Thermal recording materials

By using the compound Ar1-NH-CO-NH-C6H4-SO2-O-C6H4-NH-CO-NH-Ar2 as a color developer, combined with fluoran-type dyes and fatty acid amides, the problem of heat-sensitive recording materials in high humidity and The problem of decomposition under high temperature conditions is achieved, the image density is maintained and the durability is improved, and the dependence on high-cost components is avoided.

CN115666957BActive Publication Date: 2024-10-29KOEHLER INNOVATION & TECH GMBH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202180033419.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-10-29
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

When existing thermal recording materials are stored under high humidity and high temperature conditions, non-phenolic color developers are prone to decomposition, resulting in reduced image durability and dynamic responsiveness, and rely on special formula ingredients to improve stability, but these ingredients are costly or limited availability.

Method used

The compound Ar1-NH-CO-NH-C6H4-SO2-O-C6H4-NH-CO-NH-Ar2 is used as the color developer, combined with sensitizers such as fluoran dyes and fatty acid amides to form heat-sensitive recording materials, which avoids It eliminates reliance on specially formulated ingredients and improves image durability and storage stability.

Benefits of technology

It achieves the maintenance of image density during long-term storage under high humidity and high temperature conditions, significantly improves image durability, avoids dependence on high-cost or low-availability ingredients, and ensures the high quality of thermal printer output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003971238360000061
    Figure GDA0003971238360000061
  • Figure GDA0003971238360000062
    Figure GDA0003971238360000062
  • Figure GDA0003971238360000071
    Figure GDA0003971238360000071
Patent Text Reader

Abstract

The present invention describes a color developer of formula (I), Ar 1 NH‑CO‑NH‑C 6 H 4 ‑SO 2 ‑O‑C 6 H 4 ‑NH‑CO‑NH‑Ar 2 (I) A heat-sensitive recording material comprising a carrier substrate and a heat-sensitive color-forming layer, the heat-sensitive color-forming layer containing at least one color-forming agent and at least one phenol-free color developer, wherein the at least one color developer is a compound of formula (I), and a method for preparing such a heat-sensitive recording material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a color developer, to a heat-sensitive recording material comprising a carrier substrate and a heat-sensitive color-forming layer containing at least one color former and at least one phenol-free color developer, and to a method for preparing such a heat-sensitive recording material. Background Art

[0002] Thermal recording materials (thermal papers) for direct thermal printing applications have long been known which have a thermally sensitive color-forming layer (thermoreactive layer) applied to a carrier substrate.

[0003] The thermosensitive color-forming layer usually contains a color former and a color developer, which react with each other under the influence of heat, thereby resulting in color development. Inexpensive (bis)phenol color developers, such as bisphenol A and bisphenol S, are widely used and can be used to obtain thermosensitive recording materials with acceptable performance conditions for a variety of applications. The following thermosensitive recording materials are also known, which contain non-phenol color developers in the thermosensitive color-forming layer. These thermosensitive recording materials are all developed to improve the durability of the typeface, especially if the printed thermosensitive recording material is to be stored for a long time at higher temperatures and / or humidity. In particular, against the background of public discussion on the potential toxicity of (bis)phenol chemicals, interest in non-phenol color developers has risen sharply. The purpose here is to avoid the disadvantages of (bis)phenol color developers, but at least maintain and preferably improve the technical performance characteristics that can be achieved using phenol color developers.

[0004] Despite the enormous chemical diversity of non-phenolic color developers, the prior art regarding these materials exhibits common structural features.

[0005] For example, a 1,3-disubstituted (thio)urea substructure (Y-NH-C(X)-NH-Z, where X = S or O) is a common feature of a large number of non-phenolic color developers. Functional properties related to suitability as a color developer can be adjusted by appropriate selection of the Y and Z groups.

[0006] Sulfonylurea structure (-SO 2 Color developers containing NH-CO-NH-) are widely used because they are relatively easy to prepare and the heat-sensitive recording materials prepared by them have good application characteristics.

[0007] EP 0 526 072 A1 and EP 0 620 122 B1 disclose color developers of aromatic sulfonyl (thio) urea type. With these color developers, the following heat-sensitive recording materials can be obtained, which are characterized by having relatively high image durability. In addition, the heat-sensitive recording materials based on these color developers have usable heat sensitivity with good surface whiteness, so if the formulation of the heat-sensitive color-forming layer is appropriately designed, it is relatively easy to prepare high printing density using a commercially available thermal printer.

[0008] WO 0 035 679 A1 discloses a compound of the formula Ar'-SO 2 -NH-C(X)-NH-Ar aromatic and heteroaromatic sulfonyl (thio) urea compounds (X = S or O) and / or sulfonyl guanidine (X = NH), wherein Ar is linked to the other aromatic group through a divalent linking group. One non-phenolic color developer in this class, 4-methyl-N-(((3-(((4-methylphenyl)sulfonyl)oxy)phenyl)amino)carbonyl)benzenesulfonamide (trade name Pergafast BASF), which is widely used in practice, is characterized in that the application properties of the heat-sensitive recording materials prepared using this color developer are balanced. In particular, these materials have good dynamic responsiveness and, compared with recording materials obtained using (bis)phenol-type color developers, have higher printing durability when stored under harsh environmental conditions or with respect to hydrophobic substances.

[0009] Sulfonylureas tend to undergo hydrolytic decomposition reactions in the presence of water / moisture and at elevated temperatures (M. Eckhardt, TJ Simat, Chemosphere, 186, 1016 (2017)). Therefore, when stored in an unprinted state under elevated humidity and / or temperature conditions, the thermosensitive recording material may experience partial decomposition of the color developer.

[0010] Since the writing performance (dynamic responsiveness) of a thermosensitive recording material depends on the amount of color developer present in the thermosensitive layer, a thermosensitive recording material stored for a long time loses part of the color developer and thus loses some of its writing performance.

[0011] The above-mentioned possibility of adjusting the properties of the 1,3-disubstituted (thio)urea substructure can also be achieved by including structural units which are advantageously conjugated with the urea unit.

[0012] Such an approach is used, for example, in EP 2 923 851 A1. For example, EP 2 923 851 A1 discloses the general formula R 1 -NH-CO-NH-Ar-NH-SO 2 -R2 Color developer, where R 1 , R 2 and Ar may be an (un)substituted aryl group. A widely used non-phenolic color developer of this type is N-(2-(3-phenylureido)phenyl)benzenesulfonamide (trade name NKK Nippon Soda Co. Ltd.). Although good dynamic sensitivity can be ensured with heat-sensitive recording materials based on these color developers, the stability of the colored complex, especially with respect to plasticizers or binders, still needs to be improved.

[0013] A comparable idea is also provided in WO 2017 111032 A1, which discloses a compound of the general formula Ph-NH-CO-NH-C 6 H 4 -O-SO 2 -Ar, wherein Ar may be an (un)substituted phenyl group.

[0014] Attempts have been made at an early stage to improve the performance of non-phenolic color developers by using color developer structures containing more than one structural unit involved in the color forming process.

[0015] JP H 06 227 142 A discloses a color developer comprising: 1 -NH-C(X)-NH) n -A has two, three or more (thio)urea units (bis-, tri-, poly-ureas) which are bonded to a generally aromatic unit A (X=S or O). The color developers described in EP 633 145 A1, JP H 0 821 109 A, JP H 08 244 355 A and JP H 11 268 422 A have a similar structure.

[0016] Although di- or poly-urea derivatives have good hydrogen bridge acceptor and donor properties and are therefore suitable for stabilizing colored complexes, the hydrogen bridge network formed between the individual urea units leads to a relatively high melting point and a low solubility of these substances in typical thermal solvents from heat-sensitive layers, and therefore the thermal responsiveness (so-called dynamic sensitivity) of heat-sensitive recording materials prepared using these color developers leaves much to be desired. Summary of the invention

[0017] The object of the present invention is therefore to overcome the disadvantages of the prior art described above. In particular, the object of the present invention is to provide a color developer and a thermosensitive recording material containing the same, which recording material has a balanced application performance profile and achieves a printing density suitable for practical use, which is comparable to the printing density of thermosensitive recording materials based on known non-phenolic color developers, but at the same time also ensures a high durability of the printed image, especially when the thermosensitive layer is in contact with hydrophobic substances (such as oils, fats, plasticizers from foil materials and the like), without preferably having to rely on special formulation ingredients in the thermosensitive functional layer, such as antidegradants or special melting aids, which have limited availability and / or high prices. Another object of the present invention is to provide a color developer or a thermosensitive recording material, which is able to ensure the functional properties required for the application (especially thermal responsiveness), even when the unprinted thermosensitive recording material is stored for a long time and / or under extreme climatic conditions (high humidity and / or temperature).

[0018] These objects are achieved according to the invention by the use of compounds according to claim 1 in a thermosensitive recording material according to claim 10 .

[0019] It has surprisingly been found that the use of the color developers of class (I) according to the invention makes it possible to obtain heat-sensitive recording materials which are characterized by an excellent durability of the printing, in particular even in the case of exposure of the printed image to hydrophobic substances (e.g. plasticizers). The recording materials prepared with the color developers according to the invention also have an excellent long-term storage stability. Thus, the printing obtained in a thermal printer is hardly damaged, even after storage for several weeks in the unprinted (white) state under high ambient humidity and / or at high temperatures.

[0020] The compound according to claim 1 has the formula (I),

[0021] Ar 1 -NH-CO-NH-C 6 H 4 -SO 2 -OC 6 H 4 -NH-CO-NH-Ar 2 (I)

[0022] Among them, Ar 1 and Ar 2 Independently of one another are unsubstituted or substituted phenyl groups, naphthyl groups and / or heteroaryl groups.

[0023] Ar 1 Preferred is a phenyl group.

[0024] Ar 2Preferred is a phenyl group.

[0025] Preferably, Ar 1 By at least one C 1 -C 5 Alkyl group, alkenyl group, alkynyl group, benzyl group, formyl group, halogen group, NO 2 group, CN group, R-CO- group, RO group, RO 2 C group, R-OCO group, R-SO 2 O group, RO-SO 2 Group, R-SO 2 -NH group, R-NH-SO 2 group, R-NH-CO group or R-CO-NH group, wherein R is C 1 -C 5 an alkyl group, an alkenyl group, an alkynyl group, a phenyl group, a tolyl group or a benzyl group.

[0026] Ar 1 Particularly preferably, at least one C 1 -C 5 Alkyl group, halogen group, NO 2 group, CN group, R-CO group, RO group or RO 2 C group substituted, wherein R is C 1 -C 5 Alkyl group.

[0027] Ar 1 Monosubstituted is preferred.

[0028] Ar 1 Preference is given to monosubstituted phenyl groups.

[0029] Preferably, Ar 2 By at least one C 1 -C 5 Alkyl group, alkenyl group, alkynyl group, benzyl group, formyl group, halogen group, NO 2 group, CN group, R-CO- group, RO group, RO 2 C group, R-OCO group, R-SO 2 O group, RO-SO 2 Group, R-SO 2 -NH group, R-NH-SO 2 group, R-NH-CO group or R-CO-NH group, wherein R is C 1 -C 5 an alkyl group, an alkenyl group, an alkynyl group, a phenyl group, a tolyl group or a benzyl group.

[0030] Ar 2 Particularly preferably, at least one C 1 -C 5 Alkyl group, halogen group, NO2 group, CN group, R-CO group, RO group or RO 2 C group substituted, wherein R is C 1 -C 5 Alkyl group.

[0031] Ar 2 Monosubstituted is preferred.

[0032] Ar 2 Preference is given to monosubstituted phenyl groups.

[0033] Ar 1 and / or Ar 2 By at least one C 1 -C 5 Alkyl group substitution, preferably in the form of said C 1 -C 5 The alkyl group is a methyl group or a butyl group, and a methyl group is particularly preferred.

[0034] Ar 1 and / or Ar 2 Substituted by at least one halogen group, preferably the halogen group is a chloride group and / or a fluoride group.

[0035] Ar 1 and / or Ar 2 is substituted with at least one RO group, preferably the RO group is CH 3 O group.

[0036] Ar 1 and / or Ar 2 is substituted with at least one R-CO group, preferably the R-CO group is CH 3 -CO group.

[0037] In a particularly preferred embodiment, Ar 1 and Ar 2 Such compounds are relatively easy and inexpensive to prepare and give good results in terms of the properties described below.

[0038] In a particularly preferred embodiment, the Ar 1 -NH-CO-NH group and the Ar 2 The -NH-CO-NH groups are arranged about the -C 6 H 4 -SO 2-OC 6 H 4 The 2 and 3' positions, the 2 and 4' positions, the 3 and 2' positions, the 3 and 3' positions, the 3 and 4' positions, the 4 and 2' positions, the 4 and 3' positions or the 4 and 4' positions of the group.

[0039] Arrangement at the 3 and 2' or 4 and 3' positions is particularly preferred, since the preparation of such compounds is relatively easy and exhibits good properties.

[0040] Particularly preferred compounds of formula (I) are shown in Table 1 below:

[0041]

[0042] Table 1: Preferred compounds of formula (I) having for Ar 1 -NH-CO-NH and Ar 2 The claimed meaning of the arrangement of the -NH-CO-NH groups and Ar 1 and Ar 2 The claimed meaning of (R is as described above).

[0043] The compounds of formula (I) according to the present invention can be prepared by methods known per se.

[0044] Reaction schemes 1 to 3 illustrate possible synthetic routes to compounds of formula (I) according to the invention, examples of which are compounds according to Table 1.

[0045]

[0046]

[0047] The preferred embodiments recited for the compounds of formula (I) also apply to the processes for the preparation of said compounds.

[0048] As mentioned, the present invention also relates to a heat-sensitive recording material comprising a carrier substrate and a heat-sensitive color-forming layer containing at least one color former and at least one phenol-free color developer, wherein the at least one phenol-free color developer is a compound of the above formula (I).

[0049] The compound of formula (I) is preferably present in an amount of about 3 to about 35% by weight, particularly preferably about 10 to about 25% by weight, based on the total solid content of the heat-sensitive layer.

[0050] The choice of the carrier substrate is not critical. However, preference is given to using paper, synthetic paper and / or plastic foil as the carrier substrate.

[0051] If necessary, at least one further intermediate layer is present between the carrier substrate and the heat-sensitive layer, wherein the task of this intermediate layer is to improve the surface smoothness of the carrier for the heat-sensitive layer and to provide a thermal barrier between the carrier paper and the heat-sensitive layer. Preferably, organic hollow spherical pigments and / or calcined kaolin are used in this intermediate layer.

[0052] At least one protective layer and / or at least one layer for improving printability may also be present in the heat-sensitive recording material according to the present invention, and these layers may be applied to the front side or the back side of the substrate.

[0053] The present invention also does not impose any major restrictions on the choice of the coupler. However, the coupler is preferably a dye of the triphenylmethane type, fluoran type, azaphthalide type and / or fluorene type. Fluoran type dyes are particularly preferred couplers, because their availability and balanced application properties make it possible to provide recording materials with an attractive price / performance ratio.

[0054] Particularly preferred fluoran-type dyes are shown below:

[0055] 3-Diethylamino-6-methyl-7-phenylaminofluoran,

[0056] 3-(N-ethyl-N-p-toluamino)-6-methyl-7-phenylaminofluoran,

[0057] 3-(N-ethyl-N-isopentylamino)-6-methyl-7-phenylaminofluoran,

[0058] 3-Diethylamino-6-methyl-7-(o,p-dimethylphenylamino)fluoran,

[0059] 3-Pyrrolidinyl-6-methyl-7-phenylaminofluoran,

[0060] 3-(Cyclohexyl-N-methylamino)-6-methyl-7-phenylaminofluoran,

[0061] 3-Diethylamino-7-(m-trifluoromethylphenylamino)fluoran,

[0062] 3-N-di-n-butylamino-6-methyl-7-phenylaminofluoran,

[0063] 3-Diethylamino-6-methyl-7-(m-methylphenylamino)fluoran,

[0064] 3-N-di-n-butylamino-7-(o-chlorophenylamino)fluoran,

[0065] 3-(N-ethyl-N-tetrahydrofurfurylamino)-6-methyl-7-phenylaminofluoran,

[0066] 3-(N-methyl-N-propylamino)-6-methyl-7-phenylaminofluoran,

[0067] 3-(N-ethyl-N-ethoxypropylamino)-6-methyl-7-phenylaminofluoran,

[0068] 3-(N-ethyl-N-isobutylamino)-6-methyl-7-phenylaminofluoran, and / or

[0069] 3-Dipentylamino-6-methyl-7-phenylaminofluoran.

[0070] The couplers can be used as individual substances but also as any desired mixtures of two or more couplers, provided that the desired application properties of the recording material are not impaired thereby.

[0071] The color former is preferably present in an amount of about 5 to about 30% by weight, particularly preferably about 8 to about 20% by weight, based on the total solid content of the heat-sensitive layer.

[0072] In order to control specific application properties, it may be advantageous if at least two compounds of the general formula (I) are present as color developers in the heat-sensitive layer.

[0073] Likewise, in addition to one or more compounds of the formula (I), one or more other (bis)phenolic or non-phenolic color developers may be present in the heat-sensitive color-forming layer.

[0074] In addition to the at least one color former and the at least one color developer, the heat-sensitive color-forming layer may contain one or more sensitizers, which are also called heat-sensitive solvents, which have the advantage of making it easier to control the heat-pressure sensitivity.

[0075] In general, crystalline materials having a melting point between about 90°C and about 150°C are advantageously used as sensitizers and they dissolve the color-forming components (couplers and color developers) in the molten state without interfering with the formation of the colored complex.

[0076] Preferably, the sensitizer is a fatty acid amide (e.g., stearic acid amide, behenic acid amide or palmitic acid amide), an ethylenebisfatty acid amide (e.g., N,N'-ethylenebisstearic acid amide or N,N'-ethylenebisoleic acid amide), a fatty acid alkanolamide (e.g., N-(hydroxymethyl)stearic acid amide, N-hydroxymethylpalmitic acid amide or hydroxyethylstearic acid amide), a wax (e.g., polyethylene wax or montan wax), a carboxylic acid ester (e.g., dimethyl terephthalate, dibenzyl terephthalate, benzyl 4-benzyloxybenzoate, di-(4 The invention also includes aromatic hydrocarbons such as 4-benzylbiphenyl, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfone, 4-diphenylsulfonamide ...

[0077] The sensitizer is preferably present in an amount of about 10 to about 40% by weight, particularly preferably about 15 to about 25% by weight, based on the total solid content of the heat-sensitive layer.

[0078] In addition to the color former, the phenol-free color developer and the sensitizer, in a further preferred embodiment, at least one stabilizer (antidegradant) is optionally present in the heat-sensitive color-forming layer.

[0079] The stabilizer is preferably composed of sterically hindered phenols, particularly preferably 1,1,3-tris-(2-methyl-4-hydroxy-5-cyclohexyl-phenyl)-butane, 1,1,3-tris-(2-methyl-4-hydroxy-5-tert-butylphenyl)-butane, 1,1-bis-(2-methyl-4-hydroxy-5-tert-butyl-phenyl)-butane.

[0080] In addition, the following substances can also be used as stabilizers in the recording material according to the present invention: urea-urethane compounds of the general formula (II) (commercial product UU) or ethers derived from 4,4'-dihydroxydiphenyl sulfone, such as 4-benzyloxy-4'-(2-methylglycidyloxy)-diphenyl sulfone (trade name NTZ- , Nippon Soda Co., Ltd.), or an oligomer ether of formula (III) (trade name Japan Soda Co., Ltd.).

[0081]

[0082] Urea-urethane compounds of the general formula (II) are particularly preferred.

[0083] The stabilizer is preferably present in an amount of about 0.2 to 0.5 parts by weight relative to 1 part by weight of the phenol-free color developing agent of the at least one compound of the formula (I).

[0084] In a further preferred embodiment, the heat-sensitive color-forming layer contains at least one binder. These are preferably water-soluble starch, starch derivatives, starch-based bio-latex, methylcellulose, hydroxyethylcellulose, carboxymethylcellulose, partially or completely saponified polyvinyl alcohol, chemically modified polyvinyl alcohol or styrene-maleic anhydride copolymer, styrene-butadiene copolymer, acrylamide-(meth)acrylate copolymer, acrylamide-acrylate-methacrylate terpolymer, polyacrylate, poly(meth)acrylate, acrylate-butadiene copolymer, polyvinyl acetate and / or acrylonitrile-butadiene copolymer.

[0085] In a further preferred embodiment, at least one release agent (anti-sticking agent) or lubricant is present in the heat-sensitive color-forming layer. These agents are preferably fatty acid metal salts, such as zinc stearate or calcium stearate, or behenate, synthetic waxes, such as in the form of fatty acid amides, such as stearic acid amide and behenic acid amide, fatty acid alkanolamides, such as stearic acid hydroxymethylamide, paraffin waxes of different melting points, ester waxes of different molecular weights, propylene waxes, ethylene waxes of different hardness, and / or natural waxes, such as carnauba wax or montan wax.

[0086] The release agent is preferably present in an amount of about 1 to about 10 wt %, particularly preferably about 3 to about 6 wt %, based on the total solid content of the heat-sensitive layer.

[0087] In a further preferred embodiment, the thermosensitive color-forming layer contains pigments. One of the advantages of using these pigments is that they can fix the molten chemicals produced during the thermal printing process on their surface. Pigments can also be used to control the surface whiteness and opacity of the thermosensitive color-forming layer and its printability with traditional inks. Finally, pigments have an "extender function", for example for relatively expensive coloring functional chemicals.

[0088] Particularly suitable pigments are inorganic pigments, both synthetic and natural, preferably clays, precipitated or natural calcium carbonate, aluminum oxide, aluminum hydroxide, silicon dioxide, precipitated and pyrogenic silicon dioxide (e.g. Type), diatomaceous earth, magnesium carbonate, talc, kaolin, but also organic pigments, for example hollow pigments with styrene / acrylate copolymer walls or urea / formaldehyde condensation polymers. These can be used alone or in any mixture.

[0089] The pigment is preferably present in an amount of about 20 to about 50% by weight, particularly preferably about 30 to about 40% by weight, based on the total solid content of the heat-sensitive layer.

[0090] In order to control the surface whiteness of the heat-sensitive recording material according to the invention, optical brighteners may be incorporated into the heat-sensitive color-forming layer. These are preferably stilbenes.

[0091] In order to improve certain coating properties, it is preferred in individual cases to add further components, in particular rheology auxiliaries, such as thickeners and / or surfactants, to the mandatory components of the heat-sensitive recording materials according to the invention.

[0092] The applied weight per unit area of ​​the (dry) heat-sensitive layer is preferably about 1 to about 10 g / m 2 , preferably from about 3 to about 6 g / m 2 .

[0093] In a particularly preferred embodiment, the heat-sensitive recording material is a heat-sensitive recording material according to claim 10, wherein a dye of the fluoran type is used as a coupler and a sensitizer is additionally present, the sensitizer being selected from fatty acid amides, aromatic sulfones and / or aromatic ethers. In this preferred embodiment, it is additionally advantageous if about 1.5 to about 4 parts by weight of a phenol-free color developer according to claim 1 is present relative to 1 part by weight of the coupler.

[0094] The preferred embodiments listed with regard to the compounds of the formula (I) also apply to the heat-sensitive recording material according to the invention.

[0095] The heat-sensitive recording material according to the present invention can be obtained using a known production method.

[0096] However, the recording material according to the invention is preferably obtained by a process in which an aqueous suspension containing the starting material of the heat-sensitive color-forming layer is applied to a carrier substrate and dried, the aqueous application suspension having a solids content of about 20 to about 75% by weight, preferably about 30 to about 50% by weight, and is applied and dried by a curtain coating process at a coating equipment operating speed of at least about 400 m / min.

[0097] This method is particularly advantageous from an economic point of view.

[0098] If the solids content falls below values ​​of about 20% by weight, the economic efficiency decreases, since a large amount of water must be removed from the coating by gentle drying in a short time, which has a negative effect on the coating speed. On the other hand, if values ​​of 75% by weight are exceeded, this only leads to increased technical effort to ensure the stability of the coating color curtain during the coating process.

[0099] In the curtain coating method, a free-falling curtain of a coating dispersion is formed. By free falling, the coating dispersion in the form of a thin film (curtain) is "poured" onto a substrate in order to apply the coating dispersion to the substrate. Document DE 10196 052 T1 discloses the use of the curtain coating method in the preparation of information recording materials, which include, among other substances, heat-sensitive recording materials, wherein a multilayer recording layer is achieved by applying a curtain consisting of several coating dispersion films to a substrate (speed up to 200 m / min).

[0100] Setting the operating speed of the coating device to at least about 400 m / min has both economic and technical advantages. Preferably, the operating speed is at least about 750 m / min, particularly preferably at least about 1000 m / min, and very particularly preferably at least about 1500 m / min. It is particularly surprising that even at the latter speed, the heat-sensitive recording material obtained is not affected in any way, and the operation even runs optimally at this high speed.

[0101] In a preferred embodiment of the method according to the invention, the aqueous, degassed coating suspension has a viscosity of about 150 to about 800 mPas (Brookfield, 100 rpm, 20° C.). If the viscosity falls below values ​​of about 150 mPas or exceeds values ​​of about 800 mPas, this can lead to poor runnability of the coating material at the coating unit. The viscosity of the aqueous, degassed coating suspension is particularly preferably about 200 to about 500 mPas.

[0102] In a preferred embodiment, the surface tension of the aqueous application suspension can be adjusted to about 25 to about 60 mN / m, preferably about 35 to about 50 mN / m (measured according to the static ring method according to Du Noüy, DIN 53914) to optimize the process.

[0103] The thermosensitive color-forming layer can be formed in-line or off-line in a separate coating process. This also applies to any subsequently applied layers or intermediate layers.

[0104] Advantageously, the dried heat-sensitive color-forming layer is subjected to smoothing measures. Advantageously, the Bekk smoothness measured according to ISO 5627:1995-03 is adjusted to between about 100 and about 1000 sec, preferably between about 250 and about 600 sec.

[0105] The surface roughness (PPS) according to ISO 8791-4:2008-05 is in the range of about 0.50 to about 2.50 μm, particularly preferably in the range of about 1.00 to about 2.00 μm.

[0106] The preferred embodiments listed with regard to the compounds of the formula (I) also apply to the process for producing the heat-sensitive recording material according to the invention.

[0107] The present invention also relates to a heat-sensitive recording material obtainable by the above-mentioned process.

[0108] The above method is advantageous from an economic point of view and allows a coating apparatus with high process performance even at speeds greater than 1500 m / min without damaging the process product, i.e. the thermosensitive recording material according to the invention. The method can be carried out both online and offline, which results in an ideal flexibility.

[0109] The thermosensitive recording material according to the invention is phenol-free and well suited for POS (point of sale), label and / or ticket applications. It is also suitable for preparing parking tickets, tourist tickets, admission tickets, lottery tickets, etc., which can be printed using direct thermal processing and require that the images recorded on them have high durability in the case of long-term storage, even under adverse climatic conditions with respect to temperature and ambient humidity.

[0110] Surprisingly, it has been shown that the use of the color developers of formula (I) according to the invention can provide heat-sensitive recording materials which are characterized in particular in that they do not practically lose any of their ability to produce high image densities, even after storing the unprinted material for several weeks (even at high ambient humidity and / or at high temperatures). The heat-sensitive recording materials according to the invention therefore exhibit a surprisingly long storage capacity. DETAILED DESCRIPTION

[0111] The present invention is explained in detail below based on non-limiting examples.

[0112] Example:

[0113] Preparation of compounds of formula (I) according to the present invention.

[0114] Step A - Preparation of dinitrosulfonate (according to JP 2014 094 888 A)

[0115] A solution of 60 mmol of the corresponding nitrobenzenesulfonyl chloride in 15 mL of THF was added dropwise to a solution of 60 mmol of the corresponding nitrophenol and 84 mmol of triethylamine in 20 mL of THF at room temperature under stirring. The reaction solution was stirred at room temperature for two hours and then mixed with 65 mL of water. The suspension was stirred at room temperature for three hours and then filtered. The residue was then washed with 10 mL of water (3 to 6 times). The dinitrosulfonate was used in step B without further purification.

[0116] Step B - Reduction of the nitro group to a primary amine

[0117] 0.420 mol SnCl was stirred at room temperature. 2 ·2H 2 O is added (portioned) to 0.060mol of the product derived from step A in a solution in 200mL ethyl acetate. The reaction solution is refluxed. The reaction process is monitored by means of thin film chromatography (eluent: cyclohexane / ethyl acetate 1: 1). Once the reaction is complete (approximately 2 to 3 hours), 200mL 50% potassium carbonate aqueous solution is added, and the mixture is stirred at room temperature for 30 minutes. The phases are separated from each other. The aqueous phase is extracted with 100mL ethyl acetate. The purified organic phase is dried over magnesium sulfate. Remove the solvent under vacuum. In step C, the diaminosulfonic acid ester is used without further purification.

[0118] Step C - Preparation of bis-urea compounds.

[0119] At room temperature under agitation the solution of 15.2mmol corresponding isocyanate in 25mL ethyl acetate is added drop-wise to the solution of 7.6mmol product in 40mL ethyl acetate derived from step B. Make the reaction mixture reflux. Make the reaction mixture reflux, and monitor reaction process by means of HPLC. Once the reaction is complete, the precipitated double-urea is filtered out, washed with 10mL ethyl acetate (3 times), and dried under vacuum. Can be further purified by recrystallization from ethyl acetate or dichloromethane. In some cases, reaction soln is concentrated under vacuum, and crystallization is initiated by adding a few drops of normal hexane.

[0120] The starting compounds are commercially available.

[0121] Table 2 summarizes the compounds of formula (I) prepared for the first time herein.

[0122]

[0123]

[0124] Table 2: Composition of the compound of formula (I) prepared for the first time

[0125] Analyze the data:

[0126] I, C 26 H 22 N 4 O 5 S, M = 502.5, 3'-(3'-phenylureido)phenyl 2-(3-phenylureido)benzenesulfonate

[0127] MS(ESI):m / z(%)=503.1(100)[M+H] + .

[0128] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.88(1H,s),8.82(1H,s),8.63(1H,s),8.43(1H,s),8.17-8.16(1H,m),7.75-7.70(2H,m),7.53-7.51(2H ,m),7.46-7.43(3H,m),7.32-7.26(5H,m),7.23-7.20(2H,m),7.03-6.97(2H,m),6.55(1H,ddd,J=8.0,2.4,1.0Hz).

[0129] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.13(NH C ONH),151.80(NH C ONH),149.06,141.21,139.25,139.25,137.88,135.43,129.94,129.87,128.71,128. 66,124.57,122.82,122.69,122.31,122.00,118.60,118.34,116.89,114.27,111.37.

[0130] II, C 26 H 22 N 4 O 5 S, M = 502.5, 4'-(3'-phenylureido)phenyl 2-(3-phenylureido)benzenesulfonate

[0131] MS(ESI):m / z(%)=503.1(100)[M+H] + .

[0132] 1 H-NMR (500 MHz, DMSO-d 6): δ(ppm)=9.88(1H,s),8.73(1H,s),8.63(1H,s),8.42(1H,s),8.13(1H,dd,J=8.4,1.0Hz),7.76-7.72(1H,m),7.66(1H,dd,J=8.1,1.5H z),7.52-7.50(2H,m),7.43-7.40(4H,m),7.32-7.29(2H,m),7.28-7.25(2H,m),7.22-7.19(1H,m),7.02-6.99(1H,m),6.98-6.93(3H,m).

[0133] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.25(NH C ONH),151.88(NH C ONH),142.82,139.37,139.23,138.99,137.83,135.39,130.04,128.73,128. 64,124.83,122.92,122.80,122.32,122.14,121.89,118.96,118.58,118.25.

[0134] III, C 26 H 22 N 4 O 5 S, M = 502.5, 2'-(3'-phenylureido)phenyl 3-(3-phenylureido)benzenesulfonate

[0135] MS(ESI):m / z(%)=503.2(100)[M+H] + .

[0136] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.05(1H,s),8.98(1H,s),8.60(1H,s),8.27-8.27(1H,m),8.19(1H,s),8.03(1H,dd,J=8.3,1.3Hz),7.54-7.52(1H, m),7.43-7.37(6H,m),7.30-7.27(2H,m),7.24-7.19(3H,m),7.13(1H,dd,J=8.2,1.2Hz),7.01-6.97(2H,m),6.96-6.93(1H,m).

[0137] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.08(NH C ONH),151.53(NH C ONH),140.66,139.32,139.10,138.10,134.47,132.13,129.67,128.63,128.58,127. 45,123.73,122.11,122.07,122.03,121.81,121.13,121.03,118.43,118.05,116.91.

[0138] IV, C 26 H 22 N 4 O 5 S, M = 502.5, 3-(3-phenylureido)benzenesulfonic acid 3'-(3'-phenylureido)phenyl ester

[0139] MS(ESI):m / z(%)=503.1(100)[M+H] + .

[0140] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.13(1H,s),8.86(1H,s),8.73(1H,s),8.62(1H,s),8.23-8.22(1H,m),7.72(1H,ddd,J=8.2,2.2,1.0Hz),7.58-7.55(1H, m),7.48-7.42(6H,m),7.31-7.25(6H,m),7.00(1H,tt,J=7.4,1.1Hz),6.98(1H,tt,J=7.4,1.1Hz),6.62(1H,ddd,J=7.6,2.3,1.6Hz).

[0141] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.30(NH C ONH),152.18(NH CONH),149.34,141.17,140.91,139.27,139.11,135.07,130.09,129.86,128.68,128. 67,123.76,122.22,122.01,120.87,118.59,118.37,116.67,116.61,114.58,111.38.

[0142] V, C 26 H 22 N 4 O 5 S, M = 502.5, 4'-(3'-phenylureido)phenyl 3-(3-phenylureido)benzenesulfonate

[0143] MS(ESI):m / z(%)=503.1(100)[M+H] + .

[0144] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.13(1H,s),8.76(1H,s),8.74(1H,s),8.63(1H,s),8.19-8.19(1H,m),7.72(1H,ddd,J=8.2,2.2,1.0H z),7.58-7.55(1H,m),7.48-7.42(6H,m),7.41(1H,ddd,J=7.8,1.8,1.0Hz),7.31-7.25(4H,m),7.01-6.95(4H,m).

[0145] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.34(NH C ONH),152.33(NH C ONH),143.22,140.88,139.40,139.12,138.78,134.97,130.06,128.69,128. 67,123.76,122.31,122.24,121.92,120.99,119.04,118.62,118.30,116.74.

[0146] VI, C 26 H 22 N 4 O 5 S, M = 502.5, 2'-(3'-phenylureido)phenyl 4-(3-phenylureido)benzenesulfonate

[0147] MS(ESI):m / z(%)=503.1(100)[M+H] + .

[0148] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.15(1H,s),9.10(1H,s),8.71(1H,s),8.13(1H,s),8.05(1H,dd,J=8.3,1.5Hz),7.75-7.74(2H,m),7.60-7.58(2H, m),7.44-7.42(2H,m),7.42-7.40(2H,m),7.31-7.21(5H,m),7.14(1H,dd,J=8.2,1.4Hz),7.02-6.97(2H,m),6.95-6.92(1H,m).

[0149] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=151.71(NH C ONH),151.62(NH C ONH),145.83,139.25,138.91,138.07,132.15,129.83,128.68,128.63,127. 30,125.32,122.32,122.18,122.01,121.90,120.94,118.54,118.29,117.19.

[0150] VII, C 26 H 22 N 4 O 5 S, M = 502.5, 3'-(3'-phenylureido)phenyl 4-(3-phenylureido)benzenesulfonate

[0151] MS(ESI):m / z(%)=503.1(100)[M+H] + .

[0152] 1 H-NMR (500 MHz, DMSO-d 6): δ(ppm)=9.28(1H,s),8.84(1H,s),8.81(1H,s),8.62(1H,s),7.79-7.77(2H,m),7.72-7.71(2H,m),7.48-7.46(2H, m),7.45-7.43(2H,m),7.38-7.38(1H,m),7.32-7.24(6H,m),7.03-7.00(1H,m),6.98-6.95(1H,m),6.60-6.59(1H,m).

[0153] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.16(NH C ONH),151.93(NH C ONH),149.43,145.61,141.08,139.27,138.94,129.76,129.56,128.71,128. 64,125.98,122.36,121.96,118.56,118.35,117.60,116.51,114.74,111.47.

[0154] VIII, C 26 H 22 N 4 O 5 S, M = 502.5, 4-(3-phenylureido)benzenesulfonic acid 4'-(3'-phenylureido)phenyl ester

[0155] MS(ESI):m / z(%)=503.2(100)[M+H] + .

[0156] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.28(1H,s),8.82(1H,s),8.74(1H,s),8.63(1H,s),7.75-7.73(2H,m),7.71-7.70(2H,m),7.48-7.47(2H, m),7.44-7.43(4H,m),7.32-7.29(2H,m),7.29-7.25(2H,m),7.03-7.00(1H,m),6.98-6.96(1H,m),6.96-6.92(2H,m).

[0157] 13 C-NMR (126 MHz, DMSO-d 6):δ(ppm)=152.32(NH C ONH),151.94(NH C ONH),145.56,143.28,139.40,138.95,138.63,129.62,128.72,128.64,125.89,122.39,122.37,121.87,118.96,118.57,118.26,117.58.

[0158] IX, C 28 H 26 N 4 O 5 S, M = 530.6, 3'-(3'-(2'-tolyl)ureido)phenyl 4-(3-(2-tolyl)ureido)benzenesulfonate

[0159] MS(ESI):m / z(%)=531.1(100)[M+H] + .

[0160] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.58(1H,s),9.17(1H,s),8.09(1H,s),7.90(1H,s),7.79-7.76(4H,m),7.73-7.70(2H,m),7.40-7.39(1H,m),7.31-7.28(1H,m) ,7.27-7.24(1H,m),7.20-7.12(4H,m),7.01-6.98(1H,m),6.97-6.93(1H,m),6.59(1H,ddd,J=7.7,2.4,1.4Hz),2.25(3H,s),2.23(3H,s).

[0161] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.31(NH C ONH),152.11(NH C ONH),149.46,145.75,141.25,136.96,136.61,130.15,130.06,129.81,129.61,128.35,127.88, 126.07,126.03,125.84,123.37,122.91,121.70,121.36,117.44,116.29,114.63,111.29,17.68( C H 3),17.68( C H 3 ).

[0162] X, C 28 H 26 N 4 O 5 S, M = 530.6, 3'-(3'-(3'-tolyl)ureido)phenyl 4-(3-(3-tolyl)ureido)benzenesulfonate

[0163] MS(ESI):m / z(%)=531.1(100)[M+H] + .

[0164] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.26(1H,s),8.83(1H,s),8.73(1H,s),8.54(1H,s),7.78-7.76(2H,m),7.72-7.70(2H,m),7.40-7.39(1H,m),7.31-7.31(1H,m) ,7.29-7.21(5H,m),7.19-7.13(2H,m),6.84-6.82(1H,m),6.80-6.78(1H,m),6.59(1H,ddd,J=7.6,2.4,1.5Hz),2.29(3H,s),2.27(3H,s).

[0165] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.14(NH C ONH),151.90(NH C ONH),149.43,145.63,141.12,139.19,138.86,137.94,137.86,129.75,129.55,128.55,128.49, 125.95,123.11,122.72,119.08,118.85,117.58,116.47,115.74,115.53,114.69,111.44,21.07( C H 3 ),21.07( C H 3 ).

[0166] XI, C 28 H 26 N 4 O 5S, M = 530.6, 3'-(3'-(4'-tolyl)ureido)phenyl 4-(3-(4-tolyl)ureido)benzenesulfonate

[0167] MS(ESI):m / z(%)=531.1(100)[M+H] + .

[0168] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.23(1H,s),8.79(1H,s),8.71(1H,s),8.50(1H,s),7.77-7.75(2H,m),7.71-7.70(2H,m),7.37-7.35(3H,m), 7.33-7.31(2H,m),7.26-7.23(2H,m),7.11-7.10(2H,m),7.07-7.05(2H,m),6.60-6.57(1H,m),2.25(3H,s),2.21(3H,s).

[0169] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.18(NH C ONH),151.94(NH C ONH),149.44,145.72,141.18,136.69,136.38,131.29,130.82,129.73,129.56, 129.11,129.05,125.85,118.65,118.44,117.53,116.43,114.66,111.41,20.24( C H 3 ),20.19( C H 3 ).

[0170] XII, C 32 H 34 N 4 O 5 S, M = 586.7, 3'-(3'-(2',4',6'-trimethylphenyl)ureido)phenyl 4-(3-(2,4,6-trimethylphenyl)ureido)benzenesulfonate

[0171] MS(ESI):m / z(%)=587.2(100)[M+H] + .

[0172] 1 H-NMR (500 MHz, DMSO-d6 ): δ(ppm)=9.34(1H,s),8.86(1H,s),7.82(1H,s),7.73-7.71(2H,m),7.69-7.67(2H,m),7.61(1H,s),7.35-7.35(1H,m),7.2 9-7.28(1H,m),7.23-7.20(1H,m),6.90-6.87(4H,m),6.54-6.53(1H,m),2.23(3H,s),2.23(3H,s),2.17(6H,s),2.14(6H,s).

[0173] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.90(NH C ONH),152.59(NH C ONH),149.42,146.17,141.73,135.24,135.22,135.20,134.94,132.29,131.99, 129.62,129.49,128.26,128.19,125.50,117.25,116.19,114.21,111.23,20.37( C H 3 ),17.98( C H 3 ).

[0174] XIII, C 34 H 26 N 4 O 5 S, M = 602.7, 3'-(3'-(1'-naphthyl)ureido)phenyl 4-(3-(1-naphthyl)ureido)benzenesulfonate

[0175] MS(ESI):m / z(%)=603.2(100)[M+H] + .

[0176] 1 H-NMR (500 MHz, DMSO-d 6): δ(ppm)=9.64(1H,s),9.23(1H,s),8.91(1H,s),8.75(1H,s),8.12-8.09(2H,m ),7.99-7.96(2H,m),7.95-7.94(1H,m),7.92-7.91(1H,m),7.83-7.81(2H,m),7. 79-7.77(2H,m),7.70-7.68(1H,m),7.64-7.62(1H,m),7.61-7.45(7H,m),7.35(1 H,ddd,J=8.2,2.0,1.1Hz),7.31-7.28(1H,m),6.63(1H,ddd,J=8.0,2.4,1.0Hz).

[0177] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.63(NH C ONH),152.48(NH C ONH),149.51,145.70,141.18,133.90,133.64,133.62,133.58,129.90,129.69,128.32,128.30,126.32,126.08,126.00,125. 90,125.80,125.78,125.73,125.70,125.65,123.70,123.19,121.33,121.25,118.34,117.81,117.62,116.47,114.82,111.44.

[0178] XIV, C 28 H 26 N 4 O 7 S, M = 562.6, 3'-(3'-(4'-methoxyphenyl)ureido)phenyl 4-(3-(4-methoxyphenyl)ureido)benzenesulfonate

[0179] MS(ESI):m / z(%)=563.2(100)[M+H] + .

[0180] 1 H-NMR (500 MHz, DMSO-d 6): δ(ppm)=9.21(1H,s),8.76(1H,s),8.63(1H,s),8.42(1H,s),7.77-7.74(2H,m),7.71-7.69(2H,m),7.39-7.32(5H,m) ,7.28-7.22(2H,m),6.90-6.87(2H,m),6.87-6.84(2H,m),6.58(1H,ddd,J=7.4,2.3,1.7Hz),3.73(3H,s),3.69(3H,s).

[0181] 13 C-NMR (126 MHz, DMSO-d 6 ): δ (ppm) = 154.89, 154.61, 152.34 (NH C ONH),152.09(NH C ONH),149.44,145.81,141.28,132.28,131.92,129.71,129.55,125.74,1 20.45,120.23,117.48,116.39,114.55,113.99,113.92,111.37,55.14(O C H 3 ),55.07(O C H 3 ).

[0182] XV, C 26 H 20 Cl 2 N 4 O 5 S, M = 571.4, 3'-(3'-(4'-chlorophenyl)ureido)phenyl 4-(3-(4-chlorophenyl)ureido)benzenesulfonate

[0183] MS(ESI):m / z(%)=571.0(100)[M+H] + .

[0184] 1 H-NMR (500 MHz, DMSO-d 6): δ(ppm)=9.31(1H,s),8.95(1H,s),8.87(1H,s),8.76(1H,s),7.78-7.76(2H,m),7.72-7.69(2H,m),7.51-7.48(2H,m),7.48 -7.45(2H,m),7.37-7.36(1H,m),7.36-7.33(2H,m),7.31-7.28(2H,m),7.28-7.25(2H,m),6.61(1H,ddd,J=6.0,3.1,2.4Hz).

[0185] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=152.05(NH C ONH),151.86(NH C ONH),149.41,145.45,140.88,138.29,137.96,129.77,129.56,128.57,128. 47,126.13,126.00,125.55,120.09,119.84,117.74,116.62,114.94,111.58.

[0186] XVI, C 26 H 20 F 2 N 4 O 5 S, M = 538.5, 3'-(3'-(4'-fluorophenyl)ureido)phenyl 4-(3-(4-fluorophenyl)ureido)benzenesulfonate

[0187] MS(ESI):m / z(%)=539.2(100)[M+H] + .

[0188] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.28(1H,s),8.85(1H,s),8.84(1H,s),8.65(1H,s),7.78-7.75(2H,m),7.72-7.69(2H,m),7.50 -7.42(4H,m),7.37-7.36(1H,m),7.29-7.23(2H,m),7.16-7.06(4H,m),6.60(1H,ddd,J=7.5,2.3,1.6Hz).

[0189] 13 C-NMR (126 MHz, DMSO-d6 ): δ (ppm) = 158.49 (d, J = 29.7Hz), 156.59 (d, J = 29.3Hz), 152.26 (NH C ONH),152.05(NH C ONH),149.43,145.60,141.06,135.60(d,J=2.3Hz),135.26(d,J=2.3Hz),129.75,129.56,126.01,120.45(d, J=7.8Hz), 120.17 (d, J=7.7Hz), 117.65, 116.56, 115.27 (d, J=13.4Hz), 115.10 (d, J=13.4Hz), 114.78, 111.52.

[0190] XVII, C 30 H 26 N 4 O 7 S, M = 586.6, 3'-(3'-(4'-acetylphenyl)ureido)phenyl 4-(3-(4-acetylphenyl)ureido)benzenesulfonate

[0191] MS(ESI):m / z(%)=587.1(100)[M+H] + .

[0192] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.41(1H,s),9.24(1H,s),9.06(1H,s),8.98(1H,s),7.92-7.91(2H,m),7.89-7.87(2H,m),7.80-7.78(2H,m),7.74-7.7 3(2H,m),7.60-7.59(2H,m),7.57-7.56(2H,m),7.38-7.38(1H,m),7.28-7.27(2H,m),6.65-6.63(1H,m),2.52(3H,s),2.46(3H,s).

[0193] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=196.23( C OCH 3 ),196.14( C OCH 3 ),151.83(NH C ONH),151.69(NH CONH),149.43,145.29,143.94,143.58,140.69,130.95,130.61,129.89,129.66, 129.54,129.51,126.34,117.94,117.51,117.27,116.81,115.27,111.75,26.26( C H 3 ),26.17( C H 3 ).

[0194] XVIII, C 32 H 30 N 4 O 9 S, M=646.7, ethyl 4-(3-(4-((3-(3-(4-(ethoxycarbonyl)phenyl)ureido)phenoxy)sulfonyl)phenyl)ureido)benzoate

[0195] MS(ESI):m / z(%)=647.2(100)[M+H] + .

[0196] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.38(1H,s),9.21(1H,s),9.03(1H,s),8.95(1H,s),7.91-7.89(2H,m) ,7.88-7.86(2H,m),7.80-7.77(2H,m),7.74-7.72(2H,m),7.60-7.58(2H,m),7.5 8-7.55(2H,m),7.38-7.37(1H,m),7.28-7.27(2H,m),6.66-6.63(1H,m),4.29(2H , q, J = 7.1Hz), 4.26 (2H, q, J = 7.1Hz), 1.31 (3H, q, J = 7.1Hz), 1.29 (3H, q, J = 7.1Hz).

[0197] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=165.27( C OO),165.26( C OO),151.79(NH C ONH),151.65(NH CONH),149.40,145.26,143.87,143.52,140.65,130.21,130.20,129.82,129.59,126 .35,123.34,122.96,117.90,117.61,117.36,116.75,115.22,111.71,60.21,60.13( C H 2 ),14.11( C H 3 ).

[0198] XIX, C 28 H 20 N 6 O 5 S, M = 552.6, 3'-(3'-(4'-cyanophenyl)ureido)phenyl 4-(3-(4-cyanophenyl)ureido)benzenesulfonate

[0199] MS(ESI):m / z(%)=553.1(100)[M+H] + .

[0200] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.45(1H,s),9.32(1H,s),9.14(1H,s),9.02(1H,s),7.80-7.77(2H,m),7.76-7.71(4H,m),7.70- 7.67(2H,m),7.65-7.63(2H,m),7.62-7.60(2H,m),7.36-7.36(1H,m),7.28-7.27(2H,m),6.66-6.63(1H,m).

[0201] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=151.74(NH C ONH),151.62(NH C ONH),149.37,145.10,143.79,143.45,140.50,133.20,133.10,129.88,129.61,126. 50,119.05,119.03,118.36,118.13,118.01,116.88,115.37,111.80,103.95,103.46.

[0202] XX, C 26 H 20 N6 O 9 S, M = 592.5, 3'-(3'-(4'-nitrophenyl)ureido)phenyl 4-(3-(4-nitrophenyl)ureido)benzenesulfonate

[0203] MS(ESI):m / z(%)=593.1(100)[M+H] + .

[0204] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.52(1H,s),9.48(1H,s),9.36(1H,s),9.06(1H,s),8.20-8.17(2H,m),8.15-8.12(2H,m),7.81- 7.78(2H,m),7.75-7.73(2H,m),7.70-7.64(4H,m),7.37-7.36(1H,m),7.31-7.27(2H,m),6.69-6.66(1H,m).

[0205] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=151.60(NH C ONH),151.51(NH C ONH),149.38,145.93,145.54,145.00,141.46,141.12,140.36,129.88,129. 62,126.64,124.93,124.90,118.13,117.79,117.53,116.97,115.57,111.91.

[0206] XXI, C 27 H 23 N 5 O 8 S, M = 577.6, 3'-(3'-(4'-nitrophenyl)ureido)phenyl 4-(3-(4-methoxyphenyl)ureido)benzenesulfonate

[0207] MS(ESI):m / z(%)=578.1(100)[M+H] + .

[0208] 1 H-NMR (500 MHz, DMSO-d 6): δ(ppm)=9.37(1H,s),9.20(1H,s),9.07(1H,s),8.62(1H,s),8.18-8.15(2H,m),7.76-7.74(2H,m),7.7 1-7.66(4H,m),7.37-7.34(3H,m),7.31-7.27(2H,m),6.89-6.86(2H,m),6.67-6.65(1H,m),3.72(3H,s).

[0209] 13 C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=154.89,152.08(NH C ONH),151.64(NH C ONH),149.42,145.94,145.87,141.17,140.36,131.88,129.87,129.57,125. 63,124.94,120.44,117.59,117.51,116.95,115.56,113.97,111.94,55.13(O C H 3 ).

[0210] XXII, C 27 H 23 N 5 O 8 S, M = 577.6, 3'-(3'-(4'-methoxyphenyl)ureido)phenyl 4-(3-(4-nitrophenyl)ureido)benzenesulfonate

[0211] MS(ESI):m / z(%)=578.1(100)[M+H] + .

[0212] 1 H-NMR (500 MHz, DMSO-d 6 ): δ(ppm)=9.52(2H,s),8.75(1H,s),8.42(1H,s),8.22-8.19(2H,m),7.81-7.79(2H,m),7.75-7.73(2H,m),7.73-7.7 0(2H,m),7.37-7.36(1H,m),7.35-7.31(2H,m),7.26-7.22(2H,m),6.86-6.82(2H,m),6.60-6.56(1H,m),3.68(3H,s).

[0213] 13C-NMR (126 MHz, DMSO-d 6 ):δ(ppm)=154.60,152.33(NH C ONH),151.55(NH C ONH),149.41,145.61,144.94,141.47,141.30,132.28,129.73,129.60,126. 77,124.98,120.20,118.11,117.86,116.43,114.53,113.91,111.34,55.07(O C H 3 ).

[0214] Non-phenolic color developers from the prior art were used as contrast developers, specifically N-(2-(3-phenylureido)phenyl)benzenesulfonamide (NKK 1304, Nippon Soda) and sulfonylurea, Pergafast (PF 201, BASF).

[0215] On a laboratory scale, the aqueous coating suspension was applied using a doctor bar to a 63 g / m 2 Synthetic base paper ( FP680) on one side to form a thermosensitive color-forming layer of the thermosensitive recording paper. After drying, a thermosensitive recording paper is obtained. The application rate of the thermosensitive color-forming layer is 3.8 to 4.2 g / m 2 between.

[0216] Based on the above information, a thermal recording material or thermal paper was prepared using the following formulation of an aqueous coating suspension to form a composite structure on a carrier substrate, and then other layers, especially a protective layer, were formed in a usual manner, which will not be discussed separately here.

[0217] Preparation of dispersion for application of suspension (in each case for 1 part by weight)

[0218] The mixture was prepared by mixing 20 parts by weight of 3-N-di-n-butylamino-6-methyl-7-phenylaminofluorane (ODB-2) with 33 parts by weight of Ghosenex TM Aqueous Dispersion A (coupler dispersion) was prepared by grinding a 15% aqueous solution of L-3266 (sulfonated polyvinyl alcohol, Nippon Ghosei).

[0219] By mixing 40 parts by weight of the color developer with 66 parts by weight of Ghosenex TM Aqueous Dispersion B (color developer dispersion) was prepared by grinding together a 15% aqueous solution of L-3266.

[0220] The mixture was prepared by mixing 40 parts by weight of 1,2-diphenoxyethane with 33 parts by weight of Ghosenex TM Aqueous Dispersion C (sensitizer dispersion) was prepared by grinding a 15% aqueous solution of L-3266.

[0221] All dispersions prepared by grinding had an average particle size D of 0.80-1.20 μm. (4.3) The particle size distribution of the dispersion was measured by laser diffraction using a Coulter LS230 instrument from Beckman Coulter.

[0222] Dispersion D (lubricant dispersion) is composed of 9 parts by weight of Zn stearate, 1 part by weight of Ghosenex TM A 20% zinc stearate dispersion consisting of L-3266 and 40 parts by weight of water.

[0223] Pigment P is a 72% coating kaolin suspension ( S, BASF).

[0224] The binder consisted of a 10% polyvinyl alcohol aqueous solution (Poval 28-99, Kuraray Europe).

[0225] A heat-sensitive application suspension is prepared by mixing under stirring 1 part A, 1 part B, 1 part C, 56 parts D, 146 parts pigment P and 138 parts binder solution (all parts by weight), considering the order of introduction B, D, C, P, A, binder, and making the solids content of the mixture about 25% with water.

[0226] The thermosensitive coating suspension thus obtained is used to prepare a composite structure formed of a paper support and a thermoreactive layer.

[0227] The thermosensitive recording materials were evaluated as described below (see Tables 3, 4 and 5).

[0228] (1) Dynamic color density:

[0229] Paper (6 cm wide strips) were thermally printed with a checkerboard pattern at 10 energy levels using an Atlantek 200 test printer (Atlantek, USA) with a Kyocera print bar of 200 dpi and 560 ohms at 20.6 V applied voltage and 0.8 ms maximum pulse width. Image density (optical density, od) was measured with a SpectroEye densitometer from X-Rite at an energy level of 0.45 mJ / dot. The measurement uncertainty of the od values ​​was estimated to be ≤ 2%.

[0230] (2) Static color density (starting temperature):

[0231] The recording sheet was pressed against a series of thermostatically controlled metal stamps heated to different temperatures, with a contact pressure of 0.2 kg / cm 2 , and a contact time of 5 seconds (Thermal Tester TP3000QM, Maschinenfabrik Hans Rychiger AG, Steffisburg, Switzerland). The image density (optical density) of the images thus prepared was measured with a SpectroEye densitometer from X-Rite.

[0232] By definition, the static starting point is the lowest temperature at which an optical density of 0.2 is achieved. The accuracy of the measurement method is ≤ ± 0.5 °C.

[0233] (3) Durability test of printed images

[0234] a) Durability test of printed images under artificial aging conditions:

[0235] Samples of thermal recording paper dynamically recorded according to the method obtained from (1) were stored for 7 days under each of the following conditions: i) 50°C (dry aging), ii) 40°C, 85% relative humidity (wet aging), and iii) under artificial light from a fluorescent tube with an illumination level of 16000 Lux (light aging).

[0236] Once the test time has elapsed, the image density is measured at an applied energy of 0.45 mJ / dot and set according to the formula (Equation 1) with respect to the corresponding image density value before artificial aging.

[0237]

[0238] The distribution of the % values ​​calculated according to (Formula 1) is ≤ ±2 percentage points.

[0239] b) Durability against plasticizers:

[0240] A fresh-keeping foil containing a plasticizer (PVC foil with 20 to 25% dioctyl adipate) was brought into contact with a sample of the thermal recording paper dynamically recorded according to the method of (1), folding and air inclusion were avoided, rolled into a roll, and stored for 16 hours. One sample was stored at room temperature (20 to 22° C.), and the second sample was stored at 40° C. (20 to 22° C.). Once the foil was removed, the image density (od) was measured and set according to the formula (Formula 1) with respect to the corresponding image density value before the influence of the plasticizer.

[0241] c) Durability of adhesive:

[0242] Place a piece of transparent tesa self-adhesive tape ( A clear, transparent, #57315) and a tesa packaging tape (#04204) were respectively bonded to a sample of the thermal recording paper dynamically recorded according to the method of (1), avoiding folds and air inclusions. After storage at room temperature (20 to 22° C.), the image density (od) was measured after 24 hours and after 7 days - with the relevant adhesive tape - and assigned to it according to the formula (Formula 1) with respect to the image density value determined in a similar manner for the freshly bonded sample.

[0243] (4) Shelf life of unprinted thermal paper:

[0244] The sheet of recording paper was cut into three identical strips. One strip was dynamically recorded according to the method of (1), and the image density was measured. The other two strips were stored in an unprinted (white) state for 4 weeks in the following climates: a) 40°C and 85% relative humidity (rh) and b) 60°C and 50% relative humidity (rh).

[0245] After conditioning the paper at room temperature, the paper was dynamically printed according to the method of (1) and the image density was measured using a densitometer at an applied energy of 0.45 mJ / dot. The remaining writing performance (%) of the stored sample relative to the fresh (unaged) sample was calculated according to the formula (Formula 1).

[0246] Tables 3 to 5 summarize the evaluations of the prepared recording materials.

[0247]

[0248] *Percentage of remaining image density according to Formula 1

[0249] Table 3: Image density, onset temperature and artificial aging

[0250]

[0251] * The percentage of remaining image density according to Equation 1.

[0252] Table 4: Durability of printed images

[0253]

[0254] * The percentage of remaining image density according to Formula 1

[0255] Table 5: Writing performance after storage

[0256] It can be inferred from the above examples that the heat-sensitive recording material of the present invention exhibits the following advantageous properties in particular:

[0257] (1) The recorded images of the heat-sensitive recording material based on the color developer according to the present invention have a printing density (optical density) superior to / equivalent to that of the comparative example using a known color developer (Table 3).

[0258] (2) The temperature at which visually perceptible graying occurs in the recording material according to the present invention (static onset point) is equivalent to or higher than the temperature at which visually perceptible graying occurs in the comparative example using a known color developer (Table 3).

[0259] (3) The heat-sensitive recording materials subjected to the aging test showed high image stability that was better than or comparable to that of the comparative examples using known color developers (Table 3).

[0260] (4) After the action of the hydrophobic agent (binder, plasticizer), the printed image hardly fades or fades only slightly. Compared with the heat-sensitive recording materials using known non-phenolic color developers, the image durability is better and largely meets the requirements of marketable heat-sensitive recording materials (Table 4).

[0261] (5) Printing of the thermosensitive recording material stored under extreme conditions for several weeks resulted in an image density that was almost the same as that of the thermosensitive recording material that had not been stored (fresh) (Table 5).

[0262] (6) With the color developer according to the invention it is possible to obtain a heat-sensitive recording material which is considered to be of high quality in all critical aspects for its application. Recording materials based on known color developers do not have a relatively good / balanced performance profile in all tested properties.

Claims

1. A compound of formula (I), Ar 1 -NH-CO-NH-C6H4-SO2-O-C6H4-NH-CO-NH-Ar 2 (I) Among them, Ar 1 and Ar 2 are independently of one another unsubstituted or substituted phenyl groups, naphthyl groups and / or heteroaryl groups, wherein Ar 1 is substituted with at least one C1-C5 alkyl group, alkenyl group, alkynyl group, benzyl group, formyl group, halogen group, NO2 group, CN group, R-CO group, RO group, RO2C group, R-OCO group, R-SO2O group, RO-SO2 group, R-SO2-NH group, R-NH-SO2 group, R-NH-CO group or R-CO-NH group, wherein R is a C1-C5 alkyl group, alkenyl group, alkynyl group, phenyl group, tolyl group or benzyl group; Ar 2 It is substituted by at least one C1-C5 alkyl group, alkenyl group, alkynyl group, benzyl group, formyl group, halogen group, NO2 group, CN group, R-CO group, RO group, RO2C group, R-OCO group, R-SO2O group, RO-SO2 group, R-SO2-NH group, R-NH-SO2 group, R-NH-CO group or R-CO-NH group, wherein R is a C1-C5 alkyl group, an alkenyl group, an alkynyl group, a phenyl group, a tolyl group or a benzyl group.

2. The compound according to claim 1, wherein Ar 1 is a phenyl group.

3. A compound according to claim 1 or 2, wherein Ar 2 is a phenyl group.

4. The compound according to claim 1, wherein Ar 1 It is monosubstituted.

5. A compound according to claim 1 or 2, wherein Ar 1 It is a monosubstituted phenyl group.

6. A compound according to claim 1 or 2, wherein Ar 2 It is monosubstituted.

7. A compound according to claim 1 or 2, wherein Ar 2 It is a monosubstituted phenyl group.

8. A compound according to claim 1 or 2, wherein Ar 1 is a phenyl group, and wherein Ar 2 is a phenyl group.

9. A compound according to claim 1 or 2, wherein Ar 1 -NH-CO-NH group and the Ar 2 The -NH-CO-NH group is arranged at the 2 and 3' positions, 2 and 4' positions, 3 and 2' positions, 3 and 3' positions, 3 and 4' positions, 4 and 2' positions, 4 and 3' positions or 4 and 4' positions, respectively, with respect to the -C6H4-SO2-O-C6H4 group.

10. A heat-sensitive recording material comprising a carrier substrate and a heat-sensitive color-forming layer containing at least one color former and at least one phenol-free color developer, wherein the at least one phenol-free color developer is a compound of formula (I) according to any one of claims 1 to 9.

11. The thermosensitive recording material according to claim 10, wherein the color developer is present in an amount of 3 to 35% by weight with respect to the total solid content of the thermosensitive layer.

12. The thermosensitive recording material according to claim 10, wherein the color developer is present in an amount of 10 to 25% by weight with respect to the total solid content of the thermosensitive layer.

13. The heat-sensitive recording material according to claim 10 or 11, wherein the at least one color former is a dye of triphenylmethane type, fluoran type, azaphthalide type and / or fluorene type.

14. The heat-sensitive recording material according to claim 10 or 11, wherein one or more non-phenolic color developers are present in addition to the phenol-free color developer.

15. A process for producing a heat-sensitive recording material according to any one of claims 10 to 14, wherein an aqueous suspension containing the starting material of the heat-sensitive color-forming layer is applied to a carrier substrate and dried, wherein the aqueous application suspension has a solids content of 20 to 75% by weight and is applied and dried by a curtain coating method at a coating equipment operating speed of at least 400 m / min.

16. The process according to claim 15, wherein the aqueous application suspension has a solids content of 30 to 50% by weight.

17. The method according to claim 15, wherein coating and drying are carried out by a curtain coating process at a coating equipment operating speed of at least 1000 m / min.

18. The method according to claim 15, wherein coating and drying are carried out by a curtain coating process at a coating equipment operating speed of at least 1500 m / min.

19. A heat-sensitive recording material obtainable by a process according to any one of claims 15 to 18.

Citation Information

Patent Citations

  • methods for manufacturing an information recording material and coating solutions for use in this material

    DE10196052T1

  • Thermosensitive recording material

    EP0526072A1

  • Thermosensitive recording material

    EP0620122B1

  • Thermal recording sheet