An electrochromic film structure and its preparation method and application
By depositing a nano-columnar tungsten oxide layer and an amorphous zinc tin oxide buffer layer on a transparent conductive layer, the problem of insufficient cycling stability of tungsten oxide films at low temperatures is solved, achieving efficient electrochromic performance and stability, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202111173762.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-10-08
AI Technical Summary
Existing technologies make it difficult to fabricate flexible electrochromic devices with good cycling stability at low temperatures, especially devices based on PET substrates. This is mainly because tungsten oxide films are prone to degradation at high temperatures, resulting in insufficient cycling stability.
A nano-columnar tungsten oxide layer was deposited on a transparent conductive layer using magnetron sputtering technology and covered with an amorphous zinc tin oxide buffer layer to form an electrochromic film structure. The film performance was optimized by controlling the sputtering parameters and gas ratio.
It improves the cycling stability and optical modulation amplitude of electrochromic films, suppresses the decay of the transmittance of tungsten oxide colored states, enhances the electrochemical performance of devices, and is suitable for large-scale industrial production.
Smart Images

Figure CN113862614B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrochromic devices and applications, and in particular relates to an electrochromic film layer structure and a preparation method and application thereof. Background Art
[0002] At present, flexible electrochromic devices based on polymer substrates such as polyethylene terephthalate (PET) have attracted more and more attention in building energy-saving windows, smart car windows, multi-function displays and wearable devices. The basic requirements for electrochromic devices in the above applications are: wide light modulation range, good cycle stability, stable mechanical properties, large-area preparation and fast response speed.
[0003] Typically, a typical flexible electrochromic device contains five layers, namely, a top transparent conductive layer, a cathode electrochromic layer, a lithium ion electrolyte layer, an ion storage layer (or anode electrochromic layer), and a bottom transparent conductive layer. When a small potential is applied to the device and switched alternately, the color changes reversibly. In this structure, the cathode electrochromic layer determines the performance of the entire device. In the cathode electrochromic material, tungsten oxide (WO x ) is considered to be the most ideal candidate material due to its relatively high coloring efficiency, large dynamic modulation range and excellent environmental stability. The coloring and bleaching reaction process of the film in lithium-ion electrolyte can be expressed as: WO x (bleached state)+yLi + +ye - <=>Li y WO x (Colored state).
[0004] Long-term cycle stability is one of the key technical problems that restrict the commercialization of electrochromic devices. During the frequent coloring and bleaching process, the continuous insertion and extraction of lithium ions in the tungsten oxide matrix will lead to a certain amount of lithium ion capture, collapse and degradation of the tungsten oxide matrix structure, and surface densification caused by the ion milling effect. The above factors will irreversibly weaken the long-term cycle stability of the tungsten oxide film. In order to further improve the cycle stability of tungsten oxide, it has been proven to be an effective means to increase the degree of crystallization of the film as much as possible by increasing the process temperature. For example, Blanchard et al. (Applied Materials Today 12 (2018) 235-243) announced that tungsten oxide films prepared under a substrate bias voltage of 400 V have better cycle stability (1000 cycles). The reason is that by applying a high substrate bias voltage, the critical crystallization temperature (~350°C) for the formation of WO3 nanocrystals is reached; Shi et al. (Solar Energy Materials & Solar Cells 212 (2020) 110579) announced that the nanobowl-shaped crystalline arrays formed after annealing at 300°C have higher chemical and structural stability; Zhou et al. (Journal of Colloid and Interface Science 460 (2015) 200-208) announced that the crystalline / amorphous tungsten oxide core / shell structure prepared at 400°C in air has excellent cycle performance, and there is still an optical modulation amplitude of 68.5% after 3000 cycles.
[0005] Although high-temperature processes can help to achieve tungsten oxide electrochromic films with high cycle stability, such high process temperatures (≥200°C) are difficult to apply to the preparation of electrochromic devices on polymer substrates such as PET. This is mainly due to the poor temperature resistance of polymer materials such as PET, which are difficult to use in environments above 150°C. Therefore, there is an urgent need to find a technical means to improve the electrochromic cycle stability of flexible tungsten oxide films prepared at low temperatures. Summary of the invention
[0006] The main purpose of the present invention is to provide an electrochromic film structure and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.
[0007] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0008] An embodiment of the present invention provides an electrochromic film structure, which includes a stacked tungsten oxide layer and an amorphous zinc tin oxide buffer layer; wherein the tungsten oxide layer has a nano-columnar structure.
[0009] The embodiment of the present invention further provides a method for preparing the aforementioned electrochromic film structure, which comprises:
[0010] providing a substrate provided with a transparent conductive layer;
[0011] Using magnetron sputtering technology and taking a tungsten oxide target as a target material, a tungsten oxide layer is deposited on the surface of the transparent conductive layer;
[0012] Furthermore, magnetron sputtering technology is adopted, with a zinc tin oxide target as a target material, to deposit an amorphous zinc tin oxide buffer layer on the surface of the tungsten oxide layer, thereby obtaining an electrochromic film structure.
[0013] The embodiment of the present invention also provides the use of the aforementioned electrochromic film structure in preparing an electrochromic device.
[0014] An embodiment of the present invention further provides an electrochromic device, which includes the aforementioned electrochromic film layer structure.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] (1) The electrochromic film layer structure prepared by the present invention has a good O / W ratio (2.7-2.9), and the O / W ratio has relatively good electrochromic cycle stability, meeting the basic requirements of electrochromic devices;
[0017] (2) The tungsten oxide layer and the amorphous zinc tin oxide buffer layer in the electrochromic film structure prepared by the present invention are both amorphous;
[0018] (3) The electrochromic film layer structure prepared by the present invention has excellent cycle stability, which is beneficial to the stability of the electrochromic film;
[0019] (4) The tungsten oxide layer in the electrochromic film layer structure prepared by the present invention has a columnar structure, which helps to maintain more lithium ion binding sites in the electrochromic film and is beneficial to improving the optical modulation amplitude of the film;
[0020] (5) The electrochromic film structure prepared by the present invention can significantly inhibit the attenuation of the transmittance of the tungsten oxide colored state during the electrochemical cycle, and improve the optical modulation amplitude and the coloring efficiency; (6) The method provided by the present invention uses ceramic targets to replace traditional metal targets for reactive DC sputtering, which helps to provide sputtering stability and is suitable for future large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is the XPS spectrum of the W element in the electrochromic film layer structure prepared in Example 1;
[0023] Figure 2 The XRD pattern of the electrochromic film structure prepared in Example 1;
[0024] Figure 3a-3d Surface morphology of the electrochromic film structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 before and after electrochemical cycle treatment;
[0025] Figure 4a-4d The cross-sectional morphology diagrams of the electrochromic film structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 before and after the electrochemical cycle treatment;
[0026] Figure 5a-5d The light modulation curves of the electrochromic film structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 at 550nm and 790nm;
[0027] Figure 6a-6b The optical transmittance spectra of the electrochromic film structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 in different color change states and after electrochemical cycles;
[0028] Figure 7a-Figure 7b It is a coloring efficiency curve diagram of the electrochromic film layer structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1;
[0029] Figure 8 is a schematic structural diagram of an electrochromic device in a typical embodiment of the present invention;
[0030] Fig. 9 This is a cross-sectional morphology of the tungsten oxide layer prepared in Comparative Example 2.
[0031] Description of the drawings: 1-PET substrate, 2-transparent conductive film, 3-tungsten oxide film, 4-zinc tin oxide film, 5-electrolyte layer, 6-ion storage layer. DETAILED DESCRIPTION
[0032] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] An aspect of an embodiment of the present invention provides an electrochromic film layer structure comprising a stacked tungsten oxide layer and an amorphous zinc tin oxide buffer layer; wherein the tungsten oxide layer has a nano-columnar structure.
[0034] Specifically, the cross section of the tungsten oxide layer in the electrochromic film layer structure presents a nano-columnar structure, and the diameter of the column is 20-60nm; an amorphous zinc oxide tin buffer layer with a thickness of 3-50nm is covered on the tungsten oxide thin layer to form an electrochromic film layer structure;
[0035] In some more specific embodiments, the diameter of the columnar structure is 20 to 60 nm.
[0036] Furthermore, the tungsten oxide layer is formed by a plurality of nano-columnar structures arranged in a vertical direction and arranged closely in sequence.
[0037] Furthermore, the thickness of the tungsten oxide layer is 200-800 nm.
[0038] Furthermore, the tungsten oxide layer is a tungsten oxide thin film, wherein O / W is 2.7-2.9.
[0039] Furthermore, the thickness of the amorphous zinc tin oxide buffer layer is 3-50 nm.
[0040] Furthermore, the amorphous zinc tin oxide buffer layer is a zinc tin oxide thin film.
[0041] Furthermore, the thickness of the electrochromic film layer structure is 203-850 nm.
[0042] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned electrochromic film structure, which comprises:
[0043] providing a substrate provided with a transparent conductive layer;
[0044] Using magnetron sputtering technology and taking a tungsten oxide target as a target material, a tungsten oxide layer is deposited on the surface of the transparent conductive layer;
[0045] Furthermore, magnetron sputtering technology is adopted, with a zinc tin oxide target as a target material, to deposit an amorphous zinc tin oxide buffer layer on the surface of the tungsten oxide layer, thereby obtaining an electrochromic film structure.
[0046] In some more specific embodiments, the mass ratio of zinc oxide to tin oxide in the zinc tin oxide target is 100:(50-200).
[0047] Furthermore, the sputtering method adopted by the magnetron sputtering technology includes radio frequency sputtering or medium frequency sputtering.
[0048] In some more specific embodiments, the preparation method specifically includes: using magnetron sputtering technology, placing the substrate provided with a transparent conductive layer in a reaction chamber, using a tungsten oxide target as a target material, and using oxygen and an inert gas as a working gas to deposit a tungsten oxide layer on the surface of the transparent conductive layer, wherein the sputtering gas pressure value used in the magnetron sputtering technology is 0.4-2.0 Pa, and the sputtering power density is 2.8-4.7 W / cm 2 , the substrate temperature is 25-150°C, and the vacuum degree of the reaction chamber is 0.10×10 -2 ~10×10 -2 pa, the flow rate ratio of oxygen to inert gas is (0.2-1.5) : 4, and the thickness of the tungsten oxide layer is 200-800 nm.
[0049] In some more specific embodiments, the preparation method specifically includes: using magnetron sputtering technology, using zinc tin oxide target as target material, and using inert gas as working gas to deposit an amorphous zinc tin oxide buffer layer on the surface of the tungsten oxide layer, wherein the sputtering gas pressure value used in the magnetron sputtering technology is 0.8-1.6 Pa, and the sputtering power density is 1.89-4.7 W / cm 2 , the substrate temperature is 25-150°C, and the vacuum degree of the reaction chamber is 0.10×10 -2 ~10×10 -2 Pa, the amount of inert gas introduced is 10-30 sccm, and the thickness of the amorphous zinc tin oxide buffer layer is 3-50 nm.
[0050] In some more specific implementation schemes, the material of the substrate includes any one of PET, PVC, and PC but is not limited thereto.
[0051] Furthermore, the material of the rigid substrate includes glass or quartz, but is not limited thereto.
[0052] Furthermore, the material of the transparent conductive layer includes any one or a combination of two or more of ITO, OMO, graphene, and silver nanowires, but is not limited thereto.
[0053] In some more specific embodiments, the method for preparing the electrochromic film structure comprises:
[0054] (1) Magnetron sputtering deposition of nano-columnar tungsten oxide films
[0055] The tungsten oxide target was placed in a magnetron sputtering coating device to deposit a nano-columnar tungsten oxide film on a PET substrate covered with an ITO transparent conductive layer. The parameters in the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was O2 and Ar, and the flow ratio of O2 and Ar was (0.2-1.5):4; the substrate temperature was 25-150°C; the vacuum degree was (0.1-10) ×10 -2 Pa; the sputtering pressure is 0.4~2.0Pa; the sputtering power density is 2.8W / cm 2 ~4.7W / cm 2 ; The thickness of the tungsten oxide layer is 200 to 800 nm;
[0056] (2) Magnetron sputtering deposition of amorphous zinc tin oxide buffer layer (ZTO layer)
[0057] The zinc tin oxide (ZTO) target was placed in a magnetron sputtering coating device to deposit an amorphous zinc tin oxide buffer layer (ZTO layer) on an ITO transparent conductive PET substrate on which tungsten oxide had been deposited. The main parameters during the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was pure Ar; the substrate temperature was 25-150°C; the vacuum degree was (0.1-10)×10 - 2 Pa; the sputtering pressure is 0.8~1.6Pa; the sputtering power density is 1.89~4.7W / cm 2 ; The thickness of the ZTO layer is 3-50nm;
[0058] Wherein, the mass ratio of zinc oxide to tin oxide in the composition of the zinc tin oxide target is 100:(50-200).
[0059] Another aspect of the embodiments of the present invention further provides the use of the aforementioned electrochromic film structure in preparing an electrochromic device.
[0060] Another aspect of the embodiments of the present invention further provides an electrochromic device, which includes the aforementioned electrochromic film layer structure.
[0061] Furthermore, in the electrochromic device, the electrochromic film layer structure is disposed on a substrate including a transparent conductive layer.
[0062] Furthermore, the electrochromic device also includes an electrolyte layer, an ion storage layer as a counter electrode, a transparent conductive layer and a substrate.
[0063] Furthermore, the material of the ion storage layer includes nickel oxide.
[0064] In some specific embodiments, the electrochromic device has Figure 8 The structure shown includes (1) PET substrate, (2) transparent conductive film, (3) tungsten oxide film, (4) zinc tin oxide film, (5) electrolyte layer, and (6) ion storage layer.
[0065] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0066] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0067] Example 1
[0068] (1) Magnetron sputtering deposition of nano-columnar tungsten oxide layers
[0069] The tungsten oxide target was placed in a magnetron sputtering coating device to deposit a nanocolumnar tungsten oxide layer on a PET substrate covered with an ITO transparent conductive layer. The parameters during the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was O2 and Ar, and the flow ratio of O2 to Ar was 1:4; the substrate temperature was 80°C; the vacuum degree was 5×10 -2 Pa; the sputtering pressure is 1.2Pa; the sputtering power density is 4.7W / cm 2 ;The thickness of the tungsten oxide layer is 300nm;
[0070] (2) Magnetron sputtering deposition of amorphous zinc tin oxide buffer layer
[0071] The zinc tin oxide target was placed in a magnetron sputtering coating device, and an amorphous zinc tin oxide buffer layer was deposited on an ITO transparent conductive PET substrate on which tungsten oxide had been deposited, thereby obtaining an electrochromic film structure. The main parameters in the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was pure Ar; the substrate temperature was 80°C; the vacuum degree was 5×10 -2 Pa; the sputtering pressure is 1.2Pa; the sputtering power density is 1.89W / cm 2 ; The thickness of the amorphous zinc tin oxide layer is 18nm.
[0072] Comparative Example 1
[0073] The tungsten oxide target was placed in a magnetron sputtering coating device to deposit a nano-columnar tungsten oxide film on a PET substrate covered with an ITO transparent conductive layer. The parameters during the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was O2 and Ar, and the flow ratio of O2 to Ar was 1:4; the substrate temperature was 80°C; the vacuum degree was 5×10 -2 Pa; the sputtering pressure is 1.2Pa; the sputtering power density is 4.7W / cm 2 ; The thickness of the tungsten oxide layer is 300nm.
[0074] Comparative Example 2
[0075] The preparation method is the same as that of Example 1, except that the prepared tungsten oxide layer does not have a columnar structure.
[0076] The tungsten oxide target was placed in a magnetron sputtering coating device to deposit a nano-columnar tungsten oxide film on a PET substrate covered with an ITO transparent conductive layer. The parameters during the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was Ar, the substrate temperature was 80°C, the vacuum degree was 5×10 -2 Pa; the sputtering pressure is 1.2Pa; the sputtering power density is 2.8W / cm 2 ; The thickness of the tungsten oxide layer is 300nm, and the prepared tungsten oxide layer is as follows Fig. 9 shown.
[0077] Performance characterization:
[0078] The valence state of the elements was observed by XPS, the phase structure of the film was observed by X-ray diffractometer (XRD), the surface and cross-sectional morphology of the film were observed by scanning electron microscope (SEM), the optical modulation amplitude and electrochromic response time of the film were measured by UV-visible spectrophotometer, and the electrochemical properties, cycle stability and other electrochromic properties of the film were measured by electrochemical workstation.
[0079] Figure 1 The XPS spectrum of the W element in the electrochromic film layer structure prepared in Example 1 is shown in Table 1. It can be seen that there is a good O / W ratio in the electrochromic film layer structure, and the O / W stoichiometric ratio can be determined by W 6+ (WO3) and W 5+ (WO 2.5 ) percentages is calculated as 2.89( Figure 1 ), this O / W ratio has relatively good electrochromic cycle stability and meets the basic requirements of electrochromic devices.
[0080] Table 1 XPS results of W element in electrochromic film structure
[0081]
[0082] Figure 2 This is the XRD spectrum of the electrochromic film structure prepared in Example 1. It can be seen that the tungsten oxide film and the amorphous zinc tin oxide layer in the electrochromic film structure are both amorphous, and all diffraction peaks come from PET and ITO, and no peaks of tungsten oxide and amorphous zinc tin oxide are observed;
[0083] Figure 3a-Figure 3b The surface morphology of the electrochromic film structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1; after 2000 electrochemical cycles, the electrochromic film structure prepared in Example 1 can slow down the damage to the surface morphology of the color-changing layer film caused by the insertion and extraction of lithium ions during the cycle, and maintain the surface morphology (such as Figure 3c As shown in FIG. 1 , the surface of the tungsten oxide film prepared in Comparative Example 1 deteriorated seriously after the electrochemical cycle test. A large number of holes with a diameter of 25 nm were distributed on the entire surface of the film, and the surface grains became finer (as shown in FIG. Figure 3d This is due to the surface particle refinement caused by the ion milling effect.
[0084] Figure 4a-4b The cross-sectional morphology of the electrochromic film structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 is about 20 to 60 nm in diameter. The diameter of the columnar structure of the electrochromic film structure prepared in Example 1 is always maintained at about 20 to 60 nm before and after 2000 electrochemical cycles (e.g. Figure 4c As shown in FIG. 1 , the structure of the tungsten oxide film prepared in Comparative Example 1 deteriorates after the electrochemical cycle test. The columnar structure inside the film gradually becomes denser and coarser, the columnar structure is not obvious, and the diameter is much larger than 60 nm (as shown in FIG. Figure 4d shown).
[0085] Figure 5a-5d The light modulation curves of the electrochromic film structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 at 550nm and 790nm are shown; it can be seen that at a wavelength of 550nm, after 2000 electrochemical cycles, the coloring state transmittance of the present invention is 16.5%, and the optical modulation amplitude is 68.4% (as shown in Figure 2). Figure 5a ), which is better than 26.5% and 60.5% of the comparative examples (as shown in Figure 5b Similarly, at a wavelength of 790 nm, after 2000 electrochemical cycles, the coloring state transmittance of the present invention is 8.7%, and the optical modulation amplitude is 76.8% (as shown in FIG. Figure 5c ), which is better than 21.4% and 66.3% of the comparative examples (as shown in Figure 5d shown).
[0086] Figure 6a-6b The optical transmittance spectra of the electrochromic film layer structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 in different color change states and after electrochemical cycles; it can be seen that within the wavelength range of 300nm to 1100nm, the color state transmittance of the electrochromic film layer structure prepared in Example 1 is lower, and the optical modulation amplitude is larger, both of which are better than Comparative Example 1;
[0087] Figure 7a-Figure 7b The coloring efficiency curve of the electrochromic film layer structure prepared in Example 1 and the tungsten oxide film prepared in Comparative Example 1 is shown in FIG. 1 . It can be seen that after 2000 CV cycles, the coloring efficiency of the electrochromic film layer structure prepared in Example 1 at 550nm is 29.2 cm 2 / C, higher than the 23.4cm of the control 2 / C(such as Figure 7a ), also at 790nm, the efficiency advantage of Example 1 is more obvious (such as Figure 7b ), the present invention is 40.7cm after 2000 CV cycles 2 / C, much higher than the 28.9cm of the control group 2 / C
[0088] Example 2
[0089] (1) Magnetron sputtering deposition of nano-columnar tungsten oxide layers
[0090] The tungsten oxide target was placed in a magnetron sputtering coating device to deposit a nanocolumnar tungsten oxide layer on a PET substrate covered with an ITO transparent conductive layer. The parameters during the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was O2 and Ar, and the flow ratio of O2 to Ar was 0.2:4; the substrate temperature was 25°C; the vacuum degree was 0.1×10 -2 Pa; the sputtering pressure is 0.4Pa; the sputtering power density is 2.8W / cm 2 ;The thickness of the tungsten oxide layer is 200nm;
[0091] (2) Magnetron sputtering deposition of amorphous zinc tin oxide buffer layer
[0092] The zinc tin oxide target was placed in a magnetron sputtering coating device, and an amorphous zinc tin oxide buffer layer was deposited on an ITO transparent conductive PET substrate on which tungsten oxide had been deposited, thereby obtaining an electrochromic film structure. The main parameters in the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was pure Ar; the substrate temperature was 25-150°C; the vacuum degree was 0.1×10 -2 Pa; the sputtering pressure is 0.8Pa; the sputtering power density is 1.89W / cm 2; The thickness of the amorphous zinc tin oxide buffer layer is 10nm
[0093] Example 3
[0094] (1) Magnetron sputtering deposition of nano-columnar tungsten oxide layers
[0095] The tungsten oxide target was placed in a magnetron sputtering coating device to deposit a nanocolumnar tungsten oxide layer on a PET substrate covered with an ITO transparent conductive layer. The parameters during the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was O2 and Ar, and the flow ratio of O2 to Ar was 1.5:4; the substrate temperature was 150°C; the vacuum degree was 10×10 -2 Pa; the sputtering pressure is 2.0Pa; the sputtering power density is 4.7W / cm 2 ; Tungsten oxide layer thickness 800nm;
[0096] (2) Magnetron sputtering deposition of amorphous zinc tin oxide buffer layer
[0097] The zinc tin oxide target was placed in a magnetron sputtering coating device, and an amorphous zinc tin oxide buffer layer was deposited on an ITO transparent conductive PET substrate on which tungsten oxide had been deposited, thereby obtaining an electrochromic film structure. The main parameters in the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was pure Ar; the substrate temperature was 150°C; the vacuum degree was 10×10 -2 Pa; the sputtering pressure is 1.6Pa; the sputtering power density is 4.7W / cm 2 ; The thickness of the amorphous zinc tin oxide buffer layer is 3nm.
[0098] Example 4
[0099] (1) Magnetron sputtering deposition of nano-columnar tungsten oxide layers
[0100] The tungsten oxide target was placed in a magnetron sputtering coating device to deposit a nanocolumnar tungsten oxide layer on a PET substrate covered with an ITO transparent conductive layer. The parameters during the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was O2 and Ar, and the flow ratio of O2 to Ar was 0.8:4; the substrate temperature was 50°C; the vacuum degree was 5×10 -2 Pa; the sputtering pressure is 1.0Pa; the sputtering power density is 3.0W / cm 2 ; Tungsten oxide layer thickness 600nm
[0101] (2) Magnetron sputtering deposition of amorphous zinc tin oxide buffer layer
[0102] The zinc tin oxide target was placed in a magnetron sputtering coating device, and an amorphous zinc tin oxide buffer layer was deposited on an ITO transparent conductive PET substrate on which tungsten oxide had been deposited, thereby obtaining an electrochromic film structure. The main parameters in the sputtering process were as follows: the sputtering method was RF sputtering or medium frequency sputtering, the working gas was pure Ar; the substrate temperature was 50°C; the vacuum degree was 5×10 -2 Pa; the sputtering pressure is 1.0Pa; the sputtering power density is 2.5W / cm 2 ; Amorphous ZnO tin buffer layer thickness 10nm
[0103] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0104] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.
Claims
1. An electrochromic film structure, characterized in that: It comprises a stacked tungsten oxide layer and an amorphous zinc tin oxide buffer layer; wherein the tungsten oxide layer has a nano columnar structure, and the diameter of the columnar structure is 20-60 nm; the tungsten oxide layer is formed by a plurality of nano columnar structures arranged in a vertical direction and arranged closely in sequence; the O / W in the tungsten oxide layer is 2.7-2.9; the thickness of the amorphous zinc tin oxide buffer layer is 18 nm; The preparation method of the electrochromic film layer structure comprises: A substrate provided with a transparent conductive layer is provided; wherein the material of the substrate is selected from any one of PET, PVC, and PC; Adopting magnetron sputtering technology, using tungsten oxide target as target material, depositing a tungsten oxide layer on the surface of the transparent conductive layer; wherein the substrate temperature adopted by the magnetron sputtering technology is 25-150° C.; And, magnetron sputtering technology is used, with zinc tin oxide target as target material, to deposit an amorphous zinc tin oxide buffer layer on the surface of the tungsten oxide layer, thereby obtaining an electrochromic film layer structure; wherein the substrate temperature used in the magnetron sputtering technology is 25~150℃.
2. The electrochromic film structure according to claim 1, characterized in that: The thickness of the tungsten oxide layer is 200-400 nm.
3. The electrochromic film structure according to claim 1, characterized in that: The mass ratio of zinc oxide to tin oxide in the zinc oxide tin target is 100:(50-200).
4. The electrochromic film structure according to claim 1, characterized in that: The sputtering method adopted by the magnetron sputtering technology is selected from radio frequency sputtering or medium frequency sputtering.
5. The electrochromic film structure according to claim 1, characterized in that: The preparation method of the electrochromic film structure specifically includes: using magnetron sputtering technology, placing the substrate provided with a transparent conductive layer in a reaction chamber, using a tungsten oxide target as a target material, and using oxygen and an inert gas as working gas to deposit a tungsten oxide layer on the surface of the transparent conductive layer, wherein the sputtering gas pressure value used in the magnetron sputtering technology is 0.4-2.0 Pa, and the sputtering power density is 2.8-4.7 W / cm 2 The vacuum degree of the reaction chamber is 0.10×10 -2 ~10×10 -2 Pa, the flow rate ratio of oxygen to inert gas is (0.2-1.5):4, and the thickness of the tungsten oxide layer is 200-800 nm.
6. The electrochromic film structure according to claim 1, characterized in that: The preparation method of the electrochromic film structure specifically comprises: using magnetron sputtering technology, using zinc tin oxide target as target material, and using inert gas as working gas to deposit an amorphous zinc tin oxide buffer layer on the surface of the tungsten oxide layer, wherein the sputtering gas pressure value used in the magnetron sputtering technology is 0.8~1.6Pa, and the sputtering power density is 1.89~4.7W / cm 2 The vacuum degree of the reaction chamber is 0.10×10 -2 ~10×10 - 2 Pa, the inert gas flow rate is 10~30 sccm.
7. The electrochromic film structure according to claim 1, characterized in that: The material of the transparent conductive layer is selected from any one of ITO, OMO, graphene, and silver nanowires, or a combination of two or more thereof.
8. Use of the electrochromic film structure according to any one of claims 1 to 7 in preparing an electrochromic device.
9. An electrochromic device, characterized in that: The invention comprises the electrochromic film layer structure according to any one of claims 1 to 7.
10. The electrochromic device according to claim 9, characterized in that: The electrochromic device further includes an electrolyte layer, an ion storage layer as a counter electrode, a transparent conductive layer and a substrate.
Citation Information
Patent Citations
Electrochromism film with stable performance and preparation method thereof
CN108037628A
Stress developing appliance and its application
CN108227329A
Systems, methods, and apparatus for integrated glass units having adjustable solar heat gains
US20150177583A1
Method for forming a transparent conducting polymeric film and its use as a transparent electrode
WO2015163824A1