Stainless steel belt and processing technology

By designing stainless steel strips with fixed components, matte layers and anti-corrosion layers, the problems of complex processing technology and insufficient friction resistance of traditional stainless steel strips are solved, and automated winding and surface neatness are achieved, reducing costs.

CN111076078BActive Publication Date: 2025-03-18FUJIAN YONGJIN METAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201911218964.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-03
Publication Date
2025-03-18
Estimated Expiration
2039-12-03

AI Technical Summary

Technical Problem

The traditional stainless steel belt has complex processing technology and is troublesome to operate. The processed products lack friction resistance, the surface is not neat, it is inconvenient to wind and is easy to loosen, and the material and processing time cost is high.

Method used

A stainless steel belt is designed, adopting a structure including a fixing assembly, a matte layer and an anti-corrosion layer. The fixing assembly consists of multiple components that can be automatically coiled and fixed, and the surface is coated with a mixture of sulfurized fatty acids and extreme pressure anti-wear agents to improve friction resistance.

Benefits of technology

It realizes simple operation of stainless steel strips, automatic winding, improves friction resistance and surface neatness, and reduces the cost of material and processing time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111076078B_ABST
    Figure CN111076078B_ABST
Patent Text Reader

Abstract

The invention discloses a stainless steel belt and a processing technology, comprising a stainless steel belt body, a fixing component, a frosted layer and an anti-corrosion layer, wherein fixing components are installed on both sides of one end of the stainless steel belt body, fixing plates are welded on both sides of one end of the stainless steel belt body, a baffle is welded on the bottom of one end of the fixing plate, a threaded hole is opened at the center of the bottom of the baffle, a threaded column is sleeved inside the threaded hole, a first self-locking nut is sleeved on one end of the threaded column, and the first self-locking nut is located on one side of the baffle, a second self-locking nut is sleeved on the other end of the threaded column, and the second self-locking nut is located on the other side of the baffle, an L-shaped clamping plate is welded on the other end of the threaded column, and the L-shaped clamping plate is located on one side of the second self-locking nut. The stainless steel belt and the processing technology are simple and easy to operate, and the friction resistance of the stainless steel belt is greatly improved. Graphite can smooth out the potholes on the surface of the stainless steel belt, which is conducive to the neatness and beauty of the surface of the stainless steel belt.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of stainless steel strips, in particular to a stainless steel strip and a processing technology. Background Art

[0002] Stainless steel strip is simply an extension of ultra-thin stainless steel plate. It is a narrow and long steel plate produced mainly to meet the needs of industrial production of various metal or mechanical products in different industrial sectors. The traditional stainless steel strip processing technology is complicated and the operation is troublesome. The processed stainless steel strip does not have friction resistance and is easily damaged by friction. The processed stainless steel strip has potholes on the surface, which is not conducive to the neatness and beauty of the stainless steel strip surface. At the same time, the traditional process uses expensive materials and slow processing, which is not conducive to saving costs and time. The stainless steel strip after processing needs to be manually assisted to be rolled up, and there is no fixing measure. The rolling is extremely easy to slide loose, which is not conducive to user use. In view of these defects, it is necessary to design a stainless steel strip and processing technology. Summary of the invention

[0003] The object of the present invention is to provide a stainless steel strip and a processing technology to solve the problems raised in the above background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a stainless steel belt, comprising a stainless steel belt body, a fixing component, a frosted layer and an anti-corrosion layer, wherein fixing components are installed on both sides of one end of the stainless steel belt body, and the fixing component is composed of a baffle, a threaded column, a first self-locking nut, a threaded hole, a baffle, a second self-locking nut, a slide rail, an L-shaped card plate, a spring sleeve, a compression spring, a splint, an anti-slip pad, a fixing plate, a slideway, a slide rod and a slide block, fixing plates are welded on both sides of one end of the stainless steel belt body, a baffle is welded on the bottom of one end of the fixing plate, a threaded hole is opened at the center of the bottom of the baffle, a threaded column is sleeved inside the threaded hole, and a first Self-locking nut, and the first self-locking nut is located on one side of the baffle, the other end of the threaded column is sleeved with a second self-locking nut, and the second self-locking nut is located on the other side of the baffle, the other end of the threaded column is welded with an L-shaped clamping plate, and the L-shaped clamping plate is located on one side of the second self-locking nut, a slide rail is welded at the bottom of the fixed plate, a slide rail is provided at the bottom of the slide rail, a slider is sleeved inside the slide rail, a slide rod is welded at the bottom of the slider, and the bottom of the slide rod is connected to the top of the L-shaped clamping plate, a splint is provided on one side of the inner wall of the L-shaped clamping plate, one end of the splint and one end of the inner wall of the L-shaped clamping plate are welded with a plurality of spring sleeves, a compression spring is sleeved inside the spring sleeve, and the compression spring is located at the center of the L-shaped clamping plate and the splint.

[0005] A stainless steel strip processing technology, comprising step 1, selecting materials; step 2, rolling the steel strip; step 3, process lubrication; step 4, annealing the steel strip; step 5, flattening and fine cutting; step 6, coiling and packaging;

[0006] In the above step 1, selecting materials includes the following steps:

[0007] 1) Manually select suitable stainless steel strip materials to ensure that the thickness of the stainless steel strip is uniform and there are no obvious cracks on the surface;

[0008] 2) Place the stainless steel strip in a material storage bucket and add a certain amount of sulfuric acid aqueous solution for pickling until the surface of the stainless steel strip turns silvery white;

[0009] In the above step 2, the steel strip rolling includes the following steps:

[0010] 1) Hot rolling: The pickled stainless steel strip is manually placed in a hot rolling mill, the temperature is increased, and the hot rolling mill is used for rolling until the stainless steel strip is in a certain shape;

[0011] 2) Cold rolling: The hot-rolled stainless steel strip is cooled manually, and after cooling, it is put into a stamping machine for rolling until the stainless steel strip is in a certain shape and welded with fixed components;

[0012] In the above step 3, the process lubrication includes the following steps:

[0013] 1) The rolled stainless steel strip is manually laid out and stored in a cool place, and the surface is manually moistened with water to ensure that the surface of the stainless steel strip is moist;

[0014] 2) Mix the sulfided fatty acid and extreme pressure anti-wear agent, add a small amount of graphite and stir evenly;

[0015] 3) Use a brush to apply the mixture in 2) to the surface of the stainless steel strip three times in a row to ensure that the surface of the stainless steel strip is evenly coated;

[0016] In the above step 4, the stainless steel strip is manually leveled and placed in a bright annealing furnace for annealing for 1-2 hours, and both sides are annealed continuously until the surface of the stainless steel strip is bright;

[0017] In the above step 5, the annealed stainless steel strip is manually placed in a shearing machine, the shearing length is set, and the shearing machine performs flat shearing, and after shearing, the strip is stored in a cool place in the factory;

[0018] In the above step 6, the stainless steel strip cut in step 5 is manually rolled to ensure that each roll has the same length, and then packed into boxes.

[0019] According to the above technical solution, a frosted layer is provided on the surface of the stainless steel belt body, and an anti-corrosion layer is provided on the surface of the frosted layer.

[0020] According to the above technical solution, a baffle is welded to one end of the threaded column, and the baffle is located on one side of the first self-locking nut.

[0021] According to the above technical solution, an anti-skid pad is bonded to one end of the splint, and the thickness of the anti-skid pad is 2 mm.

[0022] According to the above technical solution, a spring hole groove is opened at the center of the spring sleeve, and the spring groove is sleeved on the outside of the compression spring.

[0023] According to the above technical solution, in step 12), the aqueous sulfuric acid solution flows over the surface of the stainless steel strip.

[0024] According to the above technical solution, the annealing temperature in step 4 is 100-200°C.

[0025] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0026] 1. The stainless steel belt and processing technology have a simple structure and are easy to operate. By screwing the first self-locking nut and the second self-locking nut, the clamping plate clamps the outside of the winding drum, and no manual assistance is required for winding. This prevents the stainless steel belt body from sliding and being difficult to wind when winding the stainless steel belt body. The winding is tighter and will not be loose, which is convenient for users to wind the stainless steel belt body. At the same time, it is easy to install and disassemble, which is conducive to users taking the stainless steel belt body.

[0027] 2. The stainless steel belt and processing technology have a simple structure and are easy to operate. When the outside world hits the stainless steel belt body, the stainless steel belt body shakes and drives the baffle to shake. The baffle squeezes the L-shaped card plate, and the L-shaped card plate squeezes the compression spring. The compression spring provides elastic force to offset the impact force caused by the shaking, protects the stainless steel belt body, avoids the shaking of the stainless steel belt body and the friction damage with the outer side of the winding drum, prolongs the service life of the winding drum, and saves resources.

[0028] 3. The stainless steel belt and its processing technology are simple and easy to operate. Sulfurized fatty acid and extreme pressure anti-wear agent are mixed and stirred, and a small amount of graphite is added and applied to the surface of the stainless steel belt for process lubrication, which greatly improves the anti-friction force of the stainless steel belt. At the same time, graphite can smooth the potholes on the surface of the stainless steel belt, which is conducive to the cleanliness and beauty of the surface of the stainless steel belt. In addition, the process uses low-priced materials and fast processing, which is conducive to saving costs and time. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0030] Figure 1 It is a three-dimensional diagram of the overall structure of the present invention;

[0031] Figure 2 is a cross-sectional view of the overall structure of the present invention;

[0032] Figure 3 is a schematic structural diagram of a fixing assembly of the present invention;

[0033] Figure 4 is a structural sectional view of the slide rail of the present invention;

[0034] Figure 5 is a structural cross-sectional view of the stainless steel strip body of the present invention;

[0035] Figure 6 is a system flow chart of the present invention;

[0036] In the figure: 1. Stainless steel belt body; 2. Fixing assembly; 3. Baffle; 4. Threaded column; 5. First self-locking nut; 6. Threaded hole; 7. Baffle; 8. Second self-locking nut; 9. Slide rail; 10. L-shaped clamp; 11. Spring sleeve; 12. Compression spring; 13. Clamp; 14. Anti-slip pad; 15. Fixing plate; 16. Slide; 17. Slide rod; 18. Sliding block; 19. Frosted layer; 20. Anti-corrosion layer. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] See also Figure 1-5The present invention provides a technical solution: a stainless steel belt, comprising a stainless steel belt body 1, a fixing component 2, a frosted layer 19 and an anti-corrosion layer 20, the surface of the stainless steel belt body 1 is provided with the frosted layer 19, and the surface of the frosted layer 19 is provided with the anti-corrosion layer 20, which is beneficial to protect the stainless steel belt body 1, and the fixing component 2 is installed on both sides of one end of the stainless steel belt body 1, and the fixing component 2 is composed of a baffle 3, a threaded column 4, a first self-locking nut 5, a threaded hole 6, a baffle 7, a second self-locking nut 8, a slide rail 9, and an L-shaped card plate 10 , a spring sleeve 11, a compression spring 12, a clamping plate 13, an anti-slip pad 14, a fixing plate 15, a slideway 16, a slide rod 17 and a slider 18. The stainless steel belt body 1 is welded with fixing plates 15 on both sides of one end, a baffle 7 is welded at the bottom of one end of the fixing plate 15, a threaded hole 6 is opened at the center of the bottom of the baffle 7, a threaded column 4 is sleeved inside the threaded hole 6, a first self-locking nut 5 is sleeved at one end of the threaded column 4, and the first self-locking nut 5 is located on one side of the baffle 7, a baffle plate 3 is welded at one end of the threaded column 4, and the baffle plate 3 is located One side of the first self-locking nut 5 is conducive to the fixation of the threaded column 4. The other end of the threaded column 4 is sleeved with a second self-locking nut 8, and the second self-locking nut 8 is located on the other side of the baffle 7. The other end of the threaded column 4 is welded with an L-shaped card plate 10, and the L-shaped card plate 10 is located on one side of the second self-locking nut 8. A slide rail 9 is welded at the bottom of the fixing plate 15, and a slideway 16 is provided at the bottom of the slide rail 9. A slider 18 is sleeved inside the slideway 16, and a slide rod 17 is welded at the bottom of the slider 18, and the bottom of the slide rod 17 is connected to the top of the L-shaped card plate 10. The L-shaped card A splint 13 is provided on one side of the inner wall of the plate 10, and an anti-slip pad 14 is bonded to one end of the splint 13, and the thickness of the anti-slip pad 14 is 2 mm, which is conducive to the fixation of the splint 13. Several spring sleeves 11 are welded on one end of the splint 13 and one end of the inner wall of the L-shaped clamping plate 10. A compression spring 12 is sleeved inside the spring sleeve 11, and the compression spring 12 is located at the center of the L-shaped clamping plate 10 and the splint 13. A spring hole groove is opened at the center of the spring sleeve 11, and the spring groove is sleeved on the outside of the compression spring 12, which is conducive to the fixation of the compression spring 12.

[0039] See also Figure 6 The present invention provides a technical solution: a stainless steel strip processing technology, including step one, selecting materials; step two, steel strip rolling; step three, process lubrication; step four, steel strip annealing; step five, flattening and precision cutting; step six, coiling and packaging;

[0040] In the above step 1, selecting materials includes the following steps:

[0041] 1) Manually select suitable stainless steel strip materials to ensure that the thickness of the stainless steel strip is uniform and there are no obvious cracks on the surface;

[0042] 2) Place the stainless steel strip in a material storage barrel and add a certain amount of sulfuric acid aqueous solution for pickling until the surface of the stainless steel strip turns silvery white and the sulfuric acid aqueous solution overflows the surface of the stainless steel strip;

[0043] In the above step 2, the steel strip rolling includes the following steps:

[0044] 1) Hot rolling: The pickled stainless steel strip is manually placed in a hot rolling mill, the temperature is increased, and the hot rolling mill is used for rolling until the stainless steel strip is in a certain shape;

[0045] 2) Cold rolling: The hot-rolled stainless steel strip is cooled manually, and after cooling, it is put into a stamping machine for rolling until the stainless steel strip is in a certain shape and welded with a fixing component 2;

[0046] In the above step 3, the process lubrication includes the following steps:

[0047] 1) The rolled stainless steel strip is manually laid out and stored in a cool place, and the surface is manually moistened with water to ensure that the surface of the stainless steel strip is moist;

[0048] 2) Mix the sulfided fatty acid and extreme pressure anti-wear agent, add a small amount of graphite and stir evenly;

[0049] 3) Use a brush to apply the mixture in 2) to the surface of the stainless steel strip three times in a row to ensure that the surface of the stainless steel strip is evenly coated;

[0050] In the above step 4, the stainless steel strip is manually leveled and placed in a bright annealing furnace for annealing for 1-2 hours, and both sides are continuously annealed until the surface of the stainless steel strip is bright, and the annealing temperature is 100-200°C;

[0051] In the above step 5, the annealed stainless steel strip is manually placed in a shearing machine, the shearing length is set, and the shearing machine performs flat shearing, and after shearing, the strip is stored in a cool place in the factory;

[0052] In the above step 6, the stainless steel strip cut in step 5 is manually rolled to ensure that each roll has the same length, and then packed into boxes.

[0053] Based on the above, the advantage of the present invention is that when the invention is used, the L-shaped card plate 10 at one end of the stainless steel strip body 1 is manually clamped on the outside of the winding drum, and the first self-locking nut 5 and the second self-locking nut 8 are rotated clockwise. The first self-locking nut 5 and the second self-locking nut 8 rotate to drive the threaded column 4 to move, and the threaded column 4 squeezes the L-shaped card plate 10. The L-shaped card plate 10 can slide inside the slide rail 9 using the slider 18. The L-shaped card plate 10 squeezes the compression spring 12, and the compression spring 12 squeezes the clamping plate 13. The clamping plate 13 clamps the outside of the winding drum to complete the fixation. At this time, the stainless steel strip body 1 can be rolled on the outside of the winding drum for winding; the stainless steel strip and the processing technology are simple and easy to operate. Sulfurized fatty acids and extreme pressure anti-wear agents are mixed and stirred, and a small amount of graphite is added and applied to the surface of the stainless steel strip for process lubrication, which greatly improves the friction resistance of the stainless steel strip. At the same time, graphite can smooth the potholes on the surface of the stainless steel strip.

[0054] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0055] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A stainless steel belt, comprising a stainless steel belt body (1), a fixing assembly (2), a frosted layer (19) and an anti-corrosion layer (20), characterized in that: A fixing assembly (2) is installed on both sides of one end of the stainless steel belt body (1), and the fixing assembly (2) is composed of a baffle (3), a threaded column (4), a first self-locking nut (5), a threaded hole (6), a baffle (7), a second self-locking nut (8), a slide rail (9), an L-shaped clamp (10), a spring sleeve (11), a compression spring (12), a clamp (13), an anti-slip pad (14), a fixing plate (15), a slideway (16), a slide rod (17) and a slider (18). A fixing plate (15) is welded on both sides of one end of the stainless steel belt body (1), a baffle (7) is welded on the bottom of one end of the fixing plate (15), a threaded hole (6) is opened at the center of the bottom of the baffle (7), a threaded column (4) is sleeved inside the threaded hole (6), one end of the threaded column (4) is sleeved with a first self-locking nut (5), and the first self-locking nut (5) is located on one side of the baffle (7), and the threaded column (4) is welded on one side of the baffle (7). ) is sleeved with a second self-locking nut (8) at the other end, and the second self-locking nut (8) is located on the other side of the baffle (7); an L-shaped card plate (10) is welded to the other end of the threaded column (4), and the L-shaped card plate (10) is located on one side of the second self-locking nut (8); a slide rail (9) is welded to the bottom of the fixing plate (15), a slideway (16) is provided at the bottom of the slide rail (9), a slider (18) is sleeved inside the slideway (16), and the slider (18) is ) is welded with a slide bar (17) at the bottom, and the bottom of the slide bar (17) is connected to the top of the L-shaped card plate (10), a clamping plate (13) is arranged on one side of the inner wall of the L-shaped card plate (10), and a plurality of spring sleeves (11) are welded at one end of the clamping plate (13) and one end of the inner wall of the L-shaped card plate (10), and a compression spring (12) is sleeved inside the spring sleeve (11), and the compression spring (12) is located at the center of the L-shaped card plate (10) and the clamping plate (13).

2. A stainless steel strip according to claim 1, characterized in that: The surface of the stainless steel belt body (1) is provided with a frosted layer (19), and the surface of the frosted layer (19) is provided with an anti-corrosion layer (20).

3. A stainless steel strip according to claim 1, characterized in that: A baffle (3) is welded to one end of the threaded column (4), and the baffle (3) is located on one side of the first self-locking nut (5).

4. A stainless steel strip according to claim 1, characterized in that: An anti-skid pad (14) is bonded to one end of the clamping plate (13), and the thickness of the anti-skid pad (14) is 2 mm.

5. The stainless steel strip according to claim 1, characterized in that: A spring hole groove is provided at the center of the spring sleeve (11), and the spring groove is sleeved on the outside of the compression spring (12).

6. The processing technology of a stainless steel strip according to claim 1 comprises step 1, selecting materials; step 2, rolling the steel strip; step 3, process lubrication; step 4, annealing the steel strip; step 5, flattening and finishing; step 6, coiling and packaging; characterized in that: In the above step 1, selecting materials includes the following steps: 1) Manually select suitable stainless steel strip materials to ensure that the thickness of the stainless steel strip material is uniform and there are no obvious cracks on the surface; 2) Place the stainless steel strip in a material storage bucket and add a certain amount of sulfuric acid aqueous solution for pickling until the surface of the stainless steel strip turns silvery white; In the above step 2, the steel strip rolling includes the following steps: 1) Hot rolling: The pickled stainless steel strip is manually placed in a hot rolling mill, the temperature is increased, and the hot rolling mill is used for rolling until the stainless steel strip is in a certain shape; 2) Cold rolling: The hot-rolled stainless steel strip is manually cooled, and after cooling, it is placed in a stamping machine for rolling until the stainless steel strip is in a certain shape, and then welded with a fixing component (2); In the above step 3, the process lubrication includes the following steps: 1) The rolled stainless steel strip is manually laid out and stored in a cool place, and its surface is manually moistened with water to ensure that the surface of the stainless steel strip is moist; 2) Mix the sulfided fatty acid and the extreme pressure anti-wear agent, add a small amount of graphite, and stir evenly; 3) manually brushing the mixture of sulfided fatty acid, extreme pressure anti-wear agent and graphite in step 2) of step 3 onto the surface of the stainless steel strip for three consecutive times to ensure that the surface of the stainless steel strip is evenly coated; In the above step 4, the stainless steel strip is manually leveled and placed in a bright annealing furnace for annealing for 1-2 hours, and both sides are annealed continuously until the surface of the stainless steel strip is bright; In the above step 5, the annealed stainless steel strip is manually placed in a shearing machine, the shearing length is set, and the shearing machine performs flat shearing, and after shearing, the strip is stored in a cool place in the factory; In the above step 6, the stainless steel strip cut in step 5 is manually rolled to ensure that each roll has the same length, and then packed into boxes.

7. A stainless steel strip processing technology according to claim 6, characterized in that: In the sub-step 2) of the step 1, the aqueous sulfuric acid solution flows over the surface of the stainless steel strip.

8. The processing technology of a stainless steel strip according to claim 6, characterized in that: The annealing temperature in step 4 is 100-200°C.

Citation Information

Patent Citations

  • Method of winding up copper foil on core

    CN1386075A

  • tape reel

    DE19836177A1