Magnesium chloride purification systems, devices and methods
The direct dehydration of ammonium magnesium and rare earth chloride hydrates in a molten salt composition addresses the complexity and inefficiency of existing electrolyte production methods, achieving high-purity anhydrous electrolytes with reduced oxide impurities and improved sustainability.
Patent Information
- Application Number
- PCT/US2026/026687
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-05
- Filing Date
- 2026-05-05
- Publication Date
- 2026-11-12
AI Technical Summary
Existing methods for producing anhydrous magnesium chloride and rare earth chloride electrolytes are complex, energy-intensive, and prone to oxide impurity formation, leading to equipment degradation and environmental harm, while current purification processes are inefficient and costly.
A method involving the use of ammonium magnesium chloride hydrates and ammonium rare earth chloride hydrates to produce anhydrous magnesium and rare earth chlorides by direct dehydration in a molten salt composition without the need for protective coverings, reducing oxide impurities through simultaneous off-gassing of H2O, NH3, and HCl molecules.
This approach yields high-purity anhydrous electrolytes with reduced oxide impurities, simplifying the process, saving energy, and avoiding equipment clogging, thus enhancing the efficiency and sustainability of magnesium and rare earth metal production.
Smart Images

Figure US2026026687_12112026_PF_FP_ABST
Abstract
Description
MAGNESIUM CHLORIDE PURIFICATION SYSTEMS, DEVICES AND METHODS CROSS REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of and priority to U. S. provisional patent application No. 63 / 799,952, filed on May 5, 2025; the content of which is herein incorporated in entirety by reference.FIELD OF TECHNOLOGY
[0002] The present technology relates to devices, methods and systems for the purification of magnesium chloride.
[0003] Environmentally friendly purification of metal salt compositions such as feedstocks for metal production via electrowinning or chemothermic processes, particularly electrolytes comprising magnesium chloride and aluminum chloride, is desirable as industries seek to decarbonize their operations. Typical impurities, such as water of hydration, magnesium oxide, magnesium hydroxide and magnesium hydroxychloride or their aluminum, rare earth metal, or other metal counterparts are problematic in the production of metal via electrolysis as they attack the graphite electrodes used in the electrochemical cell causing degradation and need for electrode replacement. Over the years, people have tried many methods for the production of pure, anhydrous, magnesium and chloride feed materials but most have failed to be operated with commercial success or are extremely expensive to build. The push for the decarbonization of the industrial economy necessarily entails the substitution of renewable energy sources for fossilbased electricity generation. A major segment of energy consumption is the production of structural metals. The smelting of steel has a large carbon footprint, and one key structural metal, aluminum, requires large quantities of electricity for its electrolytic production that consumes carbon anodes, producing carbon dioxide directly in production. Both steel and aluminum require significant mining of iron ore and bauxite in their supply chains, respectively, which has major social and environmental impacts. Magnesium metal is an attractive alternative to aluminum and steel in structural metal applications because it has the highest strength to weight ratio of all major structural metals, meaning it can be used for lightweighting of structures in transportation applications. The feedstock for magnesium metal production can be economically extracted fromseawater and brines, obviating the need for environmentally destructive mining, which is required in the production of bauxite, the principal aluminum ore, and for extraction of iron ore to make steel. Magnesium can be produced electrolytically, allowing the use of renewable and other low carbon electricity sources for its production. Magnesium electrolytic production does not directly emit carbon dioxide in the same manner as alumina cryolite electrolysis with carbon anodes, nor does it emit significant quantities of fluorinated compounds as occur in aluminum production and which are strong greenhouse gases, implying the production process can be more easily decarbonized. However, the production of electrolytic quality magnesium chloride is difficult and energy intensive due to the difficulty of removing waters of hydration and other oxygen containing compounds such as, but not limited to, magnesium hydroxide, magnesium hydroxychlorides, magnesium oxide, calcium hydroxide, calcium hydroxychloride, and calcium oxide, from magnesium chloride. Strelets, K. L., Electrolytic Production of Magnesium. 1977: Israel Program for Scientific Translations ISBN 0 7065 1567 6 (incorporated herein in its entirety), provides a broad overview of the technologies actively developed for the electrolytic production of magnesium, including the preparation of suitable electrolytes. It discloses an apparatus for the slow, stepwise dehydration of ammonium magnesium chloride hydrates before contacting it with an electrolyte melt.
[0004] One of the key issues to provide for the economic production of magnesium is the preparation of suitably pure and dry magnesium chloride. Unless handled properly, hydrous magnesium chloride undergoes hydrolysis with the loss of HC1 when attempts to remove the last two waters of hydration are made.
[0005] Molten chloride salts are conventionally used as feedstock materials in molten salt electrolyzers producing chlorine gas and molten metal. However, in the case of magnesium production, preparation of a MgCl2free of oxide impurities is challenging and the oxide impurities cause degradation to the electrolyzer devices. As such, great effort has been expended in developing methods of producing oxide-free magnesium chloride and / or oxide-free molten salt electrolytes containing an appreciable quantity of magnesium chloride. Many of these efforts, such as that given in United States Patent US No. 1,874,373, incorporated herein by reference, have resulted in complicated multi-step process designs and extensive, complicated flowsheets, which the present technology attempts to address.
[0006] Several approaches to dealing with this issue have been developed. One method that has been described is the use of ammoniate inclusion compounds. US Patent No. 5,439,563, incorporated herein by reference, describes such a process of converting magnesium chloride hydrates to anhydrous magnesium chloride ammoniate coordination compounds and their use to replenish spent magnesium chloride-based electrolytes.
[0007] A second method uses the formation of intermediate double salts, or “carnallites”, which can be dehydrated and further decomposed to anhydrous magnesium chloride without the concomitant hydrolysis that occurs upon dehydration of the chloride itself. United States Patent US No. 1,276,499, incorporated herein by reference, describes the use of anhydrous ammonium magnesium chloride (NH4CI MgCh); to prepare anhydrous magnesium chloride by introducing the anhydrous double salt into a fused salt melt. Chinese Patent CN102491382B, incorporated herein by reference, discloses that ammonium magnesium chloride double salts with up to 3 waters of hydration hydrates (NHrCl-MgCh'xEhO, where x is 3 or less) may be used to produce anhydrous magnesium chloride melts suitable for use for the electrolytic production of magnesium. However, it is known that using such methods to produce anhydrous metal chlorides from the higher-level hydrates of ammonium magnesium chloride double salts leads to unacceptable levels of impurities.
[0008] In more detail, this process, like the one described in CN102491382B, incorporated herein by reference, entails dehydrating magnesium chloride by creating a mixed “ammonium carnallite” salt of NH4CI MgCh 6H2O (generally NH4Cl-MgCl2·xH2O, where x may be 0 to 6) which is reported to be more resistant to hydrolysis than pure hydrated magnesium chloride. Such flowsheets have typically involved stepwise processes where some of the water molecules are driven off initially at low temperature, followed by a higher temperature kiln between 200°C < T < 450°C where the newly dried NH4CI MgCh O-3H2O, described in the patent as “low water ammonium carnallite”, is decomposed into anhydrous solid MgCh, as well as NH3 and HC1 vapors by heating under a cover of alumina or quartz sand. Unfortunately, these vapors are challenging to maintain in the gas phase as they condense as solids at temperatures <350°C, clogging pipework. This results in costly designs and temperamental process equipment. However, as has been noted in the above-mentioned references, the removal of ammonium chloride thus produced remains a problematic issue. Another issue is the necessity of the intermediate drying step of the initialammonium magnesium chloride hydrate. The present technology does not require the covering of the vessel in which the ammonium carnallite is decomposed into anhydrous magnesium chloride.
[0009] Rare-earth metals are conventionally produced through oxyfluoride electrolysis which requires hazardous materials and emits environmentally harmful byproducts, such as perfluorocarbons (pfc). Rare-earth chloride (REClx) electrolysis can circumvent these shortcomings, but the salts must be dry and free of oxide impurities to obtain the >99.5% purity needed in high value applications (such as NdFeB magnets) to ensure long-lasting cell life (Holcombe, B. P., Villalobos, A., Sinclair, N. S. et al. Chloride Molten Salt Electrolysis Enables Integrated and Energy-Efficient Process for NdFeB Magnet Fabrication. JOM (2025), incorporated herein by reference).
[0010] Existing technologies produce anhydrous REClxusing hydrogen chloride fluidized beds. These stepwise processes involve calcining the hydrated rare earth chloride at higher temperatures for multiple hours to prevent significant oxide formation. This calcining in an atmosphere that encourages REClxdehydration instead of hydrolysis reduces oxide formation to less than 5% (Joung Woon Kim, Wongeun Lee, Insung Hwang, Jin-young Lee, Choon Han. (2014). Thermal Decomposition Characteristics of NdC13’6H2O. Journal of the Korean Society of Mineral and Energy Resources Engineers, 51(2), 202-210). The anhydrous salt can then be melted with a eutectic of contemporary salts to form an appropriate electrolyte mixture. As stated previously, however, rare earth chloride electrolysis requires electrolyte of even higher purity than 95% so this method is not sufficient for electrolysis.
[0011] Prior attempts to produce anhydrous REClxusing ammonium chloride have also been disclosed. These stepwise processes involve heating at a low temperature to remove initial water. REClxcompounds are fully calcined to form RE2O3due to their tendency to hydrolyze during dehydration. The oxide is then subsequently heated in the presence of NH4CI to a temperature greater than NH4CI thermal decomposition (>350 °C) (A Study on the Production of Anhydrous Neodymium Chloride through the Chlorination Reaction of Neodymium Oxide and Ammonium Chloride, Minerals 2024, Joo-yun Wu, incorporated herein by reference). The evolved HC1 then hydrochlorinates the rare earth oxides and produces anhydrous REClx. The present invention aimsto avoid the need for the inefficient calcination step by enabling full dehydration to occur without out the production of the undesired hydrolysis species.SUMMARY OF TECHNOLOGY
[0012] The present technology provides for the use of ammonium magnesium chloride hydrates bearing more than 3 waters of hydration for the production of anhydrous magnesium-based electrolytes having a low proportion of magnesium hydroxide, magnesium oxide, or magnesium hydroxy chloride.
[0013] The present technology also provides for the use of ammonium magnesium chloride salts (ammonium carnallite) bearing various levels of waters of hydration (NH4Cl·MgCl2·xH2O) for the conversion of magnesium oxides, magnesium hydroxide and magnesium hydroxychloride in magnesium chloride melts into magnesium chloride, thus providing high purity anhydrous magnesium chloride melts. The present technology also provides for the reduction in magnesium oxide, magnesium hydroxide or magnesium hydroxychloride levels in magnesium chloride electrolytes. The present technology does not require the covering of the vessel in which the ammonium carnallite is decomposed into anhydrous magnesium chloride. The present technology also provides for the production of rare earth metal chloride electrolytes.
[0014] In one embodiment, the present technology provides for a method of producing a magnesium chloride electrolyte melt comprising contacting an ammonium carnallite solid having more than three waters of hydration with a molten salt composition comprising at least one of magnesium chloride, sodium chloride, or potassium chloride.
[0015] In one embodiment, the present technology provides for a method of producing a magnesium chloride electrolyte melt comprising contacting an ammonium carnallite solid having more than three waters of hydration with a molten salt composition comprising at least one of magnesium chloride, sodium chloride, or potassium chloride, and further comprising at least 1 wt.% total magnesium oxide, magnesium hydroxide or magnesium hydroxychloride and wherein the produced magnesium chloride electrolyte melt comprises less than 0.3wt.% total magnesium hydroxide, magnesium oxide, or magnesium hydroxychloride.
[0016] In one embodiment, the present technology provides for a method of producing a magnesium chloride electrolyte melt comprising contacting a mixture of solid ammonium chloride and a solid magnesium chloride hydrate with a molten salt composition comprising at least one of magnesium chloride, sodium chloride, potassium chloride.
[0017] In one embodiment, the present technology provides for a method of producing a magnesium chloride electrolyte melt comprising contacting solid ammonium chloride with a molten salt composition comprising at least one of magnesium chloride, sodium chloride, or potassium chloride, and further comprising at least lwt.% total magnesium oxide, magnesium hydroxide or magnesium hydroxychloride wherein the produced magnesium chloride electrolyte melt comprises less than 0.3 wt.% total magnesium hydroxide, magnesium oxide, or magnesium hydroxy chloride.
[0018] The present technology also provides for a method obtained for producing, purifying, or replenishing a rare earth chloride (REClx)-containing electrolyte obtained by contacting a double salt, or mixture of REClx·yH2O and NH4CI with a molten salt composition, where 1 < y < 7 and x is 2 or 3.
[0019] Once prepared, the mixed or double salt of NH4Cl-REClx·yH2O can be added via screw feeder or other solids loading device into a chamber filled with a quantity of molten electrolyte containing 0% - 10% REClx. Provided that the temperature is >450°C and the electrolyte has sufficient superheat above its freezing point to provide the required dehydration energy, then the NP Cl-REClx’yl O will land on the electrolyte and begin to simultaneously dehydrate and decompose the contained NH4C1. This causes the simultaneous off gassing of H2O, NH3, and HC1 molecules as per eqs. 5 & 6 for the neodymium and praseodymium for example. Surprisingly, the rapid dehydration of these hydrated salts results in an anhydrous electrolyte mixture substantially free of oxide impurities.
[0020] Yet another surprising aspect of the rapid dehydration of these double salts is their ability to hydrochlorinate oxide, hydroxide or hydroxychloride contaminants already present in the molten salt composition.
[0021] The present technology also provides for a method of producing, purifying or replenishing a rare earth molten salt electrolyte by the addition of NH4CI to a molten chloride electrolyte with oxide, hydroxide or hydroxychloride contamination to substantially or completely converts the oxide, hydroxide or hydroxychloride contamination to REClx.
[0022] The present technology also provides for a method of producing, purifying or replenishing a rare earth molten salt electrolyte by the simultaneous addition of RE2O3 (rare earth oxide) and NH4CI into a molten chloride electrolyte. In-situ generated HC1 converts the RE2O3 into RECk and H2O as shown in eqs. 11 & 12 as for the neodymium and praseodymium examples. This embodiment does not require REClx.yFbO as a feedstock but can use RE2O3 as a feedstock instead.
[0023] The present technology provides for the use of ammonium rare earth chloride salt hydrates for the production, purification or replenishment of anhydrous rare earth-based electrolytes having a low proportion of rare earth oxide, rare earth hydroxide and rare earth hydroxychloride. The present technology also provides for the use of ammonium rare earth chloride salt hydrates bearing various levels of waters of hydration for the conversion of rare earth oxide, rare earth hydroxide and rare earth hydroxychloride in rare earth chloride melts into magnesium chloride, thus providing high purity anhydrous rare earth chloride melts. The present technology also provides for the reduction in rare earth oxide, rare earth hydroxide and rare earth hydroxychloride levels in rare earth chloride electrolytes.
[0024] In one embodiment, the present technology provides for a method of producing, purifying or replenishing a rare earth chloride electrolyte melt comprising contacting an ammonium rare earth carnallite solid with a molten salt composition comprising at least one of rare earth chloride, sodium chloride, or potassium chloride.
[0025] In one embodiment, the present technology provides for a method of producing, purifying or replenishing a rare earth chloride electrolyte melt comprising contacting an ammonium rare earth carnallite solid with a molten salt composition comprising at least one of rare earth chloride, sodium chloride, or potassium chloride, and further comprising at least 1 wt.% total rare earth oxide, rare earth hydroxide or rare earth hydroxychloride and wherein the produced rare earth chloride electrolyte melt comprises less than 0.25 wt.% total rare earth oxide, rare earth hydroxide or rare earth hydroxy chloride.
[0026] In one embodiment, the present technology provides for a method of producing, purifying or replenishing a rare earth chloride electrolyte melt comprising contacting a mixture of solid ammonium chloride and a solid rare earth chloride hydrate with a molten salt composition comprising at least one of rare earth chloride, sodium chloride, potassium chloride.
[0027] In one embodiment, the present technology provides for a method of producing, purifying or replenishinga rare earth chloride electrolyte melt comprising contacting solid ammonium chloride with a molten salt composition comprising at least one of rare earth chloride, sodium chloride, or potassium chloride, and further comprising at least lwt.%, 2wt.%, 3wt.%, 4wt.% or 5wt.% total rare earth oxide, rare earth hydroxide or rare earth hydroxychloride wherein the produced rare earth chloride electrolyte melt comprises less than lwt.%, 0.5wt.%, 0.25wt.%, 0. lwt.%, or 0.05wt.% total rare earth oxide, rare earth hydroxide, or rare earth hydroxychloride.BRIEF DESCRIPTION OF FIGURES
[0028] All features of embodiments which are described in this disclosure are not mutually exclusive and can be combined with one another. For example, elements of one embodiment can be utilized in the other embodiments without further mention. A detailed description of specific embodiments is provided herein below with reference to the accompanying drawings in which:
[0029] Figure 1A illustrates a non-limiting process of production of magnesium chloride, aluminum chloride, iron chloride or rare earth metal electrolyte melt starting with a solution of metal chloride and a solution of ammonium chloride.
[0030] Figure IB illustrates a non-limiting process of production of metal chloride electrolyte melt starting with solid metal oxide and solid ammonium chloride.
[0031] Figure 1C illustrates a non-limiting process of reducing the metal oxide or metal hydroxy chloride content of a metal chloride electrolyte melt using solid ammonium chloride.
[0032] Figure ID illustrates a non-limiting process of production of a metal chloride electrolyte melt using solid ammonium carnallite hydrate by introducing ammonium carnallite hydrate into a chamber in thermal and fluid communication with an electrolyzer.DETAILED DESCRIPTION OF TECHNOLOGY
[0033] As used herein, the singular forms “a,” “an” and “the” include plural referents unless the context clearly dictates otherwise.
[0034] As used herein, the term “or” refers to the inclusive form of “or” unless explicitly stated to the contrary.
[0035] As used herein, ranges are inclusive, so the range “from 4 to 6, includes 4 and 6.
[0036] As used herein, ranges and amounts can be expressed as “about” a particular value or range. As used herein the term “about” also includes the exact amount. Hence “about 5 percent” means “about 5 percent” and also “5 percent.” “About” means within typical experimental error for a measurement typically used for purpose intended, or, if referred to in the context of a process parameter, the term about should be construed in the context of the sensitivity of such process to the particular parameter. When a list of parameters or ranges is preceded by the term “about”, it is intended that the term “about” applies to each of the members of the list.
[0037] As used herein, “optional” or “optionally” means that the subsequently described event or circumstance does or does not occur, and that the description includes instances where the event or circumstance occurs and instances where it does not. For example, an optional component in a system means that the component may be present or may not be present in the system.
[0038] As used herein, “weight percent” or “wt.%” refers to the concentration of a substance as the weight of that substance divided by the total weight of the composition and multiplied by 100.
[0039] As used herein, the term “brine” refers to any aqueous solution comprising metal salts. Typically, a brine will comprise sodium, calcium, potassium or magnesium compounds, typically chlorides, bromides, iodides, hydroxides, carbonates, sulfates, bicarbonates or sulfides. Typically, the magnesium compound may be a magnesium salt, a magnesium oxide, a magnesium a magnesium hydroxide, or a magnesium hydroxy halide.
[0040] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as is commonly understood by one of ordinary skill in the art to which the inventions belong. All patents, patent applications, published applications and publications, websites and other published materials referred to throughout the entire disclosure herein, unless notedotherwise, are incorporated by reference in their entirety. In the event that there are a plurality of definitions for terms herein, those in this section prevail. Where reference is made to a URL or other such identifier or address, it is understood that such identifiers can change and particular information on the internet can come and go, but equivalent information can be found by searching the internet. Reference thereto evidences the availability and public dissemination of such information.
[0041] In the present case, it is found that there is a simple method obtained for producing, purifying or replenishing a MgCh-containing electrolyte obtained by first mixing a common feedstock material, for example, 30 wt.% MgCh brine and mixing it with solid NH4CI or a solution of NH4CI. This material can then be evaporated into a concentrated mixture whereupon it can be solidified into a hydrated mixed salt, typically NLLCl-MgCh’bhhO, but the level of hydration may be varied under different evaporation conditions. This hydrated mixed salt will have the composition NH4Cl·MgCl2·xH2O, where x can range from 0-6. The present technology relates to the use of NH4Cl·MgCl2·xH2O to produce or replenish magnesium chloride electrolytes where x is greater than 3, greater than 4, greater than 5, or 6 and greater by contacting the NLLiCl-MgCh’xThO with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0042] The present technology also provides methods for the production, purification, or replenishment of a magnesium chloride electrolyte by contacting a mixture of NH4CI and MgCh’bthO with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0043] The present technology also provides methods for the production, purification, or replenishment of a magnesium chloride electrolyte by contacting a mixture of NH4Cl and Mg(OH)2with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0044] The present technology also provides methods for the production, purification, or replenishment of a magnesium chloride electrolyte by contacting a mixture of NH4CI and MgOHCl with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0045] The present technology also provides methods for the production, purification, or replenishment of a magnesium chloride electrolyte by contacting a mixture of NH4CI and MgO with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0046] The present technology also provides methods for the production, purification, or replenishment of a magnesium chloride electrolyte by contacting a mixture of NH4CI and a composition comprising MgCl2·xH2O, MgOHCl, MgO, or a mixture thereof with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl, where x is greater than 3.
[0047] In one embodiment, the present technology provides for methods of magnesium electrolyte production of replenishment wherein the contact of the mixture of NH4CI and a composition comprising MgCl2·xH2O, MgOHCl, MgO, or a mixture thereof with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer such as alumina or silica sand, or other solid powder having a melting point of greater than 500 °C.
[0048] In one embodiment, the present technology provides for methods of magnesium electrolyte production of replenishment wherein the contact of the NH4Cl·MgCl2·xH2O, where x is greater than 3, with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer such as alumina or silica sand, or other solid powder having a melting point of greater than 500°C.
[0049] In one embodiment, the present technology provides for methods of magnesium electrolyte production of replenishment wherein the contact of the mixture of NH4CI and a composition comprising MgCh’xHiO, MgOHCl, MgO, or a mixture thereof with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer of an inert gas such as nitrogen or argon.
[0050] In one embodiment, the present technology provides for methods of magnesium electrolyte production of replenishment wherein the contact of the ISHtCl-MgCh’xftO, where x is greater than 3, with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer of an inert gas such as nitrogen or argon.
[0051] The present technology provides methods to produce a magnesium chloride electrolyte from an electrolyte pre-mix, which is a molten salt composition typically comprising KC1, CaCl2, or NaCl, or a mixture thereof and further comprising little or no MgCh, MgO, MgOH2, or MgOHCl.
[0052] Typically, the electrolyte pre-mix comprises less than 0.1wt.%, less than 0.5wt.%, or less than lwt.%, total of MgCh, MgO, MgOH2, or MgOHCl, or a mixture thereof.
[0053] Typically, an electrolyte pre-mix is a molten salt composition comprising less than 1 wt.% magnesium oxides or salts and has not been previously subjected to electrolysis.
[0054] In some embodiments, an electrolyte pre-mix may comprise less than 2wt.%, 3wt.%, 4wt%, 5wt.% or 10wt.% magnesium oxides or salts
[0055] The present technology provides methods to replenish a spent magnesium chloride electrolyte from a spent magnesium chloride electrolyte wherein the spent magnesium electrolyte comprises less than 35wt.%, less than 30wt.%, less than 25wt.%, less than 20wt.%, less than 19wt.%, less than 18wt.%, less than 17wt.%, less than 16wt.%, less than 15wt.%, less than 14wt.%, less than 13wt.%, less than 12wt.%, less than 11wt.%, less than 10wt.%, less than 9wt.%, less than 8wt%, less than 7wt.%, less than 6wt.%, less than 5wt.%, less than 4wt.%, less than 3wt.%, less than 2wt.%, or less than lwt.% total MgCh, MgO, MgOH2, or MgOHCl.
[0056] In one embodiment, replenishment of the magnesium chloride electrolyte may be performed batch-wise, where upon the completion of an electrolysis operation, the now spent magnesium chloride electrolyte is replenished by the methods described herein.
[0057] In another embodiment, the replenishment may be performed continuously, to maintain a desired magnesium chloride content, without stopping the electrolysis operation.
[0058] Typically, the desired magnesium chloride content of the magnesium chloride electrolyte is between about 10wt.% and 25wt.%, 15wt.% and 25wt.%, 17wt.% and 23wt.% or 18wt.% and 22wt.%.
[0059] Preferably, the desired magnesium chloride content of the magnesium chloride electrolyte is between about 19wt.% and 21wt.%.
[0060] Typically, the electrolyte pre-mix will comprise less than 0. lwt.%, less than 0.5wt.%, less than lwt.%, less than 2.5wt.%, less than 5wt.%, less than 7.5wt.%, or less than 10wt.% total of MgCh, MgO, MgOH2, or MgOHCl.
[0061] In some embodiments, the molten salt composition may comprise KC1, CaCl2, or NaCl, or a mixture thereof.
[0062] In some embodiments, the molten salt composition may be magnesium chloride electrolyte, spent magnesium chloride electrolyte, or electrolyte pre-mix.
[0063] Typically, magnesium chloride electrolyte comprises more than 15% magnesium chloride and further comprises KC1, CaCl2, or NaCl, or a mixture thereof.
[0064] Typically, spent magnesium chloride electrolyte is magnesium chloride electrolyte which has been depleted in magnesium chloride through electrolysis. Spent magnesium chloride electrolyte typically comprises less than or equal to 15wt.% magnesium chloride.
[0065] In one embodiment, the magnesium chloride electrolyte or the molten salt composition comprises KC1 at a concentration (wt.%) of 0-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25-30%, 30-35%, 35-40%, 40-45%, 45-50%, 50-55%, 55-60%, 60-65%, 65-70%, 70-75%, 75-80%, 80-85%, 85-90%, 90-95%, or 95-100%.
[0066] In another embodiment, the magnesium chloride electrolyte or the molten salt composition comprises NaCl at a concentration (wt.%) of 0-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25-30%, 30-35%, 35-40%, 40-45%, 45-50%, 50-55%, 55-60%, 60-65%, 65-70%, 70-75%, 75-80%, 80-85%, 85-90%, 90-95%, or 95-100%.
[0067] In another embodiment, the magnesium chloride electrolyte or the molten salt composition comprises CaCl2at a concentration (wt.%) of 0-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25-30%, 30-35%, 35-40%, 40-45%, 45-50%, 50-55%, 55-60%, 60-65%, 65-70%, 70-75%, 75-80%, 80-85%, 85-90%, 90-95%, or 95-100%.
[0068] One advantage of the present technology is that it does not require extensive, or in some cases any drying of the NEUCl-MgCh’xHzO intermediate feedstock, thus saving energy and additional unit operations during the magnesium chloride electrolyte production or enrichment.
[0069] In certain embodiments, the magnesium chloride solution may be a brine.
[0070] Table 1 outlines chemical equations in accordance with some embodiments of the present technology:Table 1: Chemical Equations
[0071] Equation 1 shows an idealized dehydration of magnesium ammonium carnallite hexahydrate. Currently, this step needs to be performed in a stepwise fashion in order to avoid the hydrolysis reaction as exemplified in Equation 2.
[0072] Equation 3 shows the chlorination of magnesium oxide using magnesium ammonium carnallite hexahydrate as one embodiment of the present technology.
[0073] Equation 4 shows the chlorination of magnesium oxide using ammonium chloride as one embodiment of the present technology.
[0074] Equations 5 and 6 show an idealized dehydration of neodynium ammonium carnallite hexahydrate and praseodymium ammonium carnallite heptahydrate to their respective anhydrous chlorides. Currently, this step needs to be performed in a stepwise fashion in order to avoid the hydrolysis reaction as exemplified in Equations 7 and 8.
[0075] Equations 9 and 10 show an idealized dehydration of neodymium oxychloride and praseodymium oxychloride to their respective anhydrous chlorides.
[0076] Equations 11 and 12 show an idealized dehydration of neodymium oxide and praseodymium oxide to their respective anhydrous chlorides.
[0077] Once prepared, these crystals of NH4Cl·MgCl2·xH2O can be added into a chamber filled with a quantity of molten MgCh-containing electrolyte. Provided that the temperature is > 450 °C and the electrolyte has sufficient superheat above its freezing point, then the NH4Cl·MgCl2·xH2O will land on the electrolyte and begin to simultaneously dehydrate and thermally decompose the contained NH4CI. This causes the simultaneous off gassing of H2O, NH3, and HC1 molecules as per eqn. 1. Surprisingly, it is found that the rapid evaporation of these molecules yield an oxide-free magnesium chloride-containing electrolyte. The high temperature of the molten salt chamber combined with the abundance of water vapor which can solubilize any condensed NH4CI, protectsagainst NH4CI re-condensation in the equipment which would otherwise cause clogs in pipework and other operational problems.
[0078] Additionally, NH4Cl-MgC12’6H2O salts can be added to a magnesium chloride containing electrolyte with oxide contamination and substantially reduce the undesired oxide impurities as shown in equation 3.
[0079] In one embodiment of this invention, NH4CI is added to a molten MgCh-containing electrolyte with MgO contamination to substantially or completely convert MgO to MgCh as shown in equation 4.
[0080] n some embodiments, the contamination may comprise MgO, Mg(OH)2, MgOHCl, or a combination thereof.
[0081] In another embodiment MgO and NH4CI are fed simultaneously into an electrolyte melt. The NH4CI converts the MgO into MgCh and H2O as defined by equation 4. This embodiment does not require MgCh as a feedstock but MgO instead. This embodiment does not require NH4CI to be combined with MgC ’xhhO. Alternatively, the magnesium source may be Mg(OH)2or MgOHCl. In some embodiments, the magnesium source may be a mixture comprising MgO, Mg(OH)2, MgOHCl, or a combination thereof.
[0082] In one embodiment, the present technology provides for a method of producing an anhydrous magnesium chloride melt comprising the steps of: 1) providing a brine comprising from about 0.1wt.% to about 30 wt.% aqueous magnesium chloride between about 95 C and 200°C; 2) mixing the said about about 0.1wt.% to about 30wt.% aqueous magnesium chloride with about an equal amount of 0.1wt.% to about 30wt.% aqueous ammonium chloride between about 95°C and 200°C; 3) evaporating the mixture until the leftover solution achieves an approximate stoichiometry of NH4CbMgCh’6H2O; 4) cooling the leftover solution until it solidifies into a solid; and, 5) contacting the solid with a magnesium chloride electrolyte comprising about 0-30 wt.% magnesium chloride; thus obtaining a magnesium chloride electrolyte substantially free from magnesium hydroxide, magnesium oxide and magnesium hydroxychloride.
[0083] In one embodiment, the ratio of the volume of magnesium chloride solution to the volume of the ammonium chloride solution that is mixed prior to the evaporation is about 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1,1:1.05, 1:1.1, 1:1.15, 1:1.2, 1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45, 1:1.5, 1:1.55, 1:1.60, 1:1.65, 1:1.7, 1: 1.75, 1:1.85, 1:1.9, 1: 1.95, 1:2, or a range consisting any two of these ratios as endpoints.
[0084] In one embodiment, the ratio of the molarity of magnesium chloride solution to the molarity of the ammonium chloride solution that is mixed prior to the evaporation is about 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1, 1:1.05, 1:1.1, 1:1.15, 1:1.2, 1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45, 1:1.5, 1:1.55, 1:1.60, 1:1.65, 1:1.7, 1:1.75, 1:1.85, 1:1.9, 1:1.95, 1:2, or a range consisting any two of these ratios as endpoints.
[0085] In one embodiment, the ratio of the volume of magnesium chloride solution and the volume of the ammonium chloride solution that is mixed prior to the evaporation is about 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.7, 1:1.8, 1:2, 1:2.5, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or a range consisting any two of these ratios as endpoints.
[0086] In one embodiment, the ratio of the molarity of magnesium chloride solution and molarity of the ammonium chloride solution that are mixed prior to the evaporation is about 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.7, 1:1.8, 1:2, 1:2.5, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or a range consisting any two of these ratios as endpoints.
[0087] In one embodiment, the concentration of either the magnesium chloride solution or the ammonium chloride solution may be 5 wt.%, 10 wt.%, 15 wt.%, 20 wt.%, 25 wt.%, 30 wt.%, 35 wt.%, 40 wt.%, 45 wt.%, 50 wt.%, 55 wt.%, 60 wt.%, 65 wt.%, 75 wt.%, 80 wt.%, 85 wt.%, 90 wt.%, 95 wt %, or a range consisting any two of these ratios as endpoints.
[0088] In one embodiment, the molar ratio of MgCh to NH4CI of the evaporated solid is about 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.7, 1:1.8, 1:2, 1:2.5, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or a range consisting any two of these ratios as endpoints.
[0089] In a preferred embodiment, the molar ratio of MgCh to NH4CI of the evaporated solid is about 04-0.5:1, 0.5-0.75, 0.75-1:1, 1:1, 1:1-1.25, 1:1.25-1.5, 1:1.5-1.75, 1:1.75-2, 1:2-3, 1:3-4, or 1:4-5.
[0090] In one embodiment, the evaporated solid comprises about 3.05 to 3.5 waters of hydration per atom of magnesium.
[0091] In one embodiment, the evaporated solid comprises about 3.5 to 4 waters of hydration per atom of magnesium.
[0092] In one embodiment, the evaporated solid comprises about 4 to 5 waters of hydration per atom of magnesium.
[0093] In one embodiment, the evaporated solid comprises about 5 to 6 waters of hydration per atom of magnesium.
[0094] In one embodiment, the evaporated solid comprises about 3.05 to 6 waters of hydration per atom of magnesium.
[0095] The mixing of the ammonium chloride with the magnesium chloride may be accomplished in several ways. Non-limiting examples are described below.
[0096] In one embodiment, the ammonium chloride and magnesium chloride may be introduced as their respective aqueous solutions.
[0097] In another embodiment, solid ammonium chloride may be introduced into an aqueous solution of magnesium chloride.
[0098] In still another embodiment, solid magnesium chloride hydrate may be introduced into an aqueous solution of ammonium chloride.
[0099] In still another embodiment, a mixture of solid ammonium chloride and solid magnesium chloride hydrate may be introduced into molten magnesium chloride hydrate or molten magnesium chloride electrolyte.
[0100] In still another embodiment, solid ammonium chloride may be introduced into molten magnesium chloride hydrate or molten magnesium chloride electrolyte.
[0101] In one embodiment, crystallization of the solution which takes place in an evaporator into a hydrated NH4Cl·MgCl2·6H2O salt after NH4CI addition is performed at between about -60 °C and -20 °C, -20 °C and 20 °C, 20 °C and 60 °C, 60 °C and 100 °C, 100 °C and 140 °C, 140 °C and 180 °C, 180 °C and 220 °C, 220 °C and 260 °C, 260 °C and 300 °C, or 300 °C and 340 °C.
[0102] In one embodiment, the dehydration of the hydrated NH4Cl·MgCl2salt in the magnesium chloride melt is performed at between about 360 °C and 400 °C, 400 °C and 420 °C,420 °C and 460 °C, 460 °C and 500 °C, 500 °C and 540 °C, 540 °C and 580 °C, 580 °C and 620 °C, 620 °C and 660 °C, 660 °C and 700 °C, or 700 °C and 740 °C.
[0103] In one embodiment, the concentration of magnesium chloride in the molten salt may be 0 wt.%, 5 wt.%, 10 wt.%, 15 wt.%, 20 wt.%, 25 wt.%, 30 wt.%, 35 wt.%, 40 wt.%, 45 wt.%, 50 wt.%, 55 wt.%, 60 wt.%, 65 wt.%, 75 wt.%, or a range consisting any two of these ratios as endpoints
[0104] In one embodiment, the hydrated NH4Cl·MgCl2salt may be introduced into a molten electrolyte containing equal parts MgCF, NaCl, CaCl2, and KC1.
[0105] In one embodiment, the hydrated NH4Cl·MgCl2salt may be introduced into the molten magnesium chloride electrolyte by dropping it on top of a container holding the molten magnesium chloride electrolyte. In some embodiments, hydrated NH4Cl-MgCh salt may be added directly to the molten electrolyte in a magnesium electrolysis cell or a vessel that is in fluid communication with an electrolyzer. In some embodiments, agitation via inert gas bubbling or mechanical agitation may be used to enhance the reaction of the evaporated solid with the molten magnesium chloride electrolyte. In some embodiments the molten salt bed is fully exposed to atmosphere where air is allowed to flow over the top of the molten salt.
[0106] In another embodiment, a venturi system may be used to introduce the evaporated solid into a stream of molten magnesium chloride electrolyte.
[0107] Figures 1 A-D illustrate some of the non-limiting basic modes of operation of the system and method of production of magnesium chloride electrolyte that is substantially free of magnesium oxide or magnesium hydroxychloride.
[0108] In Figure 1A, magnesium chloride and ammonium chloride solutions are fed into the evaporator and evaporated until the solid that precipitates in the evaporator has the approximate composition of N UCl-MgCh’b foO. This solid is then transferred to a flaker, and the flaked particles are introduced into a molten salt chamber at about 500 °C, and after an appropriate time, yield the magnesium chloride electrolyte. Here, various additives may be added to the molten salt chamber that typically are in magnesium chloride electrolytes, such as, but not limited to NaCl, KC1, CaCl2, NaF, KF, CaF2, BaF2, BaCh, or combinations thereof.
[0109] Figure IB shows another non-limiting variation of the process where a mixture of solid magnesium oxide and ammonium chloride is contacted with a molten salt mass to produce molten magnesium chloride electrolyte. This process has an advantage of not requiring the evaporation of the brine mixture as performed in the example illustrated in Figure 1 A.
[0110] Figure 1C illustrates a non-limiting example where ammonium chloride is used to mitigate the use of low purity magnesium chloride feedstock. In this case, magnesium chloride containing high levels of magnesium oxide, magnesium hydroxide, or magnesium hydroxychloride, levels which would normally preclude its use in the production of high purity magnesium chloride electrolytes, can be used due to the action of the ammonium chloride to convert magnesium oxide and magnesium hydroxychloride to anhydrous magnesium chloride.
[0111] Figure ID illustrates a non-limiting example, where the process illustrated in figure 1 A partially occurs in a molten salt chamber that is in thermal communication, fluid communication or both thermal and fluid communication with an electrolyzer, so the electrolyte in the electrolyzer may be replenished as the electrolyzer is operating.
[0112] In certain embodiments, the MgO plus MgOH2plus MgOHCl content of the magnesium chloride electrolyte melt is less than 2wt.%, 1.5wt.%, lwt.%, 0.5wt.%, 0.25wt.%, 0.125wt.%, 0. lwt.%, 0.0625wt%, 0.03125wt.%, 0.02wt.%, 0.01wt.%, or O. OOlwt %.
[0113] In certain embodiments, AlCh’xFkO, FeCk’xFBO, FeCls’xFBO, PrCls’xFFO, NdCh-xFFO, or a combination thereof may be substituted for MgCh, xFBO, MgO or MgOHCl in any composition or process described herein, where x equal from 0 to 7.
[0114] Thus, present technology also provides for a method obtained for producing, purifying, or replenishing a RECly-containing electrolyte obtained by first mixing certain ratios of RECly-xH2O feedstock and NH4CI. This material can either be introduced as a solid, comminuted, a double salt or be used directly as a loose mixture of powders. The RECly·xH2O where 2 < x < 7 and y is 2 or 3.
[0115] In some embodiments, RECI XH2O starting feedstock is selected from the group consisting of NdCl3·xH2O, PrCl3·xH2O, LaCl3·xH2O, DyCl3·xH2O, EuCl3·xH2O, PmCl3·xH2O, HoCl3·xH2O, or a combination thereof, where l<x<7.
[0116] In a preferred embodiment, RECly·xH2O is a neodymium or praseodymium chloride hydrate.
[0117] In a preferred embodiment, y is 3
[0118] In a preferred embodiment, x is 6 or 7.
[0119] In some embodiments, the RECLy- H2 is AlCh’xJfcO, FeCh'xFEO, or FeCh'xFEO where x is 1 to 6
[0120] In one embodiment, the molar ratio of RECly’xFEO to NH4CI in a mixture of RECly-xH2O and NH4C1 is 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, or 10:1.
[0121] In one embodiment, the molar ratio of RECly·xH2O to NH4CI is preferably about 1: 1, 1:2, 1:3, or 1:4.
[0122] In another embodiment, a NH4Cl·RECly·xH2O double salt or a mixture of NH4CI and REClx'yFFO is contacted with to the molten salt by dropping the double salt or mixture onto the surface of a molten salt composition.
[0123] In another embodiment, a NFECl-RECly·xH2O double salt or a mixture of NH4CI and RECly·xH2O is contacted with to the molten salt by dropping the double salt or mixture onto the surface of an agitated or stirred molten salt composition. The stirring or agitation may be performed by a mechanical stirrer or agitator, or the agitation may be performed by introducing an inert gas such as nitrogen or argon into the vessel containing the molten salt composition.
[0124] In another embodiment, a NEECl RECly·xH2O double salt or a mixture of NH4CI and RECly·xH2O is contacted with to the molten salt composition by feeding the double salt or mixture into a venturi system that is fed with the molten salt composition.
[0125] In another embodiment, a NFECl-RECly·xH2O double salt or a mixture of NH4CI and RECly·xH2O, rare earth oxide, rare earth hydroxide, or rare earth hydroxychloride is contacted with to the molten salt composition wherein the surface of the molten salt composition is not covered with an inert material such as alumina or inert gas.
[0126] In one embodiment, RE2O3 and NH4CI are fed simultaneously into a molten salt composition where in-situ generated HC1 converts the RE2O3 into REClyand H2O as shown ineqs. 11 & 12 with neodymium and praseodymium as examples. This embodiment does not require RECly·xH2O as a feedstock but RE2O3 instead.
[0127] In some embodiments, the rare earth ammonium carnallite salt may be prepared by mixing a solution of ammonium chloride with a solution of rare earth chloride and evaporating the resulting solution to obtain solid NH4Cl-RECly·xH2O double salt hydrate. Others way of preparing the double salt hydrate include mixing solid RECly·xH2O where y is 2 or 3 and x is 0 to 7 into an aqueous solution of NH4CI and evaporating the resulting solution to obtain solid NH4Cl-RECly-xH2O double salt hydrate. Others way of preparing the double salt hydrate include mixing solid NH4CI into an aqueous solution of RECly, where y is 2 or 3 and evaporating the resulting solution to obtain solid NH4Cl·RECly·xH2O double salt hydrate. Others way of preparing the double salt hydrate include mixing solid NH4CI into a molten salt composition comprising RECly, where y is 2 or 3, to obtain a molten NEUCl-RECly’xIEO double salt hydrate where y is 2 or 3 and x is 1, 2, 3, 4, 5, 6, or 7.
[0128] In some embodiments, a RECly depleted electrolyte, heated from the exothermic electrolysis reaction, is circulated into the dehydration zone. Thus, significantly reducing the amount of additional energy input required to perform the dehydration of the ReClyhydrate and the thermal decomposition of the NH4CI.
[0129] In the present case, it is found that there is a simple method obtained for producing, purifying, or replenishing a rare earth-containing electrolyte obtained by first mixing a common feedstock material, for example, 30 wt.% NdCh aqueous solution and mixing it with solid NH4CI or a solution of NH4CI. This material can then be evaporated into a concentrated mixture whereupon it can be solidified into a hydrated mixed salt, typically NEUCl-NdCh’bfEO, but the level of hydration may be varied under different evaporation conditions. This hydrated mixed salt will have the composition NEUCbNdCh’xJfcO, where x can range from 0-7. The present technology relates to the use of NH4Cl·NdCl3·xH2O to produce or replenish rare earth chloride electrolytes where x is greater than 0, greater than 1, greater than 2, greater than 3, greater than 4, greater than 5, or greater than 6, by contacting the NH4Cl·NdCl3·xH2O with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0130] The present technology also provides methods for the production, purification, or replenishment of a rare earth chloride electrolyte by contacting a mixture of NH4CI and NdCl3·6H2O with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0131] The present technology also provides methods for the production, purification, or replenishment of a rare earth chloride electrolyte by contacting a mixture of NH4CI and NdOH3with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0132] The present technology also provides methods for the production, purification, or replenishment of a rare earth chloride electrolyte by contacting a mixture of NH4CI and Nd(OH)2Cl, NdOCl, or NdOHCh with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0133] The present technology also provides methods for the production, purification, or replenishment of a rare earth chloride electrolyte by contacting a mixture of NH4CI and Nd2O3, with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl.
[0134] The present technology also provides methods for the production, purification, or replenishment of a rare earth chloride electrolyte by contacting a mixture of NH4CI and a composition comprising NdCl3·xH2O, Nd(OH)2Cl, NdOHCh, NdOCl, or Nd2O3, or a mixture thereof with a molten salt composition comprising at least one of KC1, CaCl2, or NaCl, where x is 1, 2, 3, 4, 5, 6, or 7.
[0135] In one embodiment, the present technology provides for methods of rare earth electrolyte production of replenishment wherein the contact of the mixture of NH4CI and a composition comprising NdCl3·xH2O, Nd(OH)2Cl. NdOHCh, NdOCl, or Nd2Os, or a mixture thereof with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer such as alumina or silica sand, or other solid powder having a melting point of greater than 500 °C.
[0136] In one embodiment, the present technology provides for methods of magnesium electrolyte production of replenishment wherein the contact of the NHjCl-NdCh’X^O, where x is 1, 2, 3, 4, 5, 6, or 7, with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer such as alumina or silica sand, or other solid powder having a melting point of greater than 500 °C.
[0137] In one embodiment, the present technology provides for methods of magnesium electrolyte production of replenishment wherein the contact of the mixture of NH4CI and a composition comprising NdCl3·xH2O, Nd(OH)2Cl, NdOHCh, NdOCl, or Nd2O3, or a mixture thereof with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer of an inert gas such as nitrogen or argon.
[0138] In one embodiment, the present technology provides for methods of rare earth electrolyte production of replenishment wherein the contact of the NH4Cl·NdCl3·xH2O, where x is 1, 2, 3, 4, 5, 6, or 7, with a molten salt composition occurs wherein the surface of the molten salt composition is not covered by a protective layer of an inert gas such as nitrogen or argon.
[0139] The present technology provides methods to produce a rare earth chloride electrolyte from an electrolyte pre-mix, which is a molten salt composition typically comprising KC1, CaCl2, or NaCl, or a mixture thereof and further comprising little or no NdCl3, Nd(OH)2Cl, NdOHCh, NdOCl or Nd2O3.
[0140] Typically, the electrolyte pre-mix comprises less than 0. lwt.%, less than 0.5wt.%, or less than lwt.%, total of NdCl3, Nd(OH)2Cl, NdOHCh, NdOCl, or Nd2O3, or a mixture thereof.
[0141] Typically, an electrolyte pre-mix is a molten salt composition comprising less than 1 wt.% rare earth oxides or salts and has not been previously subjected to electrolysis.
[0142] The present technology provides methods to replenish a spent rare earth chloride electrolyte from a spent rare earth chloride electrolyte wherein the spent rare earth electrolyte comprises less than 20wt.%, less than 19wt.%, less than 18wt.%, less than 17wt.%, less than 16wt.%, less than 15wt.%, less than 14wt.%, less than 13wt.%, less than 12wt.%, less than 11wt.%, less than 10wt.%, less than 9wt.%, less than 8wt.%, less than 7wt.%, less than 6wt.%, less than 5wt.%, less than 4wt.%, less than 3wt.%, less than 2wt.%, or less than lwt.% total NdCl3, Nd(OH)2Cl. NdOHCh, NdOCl, or Nd2O3.
[0143] In one embodiment, replenishment of the rare earth chloride electrolyte may be performed batch-wise, where upon the completion of an electrolysis operation, the now spent rare earth chloride electrolyte is replenished by the methods described herein.
[0144] In another embodiment, the replenishment may be performed continuously, to maintain a desired rare earth chloride content, without stopping the electrolysis operation.
[0145] Typically, the desired rare earth chloride content of the rare earth chloride electrolyte is between about 10wt.% and 25wt.%, 15wt.% and 25wt.%, 17wt.% and 23wt.% or 18wt.% and 22wt.%.
[0146] Preferably, the desired rare earth chloride content of the rare earth chloride electrolyte is between about 19wt.% and 21wt.%.
[0147] Typically, the electrolyte pre-mix will comprise less than 0.1wt.%, less than 0.5wt.%, less than lwt.%, less than 2.5wt.%, less than 5wt.%, less than 7.5wt.%, or less than 10wt.% total of NdCl3, Nd(OH)2Cl, NdOHCh, NdOCl or Nd2O3.
[0148] In some embodiments, any of NdCl3, Nd(OH)2Cl, NdOHCh, NdOCl, KC1, NaCl, BaCh or CaCl2in the molten salt composition may be replaced by their respective fluoride, bromide, or iodide analogue.
[0149] In some embodiments, the molten salt composition may comprise KC1, CaCl2, or NaCl, or a mixture thereof.
[0150] In some embodiments, the molten salt composition may further comprise a rare earth fluoride, MgF2, KF, NaF, CaF2, BaF2, BaCh, BaBr2, or a mixture thereof.
[0151] In some embodiments, any of MgCl2, MgOHCl, KC1, NaCl or CaCl2in the molten salt composition may be replaced by their respective fluoride, bromide, or iodide analogue.
[0152] In some embodiments, the molten salt composition may be rare earth chloride electrolyte, spent rare earth chloride electrolyte, or electrolyte pre-mix.
[0153] Typically, rare earth chloride electrolyte comprises more than 15% rare earth chloride and further comprises KC1, CaCl2, or NaCl, or a mixture thereof.
[0154] Typically, spent rare earth chloride electrolyte is rare earth chloride electrolyte which has been depleted in rare earth chloride through electrolysis. Spent rare earth chloride electrolyte typically comprises less than or equal to 15wt % rare earth chloride.
[0155] In one embodiment, the rare earth chloride electrolyte or the molten salt composition comprises KC1 at a concentration (wt.%) of 0-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25-30%, 30-35%, 35-40%, 40-45%, 45-50%, 50-55%, 55-60%, 60-65%, 65-70%, 70-75%, 75-80%, 80-85%, 85-90%, 90-95%, or 95-100%.
[0156] In another embodiment, the rare earth chloride electrolyte or the molten salt composition comprises NaCl at a concentration (wt.%) of 0-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25-30%, 30-35%, 35-40%, 40-45%, 45-50%, 50-55%, 55-60%, 60-65%, 65-70%, 70-75%, 75-80%, 80-85%, 85-90%, 90-95%, or 95-100%.
[0157] In another embodiment, the rare earth chloride electrolyte or the molten salt composition comprises CaCl2at a concentration (wt.%) of 0-5%, 5-10%, 10-15%, 15-20%, 20-25%, 25-30%, 30-35%, 35-40%, 40-45%, 45-50%, 50-55%, 55-60%, 60-65%, 65-70%, 70-75%, 75-80%, 80-85%, 85-90%, 90-95%, or 95-100%.
[0158] One advantage of the present technology is that it does not require extensive, or in some cases any drying of the NH4Cl·NdCl3·xH2O, NdCl3·xH2O or other rare earth ammonium carnallite or rare earth chloride intermediate feedstock, thus saving energy and additional unit operations during the rare earth chloride electrolyte production or enrichment.
[0159] In one embodiment, solid NH4Cl·RECl3·xH2O, where x is 1, 2, 3, 4, 5, 6, or 7 can be added into a chamber filled with a quantity of molten RECly-containing electrolyte. Provided that the temperature is > 450 °C and the electrolyte has sufficient superheat above its freezing point, then the NH4Cl·RECl3·xH2O, where x is 1, 2, 3, 4, 5, 6, or 7, will land on the electrolyte and begin to simultaneously dehydrate and thermally decompose the contained NH4CI. This causes the simultaneous off gassing of H2O, NH3, and HC1 molecules as per eqn. 5, using NdCh as an exemplar, but applicable to other rare earth chlorides, such as Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y or other metal AICI3, FeCE or FeCE carnallites as well. Surprisingly, it is found that the rapid evaporation of these molecules yield an oxide-free rare earth chloride-containing electrolyte. The high temperature of the molten salt chamber combined with the abundance of water vapor which can solubilize any condensed NH4CI, protects against NH4CI re-condensation in the equipment which would otherwise cause clogs in pipework and other operational problems.
[0160] Additionally, NH4Cl·RECly·xH2O salts can be added to a rare earth chloride containing electrolyte with oxide contamination and substantially reduce the undesired oxide impurities as shown in equations 9-12.
[0161] In one embodiment of this invention, NH4CI is added to a molten RECly-containing electrolyte with RE2O3 contamination to substantially or completely convert RE2O3 to RECI3 as shown in equations 11 and 12.
[0162] In some embodiments, the contamination may comprise RE2O3, RE(OH)3, RE(OH)2C1, REOHQ2, REOC1 or a combination thereof.
[0163] In another embodiment, RE2O3 and NH4CI are fed simultaneously into an electrolyte melt. NH4CI converts the RE2O3 into RECI3 and H2O as defined by equations 11 and 12. This embodiment does not require RECI3 as a feedstock but RE2O3 instead. This embodiment does not require NH4CI to be combined with RECl3·xH2O. Alternatively, the rare earth source may be RE(OH)3, RE(OH)2C1, or REOHCh. In some embodiments, the rare earth source may be a mixture comprising RE2O3, RE(OH)3, RE(OH)2C1, REOHCh or a combination thereof.
[0164] In one embodiment, the present technology provides for a method of producing an anhydrous rare earth chloride melt comprising the steps of: 1) providing a solution comprising from about 0.1 wt.% to about 30 wt.% aqueous rare earth chloride between about 95 C and 200°C; 2) mixing the said about 0.1wt.% to about 30wt.% aqueous rare earth chloride with about an equal amount of 0.1wt.% to about 30wt.% aqueous ammonium chloride between about 95°C and 200°C; 3) evaporating the mixture until the leftover solution achieves an approximate stoichiometry of NH4Cl·RECl3·xH2O, where x is 1, 2, 3, 4, 5, 6, or 7; 4) cooling the leftover solution until it solidifies into a solid; and, 5) contacting the solid with a rare earth chloride electrolyte comprising about 0-30 wt.% rare earth chloride; thus obtaining a magnesium chloride electrolyte substantially free from RE2O3, RE(OH)3, RE(OH)2C1, or REOHCh.
[0165] In one embodiment, the ratio of the volume of rare earth chloride solution to the volume of the ammonium chloride solution that is mixed prior to the evaporation is about 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1, 1:1.05, 1:1.1, 1:1.15, 1:1.2, 1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45, 1:1.5, 1:1.55, 1:1.60, 1:1.65, 1:1.7, 1:1.75, 1:1.85, 1:1.9, 1:1.95, 1:2, or a range consisting any two of these ratios as endpoints.
[0166] In one embodiment, the ratio of the molarity of rare earth chloride solution to the molarity of the ammonium chloride solution that is mixed prior to the evaporation is about 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85, 1:0.9, 1:0.95, 1:1, 1:1.05, 1:1.1, 1:1.15, 1:1.2, 1.25, 1:1.3, 1:1.35, 1:1.4, 1:1.45, 1:1.5, 1:1.55, 1:1.60, 1:1.65, 1:1.7, 1:1.75, 1:1.85, 1:1.9, 1:1.95, 1:2, or a range consisting any two of these ratios as endpoints.
[0167] In one embodiment, the ratio of the volume of rare earth chloride solution and the volume of the ammonium chloride solution that is mixed prior to the evaporation is about 1:0.1,1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.7, 1:1.8, 1:2, 1:2.5, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or a range consisting any two of these ratios as endpoints.
[0168] In one embodiment, the ratio of the molarity of rare earth chloride solution and molarity of the ammonium chloride solution that are mixed prior to the evaporation is about 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.7, 1:1.8, 1:2, 1:2.5, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or a range consisting any two of these ratios as endpoints.
[0169] In one embodiment, the concentration of either the rare earth chloride solution or the ammonium chloride solution may be 5 wt.%, 10 wt.%, 15 wt.%, 20 wt.%, 25 wt.%, 30 wt.%, 35 wt.%, 40 wt.%, 45 wt.%, 50 wt.%, 55 wt.%, 60 wt.%, 65 wt.%, 75 wt.%, 80 wt.%, 85 wt.%, 90 wt.%, 95 wt %, or a range consisting any two of these ratios as endpoints.
[0170] In one embodiment, the molar ratio of RECh to NH4CI of the evaporated solid is about 1:0.1, 1:0.2, 1:0.3, 1:0.4, 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.3, 1:1.5, 1:1.7, 1:1.8, 1:2, 1:2.5, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, or a range consisting any two of these ratios as endpoints.
[0171] In a preferred embodiment, the molar ratio of RECh to NH4CI of the evaporated solid is about 0.1-0.5: 1, 0.5-0.75, 0.75-1:1, 1:1, 1:1-1.25, 1:1.25-1.5, 1:1.5-1.75, 1:1.75-2, 1:2-3, 1:3-4, or 1:4-5.
[0172] In one embodiment, the evaporated solid comprises about 3.05 to 3.5 waters of hydration per atom of rare earth element. In one embodiment, the evaporated solid comprises about 3.5 to 4 waters of hydration per atom of rare earth element. In one embodiment, the evaporated solid comprises about 4 to 5 waters of hydration per atom of rare earth element. In one embodiment, the evaporated solid comprises about 5 to 6 waters of hydration per atom of rare earth element. In one embodiment, the evaporated solid comprises about 6 to 7 waters of hydration per atom of rare earth element. In one embodiment, the evaporated solid comprises about 3.05 to 6 waters of hydration per atom of rare earth element. The mixing of the ammonium chloride with the rare earth chloride may be accomplished in several ways. Non-limiting examples are described below.
[0173] In one embodiment, the ammonium chloride and rare earth chloride may be introduced as their respective aqueous solutions.1
[0174] In another embodiment, solid ammonium chloride may be introduced into an aqueous solution of rare earth chloride.
[0175] In still another embodiment, solid rare earth chloride hydrate may be introduced into an aqueous solution of ammonium chloride.
[0176] In still another embodiment, a mixture of solid ammonium chloride and solid rare earth chloride hydrate may be introduced into molten rare earth chloride hydrate or molten rare earth chloride electrolyte.
[0177] In still another embodiment, solid ammonium chloride may be introduced into molten rare earth chloride hydrate or molten rare earth chloride electrolyte.
[0178] In one embodiment, crystallization of the solution which takes place in an evaporator into a hydrated NHCbRECh’xHzO salt, where x is 1, 2, 3, 4, 5, 6, or 7 after NH4CI addition is performed at between about -60 °C and -20 °C, -20 °C and 20 °C, 20 °C and 60 °C, 60 °C and 100 °C, 100 °C and 140 °C, 140 °C and 180 °C, 180 °C and 220 °C, 220 °C and 260 °C, 260 °C and 300 °C, or 300 °C and 340 °C.
[0179] In one embodiment, the dehydration of the hydrated NHrCl-RECh’xJfcO salt, where x is 1, 2, 3, 4, 5, 6, or 7 in the magnesium chloride melt is performed at between about 360 °C and 400 °C, 400 °C and 420 °C, 420 °C and 460 °C, 460 °C and 500 °C, 500 °C and 540 °C, 540 °C and 580 °C, 580 °C and 620 °C, 620 °C and 660 °C, 660 °C and 700 °C, or 700 °C and 740 °C.
[0180] In one embodiment, the concentration of rare earth chloride in the molten salt may be 0 wt.%, 5 wt.%, 10 wt.%, 15 wt.%, 20 wt.%, 25 wt.%, 30 wt.%, 35 wt.%, 40 wt.%, 45 wt.%, 50 wt.%, 55 wt.%, 60 wt.%, 65 wt.%, 75 wt.%, or a range consisting any two of these ratios as endpoints
[0181] In one embodiment, the hydrated NH4Cl·RECl3·xH2O salt, where x is 1, 2, 3, 4, 5, 6, or 7 may be introduced into a molten electrolyte containing equal parts RECI3, NaCl, CaCl2, and KC1.
[0182] In one embodiment, the hydrated NH4Cl·RECl3·xH2O salt where x is 1, 2, 3, 4, 5, 6, or 7, may be introduced into the molten rare earth chloride electrolyte by dropping it on top of a container holding the molten rare earth chloride electrolyte. In some embodiments, hydrated NH4Cl·RECl3·xH2O salt, where x is 1, 2, 3, 4, 5, 6, or 7, may be added directly to the moltenelectrolyte in a rare earth electrolysis cell or a vessel that is in fluid communication with an electrolyzer. In some embodiments, agitation via inert gas bubbling or mechanical agitation may be used to enhance the reaction of the evaporated solid with the molten rare earth chloride electrolyte. In some embodiments the molten salt bed is fully exposed to atmosphere where air is allowed to flow over the top of the molten rare earth chloride electrolyte.
[0183] In another embodiment, a venturi system may be used to introduce the evaporated solid into a stream of molten rare earth chloride electrolyte.
[0184] Figures 1A-D illustrate some of the non-limiting basic modes of operation of the system and method of production of rare earth chloride electrolyte that is substantially free of rare earth oxide, rare earth hydroxide, or rare earth hydroxychloride. In Figure 1 A, rare earth metal chloride and ammonium chloride solutions are fed into the evaporator, and evaporated until the solid that precipitates in the evaporator has the approximate composition of NH4Cl·RECl3·xH2O, where x is 6 or 7. This solid is then transferred to a flaker, and the flaked particles are introduced into a molten salt chamber at about 500°C, and after an appropriate time, yield the rare earth chloride electrolyte. Here, various additives may be added to the molten salt chamber that typically are in rare earth chloride electrolytes, such as, but not limited to NaCl, KC1, CaCl2, NaF, KF, CaF2, BaF2BaCh, or combinations thereof.
[0185] Figure IB shows another non-limiting variation of the process where a mixture of solid rare earth metal oxide and ammonium chloride is contacted with a molten salt mass to produce molten rare earth chloride electrolyte. This process has an advantage of not requiring the evaporation of the brine mixture as performed in the example illustrated in Figure 1A.
[0186] Figure 1C illustrates a non-limiting example where ammonium chloride is used to mitigate the use of low purity rare earth metal chloride feedstock. In this case, rear earth metal chloride containing high levels of rare earth oxide, rare earth hydroxide, or rare earth hydroxychloride, levels which would normally preclude its use in the production of high purity rare earth chloride electrolytes, can be used due to the action of the ammonium chloride to convert rare earth oxide, rare earth hydroxide and rare earth hydroxychloride to anhydrous rare earth chloride.
[0187] Figure ID illustrates a non-limiting example, where the process illustrated in figure 1A partially occurs in a molten salt chamber that is in thermal communication, fluid communicationor both thermal and fluid communication with an electrolyzer, so the electrolyte in the electrolyzer may be replenished as the electrolyzer is operating.
[0188] In certain embodiments, the rare earth oxide, rare earth hydroxide, rare earth oxychloride and rare earth hydroxychloride content of the rare earth chloride electrolyte melt is less than 2wt.%, 1.5wt.%, lwt.%, 0.5wt.%, 0.25wt.%, 0.125wt.%, 0.1wt.%, 0.0625wt.%, 0.03125wt.%, 0.02wt.%, 0.01wt.%, or0.001wt.%.
[0189] In the some of the foregoing embodiments, neodymium is used as a specific exemplar for “RE”, but it may be replaced by other rare earth element chlorides, hydroxides or hydroxychlorides. Non limiting examples of rare earth elements include lanthanum (La), cerium (Ce), praseodymium (Pr), Promethium (Pm), samarium (Sm), Europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), Thulium (Tm), Ytterbium (Yb), lutetium (Lu), scandium (Sc), and yttrium (Y). It is understood that in same cases, under certain conditions, the chlorides of these elements may for hydrated carnallites with waters of hydration exceeding 7, and in those cases, the embodiments are intended to include those cases as well.
[0190] In some of the foregoing embodiments, although not considered rare earth elements, aluminium (Al) and iron (Fe) chlorides, oxides, and hydroxychlorides may be feedstocks for the preparation or replenishment of their respective chloride electrolytes. For iron, both the +2 or +3 oxidation state salts, oxides, or hydroxychlorides may be used. So, for example, if the +2 oxidation state iron is used, the chloride feedstock will be FeCh instead of NdCh or Fe(OH)2instead of NdOH3. Likewise, FeO would be used instead of Nd2O3. Analogously, the same adjustments would be made for the hydroxychloride species.
[0191] A person skilled in the art appreciates that these non-limiting examples are but just several ways of implementing and integrating the magnesium chloride, aluminum chloride, iron chloride, or rare earth chloride electrolyte production, purification, or replenishment operations disclosed herein.
[0192] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting solid NH4Cl·MgCl2·xH2O with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0193] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting solid NH4Cl·MgCl2·xH2Owith a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl, wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0194] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting solid NH4Cl·MgCl2·xH2O with a molten salt initially comprising greater than 15 wt.% MgCh and least one of KC1, CaCl2, or NaCl.
[0195] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting solid NHrCbMgCh’xHzO with a molten salt initially comprising less than or equal 15 wt.% MgCh and least one of KC1, CaCl2, or NaCl.
[0196] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting solid NH4Cl·MgCl2·xH2O with a molten salt initially comprising at least 0.3 wt.% total of MgO, Mg(OH)2, MgOHCl, or a combination thereof.
[0197] In one embodiment, the molten salt is contained in an electrolyzer. In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0198] In one embodiment, the electrolyzer is in an operating condition. In one embodiment, the electrolyzer is in a standby condition.
[0199] In one embodiment, the NH4Cl·MgCl2·xH2O has been produced by evaporating an aqueous solution comprising MgCl2and NH4CI and x is greater than 3.
[0200] In one embodiment, the NH4Cl-MgCl2-xH2O has been produced by melting a mixture comprising MgCl2xH2O and NH4CI and x is greater than 3.
[0201] In one embodiment, the contact of the NH4Cl-MgCl2-xH2O and molten salt is made in the dehydration zone of the electrolyzer.
[0202] In one embodiment, the replenished or produced magnesium chloride electrolyte melt comprises less than 0.3 wt.% total of MgO, Mg(OH)2. MgOHCl, or a combination thereof.
[0203] In one embodiment, the molten salt is heated via an AC current.
[0204] In some embodiments, the x in NEUCl-MgCh’xEhO is greater than 3.
[0205] In some embodiments, the x in NH4Cl·MgCl2·xH2O is greater or equal to 4.
[0206] In some embodiments, the x in NH4Cl·MgCl2·xH2O is greater or equal to 5.
[0207] In some embodiments, the x in NH4Cl·MgCl2·xH2O is greater or equal to 6.
[0208] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and MgCl2·xH2O with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0209] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and MgCh’xH2O with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl, wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0210] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and MgCl2·xH2O with a molten salt initially comprising greater than 15 wt.% MgCh and at least one of KC1, CaCl2, or NaCl.
[0211] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and MgCh’xIHhO with a molten salt initially comprising less than or equal 15 wt.% MgCh and at least one of KC1, CaCl2, or NaCl.
[0212] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and MgCl2·xH2O with a molten salt initially comprising at least 0.3 wt.% total of MgO, Mg(OH)2. MgOHCl, or a combination thereof, and at least one of KC1, CaCl2, or NaCl.
[0213] In one embodiment, the molten salt is contained in an electrolyzer.
[0214] In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0215] In one embodiment, the electrolyzer is in an operating condition.
[0216] In one embodiment, the electrolyzer is in a standby condition.
[0217] In one embodiment, the contact of the NH4Cl-and MgCh’xHjO and molten salt is made in the dehydration zone of the electrolyzer.
[0218] In one embodiment, the replenished or produced magnesium chloride electrolyte melt comprises less than 0.3 wt.% total of MgO, Mg(OH)2. MgOHCl, or a combination thereof.
[0219] In one embodiment, the molten salt is heated via an AC current.
[0220] In some embodiments, the x in-MgCh’xf O is greater than 3.
[0221] In some embodiments, the x in MgCh’xHiO is greater or equal to 4.
[0222] In some embodiments, the x in MgCh’xH^O is greater or equal to 5.
[0223] In some embodiments, the x in MgCl2·xH2O is greater or equal to 6.
[0224] In some embodiments, the NH4CI and MgCl2·xH2O are in a less than 1: 1 molar ratio.
[0225] In some embodiments, the NH4CI and MgCl2·xH2O are in an about 1: 1 molar ratio.
[0226] In some embodiments, the NH4CI and MgCl2·xH2OfcO are in a greater than 1: 1 molar ratio.
[0227] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and a composition comprising MgO, Mg(OH)2, MgOHCl, or a combination thereof, with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0228] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and a composition comprising at least one of MgO, Mg(OH)2, MgOHCl, with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl, wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0229] In one embodiment, the molten salt initially comprises greater than or equal 15 wt.% MgCh and further comprises at least one of KC1, CaCl2, NaCl.
[0230] In one embodiment, the molten salt initially comprises less than 15 wt.% MgCh and further comprises at least one of KC1, CaCl2, NaCl.
[0231] In one embodiment, the molten salt initially comprises at least 0.3 wt.% total of MgO, Mg(OH)2, MgOHCl, or a combination thereof and further comprises at least one of MgCh, KC1, CaCl2, NaCl.
[0232] In one embodiment, the molten salt is contained in an electrolyzer.
[0233] In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0234] In one embodiment, the electrolyzer is in an operating condition.
[0235] In one embodiment, the electrolyzer is in a standby condition.
[0236] In one embodiment, the contact of the comminuted mixture comprising solid NH4CI and a composition comprising at least one of MgO, Mg(OH)2, MgOHCl and molten salt is made in the dehydration zone of the electrolyzer.
[0237] In one embodiment, the replenished or produced magnesium chloride electrolyte melt comprises less than 0.3 wt.% total of MgO, MgOH2MgOHCl, or a combination thereof.
[0238] In some embodiments, the NH4CI and MgO, Mg(OH)2 or MgOHCl are in a less than 1: 1 molar ratio with respect to ammonium ion and total magnesium.
[0239] In some embodiments, the NH4CI and MgO, Mg(OH)2, or MgOHCl are in a greater than 1: 1 molar ratio with respect to ammonium ion and total magnesium.
[0240] . In some embodiments, the NH4CI and MgO, Mg(OH)2 or MgOHCl are in an about 1: 1 molar ratio with respect to ammonium ion and total magnesium.
[0241] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and a composition comprising MgO with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0242] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and a composition comprising Mg(0H)2, with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, orNaCl.
[0243] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and a composition comprising MgOHCl with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0244] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid Nt CbMgCh’xlHbO and a composition comprising MgO, Mg(OH)2, MgOHCl, or a combination thereof, with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0245] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4Cl·MgCl2·xH2O and a composition comprising at least one of MgO, Mg(OH)2, MgOHCl, or a combination thereof, with a molten salt initially comprising at least one of MgCh, KC1, CaCk, or NaCl, wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0246] In one embodiment, the molten salt initially comprises greater than or equal 15 wt.% MgCh and further comprises at least one of KC1, CaCl2, NaCl.
[0247] In one embodiment, the molten salt initially comprises less than 15 wt.% MgCh and further comprises at least one of KC1, CaCl2, NaCl.
[0248] In one embodiment, the molten salt initially comprises at least 0.3 wt.% total of MgO, Mg(OH)2, MgOHCl, or a combination thereof and further comprises at least one of MgCh, KC1, CaCl2, NaCl.
[0249] In one embodiment, the molten salt is contained in an electrolyzer.
[0250] In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0251] In one embodiment, the electrolyzer is in an operating condition.
[0252] In one embodiment, the electrolyzer is in a standby condition.
[0253] In one embodiment, the contact of the composition comprising Nt Cl-MgCh’xHjO and at the at least one of MgO, Mg(OH)2 or MgOHCl, and molten salt is made in the dehydration zone of the electrolyzer.
[0254] In one embodiment, the replenished, purified, or produced magnesium chloride electrolyte melt comprises less than 0.3 wt.%, 0.1wt.%, 0.05wt.% or 0.01wt.% total of MgO, Mg(OH)2 MgOHCl, or a combination thereof.
[0255] In some embodiments, the NH4Cl·MgCl2·xH2O and the composition comprising MgO, Mg(OH)2 or MgOHCl are in a less than 1:1 molar ratio with respect to ammonium ion and total magnesium of the MgO, Mg(OH) or MgOHCl.
[0256] In some embodiments, the NH4Cl·MgCl2·xH2O and the composition comprising MgO, Mg(OH)2, or MgOHCl are in a greater than 1: 1 molar ratio with respect to ammonium ion and total magnesium of the MgO, Mg(OH)2 or MgOHCl.
[0257] In some embodiments, the NH4Cl·MgCl2·xH2O and the composition comprising MgO, Mg(OH)2 or MgOHCl are in an about 1: 1 molar ratio with respect to ammonium ion and total magnesium of the MgO, Mg(OH)2 or MgOHCl.
[0258] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid the NH4Cl·MgCl2·xH2O and a composition comprising MgO with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0259] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid the NELjCbMgCh’xHzO and a composition comprising Mg(OH)2, with a molten salt initially comprising at least one of MgCh, KC1, CaCl2, or NaCl.
[0260] In one embodiment, the present technology provides for a method of replenishing or producing a magnesium chloride electrolyte melt comprising contacting a comminuted mixture comprising solid the NELCl-MgCl2·xH2O and a composition comprising MgOHCl with a molten salt initially comprising at least one of MgCl2. KC1, CaCl2, or NaCl.
[0261] In one embodiment, the molten salt is heated via an AC current.
[0262] In some embodiments, the x in NH4Cl·MgCl2·xH2O is greater than 3.
[0263] In some embodiments, the x in NEUCl-MgCh’xHzO is greater or equal to 4.
[0264] In some embodiments, the x in NH4Cl·MgCl2-xHzO is greater or equal to 5.
[0265] In some embodiments, the x in NELCl-MgCh’xHzO is greater or equal to 6.
[0266] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting solid NH4Cl·RECl3·xH2O, where x is 1, 2, 3, 4, 5, 6, or 7 and RE is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y, with a molten salt initially comprising at least one of RECh, KC1, CaCl2, or NaCl.
[0267] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting solid NH4Cl·RECl3·xH2O, where x is 1, 2, 3, 4, 5, 6, or 7 and RE is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y, with a molten salt initially comprising at least one of RECI3, KC1, CaCl2, or NaCl, and wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0268] In one embodiment, the molten salt initially comprises greater than or equal to 15 wt.% RECl3and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0269] In one embodiment, the molten salt initially comprises less than 15 wt.% RECI3 and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0270] In one embodiment, the molten salt initially comprises at least 0.3 wt.% total of RE2O3 RE(OH)3. RE(OH)2C1, REOC1, REOHQ2, or a combination thereof.
[0271] In one embodiment, the molten salt is contained in an electrolyzer.
[0272] In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0273] In one embodiment, the electrolyzer is in an operating condition.
[0274] In one embodiment, the electrolyzer is in a standby condition.
[0275] In one embodiment, the molten salt is heated via an AC current.
[0276] In one embodiment, the NH4Cl·RECl3·xH2O has been produced by evaporating an aqueous solution comprising RECh and NH4CI.
[0277] In one embodiment, the contact of the NH4Cl·RECl3·xH2O and molten salt is made in the dehydration zone of the electrolyzer.
[0278] In one embodiment, the replenished or produced rare earth chloride electrolyte melt comprises less than 0.3 wt.%, 0.2wt.%, 0.1wt.%, 0.05wt.% or 0.01wt.% total of RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCI2, or a combination thereof.
[0279] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and RECl3·xH2O where x is 1, 2, 3, 4, 5, 6, or 7 and RE is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y, with a molten salt initially comprising at least one of RECh, KC1, CaCl2, or NaCl.
[0280] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and RECh’x^O where x is 1, 2, 3, 4, 5, 6, or 7 and RE is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y, with a molten salt initially comprising at least one of RECh, KC1, CaCl2, or NaCl, and wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0281] In one embodiment, the molten salt initially comprises greater than or equal to 15 wt.% RECl3and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0282] In one embodiment, the molten salt initially comprises less than 15 wt.% RECh and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0283] In one embodiment, the molten salt initially comprises at least 0.3 wt.%, 0.5wt.%, Iwt.%, 2wt.%, 3 wt.%, 4wt.% or 5wt% total of RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof.
[0284] In one embodiment, the molten salt is contained in an electrolyzer.
[0285] In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0286] In one embodiment, the electrolyzer is in an operating condition.
[0287] In one embodiment, the electrolyzer is in a standby condition.
[0288] In one embodiment, the molten salt is heated via an AC current.
[0289] In one embodiment, the contact of the NH4Cl· and RECl3·xH2O and molten salt is made in the dehydration zone of the electrolyzer.
[0290] In one embodiment, the replenished or produced rare earth chloride electrolyte melt comprises less than 0.3 wt.%, 0.2wt.%, 0.1wt.%, 0.05wt.% or 0.01wt.% total of RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof.
[0291] In one embodiment, the x in RECl3·xH2O is 6 or 7.
[0292] In one embodiment, the solid NH4CI and RECl3·xH2O are in about a 1: 1 molar ratio.
[0293] In one embodiment, the solid NH4CI and RECl3·xH2O are in a less than 1: 1 molar ratio.
[0294] In one embodiment, the solid NH4CI and RECl3·xH2O are in a greater than 1:1 molar ratio.
[0295] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof, with a molten salt initially comprising at least one of RECI3, KC1, CaCl2, or NaCl.
[0296] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NH4CI and RE2O3 RE(OH)3. RE(OH)2C1, REOHCh, or a combination thereof,with a molten salt initially comprising at least one of RECI3, KC1, CaCl2, or NaCl, and wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0297] In one embodiment, the molten salt initially comprises greater than or equal to 15 wt.% RECl3and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0298] In one embodiment, the molten salt initially comprises less than 15 wt.% RECI3 and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0299] In one embodiment, the molten salt initially comprises at least 0.3 wt.% total of RE2O3 RE(OH)3. RE(OH)2C1, REOHCI2, or a combination thereof.
[0300] In one embodiment, the molten salt is contained in an electrolyzer.
[0301] In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0302] In one embodiment, the electrolyzer is in an operating condition.
[0303] In one embodiment, the electrolyzer is in a standby condition.
[0304] In one embodiment, the molten salt is heated via an AC current.
[0305] In one embodiment, the contact of the RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCI2, or a combination thereof and molten salt is made in the dehydration zone of the electrolyzer.
[0306] In one embodiment, the replenished or produced rare earth chloride electrolyte melt comprises less than 0.3 wt.% total of RE2O3 RE(OH)3. RE(OH)2C1, REOHCh, or a combination thereof.
[0307] In some embodiments, the NH4CI and RE2O3 RE(OH)3, REOC1, RE(OH)2C1, or REOHCh, are in a less than 1: 1 molar ratio with respect to ammonium ion and total RE.
[0308] In some embodiments, the NH4CI and RE2O3 RE(OH)3, RE(OH)2C1, or REOHCh, are in a greater than 1: 1 molar ratio with respect to ammonium ion and total RE.
[0309] In some embodiments, the NH4CI and RE2O3 RE(OH)3, REOC1, RE(OH)2C1, or REOHCh, are in an about 1: 1 molar ratio with respect to ammonium ion and total RE.
[0310] In a preferred embodiment, the RE is Nd.
[0311] In a preferred embodiment, the RE is Pr.
[0312] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NEECl-RECl3·xH2O and a composition comprising RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof, where x is 1, 2, 3, 4, 5, 6, or 7 and RE is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y, with a molten salt initially comprising at least one of RECI3, KC1, CaCl2, or NaCl.
[0313] In one embodiment, the present technology provides for a method of replenishing or producing a rare earth chloride electrolyte melt comprising contacting a comminuted mixture comprising solid NELClvRECh’xHzO and a composition comprising RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof, where x is 1, 2, 3, 4, 5, 6, or 7 and RE is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y, with a molten salt initially comprising at least one of RECh, KC1, CaCl2, or NaCl, wherein the molten salt is at a temperature of 500 °C to 700 °C.
[0314] In one embodiment, the molten salt initially comprises greater than or equal to 15 wt.% RECl3and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0315] In one embodiment, the molten salt initially comprises less than 15 wt.% RECh and further comprises KC1, CaCl2, NaCl or a combination thereof.
[0316] In one embodiment, the molten salt initially comprises at least 0.3 wt.% total of RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof.
[0317] In one embodiment, the molten salt is contained in an electrolyzer.
[0318] In one embodiment, the molten salt is contained in an electrolyzer comprising an electrolysis zone and a dehydration zone.
[0319] In one embodiment, the electrolyzer is in an operating condition.
[0320] In one embodiment, the electrolyzer is in a standby condition.
[0321] In one embodiment, the molten salt is heated via an AC current.
[0322] In one embodiment, the NH4Cl·RECl3·xH2O has been produced by evaporating an aqueous solution comprising RECI3 and NH4CI.
[0323] In one embodiment, the NH4Cl·RECl3·xH2O has been produced by melting a mixture of RECl3·xH2O and NH4CI.
[0324] In one embodiment, the contact of the NEECl-RECl3·xH2O and a composition comprising RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCI2, or a combination thereof, and molten salt is made in the dehydration zone of the electrolyzer.
[0325] In one embodiment, the replenished or produced rare earth chloride electrolyte melt comprises less than 0.3 wt.% total of RE2O3 RE(OH)3. RE(OH)2C1, REOHCk, or a combination thereof.
[0326] In one embodiment, the NH4Cl·RECl3·xH2O and a composition comprising RE2O3RE(OH)3, REOCl, RE(OH)2Cl, REOHCl2, or a combination thereof, are in a greater than 1: 1 molar ratio with respect to ammonium ion and the total RE of the RE2O3 RE(OH)3. RE(OH)2C1, REOHCh, or a combination thereof.
[0327] In one embodiment, the NH4Cl·RECl3·xH2O and a composition comprising RE2O3RE(OH)3, RE(OH)2Cl, REOHCl2, or a combination thereof, are in an about 1:1 molar ratio with respect to ammonium ion and the total RE of the RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof.
[0328] In one embodiment, the NH4Cl·RECl3·xH2O and a composition comprising RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof, are in less than 1: 1 molar ratio with respect to ammonium ion and the total RE of the RE2O3 RE(OH)3, REOC1, RE(OH)2C1, REOHCh, or a combination thereof.
[0329] In one embodiment, the present technology provides for a method of producing, replenishing, or purifying a metal chloride electrolyte melt where in the produced, replenished, or purified metal halide electrolyte melt is substantially free from metal oxide, metal hydroxychloride, metal oxychloride and metal hydroxide, the method comprising: contacting a metal component with a molten salt composition comprising at least one of, the metal halide, NaCl, NaF, KC1, KF, CaF2, BaF2, BaCh, or CaCl2; wherein the metal of the metalcomponent is selected from the group consisting of Mg, Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc and Y and wherein the metal component is an ammonium carnallite hydrate of the formula NH4Cl-RECly·xH2O, a mixture of NH4CI and RECly, wherein y is 2 or 3, a mixture of NH4Cl-RECly-xH2O and REO, RE2O3, RE(OH)2, RE(OH)3, REOC1, RE0HC1, RE(OH)2C1, REOHCh, or a mixture NH4C1 and REO, RE2O3, RE(OH)2, RE(OH)3, REOC1, RE0HC1, RE(OH)2C1, REOHCh, or a mixture thereof, and wherein y is 2 and x is 6 when RE is Mg, and wherein y is 3 and x is 1 to 7 when RE is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y, thereby obtaining a produced, replenished, or purified metal halide electrolyte melt
[0330] The present technology also provides for the use of, not only carnallite hydrates alone, or with metal oxides or hydroxides, but also mixtures of metal chloride hydrates with ammonium chloride, and mixtures of metal oxides, hydroxychlorides, or hydroxides with metal carnallite hydrates or ammonium chloride to produce, purify, or replenish molten electrolyte compositions for the production of the corresponding metals via electrolysis.
[0331] The present technology provides for the production, purification, or replenishment of magnesium, aluminum and rare earth metal electrolyte compositions intended for electrolytic production of the corresponding metals.
[0332] In the case of the production of a metal electrolyte composition, a metal carnallite or its hydrate, a mixture of a metal carnallite, or its hydrate and a metal oxide, hydroxide, or hydroxychloride, or a mixture of a metal oxide, hydroxide, or hydroxy chloride and ammonium chloride is contacted with a molten salt composition which is substantially free from the salts, oxides, hydroxides or hydroxychlorides of the corresponding metal.
[0333] In the case of the purification of a metal electrolyte composition, the molten salt composition, as in the production process has initially a level of the corresponding metal chloride that is sufficient for the electrolytic production of the corresponding method, but also contains levels of the corresponding metal oxides, hydroxides, or hydroxychlorides that interfere with the optimal electrolytic metal production process.
[0334] It is understood that an electrolyte may need to be replenished and purified at the same time.
[0335] In the case of the replenishment of a metal electrolyte composition, the molten salt composition initially has the corresponding metal chloride concentration below the optimal level for the electrolytic production of the corresponding metal. Typically, for magnesium, optimum concentrations for magnesium chloride are between about 35wt.% and 60wt.%.
[0336] It is recognized that typical impurities in electrolytes that need to be purified or replenished may be metal oxides, hydroxides, hydroxychlorides, and combinations thereof. However, depending on the particular electrolytic process, metal, electrolyte composition, and temperature, the molten salt composition may contain some, but not all of the metal oxide, hydroxide, or hydroxychloride. In some embodiments, where reference to a comminuted mixture is referred to, the comminuted mixture may be replaced by a mixture formed from the powdered or granulated mixture components that, for example, may be simply mixed together my stirring, agitating, using a drum mixer, or other commonly known means. In some embodiments, the mixture may be further homogenized by using a ball mill or other such device to form a comminuted mixture.
[0337] While the invention has been described in connection with specific embodiments thereof, it will be understood that it is capable of further modifications and this application is intended to cover any variations, uses, or adaptations of the invention, including such departures from the present disclosure as come within known or customary practice within the art to which the invention pertains and as may be applied to the essential features hereinbefore set forth, and as follows in the scope of the appended claims.
[0338] It is appreciated that certain features of the invention, which are, for clarity, described in the context of separate embodiments, may also be provided in combination in a single embodiment. Conversely, various features of the invention, which are, for brevity, described in the context of a single embodiment, may also be provided separately or in any suitable subcombination. All combinations of the embodiments pertaining to the invention are specifically embraced by the present invention and are disclosed herein just as if each and every combination was individually and explicitly disclosed. In addition, all sub-combinations of the various embodiments and elements thereof are also specifically embraced by the present invention and are disclosed herein just as if each and every such sub-combination was individually and explicitly disclosed herein.
[0339] Tables 2 and 3 show increase in metal chloride content and concomitant decrease in oxide content of various experiments. For example, the counter-example 21 shows that without the use of ammonium chloride, or the rare earth ammonium carnallite, the level of Pr2O3in the resulting melt is above the acceptable limit for electrolysis, and the metal chloride is present at only 4wt.% in the melt as opposed to the expected 5wt.% if the reaction had been performed according to the present technology.Table 2. Metal chloride and oxide contentsTable 3. Metal chloride and oxide contentsEXAMPLES:
[0340] The examples below are given so as to illustrate the practice of various embodiments of the present disclosure. They are not intended to limit or define the entire scope of this disclosure. It should be appreciated that the disclosure is not limited to the particular embodiments described and illustrated herein but includes all modifications and variations falling within the scope of the disclosure as defined in the appended embodiments.Example 1: Electrolyte Production / Replenishment in a chamber
[0341] 30wt% NH4CI solution is combined with 30wt.% MgCh solution in a mixing vessel. The mixed solution is sent to evaporators and heated until the solution stoichiometry is approximately NH4Cl·MgCl2·6H2O. This solution is cooled on a drum flaker device to form solid pieces of salt. These solid pieces are conveyed to a feedstock hopper above a molten salt chamber ccontaining a magnesium chloride electrolyte with 10wt.% MgCh, heated by an AC current applied by via electrodes. The solid pieces are dispensed into the chamber, which due to the temperature and contact with the molten salt undergo simultaneous dehydration and decomposition whereby the contained NH4CI is broken down into NH3 and HC1 gas. The MgCh in the feedstock melts and is incorporated into the electrolyte. Minimal hydrolysis is observed in this ammonium carnallite case relative to what would be observed with the addition of MgCl2·6H2O to the melt. At the end of the addition, an electrolyte is yielded which is enriched in MgCh, and substantially free of oxide impurities ready for feeding to electrolyzers.Example 2 Reduction ofMgO and replenishment of MgCh in spent electrolyte
[0342] 30wt.% NH4CI solution is combined with 30wt.% MgCh solution in a mixing vessel. The mixed solution is sent to evaporators and heated until the solution stoichiometry was approximately NH4Cl·MgCl2·6H2O. This solution is cooled on a drum flaker device to form solid pieces of salt. These solid pieces are conveyed to a reagent hopper above a molten salt chamber, containing a magnesium chloride electrolyte, heated by an AC current applied via electrodes. Where the magnesium chloride electrolyte is “spent” electrolyte that is relatively depleted in MgCh content (e.g., 10wt.% MgCh) that has been returned from a magnesium molten salt electrolyzer. Where the spent electrolyte is “crude” in that it is contaminated with some level of oxide species (e.g., lwt.% MgO or greater). Where the molten salt chamber now takes on the role of a “chlorinating device”. The solid pieces of NThCl-MgCh’bT O are dispensed into the chamber, which due to the temperature and contact with the molten salt undergo simultaneous dehydrationand decomposition whereby the contained NH4CI is broken down into NH3 and HC1 gas. Where the action of the NEUCl-MgCh’bEhO addition into the crude electrolyte is to chlorinate it and purge it of oxide impurities. Where the molar ratio of added NH4Cl-MgCh‘6H2O to the MgO in the crude electrolyte is about 1: 1. At the end of the addition, an electrolyte is yielded which has been purged of MgO impurities to <0. lwt.% MgO.Example 3: Comminuted mixture ofNERCl and MgCh
[0343] Solid NH4CI and-MgCh’bEhO are mixed into a hopper at a 1:1 NH4Cl:MgCl2ratio. The mixed solids are conveyed to a reagent hopper above a molten salt chamber ccontaining a magnesium chloride electrolyte, heated by an AC current applied via electrodes. Where the magnesium chloride electrolyte is “spent” electrolyte that is relatively depleted in MgCh content (e.g., 10wt.% MgCh) that has been returned from a magnesium molten salt electrolyzer. Where the spent electrolyte is “crude” in that it is contaminated with some level of oxide species (e.g., lwt.% MgO or greater). Where the molten salt chamber now takes on the role of a “chlorinating device”. The solid pieces of NH4CI and MgCh’6EhO are dispensed into the chamber, which due to the temperature and contact with the molten salt the MgCh undergoes dehydration and the NH4CI is broken down into NH3 and HC1 gas. Where the addition of NH4CI into the crude electrolyte is to chlorinate the MgO present in the crude MgCh melt through the release of HC1 into the melt. Where the addition of NH4CI into the melt prevents hydrolysis of the MgCh’bEhO being added simultaneously. At the end of the addition, an electrolyte is yielded which MgO impurities have been slightly reduced, but not to the same degree as when the NEUCl-MgCh’bEhO is added, (will show higher oxide content than Example 2).Example 4 Production Replenishment with MgO instead of MgCl 2
[0344] MgO is added with NH4CI as a co-salt mixture to crude MgCh melt, where the MgO is chlorinated to yield MgCh. Solid NH4CI and MgO are mixed into a hopper in a 1: 1 NH4Cl:MgO ratio. The mixed solids are conveyed to a reagent hopper above a molten salt chamber containing anhydrous molten MgCh containing electrolyte, heated by an AC current applied via electrodes. The solid pieces of NH4CI dispensed into the chamber undergo decomposition into NH3 and HC1 gas due to the temperature of the melt. The evolved HC1 gas acts as a chlorinator to convert MgO to MgCh and H2O. The evolved water then evaporated due to the high temperature and removed from the vessel. The evolved NH3 gas is removed from the vessel and scrubbed through an HC1containing solution to form a NH4CI brine. At the end of addition, an anhydrous electrolyte melt containing MgCh remains in the vessel with less than 0.1wt.% of MgO present.Example 5 Carnallite hydrate reduction of MgO
[0345] NH4Cl-MgC12’6H2O + MgO simultaneous addition example. 30wt.% NH4CI solution is combined with 30wt% MgCh solution in a mixing vessel. The mixed solution is sent to evaporators and heated until the solution stoichiometry is approximately NJ Cl-MgCh’bFbO. This solution is cooled on a drum flaker device to form solid pieces of salt. These solid pieces are mixed in a 1:1 molar ratio with MgO in a reagent hopper above a molten salt chamber ccontaining a magnesium chloride electrolyte, heated by AC electrodes. The solid pieces of NH4Cl-MgC12’6H2O and MgO are dispensed into the chamber. The NH4Cl·MgCl2·6H2O added undergoes dehydration due to temperature and the NH4CI is broken down into NH3 and HC1 gas. Where the HC1 generated chlorinates the being added MgO present into MgCh. Where the addition of NH4CI into the melt prevents hydrolysis of the MgCh’bhhO being added simultaneously. The magnesium chloride electrolyte melt has lower MgO content than the one obtained in example 4 and further demonstrates that NE CTMgCh’bJtO is a more effective chlorinator than NH4CI alone.Example 6 NH4Cl·MgCl2·6H2O is added directly to a molten salt electrolyzer - skipping the dehydration reactor30 wt.% NH4CI solution is combined with 30wt.% MgCh solution in a mixing vessel. The mixed solution is sent to evaporators and heated until the solution stoichiometry is approximately NH4Cl·MgCl2·6H2O. This solution is cooled on a drum flaker device to form solid pieces of salt. These solid pieces are conveyed to a feedstock hopper above a molten salt electrolyzer. The solid pieces are dispensed into a chamber of said electrolyzer, partially separated from the main electrolysis chamber, which due to the temperature and contact with the molten salt undergo simultaneous dehydration and decomposition whereby the contained NH4CI is broken down into NH3 and HC1 gas. The NTUCl-MgCh’bFbO is added to a chamber which prevents evolved NH3, HC1, or water from reaching the electrolytically active area or Mg collection. This process usefully consumes some of the waste heat generated in the electrolysis. The MgCh in the feedstock melts and is incorporated into the electrolyte. Minimal hydrolysis is observed in this ammonium carnallite case relative to what would be observed with the addition of MgCl2·6H2O to the melt.At the end of the addition, an electrolyte is yielded in the electrolyzer which is enriched in MgCh, and substantially free of oxide impurities enabling the continuation of electrolysis. The <0. lwt.% oxides that are formed from the NH4Cl·MgCl2·6H2O dehydration are below the threshold of oxides required to optimized electrolyzer performance.Example 7: NH4Cl·MgCl2·6H2O added to molten chloride electrolyte
[0346] Solid NEUCl-MgCh’bEhO was prepared by mixing MgCh’bhhO and NH4CI, melted at 170°C, and allowing to cool to room temperature. An electrolyte mixture was prepared with anhydrous salts in the range of 5-15wt.% CaCl2, 40-60wt.%KCl, and 20-35wt.%NaCl. By melting the salts together and holding at 600°C. Solid NH4Cl·MgCl2·6H2O was added to the molten electrolyte melts and dissolved in the electrolyte. H2O, NH3, and HC1 gasses were released. MgO in the final melt measured at 0.02wt.%. and the MgCh concentration increased to 20wt.%.Example 8: NH4Cl·MgCl2·6H2O added to impure MgCl2molten electrolyte
[0347] Solid HrCl-MgCh’bFhO was prepared by mixing MgCh’bhhO and NH4CI, melted at 170°C, and allowing to cool to room temperature. Prepared electrolyte mixture with anhydrous 10wt.% MgCh, 5-15wt.% CaCl2, 40-60wt.% KC1, and 20-40wt.% NaCl. By melting and held at 600°C. About lwt.% MgO present in molten electrolyte. Solid NHrCl-MgCh’bFbO was added to the molten electrolyte melts and dissolved in the electrolyte. H2O, NH3, and HC1 gasses were released. MgO in the melt decreased to 0.02wt.%. MgCh concentration increased to 20wt.%Example 9: NH4CI and MgCh 6H2O added to molten depleted electrolyte
[0348] Solid NH4CI was mixed with solid MgCh’bThO in 1: 1 molar ratio. Prepared electrolyte mixture with anhydrous 10wt.% MgCh, 5-15wt.% CaCl2, 40-60wt% KC1, and 20-40wt.% NaCl was melted and held at 600°C. About lwt.% MgO present in molten electrolyte. A mixture of solid NH4CI and solid MgCh’bf O was added to the molten electrolyte melts and dissolved in the electrolyte. H2O, NH3, and HC1 gasses were released. MgO in the melt decreased to 0.05wt.%. MgCh concentration increased to 20wt.%.Example 10: Mg(OH)2and NH4Cl added to molten electrolyte
[0349] Solid Mg(OH)2was mixed with solid NH4Cl in 1:2 molar ratio. Prepared electrolyte mixture with anhydrous 10wt.% MgCh, 5-15wt.% CaCl2, 40-60wt.% KC1, and 20-40wt.% NaCl. Melted and held at 600 °C. About lwt.% MgO present in molten electrolyte. Mixture of solidMg(OH)2and solid NH4Cl was added to the molten electrolyte mix into the melt. H2O, NH3, and HC1 gasses were released. MgO in the melt decreased to 0.4wt.%. MgCh concentration increased to 20wt.%.Example 11: Mg(0H)2and NEEClMgCl2^EhO added to molten depleted electrolyte
[0350] Solid NH4Cl-MgCh’6H2O was prepared by mixing a 30wt.% MgCh and NH4CI solution, boiling it up to 170°C, and allowing to cool to room temperature. This solution was combined with solid Mg(OH)2in 1:2 molar ratio of Mg(OH)2with respect to NH4Cl·MgCl2·6H2O. Prepared electrolyte mixture with anhydrous 10wt.% MgCh, 5-15wt.% CaCl2, 40-60wt.% KC1, and 20-40wt.% NaCl. Melt and hold at 600°C. About lwt.% MgO present in molten electrolyte. Mixture of solid Mg(OH)2and solid NH4Cl·MgCl2·6H2O added to the molten electrolyte melts and dissolves in the electrolyte. H2O, NH3, and HC1 gasses are released. MgO in the melt decreases to 0.29wt.%. MgCh concentration increased to 20wt.%.Example 12: NEEClMgCl2^ hO added to molten chloride electrolyzer
[0351] Solid NH4Cl-M Ch'6H2O was prepared by mixing MgCh’bh O and NH4CI, melting at 170°C, and allowing to cool to room temperature. Prepared electrolyte mixture with anhydrous 5-15wt.% CaCl2, 45-60wt.% KC1, and 20-40wt.% NaCl. Melted and held at 600°C. No oxide present in molten electrolyte. Solid NEUCl-MgC ’bEhO was added to the molten electrolyte melts and dissolved in the electrolyte. H2O, NH3, and HC1 gasses were released. MgO in the melt measures 0.02wt.%. MgCh concentration increased to 20wt.%.Example 13: MgCh hexahydrate added to molten depleted electrolyte - counter example
[0352] Solid MgCh hexahydrate (MgCl2·6H2O) was prepared from a 30wt.% MgCh brine solution evaporating up to a temperature of 140°C and allowing to cool to room temperature. Prepared electrolyte mixture with anhydrous 10% MgCh, 5-15wt.% CaCl2, 40-60wt.% KC1, and 20-40wt.% NaCl by melting and holding at 700°C. About lwt.% MgO present in molten electrolyte. Hexahydrate added to the molten electrolyte melts and dissolves in the electrolyte. H2O and HC1 are released as gas. MgO in the melt increased to 2.2wt.%. MgCh concentration increased to 20wt.%.Example 14: Carnallite dehydration
[0353] 30 wt.% NH4CI solution at 100°C is combined with 30wt.% NdCh solution at 150°C in a mixing vessel. The mixed solution is sent to evaporators and heated until the solution stoichiometry is approximately NdCh-3(NH4Cl)-6H2O. This solution is cooled on a drum flaker device to form solid pieces of salt. These solid pieces are conveyed to a feedstock hopper above a molten salt chamber containing a chloride-based electrolyte, heated by electrodes. The solid pieces are dispensed into the chamber and contact the molten salt simultaneously dehydrating and decomposing wherein the contained NH4CI is broken down into NH3 and HC1 gas. The NdCh in the feedstock melts and is incorporated into the electrolyte with negligible hydrolysis. At the end of the addition, an electrolyte is yielded which is enriched in NdCh, and substantially free of oxide impurities (<0.1%) ready for feeding to electrolyzers to produce high purity Nd metal and CI2 gas.Example 15: Carnallite hydrochlorination of impurities
[0354] 30wt.% NH4CI solution at 100°C is combined with 30wt.% NdCh solution at 150°C in a mixing vessel. The mixed solution is sent to evaporators and heated until the solution stoichiometry is approximately NdCh-3(NH4Cl)-6H2O. This solution is cooled on a drum flaker device to form solid pieces of salt. These solid pieces are conveyed to a reagent hopper above a molten salt chamber containing a neodymium chloride electrolyte, heated by AC electrode,, where the neodymium chloride electrolyte is “spent” electrolyte that is, relatively depleted in NdCh content (e.g., 1% NdCh) that has been returned from a neodymium molten salt electrolyzer, where the spent electrolyte is “crude” in that it is contaminated with some level of oxide species (e.g., 1% Nd2Ch or greater), where the molten salt chamber now takes on the role of a “chlorinating device”. The solid pieces are dispensed into the chamber and contact the molten salt simultaneously dehydrating and decomposing wherein the contained NH4C1 is broken down into NH3 and HC1 gas, where the molar ratio of added NdCh-3(NH4Cl)-6H2O to the Nd2Ch in the crude electrolyte is about 1:1. At the end of the addition, an electrolyte is yielded which has been purged of neodymium oxide impurities to <0.1% Nd2Ch.Example 16: Nddh is added with NH4CI as a co-salt mixture to a “crude ” NdCh melt. Where the Nd2Os is hydrochlorinated to yield NdCh.
[0355] Solid NH4CI and Nd2Ch are mixed into a hopper in a 1:1 NH4Cl: Nd2Ch molar ratio. The mixed solids are conveyed to a reagent hopper above a molten salt chamber containing anhydrous molten electrolyte with >1% NdCh, heated by electrodes. The anhydrous moltenelectrolyte is spent, meaning it is depleted in NdCh content. The solid pieces of NH4CI dispensed into the chamber undergo decomposition into NH3 and HC1 gas. The evolved gasses are removed from the vessel and scrubbed through an HC1 containing solution to form an NH4CI brine. At the end of addition, an anhydrous electrolyte melt containing NdCh remains in the vessel with substantially lower Nd2Ch present than was added to the melt. <0.1% ISkhCh is present.Example 17: NdCh-3(N l4Cl) -6 l2O added directly to the electrolyzer, skipping the dehydration vessel.
[0356] 30 wt.% NH4CI solution at 100°C is combined with 30wt.% NdCh solution at 150°C in a mixing vessel. The mixed solution is sent to evaporators and heated until the solution stoichiometry is approximately: NdCh-3(NH4Cl)-6H2O. This solution is cooled on a drum flaker device to form solid pieces of salt. These solid pieces are conveyed to a reagent hopper above a molten salt electrolyzer. The NdCh-3(NH4Cl)-6H2O is added to a chamber which prevents evolved NH3, HC1, or water from reaching the electrolytically active area or Nd metal collection. The NdCh dehydrates without hydrolysis and mixes with the molten salt in the electrolyzer. The <0.1 wt.% oxides that are formed from the NdCh dehydration are below the threshold of oxides required for optimized electrolyzer performance.Example 18: NdC dlEO dehydrated without NH4CI using molten electrolyte solution
[0357] A 30wt.% solution of NdCh in water is boiled and concentrated until a solid NdCh’bT O hydrate is formed. This solution may be cooled on a drum flaker device to form solid pieces of salt. These solid pieces are conveyed to a reagent hopper above a molten salt chamber containing KC1, NaCl, and CaCl2. The evolved water evaporates and is removed from the vessel. At the end of addition, an anhydrous electrolyte melt containing NdCh remains in the vessel with <0.6wt.% Nd2Ch.Example 19: NdCh hexahydrate added to molten electrolyte - counter example.
[0358] Solid NdCh hexahydrate (NdCh’bT O) bought from chemical supplier. Prepared electrolyte mixture with anhydrous 5%- 15% CaCl2, 45%-65% KC1, and 25%-40% NaCl. Melt and hold at 700°C. Hexahydrate added to the molten electrolyte melts and dissolves in the electrolyte. H2O and HC1 are released as gas. Nd2Ch in the melt increases to 0.5wt.%. NdCh concentration calculated to reach 5 wt.% but increased only to 4wt.%.Example 20: NH4CI + NdCh OEEO added to molten electrolyte.
[0359] Solid NH4CI was mixed with solid NdCh-dHzO in 3: 1 molar ratio. Prepared electrolyte mixture with anhydrous 5%-l 5% CaCl2, 45%-65% KC1, and 25%-40% NaCl. Melt and held at 700°C. Mixture of solid NH4CI and solid NdCBCh-OFkO was added to the molten electrolyte melts and dissolves in the electrolyte. H2O, NH3, and HC1 gases were released. INchCh in the melt measured 0.05wt.%. NdCh concentration increased to 5wt.%.Example 21: PrCh heptahydrate added to molten electrolyte - counter example.
[0360] Solid PrCh heptahdyrate (PrCh-VFbO) was purchased from chemical supplier, Prepared electrolyte mixture with anhydrous 5%-l 5% CaCl2, 45%-65% KC1, and 25%-40% NaCl. Melt and hold at 700°C. The heptahydrate was added to the molten electrolyte melts and dissolves in the electrolyte. H2O and HC1 were released as gases. PriCh in the melt measured 0.5wt.%. PrCh concentration increased to 4wt.%.Example 22: NH4CI + PrChCEhO added to molten electrolyte.
[0361] Solid NH4CI mixed with solid NdCh’7H2O in 3:1 ratio. Prepared electrolyte mixture with anhydrous 5%-15% CaCl2, 45%-65% KC1, and 25%-40% NaCl. Melt and hold at 700°C. Mixture of solid NH4CI and solid PrCh-7H2O added to the molten electrolyte melts and dissolves in the electrolyte. H2O, NH3, and HC1 gasses are released. P^Ch in the melt measured 0.05wt.%. PrCh concentration increased to 5wt.%.
Claims
CLAIMS:
1. A method for producing, replenishing, or purifying a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxychloride, the method comprising contacting an ammonium magnesium chloride hydrate having greater than 3 waters of hydration with a molten salt, wherein the molten salt comprises at least one of MgCh, NaCl, KC1, CaCl2, NaF, KF, CaF2, BaF2, or BaCh; and obtaining a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxychloride.
2. The method of claim 1 wherein the ammonium magnesium chloride hydrate has 6 waters of hydration.
3. The method of claim 1 wherein the molten salt is between a temperature of 500 °C to 700 °C.
4. The method of claim 1 wherein the molten salt initially comprises at least 0.3 wt.% total of MgO, Mg(OH)2, MgOHCl, or a combination thereof.
5. The method of claim 4, wherein the obtained magnesium chloride electrolyte melt comprises less than 0.3 wt.% total of MgO, Mg(OH)2. MgOHCl, or a combination thereof.
6. The method of claim 4, wherein the contact occurs in a dehydration zone of an electrolyzer.
7. A method for producing, replenishing, or purifying a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxy chloride, the method comprising: contacting a mixture of magnesium chloride hydrate and ammonium chloride, wherein the magnesium chloride hydrate has greater than 3 waters of hydration with a molten salt, wherein the molten salt comprises at least one of MgCh, NaCl, KC1, CaCk, NaF, KF, CaF2, BaF2, or BaCh; and obtaining a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxychloride.
8. The method of claim 7 wherein the magnesium chloride hydrate has 6 waters of hydration.
9. The method of claim 7 wherein the molten salt is between a temperature of 500 °C to 70010. The method of claim 7 wherein the molten salt initially comprises at least 0.3 wt.% total of MgO, Mg(OH)2, MgOHCl, or a combination thereof.
11. The method of claim 10 wherein the obtained magnesium chloride electrolyte melt comprises less than 0.3 wt.% total of MgO, Mg(OH)2. MgOHCl, or a combination thereof.
12. The method of claim 9, wherein the contact occurs in a dehydration zone of an electrolyzer.
13. A method for producing, replenishing, or purifying a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxychloride, the method comprising: contacting a mixture of magnesium hydroxide and ammonium chloride or a mixture of magnesium oxide and ammonium chloride with a molten salt, wherein the molten salt comprises at least one of MgCl2, NaCl, KC1, CaCl2, NaF, KF, CaF2, BaF2, or BaCl2; and obtaining a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxy chloride.
14. The method of claim 13 wherein the molten salt is between a temperature of 500 °C to 700 °C.
15. The method of claim 13 wherein the molten salt initially comprises at least 0.3 wt.% total of MgO, Mg(OH)2, MgOHCl, or a combination thereof.
16. The method of claim 15 wherein the obtained magnesium chloride electrolyte melt comprises less than 0.3 wt.% total of MgO, Mg(OH)2. MgOHCl, or a combination thereof.
17. The method of claim 15, wherein the contact occurs in a dehydration zone of an electrolyzer.
18. A method for producing, replenishing, or purifying a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxy chloride, the method comprising: contacting a obtaining mixture of magnesium hydroxide and ammonium magnesium chloride hydrate or a mixture of magnesium oxide and ammonium magnesium chloride hydrate with a molten salt, wherein the molten salt comprises at least one of MgCl2, NaCl, KC1, CaCl2, NaF, KF, CaF2, BaF2, or BaCl2; and obtaining a magnesium chloride electrolyte melt that is substantially free of magnesium oxide, magnesium hydroxide and magnesium hydroxy chloride.
19. The method of claim 18 wherein the ammonium magnesium chloride hydrate has greater than 3 waters of hydration.
20. A method for producing, replenishing, or purifying a rare earth chloride electrolyte melt that is substantially free of rare earth oxide, rare earth hydroxide and rare earth hydroxychloride, the method comprising: contacting a mixture of rare earth chloride hydrate and ammonium chloride, wherein the rare earth chloride hydrate has at least 1 and less than or equal to 7 waters of hydration, with a molten salt, wherein the molten salt comprises at least one of rare earth chloride, NaCl, KC1, CaCl2. NaF, KF, CaF2, BaF2, or BaCl2; and wherein the rare earth metal is Nd, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm. Yb, Lu, Sc or Y. and obtaining a rare earth chloride electrolyte melt that has less than 0.1wt.% total rare earth oxide, rare earth hydroxide and rare earth hydroxy chloride.