Porous separator for water electrolysis, alkaline water electrolysis member, alkaline water electrolysis cell, alkaline water electrolysis apparatus, and method for producing hydrogen

The porous separator for alkaline water electrolysis addresses durability issues by optimizing permeation rates and ratios, ensuring effective hydrogen production under high-concentration alkaline conditions.

WO2026234962A1PCT designated stage Publication Date: 2026-11-12FUJIFILM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2026/015504
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-09
Filing Date
2026-04-17
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing porous separators for alkaline water electrolysis suffer from insufficient alkali durability and imbalance in ionic conductivity and liquid permeability, leading to performance degradation under high-concentration alkaline conditions.

Method used

A porous separator for water electrolysis with specific permeation rates for potassium hydroxide solutions at 25°C and 85°C, maintaining a ratio of permeation amounts and thickness within defined ranges to enhance alkali resistance and durability.

Benefits of technology

The separator exhibits excellent alkali resistance, allowing continuous hydrogen production with improved efficiency and reduced performance degradation over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2026015504_12112026_PF_FP_ABST
    Figure JP2026015504_12112026_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a porous separator for water electrolysis which contains a porous support and an organic polymer, wherein the permeation amount of a 30 mass% KOH aqueous solution at 25°C is 250 L / bar / h / m2 or less and the permeation amount of a 30 mass% KOH aqueous solution at 85°C is 400 L / bar / h / m2 or more; and an alkaline water electrolysis member, an alkaline water electrolysis cell, an alkaline water electrolysis apparatus and a method for producing hydrogen which use said separator.
Need to check novelty before this filing date? Find Prior Art

Description

Porous Separator for Water Electrolysis, Alkaline Water Electrolysis Member, Alkaline Water Electrolysis Cell, Alkaline Water Electrolysis Apparatus, and Hydrogen Production Method

[0001] The present invention relates to a porous separator for water electrolysis, an alkaline water electrolysis member, an alkaline water electrolysis cell, an alkaline water electrolysis apparatus, and a hydrogen production method.

[0002] Hydrogen is clean energy that does not emit carbon dioxide, and is used, for example, as a fuel for fuel cell vehicles and residential fuel cells. As a hydrogen production method, alkaline water electrolysis using a high-concentration alkaline aqueous solution as an electrolyte is known. If alkaline water electrolysis is performed using a power generation system that utilizes renewable energy as a power source, hydrogen can be produced without emitting carbon dioxide, so hydrogen is attracting increasing attention as a fundamental energy for a sustainable society.

[0003] In alkaline water electrolysis, the bubble-like hydrogen (2H generated at the cathode 2 O + 2e - → H 2 + 2OH - ) is prevented from moving to the anode side, and in order to prevent the bubble-like oxygen (4OH generated at the anode) - → O 2 + 2H 2 O + 4e - ) from moving to the cathode side, a gas-barrier separator (diaphragm) is disposed between the cathode and the anode. Further, in the alkaline water electrolysis system, water is consumed on the cathode side and water is generated on the anode side, so that the balance of the electrolyte across the separator will change if left as it is. To suppress this, the flow rate of the electrolyte is adjusted for each of the cathode and anode electrodes during alkaline water electrolysis. At this time, if the liquid permeability of the separator is high, the effect of the above flow rate adjustment will be diminished, so suppression of electrolyte permeation (hereinafter referred to as "suppression of liquid permeability") is also required. Furthermore, in addition to gas barrier properties and suppression of liquid permeability, this separator allows OH to pass from the cathode side to the anode side -Ionic conductivity that allows hydroxyl ions to pass through is also required. For this reason, porous membranes (microporous membranes) made of organic polymer materials are used as separators in alkaline water electrolysis. In other words, the above separator is required to achieve a balance between two conflicting properties: ensuring ionic conductivity by providing liquid permeability through the porous membrane, while suppressing liquid permeability.

[0004] As a separator used in such alkaline water electrolysis, for example, Patent Document 1 describes an alkaline electrolysis separator (1) comprising a porous support (10) and first (20b) and second (30b) porous layers provided on one and the other side of the porous support, characterized in that the porous support has a thickness (d1) of 150 μm or less and the separator has a thickness (d2) of less than 250 μm.

[0005] International Publication No. 2022 / 002904

[0006] Alkaline water electrolysis is typically carried out continuously under relatively high temperature conditions, such as 70°C or higher, using a high-concentration alkaline aqueous solution as the electrolyte. Therefore, separators in contact with high-concentration alkaline aqueous solutions are susceptible to deterioration over time due to the alkaline solution. Thus, a basic characteristic of separators is required to be the ability to suppress deterioration over time (performance degradation) due to high-concentration alkaline aqueous solutions (hereinafter referred to as "alkaline durability"). Moreover, in recent years, there has been a demand for further improvement in alkali durability in order to further improve the efficiency of water electrolysis, such as workability and cost reduction. However, the inventors have found that the separator described in Patent Document 1 does not exhibit sufficient alkali durability and there is room for improvement.

[0007] The present invention aims to provide a porous separator for water electrolysis with excellent alkali resistance. Furthermore, the present invention aims to provide an alkaline water electrolysis component, an alkaline water electrolysis cell, an alkaline water electrolysis apparatus, and a hydrogen production method using the porous separator for water electrolysis of the present invention.

[0008] The above problems of the present invention have been solved by the following means: [1] A porous separator for water electrolysis comprising a porous support and an organic polymer, wherein the permeation rate of a 30% by mass potassium hydroxide aqueous solution at 25°C is 250 L / bar / h / m 2 The following conditions apply, and the permeate rate of a 30% potassium hydroxide aqueous solution at 85°C is 400 L / bar / h / m². 2 The above is a porous separator for water electrolysis. [2] The porous separator for water electrolysis according to [1], wherein the ratio of the amount of permeation of a 30% potassium hydroxide aqueous solution at 85°C to the amount of permeation of a 30% potassium hydroxide aqueous solution at 25°C is 3.0 or more. [3] The porous separator for water electrolysis according to [1] or [2], wherein the ratio of the amount of permeation of a 30% potassium hydroxide aqueous solution at 85°C to the amount of permeation of a 30% potassium hydroxide aqueous solution at 25°C is 5.0 or more. [4] The porous separator for water electrolysis according to any one of [1] to [3], wherein the thickness is 220 μm or less.

[0009] [5] The permeate rate of a 30% potassium hydroxide aqueous solution at 25°C is 10 to 250 L / bar / h / m 2 The concentration is preferably 40 to 240 L / bar / h / m². 2 More preferably, 70 to 200 L / bar / h / m 2 More preferably, 70 to 150 L / bar / h / m 2 A porous separator for water electrolysis as described in any one of [1] to [4]. [6] The permeability of a 30% potassium hydroxide aqueous solution at 85°C is 400 to 2000 L / bar / h / m 2 The pressure is preferably 500 to 1600 L / bar / h / m 2 More preferably, 650 to 1400 L / bar / h / m 2 And more preferably 950 to 1400 L / bar / h / m 2A porous separator for water electrolysis according to any one of [1] to [5]. [7] A porous separator for water electrolysis according to any one of [1] to [6], wherein the ratio of the amount of permeation of a 30% potassium hydroxide aqueous solution at 85°C to the amount of permeation of a 30% potassium hydroxide aqueous solution at 25°C is 3.0 to 20, preferably 5.0 to 16, and more preferably 6.0 to 12. [8] A porous separator for water electrolysis according to any one of [1] to [3] and [5] to [7], wherein the thickness is 550 μm or less, preferably 15 to 250 μm, more preferably 15 to 220 μm, even more preferably 40 to 200 μm, and particularly preferably 80 to 200 μm.

[0010] [9] An alkaline water electrolysis component comprising a porous separator for water electrolysis described in any one of [1] to [8].

[10] An alkaline water electrolysis cell comprising a porous separator for water electrolysis described in any one of [1] to [8], or an alkaline water electrolysis component described in [5].

[11] An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell described in

[10] .

[12] A method for producing hydrogen, comprising electrolyzing water using the alkaline water electrolysis apparatus described in

[11] .

[13] A method for producing hydrogen according to

[12] , comprising using an alkaline aqueous solution containing 10 to 35% by mass of a metal hydroxide as the electrolyte solution, and electrolyzing water at 70 to 95°C.

[0011] In the present invention, when describing physical properties, etc., by indicating numerical ranges, if the upper and lower limits of the numerical range are described separately, either upper or lower limit can be appropriately combined to form a specific numerical range. On the other hand, when multiple numerical ranges represented using "~" are set and described, the upper and lower limits forming the numerical range are not limited to the specific combination of upper and lower limits described before and after "~" as a specific numerical range, but can be a numerical range formed by appropriately combining the upper and lower limits of each numerical range. In the present invention, a numerical range represented using "~" means a range that includes the numbers described before and after "~" as the lower and upper limits.

[0012] The porous separator for water electrolysis of the present invention exhibits excellent alkali resistance. Furthermore, the alkaline water electrolysis component, alkaline water electrolysis cell, and alkaline water electrolysis apparatus of the present invention include the porous separator for water electrolysis of the present invention and exhibit excellent alkali resistance. Moreover, the hydrogen production method of the present invention makes it possible to produce hydrogen by alkaline water electrolysis over a long period of time. The above and other features and advantages of the present invention will become clearer from the following description with reference to the attached drawings as appropriate.

[0013] Figure 1 is a schematic diagram showing one embodiment of the alkaline water electrolysis apparatus. Figure 2 is a schematic diagram showing another embodiment of the alkaline water electrolysis apparatus. Figure 3 is a schematic diagram showing yet another embodiment of the alkaline water electrolysis apparatus. Figure 4 shows a schematic cross-sectional view of the alkaline water permeability measuring device used in the example. Note that the hatching indicating the cross-sectional view in Figure 4 is omitted.

[0014] [Porous Separator for Water Electrolysis] The porous separator for water electrolysis of the present invention (hereinafter also referred to as "the separator of the present invention") is a porous separator for water electrolysis comprising a porous support and an organic polymer, wherein the permeation rate of a 30% by mass potassium hydroxide aqueous solution at 25°C is 250 L / bar / h / m 2 The following conditions apply, and the permeate rate of a 30% potassium hydroxide aqueous solution at 85°C is 400 L / bar / h / m². 2 That concludes the explanation. In porous separators for water electrolysis, regardless of the temperature and concentration of the potassium hydroxide aqueous solution (KOH aqueous solution), increasing the permeation rate of the KOH aqueous solution makes them more susceptible to deterioration over time due to alkaline aqueous solutions. Therefore, to improve alkali durability, it is common practice to reduce the permeation rate of the KOH aqueous solution. Furthermore, even if porous separators for water electrolysis have similar porous structure profiles, such as average pore size and porosity, they may not exhibit uniform (homogeneous) alkali durability. Under these circumstances, the inventors diligently investigated physical properties and structures other than the porous structure profile of porous separators for water electrolysis, and found that the permeation rate of a 30% by mass KOH aqueous solution at 25°C was W 25 While keeping the amount to a minimum, the permeate amount W of a 30% KOH aqueous solution at 85°C. 85We discovered that by deliberately increasing the amount of permeation W, it is possible to suppress deterioration over time caused by high-concentration alkaline aqueous solutions. Based on this finding, the inventors have determined that each permeation amount W 25 and W 85 The threshold values ​​are set to 250 L / bar / h / m². 2 The following and 400 L / bar / h / m 2 By setting the parameters as described above, we experimentally discovered that it is possible to suppress deterioration over time and achieve high alkali resistance, thus completing the present invention. Transmission amounts W at 25°C and 85°C. 25 and W 85 Although the reason why the porous separator for water electrolysis exhibits excellent alkali resistance by setting it as described above is not entirely clear, it is thought that the porous structure of the porous separator for water electrolysis, the contact state between the porous support and the organic polymer, etc., can be maintained overall, especially in the thickness direction, even in high-concentration alkaline aqueous solutions, and as a result, excellent alkali resistance is exhibited.

[0015] <Permeation amount W of 30% by mass KOH aqueous solution at 25°C 25 > The amount of permeate W of a 30% by mass KOH aqueous solution at 25°C in the separator of the present invention. 25 The pressure is 250 L / bar / h / m 2 The following applies: Transmission amount W 25 The pressure is 250 L / bar / h / m 2 The following applies to the transmission amount W at 85°C, as described later. 85 400 L / bar / h / m 2 When the above conditions are met, excellent alkali resistance is exhibited. In terms of further enhancing alkali resistance while maintaining gas barrier properties and suppressing liquid permeability, the permeation amount W, as described later, is particularly important. 85 The amount of transmission W that is combined with this 25 The pressure is 240 L / bar / h / m 2 Preferably, the following: 200 L / bar / h / m 2 It is more preferable that the following conditions are met: 150 L / bar / h / m 2 The following is even more preferable: Transmission amount W 25 The lower limit is not particularly limited and can be determined as appropriate. Transmission amount W 25The lower limit is, for example, 10 L / bar / h / m 2 This can be achieved, and considering ionic conductivity, 40 L / bar / h / m 2 It is preferable to set it to 70 L / bar / h / m 2 It is more preferable to have the above. In this invention, the amount of transmission W 25 It is sufficient that it is within the above range, at least within the thickness range of the separator of the present invention as described later. Transmission amount W 25 This value is calculated by setting a circularly punched separator (also called a sample) of the present invention into a filter holder (also called a sample holder), supplying a 30% by mass potassium hydroxide aqueous solution (electrolyte) adjusted to 25°C under a pressurized condition of 50 mbar to the circular separator from above, measuring the volume (mL) of potassium hydroxide aqueous solution that permeates through in 8 minutes, and calculating the permeation rate (water permeability). Details are as described in the examples below. Note that the permeation rate W is... 25 Typically, the separators measured are those in an unused state (e.g., separators immediately after manufacture, separators stored after manufacture), but used separators may also be measured.

[0016] <Permeation amount W of 30% by mass KOH aqueous solution at 85°C> 85 > The amount of permeate W of a 30% by mass KOH aqueous solution at 85°C in the separator of the present invention. 85 It is 400 L / bar / h / m 2 That's all. Transmission amount W 85 400 L / bar / h / m 2 If the above conditions are met, the transmission amount W at 25°C as described above. 25 The pressure is 250 L / bar / h / m 2 The following conditions result in excellent alkali resistance. The aforementioned permeation amount W allows for further enhancement of alkali resistance while maintaining gas barrier properties and suppression of liquid permeability. 25 The amount of transmission W that is combined with this 85 It is 500 L / bar / h / m 2 Preferably, the pressure is 650 L / bar / h / m 2 It is more preferable that the pressure be 950 L / bar / h / m 2It is even more preferable that the above conditions are met. Transmission amount W 85 There is no particular upper limit, but if it is too high, it may actually decrease alkali resistance, and gas barrier properties and liquid permeability may also be poor. Permeation amount W 85 The upper limit is, for example, 2000 L / bar / h / m² in terms of alkali resistance, gas barrier properties, and liquid permeability. 2 It can be as follows: 1600 L / bar / h / m 2 Preferably, it should be 1400 L / bar / h / m 2 The following is more preferable. In this invention, the amount of transmission W 85 It is sufficient that it is within the above range, at least within the thickness range of the separator of the present invention as described later. Transmission amount W 85 Except for changing the measurement temperature (the temperature of the potassium hydroxide aqueous solution) to 85°C, the transmission amount W 25 This value is calculated using the same method as the previous calculation method.

[0017] <Transmission amount W 25 and transmission amount W 85 Combination with > The amount of transmission W satisfied by the separator of the present invention 25 and transmission amount W 85 These are, respectively, the range defined in this invention, i.e., the transmission amount W. 25 The pressure is 250 L / bar / h / m 2 The following, and the transmission amount W 85 400 L / bar / h / m 2 The above is sufficient, but in terms of alkali resistance, the above preferred values ​​or ranges can be combined as appropriate. For example, the amount of permeation W 25 and transmission amount W 85 The combination is transmission amount W 25 The pressure is 10-250 L / bar / h / m 2 It is within the range and the transmittance W 85 The pressure is 400-2000 L / bar / h / m 2 A combination within the range is preferred. In this combination, the transmittance W 25 and transmission amount W 85The numerical range (at least one of the upper limit value and the lower limit value) of can appropriately adopt the above-described more preferable range (at least one of the upper limit value and the lower limit value) and the even more preferable range (at least one of the upper limit value and the lower limit value), respectively. Specifically, 250 L / bar / h / m 2 or less (preferably 10 to 250 L / bar / h / m 2 , more preferably 40 to 240 L / bar / h / m 2 , even more preferably 70 to 200 L / bar / h / m 2 , particularly preferably 70 to 150 L / bar / h / m 2 ) of permeation amount W 25 and 400 L / bar / h / m 2 or more (preferably 400 to 2000 L / bar / h / m 2 , more preferably 500 to 1600 L / bar / h / m 2 , even more preferably 650 to 1400 L / bar / h / m 2 , particularly preferably 950 to 1400 L / bar / h / m 2 ) of permeation amount W 85 can be combined.

[0018] <Ratio of Permeation Amount> The separator of the present invention is sufficient as long as the permeation amount W 25 and the permeation amount W 85 are within the above ranges, but from the viewpoint of further improving alkali durability, the ratio of the permeation amount W of a 30 mass% KOH aqueous solution at 85°C to the permeation amount W of a 30 mass% KOH aqueous solution at 25°C 25 85 [W 85 / W 25 is preferably 3.0 or more, more preferably 5.0 or more, and even more preferably 6.0 or more. The upper limit of the ratio [W 85 / W 25 is not particularly limited and can be set as appropriate, for example, it can be 20 or less, and from the viewpoints of alkali durability, as well as gas barrier properties and liquid permeability, it is preferably 16 or less, more preferably 12 or less. In the separator of the present invention, the ratio [W 85 / W 25 is the permeation amount W 25 and the permeation amount W​85 For each of the above ranges, and / or the amount of transmission W 25 and transmission amount W 85 For the above preferred combinations, it is preferable that they fall within each of the above ranges in terms of alkali resistance.

[0019] <Thickness> The thickness (film thickness) of the separator of the present invention is not particularly limited and can be appropriately determined considering properties such as mechanical strength and alkali resistance. For example, the thickness of the separator can be 550 μm or less. Since the separator of the present invention has excellent alkali resistance, the thickness can also be reduced, for example, 15 to 250 μm is preferred, 220 μm or less is more preferred, 15 to 220 μm is even more preferred, 40 to 200 μm is even more preferred, and 80 to 200 μm is particularly preferred. The thickness of the separator is obtained by taking a cross-sectional SEM (scanning electron microscope) image of a cross-section cut from the separator of the present invention with a razor at a magnification (for example, 400x) in which the cross-section of the separator of the present invention fits in one field of view, assuming that there are no pores in the obtained cross-sectional SEM image (assuming that the pores are filled with organic polymer), measuring the thickness at 20 equally spaced points, calculating the arithmetic mean of the obtained 20 measurements, and rounding the value to the first decimal place in μm notation.

[0020] <Average pore size> The average pore size in the surface region of the separator of the present invention is the transmission amount W described above. 25 and transmission amount W 85 The pore size can be appropriately adjusted within the range that satisfies the following conditions. For example, it can be 0.05 to 20 μm on both the front and back surfaces, preferably 0.1 to 10 μm, and more preferably 0.1 to 5 μm. The average pore size in the surface region is measured and calculated as follows: A separator of the present invention is impregnated with methanol and frozen in liquid nitrogen. A cross section is cut from the separator using a microtome (for example, Leica Corporation, product name: EM UC6). The arithmetic mean of the pore size in the region from the surface to 10% of the separator's thickness (for example, in the case of a separator with a thickness of 200 μm, the region from the surface to 20 μm) is placed in one field of view, and the value rounded to the second decimal place is defined as the "average pore size in the film surface region".

[0021] <Porosity> The porosity of the separator of the present invention is the permeation amount W described above. 25 and transmission amount W 85 The porosity can be appropriately adjusted within the range that satisfies the requirements. For example, from the viewpoint of alkali resistance, and further from the viewpoint of ion permeability and gas barrier properties, it is preferably 30 to 70%, and more preferably 40 to 60%. This porosity is the value of porosity calculated from the insertion curve by the mercury intrusion method.

[0022] <Bubble Point> The separator of the present invention has the above-mentioned transmission amount W 25 and transmission amount W 85 The pressure can be adjusted as appropriate within the range that satisfies the requirements. For example, from the viewpoint of gas barrier properties required for porous separators for water electrolysis, it is preferable that the bubble point exceeds 1 bar, and more preferably exceeds 2 bar. The bubble point is determined by measuring with a palm porometer based on the bubble point method described in ASTM (American Society for Testing and Materials) F316-86, and the pressure at which the first bubble is generated in the resulting wet curve is defined as the bubble point.

[0023] <Ion Resistance> The separator of the present invention has an ion resistance of 0.08 Ω·cm, from the viewpoint of ion permeability required for porous separators for water electrolysis. 2 Preferably less than 0.07 Ω·cm 2 Less than 0.06 Ω·cm is more preferable. 2 Less than 0.05 Ω·cm is even more preferable. 2 A value less than 0.01 Ω·cm is particularly preferable. However, a practical lower limit is 0.01 Ω·cm. 2 The above is true, and a preferred range is 0.01 Ω·cm. 2 0.08Ω・cm or more 2 Examples include values ​​less than the following. Ion resistance is a value measured by AC impedance method at 30°C with the separator of the present invention, punched out in a circular shape, set in a cell.

[0024] <Structure of the Separator of the Present Invention> The separator of the present invention is a porous separator for water electrolysis comprising a porous structure containing a porous support and an organic polymer. In the separator of the present invention, the organic polymer may be included alone as a porous material, but it is preferable that it be included as a porous material containing other components such as hydrophilic inorganic particles. The separator of the present invention is not a structure in which a porous support and an organic polymer (a porous material containing an organic polymer) are simply stacked, but a structure in which the porous support and the organic polymer are inseparable (i.e., a composite). For example, as shown in the examples described later, the separator of the present invention is a composite (or a composite with a structure equivalent to the composite obtained by this method) formed by immersing a porous support in a film-forming solution constituting a porous material and subjecting it to wet phase separation while the porous support is encased. As described above, in the present invention, the structure of a composite formed by immersing a porous support in a film-forming solution constituting a porous material and subjecting it to wet phase separation while the porous support is encased is referred to as a "structure in which a porous support is enclosed within a porous material". Furthermore, the separator of the present invention is not limited to those manufactured by the wet phase separation method described above, but also includes those manufactured by other methods, as long as they are "structures in which a porous support is enclosed within a porous material."

[0025] The specific configuration of the separator of the present invention is a porous separator for water electrolysis comprising a porous support and at least an organic polymer as a porous material, wherein the permeate amount W 25 The pressure is 250 L / bar / h / m 2 The following applies: Transmission amount W 85 400 L / bar / h / m 2As long as the above is met, there are no particular limitations. For example, the separator of the present invention preferably has a porous support and a porous material disposed on at least one of the outer surface and voids of the porous support. The "outer surface of the porous support" means the surface when the porous support is viewed from a macroscopic perspective as a film-like support having a single thickness, and the "voids of the porous support" means the holes (voids between the framework (e.g., fibers, metals, ceramics) that constitute the porous support) that the porous support has. The structure in which a porous material is disposed on at least one of the outer surface and voids of the porous support has the above-mentioned permeation amount W 25 and transmission amount W 85 The porous material can be appropriately determined within the range that satisfies the requirements, for example, the porous material may be disposed only on the outer surface of the porous support. In this case, the porous material may be disposed only on one side of the outer surface of the porous support, which is a membrane-like support, or it may be disposed on both sides of the outer surface. In the case of a structure in which the porous material is disposed on one or both sides of the outer surface, the porous material may be disposed on at least a part of each surface, or it may be disposed on the entire surface. Furthermore, the porous material may be disposed only in at least a part of the voids of the porous support. Moreover, the porous material may be disposed on at least a part of the outer surface of the porous support and at least a part of the voids. In the present invention, such forms are also included in the structure in which the porous material is disposed on at least one of the outer surface and voids of the porous support. Among these, a structure in which the porous material is disposed on the entire outer surface and the entire voids of the porous support is preferred. The porous support, porous material, organic polymer and hydrophilic inorganic particles which are constituent materials of the porous material will be described in detail below.

[0026] <Porous Support> The porous support is not particularly limited as long as it is applicable to a porous separator for water electrolysis, but it is preferably applicable to a porous separator for alkaline water electrolysis. For example, it can be selected from porous cloth, porous metal plate, and porous ceramic plate. The opening ratio of the porous support is preferably 30 to 80%, more preferably 40 to 70%. The opening ratio is the ratio of the area of ​​voids to the unit area when the porous support is viewed in a planar manner. The porous support is preferably a porous cloth, and more preferably a porous polymer cloth. The porous polymer cloth is a woven or nonwoven fabric.

[0027] The polymers constituting the porous polymer fabric are not particularly limited, and examples include polypropylene, polyethylene, polysulfone (PSU), polyphenylene sulfide (PPS), polyamide, polyethersulfone, polyphenylsulfone, polyethylene terephthalate, polyetheretherketone (PEEK), sulfonated polyetheretherketone, monochlorotrifluoroethylene, copolymer of ethylene and tetrafluoroethylene or chlorotrifluoroethylene, polyimide, polyetherimide, and m-aramid. Among the above, it is preferable that the polymer constituting the porous polymer fabric contains at least one of polypropylene, polyphenylene sulfide, and polyetheretherketone, and more preferably at least one of polyphenylene sulfide and polyetheretherketone. The polymer constituting the porous polymer fabric may be one type or two or more types.

[0028] The thickness of the porous support is preferably 30 to 150 μm, more preferably 30 to 100 μm, and even more preferably 30 to 75 μm. The thickness of the porous support is measured using a dotting thickness gauge. The thickness of the porous support in the separator can be measured and calculated by removing the porous support from the separator using a solvent that dissolves the organic polymer contained in the porous material, and then measuring the thickness of the porous support using the method described above.

[0029] <Porous materials> Porous materials have the above-mentioned permeation rate W25 and transmission amount W 85 Any separator that can satisfy the above conditions is acceptable, and as a porous separator for water electrolysis, it is preferable that it has the function of blocking the permeation of gases (preferably hydrogen gas and oxygen gas) and allowing ions (preferably hydroxyl ions) to permeate.

[0030] As described above, the porous material contains at least an organic polymer and may also contain other components such as hydrophilic inorganic particles.

[0031] (Organic Polymer) The organic polymer contained in the porous material is not particularly limited as long as it is applicable to porous separators for water electrolysis, and various organic polymers applicable to wet phase separation described later can be used to control the permeate amount W of the separator. 25 and transmission amount W 85 It is preferable because it is easy to adjust.

[0032] The organic polymer can be selected from, for example, fluororesins, olefin resins, polyester resins, aromatic hydrocarbon resins, etc. As the fluororesin, a resin selected from polyvinylidene fluoride and polytetrafluoroethylene is preferred. As the olefin resin, polypropylene resin is preferred. As the polyester resin, a resin selected from polyethylene terephthalate, polybutylene terephthalate, and polybutylene naphthalate is preferred. As the aromatic hydrocarbon resin, polystyrene resin is preferred.

[0033] Other preferred organic polymers include polysulfone (PSU), polyethersulfone, polyphenylene sulfide, polyphenylsulfone, polyacrylate, polyetherimide, polyimide, and polyamideimide.

[0034] Organic polymers may be used individually or in combination of two or more types.

[0035] The organic polymer more preferably contains at least one of polyvinylidene fluoride, polysulfone, polyethersulfone, polyphenylene sulfide, and polyphenylsulfone; even more preferably contains at least one of polysulfone, polyethersulfone, polyphenylene sulfide, and polyphenylsulfone; particularly preferably contains at least one of polysulfone, polyethersulfone, and polyphenylene sulfide; and most preferably contains polysulfone.

[0036] The mass-average molecular weight (Mw) of the organic polymer is not particularly limited. Considering the handling properties of the film-forming solution described later and the mechanical strength of the resulting separator, it can be, for example, 10,000 to 500,000, preferably 20,000 to 300,000. Mw can be determined under the following conditions. In the present invention, the larger the mass-average molecular weight of the organic polymer, the greater the permeate W of the separator. 25 and transmission amount W 85 There is a tendency to reduce the amount of permeation W. For example, if the mass-average molecular weight of a more preferable organic polymer such as polysulfone is 10,000 or more, the amount of permeation W can be reduced. 25 This can be kept below the upper limit of the above range. On the other hand, in the present invention, if the mass-average molecular weight of the organic polymer is 80,000 or less, the amount of transmission W 85The value can be increased to above the lower limit of the above range. Apparatus: HLC-8220GPC (Tosoh Corporation) Detector: Differential refractometer (RI (Refractive Index) detector) Pre-column: TSKGUARD COLUMN HXL-L 6 mm x 40 mm (Tosoh Corporation) Sample-side column: The following three columns are directly connected in order (all Tosoh Corporation) ・TSK-GEL GMHXL 7.8 mm x 300 mm ・TSK-GEL G4000HXL 7.8 mm x 300 mm ・TSK-GEL G2000HXL 7.8 mm x 300 mm Reference-side column: TSK-GEL G1000HXL 7.8 mm x 300 mm Oven temperature: 40°C Mobile phase: THF (Tetrahydrofuran) Sample-side mobile phase flow rate: 1.0 mL / min Reference-side mobile phase flow rate: 1.0 mL / min Sample concentration: 0.1% by mass Sample injection volume: 100 μL Data acquisition time: 5 to 45 minutes after sample injection Sampling pitch: 300 milliseconds

[0037] When a preferred organic polymer is selected from the above-mentioned organic polymers and its mass-average molecular weight is adjusted to the above range, particularly 10,000 to 80,000, the amount of permeation W is obtained. 25 and transmission amount W 85 A method using the above-mentioned preferred organic polymer having a specific mass-average molecular weight that can be easily adjusted to each range defined in the present invention allows for transmission of W 25 and transmission amount W 85 This is one of the preferred adjustment methods.

[0038] The content of organic polymers in the porous material is not particularly limited, but the permeate amount W of the separator 25 and transmission amount W 85 In terms of ease of adjusting to the above range, 5 to 49.99% by mass is preferred, 5 to 40% by mass is more preferred, 7 to 30% by mass is even more preferred, and 9 to 25% by mass is particularly preferred.

[0039] (Hydrophilic inorganic particles) Porous materials may contain hydrophilic inorganic particles. Hydrophilic inorganic particles are preferably selected from metal oxides and metal hydroxides.

[0040] The above metal oxides are preferably selected from zirconium oxide, titanium oxide, bismuth oxide, cerium oxide, and magnesium oxide.

[0041] The above metal hydroxides are preferably selected from zirconium hydroxide, titanium hydroxide, bismuth hydroxide, cerium hydroxide, and magnesium hydroxide.

[0042] In addition to particles selected from metal oxides and metal hydroxides, barium sulfate particles can also be used as hydrophilic inorganic particles.

[0043] In the present invention, the use of the above preferred organic polymer in combination with a metal oxide, particularly zirconium oxide, results in a transmission amount W 25 and transmission amount W 85 It is preferable in terms of ease of adjustment and alkali resistance. Hydrophilic inorganic particles may be used individually or in combination of two or more types.

[0044] The particle size of the hydrophilic inorganic particles is preferably 0.05 to 2.00 μm, more preferably 0.1 to 1.50 μm, even more preferably 0.15 to 1.00 μm, and particularly preferably 0.20 to 1.00 μm. This particle size is the median diameter (D50), and is determined by measuring the particle size distribution using laser diffraction and scattering methods, representing the particle size at which the cumulative distribution reaches 50% when the total volume of the particles is considered 100%.

[0045] When a porous material contains hydrophilic inorganic particles, the content of hydrophilic inorganic particles in the porous material is not particularly limited, but the permeate amount W of the separator 25 and transmission amount W 85 In terms of ease of adjusting to the above range, 50 to 94.99% by mass is preferred, 60 to 94.99% by mass is more preferred, 70 to 93% by mass is even more preferred, and 75 to 91% by mass is particularly preferred.

[0046] When the porous material contains hydrophilic inorganic particles, the ratio of the content of hydrophilic inorganic particles to the content of organic polymer in the porous material (content of hydrophilic inorganic particles / content of organic polymer) is preferably 10 / 1 to 1 / 1 by mass, more preferably 9 / 1 to 2 / 1, even more preferably 8 / 1 to 3 / 1, even more preferably 7 / 1 to 4 / 1, and even more preferably 6.5 / 1 to 4 / 1.

[0047] (Other components) Other components that may be contained in the porous material include, for example, components that control pore formation in wet phase separation, specifically polyethylene glycol, polyethylene oxide, polypropylene glycol, ethylene glycol, tripropylene glycol, glycerol, polyhydric alcohol, dibutyl phthalate, diethyl phthalate, diundecyl phthalate, isononanoic acid, neodecanoic acid, polyvinylpyrrolidone, polyvinyl alcohol, polyvinyl acetate, polyethyleneimine, polyacrylic acid, methylcellulose, dextran, calcium chloride, magnesium chloride, and lithium chloride. The total content of other components in the porous material is preferably 0.01 to 10% by mass, more preferably 0.05 to 5% by mass, and even more preferably 0.1 to 1% by mass.

[0048] In the present invention, when the content of organic polymers, hydrophilic inorganic particles, and other components are adjusted to the above ranges, the amount of permeation W is obtained. 25 and transmission amount W 85 This makes it easier to adjust the transmission amount W to the range defined in the present invention. 25 and transmission amount W 85 This is one of the preferred adjustment methods.

[0049] The separator of the present invention can be used as a separator placed between the cathode electrode and the anode electrode in a method for producing hydrogen by electrolyzing an alkaline aqueous solution using an electrolytic cell. Furthermore, the separator of the present invention can also be used as a separator in an anion exchange membrane type water electrolysis system. In particular, it can be suitably used as a porous separator for water electrolysis in the alkaline water electrolysis apparatus described below.

[0050] The separator of the present invention may be in the form of a long sheet wound into a roll, or it may be pre-cut into a predetermined shape according to its intended use, equipment, etc. From the viewpoint of manufacturing efficiency, it is also preferable that the separator of the present invention is in the form of a long sheet and has a thickness distribution in at least one of the width and length directions in which the thickness in the center of the sheet is greater than the thickness at both ends of the sheet. Furthermore, the separator of the present invention may be stored by immersing it in a preservation solution such as pure water. Furthermore, the separator of the present invention may be stored as a dry film without being immersed in a preservation solution.

[0051] [Method for Manufacturing Separator] The method for manufacturing the separator of the present invention provides a separator comprising a composite of a porous support and an organic polymer, wherein the permeate amount W as defined in the present invention 25 and transmission amount W 85 The present invention is not particularly limited as long as the following conditions are met. The separator of the present invention is manufactured by a method which includes forming a porous material containing an organic polymer integrally with a porous support by wet phase separation, wherein the permeate amount W 25 and transmission amount W 85This is preferable because it is easy to adjust the above range. This wet phase separation process makes it possible to obtain the separator of the present invention, which is composed of a porous material containing an organic polymer and a porous support. The separator of the present invention can be obtained by performing vapor induction phase separation and / or liquid induction phase separation as wet phase separation. Specifically, it is preferably manufactured by a method that includes impregnating a porous support with a film-forming solution containing the constituent materials of the porous material, performing water vapor induction phase separation on a laminate of the obtained porous support and a coating film containing the constituent materials of the porous material, and / or immersing the laminate (the laminate after water vapor induction phase separation if the above water vapor induction phase separation has been performed) in a condensation bath. In the present invention, it is preferable to perform the above water vapor induction phase separation and / or liquid induction phase separation using a film-forming support. For example, the separator of the present invention can be obtained by casting a film-forming solution containing the constituent materials of the porous material onto a film-forming support to form a coating film, impregnating the coating film with a porous support, and then performing wet phase separation with the film-forming support attached or with the film-forming support removed. In the present invention, wet phase separation is performed with the above-mentioned film-forming support attached, thereby reducing the amount of permeation W 25 and transmission amount W 85 This is particularly preferable because it makes it easy to adjust the value within the above range.

[0052] <Film-forming solution> The film-forming solution can be any dissolving solution containing an organic polymer that will be a constituent material of the porous material, and may contain the organic polymer and a solvent, as well as other components such as hydrophilic inorganic particles.

[0053] (Solvent) In the film-forming solution for wet phase separation, a solvent capable of dissolving the above organic polymer (a good solvent) can be used. This solvent is preferably miscible with water. The solvent is preferably selected from N-methyl-2-pyrrolidone (NMP), N-ethyl-2-pyrrolidone (NEP), N-butyl-2-pyrrolidone (NBP), N,N-dimethylformamide (DMF), formamide, dimethyl sulfoxide (DMSO), N,N-dimethylacetamide (DMAC), acetonitrile, γ-valerolactone, N,N-dimethylpropionamide, the compounds (2) and (3) listed below, and mixtures thereof, with at least one of NMP, NBP, γ-valerolactone, N,N-dimethylpropionamide, and the compounds (2) and (3) listed below being more preferred. Among the above, when γ-valerolactone, a mixture of the compounds (2) and (3) below, NEP, NMP, etc. are used as the solvent, the amount of permeation W 25 and transmission amount W 85 The amount tends to decrease, while when N,N-dimethylpropionamide, NBP, DMF, etc. are used, the amount of transmission W 25 and transmission amount W 85 The amount of permeation W tends to increase. By selecting the solvent used in the film-forming solution in this way, the amount of permeation W can be increased. 25 and transmission amount W 85 The method of selecting the solvent and the amount of permeation W can be adjusted, and the method of selecting the solvent can also be adjusted. 25 and transmission amount W 85 This is one of the preferred adjustment methods.

[0054] If the film-forming solution contains hydrophilic inorganic particles, the solvent content in the film-forming solution is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, even more preferably 25 to 70% by mass, even more preferably 30 to 65% by mass, even more preferably 32 to 60% by mass, and even more preferably 35 to 50% by mass. If the film-forming solution does not contain hydrophilic inorganic particles, the solvent content in the film-forming solution is preferably 20 to 95% by mass, more preferably 25 to 90% by mass, even more preferably 30 to 80% by mass, even more preferably 40 to 80% by mass, even more preferably 45 to 75% by mass, and even more preferably 50 to 75% by mass.

[0055] (Organic Polymers) The description of organic polymers in the film-forming solution can be applied to organic polymers contained in the film-forming solution as described above for separators. When the film-forming solution contains hydrophilic inorganic particles, the content of organic polymers in the film-forming solution is preferably 2 to 30% by mass, more preferably 4 to 20% by mass, even more preferably 5 to 15% by mass, and particularly preferably 6 to 12% by mass. When the film-forming solution does not contain hydrophilic inorganic particles, the content of organic polymers in the film-forming solution is preferably 2 to 30% by mass, more preferably 4 to 30% by mass, even more preferably 6 to 25% by mass, and particularly preferably 8 to 20% by mass.

[0056] (Hydrophilic inorganic particles) For hydrophilic inorganic particles that may be contained in the film-forming solution, the description of hydrophilic inorganic particles in the separator described above can be applied. Although hydrophilic inorganic particles are particles that exist dispersed in the film-forming solution without dissolving, in this invention, such a dispersion state is also referred to as the film-forming solution. That is, the "solution" in the film-forming solution refers to the state in which the organic polymer is dissolved in the solvent. When the above film-forming solution contains hydrophilic inorganic particles, the content of hydrophilic inorganic particles in the film-forming solution is preferably 10 to 85% by mass, more preferably 15 to 80% by mass, even more preferably 20 to 70% by mass, and particularly preferably 25 to 60% by mass.

[0057] (Other Components) The above film-forming solution may contain components other than those described above (solvent, organic polymer, and hydrophilic inorganic particles). Other components include other components that may be contained in the above porous material. Other components (also called additives) are thought to be able to control the formation of pores by at least one action, such as acting as the starting point for pore formation in the wet phase separation step described later, adjusting the viscosity of the coating solution, or adjusting the hydrophilicity of the inner wall of the formed pores. Among the additives mentioned above, using glycerol, for example, can increase the permeation amount W. 25 and transmission amount W 85 The amount tends to decrease, while when polyvinylpyrrolidone, polyethylene glycol, etc. are used, the amount of transmission W 25 and transmission amount W 85The amount tends to increase. In particular, polyvinylpyrrolidone can appropriately control the pore diameter and size distribution of the pores formed, and also the amount of transmission W 25 and transmission amount W 85 This makes it easier to adjust the value within the above range. In separators, if the pore size is too large, durability (mechanical strength, alkali resistance) and gas barrier properties deteriorate, and if it is too small, ionic resistance increases. In the present invention, additives can be selected considering durability, gas barrier properties, and ionic resistance, with polyvinylpyrrolidone being particularly preferred. In the present invention, by selecting other components used in combination with the above-mentioned preferred organic polymer and metal oxide, the permeation amount W can be increased as described above. 25 and transmission amount W 85 It is possible to adjust the amount of permeation W, and there are also ways to select other components. 25 and transmission amount W 85 This is one of the preferred adjustment methods.

[0058] If the above film-forming solution contains other components and hydrophilic inorganic particles, the total content of the other components in the above film-forming solution is preferably 0.1 to 15% by mass, more preferably 0.2 to 10% by mass, and even more preferably 0.5 to 5% by mass. If the above film-forming solution contains other components and does not contain hydrophilic inorganic particles, the total content of the other components in the above film-forming solution is preferably 1 to 25% by mass, more preferably 5 to 25% by mass, and even more preferably 7 to 20% by mass.

[0059] In the present invention, when the content of organic polymers, hydrophilic inorganic particles, and other components in the above film-forming solution are set to the above ranges, the permeation amount W 25 and transmission amount W 85 This makes it easier to adjust the transmission amount W to the range defined in the present invention. 25 and transmission amount W 85 This is one of the preferred adjustment methods.

[0060] <Formation of Porous Material by Wet Phase Separation> (Water Vapor Induced Phase Separation) In a preferred method for manufacturing the separator of the present invention, water vapor induced phase separation may be performed on the coated surface (hereinafter also simply referred to as "the coated surface of the laminate") of a laminate comprising a film-forming support, a coating film containing the constituent materials of the separator of the present invention formed on the film-forming support, and a porous support impregnated in the coating film. The laminate can be formed, for example, by casting a film-forming solution obtained by dissolving the organic polymer onto a film-forming support, immersing the porous support in the coating film obtained by casting, impregnating the porous support with the film-forming solution, and appropriately drying the surface to form the coating film.

[0061] In water vapor induction phase separation, it is preferable to use high-temperature, high-humidity water vapor as the poor solvent vapor in the water vapor induction phase separation. The relative humidity in the region where water vapor induction phase separation is performed can be, for example, 50 to 99%, more preferably 60 to 99%, and even more preferably 70 to 99%. The temperature in the region where water vapor induction phase separation is performed is, for example, preferably 55 to 85°C, more preferably 60 to 80°C, and even more preferably 60 to 75°C. The time for performing water vapor induction phase separation is, for example, preferably 1 to 35 seconds, more preferably 1 to 30 seconds, and even more preferably 1 to 25 seconds. The space in which water vapor induction phase separation is performed is not particularly limited in terms of specific adjustment methods, equipment, etc., as long as it can be a space in which the predetermined temperature and humidity are maintained. It is preferable that the space is provided so as to be continuous with the solidification bath in which liquid induction phase separation is performed after water vapor induction phase separation.

[0062] (Liquid Induction Phase Separation) In a preferred method for manufacturing the separator of the present invention, the separator of the present invention can be manufactured by impregnating the laminate that has undergone the above-mentioned water vapor induction phase separation into a solidification bath with the film-forming support still attached, or with the film-forming support removed, and performing liquid induction phase separation. Alternatively, the separator of the present invention can be manufactured by impregnating the laminate described in the above-mentioned water vapor induction phase separation (the laminate before the above-mentioned water vapor induction phase separation) into a solidification bath with the film-forming support still attached, or with the film-forming support removed, and performing liquid induction phase separation. In the present invention, when the laminate that has undergone the above-mentioned water vapor induction phase separation or the laminate described in the above-mentioned water vapor induction phase separation is impregnated into a solidification bath with the film-forming support still attached, and liquid induction phase separation is performed, the permeate amount W 25 and W 85 This makes it easier to adjust the amount W to the range described above. Therefore, the method of performing liquid induction phase separation while the above film-forming support remains stacked is effective for the amount of permeate W. 25 and transmission amount W 85 One preferred method for adjusting the above transmission amount W 25 and W 85 This is one preferred method for manufacturing separators that satisfy the requirements.

[0063] In liquid-induced phase separation, the above-mentioned organic polymer is not dissolved, and a solvent (poor solvent) that is compatible (miscible) with the solvent (good solvent) of the film-forming solution is used as the solidification bath. By immersing the laminate that has undergone the above-mentioned water vapor-induced phase separation, or the laminate described in the above-mentioned water vapor-induced phase separation, in the solidification bath, the proportion of good solvent in the coating film of the film-forming solution decreases, the organic polymer and the solvent undergo phase separation (liquid-induced phase separation), the organic polymer gels (solidifies), a porous material containing the organic polymer is formed, and the separator of the present invention can be obtained.

[0064] In the wet phase separation described above, the poor solvent used in the coagulation bath can be, for example, water, a mixed solvent of water and a hydrophilic organic solvent (an organic solvent miscible with water), a mixed solvent of water and a water-soluble polymer, or a mixed solvent of water, a hydrophilic organic solvent, and a water-soluble polymer. Examples of hydrophilic organic solvents include aprotic solvents such as N-methylpyrrolidone (NMP), dimethylformamide (DMF), dimethyl sulfoxide (DMSO), dimethylacetamide (DMAC), and N,N-dimethylpropionamide, and alcohol solvents such as ethanol, propanol, or isopropanol. Examples of water-soluble polymers include water-soluble polymers such as polyvinylpyrrolidone (PVP) or polyvinyl alcohol (PVA). Among the above, water and a mixed solvent of water and a hydrophilic organic solvent are preferred as the poor solvent, with a permeate amount W. 25 and transmission amount W 85 Water, or a mixed solvent of water and an aprotic solvent, particularly N,N-dimethylpropionamide, is more preferable because it is easier to adjust the concentration within the above range. The amount of water mixed in the mixed solvent can be appropriately determined considering the state of phase separation, and can be, for example, 10 to 90% by mass, and the permeate amount W 25 and transmission amount W 85 In terms of ease of adjustment, especially the transmittance W 25 and transmission amount W 85 In particular, the amount of transmission W 25 It is preferable to use 60 to 90% by mass in order to reduce the amount of permeate W. In the above liquid derivative phase separation, when water is used as the poor solvent, the amount of permeate W is lower than when a mixed solvent is used. 25 and transmission amount W 85 It can be made smaller.

[0065] The temperature of the coagulation bath can be determined as appropriate, and is usually preferably 5 to 90°C, more preferably 20 to 90°C, and even more preferably 40 to 70°C. In the present invention, the amount of permeate W 25 and transmission amount W 85 From the viewpoint of making it easier to adjust within the above range, it is preferable to set the temperature of the coagulation bath to a temperature lower than room temperature (25°C), for example, 5 to 30°C is preferable, 5 to 20°C is more preferable, and 5 to 10°C is even preferable. When the temperature of the coagulation bath is set low, the permeate amount W25 and transmission amount W 85 The amount tends to increase. The time for performing the coagulation bath (coagulation time) is preferably 1 to 15 minutes, more preferably 1 to 12 minutes, and even more preferably 3 to 10 minutes, from the viewpoint of controlling the pore size of the coating film on the film-forming support side. The time for performing the coagulation bath can be appropriately determined within the above range, but the amount of permeation W 25 and transmission amount W 85 From the viewpoint of making it easier to adjust to the above range, 1 to 15 minutes is preferred, and 3 to 10 minutes is more preferred. In liquid induction phase separation, a method using a solidification bath set to the above temperature with a mixed solvent of water and a hydrophilic organic solvent, and a method using a solidification bath set to the above temperature with a mixed solvent of water and a hydrophilic organic solvent for the above solidification time, are used for the permeate amount W 25 and transmission amount W 85 A suitable method for adjusting to each of the ranges defined in this invention is to provide the following.

[0066] In the above liquid-induced phase separation, the laminate may be immersed in the poor solvent to form a porous material (separator), followed by immersion in a glycol such as ethylene glycol or diethylene glycol, and water, or washing with the glycol and water. This step can remove any remaining solvent from the porous material (separator). Various known washing methods can be applied, such as immersion in a washing solution or application (spraying) of a washing solution. The conditions for immersion and washing are not particularly limited and can be determined as appropriate.

[0067] In the separator obtained by the above-described method for manufacturing separators, a certain amount of good solvent from the film-forming solution used in its manufacture inevitably remains. As a result, a separator is provided in which the total content of good solvent in the porous material is 0.01 to 5.00% by mass. The amount of residual solvent is determined by gas chromatography or after pre-drying the separator at 40°C for 12 hours. 1 The amount can be quantified as a mass percentage of 100% by mass of the dried separator using 1H-NMR (nuclear magnetic resonance) measurement.

[0068] In the present invention, the amount of transmission W 25 and transmission amount W 85The method for preparing the material within the range defined in this invention is not particularly limited, and examples include one or more combinations of the types, physical properties, and content of each component, as well as each manufacturing method or manufacturing condition described above. In this combination, the numerical ranges (at least one of the upper and lower limits) indicating the physical properties, content, and manufacturing conditions are not limited to preferred ranges, but can be appropriately adopted as more preferred ranges (at least one of the upper and lower limits), even more preferred ranges (at least one of the upper and lower limits), etc. For example, in this invention, the method of performing wet phase separation with the above-mentioned film-forming support attached is the permeate amount W. 25 and transmission amount W 85 A particularly preferred adjustment method is one that can adjust the amount W to within the range defined in the present invention. In the present invention, in addition to a method of performing wet phase separation with a film-forming support attached, a method that appropriately combines one or more of the above-described adjustment methods is also preferred, as is the amount W 25 and transmission amount W 85 This is a preferred method for adjustment. When the adjustment method to be combined with a method of wet phase separation with a film-forming support attached is specified in a numerical range, the numerical range to be combined is not limited to a preferred range, and a more preferred range (at least one of the upper and lower limits), an even more preferred range (at least one of the upper and lower limits), etc., can be adopted as appropriate.

[0069] [Alkaline Water Electrolysis] The separator of the present invention is used, for example, in alkaline water electrolysis, by being placed between the cathode and the anode. Preferred embodiments of an alkaline water electrolysis apparatus to which the separator of the present invention is applied (also referred to as "the alkaline water electrolysis apparatus of the present invention") will be described, but the alkaline water electrolysis of the present invention is not limited to these embodiments.

[0070] Figure 1 schematically shows a preferred embodiment of the alkaline water electrolysis apparatus of the present invention. In the alkaline water electrolysis apparatus (10) shown in Figure 1, a cathode electrode (12) is arranged on one side of the separator (11) of the present invention, and an anode electrode (13) is arranged on the other side. The separator (11) and each electrode (12, 13) are immersed in a high-concentration alkaline aqueous solution (14, preferably a potassium hydroxide aqueous solution or a sodium hydroxide aqueous solution). When an electric current flows between the electrodes, electrons are supplied to the cathode side, and bubble-like hydrogen (H) is produced from the water. 2 ) occurs (2H 2 O + 2e - →H 2 +2OH - ). Along with the generation of hydrogen, a hydroxyl ion (OH) is produced. - ) passes through the separator (11) and moves to the anode side, where electrons are removed and bubble-shaped oxygen (O 2 ) occurs (4OH - →O 2 +2H 2 O+4e - ). The cathode electrode (12) and anode electrode (13) described above are preferably composed of an electrode substrate (conductive material) and a catalyst layer on the electrode substrate. When a catalyst layer is included, the catalyst species may be the same or different between the cathode electrode (12) and the anode electrode (13). In the alkaline water electrolysis apparatus (10) shown in Figure 1, the separator (11) and each electrode (12, 13) are far apart, so the distance traveled by hydroxyl ions is long, which limits the improvement of ion conduction efficiency.

[0071] Figure 2 schematically shows another preferred embodiment of the alkaline water electrolysis apparatus of the present invention. The alkaline water electrolysis apparatus (20) shown in Figure 2 is a zero-gap type in which the separator (11) and each electrode (12, 13) are arranged in contact with each other in the alkaline water electrolysis apparatus (10) shown in Figure 1. Because the separator (11) and each electrode (12, 13) are in contact in the alkaline water electrolysis apparatus (20) shown in Figure 2, the distance traveled by hydroxyl ions is short, which is advantageous in terms of ion conduction efficiency. In addition, from the viewpoint of imparting suitability for renewable energy, pressurized alkaline water electrolysis apparatuses that are operated under a pressure of 10 bar or more relative to atmospheric pressure (approximately 1 bar) are also known. As an example of such a pressurized alkaline water electrolysis apparatus, an example is the alkaline water electrolysis apparatus shown in Figure 2, in which the configuration, components, etc. of the alkaline water electrolysis apparatus are appropriately adjusted to be able to handle pressurized operation (for example, operation under pressurized conditions of 10 bar or more).

[0072] Figure 3 schematically shows yet another preferred embodiment of the alkaline water electrolysis apparatus of the present invention. The alkaline water electrolysis apparatus (30) shown in Figure 3 is a configuration that includes a membrane electrode assembly. That is, a cathode catalyst layer (32) is arranged on one side of the separator (31) of the present invention, and an anode catalyst layer (33) is arranged on the other side. These catalyst layers are composed of a catalyst and its binder. Furthermore, a gas diffusion layer (34) is formed on the outer surface of these catalyst layers (the surface opposite to the side on which the separator (33) is arranged) to constitute a membrane electrode assembly. In Figure 3, a bipolar plate (35) is formed further outside the membrane electrode assembly. When an alkaline aqueous solution is supplied to the cathode catalyst layer (32) and the anode catalyst layer (33) of this membrane electrode assembly, and the cathode catalyst layer (32) and the anode catalyst layer (33) are electrically connected and current is passed, bubble-like hydrogen is generated from the cathode catalyst layer (32) and bubble-like oxygen is generated from the anode catalyst layer (33).

[0073] In the above-described alkaline water electrolysis apparatus, the components other than the separator, such as the cathode electrode, cathode catalyst layer, anode electrode, and anode catalyst layer, are not particularly limited, and ordinary components used in alkaline water electrolysis apparatuses can be appropriately applied.

[0074] Thus, in one embodiment, the present invention provides an alkaline water electrolysis apparatus in which the separator of the present invention is incorporated as a separator in the alkaline water electrolysis apparatus. Furthermore, in one embodiment, the present invention provides a method for manufacturing an alkaline water electrolysis apparatus, which includes incorporating the separator of the present invention as a separator in the alkaline water electrolysis apparatus.

[0075] [Alkaline Water Electrolysis Member] The alkaline water electrolysis member of the present invention includes the separator of the present invention. Specifically, the alkaline water electrolysis member of the present invention includes the separator of the present invention and at least one of a catalyst, an anode electrode, and a cathode electrode. The form including the separator of the present invention, an anode electrode, and a cathode electrode will be classified as the alkaline water electrolysis cell of the present invention, as described later. Forms in which the alkaline water electrolysis member of the present invention does not include an electrode but includes a catalyst include a form in which the catalyst is located on only one side of the separator of the present invention, and a form in which the catalyst is located on both sides of the separator of the present invention. Forms in which the alkaline water electrolysis member of the present invention does not include a cathode electrode but includes an anode electrode include a form in which the anode electrode is located on one side of the separator of the present invention. In this form, the catalyst may or may not be present. If a catalyst is present, the catalyst may be located on only one side of the separator of the present invention, or the catalyst may be located on both sides of the separator of the present invention. In the present invention, an alkaline water electrolytic member does not include an anode electrode but includes a cathode electrode. This configuration includes having a cathode electrode on one side of the separator. In this configuration, a catalyst may or may not be present. If a catalyst is present, the catalyst may be present on only one side of the separator, or on both sides of the separator.

[0076] [Alkaline Water Electrolysis Cell] The alkaline water electrolysis cell of the present invention includes the separator of the present invention or the alkaline water electrolysis component of the present invention. The "alkaline water electrolysis cell" includes the separator and two electrodes separated by the separator (anode electrode and cathode electrode). In this embodiment, an alkaline aqueous solution may be present as an electrolyte between both electrodes (including the separator of the present invention), and the anode electrode and cathode electrode may each further contain a catalyst. For example, if the alkaline water electrolysis cell of the present invention includes the separator of the present invention, the alkaline water electrolysis cell of the present invention can be made by combining the separator of the present invention with the anode electrode and cathode electrode. In this case, the anode electrode and cathode electrode may each independently contain a catalyst. Also, if the alkaline water electrolysis cell of the present invention does not include electrodes and includes the separator and catalyst of the present invention, the alkaline water electrolysis cell of the present invention can be made by combining them with the anode electrode and cathode electrode. In this case, the catalyst may be included in the alkaline water electrolytic member of the present invention, or it may be included separately in combination with the alkaline water electrolytic member of the present invention, similar to the anode electrode or cathode electrode. In the alkaline water electrolytic cell of the present invention, the catalyst may be included on at least one side of the separator of the present invention, or it may be included on both sides. Furthermore, if the alkaline water electrolytic cell of the present invention does not include a cathode electrode but includes the separator and anode electrode of the present invention, it can be made into the alkaline water electrolytic cell of the present invention by combining it with a cathode electrode. In this case, the anode electrode and cathode electrode may each independently contain the catalyst. Furthermore, the catalyst may be included in the alkaline water electrolytic member of the present invention, or it may be included separately in combination with the alkaline water electrolytic member of the present invention, similar to the cathode electrode. Furthermore, if the alkaline water electrolytic cell of the present invention does not include an anode electrode but includes the separator and cathode electrode of the present invention, it can be made into the alkaline water electrolytic cell of the present invention by combining it with an anode electrode. In this case, the anode electrode and cathode electrode may each independently contain the catalyst.Furthermore, the catalyst may be included in the alkaline water electrolytic member of the present invention, or it may be included separately in combination with the alkaline water electrolytic member of the present invention, similar to the anode electrode.

[0077] [Method for Producing Hydrogen] The method for producing hydrogen according to the present invention is the same as a conventional method for producing hydrogen (water electrolysis), except that it includes electrolysis of water using the alkaline water electrolysis apparatus of the present invention. In particular, a preferred method for producing hydrogen according to the present invention is one which includes using an alkaline aqueous solution containing 10 to 35% by mass of a metal hydroxide as the electrolyte solution and electrolyzing water at 70 to 95°C. Examples of metal hydroxides include sodium hydroxide and potassium hydroxide, and potassium hydroxide is preferred from the viewpoint of having a higher specific conductivity of the aqueous solution of the metal hydroxide. The content of the metal hydroxide (electrolyte) in the alkaline aqueous solution is preferably 10 to 35% by mass, more preferably 25 to 35% by mass, and even more preferably 28 to 32% by mass. The temperature of the alkaline aqueous solution used when operating the alkaline water electrolysis apparatus and producing hydrogen by electrolyzing water is preferably 70 to 95°C, more preferably 70 to 90°C. This temperature may also be 75 to 85°C or 78 to 82°C. Thus, the separator of the present invention can be suitably used in the method for producing hydrogen according to the present invention, which uses a high-temperature, high-concentration alkaline aqueous solution, by utilizing its high alkali durability. The hydrogen production method of the present invention, using the separator of the present invention, utilizes the high alkali durability exhibited by the separator of the present invention to enable hydrogen production by alkaline water electrolysis over a long period of time, for example, while maintaining hydrogen production efficiency.

[0078] The present invention will be described in more detail below based on examples, but the present invention is not to be construed as being limited thereto. The water used is deionized water. "h" represents time.

[0079] [Example 1] 8.5 g of polysulfone (trade name: Udel P-3500 LCD MB7, Mw: approximately 80,000, manufactured by Solvay) was added to 20.6 g of γ-valerolactone (manufactured by Fujifilm Wako Pure Chemical Industries) and 20.6 g of PolarClean (a mixture of the above compound (2) and compound (3), with a mixing ratio (mass ratio) of compound (2) / compound (3) = 95 / 5, manufactured by Solvay), and stirred at 60°C for 5 hours to completely dissolve. Next, 2.4 g of PVP K90 (trade name: polyvinylpyrrolidone, manufactured by Fujifilm Wako Pure Chemical Industries) as an additive was added, and after stirring at 60°C for 1 hour, ZrO 2 47.9 g of particles (E101, particle size (D50) 0.80 μm, manufactured by Lufer) were added and stirred for a further 3 hours to obtain a coating solution for film formation. The obtained coating solution was cast onto a PET (polyethylene terephthalate) film using an applicator set to a clearance of 250 μm. A woven fabric made of polyether ether ketone (PEEK) (product name: PEEKTEX, thickness 100 μm, manufactured by Sefar) was placed on top of the cast coating solution as a porous support, and the fabric was completely impregnated with the coating solution. Subsequently, it was gently immersed in a condensation bath cooled to 10°C (a mixture of 90% by mass of dimethylpropionamide and 10% by mass of pure water) and left immersed for 5 minutes (solidification time) to form a porous polysulfone structure (referred to as "PSU porous structure") (phase separation step in the condensation bath). The PET film was then washed with water at 50°C for 10 minutes, and the woven fabric and the PSU porous structure were peeled off together. Subsequently, it was washed with water at 90°C for 1 hour to obtain the separator of Example 1.

[0080] [Example 2] The separator of Example 2 was obtained in the same manner as in Example 1, except that dimethylpropionamide (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the solvent for the coating solution instead of γ-valerolactone and PolarClean.

[0081] [Example 3] The separator of Example 3 was obtained in the same manner as in Example 2, except that polysulfone (product name: Udel P-1700, Mw: approximately 60,000, manufactured by Solvay) was used instead of polysulfone (product name: Udel P-3500 LCD MB7).

[0082] [Example 4] The separator of Example 4 was obtained in the same manner as in Example 2, except that N-butyl-2-pyrrolidone (manufactured by Tokyo Chemical Industry Co., Ltd.) was used as the solvent for the coating solution instead of dimethylpropionamide, and a woven fabric made of polyphenylene sulfide (PPS) (product name: PPS0113 / 45PW, thickness 100 μm, manufactured by NBC Meshtec Co., Ltd.) was used as the porous support instead of the above woven fabric (PEEKTEX).

[0083] [Example 5] The separator of Example 5 was obtained in the same manner as in Example 4, except that the clearance of the applicator during casting of the coating solution was changed to 300 μm and the condensation bath was changed to a mixture of 10% by mass of dimethylpropionamide and 90% by mass of pure water.

[0084] [Example 6] The separator of Example 6 was obtained in the same manner as in Example 4, except that Glycerol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used instead of PVP K90 as an additive, and the clearance of the applicator during casting of the coating solution was changed to 600 μm.

[0085] [Comparative Example 1] A coating solution was prepared in the same manner as in Example 1, except that N-butylpyrrolidone was replaced with γ-valerolactone and PolarClean as solvents. Next, the coating solution cast using a comma coater set to a clearance of 250 μm was impregnated into a PPS woven fabric (product name: PPS177 / 70PW, manufactured by NBC Meshtec Co., Ltd.), and then immersed in pure water at 65°C for 1 minute to form a porous polysulfone structure. After that, it was washed with water at 70°C for 10 minutes and peeled off from the PET film to obtain the separator of Comparative Example 1.

[0086] [Comparative Example 2] 13.3 g of polysulfone (product name: Udel P-1700, manufactured by Solvay) was added to 47 g of N-butylpyrrolidone and stirred at 60°C for 5 hours until completely dissolved. Then, TiO 240 g of particles (product name: R101, manufactured by Chemars) were added and stirred for 3 hours to obtain a coating solution. The obtained coating solution was impregnated into a PPS woven fabric (product name: PPS113 / 45PW, manufactured by NBC Meshtec) using a comma coater set to a clearance of 350 μm, and then immersed in 65°C pure water for 1 minute to form a porous polysulfone structure. After that, it was further washed with water at 70°C for 10 minutes to obtain the separator of Comparative Example 2.

[0087] [Evaluation of Separators] The following measurements and evaluations were performed on each separator fabricated as described above. The results are shown in Table 1. Unless otherwise specified, the separators used for each evaluation were those that had been cut to the desired shape for the evaluation described later.

[0088] <Separator Thickness> A cross-sectional SEM (scanning electron microscope) image was acquired of a cross-section cut from the separator with a razor blade at a magnification (e.g., 200x) that allowed the entire separator cross-section to fit in a single field of view. Assuming that no pores exist in the obtained cross-sectional SEM image (assuming that the pores are filled with organic polymer), the thickness was measured at 20 equally spaced points. The arithmetic mean of the 20 obtained measurements was calculated and rounded to the first decimal place in μm, and this value is shown in Table 1 as the separator thickness. The following equipment was used for cross-sectional SEM observation. Conductive processing device: Meiwa Forsis Co., Ltd., Model: HPC-1SW osmium coater / Source: Os / Thickness: 5 nm CIS device: JEOL Ltd., Model: IB-09060CIS / Acceleration voltage: 4 kV / Processing temperature: -130°C / Pre-treatment The sample cut with a razor blade was attached to a Si wafer (100 μm thick) with epoxy resin and fixed. FE-SEM (Field Emission Scanning Electron Microscope) observation system: Carl Zeiss, Model: Ultra5, Measurement conditions: Secondary / backscattered electron image, Acceleration voltage 2kV, Aperture 30μm, Working distance 3.0mm (cross-section)

[0089] <Permeation amount W of 30% by mass KOH aqueous solution 25 and W 85> Each separator was cut into a circular shape with a diameter of 47 mm, and sample 4 was set in the alkaline water permeability measuring device shown in the schematic cross-sectional view of Figure 4. Specifically, the stainless steel mesh support 5 and sample 4 were placed on the lower part of the sample holder 2 in that order, and the upper part of the sample holder 1 was placed on top of it with a rubber O-ring packing 3 in between, and sample 4 was fixed by the lower part of the sample holder 2 and the upper part of the sample holder 1. A 30% by mass potassium hydroxide aqueous solution adjusted to 25°C or a 30% by mass potassium hydroxide aqueous solution heated to 85°C was supplied from above the sample (the location indicated by the arrow in Figure 4), and a pressure of 50 mbar was applied. The point at which droplets were visually confirmed to come out from the bottom of the sample was defined as 0 minutes, and the pressure was maintained for 8 minutes. The amount of potassium hydroxide aqueous solution that permeated the sample in 8 minutes was quantified, and the permeability of the KOH aqueous solution was calculated by unit conversion. The permeability when using a 30% by mass potassium hydroxide aqueous solution adjusted to 25°C was defined as permeability W. 25 (L / bar / h / m 2 The amount of permeation when using a 30% potassium hydroxide aqueous solution heated to 85°C is the amount of permeation W. 85 (L / bar / h / m 2 The results obtained are shown in Table 1. Note that the transmission amount W 25 and W 85 In the measurement, the thickness of sample 4 was set to be the same as the thickness of each separator manufactured in the examples and comparative examples.

[0090] <Evaluation of Alkali Durability> First, durability tests were conducted on each separator manufactured in the examples and comparative examples, and samples were obtained after the durability tests. Specifically, each separator manufactured in the examples and comparative examples was set in a sample holder so that they did not come into contact with each other, and the sample holder was placed in an autoclave and immersed in 30% KOH set at 120°C. In this immersion state, oxygen was bubbled at a rate of 20 mL / min, and back pressure was applied to achieve a pressure of 5 bar, and the samples were left standing for 3 months (durability test). The permeate amount W of each sample obtained after the durability test was measured when using a 30% KOH aqueous solution at 85°C. 85A (L / bar / h / m 2 ) the amount of permeation W of the above-mentioned <30% by mass KOH aqueous solution 25and W 85 >Measurements and calculations were performed in the same manner. For each sample, the calculated transmission amount W was... 85A and the amount of permeation W of the above-mentioned <30% by mass KOH aqueous solution 25 and W 85 > The amount of transmission W calculated 85 The rate of increase in permeation was calculated using the following formula and applied to the evaluation criteria below to assess alkali durability. The results are shown in Table 1. Rate of increase in permeation (%) = ((Permeation W) 85A / Transmission amount W 85 ) - 1) × 100 - Evaluation Criteria - S: The rate of increase in transmission is less than 30%. A: The rate of increase in transmission is 30% or more and less than 50%. B: The rate of increase in transmission is 50% or more and less than 200%. C: The rate of increase in transmission is 200% or more and less than 500%. D: The rate of increase in transmission is 500% or more.

[0091]

[0092] From the results shown in Table 1 above, the permeate amount W of a 30 mass% KOH aqueous solution at 25°C is 25 and the amount of permeation W of a 30% by mass KOH aqueous solution at 85°C 85 It was found that if both of the following do not meet the range defined in this invention, the rate of increase in permeate before and after alkali durability becomes large, and sufficient alkali durability is not observed when used in alkaline water electrolysis. Specifically, permeate amount W 25 The separator in Comparative Example 1 has a transmission amount W that is too large. 85 Even when the conditions were met, it did not show sufficient alkali resistance. On the other hand, the permeate amount W 85 The separator in Comparative Example 2, which is too small, has a transmittance of W. 25 Even when the conditions were met, it did not show sufficient alkali resistance. In contrast, the permeate amount W 25 and transmission amount W 85 In all of the separators of Examples 1 to 6, which satisfy both of the ranges defined in the present invention, the increase in permeation before and after alkali durability was suppressed, and it was found that they exhibit sufficient alkali durability when used in alkaline water electrolysis. In particular, separators having a thickness of 200 μm or less and with a permeation rate W 25 and transmission amount W 85The separators of Examples 1 to 4, which satisfy both of the parameters defined in this invention, were found to exhibit excellent alkali resistance.

[0093] Although we have described the present invention along with its embodiments, we do not intend to limit our invention in any detail of the description unless specifically designated, and we believe that it should be interpreted broadly without contradicting the spirit and scope of the invention as set forth in the appended claims.

[0094] This application claims priority based on Japanese Patent Application No. 2025-078743, filed in Japan on 9 May 2025, the contents of which are incorporated herein by reference as part of this specification.

[0095] 1. Sample holder upper part 2. Sample holder lower part 3. Rubber O-ring packing 4. Sample 5. Stainless steel mesh support 10. Alkaline water electrolysis device 11. Separator 12. Cathode electrode 13. Anode electrode 14. Alkaline aqueous solution 20. Alkaline water electrolysis device 30. Alkaline water electrolysis device 31. Separator 32. Cathode catalyst layer 33. Anode catalyst layer 34. Gas diffusion layer 35. Bipolar plate O 2 Bubble-shaped oxygen H 2 Bubble-shaped hydrogen OH - Hydroxy ion e - electronic

Claims

1. A porous separator for water electrolysis comprising a porous support and an organic polymer, wherein the permeability of a 30% potassium hydroxide aqueous solution at 25°C is 250 L / bar / h / m 2 The following conditions apply, and the permeate rate of a 30% potassium hydroxide aqueous solution at 85°C is 400 L / bar / h / m². 2 That concludes the description of the porous separator for water electrolysis.

2. The porous separator for water electrolysis according to claim 1, wherein the ratio of the amount of permeation of a 30% potassium hydroxide aqueous solution at 85°C to the amount of permeation of a 30% potassium hydroxide aqueous solution at 25°C is 3.0 or more.

3. The porous separator for water electrolysis according to claim 1, wherein the ratio of the amount of permeation of a 30% potassium hydroxide aqueous solution at 85°C to the amount of permeation of a 30% potassium hydroxide aqueous solution at 25°C is 5.0 or more.

4. The porous separator for water electrolysis according to claim 1, wherein the thickness is 220 μm or less.

5. An alkaline water electrolysis member comprising the porous separator for water electrolysis described in claim 1.

6. An alkaline water electrolysis cell comprising a porous separator for water electrolysis according to any one of claims 1 to 4, or an alkaline water electrolysis member according to claim 5.

7. An alkaline water electrolysis apparatus comprising the alkaline water electrolysis cell described in claim 6.

8. A method for producing hydrogen, comprising electrolyzing water using the alkaline water electrolysis apparatus described in claim 7.

9. A method for producing hydrogen according to claim 8, comprising using an alkaline aqueous solution containing 10 to 35% by mass of a metal hydroxide as an electrolyte solution, and electrolyzing water at 70 to 95°C.