Downhole tool annular member, plug, and well drilling method
The use of a glycolic acid polymer with low crystallinity in the annular member of downhole tools ensures sufficient expansion to match well casing diameters, addressing leakage issues and enhancing sealing reliability in hydraulic fracturing operations.
Patent Information
- Application Number
- PCT/JP2026/015369
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-16
- Publication Date
- 2026-11-12
AI Technical Summary
Existing downhole tools with biodegradable socket outers made of polyglycolic acid (PGA) fail to expand sufficiently to match the inner diameter of the well casing, leading to sealing member leakage during hydraulic fracturing.
An annular member for a downhole tool formed from a glycolic acid polymer with a crystallinity of 41.0% or less, which allows for superior expandability and prevents leakage by expanding to match the well casing diameter, ensuring reliable sealing.
The annular member effectively suppresses sealing member leakage, enabling more reliable well bore sealing and efficient hydraulic fracturing operations.
Smart Images

Figure JP2026015369_12112026_PF_FP_ABST
Abstract
Description
Annular member for downhole tool, plug, and well drilling method
[0001] The present invention relates to an annular member for a downhole tool, a plug, and a well drilling method, and more particularly to a socket placed on a downhole tool, a plug equipped therewith, and a well drilling method using the plug.
[0002] To efficiently extract and recover hydrocarbon resources such as petroleum (shale oil) or natural gas (shale gas), it is known that the production layers that produce these hydrocarbon resources are stimulated by hydraulic fracturing (HFR). Hydraulic fracturing is a method that uses fluid pressure, such as water pressure, to create constrictions and cracks (fractures) in the production layer, and efficiently extracts and recovers hydrocarbon resources through these fractures. Between the surface and the production layer, a hole called a downhole is made to form a well. When applying hydraulic fracturing, a downhole tool is installed inside the downhole to block the well during hydraulic fracturing.
[0003] A flak plug, a type of downhole tool, is composed of at least one mandrel and various components attached to the outer circumferential surface of the mandrel. Patent Document 1 discloses a flak plug comprising a mandrel, a sealing member, a retaining member (socket), a cone, a slip, and a ring-shaped fixing member, wherein each component is formed of a biodegradable resin or biodegradable metal, and polyglycolic acid (PGA) is described as an example of the biodegradable resin. The document also describes a socket configuration comprising an annular socket inner having an inner circumferential edge in contact with the outer circumferential surface of the mandrel, and an annular socket outer having a larger inner diameter than the socket inner and being movably attached to the socket inner. Furthermore, in this configuration of a socket, it is described that the sealing member deforms under pressure, and when the sealing member is pressed against the socket, the socket outer deforms so that its diameter expands, and it is preferable that the socket outer be made of a material that can deform to expand when pressure is applied from the sealing member, for example, made of PGA.
[0004] International release WO2019 / 031214A1
[0005] However, although the socket outer formed of PGA described in Patent Document 1 deforms to expand in diameter when subjected to pressure from the sealing member, the expansion is insufficient, and the socket outer may not expand to the inner diameter of the casing installed in the well bore. If the socket outer does not expand to the inner diameter of the casing, the sealing member will leak out from the gap between the casing and the socket outer, resulting in insufficient sealing of the well.
[0006] The present invention has been made in view of the above problems, and its purpose is to provide an annular member for a downhole tool that can more reliably suppress leakage of the sealing member.
[0007] An annular member for a downhole tool according to one aspect of the present invention is an annular member for a downhole tool used adjacent to a sealing member of a downhole tool, formed using a glycolic acid polymer, and having a cross-sectional area of one side of the cross-section defined by a plane containing the central axis of the annular member for the downhole tool of 20 to 400 mm². 2 The glycolic acid polymer has a crystallinity of 41.0% or less.
[0008] According to one aspect of the present invention, an annular member for a downhole tool makes it possible to more reliably suppress leakage of the sealing member.
[0009] This is a perspective cross-sectional view of a socket outer according to one embodiment of the present invention. This is a partial cross-sectional view illustrating the structure of a socket outer according to one embodiment of the present invention. This is a perspective cross-sectional view of a socket outer according to one embodiment of the present invention. This is a partial cross-sectional view illustrating the structure of a socket outer according to one embodiment of the present invention. This is a diagram schematically showing a portion of the axial cross-section of a plug according to one embodiment of the present invention. This is a diagram showing a cross-sectional view of the test system for a compression test. This is a diagram showing the measurement results of the lead time in the embodiment.
[0010] A socket outer and a plug equipped therewith, which are embodiments of the annular member for a downhole tool according to the present invention, will be described below with reference to Figures 1 to 5.
[0011] In this specification, "A to B" means A or greater and B or less, unless otherwise specified.
[0012] Figures 1 and 3 are perspective cross-sectional views of the socket outer of this embodiment. Figure 5 is a schematic diagram showing a portion of the axial cross-section of the plug of this embodiment.
[0013] [Downhole Tool] A downhole tool, as described above, is a tool used to block a well bore during hydraulic fracturing. A plug 10, a type of downhole tool, is a well drilling tool used to block a well bore. Examples of plugs in this embodiment include a flak plug and a bridge plug, but it is not limited to these. The plug 10 comprises a mandrel 1, a sealing member 2, a socket 3, cones 4 and 5, a pair of slips 6a and 6b, and a pair of ring-shaped fixing members 7a and 7b. The socket 3 is composed of a socket outer 32 and a socket inner 31.
[0014] The mandrel 1 is a component for ensuring the strength of the plug 10, and has a hollow shape.
[0015] The sealing member 2 is an annular rubber member mounted on the axial outer surface of the mandrel 1 between the socket 3 and the cone 5. The sealing member 2 deforms when the plug 10 is subjected to pressure. The sealing member 2 is made of a material that does not lose its function of sealing the well bore even in environments such as high temperature and high pressure.
[0016] The socket 3 is an annular member and is mounted adjacent to the seal member 2 on the axial outer surface of the mandrel 1, downstream of the pressure the seal member 2 receives. In this embodiment, the socket 3 is composed of two members: a socket outer 32 and a socket inner 31.
[0017] The cones 4 and 5 are formed such that when a load or pressure is applied to the pair of slips 6a and 6b toward the sealing member 2, the slips 6a and 6b slide along the inclined surfaces of the respective cones 4 and 5.
[0018] The fixing members 7a and 7b are annular members that fix the positions of the slips 6a and 6b relative to the axial direction of the mandrel 1. The fixing members 7a and 7b are arranged adjacent to the slips 6a and 6b on the outer circumferential surface of the mandrel 1.
[0019] In this embodiment, the materials used to form the mandrel 1, cones 4 and 5, a pair of slips 6a and 6b, and a pair of fixing members 7a and 7b include, for example, metal materials such as aluminum, steel, or stainless steel, fibers, wood, composite materials, and resins. The mandrel 1 may be formed from a composite material containing a reinforcing agent such as carbon fiber, specifically, a composite material containing polymers such as epoxy resin and phenolic resin. Furthermore, it is preferable that the mandrel 1, socket 3, cones 4 and 5, a pair of slips 6a and 6b, and a pair of fixing members 7a and 7b are each formed from biodegradable resins or biodegradable metals.
[0020] This makes it easier to remove the plug 10 after the well treatment has been performed using the plug 10.
[0021] In this specification, "degradable resin or degradable metal" means a resin or metal that can be easily broken down by biodegradation or hydrolysis, dissolution in water or hydrocarbons in a well, or by any chemical method.
[0022] In the plug 10, when a load is applied to the slip 6b toward the seal member 2, the slip 6b slides along the slope of the cone 5, causing the seal member 2 to deform. The well bore is then closed by the seal member 2.
[0023] In the plug 10, when the seal member 2 deforms under axial pressure inside the well, the socket 3, which is attached downstream of the pressure acting on the seal member 2, receives the deformation of the seal member 2.
[0024] [Annular Member for Downhole Tool] The socket outer 32, which is an annular member for a downhole tool, is a component that forms the socket 3 together with the socket inner 31. The socket 3 is mounted on the axial outer surface of the mandrel 1, downstream of the pressure received by the seal member 2, and adjacent to the seal member 2. The socket outer 32 has a larger inner diameter than the socket inner 31 and is movably attached to the socket inner 31.
[0025] When the sealing member 2 is subjected to pressure inside the well bore, it deforms, and when the sealing member 2 is pressed against the socket 3, the socket outer 32 deforms so that its diameter expands.
[0026] In this embodiment, the socket outer 32 is formed from a glycolic acid polymer having a crystallinity of 41.0% or less. Because it is formed from a glycolic acid polymer with a crystallinity within the above range, the socket outer 32 has excellent stretchability. Therefore, when the sealing member 2 is subjected to pressure and deforms, and the socket outer 32 expands in diameter as a result, the degree of expansion is superior to that of conventional socket outers. As a result, when the socket outer 32 expands in diameter due to the deformation of the sealing member 2 in the well bore, the socket outer 32 can expand until its outer diameter matches the inner diameter of the casing in the well bore. Furthermore, with conventional socket outers, they sometimes break before expanding sufficiently, and the desired function as a socket outer cannot be obtained. By forming the socket outer 32 from a glycolic acid polymer with a crystallinity of 41.0% or less, it is possible to prevent the socket outer 32 from becoming hard and brittle, thereby preventing the socket outer 32 from breaking before expanding to match the inner diameter of the casing. By expanding the socket outer 32 until it matches the inner diameter of the casing, the sealing member 2 is prevented from leaking from the outer circumference of the socket 3 to the downstream side of the socket 3, thereby ensuring more reliable sealing of the well borehole.
[0027] From this perspective, the crystallinity of the glycolic acid polymer should be 41.0% or less, preferably 40.5% or less, and more preferably 40.0% or less. There is no particular lower limit to the crystallinity, but for example, 25.0% or more is preferred, and 30.0% or more is more preferred.
[0028] The degree of crystallinity Xc of a glycolic acid polymer can be calculated from the density of the glycolic acid polymer using the following formula (1). In formula (1), the crystallinity of the glycolic acid polymer is ρ. c is 1,700 [g / cm³] 3 ] and the amorphous density ρ of the glycolic acid polymer a It is 1.509 [g / cm³] 3 ]
[0029] Density of glycolic acid polymer ρ [g / cm³] 3 The density is measured using the density gradient tube method. The sample for measurement is cut from the socket outer, with the cutting position being a maximum of 2 mm from the inner diameter to the outer diameter of the annular member, with an axial length of 0.5 to 1 mm and a circumferential length of 0.5 to 1 mm. Next, carbon tetrachloride, 1,2-dichloroethane, and 1,2-dibromoethane are used and mixed to prepare standard solutions with different densities (densities of standard solutions: 1.64, 1.62, 1.60, 1.58, 1.56, 1.54). The prepared standard solutions are poured into a graduated cylinder in order from the densest to the most dense to create a layer of standard solutions. The graduated cylinder containing the layered standard solutions is placed in a 23°C water bath and left to stand for one day. Then, the density sphere and sample are placed in the graduated cylinder and left to stand for one day. The measurement position of the density sphere is read on the graduated cylinder scale to create a calibration curve. After that, the measurement position of the sample is read on the graduated cylinder scale and the density is calculated from the calibration curve. Density measurements were performed with n=2, and the average of each measurement value was defined as the density ρ.
[0030] The crystallinity of the glycolic acid polymer can be adjusted, for example, by subjecting a molded article (socket outer) made of the glycolic acid polymer to heat treatment. The heat treatment is carried out for any arbitrary period of time at a temperature equal to or higher than the glass transition temperature of the glycolic acid polymer. Generally, the higher the heat treatment temperature and the longer the heat treatment time, the higher the crystallinity that can be achieved. Preferred heat treatment conditions for the socket outer in the present embodiment are a heat treatment temperature of 80°C or higher and a heat treatment time of 0.1 hours to 24.0 hours.
[0031] The glycolic acid polymer may be a homopolymer of glycolic acid, or a copolymer of glycolic acid and other monomer components. Examples of other monomer components used in the copolymer include hydroxycarboxylic acids such as L-lactic acid, D-lactic acid, 3-hydroxybutanoic acid and 1-hydroxyhexanoic acid, ester compounds composed of a diol and a dicarboxylic acid such as the condensate of 1,4-butanediol and succinic acid and the condensate of 1,4-butanediol and adipic acid, cyclic esters and lactones formed by intramolecular condensation of the aforementioned other monomer components, and cyclic carbonates such as trimethylene carbonate.
[0032] Since the socket outer 32 is formed of a glycolic acid polymer which is a degradable resin, it can degrade in a well environment. When all members constituting the plug 10 are formed of a degradable resin or a degradable metal, the plug 10 including the socket outer 32 can be easily removed after well treatment is performed using the plug 10.
[0033] The glycolic acid polymer forming the socket outer 32 may contain additives, as long as the properties thereof are not significantly impaired. Examples of the additives include various additives such as fillers, plasticizers, degradation accelerators, heat stabilizers, light stabilizers, moisture-proof agents, waterproofing agents, water repellents, lubricants, hydrophilic agents, water-absorbing agents, nucleating agents, release agents, coupling agents, pigments and dyes, as well as other thermoplastic resins and the like.
[0034] Further, in the socket outer 32 according to the present embodiment, the cross-sectional area of one side (denoted by reference numeral 32a in FIG. 1) of the cross section defined by the plane including the central axis of the socket outer 32 is 20 to 400 mm 2is. When the cross-sectional area falls within this range, the socket outer 32 is easily deformable, and sufficient diameter expansion can be achieved when the socket outer 32 receives pressure from the seal member 2. On the other hand, if the cross-sectional area of the socket outer is too small or too large, even when the crystallinity of the glycolic acid polymer is 41.0% or less, the diameter expansion of the socket outer may be insufficient, or the socket outer may fracture before sufficient diameter expansion is achieved.
[0035] Note that the central axis of the socket outer 32 in the present specification refers to a conceptual axis that is perpendicular to the radial direction of the socket outer 32 and passes through the center of the ring. In addition, the plane including the central axis in the present specification refers to any plane that is parallel to the central axis and includes the central axis. Since the socket outer 32 has an annular structure, two cross sections defined by the plane including the central axis are formed. Unless otherwise specified, reference to the cross-sectional area of the cross section means the area of one of the two cross sections. When the cross-sectional areas of the two cross sections are different, it means the smaller cross-sectional area of the two cross sections. Hereinafter, this cross section is simply referred to as the axial cross section.
[0036] In the present embodiment, the cross-sectional area of the axial cross section of the socket outer 32 is 20 to 400 mm 2 , and is appropriately set within this range according to the well environment for use (for example, the size of the casing and the like). For example, the cross-sectional area of the socket outer 32 may be 25 to 400 mm 2 , and may further be 30 to 400 mm 2 . The cross-sectional area of the axial cross section of the socket outer 32 can be measured by software such as 3D CAD. Alternatively, it can be measured by performing image analysis from a cross-sectional photograph of the socket outer 32.
[0037] In this embodiment, the shape of the socket outer 32 in the axial cross-section is a triangle with one vertex rounded, but the shape of the socket outer 32 in the cross-section is not limited to this as long as the above-mentioned cross-sectional area condition is met. Examples of the shape of the socket outer 32 in the cross-section include a triangle, a trapezoid or other quadrilateral, a wedge shape, etc. In the case of triangles and quadrilaterals, some or all of the corners may be rounded. Among these, a triangular or quadrilateral shape is preferred for the cross-section, and a triangle or quadrilateral with edge surface treatment including a chamfer or radius chamfer on at least one corner is more preferred. The dimension of the chamfer is preferably, for example, 0.1 mm or more and 1.0 mm or less. The chamfer angle is usually 45 degrees (°), but other angles may be used as needed. The radius of the radius chamfer is preferably, for example, 0.5 mm or more and 4.0 mm or less. From the viewpoint of preventing chipping of the socket outer and suppressing leakage of the sealing member from the gap between the casing and the socket outer, it is particularly preferable that the socket outer 32 be a triangle or square with a chamfered edge of 0.1 mm to 0.5 mm.
[0038] In one embodiment, the socket outer 32 has a triangular shape in its axial cross-section 32a (Figure 1). When the socket outer 32 has a triangular shape in its axial cross-section 32a, the socket outer 32 has a curved surface region C1 facing the inner wall surface of the casing, a curved surface region C2 facing the socket inner 31, and a curved surface region C3 facing the sealing member 2. It also has a common outer peripheral edge C1a defining the curved surface region C1 and the curved surface region C2, a common outer peripheral edge C1b defining the curved surface region C1 and the curved surface region C3, and a common inner peripheral edge C1c defining the curved surface region C2 and the curved surface region C3. The curved region C2 has a first tapered shape 32b that slopes in a direction such that the axial thickness of the socket outer 32 decreases from the outer peripheral edge C1a to the inner peripheral edge C1c, and the curved region C3 has a second tapered shape 32c that slopes in a direction such that the axial thickness of the socket outer 32 decreases from the outer peripheral edge C1b to the inner peripheral edge C1c. That is, the inclined surface of the first tapered shape 32b contacts the socket inner 31, and the inclined surface of the second tapered shape 32c contacts the sealing member 2.
[0039] Specifically, as shown in Figure 2, when a perpendicular line La is drawn from the outer peripheral edge C1a to the central axis of the socket outer 32, the angle θa between the curved surface region C2 and the perpendicular line La is 10 degrees (°) or more and less than 90 degrees. Also, when a perpendicular line Lb is drawn from the outer peripheral edge C1b to the central axis of the socket outer 32, the angle θb between the curved surface region C3 and the perpendicular line Lb is 10 degrees or more and less than 90 degrees. Because the socket outer 32 has the angles θa and θb, it can easily expand in diameter and reliably suppress leakage of the sealing member 2. From a similar viewpoint, the angle θa is preferably 11 degrees or more and 45 degrees or less, and more preferably 12 degrees or more and 35 degrees or less. The angle θb is preferably 20 degrees or more and 80 degrees or less, and more preferably 30 degrees or more and 75 degrees or less.
[0040] In one embodiment, the socket outer 32 has a rectangular shape in its axial cross-section 32a (Figure 3). When the shape of the socket outer 32 in its axial cross-section 32a is rectangular, the socket outer 32 has a curved surface region C1 facing the inner wall surface of the casing, a curved surface region C2 facing the socket inner 31, a curved surface region C3 facing the sealing member 2, and a curved surface region C4 located between the curved surface region C1 and the curved surface region C3. It also has a common outer peripheral edge C1a defining the curved surface region C1 and the curved surface region C2, a common outer peripheral edge C1b defining the curved surface region C1 and the curved surface region C4, a common inner peripheral edge C1c defining the curved surface region C2 and the curved surface region C3, and a common inner peripheral edge C1d defining the curved surface region C3 and the curved surface region C4. The curved region C2 has a first tapered shape 32b that slopes in a direction such that the axial thickness of the socket outer 32 decreases from the outer peripheral edge C1a to the inner peripheral edge C1c, and the curved region C3 has a second tapered shape 32c that slopes in a direction such that the axial thickness of the socket outer 32 decreases from the inner peripheral edge C1d to the inner peripheral edge C1c. That is, the inclined surface of the first tapered shape 32b contacts the socket inner 31, and the inclined surface of the second tapered shape 32c contacts the sealing member 2.
[0041] Specifically, as shown in Figure 4, when a perpendicular line La is drawn from the outer peripheral edge C1a to the central axis of the socket outer 32, the angle θa between the curved surface region C2 and the perpendicular line La is 10 degrees (°) or more and less than 90 degrees. Also, when a perpendicular line Lb is drawn from the inner peripheral edge C1d to the central axis of the socket outer 32, the angle θb between the curved surface region C3 and the perpendicular line Lb is 10 degrees or more and less than 90 degrees. Because the socket outer 32 has the angles θa and θb, it can easily expand in diameter and reliably suppress leakage of the sealing member 2. From a similar viewpoint, the angle θa is preferably 11 degrees or more and 45 degrees or less, and more preferably 12 degrees or more and 35 degrees or less. The angle θb is preferably 20 degrees or more and 80 degrees or less, and more preferably 30 degrees or more and 75 degrees or less. The curved surface region C4 can take any shape, and may or may not be a flat surface. It may also have a tapered shape.
[0042] In this embodiment, the radial thickness of the socket outer 32 is 5 mm or more and 20 mm or less. In this specification, "radial thickness of the socket outer" means the difference between the distance from the central axis to the outermost part of the outer circumference and the distance from the central axis to the inner circumference in the axial cross-section of the socket outer 32. By having a radial thickness of 5 mm or more of the socket outer 32, it is possible to prevent the socket outer 32 from breaking when the seal member 2 is deformed under pressure, before the outer diameter of the socket outer 32 expands to match the inner diameter of the casing. Furthermore, by having a radial thickness of 20 mm or less of the socket outer 32, it is possible to prevent the seal member 2 from leaking downstream before the socket outer 32 has sufficiently expanded when the seal member 2 is deformed under pressure. The radial thickness of the socket outer 32 is appropriately adjusted according to the size of the plug 10 and the environment of the well in which the plug 10 is used (e.g., the size of the casing). For example, the radial thickness of the socket outer 32 may be 6 mm or more and 19 mm or less. The radial thickness of the socket outer 32 can be measured using a caliper and a micrometer.
[0043] In this embodiment, the axial thickness of the socket outer 32 is 5 mm or more and 40 mm or less. In this specification, "axial thickness of the socket outer" means the maximum width in the axial cross-section of the socket outer 32 in the direction parallel to the axis of the socket outer 32. By having an axial thickness of 5 mm or more of the socket outer 32, it is possible to prevent the socket outer 32 from breaking before the outer diameter of the socket outer 32 expands to match the inner diameter of the casing when the seal member 2 is deformed under pressure. Furthermore, by having an axial thickness of 40 mm or less of the socket outer 32, it is possible to prevent the seal member 2 from leaking downstream before the socket outer 32 expands sufficiently when the seal member 2 is deformed under pressure. The axial thickness of the socket outer 32 is adjusted as appropriate according to the strength and shape of the seal member 2. For example, the axial thickness of the socket outer 32 may be 7 mm or more and 38 mm or less, or 10 mm or more and 35 mm or less. The axial thickness of the socket outer 32 can be measured using calipers and micrometers, etc.
[0044] We examined multiple usage examples of plugs where the socket is divided into a socket outer and a socket inner, and investigated the width W (= (casing inner diameter - socket outer outer diameter) / 2) of the gap between the outer circumference of the socket outer before expansion and the inner wall surface of the casing of the well bore where the plug was used. Then, based on each usage example, we calculated the deformation rate required for the outer circumference of the socket outer to reach the inner wall surface of the casing using the following formula. As a result, the required deformation rate was at least 5.0%. Required deformation rate (%) = (width W × 2 / socket outer outer diameter) × 100
[0045] Therefore, it is preferable that the socket outer 32 has a deformation rate of 5.0% or more when expanded in diameter. In one embodiment, it is preferable that the socket outer 32 has a deformation rate of 5.0% or more when a compression test is performed, as expressed by the following formula (2).
[0046] The compression test can be performed using a test apparatus 100, as shown in Figure 6, in which an annular outer wall 102 (assuming a casing) is positioned outside the test object 101 (socket outer). Specifically, a universal testing machine is used as the test apparatus 100, and a uniform load (maximum 200 kN) is applied from the top of the test object 101 using a jig 103a at 23°C, 50 RH, and a test speed of 10 mm / min to deform the test object 101. In this case, the test object 101 cannot expand further because it reaches the surrounding outer wall 102 when it has expanded by a certain amount. However, by adjusting the inner diameter of the outer wall 102 in advance, it is possible to determine whether the deformation rate expressed by equation (2) is 5.0% or more, or greater than a predetermined value greater than 5.0%. The load detected when the socket outer 32 contacts the outer wall 102 increases sharply, and the load decreases sharply when the socket outer 32 breaks during expansion. By selecting an arbitrary exterior wall 102 and conducting a compression test, it is possible to determine whether the deformation rate exceeds the desired value based on the behavior of the rapid increase and decrease in load during the compression test. The compression test is performed with n=5, and the average value of each measurement is taken as the deformation rate.
[0047] The required deformation rate is set appropriately according to the well environment used (e.g., casing size), but as mentioned above, it is preferably 5.0% or more. When the required deformation rate is 5.0% or more, a sufficient gap width can be secured between the inner wall surface of the well casing and the plug in the plug before deformation, thereby maintaining the transportability of the flack plug. From a similar viewpoint, a deformation rate of 7.0% or more is more preferable, and 10.0% or more is even more preferable. Furthermore, there is no particular upper limit to the deformation rate, but it may be, for example, 20% or less, or 19% or less.
[0048] The socket outer 32 in this embodiment has a lead time (decomposition lead time). In this specification, "lead time" refers to the time from the moment the socket outer is immersed in deionized water until the glycolic acid polymer on the surface of the socket outer is hydrolyzed and the thickness of the socket outer begins to decrease. The socket outer retains its shape immediately before immersion in deionized water until at least the lead time has elapsed after immersion in deionized water. In this embodiment, the lead time of the socket outer 32 when immersed in deionized water at 66°C is 2.0 hours or more. By having a lead time of 2.0 hours or more when immersed in deionized water at 66°C, it is possible to reliably maintain the function of the socket outer 32, and consequently the sealing function of the plug 10 equipped with the socket outer 32, until fracturing occurs, and to start decomposition after a desired period of time has elapsed. This contributes to shortening the process and reducing costs, and improves production efficiency.
[0049] The lead time is measured using the following method. Prepare a sample cut from the socket outer into a cube with sides of 10 mm, and measure the dimensions of the sample with calipers before immersion. Next, place a plastic net (made of polyethylene) over a beaker containing 1000 mL of deionized water so that the sample is positioned in the center, and heat the beaker in a water bath until the temperature inside the beaker reaches 66°C. After reaching 66°C, immerse the sample in the deionized water. At this time, the sample is placed on the plastic net. While maintaining the temperature, remove the immersed sample at predetermined time intervals (for example, 2 hours, 4 hours, 6 hours, 8 hours, 10 hours, etc.) and measure the dimensions of the sample after immersion with calipers. Plot the immersion time on the X axis and the dimensional change at each measurement point on the Y axis to create a linear function approximation line, and define the lead time as the X-axis value when the Y-axis value on the approximation line becomes greater than 0. The dimensional change is measured using the following procedure. Let O be the center of the cubic sample, i.e., a point inside the cube that is equidistant from all vertices. In the sample before immersion, the length in the X-axis direction of the cross section parallel to the X-axis of the cube that passes through point O is X. 1 The length in the Y-axis direction of the cross-section parallel to the Y-axis is Y1 The length in the Z-axis direction of the cross-section parallel to the Z-axis is Z 1 Then, measure these lengths with calipers and take the average of the three points to determine the sample dimension L. 1 Similarly, the length X in each axial direction is also considered for the sample after immersion. 2 , Y 2 Z 2 Measure the dimensions L of the sample 2 Determine the following: The amount of dimensional change is (dimension L before sample immersion). 1 ) - (Dimensions L after sample immersion) 2 The lead time is calculated using the following method. Lead time measurements are performed with n=3, and the average of each measurement value is taken as the lead time.
[0050] The lead time for the decomposition of the socket outer 32 can be adjusted by changing the copolymer components and ratios of the glycolic acid polymer forming the socket outer 32, or by adding a decomposition accelerator. A decomposition accelerator refers to an agent (compound) that promotes the decomposition of the glycolic acid polymer, and examples include carboxylic acid anhydrides such as aliphatic monocarboxylic acid anhydrides, aromatic monocarboxylic acid anhydrides, aliphatic dicarboxylic acid anhydrides, aromatic dicarboxylic acid anhydrides, aromatic tricarboxylic acid anhydrides, alicyclic dicarboxylic acid anhydrides, aliphatic tetracarboxylic acid dianhydrides, and aromatic tetracarboxylic acid dianhydrides.
[0051] [Well Drilling Method] A well drilling method according to one embodiment of the present invention comprises the steps of: transporting a plug 10 into a well; performing hydraulic fracturing using the plug 10; and disassembling part or all of the plug 10 by bringing it into contact with the fluid present in the well. Specifically, the plug 10 is inserted into a casing, and the plug 10 is transported to a desired position in the casing by introducing fluid from the upstream direction of transport (step of transporting the plug 10 into the well). After the plug 10 has been transported to the desired position, a load is applied to the plug 10 toward the seal member 2 side relative to the slip 6b, causing the slip 6b to slide along the slope of the cone 5, and the seal member 2 deforms, thereby closing the well bore. Next, a ball or the like (not shown) is set in the hollow part of the mandrel 1, the mandrel 1 is closed, and hydraulic fracturing is performed by introducing a fracturing fluid at high pressure (step of performing hydraulic fracturing). After hydraulic fracturing, the plug 10 is exposed to fluids present in the well, such as the fluid used for transporting the plug 10 and the fracturing fluid, which causes part or all of the plug 10 to break down from the parts that come into contact with the fluids (a step to break down part or all of the plug).
[0052] According to this embodiment, when closing the well bore using the plug 10, the deformation of the sealing member 2 allows the socket outer 32 located downstream to expand sufficiently, thus preventing the sealing member 2 from leaking out to the downstream side of the socket 3 due to the deformation of the sealing member 2. Therefore, the well bore bore can be sealed more reliably, and well drilling can be performed more efficiently.
[0053] When implementing the well drilling method of this embodiment, the above-described compression test is performed on the corresponding socket outer 32 based on the inner diameter of the casing of the target well bore. By selecting and using a plug 10 equipped with a socket outer 32 whose deformation rate derived by the above-described formula (2) is equal to or greater than the value of the following formula (3), the well bore bore can be sealed more reliably.
[0054] [Summary] Combining the above embodiments, the present invention can be summarized as follows: Embodiment 1: An annular member for a downhole tool, used adjacent to the sealing member of the downhole tool, formed using a glycolic acid polymer, wherein one of the cross-sectional areas of the cross section defined by the plane containing the central axis of the annular member for the downhole tool is 20 to 400 mm² 2 An annular member for a downhole tool, wherein the crystallinity of the glycolic acid polymer is 41.0% or less. Embodiment 2: An annular member for a downhole tool according to Embodiment 1, wherein the deformation rate represented by the above formula (2) when a compression test is performed at a test speed of 10 mm / min is 5.0% or more. Embodiment 3: An annular member for a downhole tool according to Embodiment 1 or 2, wherein the radial thickness of the annular member for the downhole tool is 5 mm or more and 20 mm or less. Embodiment 4: An annular member for a downhole tool according to any of Embodiments 1 to 3, wherein the axial thickness of the annular member for the downhole tool is 5 mm or more and 40 mm or less. Embodiment 5: An annular member for a downhole tool according to any of Embodiments 1 to 4, wherein the lead time when the annular member for the downhole tool is immersed in deionized water at 66°C is 2.0 hours or more. Embodiment 6: An annular member for a downhole tool according to any of Embodiments 1 to 5, having a tapered shape that slopes from the outer circumference to the inner circumference of the ring. Embodiment 7: A plug having the function of closing a well bore provided in a well during drilling, comprising: a hollow mandrel; an annular sealing member attached to the outer surface of the mandrel and deformed under pressure; and an annular member for a downhole tool of any of Embodiments 1 to 6 attached downstream of the pressure received by the sealing member and adjacent to the sealing member. Embodiment 8: A well drilling method comprising the steps of: transporting the plug of Embodiment 7 into a well; performing hydraulic fracturing using the plug; and disassembling part or all of the plug by bringing the plug into contact with a fluid present in the well. Embodiment 9: The well drilling method of Embodiment 8, wherein the plug is used, wherein the deformation rate expressed by the above formula (2) when the annular member for the downhole tool is subjected to a compression test at a test speed of 10 mm / min is greater than or equal to the value of the above formula (3).
[0055] The present invention is not limited to the embodiments described above, and various modifications are possible within the scope of the claims. That is, embodiments obtained by combining technical means that have been appropriately modified within the scope of the claims are also included in the technical scope of the present invention.
[0056] [Test Example 1] Compression tests were conducted on socket outers formed from glycolic acid polymer (PGA), the radial thickness, axial thickness, and axial cross-sectional area of which are shown in Table 1. The degree of crystallinity of the glycolic acid polymer for each socket outer was calculated according to Test Example 2, which will be described later. The compression test was performed using a test apparatus having a jig 103b that follows the inner tapered shape of the socket outer, which is the test subject 101, and a jig 103a that follows the other tapered shape of the socket outer, with its cross-section as shown in Figure 6. Specifically, using a universal testing machine, a uniform load (maximum 200 kN) was applied from the top of each socket outer of the test subject 101 fitted into jig 103b at 23°C, 50 RH, and a test speed of 10 mm / min, and the socket outer was deformed until it touched the outer wall 102. The deformation rate, expressed by the following formula (2), was calculated from the dimensions of the socket outer before and after the compression test. Compression tests were conducted with n=5, and the average of each measurement value was used as the deformation ratio. The results are shown in Table 1.
[0057]
[0058] In the socket outers of Examples 1 to 6, the diameter expanded to the inner wall surface of the outer wall 102 without breaking before contacting the outer wall 102. Here, the deformation rate shown in Table 1 is the deformation rate at the point when the socket outer contacts the inner wall surface of the outer wall 102 due to the expansion of the diameter.
[0059] In contrast, the socket outers of Comparative Examples 1 to 7 fractured before reaching the inner wall surface of the outer wall 102, and as a result, the deformation rate did not reach 5.0%.
[0060] [Test Example 2] The degree of crystallinity of PGA was calculated from the density of PGA using the following formula (1). In formula (1), the crystallinity of PGA is ρ c is 1,700 [g / cm³]3 ] and the amorphous density ρ of PGA a It is 1.509 [g / cm³] 3 The density of PGA is ρ [g / cm³]. 3 The density was measured using the density gradient tube method. Specifically, a sample for measurement was prepared by cutting out a section of the socket outer within 2 mm in the radial direction from the inner diameter of the socket outer, with a circumferential thickness of 0.5 to 1 mm relative to the axial cross-section of the socket outer. Next, carbon tetrachloride (Wako Pure Chemical Industries, for measuring oil content (infrared absorption)), 1,2-dichloroethane (Wako Pure Chemical Industries, reagent grade), and 1,2-dibromoethane were used, and standard solutions with different densities were prepared by mixing them (densities of standard solutions: 1.64, 1.62, 1.60, 1.58, 1.56, 1.54). The prepared standard solutions were poured into a graduated cylinder in order from the densest to the most dense to create a layered standard solution. After placing the graduated cylinder containing the layered standard solutions in a 23°C water bath and letting it stand for one day, the measurement position of the density sphere was read on the graduated cylinder scale, and a calibration curve was created. Subsequently, the measurement position of the sample was read on the graduated cylinder scale, and the density was calculated from the calibration curve. Density measurements were performed with n=2, and the average of each measurement value was defined as the density ρ.
[0061]
[0062] [Test Example 3] Lead time was measured using the following procedure. First, a sample was prepared by cutting a cube with sides of 10 mm from the socket outer of Example 2, and the dimensions of the sample before immersion were measured with calipers. Next, a resin net (made of polyethylene) was stretched over a beaker containing 1000 mL of deionized water so that the sample was placed in the center, and the beaker was heated in a water bath until the temperature inside the beaker reached 66°C. After reaching 66°C, the sample was immersed in the deionized water. At this time, the sample was placed on the resin net. After a predetermined time (48 hours, 120 hours, 216 hours) while maintaining the temperature, the sample was removed, and the dimensions of the sample after immersion were measured with calipers. The immersion time was plotted on the X axis, and the change in dimensions at each measurement point on the Y axis, and a linear function approximation line was created. The X-axis value when the Y-axis value on the approximation line became greater than 0 was defined as the lead time. Lead time was measured with n=3, and the average of the measured values was defined as the lead time. The lead time measurement results are shown in Table 1 and Figure 7. The time during which the thickness did not decrease, i.e., the lead time, was 41.2 hours.
[0063] This invention can be used in plugs that have the function of blocking well boreholes installed in wells during drilling.
[0064] 1 Mandrel 2 Sealing member 3 Socket 4, 5 Cone 6a, 6b Slip 7a, 7b Ring-shaped fixing member 10 Plug 31 Socket inner 32 Socket outer (Annular member for downhole tool)
Claims
1. An annular member for a downhole tool, used adjacent to the sealing member of the downhole tool, formed using a glycolic acid polymer, wherein the cross-sectional area of one side of the cross-section defined by the plane containing the central axis of the annular member for the downhole tool is 20 to 400 mm². 2 An annular member for a downhole tool, wherein the crystallinity of the glycolic acid polymer is 41.0% or less.
2. The annular member for a downhole tool according to claim 1, wherein the deformation rate expressed by the following formula (2) when a compression test is performed at a test speed of 10 mm / min is 5.0% or more.
3. The annular member for a downhole tool according to claim 1, wherein the radial thickness of the annular member for the downhole tool is 5 mm or more and 20 mm or less.
4. The annular member for a downhole tool according to claim 1, wherein the axial thickness of the annular member for the downhole tool is 5 mm or more and 40 mm or less.
5. The annular member for a downhole tool according to claim 1, wherein the lead time when the annular member for the downhole tool is immersed in deionized water at 66°C is 2.0 hours or more.
6. The annular member for a downhole tool according to claim 1, having a tapered shape that slopes from the outer circumference to the inner circumference of the ring.
7. A plug having the function of closing a well bore provided in a well during drilling, comprising: a hollow mandrel; an annular sealing member attached to the outer surface of the mandrel and deformed under pressure; and an annular member for a downhole tool according to any one of claims 1 to 6, attached downstream of the pressure received by the sealing member and adjacent to the sealing member.
8. A well drilling method comprising the steps of: transporting the plug described in claim 7 into a well; performing hydraulic fracturing using the plug; and disassembling part or all of the plug by bringing it into contact with a fluid present in the well.
9. The well drilling method according to claim 8, wherein the plug used is such that the deformation rate expressed by the following formula (2) when the annular member for the downhole tool is subjected to a compression test at a test speed of 10 mm / min is greater than or equal to the value of the following formula (3).