis and corresponding fast Fourier transform (FFT) pattern show the bright dots representing Ru atoms along the (101) and (110) planes of RuCh with interplanar spacings of 2.6 and 3.2 A, respectively. FIG.3F illustrates an annular dark-field scanning transmission electron microscopy image showing single-atom manganese within a RuCh matrix, according to some embodiments. Specifically, annular dark field STEM (ADF-STEM) images confirm the existence of single-atom Mn within the RuCh matrix. O atoms are not visible in either HAADF-STEM or ADF-STEM images due to much lighter atomic weight.

[0112] FIG. 3G illustrates a low-magnification high-angle annular dark-field image and corresponding elemental mapping results showing distribution of manganese, oxygen, and ruthenium, according to some embodiments. Low-magnification HAADF image combined with elemental mapping images show the uniform distribution of Mn throughout the RuCh matrix. Inductively coupled plasma optical emission spectroscopy (ICP-OES) analysis further quantified the Mn content at approximately 1.42 wt%. FIG. 3H illustrates an X-ray photoelectron spectroscopy sweep scan pattern showing manganese, oxygen, and ruthenium peaks, according2025-061-02 to some embodiments. The presence of Mn, Ru, and O was confirmed through the X-ray photoelectron spectroscopy (XPS) sweep scan pattern, which displays clear peaks attributed to these elements in the Mn(SA) / RuO2 electrocatalyst, thus demonstrating the successful incorporation of Mn species.

[0113] FIG. 4A illustrates an Mn 2p X-ray photoelectron spectroscopy spectrum of RuCh and Mn(SA) / RuO2 catalyst, according to some embodiments. From the high-resolution Mn XPS spectrum of Mn(SA) / RuO2, two distinct deconvoluted peaks assigned to the Mn3+and Mn4+species in the Mn 2p2 / 3 region at 641.2 and 644.0 eV, respectively, were observed, indicating a chemical valence for Mn ranging between +3 and +4. Conversely, the control RuCh catalyst exhibits no evidence of Mn peaks, highlighting a notable difference in chemical composition. FIG. 4B illustrates a Ru 3d X-ray photoelectron spectroscopy spectrum of RuCh and Mn(SA) / RuO2 catalyst, according to some embodiments. In the region from 288 to 270 eV of the high-resolution Ru 3d XPS spectra for both Mn(SA) / RuO2 and RuCh, two deconvoluted peaks were observed, Ru 3dv2 and Ru 3ds / 2, associated with Ru4+. Remarkably, the Ru 3 d / 2 XPS peak for RUO2, unaffected by the nearby Cis signal, shifts negatively by 0.2 eV after Mn inclusion. This is accompanied by a similar negative shift in the Ru 3p spectrum, indicating a reduction in the oxidation state of the Ru species. FIG.4C illustrates a valence-band X-ray photoelectron spectroscopy profile of RuCh and Mn(SA) / RuO2 catalyst, according to some embodiments.Mn(SA) / RuO2 features a valence band at higher energy than RuCh, verifying enhanced oxidative capacity and corrosion resistance in oxidative environments.

[0114] FIG.4D illustrates a Ru K-edge X-ray absorption near-edge structure spectrum of RUO2and Mn(SA) / RuO2 catalyst, according to some embodiments. The X-ray absorption near-edge spectroscopy (XANES) spectra at the Ru K-edge of Mn(SA) / RuO2 and RuCh are nearly identical, yet a closer examination of the XANES spectra showed a minor decrease in the near-edge absorption energy and white line peak for Mn(SA) / RuO2 compared to RuCh. This shows a slightly reduced oxidation state of Ru in Mn(SA) / RuO2. FIG.4E illustrates a Ru K-edge Fourier transformed extended X-ray absorption fine-structure spectrum of Ru02 and Mn(SA) / RuO2 catalyst, according to some embodiments. The Fourier transformed extended X-ray absorption fine- structure (FT-EXAFS) spectrum at the Ru K-edge for Mn(SA) / RuO2 closely mirrors that of RUO2, showing unchanged Ru coordination structures upon Mn incorporation.2025-061-02

[0115] FIG.4F illustrates an Mn K-edge X-ray absorption near-edge structure spectrum of Mn(SA) / RuO2 catalyst and reference materials, according to some embodiments. For the XANES at Mn K-edge, the adsorption edge of Mn(SA) / RuO2 is located between MrnO- and MnCh, illustrating that the Mn valence ranges from +3 to +4. FIG.4G illustrates an Mn K-edge Fourier transformed extended X-ray absorption fine-structure spectrum of Mn(SA) / RuO2 catalyst and reference materials, according to some embodiments. The FT-EXAFS spectrum of Mn(SA) / RuO2 at the Mn K-edge displays a main peak at approximately 1.5 A, which is very close to that of Mn in the MnCh structure, coordinated with six O atoms. FIG.4H illustrates a plot of fitted oxidation states of ruthenium and manganese for Mn(SA) / RuO2 catalyst, according to some embodiments. The average oxidation states of Ru and Mn in Mn(SA) / RuO2, determined to be +3.9 and +3.5, respectively, are confirmed based on the linear relationship between their K-edge positions (Eo) and the formal valences of reference samples.

[0116] FIG. 41 illustrates a wavelet-transform extended X-ray absorption fine-structure analysis of the Mn K-edge for reference materials and Mn(SA) / RuO2 catalyst, according to some embodiments. The wavelet transform (WT) EXAFS analysis for Mn(SA) / RuO2 shows a distinct peak for Mn-0, with no evidence of Mn-Mn bonding, precluding the formation of MuCh species and thus verifying the single-atom dispersion of Mn. These results show that incorporating single-atom Mn on the RuCh enhances the catalyst’s oxidative capacity and introduces low-valent Ru sites, visibly conducive to facilitating the OER activity and stability under varied electrolytes and oxidative potentials.

[0117] FIG. 5A illustrates a linear sweep voltammetry curve comparing oxygen evolution reaction activity of RuCh and MnsA) / RuO2, according to some embodiments. FIG. 5B illustrates a corresponding Tafel slope plot for the oxygen evolution reaction activity of RuCh and MnsA) / RuO2, according to some embodiments. The OER performance was assessed for Mn(SA) / RuO2 and Ru02 catalysts using standard three-electrode systems across varied electrolytes, including 0.5 M H2SO4 (pH 0), 0.5 M KHCO3 (pH 8.8), and 1 M KOH (pH 14). Through optimization of the Mn content in Mn(SA) / RuO2, by varying the initial mass ratio of manganese triacetate to Ru02, Mn(SA) / RuO2 synthesized at a mass ratio of 3 / 50 demonstrated best-in-class reactivity in 0.5 M H2SO4. Linear sweep voltammetry (LSV) curves and2025-061-02 corresponding Tafel slopes on glassy carbon RDE unequivocally unveil that Mn(SA) / RuO2 surpasses RuCh in activity and chemical kinetics for OER.

[0118] Specifically, Mn(SA) / RuO2 achieves a current density of 10 mA cm-2at overpotentials (ql 0) of 284 mV in 0.5 M H2SO4, 680 mV in 0.5 M KHCO3, and 326 mV in 1 M KOH with Tafel slopes of 57.7, 133.5, and 73.7 mV dec-1, respectively, outperforming Ru02 which shows overpotentials of 296 mV (pH 0), 730 mV (pH 8.8), and 382 mV (pH 14) with Tafel slopes of 66.6, 168.2, and 76.0 mV dec-1. The electrochemical impedance spectroscopy results also reveal lower charge transfer resistances for Mn(SA) / RuO2 than that of Ru02.

[0119] FIG. 5C illustrates a double-layer capacitance plot obtained from cyclic voltammetry curves for RuCE and MnsA) / RuO2, according to some embodiments. Calculation of electrochemically active surface area (ECSA) deduced from double-layer capacitance (Cai) reveals a marked enhancement in the density of active sites for Mn(SA) / RuO2 compared to RuCh, with ECSA values of 76 vs. 63 cm2(pH 0), 41 vs. 35 cm2(pH 8.8), and 88 vs. 84 cm2(pH 14), respectively. The Mn(SA) / RuO2 renders superior ECSA-normalized OER activity compared to RuCE, demonstrating the enhanced intrinsic activity toward OER due to single-atom Mn integration. Additionally, our findings indicate that our impregnation method for incorporating single-atom Mn could elevate the OER activity of commercial Ru02 catalysts across a wide pH range, underscoring its broad applicability.

[0120] FIG. 5D illustrates a chronopotentiometric curve at a current density of 10 mA cm2for RU02 and MnsA) / RuO2 on a glassy carbon rotating disk electrode in 0.5 M H2SO4, according to some embodiments. The electrochemical stability of Mn(SA) / RuO2 and Ru02 was first conducted on glassy carbon RDE at 10 mA cm'2in 0.5 M H2SO4 for 20 h. The chronopotentiometric curves reveal a marked increase in the required overpotential for pure RuCE after 17 h, in stark contrast to Mn(SA) / RuO2, which remains stable throughout the test, demonstrating the enhanced durability over Mn(SA) / RuO2.

[0121] FIG. 5E illustrates a plot of dissolved Ru and Mn ion concentrations in 0.5 M H2SO4 for MnsA) / RuO2 on carbon paper during an oxygen evolution reaction test at 10 mA cm2, according to some embodiments. The catalyst loading of Mn(SA) / RuO2 on CP was optimized to 3.2 mg cm'2in 0.5 M H2SO4, achieving an improved 7710 of 213 mV. Changes in metal concentration within the electrolyte, and structural modifications in the Mn(SA) / RuO2 / CP2025-061-02 electrode, were initially monitored. ICP-OES was employed to assess the dissolution behavior of Mn and Ru in 0.5 M H2SO4 during the 500-h OER in an H-type cell. Electrolyte samples collected from the anode side revealed distinct trends for Mn and Ru dissolution: the Ru concentration reached a peak of approximately 0.12 ppm before stabilizing, while Mn exhibited a lower maximum around 0.05 ppm and stabilized more quickly. Both Mn and Ru concentrations remained stable beyond 200 hours, indicating that the observed decline and stabilization are likely due to in-situ surface restructuring facilitated by initially high Ru ion concentrations, represented by the reaction MnCh + Ru3++ e“ RuCh + Mn2+. This restructuring may result in a more stable surface configuration, thereby supporting the sustained performance stability of the Mn(SA) / RuO2 catalyst during the OER.

[0122] FIG. 5F illustrates a chronopotentiometric curve at 10 mA cm2in 0.5 M H2SO4 for MnsA) / RuO2 on carbon paper, according to some embodiments. FIG. 5F illustrates that Mn(SA) / RuO2 maintains a prolonged lifetime with a minimal overpotential increase of only 0.04 mV / h over 1000 hours at a current density of 10 mA cm'2. Notably, the anode catalyst retains stability for over 150 hours at 100 mA cm-2, further demonstrating its robustness. The structure of the Mn(SA) / RuO2 catalyst remained intact even after prolonged OER operation in acidic conditions. FIG. 5G illustrates a chronopotentiometric curve at 10 mA cm2in 1 M KOH for MnsA) / RuO2 on carbon paper, according to some embodiments. Mn(SA) / RuO2 on CP showcases extended 1000-h stability in both 0.5 M KHCO3 (initial 7710 = 570 mV) without overpotential increase and 1 M KOH (initial 7710 = 293 mV) with negligible potential rise, confirming its exceptional durability across various conditions. Spent catalyst XPS analyses show that singleatom Mn remains intact in alkaline electrolytes.

[0123] FIG. 6A illustrates a schematic diagram of a proton exchange membrane water electrolysis cell using water as a reactant, according to some embodiments. FIG.6B illustrates an I-V curve for proton exchange membrane water electrolysis cells, according to some embodiments. The outstanding stability and reactivity of Mn(SA) / RuO2 over a wide pH range (0-14) for the OER prompted integration into the PEMWE and AWE configurations for rigorous measurements. Utilizing deionized water in the PEMWE setup, the current-voltage (I-V) polarization curves, unadjusted for iR compensation, illustrate that the Mn(SA) / RuO2-integrated electrolyzer achieves lower operational voltages of 1.59, 1.78, and 2.06 V for current densities of2025-061-02 0.5, 1, and 2 A cm'2, respectively, outpacing the performance of the RuCh-based electrolyzer, which requires voltages of 1.63, 1.84, and 2.17 V to attain the identical current densities.

[0124] FIG. 6C illustrates a chronopotentiometric curve for proton exchange membrane water electrolysis cells at a current density of 1 A cm2with a membrane, according to some embodiments. Subsequent durability tests over 60 h at 1 A cm'2indicate an undesirable voltage increase (rate: 6.3 mV / h) for the RuCh-based system, whereas the Mn(SA) / RuO2-based system exhibited markedly improved stability with a voltage rise rate of only 0.9 mV / h. This contrast in performance firmly positions Mn(SA) / RuO2 as enhancing both PEMWE system activity and stability compared to RuCh-based systems.

[0125] FIG. 6D illustrates a chronopotentiometric curve for a proton exchange membrane water electrolysis cell with a MnsA) / RuO2-based anode using a membrane, according to some embodiments. The operating voltage required to achieve a current density of 1 A cm'2in the Mn(SA) / RuO2-based electrolyzer, initially 1.78 V, was further reduced to 1.69 V by substituting membranes, making Mn(SA) / RuO2 more competitive with commercial RuCh under similar conditions. This adjustment enabled sustained operation at 1 A cm'2over 180 hours, with a lower voltage degradation rate of 0.2 mV / h.

[0126] FIG. 6E illustrates a schematic diagram of an alkaline water electrolysis cell using 1 M KOH as an electrolyte, according to some embodiments. FIG. 6F illustrates an I-V curve for alkaline water electrolysis cells, according to some embodiments. In the AWE configuration using 1 M KOH electrolyte (FIG. 6E), the electrolyzer incorporating Mn(SA) / RuO2 outperforms its RUO2counterpart (FIG.6F), requiring a lower operational voltage of 1.84 V to achieve the current density of 1 A cm'2compared to the 1.90 V needed for the RuO2-based system. FIG.6G illustrates a chronopotentiometric curve at 1 A cm2for alkaline water electrolysis cells, according to some embodiments. Notably, over a 60-h evaluation, the RuCh catalyst presents severe deactivation, with a voltage increase rate of 10.5 mV / h, which is significantly less stable than that of Mn(SA) / RuO2, which has a much lower rate of 1.6 mV / h (FIG. 6G).

[0127] FIG. 7A illustrates a computed free-energy diagram for each step of an oxygen evolution reaction process via an adsorbate-evolving mechanism pathway, according to some embodiments. Using density functional theory (DFT) calculations, the underlying mechanisms by which the inclusion of single-atom Mn enhances the RuCh surface for OER were explored.2025-061-02 Specifically, the Gibbs free energies ( G) of elementary steps involving key intermediates (i.e., OH, O, and OOH species) were quantified, which are important in dictating the overall activity of OER (2H2O(1) 02(g) + 4H+(aq) + 4e“, E° = 1.23 V). Then, the reaction pathways for the adsorbate-evolving mechanism (AEM) and lattice oxygen mechanism (LOM) were evaluated to identify the preferred OER mechanism on the Ru02 and Mn(SA) / RuO2 surfaces.

[0128] Following the AEM pathway, the PDS for the OER on the RuO2 and Mn(SA) / RuO2 surfaces are recognized as the formation of *OOH, with AG*OOH values of 1.81 and 1.61 eV, respectively. This 0.2 eV reduction in AG*OOH on the Mn(SA) / RuO2 surface suggests a facilitated *OOH formation and more favorable electrochemical reaction kinetics. By contrast, the PDS potential for the OER on RuO2 and Mn(SA) / RuO2 surfaces via the LOM is estimated at 2.58 eV and 2.30 eV, respectively — 0.77 and 0.69 eV higher than that of the AEM. Electron spin resonance (ESR) measurements further reveal that Mn(SA) / RuO2 has a lower oxygen vacancy concentration than RuO2, yet it exhibits significantly enhanced OER activity. These results, together with DFT calculations, can show that Mn as a surface stabilizer enhances OER performance by favoring the AEM rather than the LOM. Mn as a surface stabilizer can optimize the electronic structure, lowering the formation energy barriers of key intermediates (i.e., *OOH) and enhancing the AEM pathway's kinetics, thus promoting the OER more effectively on the Mn(SA) / RuO2 surface.

[0129] By calibrating the electrode chemical potential to the equilibrium potential of 1.23 V, the overpotentials for OER were determined to be 0.58 V for RuO2 and 0.38 V for Mn(SA) / RuO2 via AEM, thereby confirming the boosted activity with single-atom Mn incorporation. Additionally, the OH adsorption energy of -0.82 eV on Mn(SA) / RuO2, slightly more exothermic than -0.67 eV on RuO2, indicates that Mn as a surface stabilizer moderately enhances OH adsorption; in an acidic environment with low OH concentration, this facilitates the capture and stabilization of *OH intermediates, promoting the formation of key species like *0 and *OOH and thus favoring the AEM pathway, enhancing OER activity.

[0130] FIG. 7B illustrates a plot of energies for surface ruthenium demetallation over simulated RuO2 and MnsA) / RuO2 surfaces, according to some embodiments. In terms of stability, enthalpy change calculations for surface Ru demetallization in both RuO2 and Mn(SA) / RuO2 models indicate an increase in the energy requirement from 1.58 eV to 1.91 eV, suggesting2025-061-02 enhanced stability of surface Ru sites in Mn(SA) / RuO2 compared to RuCh. Thus, the DFT calculations corroborate the experimental findings, showing a dramatic leap in OER activity and stability with the Mn(SA) / RuO2 catalyst.

[0131] FIG. 7C illustrates an iR-corrected cyclic voltammetry curve of RuCE and MnsA) / RuO2 on glassy carbon rotating disk electrode in 1 M KOH, according to some embodiments. For analyzing the surface oxygenated species, a CV curve was obtained for the RUO2catalyst in 1 M KOH with an anodic oxidation peak at ca. 1.35 V vs. RHE, attributed to the oxidation of Ru coupled with hydroxyl deprotonation. This peak shifts negatively by 10 mV for Mn(SA) / RuO2 compared to Ru02, a pattern also observed in 0.5 M KHCO3 as the electrolyte. These observations can show that integrating single-atom Mn remarkably promotes the evolution of surface Ru species into oxyhydroxides (Ru-OOH), thereby providing highly active sites that expedite the OER, consistent with DFT predictions.

[0132] FIG. 7D illustrates a set of in situ Raman spectra obtained over Ru02 on carbon paper at oxygen evolution reaction overpotentials of 0 to 1.53 V vs. RHE in 0.5 M H2SO4, according to some embodiments. In-situ Raman spectroscopy was utilized to monitor structural changes in Mn(SA) / RuO2 during OER. The Raman spectrum indicates the crystalline structure of RUO2, with a peak at 500 cm'1related to the g mode due to the out-of-plane vibration of O atoms and two sharp peaks at 614 and 690 cm'1corresponding to theHig and / Eg modes, respectively, linked to the vibrations of O atoms around the Ru atoms. During OER in 0.5 M H2SO4, these peaks broaden and shift to lower frequencies, indicating reduced symmetry and increased vibration frequency of Ru-0 bonds in Ru02.

[0133] FIG. 7E illustrates a set of in situ Raman spectra obtained over MnSA) / RuO2 on carbon paper at oxygen evolution reaction overpotentials of 0 to 1.53 V vs. RHE in 0.5 M H2SO4, according to some embodiments. Notably, the Aig peak for RuCh shifts by about 23 cm'1when the overpotential rises from 1.23 to 1.53 V vs. RHE. In contrast, this shift is reduced to approximately 13 cm'1for Mn(SA) / RuO2, demonstrating that single-atom Mn inclusion dampens the vibration and stretching of Ru-0 bonds during OER, thereby substantially boosting the stability of Ru02. Together, these results elucidate how the incorporation of single-atom Mn can improve both the activity and stability of Ru02 for electrochemical OER across diverse pH conditions.2025-061-02

[0134] Importantly, a direct impregnation method was utilized to deposit single-atom Mn onto RuCh, a process tailored to significantly boost its OER performance across a wide pH range. This enhanced Mn(SA) / RuO2 electrocatalyst outperforms RuCh in both activity and stability, as evidenced by comprehensive testing in standard three-electrode setups and within PEMWE and AWE systems. Through combined studies with DFT, CV, and in-situ Raman spectroscopy, the important role of single-atom Mn on RuCh was illustrated, especially in stabilizing the OER process and preserving the Ru sites.Example 2: CrCh-impregnated Ru02 with argon annealing for chlorine evolution reaction

[0135] RuCh was synthesized via a co-precipitation and calcination route. Specifically, 0.75 g of RuCh 3H2O was dissolved in 150 mL of a 1:1 (v / v) water / ethanol mixture. Then, 8.6 mL of 1 M NaOH solution was added dropwise under vigorous stirring. After stirring for 1 hour, the resulting precipitate was collected by centrifugation, washed three times with water / ethanol, and dried overnight at 65 °C. The dried solid was annealed in air at 500 °C for 5 hours with a ramp rate of 5 °C / min. This yielded a black RuCh powder with a rutile crystal structure. The resulting RuCh powder was impregnated with 1.12 mM chromium chloride (CrCh) ethanol solution, using a 50:3 mass ratio of RuCh to CrCh. The mixture was dried at 70 °C for 16 hours in air. The dried powder was then thermally treated in a flowing argon atmosphere at 450 °C for 1 h, promoting surface modification and stabilization of the Cr species on the RuCh surface.

[0136] FIG. 8A illustrates an X-ray diffraction pattern of Cr-RuCE and RuCE, according to some embodiments. The sample retained the rutile structure of RuCE with no secondary phase before and after Cr addition. FIG. 8B illustrates a TEM image for Cr-RuCh, according to some embodiments. Transmission electron microscopy (TEM) revealed uniformly dispersed nanocrystals with an average particle size of approximately 30 nm. FIG. 8C illustrates a High-resolution TEM (HRTEM) image for Cr-RuCh, according to some embodiments. High-resolution TEM (HRTEM) images showed well-defined lattice fringes corresponding to the (110) and (111) planes of rutile RuCh, with interplanar spacings of ~3.2 A and ~2.6 A, respectively.

[0137] FIG. 8D illustrates a corresponding FFT pattern for FIG. 8C, according to some embodiments. The fast Fourier transform (FFT) pattern confirmed the high crystallinity of the sample and could be indexed to the (110), (111), and (201) planes along the

[0112] zone axis.2025-061-02 FIG. 8E illustrates HAADF-STEM with EDS elemental mapping results for Cr-RuCh, according to some embodiments. Analysis using low-magnification high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM), combined with energy-dispersive X-ray spectroscopy (EDS) mapping, revealed a uniform spatial distribution of Ru, O, and Cr. The absence of Cr-rich clusters supports the successful atomic-level dispersion of chromium within the RuCh matrix.

[0138] FIG. 8F illustrates Cr 2p XPS spectra of RuCh and Cr-RuCh, according to some embodiments. FIG. 8G illustrates Ru 3d XPS spectra of RuCh and Cr-RuCh, according to some embodiments. X-ray photoelectron spectroscopy (XPS) was employed to investigate the electronic interactions between chromium modifiers and the RuCh host lattice. In the Cr 2p region (FIG.8F), the Cr-RuCh sample exhibited two prominent peaks at approximately 576.4 eV (2pv2) and 586.0 eV (2pi / 2), along with satellite features characteristic of Cr3+species. These signals were absent in pristine RuCh, confirming the successful incorporation of Cr into the lattice. In the Ru 3d region (FIG. 8G), both samples displayed peaks corresponding to Ru4+at -280.7 eV (3ds / 2) and -285.4 eV (3ds / 2). However, a slight positive shift (-0.1 eV) was observed for Cr-RuCh, indicating a change in the electronic environment of Ru. This shift is attributed to electron withdrawal by the Cr modifiers, suggesting a charge redistribution effect that may facilitate enhanced catalytic activity.

[0139] FIG. 8H illustrates CER overpotentials of metal-modified RuCh at various current densities, according to some embodiments. To investigate the impact of heteroatom addition on chlorine evolution reaction (CER) activity, a series of modified RuCh samples were prepared using a range of elements, including 3d transition metals (V, Cr, Mn, Fe, Co, Ni, Cu, Zn), 4d metals (Zr, Nb, Mo), 5d metals (Ta, W), and rare-earth lanthanides (La, Ce). The catalytic performance was evaluated in 1 M NaCl (pH 1) via linear sweep voltammetry using a three-electrode configuration with a rotating disk glassy carbon electrode. Overpotentials at current densities of 10, 20, and 40 mA- cm'2were measured for direct comparison. For example, among all variants, the Cr-modified RuO2(Cr-RuO2) consistently exhibited the lowest overpotentials, highlighting its enhanced activity toward CER.

[0140] FIG. 9 illustrates a linear sweep voltammetry curve on a glassy carbon rotating disk electrode for chlorine evolution reaction of RuCh and Cr-RuCh, according to some embodiments.2025-061-02 The resulting Cr-RuCh powder was tested on GCRDE in 1 M NaCl with 0.1 M HCIO4 (pH 1) electrolyte using a standard three-electrode setup. Compared to untreated RuCh, the Cr-treated sample exhibited lower overpotential for CER.

[0141] FIG. 10 illustrates a linear sweep voltammetry curve for chlorine evolution reaction before and after 10,000 cycles of cyclic voltammetry tests of RuCh and Cr-RuCh, according to some embodiments. FIG. 11 illustrates a chronopotentiometric curve at 10 mA cm2for chlorine evolution reaction of Cr-RuCE on carbon paper, according to some embodiments. Compared to untreated RuCh, the Cr-treated sample exhibited improved current stability during extended operation.

[0142] FIG. 12 illustrates a chlorine evolution selectivity plot for RuCE and Cr-RuCE, according to some embodiments. Compared to untreated RuCh, the Cr-treated sample exhibited enhanced CER selectivity. The combination of reduced overpotential, long-term chronoamperometric stability, and enhanced chlorine evolution selectivity demonstrates the efficacy of Cr modification on RuCh. XRD analysis confirmed the retention of the rutile phase structure after CrCh treatment and thermal stabilization.Example 3: Cr-RuCh / Ti electrode via drop-casting and argon annealing

[0143] A titanium mesh (2 x 10 cm2) was first cleaned by sequential ultrasonication in acetone, ethanol, and deionized water, followed by air drying. 7.6 mL of 10 mM RuCh aqueous solution was drop-cast onto the Ti mesh and dried at room temperature. The coated substrate was then annealed in air at 500 °C for 5 hours, yielding a RuCh / Ti electrode with strong adhesion and uniform coverage. The prepared RuCE / Ti electrode was further treated by drop-casting 2.2 mL of 2.6 mM CrCh aqueous solution onto the surface, followed by air drying at room temperature. The sample was then annealed at 450 °C for 1 hour in flowing argon atmosphere to promote Cr incorporation into the RuCh matrix.

[0144] FIG. 13A illustrates an X-ray diffraction pattern of an as-prepared Cr-RuCE / Ti electrode, according to some embodiments. The Cr-RuCh / Ti electrode retained the rutile structure of RuCh after Cr addition. FIG. 13B illustrates an SEM image for a Cr-RuCh / Ti electrode according to some embodiments. FIG. 13C illustrates an SEM image for a Cr-RuCh / Ti electrode according to some embodiments. FIG. 13D illustrates an SEM image for a Cr-RuCh / Ti electrode according to some embodiments. Scanning electron microscopy revealed the well-2025-061-02 defined mesh structure of the Ti substrate, with a uniform granular RuCh (~50 nm) coating observed at higher magnification. FIG. 13E illustrates SEM-EDX mapping results for a Cr-RuCh / Ti electrode according to some embodiments. Cross-sectional SEM and corresponding EDS mapping confirmed the uniform distribution of Ru, O, and Cr across the electrode surface, indicating successful Cr incorporation.

[0145] FIG. 14A illustrates a linear sweep voltammetry curve of RuCE / Ti and Cr-RuCE / Ti electrodes for chlorine evolution reaction, according to some embodiments. The Cr-RuCh / Ti electrode was evaluated in 5 M NaCl with 0.01 M HC1CE (pH~2) using a standard three-electrode setup. Linear sweep voltammetry (LSV) measurements showed a lower overpotential for chlorine evolution reaction (CER) compared to unmodified RuCh / Ti electrodes. FIG. 14B illustrates an electrochemical impedance spectroscopy curve of RuCE / Ti and Cr-RuCE / Ti electrodes for chlorine evolution reaction, according to some embodiments. Electrochemical impedance spectroscopy (EIS) indicated reduced charge transfer resistance, suggesting improved interfacial conductivity.

[0146] FIG. 15 illustrates chronopotentiometric stability test and corresponding CL selectivity over multiple 12 h cycles, where arrows indicate electrolyte replacement to maintain CER-dominant conditions, according to some embodiments. The long-term chlorine evolution performance of the Cr-RuCh / Ti electrode was evaluated at a high current density of 0.5 A- cm'2in 5 M NaCl (pH 2). A series of chronopotentiometric tests were performed over 60 hours, with electrolyte replacement every 12 hours to minimize pH drift and suppress side reactions such as oxygen evolution. During each cycle, the Cr-RuCh / Ti electrode maintained a Ch Faradaic selectivity of up to 99.9%, with negligible performance decay over time. These results demonstrate the excellent operational stability and selectivity of the Cr-RuCh / Ti electrode system for sustained CER operation.

[0147] FIG. 16A illustrates LSV curves for a comparison of Cr-RuCh / Ti electrode before and after long-term operation, according to some embodiments. As shown in the LSV curves, the Cr-RuCh / Ti electrode retained its catalytic performance, with no observable degradation in current response, indicating excellent operational durability. FIG. 16B illustrates SEM-EDX survey spectra for a comparison of the Cr-RuCh / Ti electrode before and after long-term operation, according to some embodiments. SEM-EDX spectra showed consistent elemental2025-061-02 signals for Ru, 0, Ti, and Cr in both fresh and used samples, suggesting minimal leaching or surface composition change. These results confirm that the Cr-RuCh / Ti electrode maintains both structural integrity and electronic stability after extended high-rate operation, reinforcing its suitability for industrial chlorine evolution.Example 4: Tantalum impregnation of commercial RuCh powder

[0148] Commercial ruthenium dioxide (RuCh, 99.9%, Sigma- Aldrich) was used as the base material. The RuCh powder was impregnated with 1 mM tantalum(V) chloride (TaCh) solution in ethanol, using a 20:1 mass ratio of RuCh to TaCh. The mixture was dried at 75 °C for 18 hours to evaporate the solvent and allow for surface deposition of Ta species. No further thermal treatment was performed in this example, although such treatment may optionally be applied as described in other embodiments.Example 5: Vanadium-modified RuCh via VCh impregnation and thermal stabilization

[0149] Commercial ruthenium dioxide (RuCh, 99.9%, Sigma- Aldrich) was used as the base material. The RuCh powder was impregnated with 1.5 mM vanadium(III) chloride (VCh) solution in ethanol, using a 25:2 mass ratio of RuCh to vanadium precursor. The mixture was stirred thoroughly and dried at 80 °C for 6 hours to evaporate the solvent and deposit vanadium species on the RuCh surface. After drying, the sample was subjected to thermal stabilization at 450 °C for 1.5 hours under flowing nitrogen atmosphere.

[0150] While the invention has been described with reference to an exemplary embodiment(s), it will be understood by those skilled in the art that various changes may be made and equivalents may be substituted for elements thereof without departing from the scope of the invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the invention without departing from the essential scope thereof. Therefore, it is intended that the invention not be limited to the particular embodiment s) disclosed, but that the invention will include all embodiments falling within the scope of the appended claims.Discussion of Possible EmbodimentsClause 1. An electrode, including: an electrocatalyst including: a plurality of ruthenium dioxidecontaining particles, each of the plurality of ruthenium dioxide-containing particles having an exterior surface; and a surface stabilizer predominantly disposed on and coupled to the exterior2025-061-02 surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of transition-metal atoms including at least one transition metal selected from one of Manganese, Chromium, Tantalum, and Vanadium.Clause 2. The electrode of clause 1, wherein a molar atomic ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:15 to 1:70.Clause 3. The electrode of any one of clauses 1-2, wherein the at least one transition metal includes Manganese.Clause 4. The electrode of clause 3, wherein a mass ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:40 to 1:160.Clause 5. The electrode of any one of clauses 1-2, wherein the at least one transition metal includes Chromium.Clause 6. The electrode of clause 5, wherein a mass ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:40 to 1:60.Clause 7. The electrode of any one of clauses 1-2, wherein the at least one transition metal includes Tantalum.Clause 8. The electrode of any one of clauses 1-2, wherein the at least one transition metal includes Vanadium.Clause 9. The electrode of any one of clauses 1-8, wherein the plurality of transition-metal atoms are not a bulk substitutional dopant in a lattice of the plurality of ruthenium dioxide-containing particles.Clause 10. The electrode of any one of clauses 1-9, wherein the plurality of ruthenium dioxide-containing particles exhibit an average particle size ranging from 20 nm to 50 nm.Clause 11. A method for forming an electrocatalyst, including: impregnating a plurality of ruthenium dioxide-containing particles with a solution to form a mixture, wherein the solution includes a transition-metal precursor and a liquid, wherein the transition-metal precursor includes at least one transition metal selected from manganese, chromium, tantalum, and vanadium, and wherein a weight ratio of the plurality of ruthenium dioxide-containing particles to the transitionmetal precursor in the mixture ranges from 10: 1 to 25: 1 ; drying the mixture to form a dried mixture including a catalyst; and optionally thermally treating the dried mixture.2025-061-02 Clause 12. The method of clause 11, wherein a weight ratio of the plurality of ruthenium dioxide-containing particles to the transition-metal precursor in the mixture ranges from 12: 1 to 20:1.Clause 13. The method of any one of clauses 11-12, wherein the transition-metal precursor is in a form of a salt selected from at least one of a nitrate salt, a chloride salt, and an acetate salt.Clause 14. The method of any one of clauses 11-13, wherein drying the mixture is performed at a temperature of about 60 °C to about 120 °C.Clause 15. The method of any one of clauses 11-14, including thermally treating the dried mixture, wherein thermally treating the dried mixture includes annealing at a temperature of about 300 °C to about 600 °C.Clause 16. The method of any one of clauses 11-15, wherein the transition-metal precursor includes a vanadium precursor, and wherein the plurality of ruthenium dioxide-containing particles exhibit an average particle size ranging from 20 nm to 50 nm.Clause 17. The method of any one of clauses 11-16, wherein the catalyst includes a surface stabilizer predominantly disposed on and directly coupled to an exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of isolated transition-metal atoms.Clause 18. An electrochemical apparatus for a gas evolution reaction, including: a cathode; an anode including an electrocatalyst, wherein the electrocatalyst includes: a plurality of ruthenium dioxide-containing particles, each of the plurality of ruthenium dioxide-containing particles having an exterior surface, and a surface stabilizer predominantly disposed on and coupled to the exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of transition-metal atoms including at least one transition metal selected from one of Manganese, Chromium, Tantalum, and Vanadium; and an electrical energy source electrically coupled to the cathode and the anode.Clause 19. The electrochemical apparatus of clause 18, further including a water-containing electrolyte, wherein the anode is configured for oxygen evolution reaction, and wherein a molar atomic ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:15 to 1:70.2025-061-02 Clause 20. The electrochemical apparatus of clause 18, further including a chloride-containing electrolyte, wherein the anode is configured for chlorine evolution reaction, wherein a molar atomic ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:15 to 1:70, and wherein the plurality of transition-metal atoms include Chromium.

Claims

2025-061-02 CLAIMS:

1. An electrode, comprising:an electrocatalyst including:a plurality of ruthenium dioxide-containing particles, each of the plurality of ruthenium dioxide-containing particles having an exterior surface; and a surface stabilizer predominantly disposed on and coupled to the exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of transition-metal atoms including at least one transition metal selected from one of Manganese, Chromium, Tantalum, and Vanadium.

2. The electrode of claim 1, wherein a molar atomic ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:15 to 1:70.

3. The electrode of claim 1, wherein the at least one transition metal includes Manganese.

4. The electrode of claim 3, wherein a mass ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:40 to 1:160.

5. The electrode of claim 1, wherein the at least one transition metal includes Chromium.

6. The electrode of claim 5, wherein a mass ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:40 to 1:60.

7. The electrode of claim 1, wherein the at least one transition metal includes Tantalum.

8. The electrode of claim 1, wherein the at least one transition metal includes Vanadium.2025-061-02 9. The electrode of any one of claims 1-8, wherein the plurality of transition-metal atoms are not a bulk substitutional dopant in a lattice of the plurality of ruthenium dioxide- containing particles.

10. The electrode of any one of claims 1-8, wherein the plurality of ruthenium dioxidecontaining particles exhibit an average particle size ranging from 20 nm to 50 nm.

11. A method for forming an electrocatalyst, comprising:impregnating a plurality of ruthenium dioxide-containing particles with a solution to form a mixture, wherein the solution includes a transition-metal precursor and a liquid, wherein the transition-metal precursor includes at least one transition metal selected from manganese, chromium, tantalum, and vanadium, and wherein a weight ratio of the plurality of ruthenium dioxide-containing particles to the transit! on- metal precursor in the mixture ranges from 10: 1 to 25: 1 ;drying the mixture to form a dried mixture including a catalyst; andoptionally thermally treating the dried mixture.

12. The method of claim 11, wherein a weight ratio of the plurality of ruthenium dioxide-containing particles to the transit! on- metal precursor in the mixture ranges from 12: 1 to 20: 1.

13. The method of claim 11, wherein the transition-metal precursor is in a form of a salt selected from at least one of a nitrate salt, a chloride salt, and an acetate salt.

14. The method of any one of claims 11-13, wherein drying the mixture is performed at a temperature of about 60 °C to about 120 °C.

15. The method of any one of claims 11-13, including thermally treating the dried mixture, wherein thermally treating the dried mixture includes annealing at a temperature of about 300 °C to about 600 °C.2025-061-02 16. The method of any one of claims 11-13, wherein the transition-metal precursor includes a vanadium precursor, and wherein the plurality of ruthenium dioxide-containing particles exhibit an average particle size ranging from 20 nm to 50 nm.

17. The method of any one of claims 11-13, wherein the catalyst includes a surface stabilizer predominantly disposed on and directly coupled to an exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of isolated transition-metal atoms.

18. An electrochemical apparatus for a gas evolution reaction, comprising:a cathode;an anode including an electrocatalyst, wherein the electrocatalyst includes:a plurality of ruthenium dioxide-containing particles, each of the plurality of ruthenium dioxide-containing particles having an exterior surface, and a surface stabilizer predominantly disposed on and coupled to the exterior surface of the plurality of ruthenium dioxide-containing particles, wherein the surface stabilizer includes a plurality of transition-metal atoms including at least one transition metal selected from one of Manganese, Chromium, Tantalum, and Vanadium; andan electrical energy source electrically coupled to the cathode and the anode.

19. The electrochemical apparatus of claim 18, further including a water-containing electrolyte, wherein the anode is configured for oxygen evolution reaction, and wherein a molar atomic ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:15 to 1:70.

20. The electrochemical apparatus of claim 18, further including a chloride-containing electrolyte, wherein the anode is configured for chlorine evolution reaction, wherein a molar atomic ratio of transition metal atoms to the plurality of ruthenium dioxide-containing particles ranges from 1:15 to 1:70, and wherein the plurality of transition-metal atoms include Chromium.