A composite polymer electrolyte that facilitates uniform lithium deposition and its preparation method and application
By adding short-fiber silicate minerals and fluorine-containing polymers to the solid electrolyte, a composite polymer electrolyte is prepared, which solves the problem of insufficient ionic conductivity and migration number of the solid electrolyte at room temperature, and achieves lithium ion Uniform deposition and suppression of lithium dendrites improve the performance and safety of lithium metal batteries.
Patent Information
- Application Number
- CN202210534548.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-05-17
AI Technical Summary
Existing solid electrolytes have poor ionic conductivity and ion migration number at room temperature, which limits the effective regulation of lithium ions and the suppression of lithium dendrites, resulting in cycle life and safety issues for lithium metal batteries.
The composite polymer electrolyte is prepared by combining fluorine-containing polymers with short-fiber silicate minerals and using methods such as magnetic stirring and ultrasonic stirring to increase the conductivity and migration number of lithium ions and form a composite solid-state electrolyte with good interface contact. .
It significantly improves the uniform deposition of lithium ions and the growth of lithium dendrites, improves the cycle performance, rate performance and mechanical strength of lithium metal batteries, solves the growth problem of lithium dendrites and improves the safety of the battery.
Smart Images

Figure CN114976258B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite polymer electrolyte which is helpful for uniform lithium deposition and a preparation method and application thereof, belonging to the technical field of composite solid electrolyte material preparation. Background Art
[0002] As a clean energy with high energy density, lithium-ion batteries are widely used in various energy storage devices. -1 Ultra-high theoretical specific capacity and 0.534 g cm -3 Due to the effective mass density of lithium metal, lithium metal anode is considered to be a key component for achieving high energy density lithium-ion batteries. However, the strong reaction of highly active lithium metal with liquid organic electrolytes leads to shortened battery cycle life and safety issues, which will hinder the practical application of lithium metal batteries. Therefore, research on inhibiting lithium dendrite growth is urgent for the development of high energy density lithium-ion batteries. When solving the problems of lithium metal batteries based on traditional electrolytes, a large number of researchers will choose to adjust the organic structure of liquid electrolytes and construct anode-electrolyte interface layers. However, these strategies are based on liquid electrolytes and still have safety issues such as combustion, leakage and explosion.
[0003] In order to solve the above problems, solid electrolytes are used as substitutes for liquid electrolytes. The advantage of solid electrolytes is that they can fundamentally solve the problems of flammability and leakage of electrolytes, and solid electrolytes can effectively solve the dangers of lithium dendrite puncture due to their inherent physical and chemical properties. Among all solid electrolytes, polymer electrolytes are particularly attractive because they have good interface contact with electrodes, simple preparation process and good flexibility, but their ionic conductivity and ion migration number at room temperature are poor, resulting in slow lithium ion transfer, limiting the capacity of the battery, hindering the effective regulation of lithium ions, and resulting in limited ability to inhibit lithium dendrites. Therefore, it is very necessary to provide a composite solid electrolyte material that allows lithium ions to be uniformly deposited and improves the growth problem of lithium dendrites. Summary of the invention
[0004] In order to solve the technical problem that the ionic conductivity and ion migration number of the existing solid electrolytes are poor at room temperature, the present invention provides a composite polymer electrolyte that helps uniform lithium deposition and its preparation method and application
[0005] The technical solution of the present invention:
[0006] A composite polymer electrolyte that facilitates uniform lithium deposition and a preparation method thereof, the operation process is as follows:
[0007] S1, preparing a short fiber silicate mineral and dispersing it in a solvent I to obtain a short fiber silicate mineral dispersion;
[0008] S2, dissolving the fluorine-containing polymer in solvent I to obtain a polymer solution;
[0009] S3, under a protective gas atmosphere, adding the lithium salt and short fiber silicate mineral dispersion to the high molecular polymer solution, and magnetically stirring for 6-12 hours to obtain a composite solution;
[0010] S4, coating the composite solution to form a film, and drying at 60-100° C. for 12-36 hours to obtain a composite polymer electrolyte.
[0011] It is further defined that the mass ratio of the fluorine-containing high molecular polymer, lithium salt, short fiber silicate mineral and solvent I in the composite solution is 1:0.8:(0.15-0.25):15.
[0012] It is further defined that the operation process for preparing the short fibrous silicate mineral in S1 is: dispersing the fibrous silicate mineral in ethanol, ball milling for 2-6 hours until the length of the fibrous silicate mineral is 1-20 μm, and then drying at 50-80° C. for 12-36 hours to obtain the short fibrous silicate mineral.
[0013] It is further defined that the ball-to-material ratio during the ball milling process is (10-20):1.
[0014] It is further defined that the rotation speed during the ball milling process is 300-600 r / min.
[0015] It is further defined that the short fiber silicate mineral in S1 is dispersed in the solvent I by ultrasonic stirring for 6-12 hours to obtain a short fiber silicate mineral dispersion.
[0016] It is further defined that the fibrous silicate mineral is one or more of serpentine asbestos, actinolite asbestos, hornblende asbestos, amosite, and tremolite asbestos mixed in any proportion.
[0017] It is further defined that the fluorine-containing high molecular polymer is one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluoroethylene, and polyvinylidene fluoride-chlorotrifluoroethylene mixed in any proportion.
[0018] Further limited, solvent I is one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide, and dimethylpyrrolidone mixed in any proportion.
[0019] It is further defined that the lithium salt is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium difluorooxalatoborate mixed in any proportion.
[0020] It is further defined that the protective gas is argon or nitrogen.
[0021] It is further defined that the magnetic stirring speed is 500-1500 r / min.
[0022] The purpose of the present invention also includes preparing a composite solid electrolyte by using the above method.
[0023] The composite solid electrolyte provided by the invention is used for lithium batteries.
[0024] The present invention uses a fluorine-containing high molecular polymer as a substrate, which is conducive to the block movement of lithium ions. A pretreated fibrous silicate mineral material is added to form a composite solid polymer electrolyte. The fibrous silicate mineral in the composite solid polymer electrolyte has a greater adsorption effect on lithium ions, thereby improving the lithium ion conductivity and lithium ion migration number at room temperature, allowing lithium ions to be uniformly deposited and improving the growth problem of lithium dendrites, thereby ensuring the cycle performance, rate performance and mechanical strength of the lithium metal battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a surface SEM morphology photograph of the composite polymer electrolyte obtained in Example 2;
[0026] Figure 2 This is a surface SEM morphology photograph of the polymer electrolyte obtained in Comparative Example 1;
[0027] Figure 3 This is a comparison chart of the mechanical strength of the electrolyte obtained in Example 2 and Comparative Example 1;
[0028] Figure 4 A comparison chart of the lithium ion migration number and ion conductivity of the electrolyte obtained in Example 2 and Comparative Example 1;
[0029] Figure 5 This is a comparison chart of the rate performance of lithium batteries assembled using the electrolytes obtained in Example 2 and Comparative Example 1;
[0030] Figure 6 This is a comparison chart of the long cycle performance of lithium batteries assembled using the electrolytes obtained in Example 2 and Comparative Example 1;
[0031] Figure 7 This is a comparison chart of the voltage stability of lithium batteries assembled using the electrolytes obtained in Example 2 and Comparative Example 1;
[0032] Figure 8 This is a SEM morphology photograph of the lithium metal surface of a lithium battery assembled using the electrolyte obtained in Example 2 after cycling;
[0033] Fig. 9This is a SEM morphology photograph of the lithium metal surface of a lithium battery assembled using the electrolyte obtained in Example 1 after cycling. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0035] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art.
[0036] Embodiment 1:
[0037] Step 1, disperse serpentine asbestos in ethanol, place it in a spherical graphite tank for 4 hours, and dry the short-fiber serpentine asbestos ethanol dispersion at 60° C. for 24 hours to obtain short-fiber serpentine asbestos. The ball milling speed is 450r / min, and the ball-to-material ratio is 15:1.
[0038] Step 2: Disperse the short-fiber serpentine asbestos in dimethylpyrrolidone and stir ultrasonically for 12 hours to obtain a short-fiber serpentine asbestos dispersion.
[0039] Step 3: Disperse polyvinylidene fluoride-hexafluoropropylene in dimethyl pyrrolidone, and stir magnetically for 12 hours in an argon atmosphere until the polyvinylidene fluoride-hexafluoropropylene is completely dissolved to obtain a polyvinylidene fluoride-hexafluoropropylene solution. The magnetic stirring speed is 1000 r / min.
[0040] Step 4: Under an argon atmosphere, lithium bis(trifluoromethanesulfonic acid) imide and short fiber serpentine asbestos dispersion are added to the polyvinylidene fluoride-hexafluoropropylene solution respectively, and magnetic stirring is performed for 12 hours to obtain a uniform composite solution. The mass ratio of polyvinylidene fluoride-hexafluoropropylene, lithium bis(trifluoromethanesulfonic acid) imide, serpentine asbestos and dimethyl pyrrolidone in the composite solution is 1:0.8:0.15:15.
[0041] Step 5: Use a doctor blade coater to evenly apply the composite solution obtained in step 4 to obtain a composite slurry film with a smooth surface, and then dry it at 80° C. for 24 hours to obtain a composite polymer electrolyte.
[0042] Embodiment 2:
[0043] Step 1, disperse serpentine asbestos in ethanol, place it in a spherical graphite tank for 4 hours, and dry the short-fiber serpentine asbestos ethanol dispersion at 60° C. for 24 hours to obtain short-fiber serpentine asbestos. The ball milling speed is 450r / min, and the ball-to-material ratio is 15:1.
[0044] Step 2: Disperse the short-fiber serpentine asbestos in dimethylpyrrolidone and stir ultrasonically for 12 hours to obtain a short-fiber serpentine asbestos dispersion.
[0045] Step 3: Disperse polyvinylidene fluoride-hexafluoropropylene in dimethyl pyrrolidone, and stir magnetically for 12 hours in an argon atmosphere until the polyvinylidene fluoride-hexafluoropropylene is completely dissolved to obtain a polyvinylidene fluoride-hexafluoropropylene solution. The magnetic stirring speed is 1000 r / min.
[0046] Step 4: Under an argon atmosphere, lithium bis(trifluoromethanesulfonic acid) imide and short fiber serpentine asbestos dispersion are added to the poly(vinylidene fluoride)-hexafluoropropylene solution, respectively, and magnetically stirred for 12 hours to obtain a uniform composite solution. The mass ratio of poly(vinylidene fluoride)-hexafluoropropylene, lithium bis(trifluoromethanesulfonic acid) imide, serpentine asbestos and dimethyl pyrrolidone in the composite solution is 1:0.8:0.2:15.
[0047] Step 5: Use a doctor blade coater to evenly apply the composite solution obtained in step 4 to obtain a composite slurry film with a smooth surface, and then dry it at 80°C for 24 hours to obtain a composite polymer electrolyte with a thickness of 60 μm, referred to as PVDF-HFP / LiTFSI / ASB.
[0048] Embodiment 3:
[0049] Step 1: Disperse serpentine asbestos in ethanol, place it in a ball mill for 4 hours, ball mill the serpentine asbestos to short-fiber serpentine asbestos with a length of about 2 μm, and dry the obtained short-fiber serpentine asbestos ethanol dispersion at 60° C. for 24 hours to obtain short-fiber serpentine asbestos. The ball mill speed is 450 r / min, and the ball-to-material ratio is 15:1.
[0050] Step 2: Disperse the short-fiber serpentine asbestos in dimethylpyrrolidone and stir ultrasonically for 12 hours to obtain a short-fiber serpentine asbestos dispersion.
[0051] Step 3: Disperse polyvinylidene fluoride-hexafluoropropylene in dimethyl pyrrolidone, and stir magnetically for 12 hours in an argon atmosphere until the polyvinylidene fluoride-hexafluoropropylene is completely dissolved to obtain a polyvinylidene fluoride-hexafluoropropylene solution. The magnetic stirring speed is 1000 r / min.
[0052] Step 4: Under an argon atmosphere, add the lithium bis(trifluoromethanesulfonic acid) imide and the short fiber serpentine asbestos dispersion to the poly(vinylidene fluoride)-hexafluoropropylene solution, and stir magnetically for 12 hours to obtain a uniform composite solution. The mass ratio of poly(vinylidene fluoride)-hexafluoropropylene, lithium bis(trifluoromethanesulfonic acid) imide, serpentine asbestos and dimethyl pyrrolidone in the composite solution is 1:0.8:0.25:15.
[0053] Step 5: Use a doctor blade coater to evenly apply the composite solution obtained in step 4 to obtain a composite slurry film with a smooth surface, and then dry it at 80° C. for 24 hours to obtain a composite polymer electrolyte.
[0054] Comparative Example 1:
[0055] Step 1: Disperse polyvinylidene fluoride-hexafluoropropylene in dimethyl pyrrolidone, and stir magnetically for 12 hours in an argon atmosphere until the polyvinylidene fluoride-hexafluoropropylene is completely dissolved to obtain a polyvinylidene fluoride-hexafluoropropylene solution. The magnetic stirring speed is 1000 r / min.
[0056] Step 2: Under an argon atmosphere, lithium bis(trifluoromethanesulfonate)imide was added to the poly(vinylidene fluoride)-hexafluoropropylene) solution, and magnetic stirring was performed for 12 hours to obtain a uniform solution. The mass ratio of poly(vinylidene fluoride)-hexafluoropropylene, lithium bis(trifluoromethanesulfonate)imide and dimethylpyrrolidone in the solution was 1:0.8:15.
[0057] Step 3: Use a doctor blade coater to scrape the uniform solution obtained in step 4 to obtain a polymer slurry film with a smooth surface, and then dry it at 80° C. for 24 hours to obtain a polyvinylidene fluoride-hexafluoropropylene electrolyte with a thickness of 60 μm, referred to as PVDF-HFP / LiTFSI.
[0058] Effect example 1:
[0059] Polymer electrolyte performance test:
[0060] (1) The morphology of the polymer electrolytes obtained in Example 2 and Comparative Example 1 was observed using a scanning electron microscope (SEM). The results are as follows: Figure 1 and Figure 2 As shown in the figure, it can be seen that the composite polymer electrolyte prepared in Example 2 has a denser surface morphology and a uniform surface than the polymer electrolyte prepared in Comparative Example 1.
[0061] (2) The mechanical strength of the polymer electrolytes obtained in Example 2 (PVDF-HFP / LiTFSI / ASB) and Comparative Example 1 (PVDF-HFP / LiTFSI) was measured using a tensile tester. The specific test process is as follows: the polymer electrolyte is cut into a 2 cm × 6 cm rectangular sheet, clamped in a tensile tester, and the cross-sectional area and thickness of the polymer electrolyte are input to form a tensile test curve. The results are shown in FIG. Figure 3 As shown by Figure 3 It can be seen that the mechanical strength of PVDF-HFP / LiTFSI / ASB is greater than that of PVDF-HFP / LiTFSI, which ensures the ability to suppress lithium dendrites during battery operation and the stability of the polymer electrolyte. The mechanical strength of the composite polymer electrolytes obtained in Example 1 and Example 3 was tested in the above manner, and the results are shown in Table 1 below.
[0062] (3) Lithium ion migration test of polymer electrolytes obtained in Example 2 (PVDF-HFP / LiTFSI / ASB) and Comparative Example 1 (PVDF-HFP / LiTFSI): Li + Migration number (t Li+ ), specifically using a 10mV polarization potential to measure the initial current (I0) and steady-state current (I s The initial interface resistance (R0) and steady-state interface resistance (R0) before and after electrostatic potential polarization were obtained by impedance measurement. s ). Li+ Calculated by the Bruce-Vincent-Evans equation, the results are as follows Figure 4 As shown by Figure 4 It can be seen that the lithium ion transference number of PVDF-HFP / LiTFSI / ASB is significantly higher than that of PVDF-HFP / LiTFSI.
[0063] The Bruce-Vincent-Evans equation is as follows:
[0064]
[0065] The lithium ion migration numbers of the composite polymer electrolytes obtained in Example 1 and Example 3 were tested in the above manner, and the results are shown in Table 1 below.
[0066] (4) Ionic conductivity test of the polymer electrolytes obtained in Example 2 (PVDF-HFP / LiTFSI / ASB) and Comparative Example 1 (PVDF-HFP / LiTFSI): The solid electrolyte was placed in a steel sheet-to-steel sheet battery and heated for 10 min. 6 The ohmic impedance Re of the battery is measured under -0.01Hz conditions. In addition, the thickness and contact area of the electrolyte are measured, and then the formula is used:
[0067]
[0068] Calculate the ionic conductivity. The result is, Figure 4 As shown, the ionic conductivity of the battery using the composite polymer electrolyte of Example 2 is significantly improved compared with that of the electrolyte of Comparative Example 1.
[0069] The ionic conductivity of the composite polymer electrolytes obtained in Example 1 and Example 3 was tested in the above manner, and the results are shown in Table 1 below.
[0070] Table 1:
[0071] Example Comparative Example 1 Example 1 Example 2 Example 3 Mechanical strength (MPa) 1.4 1.7 3.1 1.6 Lithium ion migration number 0.23 0.42 0.65 0.47 Ionic conductivity (mS / cm) 0.31 0.42 0.77 0.46
[0072] Effect example 2:
[0073] Performance test of lithium batteries assembled using the electrolytes obtained in Example 1 and Comparative Example 1. The battery was assembled using CR2025 button cells, with lithium iron phosphate LFP as the positive electrode material, lithium metal Li as the negative electrode material, and PVDF-HFP / LiTFSI / ASB and PVDF-HFP / LiTFSI as solid electrolytes, respectively.
[0074] (1) Lithium battery rate performance test: Neware instrument was used to perform constant current charge and discharge rate performance test of lithium battery in the voltage range of 2.5V to 4.2V. The current rate was set to 0.1C, 0.3C, 0.5C, 1C, 2C, 3C, 4C, and 0.1C. The results are as follows: Figure 5 As shown by Figure 5 It can be seen that the battery rate performance of the battery using the composite polymer electrolyte of Example 2 is significantly improved compared with the electrolyte of Comparative Example 1.
[0075] (2) Lithium battery cycle performance test: The lithium battery constant current charge and discharge cycle performance test was performed using a Neware instrument in the voltage range of 2.5V to 4.2V, with the current set to 1C (current density of 0.45mAcm -2 ), the result is as follows Figure 6 As shown by Figure 6 It can be seen that the battery cycle performance of the battery using the composite polymer electrolyte of Example 2 is improved compared with the battery cycle performance of the electrolyte of Comparative Example 1.
[0076] The battery cycle performance of the composite polymer electrolytes obtained in Example 1 and Example 3 was tested in the above manner, and the results are shown in Table 2 below.
[0077] Table 2:
[0078]
[0079] (3) Electrolyte stability test: current density 50 μA cm -2 The electroplating time is 1h. Figure 7 As shown by Figure 7 It can be seen that the polarization voltage of the battery using the composite polymer electrolyte of Example 2 is the smallest, indicating that the electrolyte PVDF-HFP / LiTFSI / ASB of Example 2 has the ability to inhibit lithium dendrites compared with the PVDF-HFP / LiTFSI electrolyte of Comparative Example 1.
[0080] (4) The SEM images of the lithium metal surface of the battery assembled with PVDF-HFP / LiTFSI / ASB and PVDF-HFP / LiTFSI as electrolyte after cycling are shown in Figure 2. Figure 8 and 9 As shown by Fig. 9 It can be seen that the lithium metal surface morphology of the lithium battery using PVDF-HFP / LiTFSI electrolyte is uneven, and lithium dendrites or dead lithium are obviously generated. Figure 8 It can be seen that the lithium metal surface morphology of the lithium battery using PVDF-HFP / LiTFSI / ASB electrolyte is uniform, which has the effect of inhibiting the growth of lithium dendrites.
[0081] The above description is only a preferred embodiment of the present invention. In view of the fact that technicians in the field of the present invention can make appropriate changes and modifications to the above implementation, the present invention is not limited to the specific implementation described above. Some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a composite polymer electrolyte that facilitates uniform lithium deposition, characterized in that: Here are the steps: S1, preparing a short fiber silicate mineral and dispersing it in a solvent I to obtain a short fiber silicate mineral dispersion; The operation process of S1 is as follows: dispersing the fibrous silicate mineral in ethanol, ball milling for 2-6 hours until the length of the fibrous silicate mineral is 1-20 μm, and then drying at 50-80° C. for 12-36 hours to obtain short fibrous silicate mineral, wherein the ball-to-material ratio during ball milling is (10-20):1, and the rotation speed is 300-600 r / min; S2, dissolving the fluorine-containing polymer in solvent I to obtain a polymer solution; S3, under a protective gas atmosphere, adding the lithium salt and short fiber silicate mineral dispersion to the high molecular polymer solution, and magnetically stirring for 6-12 h to obtain a composite solution; S4, coating the composite solution to form a film, and drying at 60-100° C. for 12-36 h to obtain a composite polymer electrolyte; The mass ratio of the fluorine-containing polymer, lithium salt, short fiber silicate mineral and solvent I in the composite solution is 1:0.8:(0.15-0.25):15; The fibrous silicate mineral is a mixture of one or more of serpentine asbestos, actinolite asbestos, hornblende asbestos, amosite, and tremolite asbestos in any proportion; The fluorine-containing high molecular polymer is one or more of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride-trifluoroethylene, and polyvinylidene fluoride-chlorotrifluoroethylene mixed in any proportion.
2. The method for preparing a composite polymer electrolyte that facilitates uniform lithium deposition according to claim 1, characterized in that: Solvent I is a mixture of one or more of dimethylformamide, dimethylacetamide, dimethyl sulfoxide and dimethyl pyrrolidone in any proportion.
3. The method for preparing a composite polymer electrolyte that facilitates uniform lithium deposition according to claim 1, characterized in that: The lithium salt is one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium difluorooxalatoborate mixed in any proportion.
4. The method for preparing a composite polymer electrolyte that facilitates uniform lithium deposition according to claim 1, characterized in that: The protective gas is argon or nitrogen.
5. A composite solid electrolyte prepared by the method according to claim 1.
6. A lithium battery, characterized in that: The lithium battery comprises the composite solid electrolyte according to claim 5.