A tough furandicarboxylic acid polyester and preparation method thereof
By using the copolymerization technology of flexible polyester and 2,5-furandicarboxylate in polyester materials, the molecular structure and molecular weight of the flexible polyester segment are regulated, and the problem of insufficient mechanical properties of materials in the prior art is solved. The preparation of high-performance block copolyester materials is realized to meet the application needs of packaging materials.
Patent Information
- Application Number
- CN202210959731.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-08-11
AI Technical Summary
In the modified polyester materials, the mechanical properties of the blending modification method are not significantly improved. The modification of a single flexible or rigid monomer causes the Young's modulus and glass transition temperature of the material to decrease, making it difficult to meet the application of packaging materials. Require.
Tough furandiformic acid polyester is prepared by copolymerizing flexible polyester with an average molecular weight of 1000 to 30000g/mol with 2,5-furandiformate. By regulating the molecular structure and molecular weight of the flexible polyester segment, it is combined with FDCA. , EG ratio, and block copolyester with excellent mechanical properties was prepared.
Achieve significant improvements in tensile strength, Young's modulus and elongation of break, reducing the impact of oxygen barrier properties caused by flexible polyester content, meeting the material performance requirements in various application fields, and simplifying the process flow and reducing production costs.
Smart Images

Figure QLYQS_1 
Figure BDA0003792219290000021 
Figure BDA0003792219290000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester copolymerization modification, and in particular to a tough furandicarboxylic acid polyester and a preparation method thereof. Background Art
[0002] Furandicarboxylic acid-based polyesters represented by polyethylene 2,5-furandicarboxylate (PEF) have high tensile strength and Young's modulus. At the same time, the furan ring in the molecular structure gives it outstanding barrier properties, and has broad application prospects in the field of packaging materials. However, furandicarboxylic acid-based polyesters have shortcomings such as poor toughness, low tensile elongation at break, and dark product color, which restrict their industrial application. For the development of PEF, existing technologies have made many attempts to modify it.
[0003] At present, there are two main types of PEF modification: one is macromolecular blending modification, and the other is small molecule copolymerization modification.
[0004] Regarding blending modification, some researchers used melt blending to prepare PBAT / PEF blends of poly(butylene terephthalate-adipate) (PBAT) modified PEF, but the improvement in mechanical properties was not obvious (New Journal of Chemistry, 2020, 44(7): 3112-3121.). In the patent application documents with patent publication numbers CN107964221B and CN104072954B, it was proposed to use additives to form PEF composites with certain improvements in mechanical properties, but the improvement effect is still not ideal.
[0005] Regarding copolymerization modification, it is generally believed that macromolecules are difficult to be used for copolymerization modification of PEF due to reasons such as reaction sites. Usually, small molecules are used for copolymerization modification, but often one property is sacrificed to improve another property. For example, when sebacic acid is copolymerized with furandicarboxylic acid (FDCA) and ethylene glycol (EG), although the elongation at break of the obtained copolymer can be increased from 3% of PEF to a maximum of 1500%, the corresponding Young's modulus of the copolymer decreases from 2080MPa of PEF to a minimum of 30MPa (RSC Adv., 2017, 7(23): 13798-13807.). When 2,2,4,4-tetramethyl-1,3-cyclobutanediol was copolymerized with FDCA and EG, the corresponding Young's modulus of the copolymer increased from 2800 MPa of PEF to 3300 MPa, but the elongation at break of the copolymer (4%) was not improved compared with the elongation at break of PEF (5%) (Polymers, 2017, 9(9): 305-320.). When ε-caprolactone was copolymerized with FDCA and EG, the elongation at break increased from 40% to 981% when the ε-caprolactone content increased from 30% to 40%, and the tensile strength decreased from 82 MPa to 51 MPa (European Polymer Journal, 2018, 109: 191-197.). The author disclosed in patent CN 108467479B that 2,5-furandicarboxylic acid, diols and cyclic lactones were used as raw materials to prepare PEF-based copolyesters with adjustable tensile strength and elongation at break. The tensile strength and elongation at break of the copolymer prepared with a molar ratio of FDCA to ε-caprolactone of 2:1 reached 97MPa and 337%, respectively. Since the elongation at break was significantly improved, the required content of modified monomers was high. The literature reported that when the content of aliphatic modifiers was increased from 18% to 34%, the oxygen barrier property of PEF-based polyester decreased by about half (Polymer, 2018, 155: 89-98.). Chinese patent CN108659209A discloses copolyesters made of 2,5-furandicarboxylic acid or its diester, ethylene glycol or propylene glycol and C4-30 α, ω-diol esters. The tensile elongation at break of the copolyester was significantly improved, but its tensile strength decreased to varying degrees (the decrease was 1-14%).Patents CN104072954B and CN107964221B disclose a composite method for preparing a composite material by blending PEF with a polymer. Patents CN108659209B, CN 114057998 B, CN 111454439B, CN 111286012B, CN 109810248B, CN109721716B, CN 110407991B, CN 110407991B, CN 109810248A, CN 109721716B, CN104341585B, CN 108264634 B, etc. disclose a preparation method and molding processing technology for preparing PEF polyester by copolymerizing PEF with a small molecule monomer.
[0006] It is not difficult to know that although existing patents or public technologies have proposed methods for modifying PEF, they all adopt the modification method of blending modification, copolymerization of flexible monomers, rigid monomers with furandicarboxylic acid and ethylene glycol. The blending modification method is simple, but the improvement of mechanical properties is not obvious; the use of a single flexible monomer to modify PEF can increase the elongation at break of polyester, but the Young's modulus and glass transition temperature of the material are significantly reduced; the use of a single rigid monomer to modify PEF can increase the tensile strength and Young's modulus of the polymer, but the elongation at break is not significantly improved. Although copolyesters with excellent mechanical properties can be prepared by copolymerizing ε-caprolactone with FDCA and EG, the required high content of modifiers will reduce the barrier properties of the copolyester, and it is still difficult to meet the application requirements of packaging materials. Summary of the invention
[0007] In view of the problems in the prior art that the blending modification method is simple, but the mechanical properties of the blend are not significantly improved, and the tensile strength, Young's modulus, elongation at break and glass transition temperature of PEF-based polyester modified by copolymerization of small molecular monomers are still difficult to meet the application requirements of packaging materials, the present invention provides a tough furandicarboxylic acid polyester and a preparation method thereof.
[0008] The technical solution adopted by the present invention is as follows:
[0009] A tough furandicarboxylic acid polyester, the tough furandicarboxylic acid polyester comprises a 2,5-furandicarboxylic acid ethylene glycol polyester segment and a flexible polyester segment, and its structural formula is as shown in Formula 1:
[0010]
[0011] Wherein, R is a flexible polyester segment, and m ranges from 2.5 to 680.
[0012] Preferably, the flexible polyester forming the flexible polyester segment R is one or more of poly(1,4-cyclohexanedimethanol terephthalate), poly(butylene adipate terephthalate), and polycaprolactone.
[0013] Furthermore, the preparation method of the flexible polyester segment R is: adding the monomers and catalyst required for preparing R into the reactor, reacting at normal pressure at 160-180°C for 2 hours under the protection of inert gas, raising the temperature to 220-250°C, reducing the pressure to 60-100 Pa, reacting for 0.5-4 hours, and preparing R with different molecular weights.
[0014] Preferably, the raw material ratios required for preparing R are as follows: (1) Preparation of poly(butylene terephthalate adipate): using adipic acid, terephthalic acid and 1,4-butanediol as monomers, the molar ratio of the three is 0.5:0.5:2, and the amount of catalyst tetrabutyl titanate is 0.1wt% of the total amount of diacids; (2) Preparation of poly(1,4-cyclohexanedimethanol terephthalate): using terephthalic acid and 1,4-cyclohexanedimethanol as monomers, the molar ratio is 1:2, and the amount of tetrabutyl titanate is 0.1wt% of terephthalic acid; (3) Preparation of polycaprolactone: using ε-caprolactone as monomer, the amount of tetrabutyl titanate is 0.1wt% of caprolactone.
[0015] Preferably, the content of R in the tough furandicarboxylic acid polyester is 10-50 wt%.
[0016] Furthermore, the content of R in the tough furandicarboxylic acid polyester is 20-40 wt%.
[0017] Preferably, the average molecular weight of R is 1000-30000 g / mol, and the average molecular weight of R is 3000-20000 g / mol, which has a better effect.
[0018] The preparation method of tough furandicarboxylic acid polyester as described in any one of the above items, wherein the preparation process is: 2,5-furandicarboxylic acid, ethylene glycol, and dibutyltin oxide are added into a reactor, and an esterification reaction is carried out at 160-230°C and normal pressure for 2-3 hours under the protection of an inert gas, and then a prepared flexible polyester R with a certain molecular weight is added, and the temperature is gradually increased to 230-280°C, and the pressure is gradually reduced to 60-100 Pa, and a polycondensation reaction is carried out for 2-8 hours to prepare a tough furandicarboxylic acid block copolyester.
[0019] Preferably, the polycondensation reaction time is 3 to 6 hours.
[0020] Preferably, in the preparation process of ethylene glycol 2,5-furandicarboxylate, the molar ratio of ethylene glycol to 2,5-furandicarboxylic acid is 1.2 to 2:1, and the amount of dibutyltin oxide is 0.1 to 0.5 wt % of the 2,5-furandicarboxylic acid.
[0021] In summary, compared with the prior art, the present invention has the following advantages and beneficial effects:
[0022] 1. The present invention is the first to use a flexible polyester with an average molecular weight of 1000-30000 g / mol and copolymerize ethylene glycol 2,5-furandicarboxylate to prepare a PEF modified material: tough furandicarboxylic acid polyester, which has excellent tensile strength, Young's modulus and elongation at break. The tensile strength can be regulated at 38-75 MPa, the Young's modulus can be regulated at 2680-3380 MPa, and the elongation at break can be regulated at 193-885%;
[0023] 2. The present invention can prepare block copolyesters with different molecular chain structures and mechanical properties by regulating the molecular structure and molecular weight of the flexible polyester and changing the ratio of the flexible polyester segment R to FDCA and EG, so as to facilitate adaptation to different working scenarios;
[0024] 3. The present invention can achieve brittle-tough transition when the flexible polyester content is low, significantly improve the elongation at break, and reduce the impact of oxygen barrier properties caused by excessive use of aliphatic modifiers;
[0025] 4. The present invention first prepares flexible polyesters with different structures and different molecular weights, and then copolymerizes the flexible polyesters with FDCA and EG, so as to control the structure of the PEF modified material;
[0026] 5. The PEF modified material prepared by the present invention has good heat resistance and meets the requirements of various application fields for material performance;
[0027] 6. The invention has mature technology, simple and convenient operation, stable product performance, low production cost, can meet the requirements of different application fields, is convenient for industrial production, and fills the gap in the prior art. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with various examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention, that is, the embodiments described are only part of the embodiments of the present invention, rather than all of the embodiments, and some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the protection scope of the present invention.
[0029] The raw materials used in the specific embodiments of the present invention are all commercially available. In order to ensure the experimental accuracy, the temperature control error of the reaction temperature of each embodiment and comparative example does not exceed 2°C, and the reaction pressure does not fluctuate by more than 10Pa.
[0030] Example 1
[0031] Preparation of flexible polyester polybutylene terephthalate adipate with a certain molecular weight. The molar ratio of adipic acid, terephthalic acid and 1,4-butanediol is 0.5:0.5:2, the amount of catalyst tetrabutyl terephthalate is 0.1wt% of the total amount of diacid, the esterification temperature is 180℃, the esterification time is 3h, the polycondensation temperature is 230℃, and the polycondensation pressure is 100Pa. The effect of polycondensation time on the average molecular weight of polybutylene terephthalate adipate is shown in Table 1.
[0032] Table 1 Effect of polycondensation time on the average molecular weight of polybutylene terephthalate adipate
[0033]
[0034] Example 2
[0035] Preparation of flexible polyester poly(1,4-cyclohexanedimethanol terephthalate) with an average molecular weight of 9900 g / mol. The molar ratio of terephthalic acid to 1,4-cyclohexanedimethanol is 1:2, the amount of catalyst tetrabutyl terephthalate is 0.1wt% of terephthalic acid, the esterification temperature is 220°C, the esterification time is 3h, the polycondensation temperature is 260°C, the polycondensation pressure is 100 Pa, and the polycondensation time is 3h.
[0036] Example 3
[0037] Preparation of flexible polyester polycaprolactone with an average molecular weight of 1100 g / mol. The monomer is ε-caprolactone, the amount of catalyst tetrabutyl tert-butyl ester is 0.1wt% of caprolactone, the ring-opening reaction is carried out at 200°C for 4h, the polycondensation temperature is 260°C, the polycondensation pressure is 100 Pa, and the polycondensation time is 2h.
[0038] Example 4
[0039] The copolyester was prepared by using polybutylene terephthalate adipate with an average molecular weight of 6800g / mol. The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol was 1:1.8, the mass fraction of the catalyst dibutyltin oxide was 0.25% of 2,5-furandicarboxylic acid, the mass fraction of polybutylene terephthalate adipate was 25%, the esterification temperature was 200℃, the esterification time was 4h, the polycondensation temperature was 230℃, the polycondensation pressure was 100Pa, and the polycondensation time was 8h. The obtained product had a glass transition temperature of 59.4℃, a tensile strength of 75.28MPa, a Young's modulus of 3351MPa, and an elongation at break of 193%.
[0040] Example 5
[0041] The copolyester was prepared by using polybutylene terephthalate adipate with an average molecular weight of 9950g / mol. The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol was 1:1.8, the mass fraction of the catalyst dibutyltin oxide was 0.25% of 2,5-furandicarboxylic acid, the mass fraction of polybutylene terephthalate adipate was 25%, the esterification temperature was 200℃, the esterification time was 4h, the polycondensation temperature was 230℃, the polycondensation pressure was 100Pa, and the polycondensation time was 8h. The obtained product had a glass transition temperature of 58.3℃, a tensile strength of 73.33MPa MPa, a Young's modulus of 3286MPa, and an elongation at break of 224%.
[0042] Example 6
[0043] The copolyester was prepared by using polybutylene terephthalate adipate with an average molecular weight of 24700g / mol. The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol was 1:1.8, the mass fraction of the catalyst dibutyltin oxide was 0.25% of 2,5-furandicarboxylic acid, the mass fraction of polybutylene terephthalate adipate was 25%, the esterification temperature was 200℃, the esterification time was 4h, the polycondensation temperature was 230℃, the polycondensation pressure was 100Pa, and the polycondensation time was 8h. The obtained product had a glass transition temperature of 56.1℃, a tensile strength of 72.07MPa MPa, a Young's modulus of 3212MPa, and an elongation at break of 287%.
[0044] Example 7
[0045] Preparation of copolyester with 30% polybutylene terephthalate adipate (average molecular weight of 24700g / mol). The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol is 1:1.8, the mass fraction of catalyst dibutyltin oxide is 0.25% of 2,5-furandicarboxylic acid, the mass fraction of polybutylene terephthalate adipate is 30%, the esterification temperature is 200℃, the esterification time is 4h, the polycondensation temperature is 230℃, the polycondensation pressure is 100Pa, and the polycondensation time is 8h. The obtained product has a glass transition temperature of 49.5℃, a tensile strength of 62.57MPa MPa, a Young's modulus of 3200MPa, and an elongation at break of 470%.
[0046] Example 8
[0047] Preparation of copolyester with 40% polybutylene terephthalate adipate (average molecular weight of 24700g / mol). The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol is 1:1.8, the mass fraction of catalyst dibutyltin oxide is 0.25% of 2,5-furandicarboxylic acid, the mass fraction of polybutylene terephthalate adipate is 40%, the esterification temperature is 200℃, the esterification time is 4h, the polycondensation temperature is 230℃, the polycondensation pressure is 100Pa, and the polycondensation time is 8h. The obtained product has a glass transition temperature of 37.7℃, a tensile strength of 38.92MPa MPa, a Young's modulus of 2953MPa, and an elongation at break of 608%.
[0048] Example 9
[0049] The copolyester was prepared by polycondensation of polybutylene terephthalate adipate with an average molecular weight of 24700g / mol for 6h. The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol was 1:1.8, the mass fraction of the catalyst dibutyltin oxide was 0.25% of 2,5-furandicarboxylic acid, the mass fraction of polybutylene terephthalate adipate was 25%, the esterification temperature was 200℃, the esterification time was 4h, the polycondensation temperature was 230℃, the polycondensation pressure was 100Pa, and the polycondensation time was 6h. The obtained product had a glass transition temperature of 47.8℃, a tensile strength of 59.75MPa MPa, a Young's modulus of 2964MPa, and an elongation at break of 415%.
[0050] Example 10
[0051] Copolyester was prepared by using poly(1,4-cyclohexanedimethanol terephthalate) with an average molecular weight of 9900g / mol. The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol was 1:1.8, the mass fraction of catalyst dibutyltin oxide was 0.25% of 2,5-furandicarboxylic acid, the mass fraction of poly(1,4-cyclohexanedimethanol terephthalate) was 25%, the esterification temperature was 200℃, the esterification time was 4h, the polycondensation temperature was 250℃, the polycondensation pressure was 100Pa, and the polycondensation time was 6h. The obtained product had a glass transition temperature of 64.8℃, a tensile strength of 76.42MPa MPa, a Young's modulus of 3383MPa, and an elongation at break of 218%.
[0052] Embodiment 11
[0053] The copolyester was prepared using polycaprolactone with an average molecular weight of 1100 g / mol. The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol was 1:1.8, the mass fraction of the catalyst dibutyltin oxide was 0.25% of 2,5-furandicarboxylic acid, the mass fraction of polycaprolactone was 25%, the esterification temperature was 200°C, the esterification time was 4h, the polycondensation temperature was 230°C, the polycondensation pressure was 100Pa, and the polycondensation time was 4h. The obtained product had a glass transition temperature of 52.8°C, a tensile strength of 58.42MPa MPa, a Young's modulus of 2683MPa, and an elongation at break of 317%.
[0054] Example 12
[0055] At the same time, poly(1,4-cyclohexane dimethanol terephthalate) with an average molecular weight of 9900 g / mol and poly(caprolactone) with an average molecular weight of 1100 g / mol were used to prepare copolyester. The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol was 1:1.8, the mass fraction of the catalyst dibutyltin oxide was 0.25% of 2,5-furandicarboxylic acid, the mass fraction of poly(1,4-cyclohexane dimethanol terephthalate) was 20%, the mass fraction of poly(caprolactone) was 20%, the esterification temperature was 200°C, the esterification time was 4h, the polycondensation temperature was 250°C, the polycondensation pressure was 100Pa, and the polycondensation time was 8h. The obtained product had a glass transition temperature of 48°C, a tensile strength of 49.38MPa MPa, a Young's modulus of 2960MPa, and an elongation at break of 885%.
[0056] Comparative Example 1
[0057] The molar ratio of 2,5-furandicarboxylic acid to ethylene glycol is 1:1.8, the mass fraction of the catalyst dibutyltin oxide is 0.25% of 2,5-furandicarboxylic acid, the esterification temperature is 200°C, the esterification time is 4h, the polycondensation temperature is 230°C, the polycondensation pressure is 100Pa, and the polycondensation time is 8h. The obtained product has a glass transition temperature of 87.4°C, a tensile strength of 40.34MPa, a Young's modulus of 3937MPa, and an elongation at break of 10%.
[0058] From the results of the above examples 1-12 and comparative example 1, it can be concluded that the tough furandicarboxylic acid polyester and the preparation method thereof provided by the present invention can prepare block copolyesters with different molecular chain structures and mechanical properties by regulating the molecular weight and molecular structure of the flexible polyester, changing the ratio of the flexible polyester to FDCA and EG, and controlling the copolymerization process. When the content of the flexible polyester is low, the brittle-tough transition can be achieved, and the elongation at break is significantly improved.
[0059] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. A tough furandicarboxylic acid polyester, characterized in that: The tough furandicarboxylic acid polyester comprises a 2,5-furandicarboxylic acid ethylene glycol polyester segment and a flexible polyester segment, and its structural formula is as shown in Formula 1: Formula 1 Wherein, R is a flexible polyester segment, and m ranges from 2.5 to 680; the flexible polyester forming the flexible polyester segment R is poly(1,4-cyclohexanedimethanol terephthalate) with an average molecular weight of 9900 g / mol and poly(caprolactone) with an average molecular weight of 1100 g / mol; the preparation process of the tough furandicarboxylic acid polyester is as follows: 2,5-furandicarboxylic acid, ethylene glycol, and dibutyltin oxide are added into a reactor, the molar ratio of 2,5-furandicarboxylic acid to ethylene glycol is 1:1.8, and the catalyst dibutyltin oxide is used as catalyst; The mass fraction of tin oxide is 0.25% of 2,5-furandicarboxylic acid; under the protection of inert gas, esterification reaction is carried out at 160-230°C and normal pressure for 2-3 hours, and then poly(1,4-cyclohexanedimethanol terephthalate) and poly(caprolactone) are added for polycondensation reaction, the mass fraction of poly(1,4-cyclohexanedimethanol terephthalate) is 20%, the mass fraction of poly(caprolactone) is 20%, the polycondensation temperature is 250°C, the polycondensation pressure is 100Pa, and the polycondensation time is 8 hours to prepare tough furandicarboxylic acid block copolyester.
2. The tough furandicarboxylic acid polyester according to claim 1, characterized in that: The preparation process of the poly(1,4-cyclohexanedimethanol terephthalate) is as follows: terephthalic acid and 1,4-cyclohexanedimethanol are used as monomers in a molar ratio of 1:2, the amount of tetrabutyl titanate is 0.1wt% of terephthalic acid, the esterification temperature is 220°C, the esterification time is 3h, the polycondensation temperature is 260°C, the polycondensation pressure is 100Pa, and the polycondensation time is 3h; the preparation process of the polycaprolactone is as follows: the monomer is Ɛ-caprolactone, the amount of catalyst tetrabutyl titanate is 0.1wt% of caprolactone, the ring-opening reaction is carried out at 200°C for 4h, the polycondensation temperature is 260°C, the polycondensation pressure is 100Pa, and the polycondensation time is 2h.
3. A method for preparing tough furandicarboxylic acid polyester as claimed in claim 1 or 2, characterized in that: The preparation process is as follows: 2,5-furandicarboxylic acid, ethylene glycol and dibutyltin oxide are added into a reactor, and an esterification reaction is carried out at 160-230°C and normal pressure for 2-3 hours under the protection of an inert gas, and then poly(1,4-cyclohexanedimethanol terephthalate) and polycaprolactone are added for a polycondensation reaction, with a polycondensation temperature of 250°C, a polycondensation pressure of 100 Pa and a polycondensation time of 8 hours to prepare a tough furandicarboxylic acid block copolyester.
Citation Information
Cited By
Preparation method and application of bio-based furan polyester with high gas barrier property
CN120504821A
Preparation method and application of a high-gas-barrier bio-based furan polyester
CN120504821B