Positive electrode active material, positive electrode comprising same, and secondary battery comprising same

A positive electrode active material with a controlled contact angle range addresses electrolyte wettability issues, improving electrolyte penetration and enhancing the performance of lithium-ion batteries.

WO2026235299A1PCT designated stage Publication Date: 2026-11-12LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2026/005398
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-04-03
Filing Date
2026-04-16
Publication Date
2026-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face issues with electrolyte wettability, leading to localized current density imbalances and reduced battery lifespan due to low interfacial affinity and hydrophobicity of the active material surface, which can cause lithium plating and safety concerns.

Method used

A positive electrode active material with a specific contact angle range (50° to 65°) is developed, enhancing wettability by optimizing factors such as viscosity, surface tension, and immersion time, using a lithium transition metal phosphate with a carbon material layer and controlled porosity.

Benefits of technology

Improves electrolyte penetration and electrochemical performance, resulting in enhanced initial charge/discharge capacity and cycle characteristics of secondary batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material having a contact angle (θ) with an organic solvent of 50-65˚, wherein the contact angle (θ) is represented by equation 1. [Equation 1] cosθ = \{2η(ξ0h∞)2\} / (rcγτ) In equation 1, when a lower part of a holder accommodating the positive electrode active material is immersed in an organic solvent and the height (H) of the organic solvent penetrating into pores in the holder by capillary action over time (t*) is measured, η is the viscosity of the organic solvent, ξ0 is the average value of the slope of a graph obtained by fitting the height (h) versus (t*)β, t* is t / τ, t is the immersion time, τ is a constant selected from 60-180 seconds, β is the average value of the slope of a graph obtained by fitting the height (h) versus t*, h∞ is the maximum height the organic solvent can penetrate into the pores in the holder, rc is the average radius of the pores in the holder, and γ is the surface tension of the organic solvent.
Need to check novelty before this filing date? Find Prior Art

Description

Anode active material, anode including the same, and secondary battery including the same

[0001] The present invention relates to a positive electrode active material, a positive electrode including the same, and a secondary battery including the same.

[0002] With the recent rapid proliferation of battery-powered electronic devices such as mobile phones, laptops, computers, and electric vehicles, the demand for small, lightweight, and relatively high-capacity rechargeable batteries is increasing rapidly. In particular, lithium-ion batteries are gaining prominence as power sources for portable devices due to their lightweight design and high energy density. Consequently, active research and development efforts are underway to improve the performance of lithium-ion batteries.

[0003] To ensure the output characteristics and lifespan stability of lithium-ion batteries, it is essential to secure wettability, which allows the electrolyte to penetrate rapidly and uniformly into the electrodes. Electrolyte wettability is one of the key factors determining the interfacial resistance between the cathode active material and the electrolyte.

[0004] When wettability is low, dead zones occur on the surface of the active material where the electrolyte does not come into contact. This leads to localized current density imbalances, causing lithium plating, which ultimately becomes a chronic cause of reduced battery lifespan and safety issues.

[0005] Previously, methods were attempted to improve wettability by using specific additives in the electrolyte or undergoing a long impregnation process during the electrode process. However, electrolyte additives can cause side reactions at high temperatures, leading to swelling, and the extension of process time has the disadvantage of significantly reducing production efficiency. In addition, there were limitations in securing fundamental interfacial affinity due to the high hydrophobicity of the active material surface or residual lithium compounds.

[0006] In particular, the better the wettability of the surface of the positive electrode active material, the faster the electrolyte can be impregnated deep inside the electrode. Since this facilitates the smooth movement path of lithium ions and can affect the output characteristics and rapid charging performance of the secondary battery, wettability is one of the important factors to consider for the performance of the secondary battery.

[0007] The present invention is designed to solve the above-mentioned problems and aims to provide a positive electrode active material in which the contact angle between the positive electrode active material and the electrolyte solvent satisfies a specific range.

[0008] In addition, by satisfying a specific contact angle of the above-mentioned positive active material, the wettability of the positive active material is improved, and the invention aims to provide a positive and secondary battery with excellent initial charge / discharge capacity and / or cycle characteristics.

[0009] The present invention can provide a positive electrode active material in which the contact angle (θ) with an organic solvent is represented by the following formula 1, and the contact angle (θ) is 50˚ or more to 65˚ or less.

[0010] [Equation 1]

[0011] cosθ = {2η(ξ0h ∞ ) 2} / (r c γτ)

[0012] In Equation 1, the height (h) of the organic solvent that penetrates into the pores within the holder by capillary action when the lower part of the holder containing the positive active material is immersed in the organic solvent is the time (t * When measured according to ), η is the viscosity of the organic solvent, and ξ0 is (t * ) β It is the average value of the slopes of the graph fitted to the height (h) for , and t * is t / τ, where t is the immersion time, τ is a constant selected between 60 and 180 seconds, and β is t * It is the average value of the slope of the graph fitted to the height (h) for , and h ∞is the maximum height at which the organic solvent can penetrate into the pores within the holder, and r c is the average radius of the voids within the holder, and γ is the surface tension of the organic solvent.

[0013] In one embodiment, the positive electrode active material may include a lithium transition metal phosphate.

[0014] In one embodiment, the positive electrode active material may include an active material core portion and a carbon material layer provided on at least a portion of the surface of the active material core portion.

[0015] In one embodiment, the carbon material layer may contain 0.5 parts by weight or more and 2 parts by weight or less of a carbon-based material with respect to 100 parts by weight of the active material core.

[0016] In one embodiment, the average particle size (D50) of the primary particles of the positive active material may be 0.5 μm or more to 5 μm or less.

[0017] In one embodiment, the tap density of the positive active material is 0.5 g / cm³ 3 0 to 5 g / cm² 3 It may be less than.

[0018] In one embodiment, the specific surface area of ​​the positive active material is 5 m² 2 / g or more to 15 m 2 It may be less than / g.

[0019] In one embodiment, the organic solvent may include one or more selected from ester-based solvents, lactam-based solvents, ether-based solvents, ketone-based solvents, aromatic hydrocarbon-based solvents, carbonate-based solvents, alcohol-based solvents, nitrile-based solvents, amide-based solvents, dioxolane-based solvents, and sulfolane-based solvents.

[0020] In one embodiment, the porosity of the holder containing the positive active material may be 30% or more to 50% or less.

[0021] In one embodiment, the average radius (r) of the void within the holder in which the positive active material is accommodated c) may be 30 nm or more to 50 nm or less.

[0022] The present invention may also provide an anode comprising the aforementioned anode active material; a binder; and an anode material layer comprising a conductive material.

[0023] In one embodiment, the modulus of the anode material layer may be 35 MPa or more.

[0024] In one embodiment, the elongation rate of the anode material layer may be 5% or less.

[0025] In one embodiment, the anode material layer may include a dry anode sheet.

[0026] The present invention can also provide a secondary battery comprising the aforementioned positive electrode.

[0027] In one embodiment, the secondary battery may have an initial charge capacity of 153.5 mAh / g or more under 0.1C charge / discharge conditions.

[0028] The present invention also (S1) immerses the lower part of a holder containing a positive electrode active material in an organic solvent, and the height (h) of the organic solvent that penetrates into the pores within the holder by capillary action is time (t * A method for measuring the contact angle of an anode active material can be provided, comprising the steps of: (S2) measuring according to the organic solvent and the anode active material; and (S2) measuring the contact angle (θ) of the organic solvent and the anode active material from the following formula 1.

[0029] [Equation 1]

[0030] cosθ = {2η(ξ0h ∞ ) 2} / (r c γτ)

[0031] In Equation 1, η is the viscosity of the organic solvent, and

[0032] ξ0 is (t * ) β It is the average value of the slope of the graph fitted to the height (h) for, and

[0033] t* is t / τ, where t is the immersion time, and τ is a constant selected from 60 to 180 seconds, and

[0034] β is t * It is the average value of the slope of the graph fitted to the height (h) for, and

[0035] h ∞ is the maximum height at which an organic solvent can penetrate into the pores within the holder, and

[0036] r c is the average radius of the air gap within the holder, and

[0037] γ is the surface tension of the organic solvent.

[0038] In one embodiment, the step (S1) is performed by the height (h) of the organic solvent over time (t * It may include a step of calculating the average slope value β from a graph obtained by fitting the result value measured according to ).

[0039] In one embodiment, after step (S1) (S1-1), the height (h) of the organic solvent is (t) to which the β value is applied. * ) β It may include a step of calculating ξ0, which is the average value of the slope, from a graph obtained by fitting the result values ​​measured according to .

[0040] In one embodiment, the step (S1) may include a step of pressurizing the positive active material received so that the porosity inside the holder receiving the positive active material is 30% or more to 50% or less.

[0041] In one embodiment, in step (S1), the average radius (r) of the void in the holder in which the positive active material is received c It may include a step of pressurizing the positive active material received so that the thickness is 30 nm or more to 50 nm or less.

[0042] In one embodiment, in step (S1), filter paper may be included on the upper and lower portions of the holder in which the positive active material is received.

[0043] In one embodiment, the inner diameter of the holder may be 10 mm or more to 25 mm or less.

[0044] In one embodiment, the positive electrode active material may include a lithium transition metal phosphate.

[0045] In one embodiment, the positive electrode active material may include an active material core portion and a carbon material layer provided on at least a portion of the surface of the active material core portion.

[0046] In one embodiment, the carbon material layer may contain 0.5 parts by weight or more and 2 parts by weight or less of a carbon-based material with respect to 100 parts by weight of the active material core.

[0047] In one embodiment, the average particle size (D50) of the primary particles of the positive active material may be 0.5 μm or more to 5 μm or less.

[0048] In one embodiment, the tap density of the positive active material is 0.5 g / cm³ 3 0 to 5 g / cm² 3 It may be less than.

[0049] In one embodiment, the specific surface area of ​​the positive active material is 5 m² 2 / g or more to 15 m 2 It may be less than / g.

[0050] In one embodiment, the organic solvent may include one or more selected from ester-based solvents, lactam-based solvents, ether-based solvents, ketone-based solvents, aromatic hydrocarbon-based solvents, carbonate-based solvents, alcohol-based solvents, nitrile-based solvents, amide-based solvents, dioxolane-based solvents, and sulfolane-based solvents.

[0051] The present invention may also include the step of measuring the contact angle (θ) between an organic solvent and a positive active material according to the aforementioned method for measuring the contact angle of a positive active material.

[0052] As the contact angle between the positive electrode active material and the organic solvent of the electrolyte satisfies a specific range, the wettability of the positive electrode active material can be improved, thereby improving the electrochemical performance of the secondary battery.

[0053] Terms and words used in this specification and claims shall not be interpreted as being limited to their ordinary or dictionary meanings, but shall be interpreted in a meaning and concept consistent with the technical spirit of the invention, based on the principle that the inventor can appropriately define the concept of the terms to best describe his invention.

[0054] Therefore, the configurations of the embodiments described in this specification are merely one of the most preferred embodiments of the present invention and do not represent all of the technical ideas of the present invention; thus, it should be understood that various equivalents and modifications capable of replacing them may exist at the time of filing this application. In this specification, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0055] In this specification, when a part is described as “comprising” a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components. Thus, for example, a composition comprising compound A may include compounds other than A. However, the term “comprising” also encompasses, in a more restrictive sense as a specific embodiment thereof, “essentially / essentially composed of” and “composed of,” so, for example, a “composition comprising compound A” may also be (essentially / essentially) composed of compound A.

[0056] In connection with this, terms such as “comprising” or “having,” as described in this specification, are intended to specify the existence of the implemented features, numbers, steps, components, or combinations thereof, and should not be understood as precluding the existence or addition of one or more other features, numbers, steps, components, or combinations thereof.

[0057] In this specification, when it is stated that any layer is located or provided “on” or “between” another arbitrary layer, this includes not only cases where any layer is in contact with another arbitrary layer, but also cases where another layer or material, etc. exists between the two layers.

[0058] Where in this specification a quantity, concentration, or other value or parameter is given as an enumeration of a range, a preferred range, a preferred upper limit, and a preferred lower limit, it should be understood that any pair of any upper range limit or preferred value and any lower range limit or preferred value, regardless of whether the range is disclosed separately, specifically discloses all ranges that may be formed. Where a range of numerical values ​​is mentioned in this specification, unless otherwise stated, for example, without limiting terms such as greater than or less than, the range is intended to include its endpoint value and all integers and fractions within that range. The scope of the invention is not intended to be limited to the specific value mentioned when defining the range.

[0059] Among the physical properties mentioned in this specification, if the measured temperature affects the property, the property is measured at room temperature unless specifically otherwise specified. The term "room temperature" refers to a natural temperature that has not been heated or cooled, and may mean, for example, any temperature within the range of about 10°C to 30°C, about 23°C, or about 25°C. Furthermore, unless specifically otherwise specified, the unit of temperature in this specification is °C.

[0060] In addition, among the physical properties mentioned in this specification, if the measured pressure affects the physical property, unless otherwise specifically defined, the physical property is measured at atmospheric pressure, that is, at about 1 atmosphere.

[0061] In this specification, “average particle size (D 50 ")" refers to the particle size at the 50% reference of the volume-cumulative particle size distribution of the particles, and can be measured using the laser diffraction method. For example, after dispersing the powder to be measured in a dispersion medium, or after introducing the powder to be measured in a dry state into a measurement unit under vacuum, it can be measured by introducing it into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000), irradiating it with ultrasound of about 28 kHz at an output of 60 W, obtaining a volume-cumulative particle size distribution graph, and then determining the particle size corresponding to 50% of the volume-cumulative amount.

[0062] One embodiment of the present invention may provide a positive electrode active material. The positive electrode active material has a contact angle (θ) with an organic solvent represented by the following formula 1, and the contact angle (θ) may be 50˚ or more to 65˚ or less.

[0063] [Equation 1]

[0064] cosθ = {2η(ξ0h ∞ ) 2} / (r c γτ)

[0065] In Equation 1, the height (h) of the organic solvent that penetrates into the pores within the holder by capillary action when the lower part of the holder containing the positive active material is immersed in the organic solvent is the time (t * When measured according to ), η is the viscosity of the organic solvent, and ξ0 is (t * ) β It is the average value of the slopes of the graph fitted to the height (h) for , and t * is t / τ, where t is the immersion time, τ is a constant selected between 60 and 180 seconds, and β is t * It is the average value of the slope of the graph fitted to the height (h) for , and h ∞ is the maximum height at which the organic solvent can penetrate into the pores within the holder, and r c is the average radius of the voids within the holder, and γ is the surface tension of the organic solvent.

[0066] The contact angle (θ) of the above-mentioned positive active material with an organic solvent can be determined by various factors, including the physical or chemical state of the positive active material. Specifically, the contact angle (θ) may vary depending on various variables such as the transition metal composition included in the positive active material, the type of doping element, the average particle size of the positive active material, the purity of the raw material during synthesis, the mixing conditions of the raw material, the calcination temperature, the calcination time, the calcination atmosphere, the composition of the raw material, ambient humidity, temperature and pressure, the thickness or uniformity of the carbon material layer, the time of acquisition and storage of the raw material, and / or the time of synthesis and storage of the positive active material. Therefore, even small differences in the manufacturing process of the positive active material may result in a difference in the contact angle (θ) according to the present invention.

[0067] Furthermore, when the contact angle (θ) of the above-mentioned positive active material with an organic solvent satisfies a specific range, the lifespan characteristics and stability of the secondary battery using such positive active material can be improved.

[0068] The contact angle (θ) of the above positive active material with the organic solvent is expressed by Equation 1, wherein in Equation 1, the height (h) of the organic solvent penetrating into the pores within the holder by capillary action when the lower part of the holder containing the positive active material is immersed in the organic solvent is the time (t * When measured according to ), η is the viscosity of the organic solvent, and ξ0 is (t * ) β It is the average value of the slopes of the graph fitted to the height (h) for , and t * is t / τ, where t is the immersion time, τ is a constant selected between 60 and 180 seconds, and β is t * It is the average value of the slope of the graph fitted to the height (h) for , and h ∞ is the maximum height at which the organic solvent can penetrate into the pores within the holder, and r c is the average radius of the voids within the holder, and γ is the surface tension of the organic solvent.

[0069] The contact angle (θ) of the positive active material with the organic solvent represented by the above formula 1 may be 50˚ or more to 65˚ or less. Specifically, the contact angle (θ) of the above-mentioned positive active material with an organic solvent is 50˚ or more, 50.1˚ or more, 50.2˚ or more, 50.3˚ or more, 50.4˚ or more, 50.5˚ or more, 50.6˚ or more, 50.7˚ or more, 50.8˚ or more, 50.9˚ or more, 51˚ or more, 51.1˚ or more, 51.2˚ or more, 51.3˚ or more, 51.4˚ or more, 51.5˚ or more, 51.6˚ or more, 51.7˚ or more, 51.8˚ or more, 51.9˚ or more, 52˚ or more, 52.1˚ or more, 52.2˚ or more, 52.3˚ or more, 52.4˚ or more, 52.5˚ or more, 52.6˚ or more, 52.7˚ or more, 52.8˚ or more, One lower limit selected from 52.9˚ or higher, or 53˚ or higher, and 65˚ or lower, 64.9˚ or lower, 64.8˚ or lower, 64.7˚ or lower, 64.6˚ or lower, 64.5˚ or lower, 64.4˚ or lower, 64.3˚ or lower, 64.2˚ or lower, 64.1˚ or lower, 64˚ or lower, 63.9˚ or lower, 63.8˚ or lower, 63.7˚ or lower, 63.6˚ or lower, 63.5˚ or lower, 63.4˚ or lower, 63.3˚ or lower, 63.2˚ or lower, 63.1˚ or lower, 63˚ or lower, 62.9˚ or lower, 62.8˚ or lower, 62.7˚ or lower, 62.6˚ or lower, 62.5˚ or lower, 62.4˚ or lower, 62.3˚ or lower, 62.2˚ 62.1˚ or less, 62˚ or less, 61.9˚ or less, 61.8˚ or less, 61.7˚ or less, 61.6˚ or less, 61.5˚ or less, 61.4˚ or less, 61.3˚ or less, 61.2˚ or less, 61.1˚ or less, 61˚ or less, 60.9˚ or less, 60.8˚ or less, 60.7˚ or less, 60.6˚ or less, 60.5˚ or less, 60.4˚ or less, 60.3˚ or less, 60.2˚ or less, 60.1˚ or less, 60˚ or less, 59.9˚ or less, 59.8˚ or less, 59.7˚ or less, 59.6˚ or less, 59.5˚ or less, 59.4˚ or less, 59.3˚ or less, 59.2˚ or less, 59.1˚ or less, 59˚ or less, 58.9˚ or less, 58.8˚ or less, 58.7˚ or less, 58.6˚ or less, 58.5˚ or less, 58.4˚ or less, 58.3˚ or less, 58.2˚ or less, 58.1˚ or less, 58˚ or less, 57.9˚ or less, 57.8˚ or less, 57.7˚ or less, 57.6˚ or less, 57.5˚ or less, 57.4˚ or less, 57.3˚ or less, 57.2˚ or less, 57.1˚ or less, 57˚ or less, 56.9˚ or less, 56.8˚ or less, 56.7˚ or less, 56.6˚ or less, 56.5˚ or less, 56.4˚ or less, 56.3˚ or less, 56.2˚ or less, 56.1˚ or less, 56˚ or less, A range consisting of one upper limit selected from 55.9˚ or less, 55.8˚ or less, 55.7˚ or less, 55.6˚ or less, 55.5˚ or less, 55.4˚ or less, 55.3˚ or less, 55.2˚ or less, 55.1˚ or less, or 55˚ or less can be satisfied. When the contact angle (θ) of the positive active material with respect to an organic solvent satisfies the above range, the wettability of the positive active material and / or the performance of the secondary battery may be improved.

[0070] Equation 1 above represents the height (h) of the organic solvent that penetrates into the pores within the holder by capillary action when the lower part of the holder containing the positive active material is immersed in the organic solvent, with respect to time (t * It can be calculated by measuring according to ).

[0071] When the lower part of the holder containing the above-mentioned positive active material is immersed in an organic solvent, the organic solvent is absorbed upward through the pores within the holder due to capillary action. At this time, the height (h) of the organic solvent is [time]. * It can be measured according to ). In this case, time t *may mean t / τ, where t represents the immersion time and τ is a characteristic time, a constant selected between 60 and 180 seconds. For example, τ can be 60 seconds, 120 seconds, or 180 seconds. The height (h) of the organic solvent is time (t * When measuring according to ), the immersion time (t) may include a step of obtaining a height (h) value measured at unit times. The unit time may appropriately adjust the time interval according to the magnitude of the τ value. In addition, the time (t * When measuring the height (h) value of the organic solvent according to ), time (t * ) can be measured in the range from 0 or more to τ value or less.

[0072] The above β is t * As the average value of the slope of the graph fitted to the height (h) for, the height (h) of the organic solvent is time (t * It can be obtained by calculating the average value of the slope from a graph obtained by fitting the result values ​​measured according to ). Specifically, the height (h) of the organic solvent is given by time (t * The method may include a step of calculating the slope from a graph obtained by fitting the result values ​​measured according to ). Subsequently, the average value of the calculated slopes can be calculated as the β value. Unlike that known by the conventional washburn method, the β value of the present invention is calculated by the height (h) of the organic solvent versus time (t * By fitting the result values ​​obtained by measuring according to ), it can be analyzed to be identical to or closest to the actual phenomena occurring in the cathode active material. Therefore, the measurement error of the contact angle is very small.

[0073] When measuring the β value, which is the average value of the slope, the average value of the slope measured at each unit time can be measured within a range of 0 or more to τ or less. As previously mentioned, the unit time can be appropriately adjusted according to the τ value. For example, the height (h) of the organic solvent at time (t * When measuring according to ), measurements can be taken at 1-second intervals, but are not limited thereto.

[0074] The average value (β) of the above slope is the height (h) of the organic solvent over time (t * It may refer to the average of measurement results obtained by repeating the step of calculating the average value of the slope from a graph obtained by fitting the result values ​​measured according to ) at least three times. Specifically, the average value of the slope (β) is the height (h) of the organic solvent versus time (t * The average value of the β value obtained from the result obtained by repeating the step of calculating the average value of the slope from the graph obtained by fitting the result value measured according to ) 3 or more times and 10 or fewer times can be used.

[0075] The above β value may be 0.7 or higher to 1 or lower, or 0.7 or higher to 0.9 or lower. When the above β value is measured within the above range, there is an effect of improving the performance of the positive electrode or secondary battery.

[0076] The above ξ0 is (t * ) β As the average value of the slope of the graph fitting the height (h) for, the height (h) of the organic solvent is (t) to which the β value determined above is applied. * ) β It can be obtained by calculating the average value of the slope from the graph obtained by fitting the result values ​​measured according to . Specifically, from the β value obtained above (t * ) β The ξ0 value can be calculated by calculating the average value of the slope from a new graph fitted with the height (h) of the organic solvent for .

[0077] Similar to calculating the β value, the above ξ0 value can also be measured as the average value of the slope measured at each unit time within a range from 0 or greater to τ or less, and the unit time can be appropriately adjusted according to the magnitude of the τ value. The average value of the slope (ξ0) is the height (h) of the organic solvent (t * ) β The average value of ξ0 obtained from the measurement results obtained by repeating the step of calculating the average value of the slope from the graph obtained by fitting the result value measured according to 3 or more times and 10 or fewer times can be used.

[0078] Equation 1 above represents the cosine value of the contact angle (θ) between the organic solvent and the cathode active material, and can be obtained by substituting the calculated ξ0 value.

[0079] h in Equation 1 above ∞ may refer to the maximum height at which an organic solvent can penetrate into the voids within the holder, and the above h ∞ represents a constant value controlled according to the type of organic solvent, the type of positive electrode active material, the average particle size (D50) of the positive electrode active material, the porosity within the holder, the pressure within the holder, etc., and can be measured by actually measuring the organic solvent penetrating into the holder containing the positive electrode active material. For example, h ∞ It may be 1 m or less, and specifically, 0.9 m or less, 0.8 m or less, 0.7 m or less, 0.6 m or less, 0.5 m or less, 0.4 m or less, 0.3 m or less, 0.2 m or less, or 0.1 m or less.

[0080] In Equation 1 above, r c is the average radius of the air gap within the holder, and r c The value may have a correlation with the void within the holder. The r cThe value can be measured using the Washburn equation through the porosity within the holder. For example, the above r c It may be 30 nm or more to 50 nm or less, and specifically, it may satisfy a range consisting of one lower limit selected from 30 nm or more, 31 nm or more, 32 nm or more, 33 nm or more, 34 nm or more, or 35 nm or more, and one upper limit selected from 50 nm or less, 49 nm or less, 48 ​​nm or less, 47 nm or less, 46 nm or less, or 45 nm or less.

[0081] The porosity inside the holder containing the positive active material may be 30% or more to 50% or less. Specifically, the porosity inside the holder may satisfy a range consisting of one lower limit selected from 30% or more, 31% or more, 32% or more, 33% or more, 34% or more, 35% or more, 36% or more, 37% or more, 38% or more, 39% or more, or 40% or more, and one upper limit selected from 50% or less, 49% or less, 48% or less, 47% or less, 46% or less, 45% or less, 44% or less, 43% or less, 42% or less, 41% or less, or 40% or less. The porosity inside the holder can be measured from the mass of the absorbed solvent when the organic solvent is absorbed up to the maximum height of the positive active material contained inside the holder.

[0082] In addition, the average radius (r) of the void within the holder in which the above positive active material is accommodated c) may be 30 nm or more to 50 nm or less, and specifically, may satisfy a range consisting of one lower limit selected from 30 nm or more, 31 nm or more, 32 nm or more, 33 nm or more, 34 nm or more, 35 nm or more, or 36 nm or more, and one upper limit selected from 50 nm or less, 49 nm or less, 48 ​​nm or less, 47 nm or less, 46 nm or less, 45 nm or less, 44 nm or less, 43 nm or less, 42 nm or less, 41 nm or less, 40 nm or less, 39 nm or less, 38 nm or less, 37 nm or less, 36 nm or less, or 35 nm or less.

[0083] To satisfy the above conditions, the lower part of the holder containing the positive active material is immersed in an organic solvent, and the height (h) of the organic solvent penetrating into the pores within the holder by capillary action is time (t * When measured according to ), the porosity inside the holder containing the positive active material is 30% or more to 50% or less, and the average radius of the void inside the holder containing the positive active material (r c The inside of the holder containing the positive active material can be pressurized so that the thickness is 30 nm or more to 50 nm or less.

[0084] In Equation 1 above, η is the viscosity of the organic solvent and γ is the surface tension of the organic solvent.

[0085] The holder may include a receiving space capable of accommodating the positive active material inside, and the holder may have a cylindrical shape extending in the vertical direction. The holder may have a structure having symmetry in a direction perpendicular to the vertical direction, but is not limited thereto. By forming a structure having symmetry as described above, pressure imbalances can be prevented during the compression process of the positive active material being accommodated, and errors that may occur due to boundary conditions caused by the geometric structure of the analysis environment can be minimized. The holder may be made of a rigid material with chemical resistance, such as SUS or engineering plastic, but is not limited thereto.

[0086] The holder may further include a pressurizing member for pressurizing the inside of the holder in which the positive active material is contained. The pressurizing member may be disposed on the upper part of the holder, and the pressurizing member may press the holder in the direction of gravity to pressurize the inside of the holder in which the positive active material is contained.

[0087] The above-described pressure member may include a disc-shaped pressure plate having a bottom surface formed as a plane perpendicular to the vertical direction, an upper cover coupled to the upper part of the holder, and a push bar that penetrates the upper cover in the vertical direction, has a lower end coupled to the upper surface of the pressure plate, and has an upper end protruding further above the upper cover. The pressure plate may be made of Teflon, a chemical-resistant rigid material, but is not limited thereto.

[0088] The inner diameter of the holder may be 10 mm or more to 25 mm or less. Specifically, the inner diameter of the holder may satisfy a range consisting of one lower limit selected from 10 mm or more, 11 mm or more, 12 mm or more, 13 mm or more, 14 mm or more, 15 mm or more, 16 mm or more, 17 mm or more, 18 mm or more, 19 mm or more, or 20 mm or more, and one upper limit selected from 25 mm or less, 24 mm or less, 23 mm or less, 22 mm or less, 21 mm or less, or 20 mm or less.

[0089] Filter papers may be included on the upper and lower portions of the holder in which the positive active material is received. A first filter paper provided on the lower portion of the holder may serve to support the positive active material received in the holder, and a second filter paper provided on the upper portion of the holder may serve to fix the positive active material received in the holder.

[0090] The filter paper may include one or more selected from nitrocellulose, cellulose, fabric swab, cotton swab, glass wool, glass fiber, polyester, and polypropylene. For example, the filter paper may be a quantitative filter paper made of cellulose material and may include Hyundai Micro (HM) Product No. 30, but is not limited thereto. The first filter paper and the second filter paper may be made of the same material or may use different materials.

[0091] The thickness of the filter paper may be 0.1 mm or more to 0.3 mm or less. Specifically, the thickness of the filter paper may be 0.15 mm or more to 0.25 mm or less.

[0092] The above-mentioned positive electrode active material is a material that serves as a source of lithium ions during charging and discharging, and includes a material capable of absorbing and releasing lithium ions. The above-mentioned positive electrode active material may include a lithium transition metal phosphate. For example, the above-mentioned positive electrode active material may be a lithium iron phosphate-based compound (LFP) having the chemical formula LiFePO4, or LiFe x M1 (1-x) P y M2 (1-y) O4(wherein, M1 = 1 or more of Mn, Co, Ni, Al, V, B, Cd, Cu, Mg, Zn, Ti, Nb, Zr and Cr, and 0 <x≤1, M2 = Si, N, S, Cl, Br, 및 F 중 1 이상이며, 0≤y≤1)의 화학식을 갖는 리튬 철 금속 인산화물(LMFP) 등을 포함할 수 있으나, 이에 한정되는 것은 아니다.

[0093] The average particle size (D50) of the primary particles of the above-mentioned positive active material may be 0.5 μm or more to 5 μm or less. Specifically, the average particle size (D50) of the primary particles of the above-mentioned positive active material is one lower limit selected from 0.5 μm or more, 0.6 μm or more, 0.7 μm or more, 0.8 μm or more, 0.9 μm or more, 1 μm or more, 1.1 μm or more, 1.2 μm or more, 1.3 μm or more, 1.4 μm or more, 1.5 μm or more, 1.6 μm or more, 1.7 μm or more, 1.8 μm or more, 1.9 μm or more, or 2 μm or more, and 5 μm or less, 4.9 μm or less, 4.8 μm or less, 4.7 μm or less, 4.6 μm or less, 4.5 μm or less, 4.4 μm or less, 4.3 μm or less, 4.2 μm or less, 4.1 μm or less, 4 μm or less, 3.9 μm or less, It can satisfy a range consisting of one upper limit selected from 3.8 μm or less, 3.7 μm or less, 3.6 μm or less, 3.5 μm or less, 3.4 μm or less, 3.3 μm or less, 3.2 μm or less, 3.1 μm or less, 3 μm or less, 2.9 μm or less, 2.8 μm or less, 2.7 μm or less, 2.6 μm or less, 2.5 μm or less, 2.4 μm or less, 2.3 μm or less, 2.2 μm or less, 2.1 μm or less, or 2 μm or less. When the average particle size (D50) of the primary particles of the above-mentioned positive electrode active material satisfies the above range, ion transport and electron conductivity within the positive electrode are improved, thereby improving the electrochemical performance of the secondary battery.

[0094] The tap density of the above positive active material is 0.5 g / cm³ 3 0 to 5 g / cm² 3 It may be less than or equal to. Specifically, the tap density of the above-mentioned positive active material is 0.5 g / cm³ 3 Above, 0.6 g / cm³ 3 Above, 0.7 g / cm³ 3 Above, 0.8 g / cm³ 3 Above, 0.9 g / cm³ 3 Above, 1 g / cm³ 3 Above, 1.1 g / cm³ 3Above, 1.2 g / cm³ 3 Above, 1.3 g / cm³ 3 Above, 1.4 g / cm³ 3 Above, 1.5 g / cm³ 3 Above, 1.6 g / cm³ 3 Above, 1.7 g / cm³ 3 Above, 1.8 g / cm³ 3 Above, 1.9 g / cm³ 3 Above, or 2 g / cm³ 3 One lower limit selected from the above, and 5 g / cm² 3 Below, 4.9 g / cm³ 3 Below, 4.8 g / cm³ 3 Below, 4.7 g / cm³ 3 Below, 4.6 g / cm³ 3 Below, 4.5 g / cm³ 3 Below, 4.4 g / cm³ 3 Below, 4.3 g / cm³ 3 Below, 4.2 g / cm³ 3 Below, 4.1 g / cm³ 3 Below, 4 g / cm³ 3 Below, 3.9 g / cm³ 3 Below, 3.8 g / cm³ 3 Below, 3.7 g / cm³ 3 Below, 3.6 g / cm³ 3 Below, 3.5 g / cm³ 3 Below, 3.4 g / cm³ 3 Below, 3.3 g / cm³ 3 Below, 3.2 g / cm³ 3 Below, 3.1 g / cm³ 3 Less than or equal to 3 g / cm³ 3 A range consisting of one upper limit selected from the following may be satisfied. When the tap density of the positive electrode active material satisfies the above range, ion transport and electron conductivity within the positive electrode are improved, thereby enhancing the electrochemical performance of the secondary battery.

[0095] The specific surface area of ​​the above positive active material is 5 m² 2 / g or more to 15 m 2It may be less than / g. Specifically, the specific surface area of ​​the above-mentioned positive active material is 5 m² 2 / g or more, 6 m 2 / g or more, 7 m 2 / g or more, 8 m 2 / g or more, 9 m 2 / g or more, or 10 m 2 One lower bound selected from / g or greater, and 15 m 2 / g or less, 14 m 2 / g or less, 13 m 2 / g or less, 12 m 2 / g or less, 11 m 2 / g or less, or 10 m 2 A range consisting of one upper limit selected from / g or less can be satisfied. When the specific surface area of ​​the cathode active material satisfies the above range, ion transport and electron conductivity within the cathode are improved, thereby enhancing the electrochemical performance of the secondary battery.

[0096] The above-mentioned positive electrode active material may include an active material core and a carbon material layer provided on at least a portion of the surface of the active material core. The carbon material layer can increase the ion diffusion rate and electrical conductivity by forming a continuous conductive network on the surface of the active material core. In addition, the carbon material layer can also serve to improve cycle life by preventing the surface of the positive electrode active material core from oxidizing due to exposure to oxygen or moisture in the air.

[0097] The carbon material layer may include a conductive carbon material, and for example, the carbon material layer may include at least one carbon material selected from the group consisting of graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, thermo black, carbon black, carbon nanofiber, carbon nanotube, carbon fluoride, graphene, metal powder, crystalline carbon, potassium titanate, zinc oxide, titanium oxide, and polyphenylene derivatives, but is not limited thereto.

[0098] The carbon material layer may contain 0.5 parts by weight or more and 2 parts by weight or less of a carbon-based material with respect to 100 parts by weight of the active material core. Specifically, the carbon material layer may satisfy a range consisting of one lower limit selected from 0.5 parts by weight or more, 0.6 parts by weight or more, 0.7 parts by weight or more, 0.8 parts by weight or more, 0.9 parts by weight or more, 1 part by weight or more, 1.1 parts by weight or more, 1.2 parts by weight or more, 1.3 parts by weight or more, 1.4 parts by weight or more, or 1.5 parts by weight or more, and one upper limit selected from 2 parts by weight or less, 1.9 parts by weight or less, 1.8 parts by weight or less, 1.7 parts by weight or less, 1.6 parts by weight or less, 1.5 parts by weight or less, 1.4 parts by weight or less, 1.3 parts by weight or less, 1.2 parts by weight or less, 1.1 parts by weight or less, or 1 part by weight or less, based on 100 parts by weight of the active material core. When the content of the carbon material layer satisfies the above range, electron transfer of the positive electrode active material and diffusion of lithium ions can be improved, and the surface of the positive electrode active material can be protected from oxygen or moisture, thereby improving the lifespan characteristics of the secondary battery.

[0099] The above-mentioned positive active material can be manufactured by mixing raw materials and calcining the mixture at a temperature of 500°C or higher to 1000°C or lower. At this time, the raw materials may include a lithium precursor, an iron precursor, and a phosphate precursor. It may also be manufactured by a solid-state method in which raw material powders in a solid state are mixed, or by a hydrothermal synthesis method in which raw materials are dissolved in a solvent and reacted in a liquid state, but is not limited thereto.

[0100] As the lithium precursor, lithium carbonate (Li2CO3), lithium hydroxide (LiOH·H2O), lithium nitrate (LiNO3), lithium acetate (LiCH3COO), etc. may be used; as the iron precursor, iron oxalate (FeC2O4·2H2O), iron sulfate (FeSO4·7H2O), iron chloride (FeCl2), iron oxide (Fe2O3, Fe3O4), iron nitrate (Fe(NO3)3·9H2O), iron phosphate (FEPO4·nH2O), etc. may be used; and as the phosphoric acid precursor, diammonium phosphate ((NH4)2HPO4), monoammonium phosphate (NH4H2PO4), phosphoric acid (H3PO4), etc. may be used, but are not limited thereto.

[0101] When manufacturing the above-mentioned positive active material, the carbon material layer described above can be prepared by mixing the carbon material and then calcining it.

[0102] The physical properties, shape, and / or performance of the above-mentioned positive active material can be controlled according to various variables such as mixing conditions, calcination temperature, calcination time, and the composition of raw materials, and the coating content, area, thickness, and / or uniformity of the above-mentioned carbon material layer can be controlled according to various variables such as mixing conditions, calcination temperature, calcination time, and the composition and thickness of the carbon material layer. That is, the contact angle between the organic solvent and the positive active material represented by Equation 1 above can be controlled by various variables in the manufacturing process for producing the positive active material, such as raw material mixing conditions, calcination temperature, calcination time, calcination atmosphere, composition of raw materials, and composition and thickness of the carbon material layer.

[0103] The above organic solvent serves as a medium through which ions involved in the electrochemical reaction of a secondary battery can move, and any organic solvent used in an electrolyte can be used without limitation. Specifically, the above organic solvent may include one or more selected from ester-based solvents, lactam-based solvents, ether-based solvents, ketone-based solvents, aromatic hydrocarbon-based solvents, carbonate-based solvents, alcohol-based solvents, nitrile-based solvents, amide-based solvents, dioxolane-based solvents, and sulfolane-based solvents.

[0104] For example, the organic solvent is an ester-based solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; a lactam-based solvent such as N-methyl-2-pyrrolidone (NMP), 2-pyrrolidone, N-vinyl-2-pyrrolidone (NVP), N-ethyl-2-pyrrolidone (NEP), or ε-caprolactam; an ether-based solvent such as dibutyl ether or tetrahydrofuran; or a ketone-based solvent such as cyclohexanone; Aromatic hydrocarbon solvents such as benzene or fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), or propylene carbonate (PC); alcohol solvents such as ethyl alcohol or isopropyl alcohol; nitrile solvents such as R-CN (where R is a hydrocarbon group with a straight, branched, or ring structure having C2 to C20 and may include a double bond, an aromatic ring, or an ether bond); amide solvents such as dimethylformamide; dioxolane solvents such as 1,3-dioxolane; or sulfolane solvents such as sulfolane or dimethyl sulfone may be included, but are not limited thereto.

[0105] Another embodiment of the present invention may provide an anode. The anode may include an anode material layer comprising the aforementioned anode active material; a binder; and a conductive material.

[0106] The above anode may include an anode current collector and an anode material layer provided on at least one surface of the anode current collector.

[0107] The above positive current collector is not particularly limited as long as it is conductive without causing chemical changes in the battery, and may be made of, for example, copper (Cu), nickel (Ni), aluminum (Al), vanadium (V), gold (Au), platinum (Pt), chromium (Cr), iron (Fe), zinc (Zn), indium (In), germanium (Ge), lithium (Li), magnesium (Mg), stainless steel (e.g., SUS), titanium (Ti), cobalt (Co), or an alloy thereof.

[0108] The anode current collector may have a thickness of 3 μm or more to 500 μm or less, and fine irregularities may be formed on the surface of the anode current collector to increase the adhesion of the anode material layer. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. The anode current collector may be omitted depending on the case.

[0109] The above-described positive material layer may include the aforementioned positive active material. In addition to the positive active material, the above-described positive material layer may further include a conductive material or a binder.

[0110] The above conductive material is used to impart conductivity to the electrode and can be used without special limitations as long as it has electronic conductivity without causing chemical changes. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, thermo black, carbon nanotubes, carbon nanofibers; metal powder or metal fibers such as copper, nickel, aluminum, silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and one of these alone or a mixture of two or more may be used. For example, the above conductive material may include at least one selected from the group consisting of graphite, carbon black, acetylene black, ketjen black, channel black, furnace black, thermo black, carbon black, carbon nanofibers, carbon nanotubes, fluorinated carbon, metal powder, potassium titanate, zinc oxide, titanium oxide, and polyphenylene derivatives.

[0111] The above conductive material may include a linear conductive material. The above conductive material may include a linear conductive material having a length of 10 μm or more.

[0112] The above-mentioned linear conductive material comprises a conductive material having a fibrous structure, such as a cylindrical type, a tube type, or a fiber type, and may include, for example, carbon nanotubes, carbon nanofibers, nanofibers, or combinations thereof, but is not limited thereto.

[0113] For example, the conductive material may include a linear conductive material having a lower limit selected from 11 μm or more, 12 μm or more, 13 μm or more, 14 μm or more, 15 μm or more, 16 μm or more, 17 μm or more, 18 μm or more, 19 μm or more, or 20 μm or more, and may include a linear conductive material having an upper limit selected from 30 μm or less, 29 μm or less, 28 μm or less, 27 μm or less, 26 μm or less, 25 μm or less, 24 μm or less, 23 μm or less, 22 μm or less, 21 μm or less, 20 μm or less, 19 μm or less, 18 μm or less, 17 μm or less, 16 μm or less, or 15 μm or less. When the conductive material satisfies the above ranges, it can form an electron conduction network within the anode to improve electron conductivity.

[0114] The conductive material may typically be included in an amount of 0.1 weight% or more to 30 weight% or less with respect to the total weight of the anode material layer, specifically 0.5 weight% or more to 20 weight% or less, and more specifically 1 weight% or more to 10 weight% or less.

[0115] The above binder serves to improve contact between positive active materials or between positive active materials and positive components, and to improve adhesion between positive active materials and positive current collectors. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA), polyacrylonitrile (PAN), carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone (PVP), polytetrafluoroethylene (PTFE), polyethylene (PE), polypropylene (PP), ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these alone or a mixture of two or more may be used. For example, the binder may include at least one selected from the group consisting of acrylic binders, polyolefin binders, polyvinyl alcohol binders, polyvinylidene fluoride binders, polytetrafluoroethylene binders, and butadiene rubber binders.

[0116] The above binder may include a fibrous binder. The fibrous binder is a binder that undergoes fibrillation under specific conditions above a phase transition temperature, and when the above binder is included, it can serve as a support, sustain, and / or adhesive between the components included in the anode. Furthermore, by using such a fibrous binder, it is possible to manufacture a solvent-free dry anode. Specifically, the binder may include a polytetrafluoroethylene (PTFE)-based binder, but is not limited thereto.

[0117] The binder may be included in an amount of 0.1 weight% or more to 30 weight% or less with respect to the total weight of the anode material layer, specifically 0.5 weight% or more to 20 weight% or less, and more specifically 1 weight% or more to 10 weight% or less.

[0118] The anode material layer may further include additives. The additives may further include, for example, fillers, coating agents, dispersants, thickeners, ion conductivity aids, etc., and any known material generally used in electrodes may be used without limitation.

[0119] The thickness of the anode material layer may be 50 μm or more to 500 μm or less. For example, the thickness of the anode material layer may be 55 μm or more to 400 μm or less, 60 μm or more to 300 μm or less, 65 μm or more to 200 μm or less, or 70 μm or more to 100 μm or less, but is not limited thereto.

[0120] The above anode can be manufactured according to a conventional anode manufacturing method. For example, it can be manufactured by applying a composition for forming an anode material layer, comprising the above anode active material, binder, and conductive material, onto an anode current collector, and then drying and rolling.

[0121] The step of applying the above-mentioned composition for forming the anode material layer can be performed using a general coating formation method. For example, wet coating methods such as gravure coating, slot die coating, spin coating, spray coating, bar coating, and immersion coating; and dry coating methods such as thermal evaporation, electron beam evaporation, chemical vapor deposition (CVD), and sputtering may be used, but are not limited thereto.

[0122] The above anode can be manufactured by a wet process method. For example, the composition for forming the anode material layer may further include a solvent, and the types and contents of the anode active material, binder, conductive material, and additive are as described above.

[0123] The above solvent may be a solvent commonly used in the relevant technical field, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water, and one of these alone or a mixture of two or more may be used. The amount of the above solvent used is sufficient if it is sufficient to dissolve or disperse the anode active material composite, conductive material, binder, etc., considering the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that can exhibit excellent thickness uniformity when coated for anode manufacturing thereafter.

[0124] The above anode may also be manufactured by casting the composition for forming the anode material layer onto a separate support, and then laminating the film obtained by peeling off from the support onto an anode current collector.

[0125] The above anode can be manufactured by a dry process method capable of implementing high loading. For example, the above anode can be manufactured by a fiberization method. A composition for forming an anode material layer containing the above anode active material can be manufactured by including a calendering or sheeting process using a roll, but is not limited thereto.

[0126] For example, the anode can be manufactured by a method for manufacturing an anode comprising: (A) a step of forming an anode material layer; and (B) a step of stacking the anode material layer and the anode current collector.

[0127] Specifically, the step of forming the (A) anode material layer may include (a) mixing the anode active material, the conductive material, and the binder, and then forming them into a film shape through a sheeting / calendaring process.

[0128] In step (a) above, an anode material layer can be formed by mixing the anode active material, conductive material, and binder, and then forming them into a film shape through a sheeting / calendering step. At this time, the binder becomes fibrous through the sheeting / calendering step.

[0129] The above-mentioned sheeting / calendering process may utilize one or more pairs of rollers. By utilizing one or more pairs of rollers in the above-mentioned sheeting / calendering process, the binder can be fiberized by sheeting and formed into a film by calendering. At the same time, the thickness of the film can be controlled through the one or more pairs of rollers.

[0130] The above-mentioned sheeting / calendering process may be performed at a temperature of 20°C or higher and 200°C or lower. Specifically, the range may consist of a lower limit selected from 20°C or higher, 30°C or higher, 40°C or higher, 50°C or higher, 60°C or higher, 70°C or higher, or 80°C or higher, and an upper limit selected from 200°C or lower, 180°C or lower, 160°C or lower, 140°C or lower, 120°C or lower, or 100°C or lower. If the temperature of the above-mentioned sheeting / calendering process is below 20°C, the fiberization of the binder occurs less, and the strength of the anode material layer may decrease; if it exceeds 200°C, the strength of the anode material layer may not increase further even if the temperature increases, or there is a risk of deterioration of the raw materials.

[0131] The above sheeting / calendering process may be performed for 1 loop or more and 50 loops or less. Specifically, if the number of loops of the above sheeting / calendering process is less than 1 loop, the binder may not be fiberized, and if it exceeds 50 loops, fiberization may proceed excessively, so the strength of the anode material layer may not increase further or processability may deteriorate. Specifically, the number of loops of the above sheeting / calendering process may be a range consisting of one lower limit selected from 1 or more, 5 or more, 10 or more, 15 or more, 20 or more, 23 or more, or 25 or more, and one upper limit selected from 50 or less, 45 or less, 40 or less, 35 or less, or 30 or less.

[0132] The orientation of the above-mentioned sheeting / calendering process can be performed uniaxially or biaxially. Here, uniaxial means that the sheeting / calendering proceeds in one direction, and biaxial means that after performing sheeting / calendering in one direction, sheeting / calendering is performed alternately in the horizontal and vertical directions of the anode material layer. When the above-mentioned sheeting / calendering process is performed biaxially, fiberization can proceed evenly in multiple directions, thereby further improving the strength of the anode material layer.

[0133] The step of stacking the (B) anode material layer and the anode current collector may include the step of manufacturing a dry anode by stacking the anode material layer formed in the (A) step onto at least one surface of the anode current collector.

[0134] The above positive active material may be included in an amount of 60% or more to 90% or less based on the total weight of the positive material layer. Specifically, the above-mentioned positive active material comprises, based on the total weight of the positive material layer, one lower limit selected from 60 wt% or more, 61 wt% or more, 62 wt% or more, 63 wt% or more, 64 wt% or more, 65 wt% or more, 66 wt% or more, 67 wt% or more, 68 wt% or more, 69 wt% or more, 70 wt% or more, 71 wt% or more, 72 wt% or more, 73 wt% or more, 74 wt% or more, 75 wt% or more, 76 wt% or more, 77 wt% or more, 78 wt% or more, 79 wt% or more, or 80 wt% or more, and 90 wt% or less, 89 wt% or less, 88 wt% or less, 87 wt% or less, 86 wt% or less, 85 wt% or less, 84 wt% or less, 83 wt% or less, 82 wt% or less, 81 wt% or less, 80 wt% or less, It may be included in a range consisting of one upper limit selected from 79 wt% or less, 78 wt% or less, 77 wt% or less, 76 wt% or less, 75 wt% or less, 74 wt% or less, 73 wt% or less, 72 wt% or less, 71 wt% or less, or 70 wt% or less. If the content of the positive electrode active material satisfies the above range, the lifespan or performance of the secondary battery can be improved.

[0135] The modulus of the anode material layer may be 35 MPa or more. The modulus of the anode material layer may be 35 MPa or more to 100 MPa or less. For example, the modulus of the anode material layer comprises one lower limit selected from 35 MPa or more, 36 MPa or more, 37 MPa or more, 38 MPa or more, 39 MPa or more, 40 MPa or more, 41 MPa or more, 42 MPa or more, 43 MPa or more, 44 MPa or more, 45 MPa or more, 46 MPa or more, 47 MPa or more, 48 MPa or more, 49 MPa or more, 50 MPa or more, 51 MPa or more, 52 MPa or more, or 53 MPa or more, and 100 MPa or less, 99 MPa or less, 98 MPa or less, 97 MPa or less, 96 MPa or less, 95 MPa or less, 94 MPa or less, 93 MPa or less, 92 MPa or less, 91 MPa or less, 90 MPa or less, 89 MPa or less, 88 MPa or less, 87 It can satisfy a range consisting of one upper limit selected from MPa or less, 86 MPa or less, 85 MPa or less, 84 MPa or less, 83 MPa or less, 82 MPa or less, 81 MPa or less, 80 MPa or less, 79 MPa or less, 78 MPa or less, 77 MPa or less, 76 MPa or less, 75 MPa or less, 74 MPa or less, 73 MPa or less, 72 MPa or less, 71 MPa or less, or 70 MPa or less. The modulus of the anode material layer can be measured using a microindenter. For example, Anton Paar's MCT 3The step 300 equipment may be used, but is not limited thereto. Specifically, the anode material layer is heated, and an indenter jig is lowered over the anode material layer to measure in compression mode, and the modulus can be measured by measuring the degree of change in strain relative to the applied stress. When the modulus of the anode material layer satisfies the above range, the final physical properties of the electrode through a rolling process or a calendering process can be provided at a level higher than the desired level.

[0136] The elongation rate of the anode material layer may be 5% or less. The elongation rate of the anode material layer may be 1% or more to 5% or less. For example, the elongation rate of the anode material layer is one lower limit selected from 1% or more, 1.1% or more, 1.2% or more, 1.3% or more, 1.4% or more, 1.5% or more, 1.6% or more, 1.7% or more, 1.8% or more, 1.9% or more, 2% or more, 2.1% or more, 2.2% or more, 2.3% or more, 2.4% or more, 2.5% or more, 2.6% or more, 2.7% or more, 2.8% or more, 2.9% or more, or 3% or more, and 5% or less, 4.9% or less, 4.8% or less, 4.7% or less, 4.6% or less, 4.5% or less, 4.4% or less, 4.3% or less, 4.2% or less, 4.1% or less, 4% or less, 3.9% or less, 3.8% or less, It can satisfy a range consisting of one upper limit selected from 3.7% or less, 3.6% or less, 3.5% or less, 3.4% or less, 3.3% or less, 3.2% or less, 3.1% or less, or 3% or less. The elongation of the anode material layer can be measured using a microindenter. For example, Anton Paar's MCT 3Step 300 equipment may be used, but is not limited thereto. When the elongation rate of the anode material layer satisfies the above range, the quality after bonding onto the anode current collector can be improved, and it is possible to manufacture an electrode with desired physical properties during the rolling or calendering process.

[0137] The above anode material layer may include a dry anode sheet. The dry anode sheet may be manufactured by the aforementioned dry process method, but is not limited thereto. The concept of the dry anode sheet includes a dry anode film.

[0138] Another embodiment of the present invention may provide a secondary battery. The secondary battery may include the aforementioned positive electrode. In addition to the aforementioned positive electrode, the secondary battery may include a negative electrode and a separator disposed between the positive electrode and the negative electrode.

[0139] The above cathode may include a cathode current collector and a cathode material layer included on at least one surface of the cathode current collector.

[0140] The above-mentioned negative current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel (e.g., SUS), aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface treated or coated with carbon, nickel, titanium, or silver, or aluminum-cadmium alloy may be used.

[0141] The above-mentioned negative current collector can typically have a thickness of 3 μm or more to 500 μm or less, and, similar to the positive current collector, fine irregularities can be formed on the surface of the negative current collector to strengthen the bonding force of the negative active material. For example, it can be used in various forms such as a film, sheet, foil, net, porous body, foam, or nonwoven fabric.

[0142] The above-mentioned cathode material layer may optionally include a binder, a conductive material, and / or additives, etc., together with the cathode active material. The above-mentioned cathode material layer may be manufactured, for example, by applying a composition for forming a cathode material layer containing the cathode active material, etc., onto a cathode current collector and drying it, or by casting the composition for forming a cathode material layer onto a separate support and then laminating the film obtained by peeling it off from the support onto the cathode current collector. The composition for forming a cathode material layer may further include a solvent, and the solvent may be selected from examples of solvents included in the aforementioned composition for forming an anode material layer.

[0143] As the above-mentioned negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, or amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Ag, Au, In alloys, Si alloys, Sn alloys, or Al alloys; SiO₂ β Examples include metal oxides capable of doping and dedoping lithium, such as (0<β≤2), SnO2, vanadium oxide, or lithium vanadium oxide; or the above metallic compounds, such as Si-C complexes or Sn-C complexes; or complexes thereof, and any one or more of these may be used. Additionally, a metallic lithium thin film may be used as the negative electrode active material.

[0144] The above carbonaceous materials may include both low-crystallinity carbon and high-crystallinity carbon. Representative examples of low-crystallinity carbon include soft carbon and hard carbon, while representative examples of high-crystallinity carbon include amorphous, plate-like, flake-like, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, or high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.

[0145] In addition, the above carbonaceous material is amorphous carbon, inorganic material, or Si, SiO β (0<β≤2), it may be coated with a Si-based compound such as Si-C, and the carbonaceous material may be amorphous carbon, inorganic material, or Si, SiO β (0<β≤2), it may also exist in a mixed state mixed with Si-based compounds such as Si-C.

[0146] The thickness of the cathode material layer may be 10 μm or more to 500 μm or less. For example, the thickness of the cathode material layer may be 20 μm or more to 400 μm or less, 30 μm or more to 300 μm or less, 40 μm or more to 200 μm or less, or 50 μm or more to 100 μm or less, but is not limited thereto. Alternatively, the thickness of the cathode material layer may be, for example, 50 μm or more to 500 μm or less, 50 μm or more to 400 μm or less, 70 μm or more to 300 μm or less, or 80 μm or more to 200 μm or less, but is not limited thereto.

[0147] In another example, the above-mentioned cathode may be an anodeless cathode that does not contain a cathode active material that absorbs or releases lithium immediately after battery manufacturing or after discharge, and in which a lithium metal or lithium alloy is formed during the battery charging process to form the cathode active material.

[0148] In cases where the above-mentioned negative electrode active material is omitted, the negative electrode may include only a negative electrode current collector, or the negative electrode material layer included on the negative electrode current collector may include a lithium-affinity material. In cases where the negative electrode is an anodeless negative electrode, the negative electrode material layer may include a non-negative electrode coating layer containing a lithium-affinity material.

[0149] The above-mentioned cathode material layer may include a lithium-affinity material. The lithium-affinity material may include a material capable of forming an alloy or compound with lithium, and may include an element capable of forming an alloy or compound with lithium.

[0150] The above lithium-affinity material may include one or more lithium-affinity elements or lithium-affinity compounds. The lithium-affinity elements may include one or more selected from gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), indium (In), magnesium (Mg), aluminum (Al), bismuth (Bi), tin (Sn), chromium (Cr), copper (Cu), tungsten (W), germanium (Ge), lead (Pb), antimony (Sb), cobalt (Co), manganese (Mn), titanium (Ti), zirconium (Zr), iron (Fe), and zinc (Zn).

[0151] The above lithium-affinity compound may include one or more selected from lithium carbonate, lithium titanate, or oxides, nitrides, halides, sulfides, carbides, hydrides, cyanides, or hydroxides of the lithium-affinity element.

[0152] The above lithium-affinity material may include one or more lithium-affinity elements or lithium-affinity compounds, and the lithium-affinity elements may be one or more selected from gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), indium (In), magnesium (Mg), aluminum (Al), bismuth (Bi), tin (Sn), chromium (Cr), copper (Cu), tungsten (W), germanium (Ge), lead (Pb), antimony (Sb), and zinc (Zn), and the lithium-affinity compounds may be one or more selected from lithium carbonate, lithium titanate, or oxides, nitrides, halides, sulfides, carbides, hydrides, cyanides, or hydroxides of the lithium-affinity elements.

[0153] The lithium-affinity material may include a metal of the lithium-affinity element. The lithium-affinity material may include an alloy of the lithium-affinity element. Alternatively, the lithium-affinity material may include one or more compounds selected from oxides, nitrides, halides, sulfides, carbides, hydrides, cyanides, or hydroxides of the lithium-affinity element.

[0154] The above lithium-affinity material may include an alloy of the above lithium-affinity element, and an alloy of lithium and the above lithium-affinity element (Li-M 1 alloy), alloy of other metallic elements and the above lithium affinity element (M 1 -M 2 It may include two or more alloys selected from the above lithium affinity elements), or, but is not limited thereto. For example, Si-M 2 Alloy (M 2 is an alkali metal, alkaline earth metal, Group 13 element, Group 14 element, transition metal, rare earth element, or combination thereof, but is not Si) or Sn-M 2 Alloy (M 2may include alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, or combinations thereof (but not Sn), etc. The above M 2 may be Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof, and said M 1 It may be gold (Au), platinum (Pt), palladium (Pd), silicon (Si), silver (Ag), indium (In), magnesium (Mg), aluminum (Al), bismuth (Bi), tin (Sn), chromium (Cr), copper (Cu), tungsten (W), germanium (Ge), lead (Pb), antimony (Sb), cobalt (Co), manganese (Mn), titanium (Ti), zirconium (Zr), iron (Fe), zinc (Zn), or a combination thereof.

[0155] For example, the lithium-affinity compound is copper(I) oxide (Cu2O), copper(II) oxide (CuO), zinc oxide (ZnO), cobalt(II) oxide (CoO), cobalt(III) oxide (Co2O3), manganese(II) oxide (MnO), manganese(III) oxide (Mn2O3), silicon oxide (SiO2). x )(0≤x≤2), titanium dioxide (TiO2), aluminum oxide (Al2O3), zinc peroxide (ZnO2), indium oxide (In2O3), silver titanate (AgTiO3), aluminum titanate (Al2TiO5), dicalcium silicate (Ca2SiO4), lithium titanate (Li4Ti5O 12Metal oxides such as ), niobium pentoxide (Nb2O5), LLZO-based (Li-La-Zr-O) compounds, LLZTO-based (Li-La-Zr-Ta-O) compounds, LLTO-based (Li-La-Ti-O) compounds, LISICON (Lithium superionic conductor), LZPO-based (Li-Zr-PO) compounds, LZSP-based (Li-Zr-Si-PO) compounds, or LTPO-based (Li-Ti-PO) compounds; metal sulfides such as titanium sulfide (TiS2), iron sulfide (FeS), silver sulfide (Ag2S), indium sulfide (In2S3), copper sulfide (CuS), germanium sulfide (GeS), zinc sulfide (ZnS), germanium disulfide (GeS2), or tungsten disulfide (WS2); Metal nitrides such as titanium nitride (TiN), silicon nitride (Si3N4), lithium nitride (Li3N), lithium aluminum nitride (Li3AlN2), or lithium phosphate nitride (LiPON); metal fluorides such as lithium fluoride (LiF), silver fluoride (AgF), magnesium fluoride (MgF2), nickel fluoride (NiF2), zinc fluoride (ZnF2), manganese(II) fluoride (MnF2), manganese(III) fluoride (MnF3), lithium tetrafluoroaluminate (LiAlF4), lithium hexafluorophosphate (LiPF6), lithium hexafluoroarsenate (LiAsF6), lithium hexafluoroantimonate (LiSbF6), lithium tetrafluoroborate (LiBF4), and lithium difluoro(oxalato)borate (LiBF2(C2O4)). Metal carbides such as tungsten carbide (WC); or lithium chloride (LiCl), lithium bromide (LiBr), lithium iodide (LiI), lithium nitrate (LiNO3), lithium perchlorate (LiClO4), lithium decachlorodecarborate (Li2B 10 Cl 10It may include compounds such as lithium trifluoromethanesulfonate (LiCF3SO3), lithium trifluoroacetate (LiCF3CO2), lithium tetrachloroaluminate (LiAlCl4), lithium methanesulfonate (CH3SO3Li), lithium thiocyanate (LiSCN), lithium tris(trifluoromethanesulfonyl)methide (LiC(CF3SO2)3), lithium bis(trifluoromethanesulfonyl)imide ((CF3SO2)2NLi), lithium bis(fluorosulfonyl)imide ((FSO2)2NLi), lithium orthoborate (Li3BO3), lithium tetraborate (Li2B4O7), lithium metaborate (LiBO2), or lithium bis(oxalato)borate (LiB(C2O4)2), but is not limited thereto.

[0156] When including a lithium-affinity material as described above, it has the effect of suppressing lithium dendrite formation by lowering the lithium nucleation energy when lithium or lithium alloy is deposited or plated during charging and discharging.

[0157] In addition, the cathode material layer may further include a carbon material in addition to a lithium-affinity material, and the carbon material may include at least one selected from artificial graphite, natural graphite, graphitized carbon fiber, low-crystallinity carbon, high-crystallinity carbon, and amorphous carbon, and may serve to induce the formation of a metal layer containing lithium metal or a lithium alloy between the cathode material layer and the cathode current collector by transferring lithium ions supplied from the anode toward the direction of the negative current collector to which negative charge is supplied.

[0158] The above carbon material may include amorphous carbon and may be one or more selected from the group consisting of, for example, carbon black, acetylene black, furnace black, Ketjen black, and graphene, but is not limited thereto, and any amorphous carbon that can be used in all-solid-state batteries may be used without limitation.

[0159] The carbon material and the lithium-affinity material in the above-mentioned cathode material layer (non-cathode coating layer) may be included in a weight ratio of 1:1 or more to 10:1 or less, 1:1 or more to 5:1 or less, 1:1 or more to 4:1 or less, or 1.5:1 or more to 3:1 or less, but are not limited thereto.

[0160] The thickness of the above-mentioned non-cathode coating layer may be, for example, 1 μm or more to 100 μm or less, 5 μm or more to 80 μm or less, 10 μm or more to 50 μm or less, or 10 μm or more to 30 μm or less.

[0161] In the case where the above-mentioned negative electrode is an anodeless negative electrode, the secondary battery may precipitate lithium within the negative electrode during charging. Specifically, the secondary battery may further include a metal containing lithium or a lithium alloy and / or a metal layer thereof between the negative electrode current collector and the non-negative electrode coating layer, on the side of the non-negative electrode coating layer that does not face the separator, and / or within the non-negative electrode coating layer upon charging. The lithium alloy may be, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, a Li-Si alloy, etc., but is not limited thereto; any alloy used as a lithium alloy in the relevant technical field is acceptable.

[0162] The metal or metal layer included between the above-mentioned cathode current collector and the non-cathode coating layer, and / or within the non-cathode coating layer, may be composed of one of these alloys or lithium, or may be composed of various types of alloys.

[0163] The thickness of the metal layer containing the lithium or lithium alloy may be, for example, 1 μm or more to 1,000 μm or less, 1 μm or more to 500 μm or less, 1 μm or more to 200 μm or less, 1 μm or more to 150 μm or less, 1 μm or more to 100 μm or less, or 1 μm or more to 50 μm or less. When the metal layer satisfies the above range, it can perform the role of a lithium reservoir well and the cycle characteristics can be improved.

[0164] The above metal layer may be formed, for example, by precipitation between the negative current collector and the non-negative coating layer, or on the surface of the non-negative coating layer that does not face the separator, through charging after the assembly of the secondary battery. When the metal layer is formed by charging after the assembly of the secondary battery, the region between the negative current collector and the non-negative coating layer, or on the surface of the non-negative coating layer that does not face the separator, may, for example, be a lithium-free region that does not contain lithium in the initial state or after discharge of the secondary battery.

[0165] The above separator is interposed between the anode and the cathode and can serve to electrically insulate the anode and the cathode while allowing lithium ions to pass through. Any separator used in general secondary batteries can be used without particular restrictions, and it is particularly desirable that it has low resistance to the movement of electrolyte ions and excellent electrolyte moisture retention capacity.

[0166] Specifically, the above separator may be a porous polymer film, for example, a porous polymer film made of a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof. Alternatively, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fibers or polyethylene terephthalate fibers, may be used. Furthermore, a coated separator containing a ceramic material or a polymer material may be used to ensure heat resistance or mechanical strength, and may optionally be used in a single-layer or multi-layer structure. The separator may be omitted in some cases.

[0167] The above separator may have a thickness of 1 μm or more to 100 μm or less, or 5 μm or more to 50 μm or less. If the thickness of the separator is less than 1 μm, the function of the separator may not be fully exerted and deterioration of mechanical properties may occur, and if it exceeds 100 μm, the characteristics of the battery may deteriorate during high-rate charging and discharging.

[0168] In addition, the above membrane may have a porosity of 40% or more to 60% or less and may have an air permeability of 150 s / 100mL or more to 300 s / 100mL or less.

[0169] The above secondary battery may further include an electrolyte. Examples of the electrolytes that can be used in the manufacture of lithium secondary batteries include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, or molten inorganic electrolytes, but are not limited to these.

[0170] The above electrolyte may include, for example, an organic solvent and / or a lithium salt.

[0171] The above-mentioned organic solvent may be used without special restrictions as long as it can serve as a medium through which ions involved in the electrochemical reaction of a secondary battery can move, and the same applies to the aforementioned organic solvent.

[0172] In addition to the above electrolyte components, the above electrolyte may further include one or more additives for the purpose of improving the lifespan characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery, such as, for example, haloalkylene carbonate-based compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ether, ethylene diamine, n-glyme, triamide hexaphosphate, nitrobenzene derivative, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum trichloride. In this case, the above additives may be included in an amount of 0.1% by weight or more to 5% by weight or less based on the total weight of the electrolyte.

[0173] The above lithium salt can be used without special restrictions as long as it is a compound capable of providing lithium ions used in secondary batteries. For example, the above lithium salt is Li as a cation + It includes, and as anion, F - , Cl - , Br - , I - , NO3 - , N(CN)2 - , BF4 - , ClO4 - , AlO4 - , AlCl4 - , PF6 - , BF6 - , SF6 - , B 10 Cl 10 - , BF2C2O4 - , BC4O8 - , PF4C2O4 -, PF2C4O8 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , F3SO3 - , C4F9SO3 - , CF3CF2SO3 - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CH3SO3 - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - It may include at least one selected from a group consisting of

[0174] Specifically, the lithium salts mentioned above are LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 Examples include at least one selected from the group consisting of LiBOB (LiB(C2O4)2), LiCF3SO3, LiTFSI (LiN(SO2CF3)2), LiFSI (LiN(SO2F)2), LiCH3SO3, LiCF3CO2, LiCH3CO2, and LiBETI (LiN(SO2CF2CF3)2). Specifically, the lithium salt may include a single substance or a mixture of two or more selected from the group consisting of LiBF4, LiClO4, LiPF6, LiBOB (LiB(C2O4)2), LiCF3SO3, LiTFSI (LiN(SO2CF3)2), LiFSI (LiN(SO2F)2), and LiBETI (LiN(SO2CF2CF3)2).

[0175] The lithium salt may be included in the electrolyte at a concentration of 0.1 M or more and 4 M or less, specifically at a concentration of 0.1 M or more and 2 M or less, and more specifically at a concentration of 0.8 M or more and 1.6 M or less. When the lithium salt is included in the electrolyte at a concentration within the above range, the electrolyte has appropriate conductivity and viscosity, so it can exhibit excellent electrolyte performance, and lithium ions can move effectively, thereby improving the output characteristics of the secondary battery.

[0176] The above secondary battery may be pouch-type, prismatic, or cylindrical, and its shape and size may be applied without limitation as long as they are commonly used for secondary batteries. Additionally, the above secondary battery may further include a case capable of sealing the electrode assembly, such as a container, pouch, pack, or module, for housing the electrode assembly including the positive electrode, separator, and negative electrode. The case may optionally further include a sealing member.

[0177] The above secondary battery may be manufactured by manufacturing the positive electrode, separator, and negative electrode respectively, then stacking and / or laminating these layers, and then injecting an electrolyte, but is not limited thereto.

[0178] The charge capacity of the above secondary battery may be 153.5 mAh / g or more. Specifically, the above secondary battery may have an initial charge capacity of 153.5 mAh / g or more under 0.1C charge / discharge conditions, and specifically, it may be 153.5 mAh / g or more to 170.0 mAh / g or less. The initial charge capacity of the above secondary battery may serve as a measure for judging the performance of the secondary battery in the evaluation method of the secondary battery.

[0179] The present invention provides a battery module comprising the secondary battery as a unit cell, a battery pack comprising the battery module or the secondary battery, or an electric device comprising the battery pack as a power source.

[0180] The above electric device may include, but is not limited to, a power tool that moves by receiving power from an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.

[0181] One embodiment of the present invention is (S1) immersing the lower part of a holder containing a positive active material in an organic solvent, and the height (h) of the organic solvent penetrating into the pores within the holder by capillary action is time (t * A method for measuring the contact angle of an anode active material can be provided, comprising the steps of: (S2) measuring according to the organic solvent and the anode active material; and (S2) measuring the contact angle (θ) of the organic solvent and the anode active material from the above formula 1.

[0182] The above (S1) step involves immersing the lower part of a holder containing a positive active material in an organic solvent, and the height (h) of the organic solvent penetrating into the pores within the holder by capillary action is measured over time (t * It is a step of measuring according to ).

[0183] The above step (S1) is performed by the height (h) of the organic solvent at time (t * The method may include a step of calculating the average slope value β from a graph obtained by fitting the result values ​​measured according to ). Specifically, the step (S1) measures the height (h) of the organic solvent at time (t *It may include a step of calculating the slope from a graph obtained by fitting the result values ​​measured according to ). Then, the average value of the calculated slope can be calculated as the β value.

[0184] The average value of the slope above may refer to the average value measured from the graph fitted from the measurement results obtained by repeating step (S1) three or more times. Specifically, the average value of the slope (β) above may use the average value of the β values ​​obtained from the results obtained by repeating step (S1) three or more times and ten or fewer times.

[0185] The above β value may be 0.7 or higher to 1 or lower, or 0.7 or higher to 0.9 or lower. When the above β value is measured within the above range, the capillary phenomenon occurring in the positive electrode active material is accurately reflected, and the performance of the positive electrode or secondary battery can be confirmed from the contact angle (θ) between the positive electrode active material and the organic solvent.

[0186] Subsequently, after the above step (S1), (S1-1) the height (h) of the organic solvent to which the above β value is applied (t * ) β It may include a step of calculating ξ0, which is the average value of the slope, from a graph obtained by fitting the result values ​​measured according to . Specifically, from the β value obtained in step (S1), (t * ) β The ξ0 value can be calculated by calculating the average value of the slope from a new graph fitted with the height (h) of the organic solvent for .

[0187] Similar to calculating the β value, the above ξ0 value can also be measured as the average value of the slope measured at each unit time within a range from 0 or greater to τ or less, and the unit time can be appropriately adjusted according to the magnitude of the τ value. The average value of the slope (ξ0) is the height (h) of the organic solvent (t * ) βThe average value of ξ0 obtained from the measurement results obtained by repeating the step of calculating the average value of the slope, ξ0, from a graph obtained by fitting the result value measured according to the method 3 or more times and 10 or fewer times can be used.

[0188] In the above step (S1), the method may include a step of pressurizing the received positive active material so that the porosity inside the holder receiving the positive active material is 30% or more to 50% or less. Additionally, in the above step (S1), the average radius (r) of the void inside the holder receiving the positive active material c It may include a step of pressurizing the positive active material received so that the thickness is 30 nm or more to 50 nm or less.

[0189] The above step (S2) may include the step of measuring the contact angle (θ) between the organic solvent and the positive active material using Equation 1. Equation 1 represents the cosine value of the contact angle (θ) between the organic solvent and the positive active material, and can be obtained by substituting the ξ0 value obtained in the above step (S1).

[0190] The contents regarding the above-mentioned positive active material, organic solvent, holder, etc., can be applied in the same way as those described in the aforementioned positive active material, organic solvent, holder, etc.

[0191] In addition, another embodiment of the present invention includes the step of measuring the contact angle (θ) between an organic solvent and a positive active material according to the aforementioned method for measuring the contact angle of a positive active material; and can improve the performance of a positive or secondary battery containing the positive active material based on the measured contact angle (θ).

[0192] That is, if the contact angle (θ) between the organic solvent and the positive active material deviates from a predetermined reference value based on the above-mentioned measured contact angle (θ), the performance of the secondary battery containing the positive active material is determined to be poor, and the performance of the secondary battery can ultimately be improved by adjusting the organic solvent and the positive active material so that the contact angle (θ) is included within the predetermined reference value.

[0193] In the following, the present invention is described in detail with reference to examples to specifically explain the disclosure of the present invention as described above and the intended functions and effects of the present invention. However, the examples may be modified in various different forms, and the scope of this specification is not to be interpreted as being limited only to these examples. It is emphasized that the examples are provided to represent the present invention and to explain it more specifically to those skilled in the art.

[0194]

[0195] <Examples 1 to 6 and Comparative Examples 1 to 2> Preparation of positive electrode active material

[0196] A lithium carbonate precursor (Li2CO3), an iron precursor (FeC2O4·2H2O), a phosphoric acid precursor ((NH4)2HPO4), and carbon were mixed in butanediol, a reaction solvent, and a mixed powder was prepared under conditions of 150°C to 200°C. This mixed powder was calcined at 700°C to 900°C for 10 to 20 hours under an N2 atmosphere to prepare an LFP cathode active material with carbon coated on the surface of the active material core.

[0197] The LFP cathode active material of Table 1 was prepared by adjusting the composition and content of the above precursor, the mixing temperature conditions of the mixed powder, and the calcination temperature and calcination time conditions of the mixed powder differently.

[0198] The carbon coating content was analyzed using a Brucker CS / ONH analyzer (G4 phoenix).

[0199] Tap density was measured after applying a constant force using Micromeritics' GeoPyc equipment.

[0200] BET specific surface area was measured using a Micromeritics 3Flex instrument (KS A ISO 9277).

[0201] The elemental content of the active material was analyzed using Perkin Elmer’s AVIO 550max instrument (ICP analysis instrument) to analyze the elemental content of Li, Fe, and P in the active material.

[0202] 2.0 g of the prepared cathode active material was placed in each sample holder, and a push bar was used to raise the height of the cathode active material to 2.0 cm. After immersing the prepared sample holder in dimethyl carbonate (DMC), the height of the DMC absorbed by capillary action was measured every 1 second. The contact angle (θ) obtained by substituting the β and ξ0 values ​​obtained from the fitted graph from the measurement results into Equation 1 is listed in Table 1. The porosity inside the sample holder was calculated from the mass of the absorbed solvent (DMC) (measured value), and the average value was presented after 10 measurements.

[0203] τ = 60 seconds

[0204] η (viscosity of DMC) = 0.0006250 Ns / m 2 (@25℃)

[0205] h ∞ (Maximum height DMC can penetrate into the air gap within the holder) = 0.55 m

[0206] γ(Surface tension of DMC) = 0.02850 N / m(@25℃)

[0207] Classification Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Carbon Coating Content (wt%) 1.2 1.19 1.2 1.2 1.2 1.2 1.2 Particle Size (D50) (㎛) 1.05 1.05 1.1 1.1 1.05 1.05 Tap Density (g / cm³)3 )1.49 1.52 1.45 1.51 1.47 1.43 1.53 1.46BET Specific surface area (m 2 / g)10.110.910.410.210.710.610.610.5Li (wt%)4.514.654.64.644.544.614.74.54Fe (wt%)33.934.834.333.933.834.234.434.2P (wt%)19.419.719.319.919.419.419.219.3r c (m)40.9 x 10 -9 42.9 x 10 -9 43.4 x 10 -9 41.7 x 10 -9 41.4 x 10 -9 41.6 x 10 -9 42.1 x 10 -9 42.6 x 10 -9 β0.780.80.750.740.790.780.820.84ξ00.01040.01070.01050.01020.010150.01020.011650.0118cosθ0.5 8480.59010.56170.55170.55030.55300.71290.7228 Contact angle (θ)54.2°53.8°55.8°56.5°56.6°56.4°44.5°43.7°

[0208]

[0209] <Experimental Example 1>

[0210] Preparation of anode slurry

[0211] A positive electrode slurry was prepared by mixing the positive electrode active material of Examples 1 to 6 and Comparative Examples 1 to 2, carbon nanotubes as a conductive material, and PVdF (Mw. 670000 g / mol) as a binder in NMP (N-methyl pyrrolidone). The positive electrode active material : conductive material : binder in the positive electrode slurry were mixed in a weight ratio of 97 : 1 : 2, and the positive electrode slurry was prepared by mixing at 3000 rpm for 60 minutes.

[0212] Manufacturing of anodes

[0213] An aluminum foil (thickness: 15 μm) was prepared as the anode current collector, and an anode slurry was coated onto the surface of the prepared foil using a slot-die coater. Subsequently, the anode was manufactured by drying in a vacuum oven at 130°C and then rolling. At this time, the loading amount of the anode active material was 450 mg / 25 cm². 2 It was set to.

[0214] Preparation of cathode slurry

[0215] A negative electrode active material was used by mixing artificial graphite and natural graphite in a weight ratio of 5:5. Carbon black was used as the conductive agent, and a mixed binder was used by mixing SBR and CMC in a weight ratio of SBR : CMC = 2.2 : 1.1. A negative electrode slurry was prepared by mixing the negative electrode active material : conductive agent : mixed binder in water in a weight ratio of 95.9 : 0.8 : 3.3.

[0216] Manufacturing of the cathode

[0217] A copper thin sheet (thickness: 8 µm) was prepared as a cathode current collector, and a cathode slurry was coated onto the surface of the prepared sheet using a slot-die coater. Subsequently, the cathode was manufactured by drying in a vacuum oven at 130°C and then rolling. At this time, the loading amount of the cathode active material was 270 mg / 25 cm². 2 It was set to.

[0218] Battery manufacturing

[0219] An electrode assembly was fabricated by placing the anode and cathode prepared above facing each other and interposing a separator made of 15 μm polypropylene between the anode and cathode. The electrode assembly was placed in a case, and an electrolyte (EC : DMC : DEC = 1 : 1 : 1 volume ratio) was injected into the case to manufacture a secondary battery.

[0220]

[0221] Table 2 shows the results of evaluating the initial charge capacity of the manufactured secondary battery by charging it at 60°C under CC / CV, 0.1 C conditions to 4.25V and 0.05 C cut-off conditions, and then discharging it to 3.0V under CC, 0.1 C conditions.

[0222] Classification Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Comparative Example 2 Contact Angle (θ) 54.2° 53.8° 55.8° 56.5° 56.6° 56.4° 44.5° 43.7° Initial Charge Capacity (mAh / g, 0.1C) 153.7 154.6 155.0 155.6 155.8 156.1 153.0 152.8

[0223]

[0224] As shown in Table 2, it was confirmed that the initial charge capacity of the secondary battery containing the positive active material of Examples 1 to 6, which has a contact angle (θ) of 50˚ or more, was significantly superior to that of Comparative Examples 1 to 2.

[0225]

[0226] <Examples 7 to 11 and Comparative Examples 3 to 5> Preparation of positive electrode active material

[0227] A lithium carbonate precursor (Li2CO3), an iron precursor (FeC2O4·2H2O), a phosphoric acid precursor ((NH4)2HPO4), and carbon were mixed in butanediol, a reaction solvent, and a mixed powder was prepared under conditions of 150°C to 200°C. This mixed powder was calcined at 700°C to 900°C for 10 to 20 hours under an N2 atmosphere to prepare an LFP cathode active material with carbon coated on the surface of the active material core.

[0228] The LFP cathode active material of Table 3 was prepared by adjusting the composition and content of the above precursor, the mixing temperature conditions of the mixed powder, and the calcination temperature and calcination time conditions of the mixed powder differently.

[0229] The carbon coating content was analyzed using a Brucker CS / ONH analyzer (G4 phoenix).

[0230] BET specific surface area was measured using a Micromeritics 3Flex instrument (KS A ISO 9277).

[0231]

[0232] 2.0 g of each prepared cathode active material was placed in a sample holder, and a push bar was used to raise the height of the cathode active material to 2.0 cm. After immersing the prepared sample holder in dimethyl carbonate (DMC) solvent, the height of the DMC solvent absorbed by capillary action was measured every 1 second. The contact angle (θ) obtained by substituting the β and ξ0 values ​​obtained from the fitted graph from the measurement results into Equation 1 is listed in Table 3. Measurements were repeated a total of 10 times for each sample, and the average values ​​are listed in Table 3. The porosity inside the sample holder was calculated from the mass of the absorbed solvent (DMC) (measured value), and the average value was presented after 10 measurements.

[0233] τ = 60 seconds

[0234] η (viscosity of DMC) = 0.0006250 Ns / m 2 (@25℃)

[0235] h ∞ (Maximum height DMC can penetrate into the air gap within the holder) = 0.55 m

[0236] γ(Surface tension of DMC) = 0.02850 N / m(@25℃)

[0237] Classification Example 7 Example 8 Example 9 Example 10 Example 11 Comparative Example 3 Comparative Example 4 Comparative Example 5 Carbon Coating Content (wt%) 1.5 1.5 1.5 1.4 9 1.5 1.5 2 1.5 2 1.4 8 Particle Size (D50) (㎛) 1.1 8 1.1 7 1.1 6 1.1 5 1.1 9 1.2 2 1.2 1 1.1 7 BET Specific Surface Area (m² 2 / g)11.111.511.312.111.811.71212.1r c (m)41.4 x 10-9 43.0 x 10 -9 42.5 x 10 -9 41.2 x 10 -9 40.5 x 10 -9 41.5 x 10 -9 40.9 x 10 -9 41.7 x 10 -9 β0.80.760.780.820.850.770.770.76ξ00.01070.01020.01030.00930.00940.01170.0120.0122cosθ0.61 200.53470.55200.46420.48240.72900.77850.7893Contact angle (θ)52.3°57.7°56.5°62.3°61.2°43.2°38.9°37.9°

[0238]

[0239] <Experimental Example 2>

[0240] Manufacturing of dry anode films

[0241] 950 g of the positive active material of Examples 7 to 11 and Comparative Examples 3 to 5, 20 g of carbon black as a conductive material, and 40 g of PTFE (Polytetrafluoroethylene) as a binder were put into a blender and mixed for 15 minutes to prepare a positive composite material composition. Subsequently, the composite material composition was put into a kneader and kneaded at a temperature of 180°C at a speed of 80 rpm for 5 minutes to prepare an aggregate, and the aggregate was ground in a blender at a speed of 10,000 rpm for 1 minute to prepare a powder for the positive electrode.

[0242] Subsequently, in a roll-to-roll process, the anode powder was fed into a wrap roll press (roll diameter 200 nm, roll temperature 80°C, speed ratio 20 / 40 rpm) to perform powder sheeting and manufacture a film. Afterward, calendering was performed, and the anode was laminated with a primer-coated aluminum foil and arranged to be laminated onto an aluminum current collector. Subsequently, a dry anode film with a porosity of 27% was manufactured through a rolling process.

[0243]

[0244] The degree of crystallinity, modulus, and elongation of the manufactured dry anode film were evaluated, and the results are shown in Table 4.

[0245] The degree of crystallinity was measured using TA's DSC25 instrument (ASTM D3418).

[0246] Modulus and strain are Anton Paar's Microindenter (MCT 3 It was measured using ) (ASTM E384).

[0247] Classification Example 7 Example 8 Example 9 Example 10 Example 11 Comparative Example 3 Comparative Example 4 Comparative Example 5 Contact Angle (θ) 5 2.3° 5 7.7° 5 6.5° 6 2.3° 6 1.2° 4 3.2° 3 8.9° 3 7.9° Degree of Crystallinity (%) 10 8 9 1 17 15 2 2 17 Modulus of Dry Anode Film (MPa) 3 8 4 3 5 5 5 0 6 2 2 8 1 5 11 Elongation of Dry Anode Film (%) 4 3 8 3 3 7 3 5 2 8 5 7 6 7 7

[0248]

[0249] As shown in Table 4, when a dry cathode film was manufactured using the cathode active materials of Examples 7 to 11, which have a contact angle (θ) of 50˚ or more, the degree of crystallinity was low, the modulus was 35 MPa or higher, and the elongation was 5% or lower, so it was possible to manufacture a cathode by laminating it onto a cathode current collector. However, when using the cathode active materials of Comparative Examples 3 to 5, the degree of crystallinity was high, making it difficult to manufacture a film, and the modulus was less than 35 MPa and the elongation was greater than 5%, so the final physical properties of the cathode (porosity, thickness, etc.) through a rolling process or a calendering process could not be achieved.

[0250]

[0251] <Experimental Example 3>

[0252] Manufacturing of anodes

[0253] A dry anode film of Experimental Example 2 was prepared.

[0254] Manufacturing of the cathode

[0255] A negative electrode active material was used by mixing artificial graphite and natural graphite in a weight ratio of 5:5. Carbon black was used as the conductive agent, and a mixed binder was used by mixing SBR and CMC in a weight ratio of SBR : CMC = 2.2 : 1.1. A negative electrode slurry was prepared by mixing the negative electrode active material : conductive agent : mixed binder in water in a weight ratio of 95.9 : 0.8 : 3.3.

[0256] A copper thin sheet (thickness: 8 µm) was prepared as a cathode current collector, and a cathode slurry was coated onto the surface of the prepared sheet using a slot-die coater. Subsequently, the cathode was manufactured by drying in a vacuum oven at 130°C and then rolling. At this time, the loading amount of the cathode active material was 270 mg / 25 cm². 2 It was set to.

[0257] Battery manufacturing

[0258] An electrode assembly was fabricated by placing the above-mentioned positive and negative electrodes facing each other and interposing a separator made of 15 μm polypropylene between the positive and negative electrodes. The electrode assembly was placed in a case, and an electrolyte (EC : DMC : DEC = 1 : 1 : 1 volume ratio) was injected into the case to manufacture a secondary battery.

[0259]

[0260] The initial charge capacity of the manufactured secondary battery was evaluated by charging it at 60°C under CC / CV, 0.1 C conditions to 4.25V and 0.05 C cut-off conditions, and then discharging it to 3.0V under CC, 0.1 C conditions, and the results are shown in Table 5.

[0261] Classification Example 7 Example 8 Example 9 Example 10 Example 11 Comparative Example 3 Comparative Example 4 Comparative Example 5 Contact Angle (θ) 5 2.3° 5 7.7° 5 6.5° 6 2.3° 6 1.2° 4 3.2° 3 8.9° 3 7.9° Initial Charge Capacity (mAh / g, 0.1C) 1 5 7.3 1 5 7.8 1 5 5.5 1 5 9.1 1 5 4.5 1 5 2 1 5 1.1 1 5 0.8

[0262]

[0263] As shown in 5, it was confirmed that the initial charge capacity of the secondary battery containing the positive active material of Examples 7 to 11, which has a contact angle (θ) of 50˚ or more, was significantly superior to that of Comparative Examples 3 to 5.

Claims

1. The contact angle (θ) with the organic solvent is expressed by the following Equation 1, and A positive active material having a contact angle (θ) of 50˚ or more to 65˚ or less: [Equation 1] cosθ = {2η(ξ0h ∞ ) 2 } / (r c (g) In Equation 1, the height (h) of the organic solvent that penetrates into the pores within the holder by capillary action when the lower part of the holder containing the positive active material is immersed in the organic solvent is the time (t * When measuring according to ), η is the viscosity of the organic solvent, and ξ0 is (t * ) β It is the average value of the slope of the graph fitted to the height (h) for, and t * is t / τ, where t is the immersion time, and τ is a constant selected from 60 to 180 seconds, and β is t * It is the average value of the slope of the graph fitted to the height (h) for, and h ∞ is the maximum height at which an organic solvent can penetrate into the pores within the holder, and r c is the average radius of the air gap within the holder, and γ is the surface tension of the organic solvent.

2. In Paragraph 1, The above positive active material is a positive active material comprising a lithium transition metal phosphate.

3. In Paragraph 1, The above positive active material comprises an active material core portion and a carbon material layer provided on at least a portion of the surface of the active material core portion.

4. In Paragraph 3, The above carbon material layer comprises 0.5 parts by weight or more to 2 parts by weight or less of a carbon-based material with respect to 100 parts by weight of the above active material core portion, an anode active material.

5. In Paragraph 1, A positive active material having an average particle size (D50) of primary particles of the above positive active material of 0.5 μm or more to 5 μm or less.

6. In Paragraph 1, The tap density of the above positive active material is 0.5 g / cm³ 3 0 to 5 g / cm² 3 Lee Ha-in, positive electrode active material.

7. In Paragraph 1, The specific surface area of ​​the above positive active material is 5 m² 2 / g or more to 15 m 2 Anode active material with a g or less.

8. In Paragraph 1, The above organic solvent comprises one or more selected from ester-based solvents, lactam-based solvents, ether-based solvents, ketone-based solvents, aromatic hydrocarbon-based solvents, carbonate-based solvents, alcohol-based solvents, nitrile-based solvents, amide-based solvents, dioxolane-based solvents, and sulfolane-based solvents, forming an anode active material.

9. In Paragraph 1, A positive active material having a porosity of 30% or more to 50% or less of the holder containing the positive active material.

10. In Paragraph 1, The average radius (r) of the void within the holder containing the above positive active material c ) is a positive active material having a length of 30 nm or more to 50 nm or less.

11. An anode comprising an anode material layer comprising the anode active material of claim 1; a binder; and a conductive material.

12. In Paragraph 11, An anode having a modulus of 35 MPa or more of the anode material layer.

13. In Paragraph 11, An anode having an elongation rate of 5% or less of the anode material layer.

14. In Paragraph 11, The anode material layer comprises a dry anode sheet, an anode.

15. A secondary battery comprising the positive electrode of paragraph 11.

16. In Paragraph 15, The above secondary battery is a secondary battery having an initial charge capacity of 153.5 mAh / g or more under 0.1C charge / discharge conditions.