Electrode catalyst for electrochemical device, membrane electrode assembly, method for producing the same, and electrode catalyst layer for electrochemical device

By using mesoporous materials to support catalyst metal particles in electrochemical devices and controlling their number density distribution, the problem of catalyst metal poisoning is solved, and the catalyst activity and fuel cell performance are improved.

CN111063896BActive Publication Date: 2024-11-08PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN201910922480.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-17
Filing Date
2019-09-27
Publication Date
2024-11-08
Estimated Expiration
2039-09-27

AI Technical Summary

Technical Problem

In existing electrochemical devices, the problem of catalyst metal poisoning caused by polymer electrolytes is difficult to effectively solve, affecting device performance.

Method used

By using mesoporous materials to support catalyst metal particles and control the mode radius and pore volume of the mesoporous materials, the number density of the catalyst metal particles is smaller than that of the mesoporous materials, thereby reducing the polymer electrolyte and catalyst metal Contact to inhibit poisoning.

Benefits of technology

It effectively reduces the catalyst metal poisoning caused by polymer electrolytes, improves the activity of the electrode catalyst and the power generation performance of the fuel cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111063896B_ABST
    Figure CN111063896B_ABST
Patent Text Reader

Abstract

The present disclosure provides an electrode catalyst for an electrochemical device, which can reduce poisoning of catalyst metals caused by ionomers. The electrode catalyst for an electrochemical device disclosed in the present disclosure is an electrode catalyst for an electrochemical device comprising a mesoporous material and catalyst metal particles supported at least inside the mesoporous material, wherein the mesoporous material has mesopores, and before the catalyst metal particles are supported, the mode radius of the mesopores is 1 to 25 nm, and the pore volume is 1.0 to 3.0 cm 3 / g, the number density of the catalytic metal particles supported in the mesopores is smaller on the outside of the mesoporous material than on the inside of the mesoporous material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to an electrode catalyst used in an electrochemical device, an electrode catalyst layer containing the electrode catalyst, a membrane electrode assembly having the electrode catalyst layer, an electrochemical device using the membrane electrode assembly, a method for manufacturing an electrode catalyst layer of an electrochemical device, and a method for manufacturing a membrane electrode assembly of an electrochemical device. Background Art

[0002] As an example of an electrochemical device, a fuel cell is known. For example, a polymer electrolyte fuel cell includes a membrane electrode assembly (MEA) for causing a fuel gas containing hydrogen and an oxidant gas containing oxygen to undergo an electrochemical reaction (electricity generation reaction).

[0003] Generally speaking, the electrode catalyst layer constituting the membrane electrode assembly is formed by dispersing a catalyst in which a catalyst metal such as platinum is supported on a conductive material such as carbon black and a polymer electrolyte (hereinafter referred to as an ionomer) having proton conductivity in a solvent such as water or alcohol to prepare a catalyst paste, and then applying the catalyst paste to a polymer electrolyte membrane or other substrate and drying it.

[0004] In order to suppress poisoning of the catalyst metal by the ionomer, a method has been proposed in which catalyst metal particles are supported inside a carrier composed of mesoporous carbon and the carrier supported with the particles is covered with the ionomer (for example, Patent Documents 1 and 2).

[0005] Prior Art Literature

[0006] Patent Document 1: International Publication No. 2014 / 175106

[0007] Patent Document 2: International Publication No. 2014 / 185498 Summary of the invention

[0008] An object of the present disclosure is to provide, as an example, an electrode catalyst for an electrochemical device, an electrode catalyst layer for an electrochemical device, a membrane electrode assembly for an electrochemical device, and an electrochemical device, which are capable of reducing poisoning of a catalyst metal by an ionomer.

[0009] One embodiment of an electrode catalyst for an electrochemical device according to the present disclosure comprises a mesoporous material and catalyst metal particles supported at least inside the mesoporous material, wherein the mesoporous material has mesopores, and before the catalyst metal particles are supported, the mesopores have a mode radius of 1 to 25 nm and a pore volume of 1.0 to 3.0 cm 3 / g, and the number density of the catalytic metal particles supported in the mesopores is smaller on the outside of the mesoporous material than on the inside of the mesoporous material.

[0010] In addition, one embodiment of an electrode catalyst layer of an electrochemical device according to the present disclosure includes at least the electrode catalyst of the above-mentioned one embodiment and an ionomer.

[0011] In addition, one mode of the membrane electrode assembly of the electrochemical device involved in the present disclosure comprises a polymer electrolyte membrane and a fuel electrode and an air electrode, wherein the fuel electrode and the air electrode are arranged on both sides of the above-mentioned polymer electrolyte membrane and include an electrode catalyst layer and a gas diffusion layer, and at least the above-mentioned electrode catalyst layer of the above-mentioned air electrode includes the electrode catalyst layer of the above-mentioned one mode.

[0012] Furthermore, one aspect of the electrochemical device according to the present disclosure includes the membrane electrode assembly of the above aspect.

[0013] In addition, one embodiment of the method for producing an electrode catalyst for an electrochemical device according to the present disclosure comprises the step of supporting catalyst metal particles in the mesopores of a mesoporous material having mesopores having a mode radius of 1 to 25 nm and a pore volume of 1.0 to 3.0 cm 3 / g, and in the above step, the number density of the catalytic metal particles supported in the above mesopores is smaller on the outside of the above mesoporous material than on the inside of the above mesoporous material.

[0014] In addition, one aspect of the method for manufacturing a membrane electrode assembly of an electrochemical device disclosed in the present invention comprises: a step of causing the catalyst metal particles to be loaded in the mesopores of a mesoporous material having mesopores in such a manner that the number density on the outside of the mesoporous material is smaller than the number density on the inside of the mesoporous material, wherein the mode radius of the mesopores is 1 to 25 nm and the pore volume is 1.0 to 3.0 cm 3 / g; a step of supporting an ionomer in the mesoporous material supporting the catalyst metal particles; and a step of providing an electrode catalyst layer comprising a mesoporous material supporting the catalyst metal particles and the ionomer on the electrolyte membrane.

[0015] The present disclosure is configured as described above, and can reduce poisoning of the catalyst metal by the ionomer as compared with the related art. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a schematic diagram showing an example of the electrode catalyst of the present disclosure and an electrode catalyst of a comparative example.

[0017] Figure 2 It is a schematic diagram showing a schematic configuration example of a membrane electrode assembly included in the electrochemical device according to the embodiment of the present disclosure.

[0018] Figure 3 It means using Figure 2A schematic diagram of a structural example of a single cell of a fuel cell of the membrane electrode assembly shown.

[0019] Figure 4 This is a cross-sectional SEM image of a cathode catalyst layer using the electrode catalyst of the example.

[0020] Figure 5 This is a cross-sectional SEM image of a cathode catalyst layer using an electrode catalyst of a comparative example.

[0021] Figure 6 This is a table showing the performance and physical properties of cathode catalysts using the electrode catalysts of Examples and Comparative Examples.

[0022] Figure 7 These are a cross-sectional STEM image and an elemental map of a cathode catalyst layer using the electrode catalyst of the example.

[0023] Description of Reference Numerals

[0024] 1 Mesoporous carbon

[0025] 2 Mesopore

[0026] 3 Catalyst metal particles

[0027] 4 Ionomer

[0028] 5 Area 1

[0029] 6 Area 2

[0030] 10 Membrane Electrode Assembly

[0031] 11 Polymer Electrolyte Membrane

[0032] 12 Electrode catalyst layer

[0033] 13 Gas Diffusion Layer

[0034] 13a Substrate

[0035] 13b Coating layer

[0036] 14 Diaphragm

[0037] 20 single battery DETAILED DESCRIPTION

[0038] (How one aspect of the present disclosure was obtained)

[0039] As described above, generally speaking, the electrode catalyst layer possessed by the membrane electrode assembly is formed by dispersing a catalyst in which a catalyst metal such as platinum is supported on a conductive material such as carbon black and a proton-conductive ionomer in a solvent such as water or alcohol to make a catalyst paste, and then applying the catalyst paste to a polymer electrolyte membrane or other substrate and drying it.

[0040] The microstructure of the electrode catalyst layer thus produced (hereinafter referred to as a three-phase interface structure) becomes a structure in which an ionomer is covered on the catalyst. In this three-phase interface structure, it has been believed that contacting the catalyst metal with the ionomer improves performance from the perspective of supplying protons to the catalyst metal surface. However, it has been learned in recent years that the catalyst metal is poisoned by contact with the ionomer. Therefore, it is pointed out that contacting the catalyst metal with the ionomer reduces performance.

[0041] To address such a problem, Patent Documents 1 and 2 propose a method of preventing the ionomer from contacting the metal catalyst by enclosing a metal catalyst in a carbon carrier having large-capacity pores such as mesoporous carbon.

[0042] However, the inventors of the present invention have conducted intensive studies and found that part of the ionomer may infiltrate into the mesopores. Therefore, even if an electrode catalyst containing catalytic metal particles (such as Pt particles) in the mesopores is used, it is not sufficient as a means to suppress poisoning of the catalytic metal by the ionomer.

[0043] To this end, the present inventors conducted research on electrode catalysts that reduce the poisoning of catalyst metals caused by ionomers, and found that by reducing the catalyst metal particles carried in the interior of the mesoporous carbon close to the surface that is easily invaded by the ionomers, the poisoning of the catalyst metal can be reduced, thereby completing the present disclosure.

[0044] In addition, in this specification, mesoporous carbon is a porous carbon having mesopores with a mode radius of 1 to 25 nm and capable of freely controlling the pore structure by, for example, changing the mold or carbon source and / or controlling the reaction temperature and other synthesis conditions. Furthermore, it can be considered that the material used in the electrode catalyst layer disclosed in the present invention is not limited to mesoporous carbon, as long as the mode radius and / or pore volume are the same, even other mesoporous materials will have the same effect. As mesoporous materials other than mesoporous carbon, mesoporous materials composed of oxides of titanium, tin, niobium, tantalum, zirconium, aluminum, silicon, etc. can be cited.

[0045] It has been considered that the size of ionomers in the catalyst ink is several tens of nanometers and therefore Pt particles of the catalyst metal particles contained in the mesoporous carbon cannot penetrate into the mesopores with a radius of 1 to 10 nm and are not poisoned by ionomers.

[0046] However, it was found that some ionomers actually sometimes penetrate into the mesopores. In addition, since ionomers are easily adsorbed on Pt particles, ionomers that penetrate into the mesopores are adsorbed on the Pt particles supported inside the mesoporous carbon close to the surface, reducing their catalytic activity.

[0047] Therefore, it is considered that even inside the mesoporous carbon, the Pt particles supported on the portion close to the surface of the mesoporous carbon are poisoned by the ionomer. Figure 1 Schematic diagram showing an example of the electrode catalyst of the present disclosure and the electrode catalyst of the comparative example. Specifically, Figure 1 The left side of is a schematic diagram showing an example of the electrode catalyst disclosed in the present invention, Figure 1 The right side of is a schematic diagram showing an example of an electrode catalyst of a comparative example. Figure 1 In FIG. 1 , white circles represent catalyst metal particles 3 that are not affected by poisoning caused by ionomer 4, and black circles represent catalyst metal particles 3 that are affected by poisoning caused by ionomer 4. In addition, a circle indicated by a solid line including black circles and white circles represents mesoporous carbon 1. Figure 1 In FIG. 1 , the region from the surface of the mesoporous carbon to the dotted line portion represents the first region 5, and the inner side of the mesoporous carbon than the dotted line portion represents the second region 6. Figure 1 As shown, in the electrode catalyst of the present disclosure loaded with the ionomer 4, the number density of the catalyst metal particles 3 loaded in the mesopores 2 present in the first region 5 of the mesoporous carbon 1 is smaller than the number density of the catalyst metal particles 3 loaded in the second region 6. In the comparative example, the number density of the catalyst metal particles 3 loaded in the first region of the mesopores 2 of the mesoporous carbon is greater than the number density of the catalyst metal particles 3 loaded in the second region.

[0048] That is, Figure 1 As shown, it is considered that the electrode catalyst of the present disclosure carrying the ionomer 4 has a lower ratio of the catalyst metal poisoned by the ionomer 4 and a higher catalytic activity than the comparative example.

[0049] Here, the electrode catalyst of the electrochemical device involved in the first embodiment of the present disclosure comprises a mesoporous material and a catalyst metal particle supported at least inside the mesoporous material, wherein the mesoporous material has mesopores, and before the catalyst metal particle is supported, the mode radius of the mesopores is 1 to 25 nm, and the pore volume is 1.0 to 3.0 cm 3 / g, and the number density of the catalytic metal particles supported in the mesopores is smaller on the outside of the mesoporous material than on the inside of the mesoporous material.

[0050] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0051] Here, the electrode catalyst for an electrochemical device according to the first aspect of the present disclosure is an electrode catalyst for an electrochemical device before the ionomer is supported.

[0052] In addition, if the number density of the catalyst metal particles supported in the mesopores is less than that in the inner side of the mesoporous material, it is not limited to the second mode described later, and any mode may be used. For example, the number density of the catalyst metal particles supported in the mesopores may be gradually reduced from the inner side to the outer side of the mesoporous material. The gradual reduction includes, for example, a staged reduction in three or more stages.

[0053] In addition, in the electrode catalyst of the electrochemical device involved in the second embodiment of the present disclosure, the number density of the catalyst metal particles carried by the mesopores existing in the first region, a predetermined region from the surface to the inside of the mesoporous material, is smaller than the number density of the catalyst metal particles carried by the mesopores existing in the second region which is closer to the inside than the first region.

[0054] Here, the first region does not include the surface of the mesoporous carbon. In addition, the predetermined region may include a region where the ionomer invades the interior (mesopores). The predetermined region may include, for example, a region 40 nm from the surface of the mesoporous carbon. If the second region is a region that is closer to the inside than the first region, it may be any region. For example, the second region may be a region that is closer to the inside than the first region and excluding the first region. At this time, even if the number density of the catalyst metal particles supported on the mesopores in a part of the second region is less than the number density supported by the mesopores present in the first region, as long as the second region as a whole (for example, as an average value) is greater than the number density supported by the mesopores present in the first region, it is also included in the above-mentioned second method.

[0055] Furthermore, the electrode catalyst for an electrochemical device according to a third aspect of the present disclosure is the electrode catalyst for an electrochemical device according to the second aspect, wherein the catalytic metal particles are supported at a number density of mesopores in the first region that is 6% or more less than that of mesopores in the second region.

[0056] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0057] In addition, the electrode catalyst for an electrochemical device according to a fourth aspect of the present disclosure may be the electrode catalyst for an electrochemical device according to any one of the first to third aspects, wherein the average particle size of the mesoporous material is 200 nm or more.

[0058] According to this structure, the area where the ionomer intrudes into the mesopores becomes smaller relative to the pore volume of the mesopores, so the proportion of the catalyst metal affected by the poisoning caused by the ionomer becomes smaller. Therefore, it can be considered that by making the average particle size greater than 200 nm, the catalytic activity can be improved even compared with, for example, the conventional electrode catalyst layer.

[0059] In addition, the electrode catalyst for an electrochemical device according to a fifth aspect of the present disclosure may be: in the electrode catalyst for an electrochemical device according to any one of the first aspect to the fourth aspect, the mode radius of the mesopores is 3 to 6 nm.

[0060] According to this structure, when the mode radius of the mesopores is 3 nm or more, the gas can be easily supplied into the pores, and when it is 6 nm or less, the ionomer cannot easily penetrate into the pores.

[0061] Furthermore, an electrode catalyst layer of an electrochemical device according to a sixth aspect of the present disclosure includes the electrode catalyst of the electrochemical device according to any one of the first aspect to the fifth aspect and an ionomer.

[0062] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0063] Furthermore, the electrode catalyst layer of the electrochemical device according to the seventh aspect of the present disclosure is the electrode catalyst layer of the electrochemical device according to the fourth aspect, further comprising at least one of carbon black and carbon nanotubes.

[0064] According to this structure, the water drainage property of the electrode catalyst layer is improved.

[0065] In addition, the electrode catalyst layer of the electrochemical device involved in the 8th mode of the present disclosure may be: in the electrode catalyst layer of the electrochemical device of the above-mentioned 6th mode or 7th mode, the above-mentioned mesoporous material includes mesoporous carbon, and the ratio of the weight of the above-mentioned ionomer contained in the above-mentioned electrode catalyst to the total weight of the carbon including the above-mentioned mesoporous carbon is 0.7 to 0.9.

[0066] In addition, the membrane electrode assembly of the electrochemical device involved in the 9th mode of the present disclosure comprises a polymer electrolyte membrane and a fuel electrode and an air electrode arranged on both sides of the above-mentioned polymer electrolyte membrane, and the above-mentioned fuel electrode and air electrode include an electrode catalyst layer and a gas diffusion layer, and at least the above-mentioned electrode catalyst layer of the above-mentioned air electrode includes the electrode catalyst layer of the electrochemical device described in any one of the above-mentioned 6th mode to 8th mode.

[0067] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0068] Furthermore, an electrochemical device according to a tenth aspect of the present disclosure includes the membrane electrode assembly of the electrochemical device according to the ninth aspect.

[0069] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0070] In addition, the method for producing an electrode catalyst for an electrochemical device according to the eleventh aspect of the present disclosure comprises the step of supporting catalyst metal particles in the mesopores of a mesoporous material having mesopores, wherein the mode radius of the mesopores is 1 to 25 nm and the pore volume is 1.0 to 3.0 cm 3 / g, and in the above step, the number density of the catalytic metal particles supported in the above mesopores is smaller on the outside of the above mesoporous material than on the inside of the above mesoporous material.

[0071] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0072] Here, the method for producing an electrode catalyst for an electrochemical device according to the eleventh aspect of the present disclosure is a method for producing an electrode catalyst before the ionomer is supported.

[0073] In addition, the method for manufacturing an electrode catalyst for an electrochemical device involved in the 12th embodiment of the present disclosure may be: in the method for manufacturing an electrode catalyst for an electrochemical device of the above-mentioned 11th embodiment, in the above-mentioned step, the number density of the above-mentioned catalyst metal particles supported by the above-mentioned mesopores existing in a predetermined area from the surface to the inside of the above-mentioned mesoporous material, i.e., the first area, is smaller than the number density of the above-mentioned catalyst metal particles supported by the above-mentioned mesopores existing in a second area inside the above-mentioned first area.

[0074] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0075] In addition, the manufacturing method of the electrode catalyst of the electrochemical device involved in the 13th embodiment of the present disclosure is: in the manufacturing method of the electrode catalyst of the electrochemical device of the above-mentioned 12th embodiment, the above-mentioned catalyst metal particles are supported with a number density of mesopores in the above-mentioned first region being 6% or more less than the mesopores in the above-mentioned second region.

[0076] According to this structure, poisoning of the catalyst metal by the ionomer is further suppressed compared with the related art.

[0077] In addition, the method for producing an electrode catalyst for an electrochemical device according to a fourteenth aspect of the present disclosure may be such that, in the method for producing an electrode catalyst for an electrochemical device according to any one of the eleventh to thirteenth aspects, the average particle size of the mesoporous material is 200 nm or more.

[0078] According to this structure, the area where the ionomer intrudes into the mesopores becomes smaller relative to the pore volume of the mesopores, so the proportion of the catalyst metal affected by the poisoning caused by the ionomer becomes smaller. Therefore, it can be considered that by making the average particle size greater than 200 nm, the catalytic activity can be improved even compared with, for example, the conventional electrode catalyst layer.

[0079] In addition, the method for producing an electrode catalyst for an electrochemical device according to a fifteenth aspect of the present disclosure may be such that, in the method for producing an electrode catalyst for an electrochemical device according to any one of the eleventh to fourteenth aspects, the mode radius of the mesopores is 3 to 6 nm.

[0080] According to this structure, when the mode radius of the mesopores is 3 nm or more, the gas can be easily supplied into the pores, and when it is 6 nm or less, the ionomer cannot easily penetrate into the pores.

[0081] In addition, the method for manufacturing a membrane electrode assembly of an electrochemical device according to the 16th embodiment of the present disclosure comprises: a step of loading catalyst metal particles in the mesopores of a mesoporous material having mesopores in such a manner that the number density on the outside of the mesoporous material is smaller than the number density on the inside of the mesoporous material, wherein the mode radius of the mesopores is 1 to 25 nm and the pore volume is 1.0 to 3.0 cm 3 / g; a step of supporting an ionomer in the mesoporous material supporting the catalyst metal particles; and a step of providing an electrode catalyst layer comprising a mesoporous material supporting the catalyst metal particles and the ionomer on the electrolyte membrane.

[0082] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0083] In addition, the manufacturing method of the membrane electrode assembly of the electrochemical device involved in the 17th embodiment of the present disclosure is: in the manufacturing method of the membrane electrode assembly of the electrochemical device of the above-mentioned 16th embodiment, in the process of supporting the above-mentioned catalyst metal particles, the number density of the above-mentioned catalyst metal particles supported by the above-mentioned mesopores existing in the predetermined area from the surface to the inside of the above-mentioned mesoporous material, i.e., the first area, is smaller than the number density of the above-mentioned catalyst metal particles supported by the above-mentioned mesopores existing in the second area inside the above-mentioned first area.

[0084] According to this structure, poisoning of the catalyst metal by the ionomer is suppressed as compared with the related art.

[0085] In addition, the manufacturing method of the membrane electrode assembly of the electrochemical device involved in the 18th embodiment of the present disclosure is: in the manufacturing method of the membrane electrode assembly of the electrochemical device of the above-mentioned 17th embodiment, the above-mentioned catalyst metal particles are loaded with a number density of mesopores in the above-mentioned first region that is 6% or more less than the mesopores in the above-mentioned second region.

[0086] According to this structure, poisoning of the catalyst metal by the ionomer is further suppressed compared with the related art.

[0087] In addition, the method for producing a membrane electrode assembly for an electrochemical device according to the 19th aspect of the present disclosure may be: in the method for producing a membrane electrode assembly for an electrochemical device according to any one of the 16th to 18th aspects, the average particle size of the mesoporous material is 200 nm or more.

[0088] According to this structure, the area where the ionomer intrudes into the mesopores becomes smaller relative to the pore volume of the mesopores, so the proportion of the catalyst metal affected by the poisoning caused by the ionomer becomes smaller. Therefore, it can be considered that by making the average particle size greater than 200 nm, the catalytic activity can be improved even compared with, for example, the conventional electrode catalyst layer.

[0089] In addition, the method for producing a membrane electrode assembly for an electrochemical device according to aspect 20 of the present disclosure may be: in the method for producing a membrane electrode assembly for an electrochemical device according to any one of aspects 16 to 19, the mode radius of the mesopores is 3 to 6 nm.

[0090] According to this structure, when the mode radius of the mesopores is 3 nm or more, the gas can be easily supplied into the pores, and when it is 6 nm or less, the ionomer cannot easily penetrate into the pores.

[0091] Hereinafter, the embodiments of the present disclosure will be described with reference to the drawings. In addition, in the following, the same reference numerals are given to the same or corresponding components in all the drawings, and the description thereof may be omitted.

[0092] [Implementation Method]

[0093] Although a fuel cell is described as an example of the electrochemical device according to the embodiment of the present disclosure, the electrochemical device is not limited to the fuel cell, and may be a water electrolysis device that electrolyzes water to produce hydrogen and oxygen.

[0094] (Membrane Electrode Assembly)

[0095] First, refer to Figure 2 The structure of a membrane electrode assembly (MEA) 10 included in the electrochemical device according to the present disclosure will be described. Figure 2 It is a schematic diagram showing a schematic configuration example of a membrane electrode assembly (MEA) 10 included in the electrochemical device according to the embodiment of the present disclosure.

[0096] like Figure 3As shown in FIG. 1 , the membrane electrode assembly (MEA) 10 includes a polymer electrolyte membrane 11 and a fuel electrode (anode) and an air electrode (cathode) including an electrode catalyst layer 12 and a gas diffusion layer 13, and has a structure in which the polymer electrolyte membrane 11 is sandwiched between the fuel electrode and the air electrode. Figure 3 As shown, a pair of electrode catalyst layers 12 are formed on both sides of a polymer electrolyte membrane 11, and a pair of gas diffusion layers 13 are arranged so as to sandwich the pair of electrode catalyst layers 12.

[0097] (Polymer Electrolyte Membrane)

[0098] The polymer electrolyte membrane 11 is a membrane for ion (proton) conduction between the air electrode and the fuel electrode. The polymer electrolyte membrane 11 that needs to have both proton conductivity and gas barrier properties can be exemplified by ion exchange fluorine resin membranes or ion exchange hydrocarbon resin membranes. Among them, the perfluorosulfonic acid resin membrane is preferred because it has high proton conductivity and exists stably even in a power generation environment such as a fuel cell. The ion exchange capacity of the ion exchange resin is preferably 0.9 or more and 2.0 or less milliequivalents / g of dry resin. If the ion exchange capacity is 0.9 milliequivalents / g of dry resin or more, high proton conductivity is easily obtained. If the ion exchange capacity is 2.0 milliequivalents / g of dry resin or less, the swelling of the resin caused by water is suppressed, and the dimensional change of the polymer electrolyte membrane 11 is suppressed, so it is preferred. In addition, the film thickness of the polymer electrolyte membrane 11 is preferably 5 μm or more and 50 μm or less. If the film thickness is 5 μm or more, high gas barrier properties can be obtained, and if it is 50 μm or less, high proton conductivity can be obtained.

[0099] (Gas Diffusion Layer)

[0100] The gas diffusion layer 13 is a layer having both current collecting function, gas permeability and water repellency. Figure 2 As shown, it can be a structure including two layers of a substrate 13a and a coating layer 13b. The substrate 13a can be a material with excellent conductivity and gas and liquid permeability, and examples thereof include porous materials such as carbon paper, carbon fiber cloth, and carbon fiber felt. The coating layer 13b is a layer that exists between the substrate 13a and the electrode catalyst layer 12 and is used to reduce their contact resistance and improve liquid permeability (drainage). As the coating layer 13b, a conductive material such as carbon black and a water-repellent resin such as polytetrafluoroethylene (PTFE) are formed as the main components.

[0101] (Electrode Catalyst Layer)

[0102] The electrode catalyst layer 12 is a layer that promotes the electrochemical reaction rate of the electrode. The electrode catalyst layer 12 becomes a structure that includes mesoporous carbon, catalyst metal particles and ionomers (proton conductive resins), and the catalyst metal particles are at least supported on the inside of the mesoporous carbon. Furthermore, in the embodiment of the present disclosure, as a mesoporous material used in the electrode catalyst layer 12, mesoporous carbon is cited as an example for illustration, but the mesoporous material is not limited to the mesoporous carbon. As long as the mode radius and / or pore volume are the same, other mesoporous materials may also be used. As mesoporous materials other than mesoporous carbon, for example, mesoporous materials composed of oxides of titanium, tin, niobium, tantalum, zirconium, aluminum, silicon, etc. can be cited.

[0103] The mesoporous carbon according to the embodiment of the present disclosure may have a mesopore mode radius of 1 to 25 nm and a mesopore pore volume of 1.0 to 3.0 cm before supporting the catalytic metal particles. 3 / g. If the pore volume of the mesopore is 1.0cm 3 / g or more, a large amount of catalyst metal can be supported inside the mesoporous carbon. 3 / g or less, the strength of the structure as the mesoporous carbon is improved.

[0104] Furthermore, in the mesoporous carbon involved in the embodiment of the present disclosure, the mode radius of the mesopores can be set to 3 to 6 nm. In particular, the mode radius of the mesopores can be set to 3 to 4 nm. If the mode radius of the mesopores is greater than 3 nm, it is easy to supply gas into the pores, and if it is less than 6 nm, it is difficult for the ionomer to penetrate into the pores.

[0105] Furthermore, the mesoporous carbon involved in the embodiment of the present disclosure can be configured to have an average particle size of 200 to 1000 nm. If the average particle size is greater than 200 nm, the area where the ionomer intrudes into the mesopores becomes smaller relative to the pore volume of the mesopores, and thus the proportion of the catalyst metal affected by the poisoning caused by the ionomer becomes smaller. Therefore, it can be considered that by making the average particle size greater than 200 nm, the catalytic activity can be improved even compared with, for example, a conventional electrode catalyst layer.

[0106] In addition, if the average particle size is 1000 nm or less, it is easy to supply the reaction gas to the catalyst metal particles supported inside the mesoporous carbon. Furthermore, as described later, if the average particle size is 800 nm or less, it is possible to supply the catalyst metal particles with the same or more oxygen than the conventional electrode catalyst.

[0107] Furthermore, the pore volume and mode radius of the mesopores contained in the above-mentioned mesoporous carbon can be measured by nitrogen adsorption method, and then analyzed by Barrett-Joyner-Halenda (BJH) method, density functional theory (DFT) method, quenched fixed density functional theory (QSDFT) method and other methods.

[0108] In addition, the average particle size of the mesoporous carbon can be measured by using a laser diffraction particle size distribution measuring device, etc., when the mesoporous carbon is dispersed in a solvent, or by using a scanning electron microscope (SEM) or a transmission electron microscope (TEM) for observation. In the case where the mesoporous carbon is dispersed in a solvent and the particle size distribution is measured, it is necessary not to cause the mesoporous carbon to condense with each other. For this reason, the solvent can be suitable for using water, alcohol or a mixed solvent of water and alcohol. In order to further improve the dispersibility, a dispersant is preferably added to the solvent. As a dispersant, for example, perfluorosulfonic acid resin, poly (ethylene oxide) octylphenyl ether, polyoxyethylene sorbitan monolaurate, etc. can be cited. In order to further improve the dispersibility, it is preferred that a dispersion treatment is implemented after the solvent and the mesoporous carbon are mixed. As a dispersion treatment device, for example, an ultrasonic homogenizer, a wet jet mill, a ball mill, a mechanical stirring device, etc. can be cited.

[0109] The method for producing the mesoporous carbon included in the electrode catalyst layer 12 according to the embodiment of the present disclosure is not particularly limited, and for example, the method described in Patent Document 3 can be suitably used. The mesoporous carbon produced by such a method has a structure in which the pore volume of the mesopores is large and the mesopores are interconnected.

[0110] Therefore, it is easy to load catalyst metal particles in the pores, and it is easy to supply gas to the supported catalyst metal particles. In addition, in order to adjust the average particle size of the mesoporous carbon, a pulverization process can be performed after synthesis. As a pulverization method, wet bead mill, dry bead mill, wet ball mill, dry ball mill, wet jet mill, dry jet mill, etc. can be exemplified. Wherein, when using a wet bead mill, it is easy to be crushed to a fine particle size, so it is suitable.

[0111] As the catalyst metal contained in the electrode catalyst layer 12, platinum (Pt), ruthenium (Ru), palladium (Pd), iridium (Ir), silver (Ag) and gold (Au) can be exemplified. Platinum and its alloys are suitable because of their high catalytic activity for oxygen reduction reaction and good durability in the power generation environment of fuel cells. In addition, the catalyst metal can be in the form of particles. The average particle size of the catalyst metal can be, for example, greater than 1 nm and less than 20 nm, and further can be greater than 1 nm and less than 10 nm. When the average particle size of the catalyst metal particles is less than 10 nm, the surface area per unit weight of the catalyst metal becomes larger and the reactivity is improved. In addition, if the average particle size of the catalyst metal particles is greater than 1 nm, the stability of the particles is improved, and the metal is not easily melted in, for example, the power generation environment of a fuel cell.

[0112] In addition, the weight ratio of the weight of the catalyst metal to the weight of the mesoporous carbon may be 0.65 to 1.5. If the amount of catalyst metal per unit area of ​​the mesoporous carbon increases, deviating from the range of the weight ratio and causing the weight ratio of the catalyst metal to increase, it may cause the catalyst metal particles to aggregate. On the contrary, if the amount of catalyst metal per unit area of ​​the mesoporous carbon is small, deviating from the range of the weight ratio and causing the weight ratio of the catalyst metal to decrease, the amount of mesoporous carbon increases in order to ensure the required amount of catalyst metal, resulting in a thicker thickness of the electrode catalyst layer 12.

[0113] As an ionomer (proton conductive resin), an ion exchange resin can be used. Among them, perfluorosulfonic acid resin is suitable because it has high proton conductivity and exists stably even in the power generation environment of the fuel cell. The ion exchange capacity of the ion exchange resin can be set to be greater than 0.9 and less than 2.0 milliequivalents / g dry resin. When the ion exchange capacity is greater than 0.9 milliequivalents / g dry resin, high proton conductivity is easily obtained. When the ion exchange capacity is less than 2.0 milliequivalents / g dry resin, the swelling of the resin caused by water is suppressed, and the gas diffusion in the electrode catalyst layer 12 is not easily hindered.

[0114] The weight ratio of the ionomer may be 0.7 to 0.9 with respect to the total weight of the carbon contained in the electrode catalyst layer 12. The carbon includes mesoporous carbon and may further include at least one of carbon black and carbon nanotubes described below.

[0115] In order to improve the drainage performance, carbon black and / or carbon nanotubes may be added to the electrode catalyst layer 12. At this time, the electrode catalyst layer, in which the carbon generally contains carbon particles with an average particle size of 10 to 100 nm, obtains high drainage performance by capillary force. However, the average particle size of the mesoporous carbon used in the electrode catalyst layer 12 involved in the embodiment of the present disclosure is greater than 200 nm, so sometimes there are problems with drainage performance. For this reason, a structure in which at least one of carbon black and carbon nanotubes is added to the electrode catalyst layer 12 may be provided. By configuring in this way, the drainage performance of the electrode catalyst layer 12 can be improved, thereby improving the power generation performance of the fuel cell.

[0116] Furthermore, examples of carbon black include Ketjen black, acetylene black, Vulcan black, and Black Pearls black. Examples of carbon nanotubes include single-layer carbon nanotubes and multilayer carbon nanotubes. Ketjen black is suitable because it can form an effective drainage path in the electrode catalyst layer 12 even with a small amount of addition, due to its well-developed linearity of aggregates.

[0117] As a method for forming the electrode catalyst layer 12 involved in the embodiment of the present disclosure, for example, a method generally used in a fuel cell can be used. For example, the above-mentioned material is dispersed in a solvent containing water or alcohol, applied to a substrate such as a polymer electrolyte membrane, a gas diffusion layer, and various transfer membranes, and dried to form the electrode catalyst layer 12. In addition, in an embodiment of the present disclosure, as a method for manufacturing an electrode catalyst layer 12 comprising mesoporous carbon, catalyst metal particles supported at least inside the mesoporous carbon, and ionomers, the following steps may be included. That is, it may include: preparing a pore volume of 1.0 to 3.0 cm having a mode radius of 1 to 25 nm and a pore volume of 1.0 to 3.0 cm 3 / g of mesoporous carbon and an average particle size of 200nm or more; a process of making a catalyst by loading catalyst metal particles inside the mesoporous carbon; a process of mixing materials containing a catalyst, a solvent and an ionomer to make a catalyst ink; and a process of coating the catalyst ink on a substrate.

[0118] Furthermore, the electrode catalyst layer 12 of the embodiment of the present disclosure having the above-mentioned structure can be used as an electrode catalyst layer on the air electrode (cathode) side. In addition, it can also be used as an electrode catalyst layer on the fuel electrode (anode) side. Alternatively, for the electrode catalyst layer on the fuel electrode side, it can be set to the same structure as the conventional electrode catalyst layer generally used in the membrane electrode assembly 10 of the fuel cell. That is, in the membrane electrode assembly 10, it is suitable to use the electrode catalyst layer 12 having the above-mentioned structure at least as the electrode catalyst layer on the air electrode side.

[0119] Furthermore, when the fuel electrode side electrode catalyst layer is set to the same structure as the conventional electrode catalyst layer, it can be formed in the following manner. For example, the platinum catalyst and perfluorosulfonic acid resin supported on carbon black can be dispersed in a solvent containing water and alcohol, and then coated on a substrate such as a polymer electrolyte membrane, a gas diffusion layer, and various transfer films and dried to form the electrode catalyst layer.

[0120] The membrane electrode assembly 10 according to the embodiment of the present disclosure can be obtained by integrating the polymer electrolyte membrane 11 , a pair of electrode catalyst layers 12 (cathode electrode catalyst layer, anode electrode catalyst layer) and a pair of gas diffusion layers 13 (cathode gas diffusion layer, anode gas diffusion layer).

[0121] In addition, if Figure 3 As shown, by Figure 2 The membrane electrode assembly 10 shown is sandwiched on both sides by a pair of separators 14 that also serve as a supply path for the reaction gas (hydrogen or oxygen), thereby forming a single cell 20. Then, the single cells 20 can be assembled to form, for example, a fuel cell stack. Figure 3 It means using Figure 2 FIG. 1 is a schematic diagram showing a configuration example of a single cell 20 of a fuel cell including a membrane electrode assembly 10 .

[0122] [Example]

[0123] Hereinafter, embodiments according to the present disclosure will be described.

[0124] (Preparation of Electrode Catalyst)

[0125] A commercially available mesoporous carbon (Toyo Tanso Co., Ltd., CNovel) with a designed pore diameter of 10 nm was placed in a mixed solvent containing equal amounts of water and ethanol to prepare a slurry with a solid content concentration of 1 wt%. Zirconia beads with a diameter of 0.5 mm were added to the slurry, and a medium-stirred wet bead mill (Ashizawa Finetech, LabStar Mini) was used to grind the beads for 20 minutes at a circumferential speed of 12 m / s. The zirconia beads were removed from the pulverized slurry, and after evaporating the solvent, the resulting aggregates were ground with a mortar to produce a carbon carrier.

[0126] 1 g of the obtained carbon carrier was put into 400 mL of a mixed solvent of water: ethanol = 1: 1 (weight ratio) and ultrasonically dispersed for 15 minutes. After dispersion, 14 wt% of dinitrodiamine platinum nitrate solution was added dropwise in a manner that the platinum was 50 wt% relative to the carbon carrier while stirring under a nitrogen atmosphere, and heated and stirred at 80°C for 6 hours. After natural cooling, it was filtered and washed, and dried at 80°C for 15 hours. The obtained agglomerate was crushed with a mortar and heat-treated for 2 hours at 220°C in an atmosphere of nitrogen: hydrogen = 85: 15, thereby preparing an electrode catalyst. Furthermore, the above-mentioned method for preparing the electrode catalyst is an example, and any method can be used as long as the number density of the platinum particles supported in the mesopores is less than that of the mesoporous carbon on the outside than the inside of the mesoporous carbon.

[0127] [Comparative Example]

[0128] Hereinafter, comparative examples according to the present disclosure will be described.

[0129] (Preparation of Electrode Catalyst)

[0130] An electrode catalyst of the comparative example was prepared in the same manner as the electrode catalyst of the example, except that the composition of the mixed solvent used when the Pt particles were supported on the carbon support was water:ethanol=3:1 (weight ratio).

[0131] [Evaluation of catalytic activity and electrochemically active surface area]

[0132] The catalytic activity and electrochemically active surface area of ​​the electrode catalysts of Examples and Comparative Examples were evaluated in the following procedures.

[0133] Ketjen black (Lion Specialty Chemicals Co., Ltd., EC300J) of 1 / 2 of the weight of the mesoporous carbon contained in the electrode catalyst was put into a mixed solvent containing equal amounts of water and ethanol and stirred. Ionomer (DuPont, Nafion) was put into the resulting slurry in a manner of 0.8 weight ratio relative to all carbon (mesoporous carbon + Ketjen black) and ultrasonic dispersion was performed. The catalyst ink thus obtained was applied to a polymer electrolyte membrane (Gore Co., Ltd., Gore-Select III) by spraying to prepare an electrode catalyst layer.

[0134] Next, the electrode catalyst layer is set as a cathode catalyst layer, and an anode catalyst layer is formed on the main surface of the polymer electrolyte membrane opposite to the main surface provided with the cathode catalyst layer.

[0135] The anode catalyst layer was prepared by the following method. First, a commercially available platinum-supported carbon black catalyst (Tanaka Precious Metals Co., Ltd., TEC10E50E) was added to a mixed solvent containing equal amounts of water and ethanol and stirred. An ionomer (DuPont, Nafion) was added to the resulting slurry in a weight ratio of 0.8 relative to carbon, and ultrasonic dispersion treatment was performed. The catalyst ink thus obtained was applied by spraying on the main surface opposite to the main surface of the polymer electrolyte membrane provided with the cathode catalyst layer, and the anode catalyst layer was prepared.

[0136] A gas diffusion layer (GDL25BC manufactured by SGLCARBON JAPAN Co., Ltd.) was placed on each of the cathode catalyst layer and the anode catalyst layer thus prepared, and a high temperature of 140° C. was applied for 5 minutes at 7 kgf / cm 2 of pressure, thereby producing a membrane electrode assembly.

[0137] The obtained membrane electrode assembly was sandwiched between separators provided with serpentine-shaped flow channels and attached to a predetermined jig, thereby manufacturing a fuel cell.

[0138] The temperature of the obtained fuel cell unit is maintained at 80°C, and hydrogen with a dew point of 80°C is flowed into the anode side at a flow rate sufficiently larger than the amount consumed by the electrochemical reaction (redox reaction) of the fuel cell, and oxygen with a dew point of 80°C is flowed into the cathode side. At this time, the voltages of the fuel cell unit in constant current operation were measured using an electronic load device (PLZ-664WA, manufactured by Kikusui Electronics Industry Co., Ltd.). In addition, during the measurement, the resistance of the unit was measured In-Situ using a low resistance meter with a fixed frequency of 1kHz. The current value at 0.9V is read from the current-voltage curve to which the correction of the resistance value of the unit is applied, and is normalized with the amount of platinum contained in the cathode catalyst layer, thereby setting it as an indicator of catalytic activity. This is called the mass activity at 0.9V, and is generally used as an indicator of the catalytic activity of the fuel cell.

[0139] Next, the temperature of the fuel cell unit was maintained at 80°C, hydrogen with a dew point of 80°C was supplied to the anode side, and nitrogen with a dew point of 80°C was supplied to the cathode side. The working electrode of a potentio / galvanostat (HZ-3000, Hokuto Denko Co., Ltd.) was connected to the cathode, and the counter electrode and reference electrode were connected to the anode. Cyclic voltammetry was used to measure the amount of electricity generated by hydrogen adsorption on Pt. The obtained amount of electricity was divided by the theoretical value of hydrogen adsorption per unit surface area of ​​Pt (0.21 mC / cm 2 ), from which the electrochemically active surface area was calculated.

[0140] [Pt internal inclusion evaluation]

[0141] The distribution of Pt particles in the mesoporous carbon of the cathode catalysts of Examples and Comparative Examples was evaluated in the following manner.

[0142] The membrane-catalyst layer assembly was processed using an argon broad ion beam, and the cross section of the cathode catalyst layer was observed using a scanning electron microscope (S-5500, Hitachi High-Technologies Corporation). Figure 4 and Figure 5 The following are cross-sectional SEM images of the cathode catalyst layer using the electrode catalyst of the embodiment and the comparative example, respectively. Figure 4 and Figure 5 As shown in FIG. 1 , the first region and the second region of the mesoporous carbon sliced ​​into a disk were observed at 400,000 times magnification, and the number of Pt particles contained in the field of view was visually counted. Figure 4 and Figure 5 Indicated by white dots in the figure. The first region is a predetermined region from the surface to the inside of the mesoporous carbon, and the second region is a region inside the first region. The first region does not include the surface of the mesoporous carbon.

[0143] The value obtained by dividing the number of Pt particles in the second region by the number of Pt particles in the first region is defined as the Pt inclusion degree. When the Pt inclusion degree exceeds 1, the number density of Pt particles in the second region of the mesoporous carbon is greater than that in the first region of the mesoporous carbon.

[0144] [Ionomer penetration evaluation]

[0145] The degree of ionomer penetration into the mesoporous carbon of the cathode catalyst layer of the example was evaluated according to the following procedure.

[0146] The membrane-catalyst layer assembly was kept in a low-temperature condensed state while being processed with a focused ion beam, and the cross section of the cathode catalyst layer was observed using a scanning transmission electron microscope (JEM-ARM200F, JEOL Ltd.) and an energy dispersive X-ray spectrometer (detector JED2300, JEOL Ltd.). In addition, in order to reduce the damage to the sample caused by electron beam irradiation, the electron microscope observation was performed in a low-temperature condensed state. In addition, the energy dispersive X-ray spectrometer observation was also performed in a low-temperature condensed state.

[0147] Figure 6 TABLE 1 is a table showing the performance and physical properties of cathode catalysts using various electrode catalysts of Examples and Comparative Examples. Figure 6As shown, the cathode catalyst of the embodiment shows a catalytic activity of about 1.3 times that of the cathode catalyst of the comparative example. On the other hand, the electrochemically active surface areas of the two are roughly the same, and the difference in catalytic activity cannot be explained based on the electrochemically active surface area. On the other hand, if we focus on the Pt inclusion degree, the cathode catalyst of the embodiment is about 1.3 times that of the cathode catalyst of the comparative example, which shows that there is a high correlation between the Pt inclusion degree and the catalytic activity.

[0148] Here, it is believed that the Pt inclusion degree of the embodiment is higher than that of the comparative example because the ethanol ratio of the mixed solvent used when the Pt particle is supported is large. The surface of the mesoporous carbon is substantially hydrophobic, and therefore the affinity with ethanol is higher than the affinity with water. Therefore, it can be considered that: the ethanol ratio of the solvent is higher, and the solvent is more likely to penetrate into the pores of the mesoporous carbon, and the Pt particle is supported on the carbon interior.

[0149] Figure 7 It is a cross-sectional image obtained based on a scanning transmission electron microscope (STEM) and an elemental map based on energy dispersive X-ray spectroscopy of the cathode catalyst layer of the embodiment. Carbon and Pt were detected in both the first and second regions of the mesoporous carbon. On the other hand, fluorine from the ionomer was detected from the first region of the mesoporous carbon, while fluorine from the ionomer was basically not detected from the second region. Moreover, the results of high-magnification observation show that fluorine was strongly detected in the region of about 40nm from the surface of the mesoporous carbon. That is, it can be considered that the ionomer is immersed in the region of about 40nm from the surface of the mesoporous carbon, and the Pt particles contained in the region are poisoned by the catalyst. Therefore, it can be considered that the catalyst in which the number density of Pt particles carried on the outside of the mesoporous carbon is less than the number density of Pt particles carried on the inside of the mesoporous carbon shows high catalytic activity. In addition, based on the above results, the above-mentioned predetermined area of ​​the first region may include an area where the ionomer invades the interior (mesopores). For example, it can be an area including an area of ​​40nm from the surface of the mesoporous carbon.

[0150] Based on the above description, it is self-evident to those skilled in the art that numerous improvements and other embodiments of the present disclosure may be made. Therefore, the above description should be interpreted as merely illustrative and provided for the purpose of teaching those skilled in the art the best way to practice the present disclosure. The details of its structure and / or function may be substantially changed without departing from the spirit of the present disclosure.

[0151] Industrial Applicability

[0152] The present disclosure is useful in, for example, an electrode catalyst used in a membrane electrode assembly constituting a cell of a fuel cell.

Claims

1. An electrode catalyst for an electrochemical device, comprising a mesoporous material and catalyst metal particles supported at least inside the mesoporous material, The mesoporous material has mesopores. Before the catalyst metal particles are supported, the mesopores have a mode radius of 1 to 25 nm and a pore volume of 1.0 to 3.0 cm 3 / g, The number density of the catalyst metal particles supported in the mesopores is smaller on the outside of the mesoporous material than on the inside of the mesoporous material. The number density of the catalyst metal particles supported by the mesopores in a first region, which is a predetermined region from the surface to the inside of the mesoporous material, is smaller than the number density of the catalyst metal particles supported by the mesopores in a second region which is inside the first region. The first region is a region extending 40 nm from the surface of the mesoporous material toward the inside, but does not include the surface of the mesoporous material. 2 . The electrode catalyst for an electrochemical device according to claim 1 , wherein the catalytic metal particles are supported at a number density of mesopores in the first region that is 6% or more less than that of mesopores in the second region. 3 . The electrode catalyst for an electrochemical device according to claim 1 , wherein the average particle size of the mesoporous material is 200 nm or more. 4 . The electrode catalyst for an electrochemical device according to claim 1 , wherein the mode radius of the mesopores is 3 to 6 nm.

5. An electrode catalyst layer of an electrochemical device, comprising at least the electrode catalyst according to claim 1 and an ionomer. The electrode catalyst layer of the electrochemical device according to claim 5 , comprising at least one of carbon black and carbon nanotubes. 7 . The electrode catalyst layer of an electrochemical device according to claim 5 , wherein the mesoporous material comprises mesoporous carbon, and the ratio of the weight of the ionomer contained in the electrode catalyst to the total weight of carbon comprising the mesoporous carbon is 0.7 to 0.

9.

8. A membrane electrode assembly comprising a polymer electrolyte membrane and a fuel electrode and an air electrode, wherein the fuel electrode and the air electrode are arranged on both sides of the polymer electrolyte membrane and include an electrode catalyst layer and a gas diffusion layer. At least the electrode catalyst layer of the air electrode includes the electrode catalyst layer of the electrochemical device according to claim 5 . 9 . An electrochemical device comprising the membrane electrode assembly according to claim 8 .

10. A method for producing an electrode catalyst for an electrochemical device, comprising the step of supporting catalyst metal particles in the mesopores of a mesoporous material having mesopores, wherein the mode radius of the mesopores is 1 to 25 nm and the pore volume is 1.0 to 3.0 cm 3 / g, In the step, the number density of the catalyst metal particles supported in the mesopores is smaller on the outside of the mesoporous material than on the inside of the mesoporous material. In the process, the number density of the catalyst metal particles supported by the mesopores existing in a predetermined region from the surface to the inside of the mesoporous material, i.e., a first region, is smaller than the number density of the catalyst metal particles supported by the mesopores existing in a second region inside the first region. The first region is a region extending 40 nm from the surface of the mesoporous material toward the inside, but does not include the surface of the mesoporous material. 11 . The method for producing an electrode catalyst for an electrochemical device according to claim 10 , wherein the catalytic metal particles are supported at a number density of mesopores in the first region that is 6% or more less than that of mesopores in the second region. 12 . The method for producing an electrode catalyst for an electrochemical device according to claim 10 , wherein the average particle size of the mesoporous material is 200 nm or more. 13 . The method for producing an electrode catalyst for an electrochemical device according to claim 10 , wherein the mode radius of the mesopores is 3 to 6 nm.

14. A method for manufacturing a membrane electrode assembly of an electrochemical device, comprising: A step of loading the catalyst metal particles in the mesopores of a mesoporous material having mesopores, wherein the number density of the catalyst metal particles is smaller on the outside of the mesoporous material than on the inside of the mesoporous material, wherein the mode radius of the mesopores is 1 to 25 nm and the pore volume is 1.0 to 3.0 cm 3 / g; a step of causing the mesoporous material carrying the catalyst metal particles to carry an ionomer; and a step of providing an electrode catalyst layer including a mesoporous material carrying the catalyst metal particles and the ionomer on an electrolyte membrane, In the step of supporting the catalyst metal particles, the number density of the catalyst metal particles supported by the mesopores existing in a predetermined region from the surface to the inside of the mesoporous material, i.e., a first region, is smaller than the number density of the catalyst metal particles supported by the mesopores existing in a second region inside the first region. The first region is a region extending 40 nm from the surface of the mesoporous material toward the inside, but does not include the surface of the mesoporous material. 15 . The method for producing a membrane electrode assembly according to claim 14 , wherein the catalytic metal particles are supported at a number density of mesopores in the first region that is 6% or more less than that of mesopores in the second region. 16 . The method for producing a membrane electrode assembly according to claim 14 , wherein the average particle size of the mesoporous material is 200 nm or more. 17 . The method for producing a membrane electrode assembly according to claim 14 , wherein the mode radius of the mesopores is 3 to 6 nm.

Citation Information

Patent Citations

  • Electrode and fuel cell electrode catalyst layer containing same

    WO2014175106A1

  • Electrode for fuel cell and method for manufacturing same

    WO2014185498A1

  • Ordered carbon carried fuel batter with proton exchange film catalyzer and method of manufacturing the same

    CN101108342A

  • Electrode catalyst layer for fuel cells, electrode for fuel cells, membrane electrode assembly for fuel cells, and fuel cell

    CN103765643A

  • Electrode and fuel cell electrode catalyst layer containing same

    CN105163849A