A method for producing a glittering terry fabric and a glittering terry fabric
Through the use of Sailo ring spinning technology and the use of special double-hole flares, the content of photochemical fibers is reduced, the gloss effect and performance problems in terry fabrics are solved, and the production of softer, fluffy and glossy flash terry fabrics is achieved. .
Patent Information
- Application Number
- CN202211229140.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-10-08
AI Technical Summary
In the prior art, a high proportion of photochemical fibers will affect the fluffy, softness, water absorption and anti-blasting properties of the terry fabric. Chemical fibers below 50% will lead to weak gloss effect, and the terry is not upright and the product Not fluffy.
The Silo ring spinning method is used to mix different quantities of pure cotton rovings and photochemical fiber rovings, and spin them through a special asymmetric double-hole trumpet to make flash Silo yarns and interwoven with conventional cotton yarns to reduce the The content of photochemical fibers while improving the softness and gloss effect of terry fabrics.
While reducing the amount of photochemical fibers, it maintains or improves the gloss effect, soft feel, fluffy and water absorption of the terry fabric. It is not easy to bleach after multiple washings, and it is not easy to bleach, and the terry flickering effect under the light is obvious. .
Smart Images

Figure CN115538009B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, in particular to a method for producing a shiny terry fabric and the shiny terry fabric. Background Art
[0002] In the related art, conventional terry fabrics with a glossy appearance are generally made by blending glossy chemical fibers with cotton fibers in a ratio greater than 30% to obtain a blended yarn as terry yarn, which is then further used to make terry fabrics. Terry fabrics with a glossy effect are obtained through dyeing and finishing, which usually requires mixing in a higher ratio (more than 30%) of glossy chemical fibers. However, a high ratio of chemical fibers will affect the practical properties of terry fabric products, such as fluffiness, softness, water absorption, and resistance to pilling, making it difficult to meet the needs of consumers. At the same time, if the content of glossy chemical fibers in the terry fabric is less than 50%, the luster will be weak, the visual perception will be difficult, the terry will not stand upright, and the product will not be fluffy. If the content of glossy chemical fibers exceeds 50%, the product will feel slippery, the cotton feel will be lost, the water absorption will deteriorate, the appearance will have long hairiness, it will be easy to pill after washing, the terry will not be firmly clamped, and it will be easy to be pulled out.
[0003] Therefore, there is an urgent need for a new method for producing shiny terry fabrics that can reduce the content of photochemical fibers while ensuring the gloss effect and the cotton feel, water absorption and other properties of the product. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0005] To this end, an object of the present invention is to provide a method for producing a shiny terry fabric and a shiny terry fabric. The shiny terry yarn is obtained as the terry yarn by using a special siro ring spinning method to spin coarse yarns of different quantities, thereby effectively reducing the amount of shiny chemical fiber used. The terry yarn is interwoven with ground warp yarn and weft yarn to form a terry fabric. The terry fabric has a soft and fluffy hand feel and a better terry spiral effect. The terry has a more obvious shiny effect under light or sunlight, has a smooth appearance, and has excellent water absorption and feather shedding rate. It is not easy to pill or lint after repeated washing.
[0006] In order to achieve the above-mentioned purpose, the technical scheme of the first aspect of the present invention provides a method for producing a shiny terry fabric, comprising the following steps: (1) a cotton spinning process processes pure cotton roving and optical chemical fiber roving respectively, and the quantitative ratio thereof is 4:1 to 3:1; (2) a spun yarn process adopts a siro ring spinning method, a pure cotton roving and a optical chemical fiber roving are fed into a special double-hole bell mouth at the same time, and the special double-hole bell mouth presents an asymmetric double-inlet and single-outlet structure, and then the shiny siro yarn is obtained after being drafted, twisted and wound by the front roller, the middle roller and the back roller. The twist coefficient of the twin yarn is 283 to 371; (3) the twin yarn in step (2) is used as the terry yarn, and conventional cotton yarn is used as the ground warp and weft yarn to weave a terry fabric on a towel loom, wherein the height of the terry fabric is not less than 15 cm / 10 terry loops; (4) the terry fabric is brushed to obtain a pre-spiral direction, and then the terry fabric is cold-stalled and allowed to stand at room temperature for 2 to 12 hours; (5) the brushed terry fabric is desized, bleached, dyed, polished, softened, dehydrated, dried, cut and sewn to obtain a finished twinkle terry fabric.
[0007] In this technical solution, the cotton spinning process processes two kinds of rovings with different quantitative ratios respectively, and the quantitative ratio of pure cotton roving and photochemical fiber roving is 4:1-3:1. By adopting the siro ring spinning method, a pure cotton roving and a photochemical fiber roving are fed into a special double-hole trumpet at the same time. The special double-hole trumpet presents an asymmetric double-input and single-output structure, and then the flash siro yarn is obtained after being drafted, twisted and wound by the front roller, the middle roller and the back roller. The twist coefficient of the flash siro yarn is 283-371. It can spin two kinds of coarse yarns with different quantitative quantities, and the yarn quality is good, the machine breakage is reduced, the yarn has less hairiness, higher strength, low strength CV value, and obvious ply style, thereby reducing the content of photochemical fibers. At the same time, compared with conventional terry fabrics with flashing effects, the cotton fiber content is relatively high, the natural texture is better, and it has a more obvious flashing effect under light or sunlight, and it feels more fluffy and has a smoother appearance. It is not easy to pilling and hair extraction after multiple washings. With flash siro yarn as terry yarn and conventional cotton yarn as warp and weft yarn, terry fabric grey cloth is woven on a towel loom. The terry height of the terry fabric grey cloth is not less than 15cm / 10 terry loops, ensuring the beauty, softness and low feather shedding rate of the terry fabric. The terry fabric grey cloth is brushed to obtain a pre-spiral direction, and then cold-piled and allowed to stand at room temperature for 2 to 12 hours to improve the terry spiral effect. The brushed terry fabric grey cloth is desized, bleached, dyed, polished, softened, dehydrated, dried, cut and sewn to obtain a finished shiny terry fabric. Compared with traditional pure cotton terry fabric, the finished shiny terry fabric has a softer and fluffier hand feel, a better terry spiral effect, and the terry has a faint shiny effect under light or sunlight, and also has excellent water absorption and feather shedding rate performance.
[0008] In the above technical solution, preferably, the distance between the two inlet holes in the special double-hole bell mouth is 4 mm to 5 mm.
[0009] In this technical solution, since the quantitative difference between pure cotton roving and photochemical fiber roving is large and it is not easy to form yarn, a special double-hole trumpet with an asymmetric double-inlet and single-outlet structure is adopted, and the spacing between the two inlet holes is designed to be 4mm~5mm, so that pure cotton roving and photochemical fiber roving with large quantitative difference can be spun into yarn by siro ring spinning, the yarn quality is good, the machine breakage is reduced, the yarn has less hairiness, higher strength, low strength CV value, and obvious ply style.
[0010] In any of the above technical solutions, preferably, in the spinning process, the diameter of the roller on the rear roller at the end of the low-weight photochemical fiber roving is increased by 0.5mm-1.0mm relative to the end of the high-weight pure cotton roving;
[0011] In the spinning process, the false twist device is used to add false twist to the sliver output by the front roller, so as to change the fiber distribution on the yarn surface in the twisting triangle area and control the yarn twist coefficient.
[0012] In this technical solution, the diameter of the low-quantity photochemical fiber roving end of the top roller of the rear roller in the spinning process is increased by 0.5mm-1.0mm relative to the high-quantity pure cotton roving end, further ensuring that the two rovings can be spun with good quality when the quantitative difference is large, reducing the decline in drafting efficiency caused by slippery drafting and the problem of "hard head" in roving, and further reducing the occurrence of broken ends. The false twist device adds false twist to the whiskers output by the front roller, changes the fiber distribution on the yarn surface in the twisting triangle area, controls the yarn twist coefficient, and makes the twist coefficient of the flash siro yarn 283-371, making the terry fabric product fluffy and soft.
[0013] In any of the above technical solutions, preferably, the weight of the pure cotton roving is 8g / 10m-9g / 10m, the weight of the photochemical fiber roving is 2g / 10m-3g / 10m, and the count of the flash siro yarn is 36.4tex.
[0014] In this technical solution, the quantitative weight of pure cotton roving, the quantitative weight of photochemical fiber roving, and the yarn count of flash siro yarn are optimized, which is further conducive to reducing the amount of photochemical fiber used, while ensuring the flash effect and the inherent properties of terry fabric such as fluffiness and softness.
[0015] In any of the above technical solutions, preferably, the brushing process parameters in step (4) are: brushing speed 15m / min, water temperature 20℃~50℃.
[0016] In this technical solution, the brushing process parameters are further optimized, and the spiral effect of the terry loops is further improved, which is beneficial to improving the flashing effect of the terry loops.
[0017] The technical solution of the second aspect of the present invention provides a terry fabric, which is produced by the method for producing the shiny terry fabric in the above technical solution and has all the beneficial technical effects of the method for producing the shiny terry fabric in the above technical solution, which will not be repeated here.
[0018] In the above technical solution, preferably, the terry yarn in the flash terry fabric is a siro-spun structure containing photochemical fibers and cotton fibers, and the weight percentage of the photochemical fibers in the terry yarn is 20% to 25%.
[0019] In this technical solution, the content of photochemical fibers in the flashing terry fabric is significantly reduced, the cotton fiber content is relatively high, the natural texture is better, the hand feels fluffy, the appearance is smooth, and it is not easy to pilling or shedding after repeated washing. At the same time, the flashing effect is obvious under light or sunlight, and can achieve the same flashing effect as conventional terry fabric with a flashing effect, or even a better flashing effect.
[0020] The present invention provides a method for producing a glittering terry fabric and a glittering terry fabric having the following beneficial technical effects:
[0021] (1) The present invention proposes a method for producing a shiny terry fabric, wherein rovings of different quantities are siro-spun in a special siro ring spinning method to obtain shiny siro yarn as terry yarn, which effectively reduces the amount of shiny chemical fiber. When the amount of shiny chemical fiber is 20%-25%, a better shiny effect can be achieved. Moreover, the terry yarn is interwoven with the ground warp yarn and the weft yarn to form a terry fabric, which has a soft and fluffy feel and a better terry spiral effect. The terry has a more obvious shiny effect under light or sunlight, has a smooth appearance, and has excellent water absorption and feather removal performance. It is not easy to pill and lint after multiple washings.
[0022] (2) The present invention proposes a method for producing a flash terry fabric by adopting a special double-hole trumpet with an asymmetric double-inlet and single-outlet structure, and designing the inlet hole spacing to be 4mm-5mm, and increasing the diameter of the low-quantity photochemical fiber roving end roller of the rear roller in the spun yarn process by 0.5mm-1.0mm relative to the high-quantity pure cotton roving end, etc., so that two rovings of different quantities can be fed into yarn, and the yarn quality is good, the machine is not prone to end breakage, the roving is not prone to deviation, the ply style is obvious, the yarn strength is high, the yarn hairiness is less, and the strength CV value is low.
[0023] (3) Compared with traditional pure cotton terry fabric, the glittering terry fabric made by the glittering terry fabric production method proposed in the present invention has a softer and fluffier hand feel, a better terry spiral effect, and a faint glittering effect under light. At the same time, the towel has excellent water absorption and feather shedding performance. Compared with conventional terry fabric with glittering effect, the glittering terry fabric has a higher cotton fiber content, a better natural texture, a more obvious glittering effect under light or sunlight, a fluffier hand feel, a smoother appearance, and is not easy to pilling or shedding after repeated washing.
[0024] Additional aspects and advantages of the present invention will be given in part in the following description, and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0026] Figure 1 The structure schematic diagram of the double-hole bell mouth in the prior art is shown;
[0027] Figure 2 A schematic structural diagram of a special double-hole bell mouth in a method for producing a flashing terry fabric according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0028] The present invention discloses a method for producing a glitter terry fabric and a glitter terry fabric. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application described herein without departing from the content, spirit and scope of the present invention to achieve and apply the technology of the present invention.
[0029] The present invention will be further described below in conjunction with embodiments:
[0030] Example 1
[0031] The invention discloses a method for producing a shiny terry fabric. The terry yarn is a shiny siro yarn of shiny viscose fiber and cotton fiber, wherein the content of the shiny viscose fiber is 20%.
[0032] The following steps are involved:
[0033] S102, in a cotton spinning process, a pure cotton roving with a basis weight of 8 g / 10 m and a glossy viscose fiber roving with a basis weight of 2 g / 10 m are spun according to conventional technical processes;
[0034] S104, two rovings are fed in parallel into the special double-hole bell mouth of the Siro spinning frame, and the special double-hole bell mouth has an asymmetric double-inlet and single-outlet structure, such as Figure 2 As shown in the figure, the special double-hole bell mouth presents an asymmetric double-inlet and single-outlet structure, and then the flash siro yarn is made after being drafted, twisted and wound by the front roller, the middle roller and the back roller. The flash siro yarn has a yarn count of 36.4tex, a twist of 55t / dm, a bright viscose fiber content of 20%, and a cotton fiber content of 80%.
[0035] Specifically, in the spinning process, the diameter of the roller on the rear roller of the low-quantity photochemical fiber roving end is increased by 0.5mm-1.0mm relative to the high-quantity pure cotton roving end; in the spinning process, the false twist device is used to increase the false twist of the sliver output from the front roller, change the fiber distribution on the yarn surface in the twisting triangle area, and control the yarn twist coefficient. It should be noted that the following is used: Figure 1 As shown, the double-hole bell mouth structure in the prior art is difficult to realize the blending of two rovings with different quantitative quantities into yarns, and is prone to high-frequency yarn breakage, slippery drafting, etc., resulting in the inability to spin normally.
[0036] S106, using the above-mentioned flash siro yarn as the terry yarn, and conventional cotton yarn as the ground warp and weft yarn, to weave a terry fabric grey cloth on a towel loom, wherein the terry fabric grey cloth has a terry height of 17.0 cm / 10 terry loops;
[0037] S108, the terry fabric grey cloth is pressed with water by a roller with a brush and a movement direction at 90 degrees to the cloth travel direction, the roller speed is 15m / min, the water temperature is 20℃~50℃, to ensure that the terry fabric has uniform spiral loops, and then cold stacked and left to stand at room temperature for 2 hours;
[0038] S110, desizing the terry fabric according to conventional dyeing and finishing technology, loading it into an overflow machine for bleaching and dyeing, polishing and softening according to conventional process technology, and then dehydrating, drying, cutting and sewing to obtain a finished shiny terry fabric.
[0039] Example 2
[0040] The invention discloses a method for producing a shiny terry fabric. The terry yarn is a shiny siro yarn of shiny viscose fiber and cotton fiber, wherein the content of the shiny viscose fiber is 25%.
[0041] The following steps are involved:
[0042] S202, in the cotton spinning process, a pure cotton roving with a basis weight of 9 g / 10 m and a glossy viscose fiber with a basis weight of 3 g / 10 m are spun according to conventional technical processes;
[0043] S204, two rovings are fed in parallel into the special double-hole bell mouth of the Siro spinning frame, and the special double-hole bell mouth has an asymmetric double-inlet and single-outlet structure, such as Figure 2As shown in the figure, the special double-hole bell mouth presents an asymmetric double-inlet and single-outlet structure, and then the flash siro yarn is made after being drafted, twisted and wound by the front roller, the middle roller and the back roller. The flash siro yarn has a yarn count of 36.4tex, a twist of 60t / dm, a bright viscose fiber content of 25%, and a cotton fiber content of 75%.
[0044] Specifically, in the spinning process, the diameter of the roller on the rear roller of the low-quantity photochemical fiber roving end is increased by 0.5mm-1.0mm relative to the high-quantity pure cotton roving end; in the spinning process, the false twist device is used to increase the false twist of the sliver output from the front roller, change the fiber distribution on the yarn surface in the twisting triangle area, and control the yarn twist coefficient. It should be noted that the following is used: Figure 1 As shown, the double-hole bell mouth structure in the prior art is difficult to realize the blending of two rovings with different quantitative quantities into yarns, and is prone to high-frequency yarn breakage, slippery drafting, etc., resulting in the inability to spin normally.
[0045] S206, using the above-mentioned flash siro yarn as the terry yarn, and conventional cotton yarn as the ground warp and weft yarn, to weave a terry fabric grey cloth on a towel loom, wherein the terry fabric grey cloth has a terry height of 15.0 cm / 10 terry loops;
[0046] S208, the terry fabric grey cloth is pressed with water by a roller with a brush and a movement direction at 90 degrees to the cloth travel direction, the roller speed is 15m / min, the water temperature is 20℃~50℃, to ensure that the terry fabric has uniform spiral loops, and then cold stacked and left to stand at room temperature for 2 hours;
[0047] S210, desizing the terry fabric according to conventional dyeing and finishing technology, loading it into an overflow machine for bleaching and dyeing, polishing and softening according to conventional process technology, and then dehydrating, drying, cutting and sewing to obtain a finished shiny terry fabric.
[0048] Example 3
[0049] The invention discloses a method for producing a shiny terry fabric. The terry yarn is a shiny siro yarn of shiny modal fiber and cotton fiber, wherein the content of the shiny modal fiber is 25%.
[0050] The following steps are involved:
[0051] S302, in a cotton spinning process, a pure cotton roving with a basis weight of 9 g / 10 m and a bright modal fiber with a basis weight of 3 g / 10 m are spun respectively according to conventional technical processes;
[0052] S304, two rovings are fed in parallel into the special double-hole bell mouth of the Siro spinning frame, and the special double-hole bell mouth has an asymmetric double-inlet and single-outlet structure, such as Figure 2As shown in the figure, the special double-hole bell mouth presents an asymmetric double-inlet and single-outlet structure, and then the flash siro yarn is made after being drafted, twisted and wound by the front roller, the middle roller and the back roller. The flash siro yarn has a yarn count of 36.4tex and a twist of 60t / dm. The content of bright modal fiber is 25%, and the content of cotton fiber is 75%.
[0053] Specifically, in the spinning process, the diameter of the roller on the rear roller of the low-quantity photochemical fiber roving end is increased by 0.5mm-1.0mm relative to the high-quantity pure cotton roving end; in the spinning process, the false twist device is used to increase the false twist of the sliver output from the front roller, change the fiber distribution on the yarn surface in the twisting triangle area, and control the yarn twist coefficient. It should be noted that the following is used: Figure 1 As shown, the double-hole bell mouth structure in the prior art is difficult to realize the blending of two rovings with different quantitative quantities into yarns, and is prone to high-frequency yarn breakage, slippery drafting, etc., resulting in the inability to spin normally.
[0054] S306, using the above-mentioned flash siro yarn as the terry yarn, and conventional cotton yarn as the ground warp and weft yarn, to weave a terry fabric grey cloth on a towel loom, wherein the terry fabric grey cloth has a terry height of 15.0 cm / 10 terry loops;
[0055] S308, the terry fabric grey cloth is pressed with water by a roller with a brush and a movement direction at 90 degrees to the cloth travel direction, the roller speed is 15m / min, the water temperature is 20℃~50℃, to ensure that the terry fabric has uniform spirals, and then cold stacked at room temperature for 2 hours;
[0056] S310, desizing the terry fabric according to conventional dyeing and finishing technology, loading it into an overflow machine for bleaching and dyeing, polishing and softening according to conventional process technology, and then dehydrating, drying, cutting and sewing to obtain a finished shiny terry fabric.
[0057] The performance tests were conducted on Examples 1 to 3, the pure cotton terry fabric in the prior art, and the conventional terry fabric with a glittering effect. The test results are shown in Table 1 below:
[0058] Table 1 Test results of terry fabric finished products
[0059]
[0060] As can be seen from Table 1, the flash terry fabric made by the present invention is softer and fluffier than the traditional pure cotton terry fabric, and the terry spiral effect is better. The terry has a faint flash effect under the light, and the towel has excellent water absorption and feather shedding rate performance; compared with the conventional terry fabric with a flash effect, the cotton fiber content is higher, the natural texture is better, the flash effect is more obvious under light or sunlight, the hand feels fluffier, the appearance is smoother, and it is not easy to pilling or hair pulling after repeated washing.
[0061] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for producing a glittering terry fabric, characterized in that: The following steps are involved: (1) The cotton spinning process processes pure cotton roving and optical chemical fiber roving respectively, and the quantitative ratio thereof is 4:1 to 3:1; (2) The spinning process adopts Siro ring spinning, wherein a pure cotton roving and a photochemical fiber roving are simultaneously fed into a special double-hole bell mouth, wherein the special double-hole bell mouth has an asymmetric double-inlet and single-outlet structure, and then the front roller, middle roller and back roller are used for drafting, twisting and winding to obtain the flash Siro yarn, wherein the twist coefficient of the flash Siro yarn is 283-371; (3) using the flash siro yarn in step (2) as the terry yarn and conventional cotton yarn as the ground warp and weft yarns to weave a terry fabric grey cloth on a towel loom, wherein the terry height of the terry fabric grey cloth is not less than 15 cm / 10 terry loops; (4) brushing the terry fabric to obtain a pre-spiral direction, and then cold-stacking and standing at room temperature for 2 to 12 hours; (5) desizing, bleaching, dyeing, polishing, softening, dehydrating, drying, cutting and sewing the brushed terry fabric to obtain a finished shiny terry fabric.
2. The method for producing a glittering terry fabric according to claim 1, characterized in that: The distance between the two inlet holes in the special double-hole bell mouth is 4mm to 5mm.
3. The method for producing a glittering terry fabric according to claim 2, characterized in that: In the spinning process, the diameter of the roller on the rear roller at the end of the low-weight photochemical fiber roving is 0.5mm-1.0mm larger than that of the high-weight pure cotton roving. In the spinning process, the false twist device is used to add false twist to the sliver output by the front roller, so as to change the fiber distribution on the yarn surface in the twisting triangle area and control the yarn twist coefficient.
4. The method for producing a shiny terry fabric according to any one of claims 1 to 3, characterized in that: The quantitative weight of pure cotton roving is 8g / 10m~9g / 10m, the quantitative weight of photochemical fiber roving is 2g / 10m~3g / 10m, and the count of flash siro yarn is 36.4tex.
5. The method for producing a glittering terry fabric according to claim 4, characterized in that: The brushing process parameters in step (4) are: brushing speed 15m / min, water temperature 20℃~50℃.
6. A glittering terry fabric, characterized in that: The glitter terry fabric is produced by the method for producing the glitter terry fabric according to any one of claims 1 to 5.
7. The glittering terry fabric according to claim 6, characterized in that: The terry yarn in the flash terry fabric is a siro-spun structure containing photochemical fiber and cotton fiber, and the weight percentage of the photochemical fiber in the terry yarn is 20% to 25%.