Apparatus and method for analyzing charge behavior of nanoscale material
The charge behavior analysis device uses triangular wave voltage pulses to analyze nanoscale materials with high sensitivity and spatial resolution, addressing the limitations of existing methods by distinguishing complex charge mechanisms in electronic devices.
Patent Information
- Application Number
- PCT/KR2026/095896
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-14
- Publication Date
- 2026-11-12
AI Technical Summary
Existing charge behavior analysis methods, particularly contact-based methods like CAFM and AFM-PUND, struggle to accurately distinguish complex charge mechanisms such as ferroelectricity and charge traps due to high voltages causing sample damage and limited spatial resolution.
A charge behavior analysis device using a conductive AFM tip with triangular wave voltage pulses below the coercive voltage, combined with current measurement and integration, to analyze accumulated charge and distinguish mechanisms like polarization switching, ion transport, and charge traps with high sensitivity and spatial resolution.
Enables precise analysis of charge behavior in nanoscale materials with high sensitivity and spatial resolution, effectively distinguishing ferroelectric, memristor, and halide perovskite properties, suitable for next-generation electronic devices.
Smart Images

Figure KR2026095896_12112026_PF_FP_ABST
Abstract
Description
Device and method for analyzing the charge behavior of nanoscale materials
[0001] The present invention relates to an apparatus and method for analyzing the charge behavior of materials in the nanoscale region, and more specifically, to a high-sensitivity charge behavior analysis technique using Accumulative Charge Transfer Spectroscopy (ACTS) based on Atomic Force Microscopy (AFM).
[0002] With the trend toward miniaturization and high performance of electronic devices, technology for precisely analyzing the electrical properties of materials, particularly charge behavior, at the nanometer level is becoming increasingly important. To enhance the performance of various electronic devices, such as memory devices and solar cells, it is essential to precisely analyze charge transfer behavior within materials at the nanometer level.
[0003] In particular, the realization of next-generation high-performance, highly integrated, and ultra-small electronic devices requires technology capable of measuring charge transfer behavior in the nanometer range with high spatial resolution and sensitivity. This plays a crucial role in improving device performance, ensuring reliability, and developing new materials.
[0004] Methods for analyzing charge behavior at the nanoscale can be broadly classified into contact and non-contact methods. Non-contact methods include Electrostatic Force Microscopy (EFM) and Kelvin Probe Force Microscopy (KPFM), which measure electrostatic force or contact potential difference while maintaining a certain distance without the tip directly contacting the sample surface. While these non-contact methods have the advantage of minimizing sample damage, they have limitations such as limited spatial resolution and difficulty in measuring direct charge transfer characteristics.
[0005] In contrast, the contact method measures electrical properties with the AFM tip in direct contact with the sample surface, with Conductive Atomic Force Microscopy (CAFM) being a representative example. The contact method is more effective for analyzing local electrical characteristics because it can measure direct charge transfer properties with high spatial resolution at the nanometer level. In particular, since it enables direct current measurements related to the actual movement of charges, it can provide important information for understanding the operating principles of electronic devices.
[0006] Among these contact methods, current-voltage spectroscopy based on conductive atomic force microscopy (CAFM) has been widely used to analyze charge transfer characteristics in micro-regions. By analyzing the shape of current-voltage curves using CAFM-based measurements, junction characteristics can be determined. However, this method alone has limitations in accurately analyzing complex charge behavior mechanisms, such as ferroelectricity or charge traps.
[0007] Accordingly, various additional analysis methods based on CAFM have been proposed. For example, the AFM-PUND technique (Adv. Mater., 30, 1703675 (2018)), which combines atomic force microscopy (AFM) and the Positive-Up Negative-Down (PUND) technique, has been reported to analyze the hysteresis of charge behavior caused by ferroelectricity. However, this method has the disadvantage that there is a risk of sample damage because a large voltage greater than the coercive voltage required for measurement must be applied, and the measurement response area expands (radius of 200 nm or more) due to the application of a large voltage, making it difficult to analyze fine regions.
[0008] Similarly, charge behavior can occur through various mechanisms. For example, hysteresis of the current-voltage curve affecting photoelectric efficiency in halide perovskite materials is primarily attributed to ion transport, but it can also be caused by complex factors such as ferroelectricity, photo-induced capacitive effects, and charge capture / emission. Therefore, precisely elucidating the principles of charge behavior in local regions remains a difficult challenge for existing current detection technologies.
[0009] Meanwhile, contact methods offer several advantages over non-contact methods. First, direct electrical contact between the tip and the sample allows for the direct measurement of actual charge transfer, enabling more accurate analysis of electrical characteristics. Second, the extremely small contact area allows for high spatial resolution at the nanometer level, making it advantageous for analyzing local charge behavior. Third, dynamic charge behavior can be analyzed in real time by applying various voltage waveforms. These advantages play a crucial role, particularly in understanding the local electrical characteristics of nanodevices.
[0010] However, existing contact-based methods have limitations in effectively distinguishing various charge behavior mechanisms due to the use of high voltages or reliance on single measurements. Therefore, there is a need to develop new atomic force microscopy-based analysis techniques capable of effectively distinguishing charge behavior mechanisms in micro-regions.
[0011] The present invention aims to solve the problems of the aforementioned conventional technology by providing a charge behavior analysis device capable of identifying the charge behavior mechanisms of various materials at the nanometer scale with high sensitivity.
[0012] In addition, a charge behavior analysis method is provided that can analyze the charge behavior of a material with high spatial resolution by repeatedly applying triangular wave voltage pulses of low voltage amplitude and measuring the accumulated charge.
[0013] In addition, a system is provided that can effectively distinguish ferroelectric properties, ion transport properties, and charge trap properties based on the charge behavior characteristics of the material at the nanoscale.
[0014] In addition, an electronic device characteristic evaluation device including the above-mentioned charge behavior analysis device is provided.
[0015] In addition, a computer-readable recording medium is provided that stores a computer program for performing the above-mentioned charge behavior analysis method.
[0016] However, the technical problems that the embodiments of the present invention aim to solve are not limited to the technical problems described above, and other technical problems may exist.
[0017] As a technical means for achieving the above-mentioned technical problem, the first aspect of the present invention provides a device for analyzing the charge behavior of a nanoscale material, comprising: a conductive tip of an atomic force microscope (AFM) that contacts the surface of a material to apply voltage and measure current; a function generator that repeatedly generates and applies voltage pulses in the form of a triangular wave to the tip; a current amplifier that amplifies the current flowing between the tip and the material; and a device that collects and analyzes the amplified current signal in oscilloscope mode.
[0018] According to one embodiment of the present invention, the voltage pulse in the form of a triangular wave may have an amplitude below the anti-voltage capable of switching the polarization of the material, but is not limited thereto.
[0019] According to one embodiment of the present invention, the frequency of the voltage pulse in the form of a triangular wave may be 0.5 kHz to 4 kHz, but is not limited thereto.
[0020] According to one embodiment of the present invention, the analysis device may analyze the charge behavior of a material with a spatial resolution of 20 nm or less, but is not limited thereto.
[0021] According to one embodiment of the present invention, the material may include, but is not limited to, a material selected from the group consisting of ferroelectrics, memristors, halide perovskites, dielectrics, piezoelectrics, ferromagnetics, superconductors, semiconductors, and combinations thereof.
[0022] Additionally, a second aspect of the present invention comprises the steps of: performing pre-polarization at a specific location on the surface of a material using a conductive tip of an atomic force microscope (AFM); repeatedly applying a voltage pulse in the form of a triangular wave to said location; measuring a current generated in the material during each voltage pulse; and a switching current (I) from the measured current. SW ) and non-switching current (I NS A step of separating ); and integrating the switching current with respect to time to calculate the switching charge at each pulse, and accumulating it to obtain the total accumulated charge (C SW,acc A method for analyzing the charge behavior of a nanoscale material is provided, comprising the step of calculating ).
[0023] According to one embodiment of the present invention, the switching current (I SW ) and non-switching current (I NS The step of separating ) involves applying a voltage pulse in a uniform polarization state to measure the current (I meas A step of collecting ); and applying an additional voltage pulse after post-polarization to obtain a non-switching current (I NS Measure ) and the measured current (I meas Non-switching current (I) in ) NS Subtract the switching current (I SW It may include a step of calculating ), but is not limited thereto.
[0024] According to one embodiment of the present invention, the accumulated charge (C) according to the number of pulses SW,acc It may further include, but is not limited to, a step of identifying the charge behavior mechanism of the material by analyzing the change pattern of ).
[0025] According to one embodiment of the present invention, the accumulated charge (C SW,acc Identify the charge behavior characteristics of the material according to the change pattern of ), while the accumulated charge (C SW,acc Identify ferroelectric properties when ) exhibits a positive accumulation pattern that increases with the number of pulses, and the accumulated charge (C SW,acc If ) exhibits a negative accumulation pattern that decreases with the number of pulses, it may be possible to identify nasal genetic characteristics, but is not limited to this.
[0026] According to one embodiment of the present invention, the accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), wherein the accumulated charge change pattern increases according to the number of pulses and the switching current (I SW If ) shows a distinct peak, it may be identified as a material having polarization switching characteristics, but is not limited thereto.
[0027] According to one embodiment of the present invention, the accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), wherein the accumulated charge change pattern decreases with the number of pulses and the switching current (I SW If ) represents a single valley, it may be identified as a material having ion transport characteristics, but is not limited thereto.
[0028] According to one embodiment of the present invention, the accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), wherein the accumulated charge change pattern decreases with the number of pulses and the switching current (ISW If ) exhibits multiple valleys, it may be identified as a material having charge trap properties, but is not limited to this.
[0029] Additionally, a third aspect of the present invention relates to a system for identifying charge behavior characteristics of a material at the nanoscale, comprising: an atomic force microscope (AFM) that contacts the surface of the material, applies a voltage, and measures a current; a function generator that repeatedly generates and applies a voltage pulse in the form of a triangular wave to a conductive tip of the AFM; a current amplifier that amplifies the current flowing between the tip and the material; a device that collects the amplified current signal in oscilloscope mode; and a processing unit that analyzes the collected current signal to identify the charge behavior mechanism of the material based on the characteristics of the accumulated charge change pattern and the switching current, wherein the processing unit comprises an accumulated charge (C SW,acc ) increases according to the number of pulses and the switching current (I SW If ) exhibits a peak, it is identified as a material having polarization switching characteristics, and the accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW If ) exhibits a single valley, it is identified as a material with ion transport characteristics, and the accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW A charge behavior characteristic identification system is provided, which identifies a material as having charge trap characteristics when it exhibits multiple valleys.
[0030] According to one embodiment of the present invention, the charge behavior characteristic identification system may analyze the local charge behavior of a material with a spatial resolution of 20 nm or less, but is not limited thereto.
[0031] According to one embodiment of the present invention, the voltage pulse in the form of a triangular wave may have an amplitude less than or equal to the antivoltage of the substance to be analyzed and may have a frequency between 0.5 kHz and 4 kHz, but is not limited thereto.
[0032] According to one embodiment of the present invention, the system may further include, but is not limited to, a function for analyzing the correlation between the charge behavior characteristics and the surface polarization state of the material, by performing piezoelectric force microscopy (PFM) measurements at the same location as the part measured by the AFM tip to measure ferroelectricity based on electromechanical response.
[0033] In addition, the fourth aspect of the present invention provides an electronic device characteristic evaluation device comprising a charge behavior analysis device for nanoscale materials according to the first aspect of the present invention.
[0034] In addition, the fifth aspect of the present invention provides a computer-readable recording medium in which a computer program is stored, said computer-readable recording medium comprising instructions that cause the computer to perform a method for analyzing the charge behavior of a nanoscale material according to the second aspect of the present invention.
[0035] The means for solving the problem described above are merely exemplary and should not be interpreted as intended to limit the present invention. In addition to the exemplary embodiments described above, additional embodiments may exist in the drawings and the detailed description of the invention.
[0036] The charge behavior analysis device for nanoscale materials according to the present invention provides superior spatial resolution and sensitivity compared to conventional methods by analyzing accumulated charge through the repeated application of low-voltage triangular wave pulses. Specifically, by using a low voltage below the torsion voltage, it is possible to precisely analyze charge behavior in a fine region at the nanometer level (radius of 20 nm or less) while minimizing sample damage.
[0037] In addition, the method for analyzing the charge behavior of nanoscale materials according to the present invention provides the ability to effectively distinguish the charge behavior mechanisms of various materials. Specifically, the accumulated charge (C SW,acc Change pattern of ) and switching current (I SW By analyzing the characteristics of ), various mechanisms such as polarization switching in ferroelectrics, ion transport in memristors, and charge trapping in halide perovskites can be clearly distinguished. On the other hand, conventional current-voltage analysis methods had limitations in accurately distinguishing these complex charge behavior mechanisms.
[0038] Furthermore, the method according to the present invention can be used with existing atomic force microscope (AFM) hardware, allowing for implementation without additional specialized equipment. This enables high sensitivity (6.66 MV m²) -1 This means that charge behavior can be analyzed at the nanoscale, while the equipment configuration is simple and economical.
[0039] The charge behavior analysis system according to the present invention can be applied to various material systems such as ferroelectrics, memristors, and halide perovskites, and can significantly contribute to the development of next-generation nanoscale electronic devices that require analysis of electrical properties in ultrafine regions. Through this, it can promote research related to performance enhancement and quality improvement of various electronic devices such as memory devices, solar cells, and sensors.
[0040] However, the effects obtainable from this invention are not limited to those described above, and other effects may exist.
[0041] Figure 1 is a schematic diagram for ACTS analysis according to the present invention, showing the distribution of the induced electric field generated at a tip to which voltage is applied.
[0042] Figure 2 is a flowchart of a method for analyzing the charge behavior of a nanoscale material according to the present invention.
[0043] Figure 3 shows a schematic diagram of the voltage waveform of the ACTS according to the present invention and the measured current (Imeas = ISW + INS), switching current (ISW), and non-switching current (INS).
[0044] FIG. 4 illustrates a charge extraction method through the switching current (ISW) induced by the switching of polarization according to the present invention and integration with respect to time.
[0045] Figure 5 illustrates the process in which the switching charge (CSW) at each pulse in the ACTS according to the present invention is obtained through the difference in switching charges.
[0046] Figure 6 shows the PFM hysteresis curve of a selected region in the ferroelectric Pb(Zr,Ti)O3 (PZT), and the inserted image shows the PFM phase image in the corresponding region after ACTS analysis.
[0047] Figure 7 shows the switching current and the result projected onto the current-time plane for time and number of pulses in PZT.
[0048] Figure 8 shows the accumulated switching charge (CSW) for various frequencies at an amplitude of 3.5V in PZT.
[0049] Figure 9 shows the accumulated charge (CSW) at various amplitudes and frequencies in PZT.
[0050] Figure 10 shows the PFM hysteresis curve of a selected region in the ferroelectric Hf0.5Zr0.5O2 (HZO), and the inset graph shows the accumulated switching charge (CSW) due to voltages with amplitudes of 3V and 8V.
[0051] Figure 11 shows the switching current as a function of time and number of pulses in HZO and the results projected onto the current-time plane.
[0052] Figure 12 shows the ESM hysteresis curve of a selected region in TiO2, which is a memristor, and the inset graph shows the accumulated switching charge (CSW) due to voltages of 2V and 5V amplitudes at 1kHz.
[0053] Figure 13 shows the switching current as a function of time and number of pulses at 1 kHz and 5 V amplitude in TiO2 and the results projected onto the current-time plane.
[0054] Figure 14 shows the PFM hysteresis curve of a selected region in the halide perovskite CH(NH2)2PbI3 (FAPbI3), and the inset graph shows the accumulated switching charge (CSW) due to voltages of amplitudes of 1V and 0.5V at 1kHz.
[0055] Figure 15 shows the switching current and the result projected onto the current-time plane as a function of time and number of pulses at 1 kHz and 1 V amplitude in FAPbI3.
[0056] Embodiments of the present invention are described below with reference to the attached drawings to enable those skilled in the art to easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein. Furthermore, in order to clearly explain the present invention in the drawings, parts unrelated to the explanation have been omitted, and similar parts throughout the specification are denoted by similar reference numerals.
[0057] Throughout this specification, when a part is described as being "connected" to another part, this includes not only cases where they are "directly connected," but also cases where they are "electrically connected" with other elements interposed between them.
[0058] Throughout the entire specification, when a component is described as being located "on," "on top," "on top," "under," "on bottom," or "on bottom" of another component, this includes not only cases where the component is in contact with the other component but also cases where another component exists between the two components.
[0059] Throughout this specification, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0060] As used herein, terms of degree such as “about,” “substantially,” etc., are used to mean at or near the stated value when inherent manufacturing and material tolerances are presented in the stated meaning, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure in which precise or absolute values are mentioned to aid in understanding the invention. Furthermore, throughout this specification, “a step of” or “a step of” does not mean “a step for”.
[0061] Throughout this specification, the term “combination thereof” included in the Markush-type expression means one or more mixtures or combinations selected from the group consisting of the components described in the Markush-type expression, and means including one or more selected from the group consisting of said components.
[0062] Throughout the entire specification, the description "A and / or B" means "A, B, or A and B".
[0063] Hereinafter, the apparatus and method for analyzing the charge behavior of nanoscale materials according to the present invention will be described in detail with reference to embodiments, examples, and drawings. However, the present invention is not limited to these embodiments, examples, and drawings.
[0064]
[0065] As a technical means for achieving the above-mentioned technical problem, the first aspect of the present invention provides a device for analyzing the charge behavior of a nanoscale material, comprising: a conductive tip of an atomic force microscope (AFM) that contacts the surface of a material to apply voltage and measure current; a function generator that repeatedly generates and applies voltage pulses in the form of a triangular wave to the tip; a current amplifier that amplifies the current flowing between the tip and the material; and a device that collects and analyzes the amplified current signal in oscilloscope mode.
[0066] The charge behavior analysis device for nanoscale materials according to the present invention is a device capable of analyzing charge behavior at the nanometer level with high sensitivity based on an atomic force microscope (AFM). As shown in FIG. 1, when a voltage is applied to the surface of a material through an atomic force microscope tip, a non-uniform electric field is formed around the tip. This electric field has the characteristic of weakening radially as it moves away from the center of the tip, and as a result, charge behavior occurs within the material.
[0067] In the present invention, the charge behavior characteristics of a material are analyzed by applying voltage while in direct contact with the surface of the material using a conductive tip of an atomic force microscope and measuring the resulting current response. In particular, the dynamic behavior of accumulated charge can be measured by repeatedly generating and applying voltage pulses in the form of triangular waves through a function generator to the material. The current generated at this time is amplified through a current amplifier and collected and analyzed in oscilloscope mode.
[0068] According to one embodiment of the present invention, the voltage pulse in the form of a triangular wave may have an amplitude less than or equal to the anti-voltage capable of switching the polarization of the material, but is not limited thereto.
[0069] The triangular wave-shaped voltage pulse used in the present invention characteristically has an amplitude below the antivoltage of the material being analyzed. This is one of the important features that differentiate it from conventional charge behavior analysis methods. For example, in the conventional AFM-PUND technique, a large voltage above the antivoltage had to be applied to achieve complete conversion of ferroelectric materials, but this method had the disadvantage of causing sample damage and expanding the measurement area.
[0070] On the other hand, in the present invention, by using a low voltage below the coercive field, sample damage can be minimized and the measurement response area can be kept small. Despite using a low voltage amplitude, charge behavior can be measured with high sensitivity by repeatedly applying triangular wave voltage pulses and analyzing the accumulated charge response. This is because partial charge behavior can occur even at voltages below the coercive voltage due to interactions within the material.
[0071] According to one embodiment of the present invention, the frequency of the voltage pulse in the form of a triangular wave may be 0.5 kHz to 4 kHz, but is not limited thereto.
[0072] The frequency of the triangular wave-shaped voltage pulse used in the present invention can be adjusted within the range of 0.5 kHz to 4 kHz. This frequency range is an optimized value for effectively analyzing the charge behavior characteristics of various materials. At frequencies that are too low, there is a disadvantage of a longer measurement time, and at frequencies that are too high, a problem may occur where the charge behavior of the material cannot keep up with the frequency.
[0073] In particular, for materials where ion transport is important, such as halide perovskites, using high-frequency voltage pulses of 1 kHz or higher can minimize artifacts caused by ion transport and effectively analyze properties such as charge traps. By analyzing differences in charge behavior according to frequency changes, additional information about the charge behavior mechanism of the material can also be obtained.
[0074] According to one embodiment of the present invention, the analysis device may analyze the charge behavior of a material with a spatial resolution of 20 nm or less, but is not limited thereto.
[0075] The analysis device according to the present invention can analyze the charge behavior of a material with a high spatial resolution of 20 nm or less. This is a significantly improved spatial resolution compared to the conventional AFM-PUND method, which analyzed a region with a radius of about 200 nm or more. As shown in FIG. 1, the use of a low voltage amplitude limits the range of influence of the electric field to a narrow area around the tip, thereby enabling higher spatial resolution.
[0076] Such high spatial resolution is crucial for analyzing the local charge behavior of nanoscale electronic devices. In particular, as device sizes shrink to the nanometer level—such as in next-generation memory devices and ultrathin ferroelectrics—this high-resolution analysis technology can become a key technology for improving device performance and reliability.
[0077] According to one embodiment of the present invention, the material may include, but is not limited to, a material selected from the group consisting of ferroelectrics, memristors, halide perovskites, dielectrics, piezoelectrics, ferromagnetics, superconductors, semiconductors, and combinations thereof.
[0078]
[0079] The charge behavior analysis device according to the present invention can be applied to various material systems. It can analyze polarization switching characteristics in ferroelectric materials (e.g., PZT, HZO), resistance change characteristics due to ion movement in memristors (e.g., TiO2), and charge trap characteristics in halide perovskites (e.g., FAPbI3). In addition, it can be utilized to analyze charge behavior in various dielectrics, piezoelectrics, ferromagnets, superconductors, semiconductors, etc.
[0080] The reason this method is applicable to such a wide variety of materials is that the analysis method of the present invention is based on the principle of directly measuring the charge behavior within the material. Since the characteristics of charge behavior vary depending on the type of material, the device of the present invention can distinguish these differences with high sensitivity, making it suitable for analyzing the electrical properties of various material systems.
[0081] Additionally, a second aspect of the present invention comprises the steps of: performing pre-polarization at a specific location on the surface of a material using a conductive tip of an atomic force microscope (AFM); repeatedly applying a voltage pulse in the form of a triangular wave to said location; measuring a current generated in the material during each voltage pulse; and a switching current (I) from the measured current. SW ) and non-switching current (I NS A step of separating ); and integrating the switching current with respect to time to calculate the switching charge at each pulse, and accumulating it to obtain the total accumulated charge (C SW,acc A method for analyzing the charge behavior of a nanoscale material is provided, comprising the step of calculating ).
[0082] Throughout this specification, the term "Accumulative Charge Transfer Spectroscopy (ACTS)" refers to a method for analyzing the charge behavior of nanoscale materials according to the second aspect of the present invention. Unlike conventional current-based analysis methods, ACTS is a novel analysis method capable of distinguishing various charge behavior mechanisms with high sensitivity by measuring the dynamic behavior of accumulated charges.
[0083] Referring to Figure 2, the main process of the method for analyzing the charge behavior of nanoscale materials is explained as follows.
[0084] First, pre-polarization is performed at a specific location on the surface of the material using a conductive tip (S100).
[0085] The pre-polarization step (S100) is an important process for establishing the initial state of the material before starting the ACTS analysis. In this step, a sufficiently large direct current (DC) voltage is applied to a specific location on the surface of the material for a certain period of time through a conductive tip to uniformly establish the polarization state of that region. For ferroelectrics, this serves to align the polarization direction uniformly; for memristors, to establish the initial resistance state; and for halide perovskites, to establish the initial state of the charge traps. Through this pre-polarization, uniform analysis conditions are secured, ensuring that subsequent measurement results accurately reflect the intrinsic characteristics of the material. In particular, establishing identical initial conditions is essential for comparative analysis between multiple samples or between different locations within the same sample; if this process is not performed accurately, the reliability of subsequent analysis results may be compromised.
[0086] Next, a triangular wave-shaped voltage pulse is repeatedly applied to the same location (S200).
[0087] The step of applying a triangular wave-shaped voltage pulse (S200) is a core process of ACTS analysis, and is a step of continuously applying a triangular wave-shaped voltage pulse multiple times to the same location where pre-polarization has been performed.
[0088] Figure 3 shows a schematic diagram of the voltage waveform, measured current, switching current, and non-switching current of the ACTS according to the present invention. As shown in Figure 3, in the ACTS measurement, a voltage pulse in the form of a triangular wave is repeatedly applied to the surface of the material. The triangular wave waveform has a form in which the voltage starts at 0, increases to a maximum value, and then decreases back to 0. The measured current (I) when such a voltage pulse is applied meas ) is the switching current (I SW ) and non-switching current (I NS It consists of the sum of ). A voltage pulse in the form of a triangular wave is suitable for observing minute charge transfer characteristics by gradually inducing charge behavior within the material.
[0089] Next, the current generated in the material during each voltage pulse is precisely measured (S300).
[0090] In the current measurement step (S300), the current flowing between the material and the AFM tip is precisely measured in real time while each triangular wave voltage pulse is applied. In this process, a current amplifier is used to amplify minute current signals at the nanoampere (nA) or picoampere (pA) level, and the signals are collected at high resolution using an oscilloscope. The measured current (I meas ) directly reflects the electrical response of a material to changes in voltage, and includes the switching current (I) attributed to the material's charge behavior mechanism. SW Non-switching current (I) due to ) and other non-switching elements NS All of ) are included. Since the accuracy of current measurement and the signal-to-noise ratio (S / N ratio) directly affect the quality of subsequent analysis results, generally 10 7A current amplifier with the above transimpedance gain and a data acquisition system with a high sampling rate (hundreds of kHz) are used. The current-time data measured in this way is separated into switching current and non-switching current and analyzed in the next step.
[0091] Next, the measured current (I meas Switching current (I) in ) SW ) and non-switching current (I NS Separate ) (S400).
[0092] According to one embodiment of the present invention, the switching current (I SW ) and non-switching current (I NS The step (S400) of separating ) is the measured current (I) obtained by applying a voltage pulse in a uniform polarization state. meas A step of collecting ); and applying an additional voltage pulse after post-polarization to obtain a non-switching current (I NS Measure ) and the measured current (I meas Non-switching current (I) in ) NS Subtract the switching current (I SW It may include a step of calculating ), but is not limited thereto.
[0093] Switching current (I SW ) and non-switching current (I NS The process of separating ) is an important step in charge behavior analysis. First, the measured current (I) obtained by applying a voltage pulse under a uniform polarization state meas Collects ). This measured current consists of the sum of the switching current and the non-switching current (I meas = I SW + I NS ).
[0094] Next, after changing the polarization state of the material through a post-polarization process, an additional voltage pulse is applied to the non-switching current (I NSOnly ) is measured. Since the polarization state is already set after post-polarization, when a voltage pulse in the same direction is applied, no switching occurs and only non-switching current is measured.
[0095] Finally, the measured current (I meas Non-switching current (I) in ) NS Subtract the switching current (I SW Calculate )( I SW = I meas - I NS The switching current separated in this way is important information that directly reflects the charge behavior mechanism of the material.
[0096] FIG. 4 shows a switching current (I) induced by switching of polarization according to the present invention. SW It illustrates a charge extraction method through integration with respect to ) and time. Switching current is a current generated from the intrinsic charge behavior mechanisms of a material, such as polarization switching, ion migration, and charge trapping. As shown in Fig. 4, the switching current (I SW Integrating ) with respect to time yields the switching charge (C) at each pulse. SW ) can be calculated. The switching charge obtained in this way is an important parameter that directly reflects the charge behavior mechanism of the material.
[0097] Switching current is a current directly related to the charge behavior mechanism of a material (e.g., polarization switching in ferroelectrics, ion transport in memristors, charge trapping in halide perovskites, etc.), while non-switching current is a current caused by other factors. Switching current (I SW ) and non-switching current (I NS ) exhibit different characteristics, and through this, information about the charge behavior mechanism of the material can be obtained.
[0098] Next, the switching current is integrated with respect to time to obtain the switching charge (C) at each pulse. SW Calculate ) and accumulate it to obtain the total accumulated charge (C SW,accCalculates ) (S500).
[0099] FIG. 5 shows the switching charge (C) at each pulse in the ACTS according to the present invention. SW ) represents the process in which the switching charge is obtained through the difference in switching charge. As shown in Fig. 5, the switching charge calculated at each voltage pulse is accumulated to obtain the total accumulated charge (C SW,acc ...can be calculated. The change pattern of this accumulated charge tends to increase or decrease depending on the number of voltage pulses, and through the analysis of this pattern, the charge behavior mechanism of the material can be effectively distinguished. In particular, ferroelectric materials have a positive accumulation pattern in which the accumulated charge increases, while non-ferroelectric materials such as memristors or halide perovskites have a negative accumulation pattern in which the accumulated charge decreases.
[0100] By analyzing the change pattern of this accumulated charge, the charge behavior mechanism of the material can be distinguished. In particular, by analyzing the pattern of increase or decrease in accumulated charge according to the number of pulses together with the characteristics of the switching current (peak or valley shape), the charge behavior mechanism of various materials such as ferroelectrics, memristors, and halide perovskites can be effectively distinguished.
[0101] The ACTS method has the advantage of being able to analyze the charge behavior of nanoscale materials with high sensitivity and spatial resolution while using low voltage amplitudes compared to existing methods such as AFM-PUND. This is based on the principle of measuring the dynamic behavior of accumulated charges by repeatedly applying voltage pulses.
[0102] According to one embodiment of the present invention, the accumulated charge (C) according to the number of pulses SW,acc It may further include, but is not limited to, a step of identifying the charge behavior mechanism of the material by analyzing the change pattern of ).
[0103] One of the key features of the present invention is the accumulated charge (C) according to the number of pulses.SW,acc It is to identify the charge behavior mechanism of a material by analyzing the change pattern of ). The way charge accumulates within a material upon the application of repetitive voltage pulses varies depending on the charge behavior mechanism of the material.
[0104] For example, in ferroelectric materials, as voltage pulses are repeated, polarization switching occurs gradually, showing a pattern in which the accumulated charge increases. On the other hand, in non-ferroelectric materials such as memristors or halide perovskites, the accumulated charge may decrease as voltage pulses are repeated.
[0105] By analyzing the change patterns of these accumulated charges, the charge behavior mechanisms of materials can be effectively distinguished. In particular, this method allows for the clear identification of various charge behavior mechanisms that were difficult to distinguish using conventional single measurement methods.
[0106] According to one embodiment of the present invention, the accumulated charge (C SW,acc Identify the charge behavior characteristics of the material according to the change pattern of ), while the accumulated charge (C SW,acc Identify ferroelectric properties when ) exhibits a positive accumulation pattern that increases with the number of pulses, and the accumulated charge (C SW,acc If ) exhibits a negative accumulation pattern that decreases with the number of pulses, it may be possible to identify nasal genetic characteristics, but is not limited to this.
[0107] Accumulated charge (C SW,acc The change pattern of ) is an important indicator for identifying the charge behavior characteristics of a material. In the present invention, this change pattern is broadly classified into two types.
[0108] First, accumulated charge (C SW,accThe case where the charge shows a pattern of increasing with the number of pulses is termed 'positive accumulation,' and this is observed in materials with ferroelectric properties (e.g., PZT, HZO). In ferroelectric materials, as voltage pulses are repeated, polarization switching occurs gradually, leading to the accumulation of more charge; thus, the accumulated charge shows a pattern of increasing.
[0109] Second, accumulated charge (C SW,acc The case where the accumulated charge exhibits a decreasing pattern depending on the number of pulses is termed 'negative accumulation,' and this is observed in materials with non-ferroelectric properties (e.g., TiO2, FAPbI3). In non-ferroelectric materials, the accumulated charge exhibits a decreasing pattern due to mechanisms such as ion migration or charge trapping as voltage pulses are repeated.
[0110] By analyzing the change patterns of these accumulated charges, the ferroelectric and non-ferroelectric properties of the material can be clearly distinguished.
[0111] According to one embodiment of the present invention, the accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), wherein the accumulated charge change pattern increases according to the number of pulses and the switching current (I SW If ) shows a distinct peak, it may be identified as a material having polarization switching characteristics, but is not limited thereto.
[0112] The present invention relates to not only the accumulated charge change pattern but also the switching current (I SW The characteristics of ) are also analyzed to more accurately identify the charge behavior mechanism of the material. In particular, the accumulated charge change pattern increases with the number of pulses, and simultaneously, the switching current (I SW If ) shows a distinct peak, this is a typical characteristic of ferroelectric materials with polarization switching characteristics.
[0113] In ferroelectric materials, when an electric field is applied, a distinct switching current peak occurs as the polarization direction changes. This peak represents the movement of charge during the polarization switching process, and the magnitude of the peak tends to gradually decrease as the voltage pulse is repeated. This is because polarization switching is gradually completed in more regions.
[0114] Therefore, by observing the increasing pattern of accumulated charge and the distinct peak characteristics of the switching current together, the polarization switching characteristics of the material can be clearly identified. These characteristics are observed in ferroelectric materials such as PZT and HZO.
[0115] According to one embodiment of the present invention, the accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), wherein the accumulated charge change pattern decreases with the number of pulses and the switching current (I SW If ) represents a single valley, it may be identified as a material having ion transport characteristics, but is not limited thereto.
[0116] If the accumulated charge change pattern decreases with the number of pulses and the switching current (ISW) exhibits a single valley shape, this is a typical characteristic of materials with ion transport properties (e.g., TiO2 memristors).
[0117] In materials with ion transport characteristics, such as memristors, ions (e.g., oxygen vacancies) gradually move to form a conduction path as voltage pulses are repeatedly applied. During this process, the switching current exhibits a valley-shaped characteristic, and the accumulated charge shows a pattern of decreasing as the voltage pulses are repeated.
[0118] The reason these characteristics are observed in memristor materials such as TiO2 is that initially, the movement of oxygen vacancies is limited, so a small current flows, but as voltage pulses are repeated, oxygen vacancies gradually move to form conduction paths, allowing more current to flow. Consequently, the accumulated charge decreases, and the switching current exhibits a valley shape.
[0119] Through this analysis of characteristics, the ion transport characteristics of the material can be clearly identified.
[0120] According to one embodiment of the present invention, the accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), wherein the accumulated charge change pattern decreases with the number of pulses and the switching current (I SW If ) exhibits multiple valleys, it may be identified as a material having charge trap properties, but is not limited to this.
[0121] The accumulated charge change pattern decreases with the number of pulses and the switching current (I SW If it exhibits a multiple valleys shape, this is a typical characteristic of materials with charge trap properties (e.g., FAPbI3 halide perovskite).
[0122] In materials with charge trap properties, such as halide perovskites, charging and discharging of the trap state occur repeatedly when a voltage pulse is applied. During this process, the switching current exhibits multiple valley shapes, which are related to different charge transport mechanisms such as trap filling limit (TFL) and space charge limited (SCL) conduction.
[0123] The reason multiple valleys are observed in halide perovskite materials such as FAPbI3 is that as voltage increases, traps gradually fill up, and the charge transport mechanism changes at a specific threshold (VSCL, VTFL). These characteristics may vary depending on the distribution and density of charge traps.
[0124] Through this characteristic analysis, the charge trap properties of the material can be clearly identified, and furthermore, it is possible to extract important parameters such as trap density.
[0125] Additionally, a third aspect of the present invention relates to a system for identifying charge behavior characteristics of a material at the nanoscale, comprising: an atomic force microscope (AFM) that contacts the surface of the material, applies a voltage, and measures a current; a function generator that repeatedly generates and applies a voltage pulse in the form of a triangular wave to a conductive tip of the AFM; a current amplifier that amplifies the current flowing between the tip and the material; a device that collects the amplified current signal in oscilloscope mode; and a processing unit that analyzes the collected current signal to identify the charge behavior mechanism of the material based on the characteristics of the accumulated charge change pattern and the switching current, wherein the processing unit comprises an accumulated charge (C SW,acc ) increases according to the number of pulses and the switching current (I SW If ) exhibits a peak, it is identified as a material having polarization switching characteristics, and the accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW If ) exhibits a single valley, it is identified as a material with ion transport characteristics, and the accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW A charge behavior characteristic identification system is provided, which identifies a material as having charge trap characteristics when it exhibits multiple valleys.
[0126] Regarding the charge behavior characteristic identification system according to the third aspect of the present invention, detailed descriptions of parts that overlap with the first and / or second aspects of the present invention have been omitted, but even if such descriptions are omitted, the contents described in the first and / or second aspects of the present invention may be applied equally to the third aspect of the present invention.
[0127] A third aspect of the present invention relates to an integrated system capable of identifying charge behavior characteristics of various materials in an automated manner. At the center of this system is an atomic force microscope (AFM), which can apply voltage and measure current by directly contacting the surface of a material at the nanoscale. The AFM is a powerful tool capable of measuring local electrical properties of a material with spatial resolution at the nanometer level.
[0128] This system repeatedly generates and applies triangular voltage pulses to the AFM tip using a function generator. The triangular voltage pulses start at zero, increase to a maximum value, and then decrease back to zero; this process is repeated multiple times to analyze the charge behavior characteristics of the material. At this time, the minute current flowing between the tip and the material is amplified through a current amplifier and converted to a measurable level.
[0129] The amplified current signal precisely collects changes over time through a device set to oscilloscope mode. The collected current signal is transmitted to the system's processing unit for analysis. The processing unit analyzes the switching current (I) from the current signal. SW ) and non-switching current (I NS Separate ), calculate the switching charge at each pulse by integrating the switching current with respect to time, and then accumulate this to obtain the total accumulated charge (C SW,acc Produces ).
[0130] The most significant feature of this system is that it automatically analyzes the accumulated charge change patterns and switching current characteristics to identify the charge behavior mechanism of the material. Specifically, accumulated charge (C SW,acc ) increases according to the number of pulses and the switching current (I SW If ) exhibits a peak, the material is identified as a ferroelectric material with polarization switching characteristics. On the other hand, accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW If ) exhibits a single valley, it is identified as a memristor material having ion transport characteristics. In addition, the accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW If ) exhibits multiple valleys, it is identified as a halide perovskite material having charge trap properties.
[0131] Such automated identification systems are highly useful for evaluating the electrical properties of nanoscale devices and enable the efficient analysis of charge behavior mechanisms in various material systems.
[0132] According to one embodiment of the present invention, the charge behavior characteristic identification system may analyze the local charge behavior of a material with a spatial resolution of 20 nm or less, but is not limited thereto.
[0133] The atomic force microscope (AFM) used in the system according to the present invention can analyze the local charge behavior of a material with a high spatial resolution of 20 nm or less. This is a significantly improved spatial resolution compared to existing charge behavior analysis methods. For example, while the existing AFM-PUND method analyzed an area with a radius of about 200 nm or more, the system of the present invention can analyze charge behavior in an area about 10 times smaller.
[0134] The high spatial resolution of ACTS is determined by the tip diameter and voltage amplitude. In this invention, by using a low voltage amplitude below the torsion voltage, the range of influence of the electric field is minimized, thereby enabling precise measurements in smaller areas. Furthermore, through a fine tip diameter and a precise position control system, the charge behavior of nanoscale structures, such as single particles, grain boundaries, and domain walls, can be observed at high resolution.
[0135] According to one embodiment of the present invention, the voltage pulse in the form of a triangular wave may have an amplitude less than or equal to the antivoltage of the substance to be analyzed and may have a frequency between 0.5 kHz and 4 kHz, but is not limited thereto.
[0136] The triangular voltage pulse used in the system of the present invention has an amplitude below the antivoltage of the substance to be analyzed and generally operates in a frequency range between 0.5 kHz and 4 kHz. This characteristic is an important factor that differentiates the system of the present invention from existing methods.
[0137] In particular, for materials where ion transport is important, such as halide perovskites, using a high frequency of 1 kHz or higher minimizes artifacts caused by slow ion transport and allows for the observation of faster charge behavior (e.g., charge traps).
[0138] According to one embodiment of the present invention, the system may further include a function to measure ferroelectricity based on an electromechanical response at the same location as the part measured by the AFM tip, and to analyze the correlation between the charge behavior characteristics and the surface polarization state of the material, but is not limited thereto.
[0139] In addition to analyzing charge behavior using the Atomic Charge Transfer Scheme (ACTS), the system of the present invention can measure ferroelectricity based on electromechanical reactions at the same location; therefore, it may include an additional function for analyzing the correlation between the charge behavior characteristics and the surface polarization state of the material. This combined analysis function is of great help in gaining a more comprehensive understanding of the electrical properties of the material.
[0140] In addition, the fourth aspect of the present invention provides an electronic device characteristic evaluation device comprising a charge behavior analysis device for nanoscale materials according to the first aspect of the present invention.
[0141] Regarding the electronic device characteristic evaluation device according to the fourth aspect of the present invention, detailed descriptions of parts that overlap with the first aspect of the present invention have been omitted, but even if such descriptions are omitted, the contents described in the first aspect of the present invention can be applied equally to the fourth aspect of the present invention.
[0142] The above-described electronic device characteristic evaluation device can be utilized to evaluate the performance and reliability of various electronic devices, such as memory devices, solar cells, and transistors. In particular, by analyzing the local charge behavior characteristics of the device at the nanometer level, it can contribute to understanding the operating principles of the device and optimizing its performance.
[0143] In addition, the fifth aspect of the present invention provides a computer-readable recording medium in which a computer program is stored, said computer-readable recording medium comprising instructions that cause the computer to perform a method for analyzing the charge behavior of a nanoscale material according to the second aspect of the present invention.
[0144] Regarding the computer-readable recording medium according to the fifth aspect of the present invention, detailed descriptions of parts that overlap with the second aspect of the present invention have been omitted, but even if such descriptions have been omitted, the contents described in the second aspect of the present invention may be applied equally to the fifth aspect of the present invention.
[0145] The above computer program includes instructions that control the ACTS system to perform processes such as pre-polarization, application of triangular wave voltage pulses, current measurement, separation of switching current and non-switching current, calculation and accumulation of switching charge, and identification of charge behavior mechanism in an automated manner.
[0146] Computer-readable recording media can take various forms, such as hard disks, CD-ROMs, DVDs, flash memory, or other non-volatile storage devices, and programs can be stored in the form of executable files, libraries, scripts, etc. This program is designed to operate in conjunction with a hardware system for ACTS measurements, contributing to the automation and optimization of the charge behavior analysis process of nanoscale materials.
[0147] The present invention is to be explained in more detail through the following examples, but the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention.
[0148]
[0149] [Example 1] ACTS measurement results in ferroelectric PZT
[0150] The ACTS method according to the present invention is a ferroelectric material PZT(Pb(Zr 0.2 Ti 0.8 The results applied to )O3) are explained with reference to FIGS. 6, FIGS. 7, FIGS. 8, and FIGS. 9.
[0151] Figure 6 shows the PFM hysteresis curve of a selected region in the ferroelectric Pb(Zr,Ti)O3 (PZT), and the inset image shows the PFM phase image of the corresponding region after ACTS analysis. A clear hysteresis behavior with a coercive voltage of approximately 2.5 V was observed in the PFM hysteresis curve, confirming the ferroelectricity of PZT. In the PFM phase image obtained after ACTS analysis, a transition region with a radius of approximately 20 nm was observed. This is a significantly smaller region compared to the conventional AFM-PUND method (radius of approximately 200 nm), demonstrating that the ACTS method provides high spatial resolution.
[0152] Figure 7 shows the switching current and the results projected onto the current-time plane with respect to time and the number of pulses in PZT. A distinct switching current peak was observed at each voltage pulse, and the intensity of the peak tended to gradually decrease as the number of pulses increased. This is because polarization switching is completed in more regions as the pulses are repeated.
[0153] FIG. 8 shows the accumulated switching charge (C) for various frequencies (0.5kHz, 1kHz, 2kHz, 4kHz) at an amplitude of 3.5V in PZT. SW It represents. A tendency for the accumulated charge to increase with the number of pulses was observed at all frequencies, and it reached saturation after approximately the 1000th pulse. This pattern of positive accumulation is a typical characteristic of ferroelectric materials.
[0154] FIG. 9 shows the accumulated charge (C) in PZT at various amplitudes (1V-5V) and frequencies (0.5kHz-4kHz). SW It represents ). As the voltage amplitude increased, the accumulated charge increased, which is because a larger voltage induces polarization switching over a wider area. In addition, the accumulated charge tended to increase as the frequency decreased, which is because more time is given for polarization switching at lower frequencies.
[0155] Of particular note is that at PZT, 1V (6.66 MV m) -1 This indicates that a clear switching charge was observed even at low voltage amplitudes. This is consistent with the existing AFM-PUND method (133 MV m²). -1 It shows that charge behavior can be detected even at much lower voltages compared to ), proving that the ACTS method provides high sensitivity.
[0156] [Example 2] ACTS measurement results in fluorite-structured ferroelectric HZO
[0157] The ACTS method according to the present invention is a ferroelectric material HZO (Hf 0.5 Zr 0.5 The results applied to O2) are explained with reference to FIGS. 10 and FIGS. 11.
[0158] Figure 10 shows Hf, a ferroelectric material. 0.5 Zr 0.5 This shows the PFM hysteresis curve of a selected region in O2(HZO), and the inserted graph shows the accumulated switching charge (C) due to voltages with amplitudes of 3V and 8V. SW It represents ). Hysteresis behavior with a tolerance of about 3.8 V was observed in the PFM hysteresis curve, which confirms the ferroelectricity of HZO. As can be seen in the inset graph, a positive accumulation pattern was observed in which the accumulated charge increased with the number of pulses at both 3 V and 8 V amplitudes.
[0159] Figure 11 shows the switching current and the results projected onto the current-time plane as a function of time and the number of pulses in HZO. Similar to PZT, a distinct switching current peak was observed at each voltage pulse, and the intensity of the peak showed a tendency to gradually decrease as the number of pulses increased. At an amplitude of 8 V, the peak value decreased by 62.9% compared to the initial value, and at an amplitude of 3 V, it decreased by 17.6%.
[0160] Of particular note is that clear ferroelectric properties could be observed even in ultrathin HZO films with a thickness of 10 nm using the ACTS method. In ultrathin films, a strong half-voltage field is formed due to incomplete charge screening, which can make polarization switching difficult; however, the ACTS method demonstrates that charge behavior can be measured with high sensitivity even under these conditions.
[0161] [Example 3] ACTS measurement results in memristor TiO2
[0162] The results of applying the ACTS method according to the present invention to a TiO2 single crystal, which is a memristor material, will be explained with reference to FIGS. 12 and 13.
[0163] FIG. 12 shows the Electrochemical Strain Microscopy (ESM) hysteresis curve of a selected region in TiO2 memristor, and the inset graph shows the accumulated switching charge (C) due to voltages of 2V and 5V amplitudes at 1kHz. SW It represents ). In the ESM hysteresis curve, hysteretic behavior with a kinetic voltage of about 2.8 V was observed, but this is due to ion migration rather than ferroelectricity. As can be seen in the inset graph, a negative accumulation pattern was observed in which the accumulated charge decreased with the number of pulses at both 2 V and 5 V amplitudes.
[0164] Figure 13 shows the switching current as a function of time and number of pulses at 1 kHz and 5 V amplitude in TiO2, and the results projected onto the current-time plane. Unlike ferroelectric materials, the switching current in TiO2 exhibited a valley shape rather than a peak. These valleys are associated with the movement of oxygen vacancies activated by electrical stimulation.
[0165] The negative accumulation transition mechanism observed in TiO2 memristors can be explained as follows. During the pre-polarization process, a high resistance state (HRS) is established, at which point oxygen vacancies accumulate around the top surface without an electrical transmission path. As additional voltage pulses are applied, oxygen vacancies begin to move from the top surface to the bottom surface, during which time electrical charges remain difficult to transmit. Finally, the device transitions to a low resistance state (LRS) when oxygen vacancies accumulate between the top and bottom surfaces and a tunneling conduction path for electron transmission is formed.
[0166] These results show that the ACTS method can clearly distinguish the charge behavior characteristics of memristors based on ion migration.
[0167] [Example 4] ACTS measurement results in halide perovskite FAPbI3
[0168] The results of applying the ACTS method according to the present invention to the halide perovskite material FAPbI3(CH(NH2)2PbI3) will be explained with reference to FIGS. 14 and 15.
[0169] FIG. 14 shows the PFM hysteresis curve of a selected region in the halide perovskite FAPbI3, and the inset graph shows the accumulated switching charge (C) due to voltages of 1 V and 0.5 V amplitudes at 1 kHz. SW It represents ). In the PFM hysteresis curve, the typical hysteresis behavior observed in ferroelectrics was not observed, suggesting that FAPbI3 is not a ferroelectric. As can be seen in the inset graph, a negative accumulation pattern was observed in which the accumulated charge decreased with the number of pulses at both 1 V and 0.5 V amplitudes.
[0170] Figure 15 shows the switching current as a function of time and number of pulses at 1 kHz and 1 V amplitude in FAPbI3, and the results projected onto the current-time plane. Similar to TiO2, the switching current in FAPbI3 exhibited a valley shape; however, unlike TiO2, multiple valleys were observed. These multiple valleys correspond to the trap-filled limit (V). TFL ) and space charge-limited (V SCL ) Reflects the behavior of charge carriers related to conduction.
[0171] The multiple valley characteristics observed in FAPbI3 are closely related to the distribution of charge traps. As voltage increases, the traps gradually fill, and at a specific threshold (V SCL , V TFL Multiple valleys are formed as the charge transport mechanism changes in ). This characteristic clearly demonstrates that FAPbI3 is a material with charge trap properties.
[0172] In addition, through high-frequency measurements above 1 kHz, artifacts caused by ion migration could be minimized and electronic processes (charge traps) could be selectively observed. This demonstrates that the ACTS method can effectively distinguish various charge behavior mechanisms.
[0173] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will understand that other specific forms can be easily modified without altering the technical concept or essential features of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.
[0174] The scope of the present invention is defined by the claims set forth below rather than by the detailed description above, and all modifications or variations derived from the meaning and scope of the claims and the concept of equivalents thereof should be interpreted as being included within the scope of the present invention.
Claims
1. A conductive tip of an atomic force microscope (AFM) that applies voltage and measures current by contacting the surface of a material; A function generator that repeatedly generates and applies triangular wave-shaped voltage pulses to the above tip; A current amplifier that amplifies the current flowing between the tip and the material; and A device for collecting and analyzing amplified current signals in oscilloscope mode; including, Device for analyzing the charge behavior of nanoscale materials.
2. In Paragraph 1, The above triangular wave-shaped voltage pulse has an amplitude less than the anti-voltage capable of switching the polarization of the material, Device for analyzing the charge behavior of nanoscale materials.
3. In Paragraph 1, The frequency of the above triangular wave-shaped voltage pulse is 0.5 kHz to 4 kHz, Device for analyzing the charge behavior of nanoscale materials.
4. In Paragraph 1, The above analysis device analyzes the charge behavior of a material with a spatial resolution of 20 nm or less. Device for analyzing the charge behavior of nanoscale materials.
5. In Paragraph 1, The above material comprises a material selected from the group consisting of ferroelectrics, memristors, halide perovskites, dielectrics, piezoelectrics, ferromagnetics, superconductors, semiconductors, and combinations thereof. Device for analyzing the charge behavior of nanoscale materials.
6. A step of performing pre-polarization at a specific location on the surface of a material using a conductive tip of an atomic force microscope (AFM); A step of repeatedly applying triangular wave-shaped voltage pulses to the above location; A step of measuring the current generated in the material during each voltage pulse; Switching current (I) at the measured current SW ) and non-switching current (I NS Step of separating ); and The switching current is integrated with respect to time to calculate the switching charge at each pulse, and this is accumulated to obtain the total accumulated charge (C SW,acc Step of producing ); including, Method for analyzing the charge behavior of nanoscale materials.
7. In Paragraph 6, The above switching current (I SW ) and non-switching current (I NS The step of separating ) is, Current (I) measured by applying a voltage pulse in a uniform polarization state meas Step of collecting ); and By applying an additional voltage pulse after post-polarization, the non-switching current (I NS Measure ) and the measured current (I meas Non-switching current (I) in ) NS Subtract the switching current (I SW Step of calculating ); including, Method for analyzing the charge behavior of nanoscale materials.
8. In Paragraph 6, Accumulated charge (C) according to the number of pulses SW,acc The method further includes a step of identifying the charge behavior mechanism of the material by analyzing the change pattern of ), Method for analyzing the charge behavior of nanoscale materials.
9. In Paragraph 8, The above accumulated charge (C SW,acc Identify the charge behavior characteristics of the material according to the change pattern of ), Accumulated charge (C SW,acc Identify ferroelectric properties when ) exhibits a positive accumulation pattern that increases with the number of pulses, and Accumulated charge (C SW,acc Identifying nasal genetic characteristics when ) exhibits a negative accumulation pattern that decreases with the number of pulses, Method for analyzing the charge behavior of nanoscale materials.
10. In Paragraph 6, The above accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), but The above accumulated charge change pattern increases according to the number of pulses and the switching current (I SW If ) exhibits a distinct peak, it is identified as a material having polarization switching characteristics, Method for analyzing the charge behavior of nanoscale materials.
11. In Paragraph 6, The above accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), but The above accumulated charge change pattern decreases according to the number of pulses and the switching current (I SW If ) represents a single valley, it is identified as a substance having ion transport characteristics, Method for analyzing the charge behavior of nanoscale materials.
12. In Paragraph 6, The above accumulated charge change pattern and switching current (I SW Identify the charge behavior mechanism of the material based on the characteristics of ), but The above accumulated charge change pattern decreases according to the number of pulses and the switching current (I SW If ) exhibits multiple valleys, it is identified as a material having charge trap characteristics, Method for analyzing the charge behavior of nanoscale materials.
13. In a system for identifying charge behavior characteristics of a material at the nanoscale, An atomic force microscope (AFM) that applies voltage and measures current by contacting the surface of a material; A function generator that repeatedly generates and applies triangular wave-shaped voltage pulses to the conductive tip of the above AFM; A current amplifier that amplifies the current flowing between the above tip and the material; A device for collecting amplified current signals in oscilloscope mode; and A processing unit that analyzes collected current signals to identify the charge behavior mechanism of a material based on the accumulated charge change pattern and the characteristics of the switching current; Includes, The above processing unit is, Accumulated charge (C SW,acc ) increases according to the number of pulses and the switching current (I SW If ) exhibits a peak, it is identified as a material having polarization switching characteristics, and Accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW If ) exhibits a single valley, it is identified as a substance having ion transport characteristics, and Accumulated charge (C SW,acc ) decreases with the number of pulses and the switching current (I SW Identifying a material as having charge trap characteristics when it exhibits multiple valleys, Charge behavior characteristic identification system.
14. In Paragraph 13, The above-mentioned charge behavior characteristic identification system analyzes the local charge behavior of a material with a spatial resolution of 20 nm or less, Charge behavior characteristic identification system.
15. In Paragraph 13, The above triangular wave-shaped voltage pulse is characterized by having an amplitude less than or equal to the antivoltage of the substance to be analyzed and having a frequency between 0.5 kHz and 4 kHz. Charge behavior characteristic identification system.
16. In Paragraph 13, The above system further includes a function to measure ferroelectricity based on electromechanical response at the same location as the part measured by the AFM tip, and to analyze the correlation between the charge behavior characteristics and surface polarization state of the material. Charge behavior characteristic identification system.
17. An apparatus for analyzing the charge behavior of a nanoscale material according to claim 1, comprising Electronic device characteristic evaluation device.
18. In a computer-readable recording medium in which a computer program is stored, The above computer program includes instructions that cause the computer to perform the method for analyzing the charge behavior of a nanoscale material according to claim 6. Computer-readable recording medium.