Separator for water electrolysis, alkaline water electrolysis device, and hydrogen production method

A thin-film alkaline water electrolysis separator with controlled alkaline water absorption and specific thickness range addresses the challenge of maintaining ion conductivity and gas barrier properties, ensuring stable and efficient hydrogen production.

WO2026234960A1PCT designated stage Publication Date: 2026-11-12FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015502
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-17
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing alkaline water electrolysis separators face challenges in maintaining high ion conductivity while ensuring sufficient gas barrier properties, particularly when power generation fluctuates, leading to increased hydrogen gas transfer and frequent shutdowns, which increases production costs.

Method used

A thin-film water electrolysis separator with a specific thickness range of 100 to 600 μm and controlled alkaline water absorption, using a porous support and material combination, including polyphenylene sulfide, polyether ether ketone, and polysulfone, to enhance ion conductivity and gas barrier properties.

Benefits of technology

The separator achieves high ion conductivity and effective gas barrier properties, enabling stable and efficient hydrogen production by reducing unwanted gas transfer between electrodes, thus minimizing shutdowns and lowering production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015502_12112026_PF_FP_ABST
    Figure JP2026015502_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a separator for water electrolysis comprising a porous support body and a porous material other than the porous support body, wherein the thickness of the separator is 100-600 μm, and the amount of alkaline water taken into the separator is less than 70 mm; and an alkaline water electrolysis device and a hydrogen production method that use said separator.
Need to check novelty before this filing date? Find Prior Art

Description

Water electrolysis separator, alkaline water electrolysis apparatus, and hydrogen production method

[0001] The present invention relates to a separator for water electrolysis, an alkaline water electrolysis apparatus, and a method for producing hydrogen.

[0002] Hydrogen is a clean energy source that does not emit carbon dioxide and is used as fuel in fuel cell vehicles and household fuel cells, for example. Alkaline water electrolysis, which uses a high-concentration alkaline aqueous solution as an electrolyte, is a known method for producing hydrogen. By performing alkaline water electrolysis using a renewable energy power generation system as the power source, hydrogen can be produced without emitting carbon dioxide, and therefore hydrogen is attracting increasing attention as a fundamental energy source for a sustainable society.

[0003] In alkaline water electrolysis, the bubble-like hydrogen (2H) generated at the cathode is produced. 2 O + 2e - →H 2 +2OH - This prevents the oxygen (4OH) from moving to the anode, and also prevents the bubble-like oxygen (4OH) generated at the anode from moving to the anode. - →O 2 +2H 2 O+4e - To prevent the movement of hydroxide ions (H2O) to the cathode side, a gas barrier separator (diaphragm) is placed between the cathode and the anode. On the other hand, it is desirable that hydroxide ions, which are carriers of the electrolytic reaction, can pass through the separator smoothly, and the separator is required to have high ionic conductivity. For example, Patent Document 1 describes an invention of an alkaline electrolysis separator comprising a porous support and first and second porous layers provided on one and the other side of the porous support, characterized in that the porous support has a thickness of 150 μm or less and the separator has a thickness of less than 250 μm. According to the separator described in Patent Document 1, it is possible to provide a separator with sufficient mechanical quality and improved ionic conductivity.

[0004] Special Publication No. 2023-531792

[0005] To improve the ion conductivity mentioned above, reducing the thickness of the separator is effective, but thinning the separator leads to a decrease in gas barrier properties. Power generation systems that utilize renewable energy as a power source for water electrolysis (solar power, wind power, etc.) have large fluctuations in power generation, and when power generation is low, the amount of gas moving through the separator increases relatively due to the decrease in gas production. From a safety standpoint, the amount of hydrogen gas generated at the cathode moving to the anode must be kept to a minimum, and generally, the operation of the water electrolysis equipment is controlled to stop when the hydrogen gas concentration on the anode side reaches 2%. If the gas barrier properties of the separator used are insufficient, the operation will be stopped frequently, leading to an increase in the cost of hydrogen production.

[0006] The present invention aims to provide a thin-film water electrolysis separator with sufficiently enhanced gas barrier properties. Furthermore, the present invention aims to provide an alkaline water electrolysis apparatus using the above-mentioned separator, and a method for producing hydrogen.

[0007] In view of the above problems, the inventors conducted extensive research and found that by using a porous, thin-film separator of a specific thickness range, and employing the amount of 30% by mass potassium hydroxide aqueous solution absorbed as an indicator of the pore connectivity, and by performing water electrolysis using a separator with this absorbed amount suppressed to a specific low level, the above problems can be solved. The present invention was completed based on this finding and further research.

[0008] The above problems of the present invention have been solved by the following means. [1] A water electrolysis separator comprising a porous support and a porous material other than the porous support, wherein the thickness of the separator is 100 to 600 μm, and the amount of alkaline water absorbed by the separator, as determined by the following measurement method, is less than 70 mm. [Amount of alkaline water absorbed] The water electrolysis separator is cut into strips 2.0 cm wide and 15.0 cm long to obtain strip-shaped separators. At 25°C and under saturated vapor pressure, the strip-shaped separator is immersed in a 30% by mass potassium hydroxide aqueous solution at 25°C, with its length perpendicular to the liquid surface, up to a length of 10 mm from one end in the length direction of the strip-shaped separator. One minute after the start of immersion, the distance (L, unit: mm) that the potassium hydroxide aqueous solution has seeped into the strip-shaped separator in the length direction is measured, and the value obtained by subtracting 10 mm from L is taken as the amount of alkaline water absorbed (mm). The amount of alkaline water absorbed by three strip-shaped separators is measured, and the arithmetic mean of the obtained measurements is taken as the amount of alkaline water absorbed by the water electrolysis separator. [2] The water electrolysis separator according to [1], wherein the amount of alkaline water absorbed is 25 mm or less. [3] The water electrolysis separator according to [1] or [2], wherein the thickness of the water electrolysis separator is 200 μm or less. [4] The water electrolysis separator according to any one of [1] to [3], wherein the porous support contains at least one of polyphenylene sulfide and polyether ether ketone. [5] The water electrolysis separator according to any one of [1] to [4], wherein the porous material contains polysulfone. [6] The water electrolysis separator according to any one of [1] to [5], wherein the water electrolysis separator contains polyvinylpyrrolidone. [7] The water electrolysis separator according to any one of [1] to [6], wherein the alkaline water electrolysis separator is a structure in which the porous support is enclosed within the porous material. [8] An alkaline water electrolysis apparatus comprising the water electrolysis separator according to any one of [1] to [7]. [9] An alkaline water electrolysis apparatus comprising the water electrolysis separator according to any one of [1] to [7] and an anode electrode and / or cathode electrode in contact with the water electrolysis separator.

[10] A method for producing hydrogen, comprising electrolyzing water using the alkaline water electrolysis apparatus described in [8] or [9].

[0009] In this invention, a numerical range represented using "~" means a range that includes the numbers written before and after "~" as the lower and upper limits, respectively.

[0010] The water electrolysis separator of the present invention is a thin film that exhibits high ion conductivity and also has sufficiently enhanced gas barrier properties. The alkaline water electrolysis apparatus of the present invention has high ion transfer efficiency between electrodes and effectively suppresses gas transfer between electrodes. The hydrogen production method of the present invention makes it possible to produce hydrogen more efficiently and stably by alkaline water electrolysis.

[0011] Figure 1 is a schematic diagram showing one embodiment of an alkaline water electrolysis apparatus. Figure 2 is a schematic diagram showing another embodiment of an alkaline water electrolysis apparatus. Figure 3 is a schematic diagram showing yet another embodiment of an alkaline water electrolysis apparatus. Figure 4 is an explanatory diagram schematically showing a method for measuring the amount of alkaline water taken in.

[0012] [Water Electrolysis Separator] The water electrolysis separator of the present invention (hereinafter also referred to as "the separator of the present invention") is a water electrolysis separator comprising a porous support and a porous material other than the porous support. The separator of the present invention is a thin film porous structure, and its thickness is in the range of 100 to 600 μm. This allows for sufficiently high ion conductivity, which correlates with thickness. Furthermore, the separator of the present invention suppresses the amount of alkaline water taken up (absorbed) by capillary action, as described later, to a specific level. This is thought to be due to the unique state of communication, size, and distribution of pores in the porous structure of the separator of the present invention. The separator of the present invention has the above-mentioned unique porous structure that exhibits the above-mentioned amount of alkaline water taken up, and despite being a thin film within a specific thickness range, its gas barrier properties are effectively enhanced. The separator of the present invention is suitable as a separator placed between the cathode electrode and the anode electrode in alkaline water electrolysis. The separator of the present invention can also be used as a separator in anion exchange membrane type water electrolysis, etc.

[0013] The thickness of the separator of the present invention is 100 to 600 μm, and within this thickness range, the effect of thickness on the amount of alkaline water absorbed is small and substantially negligible. The thickness of the separator of the present invention is preferably 100 to 550 μm, more preferably 100 to 500 μm, even more preferably 110 to 400 μm, even more preferably 120 to 300 μm, even more preferably 130 to 250 μm, and even more preferably 140 to 230 μm. Furthermore, due to its porous structure which suppresses the amount of alkaline water absorbed, the separator of the present invention exhibits excellent gas barrier properties even in thinner shapes. Therefore, the thickness of the separator of the present invention is also preferably 200 μm or less, preferably 100 to 200 μm, preferably 120 to 200 μm, preferably 130 to 200 μm, preferably 140 to 200 μm, and also preferably 150 to 200 μm. The thickness of the separator is determined by taking a cross-sectional SEM (scanning electron microscope) image of a cross-section cut from the separator with a razor blade at a magnification (e.g., 400x) that allows the entire cross-section to fit in a single field of view. Assuming that no holes exist in the obtained cross-sectional SEM image (assuming the holes are filled), the film thickness is measured at 20 equally spaced points, the arithmetic mean of the 20 measurements is calculated, and the value is rounded to the first decimal place in μm.

[0014] The amount of alkaline water absorbed by the separator can be determined as follows: [Amount of alkaline water absorbed] Cut the separator into strips 2.0 cm wide and 15.0 cm long to obtain strip-shaped separators. Attach clips to both ends of the strip-shaped separator in the longitudinal direction to secure it. At 25°C and under saturated vapor pressure, immerse the strip-shaped separator in a 30% potassium hydroxide aqueous solution at 25°C, with the length of the strip-shaped separator perpendicular to the liquid surface, up to a length of 10 mm from one end in the longitudinal direction. One minute after the start of immersion, measure the distance (L, unit: mm; distance from the end in the longitudinal direction of the strip-shaped separator) that the potassium hydroxide aqueous solution has seeped into the strip-shaped separator by capillary action, and subtract 10 mm from L to determine the amount of alkaline water absorbed by the strip-shaped separator (mm). Furthermore, the distance (length) over which the potassium hydroxide aqueous solution has seeped into the strip-shaped separator in the length direction is measured at the center of the strip-shaped separator in the width direction (1.0 cm from both ends in the width direction). Three strip-shaped separators of the above size are randomly cut from the separator, and the amount of alkaline water absorbed by each is measured. The arithmetic mean of the obtained measurements is taken as the amount of alkaline water absorbed by the separator. Figure 4 is an explanatory diagram of the above measurement method. Note that the drawing is a schematic diagram to facilitate understanding of the present invention, and the relative sizes and positional relationships do not directly represent the actual relationships. In Figure 4, 1 is a strip-shaped separator, the vertical direction in Figure 4 is the length direction of the strip-shaped separator, and the horizontal direction in Figure 4 is the width direction of the strip-shaped separator. 2 represents a clip, and 3 represents a 30% by mass potassium hydroxide aqueous solution (25°C). The strip-shaped separator is immersed in the potassium hydroxide aqueous solution up to a length (height) of 10 mm from its lower end in the longitudinal direction. As shown in Figure 4, the strip-shaped separator is fixed at both ends in the longitudinal direction with clips in a closed space and placed at 25°C under saturated vapor pressure.

[0015] The alkaline water intake amount of the separator of the present invention is preferably 65 mm or less, more preferably 60 mm or less, even more preferably 55 mm or less, even more preferably 50 mm or less, even more preferably 45 mm or less, even more preferably 40 mm or less, even more preferably 35 mm or less, even more preferably 30 mm or less, even more preferably 25 mm or less, and even more preferably 22 mm or less. The alkaline water intake amount of the separator of the present invention is usually 10 mm or more, may be 12 mm or more, or 14 mm or more. The preferred range for the alkaline water intake amount is 10 to 65 mm, more preferably 10 to 60 mm, even more preferably 10 to 55 mm, even more preferably 10 to 50 mm, even more preferably 10 to 45 mm, even more preferably 10 to 40 mm, even more preferably 12 to 35 mm, even more preferably 12 to 30 mm, even more preferably 12 to 25 mm, and even more preferably 14 to 22 mm.

[0016] In the separator of the present invention, a preferred combination of thickness and alkaline water intake can be appropriately combined from the preferred values ​​(ranges) of thickness and alkaline water intake described above. Specifically, the thickness of the separator of the present invention is 100 to 600 μm as described above, preferably 100 to 550 μm, more preferably 100 to 500 μm, even more preferably 110 to 400 μm, even more preferably 120 to 300 μm, even more preferably 130 to 250 μm, and even more preferably 140 to 230 μm. Furthermore, the thickness of the separator of the present invention is also preferably 200 μm or less, preferably 100 to 200 μm, preferably 120 to 200 μm, preferably 130 to 200 μm, preferably 140 to 200 μm, and also preferably 150 to 200 μm. In all of the above thickness ranges (100 to 600 μm, more preferred range, even more preferred range), the separator of the present invention has an alkaline water intake of less than 70 mm, preferably 65 mm or less, more preferably 60 mm or less, even more preferably 55 mm or less, even more preferably 50 mm or less, even more preferably 45 mm or less, even more preferably 40 mm or less, even more preferably 35 mm or less, even more preferably 30 mm or less, even more preferably 25 mm or less, and even more preferably 22 mm or less. Furthermore, in all of the above thickness ranges, the separator of the present invention has an alkaline water intake of 10 to 65 mm, more preferably 10 to 60 mm, even more preferably 10 to 55 mm, even more preferably 10 to 50 mm, even more preferably 10 to 45 mm, even more preferably 10 to 40 mm, even more preferably 12 to 35 mm, even more preferably 12 to 30 mm, even more preferably 12 to 25 mm, and even more preferably 14 to 22 mm.

[0017] The separator of the present invention may be a structure in which a porous support and a porous material other than the porous support are simply laminated together, but it is preferable that the porous support and the porous material other than the porous support are in an integral and inseparable state (i.e., a composite). For example, as shown in the embodiments described later, the separator of the present invention is a composite formed by immersing the porous support in a film-forming solution constituting the porous material and subjecting it to wet phase separation while encompassing the entire thickness direction of the porous support, or a composite with a structure equivalent to the composite obtained by this method. In the present invention, the structure of this composite is referred to as "a structure in which a porous support is embedded in a porous material other than the porous support."

[0018] The separator of the present invention is preferably a "structure in which a porous support is enclosed within a porous material other than the porous support described above." In this case, it is preferable that the porous material is arranged on the entire outer surface and the entire void of the porous support. "Outer surface of the porous support" means the surface when the porous support is viewed from a macroscopic perspective as a single film with a thickness, and "voids of the porous support" means the holes (voids between the fibers constituting the porous support) that the porous support has. The porous support and porous materials other than this porous support will be described in detail below.

[0019] <Porous Support> The porous support is not particularly limited as long as it is applicable to the porous separator of water electrolysis. For example, it can be selected from porous cloth, porous metal plate, and porous ceramic plate. The aperture ratio of the porous support is preferably 30 to 80%, more preferably 40 to 70%. The aperture ratio is the ratio of the area of ​​voids to the area of ​​unit area when the porous support is viewed in a planar manner. The porous support is preferably a porous cloth, and more preferably a porous polymer cloth. The porous polymer cloth is a woven or nonwoven fabric.

[0020] The polymers constituting the porous polymer cloth are not particularly limited, and examples include polypropylene, polyethylene, polysulfone (PSU), polyphenylene sulfide (PPS), polyamide, polyethersulfone, polyphenylsulfone, polyethylene terephthalate, polyetheretherketone (PEEK), sulfonated polyetheretherketone, monochlorotrifluoroethylene, copolymer of ethylene and tetrafluoroethylene or chlorotrifluoroethylene, polyimide, polyetherimide, and m-aramid. The porous support constituting the separator of the present invention preferably contains at least one of polyphenylene sulfide and polyetheretherketone, and more preferably contains polyetheretherketone.

[0021] The thickness of the porous support is preferably 30 to 150 μm, more preferably 30 to 100 μm, and even more preferably 30 to 75 μm. The thickness of the porous support can be measured using a dotting thickness gauge. The thickness of the porous support in the separator can be measured and calculated by removing the porous support from the separator using a solvent that dissolves the organic polymer contained in the porous material, and then measuring the thickness of the removed porous support using the method described above.

[0022] <Porous Material> The separator of the present invention includes a porous material other than the porous support described above (hereinafter also simply referred to as "porous material"). This porous material is applicable to water electrolysis separators and has the function of blocking the permeation of gases (preferably hydrogen gas and oxygen gas) and allowing ions (preferably hydroxyl ions) to permeate, and can be used without particular limitation as long as it can realize a separator that satisfies the alkaline water intake amount specified in the present invention.

[0023] The porous material includes at least an organic polymer. The porous material may further include other components such as hydrophilic inorganic particles.

[0024] (Organic Polymers) As organic polymers constituting the porous material, various organic polymers applicable to the wet phase separation described later can be used, for example.

[0025] The organic polymer can be selected from, for example, fluororesins, olefin resins, polyester resins, aromatic hydrocarbon resins, etc. As the fluororesin, a resin selected from polyvinylidene fluoride and polytetrafluoroethylene is preferred. As the olefin resin, polypropylene resin is preferred. As the polyester resin, a resin selected from polyethylene terephthalate, polybutylene terephthalate, and polybutylene naphthalate is preferred. As the aromatic hydrocarbon resin, polystyrene resin is preferred.

[0026] Other preferred organic polymers include polysulfone (PSU), polyethersulfone, polyphenylene sulfide, polyphenylsulfone, polyacrylate, polyetherimide, polyimide, and polyamideimide.

[0027] Organic polymers may be used individually or in combination of two or more types.

[0028] The organic polymer more preferably contains at least one of polyvinylidene fluoride, polysulfone, polyethersulfone, and polyphenylsulfone, even more preferably contains at least one of polysulfone, polyethersulfone, and polyphenylsulfone, and even more preferably contains polysulfone.

[0029] The weight average molecular weight (Mw) of the organic polymer is not particularly limited. In consideration of the handleability of the film-forming solution described later and the mechanical strength of the obtained separator, it can be, for example, 10000 to 500000, preferably 20000 to 300000. Mw can be determined under the following conditions. Apparatus: HLC-8220GPC (manufactured by Tosoh Corporation) Detector: Differential refractometer (RI (Refractive Index) detector) Pre-column: TSKGUARDCOLUMN HXL-L 6 mm × 40 mm (manufactured by Tosoh Corporation) Sample-side column: The following three columns are directly connected in sequence (all manufactured by Tosoh Corporation) - TSK-GEL GMHXL 7.8 mm × 300 mm - TSK-GEL G4000HXL 7.8 mm × 300 mm - TSK-GEL G2000HXL 7.8 mm × 300 mm Reference-side column: TSK-GEL G1000HXL 7.8 mm × 300 mm Constant temperature bath temperature: 40°C Mobile phase: THF (tetrahydrofuran) Sample-side mobile phase flow rate: 1.0 mL / min Reference-side mobile phase flow rate: 1.0 mL / min Sample concentration: 0.1 mass% Sample injection volume: 100 μL Data collection time: 5 minutes to 45 minutes after sample injection Sampling pitch: 300 milliseconds

[0030] The content of the organic polymer in the porous material is preferably 5 to 50 mass%, more preferably 5 to 40 mass%, further preferably 7 to 30 mass%, and particularly preferably 9 to 25 mass%.

[0031] (Hydrophilic inorganic particles) The porous material may contain hydrophilic inorganic particles. The hydrophilic inorganic particles are preferably particles selected from metal oxides and metal hydroxides.

[0032] As the above metal oxide, those selected from zirconium oxide, titanium oxide, bismuth oxide, cerium oxide and magnesium oxide are preferred.

[0033] As the above metal hydroxide, those selected from zirconium hydroxide, titanium hydroxide, bismuth hydroxide, cerium hydroxide and magnesium hydroxide are preferred.

[0034] As the hydrophilic inorganic particles, besides particles selected from metal oxides and metal hydroxides, barium sulfate particles can also be used.

[0035] The hydrophilic inorganic particles may be used singly, or two or more types may be used in combination.

[0036] The particle diameter of the hydrophilic inorganic particles is preferably 0.05 to 2.00 μm, more preferably 0.1 to 1.50 μm, still more preferably 0.15 to 1.00 μm, and even more preferably 0.20 to 1.00 μm. This particle diameter is the median diameter (D50), which means the particle diameter at 50% accumulation when the particle size distribution is measured by a laser diffraction / scattering method and the total volume of the particles is taken as 100% in the cumulative distribution.

[0037] When the porous material contains hydrophilic inorganic particles, the content of the hydrophilic inorganic particles in the porous material is preferably 50 to 95 mass%, more preferably 60 to 95 mass%, still more preferably 70 to 93 mass%, and particularly preferably 75 to 91 mass%.

[0038] When the porous material contains hydrophilic inorganic particles, the ratio of the content of the hydrophilic inorganic particles to the content of the organic polymer in the porous material (hydrophilic inorganic particles / organic polymer) is, in mass ratio, preferably 10 / 1 to 1 / 1, more preferably 9 / 1 to 2 / 1, still more preferably 8 / 1 to 3 / 1, even more preferably 7 / 1 to 4 / 1, and further preferably 6.5 / 1 to 4 / 1.

[0039] The separator of the present invention has a porosity of preferably 30 to 70%, more preferably 40 to 60%. This porosity can be calculated by the following method. First, the porous separator is cut into a predetermined area (S, unit: cm 2 ) and immersed in pure water at room temperature (25°C) for 24 hours. Thereafter, excess water droplets adhering to the surface are wiped off, and the weight (w1, unit: g) and thickness (d, unit: cm) are measured. The resultant is dried in an oven at 90°C for 24 hours, and the weight (w2, unit: g) is measured again. The porosity is calculated from the following calculation formula: Porosity (%) = {1 - [(w1 - w2) / (S × d)]} × 100

[0040] The separator of the present invention may be in the form of a long sheet wound into a roll, or it may be pre-cut into a predetermined shape according to the intended use, equipment, etc. Furthermore, the separator of the present invention may be stored by immersion in a preservation solution such as pure water. Alternatively, the separator of the present invention may be stored as a dry film without immersion in a preservation solution.

[0041] [Method for Manufacturing a Water Electrolysis Separator] The method for manufacturing the separator of the present invention is not particularly limited as long as the resulting separator includes a composite of a porous support and a porous material and satisfies the thickness and alkaline water intake amount specified in the present invention. Preferably, the separator of the present invention is manufactured by a method that includes forming a porous material integrally with the porous support by wet phase separation. This wet phase separation step makes it possible to obtain the separator of the present invention, which is composed of a porous material containing an organic polymer and a porous support. For example, the separator of the present invention can be obtained by casting a film-forming solution obtained by dissolving the constituent materials of the above porous material onto a film-forming support to form a coating film, impregnating the porous support into the coating film, and then performing wet phase separation with the film-forming support attached. In this wet phase separation, the above organic polymer is not dissolved, and a solvent (poor solvent) that is compatible (miscible) with the solvent (good solvent) of the film-forming solution is used as the coagulation bath. By immersing the coating film impregnated with the porous support in the solidification bath, the proportion of good solvent in the coating film of the film-forming solution decreases. As a result, the organic polymer and the solvent undergo phase separation, causing the organic polymer to gel (solidify) and form a porous material, thus obtaining the separator of the present invention. The temperature of the solidification bath in wet phase separation is preferably low. In this way, by performing wet phase separation in a low-temperature solidification bath with the film-forming support attached, the pore formation state on both sides can be changed (the pores on the film-forming support side become larger), forming a unique interconnected state, and as a result, the amount of alkaline water intake specified in the present invention can be satisfied. The temperature of the solidification bath is preferably 0 to 40°C, more preferably 1 to 35°C, even more preferably 2 to 30°C, even more preferably 3 to 25°C, even more preferably 4 to 20°C, even more preferably 5 to 15°C, and even more preferably 6 to 12°C. Furthermore, the type of solvent used in the film-forming solution, additives, viscosity of the film-forming solution, etc., can also contribute to the formation of the unique interconnected state described above. For example, N,N-dimethylformamide is a suitable solvent for achieving the above-mentioned alkaline water uptake. Furthermore, the addition of polyvinylpyrrolidone, glycerol, etc., can also contribute to achieving the above-mentioned alkaline water uptake.The resulting porous material preferably contains 0.1 to 10.0% by mass of at least one selected from polyvinylpyrrolidone and glycerol, more preferably 0.2 to 8.0% by mass, even more preferably 0.4 to 7.0% by mass, and still more preferably 0.8 to 6.0% by mass. The time for performing the solidification bath is preferably 1 to 15 minutes, more preferably 1 to 12 minutes, and even more preferably 3 to 10 minutes, from the viewpoint of controlling the pore size of the coating film on the film-forming support side.

[0042] <Film-forming solution> The film-forming solution can be any solution of the organic polymer that constitutes the porous material, and may contain the organic polymer and a solvent, and may also contain the hydrophilic inorganic particles.

[0043] In the wet phase separation process, a solvent capable of dissolving the above-mentioned organic polymer (a good solvent) is used as the film-forming solution. This solvent is preferably miscible with water. The solvent is preferably selected from N-methyl-2-pyrrolidone (NMP), N-ethyl-pyrrolidone (NEP), N-butyl-pyrrolidone (NBP), N,N-dimethylformamide (DMF), formamide, dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAC), acetonitrile, γ-valerolactone, the compounds (2) and (3) listed below, and mixtures thereof. At least one of NMP, NBP, γ-valerolactone, the compounds (2) and (3) listed below, and DMF is more preferred, and DMF is particularly preferred.

[0044] When the film-forming solution contains hydrophilic inorganic particles, the solvent content in the film-forming solution is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, even more preferably 25 to 70% by mass, even more preferably 30 to 65% by mass, even more preferably 32 to 60% by mass, and even more preferably 35 to 50% by mass. When the film-forming solution does not contain hydrophilic inorganic particles, the solvent content in the film-forming solution is preferably 20 to 95% by mass, more preferably 25 to 90% by mass, even more preferably 30 to 80% by mass, even more preferably 40 to 80% by mass, even more preferably 45 to 75% by mass, and even more preferably 50 to 75% by mass.

[0045] When the film-forming solution contains hydrophilic inorganic particles, the content of the organic polymer in the film-forming solution is preferably 2 to 30% by mass, more preferably 4 to 20% by mass, even more preferably 5 to 15% by mass, and still more preferably 6 to 12% by mass. When the film-forming solution does not contain hydrophilic inorganic particles, the content of the organic polymer in the film-forming solution is preferably 2 to 30% by mass, more preferably 4 to 30% by mass, even more preferably 6 to 25% by mass, and still more preferably 8 to 20% by mass.

[0046] Hydrophilic inorganic particles are particles that exist dispersed in the film-forming solution without dissolving, but in this invention, such a dispersion state is also referred to as a film-forming solution. In other words, the "solution" in film-forming solution refers to the state in which the organic polymer is dissolved in the solvent. When the above film-forming solution contains hydrophilic inorganic particles, the content of hydrophilic inorganic particles in the film-forming solution is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, even more preferably 20 to 70% by mass, and particularly preferably 25 to 60% by mass.

[0047] The above film-forming solution may contain components other than those described above (solvent, organic polymer, and hydrophilic inorganic particles). For example, to control pore formation in wet phase separation, it may contain polyethylene glycol, polyethylene oxide, polypropylene glycol, ethylene glycol, tripropylene glycol, glycerol, polyhydric alcohol, dibutyl phthalate, diethyl phthalate, diundecyl phthalate, isononanoic acid, neodecanoic acid, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethyleneimine, polyacrylic acid, methylcellulose, dextran, calcium chloride, magnesium chloride, and lithium chloride. Among these, polyvinylpyrrolidone is preferred because it can further suppress the amount of alkaline water absorbed even when the resulting separator is made thinner, and can effectively enhance the gas barrier properties. When the above film-forming solution contains other components and hydrophilic inorganic particles, the total content of the other components in the above film-forming solution is preferably 0.1 to 15% by mass, more preferably 0.2 to 10% by mass, and even more preferably 0.5 to 5% by mass. If the above film-forming solution contains other components and does not contain hydrophilic inorganic particles, the total content of the other components in the above film-forming solution is preferably 1 to 25% by mass, more preferably 5 to 25% by mass, and even more preferably 7 to 20% by mass.

[0048] <Solidification Bath> In the wet phase separation described above, water, or a mixed solvent of water and a hydrophilic organic solvent (an organic solvent miscible with water) or a water-soluble polymer can be used as the poor solvent for the solidification bath. Examples of hydrophilic organic solvents include aprotic solvents such as N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), and dimethylacetamide (DMAC), and alcohol solvents such as ethanol, propanol, or isopropanol. Examples of water-soluble polymers include water-soluble polymers such as polyvinylpyrrolidone (PVP) or polyvinyl alcohol (PVA). Among the above, water is preferred as the poor solvent.

[0049] After the wet phase separation described above, the film may be immersed in a glycol such as ethylene glycol or diethylene glycol, and water, or washed with the glycol and water. This step can remove any remaining solvent from the film.

[0050] [Alkaline Water Electrolysis] The separator of the present invention can be used, for example, by placing it between the cathode and the anode in alkaline water electrolysis. Preferred embodiments of an alkaline water electrolysis apparatus to which the separator of the present invention is applied (also referred to as "the alkaline water electrolysis apparatus of the present invention") will be described, but the alkaline water electrolysis apparatus of the present invention is not limited to these embodiments.

[0051] Figure 1 schematically shows a preferred embodiment of the alkaline water electrolysis apparatus of the present invention. In the alkaline water electrolysis apparatus (10) shown in Figure 1, a cathode electrode (12) is arranged on one side of the separator (11) of the present invention, and an anode electrode (13) is arranged on the other side. The separator (11) and each electrode (12, 13) are immersed in a high-concentration alkaline aqueous solution (14, preferably a potassium hydroxide aqueous solution or a sodium hydroxide aqueous solution). When an electric current flows between the electrodes, electrons are supplied to the cathode side, and bubble-like hydrogen (H) is produced from the water. 2 ) occurs (2H 2 O + 2e - →H 2 +2OH - ). Along with the generation of hydrogen, a hydroxyl ion (OH) is produced. - ) passes through the separator (11) and moves to the anode side, where electrons are removed and bubble-shaped oxygen (O 2 ) occurs (4OH - →O 2 +2H 2 O+4e -). The cathode electrode (12) and anode electrode (13) described above are preferably composed of an electrode substrate (conductive material) and a catalyst layer on the electrode substrate. When a catalyst layer is included, the catalyst species may be the same or different between the cathode electrode (12) and the anode electrode (13). In the alkaline water electrolysis apparatus (10) shown in Figure 1, the separator (11) and each electrode (12, 13) are far apart, so the distance traveled by hydroxyl ions is long, which limits the improvement of ion conduction efficiency.

[0052] Figure 2 schematically shows another preferred embodiment of the alkaline water electrolysis apparatus of the present invention. The alkaline water electrolysis apparatus (20) shown in Figure 2 is a zero-gap type in which the separator (11) and each electrode (12, 13) are arranged in contact with each other in the alkaline water electrolysis apparatus (10) shown in Figure 1. Because the separator (11) and each electrode (12, 13) are in contact in the alkaline water electrolysis apparatus (20) shown in Figure 2, the distance traveled by hydroxyl ions is short, which is advantageous in terms of ion conduction efficiency. In addition, from the viewpoint of imparting suitability for renewable energy, pressurized alkaline water electrolysis apparatuses that are operated under a pressure of 10 bar or more relative to atmospheric pressure (approximately 1 bar) are also known. As an example of such a pressurized alkaline water electrolysis apparatus, an example is the alkaline water electrolysis apparatus shown in Figure 2, in which the configuration, components, etc. of the alkaline water electrolysis apparatus are appropriately adjusted to be able to handle pressurized operation (for example, operation under pressurized conditions of 10 bar or more).

[0053] Figure 3 schematically shows yet another preferred embodiment of the alkaline water electrolysis apparatus of the present invention. The alkaline water electrolysis apparatus (30) shown in Figure 3 is a configuration that includes a membrane electrode assembly. That is, a cathode catalyst layer (32) is arranged on one side of the separator (31) of the present invention, and an anode catalyst layer (33) is arranged on the other side. These catalyst layers are composed of a catalyst and its binder. Furthermore, a gas diffusion layer (34) is formed on the outer surface of these catalyst layers (the surface opposite to the side on which the separator (33) is arranged) to constitute a membrane electrode assembly. In Figure 3, a bipolar plate (35) is formed further outside the membrane electrode assembly. When an alkaline aqueous solution is supplied to the cathode catalyst layer (32) and the anode catalyst layer (33) of this membrane electrode assembly, and the cathode catalyst layer (32) and the anode catalyst layer (33) are electrically connected and current is passed, bubble-like hydrogen is generated from the cathode catalyst layer (32) and bubble-like oxygen is generated from the anode catalyst layer (33).

[0054] In the above-described alkaline water electrolysis apparatus, the components other than the separator, such as the cathode electrode, cathode catalyst layer, anode electrode, and anode catalyst layer, are not particularly limited, and ordinary components used in alkaline water electrolysis apparatuses can be appropriately applied.

[0055] Thus, in one embodiment, the present invention provides an alkaline water electrolysis apparatus in which the separator of the present invention is incorporated as a separator in the alkaline water electrolysis apparatus. Furthermore, in one embodiment, the present invention provides a method for manufacturing an alkaline water electrolysis apparatus, which includes incorporating the separator of the present invention as a separator in the alkaline water electrolysis apparatus.

[0056] [Method for Producing Hydrogen] The method for producing hydrogen according to the present invention is the same as a conventional method for producing hydrogen (water electrolysis), except that it includes electrolysis of water using the alkaline water electrolysis apparatus of the present invention. In particular, a preferred method for producing hydrogen according to the present invention is one which includes using an alkaline aqueous solution containing 10 to 35% by mass of a metal hydroxide as the electrolyte solution and electrolyzing water at 70 to 95°C. Examples of metal hydroxides include sodium hydroxide and potassium hydroxide, and potassium hydroxide is preferred from the viewpoint of having a higher specific conductivity of the aqueous solution of the metal hydroxide. The content of the metal hydroxide (electrolyte) in the alkaline aqueous solution is 10 to 35% by mass, preferably 25 to 35% by mass, and more preferably 28 to 32% by mass. The temperature of the alkaline aqueous solution used when operating the alkaline water electrolysis apparatus and producing hydrogen by electrolyzing water is 70 to 95°C, preferably 70 to 90°C. This temperature may also be 75 to 85°C or 78 to 82°C. Thus, the separator of the present invention can be suitably used in the method for producing hydrogen according to the present invention that uses a high-temperature, high-concentration alkaline aqueous solution.

[0057] The present invention will be described in more detail based on examples, but the present invention is not to be construed as being limited to these examples. In the following, "hr" means time.

[0058] [Example 1] 8.5 g of polysulfone (PSU, trade name: Udel P-3500 LCD MB7, Mw: approximately 80,000, manufactured by Solvay) was added to 41.3 g of dimethylformamide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and stirred at 60°C for 5 hours to completely dissolve. Next, 2.4 g of PVP K90 (trade name: polyvinylpyrrolidone, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added and stirred at 60°C for 1 hour, and then ZrO 247.9 g of particles (product name: E101, manufactured by Luxfer) were added and stirred for a further 3 hours to obtain a coating solution. The obtained coating solution was cast onto a film-forming support (PET film) with an applicator clearance of 200 μm. A woven support made of polyether ether ketone (PEEK) (PEEKTEX; Sefar) was placed on top of the cast coating solution, and the coating solution was completely impregnated into the woven support. Subsequently, the film-forming support was gently immersed in a condensation bath (pure water) cooled to 10°C to form a porous polysulfone structure (phase separation step in the condensation bath). Further washing with water at 50°C for 10 minutes removed the woven support and the porous polysulfone structure from the PET film as a single unit. Subsequently, washing with water at 90°C for 1 hour obtained the separator of Example 1. This separator is a "structure in which a porous support is embedded in a porous material other than the porous support." The separators in Examples 2-5 and Comparative Example 1 are similar.

[0059] [Example 2] The separator of Example 2 was obtained in the same manner as in Example 1, except that Glycerol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of PVP K90 in the preparation of the coating solution, this coating solution was cast onto a PET film with an applicator clearance of 250 μm, and a polyphenylene sulfide (PPS) woven fabric support (PPS0113 / 45PW; manufactured by NBC Meshtec) was used instead of a PEEK woven fabric support.

[0060] [Example 3] In Example 2, Udel P1700 (Solvey, Mw: approximately 60,000) was used as the polysulfone instead of Udel P-3500 LCD MB7 in the preparation of the coating solution, and this coating solution was cast onto a PET film with an applicator clearance of 300 μm. The separator of Example 3 was obtained in the same manner as in Example 2.

[0061] [Example 4] The separator of Example 4 was obtained in the same manner as in Example 3, except that the coating solution was cast onto a PET film with an applicator clearance of 600 μm, a woven fabric support made of PPS (PPS0358 / 50PW; manufactured by NBC Meshtec) was used as the woven fabric support, and the temperature of the solidification bath was set to 30°C.

[0062] [Comparative Example 1] The clearance of the comma coater was adjusted to 700 μm, and the dope solution prepared in Example 2 was impregnated into a PPS woven fabric support (PPS0358 / 50PW; manufactured by NBC Meshtec). The dope solution was then gently immersed in 30°C pure water (coagulation bath) to form a porous polysulfone structure. Unlike in Example 2, no film-forming support was used in this immersion. After that, the material was washed with water at 50°C for 10 minutes to obtain the separator of Comparative Example 1.

[0063] [Test Example 1] Amount of alkaline water absorbed by the separator The amount of alkaline water absorbed by each separator obtained in the above examples and comparative examples was determined by the method described above.

[0064] [Test Example 2] Evaluation of hydrogen gas leakage to the anode side. Each separator obtained in the above examples and comparative examples was set in a cell for water electrolysis evaluation, and an electrolyte (30% by mass-KOH aqueous solution) heated to 85°C was supplied to the anode and cathode at a rate of 30 mL / min. Current density was 0.1 A / cm². 2 The cell was run continuously for 60 minutes with current applied to stabilize it. Then, it was run continuously for another 60 minutes (main operation), and the extent to which hydrogen gas generated on the cathode side leaked to the anode side during this 60 minutes was evaluated. Specifically, the gas recovered from the anode side flow path during the main operation was cooled to 0°C, water vapor was removed, and then it was analyzed using a gas chromatograph (GC3210G / GL Sciences, column: MS13X) to calculate the hydrogen gas concentration (unit: volume %) in the recovered gas.

[0065] [Test Example 3] Evaluation of Cell Voltage Each separator obtained in the above examples and comparative examples was set in a cell for water electrolysis evaluation, and an electrolyte (30% by mass-KOH aqueous solution) heated to 85°C was supplied to the anode and cathode at a rate of 30 mL / min. Current density was 1.2 A / cm² 2 The cell was run continuously for 60 minutes with current applied to achieve a certain state, and then stabilized. After that, it was run continuously for another 60 minutes (main operation), and the average value of the voltage during the main operation was taken as the cell voltage.

[0066] The results of the above test examples 1 to 3 are shown in the table below.

[0067]

[0068] Normally, increasing the thickness of the separator improves gas barrier properties, but as shown in the table above, this correlation changes depending on the amount of alkaline water absorbed. That is, as shown in the table above, even though the separator thickness is less than 1 / 3 of that of Comparative Example 1, the separators of Examples 1 and 2 (thickness 170 μm and 200 μm, alkaline water absorbed amount 20 mm) clearly suppress the amount of hydrogen gas leaking to the anode side compared to the separator of Comparative Example 1 (thickness 600 μm, alkaline water absorbed amount 70 mm). Similarly, the separator of Example 3, with a thickness of 220 μm, also suppresses the amount of alkaline water absorbed to the level specified in the present invention, and the amount of hydrogen gas leaking to the anode side is clearly suppressed compared to Comparative Example 1. Likewise, the separator of Example 4 also benefits from the effects of the present invention. There is a correlation between the thickness of the separator and the cell voltage, and it can be seen that the thicker the separator, the higher the cell voltage (lower ion conductivity). This in itself is in line with conventional knowledge. It can be seen that within the thickness range of the separator defined in this invention (100 to 600 μm), the cell voltage can be suppressed to a certain extent (less than 2.90 V in the above test example).

[0069] This invention overcomes the conventional understanding that gas barrier properties increase with increasing separator thickness by changing a new indicator: the amount of alkaline water absorbed. Specifically, it was discovered that even with thinner separators, gas barrier properties can be further enhanced by suppressing the amount of alkaline water absorbed, and that this amount can be controlled by optimizing the conditions of wet phase separation.

[0070] Although we have described the present invention along with its embodiments, we do not intend to limit our invention in any detail of the description unless specifically designated, and we believe that it should be interpreted broadly without contradicting the spirit and scope of the invention as set forth in the appended claims.

[0071] This application claims priority based on Japanese Patent Application No. 2025-078741, filed in Japan on 9 May 2025, which is incorporated herein by reference as part of the description herein.

[0072] 1. Strip-shaped separator 2. Clip 3. 30% potassium hydroxide aqueous solution 10. Alkaline water electrolysis system 11. Separator 12. Cathode electrode 13. Anode electrode 14. High-concentration alkaline aqueous solution 20. Alkaline water electrolysis system 30. Alkaline water electrolysis system 31. Separator 32. Cathode catalyst layer 33. Anode catalyst layer 34. Gas diffusion layer 35. Bipolar plate O 2 Bubble-shaped oxygen H 2 Bubble-shaped hydrogen OH - Hydroxy ion e - electronic

Claims

1. A water electrolysis separator comprising a porous support and a porous material other than the porous support, wherein the thickness of the separator is 100 to 600 μm, and the amount of alkaline water absorbed by the separator, as determined by the measurement method below, is less than 70 mm. [Amount of alkaline water absorbed] The water electrolysis separator is cut into strips 2.0 cm wide and 15.0 cm long to obtain strip-shaped separators. At 25°C and under saturated vapor pressure, the strip-shaped separators are immersed in a 30% by mass potassium hydroxide aqueous solution at 25°C, with the length direction of the strip-shaped separators perpendicular to the liquid surface, up to a length of 10 mm from one end in the length direction of the strip-shaped separators. One minute after the start of immersion, the distance (L, unit: mm) that the potassium hydroxide aqueous solution has seeped into the length direction of the strip-shaped separators is measured, and the value obtained by subtracting 10 mm from L is taken as the amount of alkaline water absorbed (mm). The amount of alkaline water absorbed by three strip-shaped separators is measured, and the arithmetic mean of the obtained measurements is taken as the amount of alkaline water absorbed by the water electrolysis separator.

2. The water electrolysis separator according to claim 1, wherein the amount of alkaline water taken in is 25 mm or less.

3. The water electrolysis separator according to claim 1, wherein the thickness of the water electrolysis separator is 200 μm or less.

4. The water electrolysis separator according to claim 1, wherein the porous support comprises at least one of polyphenylene sulfide and polyether ether ketone.

5. The water electrolysis separator according to claim 1, wherein the porous material contains polysulfone.

6. The water electrolysis separator according to claim 1, wherein the water electrolysis separator contains polyvinylpyrrolidone.

7. The water electrolysis separator according to claim 1, wherein the alkaline water electrolysis separator is a structure in which the porous support is enclosed within the porous material.

8. An alkaline water electrolysis apparatus comprising a water electrolysis separator according to any one of claims 1 to 7.

9. An alkaline water electrolysis apparatus comprising a water electrolysis separator according to any one of claims 1 to 7, and an anode electrode and / or cathode electrode in contact with the water electrolysis separator.

10. A method for producing hydrogen, comprising electrolyzing water using the alkaline water electrolysis apparatus described in claim 8.