Method for manufacturing additively-manufactured article, and additive manufacturing system
By integrating a nozzle portion with the layered modeled article and using a masking member, the method addresses the challenge of processing complex shapes, ensuring comprehensive surface treatment of layered modeled articles.
Patent Information
- Application Number
- PCT/JP2026/017477
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-04-07
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for manufacturing layered modeled articles face challenges in handling nozzles due to complex shapes, particularly in internal spaces, leading to restricted ejection directions and difficulty in processing hard-to-reach areas.
Integrating a nozzle portion with the layered modeled article during manufacturing, allowing for fluid ejection from a connected processing apparatus to reach otherwise inaccessible areas, and optionally incorporating a masking member to shield or reflect the fluid.
Enables effective processing of complexly shaped articles by ensuring fluid can be applied to all surfaces, including internal spaces, without altering the article's functionality or design.
Smart Images

Figure JP2026017477_12112026_PF_FP_ABST
Abstract
Description
Method for manufacturing layered modeled article, and layered modeling system
[0001] The present disclosure relates to a method for manufacturing a layered modeled article, and a layered modeling system.
[0002] Patent Document 1 discloses a method for treating the surface of an additively manufactured layered modeled article. In this method, a blast processing apparatus having a nozzle is used. The nozzle ejects media together with air onto the surface of the layered modeled article. As a result, the surface of the layered modeled article is smoothed.
[0003] JP 2022-136707 A
[0004] When a layered modeled article is manufactured using a processing apparatus having a nozzle as in the method described in Patent Document 1, the handling of the nozzle may be restricted due to the complex shape of the layered modeled article. For example, in the case of a layered modeled article having an internal space, it may be difficult to arrange the nozzle in the internal space. Even if the nozzle could be arranged in the internal space, the ejection direction of the nozzle may be restricted. The present disclosure provides a technique that can appropriately manufacture a layered modeled article.
[0005] A method for manufacturing a layered modeled article according to one aspect of the present disclosure includes the following steps. (1) A step of modeling a layered modeled object in which a layered modeled article and a nozzle portion connectable to a processing apparatus are integrated. (2) A step of connecting the processing apparatus to the nozzle portion included in the layered modeled object, and ejecting a fluid from the nozzle portion to the layered modeled article.
[0006] A layered modeling system according to another aspect of the present disclosure includes an additive manufacturing apparatus, a processing apparatus, and a control unit. The additive manufacturing apparatus models a layered modeled object. The processing apparatus is connectable to the nozzle portion. The control unit controls the additive manufacturing apparatus and the processing apparatus. The control unit causes the additive manufacturing apparatus to model a layered modeled object in which a layered modeled article and a nozzle portion are integrated, causes the processing apparatus to connect to the nozzle portion included in the layered modeled object, and causes a fluid to be ejected from the nozzle portion to the layered modeled article.
[0007] According to the present disclosure, a layered modeled article can be appropriately manufactured.
[0008] Figure 1 is a flowchart showing an example of a method for manufacturing additively manufactured products. Figure 2 is a block diagram showing an example of the configuration of an additive manufacturing system. Figure 3 is a schematic diagram showing an example of the configuration of an additive manufacturing apparatus. Figure 4 is a schematic diagram showing an example of the configuration of a processing apparatus. Figure 5(A) is a cross-sectional view showing an example of the configuration of a direct-pressure nozzle, and Figure 5(B) is a cross-sectional view showing an example of the configuration of a suction-type nozzle. Figure 6(A) is an example of an additively manufactured product, and Figure 6(B) is an example of an additively manufactured object. Figure 7(A) is a schematic diagram showing an example of blast processing an additively manufactured product from the outside, and Figure 7(B) is a schematic diagram showing an example of blast processing an additively manufactured product using a layered nozzle. Figure 8(A) is a cross-sectional view showing an example of a nozzle, and Figure 8(B) is a cross-sectional view showing another example of a nozzle. Figure 9(A) is a longitudinal section view showing an example of a nozzle attachment, Figure 9(B) is a longitudinal section view showing another example of a nozzle attachment, Figure 9(C) is a longitudinal section view showing yet another example of a nozzle attachment, Figure 9(D) is a longitudinal section view showing yet another example of a nozzle, and Figure 9(E) is a longitudinal section view showing yet another example of a nozzle.
[0009] Embodiments of the present disclosure will be described in detail below with reference to the drawings. In the description of the drawings, identical elements are denoted by the same reference numerals, and redundant descriptions are omitted. The dimensional ratios in the drawings do not necessarily correspond to those described. The terms "top," "bottom," "left," and "right" are based on the illustrated state and are for convenience only.
[0010] (Overview of the manufacturing method of additively manufactured products) Figure 1 is a flowchart showing an example of a manufacturing method for additively manufactured products. Additively manufactured products are three-dimensional products obtained by stacking two-dimensional layers. As shown in Figure 1, the molding process is carried out as step S10. The molding process is carried out by an additive manufacturing apparatus of an additive manufacturing system described later. The additive manufacturing apparatus sintersects or melts and solidifies raw materials to form the cross-section of the molded object, and obtains an additively manufactured product by forming the cross-section of the molded object layer by layer and stacking them. An additively manufactured product is an object obtained by stacking layers, and the part of the additively manufactured product that becomes the finished product is called an additively manufactured product.
[0011] The additively manufactured object includes the additively manufactured product and the nozzle part of the processing device described later. The additively manufactured object is an integrated object (one-piece) in which the additively manufactured product and the nozzle part of the processing device are combined. The processing device is a device that sprays a fluid from the nozzle onto the surface of the object. The processing of the processing device may include, for example, smoothing, defect treatment (sealing by plastic deformation), microcrack removal, support material removal, film formation, or painting. Support material is a component that is manufactured together with the additively manufactured product to support the additively manufactured product, and may be a base or scaffolding. Support material is removed from the surface of the additively manufactured product during or after manufacturing. The fluid may be a gas or a liquid, and may include media, raw materials, or paints.
[0012] The nozzle section constitutes part or all of the nozzle of the processing device and is a component that can be attached to or removed from the processing device. The nozzle section only needs to include at least the tip of the nozzle and may also include components of the processing device other than the nozzle. The nozzle section is provided near areas of the additively manufactured product where the jet from the nozzle is difficult to reach. For example, the nozzle section is provided so that fluid can be injected into narrow or obstructed areas of the additively manufactured product.
[0013] Next, as step S12, a processing step is carried out. The processing step is performed by the processing device of the additive manufacturing system described later. First, the processing device is connected to the nozzle section created in step S10. Next, fluid is injected from the nozzle section into the additive manufactured product. Since the nozzle section can inject fluid into narrow or obstructed parts of the additive manufactured product, parts that cannot be reached by the jet stream from the nozzle attached to the processing device are processed, for example.
[0014] Next, as step S14, a removal process is carried out. The removal process may be carried out by the processing equipment used in step S12, by other equipment, or by an operator. In the removal process, for example, the nozzle part is removed from the additively manufactured product by blasting. When step S14 is completed, the flowchart shown in Figure 1 is completed, and the additively manufactured product is obtained.
[0015] (Overview of the Additive Manufacturing System) The additive manufacturing system that executes the flowchart shown in Figure 1 will be described below. Figure 2 is a block diagram showing an example of the configuration of the additive manufacturing system. As shown in Figure 2, the additive manufacturing system 1 comprises an additive manufacturing device 2, a processing device 3, and a controller 4 (an example of a control unit). The additive manufacturing device 2 is a device that builds an additively manufactured object by stacking multiple layers. The additively manufactured object built by the additive manufacturing device 2 is transported to the processing device 3. The processing device 3 is a device that processes the surface of the additively manufactured object.
[0016] Controller 4 is hardware that controls the entire additive manufacturing system 1. Controller 4 is composed of a general-purpose computer having, for example, a computing unit such as a CPU (Central Processing Unit), a storage device such as ROM (Read Only Memory), RAM (Random Access Memory), and HDD (Hard Disk Drive), and a communication device. Controller 4 may also be composed of a PLC (Programmable Logic Controller). Controller 4 is configured to communicate with the additive manufacturing apparatus 2 and the processing apparatus 3, and controls the operation of the additive manufacturing apparatus 2 and the processing apparatus 3.
[0017] The additive manufacturing system 1 may include a transport device 5. The transport device 5 is controlled by, for example, a controller 4, and transports the additively manufactured object from the additive manufacturing device 2 to the processing device 3. The transport device 5 is composed of, for example, a robot.
[0018] (Example of an additive manufacturing apparatus) Figure 3 is a schematic diagram showing an example of the configuration of an additive manufacturing apparatus. In the figure, the X and Y directions are horizontal, and the Z direction is vertical. Hereafter, the Z direction will also be referred to as the up and down direction. The additive manufacturing apparatus 2 forms three-dimensional objects. The additive manufacturing apparatus 2 forms additively manufactured objects based on, for example, three-dimensional CAD data. The three-dimensional CAD data includes data on the cross-sectional shape of each layer. The additive manufacturing apparatus 2 forms the cross-section of the additively manufactured object layer by layer based on the cross-sectional shape data.
[0019] The additive manufacturing apparatus 2 forms layers by irradiating raw materials, for example, an ultraviolet-curable resin and ceramic particles, with ultraviolet light. The ultraviolet-curable resin is a synthetic organic material that absorbs light of ultraviolet wavelengths and changes into a solid. The additive manufacturing apparatus 2 comprises a layer forming unit 20, a stage mechanism 21, and a raw material supply unit 22. The layer forming unit 20 is a component for forming layers. The stage mechanism 21 comprises a base 28. The layer forming unit 20 forms a layer of hardened raw materials by irradiating the raw materials on the base 28 with light.
[0020] The layer-forming section 20 includes, for example, an optical unit 23, light-reflecting members 24 and 26, and rotational drive sections 25 and 27. The optical unit 23 includes, for example, a light source 23a and an optical member 23b, and emits an ultraviolet laser L. The light-reflecting members 24 and 26 are, for example, carvano mirrors, and change the optical path of the ultraviolet laser L emitted from the optical unit 23.
[0021] The light-reflecting members 24 and 26 rotate around a predetermined axis of rotation by the rotation drive units 25 and 27. By controlling the rotation of the light-reflecting members 24 and 26, the layer-forming unit 20 can irradiate the ultraviolet laser L to a predetermined horizontal position at the layer-forming height position. The layer-forming height position is a height predetermined as the height at which the ultraviolet laser L is irradiated.
[0022] When the ultraviolet laser L is irradiated, the ultraviolet-curable resin contained in the raw material hardens, so that only the part irradiated by the ultraviolet laser L is formed as a layer. The layer-forming unit 20 irradiates the ultraviolet laser L to reproduce the cross-sectional shape based on the CAD data and forms one layer of the cross-section of the fabricated object.
[0023] The raw material supply unit 22 supplies raw materials onto the base 28. The raw material supply unit 22 supplies raw materials, for example, while moving horizontally. The raw material supply unit 22 includes, as an example, a head for supplying raw materials and a blade for leveling the supplied raw materials. The raw materials supplied from the head are leveled by the blade, thereby supplying one layer of raw materials onto the base 28.
[0024] The base 28 moves up and down relative to the layer forming section 20. As an example, the stage mechanism 21 includes a drive unit 29. The drive unit 29 is connected to the base 28 and moves the base 28 up and down. The drive unit 29 is, for example, an electric cylinder. The drive unit 29 moves the base 28 up and down in units of the height of one layer.
[0025] (Example of a processing device) Figure 4 is a schematic diagram showing an example of the configuration of a processing device. The processing device 3 shown in Figure 4 is a device that sprays a fixed amount of abrasive material M1 (an example of media) supplied by a supply device 30 together with gas. The processing device 3 performs blast processing, such as removing surface roughness, by spraying the abrasive material M1 onto the additively manufactured object LO. The spraying method of the processing device 3 is, for example, a direct pressure sandblasting method.
[0026] The abrasive material M1 is selected from metals, non-ferrous metals, glass, ceramics, resins, plant seeds, etc., depending on the physical properties of the additively manufactured object LO or the purpose of blasting. When dry ice particles are selected as the abrasive material M1, contamination due to residual abrasive material M1 is suppressed.
[0027] The processing apparatus 3 includes, for example, a supply device 30, a processing unit 31, a classifier 32, and a dust collector 33. The processing apparatus 3 sprays a mixed fluid of abrasive material M1 and compressed air supplied via the supply device 30 onto the additively manufactured object LO in the processing unit 31 to perform blast processing.
[0028] The processing unit 31 includes a case 34, a nozzle 35, a processing table 36, a nozzle drive unit 37, and a conveyor drive unit 38. The case 34 has an upper case 39 and a lower case 40. The case 34 has a processing chamber 41 inside. The nozzle 35 and the processing table 36 are arranged in the processing chamber 41.
[0029] The nozzle 35 is positioned, for example, at the top of the processing chamber 41 of the upper case 39. The nozzle 35 sprays abrasive material M1 together with compressed air. The nozzle 35 is, for example, a blast nozzle for direct-pressure sandblasting. The processing table 36 is a table on which the additively manufactured object LO is placed. The nozzle drive unit 37 moves the nozzle 35 so that the spraying area of the abrasive material M1 moves. The conveyor drive unit 38 moves the processing table 36 to move the additively manufactured object LO to the spraying area of the abrasive material M1.
[0030] A passing plate 42 is provided between the upper case 39 and the lower case 40. The passing plate 42 has multiple openings through which used abrasive material M1 and cutting dust can pass towards the bottom. A classifier 32 and a dust collector 33 are connected to the lower end of the lower case 40 via piping.
[0031] The dust collector 33 has a suction power source and a filter (not shown). By activating the suction power source, an airflow is generated in the processing chamber 41 and the classifier 32 toward the dust collector 33. The used abrasive material M1 and cutting chips fall to the lower end of the lower case 40, are collected as abrasive material M2, and are transported to the classifier 32 by the airflow from the dust collector 33. In the classifier 32, the abrasive material M2 is classified into reusable abrasive material M1 and the remaining powder. The classifier 32 is, for example, a cyclone. The unreusable abrasive material M1 is transported to the tank 43, and the remaining powder is transported to the dust collector 33 and collected.
[0032] The abrasive material M1 in the tank 43 is supplied to the nozzle 35 by the supply device 30. The supply device 30 has a roller 45 inside its main body 44. Grooves are formed on the outer surface of the roller 45. The inside of the tank 43 is pressurized by a pressurizing conduit 46, and the pressure fills the grooves on the outer surface of the roller 45 with the abrasive material M1 inside the tank 43. A fixed amount of abrasive material M1 is supplied to the nozzle 35 by blowing away the abrasive material M1 filled in the grooves with compressed air. The compressed air is supplied from an air supply source 47 and an auxiliary air supply source 48. The air supply source 47 and the auxiliary air supply source 48 are, for example, compressors.
[0033] Figure 5(A) is a cross-sectional view showing an example of the configuration of a direct-pressure nozzle. As shown in Figure 5(A), the nozzle 35 comprises a first nozzle body 35a and a nozzle attachment 35b (an example of a nozzle part). The first nozzle body 35a is a hollow cylindrical member, to which a supply pipe is connected, and an abrasive material M1 is supplied together with fluid through the supply pipe. The supply pipe is not particularly limited as long as it is configured to be detachably attached to the first nozzle body 35a, for example, a resin hose. A detachable nozzle attachment 35b is attached to the tip of the first nozzle body 35a.
[0034] The nozzle portion described in step S10 of Figure 1 is not particularly limited as long as the processing device 3 can be connected to it. For example, the nozzle portion may be the entire nozzle attachment 35b or a part of the nozzle attachment 35b. Alternatively, the nozzle portion may be the entire nozzle attachment 35b and a part or all of the first nozzle body 35a. Or, the nozzle portion may be the nozzle 35 and a part of the supply piping.
[0035] The blasting method of the processing device 3 may be a suction-type sandblasting method. In this case, a blast nozzle for suction-type sandblasting is used. Figure 5(B) is a cross-sectional view showing an example of the configuration of a suction-type nozzle. As shown in Figure 5(B), the nozzle 35A comprises a second nozzle body 35c and a nozzle attachment 35b (an example of a nozzle part). The nozzle 35A differs from the nozzle 35 in the structure of its body, but is otherwise identical.
[0036] The second nozzle body 35c is a hollow cylindrical member, and like the nozzle 35, a supply pipe is connected to its end, and the abrasive material M1 is supplied along with the fluid through the supply pipe. The second nozzle body 35c has a passage through which compressed air 49 for extraction is supplied. When compressed air 49 is supplied, the abrasive material M1 is supplied to the second nozzle body 35c by the suction negative pressure caused by the ejector phenomenon that occurs inside the second nozzle body 35c. In the case of a suction type, the processing device 3 does not need to be equipped with a pressurizing conduit 46.
[0037] (Examples of additively manufactured objects and additively manufactured products) Figure 6(A) is an example of an additively manufactured product, and Figure 6(B) is an example of an additively manufactured object. As shown in Figure 6(A), the additively manufactured product LP is a box-shaped product with a hollow internal space and a complex structure in which beam members exist within the internal space. As shown in Figure 6(B), the additively manufactured product LO has not only the additively manufactured product LP but also a nozzle attachment 35b (an example of a nozzle part) as an integrated unit.
[0038] Figure 7(A) is a schematic diagram showing an example of blast processing an additively manufactured product from the outside. The internal structure of the additively manufactured product LP is complex, and the nozzle 35 cannot be inserted inside the additively manufactured product LP. Also, as shown in Figure 7(A), even if the abrasive material M1 is sprayed from the outside of the additively manufactured product, the area TA to be processed cannot be processed. In contrast, as shown in Figure 7(B), by integrally manufacturing the nozzle attachment 35b with the additively manufactured product LP, the area TA to be processed can be processed simply by connecting the processing device 3 to the nozzle attachment 35b and spraying.
[0039] The nozzle attachment 35b shown in Figure 7(B) is removed in the removal process shown in step S14 of Figure 1. Although the nozzle attachment 35b is for spraying to areas that are difficult for the jet to reach, it is installed in a location that is as easy to remove as possible. For example, the nozzle attachment 35b is installed in a location that is easily reached by the jet or in a location that is easily accessible by a hand tool. In addition, the size or shape of the part connecting the nozzle attachment 35b to the additively manufactured product LP is adjusted so that it can be easily broken or shaved.
[0040] Furthermore, as shown in Figure 7(B), if there is an area TB that is not actively processed, a masking member 50 (an example of a structure) may be fabricated. The masking member 50 is fabricated together with the additively manufactured product LP, similar to the nozzle attachment 35b. The masking member 50 reflects or shields the abrasive material M1 and air sprayed from the nozzle attachment 35b. By using the masking member 50, processing in area TB can be avoided.
[0041] The masking member 50 is removed in the removal step shown in step S14 of FIG. 1. The masking member 50 is provided at a location where it can be removed as easily as possible. The masking member 50 is provided, for example, at a location easily reachable by a jet flow or a location easily reachable by a hand tool. Further, the portion connecting the masking member 50 and the additively manufactured product LP may be a thin plate member.
[0042] (Summary of Embodiments) According to the method for manufacturing the additively manufactured product LP and the additive manufacturing system 1, the additively manufactured object LO in which the additively manufactured product LP and the nozzle attachment 35b are integrated is fabricated, and a fluid is jetted from the nozzle attachment 35b to the additively manufactured product LP. By fabricating the integrated object of the additively manufactured product LP and the nozzle attachment 35b, it is possible to appropriately jet the fluid to the surface even at locations that are difficult for the jet flow to reach with the nozzle provided in the processing apparatus 3, or locations where media cannot be jetted onto the surface at an angle suitable for processing. Therefore, according to the method for manufacturing the additively manufactured product LP and the additive manufacturing system 1, the additively manufactured product LP can be appropriately manufactured.
[0043] (Modifications) While various exemplary embodiments have been described above, the present invention is not limited to the above-described exemplary embodiments, and various omissions, substitutions, combinations, and modifications may be made.
[0044] For example, the additive manufacturing apparatus 2 is not limited to a system that generates a fabricated object by irradiating a photocurable resin with light. For example, the layer forming unit may form a layer by jetting a raw material containing a resin onto the base 28, or jetting a binder onto the raw material on the base 28. As an example, the additive manufacturing apparatus and the additive manufacturing method can form a fabricated object by methods such as a method of melting a raw material at a high temperature with a laser or the like (for example, powder bed fusion), vat photopolymerization, material extrusion, binder jetting, sheet lamination, and material jetting.
[0045] When the processing apparatus 3 is a blast processing apparatus, a dry blast processing apparatus that ejects media together with compressed gas has been described as an example, but a wet blast processing apparatus that ejects a slurry in which media is suspended together with compressed gas may also be used. The dry blast processing apparatus has advantages such as high processing capability (processing force, wide coverage, processing speed) and the ability to perform processing at low cost. The wet blast processing apparatus has advantages such as suppressed dust generation from blast processing, high design quality of the processed surface, capability of fine processing, capability of uniform processing, and low risk of dust explosion occurrence.
[0046] The processing apparatus 3 is not limited to a blast processing apparatus as long as it is an apparatus that ejects media with a fluid. As an example, the processing apparatus may be a water jet processing apparatus, a film forming apparatus, or a coating apparatus.
[0047] When the processing apparatus 3 is a blast processing apparatus, the media does not need to be reused.
[0048] When a worker performs the work of transporting the layered modeled object LO from the additive manufacturing apparatus 2 to the processing apparatus 3, the layered modeling system 1 does not need to be provided with the transport apparatus 5.
[0049] The method for manufacturing the layered modeled product LP does not need to include the step of removing the nozzle portion. Even in this case, the manufacturing method achieves the effect of appropriately manufacturing the layered modeled product.
[0050] The nozzle portion formed as an integral body may be scraped off by the media in the process of ejecting the media. This is because the nozzle portion is made of the same material as the object to be surface-treated. Due to temporal change (friction deformation), the shape of the internal flow path of the nozzle portion or the shape of the tip portion deforms. Then, the ejection direction changes, the ejection range expands, or the ejection range shifts. In the manufacturing method, such temporal change may be acquired in advance by fluid analysis, and may be utilized when optimizing the nozzle shape, or may be adopted as a means for controlling the ejection range.
[0051] Furthermore, the shape of the nozzle attachment 35b may be set as appropriate. For example, Figure 8(A) is a cross-sectional view showing an example of a nozzle attachment, and Figure 8(B) is a cross-sectional view showing another example of a nozzle attachment. The internal conduit of the nozzle attachment 35b may have a rectangular cross-sectional shape as shown in Figure 8(A), or a chamfered rectangular cross-sectional shape as shown in Figure 8(B). Chamfering the corners of the conduit diameter makes it easier for the fluid to flow.
[0052] Each figure in Figure 9 is a cross-sectional view showing an example of a nozzle attachment or nozzle, and the compressed air is described assuming that it flows through the internal conduit toward the left in the drawing. Figure 9(A) is a longitudinal cross-sectional view showing an example of a nozzle attachment, Figure 9(B) is a longitudinal cross-sectional view showing another example of a nozzle attachment, and Figure 9(C) is a longitudinal cross-sectional view showing another example of a nozzle attachment. The internal conduit of the nozzle attachment 35b may have a straight cross-sectional shape as shown in Figure 9(A), or a secondary air hole 35e may be formed in a straight cross-sectional conduit as shown in Figure 9(B). The secondary air hole 35e is formed inclined in the direction in which the compressed air flows so as to connect the inside and outside of the conduit. Because secondary air is drawn in from the secondary air hole 35e by the airflow through the conduit, the injection flow rate can be increased, or the straightness of the injection flow can be improved. This can increase the finishing efficiency of the additively manufactured product LP. Furthermore, the path from the secondary air vent 35e to the pipeline in Figure 9(B) may be inclined perpendicular to the plane of the paper (i.e., inclined both horizontally and vertically). In addition to the effects described above, the vertical inclination causes the jet flow to become spiral-shaped, resulting in a stronger jet flow and improved straight-line propagation of the jet flow.
[0053] Figure 9(C) shows that a diameter-reducing section 35f and a diameter-expanding section 35g may be provided in the internal conduit of the nozzle attachment 35b, in the direction of compressed air flow. The diameter-reducing section 35f continuously reduces in diameter toward the diameter-reducing end 350f, accelerating the compressed air passing through it. The diameter-expanding section 35g continuously expands in diameter from the diameter-reducing end 350f (the other end of the expanded diameter) toward the diameter-expanding end 350g, further accelerating the compressed air by preventing it from rapidly expanding after passing through the diameter-reducing end 350f. This increases the strength of the jet flow and improves its straight-line accuracy. Alternatively, a diameter-reducing rectifier section (not shown) having a continuous cross-section of the same shape as the diameter-reducing end 350f may be connected to the diameter-reducing end 350f, and a diameter-expanding section 35g may be connected to the other end (the other end of the expanded diameter). Alternatively, a diameter-expanding rectifier section (not shown) having a continuous cross-section of the same shape as the diameter-expanding end 350g may be provided.
[0054] Figure 9(D) is a longitudinal cross-sectional view showing an example of a nozzle. As shown in Figure 9(D), a sealing material 35h may be provided at the connection point between the first nozzle body 35a (or second nozzle body 35c) and the nozzle attachment 35b. When the nozzle attachment 35b is fabricated using additive manufacturing technology, the surface roughness increases. Therefore, when assembling the nozzle attachment 35b to the first nozzle body 35a, a gap may occur at the connection point. By providing a sealing material 35h at the connection point, airtightness can be ensured.
[0055] Figure 9(E) is a longitudinal cross-sectional view showing another example of a nozzle. As shown in Figure 9(E), the first nozzle body 35a (or the second nozzle body 35c) may have a split structure. A split structure is a structure that is split in half along an axis. As described above, when the nozzle attachment 35b is fabricated using additive manufacturing technology, the surface roughness increases. Therefore, when inserting and assembling the nozzle attachment 35b into the first nozzle body 35a, the insertion process itself may become difficult. By having a split structure in the first nozzle body 35a (or the second nozzle body 35c), the nozzle attachment 35b can be held in place, thus improving ease of assembly.
[0056] Furthermore, the manufacturing method for additively manufactured products (LPs) is not limited to LPs manufactured using resin materials, but may also apply to LPs manufactured using metal materials. In the following, LPs manufactured using resin materials will be referred to as resin additively manufactured products, and LPs manufactured using metal materials will be referred to as metal additively manufactured products. Metal additively manufactured products are manufactured, for example, by melting metal powder. The surface of a metal additively manufactured product has roughness derived from layer lines and roughness derived from melting and solidification. Roughness derived from layer lines is roughness formed due to layering. Roughness derived from melting and solidification is roughness formed when the powder material solidifies without melting. Thus, the surface of a metal additively manufactured product has two types of roughness with different origins. Since the roughness derived from layer lines tends to be greater than the roughness derived from melting and solidification, the surface of a metal additively manufactured product has a heterogeneous shape with a mixture of different roughnesses.
[0057] When smoothing the surface of additively manufactured parts, different blasting approaches are required for resin-based and metal-based additively manufactured parts. Because resin-based additively manufactured parts are relatively soft, blasting with polygonal media (hard grids made of ceramics, crushed glass, metal, etc.) may result in deterioration of surface properties, such as the formation of sharp cutting marks, media punctures (residue), chipping, and shape changes. Therefore, for the surface of resin-based additively manufactured parts, methods that physically cut away the layer lines using spherical media (glass beads, ceramic beads, etc.) or soft media (plastic media, plant-derived media, etc.) are effective for smoothing the surface.
[0058] On the other hand, metal additive manufactured products have high hardness, and an oxide film is formed on their surface. Furthermore, unmelted powder may be firmly adhered to the surface of metal additive manufactured products. In addition, the surface of metal additive manufactured products has a mixture of the aforementioned layering marks and melting and solidification marks. To homogenize such a heterogeneous surface with a mixture of different roughnesses, it is necessary to remove large irregularities caused by layering marks in rough processing and to remove irregularities caused by melting and solidification, as well as irregularities caused by rough processing, in finishing processing. An effective method is to perform rough processing using polygonal media (hard grids made of ceramics, crushed glass, metal, etc.) and blast processing using spherical media (glass beads, ceramic beads, shots made of metal, etc.) as the finishing process. In rough processing, the polygonal media cuts away the large protrusions of layering marks, and in finishing processing, the spherical media plastically deforms the surface of the metal additive, smoothing out small irregularities. Rough processing and finishing processing may be performed separately, or they may be performed simultaneously by mixing multiple types of media. Furthermore, by performing blast processing using shots made of metal, it is possible to impart compressive residual stress in addition to smoothing the surface.
[0059] Incidentally, blasting with spherical media and blasting with polygonal media face similar challenges. As a specific example, when blasting from an external source, it is difficult to directly hit complexly shaped shadow areas, making it difficult to efficiently smooth the metal surface of those areas. The blasts that hit the metal surface of the shadow area are, for example, those that have bounced off other parts and do not have sufficient kinetic energy to remove layer lines or plastically deform the additively manufactured product. It is possible to increase the blasting force based on the shadow area, but this may cause over-processing in the areas where the blasts directly hit. Therefore, when blasting a shadow area from a distance, the media collides with the surrounding area before the shadow area is smoothed, resulting in over-processing. Over-processing is particularly noticeable in metal additively manufactured products, which are difficult to process.
[0060] In contrast, the manufacturing method for additively manufactured LP products allows the nozzle attachment 35b to be integrally fabricated during additive manufacturing, enabling the discharge port to be positioned near areas (shadows or internal spaces) that cannot be reached by external processing. This makes it possible to directly and precisely apply high-energy shots with minimal attenuation to the surface of metal additively manufactured products, which are difficult to process. Therefore, the manufacturing method for additively manufactured LP products is also effective in the manufacture of metal additively manufactured products, which are more difficult to process than resin additively manufactured products. However, in the case of additively manufactured ceramic products, blast processing, which uses impact force, is often unsuitable due to their high brittleness.
[0061] [Summary of Embodiments of this Disclosure] This disclosure includes the following embodiments:
[0062] (Clause 1) A method for manufacturing an additively manufactured product relating to one aspect of the present disclosure includes the following steps: (1) A step of manufacturing an additively manufactured product which is an integral part of an additively manufactured product and a nozzle part that can be connected to a processing device. (2) A step of connecting a processing device to the nozzle part included in the additively manufactured product and injecting a fluid from the nozzle part into the additively manufactured product.
[0063] In the manufacturing method described in Clause 1, an additively manufactured object is formed in which the additively manufactured product and the nozzle are integrated, and fluid is sprayed from the nozzle onto the additively manufactured product. By forming an integrated object of the additively manufactured product and the nozzle, the fluid can be properly sprayed onto the surface even in areas where the spray flow is difficult to reach with the nozzle installed in the processing device, or in areas where it is not possible to spray at an angle suitable for processing. Therefore, this manufacturing method can properly manufacture additively manufactured products.
[0064] (Clause 2) The manufacturing method described in Clause 1 may further include a step of removing the nozzle portion from the additively manufactured product after the spraying step. In this case, it is possible to avoid the nozzle portion affecting the function or design of the additively manufactured product.
[0065] (Clause 3) In the manufacturing method described in Clause 2, the spraying step may be blasting, and the removal step may be blasting to remove the nozzle portion from the additively manufactured object. In this case, since the surface treatment step and the removal step can be performed with the same processing equipment, a removal device is not required.
[0066] (Clause 4) In the manufacturing method described in Clauses 1 to 3, the spray range of the processing device may be changed by utilizing the change over time of the nozzle portion contained in the additively manufactured product. In this case, the additively manufactured product can be processed over a wide area.
[0067] (Clause 5) In the manufacturing methods described in Clauses 1 to 4, the additively manufactured product may include a structure that reflects or shields the fluid ejected from the nozzle. In this case, masking may be applied to the surface treatment of the additively manufactured product.
[0068] (Clause 6) In the manufacturing method described in Clause 1 or 2, the additively manufactured product is manufactured using a metal material, and the step of spraying the fluid may include shot blasting to remove the oxide film or unmelted powder formed on the surface of the additively manufactured product. In this case, the manufacturing method can appropriately produce metal additively manufactured products, which are more difficult to process than resin additively manufactured products.
[0069] (Clause 7) An additive manufacturing system relating to another aspect of the present disclosure comprises an additive manufacturing apparatus, a processing apparatus, and a control unit. The additive manufacturing apparatus manufactures an additively manufactured object. The processing apparatus is connectable to a nozzle. The control unit controls the additive manufacturing apparatus and the processing apparatus. The control unit causes the additive manufacturing apparatus to manufacture an additively manufactured object in which the additively manufactured product and the nozzle are integrated, and causes the processing apparatus to connect to the nozzle included in the additively manufactured object and to inject fluid from the nozzle into the additively manufactured object. This additive manufacturing system produces the same effects as the manufacturing method described above.
[0070] 1...Additive manufacturing system, 2...Additive manufacturing equipment, 3...Processing equipment, 35, 35A...Nozzle, 35b...Nozzle attachment (an example of a nozzle part), LO...Additive manufactured object, LP...Additive manufactured product, 50...Masking member (an example of a structure).
Claims
1. A method for manufacturing an additively manufactured product, comprising the steps of:
1. Manufacturing an additively manufactured product which integrates an additively manufactured product and a nozzle part that can be connected to a processing device; and 2. Connecting the processing device to the nozzle part included in the additively manufactured product and injecting a fluid from the nozzle part into the additively manufactured product.
2. The method for manufacturing an additively manufactured product according to claim 1, further comprising the step of removing the nozzle portion from the additively manufactured product after the spraying step.
3. The method for manufacturing an additively manufactured product according to claim 2, wherein the spraying step is a blasting process, and the removal step is to remove the nozzle portion from the additively manufactured product by blasting.
4. A method for manufacturing an additively manufactured product according to any one of claims 1 to 3, wherein the spray range of the processing device is changed by utilizing the change over time of the nozzle portion contained in the additively manufactured product.
5. The method for manufacturing an additively manufactured product according to any one of claims 1 to 3, wherein the additively manufactured product includes a structure that reflects or shields the fluid ejected from the nozzle.
6. The method for manufacturing an additively manufactured product according to claim 1 or 2, wherein the additively manufactured product is manufactured using a metal material, and the step of injecting the fluid includes shot blasting to remove an oxide film or unmelted powder formed on the surface of the additively manufactured product.
7. An additive manufacturing system comprising: an additive manufacturing apparatus for manufacturing additively manufactured objects; a processing apparatus connectable to a nozzle portion; and a control unit for controlling the additive manufacturing apparatus and the processing apparatus, wherein the control unit causes the additive manufacturing apparatus to manufacture the additively manufactured object, which integrates the additively manufactured object and the nozzle portion; and causes the processing apparatus to connect to the nozzle portion included in the additively manufactured object and to inject fluid from the nozzle portion into the additively manufactured object.