A secondary battery and a heating device
By using a laminated structure of the outer packaging film and the hot-melt resin layer in the sealing part of the battery outer packaging film and the composite tab, the problem of battery outer packaging materials being difficult to meet high energy density and safety is solved, and better sealing is achieved effectiveness and safety.
Patent Information
- Application Number
- CN201710053013.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-01-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2037-01-22
AI Technical Summary
Existing battery packaging materials are difficult to meet the needs of portable electronic devices for high energy density, lightness, and diversity, and are prone to short circuits, leakage, and moisture penetration during the packaging process of composite tabs and packaging films, affecting the safety of battery use.
The sealing part of the outer packaging film and the composite tab is a laminated structure composed of an outer resin layer, a metal layer and an inner resin layer. The thickness of the sealing part is ensured by the combination of the molten resin layer, the inner resin layer and the metal layer after heat melting. Within a specific range, a heating device is combined to form a sealing portion that seals the composite tab and the outer packaging film, thereby improving the sealing strength and leakage prevention effect.
It achieves a better sealing effect, avoids leakage or penetration, ensures the safety of use and high energy density of the battery, and meets the diverse needs of thinness and lightness.
Smart Images

Figure CN106784998B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of energy storage materials, and in particular, to a secondary battery and a heating device. Background Art
[0002] With the rapid development of portable electronic devices, the requirements for high energy density battery power sources are getting higher and higher, and the outer packaging materials using metal shells are difficult to meet the requirements of portable electronic devices for thin and diverse battery power sources. At present, soft outer packaging films are used as battery packaging materials, such as aluminum laminated films or steel laminated films and other multi-layer composite films as battery outer packaging materials. This requires the outer packaging material to have long-term reliability and certain tensile properties. During the long-term repeated charging and discharging of the battery, it can still maintain its structural stability, play the role of wear resistance, oxygen isolation, moisture resistance, insulation, corrosion resistance, etc., which is of great significance to the safety of battery use.
[0003] There are various specifications of aluminum-plastic composite films and stainless steel-plastic composite films, as well as composite tabs with different melting points on the market. In the process of packaging the composite tabs and the composite packaging film, if the packaging is too thin, there is a risk of short circuit. If the packaging is too thick and the strength is insufficient, there is a risk of leakage or water penetration leading to battery bloating, which affects the safety of battery use.
[0004] In view of this, this application is hereby filed. Summary of the invention
[0005] The primary invention objective of the present application is to provide a secondary battery.
[0006] The second invention objective of the present application is to provide a heating device.
[0007] In order to achieve the purpose of this application, the technical solution adopted is:
[0008] The present application relates to a secondary battery, comprising a battery element, a composite tab and an outer packaging laminate film, wherein the battery element comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte;
[0009] The outer packaging laminate film is used to package the battery element and the composite tab, and includes an outer resin layer, a metal layer and an inner resin layer stacked in sequence;
[0010] The composite tab comprises a tab metal strip, wherein the tab metal strip is provided with a head hollow foil area, a tab glue covering area and a tail connection area which are connected in sequence along the length direction of the tab metal strip; the tab glue covering area is provided with tab glue, and the tail connection area is used to connect with the battery element; the outermost layer of the tab glue is a molten resin layer;
[0011] The secondary battery comprises a sealing portion for sealing the outer packaging laminate film and the composite tab; the sealing portion comprises the tab metal strip, the hot-melted molten resin layer, the hot-melted inner resin layer, the metal layer and the outer resin layer which are sequentially stacked from the inside to the outside;
[0012] The total thickness of the outer packaging laminate film is t, and the total thickness of the composite tab is p;
[0013] The thickness of the molten resin layer is c, and the thickness of the inner resin layer is a;
[0014] The thickness of the sealing portion is h, and h satisfies the following formula:
[0015] 2t+p-(2c+2a)×95% <h<2t+p-(2c+2a)×5%。
[0016] Preferably, along the length direction of the tab metal strip, the width of the sealing portion is 0.5 to 5 mm.
[0017] Preferably, along the length direction of the tab metal strip, the width of the tab glue is greater than the width of the sealing portion.
[0018] Preferably, along the length direction of the tab metal strip, the width of the tab glue exposed from the outer packaging laminate film is greater than 0.1 mm.
[0019] Preferably, the distance between the metal layer and the tab metal strip at any position is greater than 15 μm.
[0020] Preferably, the tab molten resin layer is at least one layer, the melting point of the outermost layer of the tab molten resin layer is MP1, the melting point of the inner resin layer is MP2, and |MP1-MP2|≤15°C.
[0021] Preferably, 0 <MP2-MP1≤10℃。
[0022] Preferably, the inner resin layer is a random polypropylene resin layer and / or a cast polypropylene film, the metal layer is an aluminum layer and / or a stainless steel layer, the outer resin layer is a nylon layer and / or a polyethylene terephthalate layer; and the molten resin layer is a polypropylene layer and / or a polyethylene layer.
[0023] The present application also relates to a heating device for forming a sealing portion of a sealed composite electrode tab and an outer packaging laminate film; the composite electrode tab comprises an electrode tab metal strip, the electrode tab metal strip is provided with an electrode tab glue covering area, the electrode tab glue covering area is provided with an outermost layer of an electrode tab glue which is a molten resin layer, and the outer packaging laminate film comprises an outer resin layer, a metal layer and an inner resin layer which are sequentially stacked;
[0024] The heating device comprises at least one pair of head assemblies, each of the pair of head assemblies is provided with a head groove for forming the sealing portion, and the head grooves are symmetrically arranged;
[0025] The total thickness of the outer packaging laminate film is t, and the total thickness of the composite tab is p;
[0026] The thickness of the molten resin layer is c, and the thickness of the inner resin layer is a;
[0027] The depth of the head groove is L, and L satisfies the following formula:
[0028] 2t+p-(2c+2a)×95%<2L<2t+p-(2c+2a)×5%.
[0029] Preferably, the width of the bottom of the head groove is greater than the width of the composite pole ear, and the chamfer of the edge of the head groove is 100 to 160 degrees.
[0030] The technical solution of this application has at least the following beneficial effects:
[0031] When the electrode tab is packaged in the present application, the heat compression ratio of the sum of the internal resin layer and the molten resin layer in the outer packaging laminate film is 5% to 95%, thereby achieving a better melting effect, ensuring high sealing strength and preventing leakage or penetration. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A schematic diagram of a secondary battery package;
[0033] Figure 2 It is a schematic diagram of the cross-sectional structure of the outer packaging laminate film;
[0034] Figure 3 It is a schematic diagram of the front structure of the composite tab;
[0035] Figure 4 It is a schematic diagram of the cross-sectional structure of a single-layer composite tab;
[0036] Figure 5 It is a schematic diagram of the cross-sectional structure of a multi-layer single-layer composite tab;
[0037] Figure 6 Schematic diagram of the cross-sectional structure of the sealing part
[0038] Figure 7 It is a schematic diagram of the front structure of the sealing part;
[0039] Figure 8 It is a schematic diagram of the packaging of the heating device, the outer packaging laminate film and the composite tab;
[0040] Fig. 9 It is a partial schematic diagram of the head groove;
[0041] 10-Battery element;
[0042] 20-outer packaging laminating film;
[0043] 201-external resin layer;
[0044] 202-metal layer;
[0045] 203-internal resin layer;
[0046] 204-first adhesive layer;
[0047] 205- second adhesive layer;
[0048] 30-composite tab;
[0049] 301-ear metal strip;
[0050] 301a- empty foil area at the head;
[0051] 301b-ear glue covering area;
[0052] 301c- tail connection area;
[0053] 302-ear glue;
[0054] 302a- molten resin layer;
[0055] 40- sealing part;
[0056] 50-head assembly;
[0057] 501-Head groove. DETAILED DESCRIPTION
[0058] The present application is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present application and are not used to limit the scope of the present application.
[0059] The present application relates to a secondary battery, comprising a battery element 10, an outer packaging laminate film 20 and a composite tab 30, wherein the battery element 10 comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte;
[0060] The positive electrode plate includes a positive electrode current collector and a positive electrode active material layer coated on the surface of the positive electrode current collector, and the negative electrode plate includes a negative electrode current collector and a negative electrode active material layer coated on the surface of the negative electrode current collector;
[0061] The outer packaging laminate film 20 is used to package the battery element 10 and the composite tab 30, that is, the battery element 10 is encapsulated by the outer packaging laminate film 20. The general process is: punching the outer packaging laminate film 20 to punch out the battery cell slot; placing the battery cell in the battery cell slot, and then encapsulating it. Figure 1 During the packaging process of the outer packaging laminate film 20 and the composite tab 30, a sealing portion 40 is formed by heat pressing.
[0062] Among them, Figure 2 The figure shows a schematic cross-sectional structure diagram along the vertical direction of the surface of the outer packaging laminate film 20. The outer packaging laminate film 20 includes an outer resin layer 201, a metal layer 202 and an inner resin layer 203 stacked in sequence; a first adhesive layer 204 is disposed between the outer resin layer and the metal layer 202, and a second adhesive layer 205 is disposed between the metal layer 202 and the inner resin layer 203. The outer packaging laminate film 20 may also have a matte layer outside the outer resin layer.
[0063] Further preferably, the inner resin layer 203 is selected from a random polypropylene resin layer and / or a cast polypropylene film (CPP film), the metal layer 202 is selected from an aluminum layer and / or a stainless steel layer, and the outer resin layer is selected from a nylon layer and / or a polyethylene terephthalate layer.
[0064] The composite tab 30 is an electrode terminal electrically connected to the battery element 10 and extending to the outside through the sealing portion 40. A head empty foil area 301a, a tab glue covering area 301b and a tail connection area 301c are sequentially arranged along the length direction of the tab metal strip 301; the tab glue covering area 301b is provided with a tab glue 302, and the tail connection area 301c is used to connect with the battery element 10. Figure 3 As shown, the width of the tab metal strip 301 is y. The outermost layer of the tab glue 302 is a molten resin layer 302a.
[0065] The tab metal strip 301 may be selected from materials such as aluminum, nickel or copper-plated nickel, and the molten resin layer 302a may be selected from a polypropylene layer and / or a polyethylene layer.
[0066] Specifically, the resin layer outside the composite electrode tab 30 is a single layer, and a schematic cross-sectional structure diagram thereof along a direction perpendicular to the surface of the composite electrode tab 30 is shown in FIG. Figure 4 The resin layer outside the composite electrode 30 is multi-layer, and the outermost layer is a molten resin layer 302a, and the cross-sectional structure schematic diagram along the surface vertical direction of the composite electrode 30 is as shown Figure 5When it is a multi-layer structure, the materials of different layers have different melting points, and the outermost layer can be a resin layer with a melt heat-sealing effect. Preferably, the inner layer can be made of a material with a high melting point, thereby enhancing the insulation effect and preventing the molten resin layer 302a from overmelting, causing the tab metal strip 301 and the metal layer 202 of the packaging film to be connected and form electrochemical corrosion.
[0067] During packaging, the outermost molten resin layer 302a of the tab glue 302 is melted and compressed with the inner resin layer 203 of the outer packaging laminate film 20 to form a sealing portion 40 to ensure the sealing of the battery. The sealing portion 40 includes a tab metal strip 301, a hot-melted molten resin layer 302a, a hot-melted inner resin layer 203, a metal layer 202, and an outer resin layer 201 stacked in sequence from the inside to the outside.
[0068] In the present application, the total thickness of the outer packaging laminate film 20 is t, and the total thickness of the composite tab 30 is p;
[0069] The thickness of the inner resin layer 203 in the outer packaging laminate film 20 is a, and the thickness of the molten resin layer 302a in the composite tab 30 is c;
[0070] The thickness of the sealing portion 40 is h, and h satisfies the following formula:
[0071] 2t+p-(2c+2a)×95% <h<2t+p-(2c+2a)×5%。
[0072] In the above formulas of the present application, the units of each thickness are the same.
[0073] The schematic cross-sectional structure diagram along the vertical direction of the surface of the sealing portion 40 is as follows: Figure 6 As shown, f = a + c. That is, when the tab is packaged in the present application, the thermal compression ratio of the sum of the internal resin layer 203 and the molten resin layer 302a is 5% to 95%, so as to achieve a better melting effect, ensure high strength and prevent liquid leakage. If the thermal compression ratio is less than 5%, the thickness of the sealing part 40 is too thin, and there is a risk of short circuit; if the thermal compression ratio is greater than 95%, the package is too thick, the strength of the hot pressing is insufficient, and there is a risk of leakage or water penetration.
[0074] Further preferably, h satisfies the following formula:
[0075] 2t+p-(2c+2a)×90% <h<2t+p-(2c+2a)×10%。
[0076] Further preferably, h satisfies the following formula:
[0077] 2t+p-(2c+2a)×80% <h<2t+p-(2c+2a)×20%。
[0078] Further preferably, h satisfies the following formula:
[0079] 2t+p-(2c+2a)×70% <h<2t+p-(2c+2a)×30%。
[0080] That is, when the tab is packaged in the present application, the thermal compression ratio of the sum of the internal resin layer 203 and the molten resin layer 302a in the outer packaging laminate film 20 is 10 to 90%, and is further preferably 20 to 80%, and more preferably 30 to 70%.
[0081] In the embodiments of the present application, Figure 7 As shown, along the length direction (L-L' direction) of the tab metal strip 301, the width d of the sealing portion 40 is 0.5-5 mm. If the width of the sealing portion is too small, the sealing effect is poor. If the sealing width is too large, the battery energy density will be reduced. If the sealing width exceeds the width of the tab film, there will be a risk of corrosion and leakage.
[0082] In the embodiments of the present application, Figure 7 As shown, along the length direction (L-L' direction) of the pole ear metal strip 301, the width of the pole ear glue 302 is greater than the width of the sealing portion 40, thereby ensuring that the sealing area does not exceed the pole ear glue, avoiding the outer packaging laminate film 20 from being burned through during the sealing process, so that the metal layer 202 therein is directly connected to the pole ear metal strip 301, causing a short circuit.
[0083] Further preferably, in the embodiments of the present application, Figure 6 As shown, in order to avoid direct contact between the metal layer 202 and the tab metal strip 301 , along the length direction of the tab metal strip 301 , the width of the portion e of the tab glue 302 exposed from the outer packaging laminate film 20 is greater than 0.1 mm.
[0084] In the embodiment of the present application, the distance between the metal layer 202 and the tab metal strip 301 at any position is greater than 15 μm, thereby further ensuring that the tab metal strip 301 of the composite tab 30 has a certain insulation distance from the metal layer 202 in the outer packaging film, thereby avoiding electrochemical corrosion and short circuit.
[0085] In the embodiment of the present application, in order to further improve the sealing effect, the ear glue 302 is at least one layer, the melting point of the outermost molten resin layer 302a of the ear glue 302 is MP1, the melting point of the inner resin layer 203 is MP2, and |MP1-MP2|≤15° C. If the melting point difference between the molten resin layer 302a and the inner resin layer 203 is too large, the heat sealing melting effect is poor, the strength is low, and there is a risk of leakage and moisture penetration.
[0086] Among them, the molten resin layer 302a and the internal resin layer 203 are both made of existing known materials, and the technicians select appropriate materials for preparation according to the melting points of the existing known materials.
[0087] Further preferably, MP2-MP1>0. During the heat sealing process, the internal resin layer 203 in the outer packaging laminate film 20 is heated first. Therefore, the internal resin layer 203 uses a material with a higher melting point than the molten resin layer 302a, so that the two can soften and melt at the same time, thereby further improving the heat sealing melting effect.
[0088] More preferably, MP2-MP1≤10°C, that is, the melting point of the inner resin layer 203 is within 10°C higher than that of the molten resin layer 302a, so as to further improve the heat sealing melting effect.
[0089] The present application also relates to a heating device, such as Figure 8 As shown, a sealing portion 40 is used to form a sealed composite electrode tab 30 and an outer packaging laminate film 20. The composite electrode tab 30 includes an electrode tab metal strip 301, an electrode tab glue covering area 301b is provided on the electrode tab metal strip 301, and an electrode tab glue 302 whose outermost layer is a molten resin layer 302a is provided on the electrode tab glue covering area 301b, and the outer packaging laminate film 20 includes an outer resin layer 201, a metal layer 202 and an inner resin layer 203 which are stacked in sequence;
[0090] The heating device includes at least one pair of head assemblies 50, each of which is provided with a head groove 501 for forming a sealing portion 40, and the head grooves 501 are symmetrically arranged;
[0091] The total thickness of the outer packaging laminate film 20 is t, and the total thickness of the composite tab 30 is p;
[0092] The thickness of the molten resin layer 302a is c, and the thickness of the internal resin layer 203 is a;
[0093] The depth of the head groove 501 is L, and L satisfies the following formula:
[0094] 2t+p-(2c+2a)×95%<2L<2t+p-(2c+2a)×5%.
[0095] Further preferably, L satisfies the following formula:
[0096] 2t+p-(2c+2a)×90%<2L<2t+p-(2c+2a)×10%.
[0097] Further preferably, L satisfies the following formula:
[0098] 2t+p-(2c+2a)×80%<2L<2t+p-(2c+2a)×20%.
[0099] Further preferably, L satisfies the following formula:
[0100] 2t+p-(2c+2a)×70%<2L<2t+p-(2c+2a)×30%.
[0101] In the heating device of the present application, Fig. 9 for Figure 8 In the partial enlarged view, the width g of the bottom of the head groove 501 is greater than the width y of the composite tab 30, and the width of the mouth of the head groove 501 is I; the chamfer r of the edge of the mouth of the head groove 501 is 100 to 160 degrees. The use of this angle allows the heat-sealed molten resin to fill the slot space well, thereby improving the sealing performance of the package.
[0102] In the embodiment of the present application, the positive electrode active material layer contains a positive electrode active material, which can be selected from lithium cobalt oxide, lithium manganese oxide, nickel cobalt aluminum ternary material (NCA) or nickel cobalt manganese ternary material (NCM), etc.; the negative electrode active material layer contains a negative electrode active material, which can be selected from graphite or a material containing Si element.
[0103] The electrolyte can be solid, liquid or gel electrolyte.
[0104] When a liquid electrolyte or a gel electrolyte is used, the battery element 10 further includes a separator, and the separator is selected from polyolefin separators.
[0105] Example
[0106] Preparation of positive electrode:
[0107] The positive electrode plate includes a positive electrode current collector and a positive electrode active material layer coated on the surface of the current collector. The positive electrode current collector is made of metal foil, and aluminum foil is commonly used. The positive electrode active material layer includes a positive electrode active substance, a binder and a conductive agent. The positive electrode active substance can be a composite oxide composed of transition metals such as lithium cobalt oxide, lithium iron phosphate, nickel cobalt manganese or nickel cobalt aluminum, lithium manganese oxide, etc. The conductive agent can be a conductive material such as carbon black, carbon nanotubes, carbon fiber, graphene, conductive graphite, etc. The binder can use polytetrafluoroethylene or poly (vinylidene fluoride). The solvent can use N-methylpyrrolidone (NMP). The following example shows a certain ratio of positive electrode materials, which is not limited to this mixed ratio.
[0108] Prepare a positive electrode slurry of 97% lithium cobalt oxide: 1.8% conductive carbon black: 1.2% binder polyvinylidene fluoride. First, mix the lithium cobalt oxide and the conductive agent evenly, add the solvent NMP to evenly disperse them, and add the binder to adjust the viscosity to obtain the positive electrode slurry. The positive electrode slurry is evenly coated on the surface of the current collector, then dried at high temperature to remove the solvent, and rolled to form a certain compacted positive electrode sheet.
[0109] Preparation of negative electrode sheet:
[0110] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer coated on the surface of the current collector. The negative electrode current collector is made of metal foil, and copper foil is commonly used. The negative electrode active material layer includes a negative electrode active material, a binder and a conductive agent. The positive electrode active material can be graphite or a carbon-containing composite or a metal machine material, such as artificial graphite, natural graphite, mesophase carbon microspheres, carbon fiber, hard carbon, silicon carbon negative electrode, lithium negative electrode, etc. The conductive agent can be a conductive material such as carbon black, carbon nanotubes, carbon fiber, graphene, conductive graphite, etc. The binder can use styrene-butadiene rubber or poly (vinylidene fluoride). If necessary, a thickener such as sodium carboxymethyl cellulose (CMC) needs to be added to make the negative electrode slurry more stable, and the solvent can be N-methylpyrrolidone (NMP) or deionized water. The following example shows a certain ratio of negative electrode materials, which is not limited to this mixed ratio, and the solvent is deionized water. Prepare a negative electrode slurry of 96.5% artificial graphite: 1% conductive carbon black: 1.5% styrene-butadiene rubber: 1% CMC. First, mix the graphite and conductive carbon black evenly, add deionized water as a solvent and CMC to evenly disperse, and add styrene-butadiene rubber as a binder to adjust the viscosity to obtain the negative electrode slurry. Evenly coat the negative electrode slurry on the surface of the current collector, then dry it at high temperature to remove the solvent, and form a certain compacted negative electrode sheet by rolling.
[0111] Preparation of electrolyte:
[0112] The electrolytic solution includes an electrolyte salt and an organic solvent, and additionally a gel electrolyte may be used.
[0113] Examples of organic solvents for the electrolyte include diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, ethyl propyl carbonate, propylene carbonate, ethylene carbonate, propylene carbonate, ethyl propionate, propyl propionate, propylene sulfite, etc. Examples of electrolyte salts include LiPF6 and LiBF4.
[0114] This embodiment uses an electrolyte solvent with a ratio of 50% propyl propionate, 25% ethylene carbonate, 16% propylene carbonate, 6% ethanedinitrile, and 3% ethylene carbonate, and the LiPF6 lithium salt concentration is 1.1 mol / L.
[0115] Diaphragm:
[0116] A porous polyethylene film with a thickness of 8 μm and a porosity of 30% was used.
[0117] Battery preparation:
[0118] The positive and negative electrode sheets are cut, the negative electrode is 2 mm wider than the positive electrode sheet, the negative electrode tab is led out at the empty current collector of the negative electrode sheet, and the positive electrode tab is led out at the empty current collector of the positive electrode sheet. The width of the isolation membrane is 2.5 mm wider than the negative electrode to ensure that there is isolation membrane insulation between the positive and negative electrodes, and the opposite side of the positive electrode active material layer is wrapped by the negative electrode active material layer. The separator extends beyond the two ends of the negative electrode, and the positive and negative electrode sheets and the separator are wound to obtain a battery element 10.
[0119] like Figure 1 The battery components are placed in a packaging bag, top and side sealed, and then the electrolyte is injected to complete the packaging. After formation, the air is evacuated and sealed to form a battery.
[0120] Secondary battery packaging:
[0121] An aluminum-plastic film with a thickness of t=61 μm is used as the outer packaging laminate film, the inner resin layer is a random polypropylene resin layer, the metal layer is an aluminum layer, the outer resin layer is a nylon layer, the inner resin layer thickness of the aluminum-plastic film is a=24 μm; the total thickness of the tab is p=210 μm, the molten resin layer is c=80 μm, which is a single-layer CPP layer, and the total thickness of the tab glue molten layer is 2c=160 μm;
[0122] Among them, Examples 1 to 5 and Comparative Examples 1-1 to 1-4 use aluminum-plastic film and single-layer ear glue to heat-seal the ear. DSC tests show that the melting point MP1 of the outermost layer of the ear molten resin layer is 10°C lower than the melting point MP2 of the inner resin layer. Batteries are manufactured using the above aluminum-plastic film and ear for packaging.
[0123] When there is no heat seal compression, that is, -(2c+2a)=0;
[0124] h max =2t+p=61×2+210=332μm;
[0125] When all heat-sealing molten resin layers are lost after heat-sealing extrusion, that is -(2c+2a)×100%;
[0126] h min =2t+p-(2c+2a)=61×2+210-(80×2+24×2)=124 μm.
[0127] The purpose of experimental comparison is achieved by changing the temperature and pressure of the packaged head and the depth L of the head groove. The thickness of the sealing part of the embodiment and the comparative example is shown in Table 1:
[0128] Table 1:
[0129] serial number h(μm) d(mm) e(mm) Example 1-1 160 2 >0.1 Example 1-2 190 2 >0.1 Examples 1-3 230 2 >0.1 Examples 1-4 270 2 >0.1 Examples 1-5 310 2 >0.1 Comparative Example 1-1 125 2 >0.1 Comparative Example 1-2 320 2 >0.1 Comparative Examples 1-3 230 0.5 >0.1 Comparative Examples 1-4 230 2 <0.1
[0130] Each of the above embodiments and comparative examples formed a test cell as described above.
[0131] Detection method:
[0132] (1) Detect short circuit:
[0133] The resistance between the positive and negative electrodes, as well as the resistance between the positive and negative tabs and the metal layer of the aluminum-plastic film are measured. The battery just after packaging has a sufficiently high series resistance, and when a short circuit occurs, the resistance is reduced to the milliohm level.
[0134] (2) Detection of leakage and flatulence
[0135] Visually inspect the battery for leakage or bloating, and include any leakage or bloating after long-term cycle testing (500 times).
[0136] (3) Cycle performance
[0137] At 25°C, the battery was charged to 4.4V at a constant current of 1C, then charged to a current of 0.05C at a constant voltage, and then discharged to 3.0V at a constant current of 0.7C. This was the first cycle. The capacity retention rate of the lithium-ion battery after 500 cycles was calculated by performing multiple cycles under the above conditions.
[0138] The formula of cycle performance is: Capacity retention = 100 × (discharge capacity at the 500th cycle) / (discharge capacity at the first cycle) (%)
[0139] Also measure the thickness expansion after cycling:
[0140] Cycle thickness expansion = 100 × (500th cycle full charge battery thickness) / (first cycle full charge battery thickness) (%)
[0141] See Table 2 for relevant test data.
[0142] Table 2
[0143]
[0144]
[0145] As can be seen from Table 2, the batteries of Examples 1 to 5 with different packaging thicknesses within the appropriate packaging range have no short circuit leakage or bloating, and have excellent cycle performance, with the capacity maintained at more than 80% and the cycle expansion less than 10%.
[0146] In comparative example 1-1, due to overheat sealing, the package thickness of 125 μm was less than the appropriate range, resulting in a short circuit in the battery. The reason for the short circuit was, for example, that the metal strip of the tab contacted the metal layer of the aluminum-plastic film, resulting in a short circuit.
[0147] In Comparative Example 1-2, due to insufficient melting of the heat-sealed resin layer, there will be gas and moisture channels in the sealed area. The package thickness is 320μm, and most batteries have leakage and flatulence. The rest are unqualified for long-term cycle performance, with low capacity retention and large cycle expansion. When the heat-sealed melted resin layer drops outside the appropriate range due to thickness or the heat-sealed melt is incomplete and there are pore channels between the battery and the outside air, air and moisture will penetrate into the battery, causing battery flatulence.
[0148] In Comparative Examples 1-3, due to the narrow packaging width, there are capillary channels of different sizes between the inside of the battery and the outside world in the sealing part. Four batteries in the comparative examples leaked and swelled before cycling, and the others also had problems of low cycle capacity and large cycle expansion during long-term cycling.
[0149] In Comparative Examples 1-4, since the distance between the tab glue and the aluminum-plastic film after packaging was less than 0.1 mm, 8 batteries had short circuits. The reason was that the metal strip of the tab and the metal layer of the aluminum-plastic film were in contact and short-circuited.
[0150] Comparative Example: The above secondary battery packaging material is used (the thickness of the outer packaging laminate film t, the thickness of the inner resin layer of the aluminum-plastic film a, the total thickness of the tab p, and the molten resin layer c are the same as those in Example 1), except that in Comparative Examples 2-1 to 2-5, the DSC test MP2-MP1=20°C, and the thickness of the prepared sealing portion is shown in Table 3. The cycle performance after packaging is tested, as shown in Table 4.
[0151] Table 3
[0152]
[0153]
[0154] Table 4
[0155]
[0156] In comparative examples 2-1 to 2-5, MP2-MP1=20°C has different melting degrees due to the difference in melting point, and there will be some pore channels caused by incomplete melting at the melting interface after packaging, which will lead to battery leakage and bloating at the beginning. Other batteries will also expose cross-sectional problems in long-term cycles, leading to leakage and bloating.
[0157] Another embodiment:
[0158] The aluminum-plastic film and the three-layer ear glue ear are heat-sealed. The DSC test shows that the melting point MP1 of the outermost layer of the ear molten resin layer is 10°C lower than the melting point MP2 of the inner resin layer. The embodiment is the packaging effect within the qualified packaging range, and the comparative example is a battery packaged outside the qualified range.
[0159] An aluminum-plastic film with a thickness of t=88 μm is used as an outer packaging laminate film, the inner resin layer is a random polypropylene resin layer, the metal layer is an aluminum layer, the outer resin layer is a nylon layer, and the inner resin layer thickness of the aluminum-plastic film is a=35 μm; the total thickness of the tabs p=270 μm, the thickness of the tab metal strip is 80 μm, the thickness of the tab glue is 100 μm, the molten resin layer c=35 μm, and it is a three-layer tab glue structure. The middle skeleton layer of the tab glue is a resin layer with a higher melting point, with a thickness of 25 μm, and the total thickness of the tab glue molten layer is 2c=70 μm.
[0160] The above aluminum-plastic film and tabs are used to make batteries for packaging.
[0161] When there is no heat seal compression, that is, -(2c+2a)=0;
[0162] h max =2t+p=88×2+270=446μm;
[0163] When all heat-sealing molten resin layers are lost after heat-sealing extrusion, that is -(2c+2a)×100%;
[0164] h min =2t+p-(2c+2a)=88×2+270-(35×2+35×2)=306 μm.
[0165] The purpose of experimental comparison is achieved by changing the temperature and pressure of the packaged head and the depth L of the head groove. The thickness of the prepared sealing part is shown in Table 5. The cycle performance after packaging is tested, as shown in Table 6.
[0166] Table 5
[0167] serial number h(μm) d(mm) e(mm) Example 2-1 310 2 >0.1 Example 2-2 340 2 >0.1 Example 2-3 370 2 >0.1 Embodiment 2-4 400 2 >0.1 Embodiment 2-5 430 2 >0.1 Comparative Example 3-1 280 2 >0.1 Comparative Example 3-2 440 2 >0.1 Comparative Example 3-3 340 0.5 >0.1 Comparative Examples 3-4 340 2 <0.1
[0168] Table 6
[0169]
[0170] It can be seen from Table 6 that the batteries of Examples 2-1 to 2-5 with different packaging thicknesses within the appropriate packaging range have no short circuit leakage or bloating, and have excellent cycle performance, with the capacity maintained at more than 80% and the cycle expansion less than 10%.
[0171] In Comparative Example 3-1, due to overheat sealing, the package thickness of 310 μm was less than the appropriate range, resulting in battery leakage. The reasons for the leakage were, for example, overheat sealing of the tab metal strip and the PP melt layer of the aluminum-plastic film, resulting in a gap between the skeleton layer and the PP layer, leading to leakage.
[0172] In Comparative Example 3-2, due to the incomplete melting of the heat-sealed resin layer, there will be gas and moisture channels in the sealed area. The package thickness is 440μm, and most of the batteries have leakage and flatulence. The rest are unqualified for long-term cycle performance, with low capacity retention and large cycle expansion. When the heat-sealed melted resin layer drops outside the appropriate range due to thickness or the heat-sealed melt is incomplete and there are pore channels between the battery and the outside air, air and moisture will penetrate into the battery, causing battery flatulence.
[0173] In comparative example 3-3, due to the narrow package width, there are capillary channels of different sizes between the inside of the battery and the outside world in the sealing part. Three batteries in the comparative example leaked and swelled before cycling, and the others also had problems of low cycle capacity and large cycle expansion during long-term cycling.
[0174] In Comparative Example 3-4, since the distance between the tab glue and the aluminum-plastic film after packaging was less than 0.1 mm, 5 batteries had short circuits. The reason was that the metal strip of the tab and the metal layer of the aluminum-plastic film were in contact and short-circuited.
[0175] Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the claims. Any technical personnel in this field may make several possible changes and modifications without departing from the concept of the present application. Therefore, the scope of protection of the present application shall be based on the scope defined by the claims of the present application.
Claims
1. A secondary battery, comprising a battery element, a composite tab and an outer packaging laminate film, wherein the battery element comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte; characterized in that: The outer packaging laminate film is used to package the battery element and the composite tab, and includes an outer resin layer, a metal layer and an inner resin layer stacked in sequence; The composite tab comprises a tab metal strip, wherein the tab metal strip is provided with a head hollow foil area, a tab glue covering area and a tail connection area which are connected in sequence along the length direction of the tab metal strip; the tab glue covering area is provided with tab glue, and the tail connection area is used to connect with the battery element; the tab glue comprises an inner skeleton layer and an outermost molten resin layer, and the melting point of the skeleton layer is higher than the melting point of the molten resin layer; The secondary battery comprises a sealing portion for sealing the outer packaging laminate film and the composite tab; the sealing portion comprises the tab metal strip, the hot-melted molten resin layer, the hot-melted inner resin layer, the metal layer and the outer resin layer which are sequentially stacked from the inside to the outside; The total thickness of the outer packaging laminate film is t, and the total thickness of the composite tab is p; The thickness of the molten resin layer is c, and the thickness of the inner resin layer is a; The thickness of the sealing portion is h, and h satisfies the following formula: 2t+p-(2c+2a)×95% <h<2t+p-(2c+2a)×10%。 2. The secondary battery according to claim 1, characterized in that: Along the length direction of the tab metal strip, the width of the sealing portion is 0.5 to 5 mm.
3. The secondary battery according to claim 1, characterized in that: Along the length direction of the tab metal strip, the width of the tab glue is greater than the width of the sealing portion.
4. The secondary battery according to claim 1, characterized in that: Along the length direction of the tab metal strip, the width of the tab glue exposed from the outer packaging laminate film is greater than 0.1 mm.
5. The secondary battery according to claim 1, characterized in that: The distance between the metal layer and the tab metal strip at any position is greater than 15 μm.
6. The secondary battery according to claim 1, characterized in that: The tab molten resin layer is at least one layer, the melting point of the outermost layer of the tab molten resin layer is MP1, the melting point of the inner resin layer is MP2, and |MP1-MP2|≤15°C.
7. The secondary battery according to claim 6, characterized in that: 0 <MP2-MP1≤10℃。 8. The secondary battery according to claim 1, characterized in that: The inner resin layer is a random polypropylene resin layer and / or a cast polypropylene film, the metal layer is an aluminum layer and / or a stainless steel layer, the outer resin layer is a nylon layer and / or a polyethylene terephthalate layer; the molten resin layer is a polypropylene layer and / or a polyethylene layer.