A composite high-weather-resistant solar cell back sheet and preparation method thereof
By using the structure of the PO inner layer, the polyester support layer and the PO outer layer in the photovoltaic backplane and using polyether polyurethane adhesive for bonding, the problem of poor performance of the existing photovoltaic backplane under harsh conditions is solved, and higher weather resistance and stability are achieved.
Patent Information
- Application Number
- CN202111659983.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2025-03-21
- Estimated Expiration
- 2041-12-31
AI Technical Summary
The existing photovoltaic back panels are difficult to play a long-term role under severe conditions such as moisture, heat, and sun exposure. The glue medium connection between the composite layers is easily affected by water vapor and temperature, and the bonding strength cannot be maintained, resulting in problems such as shedding and cracking.
The structure is laminated in sequence by PO inner layer, polyester support layer and PO outer layer, and bonded with polyether polyurethane adhesive to form a tight and stable connection. In this structure, the polyester support layer consists of a specific formula polyester base material and nano-scale titanium dioxide, which enhances the aging resistance of the back plate.
It significantly improves the performance of the photovoltaic backplane such as moisture and heat resistance, UV resistance, steaming resistance, high and low temperature circulation resistance and low water vapor transmission, avoids defects such as bubbles, delamination, cracking and yellowing, making the backplane both mechanical strength and chemical stability.
Smart Images

Figure BDA0003449271580000151
Abstract
Description
Technical Field
[0001] The present invention relates to the field of IPC C08 technology, and in particular to a composite high-weather-resistant solar cell back sheet and a preparation method thereof. Background Art
[0002] In the existing photovoltaic backplane structure, when the PET layer and other layers are bonded by adhesives, there is a problem that it is difficult to strike a balance between adhesion and processability; the photovoltaic backplane has a high water vapor permeability and is difficult to function for a long time under harsh conditions such as humidity, heat, and exposure.
[0003] Chinese patent CN104559080 discloses a thermoplastic polyester polyethylene composition and its application, using polyethylene terephthalate as a thermoplastic resin, and reacting with polyethylene, maleic anhydride grafted modified ethylene vinyl acetate copolymer, antioxidant 1010 and antioxidant 168 to obtain a material used for solar cell backplane, the shrinkage rate of the obtained material is reduced, and the mechanical properties are improved; Chinese patent CN108075006 discloses a multi-layer solar cell backplane, using a first polyethylene layer, a first adhesive resin layer, a polyester layer, a second adhesive resin layer, and a second polyethylene layer for compounding, through cast compounding and electron beam radiation cross-linking, a multi-layer solar cell backplane is obtained, and the heat resistance of the backplane is improved; Chinese patent CN205395342 discloses a high water-resistant and high-reflective solar cell backplane and a solar cell module containing the same, and a backplane structure with low cost and good water resistance is formed by co-extrusion of a resin film layer, a water-resistant layer and a weather-resistant layer. However, the above-mentioned existing technologies still fail to simultaneously solve the technical problems of heat resistance, water resistance, UV aging resistance, etc. of photovoltaic backsheets; the resulting photovoltaic backsheets cannot meet the requirements of use in harsh outdoor conditions, limiting the application of photovoltaic modules.
[0004] In response to the above problems, this application has achieved multiple performance improvements of the photovoltaic backplane, such as moisture and heat resistance, UV resistance, cooking resistance, high and low temperature cycle resistance, and low water vapor permeability, by multiple optimizations of the PET structural layer and adhesive of the solar cell backplane. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present invention provides a composite high weather resistance solar cell back sheet. The structure of the solar cell back sheet is a PO inner layer, a polyester support layer and a PO outer layer stacked in sequence.
[0006] In some preferred embodiments, the thickness ratio of the PO inner layer, the polyester support layer and the PO outer layer is (1-8): (10-36): (0.5-10).
[0007] More preferably, the thickness ratio of the PO inner layer, the polyester support layer and the PO outer layer is (1-5): (15-30): (1-5).
[0008] In some preferred embodiments, the raw materials of the PO inner layer include: PE base material, UV inhibitor, antioxidant, and additive A.
[0009] Further preferably, the raw materials of the PO inner layer include: based on the total mass of the PO inner layer, 94-99% of PE base material, 0.2-2% of UV inhibitor, 0.1-2% of antioxidant, and 0-5% of auxiliary agent A.
[0010] In some preferred embodiments, the raw materials of the polyester support layer include: polyester base material, filler, toughening agent, anti-hydrolysis agent, anti-UV agent, antioxidant, and additive B.
[0011] Further preferably, the raw materials of the polyester support layer include: based on the total mass of the polyester support layer, 80-99% polyester base material, 1-15% filler, 0.5-5% toughening agent, 0.1-2% anti-hydrolysis agent, 0.1-1.5% anti-UV agent, 0-2% antioxidant, and 0-3% additive B.
[0012] In some preferred embodiments, the raw materials of the PO outer layer include: polyolefin mixture, UV inhibitor, filler, antioxidant, and additive C.
[0013] More preferably, the raw materials of the PO outer layer include: based on the total mass of the PO outer layer, 85-98% of a polyolefin mixture, 0.1-2% of an anti-UV agent, 1-10% of a filler, 0.1-2% of an antioxidant, and 0-1.5% of an additive C.
[0014] In some preferred embodiments, the PE base material has a melt flow rate of 2-10 g / 10 min, a tensile yield strength of 15-40 MPa, and an elongation at break of 400-800%.
[0015] More preferably, the PE base material has a melt flow rate of 5 g / 10 min, a tensile yield strength of 27 MPa, and an elongation at break of 650%; specifically, it is American Dow HDPE 05962B.
[0016] In some preferred embodiments, the anti-UV agent includes a combination of one or more of hindered amines, benzophenones, benzotriazoles, triazines, acrylonitriles, oxamides, and organic nickels.
[0017] More preferably, the anti-UV agent is a hindered amine. Examples of hindered amines include, but are not limited to, a combination of one or more of GW-480, GW-622, GW-944, GW-540, Tinuvin 770, UV-3853, UV-3346, and UV-3529.
[0018] More preferably, the anti-UV agent is UV-3529 and / or UV-3853, and both UV-3529 and UV-3853 are from Cytec Chemicals of the United States.
[0019] In some preferred embodiments, the antioxidant includes a combination of one or more of hindered phenols, thioether esters, phosphites, and thiols.
[0020] More preferably, the antioxidants are hindered phenols and thioether esters, and the mass ratio of hindered phenols to thioether esters is (0.5-2.5):1.
[0021] Examples of hindered phenols include at least one of antioxidant 1010, antioxidant 1076, antioxidant 1098, and antioxidant 1024.
[0022] Examples of the thioether esters include antioxidant DLTP and / or antioxidant DSTP.
[0023] In some preferred embodiments, the additive A includes one or more combinations of PS-g-EGMA, PP-g-ST, ABS-g-MAH, PE-g-ST, PP-g-MAH, and PE-g-MAH.
[0024] In some preferred embodiments, the polyester base material is PET and / or TPEE, more preferably TPEE.
[0025] In some preferred embodiments, the TPEE (thermoplastic polyester elastomer) has a melt flow rate of 2-15 g / 10 min, a tensile modulus of 15-35 MPa, and an elongation at break of >200%.
[0026] More preferably, the polyester base material is TPEE, with a melt flow rate of 5 g / 10 min, a tensile modulus of 240 MPa, and an elongation at break of 300%; specifically, it is DuPont TPEE HTR8425 NC010 from the United States.
[0027] In some preferred embodiments, the filler includes a combination of one or more of titanium dioxide, calcium carbonate, calcined kaolin, talc, wollastonite, and hollow glass microspheres.
[0028] More preferably, the filler is titanium dioxide. The titanium dioxide is nano-grade titanium dioxide produced by a gas phase method, and the specific surface area of the nano-grade titanium dioxide is 30-60 m 2 / g, and the average particle size is 15-30nm.
[0029] In some preferred embodiments, the toughening agent is preferably an ethylene copolymer, such as DuPont Elvaloy 4170.
[0030] In some preferred embodiments, the anti-hydrolysis agent includes carbodiimide, specifically N,N'-di(2,6-diisopropylphenyl)carbodiimide, CAS No. 2162-74-5.
[0031] In some preferred embodiments, the auxiliary agent B includes a coupling agent, and the coupling agent is a combination of one or more of a silane coupling agent, a titanate coupling agent, and a rare earth coupling agent.
[0032] More preferably, the coupling agent is a titanate coupling agent, such as TC-131.
[0033] In some preferred embodiments, the polyolefin mixture includes at least two of PP, PE, EPDM, POE, and OBC.
[0034] More preferably, the polyolefin mixture comprises PP (polypropylene), PE (polyethylene) and POE (polyethylene octene elastomer); the weight ratio of PP, PE and POE is (1-4): (2.5-6): (0.5-3)
[0035] In some preferred embodiments, the auxiliary agent C includes a free radical scavenger and a free radical quencher; the free radical scavenger is preferably a hindered amine, such as BASF Tinuvin 123; the free radical quencher is preferably an organic complex of nickel, such as Zantedeschia 1084.
[0036] The photovoltaic backplane is located on the back of the solar cell and builds the outermost protective barrier for the photovoltaic module. The environmental tolerance of the photovoltaic backplane directly affects the service life of the module. The existing photovoltaic backplane cannot meet the long-term stable use in humid, hot and humid environments and light conditions. On the one hand, the backplane material is prone to degradation and aging in harsh environments, and the physical and mechanical properties of the product deteriorate; on the other hand, although the composite layer structure can form a performance complementary effect to a certain extent, when the composite layers are connected by adhesive media, the adhesive layer is affected by water vapor and temperature, the bonding strength cannot be maintained, and the adhesive layer is prone to falling off and cracking.
[0037] After extensive research, the applicant found that the use of a polyester base material with a melt flow rate of 2-15g / 10min, a tensile modulus of 15-35MPa, and an elongation at break greater than 200% as the base material of the middle support layer of the backplane, combined with a specific surface area of 30-60m2 / g and an average particle size of 15-30nm of nano-grade titanium dioxide, can significantly improve the aging resistance of the photovoltaic backplane. The resulting backplane still has high mechanical strength after high and low temperature cycle treatment. The reason may be that the degradation activity of polyethylene terephthalate is inhibited under this formula system, and the carbon-carbon main chain is protected by polar molecules with the participation of alkaline small molecule additives. At the same time, inorganic particles of specific specifications are uniformly dispersed in the three-dimensional structure of the polymer space, which inhibits the penetration of water vapor, acidic components, etc. into the backplane structure to erode the material, thereby enhancing the backplane's resistance to environmental changes, improving weather resistance, and not prone to cracking and yellowing defects under conditions of humidity, high temperature, and sun exposure, thereby extending its service life.
[0038] The second aspect of the present invention provides a method for preparing a composite high-weather-resistant solar cell back sheet, wherein a PO inner layer, a polyester support layer and a PO outer layer are sequentially laminated and bonded using an adhesive to obtain a finished back sheet.
[0039] In some preferred embodiments, the adhesive includes a combination of one or more of polyurethane adhesive, epoxy resin adhesive, acrylate adhesive, and silicone adhesive.
[0040] More preferably, the adhesive is a polyurethane adhesive; and even more preferably, a polyether polyurethane adhesive.
[0041] In some preferred embodiments, the raw materials of the polyether polyurethane adhesive are, by weight, 50-70 parts of polyglycol, 30-54 parts of diisocyanate, 0.1-2 parts of catalyst, 2-15 parts of chain extender, 0-5 parts of rheological additive, and 4-66 parts of solvent.
[0042] Preferably, the polyglycol includes at least one of polyoxypropylene glycol and polyoxyethylene glycol.
[0043] Preferably, the average molecular weight of the polyglycol is 400-4000.
[0044] More preferably, the polyglycol is polyoxypropylene glycol and polyoxyethylene glycol in a weight ratio of 1:(2-5).
[0045] Preferably, the chain extender includes one or more of 1,4-butanediol, dipropylene glycol, diethylene glycol, and 1,2-propylene glycol.
[0046] More preferably, the chain extender is 1,4-butanediol and dipropylene glycol; the weight ratio of 1,4-butanediol to dipropylene glycol is (0.5-3):1.
[0047] Preferably, the diisocyanate is a diisocyanate commonly used in the art, such as TDI, MDI, HDI, and IPDI.
[0048] The use of specific polyester base materials and additives to react can improve the spatial structural density of the TPEE structural layer and optimize the mechanical properties and weather resistance of the backplane. However, the TPEE structural layer and the adhesive have poor bonding strength, the middle polyester support layer is easily separated from the upper and lower layers, and the functional layers of the backplane cannot fully play their roles. The applicant further explored and found that the use of polyether polyurethane adhesives can promote the effective bonding between the polyester support layer and the PO inner / outer layer, and improve the hydrolysis resistance of the material. It was unexpectedly discovered that the reaction activity of polyglycols with an average molecular weight of 400-4000 and diisocyanates is high, and further combined with 1,4-butanediol and dipropylene glycol with a weight ratio of (0.5-3): 1 as chain extenders, the polyurethane generated by the reaction can effectively penetrate into the backplane composite layer structure, and the bonding sites in the composite material structure increase, forming a mechanical interlocking effect. Under the action of the adhesive with high curing strength, the backplane forms a tight and stable connection effect of the PO inner layer-polyester support layer-PO outer layer. At the same time, it was found that when the polyglycol is polyoxypropylene glycol and polyoxyethylene glycol in a weight ratio of 1: (2-5), the water resistance and aging resistance of the adhesive in the backboard structure are also significantly improved. Together with the performance-optimized TPEE structural layer, the changes in the high / low temperature layer structure, the changes in the internal structure of the photovoltaic backboard under high temperature and high humidity environments and light conditions are suppressed, thereby improving the moisture and heat resistance and cooking resistance of the photovoltaic backboard, and giving the photovoltaic modules excellent processing performance and a long service life.
[0049] Beneficial effects:
[0050] The composite high-weather-resistant solar cell backsheet provided by the present invention has both processing performance and weather resistance; by optimizing the PET structural layer and the adhesive, multiple performances of the photovoltaic backsheet, such as moisture and heat resistance, UV resistance, cooking resistance, high and low temperature cycle resistance, and low water vapor transmission rate, are improved simultaneously, and defects such as bubbling, delamination, cracking, and yellowing that are prone to occur in conventional solar cell backsheets under harsh conditions are solved, so that the backsheet has both mechanical strength and chemical stability, and can meet the use requirements of photovoltaic modules under various working environments. DETAILED DESCRIPTION
[0051] Example 1.
[0052] This embodiment provides a composite high weather resistance solar cell back sheet, wherein the structure of the solar cell back sheet is a PO inner layer, a polyester support layer and a PO outer layer stacked in sequence.
[0053] The thicknesses of the PO inner layer, the polyester support layer and the PO outer layer are 30 μm, 200 μm and 40 μm respectively.
[0054] The raw materials of the PO inner layer include: based on the total mass of the PO inner layer, 96.5% of PE base material, 1% of UV inhibitor, 1% of antioxidant and 1.5% of auxiliary agent A.
[0055] The raw materials of the polyester support layer include: based on the total mass of the polyester support layer, 85.7% polyester base material, 8% filler, 2.5% toughening agent, 1% anti-hydrolysis agent, 0.6% anti-UV agent, 1.2% antioxidant and 1% auxiliary agent B.
[0056] The raw materials of the PO outer layer include: based on the total mass of the PO outer layer, 90.6% of polyolefin mixture, 0.8% of UV inhibitor, 6% of filler, 1% of antioxidant and 1.6% of auxiliary agent C.
[0057] The PE base material has a melt flow rate of 5 g / 10 min, a tensile yield strength of 27 MPa, and an elongation at break of 650%; specifically, it is American Dow HDPE 05962B.
[0058] The anti-UV agent is a hindered amine, specifically UV-3529 and UV-3853 in a weight ratio of 2:1, and both UV-3529 and UV-3853 are from Cytec Chemicals of the United States.
[0059] The antioxidants are hindered phenols and thioether esters, and the mass ratio of hindered phenols to thioether esters is 1.4:1.
[0060] The hindered phenols are specifically antioxidant 235; the thioether esters are specifically antioxidant DSTP.
[0061] The auxiliary agent A is specifically PS-g-EGMA, which is sourced from NOF Corporation.
[0062] The polyester base material is TPEE, the melt flow rate of TPEE is 5g / 10min, the tensile modulus is 240MPa, and the elongation at break is 300%; specifically, it is American DuPont TPEE HTR8425 NC010.
[0063] The filler is nano-grade titanium dioxide produced by gas phase method, and the specific surface area of the nano-grade titanium dioxide is 50m 2 / g, with an average particle size of 21nm; specifically, Degussa AEROXIDE P25.
[0064] The toughening agent is an ethylene copolymer with a melt flow rate of 8 g / 10 min, specifically DuPont Elvaloy 4170 from the United States.
[0065] The anti-hydrolysis agent is N,N'-di(2,6-diisopropylphenyl)carbodiimide, and its CAS number is 2162-74-5.
[0066] The auxiliary agent B is a coupling agent, specifically a titanate coupling agent TC-131.
[0067] The polyolefin mixture comprises PP, PE and POE; the weight ratio of PP, PE and POE is 3:4:2.
[0068] The PE has a melt index of 8 g / 10 min and a tensile yield strength of 10.3 MPa; specifically, it is American DuPont LDPE0098 S LE.
[0069] The PP has a melt index of 8.7 g / 10 min and a flexural modulus of 1500 MPa; specifically, Malaysian CIPC PP-2301.
[0070] The POE has a melt index of 0.5 g / 10 min and a tensile strength of 35 kN / m; specifically, it is ExxonMobil POE 5061 from the United States.
[0071] The auxiliary agent C is a free radical scavenger and a free radical quencher in a weight ratio of 1:1; the free radical scavenger is a hindered amine compound, specifically BASF Tinuvin 123; the free radical quencher is an organic complex of nickel, specifically Zantedeschia 1084.
[0072] The second aspect of this embodiment provides a method for preparing a composite high-weather-resistant solar cell backplane, wherein an adhesive is used to sequentially stack and bond a PO inner layer, a polyester support layer, and a PO outer layer (the coating thickness of the adhesive is 10 μm), and the layers are placed at 60°C for 3 hours to shape, thereby obtaining a finished backplane product.
[0073] The adhesive is a polyurethane adhesive, specifically a polyether polyurethane adhesive; the raw materials of the polyether polyurethane adhesive are, by weight, 64 parts of polyglycol, 40 parts of diisocyanate, 0.1 parts of catalyst, 8 parts of chain extender, 1 part of rheological additive, and 20 parts of solvent.
[0074] The polyglycol is polyoxypropylene glycol and polyoxyethylene glycol in a weight ratio of 1:3.
[0075] The average molecular weight of the polyoxypropylene diol is 2000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0076] The average molecular weight of the polyoxyethylene diol is 1000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0077] The diisocyanates are TDI (toluene diisocyanate) and IPDI (isophorone diisocyanate); the weight ratio of TDI to IPDI is 1:2.
[0078] The chain extender is 1,4-butanediol and dipropylene glycol; the weight ratio of 1,4-butanediol to dipropylene glycol is 2:1.
[0079] The rheological additive has a viscosity of 2900 mPa.s (25° C.) and is derived from Rohm and Haas RM-2020.
[0080] The catalyst is stannous octoate, and its CAS number is 301-10-0.
[0081] The solvent is ethyl acetate.
[0082] The preparation steps of the polyether adhesive are as follows: mixing raw materials except diisocyanate according to the formula amount, stirring evenly at 800 rpm to obtain material A; before use, adding diisocyanate to material A, mixing evenly, and obtaining the polyether adhesive.
[0083] Example 2.
[0084] This embodiment provides a composite high weather resistance solar cell back sheet, wherein the structure of the solar cell back sheet is a PO inner layer, a polyester support layer and a PO outer layer stacked in sequence.
[0085] The thicknesses of the PO inner layer, the polyester support layer and the PO outer layer are 30 μm, 200 μm and 40 μm respectively.
[0086] The raw materials of the PO inner layer include: based on the total mass of the PO inner layer, 98% of PE base material, 0.2% of UV inhibitor, 0.8% of antioxidant and 1% of auxiliary agent A.
[0087] The raw materials of the polyester support layer include: based on the total mass of the polyester support layer, 86% polyester base material, 5% filler, 3% toughening agent, 1.2% anti-hydrolysis agent, 0.4% anti-UV agent, 1.4% antioxidant and 2% auxiliary agent B.
[0088] The raw materials of the PO outer layer include: based on the total mass of the PO outer layer, 88% of polyolefin mixture, 1.4% of UV inhibitor, 9% of filler, 0.5% of antioxidant and 1.1% of auxiliary agent C.
[0089] The PE base material has a melt flow rate of 5 g / 10 min, a tensile yield strength of 27 MPa, and an elongation at break of 650%; specifically, it is American Dow HDPE 05962B.
[0090] The anti-UV agent is a hindered amine, specifically UV-3529 and UV-3853 in a weight ratio of 2:1, and both UV-3529 and UV-3853 are from Cytec Chemicals of the United States.
[0091] The antioxidants are hindered phenols and thioether esters, and the mass ratio of hindered phenols to thioether esters is 1.4:1.
[0092] The hindered phenols are specifically antioxidant 235; the thioether esters are specifically antioxidant DSTP.
[0093] The auxiliary agent A is specifically PS-g-EGMA, which is sourced from NOF Corporation.
[0094] The polyester base material has a melt flow rate of 5 g / 10 min, a tensile modulus of 240 MPa, and an elongation at break of 300%; specifically, it is American DuPont TPEE HTR8425 NC010.
[0095] The filler is nano-grade titanium dioxide produced by gas phase method, and the specific surface area of the nano-grade titanium dioxide is 50m 2 / g, with an average particle size of 21nm; specifically, Degussa AEROXIDE P25.
[0096] The toughening agent is an ethylene copolymer with a melt flow rate of 8 g / 10 min, specifically DuPont Elvaloy 4170 from the United States.
[0097] The anti-hydrolysis agent is N,N'-di(2,6-diisopropylphenyl)carbodiimide, and its CAS number is 2162-74-5.
[0098] The auxiliary agent B is a coupling agent, specifically a titanate coupling agent TC-131.
[0099] The polyolefin mixture comprises PP, PE and POE; the weight ratio of PP, PE and POE is 3:4:2.
[0100] The PE has a melt index of 8 g / 10 min and a tensile yield strength of 10.3 MPa; specifically, it is American DuPont LDPE0098 S LE.
[0101] The PP has a melt index of 8.7 g / 10 min and a flexural modulus of 1500 MPa; specifically, Malaysian CIPC PP-2301.
[0102] The POE has a melt index of 0.5 g / 10 min and a tensile strength of 35 kN / m; specifically, it is ExxonMobil POE 5061 from the United States.
[0103] The auxiliary agent C is a free radical scavenger and a free radical quencher in a weight ratio of 1:1; the free radical scavenger is a hindered amine compound, specifically BASF Tinuvin 123; the free radical quencher is an organic complex of nickel, specifically Zantedeschia 1084.
[0104] The second aspect of this embodiment provides a method for preparing a composite high-weather-resistant solar cell backplane, wherein an adhesive is used to sequentially stack and bond a PO inner layer, a polyester support layer, and a PO outer layer (the coating thickness of the adhesive is 10 μm), and the layers are placed at 60°C for 3 hours to shape, thereby obtaining a finished backplane product.
[0105] The adhesive is a polyurethane adhesive, specifically a polyether polyurethane adhesive; the raw materials of the polyether polyurethane adhesive are, by weight, 64 parts of polyglycol, 40 parts of diisocyanate, 0.1 parts of catalyst, 8 parts of chain extender, 1 part of rheological additive, and 20 parts of solvent.
[0106] The polyglycol is polyoxypropylene glycol and polyoxyethylene glycol in a weight ratio of 1:3.
[0107] The average molecular weight of the polyoxypropylene diol is 2000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0108] The average molecular weight of the polyoxyethylene diol is 1000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0109] The diisocyanates are TDI (toluene diisocyanate) and IPDI (isophorone diisocyanate); the weight ratio of TDI to IPDI is 1:2.
[0110] The chain extender is 1,4-butanediol and dipropylene glycol; the weight ratio of 1,4-butanediol to dipropylene glycol is 2:1.
[0111] The rheological additive has a viscosity of 2900 mPa.s (25° C.) and is derived from Rohm and Haas RM-2020.
[0112] The catalyst is stannous octoate, and its CAS number is 301-10-0.
[0113] The solvent is ethyl acetate.
[0114] The preparation steps of the polyether adhesive polyester polyol are as follows: mixing raw materials except diisocyanate according to the formula amount, stirring evenly at 800 rpm to obtain material A; before use, adding diisocyanate to material A, mixing evenly, and obtaining the polyether adhesive.
[0115] Example 3.
[0116] This embodiment provides a composite high weather resistance solar cell back sheet, wherein the structure of the solar cell back sheet is a PO inner layer, a polyester support layer and a PO outer layer stacked in sequence.
[0117] The thicknesses of the PO inner layer, the polyester support layer and the PO outer layer are 30 μm, 240 μm and 30 μm respectively.
[0118] The raw materials of the PO inner layer include: based on the total mass of the PO inner layer, 96.5% of PE base material, 1% of UV inhibitor, 1% of antioxidant and 1.5% of auxiliary agent A.
[0119] The raw materials of the polyester support layer include: based on the total mass of the polyester support layer, 85.7% polyester base material, 8% filler, 2.5% toughening agent, 1% anti-hydrolysis agent, 0.6% anti-UV agent, 1.2% antioxidant and 1% auxiliary agent B.
[0120] The raw materials of the PO outer layer include: based on the total mass of the PO outer layer, 90.6% of polyolefin mixture, 0.8% of UV inhibitor, 6% of filler, 1% of antioxidant and 1.6% of auxiliary agent C.
[0121] The PE base material has a melt flow rate of 5 g / 10 min, a tensile yield strength of 27 MPa, and an elongation at break of 650%; specifically, it is American Dow HDPE 05962B.
[0122] The anti-UV agent is a hindered amine, specifically UV-3529 and UV-3853 in a weight ratio of 2:1, and both UV-3529 and UV-3853 are from Cytec Chemicals of the United States.
[0123] The antioxidants are hindered phenols and thioether esters, and the mass ratio of hindered phenols to thioether esters is 1.4:1.
[0124] The hindered phenols are specifically antioxidant 235; the thioether esters are specifically antioxidant DSTP.
[0125] The auxiliary agent A is specifically PS-g-EGMA, which is sourced from NOF Corporation.
[0126] The polyester base material has a melt flow rate of 5 g / 10 min, a tensile modulus of 240 MPa, and an elongation at break of 300%; specifically, it is American DuPont TPEE HTR8425 NC010.
[0127] The filler is nano-grade titanium dioxide produced by gas phase method, and the specific surface area of the nano-grade titanium dioxide is 50m 2 / g, with an average particle size of 21nm; specifically, Degussa AEROXIDE P25.
[0128] The toughening agent is an ethylene copolymer with a melt flow rate of 8 g / 10 min, specifically DuPont Elvaloy 4170 from the United States.
[0129] The anti-hydrolysis agent is N,N'-di(2,6-diisopropylphenyl)carbodiimide, and its CAS number is 2162-74-5.
[0130] The auxiliary agent B is a coupling agent, specifically a titanate coupling agent TC-131.
[0131] The polyolefin mixture comprises PP, PE and POE; the weight ratio of PP, PE and POE is 2.5:5:1.5.
[0132] The PE has a melt index of 8 g / 10 min and a tensile yield strength of 10.3 MPa; specifically, it is American DuPont LDPE0098 S LE.
[0133] The PP has a melt index of 8.7 g / 10 min and a flexural modulus of 1500 MPa; specifically, Malaysian CIPC PP-2301.
[0134] The POE has a melt index of 0.5 g / 10 min and a tensile strength of 35 kN / m; specifically, it is ExxonMobil POE 5061 from the United States.
[0135] The auxiliary agent C is a free radical scavenger and a free radical quencher in a weight ratio of 1:1; the free radical scavenger is a hindered amine compound, specifically BASF Tinuvin 123; the free radical quencher is an organic complex of nickel, specifically Zantedeschia 1084.
[0136] The second aspect of this embodiment provides a method for preparing a composite high-weather-resistant solar cell backplane, wherein an adhesive is used to sequentially stack and bond a PO inner layer, a polyester support layer, and a PO outer layer (the coating thickness of the adhesive is 10 μm), and the layers are placed at 60°C for 3 hours to shape, thereby obtaining a finished backplane product.
[0137] The adhesive is a polyurethane adhesive, specifically a polyether polyurethane adhesive; the raw materials of the polyether polyurethane adhesive are, by weight, 64 parts of polyglycol, 40 parts of diisocyanate, 0.1 parts of catalyst, 8 parts of chain extender, 1 part of rheological additive, and 20 parts of solvent.
[0138] The polyglycol is polyoxypropylene glycol and polyoxyethylene glycol in a weight ratio of 1:3.
[0139] The average molecular weight of the polyoxypropylene diol is 2000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0140] The average molecular weight of the polyoxyethylene diol is 1000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0141] The diisocyanates are TDI (toluene diisocyanate) and IPDI (isophorone diisocyanate); the weight ratio of TDI to IPDI is 1:2.
[0142] The chain extender is 1,4-butanediol and dipropylene glycol; the weight ratio of 1,4-butanediol to dipropylene glycol is 2:1.
[0143] The rheological additive has a viscosity of 2900 mPa.s (25° C.) and is derived from Rohm and Haas RM-2020.
[0144] The catalyst is stannous octoate, and its CAS number is 301-10-0.
[0145] The solvent is ethyl acetate.
[0146] The preparation steps of the polyether adhesive polyester polyol are as follows: mixing raw materials except diisocyanate according to the formula amount, stirring evenly at 800 rpm to obtain material A; before use, adding diisocyanate to material A, mixing evenly, and obtaining the polyether adhesive.
[0147] Example 4.
[0148] This embodiment provides a composite high weather resistance solar cell back sheet, wherein the structure of the solar cell back sheet is a PO inner layer, a polyester support layer and a PO outer layer stacked in sequence.
[0149] The thicknesses of the PO inner layer, the polyester support layer and the PO outer layer are 30 μm, 200 μm and 40 μm respectively.
[0150] The raw materials of the PO inner layer include: based on the total mass of the PO inner layer, 96.5% of PE base material, 1% of UV inhibitor, 1% of antioxidant, and 1.5% of auxiliary agent A.
[0151] The raw materials of the polyester support layer include: based on the total mass of the polyester support layer, 85.7% polyester base material, 8% filler, 2.5% toughening agent, 1% anti-hydrolysis agent, 0.6% anti-UV agent, 1.2% antioxidant and 1% auxiliary agent B.
[0152] The raw materials of the PO outer layer include: based on the total mass of the PO outer layer, 90.6% of polyolefin mixture, 0.8% of UV inhibitor, 6% of filler, 1% of antioxidant and 1.6% of auxiliary agent C.
[0153] The PE base material has a melt flow rate of 5 g / 10 min, a tensile yield strength of 27 MPa, and an elongation at break of 650%; specifically, it is American Dow HDPE 05962B.
[0154] The anti-UV agent is a hindered amine, specifically UV-3529 and UV-3853 in a weight ratio of 2:1, and both UV-3529 and UV-3853 are from Cytec Chemicals of the United States.
[0155] The antioxidants are hindered phenols and thioether esters, and the mass ratio of hindered phenols to thioether esters is 1.4:1.
[0156] The hindered phenols are specifically antioxidant 235; the thioether esters are specifically antioxidant DSTP.
[0157] The auxiliary agent A is specifically PS-g-EGMA, which is sourced from NOF Corporation.
[0158] The polyester base material has a melt flow rate of 5 g / 10 min, a tensile modulus of 240 MPa, and an elongation at break of 300%; specifically, it is American DuPont TPEE HTR8425 NC010.
[0159] The filler is nano-grade titanium dioxide produced by gas phase method, and the specific surface area of the nano-grade titanium dioxide is 50m 2 / g, average particle size 21nm; specifically Degussa AEROXIDE P25
[0160] The toughening agent is an ethylene copolymer with a melt flow rate of 8 g / 10 min, specifically DuPont Elvaloy 4170 from the United States.
[0161] The anti-hydrolysis agent is N,N'-di(2,6-diisopropylphenyl)carbodiimide, and its CAS number is 2162-74-5.
[0162] The auxiliary agent B is a coupling agent, specifically a titanate coupling agent TC-131.
[0163] The polyolefin mixture comprises PP, PE and POE; the weight ratio of PP, PE and POE is 5:1:4.
[0164] The PE has a melt index of 8 g / 10 min and a tensile yield strength of 10.3 MPa; specifically, it is American DuPont LDPE0098 S LE.
[0165] The PP has a melt index of 8.7 g / 10 min and a flexural modulus of 1500 MPa; specifically, Malaysian CIPC PP-2301.
[0166] The POE has a melt index of 0.5 g / 10 min and a tensile strength of 35 kN / m; specifically, it is ExxonMobil POE 5061 from the United States.
[0167] The auxiliary agent C is a free radical scavenger and a free radical quencher in a weight ratio of 1:1; the free radical scavenger is a hindered amine compound, specifically BASF Tinuvin 123; the free radical quencher is an organic complex of nickel, specifically Zantedeschia 1084.
[0168] The second aspect of this embodiment provides a method for preparing a composite high-weather-resistant solar cell backplane, wherein an adhesive is used to sequentially stack and bond a PO inner layer, a polyester support layer, and a PO outer layer (the coating thickness of the adhesive is 10 μm), and the layers are placed at 60°C for 3 hours to shape, thereby obtaining a finished backplane product.
[0169] The adhesive is a polyurethane adhesive, specifically a polyether polyurethane adhesive; the raw materials of the polyether polyurethane adhesive are, by weight, 64 parts of polyglycol, 40 parts of diisocyanate, 0.1 parts of catalyst, 8 parts of chain extender, 1 part of rheological additive, and 20 parts of solvent.
[0170] The polyglycol is polyoxypropylene glycol and polyoxyethylene glycol in a weight ratio of 1:3.
[0171] The average molecular weight of the polyoxypropylene diol is 2000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0172] The average molecular weight of the polyoxyethylene diol is 1000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0173] The diisocyanates are TDI (toluene diisocyanate) and IPDI (isophorone diisocyanate); the weight ratio of TDI to IPDI is 1:2.
[0174] The chain extender is 1,4-butanediol and dipropylene glycol; the weight ratio of 1,4-butanediol to dipropylene glycol is 2:1.
[0175] The rheological additive has a viscosity of 2900 mPa.s (25° C.) and is derived from Rohm and Haas RM-2020.
[0176] The catalyst is stannous octoate, and its CAS number is 301-10-0.
[0177] The solvent is ethyl acetate.
[0178] The preparation steps of the polyether adhesive polyester polyol are as follows: mixing raw materials except diisocyanate according to the formula amount, stirring evenly at 800 rpm to obtain material A; before use, adding diisocyanate to material A, mixing evenly, and obtaining the polyether adhesive.
[0179] Example 5.
[0180] This embodiment provides a composite high weather resistance solar cell back sheet, wherein the structure of the solar cell back sheet is a PO inner layer, a polyester support layer and a PO outer layer stacked in sequence.
[0181] The thicknesses of the PO inner layer, the polyester support layer and the PO outer layer are 30 μm, 200 μm and 40 μm respectively.
[0182] The raw materials of the PO inner layer include: based on the total mass of the PO inner layer, 96.5% of PE base material, 1% of UV inhibitor, 1% of antioxidant and 1.5% of auxiliary agent A.
[0183] The raw materials of the polyester support layer include: based on the total mass of the polyester support layer, 85.7% polyester base material, 8% filler, 2.5% toughening agent, 1% anti-hydrolysis agent, 0.6% anti-UV agent, 1.2% antioxidant and 1% auxiliary agent B.
[0184] The raw materials of the PO outer layer include: based on the total mass of the PO outer layer, 90.6% of polyolefin mixture, 0.8% of UV inhibitor, 6% of filler, 1% of antioxidant and 1.6% of auxiliary agent C.
[0185] The PE base material has a melt flow rate of 5 g / 10 min, a tensile yield strength of 27 MPa, and an elongation at break of 650%; specifically, it is American Dow HDPE 05962B.
[0186] The anti-UV agent is a hindered amine, specifically UV-3529 and UV-3853 in a weight ratio of 2:1, and both UV-3529 and UV-3853 are from Cytec Chemicals of the United States.
[0187] The antioxidants are hindered phenols and thioether esters, and the mass ratio of hindered phenols to thioether esters is 1.4:1.
[0188] The hindered phenols are specifically antioxidant 235; the thioether esters are specifically antioxidant DSTP.
[0189] The auxiliary agent A is specifically PS-g-EGMA, which is sourced from NOF Corporation.
[0190] The polyester base material has a melt flow rate of 5 g / 10 min, a tensile modulus of 240 MPa, and an elongation at break of 300%; specifically, it is American DuPont TPEE HTR8425 NC010.
[0191] The filler is nano-grade titanium dioxide produced by gas phase method, and the specific surface area of the nano-grade titanium dioxide is 50m 2 / g, average particle size 21nm; specifically Degussa AEROXIDE P25
[0192] The toughening agent is an ethylene copolymer with a melt flow rate of 8 g / 10 min, specifically DuPont Elvaloy 4170 from the United States.
[0193] The anti-hydrolysis agent is N,N'-di(2,6-diisopropylphenyl)carbodiimide, and its CAS number is 2162-74-5.
[0194] The auxiliary agent B is a coupling agent, specifically a titanate coupling agent TC-131.
[0195] The polyolefin mixture comprises PP, PE and POE; the weight ratio of PP, PE and POE is 3:4:2.
[0196] The PE has a melt index of 8 g / 10 min and a tensile yield strength of 10.3 MPa; specifically, it is American DuPont LDPE0098 S LE.
[0197] The PP has a melt index of 8.7 g / 10 min and a flexural modulus of 1500 MPa; specifically, Malaysian CIPC PP-2301.
[0198] The POE has a melt index of 0.5 g / 10 min and a tensile strength of 35 kN / m; specifically, it is ExxonMobil POE 5061 from the United States.
[0199] The auxiliary agent C is a free radical scavenger and a free radical quencher in a weight ratio of 1:1; the free radical scavenger is a hindered amine compound, specifically BASF Tinuvin 123; the free radical quencher is an organic complex of nickel, specifically Zantedeschia 1084.
[0200] The second aspect of this embodiment provides a method for preparing a composite high-weather-resistant solar cell backplane, wherein an adhesive is used to sequentially stack and bond a PO inner layer, a polyester support layer, and a PO outer layer (the coating thickness of the adhesive is 10 μm), and the layers are placed at 60°C for 3 hours to shape, thereby obtaining a finished backplane product.
[0201] The adhesive is a polyurethane adhesive, specifically a polyether polyurethane adhesive; the raw materials of the polyether polyurethane adhesive are, by weight, 64 parts of polyglycol, 40 parts of diisocyanate, 0.1 parts of catalyst, 8 parts of chain extender, 1 part of rheological additive, and 20 parts of solvent.
[0202] The polyglycol is polyoxypropylene glycol and polyoxyethylene glycol in a weight ratio of 1:1.
[0203] The average molecular weight of the polyoxypropylene diol is 2000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0204] The average molecular weight of the polyoxyethylene diol is 1000, and it is sourced from Nanjing Zhongshan Petrochemical Company.
[0205] The diisocyanates are TDI (toluene diisocyanate) and IPDI (isophorone diisocyanate); the weight ratio of TDI to IPDI is 1:2.
[0206] The chain extender is 1,4-butanediol.
[0207] The rheological additive has a viscosity of 2900 mPa.s (25° C.) and is derived from Rohm and Haas RM-2020.
[0208] The catalyst is stannous octoate, and its CAS number is 301-10-0.
[0209] The solvent is ethyl acetate.
[0210] The preparation steps of the polyether adhesive polyester polyol are as follows: mixing raw materials except diisocyanate according to the formula amount, stirring evenly at 800 rpm to obtain material A; before use, adding diisocyanate to material A, mixing evenly, and obtaining the polyether adhesive.
[0211] Performance Testing Methods
[0212] 1. Hot and cold cycle test
[0213] With reference to GB / T 31034 2014, the temperature resistance of the solar cell backsheets provided in Examples 1-5 was tested;
[0214] The test conditions are -40°C to 85°C, 6h / cycle, and 400 cycles.
[0215] Fifteen parallel samples were set for each group of examples, and the number of samples M showing delamination, blistering, discoloration, cracks, and adhesive layer stickiness after the hot and cold cycles was observed and recorded in Table 1.
[0216] 2.UV test
[0217] Referring to GB / T 31034 2014, the UV resistance of the solar cell backsheets provided in Examples 1-5 was tested; the test conditions were 60 kWh·m -2 , 72h; the initial value of the elongation at break and the retention rate k1 of the solar cell backsheet are recorded in Table 1.
[0218] 3. Constant humidity and heat test
[0219] With reference to GB / T 31034 2014, the moisture and heat resistance of the solar cell backsheets provided in Examples 1-5 were tested; the test conditions were 85° C., 85% RH, 3000 h; the initial value of the elongation at break and the retention rate k2 of the solar cell backsheets were recorded in Table 1.
[0220] 4. Tensile strength
[0221] With reference to ISO 1184, the tensile strength of the solar cell backsheets provided in Examples 1-5 was tested and recorded in Table 1.
[0222] Performance test data
[0223] Table 1. Performance test results
[0224]
Claims
1. A composite high weather resistance solar cell back sheet, characterized in that: The structure of the solar cell back sheet is a PO inner layer, a polyester support layer and a PO outer layer stacked in sequence; The raw materials of the polyester support layer include: polyester base material, filler, toughening agent, anti-hydrolysis agent, anti-UV agent, antioxidant, and auxiliary agent B; The polyester base material has a melt flow rate of 2-15 g / 10 min, a tensile modulus of 15-35 MPa, and an elongation at break of >200%; The raw materials of the PO outer layer include: polyolefin mixture, UV resistant agent, filler, antioxidant, and additive C; The polyolefin mixture comprises PP, PE and POE; the weight ratio of PP, PE and POE is (1-4): (2.5-6): (0.5-3); The filler is titanium dioxide, which is nano-grade titanium dioxide produced by gas phase method, and the specific surface area of the nano-grade titanium dioxide is 30-60m 2 / g, average particle size is 15-30nm; Adhesive is used to sequentially stack and bond the PO inner layer, the polyester support layer and the PO outer layer to obtain a finished back sheet; The adhesive is a polyether polyurethane adhesive; The raw materials of the polyether polyurethane adhesive are, by weight, 50-70 parts of polyglycol, 30-54 parts of diisocyanate, 0.1-2 parts of catalyst, 2-15 parts of chain extender, 0-5 parts of rheological additive, and 4-66 parts of solvent; The average molecular weight of the polyglycol is 400-4000; The chain extender is 1,4-butanediol and dipropylene glycol; the weight ratio of 1,4-butanediol to dipropylene glycol is (0.5-3):
1.
2. The composite high weather resistance solar cell back sheet according to claim 1, characterized in that: The thickness ratio of the PO inner layer, the polyester support layer and the PO outer layer is (1-8): (10-36): (0.5-10).
3. The composite high weather resistance solar cell back sheet according to claim 1, characterized in that: The raw materials of the PO inner layer include: PE base material, UV inhibitor, antioxidant and auxiliary agent A.
4. The composite high weather resistance solar cell back sheet according to claim 3, characterized in that: The PE base material has a melt flow rate of 2-10 g / 10 min, a tensile yield strength of 15-40 MPa, and an elongation at break of 400-800%.
5. The composite high weather resistance solar cell back sheet according to claim 3, characterized in that: The anti-UV agent includes one or more combinations of hindered amines, benzophenones, benzotriazoles, triazines, acrylonitriles, oxamides, and organic nickels.
6. The composite high weather resistance solar cell back sheet according to claim 3, characterized in that: The antioxidant includes one or more combinations of hindered phenols, thioether esters, phosphites, and mercaptans.
7. A method for preparing a composite high weather resistance solar cell back sheet according to any one of claims 1 to 6, characterized in that: The preparation step of the solar cell back sheet is to use an adhesive to sequentially stack and bond the PO inner layer, the polyester support layer and the PO outer layer to obtain a finished back sheet.
Citation Information
Patent Citations
Composite backboard used for solar cell and solar cell module including the composite backboard
CN104934494A
High-efficiency solar photovoltaic cell backboard and manufacturing method thereof
CN110315823A